scieee AI-readable full text Open interactive document viewer

Enhanced carbon nanotube dispersion in 3YTZP/SWNTs composites and its effect on room temperature mechanical and electrical properties

Gallardo López, Ángela María; Morales Rodríguez, Ana; Vega Padillo, Jesús; Poyato Galán, Rosalía; Muñoz Bernabé, Antonio; Domínguez Rodríguez, Arturo

Abstract

In this work, several modifications of the colloidal processing technique and spark plasma sintering (SPS) to prepare yttria tetragonal zirconia composites (YTZP) with single walled carbon nanotubes (SWNT) have been tested with the aim of eliminating SWNT agglomerates. These modifications include high versus low energy ultrasonic agitation during colloidal processing, lyophilization of the 3YTZP/SWNT slurry and electrical insulation during sintering of the composites. Semi-quantitative microstructural characterization of the carbon nanotube distribution in the sintered composites showed that high energy ultrasonic agitation reduces drastically agglomerate size. Lyophilization of the mixed suspensions avoids SWNT bundle size growth. Combination of both produces an enhanced carbon nanotube network distribution along the grain boundaries (GB) due to the absence of carbon nanotube agglomerates and to a limited SWNT bundle size. This results in an increase of the real SWNT content in the GBs up to nominal SWNT content and therefore an enhanced SWNT efficiency in the composites. The agglomerate-free highly-dispersed composites exhibit a decrease in density together with grain size refinement, a decrease in room temperature hardness, an increase in flexural strength and a most significant increase in room temperature electrical conductivity. Improved SWNT distribution also lowers electrical percolation threshold to a very low level in SWNT ceramic composites, <1 vol% SWNT,

Full text

1 Enhanced carbon nanotube dispersion in 3YTZP/SWNTs composites and its effect on room temperature mechanical and electrical properties A. Gallardo-López a*, A. Morales-Rodríguez a, J. Vega-Padillo a, R. Poyato b, A. Muñoz a, A. Domínguez-Rodríguez a a Dpto. de Física de la Materia Condensada, ICMSE, CSIC, Universidad de Sevilla, apdo. 1065, 41080 Sevilla, Spain b ICMSE, CSIC-Univ. de Sevilla, Avda. Américo Vespucio 49, 41092 Sevilla, Spain e-mail: [email protected]* Phone numbers: +34 620612167, +34 954554448 Abstract In this work, several modifications of the colloidal processing technique and spark plasma sintering (SPS) to prepare yttria tetragonal zirconia composites (YTZP) with single walled carbon nanotubes (SWNT) have been tested with the aim of eliminating SWNT agglomerates. These modifications include high versus low energy ultrasonic agitation during colloidal processing, lyophilization of the 3YTZP/SWNT slurry and electrical insulation during sintering of the composites. Semi-quantitative microstructural characterization of the carbon nanotube distribution in the sintered composites showed that high energy ultrasonic agitation reduces drastically agglomerate size. Lyophilization of the mixed suspensions avoids SWNT bundle size growth. Combination of both produces an enhanced carbon nanotube network distribution along the grain boundaries (GB) due to the absence of carbon nanotube agglomerates and to a limited SWNT bundle size. This results in an increase of the real SWNT content in the GBs up to nominal SWNT content and therefore an enhanced SWNT efficiency in the composites. The agglomerate-free highly-dispersed composites exhibit a decrease in density together with grain size refinement, a decrease in room temperature hardness, an increase in flexural strength and a most significant increase in room temperature electrical conductivity. Improved SWNT distribution also lowers electrical percolation threshold to a very low level in SWNT ceramic composites, < 1 vol% SWNT. 2 1. Introduction Fabrication of ceramic/carbon nanotube (CNT) composites has been a special interest research topic over the past decade [1–4], although difficulties in processing have led to controversial results in properties such as hardness or fracture toughness [5–13]. The expected reinforcement effect of the carbon nanotubes in a ceramic matrix, which promoted the study of these composites, has not been unambiguously confirmed. Most studies reporting improvements in fracture toughness have used Vickers indentation method, which has been unanimously refused by the scientific community for these composites since the article by Wang et al. [14]. These authors obtained fracture toughness values for alumina/SWNT composites similar or lower than monolithic alumina by V-SENB (V-single edge notched beam) technique, showing that the extremely high toughness reported for these composites due to the absence of cracks after Vickers indentation was not obtained with other methods. Very recent studies which also use SENB techniques report no reinforcement at all due to carbon nanotubes [15]. The lack of significant reinforcement in carbon nanotube ceramic composites has been attributed to different reasons: densification problems [9,10,16], agglomeration of carbon nanotubes [17–23], damage or defects in the carbon nanotubes [24,25] and poor interfacial bonding [7]. Many steps have been made towards fabrication of pore free and uniformly dispersed carbon nanotube / ceramic composites. To improve CNT dispersion, functionalization of the carbon nanotubes by acid treatment [20,27], colloidal processing [1,3,27–29], heterocoagulation [10,16,30] and charge stabilization techniques [27] have been used. Spark plasma sintering achieve high densification and minimize damage to the CNTs [8,10,31,32] in the composites. In spite of the above mentioned efforts, still a small percentage of carbon nanotubes in ceramic / CNT composites remain in agglomerates, especially in the case of single walled carbon nanotubes [28,33] due to their high tendency to aggregate via Van der Waals forces and also due to thermodynamic considerations for the particular geometry of the SWNTs compared to the ceramic powder [25,28]. Although recent studies show that these agglomerates are not responsible for the degraded mechanical properties in alumina/SWNT composites [7,34], they are not desirable for several reasons. They introduce heterogeneities in the composites and most important, they decrease SWNT efficiency since when agglomeration occurs the real quantity of SWNT dispersed in the 3 grain boundaries does not coincide with the nominal amount of SWNT introduced in the composite. Recent works devoted to the study of processing techniques which improve the homogeneity of 3YTZP and alumina composites minimizing SWNT agglomeration [9,23,27,34–36] have shown the importance of an optimal SWNT dispersion in electrical and mechanical properties. Shin et al. [9] used dimethylformamide (DMF) solvent and tip sonication to lower electrical resistivity and increase wear resistance of the more homogeneous composites. Poorteman et al. [27] optimized electrostatic repulsion during colloidal processing and used freeze drying to obtain alumina composites with lower electrical percolation threshold. Poyato et al. [35] lowered electrical percolation threshold of 3YTZP composites and obtained a significant increase in electrical conductivity using a similar colloidal processing with tip sonication. Hu et al. [34] grew CNT in situ on fiber surfaces to prevent agglomeration and coated CNTs with pyrolytic carbon to optimize interfacial bonding of CNT to a SiC ceramic matrix improving its mechanical properties. Zhou et al. [23] used a heterocoagulation pretreatment which improved fracture toughness and flexural strength of the composites. Castillo-Rodríguez et al. [36] reported enhanced plasticity at high temperature of 3YTZP/SWNT composites with improved SWNT dispersion and pointed to interesting microstructural effects of some colloidal processing routines which include the combined used of ultrasonic probe, ball milling and lyophilization. However, the good dispersion obtained for some processing conditions was sometimes obscured by a severe degradation of SWNTs, indicating that processing still needs to be optimized. Further damage to the CNTs can also take place during sintering, due to local heating of the CNTs so electrical isolation has been proposed to minimize it [37]. Most authors report that high CNT content ceramic composites exhibit lower values of hardness, toughness or flexural strength than lower CNT content composites or even than the ceramic matrix [7,10,14–16,18,31,33,38–42]. Therefore, low content SWNT/3YTZP composites (up to 2.5 vol% SWNT) seem more interesting than high SWNT content for structural applications which require good mechanical properties, since they show mechanical properties similar or even superior to the ceramic matrix and they conduct electricity, the percolation limit reported between 0.4 and 1.5 vol% SWNT [43]. 4 Electrical conductivity of ceramic/SWNT composites is very interesting because the isolating ceramic matrix can reach high conductivity values with an appropriate amount and dispersion of the SWNT phase. Different studies have analyzed the influence of SWNT concentration on the electrical conductivity of 3YTZP/SWNT or MWNT composites [43–46], but to the best of our knowledge, only one [35] has focused on the effect of SWNT dispersion on the electrical behavior, pointing to higher conductivity with enhanced SWNT dispersion. In this work, we have prepared 3YTZP composites with 1 vol% SWNT using several different colloidal processing routines followed by SPS with the main objective of minimizing agglomeration of the SWNTs. The processing routines include high energy sonication for a better SWNT dispersion during colloidal processing, lyophilization of the slurry to avoid a possible SWNT re-agglomeration during drying and electrical isolation of the composite powder during SPS to reduce local heating of the SWNTs. These routines have been carefully applied to obtain optimal distributed SWNT in the ceramic matrix and full densification of the composites with minimum damage to the SWNTs. The different modifications in the processing routines have been introduced step by step to identify the effect of each one independently on the composite microstructure, hardness and electrical conductivity. The effect of the SWNT distribution and real SWNT percentage in grain boundaries on the room temperature electrical and mechanical properties (hardness and flexural strength) of the composites has been systematically analyzed. 2. Experimental Composites were sintered from commercial 3YTZP powders from Nanostructured and Amorphous Materials Inc. (Houston, Texas) adding 1 vol% (C–OOH) functionalized SWNTs from Nanolab Inc. (Waltham, Massachusetts). The ceramic powders were in a first place annealed at 1250°C for 30 min in air to remove additives. Colloidal processing of the powders and SWNT was carried out following a basic charge stabilization technique described elsewhere [27]. In this technique both ceramic powder and SWNT are independently suspended in a basic water solution with a small amount of 30% NH3 solution to acquire a negative surface charge. A small quantity of powder (~3 g) was prepared for each specimen. Two mixing routines have been used. The first, 5 by means of an ultrasonic bath (240 W) applied for 15 min to the independent basic suspensions and a further 15 min to the mixed ceramic powder-SWNT suspension [7]. The second one, by means of a higher power ultrasonic probe (~750 W) (Model KT- 600, Kontes Inc. Vineland, NJ) at 20 kHz and 95% amplitude applied for 5 min to the SWNT suspension during 3 cycles, and a further 5 min to the mixed suspension, refrigerating between cycles [35]. The application time of ultrasonic agitation to the suspensions (30 min total with ultrasonic bath and 20 min total with ultrasonic probe) has been lowered considerably with respect to previous works [36] to economize energy and minimize damage to the SWNTs. Drying of the composite powders has also been carried out by two routes, the first one using a hot plate at 80 °C with continuous stirring; the second one by lyophilization at - 80 °C using a Cryodos 80 lyophilizer with nylon filters to avoid powder loss during the process. The composite slurry was immediately frozen after ultrasonic mixing by immersion in liquid nitrogen. Composite powders were sintered with spark plasma sintering technique (SPS), using a Dr Sinter 1050 Sumitomo Coal Mining Co. This technique is most suitable for ceramic/SWNT composites since sintering temperatures and times are smaller than for conventional methods, thus minimizing damage to the SWNTs and also minimizing grain growth. The powders were introduced in a 15 mm inner diameter conductive graphite die coated with graphite paper and with graphite rods to exert a uniaxial stress during the process. Heating of the powders was achieved by Joule effect when electric current passed through the experimental arrangement. Since the current could also pass through the conductive nanotubes in the composite powder, electrically insulating boron nitride (BN) platelets were placed between the rods and the powders in some samples to assess a possible overheating and damage of the SWNTs when these insulators were not used. All composites were sintered at 1250°C for 5 min under 75 MPa with 200°C/min heating and 50°C/min cooling ramps. The different processing and sintering routines combining the alternative above mentioned steps (ultrasonic bath or probe; hot plate drying or lyophilization; SPS sintering with or without BN insulation) are summarized in table 1. Composites are denoted C1, C2… to C5, where C1 corresponds to the more basic approach and C5 to the more refined one. 6 Density of the sintered composites was measured by the Archimedes method using distilled water as immersion medium. Theoretical density of the composites ρ=6.04 g cm-3 was calculated using the rule of the mixtures, considering ρ=6.1 g cm-3 for 3YTZP and ρ=0.14 g cm-3 for SWNT. Agglomerate and grain size characterization was carried out by scanning electron microscopy (SEM, JEOL 6460LV) and high resolution SEM (HRSEM, Hitachi S5200) respectively on composites polished up to 1 µm diamond paste (CITIUS facilities, University of Seville). To reveal grain boundaries -for estimation of grain size-, polished samples were further annealed in air at 1150°C for 15 min. The equivalent planar diameter d=2(area/π)1/2 was used as size parameter both for 3YTZP grains and for SWNT agglomerates, using a number of grains and agglomerates not less than 200. The direct analysis of the agglomerates has been carried out on 3x2 mm2 cross sections and top surfaces to scan a sufficiently large area of the sintered samples. The maximum axial dimension and the aspect ratio of the SWNT agglomerates have also been estimated due to their characteristic elongated shape. To evaluate the presence of SWNTs, their structural integrity and the presence of other carbon allotropes after sintering, Raman vibrational spectroscopy was performed on fractured surfaces of all composites, taking six to eight spectra from each specimen (Raman Horiba Jobin LabRaman HR800 with Labsec 5.25.15 data acquisition software). The source was a green He-Ne laser (532.1 nm) of 20 mW power. Diffraction grid consisted of 600 lines per mm and the 100x objective had a confocal aperture of 100 µm. This spectroscopy was carried out in facilities belonging to the Instituto de Ciencia de Materiales de Sevilla (ICMSE). X-Ray diffraction performed on plane surfaces of the composites was used to evaluate the presence of different phases. An X-Ray diffractometer D8 Advance A25 (Bruker Co.) from CITIUS facilities was used. Vickers microhardness was evaluated on polished top surface and cross section of the specimens, to account for a possible influence of the uniaxial stress applied during sintering. A Struers Duramin microindenter was used, with loads of 1.96 N during 15 s. Flexural strength was measured as the maximum stress before breakdown, σmax, in 15x2x1 mm3 bars, the surface under tension polished to 1 µm, using a prototype three point bending test arrangement described elsewhere [34], specially designed for the small specimens’ size. Correlation with the maximum applied load, F, is given by: 7 𝜎𝑚𝑎𝑥 =3𝐿 2ℎ2𝑤𝐹 where L is the span; h and w are respectively height and width of the sample. Electrical conductivity of the composites at room temperature was estimated by impedance spectroscopy, using an Agilent 4294A analyzer which operated from 100 to 2 106 Hz. Parallelepipedic 15x2x1 mm3 bars were cut and colloidal silver paste was applied on two parallel faces. Electrodes were fired at 600 ºC for 30 min in Ar flow. The obtained impedance data was analyzed using an equivalent circuit model by means of Z-view software. 3. Results and discussion 3.1. Microstructure The differences in the experimental routines used for colloidal processing of the five SWNT/3YTZP composites in this study (see table 1) have a remarkable influence in the microstructure of the sintered bodies. Information about SWNT agglomeration and distribution into the ceramic matrix can be extracted directly or indirectly from the different characterization methods used (microstructural, mechanical and electrical). Results from microstructural characterization by BSE (backscattered electrons in SEM) carried out on polished cross sections of the composites have been used as the more direct method to quantify the SWNT dispersion (Figure 1). The presence and distribution of SWNTs and agglomerates can be clearly visualized and measured more reliably than with optical microscopy because of the high contrast due to the average atomic number difference between the ceramic 3YTZP matrix and the light C of SWNT. Grain boundaries in figure 1 are visible because of the presence of dark SWNT bundles in them, giving a picture of how the SWNT are distributed. It is most remarkable that only in C1 and C3 some large agglomerates can be observed, while composites which have been processed with high energy ultrasonic tip do not show any large SWNT agglomerates. In C2, C4 and C5 all SWNT appear located at GBs, and are especially visible in C5 (with electrical insulation during SPS). The effect of agglomeration is the coexistence of agglomerates and free-agglomerate areas depleted in SWNTs. This can also be seen in 8 SEM micrographs of fracture surfaces in composites in figure 2. C4 and C5 show SWNTs (mainly bundles) in most ceramic grain boundaries, while in C1, some SWNT are in agglomerates and less in grain boundaries. Most SWNT agglomerates appear elongated in the perpendicular direction to the sintering compression axis, as it has been previously reported elsewhere[40], which makes them easier to identify. The aspect ratio has been estimated in ~5 (see table 2). This elongation of SWNT agglomerates can influence hardness, producing anisotropy in its values when measured in the top surfaces or in cross sections of the sintered composites [40]. The direct analysis of the agglomerates has been carried out considering as agglomerates only groups or bundles of SWNT larger than 2 µm in length (typically corresponding to d~ 1-1.5 µm equivalent planar diameter). The reason for this choice is that, in cross sections, most agglomerates larger than mentioned exhibit their characteristic elongated shape, while “smaller agglomerates”, with size comparable to the ceramic grains, exhibit a rounded shape. These smaller rounded shapes in our 2D images correspond actually to cross sections of bundles whose major axes lie in planes different from the analyzed specimen cross section. Including these “smaller agglomerates” in the analysis would distort the statistics of characterization parameters such as size and aspect ratio, and would also obscure the observations of the much more typical larger elongated agglomerates. Besides, SWNTs are hardly ever found isolated, but in bundles of variable size. Therefore, the frontier between a big bundle and a small agglomerate is not so clear for sizes under ~1-1.5 µm. Our results from direct agglomerate BSE analysis (presented in table 2) indicate that the surface agglomerate density is apparently very low for all the composites. The highest value is 0.5%, found in C3, similar to C1 (0.3%) which both used low energy ultrasonic agitation and no electrical insulation during SPS. This value is also similar to the same composition with alumina matrix processed with the same conditions [40]. However, taking into account that the total SWNT content was 1 vol%, and using the Delesse principle to extrapolate volumetric to surface concentrations, these would mean that half the total SWNT of the composite C3 is in agglomerates while the other half is distributed in the grain boundaries. The use of an ultrasonic probe during processing (composites C2, C4 and C5) lowers this agglomerate surface density in an order of magnitude (0.02%), so now only 2% of 9 the total SWNT content of the composite is agglomerated while the remaining 98% is well distributed in the grain boundaries (see figure 1 and table 2). This is a huge improvement in the dispersion of SWNTs, as it can be also visualized in figure 2. The ultrasonic probe is therefore very successful in eliminating agglomerates. Another microstructural direct effect of the use of the ultrasonic probe is the smaller agglomerate size (Xmax), (half width along the major axis) although a statistical analysis cannot be carried out due to the negligible quantity of agglomerates found in these composites. In view of these results, the effect of the ultrasonic probe during processing versus lower energy (ultrasonic bath) agitation is double: most important, removing agglomerates almost totally and a secondary effect of reduction in size of the rare remaining agglomerates (40-50%). Lyophilization of the composite powder suspensions, however, seems not to have a remarkable influence in reducing agglomerates versus drying on a hot plate, since C1 and C3 composites have the same order of magnitude of agglomerate surface density. This means that significant re-agglomeration of the SWNTs does not occur during hot plate drying of the slurry. Density drop and grain size refinement are also microstructural effects of the homogeneous SWNT dispersion into the ceramic matrix, usually linked to an increased nominal CNT content in the composites [9,16,23,47]. Grain size refinement is due to the SWNT role as grain size inhibitors. Therefore, a better and increased distribution of the SWNTs in the ceramic matrix grain boundaries should also result in a decreased densification and a reduced ceramic grain size. Density of the composites actually decreases when the different modifications to the colloidal processing are used, as can be seen in table 2. Lyophilization of the slurry (C3) results in a very slight density decrease (versus C1), while the use of high energy agitation (C2 and C4) gives a more pronounced density decrease. Both mentioned modifications together with the use of electrical isolation during SPS produce the minimum density, indicating a better SWNT preservation. Figure 3 shows polished cross sections annealed in air to reveal grain boundaries. In spite of the small density decrease found, samples are highly dense and the few “pores” observed in this micrograph are due to the burning of SWNT bundles. Grain size also detailed in table 2 for the different composites, indicates again that the ultrasonic probe is more effective in SWNT dispersion than lower energy (ultrasonic bath) agitation of the powders suspensions, since composite C2 which used the probe 16 Acknowledgments The financial support for this work has been obtained from the Spanish “Ministerio de Economía y Competitividad” (MAT2012-34217) and from the Junta de Andalucía (P12-FQM-1079). XRD and microscopy studies have been performed at CITIUS facilities (Universidad de Sevilla). References [1] G.-D. Zhan, J.D. Kuntz, J. Wan, A.K. Mukherjee, Single-wall carbon nanotubes as attractive toughening agents in alumina-based nanocomposites, Nat. Mater. 2 (2003) 38–42. [2] P.J.F. Harris, Carbon nanotube composites, Int. Mater. Rev. 49 (2004) 31–43. [3] N.P. Padture, Multifunctional Composites of Ceramics and Single-Walled Carbon Nanotubes, Adv. Mater. 21 (2009) 1767–1770. doi:10.1002/adma.200802270. [4] J. Cho, A.R. Boccaccini, M.S.P. Shaffer, Ceramic matrix composites containing carbon nanotubes, J. Mater. Sci. 44 (2009) 1934–1951. [5] J. Cho, F. Inam, M.J. Reece, Z. Chlup, I. Dlouhy, M.S.P. Shaffer, et al., Carbon nanotubes: Do they toughen brittle matrices?, J. Mater. Sci. 46 (2011) 4770– 4779. [6] J. Sun, L. Gao, M. Iwasa, T. Nakayama, K. Niihara, Failure investigation of carbon nanotube/3Y-TZP nanocomposites, Ceram. Int. 31 (2005) 1131–1134. doi:10.1016/j.ceramint.2004.11.010. [7] R. Poyato, A. Gallardo-López, F. Gutiérrez-Mora, A. Morales-Rodríguez, A. Muñoz, A. Domínguez-Rodríguez, Effect of high SWNT content on the room temperature mechanical properties of fully dense 3YTZP/SWNT composites, J. Eur. Ceram. Soc. 34 (2014) 1571–1579. doi:http://dx.doi.org/10.1016/j.jeurceramsoc.2013.12.024. [8] R.K. Chintapalli, F.G. Marro, B. Milsom, M. Reece, M. Anglada, Processing and characterization of high-density zirconia-carbon nanotube composites, Mater. Sci. Eng. A. 549 (2012) 50–59. [9] J.-H. Shin, S.-H. Hong, Microstructure and mechanical properties of single wall carbon nanotube reinforced yttria stabilized zircona ceramics, Mater. Sci. Eng. A. 556 (2012) 382–387. doi:10.1016/j.msea.2012.07.001. [10] N. Garmendia, S. Grandjean, J. Chevalier, L.A. Diaz, R. Torrecillas, I. Obieta, Zirconia-multiwall carbon nanotubes dense nano-composites with an unusual balance between crack and ageing resistance, J. Eur. Ceram. Soc. 31 (2011) 1009–1014. 17 [11] A. Mukhopadhyay, B.T.T. Chu, M.L.H. Green, R.I. Todd, Understanding the mechanical reinforcement of uniformly dispersed multiwalled carbon nanotubes in alumino-borosilicate glass ceramic, Acta Mater. 58 (2010) 2685–2697. doi:10.1016/j.actamat.2010.01.001. [12] A. Peigney, F.L. Garcia, C. Estournes, A. Weibel, C. Laurent, Toughening and hardening in double-walled carbon nanotube/nanostructured magnesia composites, Carbon N. Y. 48 (2010) 1952–1960. doi:10.1016/j.carbon.2010.01.063. [13] L. Shen, Y.-H. Han, C. Xiang, H. Tang, A. Mukherjee, S. Kim, et al., Phase transformation behavior of ZrO2 by addition of carbon nanotubes consolidated by spark plasma sintering, Scr. Mater. 69 (2013) 736–739. doi:10.1016/j.scriptamat.2013.08.015. [14] X. Wang, N.P. Padture, H. Tanaka, Contact-damage-resistant ceramic/single-wall carbon nanotubes and ceramic/graphite composites, Nat. Mater. 3 (2004) 539– 544. [15] L. Melk, J.J. Roa Rovira, F. García-Marro, M.-L. Antti, B. Milsom, M.J. Reece, et al., Nanoindentation and fracture toughness of nanostructured zirconia/multiwalled carbon nanotube composites, Ceram. Int. 41 (2015) 2453–2461. doi:10.1016/j.ceramint.2014.10.060. [16] A. Duszová, J. Dusza, K. Tomášek, G. Blugan, J. Kuebler, Microstructure and properties of carbon nanotube/zirconia composite, J. Eur. Ceram. Soc. 28 (2008) 1023–1027. [17] J.P. Fan, D.Q. Zhao, M.S. Wu, Z.N. Xu, J. Song, Preparation and microstructure of multi-wall carbon nanotubes-toughened Al2O3 composite, J. Am. Ceram. Soc. 89 (2006) 750–753. doi:10.1111/j.1551-2916.2005.00774.x. [18] G. Yamamoto, T. Hashida, Carbon Nanotube Reinforced Alumina Composite Materials, in: N. Hu (Ed.), Compos. Their Prop., InTech, 2012. [19] N. Bakhsh, F.A. Khalid, A.S. Hakeem, Synthesis and characterization of pressureless sintered carbon nanotube reinforced alumina nanocomposites, Mater. Sci. Eng. A-Structural Mater. Prop. Microstruct. Process. 578 (2013) 422– 429. doi:10.1016/j.msea.2013.04.020. [20] J. Liu, A.G. Rinzler, H.J. Dai, J.H. Hafner, R.K. Bradley, P.J. Boul, et al., Fullerene pipes, Science (80-. ). 280 (1998) 1253–1256. doi:10.1126/science.280.5367.1253. [21] E. Zapata-Solvas, D. Gomez-Garcia, A. Dominguez-Rodriguez, Towards physical properties tailoring of carbon nanotubes-reinforced ceramic matrix composites, J. Eur. Ceram. Soc. 32 (2012) 3001–3020. doi:10.1016/j.jeurceramsoc.2012.04.018. 18 [22] M. Estili, Y. Sakka, Recent advances in understanding the reinforcing ability and mechanism of carbon nanotubes in ceramic matrix composites, Sci. Technol. Adv. Mater. 15 (2014) 064902. doi:10.1088/1468-6996/15/6/064902. [23] J.P. Zhou, Q.M. Gong, K.Y. Yuan, J.J. Wu, Y. fang Chen, C.S. Li, et al., The effects of multiwalled carbon nanotubes on the hot-pressed 3mol% yttria stabilized zirconia ceramics, Mater. Sci. Eng. A. 520 (2009) 153–157. doi:10.1016/j.msea.2009.05.014. [24] K.E. Thomson, D. Jiang, R.O. Ritchie, A.K. Mukherjee, A preservation study of carbon nanotubes in alumina-based nanocomposites via Raman spectroscopy and nuclear magnetic resonance, Appl. Phys. A-Materials Sci. Process. 89 (2007) 651–654. doi:10.1007/s00339-007-4253-9. [25] B.T.T. Chu, G. Tobias, C.G. Salzmann, B. Ballesteros, N. Grobert, R.I. Todd, et al., Fabrication of carbon-nanotube-reinforced glass-ceramic nanocomposites by ultrasonic in situ sol-gel processing, J. Mater. Chem. 18 (2008) 5344–5349. doi:10.1039/b809369e. [26] R. Poyato, A.L. Vasiliev, N.P. Padture, H. Tanaka, T. Nishimura, Aqueous colloidal processing of single-wall carbon nanotubes and their composites with ceramics, Nanotechnology. 17 (2006) 1770–1777. doi:10.1088/0957- 4484/17/6/038. [27] M. Poorteman, M. Traianidis, G. Bister, F. Cambier, Colloidal processing, hot pressing and characterisation of electroconductive MWCNT-alumina composites with compositions near the percolation threshold, J. Eur. Ceram. Soc. 29 (2009) 669–675. [28] I. Ahmad, H. Cao, H. Chen, H. Zhao, A. Kennedy, Y.Q. Zhu, Carbon nanotube toughened aluminium oxide nanocomposite, J. Eur. Ceram. Soc. 30 (2010) 865– 873. [29] N. Garmendia, I. Santacruz, R. Moreno, I. Obieta, Slip casting of nanozirconia/MWCNT composites using a heterocoagulation process, J. Eur. Ceram. Soc. 29 (2009) 1939–1945. [30] A. Datye, K.-H. Wu, G. Gomes, V. Monroy, H.-T. Lin, J. Vleugels, et al., Synthesis, microstructure and mechanical properties of Yttria Stabilized Zirconia (3YTZP) – Multi-Walled Nanotube (MWNTs) nanocomposite by direct in-situ growth of MWNTs on Zirconia particles, Compos. Sci. Technol. 70 (2010) 2086–2092. doi:10.1016/j.compscitech.2010.08.005. [31] K.E. Thomson, D. Jiang, W. Yao, R.O. Ritchie, A.K. Mukherjee, Characterization and mechanical testing of alumina-based nanocomposites reinforced with niobium and/or carbon nanotubes fabricated by spark plasma sintering, Acta Mater. 60 (2012) 622–632. doi:http://dx.doi.org/10.1016/j.actamat.2011.10.002. 19 [32] O. Tapasztó, L. Tapasztó, M. Markó, F. Kern, R. Gadow, C. Balázsi, Dispersion patterns of graphene and carbon nanotubes in ceramic matrix composites, Chem. Phys. Lett. 511 (2011) 340–343. doi:10.1016/j.cplett.2011.06.047. [33] A. Gallardo-López, R. Poyato, A. Morales-Rodríguez, A. Fernández-Serrano, A. Muñoz, A. Domínguez-Rodríguez, Hardness and flexural strength of singlewalled carbon nanotube/alumina composites, J. Mater. Sci. 49 (2014) 7116– 7123. doi:10.1007/s10853-014-8419-5. [34] J. Hu, S. Dong, Q. Feng, M. Zhou, X. Wang, Y. Cheng, Tailoring carbon nanotube/matrix interface to optimize mechanical properties of multiscale composites, Carbon N. Y. 69 (2014) 621–625. doi:10.1016/j.carbon.2013.12.005. [35] R. Poyato, J. Macías-Delgado, A. Gallardo-López, A. Muñoz, A. Domínguez- Rodríguez, Microstructure and impedance spectroscopy of 3YTZP/SWNT ceramic nanocomposites, Ceram. Int. 41 (2015) 12861–12868. doi:10.1016/j.ceramint.2015.06.123. [36] M. Castillo-Rodríguez, A. Muñoz, A. Morales-Rodríguez, R. Poyato, Á. Gallardo-López, A. Domínguez-Rodríguez, Influence of the Processing Route on the Carbon Nanotubes Dispersion and Creep Resistance of 3YTZP/SWCNTs Nanocomposites, J. Am. Ceram. Soc. 98 (2015) 645–653. doi:10.1111/jace.13348. [37] Q. Huang, D. Jiang, I.A. Ovid’ko, A. Mukherjee, High-current-induced damage on carbon nanotubes: The case during spark plasma sintering, Scr. Mater. 63 (2010) 1181–1184. doi:10.1016/j.scriptamat.2010.08.030. [38] T. Ukai, T. Sekino, A. Hirvonen, N. Tanaka, T. Kusunose, T. Nakayama, et al., Preparation and electrical properties of carbon nanotubes dispersed zirconia nanocomposites, Key Eng. Mater. 317-318 (2006) 661–664. [39] J. Sun, L. Gao, X.H. Jin, Reinforcement of alumina matrix with multi-walled carbon nanotubes, Ceram. Int. 31 (2005) 893–896. doi:10.1016/j.ceramint.2004.10.002. [40] A. Morales–Rodríguez, A. Gallardo–López, A. Fernández–Serrano, R. Poyato, A. Muñoz, A. Domínguez–Rodríguez, Improvement of Vickers hardness measurement on SWNT/Al2O3 composites consolidated by spark plasma sintering, J. Eur. Ceram. Soc. 34 (2014) 3801–3809. doi:10.1016/j.jeurceramsoc.2014.05.048. [41] S.W. Kim, W.S. Chung, K.-S. Sohn, C.-Y. Son, S. Lee, Improvement of flexure strength and fracture toughness in alumina matrix composites reinforced with carbon nanotubes, Mater. Sci. Eng. A-Structural Mater. Prop. Microstruct. Process. 517 (2009) 293–299. doi:10.1016/j.msea.2009.04.035. [42] A. Kasperski, A. Weibel, D. Alkattan, C. Estournès, C. Laurent, A. Peigney, Double-walled carbon nanotube/zirconia composites: Preparation by spark 20 plasma sintering, electrical conductivity and mechanical properties, Ceram. Int. 41 (2015) 13731–13738. doi:10.1016/j.ceramint.2015.08.034. [43] R. Poyato, J. Macías-Delgado, A. García-Valenzuela, Á. Gallardo-López, A. Morales-Rodríguez, A. Muñoz, et al., Mechanical and electrical properties of low SWNT content 3YTZP composites, J. Eur. Ceram. Soc. 35 (2015) 2351–2359. doi:10.1016/j.jeurceramsoc.2015.02.022. [44] S.-L. Shi, J. Liang, Effect of Multiwall Carbon Nanotubes on Electrical and Dielectric Properties of Yttria-Stabilized Zirconia Ceramic, J. Am. Ceram. Soc. 89 (2006) 3533–3535. doi:10.1111/j.1551-2916.2006.01232.x. [45] S.-L. Shi, J. Liang, Electronic transport properties of multiwall carbon nanotubes/yttria-stabilized zirconia composites, J. Appl. Phys. 101 (2007) 023708. doi:10.1063/1.2430700. [46] F.C. Fonseca, R. Muccillo, D.Z. de Florio, L.O. Ladeira, A.S. Ferlauto, Mixed ionic-electronic conductivity in yttria-stabilized zirconia/carbon nanotube composites, Appl. Phys. Lett. 91 (2007) 243107. doi:10.1063/1.2821373. [47] J.W. An, D.S. Lim, Effect of carbon nanotube additions on the microstructure of hot-pressed alumina, J. Ceram. Process. Res. 3 (2002) 201–204. [48] M.H. Bocanegra-Bernal, A. Reyes-Rojas, A. Aguilar-Elguézabal, E. Torres- Moye, J. Echeberria, X-ray diffraction evidence of a phase transformation in zirconia by the presence of graphite and carbon nanotubes in zirconia toughened alumina composites, Int. J. Refract. Met. Hard Mater. 35 (2012) 315–318. doi:10.1016/j.ijrmhm.2012.07.004. [49] O. Lourie, D.M. Cox, H.D. Wagner, Buckling and Collapse of Embedded Carbon Nanotubes, Phys. Rev. Lett. 81 (1998) 1638–1641. doi:10.1103/PhysRevLett.81.1638. [50] V. Schettino, M. Pagliai, G. Cardini, The Infrared and Raman Spectra of Fullerene C 70 . DFT Calculations and Correlation with C 60, J. Phys. Chem. A. 106 (2002) 1815–1823. doi:10.1021/jp012680d. [51] P.N. Nirmalraj, P.E. Lyons, S. De, J.N. Coleman, J.J. Boland, Electrical connectivity in single-walled carbon nanotube networks., Nano Lett. 9 (2009) 3890–5. doi:10.1021/nl9020914. 21 FIGURE CAPTIONS Figure 1. Low magnification backscattered electron scanning (BSE) images from the indicated composites cross sections, showing dark SWNT in the GBs and some large agglomerates (arrowed). a), b), c), d), and e) correspond to C1, C2, C3, C4 and C5 composites respectively. 22 Figure 2. Fracture surfaces of composites C3, C4, and C5, showing ceramic 3YTZP grains and SWNTs (arrowed) at different magnifications. 23 Figure 3. SEM micrographs of polished cross sections after annealing in air to show 3YTZP grain boundaries. a), b), c), d) and e) correspond to C1, C2, C3, C4 and C5 composites respectively. 24 Figure 4. Raman spectra from the 3YTZP / 1 vol% SWNT composites sintered in this study. (a) Spectra normalized to the 3YTZP peaks and (b) area of interest normalized to the G-band for easier comparison. 25 Figure 5. a) Optical micrographs showing Vickers indentations (1.96 N) on cross sections of the studied composites. b) Non symmetric Vickers imprint on a large SWNT agglomerate in composite C3.