Full text
2012 63 Adriana Isabel Figueroa García Magnetic nanoparticles studied by synchrotron radiation and rf transverse susceptibility Departamento Director/es Física de la Materia Condensada Bartolomé Sanjoaquín, Juan García Vinuesa, Luis Miguel Director/es Tesis Doctoral Autor Repositorio de la Universidad de Zaragoza – Zaguan http://zaguan.unizar.es UNIVERSIDAD DE ZARAGOZA
Departamento Director/es Adriana Isabel Figueroa García MAGNETIC NANOPARTICLES STUDIED BY SYNCHROTRON RADIATION AND RF TRANSVERSE SUSCEPTIBILITY Director/es Física de la Materia Condensada Bartolomé Sanjoaquín, Juan García Vinuesa, Luis Miguel Tesis Doctoral Autor 2012 Repositorio de la Universidad de Zaragoza – Zaguan http://zaguan.unizar.es UNIVERSIDAD DE ZARAGOZA
Departamento Director/es Director/es Tesis Doctoral Autor Repositorio de la Universidad de Zaragoza – Zaguan http://zaguan.unizar.es UNIVERSIDAD DE ZARAGOZA
Magnetic nanoparticles studied by synchrotron radiation and rf transverse susceptibility
Magnetic nanoparticles studied by synchrotron radiation and rf transverse susceptibility Adriana Isabel Figueroa Garc´ıa
To my dearest family, in loving memory of my dad...
Introduction 3 media; this may occur since thermal fluctuations can lead to destabilization of the magnetic state of the particles. On the contrary, biomedical applications need magnetic particles with low anisotropy, for their magnetization to be easily reversed inside biological systems. Therefore, research in magnetic nanoparticles involves several aspects to consider, from the preparation procedures to the comprehension, control and optimization of the desired properties. For instance, the possibilities of tuning the magnetic anisotropy of the particles in order to fulfill the requirements for each application seem to be of paramount importance. Different experimental approaches for a complete structural and magnetic characterization of the NPs are fundamental to attain this purpose. Following this scheme, in this dissertation we describe different studies performed on various magnetic nanoparticles systems where a proper combination of structural, electronic, and magnetic characterization methods lead to a better understanding of the NPs properties, in particular, of their magnetic anisotropy. In the first part, we make use of some synchrotron radiation techniques. The unique properties of this radiation such as broad energy spectrum, variable light polarization, and flexible time structure, have made it an enormously powerful tool in the study of magnetic phenomena and structure of materials. Extensive characterization of magnetic particles has been carried out over the last decades with synchrotron based spectroscopic techniques demonstrating their possibilities. We focus here on some X-ray absorption techniques: X- ray Absorption near edge structure (XANES), extended X-ray absorption fine structure (EXAFS) and X-ray magnetic Circular Dichroism (XMCD). These techniques constitute very useful methods to directly and selectively examine the electronic state and local structure of the atoms composing the particles, which are fundamental as resulting from the surface effects in reduced size materials. Moreover, the average coordination number, which is also a key parameter that controls the evolution of the magnetic behavior in materials, may be directly determined by EXAFS. On top of that, XMCD arises as an effective method to selectively study the magnetic properties of the particles [2, 10–15], giving access to both contributions to the total magnetic moment, the atomic orbital moment mL(currents associated with the electronic motion) and spin moment mS(intrinsic angular momentum of the electrons). The possibility of separating both contributions is especially useful in itinerant magnetic materials, which have an orbital magnetic moment induced by spin–orbit coupling. The general trend in mLis the same one as for the spin moment: the orbital moment increases with decreasing coordination [2]. However, the orbital moment does not linearly follow the spin moment, the ratio mL/mSvaries with atomic structure, dimensionality and coordination
4Introduction number. mLin NPs is very sensitive to neighboring atoms, increasing rapidly with a decrease in the coordination number, with only the two outer shells of NPs showing values being significantly different from bulk values. This enhancement of mLand its anisotropy at the NPs surface has been demonstrated to contribute significatively to the total magnetocrystalline anisotropy, as proposed by Bruno [16], following the expression ∆ESO ∝ −ξ(m⊥ L−mk L)∝ −KS with ξthe spin-orbit coupling of the atoms forming the particle surface, mk Land m⊥ Lthe in-plane and out-of-plane components of the orbital moment, respectively, and KSthe surface anisotropy constant. Therefore, the spinorbit coupling in systems of nanometric dimensions has been found to be highly relevant. In this sense, this dissertation continues previous studies of spin-orbit enhanced anisotropy observed in different cobalt NPs systems. They consist of self-organized lattices of nanometer-sized Co magnetic clusters (1-4 nm) prepared by sequential deposition of Al2O3and Co layers on a Si substrate. In these granular systems, it is possible to control the clusters size [17], the average number of neighbors to a given cluster [18], and even the surface anisotropy by capping the cobalt nanoparticles with noble metals like Cu, Ag, Au [19]. Those studies allowed quantitative determination of parameters like magnetic anisotropy [20, 21] or dipolar interactions [18]. In the case of Cometal(M) particles, with M=Cu, Ag, Au, the capping metal does not diffuse on Co, so the Co particle retains its integrity as a nearly spherical crystalline particle. A systematic increase in the surface anisotropy of Co-M NPs with capping in the trend Cu, Ag, and Au was then observed, as resulting from the previously described orbital moment anisotropy, caused by hybridization of Co atoms at the particle surface with the capping metal [11]. Beside those surface effects, the magnetic anisotropy of NPs systems may be intrinsic, such as that identified in chemically ordered CoPt alloy NPs [22]. The anisotropy of those particles is also correlated with the Co orbital anisotropy, which by hybridization with Pt, and due to the high spin-orbit coupling of the latter, gives rise to an enhanced anisotropy, albeit much smaller than in the bulk CoPt L10alloy phase [23, 24]. Therefore, in the Co-M NPs systems that we describe in this thesis, we explore the introduction of high spin-orbit non-magnetic elements and induce their alloying with Co, as a strategy to control their intrinsic anisotropy and magnetic properties. In particular, we study Co NPs capped with Tungsten (W) and Platinum (Pt). On the one hand, W (electron configuration [Xe]4f145d46s2) is a good candidate as it hybridizes with Co (electron configuration [Ar]3d74s2), its affinity to alloy with Co on sputtering grown films at room temperature is known
Introduction 5 [25], these alloys tend to become amorphous [26–29], and it has a less than half filled 5dband. This way, we end up with a system of amorphous NPs, which constitute a different type with variable anisotropy. Then, the work on Co-W NPs we describe in this dissertation is devoted to investigate the open question whether amorphous alloys may support intrinsic anisotropy, induced by alloying, irrespective of surface effects. On the other hand, for the Pt case, aside from the previously described hybridization between Pt (electron configuration [Xe]4f145d96s1) and Co, and the high spin-orbit coupling of Pt that gives rise to an enhanced anisotropy, Co-Pt NPs show perpendicular magnetic anisotropy (PMA) [30, 31], which is interesting for applications in spintronic nano-devices implemented to, for example, ultrahigh density magnetic storage, fast memory applications, and nanosensors [32, 33]. Apart from the importance of the orbital moment in nanomaterials, the spin moment still dominates their magnetism, as in the case of transition metals. Reducing the dimension leads to a narrowing of the valence dbands that generate most of the magnetic moment. The increase in the density of states at the Fermi level Efalso opens the chance to detect magnetic phenomena in materials which are non-magnetic in bulk, for example, in the noble metals of Co-M NPs described above [11], Pt NPs [34] and Au NPs [35], to cite some examples of metallic particles where such phenomena have been observed. Accordingly, in this dissertation we present a review of some of these examples as an attempt towards the comprehension of the d-band magnetism in nanostructured metals via the element-selective XMCD technique. In addition to synchrotron radiation techniques, the anisotropy may be studied by magnetometry performed in conventional laboratories. One of the rarely used, but effective methods to directly study the magnetic anisotropy of a material is the transverse susceptibility (TS) technique. This measurement system consists in probing the ac magnetic susceptibility of a material in one direction while an external bias magnetic field is applied perpendicular to the measurement direction. Analysis of the TS in magnetic materials have demonstrated its potential and versatility to study singular magnetic properties of bulk [36–38], single crystals [39], thin films [40–43] and nanoparticles (NPs) systems [44–48]. TS measurement techniques developed up to date are based on conventional inductance susceptibility techniques [46, 49, 50], magnetooptical setups [40, 43] and self-resonant circuits in the radio frequency (rf) range [51]. The latter method has demonstrated to be one of the most accurate and versatile developments to measure TS, since it may be implemented on widely used commercial Quantum Design physical properties measurement systems (PPMS). It consists of a self-resonant LC tank coupled to a tunnel
6Introduction diode oscillator (TDO), the latter acting as an active device for losses compensation in the circuit. The magnetic sample is inserted into the inductor (L) core space and its TS is probed by the shift in the resonant rf generated by changes in the sample magnetization. However, currently operating TS measurement systems for the PPMS are far from being simple and friendly to use. Changing sample usually involves soldering and desoldering the inductance coil, jeopardizing the reproducibility of the system. Moreover, previously published designs of TS susceptometers for PPMS systems [51] introduce a high heat input into the sample space, avoiding the PPMS platform to stabilize the sample temperature below 10 K, and, therefore, impeding the possibility of studying interesting lowtemperature phenomena with this technique. On the electronics design, it has been conventionally adopted the use of TDOs, which benefits of a good spectral purity, but limiting the compensation capabilities of the system and hence the range of samples feasible to measure. And finally, the necessity to install extra electronic and computing equipment to acquire data, independent to the control of the PPMS, makes the programming of experiments harder, rendering the previous systems not very efficient. Then, in the second part of this thesis, we present an implementation of a TS measurement system for the PPMS of the Servicio de Medidas F´ısicas in the Universidad de Zaragoza. We have improved several aspects of the design, electronics, and data acquisition of previously published transversal susceptometers [51], turning this magnetometric technique a relatively easy one to implement and operate within the widely used PPMS platform. We also describe the use of the developed setup to explore the magnetic anisotropy of two systems of iron oxide nanoparticles, interesting for biomedical applications. Motivation and outline This dissertation is aimed to undertake an elaborate study of different magnetic nanoparticles systems, with which we intend to demonstrate the capabilities of two experimental techniques: the X-ray absorption spectroscopies (XANES, EXAFS and XMCD) and the rf transverse susceptibility. By using these techniques for electronic, structural and magnetic characterization of nanoparticles systems, along with other complementary methods, we obtain a better understanding of the origin of their magnetic anisotropy. The manuscript is organized as follows. In Chapter 1 we describe the main experimental techniques used in the present work to study the structural and magnetic properties of NP systems. In particular, we focus on the
Introduction 7 X-ray absorption spectroscopies that make use of synchrotron radiation. In the following three chapters we describe the structural, magnetic and electronic properties of two nanoparticles systems, namely: Co-W NPs and Co-Pt NPs, studied with synchrotron radiation techniques. Hence, in Chapter 2 we describe the main properties of the amorphous Co-W alloy NPs. We demonstrate that the magnetic anisotropy of amorphous alloy nanoparticles may be originated in mechanisms other than surface effects, such as structural short range order. A continuation of this study is presented in Chapter 3, where we describe evidences of violation of Hund’s third rule in the W induced magnetic moments of this Co-W system, as consequence of hybridization effects and local structure in the Co-W alloys. Similarly, in Chapter 4 we describe the properties of the Co-Pt NPs studied, where the presence of Co-Pt alloy in these granular films is determinant in the origin of their perpendicular magnetic anisotropy. Then, a review of noble metals (Ag, Au, Pd, Pt) nanoparticles studied with synchrotron radiation is presented in Chapter 5, where we demonstrate that these techniques are very suitable to study their d-band magnetism. The last two chapters of this thesis are dedicated to the rf transverse susceptibility (TS) technique. Chapter 6 is devoted to the description of the TS technique and the developed equipment for the PPMS. Then in Chapter 7 we present a couple of examples of magnetic NPs studied with this TS measurement system, namely magnetite and maghemite NPs. Finally, we give some general conclusions and perspectives of this work at the end of this manuscript.
Chapter 1 Experimental techniques This section is addressed to briefly describe the main experimental techniques used to study the structural and magnetic properties of the nanoparticles included in this thesis. We first explain the transmission electron microscopy techniques used to explore the morphology and structure of the particles. Then, we introduce two techniques to study the magnetic properties of the samples: SQUID based magnetometry and anomalous hall effect (AHE). Finally, we focus on the description of the synchrotron radiation techniques employed, in particular those based on X-ray absorption mechanisms, which allow studying selectively and locally the structural, electronic and magnetic properties of the nanoparticles systems; these are: X-ray absorption near edge structure (XANES), extended X-ray absorption fine structure (EXAFS), and X-ray magnetic circular dichroism (XMCD). Later, we will dedicate chapter 6 to describe the magnetic transverse susceptibility technique, which has been also used to study the magnetic properties of some nanoparticles systems in this dissertation. 1.1 Transmission Electron microscopy The transmission electron microscopy (TEM) is a technique whereby an electron beam is transmitted through an ultra thin specimen, forming an image from the interaction between the transmitted electrons and the sample. TEMs are capable of imaging at a significantly higher resolution than light microscopes, owing to the small wavelength of electrons. This enables to examine fine details, even as small as a single column of atoms. This technique usually combines the high resolution imaging with elemental microanalysis and electron diffraction, so that a complete characterization of the shape, size,
10 Chapter 1. Experimental techniques chemical composition and crystalline structure of nanoparticulate materials is achieved. In a TEM microscope, an electron gun, located at the top of it, emits the electrons by thermionic or field emission. These electrons travel through vacuum in the column of the microscope where electromagnetic lenses focus them into a very thin beam. The electron beam then travels through the specimen to study. At the bottom of the microscope, the image is formed on the image plane of objective lens from the unscattered electrons. Then, projector lenses form the images on a screen or CCD camera. One of the main requirements for this technique is that the sample must be thin enough for electrons to pass through; the interaction between electrons and matter is much stronger than that with visible light, so samples for TEM observation must have thickness below 100 nm. There exists a variety of procedures to prepare samples for TEM observation, depending on the kind of materials and their nature. For example, bulk samples must be first cut to an proper size (∼3 mm in diameter, 300-400 µm thick); after that, they are thinned, first mechanically and then by ionic or electrolytic milling, until reaching the desired thickness. Some modern TEMs integrate a high angle annular dark field (HAADF) detector that allows to perform scanning transmission electron microscopy (STEM) measurements. In this mode, the electron beam is focused into a narrow spot that is scanned over the sample in a raster. The rastering of the beam across the sample makes these microscopes suitable for analysis techniques such as mapping by X-ray energy disperse spectrometry (EDX) spectroscopy and electron energy loss spectroscopy (EELS). The HAADF detector collects electrons from an annulus around the beam, forming the image only by very high angle incoherently scattered electrons, as opposed to Bragg scattered electrons in the conventional TEM images. By using a STEM and the HAADF detector, it is possible to form atomic resolution images where the contrast is directly related to the atomic number (Z-contrast image). The microscopy images and analysis of the magnetic nanoparticles in this work were performed with two TEMs, whose technical specifications are described below. 1.1.1 JEOL JEM 3000 F A JEOL JEM 3000 F Field Emission Microscope has been used by Dr. Luisa Ruiz Gonz´alez and Dr. Jos´e Mar´ıa Gonz´alez-Calbet of the Departamento
1.1. Transmission Electron microscopy 11 (b) (a) Figure 1.1: Images of the two models of transmission electron microscopes used to observe the samples. (a) JEOL JEM 3000 F Field Emission Microscope. (b) FEI TecnaiTM G2 F30 STWIN Field Emission Microscope. de Qu´ımica Inorg´anica in the Universidad Complutense de Madrid1to take some of the images of the nanoparticles systems that we show in this thesis. This microscope is shown in Fig. 1.1(a). It operates at acceleration voltages between 100 and 300 kV and it is fitted with an Oxford Instruments energy dispersive X-ray spectrometer (EDS). Its high-resolution performance (a point resolution of 0.17 nm) is then complemented by the ability to perform chemical microanalysis from sub-nanometre areas (below 0.4 nm in some cases). This microscope is equipped with a HAADF detector, so that STEM mode and EELS analysis are also possible. 1.1.2 FEI TecnaiTM G2 F30 STWIN Some of the TEM images that we show in this dissertation have taken by Dr. Cesar Mag´en and Dr. Alfonso Ibarra in a FEI TecnaiTM G2 F30 STWIN Field Emission Microscope of the Laboratorio de Microscop´ıas avanzadas, Instituto 1http://www.cnme.es/
12 Chapter 1. Experimental techniques de Nanociencia de Arag´on2, Universidad de Zaragoza. A picture of a microscope of this kind is shown in Fig. 1.1(b). In this microscope, acceleration voltages as high as 300 kV allow reaching a point resolution of 0.2 nm, line resolution of 0.10 nm, and information limit of 0.14 nm. This TEM system is fully loaded including a HAADF detector, EDX, and a Gatan Image Filter (GIF). 1.2 SQUID based magnetometry A magnetometer is an instrument used for the magnetic characterization of a material, by measuring the strength and/or direction of magnetic fields. A superconducting quantum interference device (SQUID) is the most sensitive device available for such purposes. It works as an extremely sensitive current- to-voltage convertor, so that, when integrated to a Quantum Design magnetic property measurement system (MPMS), the complete system is a magnetic flux to voltage transducer. The fact of directly measuring magnetic flux is one of the main advantages of SQUID magnetometry, allowing to measure moments on the order of 10−7emu. A picture of one of the MPMS of the Servicio de Medidas F´ısicas of the Universidad de Zaragoza,3which have been used for some of the magnetic characterization described in this manuscript, is shown in Fig. 1.2(a). A schematics of the measurement process of a magnetic sample in this equipment is displayed in Fig. 1.2(b). In a MPMS, the SQUID does not detect directly the magnetic field from the sample since it may be interfered by any flux from nearby magnetic systems, or even the earth’s magnetic field. Instead, a measurement is performed by moving a sample through a system of superconducting pick-up coils, two of them with the same sense very closely spaced, and the other two of the opposite sense, spaced symmetrically outside (see Fig. 1.2(b)). This system is located outside the sample chamber at the center of the superconducting magnet. As the sample moves through the coils, the magnetic moment of the sample induces an electric current in the detection coils. Because the detection coils, the connecting wires, and the SQUID input coil form a closed superconducting loop, any change of magnetic flux in the detection coils produces a change in the persistent current in the detection circuit, which is proportional to the change in magnetic flux. Since the SQUID is a highly linear current-to-voltage convertor, the variation in the current in the detection coils produces corresponding variations in the SQUID output voltage. Based on this profile of voltage (and thus flux) versus position 2http://ina.unizar.es/lma/index.html 3http://sai.unizar.es/medidas/index.html
1.4. X-ray absorption spectroscopies in synchrotron radiation facilities 19 single scattering process of the photoelectron scattered by surrounding atoms (see Fig. 1.5(a)), and it provides information on the local structure such as distances between neighbors, thermal and structural disorder in a material. Information on the geometry of the local structure is provided by the analysis of the multiple scattering peaks in the XANES spectra. However, XANES is harder to be described in a quantitative way since there is not an equation to parameterize this region, while it does exist for EXAFS, as it will be described below. The X-ray absorption process is a transition between two quantum states: from an initial state with an X-ray, a core-electron, and no photoelectron, to a final state with no X-ray, a core-hole, and a photoelectron. According to the Fermi’s golden rule for dipolar transitions (following the dipole selection rules ∆l=±1 and ∆s= 0), the transition probability between two electronic states, per unit time, is defined as Wif =2π ~eE0 22 |hi|ˆε·~r |fi|2ρ(Ef) (1.2) where ρ(Ef) is the density of final states, hi|is the initial state of the coreelectron, |fithe final state of the photoelectron, and ˆε·~r the dipole operator. Since the core-level electron is very tightly bound to the absorbing atom, the initial state will not be altered by the presence of the neighboring atom. The final state, on the other hand, will be affected by the neighboring atom because the photoelectron will be able to see it. The absorption coefficient µ(E) is proportional to the sum of possible final states fof the transition probability in equation 1.2. It is calculated according to the first order approximation of the time-dependent perturbation theory, based on the interaction between the electromagnetic field and the atom potential. In the EXAFS region, the spectrum reflects oscillatory variation of the X–ray absorption coefficient, µ(E), as a function of photon energy, E, beyond the absorption edge (see Fig. 1.6). We define the EXAFS fine–structure function χ(E) as χ(E) = µ(E)−µ0(E) ∆µ0(E)(1.3) where µ(E) is the measured absorption coefficient, µ0(E) is a smooth background function representing the absorption of an isolated atom, and ∆µ0(E) is the measured jump in the absorption µ(E) at the threshold energy E0. These parameters are also represented in Fig. 1.6. According to the described absorption process, the EXAFS χ(E) is propor-
20 Chapter 1. Experimental techniques tional to the amplitude of the scattered photoelectron at the absorbing atom. Therefore, EXAFS is best understood in terms of the wave–like nature of the photoelectron created in this process. Thus, it is common to convert the X–ray energy to k, the wave number of the photoelectron, being k2= 2m(E−E0)/~2, and mthe electron mass. The primary quantity for EXAFS is then χ(k), the oscillations as a function of photoelectron wave number. To emphasize the oscillations, χ(k) is often weighted by a power of k, typically k2 or k3. The different frequencies composing these oscillations correspond to different near–neighbor coordination shells, described and modeled according to the EXAFS equation χ(k) = X j NjS2 0Fj(k) exp(−2k2σ2 j) exp −2R2 j λj(k) kR2 j sin(2kRj+δj(k)) (1.4) where Fj(k) is the backscattering amplitude from each of the Njneighboring atoms, δj(k) is the total phase shift experienced by the photoelectron, Rjis the distance to the neighboring atom j,σ2 jis the disorder in the neighbor distance, parameter usually known as Debye–Waller factor, and S2 0is the amplitude reduction due to many–body effects. The term exp(−2R2 j/λj(k)) is due to inelastic losses in the scattering process, with λjbeing the electron mean free path. The EXAFS equation allows us to determine N,R, and σ2 knowing the scattering amplitude F(k) and phase–shift δ(k) for each path. Furthermore, since these scattering factors depend on the atomic number, Z, of the neighboring atom, EXAFS is also sensitive to the atomic species of the neighborhood. The EXAFS χ(k) is usually Fourier transformed into a radial structure function χ(R) that represents the data in terms of distances from the absorber. Peak positions in this radial structure function roughly correspond to the radii of the scattering shells. BM29 beamline at the ESRF The XAFS experiments on the magnetic nanoparticles system studied here were performed in collaboration with Dr. Sakura Pascarelli at the general purpose X-ray absorption spectroscopy beamline BM29 [61] at the ESRF.7 This beamline is devoted to carry out XAFS experiments at a very large 7In a recent upgrade, performed in 2011, the ESRF BM29 beamline has been relocated to the BM23 port, which is the one currently operational. For further information see http://www.esrf.eu/UsersAndScience/Experiments/ElectStructMagn/BM23/
1.4. X-ray absorption spectroscopies in synchrotron radiation facilities 21 operational energy range with reasonable X-ray flux: 4 keV to 74 keV, coming from a bending magnet. It has a high energy resolution, typically a factor 3 to 5 better than the intrinsic spectral broadening at any Kor Labsorption edge; a high spectral signal to noise ratio, above 7.0×104for well prepared samples; a high beam stability; and a high level of automation. A schematic diagram of a conventional XAFS beamline, as BM29, is shown in Fig. 1.7. The full spectrum of synchrotron light passes through an entrance slit, which helps collimate the radiation before entering a into a double–crystal monochromator. The X–rays diffract off the crystals’ lattice planes, which are aligned at an angle θwith respect to the incoming beam. Because of the Bragg scattering condition nλj= 2dsin θ, only X–rays of energy En=nhc/λjcan reflect off the crystals. Different X–ray energies can be selected by changing the angle θof the crystals. The monochromatic beam passes through an ion chamber that monitors the beam intensity I0by absorbing part of it. The beam then passes through the sample, and the intensity of the transmitted X–ray Iis measured by a second ion chamber. Taking the log of the ratio of I/I0yields the absorption. We can also determine the sample’s absorption by measuring the intensity of its X–ray fluorescence, Ifwith a detector that is out of the beam path, usually oriented at 45owith respect to the sample. Finally, the beam passes through a reference sample whose absorption edge is used to help correct for uncertainties in the beam’s energy. 1.4.2 X-ray magnetic circular dichroism Some synchrotron radiation techniques take advantage of the natural polarization of this light in the plane of the electron orbit in order to perform polarization-dependent measurements. This is the case of the X-ray magnetic circular dichroism (XMCD), where the difference between two X-ray absorption spectra recorded in a magnetic field, one measured with right circularly polarized light (+1 helicity), and one with left circularly polarized light (-1 helicity), is performed. The XMCD is then defined as XMCD(E) = µ−−µ+(1.5) where µ−and µ+are the absorption coefficients with left and right circularly polarized light, respectively. The differences in the absorption of light with opposite helicities arise from an additional dipole selection rule for dipolar transitions, ∆mj=±1 for +1 and -1 helicity, respectively, in equation 1.2; the dipole operator, ˆε·~r, must also be expressed as dependent of the light polarization. This way, XMCD reflects the difference in the density of empty states with different spin moment, so that by closely analyzing
22 Chapter 1. Experimental techniques Synchrotron storage ring Entrance slit Bending magnet Double crystal monocromator Slits Incident intensity monitor, I0 Fluorescence detector Sample Reference Sample Energy calibration detector Transmitted intensity detector, I Beam stop Si crystal Si crystal θ Experimental hutch Light beam Figure 1.7: Diagram of the assembly used in a conventional measurement of XAFS.
1.4. X-ray absorption spectroscopies in synchrotron radiation facilities 23 the XMCD signal, information can be obtained on the magnetic properties of the absorbing atom, such as its spin and orbital magnetic moment. In a simple atomic monoelectronic picture, the XMCD occurrence may be understood in terms of the two-step approach described by Sch¨ utz et al. [62]. Let us first consider an X-ray photon with helicity +1 absorbed by an electron from a spin–orbit-split core-level, for example, 2p3/2(L3edge) and 2p1/2(L2 edge), as illustrated in Fig. 1.8(a). When absorbing a circularly polarized photon, some of the orbital moment of the photon can be transferred via the spin-orbit coupling to the electron spin. This results in an effective spin polarization of the exited electrons, process known as Fano-effect [63]. From 770 780 790 800 810 -4 -2 0 0 2 4 6 8 XMCD Photon energy (eV) µ -- µ + XAS µ + µ - ( µ ++ µ -)/2 µ µ 2p3/2 2p1/2 H Core level EF M≠0 Energy (b) (a) L3 L3 L2 L2 L2 L3 L2 L3 A B Figure 1.8: (a) Diagram of the simple monoelectronic two-step picture of the resonant excitation process in a magnetic material, resulting in a XMCD signal. First a circularly polarized photon excites a spin polarized electron (Fano-effect) from a 2plevel; this spin polarized electron is used in step two to probe the spin polarized occupation levels of the 3dstates. (b) XAS spectra and XMCD signal at the Co L2,3in a system of Co-Pt NPs. In this case, a scan over the 2pabsorption edges of Co with circularly polarized light leads to non statistic absorption lines due to differently spin occupied 3dstates. This effect is reversed by inverting either the magnetization (change of the magnetic field direction) or the light polarization. In this picture the polarization of the light is reversed between the orange and green absorption curves. The difference of left and right circularly polarized scan is the dichroic signal displayed below.
24 Chapter 1. Experimental techniques the 2p3/2state, 62.5% of excited electrons carry a spin of ms= +1/2 and only 37.5% of ms=−1/2. From the 2p1/2state, 75% of excited electrons carry a spin of ms=−1/2 and only 25% of ms= +1/2. Note that the sign of spin polarization is different for the different 2pstates, provided their different spin-orbit coupling: (l+s) at the p3/2-state, and (l−s) at the p1/2-state. If there were no spin–orbit-splitting, that is, no energy gap between 2p3/2and 2p1/2states, the averaged spin polarization would be zero. With this spin and orbital polarized excited electrons, the polarization of the unoccupied final states is probed in the second step of this model. Any imbalance in either spin or orbital momentum in the final states will give rise to a dichroic effect. Thus, in a magnetic material, the exchange splitting leads to a splitting of the valence band, lowering the energy for electrons with one spin orientation (majority electrons) and rising it for the other (minority electrons), as illustrated in Fig. 1.8(a). The transition probability of electrons in a dipole transition are proportional to the unoccupied density of states, as expressed in equation 1.2. If this density of states is different for different spin orientations and the electrons are spin polarized, the absorption spectra will change when the spin polarization is inverted, as due to the change of the helicity of the incoming light. This results in spectra as the one represented in Fig. 1.8(b), where we have plotted the XAS recorded with right and left circularly polarized X-rays at the Co L2,3edges in a Co-Pt NPs sample, along with the resulting XMCD signal. To see this effect it is required that the magnetization of the sample has at least a component parallel to the incoming light. The inversion of the magnetization has the same effect on the absorption process as the inversion of the photon polarization. Thus, XMCD measurements can be performed in those two equivalent ways: either by changing the helicity while keeping constant the applied magnetic field, or by changing the direction of the magnetic field at a constant helicity of the light. XMCD became more powerful as a tool for the element-selective characterization of magnetic materials with the derivation of the magneto-optical sum rules by Thole et al. [64] and Carra et al. [65] for spin–orbit split absorption edges. Via these sum rules it is possible to determine both the spin, mS=−2µBhSzi/~, and orbital, mL=−µBhLzi/~, magnetic moments in the atom being probed with the XMCD measured at its L2,3edges. In order to write the sum rules, let us define the following integrals
1.4. X-ray absorption spectroscopies in synchrotron radiation facilities 25 A=Z L3 (µ−−µ+)dE B=Z L2 (µ−−µ+)dE (1.6) C=Z L3+L2 (µ−+µ++µ0)dE which follow the symbols and sign criteria denoted in Ref. [66]. The absorption spectrum µ0requires in principle linearly polarized radiation, but is usually approximated by µ0= 1/2(µ++µ−). Before application of the sum rules it is necessary to separate the absorption intensity due to the electron transitions we are interested in. Thus, the Cintegral must be calculated after removing the unwanted transitions into higher unoccupied states or into the continuum in the absorption spectra. It is usually performed by subtraction of a hyperbolic step function with one step at the L3and one at the L2 edge [67]. If there are less pronounced absorption maxima at the absorption edges, a reference spectrum of a similar element with a well-known number of unoccupied states should be subtracted. The sum rule for the orbital moment per unoccupied final state nhis expressed as mL nh =−2(A+B) CµB(1.7) For the spin sum rule, it is usual to define the effective spin moment, mSeff =mS+mD, which considers the dipolar term mD. The latter is expressed as a function of the expectation value of the intra-atomic magnetic dipole operator hTzi[66, 68], as mD=−7hTziµB/~, which reflects the asphericity of the spin moment distribution around the absorbing atom. In order to determine mS, one option is to assume that the angle averaged hTziis much smaller than the spin moment and can be neglected, as in the case where the absorbing atom is in a cubic (undistorted) symmetry. On the contrary, for lower symmetries or distorted systems, hTzimay be obtained from angle dependent experiments or theoretically approximated [68, 69]. For example, for non-cubic structures, hTzimight have a maximum value of hSzi/3, corresponding to the Lorentz local field at the absorbing atom site [70]. However, the angle average of hTziwith this approximation in the whole sample usually cancels out, as well.
26 Chapter 1. Experimental techniques If the angle average of hTziis zero, mSeff =mS, and the spin moment, also per nh, is written as mS nh =−3(A−2B) 2CµB(1.8) Therefore, the orbital to spin moment ratio is defined as mL mS =4(A+B) 3(A−2B)(1.9) which is independent of nhand the Cintegral. For a precise estimation of these moments, one must separate the L3and the L2contribution of the spectrum, which is fairly easy for the heavier 3d, and for 4dand 5delements since the spin-orbit split increases with the nuclear charge of the atom. Additionally, one needs to know the exact amount of d-holes in the material, for which no straight forward experimental determination procedure exists. This drawback may be solved by either obtaining the number of d-holes from band structure calculations, or by expressing the sum rules results as magnetic moments per d-hole. ID08 and ID12 beamlines at the ESRF The XMCD experiments on the magnetic nanoparticles studied here were performed at the ID08 beamline (for soft X-rays ranging between 0.3 and 1.6 keV) in collaboration with Dr. Peter Bencok and Dr. Nick Brookes, and at the ID12 beamline (for hard X-rays ranging between 2 and 20 keV) in collaboration with Dr. Fabrice Wilhelm, Dr. Alevtina Smekhova and Dr. Andrei Rogalev, in the ESRF.8These beamlines are dedicated to polarization-dependent X-ray absorption and excitation spectroscopies. Both beamlines make use of undulators to produce the polarized light for XMCD measurements. By longitudinal phasing of the magnetic arrays, the polarization of the undulator emission can be changed from linear to elliptical and circular. They complement each other to probe magnetism in a diverse range of systems with X-ray magnetooptical techniques and to study the electronic structure of materials X-ray and photoelectron emission techniques. ID08 is equipped with two APPLE II undulators providing ∼100% circular/linear beam polarization, a spherical grating monochromator with an energy resolution close to ∆E/E = 5 ×10−4at 850 eV, optics focussing down 8For further information about ID08 and ID12 beamlines, please visit http://www.esrf. eu/UsersAndScience/Experiments/ElectStructMagn
1.4. X-ray absorption spectroscopies in synchrotron radiation facilities 27 Fluorescence detector Magnet Sample Circularly polarized X-rays Undulator Total electron yield detection θ H Figure 1.9: Basic diagram of the XMCD measurement setup at ID08 and ID12. to 6-40 [60-500] microns (FWHM) vertical [horizontal] beam size, and several different UHV experimental stations and sample preparation facilities. ID12 has three helical undulators installed on the its straight section: HELIOSII, APPLE-II and the so-called “ElectroMagnet/Permanent magnet Hybrid Undulator” (EMPHU) that have been optimized to complement one another. They give ID12 the advantages of fully control of the polarization state of the incident X-ray beam over a wide energy range. ID12 uses a double-crystal monochromator with a resolution of ∆E/E =∼10−4to select the energy of the polarized X-rays for experiments. A schematics of the basic setup for XMCD experiments in these two beamlines is shown in Fig. 1.9. The polarized and monochromatized X-rays are directed through the sample, which is located at the center of a superconducting magnet. The magnetic field is applied on the direction of the incoming beam. The detection of the polarized dependent X-ray absorption spectra may be performed by fluorescence yield (FY) or total electron yield (TEY), the latter regularly used in the soft X-ray regime. The fluorescence detectors are (single- or multi-anode) ion implanted silicon photodiodes, which are characterized by a high efficiency in the X-ray range, fast time response, excellent linearity, and nearly insensitivity to magnetic fields.
2.2. Morphological and structural study 35 the Co/W film has a nearly constant thickness. Each metallic layer of about 4.2 nm thick, shows ordered zones alternating with amorphous zones. In the ordered regions, periodicity is around 0.2 nm, confirmed by fast Fourier transform (FFT) performed on some of the ordered zones (see bright spots observed in Fig. 2.3(d) and 2.3(e)). This periodicity and the distances and angles on the FFT are in agreement with the (1 1 0) planes of W bcc structure. There is also evidence of different grains within the crystalline zones on the layer, identified, for example, by the two orientation of the planes observed in the HRTEM image (see Fig. 2.3(c)), and the splitting of the spots in Fig. 2.3(d). EDS analysis show the presence of both Co and W. However, it is not easy to establish differences between ordered and disordered zones by this technique. Given the higher amount of W in this last sample, the Co-W alloy is possibly saturated, so that W starts to generate the crystalline zones identified from the images (Fig. 2.3(c)). Further discussion about W growing as a crystal in the samples is presented in the EXAFS section (see section 2.2.2). High contrast obtained in plan view HAADF STEM images for the aseries samples with tCo = 0.7 nm and tW= 0.6 and 1.5 nm (Fig. 2.5(a) and 2.5(b)) allows easier identification of the particles than in HRTEM images due to the huge Z contrast between the heavy metal particles and the light oxide matrix. In these images, brighter parts correspond to Co-W nanoparticles, and darker parts to Al2O3. Images obtained are comparable to those of similar systems of metallic nanoparticles embedded in insulator matrices [93], and the shape of the particles is similar to that of Co-nanoparticles embedded in alumina [94]. HAADF STEM images reveal that particles in sample with tW= 1.5 nm (Fig. 2.5(b)) are bigger and more closely packed than particles in sample with tW= 0.6 nm (Fig. 2.5(a)). Size distributions for samples from the aseries with tCo = 0.7nm and tW= 0.6 nm (Fig. 2.5(c)) and 1.5 nm (Fig. 2.5(d))were obtained by digital processing of the images taken, for both cross section (Fig. 2.3(a) and 2.3(b)) and plan view configurations (Fig. 2.5(a) and 2.5(b)). Results for the diameter distribution on each case were fitted using a Gaussian distribution function. The values obtained from this analysis are listed in table 2.1. The effective diameters for each configuration, hDeffiCS for Cross Section and hDeffiPV for Plan View, were obtained with the assumption that particles have circular in-plane and elliptic out-of-plane projection shape, the latter with short axis a and long axis bon each projection, so that Deff =√ab. Interparticle distance, d, and surface density of particles, NS, expressed as number of particles per nm2for the plan view images, were also obtained (see table 2.1). These two values are almost equal for both samples analyzed in plan view, which means that particles are spatially distributed on each layer in the same way for those samples from the aseries. Cross section values have a higher error since they
36 Chapter 2. Structural and magnetic properties of amorphous Co-W alloyed NPs 6 012345678 0.0 1.5x103 3.0x103 4.5x103 Plan View Cross Section Effective Diameter (nm) Density (particles per μm2) 012345678 0.0 1.5x103 3.0x103 4.5x103 6.0x103 7.5x103 Plan View Cross Section Effective Diameter (nm) Density (particles per μm2) (a) 20 nm 20 nm (b) (c) (d) Figure 2.5: HAADF STEM images in plan view configuration for the aseries samples with tCo = 0.7 nm and (a) tW= 0.6 nm and (b) tW=1.5 nm. Size distribution of plan view and cross section configurations for the samples in (a) and (b) are shown in (c) and (d), respectively. were obtained from poor contrast HRTEM images, so particle identification was less precise than in the HAADF STEM images in the plan view case. Size distributions for cross section and plan view configurations for the asamples series are shown in Fig. 2.5(c), for sample with tW= 0.6 nm, and in Fig. 2.5(d) for sample with tW= 1.5 nm, both with tCo = 0.7 nm. These distributions are centered near the same mean hDeffi; i.e., there is a slight difference between both values. hDeffifor the in-plane projection shape obtained from the plan view configuration analysis is larger than the out-of- plane projection from cross section analysis in both samples (tW= 0.6 and 1.5 nm). Thus, Co-W particles have an oblate shape. Digital analysis of the images obtained in cross section for samples from the bseries were also performed in order to identify some morphological parameters; however, size distributions in these cases were not obtained, due to the low contrast and less separation between the particles in these two samples (see Fig. 2.4(a) and 2.4(c)). A clear tendency in the size of the particles given by the Co/W ratio in the samples is also evident from the values in table 2.1, so that out-of-plane projection increases from 2.84 to 4.24 nm for samples in
2.2. Morphological and structural study 37 Table 2.1: Average particle diameter (hDeffi), distribution width (σ), interparticle distance (d), and density of particles in the layer (NS) obtained from digital analysis of TEM images taken in cross section (CS) and plan view (PV) configurations. Samples tCo tWhDeffiCS σCS dCS hDeffiPV σPV dPV NS Series (nm) (nm) (nm) (nm) (nm) (nm) (nm) (nm) (·102nm−2) a0.7 0.6 3.6(1) 0.4(2) 5.8(5) 3.87(4) 0.82(6) 5.3(5) 3.2(1) 0.7 1.5 3.9(1) 0.9(5) 6.6(7) 4.23(6) 1.0(1) 5.6(9) 3.5(1) b 0.4 1.5 2.84(2) −5.3(5) − − − − 0.7 1.5 3.9(1) 0.9(5) 6.6(7) 4.23(6) 1.0(1) 5.6(9) 3.5(1) 1.0 1.5 4.24(2) −6.7(3) − − − −
38 Chapter 2. Structural and magnetic properties of amorphous Co-W alloyed NPs the bseries, as tCo increases from 0.4 nm to 1.0 nm. The elemental composition of the nanoparticles has been measured by EDS on the plan view sample with tCo = 0.7 nm, and tW=0.6 nm. A total of 12 particles were measured yielding to an average composition with tungsten content of 27 ±6 at.%W; i.e. the particle composition is close to that of Co3W. Moreover, the composition within one particle was constant within experimental error. The relative variation in the composition of the other particles has been determined by EXAFS analysis at the Co K-edge (see section 2.2.2). From this morphological study we conclude that we have obtained a system of self-organized and uniformly dispersed amorphous Co-W alloy NPs. This occurs since W has alloyed with the preformed Co NPs, instead of growing as a homogeneous crystalline film covering the particles. The size of the amorphous particles depends on the amount of Co and W deposited on each layer. Particles formed within the layers have an oblate shape. When the amount of W increases and the Co-W alloy saturates, W grows as a crystal and fills the interparticle spaces. Previous works on Co-W thin films have led to similar amorphous structure, when such films are synthesized by sputtering, using composite targets [26, 95]. The amorphous forming ability (AFA) of Co-W has been studied in terms of the Miedema’s coordinates model, Y=|∆φ/∆n1/3 WS|, where ∆φ=φCo −φW, and ∆nWS =nWS(Co) −nWS(W), where φis the chemical potential, and nWS the electron density of the Wigner-Seitz unit cell, and Z=|(RW−RCo)/RCo|[95]. The binary alloy phase space is separated by the empirical law Y= 2.52Z−1/4in the amorphous and crystalline areas. It was found that Co-W lies in the amorphous region; the reason for this favorable AFA in this alloy is a negative heat of mixing, large atomic size differences and a low substrate temperature that avoids recrystallization via diffusion. These factors have explained satisfactorily the formation of Co-W amorphous thin films by co-sputtering [26]. In our preparation method Co nanoparticles are formed first, and a subsequent W capping supplies the alloying metal. The sputtering voltage is enough to let W and Co react, while the substrate temperature avoids crystallization. The AFA is high since the W concentration is higher that 17%, a condition needed for the formation enthalpy of the amorphous phase to be lower than the crystalline one [95]. Therefore, amorphization is favorable in the formation of Co-W NPs, just as it is in the thin film case.
2.2. Morphological and structural study 39 2.2.2 XANES and EXAFS measurements X-ray absorption near edge structure (XANES) and EXAFS spectra for both aand bsamples series were measured at the Co K(7709 eV) and W L3(10207 eV) edges using a double-crystal Si(111) monocromator in the BM29 beamline at the European Synchrotron Radiation Facility (ESRF). Measurements were performed at 300 K in fluorescence detection mode with a 13-element Ge solid state detector with digital signal processing for fluorescence X-ray absorption spectroscopy (XAS), high energy resolution and high count rate. Reference samples were also measured at different edges: Co particles embedded in alumina matrix (referred in the following as “bare Co NPs”) (Al2O3/Co)20 with tW= 0.7 nm measured at the Co Kedge, Co3W alloy measured at the Co K and W L3edges, Au capped particles with formula (Al2O3/Co/Au)25,tAu = 1.5 and 4.5 nm, measured at the Co Kand Au L3edges. The reference foils: Co metallic foil measured at the Co Kedge, W metallic foil measured at the WL3edge and Au foil measured at the Au L3edge. For each edge measured on each sample, four spectra were taken in order to have enough statistics in data treatment, following a 4 s/point count. Some of the XANES spectra at the W L3edge were recorded at the ESRF ID12 beamline, by a fluorescence detector in backscattering geometry. The APPLE-II undulator and a double - Si - (111) - crystal monocromator were used to collect the spectra. The X-ray absorption spectra were analyzed following standard procedures. A preliminary reduction of the EXAFS raw data involving background removal of the absorption data µ(E), conversion of µ(E) to χ(k), normalization and weighting scheme were performed with AUTOBK and ATHENA, programs from the simulation package IFEFFIT [96]. EXAFS data analysis and fitting were performed on all reference and samples at their respective edges. All spectra were fitted using the ARTEMIS program from the same IFEFFIT package using models based on the crystallographic information found in the ICSD6database. Atomic clusters used to generate the scattering paths for fitting were generated with ATOMS, a tool from the same simulation package [97]. Co Kedge results The X-ray absorption near edge structure (XANES) allows to study the electronic structure of Co (electron configuration [Ar]3d74s2) and W (electron configuration [Xe]4f145d46s2) atoms of the Co-W systems. Spectra at Co K 6http://icsd.iqfr.csic.es/icsd/
40 Chapter 2. Structural and magnetic properties of amorphous Co-W alloyed NPs 7680 7700 7720 7740 7760 7780 0 . 0 0 . 2 0 . 4 0 . 6 0 . 8 1 . 0 tW= 1 . 5 n m C o F o i l tC o = 0 . 4 n m tC o = 0 . 7 n m tC o = 1 . 0 n m N o r m a l i z e d X A N E S P h o t o n e n e r g y ( e V ) 0 . 4 0 . 6 0 . 8 1 . 0 - 1 . 0 - 0 . 5 0 . 0 tC o ( n m ) ∆A o f p e a k ( e V ) P e a k I P e a k I I 7680 7700 7720 7740 7760 7780 0 . 0 0 . 2 0 . 4 0 . 6 0 . 8 1 . 0 C o F o i l B a r e C o N P s tW= 0 . 6 n m tW= 1 . 5 n m tW= 4 . 5 n m P h o t o n e n e r g y ( e V ) tC o = 0 . 7 n m N o r m a l i z e d X A N E S 012345 - 0 . 8 - 0 . 6 - 0 . 4 - 0 . 2 0 . 0 P e a k I I tW ( n m ) ∆A o f p e a k ( e V ) P e a k I ( a ) P e a k I P e a k I I P e a k I P e a k I I ( b ) Figure 2.6: XANES at the Co Kedge for the Co-W NPs (a) asamples series, (b) b samples series. A spectrum for the Co foil is plotted for reference in both cases. In figure (a) a curve for bare Co NPs with tCo = 0.7 nm has been included for comparison. Insets: Variation of the areas of peak I and peak II in figure (a) and (b) as a function of tWand tCo, respectively. edge for Co-W NPs from the aand bseries are shown in Fig. 2.6(a) and 2.6(b), respectively. In both cases a Co foil XANES is plotted for reference, and a spectrum for bare Co NPs with tCo = 0.7 nm is plotted in Fig. 2.6(a) for comparison. Changes in the intensity of the pre-edge peak and the white line (denoted as peak I and peak II, respectively, in Fig. 2.6) are noticeable. The variation of the peaks areas (∆A = REf Ei(µsample −µCo-foil)dE) in series aand bis shown in the insets of Fig. 2.6(a) and 2.6(b), respectively. The integration limits were 7708.4−7721.3 eV for peak I, and 7721.3−7729 eV for peak II. The Co Kedge white line reflects its 4pempty states near the Fermi energy. The origin of peak I is at the density of states (DOS) of d−character available at the Fermi energy, projected onto the Co site [98, 99]. This is influenced by intra-atomic Co 4p−3dhybridization, as it will be further described in section 3.1.1. Moreover, in our samples, this d−DOS originates both at the Co 3d band and at the W 5dstates through interatomic Co 3d−W 5dhybridization. The intensity of peak I in Co-W NPs is clearly lower than in metal cobalt, and than bare Co NPs for the asamples series. The same reduction at peak I with respect to Co foil is observed for the bseries. Although alloying with W introduces a higher number of dholes in the system, hybridization strongly delocalizes the dempty states, depleting the intensity of peak I by reducing the d−DOS projected at the Co site. Therefore, the strong reduction of peak I at the Co Kedge of Co-W NPs is a proof of Co 4p−3d−W 5dhybridization. In series a, peak I is practically constant along the series (see inset of Fig. 2.6(a)), reflecting that Co 3d−W 5dhybridization is not affected by small variations in the amount of W for a fixed Co content. This, in principle,
2.2. Morphological and structural study 41 surprising fact strongly suggests that the alloy composition is similar for the three samples along this series, a result that will be confirmed by EXAFS (later in this section) and by magnetic analysis (section 2.3.1). In contrast, bsamples series show a clear increase of the ∆A of peak I upon increasing Co content in the NPs, as shown in the inset of Fig. 2.6(b). This trend is the expected one, as a decrease in the proportion of W (or increase of Co/W ratio) in the sample lowers the number of 5dholes available for hybridization, increasing the localization of the d−character states at the Co site. The intensity of peak II depends on both the number of available 4pstates, and the structure of the system, in a non-trivial way. The comparison of the Co metal and Co-W NPs has to be taken with care, as their structures are different (hcp and amorphous, respectively). However, the trend of ∆A of peak II in samples from the aseries indicates that the number of 4pholes is enhanced as the W content increases, suggesting an electronic transfer from Co 4ptowards W 5dstates. Accordingly, ∆A of peak II in samples from the b series slightly decreases with Co content, suggesting that, for the range of tCo and tWstudied, the number of 4pholes is reduced as the ratio Co/W increases. In short, along the aand bseries, as the Co/W ratio increases, both the 4p number of empty states and the delocalization of 3dempty states decrease. Structural analysis that can be extracted from the χ(k) EXAFS signal is better studied by its Fourier transform, shown in Fig. 2.7, performed on a krange from 2.0 to 11.9 ˚ A−1using a k2weight and a hanning window function. This R-space data show peaks which correspond to different atomic shells surrounding the absorbing atom, Co in this case. In Fig. 2.7(a), it can be seen that the position and shape of the peaks in the bare Co nanoparticles and Co foil are very similar, not only for the first coordination shell, but also for outer shells, showing that Cobalt in Co/Al2O3aggregates in a similar structure as metallic Co, as it has been reported in the literature [94]. However, the peaks for outer coordination shells are different in the W-capped Co nanoparticles. This is caused by a change in the Co coordination due to alloying between Co-W, which is also evident in Fig. 2.7(b) for the bsample series. Indeed, intensities of all peaks in both Fig. 2.7(a) and 2.7(b) are larger in the Co foil than in the particulate systems, as it is expected from the reduction in the mean Co coordination due to the size reduction. In the present study, EXAFS signal for the bare Co nanoparticles with tW= 0.7 nm was fitted using a Co - fcc metal model, where the coordination number Nwas used as a fitting parameter. A reduction from N= 12 in the metallic Co to N= 6.1 in the first coordination shell of the bare Co nanoparticles was obtained from this fit. However, recent works have demonstrated that such a strong reduction in the number of first neighbors could be
42 Chapter 2. Structural and magnetic properties of amorphous Co-W alloyed NPs 123 0 . 0 0 . 5 1 . 0 1 . 5 0123456 0 1 2 3 4 5 Co Foil Co3W tCo=1.0 nm tCo=0.7 nm tCo=0.4 nm tW=1.5nm |χ(R)| (Å-3) R(Å) 0 1 2 3 4 5tCo=0.7nm |χ(R)| (Å-3) Co Foil Co3W Bare Co NPs tW=0.6nm tW=1.5nm tW=4.5nm 123 0 . 0 0 . 5 1 . 0 1 . 5 (a) (b) Figure 2.7: Fourier transform of EXAFS signal at the Co Kedge on the Co-W samples. (a) asamples series. (b) bsamples series. Measurements for Co foil and bulk Co3W in both cases, and bare Co nanoparticles with tCo = 0.7 nm in (a) are shown for comparison. Inset: zoom of the first coordination shell in the particulate systems. an artifact of EXAFS analysis [100], due to effects of surface distortions on the nanoparticles, producing an underestimation of the average coordination number. A reduction in the EXAFS signal as a result of lower Co coordination due to alloying is also observed when the signal for the Co foil is compared with the one for bulk Co3W in Fig. 2.7(a) and 2.7(b). This behaviour supports the scheme of Co-W alloy presence in the Co-W nanoparticles. There is a further reduction in the amplitude of all peaks and lack of structure beyond the first two coordination shells in the Co-W nanoparticles systems, which is characteristic of amorphicity, thus supporting the observation of amorphous structure in the HRTEM measurements. In general, amorphous compounds are characterized by damping of their EXAFS signal compared to a reference foil, consistent with static disorder and reduction of average coordination number [101]. In the HRTEM section we have mentioned that capping the Co nanoparticles with noble metals does not affect the structure of the NPs [11]. This has
2.2. Morphological and structural study 43 20 30 40 50 60 70 80 -1000 -500 0 500 1000 1500 2000 Intensity (counts) 2 θ (º) Yobs Ycal Yobs-Ycal 0 1 2 3 4 5 0 1 2 3 Co-W NPs Fit Bulk Co3W Fit Window Bulk Co3W Co-W NPs with tCo=0.7nm tW=1.5nm |χ(R)| (Å -3 ) R (Å) W Co Figure 2.8: FT EXAFS signal at the Co Kedge for the bulk Co3W alloy and comparison with that of a Co-W alloy NPs sample. Dashed lines: best fit of the first Co coordination shell for each sample. Inset: an illustration of the structure of a Co first coordination shell. also been observed with EXAFS, so that bare and Au-capped Co nanoparticles have equivalent fcc crystal structure when comparing their Fourier transformed EXAFS signal7. However, capping the Co NPs with W completely modifies the structure of the original particles by forming an amorphous alloy. Different models were tested in order to fit the Co Kedge R-space data for the W-capped Co nanoparticles. Some of the fitting tests were performed by using a model of pure Co - fcc metal, such as the one typically used in the bare Co nanoparticles case, and by using a W - doped metal Co model. However, the best fitting model was obtained by using the Co - scattering paths of the most stable Co-W alloy,8i.e., Co3W, and determining the deviation in the average coordination (N) and interatomic distance (R) for each Co-W NPs sample. Given the high affinity of Co and W to form Co-W alloys [25, 27, 85, 86] we have assumed that all Co in the Co-W NPs samples is uniformly alloyed 7EXAFS spectra for the Au-capped Co NPs were recorded during the same experiment and compared to those for the uncapped Co-NPs, both with the same tCo = 0.7 nm. We found that both systems have fcc structure and very close first near neighbor distances. Their Fourier Transformed EXAFS profiles are almost identical, even for outher coordination shells. The first coordination shell peak in the Co - Au NPs is higher in amplitude than the uncapped ones and it increases with the content of Au in the sample due to the high crystallinity in these noble - metal capped particles. Then, contrary to the case of W deposit, noble metals - capping do not modify the crystal structure of the Co NPs. 8http://www.sgte.org/
44 Chapter 2. Structural and magnetic properties of amorphous Co-W alloyed NPs with W. Then, we have estimated the change of the Co environment when increasing the amount of W or Co in the sample, and the different trends the structural parameters follow when varying them. Due to the amorphous nature of the Co-W NPs, it is very difficult to fit the EXAFS signal beyond the first coordination shell. Moreover, as it was mentioned above, strong structural disorder in the NPs systems can lead to erroneous interpretation of the EXAFS analysis [100, 101]. Then, fitting of the Co-W NPs EXAFS signal was performed on the R-space in a range from 1.0-3.0 ˚ A using a hanning window function, so that it covered the Co first coordination shell in the alloy (see Fig. 2.8 and 2.9). For comparison, the EXAFS signal of the bulk Co3W alloy has been fitted in the same Rrange. An illustration of this Co first coordination shell in the crystal structure of the Co3W alloy is shown in the inset of Fig. 2.8. In this structure, the central Co is surrounded by a total of twelve atoms (NT= 12, typical in hcp structures), from which eight are other Co atoms (NCo−Co = 8) and the remaining four are W atoms (NCo−W= 4). The amplitude reduction factor S2 0and the shift in the threshold energy ∆E0were set to those obtained for the Co foil fit. A total of 10 fitting parameters were used for an iterative procedure, which 0 . 5 1 . 0 1 . 5 2 . 0 2 . 5 3 . 0 3 . 5 0 . 0 0 . 2 0 . 4 0 . 6 0 . 8 1 . 0 1 . 2 1 . 4 1 . 6 tW=1.5nm |χ(R)| (Å-3) R(Å) tCo=0.4nm Fit tCo=0.7nm Fit tCo=1.0nm Fit Window 0 . 0 0 . 2 0 . 4 0 . 6 0 . 8 1 . 0 1 . 2 1 . 4 tCo=0.7nm |χ(R)| (Å-3) tW=0.6nm Fit tW=1.5nm Fit tW=4.5nm Fit Window 1 . 8 1 . 9 2 . 0 2 . 1 2 . 2 2 . 3 0 . 8 0 . 9 1 . 0 1 . 1 1 . 2 1 . 3 1 . 8 2 . 0 2 . 2 2 . 4 0 . 6 0 . 8 1 . 0 1 . 2 1 . 4 1 . 6 (a) (b) Figure 2.9: Best fits to the first coordination shell on the Co Kedge R-space EXAFS signal for all five Co-W nanoparticles samples studied. (a) asamples series. (b) b samples series. Inset: zoom of the fitted peak.
2.3. Magnetic study 51 FC-ZFC Measurements M(T) at H = 50 Oe 0.5 1.0 1.5 2.0 TB=9.59K TB=8.04K tW=0.6 nm tW=1.5 nm tW=4.5 nm (emu/cm3.Co) tCo=0.7 nm TB=10.00K 010 20 30 40 50 60 70 80 0.5 1.0 1.5 2.0 2.5 3.0 3.5 TB=3.07K TB=9.59K T(K) x10 tCo=1.0nm tCo=0.7nm tCo=0.4nm (emu/cm3.Co) tW=1.5 nm TB=23.18K (a) (b) Figure 2.14: DC susceptibility curves for samples from the aseries in (a) and from the bseries in (b). of Co increases because particles are bigger and closer. These results of the magnetic interactions in the Co-W NPs are well supported by analysis of the variation of the FC/ZFC - curves height ratios [104], which show the same trend. This is, FC/ZFC - curves height ratios for the aseries are almost equal and they decrease as tCo increases for the bseries samples. Magnetization as a function of field in the paramagnetic region (M(H) at T≈3TB) for both sample series are plotted in Fig. 2.15. These M(H) curves were identical when measured with the field parallel and perpendicular to the sample plate, therefore the particle anisotropy axes are randomly distributed in all samples and the demagnetization factor plays no role in the present case. Values of the magnetization per Co atom deposited in the samples, mtot, obtained from saturation are listed in table 2.3 and plotted in Fig. 2.16. It was found that mtot decreases for samples from aseries as the W capping layer thickness increases for a constant tCo (Fig. 2.15(a) and 2.16(a)) and in samples from the bseries as the amount of Co decreases for a fixed tW(Fig. 2.15(b) and 2.16(b)). The magnetization is supported by the Co atoms since W has a negligible induced moment.9Then, there is a strong reduction on the magnetic 9See details of the induced magnetic moments in the W atoms of these samples in chapter 3.
52 Chapter 2. Structural and magnetic properties of amorphous Co-W alloyed NPs 0200 400 600 800 1000 0.00 0.15 0.30 0.45 0.60 H/T (Oe/K) tCo=0.7 nm 32 K 40 K tW=4.5 nm tW=1.5 nm M( B/Co) tW=0.6 nm 40 K 0200 400 600 800 1000 0.00 0.25 0.50 0.75 1.00 40K 12K H/T (Oe/K) tW=1.5 nm M( B/Co) tCo=0.4 nm tCo=0.7 nm tCo=1.0 nm 100K (a) (b) Figure 2.15: Magnetization curves for samples for samples from the aseries in (a) and from the bseries in (b). The dashed lines are fitted Langevin curves with hDmagi and σparameters given in table 2.3. moment of the Co atoms due to the formation of Co-W amorphous alloy. This reduction may be due to combined effect of charge transfer, hybridization and environmental effects, as it is described in Ref. [27]. According to this author, when the number of Co first neighbors is higher than 3, Co atoms carry their full magnetic moment of 1.7 µB/Co [27]. This is the case of previously studied bare Co nanoparticles [19]. However, if the Co atom has less Co atoms as first neighbors, e.g. 2 or 3 Co atoms, its magnetic moment decreases to about 0.5 µB/Co. The latter value is well in agreement with the moments found for Co atoms in the samples studied in this work. The strong reduction of the Co moment in our samples is due to a decrease in the Co coordination of the Co atoms because of the presence of W, demonstrated via EXAFS analysis in the previous section. Such decrease in T1−x−Mxalloys (Tbeing a transition metal and Musually a non-magnetic metal) has been reported in previous works [105] and will be further discussed in section 2.4. For those samples where the number of particles per unit surface, NS, was identified from the STEM images in the morphology characterization, we can easily determine the magnetic moment per particle, mPart. This is obtained by dividing the saturation magnetization by NS, both, per unit surface. mPart values are listed in table 2.3. The average amount of Co atoms per particle is also easily determined by the ratio of deposited Co and number of particles, per unit surface. The resulting moment per Co atom (table 2.3) decreases with increasing the amount of W in the aseries samples from 0.52 to 0.30 µB/Co, for tW= 0.6 and 4.5 nm, respectively. Also, it strongly decreases with reduction of the amount of Co in the bseries samples from 0.93 to 0.08 µB/Co for tCo = 1.0 and 0.4 nm, respectively. Thus, the reduction in Co moment expected for Co-W alloying [25, 27] is properly verified.
2.3. Magnetic study 53 Table 2.3: Summary of the parameters deduced from the magnetic measurements on Co-W Nanoparticles Samples tCo tWTBθ mtot mPart xin Co-W Msb hDmagiσmag hUiKeff Series (nm) (nm) (K) (K) (µB/Co) (103µB) alloy (%) (103emu/cm3) (nm) (nm) (K) (106erg/cm3) a 0.7 0.6 10.00(6) 7.3(2) 0.52(2) 1.03(1) 18.2(4) 0.413(2) 3.4(2) 0.25(5) 270(10) 1.4(3) 0.7 1.5 9.59(6) 8.0(3) 0.46(1) 0.84(1) 18.8(4) 0.367(2) 3.2(2) 0.32(5) 220(4) 1.2(2) 0.7 4.5 8.04(3) 5.9(2) 0.30(1) 0.57(1) 20.3(4) 0.235(2) 3.4(6) 0.38(5) 200(10) 1.0(5) b 0.4 1.5 3.07(6) 1.7(9) 0.088(2) −22.3(4) 0.062(2) 2.6(5) 0.25(5) − − 0.7 1.5 9.59(6) 8.0(3) 0.46(1) 0.84(1) 18.8(4) 0.367(2) 3.2(2) 0.32(5) 220(4) 1.2(2) 1.0 1.5 23.18(7) 13.3(9) 0.93(3) −14.1(4) 0.725(2) 4.4(2) 0.38(5) 890(30) 2.4(3)
54 Chapter 2. Structural and magnetic properties of amorphous Co-W alloyed NPs 0 . 0 0 . 2 0 . 4 0 . 6 0 . 8 1 . 0 0 . 0 0 . 2 0 . 4 0 . 6 0 . 8 1 . 0 tW= 1 . 5 n m tC o = 1 . 0 n m tC o = 0 . 7 n m ma t (µB/ C o ) tC o ( n m ) tC o = 0 . 4 n m 012345 0 . 0 0 . 1 0 . 2 0 . 3 0 . 4 0 . 5 0 . 6 0 . 7 tC o = 0 . 7 n m tW= 4 . 5 n m tW= 1 . 5 n m tW= 0 . 6 n m ma t (µB/ C o ) tW ( n m ) ( a ) ( b ) Figure 2.16: Total Co magnetic moment per Co atom in the Co-W NPs as deduced from the M(H) measurements. (dashed lines) Guide to the eye. (a) asamples series. (b) bsamples series. An average Co1−xWxalloy composition in the Co-W NPs may be proposed by comparing the mtot values to those measured for Co-W films deposited by rf sputtering in Ref. [26]. Values of %W in the alloy are shown in table 2.3. The W concentration that explains the reduction in magnetic moment ranges from 18.2 to 20.3 at % in the asamples series, and from 14.1 to 22.3 at % in the bsamples series. From the equilibrium magnetic properties of each sample we can determine the particle size distribution and compare it with the results obtained by HRTEM and STEM. This is obtained by fitting the M(H) curves at high T to a Langevin function, averaged over the appropriate particle size distribution. We define g(Dmag) as the gaussian distribution of a number of particles having a diameter equal to Dmag. For spherical particles, the particle magnetization is written as mpart =πMsbD3 mag/6, where Msb is defined as the particle magnetic density, calculated from the saturation magnetization values and the density of the Co-W alloy formed on each sample as Msb(x) = mtot(µB/Co)ρ(x) Mw(x)NaµB(2.1) where xgives the Co1−xWxalloy composition, ρ(x) is the density and Mw(x) the molecular weight of the alloy, Nais the Avogadro number and µB the Bohr magneton. Since there are no direct values in the literature for the densities of the Co-W alloys found for our samples, we need to calculate them. Knowing that the density for metallic Co is 8.9 g/cm3and the one for Co3W alloy is 12.7 g/cm3[106], we can apply linear approximation for ρ(x) vs. x. Given the xvalues found for our Co-W samples (listed in table 2.3) we can interpolate each composition value and get its respective density.
2.3. Magnetic study 55 The experimental data are fitted by the expression: M(H, T) =xparampara +(1 −xpara)Msb Rg(Dmag)V[M(H, T, µ)/mtot]dD Rg(Dmag)V dDmag (2.2) Let us recall that xpara gives the fraction of non-aggregated Co atoms present in the samples. In the case of bare and noble-metal capped Co NPs they give a paramagnetic contribution as a positive slope of M(H) at high fields [17, 19]. In our Co-W alloy NPs, the non-aggregated Co atoms are also alloyed with W. They do not contribute to the magnetic signal, i.e., at high fields the slope of M(H) is negligible. Then mpara in equation 2.2 is null and equation 2.2 is reduced to the second term. Results for these fits are the dashed lines in Fig. 2.15. The average magnetic diameter values hDmagiand the distribution width for the Gaussian distribution of particle size, σmag obtained are listed in table 2.3. These parameters were confirmed by fitting the equilibrium susceptibility 1/χeq(T) in the superparamagnetic temperature regime, measured for the same samples. This is, for a system of particles of that diameter and size distribution, χeq can be expressed as χeq =Rg(Dmag)V(M2 sbV/3kBT)dDmag Rg(Dmag)V dDmag (2.3) Comparing the values of hDeffiobtained from the morphological analysis described in section 2.2.1 with the hDmagiderived from this magnetic analysis, we note that the latter is smaller. From the above facts we may conclude that our amorphous Co-W NPs are composed by a magnetic Co-W alloy core surrounded by unalloyed metallic W, which tends to fill the interparticle space, as described in sections 2.2.1 and 2.2.2. 2.3.2 Magnetic anisotropy of the Co-W particles The phenomenon of superparamagnetic blocking described in the FC-ZFC curves analysis is related to the magnetic anisotropy of the particles. The anisotropy favors some particular orientations of the magnetic moment, two opposite to each other in the simplest case of uniaxial anisotropy, which are separated by activation energy barriers U. The rate at which the magnetic moment of the particles flips from one orientation to the other is determined by this anisotropy Keff, so that we write U=KeffV, with Vbeing the particle
56 Chapter 2. Structural and magnetic properties of amorphous Co-W alloyed NPs magnetic volume. The relaxation time, τ, follows an Arrhenius’ law (τ= τ0exp(U/kBT)), where τ0≈10−10 −10−13s is the inverse attempt frequency that depends on the damping of the magnetic moments by the phonons. The superparamagnetic blocking occurs when τ=te, where teis the measuring time of each experimental point, so TB∼ =αU/kBln(te/τ0) where αis a constant that depends on the width of the particle size distribution. An accurate way to obtain Uis derived from the full distribution of activation energies f(U) and then to find which value of Ucorresponds to particles with a diameter equals to Dmag. A detailed description of this procedure can be found in Ref. [17]. f(U) can be directly determined from the analysis of the imaginary part of χac(T), measured near the superparamagnetic blocking temperature TB. For non-interacting particles we write χ00 ≃π 2kBTχeq(T, U)f(Ub) (2.4) where we define Ub=kBTln(1/ωτ0), as a scaling variable, corresponding to the activation energy of those particles having τ=te= 1/ω at a given T. The frequency dependent χac should converge into a single curve when plotting χ00 vs. Ub/kB.f(U) can be determined from equation 2.4 from a χ00(Ub) fit. In Fig. 2.17 we have plotted the result obtained from this χac(T) analysis, including the χ00(Ub) fit, for the sample with tCo = 0.7 nm and tW= 1.5 nm. We also show the Arrhenius plot of ln(1/ω) vs. 1/TB, from the analysis 0 100 200 300 400 500 600 700 0 . 0 0 0 . 0 2 0 . 0 4 0 . 0 6 0 . 0 8 0 . 1 0 0 . 1 2 tC o = 0 . 7 n m tW= 1 . 5 n m 1 H z 5 H z 1 0 H z 9 0 H z 240Hz 480Hz F i t χ’’ (e m u / c m 3) Ub/ k B ( K ) 0 . 0 6 0 . 0 9 0 . 1 2 - 1 0 - 8 - 6 - 4 - 2 tW= 0 . 6 n m tW= 1 . 5 n m tW= 4 . 5 n m 1 / T B ( K - 1 ) l n ( 1 / ω) tC o = 0 . 7 n m Figure 2.17: Imaginary part of the ac susceptibility for the sample with tCo = 0.7 nm and tW= 1.5 nm plotted as a function of the scaling variable Ub. The solid line is the fitting result. Inset: Arrhenius plot of the measuring time (1/ω) as function of TB, as obtained from χ00 measurements for the aseries samples.
2.3. Magnetic study 57 obtained from χ00 measurements for the aseries samples. In the case of the sample with the lowest amount of Co (tCo = 0.4 nm and tW= 1.5 nm) this analysis was not performed since the χac signal was negligible. Keff is then obtained from U(hDmagi) = Keff(π/6)hDmagi3, where hDmagi denotes the average magnetic diameter of the spherical particles. All this analysis is performed assuming that the magnetic moment is just supported by the Co-W magnetic alloy core. The values of the average hUiand Keff obtained for all samples are shown in table 2.3. Keff in our Co-W NPs decreases with increasing tWfor the aseries samples and with decreasing tCo for the bseries samples. This gives Keff a trend directly proportional to hDmagi, suggesting that surface anisotropy is not playing an important role in the Keff as in other particulate systems [11, 19, 78–81]. Further discussion on these results will be presented in section 2.4. 2.3.3 X-ray Magnetic Circular Dichroism magnetometry The XAS and XMCD experiments at the Co L3(778.1 eV) and Co L2(793.2 eV) edges were performed at the ID08 beamline of the ESRF. An APPLE-II undulator and a spherical grating monochromator were used. The degree of polarization was ∼100%. The total electron yield (TEY) detection method was employed. The beam direction and parallel magnetic field applied had an incident angle of 10−15◦with respect to the normal to the plate sample. The XMCD signal was obtained by a direct difference of the XAS spectra recorded with opposite helicities at each magnetic field value and for both orientations of the field. The applied field was 20 kOe and the temperature was T= 7 K in all cases. XMCD is a very powerful technique that allows to perform an element selective magnetometry on our Co-W NPs. From a XMCD experiment at the L2,3edges of Co one obtains, through the sum rules [64, 65] described in section 1.4.2, the spin and orbital moments averaged over the volume of the particle, and on the number of holes nhin the empty exchange split ndsub-bands (Co 3din the present case). The sum rules have been applied to the spectra to derive the orbital, spin and total magnetic moments per 3dhole of Co, mL/nh, mS/nhand mat/nh, respectively, with the symbols and sign criteria defined in Ref. [66]. We define the constant C= (IL2+IL3), where IL2and IL3 are the white-line integrated intensities after subtraction of the contributions from transitions to the continuum. It is noteworthy that in the present case of amorphous particles, with their individual anisotropy axes oriented at random, the dipolar term mDin mSeff =mS+mDcancels out, so that the sum rule (A−2B) = −CmS/(nhµB) yields the spin component mS/nh.Aand Bare the
58 Chapter 2. Structural and magnetic properties of amorphous Co-W alloyed NPs integrated areas of the L3and L2XMCD peaks, respectively. Besides, from the ratio of the sum rules mL/mSis directly derived, which is independent of nhand of the normalization method used. XMCD also allows us to study the changes in the orbital magnetic moment in the Co-W NPs samples as a function of tWand tCo by obtaining the average mL/nhper Co atom present in the sample. In the experiments a magnetic field of 20 kOe is applied, sufficient to saturate the particle spin magnetization. The contribution of the orbital moment to the XMCD signal is the averaged projection of the local orbital magnetic moments in the direction of the applied field (parallel to the photon beam direction in the experiments). The experimental XMCD spectra at the Co L2,3edges for sample with tCo = 0.7 nm and tW= 1.5 nm is depicted in Fig. 2.18, together with its XAS, for normalization sake. All XMCD results are qualitatively similar, 770 780 790 800 810 820 830 - 0 . 3 - 0 . 2 - 0 . 1 0 . 0 0 . 1 C o L 2 , 3 tC o = 0 . 7 n m tW= 1 . 5 n m X M C D I n t e g r a l N o r m a l i z e d X M C D P h o t o n e n e r g y ( e V ) - 0 . 6 - 0 . 4 - 0 . 2 0 . 0 0 . 2 ( b ) q p 0 1 2 3 4 X A S I n t e g r a l N o r m a l i z e d X A S 0 5 1 0 1 5 2 0 ( a ) C o L 2 , 3 tC o = 0 . 7 n m tW= 1 . 5 n m Figure 2.18: Co−L2,3edges spectra of the tCo = 0.7 nm, tW= 1.5 nm sample measured at T = 5 K, H= 20 kOe and incident angle 10◦. (a) (red) Normalized XAS spectra mean curve. (green) The double-step function used is also indicated. (dark blue) Integrated white line. (b) (light blue) Normalized XMCD spectra, (orange) integrated area.
2.3. Magnetic study 59 though the actual derived Aand Bvalues differ. The derived mL/mS,mL/nh and mS/nhvalues are given in table 2.4, along with the values of the total moment mtot/nh. Self-saturation effects may affect these TEY measurements in principle. It is customarily corrected in thin films [109], and has been done in the case of rather large Co and Fe nanoparticles [110, 111]. To correct for this effect the electron escape depth parameter λeat low kinetic energies of the particular material is needed. The Co-W alloys λeat low energies is not known, but at higher energies, of the order of 100 eV, it is very near to that for Co.10 Under this hypothesis, the correction due to saturation effects would be very similar to that needed for Co particles of the same size. It has been estimated that for Co particles with diameter D= 3 nm the mSand mL, parameters obtained with the sum rules from uncorrected XAS and XMCD spectra, may be underestimated by 2 and 13%, respectively [110], which amounts to an underestimation of 3% in mtot. Such a difference is comparable to the other sources of error in these experiments, like the presence of xpara, or the size distribution of the particles. Therefore, to account for this effect, we have added this source of error to the total estimated errors in the table 2.4 data, and should take conclusions from the trends rather than from the absolute values. The variation of the mL/mSratio as a function of the amount of Co and W in the samples can be analyzed from the values listed in table 2.4. In b samples series, for tCo= 0.4 nm the ratio is much larger than the value for bulk Co (mL/mS Co Bulk= 0.078), and decreases towards that value as the tCo/tWratio increases, being quite close for tCo= 1.0 nm (mL/mS=0.071) (see Table 2.4: mtot/nh,mL/nh,mS/nhand mL/mSper Co atom as determined from XMCD measurements. For the fcc bulk Co, mL/mS= 0.078 [107], mL/nh= 0.134 and mS/nh= 0.248 µBper 3dhole [67] (3d nCo h= 2.49) [108]. Samples tCo tWmL/mS mL/nhmS/nhmtot/nh series (nm) (nm) (µB) (µB) (µB) a 0.7 0.6 0.082(1) 0.018(1) 0.216(3) 0.234(3) 0.7 1.5 0.085(1) 0.015(1) 0.172(4) 0.186(4) 0.7 4.5 0.079(2) 0.010(1) 0.120(5) 0.130(6) b 0.4 1.5 0.159(7) 0.007(1) 0.042(4) 0.048(4) 0.7 1.5 0.085(1) 0.015(1) 0.172(4) 0.186(4) 1.0 1.5 0.071(1) 0.021(1) 0.290(9) 0.310(9) 10Data obtained from the NIST Electron Effective-Attenuation-Length Database,http: //www.nist.gov/srd/nist82.cfm
60 Chapter 2. Structural and magnetic properties of amorphous Co-W alloyed NPs 0 . 4 0 . 6 0 . 8 1 . 0 0.000 0.009 0.018 0.027 0.036 tC o ( n m ) mL/nh ( µB) 0 . 0 0 0 . 0 9 0 . 1 8 0 . 2 7 0 . 3 6 tW= 1 . 5 n m mS/nh ( µB) 012345 0 . 0 0 0 . 0 1 0 . 0 2 0 . 0 3 tW ( n m ) mL/nh ( µB) 0 . 0 0 . 1 0 . 2 0 . 3 mS/nh ( µB) tC o = 0 . 7 n m ( b )( a ) Figure 2.19: Dependence of Co mL/nhand mS/nh, on the Co and W composition. (a) asamples series, (b) bsamples series. table 2.4 and Fig. 2.19(b)). The reason for this difference at low tCo/tW can be found in the unusually low value of mS/nh(0.042 µBper 3dhole) for tCo=0.4 nm. Although the mL/nhdecreases with W alloying, the reduction of mS/nhis much stronger (see Fig. 2.19(b)). Therefore, alloying with W affects essentially the difference between up and down filled states in the Co 3dband. In contrast, the mL/mSratio as a function of the W capping thickness is practically constant (see variation of mL/nhand mS/nhin Fig. 2.19(a)), i.e., the compositional Co/W ratio in the alloys obtained in asamples series is similar (see also alloys composition in table 2.3). It may be concluded that the crucial factor to reach the different alloys in the Co-W NPs depends more on the amount of Co available for alloying than on the amount of W in the sample. We may estimate nhfor each Co-W composition by substituting in the mtot/nhvalues given in table 2.4, those mtot determined from M(H) measurements in the previous section (see table 2.3). Although W may be polarized by Co, its contribution to the net magnetization is orders of magnitude lower,11 so it is considered as negligible in this analysis. Therefore, the magnetization of our samples is mainly due to the Co present in the Co-W particles, so we may assume that both SQUID and XMCD magnetometry techniques yield the average total Co moment at saturation (for the sake of comparison we have used values at H= 20 kOe). Thus, from the comparison of both values, we can extract the variation of the nhin the Co 3dband in the Co-W NPs. For the aseries samples, nhwas found to be around an almost constant value of nh=2.4(1). Within experimental errors, this result is on the order or slightly lower than that for bulk Co (nh=2.49) [108], and is well in agreement with 11XMCD measurements at the W L2,3 edges on these W-capped Co nanoparticles samples have been performed to determine the induced magnetic moment of W. It was found to be on the order of ∼10−3µB/W at 10K, which is two orders of magnitude lower than the Co moment measured in the samples. These results will be described in detail in chapter 3.
Chapter 3 Breakdown of Hund’s third rule in amorphous Co-W alloy nanoparticles In the previous chapter, we have demonstrated that the amorphous Co-W alloy NPs constitute a paradigmatic system among the specific group of magnetic nanoparticles with amorphous structure: contrary to other amorphous nanoparticle systems where the anisotropy is due to surface effects, its origin in the amorphous Co-W alloy NPs lies on the structural short range order (SRO) detected in the particles. We have also described the Co-W hybridization and electronic transfer from W 5dto Co orbitals in these Co-W NPs by analysis of X-ray absorption near edge structure (XANES) measurements at the Co K and W L3edges (the electron configuration for Co is [Ar]3d74s2and for W is [Xe]4f145d46s2). The electronic transfer from W 5dtoward Co 4pbands, and the delocalization of the Co 3dempty states were qualitatively described as a function of the Co/W ratio in these Co-W NPs samples. The effects of similar 3d−5dhybridization, in particular on 5dinduced magnetic moments, have been previously studied both experimentally and theoretically in Fe/W multilayers [120] and bulk Co100−xIrxalloys [70], to cite some examples of metallic systems. A remarkable finding in these two systems is the observation of a breakdown of Hund’s third rule of the induced orbital and spin magnetic moments in the 5dmetals. This rule states how spin and orbital total moments in a single atom should be aligned, being parallel for an atom with more than half-filled shell, and antiparallel for a less than half-filled shell [121]. In spite of its phenomenological character and of being defined for single isolated atoms, atoms in solids have been proven to ubiquitously follow this rule, too.
70 Chapter 3. Breakdown of Hund’s third rule in amorphous Co-W alloy NPs However, the two cases mentioned above are part of the few examples where this rule is not completely fulfilled [70, 120, 122–124]. In the Fe/W multilayers, the total spin and orbital magnetic moments of the 5dW shell couple in parallel (notice that W is a less than half-filled 5dband metal), and for Ir in bulk Co-Ir alloys they are antiparallel aligned (Ir is a more than halffilled 5dband metal), being, in both cases, contrary to the predictions of the Hund’s third rule [70, 120]. All these experimental findings have been possible thanks to the highly sensitive X-ray magnetic circular dichroism (XMCD) technique, which, as described in previous chapters, allows to perform element specific magnetometry, as well as to separate the contribution of the orbital and spin moments to the total magnetic moment and their relative orientation, by applying the magneto-optical sum rules [64, 65]. The structural disorder in transition metal alloys has also been demonstrated to influence their electronic configuration [123]. In fact, for amorphous Fe-Zr and Co-Zr alloy films, the induced spin and orbital moments detected in Zr (a less-than half filled 4delement) are found to be parallel aligned, thus breaking down the Hund’s third rule. However, for similar crystalline compounds Fe-Zr-Pt and Co-Zr-Pt, the induced orbital and spin moments in Zr are found to fulfill this rule. Following these results, the amorphous Co-W alloy NPs arise as an attractive system to investigate the hybridization between Co orbitals and the 5dband of W, and its consequence on the induced spin and orbital magnetic moments in W. XANES and XMCD are the best techniques to study the electronic transfer between Co and W, and examine the compliance or breakdown of the Hund’s third rule in the W atoms in Co-W systems. This chapter is then dedicated to delving into these hybridization effects, both experimentally by XANES and XMCD measurements at the Co Kand W L2,3edges, and theoretically by simulations of the XANES and XMCD signals at both edges in the amorphous Co-W alloy NPs system. The polycrystalline bulk Co3W alloy is also included in the present study, so that, by comparison to the amorphous NPs, the influence of the structural disorder is evaluated. 3.1 XANES and XMCD measurements XANES and XMCD measurements at the Co K(7709 eV), W L3(10207 eV) and W L2(11544 eV) edges on the Co-W NPs samples and the bulk Co3W alloy were performed at the ESRF ID12 beamline. Spectra for Al2O3− capped Co NPs and on a W metallic foil for reference, were also recorded, at the Co Kand W L2,3edges, respectively. The APPLE-II undulator and a double - Si - (111) - crystal monocromator were used to collect the spectra
3.1. XANES and XMCD measurements 71 at the respective energies. XANES spectra were recorded by a fluorescence detector in backscattering geometry. XMCD signal was obtained by applying a magnetic field of 10 and 50 kOe for the Co-W NPs and the Co3W alloy, respectively, normal to the sample plane and along the X-ray beam direction. Measurements were performed at 7 and 10 K for the Co-W NPs and the Co3W alloy, respectively. This field and temperature were chosen according to the magnetic properties of the Co-W NPs, so that the system was reaching its magnetic saturation under these conditions (see section 2.3.1). XMCD was obtained by differences of XANES spectra measured with opposite helicities of the light at a fixed magnetic field value, orienting the field in two inverse directions. Polarization of the circular light was over 90% at the Co Kedge and 94% at the W L2,3edges. Due to the low XMCD signal in W, several spectra were taken for each sample, being 16 spectra in average for each direction of the field. Due to experimental difficulties, the Co-W NPs sample with tCo = 0.7 nm and tW= 4.5 nm was not measured at the W L2,3edges. The absorption spectra and XMCD for the bulk Co3W alloy were corrected for self-absorption effects after their normalization of the absorption jump to unity. These corrections take into account that the sample is infinitely thick, and uses its chemical composition and density, along with some geometrical parameters of the measurement setup such as the angle of incidence of the X-ray beam and the solid angle of the detector, to estimate the effect of selfabsorption from the known energy dependence of the absorption coefficient of the sample. Details of the correction procedure can be found in Ref. [125] and references therein. 3.1.1 Co Kedge results XANES and XMCD at the Co Kedge probes the 4pempty states of the Co atom in the sample. Analysis of the XANES spectra recorded at this edge on these Co-W alloy NPs samples was described in section 2.2.2. Evidences of Co 4p−3dand Co 3d−W 5dhybridization in the Co-W system and electronic transfer from W 5dto Co orbitals were then observed. These findings were obtained not only from the observed changes of the Co Kedge XANES on the Co-W alloy NPs with respect to that of metallic Co, but also from the reduction of the magnetic moments of the Co atoms obtained in the Co-W alloy NPs by W inclusion in the alloy, as proven by analysis of the XMCD signals at the Co L2,3edges in section 2.3.3. The detection of a nonzero XMCD signal at the Co Kedge on all samples, shown in Fig. 3.1, reflects the magnetic polarization of the 4pband in Co atoms. In Fig. 3.1 we compare the XMCD spectra for all studied samples,
72 Chapter 3. Breakdown of Hund’s third rule in amorphous Co-W alloy NPs normalized to the energy jump of the absorption edge: the Al2O3capped Co NPs (Fig. 3.1(a)), the aand bsamples series (Fig. 3.1(b) and (c), respectively), and the bulk Co3W alloy (Fig. 3.1(d)). The origin of the energy scale has been chosen at the inflection point of the absorption edge. The XMCD signal in the case of the Al2O3capped Co NPs (Fig. 3.1(a)) emerges by interatomic exchange interaction between the 4pband of the absorbing Co and the 3d bands of the neighboring Co atoms. This results from the allowed symmetry operations at the Co site in this cubic structure, so that the 4p−3dbands - 0 . 0 0 6 - 0 . 0 0 4 - 0 . 0 0 2 0.000 tW= 1 . 5 n m tW= 4 . 5 n m tC o = 0 . 7 n m tW= 0 . 6 n m N o r m a l i z e d X M C D - 0 . 0 0 2 0.000 0.002 tC o = 0 . 7 n m C o / A l 2O3 N P s - 0 . 0 0 4 - 0 . 0 0 2 0.000 tW= 1 . 5 n m tC o = 1 . 0 n m tC o = 0 . 7 n m 0 1 0 2 0 3 0 4 0 5 0 - 0 . 0 0 2 0.000 B u l k C o 3W a l l o y E - E 0 ( e V ) ( a ) ( b ) ( c ) ( d ) C B A Figure 3.1: XMCD spectra at the Co Kedge for (a) Al2O3capped Co NPs, (b) Co-W NPs asample series, (c) Co-W NPs bsample series, and (d) bulk Co3W alloy.
3.1. XANES and XMCD measurements 73 mixing is only possible via the neighboring Co atoms [126]. In the Co-W alloys (Fig. 3.1(b) to (d)), with a hexagonal local structure, this signal originates at the intra-atomic exchange interaction between the 4pand 3dbands in Co. The sign of the XMCD signal in all cases is the same as in Ref. [127], indicating an antiferromagnetic coupling between 4pand 3dlevels in Co. Visible differences are observed in the Co Kedge XMCD spectra of the Co-W NPs with respect to that of Al2O3capped (see Fig. 3.1(a)); however, they are very similar to that of the Co3W alloy (Fig. 3.1(d)). The dichroic signal in the Al2O3capped Co NPs consists of a negative one-peak structure between 5 and 10 eV above the edge (marked in Fig. 3.1(a) as peak A), followed by a positive large bump between 10 eV and 30 eV (denoted in Fig. 3.1(a) as peak B), similar to what is observed in metallic Co [126] and other metal capped Co NPs [11]. Instead, in our Co-W NPs (Fig. 3.1(b) and (c)) and in the Co3W alloy (Fig. 3.1(d)) the broad negative peak A is split, giving rise to a double-peak structure formed by a trace of peak A and an additional negative peak, tagged as C in Fig. 3.1(d). This peak C is more pronounced in the XMCD signal of the bulk Co3W alloy. A similar shape of Co Kedge XMCD signal has been observed by Rueff et al. [126] in LaCo5alloys, where they discussed the effect of the rare earth on the Co KXMCD signal shape. They ascribe this extra feature in the negative peak to a contribution of the La dempty states. Then, we may conjecture that this splitting in the Co-W systems is due to the W 5dstates in the Co-W alloy. 3.1.2 W L2,3edges results XANES spectra recorded at the W L2,3were normalized as L3/L2to 2.19/1, according to Ref. [128]. Spectra measured for the Co-W NPs are shown in Fig. 3.2(a), along with the one for a metallic W foil. XANES of the bulk Co3W alloy is plotted in Fig. 3.3(a). Changes in the absorption white-line at W L2,3edges for the Co-W NPs are observed and reflect variation of the available states of 5dcharacter. Specifically, L3absorption edge appears for transitions from 2pto both 5d3/2and 5d5/2, while L2reveals only transitions from 2pto 5d3/2band. A qualitative analysis of this variation was described in section 2.2.2. We observed that an increase in the Co/W ratio in the Co-W NPs samples gave rise to an increase in the number of W 5dempty states, nW h; i.e., there is an electron transfer from W toward Co. The change in nW hfor each sample may be quantified by analysis of the W L2,3XANES spectra. The integral of the white line at the L2,3edges of each sample, rCo−W, and that for W foil, rWfoil, are defined as the sum of the individual L2and L3integrals, IL2 and IL3, respectively, calculated by first subtracting the continuum from each XANES. The continuum is artificially represented by a double-step function.
74 Chapter 3. Breakdown of Hund’s third rule in amorphous Co-W alloy NPs 10200 10250 11550 11600 - 0 . 0 0 5 0.000 0.005 0.010 P h o t o n E n e r g y ( e V ) L2 L3 N o r m a l i z e d X M C D tC o = 1 . 0 n m tW = 1 . 5 n m - 0 . 0 3 0 . 0 0 0 . 0 3 0 . 0 6 q X M C D I n t e g r a l p mW L/ m W S = 0 . 0 7 ( 4 ) - 0 . 0 0 5 0.000 0.005 0.010 L2 L3 N o r m a l i z e d X M C D - 0 . 0 3 0 . 0 0 0 . 0 3 0 . 0 6 X M C D I n t e g r a l pq mW L/ m W S = 0 . 1 3 ( 5 ) tC o = 0 . 7 n m tW = 0 . 6 n m - 0 . 0 0 5 0.000 0.005 0.010 p L2 L3 N o r m a l i z e d X M C D q mW L/ m W S = 0 . 1 2 ( 5 ) tC o = 0 . 7 n m tW = 1 . 5 n m - 0 . 0 3 0 . 0 0 0 . 0 3 0 . 0 6 X M C D I n t e g r a l 0 . 5 1 . 0 1 . 5 2 . 0 2 . 5 3 . 0 tC o = 0 . 7 n m tW= 0 . 6 n m tC o = 0 . 7 n m tW= 1 . 5 n m L2 L3 N o r m a l iz e d X A N E S tC o = 1 . 0 n m tW= 1 . 5 n m W F o i l ( d ) ( b ) ( c ) ( a ) Figure 3.2: (a) XANES spectra at the W L2,3for the Co-W NPs, and for a W reference foil. (b) to (d) show normalized XMCD signal and XMCD integral for each Co-W alloy NPs sample at the W L2,3measured at H= 10 kOe. Arrows indicate the energy at which pand qintegrals were determined.
3.1. XANES and XMCD measurements 75 0 1 2 3B u l k C o 3W a l l o y N o r m a l i z e d X A N E S L3L2 ( a ) 10200 10250 11550 11600 - 0 . 0 1 0 . 0 0 0 . 0 1 q P h o t o n E n e r g y ( e V ) N o r m a l i z e d X M C D p mL/ m S= 0 . 1 8 ( 2 ) - 0 . 0 5 0 . 0 0 0 . 0 5 ( b ) X M C D I n t e g r a l Figure 3.3: (a) XANES spectra and (b) XMCD signal and XMCD integral at the W L2,3for the Co3W alloy measured at H= 50 kOe and T= 10 K. Arrows indicate the energy at which pand qintegrals were determined. This double - step approach is extensively used for the 3dFM metals, and its accuracy in the case of W has been previously estimated to be about 94%, given its relative large white line intensity [120]. Then, assuming that for metallic W nW,foil h= 5.7 holes [120], we estimate a scaling factor C−1=nW,foil h/rW,foil = 0.1936 holes/eV. Finally, the number of holes for each Co-W sample can be calculated as nW h=C−1rCo−W. Results for these calculations for both the Co-W alloy NPs and the bulk Co3W alloy are listed in table 3.1. From these values we observe that the number of holes in W in the Co-W alloy NPs slightly increases with respect to that in metallic W, and to that found for the bulk Co3W alloy, due to hybridization of the 5dband in W with the 3dband in Co. Moreover, we notice a further increase in nW hwhen the amount of Co in the sample increases, and when tWdecreases. This means that the electronic transfer from the 5d band in W to the 3dband in Co depends on the Co/W proportion in the samples. For the Co3W alloy a slight increase in nW hwith respect to the value of metallic W is also observed. The ratio between the unoccupied states in the 5d5/2and 5d3/2bands in W, n5/2 h/n3/2 h, may be evaluated from the branching ratio IL3/IL2, following the analysis described in Ref. [129]. The results of n5/2 h/n3/2 hfor the Co-W NPs and the bulk Co3W alloy are given in table 3.1. Similar to nW h, we observe that this ratio varies depending on the Co/W proportion in the sample; i.e.,
76 Chapter 3. Breakdown of Hund’s third rule in amorphous Co-W alloy NPs Table 3.1: Values of xin the Co1−xWxalloy (values extracted from table 2.3), nW h, n5/2 h/n3/2 hratio, and mL/mSratio as calculated from the XMCD sum rules for the Co-W NPs samples in the present study and the bulk Co3W alloy. nW h= 5.7 holes for metallic W [120]. Sample x nW hn5/2 h/n3/2 hmL/mS Co-W NPs tCo (nm) tW(nm) 1.0 1.5 14.1(4) 6.09(3) 0.50(1) 0.07(4) 0.7 0.6 18.2(4) 6.06(5) 0.52(1) 0.13(5) 0.7 1.5 18.8(4) 6.00(5) 0.54(1) 0.12(5) Bulk Co3W 25(1) 5.85(2) 0.59(1) 0.18(5) Calc. Co3W 25 5.96(2) 0.57(2) 0.10(1) n5/2 h/n3/2 hincreases when the Co/W ratio decreases, being highest for the bulk Co3W alloy. XMCD signals at the W L2,3on each sample were normalized according to factors obtained from XANES normalization. Figures 3.2(b) to 3.2(d) show XMCD signals for each Co-W NPs sample, and Fig. 3.3(b) for the Co3W alloy. The XMCD integrals at L3and L2,3edges, defined as pand q, respectively, are also shown. The existence of a XMCD signal at W L2,3evidences the presence of an induced magnetic moment in the W atoms by the magnetic Co atoms in the Co-W alloy NPs and the Co3W alloy. According to the direction of the applied magnetic field, and considering that the L3XMCD signal is mostly positive, while the L2XMCD is negative, we can determine that the induced W magnetic moment orients opposite to the direction of the field. Consequently, W induced moments are antiparallel to the Co magnetic moments deduced for the Co-W NPs in section 2.3.3. This is consistent with the general trend in all transition metal series with the ndband filling: W has a less than half filled 5dband, which results in antiparallel coupling of its induced moment with that of the magnetic 3dmetal [120, 123]. Values of pand qwere used to calculate the orbital to spin moment ratio, mL/mS, in the induced magnetic moments in W by applying the magnetooptical sum rules [64, 65]. We have followed the symbol and sign criteria used in Ref. [66], so that the effective spin moment obtained from the sum rules is expressed as mSeff =mS+mD, where mDrepresents the dipolar term, proportional to the expectation value of the magnetic dipole operator hTzi. Thus, in order to determine mS, one has to consider the hTzivalue. For alloys with a non-cubic structure, like the hcp Co3W alloy, hTzimight have a maximum value of hSzi/3, corresponding to the Lorentz local field at the
3.3. Discussion 83 1 . 8 2 . 0 2 . 2 0 . 0 0 . 1 0 . 2 0 . 3 Co-W NPs Bulk Co3W alloy mL/ m S Co-W distance (Å) 1 5 2 0 2 5 Co-W NPs Bulk Co3W alloy x in Co1-xWx (% at) XMCD vs. EXAFS results for Co-W NPs and Co3W (b)(a) Figure 3.7: mL/mSratio as calculated from the W L2,3XMCD signal for the Co-W alloy NPs and for the bulk Co3W alloy, as a function of (a) the first Co-W interatomic distance obtained from EXAFS, and (b) the composition of the Co-W alloy in the samples. Dashed lines: guide to the eye. distance resulting from EXAFS analysis on the same samples. mL/mSis found to increase as the Co-W distance shortens. This trend agrees well with the one observed for calculated mL/mSversus αin Zr in the Co(Fe)-Zr alloys in Ref. [123]. In the same study, Kapaklis et al. claim that the crystallinity of the materials is determinant in the breakdown of Hund’s third rule since Zr induced moments in crystalline FeZrPt and CoZrPt alloys are found to fulfill the rule. In contrast, our observations of the breakdown of the rule on the polycrystalline bulk Co3W, both experimentally and theoretically, demonstrate that the disorder level in the sample is not its main cause; instead, the reduction of the interatomic distances between dissimilar atoms seems to be the crucial point on this very controversial topic. The Co influence on the orbital moment of W atoms in the samples may also be examined as a function of the Co/W in the alloy. In fact, mL/mSis found to scale with the W concentration in the Co-W alloy, as observed in Fig. 3.7(b). As it was described in section 3.1.2, this may be understood as an increase of the induced orbital component of the W magnetic moment as the Co/W proportion on the alloy decreases. A similar trend was observed for the mL/mSinduced in Ir in Co-Ir disordered alloys, where Hund’s third rule is also not fulfilled [70].
84 Chapter 3. Breakdown of Hund’s third rule in amorphous Co-W alloy NPs 3.4 Conclusion In all the Co-W alloy samples studied, i.e., Co-W alloy NPs and polycrystalline bulk Co3W alloy, the induced W orbital moment orients parallel to its spin moment, contrary to the prediction of Hund’s third rule for W. This breakdown has been proven by experimental and simulated XANES spectra and XMCD signals at the Co Kand W L2,3edges. Consequently, we demonstrate that W not only affects the local structure of Co NPs, but also their electronic structure. The Co 3d−W 5dhybridization is evidenced and becomes a key factor in the breakdown of this rule in the case of induced moments. Our comparison between XMCD and EXAFS results demonstrate that the influence of the Co- W spin-orbit coupling depends on the average Co-W interatomic distance, as consequence of the dependence of the strength of the hybridization. Contrary to the differences found for crystalline and amorphous Co(Fe)-Zr alloys in Ref. [123], we observe the breakdown of Hund’s third rule in both amorphous and polycrystalline Co-W systems, which suggests that this behavior is not a general behavior, but depends on the studied material and its local structure. It is worth noting that this is the pioneer observation of the breakdown of this rule on a nanoparticulated system.
Chapter 4 Structural and magnetic properties of Co-Pt nanoparticles In this section, we describe the structural and magnetic characterization performed on the Pt-capped Co-nanoparticles system. We examine the role of Co-Pt alloying in the origin and enhancement of the magnetic anisotropy in these NPs. In fact, the production of Co-Pt alloys is one of the preferred routes currently used in nanoparticles and thin films to increase their magnetic anisotropy [22, 138]. This results from the crystallization of Co-Pt alloys in the chemically ordered L10phase, which has a very high magnetocrystalline anisotropy for the bulk [23]. Moreover, many Co-Pt alloy thin films [139–142] and assembled nanoparticles systems [22, 30, 31, 138] show perpendicular magnetic anisotropy (PMA): a property which favors the easy axis of magnetization along the film normal direction. Most of these Co-Pt systems are either produced at high temperatures or annealed in order to favor the crystallization of the Co-Pt alloy in the above mentioned ordered L10phase. However, the origin of PMA in CoPt alloy systems deposited at room temperature, as in the case of the Co-Pt NPs we describe in this chapter, remains controversial [142]. Previous studies on Co-Pt alloy nanostructured systems have demonstrated the importance of a complete investigation of both the local atomic environment and their long range order to clarify the correlation between crystallographic structure and magnetic anisotropy [142]. Therefore, we have performed a systematic analysis of the structural and magnetic properties of Co- Pt NPs prepared by sequential sputtering deposition of Al2O3, Co and Pt on
88 Chapter 4. Structural and magnetic properties of Co-Pt NPs a Si substrate. The morphology and structure of the Co-Pt NPs are studied by high-resolution transmission electron microscopy (HRTEM) and extended X-ray absorption fine structure (EXAFS) measurements, with which we prove the presence of Co-Pt alloy in all samples, as it was described for the Co- W alloy NPs. However, contrary to the amorphous structure observed for the Co-W NPs, the Co-Pt alloy NPs consist of a self-organized system of crystalline particles. Their fascinating properties of strong perpendicular magnetic anisotropy are described, as observed by conventional SQUID magnetometry measured with the applied magnetic field parallel and perpendicular to the substrate plane. Their magnetic properties are also explored by anomalous Hall effect (AHE) and X-ray magnetic circular dichroism (XMCD). This work allows to have a better understanding the origin of PMA in these Co-Pt NPs. 4.1 Samples studied The samples studied in this chapter consist in Pt-capped Co-nanoparticles prepared by Dr. Cyrile Deranlot and Dr. Frederic Petroff at the Unit´e Mixte de Physique CNRS-Thales1in Palaiseau, France, by sequential sputtering deposition of Al2O3, Co and Pt on a Si substrate. The preparation procedure is the same as that previously described for the Co-W NPs in section 2.1, and illustrated in Fig. 2.1, using Pt instead of W in this case. We end up with a multilayer system, following the formula Al2O3/(Al2O3/Co/Pt)N/Al2O3, with N being the number of repetitions of the Al2O3, Co and Pt trilayer deposition. The characterization of the Co-Pt NPs that we describe in this chapter has been performed on samples with a fixed tCo = 0.7 nm, varying tPt = 0.6, 1.5, 4.5 and 6.0 nm, and N=25 in all cases. Let us recall that the Al2O3layer thickness is 3 nm in each trilayer, and 5 nm in the one deposited at the end of the process for protection purposes. 4.2 Morphological and structural study 4.2.1 Microscopy Measurements The morphology of the Co-Pt NPs samples has been studied by HRTEM and high angle annular dark field (HAADF) scanning transmission electron microscopy (STEM) measurements, performed by Dr. Luisa Ruiz Gonz´alez and Dr. Jos´e Mar´ıa Gonz´alez-Calbet of the Departamento de Qu´ımica Inorg´anica 1http://www.trt.thalesgroup.com/ump-cnrs-thales/
4.2. Morphological and structural study 89 in the Universidad Complutense de Madrid.2HRTEM images were taken in both cross section and plan view configurations, in a JEOL JEM 3000 F Field Emission Microscope fitted with an Oxford LINK Electron Dispersive Spectrometry (EDS) analyzer. Low magnification studies in cross section configuration for all four samples confirmed the presence of 25 layers in agreement to the nominal layer preparation. HRTEM images, shown in Fig. 4.1, and EDS analysis indicate that light gray layers correspond to the amorphous alumina and darker layers to the Co and Pt metals, similarly to the case of Co-W NPs described in section 2.2. In contrast to the Co-W NPs case, crystallinity in the Co-Pt NPs is observed in all four samples studied by HRTEM. Each metallic layer is about 2.3, 2.5, 5.5 and 6.7 nm thick, for the samples with tPt = 0.6, 1.5, 4.5 and 6.0 nm, respectively. In the samples with the lowest amount of Pt (tPt = 0.6 and 1.5 nm) there 200 111 (b) (d) 200 111 (c) (a) 200 111 200 111 Figure 4.1: HRTEM images in cross section configuration for samples from with tCo = 0.7 nm and (a) tPt = 0.6 nm, (b) tPt = 1.5 nm, (c) tPt = 4.5 nm and (d) tPt = 6.0 nm. Fourier transforms (FFTs) at selected zones of the images are shown. A Co-Pt particle is highlighted in (a) and (b). Pt NPs are marked in (c) and (d). 2http://www.cnme.es/
90 Chapter 4. Structural and magnetic properties of Co-Pt NPs are some signs of particulated morphology, as in the region surrounded by a white ellipse in Figs. 4.1(a) and 4.1(b). Some darker shadows inside the layers indicate the presence of Co, located at the center of the layer, suggesting that the capping Pt tends to surround the Co particle. For the other two samples (tPt = 4.5 and 6.0 nm), however, the Co-Pt nanoparticles are not easy to be identified from the images obtained in cross section configuration. Fast Fourier transform (FFT) performed on selected areas of the images shows spots that are well indexed with the interplanar distances of a fcc cell in all cases (see insets in Fig. 4.1). In Figs. 4.1(a) and 4.1(c) the periodicity found in the selected zone of the image is 0.22-0.23 nm, which is characteristic of the (1 1 1) planes of a fcc Pt structure. In Fig. 4.1(c) and 4.1(d) some small crystalline clusters in the alumina region of the samples are observed (see circled particles in the figures), which have been identified as Pt clusters with fcc structure, ranging between 2 and 3 nm in diameter. Improved contrast to better identify the Co-Pt particles is obtained by plan view STEM images, such as the one shown for the sample with tCo = 0.7 nm and tPt = 0.6 nm in Fig. 4.2(a). In this image, brighter parts correspond to Co-Pt NPs, and darker parts to Al2O3. The image obtained is comparable to those of similar systems of metallic nanoparticles embedded in insulator matrices [93], and the shape of the particles is similar to that of Co-nanoparticles embedded in alumina [94], and to the one found for the Co-W NPs (see section 2.2.1). The average diameter of the Co-Pt NPs from the image in Fig. 4.2(a) was (a) (b) Figure 4.2: STEM images in plan view configuration for the samples with tCo = 0.7 nm, and (a) tPt = 0.6 nm and (b) tPt = 1.5 nm.
4.2. Morphological and structural study 91 4.1(2) nm. STEM images for the other three samples (those with tPt = 1.5, 4.5 and 6.0 nm) did not allowed identification of the Co-Pt particles since they revealed an almost uniform Pt capping, as shown in Fig. 4.2(b) for the sample with tPt = 1.5 nm. 4.2.2 XANES and EXAFS measurements X-ray absorption (XAS) and EXAFS spectra for the Co-Pt NPs samples with tCo = 0.7 nm and tPt = 0.6, 1.5, 4.5 and 6.0 nm were measured at the Co K (7709 eV) and Pt L3(11564 eV) edges using a double-crystal Si(111) monocromator in the BM29 beamline at the European Synchrotron Radiation Facility (ESRF). Measurements were performed at 300 K in fluorescence detection mode with a 13-element Ge solid state detector with digital signal processing for fluorescence XAS, high energy resolution and high count rate. Reference samples were also measured at different edges: Co particles embedded in alumina matrix (referred in the following as “bare Co NPs”) and the Co metallic foil measured at the Co Kedge; and Pt metallic foil measured at the Pt L3 edge. For each edge measured on each sample, four spectra were taken in order to have enough statistics in data treatment, following a 4 s/point count. The X-ray absorption spectra were analyzed following standard procedures. A preliminary reduction of the EXAFS raw data involving background removal of the absorption data µ(E), conversion of µ(E) to χ(k), normalization and weighting scheme were performed with AUTOBK and ATHENA, programs from the simulation package IFEFFIT [96]. EXAFS data analysis and fitting were performed on all reference and samples at their respective edges. All spectra were fitted using the ARTEMIS program from the same IFEFFIT package using models based on crystallographic information found in the ICSD3database. Atomic clusters used to generate the scattering paths for fitting were generated with ATOMS, a tool from the same simulation package [97]. Co Kedge Normalized X-ray absorption near edge structure (XANES) spectra at the Co Kedge for Co-Pt NPs with tCo = 0.7 nm and tPt = 0.6, 1.5, 4.5 and 6.0 nm are shown in Fig. 4.3, along with the Co foil XANES, plotted for reference. Changes in the intensity and shape of the pre-edge peak and the white line (denoted as peak I and peak II, respectively, in Fig. 4.3) are appreciable and reflect changes in the electronic structure of the Co (elec- 3http://icsd.iqfr.csic.es/icsd/
92 Chapter 4. Structural and magnetic properties of Co-Pt NPs 7680 7720 7760 7800 0 . 0 0 . 2 0 . 4 0 . 6 0 . 8 1 . 0 1 . 2 tC o = 0 . 7 n m C o F o i l tP t = 0 . 6 n m tP t = 1 . 5 n m tP t = 4 . 5 n m tP t = 6 . 0 n m N o r m a l i z e d X A N E S P h o t o n E n e r g y ( e V ) P e a k I P e a k I I 0 1 2 3 4 5 6 - 1 0 1 2 P e a k I ∆A o f p e a k ( e V ) tP t ( n m ) P e a k I I Figure 4.3: XANES at the Co Kedge for the Co-Pt NPs and comparison with that of a Co foil for reference. Inset: Variation of the areas of peak I and peak II in the figure as a function of tPt. tron configuration [Ar]3d74s2) and Pt (electron configuration [Xe]4f145d96s1) atoms. Analogous to the analysis of such variation described for the Co K edge XANES in the Co-W NPs, we calculate the difference of the peaks areas (∆A = REf Ei(µsample −µCo-foil)dE). The inset of Fig. 4.3 represents the ∆A as a function of the Pt content in the samples. The integration limits were 7706.1−7717.6 eV for peak I, and 7717.6−7735.1 eV for peak II. Let us recall that the Co Kedge white line reflects the 4pempty states of Co near the Fermi energy. Variation of peak I mainly determines changes of the 3dcharacter of unoccupied states, which is influenced by Co 4p−3d hybridization. The reduction of the intensity of peak I in the Co-Pt NPs with respect to that of the Co foil, also observed for the in Co-W NPs case, reveals a delocalization of the Co 3dempty states, and is a proof of Co 4p−3d−Pt 5dhybridization. The intensity of peak II depends on both the number of available 4pstates, and the structure of the system. It is evident that the intensity of this peak II is higher and its shape different from that of the Co foil. Indeed, it looks closer to those recorded for Co-Pt alloys in Ref. [143], which may be an indication of presence of such kind of alloys in our Co-Pt particles. In any case, it is clear that the 4pempty states in the Co-Pt NPs samples increase, compared to those of the bulk Co. Both peak I and peak II are practically constant along the Co-Pt samples series (see inset of Fig. 4.3(a)), reflecting that Co 3d−Pt 5dhybridization is not affected by such variations in the amount of Pt for a fixed Co content. Similarly to the Co-W NPs case, this fact strongly suggests that the alloy
4.3. Magnetic study 99 function of the applied field, M(H), and as a function of temperature, M(T), were measured in two configurations: (1) with the field applied parallel, and (2) perpendicular to the substrate plane. The dc susceptibility measurements curves measured with a bias field of Hdc = 200 Oe, in both configurations, for the samples series with tCo = 0.7 nm, tPt = 1.5, 4.5 and 6 nm, and N= 25 are plotted in the left panel of Fig. 4.7. The shape of the curves is very different to that found for the bare Co NPs of the same tCo = 0.7 nm, which show the typical ZFC-FC curve of a superparamagnetic system with a blocking temperature TB= 27 K [18]. In the case of the Co-Pt NPs, the ZFC and FC curves measured in the parallel direction overlap even for fields as high as 50 kOe, showing a maximum at the freezing temperature Tf=365, 340 and 296 K for the samples with tPt = 1.5, 4.5 and 6 nm, respectively. The same cusp is observed in ac susceptibility data, measured with a 4 Oe exciting field. Between 0.1 and 50 Hz, these data show no dependence on frequency, therefore, the analysis of the magnetic anisotropy performed in section 2.3 from ac susceptibility measurements was not possible for these Co-Pt NPs. In all samples, increasing of the the external applied field Hdc shifts Tfto lower temperatures till the maximum is flattened and all the particles become fully polarized along Hdc, as observed in the right panel of Fig. 4.7. The dependence of Tfwith Hdc is a monotonously decreasing function M(Tf, H), as shown in Fig. 4.7. In contrast, the ZFC-FC curves measured in the perpendicular configuration show no overlapping as the temperature increases till it reaches Tf. For the ZFC curve, an increase of the magnetization with temperature is observed until T1≈140 K for the three samples in the series, which corresponds to the first shoulder observed in the curves in Fig. 4.7(a) to 4.7(c). Above T1, the particles follow a collective ferromagnetic behavior up to Tf, where both ZFC and FC curves decrease again, following a Curie-Weiss law. The M(H) were measured for all samples with both configurations at several temperatures. Fig. 4.8 shows the data recorded at 5 K. At low temperatures the hysteresis curves measured in the perpendicular direction are rather square, which indicates the presence of a ferromagnetic hard component, with a quite high coercive field of HC= 4, 3 and 1.9 kOe for the samples with tPt = 1.5, 4.5 and 6 nm, respectively, at T= 5 K. Such a ferromagnetic behavior implies that the Co-Pt particles are strongly coupled. In addition to the main reversal of the magnetization close to HC, the hysteresis curves measured at low temperatures in the perpendicular direction have a slight step near H= 0, which indicates that there is a magnetically soft component present in the sample.
100 Chapter 4. Structural and magnetic properties of Co-Pt NPs 0100 200 300 400 0.0 0.5 1.0 1.5 2.0 2.5 3.0 T(K) ZFC/FC substrate FC ⊥ substrate ZFC ⊥ substrate t Pt = 6.0 nm T f 0 1 2 3 4 5 6 0.5 1.0 1.5 2.0 2.5 3.0 χ (emu/cm 3 .Co) ZFC substrate FC ⊥ substrate ZFC ⊥ substrate t Pt = 4.5 nm T f 1 2 3 4 5 6 χ (emu/cm 3 .Co) 0.5 1.0 1.5 2.0 2.5 3.0 ZFC/FC substrate FC ⊥ substrate ZFC ⊥ substrate t Pt = 1.5 nm T f 1 2 3 4 5 6 (a) (c) (b) 0.4 0.8 1.2 1.6 2.0 M (µB/Co) 2.5 kOe t Pt = 4.5 nm 50 kOe 1 kOe 0.1 kOe 10 kOe 20 kOe 5 kOe 0.5 kOe 0.4 0.8 1.2 1.6 2.0 tPt= 1.5 nm 2.5 kOe 1 kOe 0.1 kOe 10 kOe 20 kOe 5 kOe 0100 200 300 400 0.0 0.4 0.8 1.2 1.6 2.0 T(K) t Pt = 6 nm 2.5 kOe 50 kOe 1 kOe 0.1 kOe 10 kOe 20 kOe 5 kOe 0.5 kOe (d) (f) (e) T1 T1 T1 Figure 4.7: (left panel) DC susceptibility curves measured under an applied field of Hdc = 200 Oe perpendicular and parallel to the substrate plane, and (right panel) M(T) at various fields applied in the parallel direction, (H, indicated beside each curve) for samples with tCo = 0.7, N= 25, and tPt = 1.5 nm in (a) and (d), tPt = 4.5 nm in (b) and (e), and tPt = 6 nm in (c) and (f) . (- -) M(Tf, H), superparamagneticcorrelated phase separation line. The coercive field measured in the perpendicular direction decreases with temperature till it disappears at about 200 K for all samples in the series, as shown in Fig. 4.9. HCalso decreases as tPt in the sample increases, except for some temperatures near 100 K, where HCmeasured for the sample with tPt = 6 nm is higher than that of the sample with tPt = 4.5 nm. This, in principle, unusual behavior has also been reported for Co/Pt multilayers where an oscillatory dependence of HCwith tPt and Nis observed, and has been ascribed to RKKY interactions between the Co layers through Pt [147]. There is an interesting feature in the hysteresis curve of the sample with tPt = 6 nm measured in the perpendicular configuration (Fig. 4.8(c)). In the
4.3. Magnetic study 101 -2 -1 0 1 2 t Pt =1.5 nm H substrate H⊥ substrate -1 0 1 M(µ B /Co) t Pt =4.5 nm H ⊥ substrate H substrate -20 -10 010 20 -2 -1 0 1 2 t Pt=6 nm H (kOe) H ⊥ substrate H substrate (a) (c) (b) Figure 4.8: Hysteresis loops measured at T= 5 K and Hdc perpendicular (N) and parallel () to the substrate, for the samples with tCo = 0.7 nm, N= 25, and (a) tPt = 1.5 nm, (b) tPt = 4.5 nm, and (c) tPt = 6 nm.
102 Chapter 4. Structural and magnetic properties of Co-Pt NPs 0 100 200 300 400 0 1 2 3 4 tP t = 1 . 5 n m tP t = 4 . 5 n m tP t = 6 . 0 n m HC ( k O e ) T ( K ) tC o = 0 . 7 n m N = 2 5 Figure 4.9: Temperature dependence of the coercive field measured with Hdc applied perpendicular to the substrate plane for the samples with tCo = 0.7 nm, N= 25, and (a) (N)tPt = 1.5 nm, (b) (F)tPt = 4.5 nm and (b)(•)tPt = 6 nm. first and third quadrants, the magnetization reversal in this sample apparently proceeds layer by layer. The last layer magnetization reversal involves a variation of ∆Ms/Ms= 1/12.1, where Msis the saturation moment. Indeed, if each layer contributes M1=Ms/25 to the total magnetization, the reversal of the magnetization of one layer will imply a moment difference of twice this quantity. In the direction parallel to the substrate plane the coercive field is much lower, being 0.85, 0.46 and 0.15 kOe for samples with tPt = 1.5, 4.5 and 6 nm, respectively, at 5 K (see Fig. 4.8). Such differences between the magnetization curves measured in orthogonal directions (with the bias field applied parallel and perpendicular to the substrate plane) evidence the presence of perpendicular magnetic anisotropy (PMA) in the Co-Pt samples. The easy magnetization direction has been identified to be the one perpendicular to the substrate, as observed in different Co-Pt multilayer systems [148–151], CoxPt1−xalloy films [139–142] and Co-Pt NPs systems [30, 31]. Above Tfthe M(H) curves measured in both configurations have the characteristic superparamagnetic behavior, which can be fitted to a Langevin curve of the nominal Co-Pt particle average diameter [152], following a procedure analogous to the one described in section 2.3.1.
4.3. Magnetic study 103 4.3.2 Anomalous Hall Effect magnetometry The anomalous Hall effect (AHE) measurement technique is a method frequently used to study the magnetic properties of thin films exhibiting PMA. Measurements of AHE in ferromagnetic granular systems has demonstrated its sensitivity to the local magnetic moments of individual nano-particles [153], so that hysteresis is developed in the Hall voltage versus applied field curve below the blocking temperature of magnetic particles. Thus, by measuring the variation of the hall voltage VHwith the magnetic field applied in the direction perpendicular to the substrate of our Co-Pt NPs samples, hysteresis loops comparable with those of SQUID magnetometry can be obtained. AHE measurements were performed on two of the Co-Pt NPs samples, those with tCo = 0.7 nm, and tPt = 1.5 and 6.0 nm. These measurements were carried out by Dr. Jolanta Stankiewicz in an electrical transport setup of - 2 0 - 1 0 0 1 0 2 0 - 0 . 2 - 0 . 1 0 . 0 0 . 1 0 . 2 M ( a . u . ) H ( k O e ) tC o = 0 . 7 n m tP t = 6 . 0 n m N = 2 5 T = 5 K ( b ) - 0 . 2 0 . 0 0 . 2 0 . 4 tC o = 0 . 7 n m tP t = 1 . 5 n m N = 2 5 T = 5 K M ( a . u . ) ( a ) 0246 0 . 0 0 . 1 Figure 4.10: AHE hysteresis loops measured at T= 5 K and Hdc perpendicular to the substrate for the samples with tCo = 0.7 nm, N= 25, and (a) tPt = 1.5 nm and (b) tPt = 6 nm. Inset in (b): details of the first quadrant of the hysteresis loop in (b).
104 Chapter 4. Structural and magnetic properties of Co-Pt NPs 0 50 100 150 200 250 300 0 1 2 3 4 S Q U I D A H E HC ( k O e ) T ( K ) Figure 4.11: Comparison of the HCvs. Tobtained by SQUID (•) and AHE (N) measurements with Hdc applied perpendicular to the substrate plane of the sample with tCo = 0.7 nm and tPt = 1.5 nm. Dashed line: guide to the eye. the Departamento de f´ısica de la materia condensada and Instituto de Ciencia de Materiales de Arag´on (ICMA), CSIC - Universidad de Zaragoza, and in a Quantum Design Physical Property Measurement System (PPMS) of the Servicio de medidas f´ısicas of the Universidad de Zaragoza.6The measurement configuration is that shown in Fig. 1.3 of section 1.3, with the four contacts placed at the edges of the rectangular samples. The magnetic field was varied within H=±20 kOe, and applied in the direction perpendicular the substrate. VHvs. Hloops were collected at several temperatures from 2 K to 300 K. In Fig. 4.10 we have plotted those M(H) obtained for the two Co- Pt samples at T= 5 K. These curves show a remarkable squareness and the coercive field coincides well with the one obtained by SQUID magnetometry (see Fig. 4.8). However, the soft component observed in the curves measured in the SQUID magnetometer is not detected by AHE, which instead seems to be very sensitive to the hard component. The HCvalues and their temperature dependence obtained by this method perfectly match those observed by SQUID magnetometry in Fig. 4.9, as observed in the direct comparison of HC vs. Tfor both techniques depicted in Fig. 4.11. AHE measurements also allow to examine the magnetization reversal mechanisms in our granular films. The inset of Fig. 4.10(b) reveals details of the switching of magnetization in the sample with tPt = 6.0 nm, which is consistent with the layer by layer reversing described in the previous section for the same sample. 6http://sai.unizar.es/medidas/index.html
4.3. Magnetic study 105 4.3.3 X-ray Magnetic Circular Dichroism magnetometry XANES and XMCD measurements at the Co K(7709 eV), Pt L3(11564 eV) and Pt L2(13273 eV) edges on the Co-Pt NPs sample with tCo = 0.7 nm and tPt = 1.5 nm were performed at the ESRF ID12 beamline. The APPLEII undulator and a double - Si - (111) - crystal monocromator were used to collect the spectra at the respective energies. XANES spectra were recorded by a fluorescence detector in backscattering geometry. Polarization of the circular light was over 90% in these cases. XANES and XMCD experiments at he Co L3(778.1 eV) and Co L2(793.2 eV) edges on the same Co-Pt NPs sample were performed at the ID08 beamline of the ESRF. An APPLE-II undulator and a spherical grating monochromator were used in this case. The degree of polarization at these Co L2,3edges was ∼100% and the total electron yield (TEY) detection method was employed. The XMCD signal at each edge was obtained by applying a magnetic field of 10 kOe along the X-ray beam direction, at a temperature of 10 K. This field and temperature were chosen according to the magnetic properties of the Co- Pt NPs, so that the system was reaching its magnetic saturation under these conditions (see section 4.3.1). XMCD was obtained by differences of XANES spectra measured with opposite helicities of the light at a fixed magnetic field value, orienting the field in two inverse directions. Co Kedge results XANES and XMCD at the Co Kedge probes the 4pempty states of the Co atom in the sample. Analysis of the XANES spectra recorded at this edge on these Co-Pt alloy NPs samples was described in section 4.2.2. Evidences of Co 4p−3dand Co 3d−Pt 5dhybridization in the Co-Pt particles and electronic transfer from Pt 5dto Co orbitals were then observed. As described for the XMCD at the Co Kedge in the Co-W NPs (section 3.1.1), the detection of a nonzero XMCD signal at this edge reflects the magnetic polarization of the Co 4pband caused by the intra-atomic exchange interaction with the 3dband. The XMCD signal recorded at this edge for the Co-Pt NPs sample is shown in Fig. 4.12, normalized to the absorption jump obtained in the Co KXAS spectrum after background removal. It has the same sign as the Co KXMCD of the Co-W NPs (see section 3.1.1) and as the one reported in Ref. [127], which results in an antiferromagnetic coupling between 4pand 3dlevels in Co. The shape of XMCD signal in Fig. 4.12 is indeed very similar to the one reported for ion irradiated Co-Pt films in Ref. [154]. In these Co-Pt films, changes in the electronic structure of Co atoms related to the formation of
106 Chapter 4. Structural and magnetic properties of Co-Pt NPs 7700 7720 7740 7760 - 0 . 6 0 . 0 0 . 6 1 . 2 P h o t o n e n e r g y ( e V ) N o r m a l i z e d X A S - 0 . 0 0 2 0.000 0.002 0.004 C o - P t N P s tC o = 0 . 7 n m tP t = 1 . 5 n m T = 1 2 K N o r m a l i z e d X M C D Figure 4.12: (a) (-) XANES spectra, and (b) () XMCD signal at the Co Kedge for the Co-Pt NPs with tCo = 0.7 nm and tPt = 1.5 nm. CoxPt1−xalloys induced by ion irradiation were observed. Striking similarities between the XMCD spectra of the Co-Pt films and a reference Co0.5Pt0.5L10 thin-film reference sample were shown, in terms of characteristic peaks at selected energies. This allowed to interpreted the XMCD spectrum for the irradiated Co-Pt film as the superposition of pure Co and L10Co0.5Pt0.5alloy contributions. Similarly, in our Co-Pt NPs we may state that the Co Kedge XMCD signal that we observe is a combination of these two phases, since we have demonstrated the existence of both by EXAFS analysis (see section 4.2.2). By comparing the amplitude of the Co Kedge XMCD curve for the Co- Pt NPs with that of Ref. [127], we have estimated the 4pCo moment to be -0.057(4) µB. This value has been reduced in about 35% with respect to that found for the Al2O3capped Co particles (m4p=−0.087 [11]). Such a reduction may be a consequence of the Co-Pt alloy present in the samples. Co L2,3edges results Figure 4.13 shows the XMCD spectrum measured at the Co L2,3for normal incidence of the X-rays. This spectrum has been normalized to the XAS shown in Fig. 4.13(a) in high energy limit, after background subtraction. As described in previous chapters, in order to apply the magneto-optical sum rules [64, 65] (see section 1.4.2) to the XMCD signal in Fig. 4.13(b),
4.3. Magnetic study 107 770 780 790 800 810 820 830 - 6 - 4 - 2 0 L3 L2 P h o t o n e n e r g y ( e V ) N o r m a l i z e d X M C D C o L 2 , 3 tC o = 0 . 7 n m tP t = 1 . 5 n m - 1 2 - 8 - 4 0 q X M C D i n t e g r a l p 0 2 4 6 8 N o r m a l i z e d X A S L2 L3 0 8 1 6 2 4 3 2 X A S i n t e g r a l ( a ) ( b ) Figure 4.13: Co−L2,3edges spectra of the tCo 0.7 nm, tPt = 1.5 nm sample. (a) (-) Normalized XAS spectra mean curve. (-) The double-step function used is also indicated. (- -) Integrated white line. (b) (-) Normalized XMCD spectra, (- -) integrated area. The higher limit for the p and q integrals, used for the sum rules analysis, is given in (b). the number of unoccupied states in the 3dband for Co nhis required in the calculations. Values of 3d nhreported in the literature are, for example, nh= 2.49 holes for metallic Co [108] and nh= 2.628 for Co0.5Pt0.5L10alloy films [141]. Let us recall that the Co atoms in our Co-Pt NPs are found to be in these two different environments (metallic Co and Co0.5Pt0.5L10alloy), but we are not able to quantify each of them. Therefore, the right number of 3d holes in Co atoms of our Co-Pt NPs is unknown. Thus, we have expressed the orbital and spin moments, per 3dhole in the Co atoms, as mS/nh= 0.80(1) µB,mL/nh= 0.09(1) µB, and mL/mS= 0.11(1). The spin moment mS/nh has been obtained considering that the dipolar term mDis small with respect to the total mS(see section 1.4.2).
108 Chapter 4. Structural and magnetic properties of Co-Pt NPs XMCD measurements at the Co L2,3edges on CoxPt1−xparticles prepared by vapor deposition have been recently reported [155, 156]. They find systematically larger ratios of mL/mSthan those in our Co-Pt NPs, for comparable particle sizes. In that case, the orbital to spin ratio mL/mSof Co atoms in our Co-Pt NPs is close to the value found for particles of 2.0 nm with composition close to Co3Pt [156]. With reference to other XMCD studies in Co-Pt systems, our mL/mSin Co is always larger, as compared to CoPt3films deposited on a substrate at 800 K (mL/mS= 0.09) [140], Co0.5Pt0.5L10alloy films (mL/mS= 0.063) [141], and for annealed Co0.5Pt0.5NPs with diameters of about 2.6 nm deposited on amorphous carbon matrices (mL/mS= 0.094) [22]. XMCD measurements at the Co L2,3edges as a function of incident angle (0oand 60o) were also performed, looking for anisotropy of the orbital moment. However, the results did not show clear angle dependence, which was unexpected. Pt L2,3edges results The XMCD spectra measured at the Pt L2,3edges are shown in Fig. 4.14. The non-zero values of the XMCD signal reflects the polarization of the Pt by the magnetic Co. From an XMCD experiment at the Pt L2,3edges one obtains, through the sum rules [64, 65], the spin mSand orbital mLmoments averaged over the whole sample, provided one knows by calculation or estimation the number of holes, nh, existing involved in the 2p→5dexcitations. For Pt we have derived nhfrom the white line difference with a Pt foil at the L2,3 edges XANES, similarly to the procedure followed for XANES at the W L2,3 edges in section 3.1.2. We have obtained nh= 1.80(2) holes in the 5dband, mS= 0.14(1) µB,mL= 0.027(2) µB, and mL/mS= 0.19(1) for Pt atoms in the Co-Pt NPs. The induced moment on Pt mtot = 0.16(1) µBis one order of magnitude larger than the moments induced on the Cu, Ag or Au capping cases [11]. Obviously, the reason for this difference is the proximity of Pt, with the 5d9 band, to fulfill the Stoner criterion for ferromagnetism [157], instead of the nearly filled noble metal nd10 bands (n= 3, 4 and 5 for Cu, Ag or Au, respectively). However, it is important to point out that not all Pt atoms in the Co-Pt NPs of the measured sample (tCo = 0.7 nm and tPt = 1.5 nm) are alloyed or in contact with Co atoms, as described in the HRTEM and EXAFS measurements (see section 4.2) performed in this sample. As a result, it is possible that not all Pt atoms in the sample are polarized by Co. Only those polarized Pt atoms
Chapter 5 d-band magnetism of Ag, Au, Pd and Pt nanostructured materials In this chapter we review the interesting magnetic properties of metals (M) that are not magnetic in bulk form, but when shaped in reduced dimensions. In particular, we describe the magnetic behavior of Ag, Au, Pd and Pt nanoparticles. They have in common an incompletely filled 4d- (Ag, Pd) or 5d-band (Au, Pt), that gives rise partially to this type of magnetism. By means of X-ray magnetic circular dichroism (XMCD) measurements at the Metal-L2,3 edges, the orbital and spin contributions to the magnetic moment stemming from the d-band are explored. 5.1 Magnetism in bulk metals The understanding of the magnetism of metals has attracted the attention of physicists for decades, and, as a result, very successful theories and models have been proposed to explain it. The magnetic properties of a metal in the solid state in bulk scale may be rationalized in terms of the spin-split density of states DOS. The Stoner criterion of stability with respect to ferromagnetism in metals states that long range ordering is possible only when the Stoner parameter (repulsion between electrons of opposite spin) I, times the density of states at the Fermi energy D(F) is larger than 1 [157]. As free atoms, the noble metals Ag and Au, and Pd have a full electronic dband, Ag:[Kr]4d105s1, Au:[Xe]4f145d106s1and Pd:[Kr]4d10, respectively, while Pt has a hole in the 5dorbit; Pt:[Xe]4f145d96s1. In the solid state, though,
116 Chapter 5. d-band magnetism of Ag, Au, Pd and Pt nanostructured materials Ag and Au metals have a very shallow D(F) and, correspondingly, are nonmagnetic, on one hand; Pd and Pt have a maximum in D(F) but do not fulfill the Stoner criterion and remain paramagnetic, on the other hand. This is due to the hybridization between the d-band and the sp-bands, which generates a small, albeit non-negligible number of holes, nd h, in the d-band. This parameter varies between nd h= 0.349 holes for Ag and nd h= 1.635 holes for Pt, and increases in the trend Ag<Au<Pd<Pt (see table 5.1). As a result, the four metals have a partially filled d-band. In non-magnetic metals the magnetic susceptibility response to an applied field can be explained as due to several contributions: χtotal =χdia +χLandau +χs Pauli +χSO orb +χKO orb (5.1) χdia is the diamagnetic susceptibility of the electrons in the core states, χLandau is the diamagnetic contribution due to the conduction band that splits into discrete Landau transversal orbits upon application of an external field, χs Pauli is the Pauli paramagnetism due to the spin density near the Fermi energy, χSO orb is the paramagnetic orbital component due to spin-orbit (SO) coupling, χKO orb is the Kubo-Obata paramagnetic contribution due to second order perturbation contribution of the itinerant electrons [162]. Bulk Ag and Au have an overall diamagnetic response to an applied field; i.e., the diamagnetic terms overpower the paramagnetic ones. In contrast, in Pd and Pt, which are paramagnetic, the opposite situation occurs. The approximation of considering the electron band structure as a d-band combined with a conduction band is quite reasonable in these metals, where electrons in the d-band play a role of paramount importance. Therefore, the XMCD spectroscopy at the L2,3edges, which excites electrons from a pcore level to the empty states of d-band, is the ideal experimental tool to probe the d-band magnetism, since the spin and orbital contributions are discriminated. One must be aware, though, that dipole excitation from 2pto (n+ 1)sstates cannot be ruled out and may give a non-negligible contribution. Besides, the diamagnetic contribution is not observed. A recent work on Au foil illustrates this approach beautifully [163]. The XMCD at the Au L2,3edges were measured as a function of field up to H= 100 kOe, at temperatures ranging between 2.2 and 300 K. The XMCD spectra were clearly non-zero, indicating that an induced moment appears at the 5dband and that it aligns parallel to the applied field. Moreover, the magnetic orbital and spin moments were found to depend linearly with the applied field. The orbital to spin moment ratio amounts to mL/mS=0.28, thus indicating an important orbital contribution to the susceptibility. The spin Pauli para-
5.2. Induced magnetism in nanoparticle matrix 117 Table 5.1: Collected data for bulk Ag, Au, Pd and Pt metals. nd h, number of holes at the d-band; mL/mSratio obtained from the XMCD L2,3edges analysis; χtotal total magnetic susceptibility measured with conventional magnetometry; χd, d-band susceptibility, from XMCD magnetometry; χs P auli, Pauli paramagnetic spin component; χorb orbital component. Metal Ag (4d) Au (5d)dPd (4d)ePt (5d)e nd h0.349a0.617b1.27c1.635b mL/mS0.28d0.30e0.38e χtotal (emu/mol)f-1.95×10−5-2.08×10−55.56×10−41.89×10−4 χd(emu/mol) 7.0×10−61.3×10−36.1×10−4 χs Pauli (emu/mol) 5.4×10−69.6×10−44.4×10−4 χorb (emu/mol) 1.5×10−63.2×10−41.7×10−4 aSee Ref. [164]. bPrivate communication. cSee Ref. [165]. dSee Ref. [163]. eSee Ref. [166]. fSee Ref. [167] magnetism and orbital components to the susceptibility could be deduced, and the resulting susceptibility due to the 5dband is compared to the total susceptibility in table 5.1. The bulk Pd XMCD spectra, at the Pd L2,3edges, up to H= 70 kOe and 4 < T < 300 K, were also measured [166]. The field dependence is linear, and the susceptibility decreases with increasing temperature. The two components, spin Pauli paramagnetic and orbital susceptibility were deduced and are compared to the rest in table 5.1. The orbital component could be segregated into the SO and KO terms by comparing the results with a Fe/Pd multilayer. The XMCD at the L2,3edges of bulk Pt were measured likewise [34] (see table 5.1). From table 5.1 several conclusions may be drawn. In Au, diamagnetism is dominant, but the paramagnetic d-band susceptibility is nevertheless observable. In Pd and Pt the d-band paramagnetism is partially compensated by the diamagnetic terms. Except for Ag where no data exists, the d-band magnetism of the bulk metals is paramagnetic and is attributed to the non-zero number of holes induced by hybridization of this band with the s−pones. Moreover, the mL/mSratio increases with the number of holes in the d-band. 5.2 Induced magnetism in nanoparticle matrix When any of the four metals is in contact with a strongly magnetic material, the interfacial atoms of M=Ag, Au, Pd and Pt may also become magnetic in absence of an external applied field. This phenomenon has been extensively
118 Chapter 5. d-band magnetism of Ag, Au, Pd and Pt nanostructured materials studied in T/M thin films, where T is a transition metal as Ni, Fe or Co. The case between the interfacial T=Ni and M=Pt is described in [137], where three possible mechanisms for the induction of magnetic moment atoms are discussed: (a) charge transfer by hybridization between T and M d-bands, (b) symmetry breaking at the surface atoms, and (c) spin-orbit couplings between the T and M d-bands When the metal M forms part of a magnetic nanoparticle covering it, or intrinsically as an alloy, one or more of the three mechanisms invoked to explain magnetic induction of magnetism in M is also active and magnetism in the M atom is encountered. Such a study on Co nanoparticles capped with M=Ag, Au, Pd and Pt has been performed, as described for the case of Co-Pt NPs in chapter 4. In the Ag and Au cases the Co nanoparticle remains in its integrity and M covers, without alloying, the Co nanoparticle. The effect of the metal capping is, thus, embedding the Co particle in an M matrix. The net effect is the increase of surface anisotropy at the Co nanoparticle surface atoms [11, 19]. In contrast, Pt alloys with Co forming particles with high anisotropy (see chapter 4), and Pd behaves likewise. In this section, the XMCD results obtained at the L2,3edges of the corresponding capping layer for particles with the same average diameter of hDi ≈ 3 nm are compared. The data have been obtained at the ID12 beamline, at the ESRF, and the detection technique was fluorescence in backscattering geometry. The polarization was over 90 % in the Au and Pt cases, but in the Ag and Pd it was 36 and 22 % at the L2edge and 24 and 12.6 %, at the L3edge, respectively. The field was applied with an incident angle of 75owith respect to the normal to the plate. The applied field was H= 10 −20 kOe and the temperature T= 5 −10 K, thus guarantying the magnetic saturation of the NPs magnetization. The XANES and XMCD results for the four metal-capped Co-NPs, namely, Co-Ag, Co-Au, Co-Pd and Co-Pt NPs are shown in Fig. 5.1. Co-Ag and Co-Au figures are taken from Ref. [11]. The XMCD measurements for Co-Pt NPs are those described in section 4.3.3. Results from the sum rules analysis applied to the XMCD signals in Fig. 5.1 are collected in table 5.2. In all cases the non-zero XMCD signal indicates that the ferromagnetic Co has polarized the M atoms with the total moment parallel to the Co magnetization direction. The Pauli paramagnetic contribution, calculated from table 5.1 data for the applied field, falls within the experimental error bars in the four cases. The mL/mSratio has reduced respect to the bulk metal (compare with table 5.1), with the exception of the bulk Ag, where there is no data. In the case of Ag and, even more, in Pd, the orbital moment has been practically quenched, while it is at least one order of magnitude larger in the Au and Pt cases. This feature is probably related with the fact that the
5.2. Induced magnetism in nanoparticle matrix 119 (a) (b) 11560 11600 13280 13320 -0.15 -0.10 -0.05 0.00 0.05 Pt-L 2,3 7K, 1T q Normalized XMCD Photon energy (eV) p L 3 L 2 -1.2 -0.8 -0.4 0.0 0.4 XMCD integral 11560 11600 13280 13320 0.0 0.4 0.8 1.2 1.6 Photon energy (eV) Au - L 2,3 L 3 L 2 Pt - L 2,3 7K, 1T Normalized XAS 3160 3180 3320 3340 3360 0.0 0.5 1.0 1.5 Pd - L 2,3 10K, 2T L 2 L 3 Photon energy (eV) Normalized XAS Ag - L 2,3 3160 3180 3320 3340 3360 -0.3 -0.2 -0.1 0.0 0.1 0.2 0.3 Pd - L 2,3 10K, 2T q≈0 L 2 L 3 Photon energy (eV) Normalized XMCD p -0.9 -0.6 -0.3 0.0 0.3 0.6 0.9 XMCD Integral (c) (d) Figure 5.1: Normalized XANES and XMCD at the M L2,3edges in the Co-M NPs. (a) Co-Ag NPs [11], (b) Co-Au NPs [11], (c) Co-Pd NPs and (d) Co-Pt NPs. The XANES spectra of Ag and Au L2,3edges are shown in (c) and (d), respectively, for comparison. The higher limit for the p and q integrals, used for the sum rules analysis, is given.
120 Chapter 5. d-band magnetism of Ag, Au, Pd and Pt nanostructured materials Table 5.2: Collected data for the M-capped Co NPs with hDi ≈ 3 nm. ξd, spin-orbit constant at the ndorbital; nd h, number of holes at the d-band; mL/mSratio, mL, orbital moment, mS, spin moment, mtot =mL+mS, obtained from the XMCD L2,3 edges analysis. Capping metal AgbAubPd Pt ξd(meV)a272 608 200 600 nd h0.422 0.688 1.2c1.80(2) mL/mS0.045(5) 0.10(5) -0.006(3) 0.19(1) mL(µB) 7(1)×10−41.5(5)×10−3-0.003(3) 0.027(1) mS(µB) 0.014(3) 0.015 0.45(9) 0.14(1) mtot(µB) 0.015(3) 0.016(1) 0.45(9) 0.16(1) aSee Ref. [113]. bSee Ref. [11]. cSee Ref. [165]. spin orbit coupling constant ξdis larger in the Au and Pt cases (see table 5.2). The mtot is one order of magnitude smaller in Ag and Au, with respect to Pd and Pt, which is related with the much larger nd hin the two latter cases. On the other hand, mtot is thrice as large in Pd with respect to Pt. This trend is similar to that found for the Pauli paramagnetism, and cannot be directly related to the nd hvariation, but rather to a larger exchange enhancement of the paramagnetism in the Pd case. 5.3 Intrinsic magnetic moment in M nanoparticles Here, the focus is on NPs formed by clusters of M atoms, and show single particle magnetization. There are two distinct, reported, magnetic behaviors, Langevin superparamagnetism (SP) M(H) = mPart coth mPartH kBT−kBT mPartH(5.2) with a single particle moment mPart, and temperature independent magnetism up to room temperature (TI), which may appear simultaneously or independently. Many of the reports deal with conventional magnetometric data, and doubts are cast on the influence of spurious contributions. Our approach to this problem has been to restrict ourselves to the XMCD available data because of its element selectivity that allows to discriminate the magnetization originating from the actual M metal. As in the previous sections, the M L2,3edges inform on the contribution of the nd-band to this NPs magnetism. It has been reported that Ag NPs of hDi= 2.3 nm, capped with dodecanelthiol molecules, show a spontaneous, constant moment up to room
5.3. Intrinsic magnetic moment in M nanoparticles 121 temperature. However, there are no XMCD experiments yet done on these particles [168, 169]. Although Au NPs have been extensively investigated with conventional magnetometry (SQUID), relatively few experiments have been done with XMCD. The first of these experiments detected a Langevin paramagnetism and a small TI contribution in hDi= 1.9 nm Au NPs capped with polyallyl amine hydrochloride (PAAHC). The NP magnetic moment was determined to be mPart = 0.4µB. The TI component is quite sizeable and both SQUID and XMCD data coincide below T= 100 K. The XMCD signal is very small (10−5 XMCD/XAS ratio at the L3edge) (see table 5.3) [170]. The second report concerned Au hDi= 2 nm NPs capped with dodecanethiol, where the XMCD signal was similar to that of the PAAHC capped Au NP. Again, it yields to a very minute XMCD signal (10−5XMCD/XAS ratio) [169]. However, this small XMCD signal is assigned to the surface atoms only, and the authors propose mat = 0.33 µB/magnetic Au atom. Finally, Au NPs capped with thiol and embedded in polyethylene were measured with XMCD [171], finding also a very small XMCD signal as compared to the TI component. Our contribution to this subject has been the detection of a 25 times larger XMCD signal, shown in Fig. 5.2(a), in NPs of similar size deposited on a template of the Sulfolobus acidocaldarius S-layer [35]. mPart has been estimated to be of several Bohr magnetons. As in the previous cases, the presence of sulfur (S) atoms at the template surface binding the Au particle seems to be of paramount importance to show this type of magnetism, since it does not appear on Au particles deposited on Bacilus Sphericus S-layer, where there is no S present. We demonstrate that on each Au particle the thiols and other groups present in the S-layer supply holes to the 5dband. Their spins are ferromagnetically coupled by a spin-spin exchange interactions. In addition, an appreciable orbital moment is generated by spin-orbit couplings. Hund’s third rule is complied and the orbital moment is parallel to the spins. The magnetic behavior of the particle is paramagnetic, with very low anisotropy. Thus, the external field sets the common alignment direction of the magnetization of all particles. The very large magnetic moment per Au atom observed in the XMCD measurements originates from the large charge transfer from the S-layer supporting template to the Au surface atoms, and reshuffling of holes to the particle core. Finally, we may also remark that the striking magnetic properties of these Au NPs are due to the special synthesis on a unique biological matrix containing low number of thiol groups distributed in a highly ordered way [172]. As in the case of the Ag case, Pd NPs have been reported to show a magnetic behavior due to size-effect and, or, surface atoms polarization [173],
122 Chapter 5. d-band magnetism of Ag, Au, Pd and Pt nanostructured materials (a) (b) Au-sulfo Figure 5.2: Normalized XANES and XMCD at the M L2,3edges in the (a) Au NPs [172] and (b) Pt NPs [34]. The higher limit for the p and q integrals, used for the sum rules analysis, is given.
5.3. Intrinsic magnetic moment in M nanoparticles 123 however, there is no confirmation by XMCD of this feature. Finally, Pt13 nanoparticles embedded in a NaY zeolite matrix have also shown superparamagnetic behavior at low temperature and high field, as observed first with SQUID magnetometry [174]. The Pt13 particle crystallizes in icosahedral symmetry and have 12 of its atoms at the surface, thus size and surface effect are maximized. The XMCD measurement performed at the Pt L2,3edges at T= 7 K and increasing field up to H= 60 kOe gave an unambiguous non-zero signal, as shown in Fig. 5.2(b), which proved the existence of intrinsic magnetization in these particles. The mPart deduced from the Langevin curve ranges between 3.5 and 4.9 µB, and the moment per Pt atom deduced from the experiment is too low to account for all existent particles to be magnetic, actually, only 12% seem to have this property. It may be due to the different chemical surroundings in the zeolite cavity where the cluster sits [34]. Comparing the results in table 5.3, the ratio mL/mSof Au NPs varies strongly depending on the capping material, but in two out of three cases, it is larger than in the induced magnetic case of Co-Au capping (see tables 5.2 and 5.3). The value in the case of Pt13 is larger than in the Co-Pt alloyed NPs (see tables 5.2 and 5.3). In both cases, Au and Pt NPs, there is an increase in the number of holes nd hwith respect to the corresponding bulk metal. This seems to be a necessary condition for d-band magnetism of intrinsic type. Table 5.3: Collected data for the M NPs studied with XMCD. hDi, particle diameter; nd h, number of holes at the d-band; mL/mSratio, mL, orbital moment, mS, spin moment, mat =mL+mS, obtained from the XMCD L2,3edges analysis; mPart, the NP magnetic moment deduced from the Langevin curve. Au NPs Pt NPsd PAAHCaDTbSulfolobusc Type SP TI SP SP hDi(nm) 1.9 2 2.6(1) 0.7 nd h0.762 1.85 mL/mS0.145 0.10 0.28(1) 0.32(2) mL(µB/at) 0.0110(1) 0.0055(1) mS(µB/at) 0.039(1) 0.0171(6) mtot (µB/at) 0.001 0.33 0.050(1) 0.0226(9) mPart (µB) 0.4 2.3 3.5-4.9 aSee Ref. [170]. bSee Ref. [169]. cSee Ref. [35]. dSee Ref. [34].
124 Chapter 5. d-band magnetism of Ag, Au, Pd and Pt nanostructured materials 5.4 Conclusions XMCD has been able to establish that there is d-band magnetism in the metallic Ag, Au, Pd and Pt at the nanoscale. Besides, it has shown that about 30% of this magnetism is orbital in its origin. However, this technique gives, inherently, just an average value of the mL,mScomponents over all M atoms present in the sample. Therefore, it is unable to discriminate whether the magnetism originates at the surface (by chemical bonding, symmetry breaking, or both), or in the core of the particle. In our opinion, at present this is the most intriguing question, there being arguments and theories in both directions [175]. These are, among others, some of the open questions in the fascinating realm of the magnetism of metals.
6.2. Description of the TS measurement system 131 HDC Hrf L C CMOS circuit Gel cap with sample Components inside the PPMS Dewar Components outside the PPMS Dewar (b) (a) (2) (3) (1) (4) (5) Figure 6.2: (a) Picture of the PPMS with the TS setup: (1) Model 6000 PPMS control, (2) dewar, (3) multi functional probe’s head, (4) frequency counter and (5) oscilloscope. (b) Diagram of the TS measurement system. in Fig. 6.2. The tank inductance, L, is provided by a pick-up coil located in a controlled temperature and magnetic field environment. The capacitor, C, is usually fixed at room temperature outside the insert. The standard expression to define the resonance frequency of the tank is f=1 2π√LC (6.6) In these kind of setups, the magnetic sample is inserted into a gel cap that snugly fits into the inductive coil, and ∆fis measured as an external static field (HDC) or temperature are varied. Changes in fare direct consequence of changes in L, described by the expression ∆f f≈ −∆L 2L(6.7) obtained after differentiating equation 6.6. The total inductance of the coil with the sample inside, L, is defined in terms of the empty coil inductance, L0, and the contribution of the sample, LS. The latter depends on the permeability of the sample, µ=µ0(1 + χ), where χis its volume magnetic susceptibility (dimensionless). Then, considering the geometry of the coil, i.e., its volume, V0, its length, l, and the number of turns, N, and the volume of the sample inside it, VS, the total inductance L
132 Chapter 6. Transverse susceptibility measurement system for the PPMS is expressed as L=µ0N l2 (V0+χVS) (6.8) The change in inductance ∆L, calculated after differentiating equation 6.8, is written as ∆L=µ0N l2 ∆χVS(6.9) Since we want to express ∆L/L, we divide equation 6.9 by Lobtaining ∆L L=∆χVS V0+χVS (6.10) Two approximations may be derived from this expression. On one hand, if χVSV0, equation 6.10 is reduced to ∆L L≈∆χ χ(6.11) On the other hand, if χVSV0, equation 6.10 may be written as ∆L L≈∆χη (6.12) where η=Vs/V0represents the fill factor of the coil core space. When the geometry of the measurement setup is that illustrated in Fig. 6.2(b), where the perturbing rf magnetic field inside the coil (Hrf ∼10 Oe) is oriented perpendicular to the bias field, HDC, the magnetic susceptibility of the sample being probed is its transverse component χT[51], as described in section 6.1. Therefore, combining equations 6.7 and 6.11, we arrive at the direct relation between ∆fand ∆χT, as ∆f f≈ −1 2 ∆χT χT (6.13) and from equations 6.7 and 6.12 we get ∆f f≈ −1 2∆χTη(6.14)
6.3. Design and implementation of the oscillator circuit 133 6.3 Design and implementation of the oscillator circuit TS magnetometry equipments based on self-resonant systems usually employ a tunnel diode oscillator (TDO) as their active device in the radio frequency resonator setup [51]. However, there are several important drawbacks of using TDOs for this application, which may be summarized as: 1) they are complex devices with low market availability and 2) the tuning range for accomplishing the oscillation condition is reduced, thus limiting the nature of the measurable magnetic samples. Instead, the proposed oscillator uses CMOS transistors as active devices, implementing a simple inverter cell in cross-coupled topology, which compensates the energy loss of the LC resonant tank. The choice of these devices and configuration not only solve the above mentioned TDO drawbacks, but also involve some other benefits like: 1) minimum parasitics and noise sources increasing the sensitivity and accuracy of the resonant circuit, 2) higher circuit robustness and predictability, giving a deep understanding about the block properties, and 3) much lower cost in the future case of high-volume manufacturing. Figure 6.3 shows the electronic schematic of the complete circuit, where the described oscillator is denoted in the (1) zone. The theoretical basis of the oscillator design is detailed in Ref. [178]. The main aspects of the cell modeling are described as follows. The small-signal equivalent model of the proposed oscillator is illustrated in Fig. 6.4(a). The LC tank is represented by the impedance ZL. Applying conventional circuit theory, the characteristic equation of this model is obtained as a function of the ZLtransfer function, (3) (1) (2) V0 VDD RD ZL M1 M1 M2 C2 C1 R1 Oscilloscope Frequency meter (1 MΩ) Figure 6.3: Electronic schematic of the CMOS based LC cross-coupled oscillator circuit used for TS measurements.
134 Chapter 6. Transverse susceptibility measurement system for the PPMS as A−BZL= 0 (6.15) where, A=r01 +r02 +r01r02 (gm1+gm2)≈r01r02 (gm1+gm2) (6.16) B=gm1gm2r01r02 −1≈gm1gm2r01r02 (6.17) ZLis modeled as a L−R−Ccircuit given the inherent internal DC resistance of the inductive coil, as drawn in Fig. 6.4(b). Given this model, the load transfer function, ZL, is expressed as: ZL(s) = sL +R s2LC +sCR + 1 (6.18) Substituting equation 6.18 in 6.15, the final expression of the characteristic equation results in ALCs2+s(ARC −BL)+(A−BR) = 0 (6.19) Taking into account solutions s=±jω, and equalling the real and imaginary terms to zero, the oscillation frequency and oscillation condition are functions of L,C, and R, and are expressed as f2=1 (2π)2LC [1 −Rα] (6.20) 1≤Lα RC (6.21) where α= (gm1gm2)/(gm1+gm2), and gm1,2are the characteristic transconductances of the M1,2transistors shown in Fig. 6.3. These transistors are implemented with a commercial device, ALD1105 IC (two NMOS and two PMOS transistors into a single chip). The use of this standard CMOS chip guarantees high simplicity in modeling the transistors, validating the first order quadratic approximation described in Ref. [179]. This fact is quite important because it minimizes errors when determining the shift in the resonance frequency caused by the change in inductance for the TS calculation.
6.3. Design and implementation of the oscillator circuit 135 (a) gm2Xa ZL x x gm1Xb Xb Xa r01 r02 ZL R C L ≡ (b) Figure 6.4: (a) Small-signal equivalent model of the proposed oscillator. (b) Realistic model of the LC resonant tank In addition to the inverter cell and the LC tank, the circuit includes two extra stages. One of them is an output driver working as second oscillator stage. This driver (shown in the (2) marked zone in Fig. 6.3) is made by an NMOS passively loaded common-source stage and isolates the resonator tank from the posterior measurement equipment. This alleviates the load effect, minimizing the electronic impact of the connections to the measurement setup (the oscilloscope and frequency counter that will be described below). The second additional stage (denoted in the (3) area in Fig. 6.3) is a supply isolation block consisting of a voltage amplifier in buffer topology with a RC filtering network. It is crucial to isolate the LC resonant tank since this noise could generate phase noise into the oscillation. Different voltage amplifiers were tested in the design process of this block in order to optimize the stability and working conditions, obtaining the best trade-off with a LF356 OpAmp. Since the designed circuit operates at radio frequencies, the filtering network is based on a R−2Cbypassing filter with values of 3 Ω, 2.2 nF and 220 nF, respectively (see Fig. 6.3, (3) marked area). The circuit is integrated into the PPMS, using a model P450A - PPMS Multi-Function Probe (MFP) insert, shown in Fig. 6.5(a). The components of the circuit were placed as close as possible (thus minimizing parasitic effects) and mounted on a copper double layer board with glass fiber as isolation material, which is located inside the MFP head (see Fig. 6.5(b) for details of the final board design and Fig. 6.5(c) for the location of the board circuit into the probe’s head). The capacitor of the LC tank, C= 22 pF, is located on
136 Chapter 6. Transverse susceptibility measurement system for the PPMS (b) (c) (a) Figure 6.5: (a) MFP used for the TS setup. (b) Details of the circuit board with the CMOS based circuit. (c) Location of the circuit in the MFP’s head. the circuit board, while the inductor is placed at the end of the MFP, i.e., it is inserted into the PPMS dewar since it holds the sample to be measured (see location of the insert in the PPMS dewar in Fig. 6.2(a)). Discrete devices have been employed in this prototype in order to check different frequency ranges and bias conditions. Connections between the circuit board and the coil were made by a 0.9 m long non-magnetic beryllium copper - 50 Ω semi-rigid coaxial cable, with a 2.19 mm diameter (Coax co. ref. SC-219/50 B-B). The parasitic capacitance of the coaxial is about 86 pF, and the self inductance is around 200 mH, according to the manufacturer specifications; these two contributions must be taken into account when calculating the nominal resonance frequency of the LC tank. We have chosen this specific coax to minimize the thermal leak in the probe inside the PPMS dewar at low temperatures, as we demonstrate as follows. The thermal leak introduced by the coaxial cable in the low temperature system can be estimated by calculating the heat transfer rate by thermal conductance (Q/t) of the coax, according to the dimensions and thermal conductivity (κ) of the cable.4This thermal leak for the Be-Cu coaxial cable (κ= 65.77 W m−1K−1at 300 K and cross-sectional area = 1.58×10−6m2) is 0.045 W, while the one for a conventional RG402 Cu coaxial used in similar TS setups (κ= 385.95 W m−1K−1at 300 K and cross-sectional area = 3.07×10−6m2) is 1.23 W. The reduction of the thermal transfer rate by a factor of 27 by using 4A useful tool to calculate the heat transfer by thermal conductance of several materials can be found in the Quantum Design website www.qdusa.com/techsupport/ thermalCalculator.html
6.3. Design and implementation of the oscillator circuit 137 (a) (c) (b) (d) (e) l D d Figure 6.6: (a) Diagram of the coil geometry. (b) and (c) views of the coil assembly on the universal sample board. (d) Close up of the plug-in platform. (e) Final assembly of the coil at the bottom of the MFP. a Cu-Be coax in the setup is what allowed us to reach the lowest temperature possible with a conventional probe insert for the PPMS, i.e., Tbase =1.8 K. The circuit specifications were optimized to use an inductive air coil, L, which is a 31 - turn solenoid hand - wound using a 0.3 mm in diameter Cu wire, with 10.5 mm in length and 5.5 mm in diameter. According to these dimensions, the calculated inductance of the coil is 2.73 µH. Figure 6.6(a) shows a diagram of the coil geometry. The inductance and DC resistance of the coil were measured with a LCR meter, obtaining L= 2.8µH, which results in an error of less than 3% in the estimated value, and R= 0.18Ω. The coil is assembled onto a Quantum Design universal sample board (ref. P103C, shown in Fig. 6.6(b) and 6.6(c)) that plugs into the platform assembly of the MFP, which includes a calibrated cernoxTM (a zirconium oxynitride film) thermometer (see Fig. 6.6(d).). This sample board is easy to plug in and take out from the probe, so the coil does not need to be unsoldered and different coils can be used with the same circuit, if needed. A picture of the complete assembly at the bottom of the MFP is shown in Fig. 6.6(e). The coil dimensions are designed to hold a conventional gel-cap for PPMS and Magnetic Properties Measurement System (MPMS) measurements, so that it snugly fits into the coil core space. The resulting oscillator waveform is shown in Fig. 6.7, measured with a Tektronix TDS7104 digital phosphor oscilloscope. The signal is nearly sinusoidal with an oscillation frequency around 9.2 MHz. In order to calculate the frequency and compare both experimental and calculated values, equation
138 Chapter 6. Transverse susceptibility measurement system for the PPMS 0 . 0 0 0 . 0 8 0 . 1 6 0 . 2 4 0 . 3 2 0 . 4 0 - 0 . 2 - 0 . 1 0 . 0 0 . 1 0 . 2 A m p l i t u d e ( V ) T i m e ( µs ) Figure 6.7: Measured output waveform at VDD = 7 V, C= 22 pF and L= 2.8 µH. 6.20 may be approximated to f∼1/(2π√LCtotal) (since α∼0.4 mS for the input voltage of 7 V in the measurement of Fig. 6.7, and R= 0.18 Ω, so that Rα 1). According to the values of L= 2.8µH, the circuit capacitor, C= 22 pF, the capacitance and inductance contributions of the coax, Ccoax ∼86 pF and Lcoax ∼200 mH, the calculated frequency is 9.26 MHz, giving a high accuracy between the calculated and experimental values, with an error of less than 1%. Following the oscillation condition defined in equation 6.21 and the experimental results, the circuit oscillates with an input voltage, VDD, ranging between 6.2 V and 13 V, provided by a power supply EL302P programmable PSU. The oscillation frequency of this designed rf self resonant system may be varied by correctly choosing those values of Land C, so that equations 6.21 and 6.20 are fulfilled. In any case, the upper frequency is limited by the unavoidable parasitic capacitance of the coaxial cable (Ccoax ∼86 pF for the one used in our design). For example, for L= 2.8µH used in this work, the highest frequency is around 10.2 MHz, and the lowest reachable frequency is around 5.4 MHz, the latter obtained with a C= 220 pF. 6.4 Data acquisition The output signal of the circuit is read by an Agilent 53131A frequency counter and a Tektronix TDS2022B oscilloscope (see Fig. 6.2(a)). Data acquisition is performed by a connection via the IEEE - 488 General Purpose Interface Bus (GPIB) between the frequency counter and the Model 6000 PPMS respective port. Then, the resonating frequency acquired is used in the subsequent scripts written for measuring the sample TS. Measuring sequences have been imple-
6.5. Test Measurements 139 mented using the Visual Basic interpreter within MultiVu PPMS software.5 The executable programs scripted (.BAS files - called macros in MultiVu) allow scanning both HDC field and T(controlled by the PPMS) and measuring the resonance frequency, f. All measuring sequences are programmed directly on the PPMS controller computer and Multivu software, so that no additional equipment is needed for such effect. This fact represents an advantage with respect to similar TS measurement setups. 6.5 Test Measurements 6.5.1 Test measurements on an empty coil First tests measurements were performed on the empty coil, so that we could study and characterize the response of the system resonance frequency to both HDC and T. Such tests included those of stability of the frequency with time, temperature and field. Results for these tests are shown in Fig. 6.8. The test of the resonance frequency with time for the CMOS circuit (Fig. 6.8(a)) reveals the existence of a drift, which is reduced with time from 30 Hz/min to 14 Hz/min in 150 min (see straight lines in Fig. 6.8(a)). This drift can be attributed to the time the electronics need to reach a thermal stability after they are turned on. Comparing this result with tests performed on a TDO based circuit,6it is found that both circuits have analogous drifts, but the CMOS based circuit has a smoother and easy to correct curve on each TS scans. How these corrections are performed is described later in this section. The variation of the frequency of the empty coil with magnetic field is shown in Fig. 6.8(b). The total shift in frequency for a complete 9 T unipolar scan (sweeping HDC from 90 kOe to -90 kOe) is 197 Hz. Temperature dependence of the tank resonator frequency was probed by zero field cooling of the empty coil and it is shown in Fig. 6.8(c). This measurement supplies the background signal originated at the empty coil, fbkg(T). Frequency monotonically increases as temperature is lowered. The total frequency drift with temperature was found to be around 133 Hz/K, showing that the system is very sensitive to thermal changes. This is mostly due to 5For further information see the PPMS Application Note 1070-209 of Quantum Design. www.qdusa.com/techsupport/index.html 6A TDO based resonant circuit, similar to that described in Ref. [51] was also built by us to contrast the frequency stability results of both TDO and CMOS based resonant TS systems. The f0vs. time curve for the TDO configuration had an average drift of 5 Hz/min, after 120 min. However, the frequency change with time in this case was not monotonic, showing a step-like curve that is not very simple to correct in subsequent TS scans.
140 Chapter 6. Transverse susceptibility measurement system for the PPMS Report on the CMOS based TS measurement option for the PPMS – SAI, UZ. May 2011 15 -90 -60 -30 030 60 90 9.257 9.258 9.259 9.260 L = 2.8 µH T = 300K Resonance Frequency (MHz) Magnetic Field (kOe) 050 100 150 200 250 300 9.26 9.27 9.28 9.29 9.30 9.31 Resonance Frequency (MHz) Temperature (K) L=2.8µH H DC =0 020 40 60 80 100 120 140 9.254 9.255 9.256 9.257 9.258 17 Hz/min 14 Hz/min Resonance Frequency (MHz) Time (min) L=2.8 µH T=300K HDC=0 30 Hz/min -10 -5 0 5 10 0.000 0.001 0.002 0.003 0.004 L=2.8 µH T = 10K ∆χ T /χ T (%) Magnetic Field (kOe) (a) (b) (c) (d) Figure 6.8: Test measurements of the frequency stability of the empty coil. (a) Drift with time at 300 K. The straight segments indicate the rate of the frequency variation with time at different time intervals. (b) Variation with HDC at 300 K. Arrows show the direction of the field sweeping. (c) Variation with temperature at HDC = 0. (d) TS scan at T= 10 K and with Hsat = 10 kOe, after corrections from drifts. the thermal contraction the inductive coil suffers with decreasing temperature; the estimated rate of the frequency change as consequence of the changes in the dimension of the coil has been estimated as ∼100 Hz/K, calculated with the linear thermal expansion coefficient of copper (α= 16.6×10−6K−1). A bipolar TS scan of the empty coil at T= 10 K was also performed (see Fig. 6.8(d)), where the change in resonance frequency was measured as HDC was ramped from negative to positive saturation of 1 T, and vice versa. We considered the quantity ∆χT χT % = χSat T−χT(HDC) χSat T×100 ∝∆f f0 % (6.22) where χSat Tis the transverse susceptibility at the saturating field HSat = 10 kOe. This TS scan has been corrected for the previously described time and field linear drifts, by fitting a straight line between the data at positive and negative saturation and subtracting it from the whole data set. From Fig.