Full text
Depósito de investigación de la Universidad de Sevilla https://idus.us.es/ "This document is the Accepted Manuscript version of a Published Work that appeared in final form in ACS Catalysis, copyright © American Chemical Society after peer review and technical editing by the publisher. To access the final edited and published work see https://doi.org/10.1021/cs100116m
Modifying the size of Nickel metallic particles by H2/CO treatment in Ni/ZrO2 methane dry reforming catalysts Journal: ACS Catalysis Manuscript ID: Draft Manuscript Type: Article Date Submitted by the Author: n/a Complete List of Authors: Caballero, Alfonso; University of seville, Inorganic Chemistry Gonzalez, Victor; CSIC Holgado, Juan; CSIC Pereñiguez, Rosa; CSIC Ternero, Fatima; CSIC ACS Paragon Plus Environment ACS Catalysis
1 Modifying the size of Nickel metallic particles by H2/CO treatment in Ni/ZrO2 methane dry reforming catalysts Victor M. Gonzalez-Delacruz, Rosa Pereñiguez, Fatima Ternero, Juan P. Holgado and Alfonso Caballero* Instituto de Ciencia de Materiales de Sevilla (CSIC-University of Seville) and Departamento de Quimica Inorganica, University of Seville. Avda. Américo Vespucio, 49. 41092. Seville, Spain. [email protected] Abstract The effect of a reduction process with CO or H2 on the size of nickel particles in Ni/ZrO2 dry methane reforming catalysts have been studied by means of in situ XAS and DRIFTS spectroscopies. Our results clearly indicate that a high temperature treatment with CO increases the dispersion of the nickel metallic phase. XAS results have shown a lower coordination number of Ni in the sample treated with CO than that reduced with H2. From the DRIFTS results, it can be established that, under the CO treatment, the formation of Ni(CO)4 complexes corrodes the nickel particles, decreasing their size. The formation of these gas molecules occurs without measurable losses of nickel from the catalyst which maintains the same nickel content after the hydrogen or the CO treatment at high temperature. Therefore, this airborne nickel compound, by colliding with the zirconia surface, must deposit the nickel metal atoms around onto the support. This behavior is an evidence of an important interaction between nickel and zirconia surface as unlike other supports, there is no losses of nickel during the dispersion process on zirconia. Although different effects of CO on nickel catalysts have been previously described, we have found for the first time several experimental evidences demonstrating the whole redispersion phenomenon. Keywords: Nickel catalysts, XAS, FTIR, DRIFTS, Dispersion, Dry methane reforming, Reduction with CO. 1. Introduction Reforming of methane is at present one of the most important industrial reactions, partially due to the huge reserves of natural gas [1,2]. Nowadays, Ni-based catalysts continue as the best economic and performing catalytic systems for this kind of hydrocarbon reforming reactions [3-5], and in particular for the steam reforming of Page 1 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
2 methane, which has been proposed as the source for hydrogen production [6]. Beside this reaction, the dry reforming of methane, using carbon dioxide as oxidant, has been lately extensively studied as an alternative, even though it has been pointed out as impractical for commercial hydrogen generation [7]. In spite of that, there is a great potential in the application of CO2 reforming of methane in environmental areas, such as the elimination of CO2 emissions from natural gas deposits or the utilization of these two greenhouse gases for obtaining synthesis gas (CO/H2) [8,9] which, in different proportions, is extensively used in industrial processes as methanol synthesis, hydrogenations or Fischer–Tropsch reactions [10]. However, these kinds of Ni-based materials are very sensitive to the coke deposition during reaction, which hinders their use as a long term catalyst in industrial applications. Several papers have stated that the dispersion, morphology and interaction of the nickel metallic phase with the support strongly determine the catalytic performances of these catalysts [11-14]. In general, it has been established the difficulty in preparing Ni-based catalysts of appropriate dispersion and stability. As fresh nickel catalysts usually present the oxide phase, a previous reduction process is needed to obtain the catalytic active phase of nickel before performing the reaction. This previous step, essential for obtaining an appropriate final dispersion of the reduced metallic phase, is therefore one of the most important stages in the preparation process. As the pretreatment of the catalysts with H2 is the most common process of reduction, Ni-based catalysts have been extensively studied during this process showing in some cases the existence of strong interactions between the Ni particles and the support [13,15]. On the other hand, a number of previous investigations have shown that under certain conditions, CO corrosively interacts with metallic nickel, causing changes on the metal particles sizes and even some nickel loss from the catalyst surface [16]. This effect is especially relevant in hydrocarbon reforming reactions, as beside hydrogen, CO is formed as a product. Sintering of the Ni particles during treatments with CO has also been reported by some authors [16–19]. All these effects have been assumed to be caused by nickel transport from particle to particle in the form of nickel sub/tetracarbonyls which migrate either on the support surface or through the gas phase, leading to the metal particles growth. In this work, we have studied the effect of two different processes of reduction, with H2 or with CO, in the metallic particle sizes of two different Ni/ZrO2 catalysts active for the dry reforming reaction of methane. The use of different characterization techniques, as XRD, SEM Page 2 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
3 and in situ XAS and DRIFTS, has allowed us to determine and compare the relative size of the nickel particles achieved by the two different reduction processes. 2. Experimental Catalysts preparation Two different nickel loadings were used to obtain diverse particles size and metal dispersions. A 26%wt Ni/ZrO2 and a 3%wt Ni/ZrO2 catalytic systems were prepared as powder by impregnation of a monoclinic zirconia support with a nickel nitrate solution (Ni(NO3)2·6H2O from Aldrich). Zirconia support was synthesized via forced hydrolysis [20] using an aqueous solution of ZrO(NO3)2·xH2O (from Aldrich). The powder was calcined at 850ºC during 3 hours to prevent any change on the support under reaction temperatures. Temperature Programmed Reduction (TPR) TPR experiments were done from room temperature up to 500 ◦C, with a heating rate of 10 ºC/min, holding temperature at 500ºC for 1 hour. A thermal conductivity detector (TCD), previously calibrated using CuO, and a mass spectrometer in line with the TCD, calibrated with reference mixtures, were used to detect variations of reducing agent concentration, and possible sub-products formation. A H2/Ar mixture (5% H2, 50 ml/min flow) was used for H2-reduction, while reduction with CO was accomplished with a 5% CO/He mixture. All the experimental conditions were chosen to assure that no peak coalescence occurs [21]. Catalytic activity tests Reaction was carried out in a fixed-bed tubular reactor described elsewhere [22], using 40 mg of catalysts between two pompons of quartz wool. Before reaction, samples were reduced with CO or H2 at 500ºC during 1 hour. The CH4 and CO2 reactants were mixed at a ratio of 1 diluted in He (10:10:80 in volume). Samples were heated from room temperature up to 750 ◦C at 1◦C/min rate, held at 750 ◦C during 12 h, and finally cooled down to room temperature in the same reaction mixture. Reactants and products were analyzed by means of a gas chromatograph (Varian, CP-3800) equipped with a thermal conductivity detector (TCD) and a Porapak Q packed column. X-ray diffraction (XRD) and Scanning electron microscopy (SEM) Page 3 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
4 X-ray diffractograms were recorded in a Panalytical XPert PRO device, equipped with a X’Celerator Detector (active range of 2θ = 2.18º), with a Bragg- Brentano configuration, using CuKα (λ =1.5418 A). Diagrams were collected in the range 2θ = 20º-80º, with a step of 0.05º and an acquisition time of 80 s for each point. To calculate the mean size of the crystalline particles of Nickel and nickel oxide by Scherrer formula, X-ray diffractograms were also collected in the range of 2θ = 35º-55º, with a step of 0.03º during 100 s each point. SEM images were obtained in a Hitachi S- 5200 microscopy equipped with a field emission filament, using an accelerating voltage of 5 kV. X-ray absorption spectroscopy X-ray absorption spectra (XAS) were recorded at the BM25 beam line (SPLINE) of the ESRF synchrotron (Grenoble, France). The spectra were acquired in transmission mode, using self-supported wafers of the Ni/ZrO2 sample, in a modified commercial infrared cell (Specac) able to work up to 800ºC under controlled atmosphere [13]. XAS spectra were collected at different temperatures during treatments of the samples. In all cases the self-supported pellets were prepared using the optimum weight to maximize the signal-to-noise ratio in the ionization chambers (log I0/I1 ≈ 1). Mass flow controllers were used for dosing the gases to the cell. The composition of the gas mixtures were similar to that previously used in the TPR experiment during the hydrogen or CO reduction treatments. For energy calibration, a standard Ni foil was introduced after the second ionization chamber (I1) and measured simultaneously. Typical XAS spectra of Ni K-edge were recorded from 8200 to 9100 eV, with a variable step energy value, with a minimum 0.5 eV step across the XANES region. Once extracted from the XAS spectra, the EXAFS oscillations were Fourier transformed in the range 2–11.0 Å−1. Spectra were analyzed using the software package IFEFFIT [23]. The theoretical paths for Ni–Ni and Ni–O species used for fitting the first coordination shell of the experimental data were generated using the ARTEMIS program and the FEFF 7.0 program [24]. The coordination number, interatomic distance, Debye–Waller factor and inner potential correction were used as variable parameters for the fitting procedures. Reference spectra for metallic Ni and NiO were recorded using standard reference samples. Diffuse Reflectance FTIR Spectroscopy (DRIFTS) Page 4 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
5 FTIR spectra were collected in a FTIR JASCO 6300 equipped with a Praying Mantis DRIFTS cell, using a reaction chamber able to work up to 600ºC under controlled atmosphere. Mass flow controllers were utilized for dosing the gases to the chamber, passing through the powder sample. FTIR spectra were collected in the range of 4000-700 cm-1 with a resolution of 4 cm-1 and 100 scans each. Spectra were acquired at different temperatures during the “in situ” treatment of the sample. 3. Results and discussion 3.1. Temperature Programmed Reduction (TPR) The processes of reduction of the 26 wt% Ni/ZrO2 catalyst with H2 or CO were studied by TPR experiments. According to the data obtained by these experiments, depicted in Figure 1, the main reduction peaks are similar in shape, in both cases centered around 400ºC. The total H2 consumption until 500ºC roughly corresponds to that expected for the complete reduction of the NiO phase to metallic Ni0. However, when reduced with CO, the consumption of this reducing agent is much higher than expected, mainly due to the presence of a wide new peak around 500ºC. As a subsequent oxidation treatment produces a large amount of CO2, this peak must be due to the decomposition of CO through the Boudouard reaction (2CO C + CO2). In fact, as it will be shown in section 3.4, the SEM images obtained after this CO treatment confirm the presence of carbon in the CO-reduced catalyst, which is completely eliminated by oxidation at 500ºC. 3.2. Catalytic activity in the dry reforming reaction of methane (DRM) We have studied the catalytic performance of the catalysts after the two different reduction processes, with H2 or CO, respectively, in the DRM reaction. Both 26 wt% Ni/ZrO2 samples were studied for the DRM at 750ºC using an GHSV of 1.5 × 105 L/(kg· h). First of all, it is important to remark that, as verified by SEM (images not shown), under these reaction conditions, the carbon initially formed during the reduction process with CO is eliminated through the inverse Boudouard reaction (C + CO2 2CO) using the CO2 from the gas mixture during the heating ramp. That means that initially at 750ºC, the catalyst surface must be free of carbon. As shown in Figure 2, the catalytic performance strongly depends on the reduction treatment. Although the initial activity is roughly the same in both systems, the catalyst previously reduced with Page 5 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
6 CO presents a much higher stability, especially after 9 hours in reaction conditions. After 12 hours in reaction, this system loses just a 20% of the initial methane conversion, while the same catalyst reduced in hydrogen loses a 40% of activity after the same period of time. In all cases, the selectivity was stable, with values of ca 0.90 for the H2/CO ratio, close to thermodynamic values for this reaction at that temperature. As mentioned before, several factors can influence the catalytic activity of Nicatalysts in hydrocarbon reforming reactions. Between them, the dispersion of the nickel metallic phase is one of the most important variables affecting the catalytic performances. In order to characterize the size of the nickel metallic particles, we have studied the catalysts by means of XRD and XAS after being reduced with hydrogen and CO, respectively. 3.3. X-Ray Diffraction (XRD) The crystalline phases present in the original and the reduced 26 wt% Ni/ZrO2 catalyst were analyzed using X-Ray diffraction. Oxidized sample after CO reduction has also been measured to compare with the original sample. XRD patterns of every sample contain the peaks characteristic of the monoclinic structure of ZrO2 (Figure 3), with no relevant differences between them. The main peaks corresponding to the Ni phases (oxidized and reduced) are also displayed in Figure 3. The peak at 2θ of 43.4º is characteristic of the cubic structure of NiO phase (calcined and reoxidized samples), while catalysts after CO or H2 treatment present a peak at 2θ of 44.5º, corresponding to the cubic structure of metallic Ni phase. No other nickel phases are detected by XRD measurements. The size of the particles has been estimated from these diagrams by applying the Scherrer equation [25]. The crystalline size of the ZrO2 phase is around 20nm for all the samples, with no changes after the reducing and oxidizing treatments. This is not the case for the Ni particles, where significant changes have been observed in the particle sizes as a function of the reduction treatment. As it can be seen in Table 1, the original nickel oxide particles present a diameter of 48nm. After reduction treatment, the size of the CO reduced nickel particles has decreased to 32 nm (-33%), while the reduction with hydrogen roughly maintains the initial size of the nickel particles. Moreover, this effect seems to be permanent, as after re-oxidation of the CO-reduced sample, a similar size (31nm) is obtained for the NiO particles, lower than the original ones. Page 6 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
7 3.4. Scanning Electron Microscopy (SEM) In order to further figure out the effect of the treatment with CO decreasing the size of the metallic Ni particles, a study by scanning electron microscopy has been accomplished after the successive treatments with H2, CO and oxygen. As shown in the SEM images included in Figure 4, the original sample present two different kinds of particles. The round shape particles, with a size around 20 nm that according to the XRD data must correspond to the ZrO2 phase, and the bigger ones, with an octahedral shape, related with the NiO phase. After H2 treatment at 500ºC, the Ni particles appear rounded but with a similar or slight lower size that the original NiO phase. However, after CO reduction at 500ºC, these octahedral particles evolved in smaller rounded entities, showing that the CO treatment corrodes the nickel particles, decreasing the size of the original crystallites. Besides, it is apparent the formation of carbon fibers over the catalyst, that confirming the decomposition of CO via the Boudouard reaction as previously deduced from the TPR results. After the reoxidation treatment with O2 at 500ºC, these carbon fibers disappear, without noticeable change in the shapes and sizes of the Ni/NiO particles, in agreement with the results obtained by XRD. At this point, it must be noted that the quantitative analysis of the nickel content by ICP-MS after the reduction treatment with CO and subsequent oxidation at 500ºC, shows the same nickel content on all the samples, meaning that no losses of this metal has occurred during the treatment with CO. 3.5. X-Ray Absorption Spectroscopy (XAS) The Ni particles of the 26 wt% Ni/ZrO2 system have also been characterized by in situ X-Ray Absorption during the reduction processes with CO and H2 at 500ºC. In both cases, the spectra were collected in situ, in contact with reactive gases, after cooling down to room temperature. Ni K-edge XANES spectra obtained after the different treatment are displayed in Figure 5, where also a Ni foil spectrum has been included as a reference. The original sample presents a white line and pre-edge features similar to the massive NiO compound used as a reference (not shown). Accordingly, the XANES spectra obtained after CO and hydrogen treatment roughly correspond to a metallic nickel phase, showing that the original NiO phase has been completely reduced to Ni0, in agreement with the TPR experiments (Figure 1) and with previous results on similar catalytic systems [13]. Even though an important carbon formation has been detected after CO treatment (Figure 4), no features from nickel carbides or related Page 7 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
14 treatments. All the spectra have been collected after cooling down at room temperature in contact with the gas phase. Figure 7. Fourier transform functions of the EXAFS oscillations (without phase correction) obtained for the 3 wt% Ni/ZrO2 sample submitted to the different reduction treatments. All the spectra have been collected after cooling down at room temperature in contact with the gas phase. Figure 8. FTIR spectra of the 3 wt% Ni/ZrO2 sample during reduction treatment with CO. All the spectra have been collected at the indicated temperature, in contact with the gas phase. Solid lines: Spectra under CO atmosphere (Gas mixture: 5% CO/Ar). Dash: Spectra after CO evacuation. Scheme 1. Schematic evolution of the shape of the nickel particles submitted to a reducing treatment with CO. 1) NiO particle; 2) CO molecules react with Oxygen atoms of NiO producing CO2. 3) When the Particle is partially reduced, some CO molecules form tetracarbonyls with nickel atoms, depositing the metal atoms around onto the support. 4) Finally, metallic particles of Ni show a smaller size than the original particle of NiO. Table 1. Crystalline size of the NiO and Ni phases in the 26 wt% Ni/ZrO2 system after the indicated treatments, calculated from XRD results by applying the Scherrer equation. Table 2. Structural parameters for Ni obtained by fitting analysis of the EXAFS spectra of 26 wt% Ni/ZrO2 catalyst submitted to the indicated treatments. Table 3. Structural parameters for Ni obtained by fitting analysis of the EXAFS spectra of 3 wt% Ni/ZrO2 catalyst submitted to the indicated treatments. Page 14 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
15 Table 1 Crystalline size (nm) 26wt% Ni/ZrO2 NiO Ni Calcined 48 -- H2-reduced -- 46 CO-reduced -- 32 Oxidized after CO reduction 31 -- Table 2 26wt% Ni/ZrO2 Ni-Ni (Å) C.N. D-W factor (Å2x10-3) ∆E0 (eV) H2-reduced 2.48 12.0 5 5.8 CO-reduced 2.49 12.0 6 -6.8 Ni foil 2.48 12.0 5 6.7 Estimated errors: Interatomic distance, < ±0.02A; Coordination number (C.N.), < ±10% Table 3 3wt% Ni/ZrO2 Ni-Ni (Å) C.N. D-W factor (Å2x10-3) ∆E0 (eV) H2-reduced 2.50 11.8 6 -7.0 CO-reduced 2.49 10.2 9 -2.3 Ni foil 2.48 12.0 5 6.7 Estimated errors: Interatomic distance, < ±0.02A; Coordination number (C.N.), < ±10% Page 15 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
16 Table of Contents (TOC) graphic 1) CO 2 2) 3) 4) CO Ni O Ni(CO)4 Page 16 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
61x47mm (600 x 600 DPI) Page 17 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
62x48mm (600 x 600 DPI) Page 18 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
61x47mm (600 x 600 DPI) Page 19 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
Page 20 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
56x39mm (600 x 600 DPI) Page 21 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
56x39mm (600 x 600 DPI) Page 22 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60
56x39mm (600 x 600 DPI) Page 23 of 25 ACS Paragon Plus Environment ACS Catalysis 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60