THERMO-MECHANICAL PROPERTIES OF MATERIALS FOR FUEL CELLS PhD Thesis presented by Desirée Ciria Matamoros To obtain the Doctor’s degree from Université Paris-Saclay Speciality « Physics » And Universidad de Sevilla Speciality «Science and Technology of New Materials » Gif sur Yvette, 06 November 2017 Composition of the jury M. Alfonso Bravo León Professor, Universidad de Sevilla, Spain M. Tor Grande Professor, Norwegian University of Science and Technology, Norwey M. Pierre-Marie Geffroy Chargé de Recherche - CRNS, France Mme. Veronique Aubin Professor, Université Paris-Saclay, France M. Guilhem Dezanneau Head of SPMS Laboratory, Université Paris-Saclay, France Supervisor M. Manuel Jiménez Melendo Professor, Universidad de Sevilla, Spain Supervisor
3 ACKNOWLEDGEMENTS On the one hand, I would like to express my gratitude to the following people from CentraleSúpelec who have kindly helped me in my research and in the preparation of this thesis. To begin with, my deepest thanks and sincere appreciation to my supervisors. I would like to say a big thank you to Dr. Guilhem Dezanneau, my thesis director in France, for giving me the opportunity to continue working in research, for guiding me during this work, for his kind attention, patience, comprehension and invaluable help with my personal and professional issues. Thank you Guilhem for everything. A very special thanks to Dr. Veronique Aubin, for her encouragement, helpful advice, great help and for the time devoted to carrying out the simulations and discussing the results. I would like to thank all members of SPMS and MSSMAT laboratory, for their technical help and support. Moreover, I would particularly like to thank Nicolas Roubier for his total availability, his endless help and kind attention; Eva Heripre for her ideas, cooperation and time; Christine Vinée-Jacquing for her thoughtful attention and help. And my heartfelt gratitude goes to Xavier Brill for his kindness, constant help and for his friendship. I am also thankful to all PhD students from both laboratories, especially to Anastasia, Charles, Charlotte, Fabien, Gilles, Halyna and Michael for their kind assistance and suggestions. A special thanks to Chen Yi for our talks, walks and dinners, for his trust, his support and for the time we spent together. Come on Chen Yi! And naturally, thank you to Cintia, my companion from the start, with whom I have shared every minute of this PhD. I must thank you for always trusting me, for your company, your constant help, support and understanding, for the moments we spent together and for making this hard journey more pleasant. It wasn’t easy my friend, but we managed it in the end. Without you, this adventure would never have been the same. Thanks for everything. I also wish to express my sincere gratitude to Florencia Mariscal for opening up her home to me when I arrived in Paris, for offering me her selfless assistance at all times, for her amiable, friendly treatment and for her incredible human qualities. I have no words to thank you for so much generosity, I was so fortunate to have you with me.
4 On the other hand, I would also like to extend my heartfelt gratitude to the following people from the University of Sevilla who have helped and contributed to making this work possible. En primer lugar, mi más sincero agradecimiento al Dr. Manuel Jiménez-Melendo, mi director de tesis en España, por haber confiado en mí, por su infinita paciencia y ayuda, por el constante apoyo y ánimo que me ha brindado desde el principio, y por su total disponibilidad. Asimismo, he de agradecerle por sus enseñanzas, por los largos días de trabajo en el laboratorio, por el tiempo dedicado a discutir los resultados y preparar esta memoria, y por el enorme compromiso que tiene con su trabajo. Con su entusiasmo, generosidad, profesionalidad y cercanía ha sido un auténtico placer poder trabajar a su lado. Al Dr. Alfonso Bravo León por su amabilidad, por sus sugerencias e ideas siempre acertadas y por el tiempo dedicado a aclarar algunas dudas de este trabajo. Agradecer también a todos los miembros del grupo de investigación de Materiales Biomiméticos y Multifuncionales y del CITIUS por su tiempo, paciencia y colaboración, en especial al Dr. Joaquín Ramírez por su trato amable y su ayuda. Al Dr. Javier Quispe por su gran ayuda, por mostrarse siempre solícito y por su amistad. A Carmen, Antonio, Pilar, Fredy y Saúl por su atención, ayuda y por el tiempo que hemos compartido. Además quiero expresar especialmente mi gratitud a Aurora por sus consejos, su paciencia, su ayuda y su generosidad. Y como no a Rafa, mi compañero de laboratorio, estancias, congresos y piso, hemos vivido un poco de todo juntos y quiero darte las gracias por haber estado siempre ahí, nada hubiera sido lo mismo sin ti. Además agradeceros a todos por el extraordinario ambiente de amistad, ya que es muy estimulante trabajar en unas condiciones tan agradables. A Nuria, Marta, Carmen Y Rosana, con las que coincidí por casualidad en algún congreso o estancia y enseguida nos hicimos inseparables. Gracias chicas por esas horas y horas de conversaciones y de paseos turísticos, por vuestra compañía y por vuestra amistad. A mis amigos Kiko, Juan, Fati, Almudena, Miguelón, Bea y Alex, por estar siempre a mi lado, por vuestras reconfortantes visitas, por vuestra compresión y por vuestra valiosa amistad. Agradecer también a Nikki por su tiempo y su ayuda. Y a Pilar por su amabilidad, por su compañía, y por los momentos que hemos vivido juntas.
5 Y muy especialmente a mi amigo Víctor por su constante apoyo, por su paciencia, por sus comentarios y sugerencias, y por ofrecerme siempre su ayuda humilde y desinteresada. Gracias amigo. Finalmente, un agradecimiento muy especial merecen mis padres, mi hermana y mis abuelos por creer tanto en mí, por el cariño que siempre me han dado haciendo que les sienta a centímetros incluso estando a miles de kilómetros, por su infinita generosidad y por el ánimo y el apoyo firme e incondicional prestado en todo momento, no sólo a la hora de realizar este trabajo sino a lo largo de mi vida. También he de agradecer a mis tíos, Puri y José, por su constante preocupación, apoyo y ayuda. Y como no a Sofía, que a tu corta edad has sido capaz de entender mis ausencias, sacar lo mejor de mí y mostrarme siempre el lado más dulce de la vida. Yo no sería nada sin vosotros, os quiero.
6
7 CONTENTS Abstract .................................................................................................................................. 13 Résumé ................................................................................................................................... 15 Resumen................................................................................................................................. 17 CHAPTER 1. INTRODUCTION 19 1.1 Fuel cells ..................................................................................................................... 19 1.1.1 Solid Oxide Fuel Cells (SOFCs) ..................................................................................... 20 1.1.2 Electrolyte materials for SOFCs ................................................................................... 22 1.1.2.1 Lanthanum Silicate ........................................................................................... 23 1.1.2.2 Yttrium-doped Barium Zirconate ..................................................................... 24 1.2 Importance of mechanical properties in SOFCs .................................................................. 25 1.2.1 Thermo-elastic properties .......................................................................................... 27 1.2.2 Creep behaviour .............................................................................................................. 28 1.2.2.1 Diffusional creep .............................................................................................. 29 1.2.2.2 Grain boundary sliding ..................................................................................... 31 1.2.2.2.1 Diffusion-accommodated process: Ashby-Verrall model ............... 31 1.2.2.2.2 Dislocation-accommodated process .............................................. 32 1.2.2.3 Interface-reaction creep .................................................................................. 33 1.2.2.3.1 Diffusion creep controlled by interface-reaction ........................... 33 1.2.2.3.2 GBS creep controlled by interface-reaction ................................... 33 1.2.2.4 Phenomenological relationships for superplasticity ........................................ 34 1.2.3 Previous results in SOFC electrolytes ....................................................................... 35 1.2.3.1 Yttria-Stabilised Zirconia ............................................................................ 35 1.2.3.2 Apatites-compounds ................................................................................. 35 1.2.3.3 Proton-conducting compounds ................................................................. 36 1.3 References ..................................................................................................................... 36
Contents 8 CHAPTER 2. PREPARATION OF MATERIALS 47 2.1 Introduction .......................................................................................................................... 47 2.2 Lanthanum Silicate .................................................................................................................. 48 2.2.1 Commercial starting precursors for LSO nanopowders preparation ............................ 49 2.2.2 Freeze-drying synthesis .............................................................................................. 49 2.2.3 Compaction of LSO nanopowders .............................................................................. 51 2.2.4 High temperature sintering ........................................................................................ 51 2.2.4.1 Conventional sintering ............................................................................... 51 2.2.4.2 Spark plasma sintering ............................................................................... 51 2.3 Yttrium-doped Barium Zirconate ...................................................................................... 52 2.3.1 Commercial starting precursors for BZY nanopowders preparation ............................ 53 2.3.2 Modified EDTA-citrate complexing synthesis .............................................................. 53 2.3.3 Compaction of BZY nanopowders ............................................................................... 55 2.3.4 High temperature sintering ........................................................................................ 55 2.3.5 Commercial Yttrium-doped Barium Zirconate ............................................................ 56 NiO-extraction ....................................................................................................... 56 2.4 References .................................................................................................................... 56 CHAPTER 3. STRUCTURAL AND MICROSTRUCTURAL CHARACTERIZATION 61 3.1 Introduction .................................................................................................................... 62 3.2 Characterization techniques ............................................................................................. 62 3.2.1 X-Ray Diffraction .............................................................................................................. 62 3.2.2 Particle size ...................................................................................................................... 64 3.2.3 Density ............................................................................................................................. 64 3.2.4 Electron microscopy analysis ...................................................................................... 64 3.2.4.1 Preparation of samples .................................................................................... 65 3.2.4.2 Morphological parameters .............................................................................. 65 3.2.4.2.1 Grain size ........................................................................................ 65 3.2.4.2.2 Form factor ..................................................................................... 67 3.2.4.2.3 Orientation angle ............................................................................ 67 3.3 Experimental results ........................................................................................................ 68 3.3.1 Lanthanum Silicates ......................................................................................................... 68 3.3.1.1 Density ............................................................................................................. 68 3.3.1.2 X-Ray Diffraction analysis ................................................................................. 68
Contents 9 3.3.1.3 Particle size ...................................................................................................... 70 3.3.1.4 Microstructural analysis ................................................................................... 72 3.3.2 Yttrium-doped Barium Zirconate ................................................................................ 75 3.3.2.1 Density ............................................................................................................. 75 3.3.2.2 X-ray diffraction analysis .................................................................................. 75 3.3.2.3 Particle size ...................................................................................................... 78 3.3.2.4 Microstructural analysis ................................................................................... 79 3.3.3 Yttrium-doped Barium Zirconate after NiO-extraction ................................................ 82 3.3.3.1 Density ............................................................................................................. 82 3.3.3.2 X-ray diffraction analysis .................................................................................. 82 3.3.3.3 Microstructural analysis ................................................................................... 85 3.4 References ......................................................................................................................... 87 CHAPTER 4. ROOM-TEMPERATURE MECHANICAL CHARACTERIZATION 91 4.1 Introduction ..................................................................................................................... 91 4.2 Experimental characterization of room-temperature mechanical properties ..................... 92 4.2.1 Experimental procedure ............................................................................................. 92 4.2.1.1 Nanoindentation .............................................................................................. 93 4.2.1.2 Mechanical compression tests with optical imaging ....................................... 95 4.2.1.3 Resonant Ultrasound Spectroscopy ................................................................. 97 4.2.1.4 Microindentation ........................................................................................... 100 4.2.2 Experimental results ...................................................................................................... 101 4.2.2.1 Room-temperature mechanical properties of Lanthanum Silicate ............... 101 4.2.2.1.1 Nanoindentation ........................................................................... 101 4.2.2.1.2 Mechanical compression tests with optical imaging .................... 103 4.2.2.1.3 Resonant Ultrasound Spectroscopy .............................................. 103 4.2.2.1.4 Microindentation .......................................................................... 104 4.2.2.1.5 Comparison of the different techniques ...................................... 105 4.2.2.2 Room-temperature mechanical properties of Y-doped Barium Zirconate .... 105 4.2.2.2.1 Nanoindentation ........................................................................... 105 4.2.2.2.2 Mechanical compression tests with optical imaging .................... 107 4.2.2.2.3 Resonant Ultrasound Spectroscopy .............................................. 108 4.2.2.2.4 Microindentation .......................................................................... 108 4.2.2.2.5 Comparison of the different techniques ...................................... 110
Résumé 16 Ces céramiques denses ont ensuite été caractérisées sur le plan des propriétés mécaniques à différentes températures. Tout d’abord, les propriétés mécaniques des céramiques LSO et BZY ont été évaluées par différentes techniques à température ambiante dans le Chapitre 4. Les méthodes de nanoindentation, de microindentation, de résonance ultrasonore, de tests en compression et la méthode théorique de la théorie de la fonctionnelle densité ont été utilisées afin de déterminer les propriétés élastiques, de dureté et de résistance à la fracture des matériaux obtenus. L’influence de la température sur les propriétés thermoélastiques a été explorée dans le Chapitre 5. Dans ce chapitre, des calculs par éléments finis ont également permis de caractériser l’état de stress résiduel présent au sein de l’oxyapatite après la procédure de frittage ou lors des essais mécaniques. Nous avons ensuite évalué la réponse mécanique des deux matériaux dans des conditions proches de celles de fonctionnement d’une pile i.e. à 700 °C sous atmosphère contrôlée, successivement oxydante et réductrice (Chapitre 6). Ce chapitre est également consacré à l’étude des mécanismes de déformation plastique à haute température et à l’extraction des paramètres de fluage. Finalement, le Chapitre 7 dresse une conclusion regroupant les principaux résultats. Mots clés: Piles à combustible à oxide solide, matériaux d’électrolyte, propriétés mécaniques, fluage
17 RESUMEN Las pilas de combustible de óxido sólido (SOFCs) ofrecen una alternativa real a las tecnologías de producción de electricidad convencionales ya que son más limpias, eficientes y respetuosas con el medio ambiente. Sin embargo, la principal limitación de las SOFC radica en su insatisfactoria durabilidad y fiabilidad debido a las altas temperaturas de funcionamiento y a los ciclos térmicos característicos de estos dispositivos. Actualmente se está realizando una intensa búsqueda de materiales para SOFC con el objetivo de reducir la temperatura de trabajo y superar estas limitaciones. Entre los diferentes candidatos que han surgido, el Silicato de Lantano (LSO) y el Zirconato de Bario dopado con Itrio (BZY) han sido considerados como potenciales alternativas para ser utilizados como electrolitos en pilas de combustible de óxido sólido a temperaturas intermedias. Mientras numerosos estudios se han centrado en la caracterización y optimización de las propiedades microestructurales y electroquímicas de los componentes que forman una SOFC, todavía hay muy pocos trabajos de investigación sobre las propiedades mecánicas y su influencia en la vida útil de una SOFC. La fiabilidad y durabilidad de estos dispositivos no sólo depende de su estabilidad electroquímica, sino también de su capacidad estructural para soportar las tensiones residuales que aparecen en el proceso de fabricación de la pila y tensiones mecánicas que surgen durante la operación. Debido al hecho de que las SOFCs están compuestas por apilamiento de varias celdas individuales y que a su vez estas están constituidas por capas frágiles individuales en íntimo contacto, estas tensiones se originan principalmente por la diferencia entre el coeficiente de dilatación térmica y las propiedades elásticas de capas adyacentes y por la deformación plástica causada por fluencia. La incompatibilidad de tensiones puede provocar el fallo mecánico de una sola celda y tener consecuencias dramáticas en toda la pila. Por lo tanto, el conocimiento de las propiedades mecánicas de cada componente es una cuestión esencial para la integridad mecánica y el desarrollo de las SOFCs (Capítulo 1). El objetivo de esta tesis doctoral es la fabricación y caracterización estructural, microestructural y mecánica del Silicato de Lantano y Zirconato de Bario dopado con Itrio. Con este fin, se prepararon cerámicas de alta densidad (d > 97%) mediante sinterización convencional o asistida por descarga eléctrica pulsada a partir de nanopolvos sintetizados mediante rutas químicas. Los detalles de las rutas de síntesis y las condiciones de sinterización se describen en el Capítulo 2. Los nanopolvos y masivos obtenidos fueron caracterizados estructural y microestructuralmente por difracción de rayos X, análisis de tamaño de partícula por difracción láser y microscopía electrónica de barrido y transmisión en el Capítulo 3.
Resumen 18 Los cerámicos densos se caracterizaron mecánicamente a diferentes temperaturas. En primer lugar, se examinaron las propiedades mecánicas de los compuestos LSO y BZY mediante diferentes técnicas a temperatura ambiente en el Capítulo 4. Nanoindentación, microindentación, espectroscopía de resonancia ultrasónica, ensayos de compresión y cálculos DFT fueron usados para determinar sus constantes elásticas, su dureza y su tenacidad de fractura. A continuación, se estudió la evolución de las propiedades termoelásticas de ambos materiales con la temperatura en el Capítulo 5. En este capítulo también se realizaron simulaciones numéricas de elementos finitos para caracterizar el estado de tensión y predecir la fractura en el Silicato de Lantano. Posteriormente, se evaluó la respuesta mecánica de ambos materiales electrolíticos mediante ensayos mecánicos de compresión a temperaturas de funcionamiento de las pilas de combustible de óxido sólido (700 ° C) y en diferentes atmósferas (Capítulo 6). Además, este capítulo también se dedica al estudio de los mecanismos de fractura y deformación plástica de estos compuestos a alta temperatura por medio de experimentos de fluencia. Finalmente, el Capítulo 7 resume las conclusiones más relevantes derivadas de este trabajo. Palabras clave: Pilas de combustible de óxido sólido, materiales electrolíticos, propiedades mecánicas, fluencia.
19 Chapter 1 INTRODUCTION Contents 1.1 Fuel cells ..................................................................................................................... 19 1.1.1 Solid Oxide Fuel Cells (SOFCs) ................................................................................. 20 1.1.2 Electrolyte materials for SOFCs ............................................................................... 22 1.1.2.1 Lanthanum Silicate ........................................................................................... 23 1.1.2.2 Yttrium-doped Barium Zirconate ..................................................................... 24 1.2 Importance of mechanical properties in SOFCs .................................................................. 25 1.2.1 Thermo-elastic properties ....................................................................................... 27 1.2.2 Creep behaviour ...................................................................................................... 28 1.2.2.1 Diffusional creep .............................................................................................. 29 1.2.2.2 Grain boundary sliding ..................................................................................... 31 1.2.2.2.1 Diffusion-accommodated process: Ashby-Verrall model ......................... 31 1.2.2.2.2 Dislocation-accommodated process ......................................................... 32 1.2.2.3 Interface-reaction creep .................................................................................. 33 1.2.2.3.1 Diffusion creep controlled by interface-reaction ...................................... 33 1.2.2.3.2 GBS creep controlled by interface-reaction .............................................. 33 1.2.2.4 Phenomenological relationships for superplasticity ........................................ 34 1.2.3 Previous results in SOFC electrolytes ...................................................................... 35 1.2.3.1 Yttria-Stabilised Zirconia .................................................................................. 35 1.2.3.2 Apatites-compounds ........................................................................................ 35 1.2.3.3 Proton-conducting compounds ....................................................................... 36 1.3 References ..................................................................................................................... 36 1.1 FUEL CELLS In order to cope with the climate change environmental threat and the exhaustion of fossil fuel reserves, the development of sustainable, more effective and cleaner energy sources becomes in a major global challenge. Among the different solutions, fuel cells have stood out in the last years
Chapter 1. Introduction 20 as one of the most promising alternatives for sustainable energy production and one that is compatible with preservation of the environment [1-3]. They are electro-chemical devices that convert chemical energy present in fuels into electricity and heat. Moreover, fuel cells are the only technology of energy-production potentially fed by renewable fuels which can be used for stationary and mobile applications [4]. The operating principle of a fuel cell is similar to that of a battery in the sense that both generate electrical energy through electrochemical processes, however, in a fuel cell the chemical energy is provided by an oxidant and a fuel supplied from external sources. Therefore fuel cell electricity generation cannot run out while fuel is continuously supplied, in contrast to the characteristic charge - discharge cycles of the batteries [4]. A single fuel cell presents a sandwich type geometry and consists of three main components: cathode, electrolyte and anode. An oxidant and a fuel are fed to the cathode and anode, respectively, where the oxidant is reduced and the fuel oxidized (Figure 1.1). These halfreactions generate a chemical potential gradient of ions from one side of the electrolyte to the other and therefore, direct-current electricity is produced in the external circuit. Figure 1.1. A schematic representation of a working fuel cell. 1.1.1 Solid Oxide Fuel Cells (SOFCs) Among all types of fuel cells, those based on solid oxides have been considered as a leading technology for future power generation. SOFCs have received special interest because of their low levels of pollutant emissions, fuel flexibility and high efficiency [3-5]. Solid Oxide Fuel Cells require oxidant reactants such as air or oxygen, and fuel such as hydrogen to electrochemically react and generate electricity. Schematics representations of SOFCs based on oxide-ion conducting and proton conducting electrolytes are shown in Figure 1.2. In a conventional SOFC utilizing oxide-ion conducting electrolyte, the oxygen is partially reduced at the cathode giving rise to O2- anions which migrate across the electrolyte to the anode side, where they react with H2 to form water and
Chapter 1. Introduction 21 generate an electrical voltage. In Proton Conducting Fuel Cells (PCFCs), hydrogen is oxidized at the anode giving rise to H+ ions that are transported to the cathode side across the proton conducting electrolyte. H+ ions then react with O2 to form water. The main advantage of PCFCs compared to the classical SOFCs lies in the fact that H2O is produced at the cathode instead of at the anode. This allows the hydrogen to be completely utilized without compromising the system overall efficiency [4]. Figure 1.2. Schematic representations of the reactions taking place in a SOFC during operation for (a) oxide-ion conducting electrolyte, and (b) proton conducting electrolyte. In contrast to other fuel-cell types, SOFCs are composed of solid-state ceramics and require operating temperatures ranging between 500 and 1000 °C. The best established SOFC systems are those based on an Yttria-Stabilized Zirconia (YSZ) electrolyte, which requires operating temperatures between 800 - 1000 °C [5-7] to achieve sufficient ionic conductivity in order to assure the efficient transport of O2-. These high operating temperatures are directly linked to the main limitations of SOFCs, which lie mainly in their unsatisfactory durability and reduced lifetime. These problems are caused by the difficulty of maintaining the sealing of the cells, by the too short-term stability of the materials and by the mechanical incompatibility between electrodes and electrolyte due to the thermal cycling to which the SOFCs components are subjected during operation [8]. To overcome such disadvantages, lowering the working temperature to 500 - 700 °C becomes an important challenge in improving SOFC technology. For this purpose, there has been huge interest in the development of new electrolyte materials which exhibit high ion conductivities at intermediate temperatures combined with low electronic conductivity, high density and good chemical stability [3]. a) b)
Chapter 1. Introduction 22 1.1.2 Electrolyte materials for SOFCs In the attempt to search for an alternative to replace YSZ electrolytes, different candidates have emerged. On the one hand, materials science research has been mainly focused on developing new oxygen ion conducting electrolytes for intermediate-temperature solid oxide fuel cells (ITSOFC) [9-11]. In particular, several families of oxide-ion conductors have attracted considerable interest and are being widely investigated; some of them are: fluorite oxides such as Ceria-Gadolinia [12], perovskite oxides such as Strontium and Magnesium doped Lanthanum Gallate [13, 14], LAMOX oxides [15, 16] and apatites such as Lanthanum Silicate [17-20]. On the other hand, protonconducting perovskite materials have recently received increasing attention for SOFC electrolyte applications because of the higher mobility of protons with respect to the oxygen ions , which allows for safe reduction of the operating temperature of SOFCs (450 - 700 °C) without degrading performance [3, 21-24]. The most interesting proton conducting materials for electrolytes are doped Barium Cerate [25-31] and doped Barium Zirconate [21, 22, 24, 32-37]. Figure 1.3 shows a plot of the conductivity of Yttria-Stabilized Zirconia together with the new families of oxide-ion and proton conductors electrolytes discussed above. It can be observed that all the ceramics exhibit higher conductivities than YSZ at temperatures ranging from 500 to 700 °C, what explains the growing interest that these materials have received since they could be successfully used to reduce the SOFC operating temperatures. Figure 1.3. Comparison of (ZrO2)0.92(Y2O3)0.08 (YSZ) total conductivity with others oxide ion and proton conductors electrolytes as a function of temperature [3]: La2Mo2O9 (LAMOX), Ce0.8Gd0.2O1.9 (CGO), La0.9Sr0.1Ga0.8Mg0.2O2.85 (LSGM), La10(SiO4)6O3 (Si-Apatite), BaCe0.9Y0.1O3 (BCY), and BaZr0.8Y0.2O3 (BZY).
Chapter 1. Introduction 23 This thesis was focused on the mechanical characterization of two of these materials: Lanthanum Silicate and Yttrium-doped Barium Zirconate, since their ion conductivities at intermediate temperatures together with the lack of electronic conductivity and chemical stability, required for electrolyte application in SOFC, contributed to the consideration of these compounds as two of the most promising materials to be used as SOFC electrolytes. Their characteristics, crystal structure and ion-conductivity are briefly described below. 1.1.2.1 Lanthanum Silicate Rare-earth-based oxy-apatites La9.33+xSi6O26+3x/2 have been considered as a potential alternative to Yttria-Stabilized Zirconia (YSZ) to be used as electrolyte material for intermediate and low temperature Solid Oxide Fuel Cells due to their high oxide-ion conductivity, chemical stability, thermal properties and low conductivity activation energy [18, 38-40]. The oxy-apatite structure usually shows hexagonal symmetry and can be described in the P63/m space group. It involves two non-equivalent positions for La ions, one for Si, and four positions for O ions (Figure 1.4) [41], where O1 - O3 ions form SiO4 tetrahedra with La2 located in two cavity sites, one 7-coordinated and another 9-coordinated, and O4 ion arranged along the c axis, forming the O4 column along which oxide ions can migrate. These channels are presumed to be responsible for the high oxide ion conduction of this material [42-44]. Figure 1.4. Crystal structure of La9.33Si6O26 oxy-apatite [41]. Lanthanum Silicates with this apatite-type structure are of great interest, exhibiting conductivities even higher than those of the well-known oxide ionic conductor YSZ at intermediate temperatures [17, 20, 42, 45, 46]. For example, Nakayama et al. [18] have reported that the
Chapter 1. Introduction 24 conductivity of Lanthanum Silicates is 4.3 × 10–3 Scm–1 at 500 °C, whereas for YSZ it is 1.1 × 10−3 Scm−1 at 500 °C [5]. 1.1.2.2 Yttrium-doped Barium Zirconate Yttrium-doped Barium Zirconate is another attractive material to be used as electrolyte material for intermediate temperature SOFCs because it combines a high proton conductivity with high chemical stability in CO2 containing atmospheres [21, 26, 47, 48]. Y-substituted Barium Zirconate structure shows a cubic perovskite symmetry, similar to BaZrO3 (Figure 1.5), which can be described in the Pm3 m space group. Yttrium is considered as one of the most suitable dopants for Barium Zirconate to achieve the highest proton conductivity [21, 22, 37] (for doping content up to 20% of Y), presumably as a result of the good matching between Zr4+ and Y3+ ionic radii (0.72 Å and 0.90 Å [49], respectively). The fast proton mobility and the entropic stabilization of protonic defects through water incorporation lead to the high proton conductivity of this material [21, 22, 50]. Figure 1.5. Crystal structure of Barium Zirconate [51]. Electrical measurements of BZY demonstrated very high bulk proton conductivity, in particular, Pergolesi et al. [35] have found that the conductivity of grain boundary-free Yttriumdoped Barium Zirconate thin films is 0.11 S cm−1 at 500 °C. However, the proton conductivities reported in the literature by other authors vary by more than one order of magnitude [52-54]. This poor reproducibility of the conductivity properties is due to the difficulty of fabricating dense compounds [21]. Moreover proton conductivity seems to be strongly affected by grain size, Ba evaporation and secondary phases.
Chapter 1. Introduction 25 1.2 IMPORTANCE OF MECHANICAL PROPERTIES IN SOFCS Aside from the characterization of the chemical and electro-chemical behaviour of ceramic SOFC materials, which has been addressed in numerous studies since this property gives the functionality to these materials, it also is essential to characterize their mechanical behaviour because SOFCs are subjected to long-term operation and thermal cycles that may cause mechanical degradation. Therefore, different mechanical phenomena, such as micro-cracks, creep, electrodeelectrolyte delamination, microstructural evolution, etc., can compete with other chemical or electro-chemical effects that limit the overall performance of the device and potentially lead to its ultimate failure. In order to understand the origin of these mechanical phenomena it is necessary to know the arrangement of the different materials in a functional SOFC system. As mentioned above, a single cell is composed of an electrolyte in intimate contact with an anode and a cathode. Moreover, stacking of several single cells is required to generate an applicable amount of electricity for real applications. In this configuration, an interconnect plate is always installed between neighbouring fuel cells to provide the electronic contact [55], while a sealant is required to obtain gas tightness [56]. In order to maximize the electrode-interconnect contact, these stacks are subjected to a minimum compression pressure of 64 - 74 kPa [57]. A schematic representation of SOFC stack is shown in Figure 1.6. Figure 1.6. A schematic representation of planar SOFC stack [58] under compression.
Chapter 1. Introduction 32 Figure 1.9. Grain deformation according to Ashby and Verrall model [98]. (a) Initial state, (b) intermediate state: necking, and (c) final state. Equation 1.4 predicts a steady-state strain rate about an order of magnitude faster that Equation 1.3, since less matter diffusion is needed for a given strain than in the Nabarro-Herring and Coble models, and the diffusive paths length are shorter [98]. This model explains successfully the mechanical and microstructural features observed in different ceramic materials with grain sizes between 1 and 10 µm, such as UO2 [99], NiO [100], YSZ [101], YBCO [102], and YAG [103]. Yet despite the success of the Ashby-Verrall model, it has been criticized because of its 2D nature, which leads to unrealistic diffusion paths. Spingarn and Nix [104] modified the topology of the grainswitching process to produce a more realistic transient configuration during the change of the grain shape, but leading to the same final grain configuration. 1.2.2.2.2 Dislocation-accommodated process Another mechanism that can account for the accommodation of grain boundary sliding is the movement and multiplication of dislocations. Numerous models have been proposed for this accommodation mechanism [97, 105-109], although none of them is able to completely explain the deformation process in polycrystalline materials. In general, all these models lead to a steady-state strain rate equation as follows: B pn Gb b σ ε = A k T d G D (1.5) where A is a constant, G is the shear modulus, b is the Burgers vector, D a diffusion coefficient and p and n the exponents of grain size and stress, respectively. Some models introduce a threshold stress 0 necessary to iniciate the sliding, modifying the Equation 1.5 with the effective stress - 0. Dislocation-accommodated grain boundary sliding mechanisms can be based on stacking of dislocations or movement of individual dislocations. a) b) c)
Chapter 1. Introduction 33 1.2.2.3 Interface-reaction creep The aforementioned models are based on the assumption that grain boundaries act as perfect sources and sinks for vacancies. If this assumption is not satisfied, the creep rate will be controlled by interface reaction [110], i.e. by the processes of absorption/emission of vacancies by grains boundaries. Burton [111] for the case of diffusional creep, and Ashby and Verrall [98] and Burton [112] for the case of GBS, developed models to account for this process. 1.2.2.3.1 Diffusion creep controlled by interface-reaction The operation of sources and sinks for vacancies at grain boundaries is required by diffusional creep as shown in Figure 1.7. Considering that dislocations having a component of their Burger's vector perpendicular to the grain boundary can act as sinks and sources by climbing along the boundary, Burton [111] model led the process of diffusion creep controlled by interfacereaction in the case of bulk diffusion, defining the creep rate as: 2 B lat j Pσ ε= 8πEdk T Z -1 b ΩD (1.6) where Pj is the probability of finding a jog on a dislocation, Z the coordination number and E the energy per unit length of a dislocation line. 1.2.2.3.2 GBS creep controlled by interface-reaction Burton [112] introduced the characteristic-area concept as the product of the grain diameter and the spacing between linear defects at the interfaces. Taking into account the same considerations than in the case of diffusional creep, the strain rate equations for the grain boundary sliding accommodated by interface-reaction are given by: B 2 lat Gb b σ ε = A k T d G D B 22 gb Gb b σ ε = A k T d G D (1.7) (1.8) In both equations A Pj/ , where Pj has a meaning analogous to the previous case and is a constant 1.
Chapter 1. Introduction 34 In a similar way to Burton’s development, and assuming that there is a viscous force opposing the movement of dislocations along the grain boundaries, Ashby and Verral propose the following equation: 2 βbM σ ε=0.84ΩG d (1.9) where M is the mobility of the boundary dislocation and a constant of the order of unity. Consideration of the IRC process leads to an increase of one unit in the stress exponent n and a decrease also in one unit of the exponent of grain size p with respect to the original expressions 1.2.2.4 Phenomenological relationships for superplasticity Many different models have been developed to explain superplasticity based in different relaxation processes of the stresses generated by the sliding of the grains on each other: dislocation motion inside the volume of the grains or along the grain boundaries, diffusional flow, interfacereaction-controlled diffusion (i.e. boundaries are not perfect sources and sinks for point defects), grain boundary migration or cavitation. None of them, however, is able to explain successfully the body of experimental data in superplastic materials. Sherby et al. [113] carried out a phenomenological study of fine-grained superplastic metals taking into account the following considerations: (i) most fine-grained metal materials under superplastic conditions exhibit an stress exponent n =2 ( 2); (ii) the temperature-dependence of strain rate corresponds to the atoms diffusion by either along the grain boundaries ( Dgb) or through the volume of the grains ( Dlat); (iii) for grain boundary diffusion, the strain rate is d-3 while for lattice diffusion is d-2. With these considerations, the authors proposed the following phenomenological relationships: 22 6 lat B 32 5 gb B Gb b σ ε = 8x10 D k T d G Gb b σ ε = 2x10 D k T d G (1.10) (1.11) The strain rate values predicted by these expressions reproduce the experimental results of all the studied materials within an order of magnitude. Equation 1.10 has been shown to account for the superplastic deformation of fine-grained Yttria-Stabilized tetragonal Zirconia with a grain size smaller than 1 µm [91] and Equation 1.11 for fine-grained YBa2Cu3O7-x superconductor [114].
Chapter 1. Introduction 35 1.2.3 Previous results in SOFC electrolytes Although the knowledge of the mechanical properties of SOFC components have received a growing interest in recent years, the available data still remain scarce. In the present section a brief literature review is performed in which previous results concerning the mechanical characterization of electrolyte materials are presented. 1.2.3.1 Yttria-Stabilised Zirconia 8 mol% Yttria-Stabilised Zirconia (8YSZ) is the SOFC electrolyte material more used and studied due to its excellent electrical and thermal properties. The evolution of the coefficient of thermal expansion of 8YSZ has been evaluated in different works by dilatometry from room temperature to 1273 K [115-118]. The results obtained were very closed and in the range of 10.0 - 11.0 x 10-6 K-1. On the other hand, various studies have been devoted to investigate the elastic properties of 8YSZ using different techniques at room temperature and all of them reported comparable values between 190 and 223 GPa [119-123]. For example, Selçuk et al. [124] determined the elastic constant of 8YSZ by the impulse excitation technique (IET) and found values of Young’s modulus (E) and Poisson ratio (ν) in the ranges of 219 - 223 GPa and 0.319 - 0.321, respectively. Similarly, Radovic et al. [125] reported values of 216 GPa and 0.315 measured by Resonant Ultrasound Spectroscopy for the same composition at room temperature. The temperature dependence of Young`s modulus for 8YSZ has been also addressed in several studies, and all of them showed similar results [121, 123, 126]. Selçuk et al. [126] found an average value of E of 216 ± 5 GPa at 298 K and 155 ± 8 GPa at 1173 K. They also determined the fracture toughness by double-torsion loading at the same temperatures obtaining values of 1.61 ± 0.12 MPa·m1/2 at room temperature and 1.02 ± 0.05 MPa·m1/2 at 1173 K. Concerning the creep behaviour, data on bending tests in the temperature range of 1223 - 1563 K for 8YSZ with a grain size between 2.4 - 6.9 µm led to a stress exponent close to the unity and an energy activation ≃ 400 kJ/mol, indicating that grain boundary sliding accommodated by diffusion is the main deformation mechanism [122, 127]. 1.2.3.2 Lanthanum Silicate To our knowledge, very few studies have reported mechanical properties of apatites compounds. Santos et al. [128] obtained La9.33Si2Ge4O26 compounds through different sintering temperatures and evaluated their mechanical properties by means of nano and microindentation
Chapter 1. Introduction 36 tests. They reported values of Young’s Modulus, nanohardness and microhardnes in the ranges of 106 - 135 GPa, 7.3 - 9.6 GPa and 2.9 - 5.8 GPa, respectively. These results showed a strong dependence of the mechanical properties on the microstructure and the experimental condition used. On the opposite, the values of fracture toughness remained practically constant (3.5 to 3.9 MPa·m1/2) with the sintering temperature. In the same line, Suarez et al. [129] measured the microhardness of different La9.33Si6O26 ceramics obtaining values between 6.99 and 7.57 GPa. They concluded that higher densifications lead to higher values of microhardness while an increase in the grain size tend to decrease this property. Concerning the temperature dependence of the coefficient of thermal expansion in LSO compounds, Iwata et al. [130] reported a value of 9.4 x 10-6 K-1 for La9.33Si6O26 measured by high-temperature X-ray diffraction (HT-XRD) in the range of temperature from 295 to 1073 K, and Jiang et al. [131] found values between 9.7 x 10-6 and 10.3 x 10-6 K-1 for La10Si6O27 compounds by thermo-mechanical analysis at temperatures between 298 and 1173 K. Unlike the case of the elastic properties and hardness, the coefficient of thermal expansion was found to be independent of the processing method and material microstructure. 1.2.3.3 Yttrium-doped Barium Zirconate The data available in the literature about mechanical properties of BZY is even scarcer than for Lanthanum Silicate compounds. To our knowledge, there is no information about the elastic properties and creep behaviour of these material. Only one previous work by Sazinas et al. [132] studied the hardness and fracture toughness of BaZr1-xYxO3-x/2 (x = 0.1 and 0.2) by microindentation. They found values of microhardness and fracture toughness ranging from 675 to 1005 Hv and 1.49 to 2.43 MPa.m1/2, respectively, for different hydration/dehydration conditions. On the other hand, Han et al. [133] measured the thermal expansion coefficient by HT-XRD on 2 to 30 at% yttriumdoped Barium Zirconate from room temperature to 1273 K. They found values from 8.47 x 10-6 K-1 to 10.2 x 10-6 K-1 increasing the doping level. Whereas, Lyagaeva et al. [134] reported a mean thermal expansion coefficient of BZY compounds of 8.2 x 10-6 K-1 in the temperature range of 323 - 1173 K. 1.3 REFERENCES 1. Boudghene Stambouli, A. and E. Traversa, Fuel cells, an alternative to standard sources of energy. Renewable and Sustainable Energy Reviews, 2002. 6(3): p. 295-304. 2. Traversa, E., Toward the miniaturization of solid oxide fuel cells. The Electrochemical Society Interface, 2009. 18(3): p. 49.
Chapter 1. Introduction 37 3. Malavasi, L., C.A.J. Fisher, and M.S. Islam, Oxide-ion and proton conducting electrolyte materials for clean energy applications: structural and mechanistic features. Chemical Society Reviews, 2010. 39(11): p. 4370-4387. 4. Fabbri, E., D. Pergolesi, and E. Traversa, Materials challenges toward proton-conducting oxide fuel cells: a critical review. Chemical Society Reviews, 2010. 39(11): p. 4355-4369. 5. Steele, B.C.H. and A. Heinzel, Materials for fuel-cell technologies. Nature, 2001. 414(6861): p. 345-352. 6. Singhal, S.C., Solid oxide fuel cells for stationary, mobile, and military applications. Solid State Ionics, 2002. 152: p. 405-410. 7. de Souza, S., S.J. Visco, and L.C. De Jonghe, Reduced‐temperature solid oxide fuel cell based on YSZ thin‐film electrolyte. Journal of the Electrochemical Society, 1997. 144(3): p. L35- L37. 8. Lefebvre-Joud, F., G. Gauthier, and J. Mougin, Current status of proton-conducting solid oxide fuel cells development. Journal of Applied Electrochemistry, 2009. 39(4): p. 535-543. 9. Brett, D.J.L., et al., Intermediate temperature solid oxide fuel cells. Chemical Society Reviews, 2008. 37(8): p. 1568-1578. 10. Hibino, T., et al., A low-operating-temperature solid oxide fuel cell in hydrocarbon-air mixtures. Science, 2000. 288(5473): p. 2031-2033. 11. Steele, B., Appraisal of Ce 1− y Gd y O 2− y/2 electrolytes for IT-SOFC operation at 500 C. Solid state ionics, 2000. 129(1): p. 95-110. 12. Torrens, R.S., N.M. Sammes, and G.A. Tompsett, Characterisation of (CeO2)0.8(GdO1.5)0.2 synthesised using various techniques. Solid State Ionics, 1998. 111(1): p. 9-15. 13. Ishihara, T., H. Matsuda, and Y. Takita, Doped LaGaO3 Perovskite Type Oxide as a New Oxide Ionic Conductor. Journal of the American Chemical Society, 1994. 116(9): p. 3801-3803. 14. Ma, X.Q., et al., Intermediate temperature solid oxide fuel cell based on fully integrated plasma-sprayed components. Journal of Thermal Spray Technology, 2005. 14(1): p. 61-66. 15. Lacorre, P., et al., Designing fast oxide-ion conductors based on La2Mo2O9. Nature, 2000. 404(6780): p. 856. 16. Goutenoire, F., et al., Crystal Structure of La2Mo2O9, a New Fast Oxide− Ion Conductor. Chemistry of materials, 2000. 12(9): p. 2575-2580. 17. Nakayama, S., et al., Ionic conductivity of lanthanoid silicates, Ln10(SiO4)6O3(Ln = La, Nd, Sm, Gd, Dy, Y, Ho, Er and Yb). Journal of Materials Chemistry, 1995. 5(11): p. 1801-1805. 18. Nakayama, S. and M. Sakamoto, Electrical properties of new type high oxide ionic conductor RE10Si6O27 (RE = La, Pr, Nd, Sm, Gd, Dy). Journal of the European Ceramic Society, 1998. 18(10): p. 1413-1418.
Chapter 1. Introduction 38 19. Tao, S. and J.T.S. Irvine, Preparation and characterisation of apatite-type lanthanum silicates by a sol-gel process. Materials Research Bulletin, 2001. 36(7–8): p. 1245-1258. 20. Abram, E.J., D.C. Sinclair, and A.R. West, A novel enhancement of ionic conductivity in the cation-deficient apatite La9.33(SiO4)6O2. Journal of Materials Chemistry, 2001. 11(8): p. 1978-1979. 21. Proton-Conducting Oxides. Annual Review of Materials Research, 2003. 33(1): p. 333-359. 22. Kreuer, K.D., Aspects of the formation and mobility of protonic charge carriers and the stability of perovskite-type oxides. Solid State Ionics, 1999. 125(1–4): p. 285-302. 23. Duan, C., et al., Readily processed protonic ceramic fuel cells with high performance at low temperatures. Science, 2015. 24. Zhu, B., X. Liu, and T. Schober, Novel hybrid conductors based on doped ceria and BCY20 for ITSOFC applications. Electrochemistry Communications, 2004. 6(4): p. 378-383. 25. Shima, D. and S.M. Haile, The influence of cation non-stoichiometry on the properties of undoped and gadolinia-doped barium cerate. Solid State Ionics, 1997. 97(1–4): p. 443-455. 26. Katahira, K., et al., Protonic conduction in Zr-substituted BaCeO3. Solid State Ionics, 2000. 138(1–2): p. 91-98. 27. Medvedev, D.A., et al., Advanced materials for SOFC application: Strategies for the development of highly conductive and stable solid oxide proton electrolytes. Progress in Materials Science, 2016. 75: p. 38-79. 28. Medvedev, D., et al., Sulfur and carbon tolerance of BaCeO3–BaZrO3 proton-conducting materials. Journal of Power Sources, 2015. 273: p. 716-723. 29. Shishkin, M. and T. Ziegler, Structural, electronic, stability and reduction properties of perovskite surfaces: The case of rhombohedral BaCeO3. Surface Science, 2012. 606(13): p. 1078-1087. 30. Dauter, J., et al., Studies on Chemical Stability and Electrical Properties of Proton Conducting Perovskite-Like Doped BaCeO3. Journal of The Electrochemical Society, 2010. 157(10): p. B1413-B1418. 31. LÜ, J., et al., Chemical stability of doped BaCeO3-BaZrO3 solid solutions in different atmospheres. Journal of Rare Earths, 2008. 26(4): p. 505-510. 32. Babilo, P., T. Uda, and S.M. Haile, Processing of yttrium-doped barium zirconate for high proton conductivity. Journal of Materials Research, 2007. 22(5): p. 1322-1330. 33. Yamazaki, Y., R. Hernandez-Sanchez, and S.M. Haile, High Total Proton Conductivity in Large-Grained Yttrium-Doped Barium Zirconate. Chemistry of Materials, 2009. 21(13): p. 2755-2762. 34. Tong, J., et al., Solid-state reactive sintering mechanism for large-grained yttrium-doped barium zirconate proton conducting ceramics. Journal of Materials Chemistry, 2010. 20(30): p. 6333-6341.
Chapter 1. Introduction 39 35. Pergolesi, D., et al., High proton conduction in grain-boundary-free yttrium-doped barium zirconate films grown by pulsed laser deposition. Nat Mater, 2010. 9(10): p. 846-852. 36. Iwahara, H., et al., Protonic conduction in calcium, strontium and barium zirconates. Solid State Ionics, 1993. 61(1): p. 65-69. 37. Schober, T. and H.G. Bohn, Water vapor solubility and electrochemical characterization of the high temperature proton conductor BaZr0.9Y0.1O2.95. Solid State Ionics, 2000. 127(3– 4): p. 351-360. 38. Okudera, H., et al., Structure of oxide ion-conducting lanthanum oxyapatite, La9.33(SiO4)6O2. Solid State Ionics, 2005. 176(15–16): p. 1473-1478. 39. Tian, C., et al., Direct synthesis of La9.33Si6O26 ultrafine powder via sol–gel self-combustion method. Journal of Alloys and Compounds, 2008. 458(1–2): p. 378-382. 40. Nakao, T., et al., Chemical stability of La10Si6O27 and its application to electrolytes for solid oxide fuel cells. Solid State Ionics, 2008. 179(27–32): p. 1567-1569. 41. Matsunaga, K. and K. Toyoura, First-principles analysis of oxide-ion conduction mechanism in lanthanum silicate. Journal of Materials Chemistry, 2012. 22(15): p. 7265-7273. 42. Leon-Reina, L., et al., Interstitial oxygen conduction in lanthanum oxy-apatite electrolytes. Journal of Materials Chemistry, 2004. 14(7): p. 1142-1149. 43. Masubuchi, Y., et al., Oxide ion conduction mechanism in RE9.33(SiO4)6O2 and Sr2RE8(SiO4)6O2 (RE = La, Nd) from neutron powder diffraction. Solid State Ionics, 2006. 177(3–4): p. 263-268. 44. León-Reina, L., et al., Crystalchemistry and Oxide Ion Conductivity in the Lanthanum Oxygermanate Apatite Series. Chemistry of Materials, 2003. 15(10): p. 2099-2108. 45. Nakayama, S. and M. Sakamoto, Ionic conductivities of apatite-type LaX(GeO4)6O1.5X−12 (X=8–9.33) polycrystals. Journal of Materials Science Letters, 2001. 20(17): p. 1627-1629. 46. Susumu, N., A. Hiromichi, and S. Yoshihiko, Ionic Conductivity of Ln10(SiO4)6O3 (Ln = La, Nd, Sm, Gd and Dy). Chemistry Letters, 1995. 24(6): p. 431-432. 47. Ryu, K.H. and S.M. Haile, Chemical stability and proton conductivity of doped BaCeO3– BaZrO3 solid solutions. Solid State Ionics, 1999. 125(1–4): p. 355-367. 48. Akbarzadeh, A.R., et al., Combined theoretical and experimental study of the lowtemperature properties of ${\mathrm{BaZrO}}_{3}$. Physical Review B, 2005. 72(20): p. 205104. 49. Shannon, R., Revised effective ionic radii and systematic studies of interatomic distances in halides and chalcogenides. Acta Crystallographica Section A, 1976. 32(5): p. 751-767. 50. Nomura, K. and H. Kageyama, Transport properties of Ba(Zr0.8Y0.2)O3 − δ perovskite. Solid State Ionics, 2007. 178(7–10): p. 661-665. 51. Kedvik, E., Chemical Expansion in Barium Zirconate. 2014, Chalmers University of Technology, Göteborg, Sweden.
Chapter 1. Introduction 40 52. Slade, R.C.T., S.D. Flint, and N. Singh, Investigation of protonic conduction in Yb- and Y- doped barium zirconates. Solid State Ionics, 1995. 82(3): p. 135-141. 53. Bohn, H.G. and T. Schober, Electrical Conductivity of the High‐Temperature Proton Conductor BaZr0.9Y0.1O2.95. Journal of the American Ceramic Society, 2000. 83(4): p. 768- 772. 54. Snijkers, F.M.M., et al., Proton conductivity and phase composition in BaZr0.9Y0.1O3−δ. Scripta Materialia, 2004. 50(5): p. 655-659. 55. Minh, N.Q., Ceramic Fuel Cells. Journal of the American Ceramic Society, 1993. 76(3): p. 563-588. 56. Dicks, J.L.a.A., Fuel Cell Systems Explained. 2003. 57. Dey, T., et al., Study of contact resistance at the electrode–interconnect interfaces in planar type Solid Oxide Fuel Cells. Journal of Power Sources, 2013. 233: p. 290-298. 58. Berke, R. and M.E. Walter, Mechanical Characterization and Modeling of Solid Oxide Fuel Cells and Stacks, in Experimental and Applied Mechanics, Volume 6: Proceedings of the 2011 Annual Conference on Experimental and Applied Mechanics, T. Proulx, Editor. 2011, Springer New York: New York, NY. p. 37-44. 59. Gazzarri, J.I. and O. Kesler, Short-stack modeling of degradation in solid oxide fuel cells. Journal of Power Sources, 2008. 176(1): p. 138-154. 60. Nakajo, A., et al., Mechanical reliability and durability of SOFC stacks. Part I : Modelling of the effect of operating conditions and design alternatives on the reliability. International Journal of Hydrogen Energy, 2012. 37(11): p. 9249-9268. 61. Liu, Y.L., et al., Microstructural studies on degradation of interface between LSM–YSZ cathode and YSZ electrolyte in SOFCs. Solid State Ionics, 2009. 180(23): p. 1298-1304. 62. Hagen, A., et al., Degradation of anode supported SOFCs as a function of temperature and current load. Journal of the Electrochemical Society, 2006. 153(6): p. A1165-A1171. 63. Simwonis, D., F. Tietz, and D. Stöver, Nickel coarsening in annealed Ni/8YSZ anode substrates for solid oxide fuel cells. Solid State Ionics, 2000. 132(3): p. 241-251. 64. Tanasini, P., et al., Experimental and theoretical investigation of degradation mechanisms by particle coarsening in SOFC electrodes. Fuel Cells, 2009. 9(5): p. 740-752. 65. Vels Jensen, K., et al., Microstructural and chemical changes at the Ni/YSZ interface. Solid State Ionics, 2001. 144(3): p. 197-209. 66. Liu, Y.L. and C. Jiao, Microstructure degradation of an anode/electrolyte interface in SOFC studied by transmission electron microscopy. Solid State Ionics, 2005. 176(5): p. 435-442. 67. Mitterdorfer, A. and L.J. Gauckler, La2Zr2O7 formation and oxygen reduction kinetics of the La0.85Sr0.15MnyO3, O2(g)|YSZ system. Solid State Ionics, 1998. 111(3): p. 185-218. 68. Chen, M., et al., LSM–YSZ reactions in different atmospheres. Fuel Cells, 2009. 9(6): p. 833- 840.
Chapter 1. Introduction 41 69. Lara-Curzio, E., et al., Effect of thermal cycling and thermal aging on the mechanical properties of, and residual stresses in, Ni-YSZ/YSZ bi-layers. IV. A, 2009. 11: p. 383-391. 70. Kübler, J., R. Primas, and B. Gut, Mechanical strength of thermally aged and cycled thin zirconia sheets, Advances in Science and Technology, Ceramics: Charting the Future, ed. P. Vincenzini, Techna, Florence, Italy. 1995, ISBN 88-86538-02-2. 71. Nakajo, A., et al., Compilation of mechanical properties for the structural analysis of solid oxide fuel cell stacks. Constitutive materials of anode-supported cells. Ceramics International, 2012. 38(5): p. 3907-3927. 72. Selçuk, A. and A. Atkinson, Elastic properties of ceramic oxides used in solid oxide fuel cells (SOFC). Journal of the European Ceramic Society, 1997. 17(12): p. 1523-1532. 73. Atkinson, A. and A. Selçuk, Mechanical behaviour of ceramic oxygen ion-conducting membranes. Solid State Ionics, 2000. 134(1): p. 59-66. 74. Ivers-Tiffée, E., A. Weber, and D. Herbstritt, Materials and technologies for SOFC- components. Journal of the European Ceramic Society, 2001. 21(10): p. 1805-1811. 75. Chiang, L.-K., et al., Thermo-electrochemical and thermal stress analysis for an anodesupported SOFC cell. Renewable Energy, 2008. 33(12): p. 2580-2588. 76. Nakajo, A., et al., Mechanical reliability and durability of SOFC stacks. Part II: Modelling of mechanical failures during ageing and cycling. International Journal of Hydrogen Energy, 2012. 37(11): p. 9269-9286. 77. Bouhala, L., et al., Study of interface influence on crack growth: Application to Solid Oxide Fuel Cell like materials design. Materials & Design, 2010. 31(3): p. 1033-1041. 78. Biswas, S., et al., High-temperature mechanical properties of reduced NiO–8YSZ anodesupported bi-layer SOFC structures in ambient air and reducing environments. Ceramics International, 2013. 39(3): p. 3103-3111. 79. Young, J.L. and V.I. Birss, Crack severity in relation to non-homogeneous Ni oxidation in anode-supported solid oxide fuel cells. Journal of Power Sources, 2011. 196(17): p. 7126- 7135. 80. Nakajo, A., et al., The effects of dynamic dispatch on the degradation and lifetime of solid oxide fuel cell systems. Journal of The Electrochemical Society, 2011. 158(11): p. B1329- B1340. 81. Gazzarri, J.I. and O. Kesler, Non-destructive delamination detection in solid oxide fuel cells. Journal of Power Sources, 2007. 167(2): p. 430-441. 82. Pandey, A., et al., In-situ Young's moduli of the constitutive layers in a solid oxide fuel cell. Journal of Power Sources, 2015. 273: p. 522-529. 83. Radovic, M. and E. Lara-Curzio, Elastic Properties of Nickel-Based Anodes for Solid Oxide Fuel Cells as a Function of the Fraction of Reduced NiO. Journal of the American Ceramic Society, 2004. 87(12): p. 2242-2246.
Chapter 2. Preparation of materials 48 2.2 LANTHANUM SILICATE Densification is a serious challenge in the fabrication of La9.33+xSi6O26+3x/2 compounds. Many efforts have thus been made to prepare fully dense ceramics for SOFC electrolyte applications, where flow gas impermeability and thus low porosity (which greatly limits the electrical performance [17]) are required. The most widely technique used for the preparation of these compounds is via conventional solid-state reaction methods, where very high temperatures (> 1600 ºC) are necessary to obtain relative densities higher than 90% (Table 2.1). The sol-gel route has been also proposed to decrease the formation temperature of the oxy-apatite phase; this technique however, leads to densities lower than 95% after conventional sintering (Table 2.1). Table 2.1. Preparation techniques, sintering temperatures and relative densities for La9.33Si6O26 oxyapatite. Technique Sintering temperature ( °C) Relative density (%) Reference Solid-state reaction 1500 - 1500 70 - 80 [18] Solid-state reaction 1600-1700 > 90 [19] Solid-state reaction 1600 97 [20] Solid-state reaction 1700 95 [15] Sol-gel 1400 69 [21] Sol-gel 1400 66 [22] Sol-gel 1450 92 [23] Sol-gel 1500 90 [6] Freeze drying + Conventional sintering 1500 > 95 [1, 2] Freeze drying + Spark plasma sintering 1250 100 [1, 2] In this context, previous works of our research group have shown two strategies to achieve excellent results in the densification of Lanthanum Silicate by combining highly dispersed nanopowders obtained by freeze drying with conventional or spark plasma sintering, which resulted in densities between 95 % and 100 % [1, 2]. Therefore, in this work, these two routes have been followed to prepare fully dense materials.
Chapter 2. Preparation of materials 49 2.2.1 Commercial starting precursors for LSO nanopowders preparation Two high purity commercial precursors were used as starting materials: lanthanum acetate sesquioxide La(CH3COO)3·1.5H2O and tetraethoxysilane (TEOS, Si(OC2H5)4, their characteristics are summarized in Table 2.2. Table 2.2. Commercial precursors used for the preparation of La9.33Si6O26. Precursor Vendor Purity (%) Molecular weight (g/mol) La(CH3COO)3·1.5H2O Alfa-Aesar 99.9 343.05 Si(OC2H5)4 Alfa-Aesar 99.9 208.33 Stoichiometric amounts of precursors were used to form the La9.33Si6O26 compound according to the following equation: 9.33La(CH3COO)3 ·1.5H2O + 6Si(OC2H5)4 + 128O2 La9.33Si6O26 + 104CO2 + 116H2O 2.2.2 Freeze-drying synthesis Freeze-drying allows the preparation of a large variety of high purity powders with an accurate control of the composition [24, 25]. It consists in the instant freezing of a solution and the further ice sublimation under vacuum conditions [26], resulting in highly dispersed precursor nanoparticles. A subsequent conventional thermal treatment is necessary to remove the organic ligands and form the desired phase. La9.33Si6O26 (LSO) was synthesized by the freeze drying method following the experimental process presented in Figure 2.1. Firstly, lanthanum acetate was dissolved in 200 ml of ultra-pure water with magnetic stirring until a transparent solution was obtained. Then, TEOS was put in another beaker, and acetic acid and a small amount of deionized water were added. The mixture was stirred, resulting in a clear transparent solution. Acetic acid acts as a double agent since it catalyzes and controls the TEOS hydrolysis reaction. The volumetric ratio, r = Vacetic acid/ VTEOS, was set to 4 [1, 2]. The two aforementioned solutions were then mixed, and ultra-pure water was added up to a total volume of 600 mL, with a pH value close to 4. The resulting solution was sprayed in a liquid nitrogen bath to form a “snow” containing water and the precursors. Due to the instantaneous freezing, the homogeneity of the original solution was retained in the solid phase. These frozen droplets were transferred into the freeze-dryer chamber, where the dehydration process was carried out in a Christ Alpha 2-4 LSC apparatus under vacuum (≤1 Pa). By maintaining
Chapter 2. Preparation of materials 50 the temperature of the condenser at -47 °C for 48 hours, water was continuously removed by sublimation and the temperature of the powder increased up to +4 °C. Finally the precursor was progressively warmed up to +50 ºC to get rid of the adsorbed water. The resulting powder was a whitish amorphous precursor. Figure 2.1. Freeze-drying synthesis process for La9.33Si6O26 nanopowders. Calcination is a thermal treatment by which a set of chemical reactions of decomposition produce a new compound. It is commonly used in the production of simple oxide powders from carbonates, hydroxides, nitrates, sulfates, etc. This step of the fabrication process is essential to remove any residual carbon species and form pure oxy-apatite nanopowders. After freeze-drying, the precursors contain a high amount of organic residues and ligands, which decompose between room temperature and 900 °C, this decomposition being associated with an important weight loss (∼45%). The thermal treatments at T > 900 °C lead to well crystallised powder without any parasitic phase [2]. In this work, freeze-dried powder calcination was carried out at 1000 °C for 4 hours, with heating/cooling rates of 5 °C/min, in air. Precursor La9.33Si6O26 nanopowders Clear transparent solution (pH = 3.8) La(CH3COO)3·1.5H2O + ultra-pure water Si(OC2H5)4+ acetic acid + ultra-pure water Frozen solution - "snow" SPRAY FREEZING Calcination 1000 ºC / 4h, air FREEZE DRYING
Chapter 2. Preparation of materials 51 2.2.3 Compaction of LSO nanopowders Cold mechanical compaction increases the cohesion between particles in the powder and allows to obtain easy-to-handle compact pellets, which are later on subjected to sintering at high temperature. In this work, a double pressing system was used, consisting of: · Uniaxial pressing: A pre-compaction of the nanopowders was performed on a uniaxial press under 100 MPa for 3 min in a 20 mm diameter cylindrical steel die filled with about 6 g of powder. After pressing, pellets of 20 mm in diameter and 7 mm in height were obtained. · Isostatic pressing: These pellets were vacuum-packed in plastic bags using a domestic vacuum sealer and then isostatically pressed at 750 MPa for 10 min. Pellets of 19 mm in diameter and 6 mm in height were finally obtained. 2.2.4 High-temperature sintering In order to prepare fully dense materials from the freeze-dried nanopowders, two different sintering routes have been used: conventional and spark plasma sintering. 2.2.4.1 Conventional sintering Conventional sintering is the pressureless sintering of a previously pressed powder. Powder compacts were placed on an alumina crucible covered previously with a layer of Lanthanum Silicate powder and then sintered at 1500 °C for 12 h in air. Very slow heating/cooling rates were used, 2 °C/min, in order to avoid possible internal residual stresses which could cause the formation and propagation of cracks. After sintering, the pellets dimensions decreased to approximately 15 and 5 mm in diameter and height, respectively. 2.2.4.2 Spark Plasma Sintering Spark plasma sintering (SPS) is a powerful technique to sinter powders applying an external pressure and an electric field simultaneously. It allows a faster densification at lower temperatures than conventional sintering methods [27], giving rise to materials with higher densities, smaller grain sizes, cleaner grain boundaries, in addition to other interesting properties [28]. SPS has been carried out in a Dr. Sinter SPS furnace (Plateforme frittage flash, Thiais, France) (Figure 2.2) which allows the recording of the shrinkage, shrinkage rate, temperature, current, voltage and pressure in real time.
Chapter 2. Preparation of materials 52 Before SPS treatment, a 20 mm-diameter high-strength graphite mold/dies ensemble was filled with about 6 g of calcined LSO powder. To minimize heat losses, the mold was lined with a foil of graphite and surrounded by a blanket of graphite (Figure 2.7). The mold/die/powder assembly was then put into the sintering chamber and a thermocouple was inserted into the graphite die to measure the temperature. The assembly was progressively heated up to 1250 °C under a constant pressure of 100 MPa. Firstly, the temperature was increased up to 600 °C at a rate of 200 °C/min. After this first step, the target temperature of 1250 °C was reached at a heating rate of 50 °C/min and maintained for 5 min. After that, both the heating and pressure were rapidly released. The system took around 10 min cooling-down naturally. The whole sintering process, from sample preparation until final cooling, lasted less than 1 h. The pellets were finally submitted to a conventional thermal treatment at 800 °C in air for 24 h to burn all residual carbon species. Figure 2.2. Spark-plasma sintering system: (a) Hot press furnace (left), unit control (center) and power unit (right). (b) Detail of the chamber interior during sintering. (c) Die, blanket and graphite foil used in the process. 2.3 YTTRIUM-DOPED BARIUM ZIRCONATE In order to prepare fully dense and pure BaZr1-xYxO3-δ compounds, several approaches have been developed. High sintering temperature (> 1700 °C) and long sintering time enable density values higher that 90%. For example, Iguchi et al. [41] obtained 97% dense BaZr0.95Y0.05O3 at 1700 to 1800 °C, while Duval et al. [42] reported densities of about 91% at 1720 °C for BaZr0.9Y0.1O3, which unfortunately also lead to variation in chemical composition due to Barium evaporation and the emergence of parasite phases, which have a detrimental effect on the proton conductivity [39, b) a) c)
Chapter 2. Preparation of materials 53 41, 43]. To overcome the disadvantages, wet chemical methods were adopted to obtain high quality nanopowders and the desired perovskite compound [44, 45]. In the present work, Y-substituted Barium Zirconate has been synthesized by the modified EDTA-citrate complexing method, and sintered at high temperature by conventional sintering following the suggestion of Babilo et al. [46]. It has been also used a commercial NiO-added BZY sintered pellet, as explained below. 2.3.1 Commercial starting precursors for BZY nanopowders preparation High purity commercial precursor powders of Barium Nitrate Ba(NO3)2, Yttrium Nitrate (Y(NO3)3·6H2O) and Zirconium Nitrate (ZrO(NOx)·yH2O) were used as starting materials . Their characteristics are summarized in Table 2.3. Table 2.3. Commercial precursors used for the preparation of BaZr0.85Y0.15O2.925. Precursor Vendor Purity (%) Molecular weight (g/mol) Ba(NO3)2 Alfa-Aesar 99.95 261.35 Y(NO3)3·6H2O ZrO(NO3)2·5.69H2O Alfa-Aesar Strem chemicals 99.9 99.9 383.01 231.23 Stoichiometric amounts of precursors were used to form the BaZr0.85Y0.15O2.925 compound according to the following equation: Ba(NO3)2 + 0.15Y(NO3)3·6H2O + 0.85ZrO(NO3)2·5.69H2O BaZr0.85Y0.15O2.925 + 2.08N2 + 5.19O2 +5.74H2O 2.3.2 Modified EDTA-citrate complexing synthesis The modified EDTA–citrate complexing method is a successful wet chemical route used to synthetize a large variety of oxide materials [47]. Due to the EDTA-citrate combination, several metal ions present in a solution are chelated to make up metal complexes which undergo polyesterification, when heated, to form a polymer with the metal ions uniformly distributed throughout [48] . As a result, ultrafine powders of high purity and homogeneity are obtained [49, 50]. Taking into account the advantages of this method, BaZr0.85Y0.15O2.925 (BZY) was prepared by the modified EDTA-citrate complexing synthesis following the experimental process presented on Figure 2.3.
Chapter 2. Preparation of materials 54 Figure 2.3. Microwave-assisted citric acid-EDTA synthesis process of BaZr0.85Y0.15O2.925 nanopowders. First of all, the necessary amounts of nitrates were dissolved in 150 ml of ultra-pure water with magnetic stirring until a transparent solution was obtained. Afterwards, citric acid and EDTA were added as chelating agents. The cooperation of citrate and EDTA allows obtaining more stable chelate complexes [50]. The mole ratio of (EDTA acid): (citric acid): (total metal ions) was fixed at 1.5:1.5:1. Then, aqueous ammonia was added to the solution to facilitate the EDTA dissolution, forming a water-soluble ammonium salt [3] with a pH value adjusted to about 8. Solution was heated up under continuous stirring to obtain a viscous gel. Then, dry gel combustion was carried out into a domestic microwave for 2 h, obtaining a black porous precursor. After this synthesis step, the precursor was calcined to obtain a pure crystalline phase. It was first ground into an agate mortar and placed in an alumina crucible. Then, calcination was carried out at 1000 °C for 5 h in air, with heating/cooling rates of 3 °C/min. Once finished the thermal treatment, the black precursor became a whitish powder (Figure 2.4). Ba(NO3)2 + Y(NO3)3 · 6H2O + ZrO(NO3)2· 5.69H2O EDTA + Citric acid Clear transparent solution (pH = 8) Precursor (black powder) BaZr0.85Y0.15O2.925 nanopowders Grinding / Calcination Heating 100 °C / Microwave 2h NH3·H2O for increasing pH
Chapter 2. Preparation of materials 55 Figure 2.4. (a) Black porous sponge-puffy stuff; (b) Black milled precursor; (c) Whitish powder after calcination. 2.3.3 Compaction of BZY nanopowders Cold mechanical compaction was used to obtain compact pellets of BZY15, which were later on sintered at high temperature. Firstly, a pre-compaction of nanopowders was performed by means of a uniaxial press. For this propose, a powder amount of 6 g was loaded into a 20 mmdiameter cylindrical steel mold and pressed at 100 MPa for 3 min, obtaining pellets of 20 mm in diameter and 8 mm in thickness. These pellets were vacuum packed in plastic bags using a domestic vacuum sealer and subsequently isostatically pressed at 750 MPa for 10 min. 17 mm-diameter and 7 mm-height pellets were obtained. 2.3.4 High temperature sintering High temperature pressureless sintering was carried out after powder compaction to obtain a fully dense material. The pellets were placed in an alumina crucible and fully covered by BZY powder with a 10 wt%-excess Barium carbonate, as suggested by Babilo et al. [46] (Figure 2.5), to avoid Barium evaporation found at temperatures above 1550 °C [43, 51] . Conventional sintering was performed at 1600 °C during 24 h in air, with very slow heating/cooling rates of 3 °C/min. Figure 2.5. Sintering configuration: BaZr0.85Y0.15O2.925 green pellet covered with a powder mixture of BYZ and BaCO3 (10 wt%) [46]. (a (b (c BaZr0.85Y0.15O2.925 powder + 10 wt% BaCO3 powder Alumina crucible Alumina tube BaZr0.85Y0.15O2.925 pellet
Chapter 2. Preparation of materials 56 2.3.5 Commercial Yttrium-doped Barium Zirconate In order to overcome the low sinterability of Barium Zirconate, a new approach based on the use of additives (mostly transtision metal oxides: NiO, ZnO, CuO, …) during the fabrication process has been recently proposed [52-54]. It results in dense materials with grain sizes of typically 2 - 4 µm, and therefore limited grain-boundary resistance. Yttrium-doped Barium Zirconate was prepared through this strategy starting from stoichiometric amounts of simple precursors (ZrO2, Y2O3 and BaCO3 or BaSO4) with 1-2 wt% transition metal oxide addition. The overall mixture was ball-milled during 24 h, pressed into a pellet and sintered at 1400 - 1550 °C for 24 h. The resulting compounds have densities higher than 90 %. In this sense, Nikodemski et at. [54] have reported densities higher than 98% in 20% Yttrium-doped Barium Zirconate with 1 wt% NiO sintered at 1500 °C for 24 h; the grain size was in the 3 - 5 µm range. Different explanations have been proposed to explain the efficiency of such a process [54]. With NiO addition, it has been suggested that low melting point intermediate phases, such as BaY2NiO5 or BaNiO4, are formed, enhancing the sintering rate through the presence of a liquid phase [53]. This material also shows a high total proton conductivity, similar to that of bulk material [53]. In this study, BaZr0.85Y0.15O2.925 with 1 wt% NiO-content provided by NorecsTM in the form of large pellets of 20 mm in diameter and 5 mm in thickness has been studied. NiO-extraction In order to study the influence of Nickel on the mechanical properties, the mechanical characterization was also carried out on the BZY commercial samples after NiO-extraction. For NiO-extraction, commercial ceramics were placed in an alumina crucible and surrounded with a powder mixture of BZY15 with 10 wt% excess of barium carbonate, as shown in Figure 2.5. Then, a firing cycle was carried out at 1600 °C for 120 h in air, with very slow heating/cooling rates of 3 °C/min. NiO extraction is based on the NiO diffusion along grain boundaries towards the sample surface, where it sublimes and is captured by the surrounding BZY powder [55]. 2.4 REFERENCES 1. Chesnaud, A., et al., Preparation of transparent oxyapatite ceramics by combined use of freeze-drying and spark-plasma sintering. Chemical Communications, 2007(15): p. 1550- 1552.
Chapter 2. Preparation of materials 57 2. Chesnaud, A., et al., Influence of synthesis route and composition on electrical properties of La9.33 + xSi6O26 + 3x/2 oxy-apatite compounds. Solid State Ionics, 2008. 179(33–34): p. 1929-1939. 3. Iakovleva, A., Study of novel proton conductors for high temperature Solid Oxide Cells. 2016, CentraleSupelec, Université Paris-Saclay, France. 4. Nakayama, S. and M. Sakamoto, Electrical properties of new type high oxide ionic conductor RE10Si6O27 (RE = La, Pr, Nd, Sm, Gd, Dy). Journal of the European Ceramic Society, 1998. 18(10): p. 1413-1418. 5. Okudera, H., et al., Structure of oxide ion-conducting lanthanum oxyapatite, La9.33(SiO4)6O2. Solid State Ionics, 2005. 176(15–16): p. 1473-1478. 6. Tian, C., et al., Direct synthesis of La9.33Si6O26 ultrafine powder via sol–gel self-combustion method. Journal of Alloys and Compounds, 2008. 458(1–2): p. 378-382. 7. Nakao, T., et al., Chemical stability of La10Si6O27 and its application to electrolytes for solid oxide fuel cells. Solid State Ionics, 2008. 179(27–32): p. 1567-1569. 8. Matsunaga, K. and K. Toyoura, First-principles analysis of oxide-ion conduction mechanism in lanthanum silicate. Journal of Materials Chemistry, 2012. 22(15): p. 7265-7273. 9. Leon-Reina, L., et al., Interstitial oxygen conduction in lanthanum oxy-apatite electrolytes. Journal of Materials Chemistry, 2004. 14(7): p. 1142-1149. 10. Masubuchi, Y., et al., Oxide ion conduction mechanism in RE9.33(SiO4)6O2 and Sr2RE8(SiO4)6O2 (RE = La, Nd) from neutron powder diffraction. Solid State Ionics, 2006. 177(3–4): p. 263-268. 11. León-Reina, L., et al., Crystalchemistry and Oxide Ion Conductivity in the Lanthanum Oxygermanate Apatite Series. Chemistry of Materials, 2003. 15(10): p. 2099-2108. 12. Nakayama, S. and M. Sakamoto, Ionic conductivities of apatite-type LaX(GeO4)6O1.5X−12 (X=8–9.33) polycrystals. Journal of Materials Science Letters, 2001. 20(17): p. 1627-1629. 13. Nakayama, S., et al., Ionic conductivity of lanthanoid silicates, Ln10(SiO4)6O3(Ln = La, Nd, Sm, Gd, Dy, Y, Ho, Er and Yb). Journal of Materials Chemistry, 1995. 5(11): p. 1801-1805. 14. Susumu, N., A. Hiromichi, and S. Yoshihiko, Ionic Conductivity of Ln10(SiO4)6O3 (Ln = La, Nd, Sm, Gd and Dy). Chemistry Letters, 1995. 24(6): p. 431-432. 15. Abram, E.J., D.C. Sinclair, and A.R. West, A novel enhancement of ionic conductivity in the cation-deficient apatite La9.33(SiO4)6O2. Journal of Materials Chemistry, 2001. 11(8): p. 1978-1979. 16. Steele, B.C.H. and A. Heinzel, Materials for fuel-cell technologies. Nature, 2001. 414(6861): p. 345-352. 17. Panteix, P.J., et al., Influence of porosity on the electrical properties of La9.33(SiO4)6O2 oxyapatite. Ceramics International, 2008. 34(7): p. 1579-1586.
Chapter 3. Structural and microstructural characterization 64 where Ykobs and Ykcalc are the observed and calculated intensities of the kth reflection at the completion of refinement procedure, respectively. Good agreement between observed and computed reflections results in a small value of the RBragg index. 3.2.2 Particle size The particle size distribution of the calcined powders was measured using a Malvern Zetasizer Nano ZS particle size analyzer (Functional Characterization Service, CITIUS, University of Sevilla, Spain), which allows the determination of particle diameters in the range 0.6 nm - 6 µm. This equipment uses the low angle laser light scattering technique to measure particle sizes through the intensity and angle of the dispersed beams by the suspended particles in a given medium. For the measurements, a suspension of 0.5 g of calcined powder in 25 ml of ethanol was prepared under 30 min-ultrasonication. 3.2.3 Density The density of the sintered compounds was determined by two different ways. On the one hand, by direct measurement of mass and dimensions, using a balance and a caliper, respectively. On the other hand, using the Archimedes’ method, by means of an analytical balance equipped with a hydrostatic weighing accessory. The measurements were performed at ambient conditions using distilled water as immersion medium. The density was then calculated by the following equation: 2 d H O w i W · ρ ρ=W - W (3.5) where Wd, Ww and Wi are the weight in dry, wet, and immersion conditions, respectively, and ρH2O is the water density at room-temperature. Finally, the relative density was obtained from the theoretical density. 3.2.4 Electron microscopy analysis The microstructural characterization of the materials was performed using a highresolution FEI Teneo scanning electron microscope, equipped with an X-ray dispersive energy microanalysis system (EDS, Energy Dispersive X-ray Spectroscopy), and also with a FEI Talos transmission electron microscope operating at 200 kV voltage (Microscopy Service, CITIUS, University of Seville).
Chapter 3. Structural and microstructural characterization 65 3.2.4.1 Preparation of samples For SEM observations, sintered samples were carefully polished using SiC papers (1500 grit and 2500 grit, Buehler), and then ultrasonically cleaned in acetone for 15 min. After polishing, and in order to reveal grain boundaries, the samples were thermally etched at a temperature 20% below the sintering temperature for 3 hours and then mounted on aluminum holders using carbon paper. It was not necessary to deposit any conductive coating on the surface of the sample due to the low voltage used (1 - 5 kV). For TEM observations, the samples were cut into thin slices of less than 100 µm-thickness using a high precision diamond saw. Afterwards, the slices were polished down to 50 µm and then dimpled using a dimple grinder to less than 20 µm-thickness in the center of the disc. Finally, the slices were ion-milled using argon at low incidence angles until a hole was formed. 3.2.4.2 Morphological parameters The most relevant morphological parameters taken into account for the microstructural characterization of the different materials were the grain size d, the form factor F and the orientation angle θ of the grains. These parameters were measured from SEM micrographs using the Image J semiautomatic image analyzer software averaging over more than 500 grains on each material. 3.2.4.2.1 Grain size The grain size has been taken as the equivalent planar diameter d, defined by: 1 2 4·Area d= π (3.6) where Area is the measured grain surface. It has been found (see later in this Chapter) that the grain size distributions are consistent with a lognormal law, as found in many other ceramics [4]. The lognormal distribution law is given by [5, 6]: 2 2 2 ln 11 (d|µ,σ)= exp - d2 d/ σ 2 μ πσ f (3.7) with the normalization condition:
Chapter 3. Structural and microstructural characterization 66 0 (d|µ,σ)d d =1f (3.8) The parameters μ and σ are related to the mean grain size 𝑑 and its standard deviation σd by: 2 σ d = µ exp 2 ; 1 2 2 2 d σ σ = µ exp exp σ -1 2 (3. 9) The parameters μ and σ of the lognormal distribution that best fit a set of experimental results are easily obtained from the representation of the accumulated fraction of grains n versus grain size d. This fraction is given by: 0 d n= x dxf (3.10) which, for a lognormal distribution, results: d2 2 20 ln x /µ 11 n = exp - dx x2σ 2πσ (3.11) By making the substitution: 1x u x = ln σµ ; x 1 du = dx σ (3.12) Equation 3.11 is rewritten as: u d '2 - 1u n= exp du 2 2π (3.13) Equivalently: 1d n= Z ln σµ (3.14) where Z(y) is the error function given by: y2 - 1u Z y = exp - du 2 2π (3.15) Inverting this equation, finally results in:
Chapter 3. Structural and microstructural characterization 67 -1 1 d 1 1 Z n = ln = lndlnμ σ µ σ σ (3.16) The plot of Z-1 (n) versus ln(d) is therefore a straight line, called Henry's line, which can be written as: -1 Z n = A ln d +B 1 σ=A ; B µ = exp - A (3.17) where ln(µ) is the average value of ln(d), 𝑙𝑛(𝜇) = 𝑙𝑛(𝑑) , and σ is the standard deviation of ln(d). The mean value of 𝑑 and its standard deviation σd (Equation 3.9) can also be easily expressed as a function of the parameters A and B of the Henry's line: 2 B1 d = exp - + A 2A ; 1 -2 d22 B σ = exp - + exp - A 11 2A 1 A (3.18) 3.2.4.2.2 Form factor The form factor is a dimensionless parameter which gives quantitative information of the grain shape. It is defined as: 2 4 πArea F= Grain perimeter (3.19) It has a maximum value of 1 for a circle and 0 for a segment. For polygonal grains with N sides, it is easily found that: π /N F=tg π / N (3.20) 3.2.4.2.3 Orientation angle The orientation angle of a grain, θ, is defined as the orientation of the largest diameter of the grain relative to a direction of reference. For non-circular grains, the distribution of this parameter gives information about the preferential alignment of the grains.
Chapter 3. Structural and microstructural characterization 68 3.3 EXPERIMENTAL RESULTS 3.3.1 Lanthanum Silicates 3.3.1.1 Density By using the theoretical density of La9.33Si6O26, 5300 kg/m3, relative density values higher than 95% (required for the desired application) were achieved by the two different routes chosen for the material preparation. Table 3.2. Relative densities of La9.33Si6O26 compounds. Material Synthesis Sintering Relative density (%) Mass / volume Archimedes LSO-CS Freeze-drying CS at 1500 °C 97.1 ± 0.8 96.7 ± 0.2 LSO-SPS Freeze-drying SPS at 1250 °C 99.6 ± 0.4 100.0 ± 0.2 Table 3.2 shows that the combination of freeze-drying and spark plasma sintering yields higher densities than conventional sintering and allows to obtain fully dense compounds (almost 100% of the theoretical density). These results are in accordance with what was reported by Chesnaud et al. [7] in a previous work following the same fabrication routes. 3.3.1.2 X-Ray Diffraction analysis Calcined nanopowders Identification of the crystalline phases was performed at room temperature using X-ray diffraction (XRD) and the diffraction patterns of the PDF-2002 database collected in Table 3.1. Figure 3.1 displays the XRD pattern of the powder obtained after calcination. Comparison with PDF-2002 reference patterns confirms the presence of La9.33Si6O26 single phase (P63/m). The crystallites size was estimated to be about 80 - 90 nm from the diffraction peaks width by using the Scherrer equation.
Chapter 3. Structural and microstructural characterization 69 Figure 3.1. XRD pattern of calcined LSO powder (black). PDF-2002 XRD pattern of La9.33Si6O26 (red). Le Bail fitting of diffraction patterns was carried out using the space group P63/m and the initial unit cell parameters a = 9.728(6) Å and c = 7.190(4) Å reported by León-Reina et al. [8]. Table 3.3. Refined cell parameters of La9.33Si6O26 calcined powders. Material a (Å) b (Å) c (Å) V (Å3) Rwp GOF RBragg La9.33Si6O26 9.729(3) - 7.183(2) 588.76(4) 11.12 1.10 0.415 Refined cells parameters, gathered in Table 3.3, are similar to those found in the literature for the calcined powder. For example, Célérier et al. [9] reported unit cell parameters for La9.33Si6O26 of a = 9.726(3) Å and c = 7.184(5) Å, while Kolisch et al. [10] have presented values of a = 9.713(5) Å and c = 7.186(5) Å. Sintered ceramics After sintering, both LSO-CS and LSO-SPS materials present a single lanthanum silicate crystalline phase. In order to obtain a more detailed structural information, Le Bail fitting of the diffraction patterns was carried out in the P63/m space group taking into account once again the structural description given by León-Reina et al. [8]. Figure 3.2 shows XRD patterns of LSO-CS and LSO-SPS sintered ceramics. Bragg angle positions corresponding to the structure are indicated by red vertical bars. I PDF 49-0443 La9.33Si6O26 Lanthanum Silicate
Chapter 3. Structural and microstructural characterization 70 Figure 3.2. X-ray diffraction diagram for La9.33Si6O26 sintered ceramics. The refined parameters deduced from the Le Bail method are summarized in Table 3.4, which are in good agreement with literature data for La9.33Si6O26 ceramics [7, 10-13]. For instance, Sansom et al. [14] found a = 9.721(3) and c = 7.187(3), similar to the present results. Table 3.4. Refined cell parameters of La9.33Si6O26 sintered compounds. Material a (Å) b (Å) c (Å) V (Å3) Rwp GOF RBragg LSO-CS 9.724(5) - 7.186(4) 588.49(3) 12.22 1.38 0.627 LSO-SPS 9.723(6) - 7.183(4) 588.01(8) 11.32 1.30 0.542 It can be thus conclude that the two sintered materials, LSO-CS and LSO-SPS, exhibit indentical lattice parameters, which are indeed the same as in the original calcined powder (Table 3.3). 3.3.1.3 Particle size Figure 3.3 shows the particle size distribution of the La9.33Si6O26 as-obtained nanopowders after calcination, of five measurements, which yields an average particle size of 550 ± 60 nm, much larger than the mean value of 85 nm obtained by XRD. This difference, along with the microstructural results of the sintered material (presented later in section 3.3.1.4), which shows an average grain of about 200 nm, suggest that the sizes measured by the laser diffraction technique correspond to powder agglomerates and not to individual single-crystallite particles. To confirm
Chapter 3. Structural and microstructural characterization 71 this result, an additional analysis of the powders was performed by transmission electron microscopy (TEM). To this end, several drops of the same suspension were placed on carbon-coated copper TEM grids (200 mesh). Observations were then performed on a Philips CM200 microscope (Microscopy Service, CITIUS, University of Sevilla, Spain) operating at 200 kV. Figure 3.3. Particle size distribution of La9.33Si6O26 as-obtained nanopowders after calcination. The morphology of the La9.33Si6O26 nanopowder is shown in Figure 3.4. It can be seen agglomerates of 300 - 800 nm, which consist of irregular particles of average size of about 100 nm. This value correlates well with the crystallite sizes calculated from XRD analysis, confirming the nanometric nature of the LSO powder. On the other hand, the size of the agglomerates observed by TEM agrees with the value measured by laser diffraction. Figure 3.4. TEM micrographs of La9.33Si6O26 as-obtained nanopowders after calcination. 100 nm 200 nm
Chapter 3. Structural and microstructural characterization 72 3.3.1.4 Microstructural analysis Figure 3.5 shows SEM micrographs of La9.33Si6O26 sintered in air through conventional sintering at 1500 °C for 12 h. These images clearly reflect a homogenous and dense microstructure consisting of equiaxed grains with average sizes of about 1 μm and delimited by well-defined grain boundaries. Porosity is small in agreement with density measurements. Figure 3.5. SEM micrographs of sintered LSO-CS compounds. Figure 3.6. SEM micrographs of sintered LSO-SPS compounds. Figure 3.6 shows SEM micrographs of La9.33Si6O26 sintered in vacuum through spark plasma sintering at 1250° C for 5 min. These materials present a fine-grained microstructure consisting of equiaxed grains with grain sizes in the range 100 - 500 nm, with practically no porosity. These results show a large difference in grain size between both materials, indicating the influence of the sintering method on the microstructure. The lower temperature and shorter sintering time used during SPS restrict strongly the grain growth. 5 µm 1 µm 5 µm 1 µm
Chapter 3. Structural and microstructural characterization 73 Figure 3.7. Morphological distributions of La9.33Si6O26 compounds made from conventional sintering (LSO-CS) and Spark plasma sintering (LSO-SPS): (a) Grain size; (b) Henry’s lines for the grain size distribution; (c) Form factor; (d) Orientation angles. The morphological parameters d, F and θ of the different materials were measured from SEM micrographs and are summarized in Table 3.5 and displayed in Figure 3.7. Though the grain size of LSO-CS is larger than LSO-SPS materials, they exhibit similar grain size-scaled distributions, corresponding to a lognormal law. Regarding the form factor F, both materials have equiaxed grains with average values of 0.8, which means a stable grain distribution. The absence of preferential directions in the polycrystal is also reflected in the orientation angle formed by the maximum diameter of the grain with an arbitrary direction. Average values, close to 90° and standard deviation near 45°, indicate the absence of preferred directions in grain populations.
Chapter 3. Structural and microstructural characterization 80 Figure 3.16. Morphological distributions of BaZr0.85Y0.15O2.925 compounds: (a) Grain size; (b) Form factor; (c) Orientation angles; (d) Henry’s lines for the grain size distribution. The morphological parameters d, F and θ of the different materials were measured from SEM micrographs and are summarized in Table 3.9 and displayed in Figure 3.16. All the compounds exhibit similar distributions, corresponding to a lognormal law. Regarding the form factor F, they have equiaxed grains with average values of 0.8, which means a stable grain size distribution. The absence of preferential directions in the polycrystal is also reflected in the orientation angle formed by the maximum diameter of the grain with an arbitrary direction. Average values close to 90° and standard deviation near 45°, indicate the absence of preferred directions in grain populations.
Chapter 3. Structural and microstructural characterization 81 Table 3.9. Morphological parameters of BaZr0.85Y0.15O2.925 compounds: grain size d, grain size lognormal distribution parameters µ, σ, form factor F and orientation angle θ. Material d (µm) µ (µm) σ (µm) F θ (°) BZY (lab-made) 0.2 ± 0.1 0.18 0.22 0.8 ± 0.1 84 ± 52 BZY-NiO (commercial) 1.6 ± 0.6 1.37 0.27 0.8 ± 0.1 85 ± 52 Finally, in order to complete the microstructural characterization, TEM observations were carried out on all the materials. Figure 3.17 and Figure 3.18 show typical images of the internal structure of the grains in the different compounds. Lab-made BZY grains are often very stressed, with dislocations arranged in dense tangles and also forming pile-ups and low-angles subboundaries. On the opposite, BZY-NiO grains are generally free of defects, with clean and straight grain boundaries and well-defined triple points. Figure 3.17. TEM images of sintered lab-made BZY compounds. ( aI) ( aII) ( b) 400 nm 300 nm 10 nm 100 nm
Chapter 3. Structural and microstructural characterization 82 Figure 3.18. TEM images of sintered commercial BZY-NiO compounds. 3.3.3 Yttrium-doped Barium Zirconate after NiO-extraction 3.3.3.1 Density By using the theoretical density of 15% Yttrium-doped Barium Zirconate (6166 kg/m3), the relative density of BZY after NiO-extraction was 95.4 ± 0.9 % which contrast with the value of 99% of the material before the extraction process. This decrease in density reveals the influence of sintering aids in densification as it was already tested by Tong et al. [15] and Nikodemski et al. [16]. 3.3.3.2 X-ray diffraction analysis In order to ensure that the extraction process did not modify the Yttrium-doped Barium Zirconate crystalline phase, X-ray diffraction was performed and the data obtained were compared with that of BZY-NiO. Figure 3.19 shows the XRD patterns of the different commercial BZY-NiO compounds where it can be observed that, in /BZY after NiO-extraction, all the peaks of the BaZr0.85Y0.15O2.925 cubic phase are present. Moreover, in comparison with BZY-NiO, the extra peaks of BaY2NiO5 which come from the NiO used as additive in the sintering step have disappeared, as can be more easily observed in the magnified pattern of the Figure 3.19. The lattice parameter deduced from the Le Bail method for the material after NiO-extraction was 4.223 (3) Å, the same value found for BZY and slightly higher than for BZY-NiO (Table 3.8). 2 µm 5 µm
Chapter 3. Structural and microstructural characterization 83 Figure 3.19. X-ray diffraction diagram of commercial BZY sintered ceramic. Full (upper) and magnified (lower) patterns. Simultaneously with XDR, X-Ray Fluorescence (XRF) measurements were collected for BZY- NiO and BZY after NiO-extraction to identify the elemental composition of the samples. Figure 3.20 shows the XRF spectra of both materials. No evidence of Ni after the NiO-extraction process was found, in agreement with the XRD measurements.
Chapter 3. Structural and microstructural characterization 84 Figure 3.20. X-ray fluorescence analysis of BZY-NiO (a) before and (b) after NiO-extraction. A magnetometry technique has been used in order to quantify any possible residual nickel content after NiO-extraction, not detected by XRD or XRF. This technique allows the measurement of ferromagnetic elements down to the parts per million level. To this end, the samples were annealed in a reducing atmosphere of 5% H2/Ar at 800 °C for 24 hours, and then analyzed in a MPMS 5 Quantum Design magnetometer (Plateforme Technique de l’ICMMO, Magnetic measurements service, France) at 300 K under an uniform field of -60000 Oe to 60000 Oe. Figure 3.21 shows the magnetization curves for the commercial material before and after the NiO-extraction. NIST standard of 54.888 emu/g-Ni was used to determine the amount of metallic Ni in the samples. In this way, the BZY-NiO after annealing had a magnetic moment of 0.155 emu/g-Ni, corresponding to an amount of metallic Ni of about 0.3 wt%, which is in roughly agreement with the NiO content of 1 wt% introduced in the process. On the contrary, the specimens after NiO-extraction exhibited a null magnetic moment, indicating the absence of Ni and therefore the success of the extraction process.
Chapter 3. Structural and microstructural characterization 85 Figure 3.21. Magnetization curve for BZY-NiO before and after NiO-extraction. 3.3.3.3 Microstructural analysis Figure 3.22 shows back-scattered electron images of BZY ceramic after NiO-extraction. This material presents a microstructure with equiaxed and large grains (from 2 to 20 µm). Figure 3.22. Back-scattered electron micrographs of BZY after NiO-extraction (left) and their equivalent images with secondary electrons detector (right). 50 µm 50 µm 50 µm 50 µm
Chapter 3. Structural and microstructural characterization 86 A comparison with the original material with NiO, which exhibited a grain size of 1.6 µm with no pores (Figure 3.15), these images reflect a significant grain growth as well as an increase in porosity during the NiO-extraction. Coarsening of the BZY microstructure has been also reported by Coors et at. [25] after subjecting BZY-NiO compounds to a similar NiO-extraction process; in this case, they used a heat treatment at 1600 °C for 16 hours and observed an increase in the average grain size from 5 to 6.5 µm. Due to the fact that the amount of time required for a total extraction depends on the dimensions of the samples, it has been tested that 120 hours were necessary for a successful NiO-extraction in the case of specimens of 3 x 3 x 5 mm3. This long high-temperature heat treatment favoured a significant grain growth as well as an increase in porosity. As evidenced by Figure 3.22, the black regions are porosity, which consisted in cavities of about 10 µm preferably located at multiple grain junctions. The morphological parameters d, F and θ of BZY after NiO-extraction were measured from Back-scattered electron micrographs and are summarized in Table 3.10. This material exhibits similar distribution, form factor and angle orientation than the others BZY compounds (Table 3.9) which means a stable grain size distribution with absence of preferential directions in the polycrystal. However, these results show a large difference in grain size with respect to the other ceramics, confirming the influence of the long firing cycle in the microstructure as just commented above. Table 3.10. Morphological parameters of BZY after NiO-extraction: grain size d, grain size lognormal distribution parameters µ, σ, form factor F and angle orientation θ. Material d (µm) µ (µm) σ (µm) F θ (°) BZY after NiO-extraction 9 ± 3 8.32 0.23 0.8 ± 0.1 87 ± 53 Finally TEM observations were carried out on the materials. Figure 3.23 shows typical images of the internal structure of the grains, where most of them display large densities of dislocation and other defects, not seen in the original material (Figure 3.18).
Chapter 3. Structural and microstructural characterization 87 Figure 3.23. TEM images of sintered BZY compounds after NiO-extraction. 3.4 REFERENCES 1. Le Bail, A., Whole powder pattern decomposition methods and applications: A retrospection. Powder Diffraction, 2012. 20(4): p. 316-326. 2. Paufler, P., R. A. Young (ed.). The Rietveld Method. International Union of Crystallography. Oxford University Press 1993. 298 p. Price £ 45.00. ISBN 0–19–855577–6. Crystal Research and Technology, 1995. 30(4): p. 494-494. 3. Toby, B.H., R factors in Rietveld analysis: How good is good enough? Powder Diffraction, 2006. 21(1): p. 67-70. 4. Bravo-León, A., M. Jiménez-Melendo, and A. Domínguez-Rodríguez, Mechanical and microstructural aspects of the high temperature plastic deformation of yttria-stabilized zirconia polycrystals. Acta Metallurgica et Materialia, 1992. 40(10): p. 2717-2726. 5. Kurtz, S.K. and F.M.A. Carpay, Microstructure and normal grain growth in metals and ceramics. Part I. Theory. Journal of Applied Physics, 1980. 51(11): p. 5725-5744. 2 µm 5 µm 3 µm 3 µm
Chapter 3. Structural and microstructural characterization 88 6. Kurtz, S.K. and F.M.A. Carpay, Microstructure and normal grain growth in metals and ceramics. Part II. Experiment. Journal of Applied Physics, 1980. 51(11): p. 5745-5754. 7. Chesnaud, A., et al., Influence of synthesis route and composition on electrical properties of La9.33 + xSi6O26 + 3x/2 oxy-apatite compounds. Solid State Ionics, 2008. 179(33–34): p. 1929-1939. 8. Leon-Reina, L., et al., Interstitial oxygen in oxygen-stoichiometric apatites. Journal of Materials Chemistry, 2005. 15(25): p. 2489-2498. 9. Célérier, S., et al., New chemical route based on sol–gel process for the synthesis of oxyapatite La9.33Si6O26. Ceramics International, 2006. 32(3): p. 271-276. 10. Kolitsch, U., H.J. Seifert, and F. Aldinger, The Identity of Monoclinic La2O3 and Monoclinic Pr2O3 with La9.33(SiO4)6O2 and Pr9.33(SiO4)6O2, Respectively. Journal of Solid State Chemistry, 1995. 120(1): p. 38-42. 11. Lambert, S., et al., Structural investigation of La9.33Si6O26- and La9AESi6O26+δ-doped apatites-type lanthanum silicate (AE=Ba, Sr and Ca) by neutron powder diffraction. Journal of Solid State Chemistry, 2006. 179(8): p. 2602-2608. 12. Masubuchi, Y., et al., Oxide ion conduction mechanism in RE9.33(SiO4)6O2 and Sr2RE8(SiO4)6O2 (RE = La, Nd) from neutron powder diffraction. Solid State Ionics, 2006. 177(3–4): p. 263-268. 13. Okudera, H., et al., Structure of oxide ion-conducting lanthanum oxyapatite, La9.33(SiO4)6O2. Solid State Ionics, 2005. 176(15–16): p. 1473-1478. 14. Sansom, J.E.H., et al., A comparison of the effect of rare earth vs Si site doping on the conductivities of apatite-type rare earth silicates. Journal of Solid State Electrochemistry, 2006. 10(8): p. 562-568. 15. Tong, J., et al., Proton-conducting yttrium-doped barium cerate ceramics synthesized by a cost-effective solid-state reactive sintering method. Solid State Ionics, 2010. 181(33–34): p. 1486-1498. 16. Nikodemski, S., J. Tong, and R. O'Hayre, Solid-state reactive sintering mechanism for proton conducting ceramics. Solid State Ionics, 2013. 253: p. 201-210. 17. Nomura, K. and H. Kageyama, Transport properties of Ba(Zr0.8Y0.2)O3 − δ perovskite. Solid State Ionics, 2007. 178(7–10): p. 661-665. 18. Iguchi, F., et al., The relationship between chemical composition distributions and specific grain boundary conductivity in Y-doped BaZrO3 proton conductors. Solid State Ionics, 2009. 180(6–8): p. 563-568. 19. Duval, S., Y-Substituted Barium Zirconate, a Proton Conducting Electrolyte for Applications at Intermediate Temperatures 2008, University of Munich. 20. Park, K.-Y., et al., Electrical and physical properties of composite BaZr0.85Y0.15O3−d- Nd0.1Ce0.9O2−δ electrolytes for intermediate temperature-solid oxide fuel cells. Journal of Power Sources, 2016. 336: p. 437-446.
Chapter 3. Structural and microstructural characterization 89 21. Kreuer, K.D., et al., Proton conducting alkaline earth zirconates and titanates for high drain electrochemical applications. Solid State Ionics, 2001. 145(1–4): p. 295-306. 22. S. P. Shafi, L.B., S. Boulfrad and E. Traversa, Yttrium and Nickel Co-Doped BaZrO3 as a Proton-Conducting Electrolyte for Intermediate Temperature Solid Oxide Fuel Cells. The Electrochemical Society, 2014. 23. Magrez, A. and T. Schober, Preparation, sintering, and water incorporation of proton conducting Ba 0.99 Zr 0.8 Y 0.2 O 3− δ: comparison between three different synthesis techniques. Solid State Ionics, 2004. 175(1): p. 585-588. 24. Tong, J., et al., Solid-state reactive sintering mechanism for large-grained yttrium-doped barium zirconate proton conducting ceramics. Journal of Materials Chemistry, 2010. 20(30): p. 6333-6341. 25. Coors, W.G., et al., Fabrication of Yttrium-Doped Barium Zirconate for High Performance Protonic Ceramic Membranes. Perovskite Materials - Synthesis, Characterisation, Properties, and Applications. 2016.
Chapter 4. Room-temperature mechanical characterization 96 Figure 4.3. Compression test setup and optical acquisition system. In order to measure accurately the displacements between successive images, the specimen was marked along its longitudinal and transversal axes, which allowed to obtain the evolution in the position of each marker between the first image and the deformed ones, and determine the strain along both axes. As indicated at the beginning of this chapter, the Young’s modulus and Poisson ratio were determined by considering the materials to be elastic isotropic. In 2D, the isotropic elastic strainstress relationship (y-axis being axis of symmetry) can be written as: yy xx yx ε ε ε 10 EE 10 EE 1 00 2G yy xx yx σ σ σ (4.7) where ɛij and σij are the strain and the stress tensor respectively, and the parameters E, ν and G are the corresponding elastic properties that can be determined from 2D experiments. In a mechanical compression test, a uniaxial stress σ is applied, then the stress vector can be written as: yy xx yx 0 0 (4.8) Considering a prismatic specimen of section S under a load F, the applied stress σ is defined by the following equation: Load Cell Camera Specimen Long distance lens Light Load Camera
Chapter 4. Room-temperature mechanical characterization 97 Therefore, from Equation 4.7 only two elastic constants can be determined, the Young´s modulus E and Poisson ratio ν, which are defined as follows: yy E (4.10) xx yy (4.11) During the image acquisition, the longitudinal ɛyy and transversal ɛxx strains were calculated in real time both during the loading and unloading steps. 4.2.1.3 Resonant Ultrasound Spectroscopy These experiments were carried out using a typical RUS setup (SPMS Laboratory, CentraleSupelec, France) which was used to determine the elastic properties with a very high accuracy. The RUS method is based on the measurement of the resonant frequencies of vibration of a specimen with well-defined geometry. A parallelepipedic sample was placed between two piezoelectric transducers, one of them being used to excite the mechanical resonances of the specimen, whereas the opposite transducer is used to detect them (Figure 4.4). The frequency was swept between 0.2 and 2 MHz allowing to activate the sample’s resonant modes. When the frequency corresponds to one of the own resonance frequencies of the specimen, a large response is detected at the receptor transducer and appears as a peak in the resonance spectrum [5]. The mechanical resonance of a given solid depends on its elastic constants, density and geometry [6]. Therefore by measuring a large quantity of resonant modes on one sample, the elastic constants can be then determined by solving two processes: the direct and inverse problems. The direct problem implies the calculation of the mechanical resonance from known material properties while the inverse problem is based on finding the best fit between the measured and the calculated (direct process) frequencies to determine the elastic components. F S (4.9)
Chapter 4. Room-temperature mechanical characterization 98 Figure 4.4. (a) A schematic representation of a typical RUS setup and (b) several resonant frequencies of vibration for a prismatic specimen [5]. Direct process In the direct problem, the natural resonant frequencies ω of an elastic solid can be calculated if the elastic tensor Cijkl, volume V, and density ρ are given. This procedure seeks stationary points of the Lagrangian L for a freely vibrating elastic body [6]. 22 i ijkl i,j k,l V 1 L u C dV 2uu (4.12) where ui is the ith component of the displacement field and the indices following a comma denote differentiation with respect to that coordinate. ui is expanded in a complete set of basis functions , following the Rayleigh-Ritz method: ii ua (4.13) where aiα is the expansion coefficient. The are chosen depending on the geometry of the specimen and, for parallelepipeds, the Legendre polynomials are selected [5]. Substituting in Equation 4.12, this can be rewritten in a matrix form as: 2 T T 1 L a a a 2Ma (4.14) (a) (b) Drive transducer Pickup transducer transducer Signal Measured spectrum
Chapter 4. Room-temperature mechanical characterization 99 where a is the vector containing the expansion coefficients, and M and are the mass and stiffness matrices, respectively, of the vibration problem. Equation 4.12 is stationary if the displacements ui are solutions of freely vibrating elastic body, therefore by setting δL=0, the equation turns to: 2 aMa (4.15) Thus, the natural resonant frequencies of an elastic solid can be determined straightforward if the geometry, density and elastic tensor of the specimen are well known. Inverse process In the inverse problem, the elastic components are generally estimated through an optimization process in which the stiffness components are adjusted until the best fitting between the measured and computed frequencies is found [7]. The cost function is defined and minimized as: 2 meas pred n n ij meas nn f f C Ff (4.16) where fnmeas are the frequencies measured, fnpred are the frequencies predicted and Cij are the stiffness constants. The main difficulty in this procedure is to obtain a good pairing between calculated and measured modes. Determination of the elastic constants Assuming that the material behavior is isotropic, only two elastic constants are required to define the elastic tensor: 11 12 12 12 11 12 12 12 11 11 12 ij 11 12 11 12 000 000 00 C C C C C C C 0 0 0 0 0 0 2 0 0 0 0 0 2 0 CCC 00 C CCC CC 002 where C11 is also defined as the longitudinal modulus L, and 11 12 2 CC as the shear modulus G. These two constants are related to the Young’s modulus and the Poisson ratio by the following equations:
Chapter 4. Room-temperature mechanical characterization 100 G 3L 4G ELG (4.17) L -2G =2 L -G (4.18) Therefore, E and ν determination can be performed once the elastic tensor is extracted by the inverse problem. 4.2.1.4 Microindentation Mechanical properties were also investigated by microindentation using a Wolpert Teswell indenter (Mechanical Testing Laboratory, MSMAT, CentraleSupelec, France) equipped with a Vickers diamond tip. The experiments were performed on polished surfaces at room temperature. A load of 2 N and A hold time at the maximum load of 10 s were selected and kept constant for all indentations. At least 10 indentation tests were performed on each material. The Vickers hardness, Hv, was calculated using the following equation: V2 P H =1.8544 d (4.19) where P is the applied load (kg) and d is the mean length of the diagonals (mm) (Figure 4.5). The hardness values were converted in GPa for comparison with the nanoindentation measurements. Figure 4.5. A schematic representation of Vickers microindentation. The fracture toughness KIC was estimated by applying the normalized Niihara’s expression [8]: Vickers indenter Specimen d
Chapter 4. Room-temperature mechanical characterization 101 -1.5 0.6 0.5 IC V 9.518 c K = H a a (4.20) where a and c are half of the indentation diagonal (d) and radial crack length, respectively (Figure 4.5). Due to the criterion c / a > 2.5, the Niihara’s equation was used to determine the fracture toughness. The measurement of the diagonals of the residual indents and of the radial-crack diameters were done with an optical microscope Alicona InfiniteFocus (Microscopy Resource Centre, MSSMAT, CentraleSupelec, France). 4.2.2 Experimental results 4.2.2.1 Room-temperature mechanical properties of Lanthanum Silicate 4.2.2.1.1 Nanoindentation Typical load-displacement curves for the different oxy-apatite compounds are shown in Figure 4.6 along with SEM micrographs of their respective indentations performed at 500 mN. Based on the upper one-third sections of these curves, the Young’s modulus and nanohardness were determined as a function of the applied load (Table 4.1). The results for each material represent the mean value of all the indents and the associated error is the standard deviation of the values. a)
Chapter 4. Room-temperature mechanical characterization 102 Figure 4.6. (a) Load-depth indentation curves from La9.33Si6O26 materials at 500mN. SEM micrographs of indents performed at 500 mN for (b) LSO-CS and (c) LSO-SPS. Table 4.1. Young's modulus E, hardness H and fracture toughness KIC of La9.33Si6O26 compounds as a function of the applied load. The results gathered in Table 4.1 for the LSO-CS compounds show a slight decrease with increasing load. This tendency is due to the ISE [2] and has been also reported in other studies on mechanical properties by nanoindentation [9-11]. For applied loads higher than 100 mN, the values show a stabilization because the penetration depth is larger (100 and 500 mN correspond to penetration depths of 750 and 1750 nm, respectively) and the influence of the surface defects is therefore lower. In order to study the overall mechanical properties of a polycrystalline material, it is essential to control the indent size according to the grain size of the sample [12]. For this, the contact diameter of the indenter must be one order of magnitude larger than the average grain size. In LSO-CS samples, the grain size is 1.1 ± 0.6 µm, therefore an indentation depth of 1750 nm, which would result in an equivalent contact diameter of about 12 µm, appears to agree with the requirements for determining the macroscopic mechanical properties. Figure 4.6b shows the contact area of an indentation performed at 500 mN in which it is possible to compare the grain size of the ceramic with the residual imprint of the indenter. Applied load (mN) LSO-CS LSO-SPS E (GPa) H (GPa) E (GPa) H (GPa) 10 147 ± 10 11 ± 2 132 ± 5 10.3 ± 0.7 30 142 ± 8 10.2 ± 0.6 133 ± 5 10.1 ± 0.7 60 143 ± 6 10.5 ± 0.7 131 ± 4 9.9 ± 0.6 100 138 ± 6 9.8 ± 0.8 131 ± 3 9.8 ± 0.5 500 138 ± 3 9.5 ± 0.4 129 ± 3 9.8 ± 0.4 10 µm 10 µm b) c)
Chapter 4. Room-temperature mechanical characterization 103 In contrast with the LSO-CS results, the Young’s modulus and the hardness of the LSO-SPS material remain practically constant with the different loads. This could be explained by the high relative sample density (99.6 ± 0.4 %) with practically no porosity and very small grain size (0.2 ± 0.1 μm). For an applied load of 10 mN, the penetration depth is 230 nm, which corresponds to an equivalent contact diameter of about 1.6 µm, i.e., one order of magnitude larger than the grain size, indicanting that, even at the minimum load, reliable values of the macroscopic mechanical properties can be obtained. Similar values of H were determined for both materials, however the Young’s modulus of LSO-SPS is slightly lower than that of the LSO-CS. To the author’s knowledge, only one previous work deals with the mechanical properties by nanoindentation of similar Lanthanum silicates compounds [13]. In this case, it was reported a Young’s Modulus of 135 GPa and a nanohardness of 9.6 GPa for the samples with the highest density, which are in good agreement with the results obtained in this work. 4.2.2.1.2 Mechanical compression tests with optical imaging The mechanical parameters such as the Young’s modulus and Poisson ratio were determined by the stress and strain measurement within the elastic range of specimens. The experimental results, summarized in Table 4.2, show similar values of ν for both materials while E is slightly higher for LSO-CS. The uncertainty is given by the standard deviations of the values from the different loading/unloading cycles. Table 4.2. Young's modulus E and Poisson ratio υ of La9.33Si6O26 compounds determined by mechanical compression tests. Material E (GPa) ν LSO-CS 141 ± 22 0.31 ± 0.07 LSO-SPS 136 ± 16 0.32 ± 0.08 4.2.2.1.3 Resonant Ultrasound Spectroscopy Table 4.3 shows the experimental results obtained by RUS with an extremely low uncertainty, which comes from the error between the experimental and computed frequencies. With this technique both Young’s modulus and Poisson ratio for LSO-CS were slightly higher than those for LSO-SPS.
Chapter 4. Room-temperature mechanical characterization 104 Table 4.3. Young's modulus E and Poisson ratio ν of La9.33Si6O26 compounds determined by RUS. Material E (GPa) ν LSO-CS 135 ± 1 0.31 ± 0.01 LSO-SPS 129 ± 1 0.28 ± 0.01 4.2.2.1.4 Microindentation Typical Vickers indents of the La9.33Si6O26 compounds are shown in Figure 4.7. In both cases symmetrical pyramid indents were observed in which a single crack propagates from each corner. Based on these indentations, Vickers hardness and fracture toughness were determined for each ceramic (Table 4.4). Figure 4.7. SEM images of Vickers microindentations on the surface of (a) LSO-CS and (b) LSO-SPS. Table 4.4. Vickers hardness HV and fracture toughness KIC of La9.33Si6O26 compounds. Material HV HV (GPa) KIC (MPa m1/2) LSO-CS 744 ± 24 7.3 ± 0.2 1.2 ± 0.1 LSO-SPS 787 ± 12 7.7 ± 0.1 1.3 ± 0.1 Table 4.4 summarizes the experimental results obtained by microindentation where HV is also given in GPa for comparison with the values measured by nanoindentation (Table 4.1). Similar values of fracture toughness were obtained for both materials, however LSO-SPS presents a slightly higher hardness than LSO-CS. Several parameters can affect the hardness of a ceramic material such as chemical bond strength, grain size, porosity and applied load among others [12]. The Hall- Petch law describes the relationship between the yield strength Y and the grain size and predicts 20 µm a) b) 20 µm
Chapter 4. Room-temperature mechanical characterization 105 that Y is inversely proportional to grain growth. On the other hand, Vickers hardness can be directly related to the yield strength through the following equation [14]: Y HV =3σ (4.21) Therefore a decrease in grain size implies an increase in hardness because the grain boundaries block the dislocations generated by the indenter [12]. Then, hardening of LSO-SPS could be attributed to the higher grain boundary density due to its smaller grain size in comparison with LSO-CS (0.2 and 1.1 µm, respectively). Concerning these oxy-apatites, only one previous work deals with the mechanical properties of similar compounds by microindentation [15]. In this case, it was reported a Vickers hardness of 7.57 ± 0.24 GPa for La9.33Si6026, which agrees with the results obtained in this work. 4.2.2.1.5 Comparison of the different techniques From the comparison of the mechanical parameters determined using the different techniques, the values of Young’s modulus obtained were in the range of 135 - 141 GPa for LSO-CS and 129 - 136 GPa for LSO-SPS, while the values of Poisson ratio obtained were in the range of 0.29 - 0.32 for both materials. Although all the techniques showed similar results of the elastic parameters for the two compounds, it worth mentioning that, compression tests showed the values with the highest uncertainty while RUS was the most precise technique. Concerning hardness, the values obtained by nanoindentation were 9.6 and 9.8 GPa for an applied load of 500 mN, whereas by microindentation they were 7.3 and 7.7 GPa at 2 N for LSO-CS and LSO-SPS, respectively. As expected, microhardness is significantly lower than nanohardness because of the differences in load. These values are in concordance with the well-known hardness dependence on the applied load, as found in other ceramics [10, 11, 16]. 4.2.2.2 Room-temperature mechanical properties of Yttrium-doped Barium Zirconate 4.2.2.2.1 Nanoindentation Figure 4.8 shows typical load-displacement curves obtained from sintered Yttrium-doped Barium Zirconate compounds at the maximum applied load of 500 mN together with SEM
Chapter 4. Room-temperature mechanical characterization 112 66 2 i i j i i,j i i j E 1 E E E 0 2 (4.22) where E(0) refers to the equilibrium configuration, the first derivatives being zero. According to this equation, the elastic constants can then be obtained by evaluating the energy as a function of strain. In both approaches, several perturbations are used in order to fit the linear behaviour of the stress with applied strain with a significant amount of points (typically 10 points are used thus 10 DFT calculations are made to determine one elastic coefficient Cij). In all cases, the maximum applied strain was limited to 1% in order to respect the laws presented before. 4.3.1.1 DFT Calculations details for Lanthanum Silicate oxy-apatites For the determination of the elastic tensor in oxy-apatite, calculations were performed using the commercial program VASP. The interactions between electrons and ions were described by the potential Projector Augmented Wave (PAW) method [23] within the generalized gradient approximation (GGA). The wavefunctions are then expanded in terms of a discrete plane wave basis set, which is truncated at a predefined maximum cut-off energy, the rest of the coefficients in the expansion are set to zero. A careful analysis of the convergence of the calculated total energy, within a given tolerance, with the cut-off energy was firstly conducted, showing that a value of 800 eV was adequate enough to ensure stress and energy values convergence. The k-point mesh for the Brillouin zone integration was selected according to the Monkhorst–Pack scheme with 6*6*6 Brillouin zone sampling. The nominal composition La9.33Si6O26 supposes that it exists one lanthanum vacancy in the structure per 3 unit cells. The presence of this lanthanum vacancy complicates the analysis since it breaks the overall symmetry. Thus, in order to keep the hexagonal symmetry to calculate the elastic properties, the lanthanum sites were thus kept fully occupied which leads to a nominal composition of La10Si6O26 per unit cell. From a solid state chemistry point of view, this corresponds to a situation where the original compound La10Si6O27 would have lost 1 oxygen atom (ideally the interstitial one), for instance in reducing conditions. The main advantage of such an approach is that, all along the analysis, we can perform the calculations in the original hexagonal cell with unit cell parameters a ≃ 9.8 Å and c ≃ 7.2 Å and thus keep a simplified elastic tensor. The elasticity tensor for a hexagonal
Chapter 4. Room-temperature mechanical characterization 113 phase only presents 5 independent elastic coefficients, while null and coupled coefficients exist due to symmetry as represented in Figure 4.11: Figure 4.11. Simplified scheme of the elastic tensor in hexagonal phase, where ()/ 11 12 XCC2 [24]. 4.3.1.2 DFT calculations for Yttrium-doped Barium Zirconates Calculations were performed using the code ABINIT. The interaction of electron-ion was taken into account here in the same form than for oxy-apatite. The wave functions were expanded in a set of plane waves up to a kinetic energy cut-off of 680 eV, which ensured a good convergence of energy and stress values. The k-point meshes were selected according to the Monkhorst-Pack scheme. Depending on the size of the system, containing respectively 5, 40 and 135 atoms, the Brillouin zone sampling was adapted to be 6*6*6, 4*4*4 and 2*2*2, respectively. Several calculations were performed to take into account the presence of defects like dopant ions, oxygen vacancies and protons. The main difficulty here lies in the choice of a system of limited size that would be representative of the whole disordered material. In particular, it is clear that the introduction of these defects breaks the original cubic symmetry of BaZrO3. 4.3.2 DFT calculation results 4.3.2.1 Elastic properties of Lanthanum Silicate Prior to the calculations of the elastic coefficients, we determined the ground state of the La10Si6O26 composition through DFT calculations. Lattice constants and internal positions in the perfect unit cell were fully optimized until the free energy difference between two optimisation runs was below 10-6 eV. We verified that the values of the stress components for this configuration were smaller than 0.005 GPa. The refined cell parameters after relaxation were a = 9.8259 Å and c = 7.2651 Å, which are in very good agreement (error ~1%) with the cell parameters a = 9.7248 Å and c = 7.1895 Å measured for La9.33Si6O26 at room temperature [25] and with a = 9.7393 Å and c = 7.2071 Å measured for La10Si6O27 [26].
Chapter 4. Room-temperature mechanical characterization 114 The elastic coefficients were then calculated considering 10 configurations for each of the specific stress-strain configurations. The resulting elastic tensor is the following: ij 66.4(4) 84.6(9) 0 0 0 66.4(4) 84.6(9) 0 0 0 84.6(9) 84.6(9) 194.1(7) 0 0 0 (G 0 0 0 49.9(9) 0 0 0 0 0 0 49 177.6 .9(9) (8) 177 0 0 0 0 0 0 .6(8) C P 55.6 a (6) ) These calculations reveal a slight anisotropy of the elastic tensor, in particular a ~8% difference for the elastic longitudinal response between a, b axes and c axes. We will see in the following chapter that this anisotropic elastic tensor coupled to the anisotropic thermal expansion is at the origin of the presence of residual stresses in oxy-apatites polycrystalline materials, in particular after sintering. Table 4.9 shows the elastic properties of lanthanum silicate polycrystals calculated by DFT calculations, which are comparable to the elastic coefficients mentioned above. Table 4.9. Elastic properties of lanthanum silicate polycrystals deduced from the elastic tensor calculated by DFT calculations. Averaging scheme Bulk modulus (GPa) Young’s modulus (GPa) Shear modulus (GPa) Poisson’s ratio Voigt 112.8 134.4 51.6 0.301 Reuss 111.7 133.6 51.4 0.300 Hill 112.0 134.0 51.5 0.301 4.3.2.2 Elastic properties of Y-doped Barium Zirconate Firstly, pure Barium Zirconate has been modelled. The material has cubic symmetry and the cell parameter as refined to be a = 4.235 Å. Different Y-doping levels have been then tested, where the compensating charge (usually oxygen vacancy) was in this case defined as a charge spreading over the whole supercell (jellium). Elastic properties were not calculated for dry BZY i.e. when the yttrium-dopant is compensated by an oxygen vacancy because it supposes to use a much bigger supercell. And more important, symmetry properties are fully lost in this case making the elastic tensor determination very complex (if not meaningless). BZY properties were nevertheless calculated in its wet state i.e. when the dopant is compensated by a proton, the oxygen lattice being in this case fully occupied. For wet BZY, the doping level was 12.5% and the proton was set at its
Chapter 4. Room-temperature mechanical characterization 115 more stable position, the first neighbour position in reference to the dopant as shown in previous calculations. The resume of these calculations are reported in Table 4.10. Table 4.10. Results of calculated cell parameters and elastic parameters for pure and Y-doped Barium Zirconate (the actual supercell has orthorhombic symmetry with a = 4.267 Å, b = 4.234 Å, c = 4.279 Å; the actual Young’s moduli along a, b and c axes are respectively 207, 209, 230 GPa). Doping level a cell parameter (Å) Young’s modulus (GPa) Poisson’s ratio Bulk modulus (GPa) Shear Modulus (GPa) 0 % 4.235 259 0.215 150.8 107 3.7 % 4.251 253 0.213 142.9 104 12.5 % 4.284 231 0.207 130.4 96 12.5% + H+ 4.260£ 215¥ These results clearly show that the doping with Yttrium tends to diminish the elastic coefficients, keeping almost constant the Poisson ratio. Moreover, the presence of protons tends to reduce even more the Young’s modulus. Further works are nevertheless needed to determine more efficiently and more precisely the elastic coefficients for large supercells, that would keep the observed cubic symmetry. This goes well beyond the objective of the current work. It seems nevertheless clear from these calculations that dry and wet BZY compounds should present different elastic coefficients. 4.4 REFERENCES 1. Pharr, G.M., Measurement of mechanical properties by ultra-low load indentation. Materials Science and Engineering: A, 1998. 253(1–2): p. 151-159. 2. Oliver, W.C. and G.M. Pharr, An improved technique for determining hardness and elastic modulus using load and displacement sensing indentation experiments. Journal of materials research, 1992. 7(06): p. 1564-1583. 3. Doerner, M.F. and W.D. Nix, A method for interpreting the data from depth-sensing indentation instruments. Journal of Materials research, 1986. 1(04): p. 601-609. 4. Oliver, W.C. and G.M. Pharr, Measurement of hardness and elastic modulus by instrumented indentation: Advances in understanding and refinements to methodology. Journal of materials research, 2004. 19(01): p. 3-20. 5. Leisure, R.G. and F. Willis, Resonant ultrasound spectroscopy. Journal of Physics: Condensed Matter, 1997. 9(28): p. 6001.
Chapter 4. Room-temperature mechanical characterization 116 6. Migliori, A., et al., Resonant ultrasound spectroscopic techniques for measurement of the elastic moduli of solids. Physica B: Condensed Matter, 1993. 183(1): p. 1-24. 7. Bernard, S., Q. Grimal, and P. Laugier, Resonant ultrasound spectroscopy for viscoelastic characterization of anisotropic attenuative solid materials. The Journal of the Acoustical Society of America, 2014. 135(5): p. 2601-2613. 8. Niihara, K., R. Morena, and D. Hasselman, Evaluation ofK Ic of brittle solids by the indentation method with low crack-to-indent ratios. Journal of Materials Science Letters, 1982. 1(1): p. 13-16. 9. Roa, J.J., et al., Nanohardness and Young's modulus of YBCO samples textured by the Bridgman technique. Nanotechnology, 2007. 18(38): p. 385701. 10. Milman, Y.V., А.А. Golubenko, and S.N. Dub, Indentation size effect in nanohardness. Acta Materialia, 2011. 59(20): p. 7480-7487. 11. Morales, M., et al., Mechanical properties at the nanometer scale of GDC and YSZ used as electrolytes for solid oxide fuel cells. Acta Materialia, 2010. 58(7): p. 2504-2509. 12. McColm, I.J., Ceramic hardness. 1990, New York: Plenum Press. 13. Santos, M., et al., Mechanical properties of sintered La9.33Si2Ge4O26 oxyapatite materials for SOFC electrolytes. Ceramics International, 2012. 38(8): p. 6151-6156. 14. Knott, J.F., Fundamentals of fracture mechanics. 1973: Gruppo Italiano Frattura. 15. Suarez, G., et al., Electrophoretic deposition for obtaining dense lanthanum silicate oxyapatite (LSO). Ceramics International, 2016. 42(16): p. 19283-19288. 16. Roa, J.J., et al., Determination of hardness, Young's modulus and fracture toughness of lanthanum tungstates as novel proton conductors. Ceramics International, 2011. 37(5): p. 1593-1599. 17. Cook, R.F. and G.M. Pharr, Direct Observation and Analysis of Indentation Cracking in Glasses and Ceramics. Journal of the American Ceramic Society, 1990. 73(4): p. 787-817. 18. Sazinas, R., M.-A. Einarsrud, and T. Grande, Toughening of Y-doped BaZrO3 proton conducting electrolytes by hydration. Journal of Materials Chemistry A, 2017. 5(12): p. 5846-5857. 19. Vassen, R., et al., Zirconates as New Materials for Thermal Barrier Coatings. Journal of the American Ceramic Society, 2000. 83(8): p. 2023-2028. 20. Sholl, D. and J.A. Steckel, Density functional theory: a practical introduction. 2011: John Wiley & Sons. 21. Perdew, J.P. and S. Kurth, Density functionals for non-relativistic Coulomb systems in the new century, in A primer in density functional theory. 2003, Springer. p. 1-55. 22. Fiolhais, C., F. Nogueira, and M.A. Marques, A primer in density functional theory. Vol. 620. 2003: Springer Science & Business Media.
Chapter 4. Room-temperature mechanical characterization 117 23. Kresse, G. and D. Joubert, From ultrasoft pseudopotentials to the projector augmentedwave method. Physical Review B, 1999. 59(3): p. 1758. 24. Nye, J.F., Physical properties of crystals: their representation by tensors and matrices. 1985: Oxford university press. 25. Sansom, J., D. Richings, and P. Slater, A powder neutron diffraction study of the oxide-ion- conducting apatite-type phases, La 9.33 Si 6 O 26 and La 8 Sr 2 Si 6 O 26. Solid State Ionics, 2001. 139(3): p. 205-210. 26. Chesnaud, A., et al., Influence of synthesis route and composition on electrical properties of La9.33 + xSi6O26 + 3x/2 oxy-apatite compounds. Solid State Ionics, 2008. 179(33–34): p. 1929-1939.
Chapter 4. Room-temperature mechanical characterization 118
119 Chapter 5 THERMO-MECHANICAL CHARACTERIZATION Contents 5.1 Introduction ................................................................................................................................... 120 5.2 Experimental characterization of thermo-mechanical properties ................................................... 120 5.2.1 Experimental procedure ................................................................................................ 120 5.2.1.1 High-temperature X-Ray diffraction ...................................................................... 121 5.2.1.2 Thermo-mechanical analysis .................................................................................. 121 5.2.1.3 High-temperature Resonant Ultrasound Spectroscopy ........................................ 122 5.2.2 Experimental results ...................................................................................................... 123 5.2.2.1 Thermo-mechanical properties of Lanthanum Silicate ......................................... 123 5.2.2.1.1 Coefficient of thermal expansion ............................................................... 123 5.2.2.1.2 Elastic constants ......................................................................................... 125 5.2.2.2 Thermo-mechanical properties of Yttrium-doped Barium Zirconate ................... 126 5.2.2.2.1 Coefficient of thermal expansion ............................................................... 126 5.2.2.2.2 Elastic constants ......................................................................................... 128 5.3 Numerical simulation of residual stresses state in lanthanum silicate ............................................ 129 5.3.1 Computation procedure ................................................................................................ 130 5.3.1.1 Description of microstructure ................................................................................ 130 5.3.1.2 Numerical simulations ............................................................................................ 132 5.3.1.2.1 Material properties .................................................................................... 132 5.3.1.2.2 Loading and boundary conditions ............................................................. 133 5.3.1.3 Analysis of Stress fields: Localization and prediction of fracture .......................... 136 5.3.1.3.1 Maximum principal stress theory .............................................................. 136 5.3.1.3.2 Stress intensity approach ........................................................................... 137 5.3.1.4 Strategy of Simulations .......................................................................................... 138 5.3.1.4.1 Determination of the Mesh Size ................................................................ 138 5.3.1.4.2 Multiple realizations .................................................................................. 139 5.3.2 Computation results ...................................................................................................... 140
Chapter 5. Thermo-mechanical characterization 120 5.3.2.1 Distribution of stresses ................................................................................................140 5.3.2.2 Prediction of failure .....................................................................................................143 5.4 References ................................................................................................................................... 145 5.1 INTRODUCTION This chapter studies the influence of the temperature on the mechanical properties, including the coefficient of thermal expansion and elastic constants, of Lanthanum Silicates and Yttrium-doped Barium Zirconate. Besides the characterization of the materials as a function of temperature, this information is useful to simulate their behaviour and understand their mechanical response, which is particularly interesting in the case of oxy-apatite because of its anisotropic thermo-elastic properties. The last part of this chapter is therefore focused on studying the residual stress state of this material by finite elements numerical simulations, in order to get a deeper understanding of the potential failure mechanisms and to improve the fabrication processes and applications. 5.2 EXPERIMENTAL CHARACTERIZATION OF THERMO-MECHANICAL PROPERTIES 5.2.1 Experimental procedure In this study, the coefficient of thermal expansion was experimentally determined at atomic and macroscopic scales by high-temperature XRD and thermo-mechanical analysis, respectively, while the temperature dependence of Young’s modulus, Poisson ratio and shear modulus was measured by high-temperature RUS. The macroscopic temperature dependence of the thermal expansion coefficient and elastic constants of samples was determined considering the materials to be isotropic, as the grains are randomly oriented in the samples. However, HT-XRD allows to evaluate the possible anisotropic evolution of the coefficient of thermal expansion at the crystal scale, which is especially interesting in the case of the Lanthanum silicate due to its anisotropic nature. Experiments were carried out in air on specimens of approximately 5 x 3 x 3 mm3 in size which were cut from the sintered pellets with a low-speed diamond saw. After cutting, the samples were rectified to eliminate imperfections and to ensure completely flat-parallel surfaces to avoid wrong estimations of the mechanical parameters.
Chapter 5. Thermo-mechanical characterization 121 5.2.1.1 High-temperature X-Ray diffraction The linear thermal expansion coefficient (α) of the different materials was measured by means of high-temperature X-Ray diffraction. XRD analysis was carried out on a Bruker D8C diffractometer (X- ray Laboratory, CITIUS, University of Seville, Spain) with Ni-filtered Cu-Kα radiation (λ = 1.54060 Å) in Bragg-Brentano configuration and equipped with an Anton Paar XRK 900 high-temperature chamber. Measurements were carried out on LSO calcined nanopowders and BZY sintered ceramics from room temperature up to 900 °C with heating and cooling ramps of 10 °C/min. Data were collected every 50 °C at constant temperature during the heating/cooling ramps in the 2θ region between 20° and 90° in steps of 0.02° and an acquisition time of 0.2 s/step. Recorded XRD spectra were analyzed by the Le Bail refinement method [1] using the TOPAS 4.2 Bruker AXS software package . The coefficient of thermal expansion was determined from the relative change in unit cell parameter with temperature: XRD o 1Δa α= aΔT (5. 1) where Δa is the variation of the unit cell parameter corresponding to a temperature change ΔT, and ao is the lattice parameter at room temperature. In the case of LSO, both cells parameters a and c can be evaluated with this method in order to study the anisotropic thermal behaviour of a single crystal. 5.2.1.2 Thermo-mechanical analysis The thermal expansion coefficient was also evaluated by thermo-mechanical analysis, a technique used to measure macroscopic dimensional changes of a material as a function of temperature. Measurements were performed using a TMA Q1000 Thermo-mechanical analyzer (Functional Characterization Laboratory, CITIUS, University of Sevilla, Spain) from room temperature up to 1000 °C with heating/cooling ramps at 5 °C/min. Measurements were carried out at a constant load of 500 mN. For the macroscopic case, bulk specimen is isotropic, and Equation 5.1 can be rewritten as: TMA 0 1ΔL α = LΔT (5.2)
Chapter 5. Thermo-mechanical characterization 128 Figure 5.6. Relative thermal expansion of BZY and BZY-NiO as a function of temperature. 5.2.2.2.2 Elastic constants Figure 5.7 shows the variations of the Young’s modulus, Poisson ratio and shear modulus of home-made BZY with temperature. Both elastic moduli decrease with increasing temperature, while the Poisson ratio remains once more practically constant. The same behaviour was found in the oxyapatite. As can be observed in Figure 5.7a, the Young’s modulus decreases from 204 to 176 GPa in the range of temperatures from 288 to 1300 K, which means a drop of about 13%. The shear modulus decreases from 82 to 71 GPa, exhibiting also a reduction of 13% in the same range of temperatures (Figure 5.7c). These results are again in good agreement with the expected reduction of about 1% for each 100 K of temperature increase [8]. As discussed previously for the case of the oxy-apatite, the Poisson ratio follows the relative change between E and G with temperature (Equation 5.3), thus remaining constant with a value of 0.24 ± 0.01 (Figure 5.7b). This result is identical to that of BZY measured at room temperature in our laboratory (Chapter 4), confirming the excellent reproducibility of the results. K-1 K-1
Chapter 5. Thermo-mechanical characterization 129 Figure 5.7. Temperature dependence of (a) Young’s modulus, (b) Poisson ratio and (c) shear modulus of BZY. The uncertainty is about 7% in Young’s modulus, 8% in the Poisson ratio and 0.3% in the shear modulus. 5.3 NUMERICAL SIMULATION OF RESIDUAL STRESSES STATE IN LANTHANUM SILICATE Many physical phenomena that occur in a polycrystalline material are intimately related with the local mechanical fields developed in its microstructure. It is well-known that the distribution of these mechanical stress fields depend on the polycrystal morphology, orientation grain distribution and crystal behaviour of the material. These microstructural factors mainly control the global behaviours of the material and are generally used to predict local phenomena such as fracture [17]. In brittle materials, fracture is governed by the opening of local cracks which spread through the material causing the macroscopic failure. In some polycrystalline ceramics, such as Lanthanum silicate, crack initiation might be sensitive to the residual stress localization developed along the grains boundaries which come from the crystalline anisotropy of elastic constant and thermal expansion [18]. Therefore, it is of high relevancy to evaluate the stress fields developed between individual crystals in order to be able to predict the mechanical failure of the material. In this context, finite elements
Chapter 5. Thermo-mechanical characterization 130 method appears as a very efficient tool to simulate the mechanical behaviour of a polycrystalline aggregate taking into account microstructural and structural details of the material. The main objective of this section is to characterize the residual stress state and to predict the fracture probability in Lanthanum Silicates for a given thermo-mechanical conditions by using finite elements numerical simulation. This study uses methods proposed in the work of Kanit et al. [19], where finite elements numerical simulation was used to determine the effective properties of a specific random microstructure generated by Voronoi tessellations. 5.3.1 Computation procedure In order to obtain realistic results of the state of stress in oxy-apatite ceramics from simulations which could be used to understand the experimental failure of the material, it was necessary to create a polycrystal as similar as possible to the original compound and to submit it to the “same conditions” of sintering and compression testing that were used experimentally. The model chosen for the description of microstructure, material properties and experimental conditions used in this study are briefly described below. 5.3.1.1 Description of microstructure For the purpose of simulating microstructure, it may be possible to employ real microstructure obtained directly by experimental three-dimensional reconstructions from samples using Electron Back-Scatter Diffraction measurements [20-22] or Diffraction Contrast Tomography (DCT) [23-26]. However, these methods are lengthy and expensive since a sophisticated experimental facilities are required. As an alternative, computational methods have been developed to create artificial microstructures at a lower time-consuming and cost. It is in this point where finite element method based on the Voronoi cells was developed by Ghosh and Moorthey et al. [27]. In this work, the representation of the grains in a polycrystal was performed by a threedimensional Voronoï mosaic. This choice was motivated by the fact that the oxy-apatite exhibits a simple microstructure with only one phase and a uniform distribution of the grains with defect-free and equiaxial grains as mentioned previously (see Chapter 3).
Chapter 5. Thermo-mechanical characterization 131 The principle of construction of the Voronoi tessellations is based on proximity to a given set of points to divide the space into regions. These points, called seeds, are randomly distributed in space. For a finite set of seeds S1, S2, S3 … it is possible to make partitions of the space into cells (grains) C1, C2, C3… depending on the distance that every point M in the volume has to the seeds, taking into account that M belongs to Ci if it is closer to Si than to any Sj (j≠i). The points which are equidistant to the two nearest seeds form a line called half-space (grain boundary). The Voronoi cells Ci are defined by the intersection of several half-spaces as a polyhedron (Figure 5.8). Figure 5.8. 2D Voronoi mosaic of seven random seeds (S) with their corresponding cells. Figure 5.9. 3D Voronoi tessellations of 200 cells [17].
Chapter 5. Thermo-mechanical characterization 132 In the generation of a polycrystal as Voronoi tessellation was necessary to define the number of grains, which were created according to a uniform distribution that was similar to the grain size distribution found for Oxy-apatite (Section 3.3.1.4). Then, the mesh size was imposed and the tessellation was optimized regarding to the element size by removing the smallest edges and faces in order to improve the quality of the mesh. The generation of polycrystals and meshing was conducted with Neper software [17]. 5.3.1.2 Numerical simulations Based on the obtained polycrystal, the numerical simulations were performed using the finite element method. For each grain, was imposed a random orientation defined by Euler angles of a random isotropic crystallographic texture. Euler angles determine the orientation of one grain with respect to the reference system of the aggregate. Moreover, other input parameters were defined such as material properties (taking into account potential anisotropies) and loading and boundary conditions, which are briefly described below. The numerical simulations were conducted with Abaqus. 5.3.1.2.1 Material properties As indicated in Chapter 4, Lanthanum Silicate can be approximately described as an orthotropic material due to the hexagonal symmetry of the oxy-apatite crystal structure (hexagonal cells can be also expressed in an orthotropic lattice by using a’ = a, b’ = 2b+a, c’ = c). In order to characterize the residual stresses state in LSO, its thermo-elastic properties had to be defined. For this purpose, the full elastic tensor was taken from DFT calculation at 0 K (Section 4.4.1) while the anisotropy thermal expansion coefficients were taken from literature date, where Fukuda et al. [3] found that the linear expansion coefficient of the a-axis was 6.8(3) x 10-6 K-1 and that of the c-axis was 2.9(4) x 10-6 K-1 in the temperature range of 298 to 573 K. The choice of these thermal expansion coefficients at low temperature was motivated by the fact that we did not perform yet HT XRD characterization when these computations were realized. The idea was then to make first simulations to evaluate the method and the order of magnitude of the results. Currently, new calculations are being done using our own data of thermal expansion and reasonable evolution of elastic tensor evolution with temperature based on our RUS data. Therefore, based on the results presented in Section 0 about the evolution of E and α of polycrystalline material with temperature, it must be clarified that the numerical simulations
Chapter 5. Thermo-mechanical characterization 133 presented here were carried out in the extreme case of the highest anisotropy in particular concerning thermal expansion coefficients. 5.3.1.2.2 Loading and boundary conditions Two different loading conditions were applied to the aggregate in this work: thermal (th) and thermal-mechanical loading (th-m). The interest of choosing these loadings lies in the fact that the material is subjected to these conditions during sintering and during its use as electrolyte for SOFCs. In order to analyze separately the effect of both loading conditions in the state of stress of LSO, two different steps were defined. In the first step, a decrease in temperature from 1500 °C was imposed to simulate the sintering process, while in the second step mechanical loading was applied, which consisted in a compression pressure of 450 MPa (similar to some of the working conditions for the electrolyte part in Solid Oxide Cells devices [28]). Considering a LSO polycrystal of a given volume element V, two types of boundary conditions, kinematic and uniform boundary conditions, were imposed in order to characterize its overall residual stresses state, since previous works showed that the actual behaviour lies between those induce by these two boundary conditions [29, 30]. The surfaces and the boundary conditions are summarized in Table 5.1. Kinematic boundary conditions (KBC): 1. Thermal loading: The displacement u is imposed on all the surfaces. There is no displacement normal to surfaces S1, S2 and S3 (see Table 5.1 for the labels of surfaces). 1 2 3 i M S ,S ,S u(M) n =0 (5.4) where ni is the normal to surface Si. Besides, in order to keep all the surfaces plane and parallel to themselves during the loading, the following condition is imposed on the three other surfaces: 4 5 6 i i M S ,S ,S u (M) n =u (A) n (5.5) where A is the intersection of surfaces S4, S5 and S6.
Chapter 5. Thermo-mechanical characterization 134 Under this conditions a thermal loading was imposed: M V ΔΤ(M)= -1500 (5.6) 2. Thermo-mechanical loading: Keeping the boundary conditions of the thermal step still applied, a pressure p of 450 MPa is added on surface S1: 11 σ n = -p n (5.7) Static boundary conditions (SBC): 1. Thermal loading: A pressure equal to 0 is imposed on all the surfaces: i i M S σ n = 0 (5.8) Then, the same thermal loading than in the previous case (Equation 5.6) was applied. 2. Thermo-mechanical loading: A pressure of 450 MPa is added on surfaces S1 and S6 (keeping once again the boundary condition of thermal step applied): i i i 1 6 16 M S ,S σ n = -p n n =n ,n (5.9) It is necessary to clarify that during these two steps and in order to avoid rigid body motion, on three points, B, C and D which correspond to three corners belonging to S6, the following displacements are also imposed: u (B)= 0 u (C) x = 0 u (C) y = 0 u (D) y = 0 (5.10)
Chapter 5. Thermo-mechanical characterization 135 Table 5.1. Boundary conditions applied for the different loading steps. Kinematic (KBC) and Static boundary conditions (SBC). BC Thermal step Mechanical step K B C M V ΔΤ(M)= -1500 M V ΔΤ(M)= -1500 S B C u (B)= 0 u (C) x = 0 u (C) y = 0 u (D) y = 0 M V ΔΤ(M)= -1500 2 3 i 4 5 6 i i yy 1 M S ,S u (M) n = 0 M S ,S ,S u (M) n = u (A) n M S σ n = -450 n S5 S3 S4 S1 S6 S2 1 2 3 i 4 5 6 i i M S ,S ,S u (M) n =0 M S ,S ,S u (M) n =u (A) n B C D 2 3 4 5 i yy 16 M S ,S ,S ,S u(M) n = 0 M S ,S σ n = -450 n ii i M S σ n = 0 n S1 S3 S4 S2 S5 S6 D B C u (B)= 0 u (C) x = 0 u (C) y = 0 u (D) y = 0 M V ΔΤ(M)= -1500
Chapter 5. Thermo-mechanical characterization 136 5.3.1.3 Analysis of Stress fields: Localization and prediction of fracture 5.3.1.3.1 Maximum principal stress theory The interest for studying the state of stress in a material lies in the possibility to determine a failure criterion. The stress state at a point M of a material is given by the stress tensor which is defined by only six independent stress components: three normal components which define the normal component of the stress vector applied to surfaces normal to X, Y or Z and three shear components which characterize the tangential components of the stress vector applied to the same surface (Figure 5.10). Knowing this stress tensor, it is possible to calculate the stress vector applied on every surface passing through point M. Due to the local equilibrium, the stress tensor is symmetrical. Figure 5.10. Stress components. The values of these components depend on the coordinate system orientation in which the tensor is written so, for a particular orientation, it is possible to define a coordinate system (oriented to the eigen-vectors of σ ), in which σ is given by: xx yy zz σ 0 0 σ = 0 σ 0 00σ (5.11) where the normal components become to the principal stresses. Normal components: ,, xx yy zz Shear components: , , , , , xy yx xz zx yz zy Z X Y M
Chapter 5. Thermo-mechanical characterization 137 For brittle materials, failure is governed by opening of cracks, which depends on the stress intensity factor applied to the crack and then, to the normal stress applied on the plane of the crack. There are numerous proposed theories to predict material failure. However the maximum principal stress is the criterion mostly used to predict the failure of brittle materials, since cracks initiate where the principal stress is maximum and typically propagate perpendicularly to the principal stress direction [31]. The maximum principal stress I can be defined in 2D as: 22 xx yy xx yy xy I 11 σ = (σ +σ )+ σ +σ +4τ 22 (5.12) According to the maximum principal stress theory [32], failure occurs in brittle materials with a certain probability (modelled by Weibull theory) once the maximum principal stress exceeds the value of the maximum strength in simple tension. In this work, all the analyses of the state of stress in finite element numerical simulations were carried out according to this criterion. 5.3.1.3.2 Stress intensity approach Stress localizations are usually discussed in terms in which a flaw is introduced into a body that was under uniform stress. In this context, the stress intensity factor K is one of the most fundamental parameters used in fracture mechanics [33, 34] to characterize the stress state near the crack-tip caused by an uniform load or residual stresses in a linear elastic material [34]. Figure 5.11. Schematic representation of a through crack of length a in an infinite plane subject to an uniform stress σ.
Chapter 5. Thermo-mechanical characterization 144 the bulk proportionally increases and the type of boundary conditions imposed is of less importance. Results tend to converge towards the same values for large volumes, independently from the boundary conditions. The probability of failure increase when the mechanical loading is applied, what are in good agreement with the stronger localizations after the mechanical step already analyzed in Figure 5.13 and Figure 5.14. Figure 5.17. Mean volume fraction of elements subjected to stresses higher than 600 MPa and standard deviation of mean values as function of volume size for the different boundary conditions. (a) thermal and (b) thermo-mechanical loading. Prediction of failure was performed from the stress intensity factor taking into account the criterion of 600 MPa and fracture toughness of Lanthanum silicate obtained experimentally in this work (section 4.3.1), where a value of KIC = 1.2 ± 0.1 MPa m1/2 were found. From Equation 6.1 a value of a = 0.98 µm was determined, what indicates that any crack in the material of 1.96 µm in length (2a) could propagate and lead to material failure if the stress concentration near the crack-tip exceeded the criterion of 600 MPa. Another way of having a non-local approach to failure is to consider, not only the stress distribution of elements subjected to a high level of stress but also of grains. Stress tensor was averaged in every grain and the maximum principal stress of the mean stress tensor was calculated. Figure 5.18 shows the volume fraction of grains in which the maximal principal stress is greater than 100 MPa for the different loading and boundary conditions as a function of volume size. Once again the standard deviation of mean value becomes smaller and the results converge towards the same value when the a) b)
Chapter 5. Thermo-mechanical characterization 145 volume size increases. Considering the total volume fraction of 1000 grains as 1, these results indicate that about 79% and 86% of grains were subjected to stresses higher than 100 MPa after the thermal and mechanical loading, respectively. A parallel study in the same conditions indicated that only about 23% and 34% of grains were subjected to stresses higher than 200 MPa while it was not found stressed grains at stress levels higher than 400 MPa, due to this it was not possible to apply the same criterion used above for the volume fraction of elements. Figure 5.18. Mean values of volume fraction of grains subjected to stresses higher than 100 MPa and standard deviation of mean values as function of volume size for the different boundary conditions. (a) thermal and (b) thermo-mechanical loading. When considering stresses averaged over grains, the difference between the two loadings applied (thermal and thermal-mechanical loading) is very low. This averaging is probably too rough to be able to distinguish both contribution. Due to this, the first criterion should be kept in the future. 5.4 REFERENCES 1. Le Bail, A., Whole powder pattern decomposition methods and applications: A retrospection. Powder Diffraction, 2012. 20(4): p. 316-326. 2. Carpenter, M.A. High-Temperature Resonant Ultrasound Spectroscopy. University of Cambridge. 3. Fukuda, K., T. Asaka, and T. Uchida, Thermal expansion of lanthanum silicate oxyapatite (La9.33+2x(SiO4)6O2+3x), lanthanum oxyorthosilicate (La2SiO5) and lanthanum sorosilicate (La2Si2O7). Journal of Solid State Chemistry, 2012. 194: p. 157-161. a) b)
Chapter 5. Thermo-mechanical characterization 146 4. Iwata, T., et al., Structural change of oxide-ion-conducting lanthanum silicate on heating from 295 to 1073 K. Solid State Ionics, 2007. 178(27): p. 1523-1529. 5. Jiang, S.P., et al., Synthesis and characterization of lanthanum silicate apatite by gel-casting route as electrolytes for solid oxide fuel cells. Journal of Power Sources, 2009. 189(2): p. 972- 981. 6. Gauckler, L.J., et al., Solid oxide fuel cells: systems and materials. CHIMIA International Journal for Chemistry, 2004. 58(12): p. 837-850. 7. Yokokawa, H., et al., Electrolytes for solid-oxide fuel cells. MRS bulletin, 2005. 30(8): p. 591-595. 8. Wachtman, J.B., W.R. Cannon, and M.J. Matthewson, Mechanical properties of ceramics. 2009, Hoboken, N.J.: Wiley. 9. Ren, F., et al., The high-temperature elastic moduli of polycrystalline PbTe measured by resonant ultrasound spectroscopy. Acta Materialia, 2008. 56(20): p. 5954-5963. 10. Soga, N., E. Schreiber, and O.L. Anderson, Estimation of bulk modulus and sound velocities of oxides at very high temperatures. Journal of Geophysical Research, 1966. 71(22): p. 5315-5320. 11. Fukuhara, M. and I. Yamauchi, Temperature dependence of the elastic moduli, dilational and shear internal frictions and acoustic wave velocity for alumina, (Y)TZP and β′-sialon ceramics. Journal of Materials Science, 1993. 28(17): p. 4681-4688. 12. Han, D., N. Hatada, and T. Uda, Chemical Expansion of Yttrium-Doped Barium Zirconate and Correlation with Proton Concentration and Conductivity. Journal of the American Ceramic Society, 2016. 99(11): p. 3745-3753. 13. Gladysz, G.M. and K.K. Chawla, Coefficients of thermal expansion of some laminated ceramic composites. Composites Part A: Applied Science and Manufacturing, 2001. 32(2): p. 173-178. 14. Yamanaka, S., et al., Thermochemical and thermophysical properties of alkaline-earth perovskites. Journal of Nuclear Materials, 2005. 344(1): p. 61-66. 15. Yamanaka, S., et al., Thermophysical properties of BaZrO3 and BaCeO3. Journal of Alloys and Compounds, 2003. 359(1): p. 109-113. 16. Lyagaeva, J., et al., A detailed analysis of thermal and chemical compatibility of cathode materials suitable for BaCe0.8Y0.2O3−δ and BaZr0.8Y0.2O3−δ proton electrolytes for solid oxide fuel cell application. International Journal of Hydrogen Energy, 2017. 42(3): p. 1715-1723. 17. Quey, R., P.R. Dawson, and F. Barbe, Large-scale 3D random polycrystals for the finite element method: Generation, meshing and remeshing. Computer Methods in Applied Mechanics and Engineering, 2011. 200(17): p. 1729-1745. 18. Yousef, S.G., et al., Microcrack Evolution in Alumina Ceramics: Experiment and Simulation. Journal of the American Ceramic Society, 2005. 88(10): p. 2809-2816.
Chapter 5. Thermo-mechanical characterization 147 19. Kanit, T., et al., Determination of the size of the representative volume element for random composites: statistical and numerical approach. International Journal of Solids and Structures, 2003. 40(13): p. 3647-3679. 20. Brands, D., et al., On the Reconstruction and Computation of Dual-Phase Steel Microstructures Based on 3D EBSD Data. PAMM, 2011. 11(1): p. 503-504. 21. Schwartz, J., O. Fandeur, and C. Rey, Numerical approach of cyclic behaviour of 316LN stainless steel based on a polycrystal modelling including strain gradients. International Journal of Fatigue, 2013. 55: p. 202-212. 22. Brands, D., et al., Computational modeling of dual-phase steels based on representative threedimensional microstructures obtained from EBSD data. Archive of Applied Mechanics, 2016. 86(3): p. 575-598. 23. Ludwig, W., et al., New opportunities for 3D materials science of polycrystalline materials at the micrometre lengthscale by combined use of X-ray diffraction and X-ray imaging. Materials Science and Engineering: A, 2009. 524(1): p. 69-76. 24. Proudhon, H., et al., Coupling Diffraction Contrast Tomography with the Finite Element Method Advanced Engineering Materials, 2016. 18(6): p. 903-912. 25. Peetermans, S., et al., Cold neutron diffraction contrast tomography of polycrystalline material. Analyst, 2014. 139(22): p. 5765-5771. 26. Thomas J. Marrow, A.K., P. Reischig, S. Rolland du Roscoat, W. Ludwig, Diffraction contrast tomography of polycrystalline alumina. 2009. 27. Ghosh, S. and S. Moorthy, Elastic-plastic analysis of arbitrary heterogeneous materials with the Voronoi Cell finite element method. Computer Methods in Applied Mechanics and Engineering, 1995. 121(1): p. 373-409. 28. Nakajo, A., et al., Mechanical reliability and durability of SOFC stacks. Part I : Modelling of the effect of operating conditions and design alternatives on the reliability. International Journal of Hydrogen Energy, 2012. 37(11): p. 9249-9268. 29. Huet, C., Application of variational concepts to size effects in elastic heterogeneous bodies. Journal of the Mechanics and Physics of Solids, 1990. 38(6): p. 813-841. 30. Hazanov, S. and C. Huet, Order relationships for boundary conditions effect in heterogeneous bodies smaller than the representative volume. Journal of the Mechanics and Physics of Solids, 1994. 42(12): p. 1995-2011. 31. Wang, J., et al., Maximum mean principal stress criterion for three-dimensional brittle fracture. International Journal of Solids and Structures, 2016. 102: p. 142-154. 32. Rankine, W.J.M., On the Stability of Loose Earth. Philosophical Transactions of the Royal Society of London, 1857. 147: p. 9-27.
Chapter 5. Thermo-mechanical characterization 148 33. Zhu, X.-K. and J.A. Joyce, Review of fracture toughness (G, K, J, CTOD, CTOA) testing and standardization. Engineering Fracture Mechanics, 2012. 85: p. 1-46. 34. Anderson, T.L. Fracture mechanics : fundamentals and applications. 2005.
149 Chapter 6 HIGH-TEMPERATURE MECHANICAL CHARACTERIZATION Contents 6.1 Introduction ................................................................................................................................... 150 6.2 Working conditions experiments (T = 700 °C) ................................................................................... 150 6.2.1 Experimental procedure .......................................................................................... 150 6.2.2 Experimental results ................................................................................................ 151 6.2.2.1 Mechanical response of Lanthanum Silicates in SOFC WCs ........................... 151 6.2.2.2 Mechanical response Yttrium-doped Barium Zirconate in PCFC WCs ........... 151 6.3 Creep experiments (T > 1000 °C) ....................................................................................................... 156 6.3.1 Experimental procedure .......................................................................................... 156 6.3.1.1 Mechanical magnitudes ................................................................................... 157 6.3.1.2 High-temperature mechanical tests ................................................................ 159 6.3.1.3 Steady-state deformation ................................................................................ 160 6.3.1.4 Determination of creeps parameters .............................................................. 161 6.3.1.4.1 Conventional method ........................................................................... 162 6.3.1.4.2 Differential method .............................................................................. 162 6.3.2 Experimental results ................................................................................................ 163 6.3.2.1 High-temperature mechanical behavior of LSO-CS ........................................ 163 6.3.2.1.1 Fragile-ductile transition ...................................................................... 163 6.3.2.1.2 Microstructure after deformation ....................................................... 165 6.3.2.1.3 Creep parameters ................................................................................ 170 6.3.2.1.4 High-temperature deformation mechanism ....................................... 176 6.3.2.2 High-temperature mechanical behavior of LSO-SPS ...................................... 178 6.3.2.2.1 Fragile-ductile transition ...................................................................... 178 6.3.2.2.2 Microstructure after deformation ....................................................... 180 6.3.2.2.3 Creep parameters ................................................................................ 182 6.3.2.2.4 High-temperature deformation mechanism ....................................... 187 6.3.2.3 High-temperature mechanical behavior of BZY .............................................. 189 6.3.2.3.1 Fragile-ductile transition ...................................................................... 189
Chapter 6. High-temperature mechanical characterization 150 6.3.2.3.3 Creep parameters ................................................................................ 193 6.3.2.3.4 High-temperature deformation mechanism ....................................... 199 6.4 References ................................................................................................................................... 202 6.1 INTRODUCTION This chapter focuses on the study of the mechanical behaviour of Lanthanum Silicate and Yttrium-doped Barium Zirconate materials at intermediate and high temperatures. On one hand, compressive mechanical tests have been carried out in conditions similar to SOFC/PCFC operating conditions to check the response of the different materials for applications as electrolytes. On the other hand, creep experiments were performed to identify the atomistic mechanisms of plastic deformation and the origin of failure of these materials at high temperatures. 6.2 WORKING CONDITIONS EXPERIMENTS (T = 700 °C) Mechanical essays in working conditions were performed with specimens of approximately 5 x 3 x 3 mm3 in size which were cut from the sintered pellets with a diamond saw. After cutting, the samples were rectified to eliminate imperfections and to ensure that they were completely flatparallel. The experiments were carried out in compression on a universal deformation machine (Microtest, University of Seville, Spain) equipped with a controlled-atmosphere system and alumina cylindrical dies of 25 mm in diameter and 300 mm in height. The tests were performed under constant load at 700 °C in different atmospheres i.e. dry air, dry argon and dry 5% hydrogen in Argon (residual water is as much of few ppm). Nominal stresses between 100 and 550 MPa were applied to the samples, according to the stresses estimated for electrolytes in SOFC operating conditions [1, 2] The atmosphere was controlled by monitoring the gas flow in the chamber, which was fixed at 400 ml/min, and the temperature of 700 °C was chosen as a typical operating temperature of PCFCs. The samples were heated in air at a rate of 10 °C/min up to the target temperature of 700 °C, where a 2 h dwell was used to ensure the equilibrium of the machine/sample assembly; a small load of 2 MPa was applied during the heating process to avoid the loss of contact between sample and alumina dies. Then, the samples were loaded at a constant
Chapter 6. High-temperature mechanical characterization 151 cross-head speed of 10 µm/min up to the desired final stress, where the atmosphere was successively changed from air to argon and finally to 5% H2/95% Ar. 6.2.2.1 Mechanical response of Lanthanum Silicates in SOFC working conditions Both conventionally sintered and SPS oxy-apatites were subjected to this kind of experiments at 150, 300 and 450 MPa, and their stress responses are displayed in Figure 6.1. Both materials exhibit the same behaviour, remaining intact throughout the atmosphere changes, indicating that they did not undergo any significant mechanical-chemical degradation during testing. Figure 6.1. Stress response during compression tests at 700 °C under various atmospheres of (a) LSOCS, and (b) LSO-SPS. 6.2.2.2 Yttrium-doped Barium Zirconate Figure 6.2 shows the results of the mechanical tests performed on BZY and BZY-NiO. The former material behaves identical to the oxy-apatites, remaining unaffected by the surrounding atmosphere. The same behaviour was also found in BZY-NiO at stresses lower than 300 MPa. However, when the stress level increased up to 350 MPa, the specimens stayed intact under air and argon, but failed catastrophically after about 10 min under H2 atmosphere. Identical behaviour was found at 560 MPa. The samples literally exploded into many small fragments. These results indicate that the commercial material underwent severe modifications under hydrogen atmosphere at 700 °C, which favours crack formation and propagation and final sample failure. This
Chapter 6. High-temperature mechanical characterization 152 point is crucial for fuel cell applications since the observed compressive stress at which failure occurs (350 MPa and above) is within the stress range estimated for the electrolyte part under typical SOFC operating conditions (from 140 [2] to 450 MPa [1]). Figure 6.2. Stress response during compression tests at 700 °C under various atmospheres for (a) BZY, and (b) BZY-NiO. In order to better understand the failure mechanism of these samples prepared with NiO additive, HR-TEM studies were carried out. Because of the lack of information by the supplier, the original BZY-NiO material was firstly investigated. Figure 6.3. EDS mapping of original BZY-NiO particles. (a) HAADF image, and EDS filtered images for elements: (b) Ni, (c) O, (d) Ba, (e) Zr and (f) Y. a) b) c) d) e) f) (1) (2) (3) (2)
Chapter 6. High-temperature mechanical characterization 153 Figure 6.3 shows an example of EDS image which helps identifying where the Ni element locates. Particle #1, as identified on the HAADF image, would correspond to BaZr0.85Y0.15O2.925 phase, while particles #2 and #3 contains only Ni and O species, and would correspond to NiO. EELS in STEM mode was used to obtain high-resolution information about the material composition. The fine electronic structure of Ni-rich particles was studied by EELS at Oxygen K edge and Nickel L2,3-edges. Figure 6.4b and c shows the O-K and Ni-L2,3 edge spectra after background subtraction obtained for the Ni-rich particle #3 in the area marked with a circle in Figure 6.4a. For an appropriate comparison, similar analyses were also performed on pure NiO (Sigma Aldrich), which has been used as a reference sample (Figure 6.4b and c). The O-K edge ELNES (electron energy loss near-edge structure) of NiO (Figure 6.4 b) consists of five major peaks at 532, 538, 541, 547, and 562 eV. The first peak can be attributed to transitions from O 1s core states to the band mainly consisting of Ni-3d orbitals. The next three peaks at 535 - 550 eV correspond to transitions to the Ni-4sp band, and the last peak results from multiple scattering within oxygen shells [3, 4]. On the other hand, Ni-L2,3 edges ELNES (Figure 6.4c) consists of two peaks resulting from spin-orbit coupling: L3is the main and most intense peak and comes from 2p3/2 transitions; and L2 is the peak at higher energy loss and less intense, coming from 2p1/2 transitions. The position and shape of these contributions are sensitive to the oxidation state of the transition metals involved. As can be seen in Figure 5.4, the O-K and Ni-L2,3 fine structure (i.e., peak shapes and energy loss positions) of the selected area matches exactly with the NiO reference sample (as well as with literature [3]), confirming that these Ni-rich particles are indeed NiO. Figure 6.4. TEM characterization of as-received BZY-NiO. (a) HAADF and EDS-filtered image. Selected area for EELS analysis is marked with a red circle, (b) EELS spectra at Oxygen K-edge of BZY-NiO and NiO (reference sample) and (c) Idem at Ni L2,3-edge. In addition, Figure 6.5 shows the selected area electron diffraction pattern of particle #3, which was indexed in the Fm-3m space group with a cell parameter a ≃ 4.2 Å, very close to that of NiO. Similar analyses were performed on other particles, which showed that Ni only appeared at a) b) c) (1) (2) (3) 520 530 540 550 560 570 580 590 Intensity (a.u.) Energy Loss (eV) NiO_reference Zone 1 840 850 860 870 880 890 Intensity (a.u.) Energy Loss (eV) NiO_reference Zone 1 520 530 540 550 560 570 580 590 Intensity (a.u.) Energy Loss (eV) Ni metallique-reference Zone 1 840 850 860 870 880 890 Intensity (a.u.) Energy Loss (eV) Ni metallique-reference Zone 1