Full text
High thermoelectric performance in Bi2-xPbxBa2Co2Ox promoted by directional growth and annealing M. A. Madre1, F. M. Costa2, N. M. Ferreira2, S. I. R. Costa3, Sh. Rasekh1, M. A. Torres1, J. C. Diez1, V. S. Amaral2,3, J. S. Amaral2,3, A. Sotelo1,* 1Instituto de Ciencia de Materiales de Aragón, ICMA (CSIC-Universidad de Zaragoza), Mª de Luna, 3. 50018 Zaragoza, Spain. 2i3N, Departamento de Física, Universidade de Aveiro, 3810-193 Aveiro, Portugal 3CICECO, Materials and Ceramic Eng. Dept., University of Aveiro, 3810-193 Aveiro (Portugal) Abstract Bi2-xPbxBa2Co2Oy (x=0.0, 0.2, 0.4, and 0.6) misfit compounds were grown by the laser floating zone technique. Microstructural analysis has shown the formation of thermoelectric grains together with high amount of secondary phases. Thermoelectric grains orientation is increased until 0.4Pb, while further substitution drastically destroys the preferential grain orientation. Electrical resistivity is very low compared with the values obtained in sintered materials, spectacularly increasing power factor. Moreover, the performance of these materials was further improved subjecting the as-grown samples to a postannealing step due to the rise of thermoelectric phase content. These microstructural modifications led to a high decrease of electrical resistivity, improving power factor in around a factor two at room temperature, compared with the as-grown samples. Moreover, the low thermal conductivity of the textured annealed samples leads to a maximum estimated ZT value of 0.53 for the 0.2 Pb-doped samples, much higher than the reported in literature. Keywords: Ceramics; Doping; Grain growth; Electrical properties; Thermopower Corresponding author: Andres Sotelo e-mail: [email protected] Address: C/Maria de Luna, 3. 50018-Zaragoza (Spain) Tel: +34 976762617
Fax: +34 976761957
1. Introduction Nowadays, there is a great and growing interest in the development of new and clean energy sources in order to fight against global warming. These green energy sources should decrease the release of greenhouse gases, as CO2, produced in the classical energy transforming systems. On the other hand, it is still difficult to avoid the use of fossil fuels in many applications, as in automobiles or electrical power production, with a relatively low efficiency (∼ 40 %) [1]. In this scenario, thermoelectric (TE) energy conversion, based on the well-known Seebeck effect, can be used to transform solar energy into electricity at lower cost than photovoltaic energy [2]. Moreover, it has shown important advantages (for example, they are silent and have non moving parts) to be applied in harvesting waste heat in these classical energy transforming systems [3]. The efficiency characterization of these TE materials is performed through the dimensionless figure of merit, ZT, which is calculated as T S2 ρ-1 κ-1, where T, S, ρ, and κ are the absolute temperature, Seebeck coefficient, electrical resistivity and thermal conductivity, respectively [4]. As a consequence, a high performance TE material should have low thermal conductivity, high power factor (PF = S2 ρ-1), and high working temperatures. At present, some practical applications of TE devices can be found in vehicles exhausts and in cooling systems. These TE devices are formed by different intermetallic or semiconducting materials, as Bi-Te-based ones, with high associated costs, and relatively low working temperatures. Moreover, most of these materials are composed of scarce, heavy, and/or toxic elements which are not environmental friendly. Nevertheless, since the discovery in 1997 of good TE properties in NaxCoO2 [5], many studies have been performed in transition metal oxide (TMO’s) based materials. These materials, such as Bi2Ca2Co2Ox [6,7], Bi2Sr2Co2Ox [8,9], Bi2Ba2Co2Ox [10], or Ca3Co4O9 [11,12], are based in cheaper, more abundant and environmentally friendly, and chemically stable at high temperatures under air. All these characteristics have greatly increased the interest in these TMO’s-based materials. Crystallographic studies of these materials have shown that they can be described by a monoclinic structure formed by two different sublattices which are alternately stacked [13]. One is the CoO2 conductive layer with CdI2-type
structure, while the other one is an insulating rock-salt-type. Both sublattices possess the same lattice parameters, except in the b-axis length, leading to a misfit along this direction [14]. As it is well-known, these materials show a very important crystallographic anisotropy which is reflected in a high electrical conductivity one. As a consequence, the alignment of grains along their conducting planes can be used to drastically reduce the electrical resistivity in the bulk materials. This process would allow enhancing ZT to values close to the obtained in single crystals. Many techniques have been used to produce such grain alignment, as hot-pressing [15], spark plasma sintering (SPS) [16], laser floating zone (LFZ) [17], or the electrically assisted laser floating zone [18], which have shown their ability to improve TE performance of bulk materials by the alignment of grains. On the other hand, doping processes have been also shown that TE properties can be tuned up by using the adequate dopants and proportions, as it is the case of different metals for Ca substitution in Ca3Co4O9 [19], or Pb for Bi in Bi2Sr2Co1.8Ox [20]. Moreover, the synthesis techniques can also drastically modify the grain sizes and their connectivity, leading to improved properties in the final bulk materials [21]. Taking into account the above considerations, the aim of the present work is studying the effect of relatively low Pb substitutions for Bi in the Bi2Ba2Co2Ox thermoelectric material. Pb has been selected as dopant due to its unique properties which make it essential in many compounds and applications, as for example in PZT piezoelectrics [22], or as dopant, stabilizing the High-Tc Bi- 2223 superconducting phase [23]. It has been prepared by a polymer solution method developed in our laboratory [24], followed by texturing using the laser floating zone melting technique [17]. Moreover, as it was determined in previous works in similar systems, the as grown materials possess a high amount of secondary phases [25]. As a consequence, some samples were annealed to increase the amount of the thermoelectric phase. The thermoelectric properties of these Bi2-xPbxBa2Co2Oy textured ceramics (with x=0, 0.2, 0.4, and 0.6), before and after annealing, have been determined and correlated with their structure and microstructure. 2. Experimental
The Bi2-xPbxBa2Co2Oy ceramics (with x=0, 0.2, 0.4, and 0.6) were prepared from Bi(CH3CO2)3 (99.99 + %, Aldrich), Pb(CH3CO2)2 • 3H2O (≥ 99%, Aldrich), Ba(CH3CO2)2 (≥ 99%, Aldrich), and Co(CH3CO2)2 • 4H2O (98%, Panreac) commercial powders. They were weighed in the appropriate proportions and dissolved in a mixture of distilled H2O and glacial acetic acid (ACS Reagent, Panreac). To the clear pink solution, Polyethylenimine (PEI) (50% aqueous, Aldrich) was added to the above solution which turned darker immediately due to the nitrogen-metal bond formation. Partial evaporation of water and acetic acid has been performed in a rotary evaporator until a final volume of around 20 % of the initial one. The concentrated solution was then placed onto a hot plate for further solvent evaporation until a very dark pink paste appeared. Further heating turn this paste to violet colour, followed by a slow autocombustion with the release of brown fumes (nitrogen oxides). The mixture was manually milled and thermally treated at 700 and 750ºC for 12 h, with an intermediate milling, following the procedure described elsewhere [26] to decompose the alkaline earth carbonates. This decomposition step is very important to produce well aligned grains by the laser floating zone, due to the fact that the remaining carbonates would decompose during the texturing process inside the molten zone. As a consequence, the melt would be disturbed by the CO2 bubbles produced in the decomposition process, leading to the growth front destabilization and producing grains misalignments. The final powder was then isostatically pressed under 200 MPa during one minute to produce cylindrical green ceramics (2-3 mm diameter). These cylinders were used as feed in a LFZ device equipped with a continuous power Nd:YAG laser (λ = 1064 nm), following the experimental procedure described elsewhere [27]. All the LFZ-grown samples were processed at 30 mm h-1 under air with a seed rotation of 3 rpm to maintain the cylindrical geometry. Moreover, the feed was rotated at 15 rpm in the opposite direction, in order to ensure compositional homogeneity of the molten zone. After the texturing process, long (> 150 mm) and geometrically homogeneous textured cylindrical rods of around 2 mm diameter were produced. The textured bars were cut into suitably sized pieces for their TE characterization (∼ 15 mm long). As mentioned previously, as-grown materials are characterized by a relatively high amount of secondary
phases. As a consequence, some of the samples were annealed at 700 ºC for 24 h, in air atmosphere, to increase the proportion of the thermoelectric phase in the samples. The identification of the main phases in the textured samples was performed by powder X-ray diffraction (XRD) utilizing a Rigaku D/max-B X-ray powder diffractometer (CuKα radiation) with 2θ ranging between 10 and 70 degrees. In order to determine the adequate temperature for annealing the as-grown samples, DTA analyses were performed in a TA Instrument (SDT Q600) system between room temperature and 800 ºC. Microstructural observations were performed on polished as-grown and annealed samples using backscattered electrons in a Zeiss Merlin field emission scanning electron microscope (FESEM) equipped with an energy dispersive spectrometry (EDS) analysis system. Micrographs of these samples have been recorded to analyze the different phases and their distribution. Steady-state simultaneous measurements of resistivity and Seebeck coefficient were determined by the standard dc four-probe technique in a LSR-3 apparatus (Linseis GmbH) between 50 and 650 ºC under He atmosphere, with an estimated error of 4 % in each parameter. From these data, samples performances were determined using PF values. Finally, thermal conductivity was determined at room temperature in the annealed samples using the transient plane source technique (Hot Disk TPS 2500 s), which possess an accuracy better than 5 %, as indicated by the system manufacturer. This method uses an electrically conducting pattern element acting both as a temperature sensor and heat source, insulated with two thin layers of Kapton (70 µm). The TPS element is assembled between two samples of similar characteristics with both faces in contact with the two samples surfaces. The measurements were performed with heating power ranging from 7 to 9 W and measurement time from 20 to 80 s. From the PF and κ values, ZT has been determined at room temperature and estimated at higher temperatures, together with its calculated error from the uncertainties of each physical parameter (S, ρ, and κ). For this estimation, the κ behaviour with temperature has been consulted in other works where it has been found to be nearly constant [28] or decreasing [29] when the temperature is increased. As a
consequence it has been assumed that, in the worst case, κ would be unchanged with T. 3. Results and discussion 3.1. As-grown samples Powder XRD data for as-grown samples with different Pb content are plotted (from 10 to 40 ° for a better clarity) in Fig. 1. They show similar patterns where most of the peaks correspond to the (00l) planes of the misfit cobaltite Bi2Ba2Co2Oy [28]. Even if minor differences are found in weak peaks, the cobaltite phase appears as the major one, independently of the Pb content. Peak marked with a * in the plot corresponds to a Bi-Ba-O solid solution with P121/n1 space group [30]. Moreover, the proportion of the secondary phase is decreasing, compared to the thermoelectric one, when the Pb content in the samples is raised, as can be observed by the decrease of its (200) peak intensity. Scanning electron microscopy was performed on longitudinal polished sections of the as-grown samples, and representative images of all samples are displayed in Fig. 2. In these images, three main contrasts can be seen (indicated by numbers in Fig. 2a for clarity). The major phase in all samples (grey contrast, #1) has been identified by EDS as the misfit thermoelectric (Bi,Pb)2Ba2Co2Oy one. In the case of the Pb-doped samples, this phase has a Pb content of around 0.4 for the 0.2Pb-doped one, slightly decreasing for higher Pb nominal composition. Dark grey contrast (#2) corresponds to the Ba2Co3Oz secondary phase, while the white contrast (#3) has been identified as Bi5Ba4Ox, in agreement with the XRD data. Moreover, this last phase has an increasing Pb content with the nominal one, reaching a Bi:Ba:Pb proportion of 5:4:1 for the highest Pb nominal composition. This type of phases (plumbate-like ones) are well common in other Pb-doped systems [31] for their ability to admit very high Pb proportions, which can explain the slight decrease of Pb in the thermoelectric (Bi,Pb)2Ba2Co2Oy phase. Finally, in 0.6Pb-doped samples, a new contrast appears (black one, #4) which corresponds to Co-oxide. Other feature that can be observed in these microstructures is the decrease of Ba2Co3Oz secondary phase when Pb content is raised while the thermoelectric one increases, in agreement with the XRD data. On the other hand, the plumbate-
like phase content seems to slightly increase with Pb-content. All these features are maintained until 0.4 Pb nominal content and further Pb substitution produces new phases (#4 in Fig. 2d) and clearly destroys the grain orientation in the bulk material. In any case, it can be easily seen that the best aligned grains are those found in samples with 0.2 Pb substitution. The temperature dependence of the electrical resistivity, as a function of the Pb content, is given in Fig. 3. As it can be easily seen, ρ(T) curves show a semiconducting-like behaviour (dρ/dT < 0) in the whole temperature range. Moreover, the curve slope tends to be lower when Pb content is raised. This is in agreement with previous works which showed that Bi substitution by Pb increases the hole carrier concentration in similar systems [20,32]. This is due to the fact that Pb2+ is substituting Bi3+ in the RS structure leading to a decrease on the effective charge in this structure. As a consequence, the charge in the conducting layer has to be raised in order to compensate the changes in the RS layer, increasing the relative proportion of Co4+ in this layer. From Koshibae expression [33], the higher relationship between Co4+ and the total Co in the conducting layer (Co3++Co4+) increases the carrier concentration, leading to lower electrical resistivity values at room temperature. On the other hand, the evolution of resistivity for the Pb doped samples clearly agree with the SEM and EDS data discussed previously. In fact, the lowest resistivity is measured on 0.2Pb doped samples due to their higher grain orientation (see Fig. 2) and to the fact that Bi2Ba2Co2Oy thermoelectric phase has the highest Pb content. Further Pb substitution produces higher grain misalignment and a slight decrease of Pb in the thermoelectric phase, leading to increased resistivity values compared to the 0.2Pb doped samples. The minimum resistivity value (∼ 11 mΩ cm) at 650 ºC has been obtained for the 0.2Pb doped samples, which is slightly higher than the best results obtained in pure Bi2Ba2Co2Oy textured by the LFZ technique at low rates (∼ 8.5 mΩ cm) [34], but much lower than the obtained in sintered materials (∼ 33 mΩ cm) [28]. Fig. 4 displays the variation of Seebeck coefficient with temperature as a function of Pb content. As can be easily seen in the plot, S is positive in the whole measured temperature range, indicating a conduction mechanism mainly governed by holes. Moreover, all the samples show similar S values at room
temperature (~ 130 µV K-1) which are slightly higher than the obtained in textured materials grown by the LFZ technique at low rates (~ 120 µV K-1) [34], and much higher than the measured in sintered materials at the same temperature (~ 85 µV K-1) [28]. On the other hand, different behaviours can be observed for the undoped and for the doped samples. The raise of S with temperature for the undoped samples is much lower than for the Pb doped ones. As a consequence, all the Pb doped samples reach higher S values at 650 ºC than the undoped ones. The highest S value at 650 ºC has been obtained for the 0.4Pb doped samples (~ 205 µV K-1), which is around 35 % higher than the obtained in the undoped samples, and slightly higher (~ 5 %) than the measured in the other Pb doped ones. Moreover, this value is slightly higher than the obtained in textured materials grown by the LFZ technique at low rates (~ 185 µV K-1) [34], and much higher than the measured in sintered materials at the same temperature (~ 110 µV K-1) [28]. From the above data, PF has been calculated and presented, as a function of Pb content, in Fig. 5, where it can be clearly seen that the PF of the 0.2Pb doped samples raise, in a very important manner, with respect to the values obtained in undoped ones (∼ 100 % in the whole measured temperature range). Further Pb doping starts to decrease PF values with respect to the 0.2Pb doped ones. This evolution is in clear agreement with the microstructural features discussed previously which showed that the best oriented grains and the highest amount of TE phase was obtained in the 0.2Pb doped samples. The highest PF values at room temperature and at 650 ºC (around 0.12 and 0.34 mW K-2 m -1, respectively) are much higher than the obtained in solid state sintered materials (∼ 0.035 and 0.040 mW K-2 m-1, respectively) [28]. Moreover, they are also higher than the obtained at different growth rates. On the other hand, they are very close to the values obtained in pure Bi2Ba2Co2Oy materials textured at low rates (about 0.40 mW K-2 m-1 at 650 ºC) [34]. It is important to highlight that all the above described results are around the best ones obtained in Bi2Ba2Co2Oy materials. Taking into account that the amount of secondary phases in the studied samples is relatively high, an annealing process could promote the formation of a higher proportion of TE phase. Consequently, this thermal treatment would decrease the amount of
References [1] Biswas K, He J, Blum ID, Wu C-I, Hogan TP, Seidman DN, Dravid VP, Kanatzidis MG. High-performance bulk thermoelectrics with all-scale hierarchical architectures. Nature 2012;489:414–8. [2] Liu W, Yan X, Chen G, Ren Z. Recent advances in thermoelectric nanocomposites. Nano Energy 2012;1:42–56. [3] Elsheikh MH, Shnawah DA, Sabri MFM, Said SBM, Hassan MH, Bashir MBA, Mohamad M. Renew Sust Energ Rev 2014;30:337–55. [4] Rowe DM. Thermoelectrics Handbook: Macro to Nano. first ed. Boca Raton:CRC Press;2006. [5] Terasaki I, Sasago Y, Uchinokura K. Large thermoelectric power in NaCo2O4 single crystals. Phys Rev B 1997;56 (20):12685–7. [6] Sotelo A, Rasekh Sh, Madre MA, Guilmeau E, Marinel S, Diez JC. Solutionbased synthesis routes to thermoelectric Bi2Ca2Co1.7Ox. J Eur Ceram Soc 2011;31:1763–9. [7] Sun N, Dong ST, Zhang BB, Chen YB, Zhou J, Zhang ST, Gu ZB, Yao SH. Chen YF. Intrinsically modified thermoelectric performance of alkaline-earth isovalently substituted [Bi2AE2O4][CoO2]y single crystals. J Appl Phys 2013;114:043705. [8] Rubesova K, Hlasek T, Jakes V, Huber S, Hejtmanek J, Sedmidubsky D. Effect of a powder compaction process on the thermoelectric properties of Bi2Sr2Co1.8Ox ceramics. J Eur Ceram Soc 2015;35:525–31. [9] Diez JC, Guilmeau E, Madre MA, Marinel S, Lemmonier S, Sotelo A, Improvement of Bi2Sr2Co1.8Ox thermoelectric properties by laser floating zone texturing. Solid State Ionics 2009;180:827–30. [10] Hervieu M, Maignan A, Michel C, Hardy V, Creon N, Raveau B. Metallicity and thermopower of the misfit cobaltite [Bi2Ba1.8Co0.2O4]RS[CoO2]2. Phys Rev B 2003;67:045112. [11] Wu N, Holgate TC, Nong NV, Pryds N, Linderoth S. High temperature thermoelectric properties of Ca3Co4O9+δ by auto-combustion synthesis and spark plasma sintering. J Eur Ceram Soc 2014;34:925–31. [12] Sotelo A, Constantinescu G, Rasekh Sh, Torres MA, Diez JC, Madre MA. Improvement of thermoelectric properties of Ca3Co4O9 using soft chemistry synthetic methods. J Eur Ceram Soc 2012;32:2415–22.
[13] Leligny H, Grebille D, Perez O, Masset AC, Hervieu M, Raveau R. A fivedimensional structural investigation of the misfit layer compound [Bi0.87SrO2]2[CoO2]1.82. Acta Cryst B 2000;56:173–82. [14] Maignan A, Hébert S, Hervieu M, Michel C, Pelloquin D, Khomskii D, Magnetoresistance and magnetothermopower properties of Bi/Ca/Co/O and Bi(Pb)/Ca/Co/O misfit layer cobaltites. J Phys: Condens Matter 2003;15:2711– 23. [15] Wang H, Sun X, Yan X, Huo D, Li X, Li JG, Ding X. Fabrication and thermoelectric properties of highly textured Ca9Co12O28 ceramic. J Alloys Compds 2014;582:294–8. [16] Butt S, Liu YC, Lan JL, Shehzad K, Zhan B, Lin Y, Nan CW. Hightemperature thermoelectric properties of La and Fe co-doped Ca–Co–O misfitlayered cobaltites consolidated by spark plasma sintering. J Alloys Compds 2014;588:277–83. [17] Diez JC, Rasekh Sh, Madre MA., Guilmeau E, Marinel S, Sotelo A. Improved Thermoelectric Properties of Bi-M-Co-O (M = Sr, Ca) Misfit Compounds by Laser Directional Solidification. J Electron Mater 2010;39:1601– 5. [18] Ferreira NM, Rasekh Sh, Costa FM, Madre MA, Sotelo A, Diez JC,Torres M.A. New method to improve the grain alignment and performance of thermoelectric ceramics. Mater Lett 2012;83:144–7. [19] Abdellahi M, Bahmanpour M, Bahmanpour M. Modeling Seebeck coefficient of Ca3-xMxCo4O9 (M=Sr, Pr, Ga, Ca, Ba, La, Ag) thermoelectric ceramics. Ceram Int 2015;41:345–52. [20] Sotelo A, Rasekh Sh, Guilmeau E, Madre MA, Torres MA, Marinel S, Diez JC, Improved thermoelectric properties in directionally grown Bi2Sr2Co1.8Oy ceramics by Pb for Bi substitution. Mater Res Bull 2011;46:2537–42. [21] Rasekh Sh, Madre MA, Sotelo A, Guilmeau E, Marinel S, Diez JC. Effect of synthetic methods on the thermoelectrical propertiesof textured Bi2Ca2Co1.7Ox ceramics. Bol Soc Esp Ceram V 2010;49:89–94. [22] Xie R, Liu C, Zhao Y, Jin P, Zhou KC, Zhang D. Gelation behavior and mechanical properties of gelcast lead zirconatetitanate ceramics. J Eur Ceram Soc 2015;35:2051–6.
[23] Sotelo A, de La Fuente GF, Lera F, Beltran D, Sapina F, Ibanez R, Beltran A, Bermejo MR. Novel Polymer Solution Synthesis of the 110 K Superconducting Phase in the Bismuth. System Chem Mater 1993;5:851–6. [24] Madre MA, Rasekh Sh, Diez JC, Sotelo A. New solution method to produce high performance thermoelectric ceramics: A case study of Bi-Sr-Co-O. Mater Lett 2010;64:2566–8. [25] Rasekh Sh, Constantinescu G, Torres MA, Madre MA, Diez JC, Sotelo A. Growth rate effect on microstructure and thermoelectric properties of melt grown Bi2Ba2Co2Ox textured ceramics. Adv Appl Ceram 2012;111:490–4. [26] Sotelo A, Guilmeau E, Madre MA, Marinel S, Lemmonier S, Diez JC. Bi2Ca2Co1.7Ox thermoelectric ceramics textured by laser floating zone method Bol Soc Esp Ceram V 2008;47:225–8. [27] de la Fuente GF, Ruiz MT, Sotelo A, Larrea A, Navarro R.Microstructure of laser floating zone (LFZ) textured (Bi,Pb)-Sr-Ca-Cu-O superconductor composite. Mater Sci Eng A 1993;173:201–4. [28] Hao H, Yang H, Liu Y, Hu X. High-temperature Thermoelectric Properties of Cu-substituted Bi2Ba2Co2-xCuxOy Oxides. J Mater Sci Technol 2011;27:525– 8. [29] He QL, Qin Z, Zhang J, Gao F, Hu X, Song HZ. Enhanced Thermoelectric Properties of Hole-Doped Bi2-xBaxSr2Co2Oy Ceramics. J Electron Mater 2014;43:1432–5. [30] Kennedy BJ, Howard CJ, Knight KS, Zhang ZM, Zhou QD. Structures and phase transitions in the ordered double perovskites Ba2BiIIIBiVO6 and Ba2BiIIISbVO6. Acta Cryst B 2006;62:537–46. [31] Madre MA, Amaveda H, Mora M, Sotelo A, Angurel LA, Diez JC. Ag doped (Bi1.6Pb0.4)Sr2CaCu2O8+δ textured rods. Bol Soc Esp Ceram V 2008;47:148–52. [32] Rasekh Sh, Madre MA, Diez JC, Guilmeau E, Marinel S, Sotelo, A. Effect of Pb substitution on the thermoelectrical properties of textured Bi2Ca2Co1.7Oy ceramics prepared by a polymer solution method. Bol Soc Esp Ceram V 2010;49:371–6. [33] Koshibae W, Tsuitsui K, Maekawa S. Thermopower in cobalt oxides. Phys Rev B 2000;62:6869–72.
[34] Constantinescu G, Rasekh Sh, Torres MA, Madre MA, Diez JC, Sotelo A. Enhancement of the high-temperature thermoelectric performance of Bi2Ba2Co2Ox ceramics. Scr Mater 2013;68:75–8. [35] Kobayashi W, Muguerra H, Hebert S, Grebille D, Maignan A. Metallicity and positive magnetoresistance induced by Pb substitution in a misfit cobaltate crystal. J. Phys.: Cond. Matter 2009;21:235404. [36] Sakai K, Karppinen M, Chen JM, Liu RS, Sugihara S, Yamauchi H. Pb-for- Bi substitution for enhancing thermoelectric characteristics of [(Bi,Pb)2Ba2O4±ω]0.5CoO2. Appl Phys Lett 2006;88:232102. [37] Populoh S, Aguirre MH, Brunko OC, Galazka K, Lu Y, Weidenkaff A. High figure of merit in (Ti,Zr,Hf)NiSn half-Heusler alloys. Scr. Mater. 2012;66:1073– 1076. [38] Thiel P, Populoh S, Yoon S, Weidenkaff A. Enhancement of redox– and phase-stability of thermoelectric CaMnO3+δ by substitution. J. Solid State Chem. 2015;229:62–67.
Figure captions Figure 1. Powder XRD plots of the Bi2-xPbxBa2Co2Ox as-grown samples with different Pb contents. x = 0.0 (a), 0.2 (b), 0.4 (c), and 0.6 (d). Diffraction planes indicates the Bi2Ba2Co2Ox phase while * shows the peak corresponding to the BiBaO3 secondary phase. Figure 2. Scanning electron micrographs obtained on transversal polished sections of Bi2-xPbxBa2Co2Ox as-grown samples with x= 0.0 (a), 0.2 (b), 0.4 (c), and 0.6 (d). Different contrasts are #1: grey one, associated to the thermoelectric (Bi,Pb)2Ba2Co2Ox phase; #2: dark grey, Ba2Co3Oy; #3: white, Bi5Ba4Oz with plumbate-like composition (around Bi5Ba4PbOz) in the Pbsubstituted samples; and #4: black, Co-oxide. Figure 3. Temperature dependence of the electrical resistivity for the as-grown Bi2-xPbxBa2Co2Ox samples, for x= 0.0 ; 0.2 0.4 ▲; and 0.6 T. Figure 4. Temperature dependence of the Seebeck coefficient for the as-grown Bi2-xPbxBa2Co2Ox samples, for x= 0.0 ; 0.2 0.4 ▲; and 0.6 T. Figure 5. Temperature dependence of power factor for the as-grown Bi2- xPbxBa2Co2Ox samples, for x= 0.0 ; 0.2 0.4 ▲; and 0.6 T. Figure 6. Powder XRD plots of the Bi2-xPbxBa2Co2Ox as-grown samples with different Pb contents. x = 0.0 (a), 0.2 (b), 0.4 (c), and 0.6 (d). Diffraction planes indicates the Bi2Ba2Co2Ox phase while * shows the peak corresponding to the BiBaO3 secondary one. Figure 7. Scanning electron micrographs obtained on transversal polished sections of Bi2-xPbxBa2Co2Ox annealed samples with x= 0.0 (a), 0.2 (b), 0.4 (c), and 0.6 (d). Different contrasts are #1: grey one, associated to the thermoelectric (Bi,Pb)2Ba2Co2Ox phase; #2: dark grey, Ba2Co5Oy; #3: white, and Bi2Ba4Oz with plumbate-like composition (around Bi2Ba4PbOz) in the Pbsubstituted samples.
Figure 8. Temperature dependence of the electrical resistivity for the annealed Bi2-xPbxBa2Co2Ox samples, for x= 0.0 ; 0.2 0.4 ▲; and 0.6 T. Figure 9. Temperature dependence of the Seebeck coefficient for the annealed Bi2-xPbxBa2Co2Ox samples, for x= 0.0 ; 0.2 0.4 ▲; and 0.6 T. Figure 10. Temperature dependence of power factor for the annealed Bi2- xPbxBa2Co2Ox samples, for x= 0.0 ; 0.2 0.4 ▲; and 0.6 T. Figure 11. Estimated temperature dependence of ZT for the annealed Bi2- xPbxBa2Co2Ox samples, for x= 0.0 ; 0.2 0.4 ▲; and 0.6 T.
Figure 1
Figure 2
Figure 3
Figure 4
Figure 11