scieee AI-readable full text Open interactive document viewer

Fabrication and characterization of graphene nanostructures

Navickaite, Gabriele

Abstract

[ANGLÈS] We fabricate graphene nanostructures for experimental studies on graphene plasmonics and graphene-quantum dot interactions. We use a focused ion beam to mill structures in a substrate, and deposit graphene on top. For plasmonics, we produce free-standing graphene membranes with widths up to 2 µm on a gold substrate. For strong interactions with quantum dots, we produce a hybrid system consisting of 750 nm and 1 µm wide circles and trenches in a SiO2 substrate, quantum dots, and free-standing graphene membranes. Using chemical doping, we induce changes in the Fermi level of graphene up to around 200 meV, we observe a spontaneous decay of the doping on a time scale of two days. We find that our graphene technique yields mobilities of 3200 cm2/Vs.

Full text

Master Erasmus Mundus in Photonics Engineering, Nanophotonics and Biophotonics Europhotonics MASTER THESIS WORK Fabrication and Characterization of Graphene Nanostructures Gabrielė Navickaitė Supervised by Dr. Frank Koppens (Institute of Photonic Sciences, ICFO) Presented in Barcelona, on 6th of September 2012 Registered at Abstract We fabricate graphene nanostructures for experimental studies on graphene plasmonics and graphene-quantum dot interactions. We use a focused ion beam to mill structures in a substrate, and deposit graphene on top. For plasmonics, we produce free-standing graphene membranes with widths up to 2 µ m on a gold substrate. For strong interactions with quantum dots, we produce a hybrid system consisting of 750 nm and 1 µ m wide circles and trenches in a SiO 2 substrate, quantum dots, and free-standing graphene membranes. Using chemical doping, we induce changes in the Fermi level of graphene up to ∼ 200 meV, we observe a spontaneous decay of the doping on a time scale of two days. We nd that our graphene technique yields mobilities of 3200 cm2 /V·s . 1 Contents 1 Introduction 3 2 Theoretical Background 4 2.1 Graphene .................................... 4 2.1.1 Electronic Structure . . . . . . . . . . . . . . . . . . . . . . . . . . 4 2.1.2 Electronic Transport . . . . . . . . . . . . . . . . . . . . . . . . . . 5 2.1.3 Synthesis ................................ 6 2.2 Grapheneplasmons............................... 7 3 Fabrication techniques 11 3.1 Structuring ................................... 11 3.1.1 Focused Ion Beam Lithography . . . . . . . . . . . . . . . . . . . . 11 3.1.2 Optical Lithography . . . . . . . . . . . . . . . . . . . . . . . . . . 16 3.2 Mechanical Exfoliation . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 17 3.3 Transfer ..................................... 19 3.3.1 Transfer of graphene akes . . . . . . . . . . . . . . . . . . . . . . . 19 3.3.2 Transfer of CVD graphene . . . . . . . . . . . . . . . . . . . . . . . 21 3.4 Chemical doping of graphene . . . . . . . . . . . . . . . . . . . . . . . . . . 22 4 Characterization techniques 23 4.1 Ramanspectroscopy .............................. 23 4.2 4probesmeasurement ............................. 24 4.3 Fluorescence quenching . . . . . . . . . . . . . . . . . . . . . . . . . . . . 25 5 Results 27 5.1 Hybrid graphene/quantum dots devices . . . . . . . . . . . . . . . . . . . 27 5.1.1 Fabrication ............................... 27 5.1.2 Characterization ............................ 30 5.2 Suspended graphene nanostructures for plasmonics . . . . . . . . . . . . . 32 5.2.1 Fabrication and characterization . . . . . . . . . . . . . . . . . . . . 32 5.2.2 Doping.................................. 36 5.3 Mobilitymeasurement ............................. 40 2 1 Introduction Interactions between light and graphene can be very strong, opening a new eld of possible applications, such as photodetectors, chemical sensors etc. Two approaches towards the enhancement of the light-graphene interaction are presented in this thesis: surface plasmon enhanced interaction of light with nanostructured graphene and strong interaction of graphene with quantum dot excitations. Graphene, being just one atom thick, induces new challenges for fabrication. In particular, nanofabrication of graphene is an emerging new eld of engineering, important for nanoelectronics and nanophotonics. In parallel, integration of graphene with other materials, like metals or quantum dots into novel hybrid systems is important for solar cells and photodetectors. This thesis describes a project with the aim to overcome these new technological challenges and produce devices for graphene plasmonics and graphene opto-nano-mechanics. We present work towards the fabrication of graphene nanoribbons for observing localized plasmonic resonances, and a hybrid graphene-quantum dot system for graphene motion detection. In chapter 2 we present theoretical background of graphene and its extraordinary properties. In chapter 3 we present sample fabrication techniques. Chapter 4 introduces sample characterization techniques, and in chapter 5 we present the main experimental results of the thesis. 3 2 Theoretical Background 2.1 Graphene Graphene is a single atomic layer of carbon with a hexagonal lattice. Two-dimensionality of graphene results in an extraordinary electronic structure. Graphene was rst isolated in 2004 [1] and this discovery resulted in a Nobel Prize in Physics in 2010 for Andre Geim and Konstantin Novoselov. Graphene is an interesting material to investigate from a fundamental physics point of view, as it has the half integer Hall eect and electrons are described as Dirac fermions. On the other hand, interesting applications of graphene arise due to it being a zero band gap material. In a large part of the electromagnetic spectrum, graphene absorbs ∼ 2,3 % of light, which is very high considering that graphene is only one atom thick. The described properties of graphene have resulted in enormous interest and intense research from the electronics, photonics, and plasmonics perspective. 2.1.1 Electronic Structure Figure 1: Electronic dispersion in the hexagonal lattice. On the right picture: close up of the energy bands close to one of the Dirac points. From [2] Graphene has an interesting band structure resulting in the extraordinary properties due to its two-dimensionality. Carbon atoms form a hexagonal lattice, resulting in the sublattice consisting of 4 atoms. Each atom in a sub-lattice has 3 neighbor atoms at about 1,42 Å distance and is bonded to them by σ bonds. The forth bond is π bond and is oriented in the z-direction. As there is no atoms to bond in the z-direction, π - bonds are hybridized together to form the so called π - band and π∗ - band. Those bands are responsible for most of the peculiar electronic properties of graphene [3] and for its strong interaction with the substrate. In Figure 1 the energy versus momentum dispersion relation for graphene is imaged. Graphene is a zero band-gap material as conduction and valence bands meet at the Dirac 4 points. The Dirac points are positions in momentum space at the edge of the Brillouin zone. The Fermi energy for neutral graphene is at the Dirac point, although it might be signicantly altered by chemical or electrical doping. In chemical doping graphene is interacting with the other material through mentioned π bands while in electrical doping Fermi energy is shifted by created electrical potential. While shifting the Fermi energy to the valence or conduction band, the polarity of the carriers changes from electrons to holes and vice-versa. If a region near one of the Dirac points is examined more carefully (Figure 1 on the right) a linear cone-like dispersion is noticed. The linear dispersion relation is well described by the Dirac equation for mass-less fermions [3]. Employing the tight binding approximation for the Dirac Hamiltonian calculation, a velocity of charges in graphene can be evaluated, resulting with Fermi velocity in ∼ 10 6m /s , which is 1/300th of the speed of light in vacuum. With this speed, charges behave as relativistic particles in graphene, enabling tests of relativistic physics on a table top and opening new possibilities for fast electronics. 2.1.2 Electronic Transport Corresponding to graphene ´ s unique band structure described in previous section, graphene exhibits novel transport eects such as the ambipolar eld eect and minimum conductivity. Figure 2: Ambipolar electric eld eect in single layer graphene. The insets show lowenergy spectrum, indicating changes in the position of the Fermi energy with changing gate voltage. From [4] 5 By applying a gate voltage between a back gate and graphene, the charge carrier density in graphene may be tuned. With applied positive voltage electrons are owed into graphene and their concentration, typically, is tuned from 10 11 to 10 13 cm −2 , which corresponds to 10 to 400 meV shift of the Fermi energy [5]. With applied negative voltage holes become the dominant charge carriers. The gate voltage induces a surface charge density: n = 0Vg te (1) where 0 and t are the permittivity and thickness of the insulating substrate, respectively, e is the electron charge and Vg is the gate voltage. It is worth noting that carrier density is accurately tuned by the gate voltage just away from the Dirac point. At the Dirac point, carrier density theoretically should be equal to zero, but thermally generated carriers and electrostatic spatial inhomogeneity limit the minimum charge density, resulting in a nite minimum conductivity, typical for each individual sample. Carrier mobility, µ , is an important parameter to quantify the eect of scattering processes from the interaction with the substrate, defects in graphene itself and temperature. Carrier mobility can be extracted from the resistivity of graphene: µ=1 enρ (2) In the lab, it is more practical to extract the eld-eect mobility: µF E =1 C dσ dVg (3) where C is the gate capacitance, σ=1 /ρ and Vg is the gate voltage. From 2 it is seen that mobility can be extracted if the resistivity is known. Experimentally, resistivity of the graphene is measured using a standard 4-probe technique, that is explained in more detail in Characterization part of the thesis (Ch. 5.1.2). 2.1.3 Synthesis The aim of graphene synthesis is to produce high carrier mobility and a low density of defects. Nowadays two main techniques to produce graphene are widely used. One technique is mechanical exfoliation which results in small (up to 1 mm [6]) graphene akes that have high mobility, but the method is random, can not be well controlled and is time consuming. Another technique, Chemical Vapor Deposition (CVD), employs a transition substrate, results in bigger areas, but the synthesized layer has more defects and usually lower mobility. 6 Mechanical exfoliation was developed by Geim and Novoselov. This technique employs highly oriented pyroelectric graphite as a precursor. There are a few techniques to obtain graphene akes, two of which were used during the project and are described in detail in the Fabrication part of the thesis (Ch. 3.2). The main idea of mechanical exfoliation is that forces acting between layers are weaker than in-plane forces between the carbon atoms and it is possible to separate stacked layers of graphite. Dierent kinds of sticky tape may be used to rip-o graphite layers. Few-layer graphene akes were found to have ballistic transport at room temperature and mobilities as high as 15 000 cm2 /Vs and 60 000 cm2 /Vs at 4 K [7]. During CVD process, carbon is supplied in gas form and a metal serves as both catalyst and substrate to grow the graphene layer. Dierent metals may be used, such as Ni, Pd, Ru or Cu. Graphene growth on copper is mostly used as it results in high mobility (up to 16 000 cm2 /Vs , [8]). During the CVD process, a 25 µm thick copper foil is heated to 1000 ° C in a ow of hydrogen at low pressure and then exposed to methane ow at particular ow and pressure. During the process the graphene layer is strained on the copper foil due to the high temperature growth [9]. Usually there is a need to transfer graphene layer from copper to the other substrate and the resulting layer contains cracks and wrinkles. Other techniques to grow graphene layer exist: thermal decomposition of SiC, molecular beam deposition and etc, result in good quality graphene with high mobility. 2.2 Graphene plasmons Plasmons are quasi particles of plasma oscillations. Surface plasmons polaritons (SPPs) are propagating solutions to Maxwell ´ s equations at a metal-dielectric interface [10]. Metal plasmonics are involved in many elds, and new applications emerge, such as optical nanoantennas [11], photonic metamaterials [12], optical biosensing [13, 14], etc. The SPP property that enables many applications is tight light connement[15]. Noble metals are known as good plasmonic materials [16], but they are hardly tunable and exhibit large Ohmic losses that limit their optical applications [15]. Graphene is an alternative plasmonic material as it provides tighter connement and long plasmon propagation distance. Graphene plasmons may be involved to enhance lightmatter interaction [17]. Moreover, graphene is a tunable plasmonic material, as doping level (carrier density) denes the plasmon resonance [18]. Recently, in [18] was reported the rst experimental launch and detection of propagating optical plasmons in tapered graphene nanostructures using near-eld scattering microscopy with infrared excitation light. Before, graphene plasmons were registered only spectroscopically [19, 20]. 7 Figure 3: Propagating and localized graphene plasmons. a) Experimental conguration for launching and detecting propagating surface waves in graphene. An AFM tip is illuminated by λ0 - infrared laser radiation. b) Near-eld amplitude image of a tapered graphene ribbon. c) Color scale image of the calculated local density of optical states (LDOS). From [18] In Figure 3 propagating and localized plasmons are imaged. A metalized AFM tip is illuminated with infrared radiation, launching plasmons into graphene. Plasmons propagate and get reected from taper edges creating interference fringes. The plasmons are detected by scattering from the AFM tip back into detector. Interference maxima are separated by half a plasmon wavelength ( λp /2). Experimentally found plasmon wavelength is 40 times smaller than the free space excitation wavelength. Due to the diraction limit, a small wavelength is desired for tight light connement. Plasmon wavelength reduction can be explained by the two-dimensionality of graphene and its unique optical conductivity: 2π λp≈ω(εr+ 1) 4πIm {σ} (4) where λp - plasmon wavelength, εr - substrate permittivity, σ - optical conductivity and ω - frequency of excitation radiation. The plasmon wavelength, for a doping level EF exceeding Ep , is given by: λp≈λ0αEF EP 4 εr+ 1 (5) where λ0 is excitation wavelength, EF - Fermi energy, Ep - plasmon energy and α - the ne structure constant, α≈1/137 . A standing plasmon wave is formed at a certain width of the taper corresponding to the resonant conditions (doping level and excitation wavelength). The interference pattern, recorded by scanning an AFM tip, is closely related to the local density of optical states 8 Precise focusing of the ion beam is important because it denes the minimal spot size that may be reached. If the focus is not sharp, the actual size of the structures is dierent form the values dened in NPVE software. In that case a smaller size of the structure may be dened in the software to compensate for imperfect focus. A test of the structure size is performed and the desired size selected (Figure 6). Dose Figure 7: Examples of the dose tests. a) A dose test on the silica. The depth is measured and the desired dose is chosen. b) A dose test on gold. A dose for the best removal of the top layer is chosen. c) A dose test of gold on silica, where not only the top layer is wanted to remove but also the certain depth of silica. The ion beam dose denes the depth of the milled structures. It is dierent for dierent material and layer thickness. A test of the dose is made before a new design is implemented, or when a new material or thickness is used (Figure 7). The resulting dose is dierent for dierent focus of the ion beam, so for precise structuring the dose should be dened each time the system is set up. Using the software, the milling dose is dened. The dose is varied by changing the dwell time or the number of scans across the structure. For smaller structures (around 50 nm), it is recommendable to make just one or two scans through the structure and vary the dwell time parameter, because it results in better quality of the structure, as more scans result in broadening of the structure. For bigger structures (in the order of 1 m m) the milling time is constant (1 m s) and the number of scans denes the total dose, as more scans result in more even distribution of used dose across the structure. Also there is possibility to choose the direction of milling (inside-out or outside-in, up or down the structure). This parameter is critical for small and precise geometry structures, for example while making nanoantennas [29]. Dierent milling direction results in dierent redeposition of the evaporated material. In order to correct for redepositing the material on top of the structures, a second scan with a smaller dose may be performed. 15 Astigmatism Correction of the astigmatism is important to attain the correct shape of the milled structures. In Figure 8 examples of astigmatism distorted structures are given. Astigmatism correction has to be performed not only for the ion beam, but also for the electron beam, because it aects the quality of the images made. Astigmatism correction is an iterative process, in the sense that after correcting the astigmatism in one direction (for example X), the focus procedure has to be repeated and then astigmatism in the other direction may be corrected and the beam focused again. The astigmatism correction procedure is repeated a few times, until a wanted result is reached. Figure 8: Examples of astigmatism distorted structures. a) Astigmatism in both spatial directions also the imaging system (the electron beam) is astigmatic b) Not well focused beam and astigmatism in both spatial directions c) Corrected astigmatism 3.1.2 Optical Lithography As mentioned before optical lithography is used for the structures that do not require nanometer precision. As nanostructures are dicult to nd in macro scale (using optical microscope), optical lithography was used in order to make markers for dening the position of the structures that were made by FIB afterward. Also pads of gold for plasmonic nanocavities were done using optical lithography. Contact lithography was used in order to reduce light diraction from the edges of the mask structures. Optical lithography includes several steps:  Spin-coating of the photo resist,  Alignment of the mask to the sample,  Exposure,  Development,  Evaporation,  Lift-o. Substrate cleaning before spin-coating resist is an important part of the process as dust particles trapped in the resist may damage the mask and also would result in a worse 16 quality of the structures. Coated substrate is aligned with the mask and then exposed with the UV light. Exposure time depends on the photo resist used and the particular device provided light ux. After exposure the sample is developed, during which, depending on the polarity of the photo resist and the mask used (pattern wanted to achieve), exposed or unexposed parts of the resist are removed. With sample baking at a certain temperature and a double exposure, it is possible to invert the structure provided by the optical mask (get negative of it). After development of the sample etching or evaporation may be performed depending if structures are wanted to be hollow or prominent. In our case we wanted to get an extra layer of gold on silica substrate so after development of the exposed resist an evaporation was performed. In order to have better gold adhesion to silica a thin layer of titanium (from 2 nm to 4 nm) is evaporated at the beginning of the process. For the use of markers 100 nm of gold was evaporated. Also the pads for purpose of contacting had to be thick enough not to be destroyed during wire bonding procedure. After the evaporation a lift-o process is performed in order to dispose metal evaporated all over the sample and leave just in those areas where resist was washed away during development. 3.2 Mechanical Exfoliation As mentioned in the rst chapter exfoliated graphene has better quality than that produced by CVD. But this method is not highly reproducible and is relatively slow. During the project, two techniques for making graphene akes were used. Figure 9: A single layer graphene ake on 90 nm of SiO2 layer Both of them include the same rst step of exfoliating a piece of graphite from one sticky tape to the other until a thin layer of graphite is reached. This process is a compromise between two goals to have thin enough layers of graphite but also to keep large coverage area. Mechanical exfoliation is a random process so the bigger the area 17 covered by graphite, the bigger the chance to nd a single layer graphene ake. Also a piece of graphite is tried to cleave in a way that as big as possible plane crystal surface is reached. Next step is graphite transfer on to the substrate. In order to be able to visualize thin akes a special substrate is used (silica on silicon). Additional contrast is given by the constructive interference between the light reected from the surface of the substrate and the lower interface of silica with silicon. In order to have constructive interference a thickness of the silica layer has to be chosen properly, usually a 285 nm or 90 nm thickness is used. One of the most important parts in mechanical exfoliation is the cleanness of the substrates. In order to check if a substrate is clean a dark eld microscopy is used. In the dark eld microscope, only light scattering objects are visible and in this case it is dirt or dust particles. For cleaning a substrate a few procedures can be performed: besides the usual chemical cleaning (acetone, isopropanol, nitrogen blow drying), samples can be cleaned in oxygen plasma cleaner or heated to 350 ° C. Also more aggressive piranha treatment could be performed. It is worth noting that oxygen plasma cleaning has not only a function of dirt etching but also chemically activating the surface for better interaction with graphene (graphite). In the rst graphene exfoliation technique a sticky tape with graphite was pressed on to the substrate and then gently brushed for about 5 min. This method did not result in a big yield of akes transferred and also the average ake dimensions were on the order of 5 µ m on 5 µ m. Flakes of this size are too small for plasmonic experiments in the mid-infrared part of the spectrum, in which the wavelength of light is on the order of 10 µ m. In order to have bigger graphene akes another technique was employed. For transfer of akes from sticky tape to the substrate an alternate method is used. A tape is pressed to the substrate trying not to have air bubbles in between. Then substrates with tapes are placed in MIBK solution on 50 ° C until the tape peels o by itself, leaving akes on the substrate. After that, the substrates are held in isopropanol for 2 min also on 50 ° C, followed by nitrogen blow drying. The next step is heating the substrates on 150 ° C for 10 - 15 min in order to evaporate the residues of the solvent. After the substrates cool down a second exfoliation can be performed during which a sticky tape is gently pressed to the substrate and with slow removal of the tape thick graphite layers are removed or thinned. The last step could be repeated a few times. The described technique resulted in a bigger yield of transferred akes as well as bigger size of graphene akes (on the order of 20 µ m by 20 µ m). Last step of mechanical exfoliation is the identication of single layer graphene akes, using optical microscopy and Raman spectroscopy. The Raman spectrum and its characteristics are presented in more detail in the 4th chapter. 18 3.3 Transfer In order to have suspended graphene, it has to be transferred on the structures. After exfoliating and characterizing a graphene ake there is a need of technique to transfer it on to the other substrate. Also CVD graphene may be transferred on patterned structures. There are a few main transfer techniques used, described in [30], [23]. 3.3.1 Transfer of graphene akes Figure 10: A single layer graphene ake with the cellulose solution on top, before the transfer. A picture is made in order to be able to recover the position of the akes when cellulose is transferred on the surface of the water. In order to transfer akes of graphene a wedging transfer technique described in [30] was used. A drop of Cellulose acetate butyrate, 30 mg /ml solved in Ethyl acetate is put on the identied ake. Then plasma treatment of the substrate for 5 s is performed in order to make surface hydrophobic. After, the cellulose solution is put around the rst drop. When cellulose gets dry the edges of it are scratched away such that water would be able to penetrate between cellulose and substrate. Next objective is to transfer cellulose solution with trapped graphene on to the surface of deionized water. A petri dish is lled with deionized water and substrate with scratched cellulose is slowly dipped at 45 º angle. Water starts slowly lifting o the edges of the cellulose, if cellulose does not lift o from the rst dipping, the procedure is repeated until it does. The pureness of the water is important in the sense that all the particles that are inside the water may contaminate graphene ake and reduce it's quality. For that reason a petri dish is cleaned in acetone and isopropanol and oxygen plasma cleaned for 30 s from both sides. A substrate on which a ake is to be transferred is cleaned thoroughly (in acetone and isopropanol for 10 min and plasma cleaned for 30 s) as the sticking of the graphene to the substrate depends on the surface properties. Substrate is sunk at the bottom of the petri 19 dish. Petri dish with oating cellulose and substrate at the bottom is placed under the microscope. Microscope is focused on the substrate and target place is positioned to the center of the eld of view. Afterwards, the focus is changed to the surface of the water, the cellulose is trapped with two needles that can be positioned with micro manipulator in 3 directions. It is hard to see graphene under cellulose as it does not have an interference enhanced contrast with the substrate. It is possible to position graphene according to the surrounding thicker graphite pieces. A focus of the ake is changed by either changing the distance to the objective or the applied force with the micro manipulator. Once the cellulose is trapped micromanipulators applied force should not be changed anymore. The water level in the petri dish is slowly reduced and the petri dish is raised towards the focus at the same velocity in order for cellulose not to lose contact with the needles. The water is removed until cellulose lands on the substrate, the most careful alignment is then performed as it is possible to see in focus the ake and the structure. It is still possible to move cellulose on the top of the substrate as there is still some water trapped, but the applied force on the needles should be chosen carefully as it may scratch the substrate. In case of silica on silicon scratching of the top layer would result in leakage while applying back gate voltage. After the water evaporates cellulose is dissolved with ethyl acetate (for half an hour on the stirring plate with around 40 turns per minute). It is important to let the water dry until no water is trapped between cellulose and the substrate as presence of water may result in ake not sticking to the substrate and being washed away with ethyl acetate. Figure 11: The sample with the transferred cellulose and graphene under it. Graphene is not visible in the picture, alignment was done according to surrounding graphite pieces. The graphene is transferred onto 4 probes for mobility measurements. 20 3.3.2 Transfer of CVD graphene It is possible to buy CVD graphene on copper as well as on silica substrate. If CVD graphene is to be transferred from silica substrate the same procedure as wedging is used while transfer from copper employs dierent transfer method. Figure 12: Schematics of CVD graphene transfer. a) CVD graphene on copper and PMMA layer before the transfer. Graphene layer from the bottom of copper is etched with oxygen plasma. b) CVD graphene on copper and PMMA layer during the etching process in FeCl 3 solution c) Glass slide with graphene and PMMA on top during the transfer from acid to water d) Graphene with PMMA on top on the surface of the water e) Graphene with PMMA on the substrate A copper foil with graphene deposited on both sides is cut in the dimensions that are needed. One side of the copper foil is etched with oxygen plasma (for 30 s). A layer of PMMA is spin-coated on the other side and baked, spin-coating and baking parameters depends on the resist used, in our case it was 3000 rpms for 30 s and 180 ° C baking for 1 minute. The PMMA layer has a protective and support function for the graphene. Other side of the copper is carefully cleaned with acetone. Next step is immersion of the copper with graphene and PMMA layer to the etching solution, in our case it was 1 molar concentration of FeCl3 acid. Other acids could be used also, but according to [31] FeCl3 etching results in slow and eective etching of copper and does not form gaseous products or precipitates. That results in better quality graphene with less wrinkles and mechanical stress. After copper is etched away and structure becomes transparent it is recommendable to leave it in etching solution for 60 - 80% of the time longer. Etching time depends on acid concentration and temperature, according to the recipe used etching was performed at 70 ° C and it usually took 40-50 min. The next step is to transfer PMMA with the graphene at the bottom to the substrate. In order to stop the etching process, PMMA is transferred on the surface of deionized water with a clean glass or silicon substrate. Then it can be transferred to the actual substrate and dried with nitrogen ow. A drop of PMMA is put on top of the transferred lm, for reduction of the mechanical stress, and let dry for about 30 min at room temperature. The last step is PMMA removal. It is important that PMMA would be removed as 21 much as possible, for that reason it might be left for a few hours in NMP at 70 ° C and then cleaned with acetone and isopropanol. 3.4 Chemical doping of graphene Beside the electrical gate doping of graphene it is possible to dope it chemically. Two mechanisms of chemical doping exist: surface transfer and substitutional doping. In surface transfer an exchange of electrons is achieved by the interaction of material that is wanted to be doped and doping material. Surface transfer doping does not disturb graphene structure and is usually reversible process, spontaneously decaying in time. Substitutional doping relies on the substitution of carbon atoms by atoms with dierent number of valence electrons. The incorporation of dierent atoms results in disruption of graphene structure and its sp 2 hybridization [32]. In the scope of the thesis surface transfer chemical doping using nitric acid was performed. Doping with nitric acid results in p-type doping. During the doping process graphene is exposed to 60 % nitric acid vapor. A beaker with 10 ml of nitric acid is placed in the plastic jar of approximate volume of 800 ml, a graphene sample is mounted underneath the lid. The doping process is temperature dependent as it determines the vapor concentration produced, in our case doping was performed in room temperature (21 º C). The time of graphene interaction with vapor determines the eect of doping, results are presented in Results section. 22 4 Characterization techniques 4.1 Raman spectroscopy Raman spectroscopy is a powerful tool for graphene characterization. Raman spectrum provides information about the electronic structure of the material. Rotational, vibrational and other low-frequency modes of the electronic system can be probed due to inelastic scattering. As vibrational modes are typical for chemical bonds, and each material has its unique Raman spectrum, this technique is usually used as an identication technique of the specic material. Graphene is one of the materials that have a typical Raman spectrum ngerprint. From Raman spectrum of graphene it is possible not only to identify the number of layers but also to judge about graphene quality or doping level. [33] Raman spectrum of the graphene has 3 typical peaks: the G band at around 1580 cm−1 , 2D peak at around 2680 cm−1 and D band at around 1350 cm−1 which is a disorder induced peak and good quality graphene does not have it. The intensity ratio of the G and D band can be used to characterize the number of defects in graphene [3]. Graphene interaction with the substrate is very important, SLG on dierent substrates has dierent Raman spectra. [34] Most commonly used substrate is silica, so typical features for graphene on silica will be presented, but it should be kept in mind that while dealing with other substrates Raman calibration should be considered. There are few features of Raman spectrum of graphene that testify it being single layer. First feature is ratio between G and 2D peaks intensity, for SLG on silica it should be not less than 2. Other typical feature is 2D peak width at FWHM and its shape. It should be not more than 35 cm−1 broad and have symmetrical Lorentzian shape. A typical Raman spectrum of SLG on SiO 2 is depicted in Figure 13. Figure 13: Typical Raman spectrum of graphene In Figure 14 change of G peak position and the ratio between G and 2D intensity 23 as a function of doping are imaged. These plots from [33] were used to estimate doping of particular sample from Raman spectra. Although in order to judge about the doping of particular sample a 4 probe measurement should be performed for calibrating doping level and shifts in Raman spectrum features as dierent substrates give dierent intrinsic doping. Figure 14: a) Position of the G peak as a function of electron and hole doping. The solid blue line is the predicted non-adiabatic trend from [35]. b) The inuence of hole and electron doping on the ratio between 2D and G peaks. From [33] 4.2 4 probes measurement 4 probes measurement is a way to measure graphene resistivity. It is possible to measure device resistance using just 2 probes, but in that case the resistance of the contacts is included. Usually contact resistance is much smaller than electronic device itself, but in graphene devices, as the resistance is small away from the charge neutrality point and the sample is small, contact resistance may dominate the measured eect. When a 4 probes measurement is done the contact resistance is subtracted, as there is a constant current owing between source and the drain and the drop of voltage between two contacts inbetween them is measured. From this measurement it is possible to dene mobility and intrinsic doping of the sample, as Dirac peak minimum position is changed with doping and the shape of the peak denes mobility. It is possible to measure back gate voltage dependence of the resistance of graphene with a fth probe contacting silicon. A typical sample schematics to measure transport properties of graphene are pictured in Figure 15. Graphene is deposited on oxidized silicon wafer, electrical contacts, usually made from gold, are deposited by lithographic processes. An applied gate voltage on the back gate creates an electrostatic potential dierence 24 Figure 20: Sample with trenches structures: a) Optical microscopy b) Photoluminescence scan c) AFM images. Dashed black line follows the boundary of bilayer graphene. Bright area in b) image is uncovered area, which is not quenched by graphene. It was possible to see graphene eect on the quantum dots from the PL measurements (Figure 20). Area that is not covered with graphene is brighter, compared with the area that is cover with bilayer graphene. Trenches are brighter, as there quantum dots are in a distance from graphene and quenching eect is decreased. It was not possible to have a reproducible result on graphene deection, as graphene membranes were not at and was dependent on surface roughness and inhomogeneities. 31 5.2 Suspended graphene nanostructures for plasmonics 5.2.1 Fabrication and characterization As mentioned in the theoretical part of the thesis next step of graphene plasmons investigation is to fabricate samples of suspended graphene and check if that increases plasmons propagation length. Gold was chosen as a substrate on which to suspend graphene as it reects plasmons from the edges, because of the dielectric contrast between gold and air. Trying to repeat the experiment described in [18], but with suspended graphene, taper shaped holes were milled with FIB in gold (40 nm) on silica on silicon substrate. The dose of the milling was chosen to remove all the gold layer. 4 dierent widths of the base of the triangles were chosen (around 500 nm, 800 nm, 1,5 m m and 2 m m) and the same length (5 m m) in order to have a dierent taper angle, to check if that aects graphene suspension on the substrate. Graphene can be suspended just on small structures, because if structure is too big graphene just follows the conformation of the substrate. Made structures are imaged in Figure 21. The pattern was repeated in order to ll bigger area that it would be more convenient for graphene ake transfer (easier to position a ake and possible to see structures with optical microscope). Figure 21: Triangle shape holes in gold of 4 dierent width to length ratios After a ake transfer and imaging with AFM we could conclude that graphene was suspended just up to 500 nm width of the taper and for the bigger width it was collapsing inside the taper and touching silica. Sample was investigated with scattering-type scanning near-eld optical microscopy and no plasmons could be visualized. The width of 500 nm is not enough to see the propagating plasmons. There was a need of designing dierent structure in order to keep graphene suspended up to bigger widths of the taper. The structure that could support graphene is a bridge. Tapers with bridges starting from 500 nm width of the taper and repeated every 200 nm (after the width of the taper 32 increased to 2 m m, every 100 nm) were made. The maximum width of the taper is 3 m m and length 10 m m. Taper pattern was repeated for the same reasons as mention before. The bridges for graphene support are 40 nm wide. The dose of the milling was chosen sucient to remove all the layer of gold (around 40 nm). The challenge of making this kind of structure is that bridges are removed while milling structures of just 200 nm or 100 nm close to each other (Figure 22). FIB milling current of 2 pA and 30kV acceleration voltage were used in order to have precise structures. A few tests were made in order to dene the distance between the trapeziums that would result in not removed gold in between them. Figure 22: Taper structures with bridges for supporting graphene suspension After exfoliated graphene transfer on the mentioned structures, AFM imaging showed suspended graphene with around 15 nm sagging inside the structure (Figure 23). Graphene collapsed in some of the trenches, but then other bridges were supporting graphene in the next trenches. Graphene got suspended up to 2 m m width of the taper, that would be enough to image plasmons. In order to tune plasmon resonance it is necessary to change the doping of graphene. It is not clear how suspended graphene on gold would react to doping with changing back gate voltage. There are two eects that are aecting doping in suspended graphene, one is that carriers from gold are diusing to graphene and giving 33 it intrinsic doping and the other eect is gold screening the applied electrical eld and reducing the eective length of the graphene where electric eld is induced. The sum of these eects may limit the eect created with back gate voltage. Raman spectroscopy was chosen as a tool to monitor change of graphene doping. Back gate voltages up to 60 V were applied recording Raman spectrum for dierent voltages. There was no noticeable doping up to 24 V and after applying 60 V sample started leaking, so no conclusive results were achieved. Figure 23: AFM images of graphene on tapers with bridges for support In order to reduce the eect of gold screening the thickness of the gold layer was reduced to 10 nm for the next sample. The spacing between the bridges was increased to 400 nm in order to have bigger suspended graphene areas. The depth of the structures was chosen to be around 100 nm, for that reason not only gold but part of the silica layer had to be milled. The new conguration of the structure was giving a new challenge, as the thinner gold layer is easily destroyed with ions and while milling even deeper to the silica it is complicated to leave golden bridges not aected. After a few test the milling parameters of the FIB and structure geometry were dened that were resulting in wanted structures (2 pA milling current and 30 kV acceleration voltage, 0,2 nC / m m 2 dose, that was achieved with many scans of 1 m s). Mechanically exfoliated ake was transferred on the top of the mentioned structures. AFM images (Figure 24 and Figure 25) show suspended graphene. It is seen that graphene does not form a at and uniform membrane, but rather wrinkled and stretched at the support bridges interface. Repeating the trend noticed from the previous sample graphene 34 collapses in some of the trenches and always in the rst narrowest triangle. The wrinkles tend to point toward the collapsed trenches indicating induced mechanical stress. Raman experiment with applied dierent back gate voltages was repeated for this sample. Results are presented in the next section, comparing them with a control sample of CVD graphene. Figure 24: AFM images of the suspended single layer graphene on taper structure with the bridges for graphene support Figure 25: AFM images of the suspended single layer graphene structures with better resolution. Graphene does not form a at and uniform membrane, but rather wrinkled and stretched at the support bridges interface. By designing the structure with support bridges we made freestanding graphene with widths up to ∼ 2 m m. 35 5.2.2 Doping In theoretic part of the thesis two ways to change carrier concentration in graphene were presented. Both methods are relative for dierent applications, in the scope of the project there was a need to induce doping, control and dene it. Experimental results are presented in this section. Back gate doping Figure 26: Raman spectra of the CVD graphene Hall bar sample. The curves are oset for clarity. As we were not sure if we would be able to see back gate doping on suspended graphene structures due to gold screening and diusion of the carriers to the graphene, a test of the Raman measurement was done on a CVD graphene sample. CVD graphene was etched and contacted to form a Hall bar. In Figure 26 Raman spectra for 4 dierent back gate voltages is presented, spectra were measured while increasing voltage. In order to avoid sample damage with increase of voltage, it was increased in 0.02 V steps. It was noticed that spectra response is not the same while increasing back gate voltage and for the spectra taken while decreasing the voltage. We were paying attention to the G peak position and ratio between G and 2 D peaks, as these parameters indicate the change of doping [33]. The resolution of the spectrometer used (inVia Raman microscope, by Renishaw) is 1 cm−1 , the G peak shifts noticed were less than the resolution, but applying Lorentzian ts to the data it is possible to see 36 G peak position change (Figure 28, Figure 27) for both, CVD graphene Hall bar and suspended graphene samples. Figure 27: G peak of the CVD graphene Hall bar sample. Solid lines are Lorentzian ts. The curves are oset for clarity. 37 Figure 28: G peak of the suspended graphene structures on gold. Solid lines are Lorentzian ts. The G peak changes position with applied voltage, indicating a change in the carrier density in graphene. The curves are oset for clarity. In Figure 29 G the peak position and the ratio between G and 2 D peak intensity for the CVD graphene Hall bar sample and the sample with suspended graphene are presented. Values are not the same for increasing and decreasing voltage, indicating a drift of the Dirac peak (e.g. due to air exposure). Therefore, the observations are not 100% conclusive. The trend for CVD graphene and suspended graphene samples is evident, as while increasing voltage G peak position shifts to lower values and ratio between the intensity of G and 2 D peaks gets higher, and while decreasing back gate voltage G peak position keeps slowly shifting to lower values. The ratio between G and 2D peaks intensity 38 acts dierent while decreasing back gate voltage: it keeps getting higher for CVD Hall bar sample and decreases for suspended graphene sample. Figure 29: G peak position change with applied back gate voltage: a) For CVD graphene Hall bar sample c) for suspended graphene structures on gold; Intensity ratio between G and 2D peaks change with applied back gate voltage: b) For CVD graphene Hall bar sample d) for suspended graphene structures on gold. Dierent data sets for the values while increasing and decreasing voltage. Chemical doping An alternative to back gate doping is chemical doping. Chemical doping is not an interactive way to dope graphene, but it may result in much higher doping and it does not require contacting of graphene. CaF2 was chosen as a new substrate, as it does not absorb radiation in the mid-infrared and is often used as an optics material for applications in this range of wavelengths. In Figure 30 normalized Raman spectra of single layer graphene on CaF2 before and after 17 minutes of chemical doping with nitric acid vapor is presented. A G peak position shift of 5 cm−1 was achieved and the ratio between 2D and G peaks decreased from 10 to 2,7 (Figure 31). Relating the induced G peak position shift with the graphene doping results presented in [33] (Figure 14), the corresponding Fermi energy shift is found to be ∼ 200 meV. The change of the ratio between 2D and G peaks could not be compared as it is highly substrate dependent. In the mentioned experiment the substrate is silica and in our case it is CaF 2 . The drawback of chemical doping is that the induced eect decreases in time (data is presented in Appendix). 39 Figure 30: Single layer graphene spectra before and after chemical doping with nitric acid. The G peak is aected by the chemical treatment. Figure 31: G peak of single layer graphene before and after chemical doping with Lorentzian ts. Induced G peak shift due to doping is 5,02 cm −1 . The height of the peak is reduced by the factor of ∼ 3 due to doping. 5.3 Mobility measurement High mobility is essential for plasmonic applications of graphene. In order to estimate mobility of the graphene that may be reached with our mechanical exfoliation and wedging 40 Figure 39: 4 probes measurement results after 3 weeks. a) Resistance dependence on back gate voltage. b) Mobility dependence on back gate voltage. Highest mobility is 1000 cm2 /V·s , indicating that graphene mobility decreases in time, although sample was stored in controlled temperature and humidity atmosphere. 47 References [1] S. V. Morozov D. Jiang Y. Zhang S. V. Dubonos I.V. Grigorieva K. S. Novoselov, A. K. Geim and A. A. Firsov. Electric eld eect in atomically thin carbon lms. Science , 306:666, 2004. [2] N. M. R. Peres K. S. Novoselev A. H. Castro Neto, F. Guinea and A. K. Geim. The electronis properties of graphene. Reviews of Modern Physics , 81:109162, 2009. [3] N. Ghattamaneni B. Harack M. Hilke A. Horth N. Majlis M. Massicotte L. Vandsburger E. Whiteway D. R. Cooper, B. D'Anjou and V. Yu. Experimental review of gra. asXiv:1110.6557v1 [cond-mat.mes-hall] , 2011. [4] A. K. Geim and K. S. Novoselov. The rise of graphene. Nature M , 6:183, 2007. [5] E. Rimini V. Raineri and F. Giannazzo. Mesoscopic transport properties in exfoliated graphene on sio2/si. Nanosience and nanotechnology letters , 3:5558, 2011. [6] A. K. Geim. Graphene: Status and prospects. Science , 324:15301534, 2009. [7] S. V. Morozov D. Jiang M. I. Katsnelson I. V. Grigirieva S. V. Dubonos K.S. Novoselov, A. K. Geim and A. A. Firsov. Two-dimensional gas of massless dirac fermions in graphene. Nature , 438:197, 2005. [8] A. Venugopal J. An J. W. Suk B. Han M. Borysiak W. Cai A. Velamakanni Y. Zhu L. Fu E. M. Vogel E. Voelkl L. Colombo X. Li, C. W. Magnuson and R. S. Ruo. Graphene lms with large domain size by a two-step chemical vapor deposition process. Nano Letters , 10:43284338, 2010. [9] J. Maassen V. Yu, E. Whiteway and M. Hilke. Straining graphene bu chemical vapour deposition on copper. ArXiv: 1101 1884v1 , 2011. [10] M. Spasenovic. Surface plasmon polaritons and light at interfaces: propagating and evanescent waves . PhD thesis, Institute for atomic and molecular physics (AMOLF), 2011. [11] N. van Hulst L. Novotny. Antennas for light. Nature Photonics , 5:8390, 2011. [12] L. Jiang J. Y. Ou, E. Plum and N. I. Zheludev. Recongurable photonis metamaterials. Nano Letters , 11:21422144, 2011. [13] H. Kneipp L. T. Perelman I. Itzkan R. R. Dasari K. Kneipp, Y. Wang and M. S. Feld. Single molecule detection using surface-enhanced raman scattering. Physical Review Letters , 78:16671670, 1997. 48 [14] C. Oubre N. K. Grady C. Hollars S. M. Lane T. R. Huser P. Nordlander C. E. Talley, J. B. Jackson and N. J. Halas. Surface-enhanced raman scattering form induvidual au nanopraticles and nanoparticles dimer substrates. Nano Letters , 5:15691674, 2005. [15] D. E. Chang F. H. L. Koppens and F.J. Garcia de Abajo. Graphene plasmonics: a platform for strong light-matter interactions. Nano , 11:33703377, 2011. [16] G. V. Naik N. K. Emani V. M. Shalaev P. R. West, S. Ishii and A. Boltasseva. Searching for better plasmonic materials. Laser Photonics , 4:795808, 2010. [17] F. H. L. Koppens S. Thongrattanasiri and F. J. Garcia de Abajo. Complete optical absorption in periodically patterned graphene. Physical Review Letters , 108, 2012. [18] P. Alonso-Gonzalez S. Thongrattanasiri F. Huth J. Osmond M. Spasenovic A. Centeno A. Pesquers P. Godignon A. Zurutuza Elorza N. Camara F. J. Garcia de Abajo R. Hillenbrand J. Chen, M.Badioli and F. H. L. Koppens. Optical nano-imaging of gate-tunable graphene plasmons. Nature , 487:7781, 2012. [19] T. Seyller K. Horn A. Bostwick, T. Ohta and E. Rotenberg. Quasiparticle dynamics in graphene. Nature Physics , 3:3640, 2007. [20] R. R. Nair R. Jones M. Gass A. L. Bleloch K. S. Novoselov A. Geim T. Eberlein, U. Bangert and P. R. Briddon. Plasmon spectroscopy of free-standing graphene lms. Physical Review B , 77:233406, 2008. [21] H. Buljan M. Jablan and M. Soljacic. Plasmonics in graphene at infrared frequencies. Physical Review B , 80:245435, 2009. [22] Sikes Z. Jiang M. Klima G. Fudenberg J. Hone P. Kim H. L. Stormer K. I. Bolotin, K. J. Ultrahigh electron mobility in suspended graphene. Solid State Communications , 146:351355, 2008. [23] I. Meric C. Lee L. Wang S. Sorgenfrei K. Watanabe T. Taniguchi P. Kim K. L. Shepard C. R. Dean, A. F. Young and J. Hone. Boron nitride substrates for high-quality graphene electronics. Nature N , 5:711726, 2010. [24] R. Kim M. Freitag T. Low, V. Perebeinos and P. Avouris. Cooling of photoexcited carriers in graphene by internal and substrate phonons. Physical Review B , 86, 2012. [25] H. Y. Chiu M. Engel A. A. Bol R. Krupke M. Burghard K. Kern R. S. Sundaram, M. Steiner and P. Avouris. The graphene-gold interface and its implications for nanoelectronics. Nano Letters , 11:38333837, 2011. 49 [26] K. Kurihara K. Iwadate H. Namatsu, M. Nagase and K. Murase. 10 nm silicon lines fabricated in (110) silicon. Microelectron Eng , 27:71, 1995. [27] Kuo-Dong Huang Shu-Fen Hu, Chin-Lung Sung and Yue-Min Wan. Proximity eect of electron beam lithography for single-electron transistor. Applied Physics Letters , 85:3893, 2004. [28] Instruction Manual AURIGA series . [29] L. Neumann. Control of optical elds and single photon emitters by advanced nanoantenna structures . PhD thesis, ICFO - Institute of Photonic Sciences, 2012. [30] H. Zandbergen-L. M. K. Vandersypen G. F. Schneider, V. E.Calado and C.Dekker. Wedging transfer of nanostructures. Nano Letters , 10:19121916, 2010. [31] H. Kim C. Mattevi and M. Chhawalla. A review of chemical vapour deposition of graphene on copper. Journal of Mate , 21:33243334, 2011. [32] Y. Liu H. Liu and D. Zhu. Chemical doping of graphene. Journal of Materials Chemistry , 21:33353345, 2010. [33] B. Chakraborty S. Piscanec S. K. Saha U. V. Waghmare K. S. Novoselov H. R. Krishnamurthy A. K. Geim A. C. Ferrari A. Das, S. Pisana and A. K. Sood. Monitoring dopants by raman scattering in an electrochemically top-gated graphene transistor. Nature Nanotechnology , 3:210215, 2008. [34] T. Yu Z. Ni, Y. Wang and Z. Shen. Raman spectroscopy and imaging of graphene. Nano Res , 1:273291, 2008. [35] C. Casiraghi K.S. Novoselov A. K. Geim A. C. Ferrari S. Pisana, M. Lazzeri and F. Mauri. Breakdown of the adiabatic born-oppenheimer approximation in graphene. Nature Mater , 6:198201, 2007. [36] A. Liscio M. Gazzano P. Samori E. Treossi, M. Melucci and V. Palermo. Highcontrast visualization of graphene oxide on dye-sensitized glass, quarts, and silicon by uorescence quenching. Journal of American Chemical Society , 131:1557615577, 2004. [37] F. Kim W. Yuan K. R. Shull J. Kim, L. J. Cote and J. Huang. Graphene oxide sheets at interfaces. Journal of American Chemical Society , 132:81808186, 2010. [38] C. Nuckolls T. F. Heinz Z. Chen, S. Berciaud and L. E. Brus. Energy transfer from individual semiconductor nanocrystals to graphene. ACS nano , 4:2964, 2010. 50 [39] G. Gomez-Santos and T. Stauber. Fluorescence quenching in graphene: A fundamental ruler and evidence for transverse plasmons. Physical Review B , 84, 2011. [40] B.N.J Persson and N.D. Lang. Electron-hole-par quenching of excited states near a metal. Physical Review B , 26:54095415, 1982. [41] Kevin Schaedler. Detection of graphene motion through light-matter interactions. Master's thesis, Institute of Photonic Sciences (ICFO), 2012. [42] Z. Q. Wang C. L. Wong, M. Annamalai and M. Palaniapan. Characterization of nanomechanical graphene drum structures. Journal of Micromechanics and Microengineering , 20:115029, 2010. 51