Full text
Francisco Tomé Ferreira Teixeira Mechanical behavior of PA12 lattice structures produced by SLS Mechanical behavior of PA12 lattice structures produced by SLS Francisco Tomé Ferreira Teixeira UMinho | 2021 abril de 2021
2
Francisco Tomé Ferreira Teixeira Mechanical behavior of PA12 lattice structures produced by SLS Dissertação de Mestrado Mestrado Integrado em Engenharia de Polímeros Trabalho efetuado sob a orientação do(a): Professor Doutor António José Vilela Pontes Doutora Cátia Samanta Ribeiro da Silva abril de 2021
i DIREITOS DE AUTOR E CONDIÇÕES DE UTILIZAÇÃO DO TRABALHO POR TERCEIROS Este é um trabalho académico que pode ser utilizado por terceiros desde que respeitadas as regras e boas práticas internacionalmente aceites, no que concerne aos direitos de autor e direitos conexos. Assim, o presente trabalho pode ser utilizado nos termos previstos na licença abaixo indicada. Caso o utilizador necessite de permissão para poder fazer um uso do trabalho em condições não previstas no licenciamento indicado, deverá contactar o autor, através do RepositóriUM da Universidade do Minho. Atribuição - Não Comercial - Sem Derivações CC BY-NC-ND
ii ACKNOWLEDGEMENTS The present dissertation was a great challenge to me, and I wouldn't be more grateful for the possibility to conclude my university career with the research of an interesting and promising technology labeled Additive Manufacturing. It was made possible thanks to several. For this purpose, I could not fail to express my gratitude to several people, in no specific order, who made it possible and accompanied me throughout this journey. With great respect and gratitude, I would like to thank: - Pr. Dr. António J. Pontes, for his invaluable scientific guidance, support and all the patient, availability, advices and suggestions throughout this research; - Dr. Cátia Silva and Msc. André Lima, for their continuously guidance and help to circumvent the encountered obstacles; - To the DONE Lab, for allowing me to perform this research in its facilities; - To the Department of Polymer Engineering of the University of Minho, for providing me full access to their labs to carry out some of the experimental work. To the technician Manuel Escourido, for the essential collaboration and help in compression tests; - To the Polymer Engineering Innovation Center (PIEP), for providing me the realization of impact tests, specially, to Eng. Andreia Vilela for the essential help. To conclude, my sincere gratitude goes to my family, especially my parents and brother, and friends for all the unconditional support during this journey.
iii STATEMENT OF INTEGRITY I hereby declare having conducted this academic work with integrity. I confirm that I have not used plagiarism or any form of undue use of information or falsification of results along the process leading to its elaboration. I further declare that I have fully acknowledged the Code of Ethical Conduct of the University of Minho.
iv ABSTRACT Taking into account the rapid technological evolution and the growing demand, for the industrial sector to meet the most diverse needs of the market, Additive Manufacturing (AM) technology appears as a transformative approach to industrial production that enables the creation of lighter, stronger parts and systems. The versatility of this type of technology allows a reduction in production time and energy consumption, as well as, reducing material waste in the production of a product. It is in this last point that the technologies of AM stand out when comparing to the technologies of conventional manufacture. In AM technologies, it is possible to carry out the deposition of material in a controlled manner, where it is really necessary and, at the same time, ensure the necessary mechanical properties to meet the product requirements. Due to its versatility and rapid technological advances, it has become possible to implement typological optimization in AM. In this context, this study aims to investigate the mechanical behavior of lattice structures to support further investigations based on Topology Optimization (TO). The study of the mechanical behavior of these structures allows an intelligent distribution of these structures along a given structure in order to absorb the amount of energy needed for the impact, presenting competitive manufacturing times and costs. In the course of this research, the manufacturing technique to be used will focus on the Powder Bed Fusion (PBF) process, more specifically in the EOS P396 equipment with the polymeric material polyamide 12 (PA12), that will shape the desired lattice structures, which are constituted by different topologies and volume fractions. The purpose of this development is focused on obtaining the experimental mechanical properties of certain types of cellular structures in order to compare them with the properties obtained from the simulations. Thus, strut-based (BCC) and Triply Periodic Minimal Surfaces (Schwarz-P and Neovius) lattice structures were defined based on different independent variables, such as, cell size, strut diameter/ surface thickness and shell thickness. The defined structures were evaluated by compression and impact mechanical tests. It was found that beside geometrical design, the relative densities of the unit cells could also significantly influence the impact energy absorption performance. KEYWORDS: Additive Manufacturing, Compression tests, Energy absorption, Impact tests, Lattice Structures, Lightweight, Selective Laser Sintering.
v RESUMO Tendo em conta a rápida evolução tecnológica e a crescente procura do sector industrial para satisfazer as mais diversas necessidades do mercado, as tecnologias de Fabrico Aditivo (FA) aparece como uma abordagem transformadora da produção industrial que permite a criação de peças e sistemas mais leves e fortes. A versatilidade deste tipo de tecnologia permite uma redução do tempo de produção e do consumo de energia, bem como a eliminação do desperdício de material na produção de um produto. É neste último ponto que as tecnologias de FA se destacam no que diz respeito às tecnologias de fabrico convencional. Nas tecnologias FA, é possível realizar a deposição de material de forma controlada, onde é realmente necessário, e ao mesmo tempo, garantir as propriedades mecânicas necessárias para satisfazer os requisitos do produto. Neste contexto, este estudo destina-se a investigar o comportamento mecânico de lattice structures para apoiar investigações posteriores que têm por base a Otimização Topológica (OT). O estudo do comportamento mecânico destas estruturas permite uma distribuição inteligente destas mesmas ao longo de uma determinada estrutura de forma a absorverem a quantidade de energia necessária ao impacto, apresentando tempos e custos de fabrico competitivos. No decurso desta investigação, a técnica de fabrico a ser utilizada centrou-se no processo de Powder Bed Fusion (PBF), mais especificamente no equipamento EOS P396 com o material polimérico poliamida 12 (PA12), que dará forma às lattice structures, constituídas por diferentes células unitárias e frações de volume. O objetivo deste desenvolvimento focouse na obtenção das propriedades mecânicas experimentais das estruturas celulares de maneira a compará-las com as propriedades obtidas a partir das simulações. Assim, as lattice structures baseadas em strut-based (BCC) e Triply Periodic Minimal Surface (TPMS) (Schwarz-P e Neovius) foram definidas com base em diferentes variáveis independentes, tais como, tamanho da célula unitária, diâmetro da viga/ espessura da superfície e espessura da casca. As estruturas definidas foram avaliadas mecanicamente através de testes de compressão e impacto. Verificou-se assim que, para além do desenho geométrico, as densidades relativas das células unitárias também podiam influenciar significativamente o desempenho de absorção de energia de impacto. PALAVRAS-CHAVE: Fabrico Aditivo, Ensaios de compressão, Energia absorvida, Ensaios de impacto, Estruturas de treliça, Peso reduzido, Sinterização Seletiva a Laser.
vi CONTENT DIREITOS DE AUTOR E CONDIÇÕES DE UTILIZAÇÃO DO TRABALHO POR TERCEIROS .................................................................................................................................... I ACKNOWLEDGEMENTS ........................................................................................................... II STATEMENT OF INTEGRITY.................................................................................................. III ABSTRACT .................................................................................................................................. IV RESUMO........................................................................................................................................ V CONTENT .................................................................................................................................... VI LIST OF FIGURES ...................................................................................................................... IX LIST OF TABLES ........................................................................................................................ XI LIST OF ABBREVIATIONS ..................................................................................................... XII 1. INTRODUCTION ...................................................................................................................... 1 CONTEXTUALIZATION ............................................................................................... 1 INTRODUCTION TO DONELAB ................................................................................... 2 OBJECTIVE ................................................................................................................. 2 ORGANIZATION OF THE RESEARCH ........................................................................... 2 2. LITERATURE REVIEW ........................................................................................................... 3 HISTORY OF ADDITIVE MANUFACTURING ............................................................... 3 INTRODUCTION TO ADDITIVE MANUFACTURING ..................................................... 4 Processes ........................................................................................................... 5 Materials ............................................................................................................ 6 Applications of Additive Manufacturing ........................................................ 7 Advantages vs drawbacks ................................................................................ 8 Main future issues ............................................................................................. 9 AM TECHNIQUES ...................................................................................................... 9 Vat photopolymerization (VAT) ..................................................................... 9 Powder Bed Fusion (PBF) ............................................................................. 10 Binder Jetting (BJ) .......................................................................................... 11 Material Jetting (MJ) ...................................................................................... 12 Sheet Lamination (SL) ................................................................................... 12 Material Extrusion (ME) ................................................................................ 13
xiii Material Extrusion ME Material Jetting MJ Melting Temperature Tm Molecular weight Mw Multi Jetting Fusion MJF Nano Particle Jetting NPJ Neovius N Neovius reference sample NR Neovius shell thickness sample NS Neovius surface thickness sample NT Polyamide PA Polycarbonate PC Polylactic Acid PLA Powder Bed Fusion PBF Schwarz-P P Schwarz-P reference sample PR Schwarz-P shell thickness sample PS Schwarz-P surface thickness sample PT Scanning Electron Microscopy SEM Selective Laser Sintering SLS Sheet Lamination SL Stereolithography SLA Stereolithography file format STL Topology Optimization TO Triply Periodic Minimalistic Surfaces TPMS Ultrasonic Additive Manufacturing UAM Ultraviolet UV United Kingdom UK United States dollar USD United States of America USA Vat Photopolymerization VAT Three-dimension 3D
Chapter 1. Introduction 1 1. INTRODUCTION CONTEXTUALIZATION Over the last years, technology has transformed every industry, and manufacturers are only beginning to embrace the latest innovations. After overcoming several industrial revolutions, today we are going through the fourth industrial revolution (Industry 4.0), with innovations that can sense the health of equipment, augmented reality, and self-learning and self-healing machines. It leads to the digitalization era: everything is digital. Since last decade, Additive Manufacturing (AM) technology has been improved rapidly to fulfil the needs of people and various industries. It is often bundled together with robotics, digitization and big data in the “Industry 4.0” vision of the factory of the future. An interesting fact about this technology, is that most of the general public is unaware that it has existed for several decades - the first commercial systems came on the market in the late 1980s. All its versatility, both in terms of processes and materials, allowed a rapid expansion in various industrial sectors, aiming in the near future to replace existing conventional manufacturing methods - standardization of technology. The ability of freedom to design fully functional products, as well as the ecological/environmental advantage are intrinsic features of AM. However, the undesirable effects that reside in the control aspects of the process consider it a technology of low productivity, poor quality and uncertainty of the mechanical properties of the final parts. Optimization is difficult due to limited modelling approaches and the physical phenomena associated, such as melting/ solidification and vaporization, heat and mass transfer, are complex. One of the main objectives of the industry is to maximize the performance of a given part, while minimizing its costs. One of these costs is related to the amount of material to be used to produce a part. Nowadays, the use of AM technologies has been more and more frequent due to its potential ability to produce any kind of shape, without any constraints. From here emerges a kind of bio-inspired configurations, based on repeating unit cells, composed by patterning webs or trusses that can, not only save material waste, but also, be self-supporting. These types of structures, commonly known as lattice structures (LS), can be automatically generated in a Computer Aid Design (CAD) systems. Even though they present high strength/low mass ratios by replacing solid material in parts, their prediction still presents several uncertainties, when it comes to shaping parts according to consumer requirements.
Chapter 1. Introduction 2 According to the potential of the LS, several experimental analyses of additive manufactured parts has been done to support the existing software tools to design and optimize cell structures, involving design considerations of each unit cell. INTRODUCTION TO DONELAB DONE Lab – Advanced Manufacturing of Product and Tools, is a laboratory created at the University of Minho in 2016. The laboratory emerged from a partnership between the University of Minho and Bosch Car Multimedia Portugal, aiming the research & innovation in the field of additive manufacturing, in order to give support to companies to enhance the innovation and time production of products. OBJECTIVE The outcome of this research paves the way for implementing additively manufactured cellular materials. It gives a solid foundation of an experimental analysis of additive manufactured lattice structures with diverse unit cell in compression and impact tests. For this purpose, different topological cellular structures with distinct cellular independent variables were produced from Polyamide 12 (PA 12) powder by implementing Selective Laser Sintering (SLS) technology. Thus, the aim of this investigation promotes the relationship between the specimen relative density value and energy absorption capacity. ORGANIZATION OF THE RESEARCH This dissertation is divided into six main chapters. Chapter 1 presents a brief contextualization of the dissertation theme, its relevance, and the description of its objective. Chapter 2 presents a brief description of the history of AM and, its main principles and technologies. It is also described, in more detail, the SLS process used in the fabrication of the samples. Also, basic lattice concepts are presented, including a succinct description of the different topologies. This introductory detailed section presents some general background, in order to allow an easier and better understanding of the other topics covered. Chapter 3 describes the methodology carried out for the design, shape definition and overall dimensions, material, and process parameters for the production of the cellular samples. The experimental procedure of compressive and impact tests, for the characterization of samples, is also described in this chapter. Chapter 4 present the analysis and data treatment of the obtained experimental results. In conclusion, Chapters 5 and 6 cover the conclusion marks and further research to improve AM technology, respectively.
Chapter 2. Literature review 3 2.LITERATURE REVIEW The present chapter describes some fundamental concepts in order to facilitate the understanding of the present dissertation. It starts by briefly reporting the history of the AM, presenting, in the following, the various processes attached to it. At another point, a more detailed presentation of the SLS technique is made. Finally, with a greater focus of interest, the section related to lattice structures appears, where the theoretical basis for the prediction of properties are described. HISTORY OF ADDITIVE MANUFACTURING Despite the little use and, consequently, lack of knowledge of AM, this technology has been around for nearly 40 years [1]. Its roots lie in new patterns of consumption and use of products resultant from the second industrial revolution. From here, comes the concept of rapid prototyping, opening doors to the AM technology. Despite their similarities, they present small differences in terms of price, complexity of the printing method, material choices and precision. That said, AM makes reference to any manufacturing technology that uses layer-by-layer deposition and Rapid Prototyping is an application used in the AM [2] [3]. A historical analysis reveals that the first attempt to implement the AM was from topography and photosculpture [4], [5]. The first one consisted of cutting the wax plates along the topographical contour lines firstly, and then, stacking and smoothing these plates in order to produce three-dimensional part. This part corresponds to the terrain indicated by the contour lines. The second one related to the “intersection of two laser beams of differing wavelength in the middle of a vat of resin, attempting to polymerize the material at the point of intersection”, that led to appearing of the first commercial SLS printer, in 1990 [5], [6]. During the first decade of 2000, AM technology was seen as a potential fast manufacturing method for very limited purposes as, for example, in the jewelry field, for small quantities of production and with small size parts. That is, it was seen as an auxiliary manufacture technique to the production lines. From 2010 onward, AM began to have its due value where some industries adopted AM technologies as their main method of manufacture. The first companies that adopted this kind of manufacturing system were the in-the ear hearing aids, in 2011. With more complexity applications, such as dental, biomedical and aerospace companies also began to embark in the same way. Simultaneously, metals AM processing technologies also had a significant interest and growth [6] [7].
Chapter 2. Literature review 4 Nowadays, the evolution of AM is due to the creation of new companies, with interest of companies already implemented in the market, with the creation of the most diversified 3D printers, as well as, with the development of new materials. This constant effort and dedication have enhanced AM to acquire an increasing importance in the most diverse areas from the automotive to the food industry. Considering the technological advances in recent years, the AM success is in constant growth at the industrial market level [3], [6]. INTRODUCTION TO ADDITIVE MANUFACTURING The way products are designed, manufactured and distributed to end users is changing by the potentially of AM technology. Additive Manufacturing is a general term, encompassing a wide variety of systems used to create three-dimensional physical parts and models, directly from digital data [8]. American Society for Testing and Materials (ASTM) defined this bottom-up process as “a process of joining materials to make parts from 3D model data, usually layer upon layer, as opposed to subtractive manufacturing and formative manufacturing methodologies” [9]. The term 3D printing is mostly used as a synonym for AM but there are also other, not so frequent, historical terms, such as, additive fabrication, additive processes, additive techniques, additive layer manufacturing, layer manufacturing, solid freeform fabrication, and freeform fabrication [5], [10], [11]. Succinctly, AM processes are based on the fabrication of parts, by creating successive cross-sectional layers, of an object. As showed in Figure 1, AM process begins with a threedimensional (3D) solid model, which is initially modeled or scanned as a Digital Computer Aided Design (CAD) file, and then sliced into thousands of layers by preparation software as Standard Tessellation Language (STL) file. Finally, each layer is created via the selective deposition of material and/or energy to fuse the raw material to produce a printed part [4], [10]. With the usage of customized material properties, it permits manufacturing intricate and complex shapes much more simply than conventional methods, providing the potential to reduce production costs, energy consumption, and, consequently, ecological footprint [12]. Parts can also be built from 3D imaging data generated by 3D scanning or medical imaging devices. Materials used in AM are broadly classified as liquid, powder, filament or sheets. Polymers were the primary type of materials used in additive manufacturing, but plaster, metals, silica sand, paper, ceramics and biological materials, are also available in AM [13] [14]. AM systems range from large industrial machines, suitable for shop floor and laboratory environments, to smaller desktop printers [12]. Nowadays, this technology counts with several different processes including vat polymerization, powder bed fusion, material extrusion and material jetting as the most popular ones [9], [15].
Chapter 2. Literature review 5 Although AM has been in use for decades, new advancements and applications are being developed every day [4], [16], [17]. Figure 1 – AM process flow [18]. Processes Due to the identical procedure presented by the different AM processes, it is wrong, but common, to assign the term AM to all the processes involved. Throughout the history of AM, the constant and successive development of new processes and materials has forced certain researchers to rethink how to classify them. In order to choose the process that best suits a given application, several classifications have been released [19]. The task was not easy because each process offers variations in dimensional accuracy, surface finish and post-processing requirements. Over the past few, the American Society for Testing and Materials (ASTM) committee ASTM F42 – Additive Manufacturing has been formed to come up with terminology and standards that help grow the industry and let different stakeholders talk to each other on the same terms. In 2010, it formulated a set of standards that classify the range of Additive Manufacturing processes into 7 categories such as Vat Photopolymerization, Powder Bed Fusion, Material Extrusion, Material Jetting, Binder Jetting, Direct Energy Deposition and Sheet Lamination. This classification is based on the type of material to be used, on the machine technology and on the expected functions [1].
Chapter 2. Literature review 6 Materials As stated in the previous point, the choice of the appropriate material is related to the type of process to use [20]. For a material to be reliable to any AM technology, it must include the ability to produce the raw material in a manner compatible with the specific AM process, adequate processing of the material through AM, the ability to be post-processed to improve geometry and properties, and manifestation of the performance characteristics required in service [14]. In general, a specific material class is associated with a certain technology and application. Initially, AM was implemented with the intention of producing plastic products, regardless of the process to be used [15]. Over intense years of research and development, AM has begun to embark on new paths, capable of producing complex parts using other materials. Actually, a wide range of materials that can be used in AM include a diversity of polymers, ceramics, metals, and composites can be used for AM [8]. Materials can be found in liquid, filament, powder and solid sheet states, depending on the process in question. A polymer is a large molecule made up of chains or rings of linked repeating subunits, which are called monomers. Polymers tend to have high molecular masses due to the join of many monomers. The versatility, adaptability and properties makes polymers the most used class of materials in AM [21]. Among the currently commercial materials, Table 1 shows that material extrusion processes use, in majority, amorphous polymers but also semi-crystalline, those of vat photopolymerization are limited to photosensitive thermosets, material jetting typically uses photosensitive thermoset polymers, powder bed fusion is mostly limited to semi-crystalline polymers, metal powder bed fusion uses metal alloys that are suitable in casting or welding, while binder jetting and some sheet lamination use practically any raw material as long as it can be converted into powder or foil and, finally, Directed energy deposition resources to metallic powder or wire feedstock [14]. Table 1 – Current commercial materials directly processed by AM [14]. Amorphou s Semicrystallin e Thermose t Material extrusio n Vat polymerizatio n Materia l jetting Powde r bed fusion Binde r jetting Sheet laminatio n Direct energy depositio n ABS X X PC X X PC/ABS Blend X X PLA X X Polyetherimide (PEI) X X Acrylics X X X Acrylates X X X Epoxies X X X PA (Nylon) 11 and 12 X X Polystryrene (PS) X X Polypropylene (PP) X X Polyester (“Flex”) X
Chapter 2. Literature review 7 Polyetheretherkeyton e (PEEK) X X X Thermoplastic polyurethane X X Chocolate X X Paper X Aluminium alloys X X X X Co-Cr alloys X X X Gold X Nickel alloys X X X Silver X Stainless steel X X X X Titanium, comercial purity X X X X Ti – 6Al – 4V X X X X Tool steel X X X Applications of Additive Manufacturing At the start of this new manufacturing ideology, AM began to be applied in the area of rapid prototyping and then tooling [20]. With the progressive development of innovation, AM has been able to make positive progress in the latter and thus, attract greater attention from the most diverse industrial sectors. The parts that were previously produced as prototypes are, nowadays, produced as final products. In the aerospace sector, in which it needs to produce highly complex aviation components from advanced materials, is one of the examples of its application [22], [23]. In this area, complex additive manufacturing processes must be developed to meet the industry’s stringent requirements and to ensure the robust performance of parts, comparing to traditional manufacturing methods [24], [25]. Another milestone in the AM was when NASA launched the first 3D printer in International Space Station to experiment printing parts in zero gravity [3]. In the automotive sector, although AM is limited to the production of end-use parts, in low volume, for luxury or racing vehicles, it is a source of cost savings when it comes to industrial production. Due to the fact that this sector is constantly changing, the development of a new product is critical. For this, the work in AM is fundamental because it reduces cycle times, and production and product costs, when a visual analysis or quality control is intended [26]. In the medical sector, the parallel development of biomaterials has provided the development and expansion of certain AM processes. Its application, with promising expansion, is now present in the customization of, for example, implants, prostheses and organ replacement [27]–[29]. With the current environmental concern to reduce CO2 emissions and consumption of natural resources, there are ample opportunities in the energy sector where AM can be crucial. In highlight is the rapid production of prototypes to reduce the cost and lead-time of research and the development of new products. Adding to this, the energy efficiency and power density can be explored by creating newer prototypes [30], [31]. In the architecture sector, the use of AM facilitates the construction of models, of complex ideas difficult to reproduce on paper [32].
Chapter 2. Literature review 8 Among other sectors where AM is an asset, it is an ideal technology in the repositioning of spare parts, craft and hobby items, educational uses, unique requirements and fashion accessories [33]. When it is intended to make a product for a particular application, not all AM processes are able to perform it. Therefore, depending on the application in question, the AM process that best meets the desired needs is chosen. Regardless of the sector in which AM technology is applied, its overview will always be seen from a planning, simulation and evolution perspective, until the day it is fully implemented in the industrial production lines. Advantages vs drawbacks With the usage of AM technology, development has become easier than ever before. Nowadays, any project can be manufactured using nothing but a 3D printer and the desired raw material [34]. This has paved the way for customized products as it allows the creation of fully customized 3D-designs by simply modifying the 3D model in the software and get them printed by a time and cost efficiency production. Instead of traditional manufacturing methodologies, such as, conventional injection molding or machining/subtractive technologies, the AM dramatically reduces or completely avoid the use of tools, reducing the speed and the cost of enduse parts productions. AM allows the fabrication of complex geometries, with high precision, efficient material usage, design flexibility, and also the production of customized products according to any requirement of the consumer. It may even generate new employment opportunities [8], [21], [32], [35]. When comparing to injection molding production, it is estimated that AM methods are most cost-effective for targeted fabrications runs ranging from 50 to 5000 units [36]. In comparison with machining technologies, although the waste associated with AM is low, a significant percentage of it is still recyclable [10]. The development of production processes, the AM technologies can be a potential to support environmental sustainability in the manufacturing field [37]. Without exception to existing technologies, AM also has certain disadvantages which have been counteracted by successive investigations. It presents higher costs for large production runs and in materials, size restrictions, poor surface finish and accuracy, and needs software improvement for standardization [4], [32], [38].
Chapter 2. Literature review 9 Main future issues The rise of AM is making a significant impact on how parts and products are designed and manufactured. It is also directed by the part geometry and application need. Despite its great development over the last few years, its implementation in industries is still not fully accepted. In the near future, AM's main goals will be to reduce machine, material and maintenance costs. So that, the change of conventional manufacture by AM is possible with the enlargement, development and identification of applications exclusively for its use [39]. To achieve these goals, AM technology and its applications require significant further research and development in terms of designs, materials, new processes and machines, process modeling, process control, bioadditive manufacturing, and energy and sustainability applications, as well as, the improvement of certain processing parameters of existing technologies [8], [15]. The advantages that AM claims to differentiate itself from traditional manufacturing need further research for it to become a more practical alternative, but the new research towards these developments is slow due to the interfaces of research laboratories and commercial machine manufacturers gaps between academia and industrial settings. AM TECHNIQUES Through extensive research over the past years, significant progress has been made in the development of new AM technologies. In the early 1990s, Kruth starts to categorize additive manufacturing techniques from liquid-based, powder-based and solid-based systems according to different material creation. And direct-3D and 2D-layers techniques according to different shape building [19]. Most recently, ASTM F42 committee has classified AM techniques into seven different categories. This section begins by briefly describing the different existing techniques, ending with a more thorough approach to the technology used in this research: SLS. Vat photopolymerization (VAT) Vat-photopolymerization consists in a process of taking a vat of photosensitive resin and then, curing that resin through selective exposure to, usually, UV light range. A laser or light source generates a UV beam that cures focused surface areas point-by-point or layer-by-layer. In either case, it initiates with the polymerization to create the desired part, in a layer-by-layer fashion on a top-down construction platform (Figure 2). The materials are photocurable epoxy or acrylate resins. Ceramics or metals are not suitable. High accuracy, flexibility for the production of small and large parts and smooth surface finish are some of its advantages [21], [40], [41].
Chapter 2. Literature review 16 Technology SLS is a powder-based thermal 3D printing manufacturing process that uses thin layers in the order of one-tenth of a millimeter thick [13]. It uses a laser to sinter or melt layers of powder to grow the part. It starts with the integration of a 3D CAD file to create 2D slices. The entire build area is heated up too close to the melting temperature of the material, and then, there’s a laser that actually melts thermally the powder where the 3D CAD file want to the solid part be. This warmup is achieved due to the presence of infrared heaters, above the building platform and above the feed tanks, to minimize and prevent the deformation of the part due to non-uniform thermal expansion. The sintering occurs due to physico-chemical reaction [13], [60]. The atmosphere of the chamber is composed by an inert gas, typically nitrogen, in order to minimize oxidation and degradation of the powdered material. The build platform drops down as each layer is grown and the new layer of powder is added on top. This procedure is performed repeatedly until the solid part is obtained. The end of the process is a cooling period, proportional to the sintered volume. This prevent powder degradation when exposed to the atmosphere (oxygen), and possible warping due to uneven thermal contraction [61]. Parts and involving non-sintered powder can only be removed after reaching glass transition temperature or below 45 – 60 ºC. Since the raw material is polymeric, the non-sintered material is easily brushed away and parts can be excavated like an archeology dig. Optionally, parts can go through a custom post-processing phase, such as painting, sanding or surface finishing, depending on the customer's requirements or needs, or the application. There are varied options after that part comes out of the machine [62]. The process explained above is summarized in Figure 10. Figure 10 - SLS process sequence [63].
Chapter 2. Literature review 17 Process parameters Parts' accuracy in SLS can arise from a strongly independent parameters that can be controlled and varied for a particular application. Thus, they can be classified into (1) powderrelated parameters (particle shape, size and distribution, powder bed density, layer thickness, material properties); (2) laser-related parameters (laser power, spot size, pulse duration, pulse frequency); (3) temperature-related parameters (powder bed temperature, powder feeder temperature, temperature uniformity); (4) scan-related parameters (scan speed, scan spacing, and scan pattern); and (5) part parameters (part orientation, part position) [13], [64]. (i) Powder parameters Powder parameters can be divided into several factors that are interrelated. The different properties of SLS powders can be divided into intrinsic (e.g., thermal, optical and rheology) and extrinsic ones (particle and powder). Intrinsic properties are typically determined from the molecular structure of the polymer itself and cannot be influenced easily, whereas production of powder controls extrinsic properties [65]. These characteristics play a significant role in powder performance that compromises the performance of the final product [66]. Since the powder is distributed by roller or blade systems, the particles should have spherical form to induce a free flowing behavior and the powdered raw material formed by these particles must have a certain particle size distribution. Thus, the potato shaped particle and the distribution from 20 µm to 80 µm are the most commonly used for commercial PA 12 powder [65], [67]. The irregular and random packing of particles forms the porosity. It tends to be larger on the surface of the layer, than inside the part, and increases with the decrease of the laser energy due to the incomplete fusion of the particles. Regarding the molecular weight, 𝑀𝑤, of the powder, there is a suitable optimum range. Polymers with high 𝑀𝑤 allow to obtain functionally strong parts. However, they can lead to difficulty in spread the powder because of high viscosities, but can reduce shrinkage and, consequently, improving dimensional accuracy [68]. Coupled with the 𝑀𝑤 is the density of the powder. Powder densities generally range from 50% to 60%, for most commercially available powders. Generally, the higher the powder packing density, the better the mechanical properties of the part [69]. The layer thickness is another important parameter. Its decrease results in more time part processing. The increase in layer thickness beyond limits results in an increase of the stair
Chapter 2. Literature review 18 stepping problem, poor sintering, rougher surfaces on parts and the part cannot be produced properly. To ensure that the powder fusion occurs at direct contact of the laser on the particle, the layer thickness is recommended to be at least two times the average size of the particle [69], [70]. (ii) Laser/ temperature parameters Similar to laser cutting and laser welding, SLS uses a linearly traversing laser beam to selectively fuse powder particles. All the laser irradiation incident with the powder surface is assumed to be absorbed or reflected according to the optical properties of the powder. So, there must be a balance between the laser power and the bed temperature [71]. High laser power and bed temperature produce dense parts with a partial growth, poor recycling and difficulty in cleaning. For low laser power and bed temperature, the dimensional accuracy of the produced parts is improved but it results in lower density parts with a great tendency for layer delamination. High laser power combined with low bed temperature have a tendency for non-uniform shrinkage and accumulation of residual stresses [13]. Increasing the laser power incident in the powder can fabricate higher strength parts. This increase is made until the thermal degradation of the powder [69]. Relatively to bed temperature, it is increased as high as possible but, 3oC – 4oC below the melting temperature of the powder for semi-crystalline polymers. This increase is also good for reducing consumption of energy due to the need of lower laser power, but it can result in an unwanted binding [13], [72]. The desirable re-crystallization of the powder occurs at low bed temperatures, but at very low bed temperatures, the mechanical properties are poor due to non-uniform fusion of powder particles and increased porosity [73]. In order to find the suitable operating window of the LS process, the distance between the melting and crystallization peaks of the Differential Scanning Calorimetry (DSC) peaks can be used to indicate it. The distance between the melt and recrystallization peaks is the processing window for the bed where the corresponding area promotes good control of sintering when the powder absorbs energy from the laser and allows effective part consolidation by avoiding premature crystallization on cooling [74]. (iii) Scan parameter Scan spacing or hatch spacing is the distance between parallel laser scans. Scan spacing has a significant effect on all mechanical properties, such as, ultimate tensile strength, elongation, yield strength, and Young’s modulus. That is, for shorter distances are required high laser energy, resulting in over sintering. However, too large scan distance results in incomplete sintered crosssection. As stated by S. Singh et al., scan spacing is proportional to the energy density used [69].
Chapter 2. Literature review 19 Scan speed is a process parameter that controls the part build time and is directly related with the laser power. A higher scanning speed decreases the degree of melting of the particles as the particles do not have enough time to melt. Lower scanning speed can degrade the particles. At these scan speeds, laser power has limited effect on sinter width. If power applied is less, no binding reaction occurs, and melting could not take place properly. Having said this, there must be a balance between the scanning speed and laser power for a correct part production [75]. (iv) Part parameters The orientation of the part is an important parameter that describes the rotation of the part, in the build space, around the axes of the machine’s coordinate system [76]. It is an important parameter due to its influence not only on the resulting surface quality but also on stair stepping effect. Also, the accuracy of part’s details and the building time and costs, due to the building height, are strongly influenced by the build orientation. Research conducted by Ajoku et al. [77] found that parts built parallel to the layer orientation (0°) had better tensile properties than parts built perpendicular to layer orientation (90°). Another research made by Caulfield et al. [78] found similar results where the perpendicular orientation resulted in a better geometric accuracy but in a lower density, yield strength, tensile modulus, and fracture strength than the parallel oriented parts (Figure 11). Figure 11 - Building direction of SLS parts [79]. Materials SLS technology starts with the usage of polymers due to their ability to be easily processed by melting, and their good mechanical properties. PC was initially used as the starting materials for both experimentation and modeling in SLS [64]. With the progressive development of this technology, the approach applied to this process with polymer powders was, posteriorly, extended to metal-polymer powders, where the polymer acts as a binder, metal and ceramics [80].
Chapter 2. Literature review 20 Within the existing types of polymers, SLS technology mostly uses thermoplastics. Depending on the use of amorphous or semi-crystalline thermoplastics, these determine the SLS manufacturing parameters and limit the purpose of the parts produced. Amorphous polymers, like PC powders, are able to produce parts with very good dimensional accuracy, feature resolution and surface finish (depending on the grain size). However, they are only partially consolidated. As a consequence, these parts are only useful for applications that do not require part strength and durability. Semi-crystalline polymers, like nylons (e.g. PA12), on the contrary, can be sintered to fully dense parts with mechanical properties that approximate those of injection molded parts. The good mechanical properties of these nylon-based parts make them particularly suited for high strength functional prototypes [81]. According to the specific properties of PA12, its use, as well as the mixtures it provides, is quite attractive. It exhibits good resistance to solvents, high strength and wear resistance. PA12 based powders, including PA2200 supplied by EOS GmbH, appears as the most used materials in laser sintering process for rapid manufacturing of functional parts [62]. Recycling of material An average of 10% – 20% of the powdered material in the LS building chamber is sintered and could be reused. However, the powder properties deteriorate along the builds, which ultimately affects the quality of produced parts. These differences are due to the process conditions, such as, temperature and time, the LS machine design, and properties of the powder used for parts fabrication [62]. A standard technique of material recycling is to mix the recycled powder collected from previous builds with new powder and use it in the next build. The part quality is dependent on the input material properties and powder management. The older the material is, the newer material is required and vice versa. However, it is impossible to know the recycled powder quality, and therefore, exactly how much new material is needed to refresh it. At some point, the old material should be fully discarded in order to avoid dramatic deterioration of the part quality and waste of new material [62]. When you want to recycle material, it is necessary to take into account (i) the percentage of virgin and recycled material to be used and (ii) the number of times the recycled material was used. In order to promote a good balance between the cost of the raw material and the properties of the final part, the EOS’s machines recommends a mixture in a range of 30% - 50% virgin PA2200 material with 50%-70% of powder from the part bed [82]. In this research, was used a mixture ratio of 30% of virgin with 70% of processed material in the manufacture of the samples.
Chapter 2. Literature review 21 Advantages vs Disadvantages Most importantly, SLS allows users to process a wide range of thermoplastic materials including engineering and high-performance plastics with specific mechanical properties and lowered anisotropy. Because of this advantage, laser sintered parts are durable enough to be used in applications where they are subjected to mechanical loads. Another positive side of SLS, it can fabricate lightweight parts, due to porosity, which may be employed in applications that require large surface areas, for example, scaffolds for cell growth in tissue engineering. SLS presents a wide range of materials that can be reused. This leads to a reduction in emissions due to the need to produce less raw materials [17], [82], [83]. On the other hand, the SLS parts present rough surfaces and poor reusability of nonsintered powder. In the interface between solidifying layers and ready-built portions of the manufactured part, both thermal gradients and densification due to sintering induce residual stresses. The relaxation of these stresses may result in warpage or breakage influenced by powder properties and processing parameters. Its dimensional accuracy is limited by the size of particles of the material and by after melting, attachment of non-melted particles or waviness and roughness of struts. Also, the oxidation needs to be avoided by executing the process in an inert gas atmosphere and for the process to occur at constant temperature, near the melting point [17], [74], [83]. Applications In general, SLS technology started with the creation of visual prototypes, as a form of validation. However, the advance and development of the technology opened the range to different possible applications. Nowadays, the parts produced by SLS technology are not mere prototypes, but final parts. That said, it is possible to find SLS technology in different applications, such as medicine, aerospace, heat exchangers, lightweight structures and others, like, micro-tooling [10], [34], [84]. LATTICE STRUCTURES (LS) As stated in section 1.1, AM techniques offer great possibilities to develop parts with high complexity and customizability, such as, Cellular Structures (CS) which are ubiquitous in biological systems, structural engineering and materials science (Figure 12). Their concept, including foams, honeycombs, lattices, and similar constructions, comes from keeping material
Chapter 2. Literature review 22 only in the vital regions of a part to attain a lightweight structure, while maintaining the high specific mechanical properties, such as, strength and energy absorption [85], [86]. Figure 12 - The figures on the left are photos of cellular structures from nature, while those on the right are configurations of the corresponding artificial cellular structures with their unit cells. a) Cork, b) pollen particles of club moss, c) rhombic dodecahedron cells, d) tetrakaidecahedron cells, e) Luffa, f) glass sponge, g) cells with octahedron trusses, h) cells with Kagome trusses, i) “plumber’s nightmare” structure of amphiphilic membranes separating oil and water, j) cross section through a sea urchin skeletal plate, k) cells with P-surface, and l) cells with D-surface [87]. The first traditional methods to manufacture LS appear in the form of weaving, braising and casting [88], [89]. The production of Lattice Structures (LS) is difficult, tedious and time consuming, if not impossible, to produce using conventional manufacturing processes. Nowadays, LS have become more prominent recently, which are capable to reduce (1) the amount of material utilized in the manufacturing process, (2) the amount of time taken to produce an object, (3) the amount of energy utilized in the manufacturing process and (4) optimize the strength of the produced object while minimizing the weight [90]–[92]. When comprising a single material, LS are easily recycled [90]. They fill a fragment in manufacturing satisfying the requirements of energy absorption, acoustic and vibrational damping, high strength-to-weight ratios and thermal management [94], [95]. With the advance in micro and nanoscales manufacturing, the use of LS has been increasing, which corresponds directly to an increase in the use of AM technologies [93]. LS fabrication is limited to the restrictions of AM processes due to the dependence on AM methods, such as, speed, build space and resolution [92].
Chapter 2. Literature review 23 The development of new LS solutions requires a review of the existing published research and innovation, as well as, a summary of the latest trends in structure research, which makes possible the identification of potential future research areas [96]. The large amount of potential LS is a great advantage for any given purpose to be utilized in innovative and unique designs, exploiting the innate natures and benefits of the LS [93], [97]. Brief unit cell description The structure of a crystalline solid is best described by considering its simplest repeating unit, which is referred to as unit cell. It is well known as primitive cell [98]. The unit cell consists of lattice points that represent the locations of atoms or ions under the action of suitable crystal translation operators. The entire structure then consists of this unit cell repeating in three dimensions, as illustrated in Figure 13 [99]. Figure 13 – Representation of a unit cell and it lattice points repeating in all directions. Analogously, the structure of solids can be described as if they were 3D of a piece of wallpaper, specifying the size, shape, and contents of the simplest repeating unit in the design. Wallpaper has a regular repeating design that extends from one edge to the other. Crystals have a similar repeating design, but in this case, the design extends in three dimensions from one edge of the solid to the other. A description of a 3D crystal can be made by specifying the size, shape, and contents of the simplest repeating unit and the way these repeating units stack to form the crystal. In short, the unit cell is the simplest repeating unit in the crystal which opposite faces are parallel, and the edge of the unit cell connects equivalent points.
Chapter 2. Literature review 24 Design of lattice structures For the fabrication of each part by AM, the LS can be created and stimulated, manually or mathematically, by various CAD software. To create LS, there are available commercial 3D software tools that aid in the design, such as Autodesk Within Medica (Autodesk, Inc., USA), Materialise Magics (Materialise NV), nTopology Element (nTopology, Inc., USA) and Simpleware CAD (Simpleware, Exeter, UK). But the merging of LS with the objects, the availability of a small selection of unit cell types, the lack of Finite Element Analysis (FEA) integration and the limited optimization capabilities are some of the issues of these softwares. Finally, a STL file format of a particular 3D CAD model is achieved containing only the geometry surface [100]. The other way to produce LS is by using lattice generator which is a free open-source program, that can automatically generate various lattice geometries in STL file format [101]. (i) Unit cell design The unit cell plays a key role in characterization of the whole LS. It can be drawn from two different methods: primitive based method and implicit surface-based method. The primitive based method relies on Boolean operations of simple geometric primitives, in which, the unit cell consists of some geometric primitives. Figure 14 shows the example of two primitive based topologies (Figure 14 -- a and b) and some strut-based LS (Figure 14 – c). Figure 14 - Schematics of the primitive based method: (a) Boolean subtraction of the cube and a sphere, (b) Body Centered Cubic (BCC) strut-based LS and (c) others strut-based LS [102], [103] (c)
Chapter 2. Literature review 25 The implicit surface-based method uses mathematical equations to represent the surface of a unit cell in 3D space. These equations form the well-known TPMS which overall mechanical properties are significantly influenced by the porosity of the unit cell (Figure 15). In contrast to the primitive based method, this porosity can be parametrically controlled by specifying different terms in the equations [104]. Figure 15 - TPMS unit cell topologies [105]. (ii) Pattern strategies According to the configurations of the LS, each configuration has its own characteristics, being therefore more prone to a certain application. LS result from the patterning of unit cells in a 3D space. Pattern design can create LS from an array of unit cells using different methods, such as: - Direct patterning, also called uniform patterning or periodic LS, copies the unit cell along the x-, y- and z-axis creating parallelepiped shaped three-dimensional arrays., in which the unit cells are translationally repeated Figure 16 [106]–[108].
Chapter 2. Literature review 32 Figure 24 - Force-Deflection curves: (a) Typical curve for tough polymer, (b) Curve for a fiber reinforced material [131]. (i) Maxwell’s criterion Strut-based topologies can be characterized by their Maxwell number, M, from the Equation 3, which is dependent on the number of struts, s, and nodes, n. 𝑀 = 𝑠−3𝑛+6 (3) If M < 0, there are too few struts to equilibrate external forces without equilibrating moments induced at the nodes, causing bending stresses to develop in struts and leading to bending-dominated behavior. If M 0, external loads are equilibrated by axial tension and compression in struts meaning that no bending occurs at nodes, making these structures stretchdominated [130]. Due to these phenomena, the stretch-dominated architectures are more stiff and strong (higher modulus and yield strength) compared to the bending-dominated architecture with the same relative density [129]. (ii) The Gibson–Ashby model The most significant theoretical work regarding the deformation and mechanical properties of cellular solids is that of semi-empirical formulae of Gibson and Ashby, treating foams as arrays of connected beams and provided a series of equations relating their mechanical properties to their relative density, such as Young’s modulus, plateau strength, and densification strain. For cellular solids, made from materials that have a plastic yield point, Gibson and Ashby
Chapter 2. Literature review 33 introduced the Equations 4 a - c, where the relevant physical properties are given in Table 2 [133], [134]: 𝐸𝑙𝑎𝑡𝑡. 𝐸𝑠𝑜𝑙. = 𝐶1∙(𝜌𝑙𝑎𝑡𝑡. 𝜌𝑠𝑜𝑙. )𝑛 (4a) 𝜎𝑝𝑙. 𝑙𝑎𝑡𝑡. 𝜎𝑦 𝑠𝑜𝑙. = 𝐶5∙(𝜌𝑙𝑎𝑡𝑡. 𝜌𝑠𝑜𝑙. )𝑚 (4b) 𝜀𝐷= 1−𝛼(𝜌𝑙𝑎𝑡𝑡. 𝜌𝑠𝑜𝑙. ) (4c) From the equations described above, the prefactors C1, C5 and play a significant role in determining the mechanical properties and deformation behavior of LS. For the prefactors C1 and C5, which include all of the geometric constants of proportionality, Gibson, Ashby et al. provide a range of values from 0.1 -- 4.0 and 0.1 -- 1.0, respectively, while n and m are about 2 and 1,5, respectively, when deformation occurs by bending of the cellular struts or walls. For the value of , it varies between 1.4 -- 2.0. [133]. Table 2 - Physical and mechanical properties for the description of lattices under compression [134]. Notation Physical or mechanical property 𝝆𝒍𝒂𝒕𝒕. 𝝆𝒔𝒐𝒍. 𝝆∗ Density of the lattice structure Density of the material constituting the lattice struts or walls Relative density, or volume fraction, of the lattice; equal to 𝜌𝑙𝑎𝑡𝑡./𝜌𝑠𝑜𝑙. 𝜺𝑫 Densification strain of the lattice 𝑬𝒍𝒂𝒕𝒕. 𝑬𝒔𝒐𝒍. 𝑬∗ Elastic modulus of the lattice structure Elastic modulus of the material constituting the lattice struts or walls Relative elastic modulus of the lattice; equal to 𝐸𝑙𝑎𝑡𝑡./𝐸𝑠𝑜𝑙. 𝝈𝒍𝒂𝒕𝒕. 𝝈𝒑𝒍.𝒍𝒂𝒕𝒕. 𝝈𝒚 𝒔𝒐𝒍. 𝝈∗ Effective stress of the lattice structure Plastic collapse strength, or plateau strength, of the lattice Yield strength of the material constituting the lattice struts or walls Relative collapse strength of the lattice; equal to 𝜎𝑝𝑙.𝑙𝑎𝑡𝑡../𝜎𝑦 𝑠𝑜𝑙. To use the equations above for effective LS design, either by manually selecting an appropriate volume fraction or through implementation of a combined lattice TO approach, one
Chapter 2. Literature review 34 must know the Gibson-Ashby prefactors and exponents for the chosen lattice cell type. They may be determined from experimental compressive tests, by manufacturing and testing lattice specimens of varying their relative densities, and then, applying appropriate fitting to the mechanical data [135]–[137], by finite element calculations and by the construction of analytical models based on structural failure mechanisms [138], [139]. (iii) Finite Element Analysis, FEA FEA is an alternative approach delivering insight in the mechanical characteristics. The loading conditions are simulated in CAE software and the computer numerically calculates an estimation of the effective mechanical response using the Finite Element Method (FEM). This strategy completely relies on computational procedures and does not require the fabrication of physical parts. This makes the measurement of the mechanical properties a faster and low-cost than experimental tests. Engineers often adopt FEA in conceptual stages to avoid fabricating numerous prototypes. Inherently, the method is only an estimation and produces errors, constituting a drawback. Powerful computers and advanced CAE systems are required to minimize errors and obtain accurate solutions [92], [140]. For this report, mechanical compression and impact tests to know the properties of each structure were considered to facilitate the prediction of the theoretical behavior. According to the technical datasheet of the material in question, the simulations were performed. If, in a first attempt, the simulation corresponds to the experimental tests, it is excellent. Otherwise, it is necessary to understand the mechanical tests of the structure in question and make certain adjustments until reliable simulations are obtained. Once this similarity, between the real and the virtual, for a given parameter has been achieved, it is varied twice more in order to improve and extend the software capabilities, for future applications of these structures on parts with preestablished requirements. This way, it is possible to optimize the topology of LS. The smaller the difference between the simulations and the experimental tests, the more time is gained when you want to reach the final product, and the less money is spent on prototype production. Advantages vs Disadvantages LS are an attractive option for many design applications, particularly lightweight applications, due to the high specific strength and stiffness provided by their porous structure. The deformation behavior of cellular structures also means they are useful for energy absorption applications [90]. On the other hand, complex LS with overhang areas needs support structures to ensure an accurate building process [141].
Chapter 2. Literature review 35 Applications A wide variety of industries exploit the benefits of LS. This type of structures is widely employed in the medical industry, where they ca be useful by replacing tissues and bones. LS drastically decreased invasiveness and recovery time [86], [108]. Another application for LS is in the automotive industry, due to the weight reduction and increased ease of recycling of automotive parts [142]. In aerospace, LS aim to increase the performance-to-weight ratio, in order to build efficient vehicles with strong and lightweight parts [143]. LS can also be employed in protective applications due to the energy-absorption properties. Energy-adsorption is based in the ability of distributing an impact shock across the object [144]. In addition to presents applications fields, LS can also be applied in architecture industry.
Chapter 3. Methodology 36 3.METHODOLOGY Maintaining the process conditions of SLS technology, the objective of this research is to investigate the effect of changing both the architecture and as-built morphological properties of 3 different topologies types of LS on their mechanical behavior. This section presents the description of the experimental part of this report, involving the mechanical response of 3D regular cellular structures, with different topologies, subjected to uniaxial compressive and impact tests. DESIGN OF LATTICE-BASED SPECIMENS In the current study, strut based and TPMS cells are used to create architecture cellular materials. The CAD software used for the 3D modeling of the samples was Siemens NX CAD. Therefore, one-unit cell of the type of manually generated structures (strut-based) and two of the type of mathematically generated structures (TPMS) were chosen. Within the first type, the Body Centered Cubic cell (BCC) was chosen as the driving cell for this new way of producing functional and lightweight parts and its simplicity of design (Figure 25 - a). Within the second, the Gyroid unit cell was initially chosen due to its interesting mechanical performance, when applied to end use parts. This unit cell was eventually changed due to its complex and ingenious three-dimensional modeling in the CAD software during linear patterning in order to obtain the overall sample shape. That is, the unions of the surfaces were not smooth according to the equation which constitutes the unit cell. Instead of this, Schwarz-P (P) and Neovius (N) unit cells were selected, classified as open cells (Figure 25 – b, c). The choice of three cellular units has allowed broader results to be obtained as a means of comparing the mechanical performance of each structure. Figure 25 –(a) BCC, (b) Schwarz-P and (c) Neovius unit cells modelled by Siemens NX CAD. (a) (b) (c)
Chapter 3. Methodology 37 Overall dimensions It is known in advance that, depending on the type of mechanical test to be performed, a certain shape and dimensions of the test sample are required. As previously mentioned, for this study, mechanical compression and impact tests were performed. That said, the forms adopted for the compression and impact tests were quadrangular (parallelepiped) and circular (cylinder) primers, respectively. According to a study carried out, by several researchers, and related to the mechanical properties of LS, a minimum number of 2 cellular units present in each x, y and z axis is sufficient to obtain reliable results in the compression tests [145]. Thus, the adopted overall dimensions were 40 x 40 x 80 mm according to the test norm ASTM D 695 - 02. For the impact tests, the overall dimensions used in the production of the flat discs were 60 mm in diameter and 20 mm in height. The diameter of the test samples was pre-established according to ISO 6603-1-2000, while the height value was defined considering the available height space of the testing machine (Figure 26). Figure 26 -Overall dimensions of compressive test samples (left image) and impact test samples (right image). In an intuitive way, the dimensional accuracy of SLS specimens is expressed by error 𝑆1. For each sample, three measurements were made for each axial x, y and z axis. Thus, the dimensional accuracy of the SLS in each axis can be defined from the Equation 5, 𝑆1= [𝐴1−𝐴0 𝐴0]×100% (5) 20 mm 60 mm z y x z y x 80 mm
Chapter 3. Methodology 38 where 𝐴0 is the design size given by the computer and 𝐴1 is the real size measured by a vernier caliper. If the 𝑆1 error value is positive, it means that the polymeric powder expands and if it is negative, the powder contracts [146]. Variable parameters of unit cells As described in section 2.4.1, LS are composed of several unit cells, with specific parameters that determine the mechanical performance of the part. From the possible parameters include cell size, shell and surface/strut thicknesses for compression tests, and shell and surface/strut thicknesses for impact tests were selected in this study (Figure 27). It should be noted that the strut diameter of the strut-based unit cell and the surface thickness of the TPMS unit cells are both the same parameter. In order to simplify the presentation and understanding of the results, the term surface thickness was used for both cases. Figure 27 – Variable paramters of the research. The original structures topologies modelled by Siemens NX CAD have different massinertia properties. In order to understand the behavior of each parameter on the produced samples, Equation 6 represents the way to determine the value of a relative density of different cell topologies based on measured structure dimensions and defined densities: 𝜌𝑟=𝜌𝑣 𝜌𝑚 ; 𝜌𝑣=𝑚 𝑉 (6) where 𝜌𝑟 – relative density of the cellular structure, 𝜌𝑣 – density of the structure, 𝜌𝑚 – material density, 𝑚 – produced model mass, 𝑉 – produced model volume.
Chapter 3. Methodology 39 Due to the large number of samples to be studied, the list below represents the nomenclature assigned, where the numbers 1 and 2 represent the variation of the parameter in question: BCC (B) Schwarz – P (P) Neovius (N) BR - B Reference PR - Reference NR - Reference BT1 - B Surface Thickness 1 PT1 - Surface Thickness 1 NT1 - Surface Thickness 1 BT2 - B Surface Thickness 2 PT2 - Surface Thickness 2 NT2 - Surface Thickness 2 BC1 - Cell size 1 PC1 - Cell size 1 NC1- Cell size 1 BC2 - Cell size 2 PC2 - Cell size 2 NC2 - Cell size 2 BS1 - Shell thickness 1 PS1 - Shell thickness 1 NS1 - Shell thickness 1 BS2 - Shell thickness 2 PS2 - Shell thickness 2 NS2 - Shell thickness 2 To make possible the understanding of the mechanical behavior of cellular structures by varying each parameter of the respective unit cell topology, the relative density must be maintained. So that, Appendix 1 shows the relative densities of the overall LS used in this research (17% > 𝜌∗>23% for compressive tests and 21%> 𝜌∗>39% for impact tests). Here, it is necessary to add a fundamental point regarding the unit cell size parameter. In order to maintain the relative density, when the cell size is varied, the walls thickness of the cells must be varied, which in no way interferes with the objective in study. From here, the base values showed in each parameter tables dictate the reference sample, R. (i) Surface/diameter thickness, T In the three different unit cells the surface thickness has been varied 3 times. That said, according to the Table 3 it is possible to observe, in more detail, how this parameter varies. Table 3 -Variation of surface thickness parameter (T). Surface thickness [mm] BT1 BR BT2 1,70 2,00 2,30 PT1 PR PT2 0,57 0,76 0,98 NT1 0,38
Chapter 3. Methodology 40 NR NT2 0,51 0,65 (ii) Cell size, C In order to understand the influence of the unit cell size, three sizes of each unit cell topology were chosen that best fit the defined overall dimensions of the structure. Table 4 shows that variation. The study of this parameter was only made in the compression tests. That is, since two is the minimum number of unit cells present in each of the three-dimensional Cartesian axes to obtain consistent results [145], the cell size did not enter in the impact tests due to the fact that the maximum sample height specified by the test machine used is 20 mm. However, since the size of the reference cell is at least 10 mm high, only two cells on the z-axis can be manufactured. Table 4 - Variation of unit cell size parameter (C). BCC Schwarz-P Neovius Cell size [mm] 10 x 10 x 10 13,33 x 13,33 x 13,33 20 x 20 x 20 (iii) Shell thickness, S With regard to shell thickness, the overall dimensional integrity of the samples was maintained, that is, the total height of 80 mm was maintained. As showed in Table 5, the shell thickness was changed between 0, 1, 2 for compression tests and 1, 2 and 3 for impact tests. Table 5 - Variation of the shell thickness parameter (S). BCC Schwarz-P Neovius Compression tests Impact tests Shell thickness [mm] 0 1 2 1 2 3 EXPERIMENTAL TESTS Typically, any scientific study concerning material characterization requires testing at least three test samples of the same design configuration and dimensions. The same was done in the present experimental work in order to obtain reliable results, averages and standard deviations. Considering all the parameters mentioned in the previous section, the number of times each one
Chapter 3. Methodology 41 of them varies and their respective clones, a total of 108 tests were performed: 63 compression tests and 45 impact tests. Each sample has been duly identified with the nomenclature referred to in section 3.1.2 in order to facilitate its recognition after extraction of the parts after production and subsequently in the respective mechanical tests. Material and technology PA12 powders are the most used materials in the SLS process. The PA12 molecule structure, constituted by carbon atoms and amide group, provide strong bonds, mainly the hydrogen bonding, that determine mechanical and thermal properties of the molecule [147], [148]. It is a semi-crystalline polymer and has a highly heterogeneous microstructure due to containing both amorphous and crystalline phases. The mechanical properties of semi-crystalline polymers are a function of the amount and morphology of the crystalline regions. The crystalline region is responsible for the strength, whereas the amorphous region provides ductility by allowing the polymer to yield without breaking [149]. According to some studies, the mechanical properties of PA 2200 manufactured samples well match with the datasheet data. In [150], the tensile elastic modulus of PA 2200 was obtained as 1,35 ± 0.04 GPa and the yield strength as 23,3 ± 0.5 MPa; while compressive elastic modulus and yield strength as 1,14 ± 0.03 GPa and 48,1 ± 0.9 MPa, respectively. In [134], the tensile elastic modulus obtained was 1,80 ± 0,05 GPa and the yield strength was 29,1 ± 0,8 MPa; the results for the compressive behavior using cubes of size 20 mm3 were compressive elastic modulus as 1,59 ± 0,02 GPa and respective yield strength as 44,5 ± 0,3 MPa. Appropriately modified for its implementation in the AM, the raw material that constituted the research samples was PA 2200 composed by 70% of recycled material and 30% of virgin material. In the Table 6 it is possible to check its traction properties at a speed of 10 mm/min with a 50 kN load cell, at room temperature. Further details about the PA 2200 can be found in the technical sheet provided by the supplier (Appendix 2). Table 6 - Mechanical properties of PA 2200 in tension tests (70% recycled with 30% virgin material) [151]. Property [Unit] E [MPa] σYield [MPa] σBreak (MPa) εYield [%] εBreak [%] Part at 0º (70% - 30%) 1531,65 ± 20,77 44,68 ± 0,71 43,12 ± 0,65 11,17 ± 0,11 17,53 ± 0,85 Note: E – Young’s Modulus σYield – Yield stress σBreak – Break stress εYield – Yield strain εBreak - -Break strain
Chapter 4. Results and discussion 48 cells in contact with the shell and the shell is higher in the NR samples (shell thickness of 1 mm), which makes the discrepancy larger. Figure 30 - Shell thickness of Neovius samples: a) without shell (NS1), b) 1 mm (NR) and c) 2 mm of shell thickness (NS2). In general, the comparison between each cell topology is more precise when it comes to the independent variable C, followed by S and T. However, the N cellular structures are the ones that present the greatest discrepancies when compared to the modelled structures. Next, are P and, finally, B. In order to minimize these discrepancies, it is necessary to take into account the minimum size of the structural cells, essentially in the case of TPMS cells of greater complexity, in order to facilitate the extraction of non-sintered powder. This is because, at the end of each mechanical test, by shaking the sample or even the simple fact of put it on the table, it was possible to observe the non-sintered powder coming out of its interior. During these tests it was also possible to verify the presence of PA2200 powder on the lower Teflon sheet. This happened in greater abundance in N samples. Adding to this, possible overheating may have occurred during the manufacture of the samples, inducing the sintering of the neighbor powder. From the discrepancies described above, it is possible to conclude that the non-sintered powder, present in the samples, did not completely affect the respective mechanical performances of the samples with "defective" relative densities (Figure 31). The mechanical tests were carried out in the same way. (a) (b) (c)
Chapter 4. Results and discussion 49 Figure 31 - Compressive stress-strain curves of Neovius surface thicknesses (NT). Reference samples, R The study of out-of-plane properties highlights the mechanisms by which cellular solids deform and fail. Starting with the comparative principle that R samples are the base variable of each parameter, in each 3 different topologies, their values serve as a comparison for the parameters presented in the following sections. According to Figure 32, it presents a typical stress-strain curve characteristic of compressive deformation in plastically yielding open cellular solids. That is, the three stages of the deformation of B, P and N lattice structures, such as linear-elastic, plastic plateau and densification stages are showed. So, at a first stage, when the samples are compressed elastically in the z-direction, bending of the cell walls contributes to a homogeneous deformation of the lattice samples. It finishes at yield point which is, approximately, at a strain of 5% for B, 3% for P and 4% for N. At this point, the deformation starts to localize at a plastic plateau of roughly constant strength which sets the post-yield behavior. This differentiating feature of LS samples corresponds as bending-dominated for B due to overlapping underlying layers without the occurrence of rupture. Stretching-dominated for P and N due to the concavities present in stressstrain curves relative to the layer breakage. It ends, approximately, at 45%, 56% and 50% densification strains, in the respective order. The densification occurs between this point until 75% strain. 0 2 4 6 8 10 12 14 16 010 20 30 40 50 60 70 80 Compressive stress [MPa] Deformation [%] NT1 NR NT2
Chapter 4. Results and discussion 50 Figure 32 - Compressive stress-strain curves of reference samples (R). Focusing on the NR compressive stress-strain curve, it shows a decrease in strength at, approximately, 38% strain before reaching the densification region. Its wide amplitude that goes beyond the plateau strength draws attention to the fact that there was no cell breakdown, but a significant flexion that provided a slip between the samples and the compressive plates (Figure 33). At a specific strain, the overlapping of the cells provides the slippage of the Teflon sheets which it does not interfere in the results obtained because the densification occurs before these sheets move. 0 2 4 6 8 10 12 14 010 20 30 40 50 60 70 80 Compressive stress [MPa] Strain [%] BR PR NR 0 2 4 6 8 10 12 14 010 20 30 40 50 60 70 80 Compressive stress [MPa] Strain [%] NR Figure 33 - Representation of the slippage of Teflon sheets during the compressive test.
Chapter 4. Results and discussion 51 In general, it is possible to conclude that the compressive behavior is ductile, due to the post peak softening that tends to stabilize in a horizontal plateau, with residual resistance. It should be noted that the critical stresses of the NR structure, in comparison with the other topologies, stand out. From the above chart, it was possible to obtain the mechanical properties shown in Table 10. The NR lattice achieves its yield point at a compressive strength and strain of 4,4 kN, and 3,76%, respectively, At this point, PR resist around 1,5 kN at 2,98% and BR around 0,7 kN at 5,07%. As the yield point occurs to similar strains, the NR is the one that presents an improved performance for higher stresses. That is, it would be the most correct option to preserve the structures integrity when submitted to compressive forces. Although the yield point of the three structures seems to occur relatively early, the structures do not recover their initial shape after bearing a load of approximately 67 kg, 153 kg and 432 kg when using BR, PR and NR, respectively. With a remarkable advance, the modulus of elasticity and the plateau strength of NR are the largest ones, that is, it is the most rigid structure. This is caused by the fact that the cell is more closed and, by the larger contact area between the unit cells when they are replicated. Due to its high and extended plateau regime, until 50,9 %, a higher energy absorption capacity of 170,7 J is guaranteed. Although the maximum range between the three densification strains is of 11%, it can be concluded that the absorbed energy is mainly influenced by plateau strength. The greater the plateau strength, the greater the energy absorbed by the lattice structure. Table 10 – Compressive mechanical properties of reference (R) LS. 𝑬 𝝈𝒀 𝜺𝒀 𝜺𝑫 𝝈𝒑𝒍 𝑾𝑫 Units [MPa] [MPa] [%] [%] [MPa] [J] BR 10,16 ± 0,47 0,42 ± 0,01 5,07 ± 0,10 45,15 ± 2,02 0,86 ± 0,03 35,50 ± 2,66 PR 39,32 ± 0,21 0,96 ± 0,01 2,98 ± 0,05 56,16 ± 3,55 1,50 ± 0,02 81,40 ± 6,20 NR 99,53 ± 2,04 2,72 ± 0,16 3,76 ± 0,20 50,94 ± 1,00 3,53 ± 0,19 170,73 ± 8,26 Note: E – Young’s Modulus σY – Yield stress εY – Yield strain εD – Densification strain σpl - Plateau stress WD - Energy absorption
Chapter 4. Results and discussion 52 Unit cell parameters In order to understand the mechanical performance of the LS, this point addresses, in a detailed and individual way, the influence of the surface thickness, unit cell size and shell thickness on the LS. (i) Surface thickness, T As one of the most important parameters in the variation of the relative density, the surface thickness has a high importance in the mechanical performance of cellular structures. From Table 3, it is possible to observe the variations in the thickness of the surfaces relative to the reference unit cell, being T1 of lower thickness and T2 of upper thickness. Here, the comparison between the results was made separately between the 3 thicknesses, according to each different relative density. Therefore, first the results for T1 and then T2 were discussed. Figure 34 represents the results referring to the lower surface thickness, T1. From it, it is possible to observe a better mechanical performance by NT1. It reaches a compression yield strength at 3,89 kN. Next one finds the PT1 with, approximately, 1/3 of the NT1 force with 1,07 kN. Finally, with a lower compression force at the yield point, comes the BT1 with 0,35 kN. Regarding the yield strain, it is higher for BT1 (6,9%), followed by NT1 (3,5%) and PT1 (2,9%). The modulus of elasticity of NT1 is much higher than the other cellular structures, hence being the most rigid structure (Table 11). The plateau region extends to strains of 51,0% for BT1, 57,7% for PT1 and 53,1% for NT1. Since the range of densification strains is small, and the plateau strength increases in the order of B, P and N, it is possible to see, from the Figure 37 - c, that the energy absorbed by NT1 is higher and that of BT1 is lower. In addition, PT1 withstands higher loads than BT1, equaling between 57% and 65% deformation. From 65% to 75% deformation, BT1 ends up being stronger than PT1. Thus, for the lower surface thickness parameter, the energy absorption is higher for NT1.
Chapter 4. Results and discussion 53 Figure 34 - Compressive stress-strain curves of lower surface thickness (T1). To enable comparison between results, the Figure 36 represents the curves relating to an increase in surface thickness of the reference unit cells, T2 (upper surface thickness). But first, it is necessary to report an important fact during the compressive tests of NT2 that interfere with the coherence of the obtained results: a significant slippage occurred between the tested samples and the compression plates before the densification strain (Figure 35). From the graphic, this effect starts at a strain of, approximately, 36%. 𝝆 Figure 35 - Slippage of NT2 specimens before the densification strain. 0 2 4 6 8 10 12 14 010 20 30 40 50 60 70 80 Compressive stress [MPa] Deformation [%] BT1 PT1 NT1 NT2_1 NT2_2 NT2_3
Chapter 4. Results and discussion 54 Figure 36 - Compressive stress-strain curves of upper surface thickness (T2). From Table 11, the resistance of the structures to the compression force at the yield point was higher for NT2 with a capacity of 5.0 kN, followed by PT2 with 2.7 kN and BT2 with 1.1 kN (approximated values). The plateau region extended to 43,1%, 59,0% and 52,7% strain for BT2, PT2 and NT2, respectively. Between 49% and 74% of strains, BT2 has a higher mechanical resistance than the other two, but from 68% strain, its performance is losing quality due to the disassociation of the cells in contact with the shell. Regarding NT2 and PT2, already in the densification regime, they maintained an identical behavior until the end of the test, with NT2 having a higher resistance. Despite of the circumstances, the NT2 structure presents a higher modulus of elasticity as well as a higher capacity of energy absorption. This is due to the fact that there is a larger contact area between the unit cells. An increase in the thickness of cell walls of cellular structures increases the relative density. Then the resistance to cell wall bending and cell collapse goes up, giving a higher modulus and plateau strength. Due to the slip effect that occurred during the trials it can be concluded that it affected the densification strain and plateau strength values. The larger the slippage of the sample, the later the densification occurs. Table 11 -Compressive properties varying the surface thickness parameter (T). 𝑬 𝝈𝒀 𝜺𝒀 𝜺𝑫 𝝈𝒑𝒍 𝑾𝑫 Units [MPa] [MPa] [%] [%] [MPa] [J] BT1 4,07 ± 0,15 0,22 ± 0,00 6,94 ± 0,03 51,00 ± 0,08 0,43 ± 0,01 19,72 ± 0,45 0 2 4 6 8 10 12 14 16 18 20 010 20 30 40 50 60 70 80 Compressive stress [MPa] Deformation [%] BT2 PT2 NT2
Chapter 4. Results and discussion 55 BR 10,16 ± 0,47 0,42 ± 0,01 5,07 ± 0,10 45,15 ± 2,02 0,86 ± 0,03 35,50 ± 2,66 BT2 21,43 ± 0,41 0,72 ± 0,01 4,62 ± 0,06 43,05 ± 0,12 1,54 ± 0,02 60,53 ± 0,96 PT1 27,07 ± 0,20 0,67 ± 0,00 2,90 ± 0,02 57,69 ± 0,36 1,02 ± 0,01 56,88 ± 0,27 PR 39,32 ± 0,21 0,96 ± 0,01 2,98 ± 0,05 56,16 ± 3,55 1,50 ± 0,02 81,40 ± 6,20 PT2 65,49 ± 4,53 1,68 ± 0,10 2,99 ± 0,01 59,02 ± 0,95 2,74 ± 0,05 155,88 ± 5,60 NT1 97,01 ± 1,30 2,44 ± 0,15 3,51 ± 0,17 53,07 ± 0,92 3,24 ± 0,21 163,83 ± 9,47 NR 99,53 ± 2,04 2,72 ± 0,16 3,76 ± 0,20 50,94 ± 1,00 3,53 ± 0,19 170,73 ± 8,26 NT2 116,61±5,81 3,15 ± 0,18 3,65 ± 0,19 52,65 ± 1,13 4,16 ± 0,29 208,31 ± 12,12 Note: E – Young’s Modulus σY – Yield stress εY – Yield strain εD – Densification strain σpl - Plateau stress WD - Energy absorption In short, the compressive modulus and strength increase with increasing thickness and, consequently, with relative density. From the Figure 37 it is possible to observe that the N cellular structure presents better mechanical performance, which is higher the thicker of the surface is. It is also be noted that the variation from R structures to T2 structures is higher than the variation from T1 to R structures.
Chapter 4. Results and discussion 56 Figure 37 – Compressive (a) modulus, (b) plateau strength and (c) energy absorbed of B, P and N lattice structures at a strain of 1,3 mm/min varying the surface thickness (T). (ii) Cell size, C Unlike the parameter described in the previous point, this point deals with the influence on the structural mechanical performance, when the cell size variation is given. Here, the relative density of the standardized unit cell about 17,8% is maintained. Having said this, Figure 38 and Figure 39 represent the compressive stress-strain curves for C1 and C2 variations, corresponding to the cubic unit cell sizes of 13,33 mm and 20 mm edge, respectively. The third variant is the reference cell size with 10 mm edge, which was previously discussed in section 4.1.1. As in the reference sample, NC1 cellular structure suffered the same slippage effect before reaching its densification region, affecting the obtained experimental values, such as, the plateau strength and the densification strain. 0 50 100 150 15 20 25 30 Modulus of Elasticity [MPa] Relative density [%) B P N 0 1 2 3 4 5 15 20 25 30 Plateau strength [MPa] Relative density [%] B P N 0 50 100 150 200 250 15 20 25 30 Energy absorption [J] Relative density [%] B P N a) b ) c)
Chapter 4. Results and discussion 57 Figure 38 - Compressive stress-strain curves of 13,33 mm cell size (C1). According to the reported data, Table 12 shows their mechanical properties. Even though certain tabulated values do not correspond to the exact experimental values due to the slippage, NC1 lattice leads the mechanical performance with a modulus of elasticity of 94,1 MPa and a plateau strength of 2,3 MPa, where densification begins at a deformation of 55,9%. Next comes PC1 in which the densification begins at 49,4% deformation and, finally, BC1 with a densification deformation of 45,2%. BC1, PC1 and NC1 present a planar regime that stagnates at compression forces of approximately 0,8 MPa, 1,5 MPa and 2,3 MPa, respectively, NC1 being capable of absorbing a greater amount of energy. 0 2 4 6 8 10 12 010 20 30 40 50 60 70 80 Compressive stress [MPa] Deformation [%] BC1 NC1 PC1
Chapter 4. Results and discussion 64 for P and N, the pre-factors of performance characterization stated as C1, C5, and were obtained and summarized in Table 14. Table 14 - Gibson-Ashby formula coefficients of several lattice structures. C1 C5 C1 C5 0,1 – 4,0 0,1 - 1 1,4 - 2 0,1 – 4,0 0,1 - 1 1,4 - 2 BR PR NR 0,13 0,11 0,24 0,18 0,15 0,29 2,43 1,94 1,83 BT1 PT1 NT1 0,09 0,09 0,25 0,13 0,12 0,28 2,85 2,19 1,82 BT2 PT2 NT2 0,18 0,14 0,23 0,23 0,20 0,28 2,04 1,36 1,42 BC1 PC1 NC1 0,14 0,11 0,27 0,17 0,15 0,23 2,51 2,24 1,95 BC2 PC2 NC2 0,15 0,12 0,29 0,18 0,16 0,26 2,44 1,72 2,01 BS1 PS1 NS1 0,13 0,12 0,26 0,19 0,17 0,30 2,19 1,85 1,81 BS2 PS2 NS2 0,12 0,10 0,29 0,16 0,13 0,28 2,17 1,64 1,77 The C1 and C5 pre-factors of B, P and N structures are within the given ranges. The coefficients of exceed 2 in all B and in PT1 and PC1 lattice structures, which is related to the matrix material of PA2200. The toughness of PA2200 is comparatively lower than ordinary plastic lattice after SLS processing. Thus, the densification strain gets smaller in the lattice structures obtained. IMPACT TESTS As in the compression tests, this section reports and discuss the results obtained during the impact tests, according to the two different independent variables of the unit cell, such as, surface and shell thicknesses. During these tests, the impactor energy of 98 J was maintained. For this purpose, in a first analysis, the results relative to the reference sample, R, are addressed. Then, each cell parameter in order to access the impact properties of the produced samples are addressed individually. Before proceeding to the detailed analysis of the results obtained, it is necessary to mention the dimensional precision and the resulting relative densities. According to the Table 15, it is possible to verify that the produced samples shrink in diameter but expand in height in a higher proportion. Comparing to the modelled dimensional volume, it is obtained the general expansion of the produced samples in a maximum value of 0,67% ± 0,10 belonging to sample N.
Chapter 4. Results and discussion 65 Table 15 - Dimensional accuracy of impact test samples. In comparative terms, between the modelled and experimental relative densities of the produced samples, it is possible to verify, based in Table 16, that there was greater discrepancy between the N samples. Such deviations are due to the geometry of the structural cell, making it difficult to extract the non-sintered powder. Once again, the non-sintered powder did not affect the impact properties obtained. Table 16 - Experimental and modelled relative densities of impact test samples. Relative density [%] Experimental CAD model Experimental CAD model BR PR NR 28 ± 0,36 28 ± 0,40 30 ± 0,72 25 25 24 BT1 PT1 NT1 23 ± 0,15 24 ± 0,04 25 ± 0,16 21 21 20 BT2 PT2 NT2 32 ± 0,21 32 ± 0,09 33 ± 0,99 29 29 28 BS1 PS1 NS1 36 ± 0,25 36 ± 0,18 37 ± 0,78 32 32 32 BS2 PS2 NS2 44 ± 0,38 44 ± 0,77 47 ± 0,12 40 39 40 Reference samples, R The impact tests were performed considering the methodology described above. Figure 44 presents the Force-Deflection curves relative to the R samples. In a general way, the three different curves present an initial ascension of the until a first damage peak. This represents the force necessary to penetrate the upper shell and it occurs before reaching the lattice core. Such peaks are often associated with localized splitting, resulting in the load drop and change in specimen compliance. Then, the local damage stops growing, requiring increased force and energy for the damage to progress further, at maximum force. For NR sample, the test ends at a maximum point, where the compaction of the cell layers occurs before the strike reaches the lower S1 (%) BCC Schwarz – P Neovius Diameter -0,16 ± 0,06 -0,17 ± 0,03 -0,16 ± 0,05 Height 0,81 ± 0,08 0,99 ± 0,26 0,99 ± 0,12 Volume 0,48 ± 0,16 0,64 ± 0,24 0,67 ± 0,10
Chapter 4. Results and discussion 66 shell. The strike ends up penetrating the sample in its entirety by drag force. In PR sample, the unitary constituent cells are capable of further deformation and, consequently, delay the complete penetration of the strike. The fact of the existence of the bottom shell, it also contributed to this delay. Graphically, this effect is represented by the prolongation of the curve, after the maximum peak, and before an abrupt fall of force occurs. For the BR sample, after the first damage peak, the force required to break the successive cell layers remains practically constant until the strike penetrates the bottom shell. Figure 44 – Impact force-deflection curves of reference test samples (R). Table 17 represents the R impact properties obtained in the experimental tests. From the presented values, it is possible to conclude that NR sample resists a maximum impact force of 3527,4 N, followed by PR with 2987,3 N and, finally, BR with 1930,2 N. Still referring to the maximum peak, although BR presents a lower impact capacity than the remaining samples, it is capable of absorbing a greater amount of energy. This is related to the fact that it is reached when the dart is very close to the lower shell, after approximately 17,93 mm. Such maximum peak occurs at deformations of 12,02 mm and 10,03 mm for P and N, respectively. At the end of the tests, when the puncture point is reached, PR is the structure with the highest absorption energy (30,88 J), followed, orderly, by NR (28,03 J) and BR (22,65 J). The greatest interval of energies, between the maximum point of force and the puncture point, belongs to the PR with 9,18 J, which also presents a greater interval traversed by the dart between these same points, with the value of 3,82 mm. That said, NR cellular structure is the one with the best of impact force, but PR lattice 0 1000 2000 3000 4000 5000 6000 7000 8000 0 5 10 15 20 25 30 35 40 Force [N] Deflection [mm] BR PR NR
Chapter 4. Results and discussion 67 structure is the one with the best impact absorber. The impact failure of R lattice structures consists on a yielding followed by stable cracking. Table 17 - Impact mechanical properties of the Reference Samples (R). Maximum force Deflection at maximum force Energy to maximum force Puncture deflection Puncture energy Units [N] [mm] [J] [mm] [J] BR 1930,19 ± 248,22 17,93 ± 2,28 22,10 ± 5,16 18,25 ± 2,18 22,65 ± 5,12 PR 2987,25 ± 128,79 12,02 ± 0,94 21,70 ± 1,83 15,84 ± 0,28 30,88 ± 0,07 NR 3527,38 ± 220,94 10,03 ± 0,51 21,76 ± 1,97 12,57 ± 0,95 28,03 ± 2,67 Unit cell parameters In order to understand the impact mechanical performance, of each lattice structure, composed by B, P and N topologies, this section makes an individualized characterization of each independent cellular variable, first for the surface thickness and then, for the shell thickness. (i) Surface thickness, T Knowing beforehand that the thickness of the unit cells is a parameter with high importance in the mechanical performance of lattice structures when submitted to compressive forces, it was also studied when submitted to an impact force. Despite the different general dimensions between compression and impact samples, thus providing different relative densities, the relative density of the unit cell was maintained in order to compare them. Before continuing to discuss the results obtained, it is necessary to mention that deformed samples were not accepted due to the force exerted by the closing unit. That said, it is possible to anticipate that only one of the clones of the BT1 sample underwent a remarkable bending before being tested and was eventually excluded from the study (Figure 45).
Chapter 4. Results and discussion 68 Figure 45 -BT1 test specimen after clamping force: a) with deformation and b) without deformation. In a quick visual interpretation, it is possible to observe, in Figure 46 and Figure 47 corresponding, respectively, to lower (T1) and upper (T2) surface thicknesses, that NT1 resists to higher and BT1 to lower impact forces for the first ones, and the PT2 presents the highest and, once again, BT2 the smallest resistance for the second ones. Figure 46 - Impact force-deflection curves of lower surface thickness test samples (T1). 0 1000 2000 3000 4000 5000 6000 7000 8000 0 5 10 15 20 25 30 35 40 Force [N] Deflection [mm] BT1 PT1 NT1 a b
Chapter 4. Results and discussion 69 Figure 47 - Impact force-deflection curves of upper surface thickness test samples (T2). In a more detailed analysis, Table 18 presents the impact properties of greater relevance according to the results obtained. As for the T1 thickness, the NT1 has the highest impact rigidity, reaching a maximum force of 2978 N, when the dart penetrates half of the structure. It has the capacity to absorb the highest amount of energy at the peak of maximum force (20,9 J) and its drilling deflection occurs about 2 mm after this peak, capable of absorbing 25,7 J. Secondly, is PT1, with 2068 N of maximum force when the dart penetrates 13 mm of the structure. At this point, it has the capacity to absorb 16,9 J. The perforation deflection occurs at approximately 4 mm after this peak of maximum force with an absorption energy of 23,3 J. The use of this cellular topology becomes advantageous due to the greater delay of the perforation deflection, which allows it to absorb a greater amount of energy. Finally, between the three different topologies, BT1 is the structure that presents lower impact properties. This less rigid structure, besides supporting an impact load of 1348 N, is reached even at the end of the drilling of the dart, at approximately 18 mm. Its energy absorption capacity is around 12,5 J. Due to the initial and final peaks, represented by the curves, it is possible to conclude that the impact failure of the T1 samples occurred in its entirety. For NT1, the final peak is of lesser amplitude and it may be justified by the fact that the lower shell is not able to withstand the impact imposed by the strike, ending up breaking by drag force. As far as T2 thickness is concerned, the order of leadership has changed. The result of this increase in surface thickness, allowed PT2 to reach the greater rigidity with the capacity to withstand 4799 N of maximum force. With about 100 N less, it follows NT2. Although PT2 has a maximum impact force higher than NT2, the latter reaches such a force at a lower impactor 0 1000 2000 3000 4000 5000 6000 7000 8000 0 5 10 15 20 25 30 35 40 Force [N] Deflection [mm] BT2 PT2 NT2
Chapter 4. Results and discussion 70 deflection, just over 2 mm difference. At the end of the table there is BT2, with the capacity to support 2655 N. In terms of energy absorbed, PT2 is the structure that absorbs the most energy reaching 30,1 J, followed by NT2 with 23,8 J and, finally, BT2 with 20,9 J. Once the maximum peak is exceeded, the puncture deflection is analyzed. At this point, it is possible to verify that, among the three topologies, the PT2 reaches 42,6 J of maximum absorbed energy, after deforming 3 mm. This potentiality lies in the fact that the constituent cells are able to deform easily, leading to a slightly longer shell break than an abrupt one. Regarding BT2 and NT2, BT2 is able to prolong its deformation in relation to NT2, which allows it to absorb more energy before the rupture is complete. The inability of NT2 to prolong the penetration of the dart and, thus, absorb a greater amount of energy falls on the complex form of the constituent cellular unit. Once again, the resistance that the cell walls exert as the dart pierces the sample is such that, upon reaching a certain point of compaction of the constituent cells, this force is capable of breaking the nearby cells before the dart reaches them. Graphically, this effect is represented by the abrupt post-peak drop of maximum force. Experimentally, the dart is not able to break the sample in its entirety but, by drag force, it ends up doing so. Table 18 – Impact mechanical properties varying the surface thickness parameter (T). Maximum force Deflection at maximum force Energy to maximum force Puncture deflection Puncture energy Units [N] [mm] [J] [mm] [J] BT1 1348,79 ± 101,57 17,91 ± 0,06 12,47 ± 0,09 18,20 ± 0,17 12,85 ± 0,26 BR 1930,19 ± 248,22 17,93 ± 2,28 22,10 ± 5,16 18,25 ± 2,18 22,65 ± 5,12 BT2 2655,32 ± 348,54 11,62 ± 3,21 20,87 ± 6,25 15,50 ± 1,78 30,34 ± 7,21 PT1 2068,14 ± 38,78 13,04 ± 2,24 16,97 ± 3,68 16,94 ± 0,14 23,39 ± 0,52 PR 2987,25 ± 128,79 12,02 ± 0,94 21,70 ± 1,83 15,84 ± 0,28 30,88 ± 0,07 PT2 4799,11 ± 258,63 10,66 ± 0,58 30,11 ± 3,74 13,71 ± 0,66 42,63 ± 4,95
Chapter 4. Results and discussion 71 NT1 2978,45 ± 97,57 10,29 ± 1,18 20,91 ± 3,75 12,14 ± 0,27 25,74 ± 0,80 NR 3527,38 ± 220,94 10,03 ± 0,51 21,76 ± 1,97 12,57 ± 0,95 28,03 ± 2,67 NT2 4695,87 ± 177,34 8,49 ± 0,47 23,75 ± 2,48 8,97 ± 0,43 25,50 ± 2,37 In short, regarding to T1 thickness, N is the most rigid topology, ideal for absorbing impacts. For T2 thickness, P is the ideal lattice structure. Between T1 and R thicknesses, there is a turning point that makes P, despite resisting a lower maximum impact force, capable in absorbing a great amount of energy. Between the R and T2 thicknesses there is another turning point. From a certain thickness, B is capable of absorbing a greater amount of energy comparing to N, and despite having a lower maximum impact force peak. Generally, the greater the cell surface thickness, the greater the stiffness of the cellular structure and, consequently, the lower its deflection. As for the energy absorbed by this type of structures, it also increases with the increase in surface thickness, with the exception of N. In topological terms, the unit cell P presents a very interesting performance. The use of the ideal topological unit takes into account the specifications of the final product. (ii) Shell thickness, S In order to complement the optimization of a cellular structure, the study of the shell thickness appears. To this end, the thickness of the shell was varied in relation to the reference thickness of 1 mm. The first increase in shell thickness corresponds to 2 mm, S1, where the respective curves obtained from the tests performed are represented in the Figure 48. From this, it is possible to verify that the three cellular topologies present a remarkable first damage peak. Focusing individually on each curve, the BS1 structure presents a decrease in the impact force after the peak, due to the change in the integrity of the first cellular layer by the deflection of the shell. Once the first layer is broken, the impact force tends to stabilize until the end of the test. The force required for the lower and upper shell breakage are similar, which indicates that the cellular compaction is scarce. This effect is noticeably reflected in the absolute deformation of the sample. In PS1, the lower shell is the one that most hinders the penetration of the dart (rise of the curve at the end of the test), requiring greater impact force from the striker. Its total rupture occurs through the drag force caused by successive compaction of the cellular layers. In NS1, the impact force
Chapter 4. Results and discussion 72 achieved by the sample is mostly concentrated in the constituent core that eventually ruptured under the action of the drag force, after reaching maximum compaction. The opportunity for the core to reach such values is contemplated by the presence of the bottom shell. From the curves drawn, Table 19 presents the mechanical properties relative to each cellular sample. From this, it can be seen that PS1 is the most rigid structure, presenting the highest impact force (4204 N) after a striker penetration of 13 mm. With an intermediate capacity of 4057 N, it follows NS1 when it is reached by a penetration of, approximately, 10 mm. Finally, with a lower capacity is BS1 with 1944 N and 17,5 mm of deflection. In the same order, each structure presents 35,1 J, 26,8 J and 21,8 J. After the maximum force peak, at a puncture deflection, BS1 remained practically unchanged with the rise of approximately 1 J suffering the deflection of 1 mm. PS1 suffered 1,7 mm of deflection reaching 41 J of absorbed energy. NS1 suffered a significant deformation in relation to the other structures (4 mm), surprising PS1 with an impact absorption energy close to 40 J. Although PS1 is the most rigid cell structure, the parameter S1 had a greater impact on NS1. Figure 48 - Impact force-deflection curves of 2 mm shell thickness (S1). According to the increase in shell thickness corresponding to 3 mm, S2, the impact properties for samples BS2, PS2 and NS2 were not very consistent, and this can be verified from the large standard deviation values presented (Figure 49). Regarding PS2, despite the large deviation, it is possible to verify some coherence by the overlapping of the curves of the three clones tested in the first damage peak and in the puncture deflection. In the BS2 and NS2 clones’ curves, there is little repeatability between samples. To try to decipher the interference of the shell thickness in NS2, five samples were tested. Initially 3 samples were tested and NS1_1 sample 0 1000 2000 3000 4000 5000 6000 7000 8000 0 5 10 15 20 25 30 35 40 Force [N] Deflection [mm] BS1 PS1 NS1
Chapter 4. Results and discussion 73 was found to be very different from the other ones. In order to understand the exact behavior of NS2, two more samples were tested. After all, the behavior tends to the NS1_1 side, but the discrepancy between values is very large. That said, all the samples tested were kept predicting its impact properties. Figure 49 – Impact force versus deflection of the clones of 3 mm shell thickness parameter (S2) in each topology. From the curves represented in the Figure 50, it is possible to observe the average curves of each structure corresponding to S2. From the BT2 and PT2 curves it is possible to clearly verify the penetration of the dart through the upper shell (first peak), the core of the samples (second peak) and the lower shell (last peak). For NT2, the lower shell is not represented by a last peak, but it is noticed by the decrease of the impact force with negative slope, practically, constant before the sample is penetrated in its totality. The negative slope of the curve is due to a mixture of the breakage of the constituent cells with the help of support of the lower shell. This delays the complete penetration of the striker, which eventually occurs by drag force. According to the values presented in Table 19, it is possible to conclude that NS2 is the most rigid structure, supporting 6017 N when the structure suffers a deflection of 12,5 mm. At this maximum peak, an amount of energy of 51,3 J is absorbed. When it reaches the perforation deflection, the sample is capable of absorbing 60,9 J after deforming another 2,3 mm. This absorption is possible due to the fact that the sample does not break right after the maximum peak force. Labelled as the second 0 2000 4000 6000 8000 010 20 30 40 Force [N] Deflection [mm] BS2 BS2_1 BS2_2 BS2_3 0 2000 4000 6000 8000 010 20 30 40 Force [N] Deflection [mm] PS2 PS2_1 PS2_2 PS2_3 0 2000 4000 6000 8000 010 20 30 40 Force [N] Deflection [mm] NS2 NS2_1 NS2_2 NS2_3 NS2_4 NS2_5
80 models made by additive manufacturing (rapid manufacturing),” J. Cranio-Maxillofacial Surg., vol. 41, no. 7, pp. 603–609, 2013. [28] M. Javaid and A. Haleem, “Additive manufacturing applications in medical cases: A literature based review,” Alexandria J. Med., vol. 54, no. 4, pp. 411–422, 2018. [29] C. M. González-Henríquez, M. A. Sarabia-Vallejos, and J. R. Hernandez, “Antimicrobial polymers for additive manufacturing,” Int. J. Mol. Sci., vol. 20, no. 5, 2019. [30] R. Huang et al., “Energy and emissions saving potential of additive manufacturing: the case of lightweight aircraft components,” J. Clean. Prod., vol. 135, pp. 1559–1570, 2016. [31] A. Zhakeyev, P. Wang, L. Zhang, W. Shu, H. Wang, and J. Xuan, “Additive Manufacturing: Unlocking the Evolution of Energy Materials,” Adv. Sci., vol. 4, no. 10, 2017. [32] B. Berman, “3-D printing: The new industrial revolution,” Bus. Horiz., vol. 55, no. 2, pp. 155–162, 2012. [33] D. Mac Sithigh, “When the Dealin’s Done: Recent Developments in Online Gambling Law and Policy.,” SCRIPTed, vol. 11(2), no. 1, p. 171, 2014. [34] M. Attaran, “The rise of 3-D printing: The advantages of additive manufacturing over traditional manufacturing,” Bus. Horiz., vol. 60, no. 5, pp. 677–688, 2017. [35] G. Harsha Vardhan, G. H. Charan, P. V. S. Reddy, and K. Sampath Kumar, “International Journal on Recent and Innovation Trends in Computing and Communication 3D Printing: The Dawn of a New Era in Manufacturing,” no. August, pp. 2373–2376, 2014. [36] B. Sedacca, “Hand built by lasers,” Eng. Technol., vol. 6, no. 1, pp. 58–59, 2011. [37] M. Leino, J. Pekkarinen, and R. Soukka, “The role of laser additive manufacturing methods of metals in repair, refurbishment and remanufacturing - Enabling circular economy,” Phys. Procedia, vol. 83, pp. 752–760, 2016. [38] Series Editors. 2002. [39] D. L. (The U. of T. at A. ) Bourell, M. C. (Missouri U. of S. and T. ) Leu, and D. W. (Georgia I. of T. ) Rosen, “Roadmap for Additive Manufacturing,” Univ. Texas Austin, p. 92, 2009. [40] X. Wang, M. Jiang, Z. Zhou, J. Gou, and D. Hui, “3D printing of polymer matrix composites: A review and prospective,” Compos. Part B Eng., vol. 110, pp. 442–458,
81 2017. [41] J. Z. Manapat, Q. Chen, P. Ye, and R. C. Advincula, “3D Printing of Polymer Nanocomposites via Stereolithography,” Macromol. Mater. Eng., vol. 302, no. 9, pp. 1– 13, 2017. [42] B. Stucker, “Additive Manufacturing Technologies: Technology Introduction and Business Implications,” Front. Eng. 2011 Reports Leading-Edge Eng. from 2011 Symp., vol. 0, p. pages 1-9, 2012. [43] J. Klingelnberg, Manufacturing Process. Elsevier Inc., 2016. [44] P. Calvert, “Inkjet printing for materials and devices,” Chem. Mater., vol. 13, no. 10, pp. 3299–3305, 2001. [45] Hue P. Le, “Progress and Trends in Ink-jet Printing Technology,” J. Imaging Sci. Technol., vol. 42, no. 1, pp. 49–62, 1998. [46] B. J. De Gans, P. C. Duineveld, and U. S. Schubert, “Inkjet printing of polymers: State of the art and future developments,” Adv. Mater., vol. 16, no. 3, pp. 203–213, 2004. [47] Redwood Ben, “Additive Manufacturing Technologies: An Overview | 3D Hubs,” Knowledge base, 2017. [Online]. Available: https://www.3dhubs.com/knowledgebase/additive-manufacturing-technologies-overview/. [Accessed: 17-Sep-2020]. [48] “Material jetting - MJ, NPJ, DOD | Make.” [Online]. Available: https://make.3dexperience.3ds.com/processes/material-jetting. [Accessed: 03-Mar-2021]. [49] “Sheet Lamination| Additive Manufacturing Research Group | Loughborough University,” 2019. [Online]. Available: https://www.lboro.ac.uk/research/amrg/about/the7categoriesofadditivemanufacturing/she etlamination/. [Accessed: 17-Sep-2020]. [50] I. Gibson, D. W. Rosen, and B. Stucker, “Additive manufacturing technologies: Rapid prototyping to direct digital manufacturing,” Addit. Manuf. Technol. Rapid Prototyp. to Direct Digit. Manuf., no. 1991, pp. 1–459, 2010. [51] E. MacDonald and R. Wicker, “Multiprocess 3D printing for increasing component functionality,” Science (80-. )., vol. 353, no. 6307, 2016. [52] J. Y. Lee, J. An, and C. K. Chua, “Fundamentals and applications of 3D printing for novel materials,” Appl. Mater. Today, vol. 7, pp. 120–133, 2017. [53] S. H. Huang, P. Liu, A. Mokasdar, and L. Hou, “Additive manufacturing and its societal
82 impact: A literature review,” Int. J. Adv. Manuf. Technol., vol. 67, no. 5–8, pp. 1191–1203, 2013. [54] J. Shah, B. Snider, T. Clarke, S. Kozutsky, M. Lacki, and A. Hosseini, “Large-scale 3D printers for additive manufacturing: design considerations and challenges,” Int. J. Adv. Manuf. Technol., vol. 104, no. 9–12, pp. 3679–3693, 2019. [55] R. Langdon, Rapid prototyping, vol. 23, no. 5. 1998. [56] P. Kocovic, 3D Printing and Its Impact on the Production of Fully Functional Components. 2017. [57] “Selective Laser Sintering Equipment Market by Material & Industry - Global Forecast to 2023 | MarketsandMarkets.” [Online]. Available: https://www.marketsandmarkets.com/Market-Reports/selective-laser-sintering- equipment-market-27853684.html. [Accessed: 17-Sep-2020]. [58] D. King and T. Tansey, “Alternative materials for rapid tooling,” J. Mater. Process. Technol., vol. 121, no. 2–3, pp. 313–317, 2002. [59] M. Król, M. Kujawa, L. A. Dobrzański, and T. Tański, “Influence of technological parameters on additive manufacturing steel parts in Selective Laser Sintering,” Arch. Mater. Sci. Eng., vol. 67, no. 2, pp. 84–92, 2014. [60] S. Singh, S. Ramakrishna, and R. Singh, “Material issues in additive manufacturing: A review,” J. Manuf. Process., vol. 25, pp. 185–200, 2017. [61] X. Li et al., “Thermal simulation of the cooling down of selective laser sintered parts in PA12,” Rapid Prototyp. J., vol. 24, no. 7, pp. 1117–1123, 2018. [62] D. T. Pham, K. D. Dotchev, and W. A. Y. Yusoff, “Deterioration of polyamide powder properties in the laser sintering process,” Proc. Inst. Mech. Eng. Part C J. Mech. Eng. Sci., vol. 222, no. 11, pp. 2163–2176, 2008. [63] “How does additive manufacturing work?” [Online]. Available: https://www.eos.info/en/industrial-3d-printing/additive-manufacturing-how-it-works. [Accessed: 07-Jan-2021]. [64] S. Kumar, “Selective Laser Sintering: A Qualitative and Objective Approach,” Jom, vol. 55, no. 10, pp. 43–47, 2003. [65] M. Schmid, A. Amado, and K. Wegener, “Polymer powders for selective laser sintering (SLS),” AIP Conf. Proc., vol. 1664, 2015.
83 [66] A. T. Sutton, C. S. Kriewall, M. C. Leu, and J. W. Newkirk, “Powder characterisation techniques and effects of powder characteristics on part properties in powder-bed fusion processes,” Virtual Phys. Prototyp., vol. 12, no. 1, pp. 3–29, 2017. [67] G. M. Vasquez, C. E. Majewski, B. Haworth, and N. Hopkinson, “A targeted material selection process for polymers in laser sintering,” Addit. Manuf., vol. 1, pp. 127–138, 2014. [68] J. Kruth, G. Levy, R. Schindel, T. Craeghs, and E. Yasa, “Consolidation of Polymer Powders by Selective Laser Sintering_PMI08_Kruth_Levy_Keynote.” [69] S. Singh, V. S. Sharma, and A. Sachdeva, “Progress in selective laser sintering using metallic powders: A review,” Mater. Sci. Technol. (United Kingdom), vol. 32, no. 8, pp. 760–772, 2016. [70] S. Berretta, O. Ghita, and K. E. Evans, “Morphology of polymeric powders in Laser Sintering (LS): From Polyamide to new PEEK powders,” Eur. Polym. J., vol. 59, pp. 218– 229, 2014. [71] J. D. Williams and C. R. Deckard, “Emerald Article : Advances in modeling the effects of selected parameters on the SLS process Advances in modeling the effects of selected parameters on the SLS process,” Group, vol. 4, no. 2, pp. 90–100, 2011. [72] W. S. Tan, C. K. Chua, T. H. Chong, A. G. Fane, and A. Jia, “3D printing by selective laser sintering of polypropylene feed channel spacers for spiral wound membrane modules for the water industry,” Virtual Phys. Prototyp., vol. 11, no. 3, pp. 151–158, 2016. [73] S. Singh, V. S. Sharma, A. Sachdeva, and S. K. Sinha, “Optimization and analysis of mechanical properties for selective laser sintered polyamide parts,” Mater. Manuf. Process., vol. 28, no. 2, pp. 163–172, 2013. [74] D. L. Bourell, T. J. Watt, D. K. Leigh, and B. Fulcher, “Performance limitations in polymer laser sintering,” Phys. Procedia, vol. 56, no. C, pp. 147–156, 2014. [75] C. A. Chatham, T. E. Long, and C. B. Williams, “A review of the process physics and material screening methods for polymer powder bed fusion additive manufacturing,” Prog. Polym. Sci., vol. 93, pp. 68–95, 2019. [76] B. Leutenecker-Twelsiek, C. Klahn, and M. Meboldt, “Considering Part Orientation in Design for Additive Manufacturing,” Procedia CIRP, vol. 50, pp. 408–413, 2016. [77] U. Ajoku, N. Hopkinson, and M. Caine, “Experimental measurement and finite element modelling of the compressive properties of laser sintered Nylon-12,” Mater. Sci. Eng. A,
84 vol. 428, no. 1–2, pp. 211–216, 2006. [78] B. Caulfield, P. E. McHugh, and S. Lohfeld, “Dependence of mechanical properties of polyamide components on build parameters in the SLS process,” J. Mater. Process. Technol., vol. 182, no. 1–3, pp. 477–488, 2007. [79] P. Titanium and I. Anisotropy, “<MECHANICAL PROPERTIES OF SELECTIVE LASER MELTED AlSi10Mg.pdf>,” 2020. [80] I. Gibson and D. Shi, “Material properties and fabrication parameters in selective laser sintering process,” Rapid Prototyp. J., vol. 3, no. 4, pp. 129–136, 1997. [81] X. Wang and T. Laoui, “To cite this document : Lasers and materials in selective laser sintering,” vol. 23, no. 4, pp. 357–371, 2006. [82] E. O. Olakanmi, R. F. Cochrane, and K. W. Dalgarno, “A review on selective laser sintering/melting (SLS/SLM) of aluminium alloy powders: Processing, microstructure, and properties,” Prog. Mater. Sci., vol. 74, pp. 401–477, 2015. [83] S. C. Ligon, R. Liska, J. Stampfl, M. Gurr, and R. Mülhaupt, “Polymers for 3D Printing and Customized Additive Manufacturing,” Chem. Rev., vol. 117, no. 15, pp. 10212– 10290, 2017. [84] C. Y. Yap et al., “Review of selective laser melting: Materials and applications,” Appl. Phys. Rev., vol. 2, no. 4, 2015. [85] F. W. Zok, R. M. Latture, and M. R. Begley, “Periodic truss structures,” J. Mech. Phys. Solids, vol. 96, pp. 184–203, 2016. [86] D. Mahmoud and M. Elbestawi, “Lattice Structures and Functionally Graded Materials Applications in Additive Manufacturing of Orthopedic Implants: A Review,” J. Manuf. Mater. Process., vol. 1, no. 2, p. 13, Oct. 2017. [87] S. C. Han, J. W. Lee, and K. Kang, “A New Type of Low Density Material: Shellular,” Adv. Mater., vol. 27, no. 37, pp. 5506–5511, 2015. [88] K. J. Kang, “Wire-woven cellular metals: The present and future,” Prog. Mater. Sci., vol. 69, pp. 213–307, 2015. [89] H. N. G. Wadley, N. A. Fleck, and A. G. Evans, “Fabrication and structural performance of periodic cellular metal sandwich structures,” Compos. Sci. Technol., vol. 63, no. 16, pp. 2331–2343, 2003. [90] T. Maconachie et al., “SLM lattice structures: Properties, performance, applications and
85 challenges,” Mater. Des., vol. 183, p. 108137, 2019. [91] D. Li, W. Liao, N. Dai, G. Dong, Y. Tang, and Y. M. Xie, “Optimal design and modeling of gyroid-based functionally graded cellular structures for additive manufacturing,” CAD Comput. Aided Des., vol. 104, pp. 87–99, 2018. [92] M. Helou and S. Kara, “Design, analysis and manufacturing of lattice structures: An overview,” Int. J. Comput. Integr. Manuf., vol. 31, no. 3, pp. 243–261, 2018. [93] T. Tancogne-Dejean, A. B. Spierings, and D. Mohr, “Additively-manufactured metallic micro-lattice materials for high specific energy absorption under static and dynamic loading,” Acta Mater., vol. 116, pp. 14–28, 2016. [94] P. Dziewit, P. Paweł, J. Janiszewski, M. Sarzyński, M. Grązka, and P. Robert, “Mechanical Response of Additive Manufactured Regular Cel Structures in Quasi-Static Loading Conditions - Part I Experimental Investigations,” Chest, vol. 148, no. 4, p. 558A, 2017. [95] M. G. Rashed, M. Ashraf, R. A. W. Mines, and P. J. Hazell, “Metallic microlattice materials: A current state of the art on manufacturing, mechanical properties and applications,” Mater. Des., vol. 95, pp. 518–533, 2016. [96] G. Dong, Y. Tang, and Y. F. Zhao, “A survey of modeling of lattice structures fabricated by additive manufacturing,” J. Mech. Des. Trans. ASME, vol. 139, no. 10, 2017. [97] X. Zheng et al., “Ultralight, ultrastiff mechanical metamaterials,” Science (80-. )., vol. 344, no. 6190, pp. 1373–1377, 2014. [98] P. K. Misra, Physics of Condensed Matter. Elsevier, 2012. [99] N. E. Mealy and M. Bayés, “Asm-8,” Drugs Future, vol. 30, no. 1, p. 63, 2005. [100] B. K. Nagesha, V. Dhinakaran, M. Varsha Shree, K. P. Manoj Kumar, D. Chalawadi, and T. Sathish, “Review on characterization and impacts of the lattice structure in additive manufacturing,” Mater. Today Proc., vol. 21, no. xxxx, pp. 916–919, 2020. [101] M. McMillan, M. Jurg, M. Leary, and M. Brandt, “Programmatic Lattice Generation for Additive Manufacture,” Procedia Technol., vol. 20, no. January 2016, pp. 178–184, 2015. [102] W. Tao and M. C. Leu, “Design of lattice structure for additive manufacturing,” Int. Symp. Flex. Autom. ISFA 2016, no. August, pp. 325–332, 2016. [103] J. Feng, J. Fu, Z. Lin, C. Shang, and B. Li, “A review of the design methods of complex topology structures for 3D printing,” Vis. Comput. Ind. Biomed. Art, vol. 1, no. 1, pp. 1–
86 16, 2018. [104] P. Jorge, in Virtual and Physical. . [105] “Triply Periodic Minimal Surfaces.” [Online]. Available: http://facstaff.susqu.edu/brakke/evolver/examples/periodic/periodic.html. [Accessed: 08- Jan-2021]. [106] R. Gümrük and R. A. W. Mines, “Compressive behaviour of stainless steel micro-lattice structures,” Int. J. Mech. Sci., vol. 68, pp. 125–139, 2013. [107] D. W. Abueidda, M. Elhebeary, C. S. (Andrew) Shiang, S. Pang, R. K. Abu Al-Rub, and I. M. Jasiuk, “Mechanical properties of 3D printed polymeric Gyroid cellular structures: Experimental and finite element study,” Mater. Des., vol. 165, p. 107597, 2019. [108] D. J. Yoo, “Computer-aided porous scaffold design for tissue engineering using triply periodic minimal surfaces,” Int. J. Precis. Eng. Manuf., vol. 12, no. 1, pp. 61–71, 2011. [109] G. Dong, D. Tessier, and Y. F. Zhao, “Design of shoe soles using lattice structures fabricated by additive manufacturing,” Proc. Int. Conf. Eng. Des. ICED, vol. 2019-Augus, no. August, pp. 719–728, 2019. [110] K. Lee, “2008 International Symposium on Flexible Automation,” vol. 2008, pp. 1–8, 2008. [111] Y. M. Shabana, N. Noda, and K. Tohgo, “Elasto-Plastic Thermal Stresses in Functionally Graded Materials Considering Microstructure Effects,” Curr. Adv. Mech. Des. Prod. VII, pp. 223–231, 2000. [112] M. A. Wettergreen, B. S. Bucklen, B. Starly, E. Yuksel, W. Sun, and M. A. K. Liebschner, “Creation of a unit block library of architectures for use in assembled scaffold engineering,” CAD Comput. Aided Des., vol. 37, no. 11, pp. 1141–1149, 2005. [113] S. Hyun, A. M. Karlsson, S. Torquato, and A. G. Evans, “Simulated properties of Kagomé and tetragonal truss core panels,” Int. J. Solids Struct., vol. 40, no. 25, pp. 6989–6998, 2003. [114] M. Abdelhamid and A. Czekanski, “Impact of the lattice angle on the effective properties of the octet-truss lattice structure,” J. Eng. Mater. Technol. Trans. ASME, vol. 140, no. 4, pp. 1747–1769, 2018. [115] H. N. G. Wadley, “Multifunctional periodic cellular metals,” Philos. Trans. R. Soc. A Math. Phys. Eng. Sci., vol. 364, no. 1838, pp. 31–68, 2006.
87 [116] H. E. Pettermann and J. Hüsing, “Modeling and simulation of relaxation in viscoelastic open cell materials and structures,” Int. J. Solids Struct., vol. 49, no. 19–20, pp. 2848– 2853, 2012. [117] I. Maskery, A. O. Aremu, L. Parry, R. D. Wildman, C. J. Tuck, and I. A. Ashcroft, “Effective design and simulation of surface-based lattice structures featuring volume fraction and cell type grading,” Mater. Des., vol. 155, pp. 220–232, 2018. [118] Y. Wang, “Periodic surface modeling for computer aided nano design,” CAD Comput. Aided Des., vol. 39, no. 3, pp. 179–189, 2007. [119] J. C. Dinis et al., “Open Source Software for the Automatic Design of Scaffold Structures for Tissue Engineering Applications,” Procedia Technol., vol. 16, pp. 1542–1547, 2014. [120] “Body Centered Cubic Structure (BCC) | MATSE 81: Materials In Today’s World.” [Online]. Available: https://www.e-education.psu.edu/matse81/node/2132. [Accessed: 17-Sep-2020]. [121] P. Platek, J. Sienkiewicz, J. Janiszewski, and F. Jiang, “Investigations on mechanical properties of lattice structures with different values of relative density made from 316L by selective laser melting (SLM),” Materials (Basel)., vol. 13, no. 9, 2020. [122] M. Ross, “Schwarz’ P and D surfaces are stable,” Differ. Geom. its Appl., vol. 2, no. 2, pp. 179–195, 1992. [123] M. Iqbal Mohammed, “Design and fabrication considerations for three dimensional scaffold structures,” KnE Eng., vol. 2, no. 2, p. 120, 2017. [124] J. Shin et al., “Finite element analysis of Schwarz P surface pore geometries for tissueengineered scaffolds,” Math. Probl. Eng., vol. 2012, no. June 2015, 2012. [125] “Neovius_surface @ wikivisually.com.” . [126] Robert Ferreol, “Neovius surface,” 2017. [Online]. Available: https://mathcurve.com/surfaces.gb/neovius/neovius.shtml. [Accessed: 17-Sep-2020]. [127] F. N. Habib, P. Iovenitti, S. H. Masood, and M. Nikzad, “Fabrication of polymeric lattice structures for optimum energy absorption using Multi Jet Fusion technology,” Mater. Des., vol. 155, no. 2017, pp. 86–98, 2018. [128] I. Maskery et al., “An investigation into reinforced and functionally graded lattice structures,” J. Cell. Plast., vol. 53, no. 2, pp. 151–165, 2017. [129] M. F. Ashby, “The properties of foams and lattices,” Philos. Trans. R. Soc. A Math. Phys.
88 Eng. Sci., vol. 364, no. 1838, pp. 15–30, 2006. [130] M. Leary et al., “Inconel 625 lattice structures manufactured by selective laser melting (SLM): Mechanical properties, deformation and failure modes,” Mater. Des., vol. 157, no. 2017, pp. 179–199, 2018. [131] L. Warnet and P. E. Reed, “Falling Weight Impact Testing Principles,” pp. 66–70, 1999. [132] A. Beharic, R. Rodriguez Egui, and L. Yang, “Drop-weight impact characteristics of additively manufactured sandwich structures with different cellular designs,” Mater. Des., vol. 145, no. 2017, pp. 122–134, 2018. [133] R. S. Lakes, “Cellular solids,” Journal of Biomechanics, vol. 22, no. 4. p. 397, 1989. [134] I. Maskery et al., “Insights into the mechanical properties of several triply periodic minimal surface lattice structures made by polymer additive manufacturing,” Polymer (Guildf)., vol. 152, pp. 62–71, 2018. [135] A. S. Dalaq, D. W. Abueidda, and R. K. Abu Al-Rub, “Mechanical properties of 3D printed interpenetrating phase composites with novel architectured 3D solid-sheet reinforcements,” Compos. Part A Appl. Sci. Manuf., vol. 84, pp. 266–280, 2016. [136] C. Yan, L. Hao, A. Hussein, and P. Young, “Ti-6Al-4V triply periodic minimal surface structures for bone implants fabricated via selective laser melting,” J. Mech. Behav. Biomed. Mater., vol. 51, pp. 61–73, 2015. [137] C. Yan, L. Hao, A. Hussein, P. Young, J. Huang, and W. Zhu, “Microstructure and mechanical properties of aluminium alloy cellular lattice structures manufactured by direct metal laser sintering,” Mater. Sci. Eng. A, vol. 628, pp. 238–246, 2015. [138] K. Ushijima, W. J. Cantwell, R. A. W. Mines, S. Tsopanos, and M. Smith, “An investigation into the compressive properties of stainless steel micro-lattice structures,” J. Sandw. Struct. Mater., vol. 13, no. 3, pp. 303–329, 2011. [139] S. N. Khaderi, V. S. Deshpande, and N. A. Fleck, “The stiffness and strength of the gyroid lattice,” Int. J. Solids Struct., vol. 51, no. 23–24, pp. 3866–3877, 2014. [140] G. Maliaris, I. T. Sarafis, T. Lazaridis, A. Varoutoglou, and G. Tsakataras, “Random lattice structures. Modelling, manufacture and FEA of their mechanical response,” IOP Conf. Ser. Mater. Sci. Eng., vol. 161, no. 1, 2016. [141] A. Seharing, A. H. Azman, and S. Abdullah, “A review on integration of lightweight gradient lattice structures in additive manufacturing parts,” Adv. Mech. Eng., vol. 12, no. 6, pp. 1–21, 2020.
89 [142] C. Borsellino and G. Di Bella, “Paper-reinforced biomimetic cellular structures for automotive applications,” Mater. Des., vol. 30, no. 10, pp. 4054–4059, 2009. [143] E. Frulloni, J. M. Kenny, P. Conti, and L. Torre, “Experimental study and finite element analysis of the elastic instability of composite lattice structures for aeronautic applications,” Compos. Struct., vol. 78, no. 4, pp. 519–528, 2007. [144] Z. Ozdemir et al., “Energy absorption in lattice structures in dynamics: Experiments,” Int. J. Impact Eng., vol. 89, pp. 49–61, 2016. [145] D. W. Abueidda, M. Bakir, R. K. Abu Al-Rub, J. S. Bergström, N. A. Sobh, and I. Jasiuk, “Mechanical properties of 3D printed polymeric cellular materials with triply periodic minimal surface architectures,” Mater. Des., vol. 122, pp. 255–267, 2017. [146] S. Singh, A. Sachdeva, and V. S. Sharma, “Investigation of Dimensional Accuracy/Mechanical Properties of Part Produced by Selective Laser Sintering,” Int. J. Appl. Sci. Eng. Int. J. Appl. Sci. Eng, vol. 10, no. 10, pp. 59–68, 2012. [147] Q. Wang, Z. Yang, Z. Lu, and X. Li, “Mechanical responses of 3D cross-chiral auxetic materials under uniaxial compression,” Mater. Des., vol. 186, p. 108226, 2020. [148] W. A. Y. Yusoff, D. T. Pham, and K. D. Dotchev, “The Impact of Employing Different Quality PA2200 Powder Grades to Shrinkage on Sintered Part in Selective Laser Sintering Process,” Appl. Mech. Mater., vol. 789–790, pp. 126–130, 2015. [149] S. Gümüs et al., “Failure behavior of PA12 based SLS lattice structure with macroporosity,” MATEC Web Conf., vol. 188, 2018. [150] L. Bai et al., “Mechanical properties and energy absorption capabilities of functionally graded lattice structures: Experiments and simulations,” Int. J. Mech. Sci., vol. 182, no. April, p. 105735, 2020. [151] A. C. Lopes, Á. M. Sampaio, C. S. Silva, and A. J. Pontes, “Study and evaluation of different combinations of virgin and processed PA material for Selective Laser Sintering technology,” 8th Int. Conf. Polym. Mould. Innov., 2018. [152] Q. M. Li, I. Magkiriadis, and J. J. Harrigan, “Compressive strain at the onset of densification of cellular solids,” J. Cell. Plast., vol. 42, no. 5, pp. 371–392, 2006.