scieee AI-readable full text Open interactive document viewer

Characterization of Fibrin and Collagen Gels for Engineering Wound Healing Models

Moreno-Arotzena , Oihana; García-Aznar, José Manuel; Meier, Johann G; del Amo, Cristina

Abstract

Hydrogels are used for 3D in vitro assays and tissue engineering and regeneration purposes. For a thorough interpretation of this technology, an integral biomechanical characterization of the materials is required. In this work, we characterize the mechanical and functional behavior of two specific hydrogels that play critical roles in wound healing, collagen and fibrin. A coherent and complementary characterization was performed using a generalized and standard composition of each hydrogel and a combination of techniques. Microstructural analysis was performed by scanning electron microscopy and confocal reflection imaging. Permeability was measured using a microfluidic-based experimental set-up, and mechanical responses were analyzed by rheology. We measured a pore size of 2.84 and 1.69 µm for collagen and fibrin, respectively. Correspondingly, the permeability of the gels was 1.00·10-12 and 5.73·10-13 m2. The shear modulus in the linear viscoelastic regime was 15 Pa for collagen and 300 Pa for fibrin. The gels exhibited strain-hardening behavior at ca. 10% and 50% strain for fibrin and collagen, respectively. This consistent biomechanical characterization provides a detailed and robust starting point for different 3D in vitro bioapplications, such as collagen and/or fibrin gels. These features may have major implications for 3D cellular behavior by inducing divergent microenvironmental cues. Moreno-Arotzena , Oihana; Meier, Johann G; del Amo, Cristina; García-Aznar, José Manuel

Full text

Materials 2015, 8, 1636-1651; doi:10.3390/ma8041636 materials ISSN 1996-1944 www.mdpi.com/journal/materials Article Characterization of Fibrin and Collagen Gels for Engineering Wound Healing Models Oihana Moreno-Arotzena 1, Johann G. Meier 2, Cristina del Amo 1 and José Manuel García-Aznar 1,* 1 Multiscale in Mechanical and Biological Engineering (M2BE), Department of Mechanical Engineering, Aragon Institute of Engineering Research (I3A), Universidad de Zaragoza, Mariano Esquillor Street, 50018 Zaragoza, Spain; E-Mails: [email protected] (O.M.-A.); cdelam[email protected] (C.A.) 2 ITAINNOVA Instituto Tecnológico de Aragón, 7-8 María de Luna Street, 50018 Zaragoza, Spain; E-Mail: [email protected] * Author to whom correspondence should be addressed; E-Mail: jm[email protected]; Tel.: +34-976-762-796; Fax: +34-976-762-670. Academic Editor: Amir A. Zadpoor Received: 27 February 2015 / Accepted: 2 April 2015 / Published: 10 April 2015 Abstract: Hydrogels are used for 3D in vitro assays and tissue engineering and regeneration purposes. For a thorough interpretation of this technology, an integral biomechanical characterization of the materials is required. In this work, we characterize the mechanical and functional behavior of two specific hydrogels that play critical roles in wound healing, collagen and fibrin. A coherent and complementary characterization was performed using a generalized and standard composition of each hydrogel and a combination of techniques. Microstructural analysis was performed by scanning electron microscopy and confocal reflection imaging. Permeability was measured using a microfluidic-based experimental set-up, and mechanical responses were analyzed by rheology. We measured a pore size of 2.84 and 1.69 μm for collagen and fibrin, respectively. Correspondingly, the permeability of the gels was 1.00·10−12 and 5.73·10−13 m 2. The shear modulus in the linear viscoelastic regime was 15 Pa for collagen and 300 Pa for fibrin. The gels exhibited strain-hardening behavior at ca. 10% and 50% strain for fibrin and collagen, respectively. This consistent biomechanical characterization provides a detailed and robust starting point for different 3D in vitro bioapplications, such as collagen and/or fibrin gels. These features may have major implications for 3D cellular behavior by inducing divergent microenvironmental cues. OPEN ACCESS Materials 2015, 8 1637 Keywords: wound healing; 3D; in vitro; hydrogel; scaffold; biomechanical; biophysical; microstructure; permeability; rheology 1. Introduction Wound healing demonstrates the capacity of skin to regenerate in an orchestrated manner. However, pathological healing processes, such as fibrosis, hypertrophic scars or ulcers, can lead to major disabilities or even death and have a high global incidence [1]. As a reference, 3–6 million people in the United States were affected by these disorders in 2010 [2]. The healing process is the result of a complex interaction of many factors that regulate the development of wounds. This complexity has been addressed by means of diverse approaches. In vivo [3], in vitro [4,5] and in silico [6] studies have been performed to elucidate fundamental wound healing mechanisms. In vitro assays have been developed to analyze reepithelialization [7,8]. However, a more complex 3D process occurs in full-thickness injury healing [9]. Novel methodologies based on microfluidic techniques are being developed that offer unique features for the rational design of physiologically relevant in vitro systems [10], which could be directed to mimic wound healing processes. Hydrogels have been employed to resemble the extracellular matrix (ECM) [11,12]. Although progress has been made, knowledge of the most adequate conditions to recreate the local microenvironment of wound healing remains lacking. In a reductionist simplification of the environmental complexity of the wound healing scenario, three main actors can be distinguished: cells, environmental signaling and the ECM. Most previous studies have focused on analyzing the cell-environment signaling interaction [13]. The regulatory role of the ECM is considered critical for cellular processes, e.g., wound healing [14,15]. The ECM is a 3D fibrillar network that provides both architectural scaffolding and a heterogeneous signaling distribution in the whole cell vicinity. The biomechanical cues arising from the ECM play a fundamental role in the modulation of cellular behavior and mechanotransduction in wound healing [15]. The contributions of matrix stiffness and microstructure on cell behavior have been widely demonstrated [16,17]. Recent evidence also indicates a relevant role of interstitial flow [18–20] and ECM confinement level [21–23] on basic cellular processes, e.g., 3D cell migration. Therefore, to develop accurate biomimetic in vitro models, it is crucial to select the most adequate material to resemble the ECM in vivo. In wound healing, the primary matrices are the fibrin clot and the granulation tissue, which is mainly formed by newly-deposited collagen [15]. To represent these local microenvironments, biomimetic hydrogels composed of fibrin or collagen I, respectively, are typically used [24,25]. These proteins are very useful because they self-assemble at a proper ionic strength [26]. However, for applications with the objective of recreating wound healing environments, a profound knowledge of the biomechanical and biophysical properties of both hydrogels is required. In this regard, multiple studies have analyzed the microstructural features and bulk stiffness of similar hydrogels [27–30]. As elements of the microstructure, fiber arrangement and diameter have been extensively studied by scanning electron microscopy (SEM) [31] and confocal reflection imaging (CRI) [32]. Rheological [29,30,33,34], axial tensile tests [28,35] and other techniques [36,37], as well as Materials 2015, 8 1638 assays at the individual fiber level [38,39] have been performed. A limited number of studies have also quantified the hydraulic resistance of gel scaffolds to fluid flow. These studies have focused on improving the nutrient diffusion in scaffolds for tissue engineering applications [40,41] or analyzing 3D cell migration [18,42]. The application of collagen and fibrin hydrogels as scaffolds in tissue engineering and in vitro experiments and their biomechanical characterization have increased remarkably [27,29,35]. However, these studies have employed a wide diversity of hydrogel compositions and different measurement methods [43]. Modification of the gel composition, polymerization temperature or pH alters various biophysical properties [44]. These variations hinder the application of hydrogels in the controlled representation of microenvironments for wound healing experiments, as well as the analysis of the impact of these parameters on the cell response. Due to the infeasibility of addressing all possible combinations, in this work, we chose generalized and defined compositions for the gel scaffolds. The chosen specific collagen and fibrin gels have been widely used as physiologically-relevant matrix representations [33,43,45], in applications such as wound healing. Our main aim was to establish a quantitative evaluation of the functional behavior of both hydrogels under experimental conditions that were as comparable as possible. Therefore, we assessed not only the microstructural and rheological properties of both scaffolds, but also their hydraulic resistance to fluid flow. We obtained coherent and corresponding datasets for each hydrogel composition using four complementary experimental techniques that have not previously been used in combination for these gels. This work reports the complete characterization of relevant parameters for biomimetic matrices for 3D in vitro assays and primarily focuses on mimicking wound regeneration using widely-used collagen and a fibrin hydrogel compositions. The presented methodology could also be suitable for the study of other scaffolds and their variations. 2. Experimental Section 2.1. Preparation of Fibrin and Collagen Gels 2.1.1. Fibrin Gels Plasminogen-, fibronectin- and factor XIII-depleted human fibrinogen (American Diagnostica GmbH) was diluted in buffer (50 mM Tris, 100 mM NaCl and 5 mM EDTA) as indicated by the provider. The fibrinogen was mixed with human FXIII (American Diagnostica GmbH) and allowed to polymerize in the presence of human alpha-thrombin (American Diagnostica GmbH), CaCl2 (Sigma) and cell culture media FGM-2 BulletKit (Lonza). Finally, the hydrogels were hydrated and stored in an incubator for 24 h before initiating any experiment. The pH of the gels was 7.4, and the concentration of each constituent per final volume was 3.3 mg·mL−1 fibrinogen, 22 μg·mL−1 FXIII, 1 U·mL−1 thrombin and 5 mM CaCl2. Materials 2015, 8 1639 2.1.2. Collagen Gels The procedure for constructing collagen gels was adapted from a previous work by Shin et al. [46]. Collagen type I (BD Biosciences) was buffered to a final concentration of 2 mg·mL−1 with 10× DPBS (Gibco) supplemented with calcium and magnesium, cell culture media FGM-2 BulletKit (Lonza) and cell culture-grade water (Lonza). The pH of the dilution was adjusted to 7.4 with NaOH. Mixtures were allowed to polymerize inside humid chambers at 37 °C. Next, the gels were hydrated and stored in an incubator for 24 h before experimentation. 2.2. Scanning Electron Microscopy Hydrogels were fixed with 2.5% glutaraldehyde (Sigma-Aldrich) followed by 1% electron microscopy grade osmium tetroxide (Ted Pella, Inc., Redding, CA, USA). The hydrogels were subsequently dehydrated in 30%, 50%, 70%, 80% and 95% ethanol solutions, respectively. Gels were freeze-fractured in liquid nitrogen before a final dehydration step in 100% ethanol. The gels were finally subjected to critical point drying using a Baltec CPD030. The samples were sputter-coated with gold-palladium for 4 min using an Emitech K550, resulting in a layer thickness of 15 nm. The samples were visualized by high-resolution imaging with a Merlin field emission scanning electron microscope (FESEM) from Zeiss with a beam voltage of 1 kV and a magnification of 80–120 kX. 2.3. Confocal Reflection Imaging Confocal reflection was performed using a Leica SP2 equipped with a 63×/1.4 N.A. (numerical aperture) oil immersion lens. The samples were excited at 488 nm with an argon laser and detected at 479–498 nm. 2.4. Microstructural Analysis To elucidate the microstructural features of the 3D networks, confocal reflection imaging (CRI) and SEM images were acquired as previously described. The void ratio, pore size and fiber radius were evaluated using the free software ImageJ [47]. For the fiber radius and pore size measurements, a straight line and measurement tools were employed. For void ratio analysis, confocal reflection images were binarized. The fiber-to-pore ratio was subsequently calculated from the areas of white (pores) and black (fibers) pixels within the binary images. Three independent sets were examined for each hydrogel, and the data are presented as the mean ± SEM. 2.5. Permeability Experiments To measure Darcy’s permeability () of the hydrogels, a specific microfluidic-based experimental set-up was employed. This set-up reproduced the hydraulic environment of the in vitro physiological studies of wound healing. A microfluidic platform was used to assess the permeability values of both hydrogels. The gels were allowed to polymerize within the microfluidic devices, which were fabricated as described by Shin et al. [46]. Medium reservoir tubes were inserted into the channel outlets (shown in Materials 2015, 8 1640 Figure 1) as described by Sudo et al. [48]. The difference in height of the media columns on both sides of the gel caused a pressure gradient of 500 or 13 mm of H 2 O for fibrin and collagen, respectively. Figure 1. Microfluidic-based experimental set-up for permeability measurements. (a) The schematic shows the arrangement of the media columns with respect to the geometry. The design comprises a central gel cage (fuchsia) and two main media channels (pink), which are connected to the corresponding media columns. (b) A picture of an actual experiment demonstrates a pressure difference of approximately 100 Pa across the gel induced by the height difference between the media columns on both sides of the geometry. From Darcy’s law, the relationship between the pressure difference and the permeability is as follows: ∆P󰇛t󰇜∆P 󰇛0󰇜e  (1) where  is time, ∆󰇛󰇜 is the pressure difference at each time point and ∆󰇛0󰇜 is the initial pressure difference. The constant  is related to the permeability , as shown below [48]: K󰇛m󰇜c μ LA ρgA (2) where μ and ρ are the viscosity and density of the fluid, respectively,  is the length of the gel through which the pressure drop is established,  is the area of the media reservoirs,  is the acceleration due to gravity and  is the cross-sectional flow area. Therefore, Equation (1) states that, for a given initial pressure difference, the pressure difference will tend to equilibrium with an exponential decay. Based on this interpretation, by tracing the experimental pressure difference drop over time, the measured data points were fitted using Equation (1), and the value of  was obtained for each hydrogel. Finally, to characterize the interstitial resistance to flow, Equation (2) was solved for, and Darcy’s permeability values were determined. 2.6. Rheology For the rheological measurements, a Bohlin Gemini 200 HR Nano rheometer was used. The lower torque limit of the instrument was 3 nN·m in oscillation. All tests were performed using a cone-plate geometry with a diameter of 40 mm, a cone angle of 1° and a truncation height of 30 µm. The temperature was maintained at 37 °C ± 0.1 °C using a Peltier plate. The samples were pipetted onto the rheometer plate by filling its gap, as demonstrated in Figure 2. To prevent evaporation, the shear gap was covered with a 0.1 Pa·soil, used for calibration. Materials 2015, 8 1641 Figure 2. Image sequence of the gel filling process on the rheometer. Once the sample was mixed, it was pipetted in situ onto the rheometer plate (a); then, the gap was adjusted (b), and the sample was covered with oil (c) to prevent evaporation; the set-up was then ready to conduct the experiment (d). The curing reaction was traced by measuring the evolution of the shear modulus over time at a constant temperature of 37 °C, an oscillation frequency of 1 rad·s −1 and an applied strain amplitude of 0.005. The dependence of the sample moduli on the oscillatory strain amplitude was measured at a constant temperature of 37 °C for excitation frequencies of 0.1 Hz and 0.01 Hz. The strain amplitude was varied in a logarithmically-equidistant interval of 10 measurement points per decade from 0.001 to 1. For each point, data from 6 periods were accumulated. 3. Results and Discussion 3.1. Microstructural Study Confocal reflection and SEM images were acquired to visualize both the collagen and fibrin hydrogels. As shown in Figures 3 and 4, the lattices of fibrin were more entangled than those of collagen. The collagen networks exhibited twisted patterns formed by bundled fibers, consistent with that reported by Lai et al. [28,35]. The assembled fibrin fibers were straighter and appeared more individually, consistent with its role in physiological clot structures [49]. In addition to this qualitative assessment, microstructural features, such as the void ratio, pore size and fiber radius, were estimated from the images and are summarized in Table 1. As shown in the images, the fiber density of the fibrin networks was greater than that of the collagen matrices, leading to void ratios of approximately 71% and 80%, respectively. Accordingly, the pore size was 1.69 μm for fibrin and 2.84 μm for collagen. The fiber radii were approximately 79 and 66 nm for fibrin and collagen, respectively. For the collagen fibers, the variation of the measured data was quite high, probably due to the variability introduced by the characteristic bundling. Table 1. Microstructural characteristics of the hydrogels † . Collagen Fibrin Void ratio (%) 80.15 ± 1.82 71.46 ± 1.00 Pore size (μm) 2.84 ± 0.94 1.69 ± 0.33 Fiber radius (nm) 79.51 ± 33.16 66.53 ± 13.57 † Data are the mean ± SEM. Materials 2015, 8 1642 Figure 3. 3D network of the hydrogels. The confocal reflection images show the arrangement of the fibrillar networks for (a,b) fibrin and (c,d) collagen gels. (a) and (c) show a general view; (b) and (d) are zoomed images of the right-bottom corner of the previous images, respectively. Fibers composing the collagen networks are twisted, whereas the fibers in the fibrin appear straighter. Scale bars correspond to 10 μm. Figure 4. Fiber layout within hydrogels. SEM images of (a,b) fibrin and (c,d) collagen gels acquired at magnifications of 80–120 kX show the morphological features of the fibers. The collagen fibers exhibit characteristic bundling, whereas the fibrin fibers are formed more individually. The scale bars correspond to 200 nm. Materials 2015, 8 1643 3.2. Permeability Quantification Previous work has primarily focused on analyses of microstructure and bulk stiffness due to the key roles of these properties in basic cellular events in 2D [50]. However, wound healing primarily occurs under 3D conditions, and there is accumulating evidence that the confinement of cells has a crucial role on their behavior [21,22,51,52]. A bulk quantity that relates to the confinement feature of hydrogels is their hydraulic resistance. The hydraulic resistance of hydrogel matrices not only controls the transport of nutrients and the shear stress exerted on cells, but also regulates the directional migration of the cells [42,53]. Therefore, in this characterization, we include the assessment of the hydraulic resistance to fluid flow of the scaffolds, because it is key to the rational design and interpretation of physiologically-relevant microsystems. To quantify the hydrogel permeability, we generated an initial pressure difference across both hydrogels. As shown in Figure 5, the decrease in pressure difference over time was then monitored. The obtained data points were then fitted to an exponential function formatted as in Equation (1), and R2 values of 0.96 and 0.98 for fibrin and collagen, respectively, were obtained. The exponent coefficient values󰇛󰇜 from the fitting were 0.13 h−1 or 4.00·10−05 s−1 for fibrin and 0.24 h−1 or 7.00·10−05 s−1 for collagen. Likewise, by solving Equation (2) for, we calculated Darcy’s permeability for fibrin and collagen: 5.73·10−13 and 1.00·10−12 m2, respectively. The values of and  are provided in Table 2. These parameters establish the resistance that a particular porous matrix exerts on the convective fluid flow, i.e., the velocity with which a pressure difference will tend toward equilibrium. Figure 6 illustrates, for a given initial pressure difference, the pressure difference decay for both hydrogels. Pressure equilibrium is achieved more rapidly in the collagen gels than the fibrin gels, indicating less resistance to flow and consistent with the greater void ratio and pore size of the collagen gel observed in the image analysis and other previous measurements [41,42]. Figure 5. Pressure difference drop over time in hydrogels. The experimental data points of the pressure difference vs. time were plotted and fitted to an exponential function for fibrin (left) and collagen (right) gels. The resulting expressions and R2 values are also indicated. The exponent coefficient determines the value of the permeability (). Table 2. Resistance to fluid flow. Collagen Fibrin Exponent coefficient, c (s−1) 7.00·10−05 4.00·10−05 Darcy’s permeability, K (m2) 1.00·10−12 5.73·10−13 Materials 2015, 8 1644 Figure 6. Comparison of the pressure difference drop for both hydrogels. The curves show the pressure difference drop over time for a given initial pressure difference for the collagen and fibrin hydrogels. Compared with collagen, the lower permeability (K) of the fibrin results in a slower function decay. 3.3. Mechanical Response The polymerization was traced for 3 h, beginning immediately after the gel solution was pipetted and set within the rheometer plate. Figure 7 shows the evolution of the shear modulus (G’) over time at a constant temperature of 37 °C. The biexponential function given in Equation (3) fits the measured data points well, thus suggesting two processes with distinct reaction rates (a fast and a slow rate), t 1 and t 2 , resulting in an increase in the value of the modulus: 󰆒󰇛󰇜󰆒1󰇡    󰇢󰆒1󰇡    󰇢 (3) where G’1 and G’2, are the associated parameters that characterize the modulus contribution of each process and xc is the parameter that adjusts the time scale to the beginning of the reactions. Figure 7. Time evolution of the shear modulus (G’) of the hydrogels. The temperature was maintained at 37 °C; the excitation frequency was 1 rad·s−1; and the strain amplitude was 0.005. The lines are fits to the biexponential Equation (3). Note that the polymerization of the gels was not yet complete, cf. Figure 8. Materials 2015, 8 1651 50. Engler, A.J.; Sen, S.; Sweeney, H.L.; Discher, D.E. Matrix Elasticity Directs Stem Cell Lineage Specification. Cell 2006, 126, 677–689. 51. Prentice-Mott, H.V.; Chang, C.-H.; Mahadevan, L.; Mitchison, T.J.; Irimia, D.; Shah, J.V. Biased Migration of Confined Neutrophil-like Cells in Asymmetric Hydraulic Environments. Proc. Natl. Acad. Sci. USA 2013, 110, 21006–21011. 52. Wolf, K.; Friedl, P. Extracellular Matrix Determinants of Proteolytic and Non-Proteolytic Cell Migration. Trends Cell Biol. 2011, 21, 736–744. 53. Shi, Z.-D.; Tarbell, J.M. Fluid Flow Mechanotransduction in Vascular Smooth Muscle Cells and Fibroblasts. Ann. Biomed. Eng. 2011, 39, 1608–1619. 54. Ulrich, T.A.; Jain, A.; Tanner, K.; MacKay, J.L.; Kumar, S. Probing Cellular Mechanobiology in Three-Dimensional Culture with Collagen-Agarose Matrices. Biomaterials 2010, 31, 1875–1884. 55. Pritchard, R.H.; Huang, Y.Y.S.; Terentjev, E.M. Mechanics of Biological Networks: From the Cell Cytoskeleton to Connective Tissue. Soft Matter 2014, 10, 1864–1884. 56. Shah, J.V.; Janmey, P.A. Strain Hardening of Fibrin Gels and Plasma Clots. Rheol. Acta 1997, 36, 262–268. 57. Mitsak, A.G.; Dunn, A.M.; Hollister, S.J. Mechanical Characterization and Non-Linear Elastic Modeling of Poly(glycerol Sebacate) for Soft Tissue Engineering. J. Mech. Behav. Biomed. Mater. 2012, 11, 3–15. 58. Legant, W.R.; Miller, J.S.; Blakely, B.L.; Cohen, D.M.; Genin, G.M.; Chen, C.S. Measurement of Mechanical Tractions Exerted by Cells in Three-Dimensional Matrices. Nat. Methods 2010, 7, 969–971. 59. Doyle, A.D.; Petrie, R.J.; Kutys, M.L.; Yamada, K.M. Dimensions in Cell Migration. Curr. Opin. Cell Biol. 2013, 25, 642–649. 60. Ehrbar, M.; Sala, A.; Lienemann, P.; Ranga, A.; Mosiewicz, K.; Bittermann, A.; Rizzi, S.C.; Weber, F.E.; Lutolf, M.P. Elucidating the Role of Matrix Stiffness in 3D Cell Migration and Remodeling. Biophys. J. 2011, 100, 284–293. 61. Kubow, K.E.; Conrad, S.K.; Horwitz, A.R. Matrix Microarchitecture and Myosin II Determine Adhesion in 3D Matrices. Curr. Biol. 2013, 23, 1607–1619. © 2015 by the authors; licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution license (http://creativecommons.org/licenses/by/4.0/).