Full text
UPCommons Portal del coneixement obert de la UPC http://upcommons.upc.edu/e-prints Mudarra, M. [et al.] (2015) Sublinear dispersive conductivity in polyetherimides by the electric modulus formalism. IEEE transactions on dielectrics and electrical insulation . Vol. 22, issue 6. Pp. 3327- 3333. Doi: http://dx.doi.org/10.1109/TDEI.2015.004858. © 2015 IEEE. Es permet l'ús personal d'aquest material. S’ha de demanar permís a l’IEEE per a qualsevol altre ús, incloent la reimpressió/reedició amb fins publicitaris o promocionals, la creació de noves obres col·lectives per a la revenda o redistribució en servidors o llistes o la reutilització de parts d’aquest treball amb drets d'autor en altres treballs.
Mudarra, M. [et al.] (2015) Sublinear dispersive conductivity in polyetherimides by the electric modulus formalism. IEEE transactions on dielectrics and electrical insulation . Vol. 22, issue 6. Pp. 3327- 3333. Doi: http://dx.doi.org/10.1109/TDEI.2015.004858. (c) 2015 IEEE. Personal use of this material is permitted. Permission from IEEE must be obtained for all other users, including reprinting/ republishing this material for advertising or promotional purposes, creating new collective works for resale or redistribution to servers or lists, or reuse of any copyrighted components of this work in other works.
Sublinear Dispersive Conductivity in Polyetherimides by the Electric Modulus Formalism !Miguel Mudarra, Jordi Sellarès, Juan Carlos Cañadas and José Antonio Diego Universitat Politècnica de Catalunya Dept de Física i Enginyeria Nuclear, Campus en Terrassa de la UPC C. Colom, 11, 08222 Terrassa, Barcelona, Spain ABSTRACT Dynamic Electrical Analysis shows that the electrical properties of polyetherimide at temperatures above the glass transition are strongly influenced by space charge. We have studied space charge relaxation in two commercial grades of polyetherimide, Ultem 1000 and Ultem 5000, using this technique. The electric modulus formalism has been used to interpret their conductive properties. In both grades of polyetherimide, asymmetric Argand plots are observed, which are related to a sublinear power-law dependency (ωn with n<1) in the real part of the conductivity. This behavior is attributed to correlated hopping. The imaginary part of the electric modulus exhibits a peak in the low frequency range associated with conduction. The modelisation of this peak allows us to obtain the dependence, among other parameters, of the conductivity (σ0), the fractional exponent (n) and the crossover frequency (ωp) on the temperature. The α relaxation, which appears at higher frequencies, has also to be modeled since it overlaps the conductivity relaxation. The study of the parameters in terms of the temperature allows us to identify the ones that are thermally activated. The difference between the conductivity relaxation time and the Maxwell relaxation time indicates the presence of deep traps. The coupling model points out that the correlation of the ionic motion diminishes with temperature, probably due to increasing disorder due to thermal agitation. Index Terms — Conductivity, polyetherimide, electric modulus, correlated hopping, broadband dielectric spectroscopy. 1 INTRODUCTION POLYETHERIMIDE (PEI) is an amorphous thermoplastic resin with a high glass transition temperature. This resin is used for high performance electrical devices and biomedical applications. For many of these applications it is important to know the relaxational behavior of the material to foresee its response. Among these relaxations, those related to space charge play an especially important role in the electrical response of the material. Our study is focused on two commercial grades of PEI Ultem 1000 (U1000) and Ultem 5000 (U5000). These resins have similar chemical structure, but U1000 is meta-linked whereas U5000 is para-linked (Figure 1). Previous studies show that the dielectric strength of U5000 is higher than in the case of U1000 over a wide temperature range and the value of this magnitude diminishes with the temperature in both grades [1]. The differences are attributed to the remanent electrical field due to space charge, as charge injection from the electrode is more efficient in the case of U1000. Krause, Yang and Sessler have observed that in corona charged samples surface charge decays faster in the case of U5000 and that this grade is more sensitive to the change of the polarity of the applied field [2]. They attribute these differences to a more continuous band structure due to the existence of an ordered morphology in U5000 films. It is also known that the loss factor of U1000 increases sharply for temperatures close to the glass transition temperature due to conductive processes [3]. In the case of thermally stimulated depolarization currents (TSDC) measurements, the relaxation of space charge is associated with the ρ relaxation, which appears at temperatures higher than the α relaxation, associated to the glass transition [4]. This peak was studied by means of the general order kinetic model [5-8], that provides information about the relaxation mechanism for space charge and it was concluded that recombination was the most likely relaxation mechanism and that the depth of the traps is approximately 2.6 eV [4]. In this paper we present a relaxational study of the conductivity of PEI to improve the understanding of the mechanisms related to space charge in this material. The α relaxation has also been studied since both relaxations are so close that they overlap and cannot be studied on their own. Manuscript+received+on+24+August+2014,+in+final+form+6+February+2015,+accepted+ 29+March+2015.+
Figure 1. Chemical structures of U1000 (a) and U5000 (b). Data will be obtained by means of the dynamic electrical analysis (DEA) technique and interpreted using the electric modulus formalism [9-12]. The electric modulus (𝑀∗) can be obtained from the permittivity (𝜀∗) through 𝑀∗=𝜀∗!! (1)! The conductivity relaxation appears as a flex in the imaginary part of the permittivity. Instead, in the electric modulus it appears as peak allowing an easier interpretation of the data. The electric modulus formalism has been used to study the conductivity relaxation in polymers [13,14], glasses [15], crystals [16], ceramics [17] and composites [18,19], among other materials, as epoxy resines [20]. We expect to find a sublinear frequency dispersive AC conductivity as in many other systems [21]. In this case the real part of the conductivity σ′(ω) can be expressed as 𝜎!𝜔=𝜎!+𝐴𝜔! (2) where σ0 is the DC conductivity, A is a temperature dependent parameter and n is a fractional exponent which ranges between 0 and 1 and has been interpreted by means of many body interactions among charge carriers [22]. This behaviour, termed universal dynamic response, has been observed in highly disordered materials like ionically conducting glasses, polymers, amorphous semiconductors and also in doped crystalline solids [15, 16, 19, 23-26]. Equation 2 can be derived from the universal dielectric response function [27] for the dielectric loss of materials with free hopping carriers. With regards to the α relaxation, we will consider that the relaxation time follows the Havriliak–Negami equation and has a Vogel– Tammann–Fulcher dependence on temperature. It will be of particular interest to find the dependence of the obtained parameters on the temperature [28]. All in all, the parameters that result from the modelisation will allow us to characterize the relaxational behaviour of U1000 and U5000 above Tg and to obtain information about the space charge mechanisms in PEI. 2 EXPERIMENTAL Two grades of PEI, U1000 and U5000, were supplied by General Electric. DSC measurements indicate that their glass transition temperatures (Tg) are: Tg ≈ 220 ◦C in the case of U1000 and Tg ≈ 235 ◦C for U5000. Samples of U1000 and U5000 were cut from sheets of 125 μm in square portions with a side of 25 mm. The samples were placed between gold plated electrodes with radius 20 mm and measured using a Novocontrol BDS40 dielectric spectrometer with a Novotherm temperature control system. The real and imaginary parts of the electrical permittivity were measured at five points per decade between 10−2 Hz and 106 Hz at isothermal steps of 5 ◦C each at temperatures ranging between 230 ◦C and 285 ◦C in the case of U1000 and between 255 ◦C and 290 ◦C in the case of U5000. These temperature ranges are above the respective glass transition of the PEI grades in order to get a substantial contribution of the conductive processes. 3 RESULTS AND DISCUSSION The loss factor (ε′′) and the imaginary part of the electric modulus (M′′) of U1000 and U5000 are plotted in Figure 2 as a function of the frequency for a temperature T = 255 oC, which lies above Tg in both cases. It can be seen that the conductive processes in both materials result in a sharp increase of the loss factor at low frequencies. In the case of the imaginary part of the electric modulus, these effects are evidenced by a peak. This is certainly more convenient to model [12, 29]. For this reason we have choosed the electric modulus formalism to study the conductivity relaxation. Figure 2. Imaginary part of the electric modulus at T = 255 oC of U1000 (∎) and U5000 (▲). Loss factor of U1000 (!) and U5000 (▼) at the same temperature. Figure 3. Argand’s plot of the electric modulus M∗ of U1000 (∎) and U5000 (●) at T = 255 oC. (Frequency of plotted data increases from left to right). In Figure 3 we have plotted the electric modulus in Argand’s plane, for temperatures close to the glass transition temperature of U1000. The corresponding plots of the electric modulus show two arcs, i.e., the conductive processes result in an arc for low frequencies and for higher frequencies we can observe another arc that can be associated with the α relaxation. Depressed arcs are observed in the case of the relaxation associated with conductive processes that can be related to a dispersive regime [30]. N O = O = O C CH 3 CH 3 ON O = O = N O = O = O C CH 3 CH 3 ON O = O = 10-2 10-1 100101102103104105 0,00 0,02 0,04 0,06 0,08 0,10 0,12 Imaginary part of electric modulus, M'' frequency (Hz) 10-1 100 101 102 Loss factor, ε'' 0,00 0,05 0,10 0,15 0,20 0,25 0,30 0,00 0,02 0,04 0,06 0,08 0,10 0,12 Imaginary part of electric modulus, M'' Real part of electric modulus, M'
Figure 4. Real and Imaginary parts of the electric modulus of U1000 versus the frequency for several temperatures. Real part: ∎, 240 oC; ●, 250 oC; ▲, 280 oC; Imaginary part: ▼, 240 oC; ♦, 250 oC; ✕, 280 oC. The symbols are measured values and the continuous curves are the calculated values using the values of Table 1, which result from the fitting process to equation 9 In Figure 4 we have plotted the peak associated with the conductive process in U1000 for several temperatures above the glass transition. It can be noted that the peak shifts to higher frequencies with the temperature. To study the charge transport process at these temperatures we have assumed a sublinear frequency dispersive AC conductivity, as depressed arcs observed in Figure 3 for low frequencies can be associated with a dispersive regime. Power-law dependencies of conductivity, as in the case of equation (2), imply a powerlaw dependence of the form (jω)n for the complex conductivity [31]. Therefore, this magnitude can be written: 𝜎∗𝜔=𝜎!+𝐴𝑗𝜔 !+𝑗𝜔𝜀!𝜀!! (3) where ε∞C refers to the permittivity at high frequency. A crossover frequency ωp can be defined as 𝜔! !=!! ! (4) so that equation (3) can be rewritten as 𝜎∗𝜔=𝜎!+𝜎! ! !! ! +𝑗𝜔𝜀!𝜀!!! (5) This frequency ωp is associated with the crossover from the power-law dependence observed at high frequency to a frequency independent DC regime that occurs at low frequencies. Finally the contribution to the permittivity is 𝜀! ∗=−!!∗ !!! (6) The α relaxation can be modelized by means of Havriliak- Negami equation 𝜀!! ∗=𝜀!!" +∆! !!!!"!" !!" !!" (7) where ε∞HN refers to the permittivity at high frequencies and ∆𝜀=𝜀!!−𝜀!!" (8) is the relaxation strength. Therefore the electric modulus over the frequency range considered can be expressed as: 𝑀∗=(𝜀! ∗+𝜀!" ∗)!! (9) Electric modulus versus frequency data have been fitted to equation (9). The real and imaginary parts of the electric modulus, M ∗ (ω), were calculated from the complex permittivity and were fitted to the real and imaginary parts of the electric modulus given by equation (9) simultaneously. Eight independent parameters were used in the fitting process: σ0, ωp, ε∞C, n, ε∞HN , τHN, αHN and βHN. Figure 5. Imaginary part of the electric modulus at T = 255 oC of U1000: line is the value calculated by means of equation 9; symbols indicate the separate contributions of conductive process given by equation (6) (▲) and main relaxation α (●) given by equation 7. Parameters σ0, ωp , ε∞C , n characterize conductive process, whereas that parameters ε∞HN , τHN, αHN and βHN characterize main relaxation α using the values of Table 1 which result from the fitting process to equation (9). The study of the two contributions to electric modulus, given by equations (6) and (7), indicates that the first contribution (which is characterized by four of the parameters: σ0, ωp, ε∞C, n) helps to explain appropriately the contribution of conductive processes, whereas that the second contribution (which is characterized by the four remaining parameters, ε∞HN, τHN, αHN and βHN ) explains main relaxation α. Both contributions are plotted separately in Figure 5. It can be noted that each process (and, therefore, each set of four parameters) mainly contributes in a different frequency range, and the whole set of eight parameters is required to explain adequately the experimental response observed over the whole frequency range. Figure 6. Arrhenius plot of DC conductivity ∎, U1000; ●, U5000. In this work we have used simulated annealing to carry out the fitting process. This method has been successfully used in the analysis of thermally stimulated depolarization currents [32, 33] and dielectric spectroscopy data [34]. The values of the parameters obtained are shown in Tables 1, 2, 3 and 4. A good agreement between experimental and calculated data (symbols and continuous line respectively) has been obtained as it can be seen in Figure 4. Table 1. Parameters associated with conductive processes: U1000 case. All parameters are fit results. T(ºC) 𝜎!(𝛺!!!cm!!) 𝜔!(𝑠!!) n 𝜀!! 10-2 10-1 100101102103104105106 0,00 0,05 0,10 0,15 0,20 0,25 0,30 Real part of electric modulus, M' frequency (Hz) 0,00 0,02 0,04 0,06 0,08 0,10 Imaginary part of electric modulus, M'' 1,75 1,80 1,85 1,90 1,95 2,00 1x10-11 1x10-10 1x10-9 1x10-8 DC conductivity, σ0 (S m-1) Inverse temperature, 1000/T (K-1)
230 0.271×10−10 14.9 0.678 5.00 235 0.490×10−10 59.8 0.596 5.00 240 0.896×10−10 90.8 0.628 4.91 245 0.156×10−9 375.5 0.546 4.92 250 0.272×10−9 787.4 0.524 4.88 255 0.473×10−9 0.590×104 0.429 4.88 260 0.803×10−9 0.165×105 0.407 4.85 265 0.133×10−8 0.567×105 0.344 4.81 270 0.201×10−8 0.552×106 0.202 4.76 275 0.345×10−8 0.430×106 0.315 4.72 280 0.483×10−8 0.588×107 0.144 4.64 285 0.748×10−8 0.726×106 0.217 4.00 Table 2. Parameters associated with conductive processes: U5000 case. All parameters are fit results. T(ºC) 𝜎!(𝛺!!!cm!!) 𝜔!(𝑠!!) n 𝜀!! 255 0.368×10−9 0.181×104 0.526 4.28 260 0.577×10−9 0.204×104 0.580 4.25 265 0.904×10−9 0.824×104 0.507 4.24 270 0.139×10−8 0.569×105 0.373 4.22 275 0.213×10−8 0.144×106 0.365 4.17 280 0.322×10−8 0.346×106 0.332 4.10 285 0.499×10−8 0.198×106 0.381 3.99 290 0.624×10−8 0.120×106 0.303 3.72 Table 3. Parameters associated with α relaxation: U1000 case. All parameters are fit results except ∆ε that is calculated by means of equation (8). T(ºC) 𝜀!!" 𝜏!" (s) 𝛼!" 𝛽!" ∆𝜀 230 3.51 0.119 0.655 0.748 1.49 235 3.50 0.189×10−1 0.729 0.627 1.50 240 3.48 0.393×10−2 0.813 0.549 1.43 245 3.46 0.123×10−2 0.865 0.494 1.46 250 3.45 0.377×10−3 0.907 0.462 1.43 255 3.43 0.138×10−3 0.899 0.464 1.45 260 3.40 0.575×10−4 0.922 0.443 1.45 265 3.37 0.245×10−4 0.929 0.436 1.44 270 3.35 0.111×10−4 0.926 0.439 1.41 275 3.32 0.564×10−5 0.925 0.443 1.40 280 3.25 0.291×10−5 0.921 0.435 1.39 285 3.19 0.163×10−5 0.929 0.449 1.30 Table 4. Parameters associated with α relaxation: U5000 case. All parameters are fit results except ∆ε that is calculated by means of equation (8). T(ºC) 𝜀!!" 𝜏!" (s) 𝛼!" 𝛽!" ∆𝜀 255 3.65 0.781×10−3 0.803 0.365 0.63 260 3.61 0.248×10−3 0.864 0.309 0.64 265 3.59 0.840×10−4 0.845 0.315 0.65 270 3.54 0.367×10−4 0.854 0.284 0.68 275 3.50 0.150×10−4 0.835 0.298 0.67 280 3.43 0.689×10−5 0.822 0.299 0.67 285 3.33 0.356×10−5 0.839 0.284 0.66 290 3.11 0.208×10−5 0.847 0.283 0.61 The DC conductivity (σ0) of both grades of PEI increases with the temperature as it can be seen in Tables 1 and 2. Figure 6 shows an Arrhenius plot of the conductivity where it can be seen that it is thermally activated. This increase has been attributed to an increase of carrier mobility [13]. Conductivity can be fitted to 𝜎!=𝜎!!" exp(!! !") (10) Table 5. Preexponential factors (PF) and activation energies (Ea) of conductivity (σ0) and relaxation times (<τ> and τp), obtained from the corresponding Arrhenius plots. Ultem 1000 Magnitude log!"( PF !/1s) Ea (eV) 𝜎! 14.4 1.08 <𝜏> -25.1 1.10 𝜏! -56.6 2.44 U5000 Magnitude log!"( PF !/1s) Ea (eV) 𝜎! 10.8 0.92 <𝜏> -22.1 1.96 𝜏! -58.4 2.56 The activation energies and preexponential factors can be seen in Table 5. U1000 presents a slightly higher activation energy for the DC conductivity.' Concerning the relaxation time associated with space charge relaxation, it has been proposed that the crossover frequency can be associated with a characteristic time τp by means of 𝜏!=2𝜋/𝜔!. Experimental evidence has been given to support the idea that this characteristic time is actually the same time that an average relaxation time 𝜏![31], which can be defined in terms of the area under the Kohlrausch-Williams-Watts (KWW) function as 𝜏=Φ𝑡𝑑𝑡 =!(!!)!∗ ! ! ! (11) where τ* and β are the parameters that define the KWW response function Φ𝑡=exp![−(𝑡𝜏∗)!] (12) This average relaxation time 𝜏 corresponds to the Maxwell relaxation time, this is, the time that an out–of– equilibrium conductor needs to reach electrostatic equilibrium. It is related to the DC conductivity according to the expression [12] 𝜏=!!!!! !! (13) Figure 7. Characteristic time τp (associated with crossover frequency τp = 2π/ωp: ∎ , U1000; ●, U5000. Maxwell relaxation time ⟨ τ ⟩ : △ U1000; ▽ U5000. We have calculated the values of 𝜏 and τp. An attempt to compare both magnitudes in an Arrhenius plot can be seen in Figure 7. As it can be seen, both quantities represent a thermally activated relaxation time of the form 𝜏=𝜏!"exp!(!! !") (14) 1,76 1,80 1,84 1,88 1,92 1,96 2,00 1x10-7 1x10-5 1x10-3 1x10-1 1x101 Characteristic time τp , Maxwell relaxation time <τ> (s) Inverse temperature, 1000/T (K-1)
The activation energies and preexponential factors can be seen in Table 5. For both types of relaxation time, the activation energy in the case of U5000 is higher. It can also be noticed that the activation energy of τp is higher than the one of 𝜏. It should be clear that these quantities do not represent the same magnitude since their values differ in several orders of magnitude, specially at high temperatures. The agreement between these values was used by León et al to support the hypothesis of a common origin for both DC and AC regimes [31]. Nevertheless, in the following lines we will explain how our results can be reconciled with the idea that both quantities are, at least, related. In our opinion, the physical meaning of τp is just an estimation of the time that separates the relaxation processes for which predominates DC conduction (τ > τp) or predominates AC (τ < τp) conduction. The mechanism that leads to DC regime are long range displacements [23] where the carriers move in the same direction but at higher frequencies short range hopping of the carriers occurs, which is viewed as a correlated motion in which the carrier performs several reiterated forward– backward hops before completing any successful forward displacement. Reiterative hopping is the origin of the dispersive regime and it occurs when the frequency is higher than the crossover frequency below which successful hops can be completed. The high value of 𝜏 that we have found at high temperatures, in the case of macromolecular materials can be explained on the basis that the microscopic processes that lead to conduction may not be reduced to mere hops over a barrier between adjacent sites. Amorphous polymers, such as PEI, are disordered materials and charge may be located in deep traps. This kind of charge plays a relevant role in microscopic relaxation processes. When the temperature is increased deeply trapped charge may get not enough thermal energy to jump over the potential barrier, but to reach a intermediate energy level, resulting in a more complex relaxation behaviour. If one assumes that the only process that contributes to electrical conduction is hopping, as it has been observed at high temperatures in other polymers [35] the crossover frequency can be associated with the frequency below which carriers can follow the variations of the applied field, so that their characteristic relaxation time is shorter than the applied field period. At such frequencies, DC conductivity determines the relaxation process and, therefore, the Maxwell time determines the crossover frequency. But if deep traps are present, carriers deeply trapped have a longer relaxation time, so that their contribution should be evident at frequencies below the crossover frequency and their effect should represent a slowing down of space charge relaxation process. On the other hand, charge located in deep traps can not follow the field oscillations at higher frequencies and it does not contribute to the relaxation process. Therefore, the presence of deep traps can be associated with a slowing down of the relaxation process, that results in an apparent Maxwell time longer than the relaxation time that corresponds to the crossover frequency. The higher value of 𝜏!and the higher activation energy of τp can thus be explained by the presence of deep traps. The temperature dependence of the fractional exponent n is shown in Figure 8. This parameter characterizes the power– law conduction regime, which is associated with the slowing down of the relaxation process in the frequency domain as a result of the cooperative effects, in the same way as the KWW function does in the time domain. An important connection between these two approaches stems from the coupling model of Ngai and Kannert [36]. This model predicts a power-law conductivity associated with the KWW relaxation function (equation 12) given by 𝜎!"" =𝐵𝑒𝑥𝑝(−!! !")𝜔!!! (15) Therefore, if any other contribution is sufficiently smaller than that of σKWW, then the conductivity of the material may be described by σKWW(ω) [36]. In that case, the sublinear dispersive AC conductivity observed in PEI can be associated with a KWW relaxation mechanism with 𝛽=1−𝑛 where n is the power-law exponent determined from σ(ω). Figure 8. Fractional exponent n as a function of temperature (Dashed lines are a guide for the eye): ∎ , U1000; ●, U5000. The stretched exponential relaxation time has been associated with a slowing of the relaxation process that results from correlated hopping. according to this interpretation, the stretched exponential parameter 𝛽 represents a correlation index of carrier motion. One would expect 𝛽 to be close to zero for strongly correlated systems and close to 1 for random Debye–like hops. As we can see in Figure 8 the power–law exponent 𝑛=1−𝛽 decreases with temperature for both grades, indicating that correlation of carriers motion decreases with temperature. This can be associated with the increasing disorder due to thermal agitation of polymer chain segments. In Tables 3 and 4 we can see the evolution of the fitting parameters for the α relaxation. The αHN parameter indicates the non-exponentiality of the relaxation. This is, αHN = 1 is a Debye-like relaxation and αHN < 1 indicates that the relaxation extends over a wider range than a Debye relaxation. The non– exponentiality maybe due to a distribution of relaxation times or to cooperativity. As the temperature increases and attains values progressively further from the Tg of the material, the value of αHN is closer to 1. In this case this is due to less cooperativity as the glass transition is left further away. On the other hand, the parameter βHN decreases, which means that a broader range of relaxation modes are excited at temperatures further from Tg, but at the expense of a lower overall dielectrics strength, as it can be seen in the Tables. This is analogous to what happens in TSDC when a poling temperature far from the optimal one is employed. Table 6. Preexponential factor τHN0, EW and T0 obtained by fitting the relaxation time τHN to equation 16. Grade τHN0 (s) EW (eV) T0 (K) U1000 1.43×10−11 0.11 446 500 510 520 530 540 550 560 570 0,1 0,2 0,3 0,4 0,5 0,6 0,7 Fractional exponent, n Absolute temperature, T (K)
U5000 4.95×10−12 0.12 452 In the case of the α relaxation, Figure 9 shows that the relaxation time τHN decreases with temperature following the Vogel–Fulcher–Tammann (VFT) equation 𝜏!" =𝜏!"!exp(!! !!!! ! ) (16) for both PEI grades. The result of the fits can be seen in Table 6. This behaviour is typical of cooperative non-exponential relaxations. This is not surprising since the α relaxation is related to the glass transition of the material. The value of T0 is lower in U1000 than in U5000. This is due to the fact that they should follow a pattern similar to Tg. Figure 9. Relaxation time τHN as a function of temperature: ∎, U1000; ●, U5000. Dashed lines are curves fitted to VFT equation. 4 CONCLUSION Conductive processes in two grades of commercial PEI have been studied and it has been found that they condition the electrical behaviour of these materials at high temperatures and low frequencies. The electric modulus formalism has been useful in order to interpret dynamic electrical analysis data to characterize these processes. The α relaxation has also been studied due to its proximity to the conductive relaxation that made impossible to study just the conduction on their own. The dispersive conductivity observed in both grades of PEI can be explained by means of a sublinear frequency dispersive AC conductivity. This behaviour is the result of correlated hopping. The DC conductivity is thermally activated, probably due to an increase of carriers. Among the parameters studied, there is the crossover relaxation time τp. The physical meaning of τp is just an estimation of the time that separates the relaxation processes for which predominates DC conduction (τ > τp) or predominates AC (τ < τp) conduction. In the literature [31], experimental evidence of the equivalence of the crossover relaxation time with the Maxwell relaxation time has been presented but in our case the presence of deep traps can produce a slowing down of the relaxation process. This results in an apparent Maxwell time longer than the crossover relaxation time. Both relaxation times are thermally activated. This is to be expected in the case of the Maxwell relaxation time, since it is calculated from the DC conductivity. In the case of the crossover relaxation time, this fact reinforces the idea that it is physically related to the Maxwell relaxation time. The higher activation energy in the case of the crossover relaxation time can also be attributed to the presence of deep traps. The power–law exponent n decreases with temperature for both grades, indicating that correlation of ionic motion decreases with temperature. This can be associated with the increasing disorder due to thermal agitation of polymer chain segments. The behaviour of the α relaxation is typical of cooperative non-exponential relaxations. This happens because the α relaxation is related to the glass transition of the material. As the temperature attains values further to Tg the response from the α relaxation becomes less cooperative even though a broader range of the relaxation is involved. ACKNOWLEDGMENT This work has been partially supported by project 2014 SGR 957 (AGAUR). REFERENCES [1] N. Zebouchi, V. H. Truong, R. Essolbi, M. Se-Ondoua, D. Malec, N. Vella, S. Malrieu, A. Toureille, F. Schue !, and R. G. Jones, “The electric breakdown behaviour of polyetherimide films,” Polym. Int’l., Vol. 46, No. 1, pp. 54–58, 1998. [2] E. Krause, G. M. Yang, and G. M. Sessler, “Charge dynamics and morphology of Ultem 1000 and Ultem 5000 PEI grade films,” Polym. Int’l., Vol. 46, No. 1, pp. 59–64, 1998. [3] R. Díaz-Calleja, S. Friederichs, C. Jaïmes, M. J. Sanchis, J. Belana, J. C. Cañadas, J. A. Diego, and M. Mudarra, “Comparative study of mechanical and electrical relaxations in poly(etherimide), Part 2,” Polym. Int’l., Vol. 46, No. 1, pp. 20–28, 1998. [4] J. Belana, J. C. Cañadas, J. A. Diego, M. Mudarra, R. Díaz-Calleja, S. Friedericks, C. Jaïmes, and M. J. Sanchis, “Comparative study of mechanical and electrical relaxations in poly(etherimide), Part 1,” Polym. Int’l., Vol. 46 No. 1, pp. 11–19, 1998. [5] R. Chen and Y. Kirsh, Analisys of Thermally Stimulated Processes. Oxford: Pergamon Press, ch. 2, pp. 35–92, 1981. [6] M. Mudarra and J. Belana, “Study of poly(methyl methacrylate) space charge relaxation by TSDC,” Polymer, Vol. 38, pp. 5815–5821, 1997. [7] M. Mudarra, J. Belana, J. C. Cañadas, and J. A. Diego, “Polarization time effect on PMMA space charge relaxation by TSDC,” J. Polym. Sci. Pol. Phys., pp. 1971–1980, 1998. [8] M. Mudarra, J. Belana, J. C. Cañadas and J. A. Diego, “Windowing polarization: considerations to study the space charge relaxation in poly(methyl methacrylate) by thermally stimulated depolarization currents,” Polymer, Vol. 40, pp. 2659–2665, 1999. [9] C. T. Moynihan, “Description and analysis of electrical relaxation data for ionically conducting glasses and melts,” Solid State Ionics, Vol. 105, pp. 175–183, 1998. [10] P. Pissis and A. Kyritsis, “Electrical conductivity in hydrogels,” Solid State Ionics, Vol. 97, pp. 105–113, 1997. [11] J. R. Macdonald, “Resolution of conflicting views concerning frequency–response models for conducting materials with dispersive relaxation, and isomorphism of macroscopic and microscopic models,” Solid State Ionics, Vol. 150, pp. 263–279, 2002. [12] I. M. Hodge, K. L. Ngai, and C. T. Moynihan, “Comments on the electric modulus function,” J. Non–Cryst. Solids, Vol. 351, pp. 104–115, 2005. [13] M. Mudarra, J. Belana, J. C. Cañadas, J. A. Diego, J. Sellarès, R. Díaz- Calleja, and M. J. Sanchis, “Space charge relaxation in polyetherimides by the electric modulus formalism,” J. Appl. Phys., Vol. 88, pp. 4807– 4812, 2000. [14] H. Lu, X. Zhang, and H. Zhang, “Influence of the relaxation of Maxwell–Wagner–Sillars polarization and DC conductivity on the dielectric behaviors of nylon 1010,” J. Appl. Phys., Vol. 100, p. 054104(7pp), 2006. 500 510 520 530 540 550 560 570 -6,0 -5,0 -4,0 -3,0 -2,0 -1,0 Relaxation time, log(τHN / s) Absolute temperature, T (K)
[15] S. Lanfredi, P. S. Saia, R. Lebullenger, and A. C. Hernandes, “Electric conductivity and relaxation in fluoride, fluorophosphate and phosphate glasses: analysis by impedance spectroscopy,” Solid State Ionics, Vol. 146, pp. 329–339, 2002. [16] A. Rivera, J. Santamaría, and C. León, “Electrical conductivity relaxation in thin–film yttria–stabilized zirconia,” Appl. Phys. Lett., Vol. 78, pp. 610–612, 2001. [17] J. Liu, C.-G. Duan, W.-G. Yin, W. N. Mei, R. W. Smith, and J. R. Hardy, “Dielectric permittivity and electric modulus in Bi2Ti4O11,” J. Chem. Phys., Vol. 119, pp. 2812–2819, 2003. [18] G. C. Psarras, E. Manolakaki, and G. M. Tsangaris, “Dielectric dispersion and AC conductivity in iron particles loaded polymer composites,” Compos. Part A–Appl. S., Vol. 34, pp. 1187–1198, 2003. [19] M. D. Migahed, M. Ishra, T. Fahmy, and A. Barakat, “Electric modulus and AC conductivity studies in conducting PPy composite films at low temperature,” J. Phys. Chem. Solids, Vol. 65, pp. 1121–1125, 2004. [20] Fuqiang Tian and Ohki, Y., "Electric modulus powerful tool for analyzing dielectric behavior," IEEE Trans. Dielectr. Electr. Insul., Vol.21, No. 3, pp. 929-931, 2014. [21] A. K. Jonscher, Dielectric Relaxation in Solids. Chelsea Dielectric Press, 1983, ch. 5, pp. 161–253. [22] A.K. Jonscher, Dielectric Relaxation in Solids. Chelsea Dielectric Press, 1983, ch. 8, pp. 310–370. [23] D. L. Sidebottom, P. F. Green, and R. K. Brow, “Two contributions to the AC conductivity of alkali oxide glasses,” Phys. Rev. Lett., Vol. 74, pp. 5068–5071, 1995. [24] D. L. Sidebottom, P. F. Green, and R. K. Brow, “Scaling parallels in the non-debye dielectric relaxation of ionic glasses and dipols supercooled liquids,” Phys. Rev. B, Vol. 56, pp. 170–177, 1997. [25] C.León, M.L.Lucía, J.Santamaría and F.Sánchez-Quesada,“Universal scaling of the conductivity relaxation in crystalline ionic conductors,” Phys. Rev. B, Vol. 57, No. 1), pp. 41–44, 1998. [26] P. S. Anantha and K. Hariharan, “AC conductivity analysis and dielectric relaxation behaviour of NaNO3–Al2O3 composites,” Mat. Sci. Eng. B– Solid, Vol. 121, pp. 12–19, 2005. [27] H. M. Millany and A. K. Jonscher, “Dielectric properties of stearic acid multilayers,” Thin Solid Films, Vol. 11, pp. 257–273, 1980. [28] D. P. Almond, A. R. West, and R. J. Grant, “Temperature dependence of the AC conductivity of Naβ–alumina,” Solid State Commun., Vol. 44, pp. 1277–1280, 1982. [29] H. W. S. Jr. and P. Avakian, “Conductivity and the electric modulus in polymers,” J. Polym. Sci. Pol. Phys., Vol. 30, pp. 637–641, 1992; and J. R. Macdonald, Impedance Spectroscopy: Emphasizing Solid Materials and Systems. Wiley–Interscience, ch. 2, pp. 27–132, 1987. [30] J. R. Macdonald, Impedance Spectroscopy: Emphasizing Solid Materials and Systems. Wiley–Interscience, ch. 2, pp. 27–132, 1987. [31] C. León, M. L. Lucía, and J. Santamaría, “Correlated ion hopping in single–crystal yttria–stabilized zirconia,” Phys. Rev. B, Vol. 55, No. 2, pp. 882–887, 1997. [32] E. Laredo, N. Suarez, A. Bello, and J. M. G. F. B. R. de Gáscue, M. A. Gomez, “α, β and γ relaxations of functionalized HD polyethylene: a TSDC and a mechanical study,” Polymer, Vol. 40, pp. 6405–6416, 1999. [33] M. Grimau, E. Laredo, A. Bello, and N. Suarez, “Correlation between dipolar TSDC and AC dielectric spectroscopy at the PVDF glass transition,” J. Polym. Sci. Pol. Phys., Vol. 35, pp. 2483–2493, 1997. [34] A. Bello, E. Laredo, and M. Grimau, “Distribution of relaxation times from dielectric spectroscopy using monte carlo simulated annealing: Application to α-PVDF,” Phys. Rev. B, Vol. 60, pp. 12 764–12 774, 1999. [35] J. Ho and T. R. Jow, “High field conduction in biaxially oriented polypropylene at elevated temperature”, IEEE Trans. Dielectr. Electr. Insul., Vol. 19, No. 3, pp. 990–995, 2012. [36] D. L. Sidebottom, P. F. Green, and R. K. Brow, “Comparison of KWW and power law analyses of an ion–conducting glass,” J. Non–Cryst. Solids, Vol. 183, pp. 151–160, 1995. Miguel Mudarra received his degree and master level in physics at the Universitat Autònoma de Barcelona. He obtained the Ph.D. degree at the Universitat Politècnica de Catalunya (UPC). He is currently an Associate Professor and Director of the School of Industrial and Aeronautical Engineering of the UPC. His research interest includes space charge formation and relaxation processes in solid insulating materials, electric charge measurement methods, and electrostatic phenomena Jordi Sellare`s received his degree in physics (1992) and his Ph.D. degree (1997) at the Universitat de Barcelona (UB). Currently he is associate professor at Universitat Politècnica de Catalunya (UPC). His research interests include the study of the glass transition, dielectric relaxation in solids and determination of the charge profile in poled dielectrics. Juan Carlos Cañadas was born in Barcelona, Spain, in 1963. He graduated from the Faculty of Physics, University of Barcelona, Spain, in 1987 and received the Ph.D. degree in physics science from the Technical University of Catalonia (UPC), Terrassa, Spain in 1999. He is currently a Professor in the Department of Physics and Nuclear Engineering of the Technical University of Catalonia, where he is also member of the research Group of Dielectric Materials. His current research interests include the electrical properties of dielectric materials (relaxations, space charge distribution, the glass transition) and the electrical characterization of insulating José Antonio Diego received the degree in physics science from the Universitat Autònoma de Barcelona, Barcelona, Spain, in 1987. In 1993, he received the Ph.D. degree in physics science from the same university. He is currently Professor in the Department of Physics and Nuclear Engineering of the Technical University of Catalonia (UPC), where he has been working in cable studies since 1999. His current research interests include the electrical properties of dielectric materials and space charge, as well as the glass transition in polymers and numerical approaches.