Full text
Final Master Project Characterization of polycaprolactone/mesoporous silica composite membranes Author Iván Vera Alaya Director Dr. Silvia Irusta Alderete NANOSTRUCTURED MATERIALS FOR NANOTECHNOLOGY APPLICATIONS Institute of Nanoscience of Aragon University of Zaragoza 2014-2015
Acknowledgements First I would like to thank my supervisor Dr. Silvia Irusta for the opportunity to work on this research group, for their great help and patience during this project, and for the support when perform FTIR. I would also like to thank all my lab mates and my classmates. I especially want to thank Laura López and Ismael Pellejero for their advice and for the great help they have provided me, without which it would be impossible to finish this project on time, and Ángela López for letting me use the equipment whenever I needed it for my experiments. Also deserve special attention Nuria Navascues and Carlos Cuestas for their help in making the TGA and SEM analyses. Last but not least, I want to thank my friends, especially María Picazo for her encouragement, her understanding and her continued support throughout the course. Without her I had not started this master and, of course, I could not have been able to finish it. Many thanks “Pollo”.
Abstract In the present project polycaprolactone (PCL) with mesoporous silica (MCM-41) as filler based membranes were prepared and characterized. PCL was chosen because it is biocompatible, biodegradable and has an excellent tensile strength. Because of these characteristics PCL has found diverse applications in several fields: packaging, tissue engineering, drug delivery, etc. MCM-41 is a mesoporous material with hexagonal arrangement of uniform mesopores, highly specific surface (up to 1500 m2/g), and adjustable pore diameter (2-10 nm). Composite membranes were prepared by casting and solvent evaporation method. The inorganic loading of the membranes was measured by Thermogravimetric Analysis (TGA) while structure and morphology were analyzed by Fourier Transform Infrared Spectroscopy (FTIR) and Scanning Electron Microscope (SEM). Permeability test were carried out in a home-made experimental plant. The gases used for permeation were oxygen and carbon dioxide. Theoretical and experimental selectivity were compared. Incorporating MCM-41 nanoparticles reduced O2 and CO2 permeation around 20% and 80% respectively, compared to pristine PCL. Also, incorporating these nanoparticles functionalized with EPTES caused a greater decrease in O2 and CO2 permeation, 26% and 90% respectively. For both composite membranes a higher O2/CO2 selectivity was obtained.
i Table of Contents 1. Introduction ......................................................................................................................... 1 1.1. Poly(ε-caprolactone) ................................................................................................. 5 1.2. PCL Composites ....................................................................................................... 6 2. Objectives. ............................................................................................................................ 8 3. Experimental Part ............................................................................................................... 9 3.1. Materials .................................................................................................................... 9 3.1.1. Synthesis of MCM-41 .................................................................................. 9 3.1.2. Functionalization of MCM-41 ...................................................................... 9 3.1.3. Synthesis of PCL and PCL composites ...................................................... 10 3.2. Preparation of PCL membranes .............................................................................. 10 3.3. Thermogravimetric Characterization ...................................................................... 11 3.4. FTIR Characterization ............................................................................................. 12 3.5. Scanning Electron Microscope Characterization .................................................... 12 3.6. Permeation Characterization ................................................................................... 12 3.6.1. Equipment ................................................................................................... 12 3.6.2. Permeation Measurement ........................................................................... 15 3.6.2.1. Calibration of the equipment .......................................................... 15 3.6.2.2. Membrane stabilization .................................................................. 15 3.6.2.3. Permeate, Retentate and Feed Measurement .................................. 16 3.6.2.4. Permeation Calculation .................................................................. 17 4. Results and Discussion ...................................................................................................... 19 4.1. Thermogravimetric Characterization ...................................................................... 19 4.2. FTIR Characterization ............................................................................................. 22 4.3. Scanning Electron Microscope Characterization .................................................... 26 4.4. Permeation Characterization ................................................................................... 32 5. Conclusion and Future Work ........................................................................................... 39 References .............................................................................................................................. 40
ii Figures Figure 1. Basics principle of membrane process ....................................................................... 1 Figure 2. Types of membranes and transport mechanisms ....................................................... 2 Figure 3. Scheme of the structure of inorganic membrane........................................................ 4 Figure 4. ROP polymerization of ε-capolactone ....................................................................... 5 Figure 5. Structure of CTAB (a) and TEOS (b) ........................................................................ 9 Figure 6. Structure of EPTES .................................................................................................. 10 Figure 7. Teflon caster ............................................................................................................. 11 Figure 8. Membrane samples: (a) Membrane after the casting process and (b)Membrane with the optimized size for the permeation measurements...................................................... 11 Figure 9. Scheme of the permeation plant ............................................................................... 13 Figure 10. Permeation module. (a) Side view (b) Position of the components (c) Inner side view (d) Scheme of the module ....................................................................................... 14 Figure 11. Membrane with defects (a) and enlargement of the marked zone (b) .................... 16 Figure 12. Membrane cracks after permeation measurements ................................................ 17 Figure 13. TGA analysis of the membranes ............................................................................ 19 Figure 14. Degradation temperature of the membranes .......................................................... 20 Figure 15. TGA analysis of the fillers ..................................................................................... 21 Figure 16. Degradation temperature of the fillers ................................................................... 21 Figure 17. FITR spectra of PCL: (a) Complete frequency range and (b) Low frequency range ........................................................................................................................................ 22 Figure 18. FTIR spectrum of MCM-41 ................................................................................... 23 Figure 19. FTIR spectrum of MCM-41 functionalized with EPTES ...................................... 24 Figure 20. FTIR spectra of fillers in the high (a) and low (b) frequency range ...................... 25 Figure 21. SEM images of pristine PCL membrane at different magnifications .................... 27 Figure 22. SEM images of PCL-MCM41 (a) and magnification of the marked zone (b) ....... 29 Figure 23. Detail of the MCM-41 nanoparticles ..................................................................... 29 Figure 24. SEM images of PCL-MCM41-EPTES (a) and magnification of the marked zone (b) .................................................................................................................................... 31 Figure 25. Stabilization time of a PCL membrane with O2 ..................................................... 32
iii Figure 26. Stabilization time of a PCL membrane with CO2 .................................................. 33 Figure 27. Permeation comparison between individual gases and mixtures through a PCL membrane ........................................................................................................................ 33 Figure 28. Permeation of membranes with individual gases ................................................... 35 Figure 29. Proposed reaction mechanism between CO2 and amino groups ............................ 36 Figure 30. Permeation of membranes with a mixture of gases ............................................... 37 Tables Table 1. Main polymers used in organic membranes ................................................................ 3 Table 2. Conditions of the columns ......................................................................................... 15 Table 3. Results of the TGA analysis ...................................................................................... 20 Table 4. Characteristic infrared bands of PCL ........................................................................ 23 Table 5. Characteristic infrared bands of MCM-41 and MCM-41 functionalized with EPTES ..................................................................................................................................... 24 Table 6. FTIR bands related EPTES ....................................................................................... 26 Table 7. EDX results of a pristine PCL membrane ................................................................. 28 Table 8. EDX results of a PCL-MCM41 membrane ............................................................... 30 Table 9. EDX results of a PCL-MCM41-EPTES membrane .................................................. 31 Table 10. Permeation summary ............................................................................................... 38
Iván Vera Alaya – Final Master Project Introduction 1 1. Introduction Membrane technology is one of the fastest growing fields in the last years in separation process. Even though these processes are a relatively new type of separation technology, several membranes processes, particularly pressure-driven processes including reverse osmosis, nano-filtration, ultra and microfiltration, are already applied on industrial scale [1]. The concept of membrane separation process is a relatively simple process because ideally include only two flows (feed and permeate) and a separator element (membrane), as seen in Figure 1. Figure 1. Basic principle of membrane process However, the increasing complexity of separation operations makes membrane processes complex. Membrane methods are able to separate very diverse mixtures, beginning from gas mixtures containing the smallest molecules like H2 and He, to mixtures of particles beyond molecular sizes, such as viruses or bacterial cultures. Gaseous, liquid, and supercritical media, even solids in a suspension, can be separated by membranes. Due to this variety of substances capable of separating, membranes have found a wide application in diverse fields such as medicine, ecology, power engineering, chemical industry, agriculture, etc [2].
Iván Vera Alaya – Final Master Project Introduction 2 In general, some of the main advantages of separation processes based in membranes are [3]: - Separation is performed continuously - Low energy consumption - Easily combine with other separation processes - Easy scale-up - Adjustable membrane properties Considering the structure of membranes, it can be classified into two main groups: porous and dense membranes [4]. Porous membranes have a highly voided structure interconnect by pores. These pores are extremely small, of the order of 0.01 to 10 microns. In this type of membranes, basically two mechanisms of gas transport occur, as shown in Figure 2. The first mechanism is based on Knudsen diffusion in which permeation is inversely proportional to molecular weight of the permeants. The other mechanism is molecular sieve where permeation is inversely proportional to the size of molecules: particles smaller than the pores will pass through the membrane, and larger particles are rejected. In contrast, dense membranes consist of a dense film, without pores, through which permeants first dissolve in the membrane and then diffuse through it under the driving force of pressure, concentration, or potential gradient (solution-diffusion mechanism). The separation of components depends on their solution and diffusion in the membrane. Most gas separation, pervaporation, and reverse osmosis use this type of membranes. Figure 2. Types of membranes and transport mechanisms
Iván Vera Alaya – Final Master Project Introduction 3 Finally, considering the material, the membranes can be classified in organic and inorganic [5]. The first organic membranes were prepared from cellulose and derivatives of it, however, while still being used, it has low thermal resistance and limited resistance to chemicals. Thanks to advances in the field of synthetic polymers in recent years, these membranes of cellulose have been replaced by polymeric membranes improving quantitatively the properties. In Table 1 [3] the main polymers used in the manufacture of membranes is shown. Table 1. Main polymers used in organic membranes Polymer MF UF RO GS PV Cellulose and derivates * * * * * Polydimethylsiloxane (PDMS) * * Polyethylene (PE) * * Polypropylene (PP) * Polyvinyl chloride (PVC) * * Polyvinyl fluoride (PVF) * * Polymethylpentene (PMP) * Polyester (UP) * Polyvinyl alcohol (PVA) * Polyacrylonitrile (PAN) * * * * Polycarbonate (PC) * * Polytetrafluoroethylene (PTFE) * * Polyamide (PA) * Polyamide-imides (PAI) * * Polysulfone (PSU) * * * * Polyether-sulfone (PES) * Polyphenylene oxides (PPO) * * * Polyesteramide (PEA) * Polybenzimidazole (PBI) * * MF: Microfiltration; UF: Ultrafiltration; RO: Reverse Osmosis; PV: Pervaporation; GS: Gas Separation
Iván Vera Alaya – Final Master Project Experimental Part 10 trimethoxysilane, C 8 H 22 N 2 O 3 Si, ≥80%, Sigma-Aldrich), Figure 6, were added and stirred for 3.5 h. Finally, the solution was cooled at room temperature, filtered under vacuum and washed several times with toluene (≥99.5%, Sigma-Aldrich) to recover the solid. Figure 6. Structure of EPTES 3.1.3. Synthesis of PCL and PCL composites PCL and PCL composites were produced by Nanostructured Films and Particles group (NFP) at the Institute of Nanoscience of Aragon (INA) by in situ polymerization of ɛ-caprolactone monomer (97%, Sigma-Aldrich) using SnCl 2 ·2H 2 O (98%, Sigma-Aldrich) as catalyst [27]. Three samples of PCL were used in this project: pristine PCL, PCL filled with 1.74% wt of MCM-41 (PCL-MCM) and PCL filled with 2.01% wt of MCM-41 functionalized with EPTES (PCL-MCM-EPTES). Tasks 2.1.1 to 2.1.3 were carried out by other members of the NFP group. 3.2. Preparation of PCL membrane PCL membranes were produced by solution casting and solvent evaporation method [28]. First, 0.75 g of solid PCL was placed in an oil bath at 80 ºC 5 minutes to facilitate dissolution. Then 20 mL of chloroform were added and the solution was stirred at 300 rpm during 27 minutes. After this time the solution was cooled with wet paper for 2 min. Finally the solution was cast on a Teflon caster (Figure 7) and the solvent was evaporated (in a hood) at room temperature for 24 hours. PCL composite membranes were prepared by the same method using the PCL with fillers as raw material.
Iván Vera Alaya – Final Master Project Experimental Part 11 Figure 7. Teflon caster Membranes were cut to the appropriate size to fit in the permeation module, which in this case was 25 mm in diameter, as shown in Figure 8. Thickness of the membranes were measured with a micrometer (Baxlo 4000), obtaining an average of 60 μm. Figure 8. Membrane samples: (a) Membrane after the casting process and (b) Membrane with the optimized size for the permeation measurements 3.3. Thermogravimetric Characterization The degradation temperature of PCL and PCL composites, and the amount of silica in the polymer were evaluated by Thermal Gravimetric Analysis (TGA) using an Universal Analysis Q5000 instrument. Samples were placed in a platinum melting cup (a) (b) 25 mm
Iván Vera Alaya – Final Master Project Experimental Part 12 and TG analyses were carried out at a rate of 5 °C/min from 30 to 800oC under N2 atmosphere. The amount of filler dispersed in PCL membrane was calculated from the remaining mass. MCM-41 and MCM-41 functionalized powders were also analyzed in the same conditions. 3.4. FTIR Characterization PCL and PCL composites were analyzed by FTIR spectroscopy (Vertex 70 spectrometer) in the 4000-600 cm-1 region. The number of scans was fixed to 40 with a resolution of 4 cm-1. MCM-41 and MCM-41 functionalized powders were also analyzed in the same conditions. 3.5. Scanning Electron Microscope Characterization The morphology of the membranes and the distribution of silica particles were examined using Scanning Electron Microscopy (SEM), FEI Inspect F50. In order to improve image resolution, all samples were coated with a 15 nm platinum layer deposited by sputtering (SC7620 Mini Sputter Coater, Quorum Technologies) to minimize electron damage to the sample, electron beam voltage was fixed at 10 kV maximum. 3.6. Permeation Characterization 3.6.1. Equipment Permeation experiments were carried out in an home-made experimental plant, which scheme is depicted in Figure 9. The plant was controlled by a software (based in labView® and developed by electronic instrumentation service of University of Zaragoza) that allowed modify mass flow controllers (MFC), and a system of electrovalves (EV) to select the appropriate gas feeds for membrane experiments. O2 and CO2 (99.99% and 99.999% respectively) feed mixtures the permeation module and He (99.9%) was used as a carrier. Permeate and retentate are selected alternativately
Iván Vera Alaya – Final Master Project Experimental Part 13 (manual valves V1 and V2) and carry to a gas analyzer (Micro gas chromatograph) for quantification. Figure 9. Scheme of the permeation plant
Iván Vera Alaya – Final Master Project Experimental Part 14 Membrane module (Pall Corporation PN1209) is shown in Figure 10: the membrane was placed on a metal grid inside the module and by an o-ring was achieved to remained it sealed. Figure 10. Permeation module. (a) Side view (b) Position of the components (c) Inner side view (d) Scheme of the module As seen in the Figure 10.d, this module consists in two concentric tubes through which gases circulate. The inlet gases, feed and carrier, flow through the inner tube, and the exit gases, permeate and retentate, on the outside. Finally, after passing through the system gases were analyzed using a Variant CP-4900 Micro-gas chromatograph equipped with two columns, a molecular sieve (Molsieve 5A) to separate O2 and N2 in this case, and a PoraPlot Q (PPQ 10) column to quantify CO2. Table 2 shows the conditions of temperature and pressure used for the analysis of the two columns.
Iván Vera Alaya – Final Master Project Experimental Part 15 Table 2. Conditions of the columns Channel A (Molsieve 5Ᾰ) Channel B (PPQ 10) Column Temperature (ºC) 70 60 Injector Temperature (ºC) 110 110 Pressure (kPa) 120 100 3.6.2. Permeation Measurement 3.6.2.1. Calibration of the equipment Before using the equipment, calibration of mass flow controllers and the micro gas chromatograph was performed. First, flow controllers were calibrated, for this purpose the gauges were open to different apertures and the flow was measured with a bubblemeter to obtain a calibration line: flow (mL/min) vs. % aperture. The micro gas chromatograph was calibrated similarly measuring known concentrations of gases to obtain a relationship between the peak areas measured and the gas concentration. 3.6.2.2. Membrane Stabilization In order to get good peak resolution it was necessary column regeneration. For regeneration procedure columns were kept at 250 ºC for 24 h to ensure that any gas which could affect the measurements was eluded from the system. After completing this process, a membrane was placed on the support and the system was stabilized with a mixture of 20 mL/min of O2 or CO2 and 20 mL/min of He for 30 minutes to remove any gas that may remain in the pipes or in the membrane module. In order to check the absence of pores or defects in the membrane, during the stabilization time, the pressure in the retentate line was increased up to 0.5 bar. It was found that with defective membranes it was not possible to achieve this pressure.
Iván Vera Alaya – Final Master Project Experimental Part 16 Further analysis of these membranes by SEM revealed the presence of pores and holes, as shown in Figure 11. Figure 11. Membrane with defects (a) and enlargement of the marked zone (b) 3.6.2.3. Permeate, Retentate and Feed Measurement A feed gas flow, 50 mL/min of O2, CO2, or mixtures of these gases, were introduced to the membrane module through the retentate side, and the same flow of carrier, He, for the permeate side. The position of the manual valve allowed the selection of the retained or permeated. Furthermore, through the system of valves was possible to send the feed directly to the chromatograph without passing through the membrane to check the feed composition and close the mass balance. All gas flows (retentate, permeate, feed and carrier) were measured using a bubblemeter in each experiment for subsequent calculations and also to check that there was no leakage in the system. All measurements were performed at atmospheric pressure and with 1.5 bar. Due to the thickness of the membrane (60 μm), it was found that pressures higher than 0.75 bar just breaking membranes, as shown in Figure 12.
Iván Vera Alaya – Final Master Project Experimental Part 17 Figure 12. Membrane cracks after permeation measurements 3.6.2.4. Permeation Calculation Permeability of the membranes was calculated by Equation 1, where P is permeability (mol·m·s -1 ·m -2 ·Pa -1 ), F is the molar flux of gas (mol/s) which flows through an effective membrane area (A [m 2 ]) with a determinate thickness (e [m]), under a partial pressure gradient across the membrane (ΔP [Pa]) [29]. ∆ ( Equation 1) The pressure gradient used was calculated as an average logarithmic pressure difference as shown in Equation 2 using partial pressures of each interest gasses (O 2 and CO 2 ). ∆ ∆ ∆ ∆ ∆ ( Equation 2) ∆ ( Equation 3) ∆ ( Equation 4)
Iván Vera Alaya – Final Master Project Experimental Part 18 Operating conveniently Equation 2, and taking into account that the total pressure of the feed is the same as the total pressure of the retentate, and the partial pressure in the carrier is zero (in this flow there is only He), the following equation is obtained based on mole fractions. ∆ ( Equation 5) To facilitate comparison among measurements and also with the literature, and to avoid very small numbers, the unit used in this work is the Barrer [30]. 1 3.348 10 (Equation 6) Finally, selectivity, of the membranes was calculated from the gas permeation as shown in Equation 7. / (Equation 7)
Iván Vera Alaya – Final Master Project Results and Discussion 19 4. Results and Discussion 4.1. Thermogravimetric Characterization The thermal stability of PCL and PCL composite membranes was studied using TGA. Figure 13 shows the weight loss for each membrane vs. temperature. As can be seen, membrane decomposition starts at 250 ºC. At temperature higher of 400 °C the polymer was completely decomposed. In the nanocomposites membranes the final residue was less than 2 wt %. The membrane with MCM-41 presented around 1.35% and the membrane with functionalized MCM-41 1.4%, which corresponded to the amount of filler in each membrane. Figure 13. TGA analysis of the membranes Representing the derivative weight loss as a function of temperature Figure 14 is obtained, which allows to clearly see the variation in degradation temperature. 0 100 200 300 400 500 600 700 800 0 20 40 60 80 100 Weight Loss (%) Temperature (°C) PCL PCL-MCM PCL-MCM-EPTES
Iván Vera Alaya – Final Master Project Results and Discussion 26 peaks, there are four peaks corresponding to the NH2 groups introduced by EPTES at 3360, 3300, 1675 and 1570 cm-1. Finally another important difference between both spectra is the peak at 3745 cm-1 corresponding to free silanol groups. The absence of this peak in the functionalized silica confirms that the amine groups of the EPTES are bonded to free silanol groups during functionalization step. These peaks together with the peaks corresponding to NH2 groups confirm the functionalization of the silica [37-38]. The peaks of interest indicated in Figure 20 are tabulated in Table 6. Table 6. FTIR bands related EPTES Position (cm-1) Vibrator 3745 Free silanol groups 3360 Asymmetric NH2 stretching 3300 Symmetric NH2 stretching 2950 Asymmetric CH2 stretching 2865 Symmetric CH2 stretching 1675 Deformation mode of NH2 1635 Stretching mode of H2O 1570 NH2 bending 1470 Asymmetric CH3 stretching 1370 Symmetric CH3 stretching 4.3. Scanning Electron Microscope Characterization The morphology of the membranes of both PCL and PCL composite were analyzed by SEM. This technique was also useful to confirm the presence of silica nanoparticles. Finally using Energy-Dispersive X-ray spectroscopy (EDX) the composition of both particles membranes were analyzed. First PCL pristine membrane was measured to use as a control membrane. Different points of the sample were analyzed in order to check the homogeneity of the membrane and the absence of defects. Results are shown in Figure 21.
Iván Vera Alaya – Final Master Project Results and Discussion 27 Figure 21. SEM images of pristine PCL membrane at different magnifications As seen in Figures 21a and 21b, PCL pristine membrane is not completely flat but has a certain surface roughness. This roughness is due to its preparation by the casting process. However at higher magnification, Figure 21c and 21d, it can be seen that the membrane has high homogeneity and no defects such as pores or holes. In order to check the composition of the membrane, and the absence of impurities, several EDX analysis of the area shown in Figure 21d were performed. This area was chosen because there are shapes that seem small particles. After analysis by EDX, it was confirmed that these shapes are areas where the polymer is not completely flat, resulting in those forms which are easily confused with particles or impurities. Due to the conditions used: spot 2.5 and a voltage of 10kV, the electron beam is capable of penetrating a depth of about 1.3 micron so both the silica nanoparticle and the polymer beneath were analyzed to determine the composition of the membranes.
Iván Vera Alaya – Final Master Project Results and Discussion 28 The results of these analyses are shown in Table 7. A summary of results obtained from each point marked in the figure in weight %, and an average with standard deviation are shown. Table 7. EDX results of a pristine PCL membrane Spectrum C O Si 1 74.16 25.84 - 2 77.04 22.96 - 3 73.77 26.23 - 4 76.43 23.57 - 5 75.28 24.72 - 6 73.21 26.79 - Mean 74.98 ± 1.53 25.02 ± 1.53 - As seen in Table 7, this membrane contains only carbon and oxygen in a proportion of 75 and 25% respectively. As mentioned above, those results confirm the absence of impurities in the membrane. In Figure 22, images of PCL membrane with MCM-41 are shown. These membranes have a similar PCL pristine membrane homogeneity, with no pores and defects, confirming that the introduction of MCM-41 does not change the homogeneity of the membranes. Additionally as shown in Figure 22a, no aggregation of the silica nanoparticles was observed. Grainy surface, seen in Figure 22b is due to the platinum coating. 1 6 4 2 3 5
Iván Vera Alaya – Final Master Project Results and Discussion 29 Figure 22. SEM images of PCL-MCM41 (a) and magnification of the marked zone (b) Without high magnification it is possible to see the silica particles. Due to the method of preparing the membranes, it is possible that most of these nanoparticles are dispersed in the surface of the membrane. As long as these experiments were performed a large number of particles were measured as shown in Figure 23. After analyzing these measurements can be concluded that the particles used in this project have a rectangular shape with an average dimensions of 150 x 90 nm. Figure 23. Detail of the MCM-41 nanoparticles (a) (b)
Iván Vera Alaya – Final Master Project Results and Discussion 30 As in the case of pristine PCL, these membranes were also analyzed by EDX on the area shown in figure 22a. The results of this analysis are shown in Table 8. Table 8. EDX results of a PCL-MCM41 membrane Spectrum C O Si 1 64.29 32.69 3.02 2 62.69 34.97 2.34 3 63.10 33.43 3.47 4 61.06 35.81 3.13 5 65.71 31.57 2.72 6 61.48 35.68 2.84 Mean 63.06 ± 1.74 34.03 ± 1.73 2.92 ± 0.38 As can be seen, the results in Table 8 confirm the presence of silica. The MCM-41 concentration in the membranes used was 2%, so the fact that the EDX analysis shows a concentration around 3%, suggest that these nanoparticles are slightly concentrated on the surface of the membrane. Finally, a difference in the percentage of oxygen compared to the membrane of pristine PCL (≈ 25%) is observed. This increase in oxygen percentage could be due to oxygen present in the MCM-41 structure. Figure 24 shows images of PCL membranes with MCM-41 functionalized with EPTES. As in the previous case, no defects were observed in the membrane. 1 2 5 3 6 4
Iván Vera Alaya – Final Master Project Results and Discussion 31 Figure 24. SEM images of PCL-MCM41-EPTES (a) and magnification of the marked zone (b) As seen in Figure 24, these particles show similar shape and size compared with the non functionalized MCM-41. However, a greater dispersion in the case of the functionalized particles was observed, probably due to the good interaction between EPTES and polymer. Table 9 shows the results of EDX analysis of the displayed image area at Figure 24a, showing a similar composition than the previous one. Table 9. EDX results of a PCL-MCM41-EPTES membrane Spectrum C O Si 1 66.24 30.95 2.81 2 64.63 32.25 3.12 3 63.05 33.65 3.30 4 65.82 31.34 2.84 5 67.58 29.67 2.75 6 64.37 32.66 2.97 Mean 65.28 ± 1.60 31.75 ± 1.40 2.97 ± 0.21 (a) (b) 1 2 4 6 5 3
Iván Vera Alaya – Final Master Project Results and Discussion 32 4.4. Permeation Characterization O2 and CO2 permeation of composite membranes was measured by the experimental set up described in section 2.6.1. These values were compared with the pristine PCL membrane to determine the change in the permeability due to the presence of filler. Two types of experiments were performed: measurement of permeation of individual gases, and measurement of permeation of an equimolecular mixture. It was necessary to determine the stabilization time of the system in which these gases were completely removed to ensure that the measurements made subsequently were only the chosen gas permeating through the membrane due to the possible contamination of module and pipes with atmospheric gases during the placement of the membranes. Therefore, a pristine PCL membrane was placed and left under a stream of 20 mL/min of O2 as feed and 20 mL/min of He as sweep gas overnight measuring the permeated at intervals of 3 minutes. As can be seen in Figure 25, after 20-30 minutes no significant changes were observed in the permeation values. The same experiment was performed with CO2 and a similar result was obtained (Figure 26). Figure 25. Stabilization time of a PCL membrane with O2 0,00 0,25 0,50 0,75 1,00 13,0 13,1 13,2 13,3 13,4 0 100 200 300 400 500 600 700 Permeability (Barrer) Time (h)
Iván Vera Alaya – Final Master Project Results and Discussion 33 Figure 26. Stabilization time of a PCL membrane with CO2 The individual gas permeation through pristine PCL membrane is shown in Figure 27 compared with the gas mixture at two different pressures. In both cases higher O2 permeation was observed. Figure 27. Permeation comparison between individual gases and mixtures through a PCL membrane 0,00 0,25 0,50 0,75 1,00 13,0 13,1 13,2 13,3 13,4 30 40 50 60 70 80 90 Permeability (Barrer) Time (h) 0 100 200 300 400 500 CO2 Permeability (Barrer) CO2 O2 O2 0 Bar 0.5 Bar Individual Gases Gas Mixture O2 0 Bar 0.5 Bar AP 0 Bar AP 0.5 Bar P 0 Bar P 0.5 Bar Δ Δ
Iván Vera Alaya – Final Master Project Results and Discussion 34 The permeation of gases through polymeric membranes usually occurs by two mean contributions: a dissolution phenomenon and a diffusion process across the membrane (solution-diffusion model). As a semi-crystalline polymer, polycaprolactone consists of an impermeable crystalline part, which will create a tortuous pathway through the membrane, and a permeable amorphous part where the solution and gas diffusion will occur. Furthermore, at 20 °C (temperature at which the experiments were carried out), the amorphous part of the polymer is in the rubbery state, in which the polymer chains have flexibility and mobility to allow the gas molecules diffuse through them [16]. PCL shows high solubility for CO2 due to two types of interactions: polar interactions between this gas and the ester groups of the polymer [17] and specific interactions (Lewis acid-base interactions) between CO2 and oxygen of the carbonyl groups [39]. These interactions increase considerably the solution phenomenon, however diffusion is reduced. By contrast the O2 barely interacts with the membrane, and its smaller kinetic diameter [30] favors diffusion through it. The higher permeation of oxygen would indicate that the solubility mechanism is not dominant in the transport of gases [9]. Considering the permeation gas mixture, two differences were observed compared to individual gases: oxygen permeation is higher, and the CO2 permeation is lower. These differences are due to the plasticizing effect of CO2 [40-42]. Because of this effect, the CO2 is capable of swelling the membrane, creating spaces between the polymer chains and thereby increasing the diffusion of O2, and therefore the permeation. The decrease in the permeation of CO2 may be due to the increase of the oxygen diffusion through the membrane. This gas could be capable of oxidizing groups in the polymer chains, promoting the interaction of CO2 and thereby decreasing its permeation. Finally, in all cases, increasing pressure an increase in permeation was observed. According Naito et al. [43] pressure in these polymers has two effects: one is due to the hydrostatic pressure that compresses the matrix, decreasing the movement of polymer chains and therefore the gas diffusion. The other effect is due to the dissolution of gas in the polymer. Considering that the amorphous zones of the polymer behaves like a liquid, the increment in pressure causes an increase in the dissolution of gas, which has
Iván Vera Alaya – Final Master Project Results and Discussion 35 the effect of swelling the matrix (plasticizing) and thereby increases the permeation. By using low pressures (ΔP = 0.5 bar) the effect of the dissolution is dominant in these membranes considering the effect of hydrostatic pressure practically negligible. The effect of dissolution depends on the size of the molecule, for this reason, when the pressure increases, in both cases the oxygen permeation is higher. In Figure 28 the individual gas permeation of pristine PCL and PCL composite membranes is shown. Figure 28. Permeation of membranes with individual gases Comparing pristine PCL with PCL filled with MCM-41 a decrease in permeation is observed for both gases due to a set of phenomena. On the one hand, according to Sadeghi et al. [9], in a semi crystalline polymer the silica is preferably to be placed into the amorphous zones. This breaks the packaging of the chains decreasing its flexibility and mobility, while increasing tortuosity, resulting in a decrease in the gas diffusion and thus a decreasing in the permeation. On the other hand, due to in situ polymerization and taking into account that the cross sectional areas of polymeric chain are about 1 nm2 or less, the polymer is able to penetrate into the pores of the silica during polymerization and increase the matrix-filler contact [7]. In the interior of the MCM-41 gas transport occurs through Knudsen 0 50 100 150 200 250 Permeability (Barrer) PCL PCL-MCM41 PCL-MCM41-ETES CO2 CO2 CO2 O2 O2 0 Bar 0.5 Bar O2 0 Bar 0.5 Bar P 0 Bar P 0.5 Bar Δ Δ
Iván Vera Alaya – Final Master Project References 42 [22] Lee, E. J., et al. (2010). Nanostructured poly(ε-caprolactone)-silica xerogel fibrous membrane for guide bone regeneration. Acta Biomaterialia, 6, 3557-3565. [23] Azeredo, H. (2009). Nanocomposites for food packaging applications. Food Research International, 42, 1240-1253. [24] Tang, X. Z., et al. (2013). Recent advances in biopolymers and biopolymer-based nanocomposites for food packaging materials. Critical Review in Food Science and Nutrition, 52, 426-442. [25] Wan, Y., et al. (2009). Thermophysical properties of polycaprolactone/chitosan blend membranes. Thermochimica Acta, 487, 33-38. [26] Zeng, W., et al. (2005). Organic modified mesoporous MCM-41 through solvothermal process as drug delivery system. Materials Research Bulletin, 40, 766-772. [27] López, L. Desarrollo de nanocomposites basados en poly(ε-caprolactona) (Doctoral Thesis pending publication). Universidad de Zaragoza, España. [28] Tang, Z.G., et al. (2004). Surface properties and biocompatibility of solvent-cast poly[ɛ-caprolactone] films. Biomaterials, 25, 4741-4748. [29] Stern, S.A. (1968). The “barrer” permeability unit. Journal of Polymer Science Part A-2: Polymer Physics, 6, 1933-1934. [30] Yampolskii, Y., Pinnau, I., & Freeman, B. (2006). Transport of gases and vapors in glassy and rubbery polymers. In Material science of membranes for gas and vapor separation (pp. 1-47). Oxford, UK: Wiley. [31] Liang, J.-Z. (2013). Reinforcement and quantitative description of inorganic particulate-filled polymer composites. Composites: Part B, 51, 224-232. [32] Lucy, B., et al. (2007). Síntesis y caracterización de nanohíbridos poliestireno/sílica mesoporosa MCM-41. Scientia et Technica Año XIII, 36, 971-976. [33] Elzein, T., et al. (2004). FTIR study of polycaprolactone chain organization at interfaces. Journal of Colloid and Interface Science, 273, 381–387.
Iván Vera Alaya – Final Master Project References 43 [34] Zholobenko, V.L., et al. (1997). Synthesis of MCM-41 materials: an in situ FTIR study. Microporous Materials, 11, 83-86. [35] Franco, R.L.M., et al. (2013). Textural properties of nickel, palladium and titanium oxides supported on MCM-41 materials and their application on oxidative desulfurization of dibenzothiophene. Materials Research, 16, 1448-1456. [36] Grieken, R.V., et al. (2010). Sulfonated polystyrene-modified mesoporous silica for acid catalyzed processes. Chemical Engineering Journal, 161, 388-396. [37] Li, S.Y., et al. (2013). 3-aminopropyltriethoxysilanes modified porous silicon as a voltammetric sensor for determination of silver ion. International Journal of Electrochemical Science, 8, 1802-1812. [38] Bacsik, Z., et al. (2011). Mechanisms and kinetics for sorption of CO2 on bicontinuous mesoporous silica modified with n-propylamine. Langmuir, 27, 11118-11128. [39] Kazarian, S. G., et al. (1996). Specific intermolecular interaction of carbon dioxide with polymers. Journal of the American Chemical Society, 118, 1729-1736. [40] Horn, N. R., et al. (2011). Carbon dioxide plasticization and conditioning effects in thick vs. thin glassy polymer films. Polymer, 52, 1619-1627. [41] Minelli, M., et al. (2013). Permeability and solubility of carbon dioxide in different glassy polymer system with and without plasticization. Journal of Membrane Science, 444, 429-439. [42] Neyertz, S., et al. (2014). The effect of structural isomerism on carbon dioxide sorption and plasticization at the interface of a glassy polymer membrane. Journal of Membrane Science, 460, 213-228. [43] Naito, Y., et al. (1991). The effect of the pressure on gas permeation through semicrystalline polymers above the glass transition temperature. Journal of Polymer Science: Part B: Polymer Physics, 29, 457-462.