scieee AI-readable full text Open interactive document viewer

Repositorio Institucional de Documentos

Abstract

En el mundo de los nanomateriales la sílice es uno de los compuestos mas estudiados debido a sus propiedades y la versatilidad que ofrece en cuanto aplicaciones. En este proyecto se desarrolla un nuevo método de obtención de sílice funcionalizada con moléculas fluorescentes y nanoparticulas metálicas lo cual le confiere al material nuevas propiedades que lo hacen válido para uso como marcadores, catálisis, aplicaciones biómedicas... Moreno Berdejo, Nuria; Santamaría Ramiro, J. M. ; Lobera González, Maria Pilar

Full text

Synthesis and characterization of fluorescent hollow silica nanoparticles: Control of size and metal incorporation for several nanotechnology applications FINAL MASTER PROJECT DIRECTED BY Jesús Santamaría Ramiro Mª Pilar Lobera González Nuria Moreno Berdejo Master Degree in Nanostructured Materials for Nanotechnology Applications September, 2015 Dpto. Ingeniería Química y Tecnología del Medio Ambiente Instituto de Nanociencia de Aragón Facultad de Ciencias UNIVERSIDAD DE ZARAGOZA ACKNOWLEDGMENTS This report means the end of a year of work and the end of my master, however this would not been possible without the help of many people, so I would like to begin by thanking. In the first place, thanks to Pilar Cea for her efforts in the difficult task to organizing and coordinating the master and thanks to Ciber-BBN for the award of the grant to carry out my final master project. Thanks to my directors, Jesús Santamaría and Pilar Lobera for their guiding me in daily work, understanding and good advice. Also, thanks to Francisco Balas who gave me the opportunity to work with him and deposited on me the confidence to develop this project. And I can not forget to thank to the person who has been really my teacher in the laboratory, for his useful advice, his encouragement words and his enormous patience: Thanks Alberto Clemente. Thanks to all members of NFP group: from all doctors who have taught and during this year to all my lab partners who make a great time, who are the responsibles of a nice environment in the laboratory and who have been my (necessary) coffee-time partners. Specially, thanks to Nuria Navascués for all her help and patience (and for all hours of TEM). And finally,but no least, I want to thank to all my family, specially to my parents for their effort, their trust in me and their unconditional support and thanks to David to share and support me in the worst moments and to be the responsible for the best ones. CONTENTS 1. INTRODUCTION ....................................................................................................... 1 2. OBJECTIVES ............................................................................................................... 6 3. METHODOLOGY ....................................................................................................... 7 3.1 CHEMICALS ...................................................................................................................... 7 3.2 SYNTHESIS FLUORESCENT SiO2 NANOPARTICLES ................................................ 7 3.3 SYNTHESIS HOLLOW FLUORESCENT SiO2 NANOPARTICLES .............................. 8 3.4 METAL INCORPORATION ............................................................................................. 9 3.5 CHARACTERIZATION TECHNIQUES ........................................................................ 10 TRANSMISSION ELECTRON MICROSCOPY............................................................... 10 UV-VIS ABSORBANCE ................................................................................................... 11 PHOTOLUMINESCENCE ................................................................................................. 11 NITROGEN ADSORPTION ISOTHERM: BET ............................................................... 11 1H-NUCLEAR MAGNETIC RESONANCE...................................................................... 12 X-RAY PHOTOELECTRON SPECTROSCOPY (XPS) ................................................... 12 4. RESULTS AND DISCUSSION ................................................................................. 13 4.1 STUDY OF THE HOLLOWING PROCESS ................................................................... 13 EVOLUTION OF HOLE FORMATION ........................................................................... 13 TEMPERATURE EFFECT ................................................................................................ 14 pH EFFECT ........................................................................................................................ 15 IONIC STRENGTH EFFECT ............................................................................................ 16 INFLUENCE OF SYNTHESIS ROUTHE OF FLUORESCENCE SILICA NANOPARTICLES ............................................................................................................ 17 MECHANISM OF FORMATION OF FLUORESCENT HOLLOW SILICA NANOPARTICLES ............................................................................................................ 19 4.2 METAL INCORPORATION ........................................................................................... 23 4.3 APPLICATIONS .............................................................................................................. 27 5. CONCLUSIONS ........................................................................................................ 29 6. REFERENCES ........................................................................................................... 30 7. ATTACHMENTS ......................................................................................................... i 7.1. 1H-NMR SPECTRA ............................................................................................................ i 7.2. XPS RESULTS ................................................................................................................. iii 7.3 LASER EXPERIMENT ..................................................................................................... iv Introduction 1 1. INTRODUCTION Nanotechnology is a emerging science focused in the design, fabrication and application of nanostructures or nanomaterials, and the fundamental understanding of the relationships between physical properties or phenomena and material dimensions.1 Materials at nanometer scale may exhibit physical properties distinctively different from that of bulk which have being exploited in different fields such as enviromental technology, improve electronic devices, catalysis, energy production or in biomedicine for early detection of diseases (bioimaging and biosensors) and treatment thereof (controlled drug delivery).2 Of all the existing nanomaterials, one of the most studied has been structures based on silicon dioxide (SiO2) or commonly named silica. This compound consists in a polymer formed by tetrahedral SiO4 units interconnected. Thanks to its versatility, nontoxicity, biocompatibility and wide range of applications, researchs based on this materials has growth in the last years (Fig. 1). Fig. 1. Number of publications related to silica nanomaterials.3 Synthesis of silica nanostructures has been developed mainly by sol-gel process obtaining amorphous solids with high conectivity between SiO4 units and higly hydroxylated surfaces. This method is based on a chemical process consisting in hydrolysis and condensation reactions between the initial precursors (alkoxy silicates) in different parts of the reaction mixture. In this manner the precursors begin to bind forming a colloidal structures (sol) and when this process continues, sol increases its viscosity and the polymeric chains grow up to macroscopic groups (gel)4,5 (Fig. 2a). This method allows the modulation of the polimerization process according to pH and salt concentration in order to obatin different structures (Fig. 2b). 0 500 1000 1500 2000 2500 3000 2005200620072008200920102011201220132014 Number of publications Year Introduction 2 According to their textural properties and morphology different types of silicabased nanostructures can be distinguished which could be used in several applications. The following scheme (Fig. 3) summarizes this classification. Fig. 3. Classification of different silica nanostructures. a b Fig. 2. a) Scheme of a sol-gel process.4 b) Polymerization behaviour of silica describin the sol-gel process.6 SiO2 NANOSTRUCTURES Pure silica nanoparticles Porous structures Functionalizated silica Introduction 3  Pure silica nanoparticles This type is referring to pure and dense spherical silica nanoparticles. Some of the widely used methods to synthesize pure silica nanoparticles are sol-gel process, reverse microemulsion and flame synthesis. The sol-gel process is widely used to produce pure silica particles through systematic monitoring of reaction parameter. In this way, Stöber7 synthesis is the most common method for synthesizing colloidal silica-based nanoparticles that are <100 nm in size. This method shows some disadvantages such as the nanoparticles are not uniform size and, due to the pH and the high concentrations of alcohols, this process is incompatible with doping some biomolecules such as proteins. In reverse microemulsion, the surfactants molecules dissolved in organic solvents, forms spherical micelles. In presence of water, the polar head groups organize themselves to form microcavities containing water, which is often called as reverse micelles where a water-in-oil (w/o) microemulsion creates a nanodroplets system which acts a nanoreactors where a controlled synthesis is carried out. In comparasion to Stöber method, this synthesis needs a much longer time but shows highly efficient to the fabrication of spherical and monodispersed nanoparticles.8 The major drawbacks of the reverse microemulsion approachs are high const and difficulties in removal of surfactants in the final products. However, this method was successfully applied for the coating of nanoparticles with different functional groups for various applications.9 Silica nanoparticles can also be produced through high temperature flame descomposition of metal-organic precursors. This process is also referred to as chemical vapor condensation (CVC). In a typical CVC process, silica nanoparticles are produced by reacting silicon tetrachloride, SiCl4 with hydrogen and oxygen. Difficulty in controlling the particle size, morphology and phase composition is the main disadvantage of the flame synthesis. Nevertheless, this is the prominent method that has been used to commercially produce silica nanoparticles in powder form.10,11  Porous structures A porous material can be classfied according to the porous size in microporous (less than 2 nm), mesoporous (2-50 nm) or macroporous (greater than 50 nm). In the case of silica, mesoporous nanoparticles has been the most studied due to their properties such as mechanical resistance, chemical and thermal stability, biocompatibility, high surface area, high porosity with high pore volume and Introduction 4 modificable pore size.12,13 All these characteristics allow the use of mesoporous silica in biomedical applications as drug delivery because the porous allow the storage of several molecules. Some examples of mesoporous silica structures are MCM-41, SBA-15,SBA-16 or FDU-12.4  Functionalized silica There are different ways to functionalize so dense as hollow silica nanoparticles: by covalent linked on the surface or within the structure of the nanoparticle. The high concentration of –OH groups on the surface of silica nanoparticles allows the possibility of its surface modification by covalent bond with several molecules forming hybrid structures with different functionalities.4 On the other hand, silica precursors can be convalently modified with different molecules, such as luminophores, in order to synthesize functionalizated nanoparticles which can be used as luminiscent markers.14 Some of these luminophores are fluorescein isothiocyanate (FITC), rhodamine, cyanine or ruthenium complexes. This project has been focused in the use of FITC (Fig. 4) as luminophore. It is a organic molecule with fluorescence properties belonging to the group of xanthenes and shows very high molar absorptivity at 488 nm and high quantum yield with a emission spectra at 490 nm.15 Fig. 4. Structure of FITC. Finally, in the case of porous and hollow silica nanoparticles, the synthesis of nanohybrids is a way to obtain functionalized silica nanostructures. For this end, several useful loads such as metal nanoparticles, quantum dots or drugs can be introduced inside of cavities of silica nanoparticles. These useful loads could have magnetic or optical properties, could be used in catalysis, as bactericide, etc. Introduction 5 Traditionally, two approaches can be followed to synthesize nanohybrids: first using a template which is covered by porous silica and after the template is removed generating a hole where useful loads can be introduced (Fig. 5a) or second, starting from the useful load, cover it by a template and after synthesize a shell of silica around the template. Finally, the template is removed remaining the useful load inside the structure (Fig. 5b). In this way these generated nanohybrids can act as transport vehicles.16 Fig. 5. Scheme of the most common processes to introduce useful loads in hollow silica nanoparticles. Even so, the controllable synthesis of nanohybrids with a narrow particles size distribution by a simple and scalable method is still a great challenge.17 In this project, we present one-step synthesis of monodisperse silica-based nanohybrids. The proposed method started from fluorescence dense silica nanoparticles obtained by microemulsion, followed by the introduction of different useful loads in one step, taking advantage of the hollowing process. a b template silica useful load Objectives 6 2. OBJECTIVES The core idea of this master final project was to study and control the process of formation fluorescent hollow silica nanoparticles proposing a mechanism to explain this phenomena. To that end, different experiments was carried out in order to find out the influence in the hollowing process of both synthesis routhe of fluorescent SiO2 nanoparticles and effect of aging conditions. In addition to primary objective in this final master project, and taking advantage of the control of the hollowing process, series of experiments were conducted in order to introduce several useful loads obtaining fluorescent and functionalized silica-based nanohybrids which can be used in different applications. Finally, an overview of potential applications for synthesized silica-based nanohybrids in different fields as selective catalyst, markers, bactericide, photonics, etc. were addressed. Results and Discussion 13 4. RESULTS AND DISCUSSION 4.1 STUDY OF THE HOLLOWING PROCESS When a sample of fluorescent silica nanoparticles (Fig. 9a) was aged in water during 5 days, fluorescent hollow nanoparticles were obtained (Fig. 9b). Fig. 9. TEM images of fluorescent silica nanoparticles after their storage during 5 days a) in ethanol b) in water. EVOLUTION OF HOLE FORMATION This process was followed along the time in order to study the evolution of the hole formation. During the hole formation process, the evolution of interior void diameter (Dh) was monitored during a month by TEM analysis (Fig. 10). Representative TEM image (Fig. 10a) indicates formation of solid silica nanoparticles with uniform particle size of 60 ± 8 nm (Dp). Fig. 11b and Fig. 11c show how the size of the hole was increased progressively along the time up to 40 nm, mantaining the size of the nanoparticle, until the formation of a stable suspension of hollow fluorescent nanoparticles even a month after storage in aqueous media. (a) (b) Results and Discussion 14 Fig. 10. (a,d) TEM image of fluorescent dense silica nanospheres with the histogram showing particle size distributions were shown. (b,c,d,f) TEM image of fluorescent hollow silica nanosheperes at different aging time and histograms showing particles size distribution were shown. TEMPERATURE EFFECT The fluorescent SiO2 nanoparticles were suspended in an ethanol-water mixture (1:1) and refluxing for 5 hours (T80ºC). Fig. 11a shows similar hole evolution than the obtained after storage in aqueous media during 5 days at 25ºC in dark. Moreover, the fluorescent properties remained unchanged. So, the hollowing process can be accelerated with the increase of temperature due to higher diffusivity of water molecules into the pristine SiO2 nanoparticles. However, the storage in aqueous media at lower temperatures do not slow down the hollowing process. Fig. 11b shows that mean void Results and Discussion 15 diameter obtained after an aging process in aqueous media during 5 days at 4ºC in dark was similar than the obtained after the same aging process at 25ºC. Fig. 11. Hollow fluorescent silica nanoparticles formed by aging in a) 80ºC at reflux during 5 hours b) at 4ºC during 5 days. pH EFFECT Fluorescent SiO2 nanoparticles were aging during a month at 25ºC in dark using aqueous solutions with different pH conditions. Fluorescent silica nanoparticles were showed at TEM (Fig. 12). The particle size distribution remained unchanged around 56 nm with the pH used in the aging medium. Futhermore a retardation of complete hydrolysis of siloxanes groups located in the core of the silica nanoparticles was observed at pH=2, and no formation of the inner hole is observed after a month of aging (Fig. 12a). However in the same time of aging, an increase in the pH of the aging medium accelerates the hydrolysis rate of inner siloxanes groups and enables the formation of an inner hole up to 41 nm. As expected, the SiO2 nanoparticles aged at pH=9 were degradated. Thus, the fluorescent silica nanoparticles can be tailor-made depending the pH conditions of aqueous media used for their aging. (a) T=80ºC (b) T=4ºC Dp = 75 ± 15 nm Dh= 29 ± 16 nm Dp = 65 ± 7 nm Dh= 32 ± 6 nm Results and Discussion 16 Fig. 12. Evolution of hollowing process at different pHs. IONIC STRENGTH EFFECT 5-days aging test were realized increasing the concentration of ions in the aqueous media used, specifically a ionic strength of I = 0.0342 M was used. The results shown that when the concentration of ions was increased the formation of the hole was delayed, even inhibited (Fig. 13a). Moreover, only an early stage of the hollowing process was observed when the aging process of the SiO2 nanoparticles was accelerated by refluxing them for 5 hours in a ethanol-water mixture (1:1) with the same ionic strength of than in the previous experiment (Fig. 13b). Higher concentration of ions in the aging aqueous media were related with a delay in the formation of hollow silica nanoparticles. Fig. 13. Fluorescent silica nanoparticles (62 ± 6 nm) after aging in NaCl solution (I=0.0342 M) during a) 5 days b) 5 hours at reflux. (a) (b) Dp = 56 ± 7 nm Dh= 0 nm Dp = 54 ± 7 nm Dh= 21 ± 8 nm Dp = 59 ± 7 nm Dh= 45 ± 10 nm Results and Discussion 17 INFLUENCE OF SYNTHESIS ROUTHE OF FLUORESCENCE SILICA NANOPARTICLES Diverse modifications in the synthesis routhe of fluorescent silica nanoparticles were carried out in order to study their influence in the hollowing process. In all cases, the SiO2 nanoparticles were aging in aqueous media during 5 days at 25ºC in dark. First, the water/Si ratio (R) used in the synthesis of the fluorescent SiO2 nanoparticles was increased. The results showed that an increase of the water/Si ratio used in the synthesis (eg. an increase in the amount of water) retards the hole formation being the diameter lower ( Fig. 14). Fig. 14. Evolution of fluorescent silica nanoparticles at different water/Si synthesis ratios a) 30, b) 40 and c) 50 after 5 days of aging time. As second approach, the microemulsion media (Cyclohexane, TritonX-100 and 1-hexanol) was replaced by the same volume of ethanol to perform the synthesis of fluorescent SiO2 nanoparticles through a sol-gel method. According to Fig. 15, the microemulsion is responsible for obtaining a monodisperse fluorescent SiO2 nanoparticles, controlling their size and shape, while the synthesis carried out through a sol-gel method in ethanol solution turned out to have SiO2 nanoparticles with great polydispersity. Two populations were identified: one of 156 ± 28 nm and another of 69 ± 13 of size. Also, the hollowing process was studied in these polydispersed nanoparticles obtained by sol-gel method. After 5 days of aging in water only bigger nanoparticles showed inner hole (Fig. 15). (a) Dp = 59 ± 7 nm Dh= 29 ± 9 nm (a) R=30 Dp = 66 ± 13 nm Dh= 22 ± 8 nm (b) R=40 Dp = 61 ± 8 nm Dh= 0 nm (c) R=50 Results and Discussion 18 Fig. 15. Two populations of fluorescent silica nanoparticles synthesized in ethanol media after 5 days of aging in water. Holes are only observe in higher nanoparticles. Finally, non-fluorescent SiO2 nanoparticles were synthesized and their hollowing process was studied. Two approaches were carried out: first, using only APTES solution as conjugated and second, without any conjugated molecule. Fig. 16. Non-fluorescent silica nanoparticles using as Si source a) TEOS and APTES b) only TEOS. In both cases there are not difference in the size and shape regarding those obtained in the original synthesis of fluorescent SiO2 nanoparticles. Fig. 16 shows the hollow SiO2 nanoparticles after 5 days of aging time in aqueous media. In both cases, the diameter of the hole is slightly less than in the orginal particles (from 11 to 14 nm). (a) Si source:APTES+TEOS Dphigher = 156 ± 28 nm Dpsmaller = 69 ± 13 nm Dh = 26 ± 10 nm Dp = 55 ± 3 nm Dh= 11 ± 2 nm Dp = 52 ± 6 nm Dh= 14 ± 2 nm (b) Si source: TEOS Results and Discussion 19 This phenomena could be due to the non presence of large hydrophobic groups allowing higher number and better packing of the hydrolyzable chains (which contains Si-O-Et groups). MECHANISM OF FORMATION OF FLUORESCENT HOLLOW SILICA NANOPARTICLES The analysis of all of this experiments and the characterization techniques allowed to propose a mechanism to explain the formation process of hollow SiO2 nanoparticles. Role of organic and siloxane groups was crucial in the formation of hollow silica nanoparticles as well the amount of water used during the synthesis. The process started with the synthesis of fluorescence silica nanoparticles in a microemulsion (w/o) media. As shown above, this procedure allowed the obtention of nanostructures with controlled shape and size. A nanodroplets system was formed which acted a nanoreactors where a synthesis of the nanoparticles was carried out being regulated the accesibility of each reagent according to their hydrophobic or hydrophilic character (and their stearic impediment). Once NH4OH was added into the microemulsion, TEOS and FITC-APTES conjugate (as silica sources) were catalytically hydrolyzed to form silanol groups, moved into the water droplet in the microemulsion and co-condensed to form an organic-inorganic siloxane framework. These seminal siloxane groups were assumed to crosslink [SiO4] tetrahedra with [O3Si-R] units, where R is FITC molecules covalently linked to APTES by thiourea bonds (Fig. 17). Since these condensation reactions occurred in the aqueous droplets within the microemulsion, it could be proposed that more hydrophobic [O3Si-R] units were mainly oriented inward as the silica nanoparticle was growing. This feature could in turn reduce the access of water molecules to the inner part of the forming nanoparticle. In such way, water becomes the limitant reagent and resulting in an inefficient hydrolysis and condensation reactions during formation of siloxane framework. That is, nanoparticles are formed by a dense shell of polymerized SiO2, while inside the nanoparticle, where the most hydrophobic groups are oriented, there are etoxi groups which have not been hydrolyzed. So, the core of the nanoparticles is formed by a silice gel with lower density. Results and Discussion 20 Fig. 17. Hydrolysis of silica precursors APTES and TEOS. Density profiles obtained by STEM shows the existence of a lower density region in the inner zone of the fluorescent silica nanoparticles. The presence of this region was also confirmed by BET measures (Fig. 19) when the adsorption and desorption of nitrogen by dense and hollow nanoparticles could be compared. First, the obtention of porous silica nanoparticles with a porous size around 3-4 nm and the presence of a inner hole hollow were confirmed. The surface area of the hollow SiO2 nanoparticles are 292 m2/g, which are larger than those of dense one, 122.9 m2/g. A steep decline in the adsorbed nitrogen at a relative pressure of 0.5 in the hysteris loop, allowed to propose a bottleneck structure connecting the porous and the inner hollow region. Fig. 18. Density profile of fluorescent silica nanoparticles after 5 days of aging in water. Results and Discussion 21 Fig. 19. Isotherms of nitrogen adsorption and desorption for a) dense and b) hollow fluorescent silica nanoparticles When fluorescent silica nanoparticles were aged in aqueous media, water molecules diffuses through the inner part of the nanoparticles and the hydrolysis of organosiloxanes were complete and some R groups were formed. This R groups were released through the outer liquid media, so the interior void was created. In order to check what molecules left the nanoparticles during the hollowing process, assynthesized fluorescent silica nanoparticles were aged in aqueous media and the supernatants obtained at different times were measured by UV-Vis spectroscopy. The spectra of the supernatants demonstrated a broad absorption peaks at 490 nm (Fig. 20). In all cases, the intensity of absorption peak gradually increased with the aging.time. To clarify the nature of absorbing species, the UV-Vis spectrum of the dye molecule and FITC-APTES conjugate in aqueous medium at pH 6.5 were measured. The FITC spectrum has distinctive features of dianion fluoresceine in polar solvents such as water or ethanol. It has its main absorption peak at 490 nm and has a very weak absorption in the region of 350-400 nm. The FITC-APTES conjugate spectrum has a wide absorption with a maximum at 490 nm, a slight absorption in the region of 350- 400 nm. It can be observed that the absorption peak of the supernatants was similar at the FITC-APTES peak, so probably, part of these molecules leave the nanoparticle during the hollowing process. (b) (a) Results and Discussion 22 Fig. 20. UV-VIS spectra of FITC (blue), APTES-FITC-APTES conjugated (red) and supernatants at different aging times (dotted lines). In addition, fluorescence measures were realized at different aging times (Fig.21). The results showed an increased emission at 516 nm where FITC-APTES conjugated shows maximum emission. This is due to fluorescent FITC-APTES molecules left the silica structure during the aging time and they were free in solution where their emission was higher than when they were inside the particle. This result is consistent with those obtained by UV-Vis. Once the hollowing process was finished, the fluorescence emission of a water suspension of hollow nanoparticles was stable over time. This means that fluorescent hollow SiO2 nanoparticles are stable strucutures where the hydrolysis reaction does not taking place because all the Si-O-Et groups had been hydrolyzed and where fluorescent molecules do not leave the nanoparticle structure. Finally, the supernatants were analyzed by 1H-NMR (see annex 1) and they were compared with the spectra obtained for APTES, FITC and FITC-APTES conjugated in deuterated methanol. In this case, the presence of a different peaks corresponding to ethanol molecules (1.17 and 3.65 ppm) confirmed that the hydrolysis reaction had been carried out during the aging time. However, due to poor detection limit of the equipment, the presence of peaks from aromatic rings corresponding to FITC-APTES conjugate (between 7 and 7.5 ppm) was very weak, so their concentration in solution 300 350 400 450 500 550 600 0.0 0.2 0.4 0.6 0.8 FITC-APTES FITC Absorbance (a.u.) (nm) Supernatants t=0 t=1d t=4d Conclusions 29 5. CONCLUSIONS In this work, we present one-step synthesis of monodisperse silica-coated nanohybrids by means of in situ growth of nanoparticles cores during the hollow silica nanoparticles formation by w/o microemulsion. A mechanism for the formation of fluorescent hollow silica nanoparticles was proposed. And it has allowed us to tailor the synthesis of SiO2-based hollow nanoparticles by controlling the synthesis and aging conditions. Last but not least, we were able to introduce different useful loads as metal nanoparticles taking advantage of the knowledge acquired of the hollowing process of SiO2 nanoparticles. As a result, functionalized silica-based nanostructures useful for different applications were obtained by a simple method. References 30 6. REFERENCES 1. G. Cao, Nanostructures and Nanomaterials. Synthesis, Properties and Applications. Imperial College Press, 2004 2. http://www.nanotecnologia.cl 3. www.scopus.com 4. D. Carmona.PhD Thesis, Universidad de Zaragoza, 2013. 5. C.J. Brinker et al. Sol-gel scince. Academic Press, 1990. 6. K. Natte.. PhD Thesis. University of Berlin, 2013. 7. W. Stöber et al. Journal of Colloid and Interface Science, 26, 62-69, 1968. 8. D. Knopp et al. Analytica Chimica Acta, 647, 14-30, 2009. 9. R. P. Bagwe et al. Langmuir, 22, 9, 4357–4362, 2006. 10. K. Wegner et al. Chemical Engineering Science, 5,4581-4589, 2003. 11. W. Teoh et al. Nanoscale, 2, 1324-1347, 2010. 12. M. Llinas et al.Afinidad LXXI, 565, 20-31, 2014. 13. Y. Wang et al.Nanomedicine: Nanotechnology, Article in Press, 2014 14. S. Santra et al. Anal. Chem. 73, 4988-4993, 2001. 15. S. Santa, B. et al. Journal of Luminescence 117, 75-82, 2006. 16. Z. Li et al. Journal of Controlled Release 98, 245-254, 2004. 17. J. Lee et al. Nanotoday 9, 631-667, 2014. 18. S. Santra et al.Chem. Commun. 2810-2811, 2004. 19. Y. Jin et al. Coordination Chemisty Reviews 253, 2998-3014, 2009. 20. I. Bilecka et al. One-minute synthesis of crystalline binary and ternary metal oxide nanoparticles.Chem. Commun., 886-888, 2008. 21. R. Sjöback et al.Spectrochimica Acta Part A, 51, L7-L21, 1995. 22. T. Gao et al. Nanopart Res, 15:1370, 1-9, 2013. 23. Y. Chang et al. 2013. 24. H. Wang et al. American Chemical Society, 86, 3013-3019,2014. 25. K. Hori et al. Science and Technology of Advanced Materials 7, 678-684, 2006. 26. J. Lee et al. Adv. Mater. 20, 1523-1528, 2008. 27. V. Evangelista et al. Applied Catalysis B: Environmental, 166-167, 518-528, 2015. 28. S. Laurent et al. Chemical Reviews, 108, 2064-2110, 2008. Attachments i 7.ATTACHMENTS 7.1. 1H-NMR SPECTRA 1H-NMR spectra corresponding to different species in deuterated methanol has been showed below: APTES FITC Attachments ii APTES-FITC CONJUGATE SUPERNATANT Attachments iii 7.2. XPS RESULTS The following table shows the results obtained in XPS experiment for metalsilica nanohybrids. C 1s O 1s Si2p Metal Pt/SiO2 74.98 21.60 3.41 0 58.21 26.38 15.32 0.09 62.92 22.06 14.91 0.11 67.71 19.25 12.93 0.10 68.42 18.81 12.66 0.10 67.59 19.29 13.01 0.10 Ag/SiO2 76.74 20.54 2.64 0.07 76.43 14.72 8.69 0.16 80.47 12.01 7.38 0.13 79.89 12.83 7.16 0.12 82.72 10.57 6.58 0.12 81.73 11.20 6.91 0.15 Fe/SiO2 73.44 22.97 2.58 1.00 85.68 5.60 1.76 6.95 88.37 4.19 1.01 6.42 87.14 4.35 0.76 7.74 89.61 2.98 0.24 7.17 89.71 3.20 0.19 6.89 89.22 3.14 0.37 7.27 88.65 2.49 0.35 8.505 88.84 2.38 0.08 8.69 88.13 2.69 0 9.17 Au/SiO2 75.43 21.21 3.35 0 52.20 28.99 18.45 0.36 54.66 27.31 17.68 0.34 60.49 24.21 15.03 0.27 61.74 22.70 15.28 0.27 62.11 22.35 15.24 0.30 62.42 22.84 15.43 0.30 60.58 22.97 16.14 0.30 62.07 21.57 16.03 0.33 60.00 24.14 15.52 0.34 Attachments iv 7.3 LASER EXPERIMENT The following graph show the increase of temperature when a sample of Au@SiO2 was irradiated by a laser at 540 nm. The graph shows a weak increase in the temperature due to absorbed radiation by gold nanoparticles. 25 30 35 40 0 5 10 Temperature (ºC) Time (min) Au@SiO2-FITC References 5 References 6 Attachments 7 8