Shear strength of reinforced concrete beams with FRP longitudinal and transverse reinforcement
Full text
TESI DE MÀSTER Master MÀSTER UNIVERSITARI EN ENGINYERIA DE CAMINS, CANALS I PORTS Títol SHEAR STRENGHT OF REINFORCED CONCRETE BEAMS WITH FRP LONGITUDINAL AND TRANSVERSAL REINFORCMENET Autor SANDRA ANDREEA GRADINARU Tutors EVA OLLER IBARS DENISE CARINA SANTOS FERREIRA Departament ENGINYERIA DE LA CONSTRUCCIÓ Intensificació ESTRUCTURES Data Julio 2015
ABSTRACT During the last decades the use of fiber reinforced polymers (FRP) has been introduced in the field of structural engineering, first as external reinforcement and later as passive and active reinforcement. The emergent interest in this material is due to its many advantages compared with the steel: it is more resistant and durable against corrosion, as well as, lighter and magnetically inert. These qualities allow decreasing the complexity complex and cost of the reinforcement construction tasks while allowing the service life of structures to increase. Nowadays, general shear resistance mechanisms in reinforced concrete are still under discussion. Specifically the use of FRP as shear reinforcement for concrete structures has not yet been deeply studied and the currently available data are insufficient to formulate rational design guidelines. The effects of shear on the response of concrete beams with longitudinal and transversal FRP reinforcement is numerically studied in this work through a 1D non-linear fiber model accounting for the axial–bending–shear interaction. Experimental data from FRP RC beams available in literature, are compared with the numerical results. As this beam model is shear sensitive, the effects of shear in the structural response are evaluated. A good correlation in terms of ultimate loads, deflections, strains in the concrete and reinforcement is observed between the experimental data and the computed results. The numerical model is also able to reproduce the cracking widths and pattern when increasing the applied load. Once the model is validated, it can be used to assess the accuracy of the analytical expressions present in the current codes of practice and contribute for their enhancement. Keywords: nonlinear numerical modeling, shear, FRP stirrups, reinforced concrete. i
Table of Contents ABSTRACT ........................................................................................................................................... i List of figures .................................................................................................................................... v List of tables .................................................................................................................................. viii 1 Introduction ............................................................................................................................ 1 1.1 Problem statement .......................................................................................................... 1 1.2 Objectives ......................................................................................................................... 2 1.3 Structure of the thesis ...................................................................................................... 3 2 Beams reinforced with longitudinal and transversal FRP bars ............................................. 4 2.1 FRP bars ............................................................................................................................ 4 2.1.1 Properties of the constituent materials ................................................................ 4 2.1.2 Properties of composite materials ....................................................................... 10 2.2 Existing experimental programs of shear tests on concrete beams reinforced with longitudinal and transversal FRP ............................................................................................... 13 2.3 Analytical formulations for shear resistance of FRP reinforced concrete elements ..... 19 2.3.1 (ACI-440.1R-06) ....................................................................................................... 22 2.3.2 (CNR-DT 204/2006) ................................................................................................. 23 2.3.3 (JSCE 1997) .............................................................................................................. 24 2.3.4 (CSA S806-12) .......................................................................................................... 25 2.3.5 Proposal by (Fico et al. 2008) .................................................................................. 27 2.3.6 Proposal by (Nehdi et al. 2007)............................................................................... 28 2.3.7 Proposal by (Hegger et al. 2009) ............................................................................. 28 ii
3 Non-linear shear-sensitive fiber beam model ..................................................................... 30 3.1.1 Structural scheme ................................................................................................... 30 3.1.2 Finite element ......................................................................................................... 31 3.1.3 Sectional level ......................................................................................................... 32 3.1.4 Material models ...................................................................................................... 32 3.1.5 Representation of cracks ........................................................................................ 34 4 Numerical analysis of FRP RC beams ................................................................................... 35 4.1 Description of the experimental campaign .................................................................... 35 4.1.1 General .................................................................................................................... 35 4.1.2 Materials ................................................................................................................. 36 4.1.3 Geometry ................................................................................................................ 37 4.1.4 Experimental setup for shear tests ......................................................................... 39 4.1.5 Failure modes .......................................................................................................... 41 4.2 Numerical model ............................................................................................................ 47 4.3 Comparison of numerical and experimental results ...................................................... 50 4.3.1 Test beam: S6BN-0.8-11 ......................................................................................... 50 4.3.1.1 Load vs. displacement ..................................................................................... 52 4.3.1.2 Strains in the FRP longitudinal reinforcement ................................................ 53 4.3.1.3 Strains in the FRP transversal reinforcement .................................................. 54 4.3.1.4 Longitudinal strains in concrete ...................................................................... 55 4.3.1.5 Transversal strain in the concrete web ........................................................... 56 4.3.1.6 Crack patterns .................................................................................................. 56 4.3.1.7 Other numerical results ................................................................................... 59 iii
4.3.2 Other tests beams ................................................................................................... 61 4.3.2.1 Load vs displacement ...................................................................................... 61 4.3.2.2 Strains in the FRP longitudinal reinforcement ................................................ 62 4.3.2.3 Strains in the FRP transversal reinforcement .................................................. 63 4.3.2.4 Longitudinal strains in concrete ...................................................................... 65 4.3.2.5 Transversal strain in the concrete web ........................................................... 66 5 Conclusions............................................................................................................................ 67 References .................................................................................................................................... 70 iv
List of figures Figure 1: Basic material components that are combined to create an FRP composite (BaNthia et al. 2006) .......................................................................................................................................... 4 Figure 2: Diagram stress-strain of FRP (BaNthia et al. 2006).......................................................... 5 Figure 3: Stress-strain properties of typical fibers.(BaNthia et al. 2006) ....................................... 7 Figure 4: failure in stirrups at the bent zone of L05-1 (Bentz et al. 2010) .................................... 16 Figure 5: Flexural compression failure in constant moment region of L20-2(Bentz et al. 2010) . 16 Figure 6: Types of shear failure in experimental trials(Spadea 2010) .......................................... 17 Figure 7: Limiting strain according to the Strain Approach(Clarke 1996) .................................... 21 Figure 8: General characteristics of the fiber beam models (Ferreira 2013) ............................... 31 Figure 9: Fiber beam model in CONSHEAR: a) general characteristics b) finite element for the 2D case (Ferreira 2013) ................................................................................................................. 31 Figure 10: Assumptions of the model at the section level (Ferreira 2013) .................................. 32 Figure 11: Constitutive model for the concrete: (a) smeared crack, (b) compression, (c) tension (Ferreira 2013) .............................................................................................................................. 33 Figure 12: Constitutive model for the reinforcement (Ferreira 2013) ......................................... 33 Figure 13: Scheme of the post-processing method for the representation of the cracks (Ferreira 2013) ............................................................................................................................................. 34 Figure 14: Experimental tests on the beam (Kurth 2012) ............................................................ 35 Figure 15: Reinforcement drawing (Kurth 2012) .......................................................................... 38 Figure 16: Type of stirrups (Kurth 2012) ....................................................................................... 38 Figure 17: Experimental set-up of shear tests (Kurth 2012) ........................................................ 39 Figure 18: Metrology of concrete (Kurth 2012) ............................................................................ 40 v
Figure 19: Metrology of reinforcement (Kurth 2012) ................................................................... 41 Figure 20: Cracking at failure in experimental S4AH-0.8-7 (rw = 0.75%, fcm =42.2 N/mm2 (Kurth 2012) ............................................................................................................................................. 41 Figure 21: Damaged stirrups (Type A and B) after failure in experiments with a shear reinforcement degrees ρw of 0.75% (Kurth 2012) ........................................................................ 42 Figure 22: Damaged double headed bolt (type C) after failure while trying S12CH-0.7-23 (ρw = 0.75%, fcm = 73.1 N / mm²)(Kurth 2012) ....................................................................................... 42 Figure 23: Cracking at failure in experimental S6BN-2.3-12 (ρw = 2.26%, fcm = 30.7 N / mm²)(Kurth 2012) ......................................................................................................................... 43 Figure 24: Cracking at failure in experimental S2AN-2.3-4 (ρw = 2.26%, fcm = 33.5 N / mm²)(Kurth 2012) ......................................................................................................................... 43 Figure 25: Discretization of the cross section ............................................................................... 47 Figure 26: Shear resistant zone .................................................................................................... 47 Figure 27: Discretization of the beam ........................................................................................... 48 Figure 28: Longitudinal and transversal reinforcement of the test beams (Kurth 2012) ............ 49 Figure 29: FRP stirrups configurations (Kurth 2012) .................................................................... 49 Figure 30: Plan of reinforcement for test beam: S6BN-0.8-11(Kurth 2012) ................................ 50 Figure 31: Beam cross-sections for test beam: S6BN-0.8-11(Kurth 2012) ................................... 50 Figure 32: Metrology of concrete and sensors considered for comparison with the numerical results (Kurth 2012) ...................................................................................................................... 51 Figure 33: Metrology of reinforcement and sensors considered for comparison with the numerical results(Kurth 2012) ...................................................................................................... 51 Figure 34: Experimental and numerical deflection in the center of the beam for test S6BN-0.8- 11 .................................................................................................................................................. 52 vi
Figure 35: Experimental and numerical results for the strains in longitudinal FRP reinforcement for test S6BN-0.8-11 ...................................................................................................................... 53 Figure 36 : Experimental and numerical results of Strains in stirrups along the length of the beam for test S6BN-0.8-11 ........................................................................................................... 54 Figure 37: Experimental and numerical results of concrete deformation for test S6BN-0.8-11 . 55 Figure 38: Shear-strain of concrete numerical and experimental results for test S6BN-0.8-11 .. 56 Figure 39: Cracking width for test S6BN-0.8-11............................................................................ 58 Figure 40: Location of measured cracks ....................................................................................... 58 Figure 41: Strain in the stirrups for different positions of the sensors test S6BN-0.8-11 ............ 59 Figure 42: Strains in stirrup height at the bent zone for testS6BN-0.8-11 ................................... 60 Figure 43: Experimental and numerical deflection in the center of the beam for tests S2AN-0.8- 3, S4AH-0.8-7, S8BH-0.8-15 and S10CN-0.7-19 ............................................................................ 61 Figure 44: Experimental and numerical results of strains in the FRP longitudinal reinforcmenet for tests S2AN-0.8-3, S4AH-0.8-7, S8BH-0.8-15 and S10CN-0.7-19 .............................................. 62 Figure 46: Experimental and numerical results of strains in stirrups along the length of the beam for tests S2AN-0.8-3, S4AH-0.8-7, S8BH-0.8-15 and S10CN-0.7-19 .............................................. 64 Figure 45: Experimental and numerical results of longitudinal concrete deformation for tests S2AN-0.8-3, S4AH-0.8-7, S8BH-0.8-15 and S10CN-0.7-19 ............................................................ 65 Figure 47: Numerical and experimental of transversal strain in the concrete web results for tests S2AN-0.8-3, S4AH-0.8-7, S8BH-0.8-15 and S10CN-0.7-19 ............................................................ 66 vii
List of tables Table 1: Properties of the composite matrix (Alzate 2012) ............................................................ 6 Table 2: Properties of the glass fibers (Feldman 1989, Kim 1995) ................................................. 8 Table 3: Properties of the carbon fibers (Feldman, 1989) .............................................................. 9 Table 4: Properties of the aramid fibers (Feldman, 1989) ............................................................. 9 Table 5: Properties of fiber reinforced polymers ......................................................................... 12 Table 6: Limit strain value(Fico et al. 2008) .................................................................................. 27 Table 7: Characteristics of longitudinal reinforcement (Kurth 2012) ........................................... 36 Table 8: Characteristics of transversal reinforcement (Kurth 2012) ............................................ 37 Table 9: Types of failure for the experimental beams .................................................................. 44 Table 10: Beam dimensions, concrete properties, longitudinal reinforcement, and transversal reinforcement(Kurth 2012) ........................................................................................................... 46 Table 11: Cracking patterns at different load levels for test S6BN-0.8-11 ................................... 57 viii
fibers for specific applications depends on a number of factors including the required strength, the stiffness, durability considerations, cost constraints, and the availability of component materials. Figure 3 shows typical stress-strain curves for various types of fibers. Note that these curves are for the pure fibers only, and they do not include the effects of the polymer matrix. Figure 3: Stress-strain properties of typical fibers.(BaNthia et al. 2006) It can be observed that FRP materials, unlike steel, do not offer plasticity, and have a linearelastic behaviour till rupture; also present a higher ultimate strength than conventional steel. As can be observed in Figure 3, the modulus of elasticity of the glass and aramid fibers is lower than that of steel; the standard carbon and high-modulus carbon fibers present very similar elasticity modulus, and ultra-high modulus carbon is clearly superior. It can also be seen that, while the ultimate strength of aramid, glass and ultra-high modulus carbon fibers are very similar, the standard carbon fibers strength is far superior. Contrasting with the ductile response exhibited by steel, FRP fibers do not yield before failure, presenting small deformations near failure; this is the reason why most codes and analytical models limit the deformation of FRP to avoid brittle failures. 7
Typical FRP reinforcement products are grids, bars, fabrics, and ropes. The bars have various types of cross-sectional shapes (square, round, solid, and hollow) and deformation systems (exterior wound fibers, sand coatings, and separately formed deformations). Subsequently, the 3 types of fiber studied are presented in more detail. o Glass fibers Glass fibers are the most economical, and consequently the most commonly used fibers in structural engineering applications. They are characterized by their high strength, low thermal conductivity and low stiffness that can lead to excessive deformations in structures reinforced with this type of material. There are several different grades available, but the most common are E-glass and the more expensive, but stronger, R-glass. Table 2 shows the typical range of values of the mechanical properties of these types of fiber. Type Modulus of elasticity (GPa) Tensile Strength (GPa) Ultimate strain (%) E 70 1.9 – 3.0 3.0 – 4.5 S 85-90 3.5 – 4.8 4.5 – 5.5 Table 2: Properties of the glass fibers (Feldman 1989, Kim 1995) o Carbon fibers The carbon fibers have a very high ultimate strength, and are used to replace glass in those cases where the stiffness of the latter are insufficient, since the elastic modulus of the carbon fibers is considerably greater. This material has a high price due to the difficulty and cost of its production process. It presents a good resistance to thermal, chemical, and environmental effects, also good fatigue behaviour. Carbon fibers are an ideal choice for structures which are weight and/or deflection sensitive. 8
There are 2 types of carbon fiber: the high resistance (RH) and high modulus (HM) whose characteristics are shown in Table 3. Type Modulus of elasticity (GPa) Tensile Strength (GPa) Ultimate strain (%) HR 215 – 235 3.5 – 4.8 1.4 – 2.0 HM 350 – 500 2.5 – 3.1 0.5 – 0.9 Table 3: Properties of the carbon fibers (Feldman, 1989) o Aramid Aramid fibers are characterized by high strength and good fatigue behaviour. They have a high modulus of elasticity, showing little deformation at failure. However, despite having a high tensile resistance, the compressive behaviour is not linear and ductile. They have an anisotropic structure, which have better performance in the direction of the fiber and are industrially available in both continuous and discontinuous form. This material presents resistance to chemical attacks, but has low resistance to ultraviolet radiation. Its common mechanical characteristics are indicated in Table 4. Type Modulus of elasticity (GPa) Tensile Strength (GPa) Ultimate strain (%) High module 115 – 130 3.5 – 4.0 2.5 – 3.5 Low module 70 – 80 3.5 – 4.1 4.3 – 5.0 Table 4: Properties of the aramid fibers (Feldman, 1989) 9
2.1.2 Properties of composite materials The properties of the resulting composite material will be conditioned by the type of matrix and the type of fiber chosen and by the volumetric amount and orientation. Thereof the modulus of elasticity of the composite material can be obtained by applying the so-called "rule of mixtures", which allows to express the properties of a compound according to the properties of materials that comprise it (in this case the matrix and fibers) and their volume fractions. This requires making the assumption that the bond between the fiber and the matrix is perfect, so there is no discontinuity in the deformation ε through the interface when a tensile or compressive load is applied in the direction parallel of the fibers. Hence, compatibility of deformations is assumed: (2.1) If the materials are considered perfectly elastic, the stresses σ can be calculated as: (2.2) (2.3) The load supported by the composite Fc can be expressed as the sum of the loads carried by the matrix Fm and the fibers Ff, according to the following expression: (2.4) In terms of stress σ: (2.5) With Ac , Am , Af representing respectively the sectional areas of the composite , the matrix , and fiber. 10
Dividing equation (2.5) by Ac results in: (2.6) Where the following expression of volume fractions V can be set as: (2.7) (2.8) Rewriting equation (2.6) comes: (2.9) Where Ec is the elastic modulus of the composite, Em the elastic modulus of the matrix, and Ef the elastic modulus of the fiber. And, since the volume of the matrix Vm plus the volume of the fibers Vf is equal to 1: (2.10) Equation (9) can be rewritten as: (2.11) Consequently the elastic modulus of FRP composite material can be obtained as the sum of the modulus of elasticity multiplied by their volume fractions components. FRP products are characterized by having an elastic behaviour to failure, and to develop a high tensile strength (greater than steel) in the direction of the fibers. This anisotropy considerably affect the shear strength, which is very small compared to the tensile strength. 11
In summary, the main advantages of FRP as structural reinforcement material are: o High resistance to corrosion; o Lightweight; o High tensile resistance; o reduced installation time and cost; o Low maintenance; o Good behaviour to fatigue. There are also some disadvantages that must be taken into account in the design in order to avoid inadequate structural response, such as: o Brittle failure because there is no plastic branch and therefore no ductility; o Lower modulus of elasticity or similar to steel, that may lead to high deformations; o High cost; o High vulnerability of the matrix at elevated temperatures. The reduced weight of the fibers compared to steel and concrete and their high resistance / weight ratio is one of the characteristics that make them more attractive to structural applications. This allows not only significant savings in material (which is very significant because of its high cost) but also facilitates the construction process. Table 5 summarizes the main characteristics of composite materials FRP. Unidirectional composite materials Fiber weight (%) Density (kg/m3) Tensile elastic module (GPa) Tensile Strength (GPa) Glass-Polyester(GFRP) 50-80 1600-2000 20-55 400-1800 Carbon-Epoxy (CFRP) 65-75 1600-1900 120-250 1200-2250 Aramid-Epoxy(AFRP) 60-70 1050-1250 40-125 1000-1800 Table 5: Properties of fiber reinforced polymers 12
2.2 Existing experimental programs of shear tests on concrete beams reinforced with longitudinal and transversal FRP The use of FRP as reinforcing material in structural concrete is relatively new. Several research groups worldwide are recently dedicated to the experimental and numerical study of the structural behaviour of concrete elements reinforced with FRP. As bending behaviour in RC is seen as solved by the actual state-of-the-art, the main concern now is shear. This is the reason why this work is focused on shear tests. In conventionally steel RC beams, there are different failure modes depending on the longitudinal and transversal reinforcement ratios and on the shear span to depth ratio. FRP RC beams with FRP stirrups present different failure modes due to the linear elastic behaviour of the FRP reinforcement. In steel RC beams, if the longitudinal reinforcement ratio is low, failure may be often due to a flexural-shear mechanism. Usually, first flexural cracks initiate, and subsequently develop inclined through the web. As the load increases, damage concentrates around the so-called shear critical crack. After increasing the applied load, a second branch of the crack develops inside the concrete chord, eventually connecting the first crack and the point where the load is applied, producing failure. For this type of failure, the increment of tensile force in the longitudinal reinforcement due to the inclined crack, which depends on the shear force, will commonly produce yielding of the longitudinal reinforcement. This is not the case for FRP longitudinal reinforcement, which is linear elastic up to failure, and which has an ultimate tensile strength higher than the steel yielding stress. In addition, designers are often required to use FRP longitudinal reinforcement ratios higher than the balanced reinforcement ratios to meet the serviceability criteria. If the longitudinal reinforcement ratio is high enough, the transversal steel stirrups of steel RC beams might yield, and concrete chord crushing can be observed (brittle shear failure). This 13
type of failure can also develop in FRP RC beams with FRP stirrups. However, in this case, concrete crushing will occur if the FRP stirrups do not have previously failed locally in the bent zone. Finally, in thin-walled beams, the web of the beam can crush if the inclined compressive stresses exceed the concrete strength. The failure modes of some of the existing experimental programs have been analysed to evaluate the shear behaviour of FRP RC beams with FRP stirrups. As experimentally observed, the main difference of the shear behaviour of beams with FRP stirrups compared to conventional beams with steel stirrups is that stirrups do not yield, and they usually fail in their bottom bent zone. This type of failure can be explained by the fact that bending of the FRP bars into the stirrups configuration, significantly reduces its strength at the bent portions, due to their unidirectional characteristics. A summary of the response and failure modes of some of the existing experimental programs is presented in the following. o (Nagasaka et al. 1933) (Nagasaka et al. 1933), tested 35 half-scale rectangular beams with different type (CFRP, GFRP, AFRP, Hybrid, steel) and ratio (0, 0.5, 1.0 and 1.5%) of transversal reinforcement, different concrete strengths and clear span. Half of the specimens with FRP stirrups (12 out of 24 tests) failed due to breaking of the stirrups at the bent zone and the rest of the specimens failed due to the crushing of concrete struts formed between two adjacent diagonal cracks or by crushing from flexural-compression. 14
o (Ahmed et al. 2010) The experimental campaign by Ahmed et al. (2010) consisted on 3 beams with T-shape section with CFRP stirrups of 9.5mm diameter with different spacings. The tensile strength of the stirrups was around ftu = 1538 N/mm2 and their bend strength was 712 N/mm2 (46%•ftu). Two of the three beams failed in diagonal tension failure due to the rupture of the stirrups initiated at the bent part, and the remaining one failed in flexure. o (Shehata et al. 2000) Tests conducted by (Shehata et al. 2000) consisted on 10 beams with T-shape cross section critical to shear: 4 with CFRP stirrups, 4 with GFRP stirrups, 1 with steel stirrups and 1 without shear reinforcement. The test variables were the material properties and spacing of stirrups, and the type of flexural reinforcement (8 specimens with steel strands, 2 specimens with CFRP strands). All beams failed in shear before yielding or rupture of the longitudinal reinforcement. In the 8 beams with FRP stirrups, shear failure was initiated by rupture of the FRP stirrups at the bent zone (6 beams) or by crushing of the concrete in the shear span (2 beams). According to the experimental results, the effective stress in the stirrups at failure was as low as 50% of the strength parallel to the fibers provided that shear failure occurs due to the rupture of the stirrups. For closely spaced stirrups, a lower contribution of the stirrups was obtained. It might be because the chance for the diagonal crack to intersect the bent zone of the stirrups is higher.(Zhao et al. 1995) o (Bentz et al. 2010) The experimental program conducted by (Bentz et al. 2010) consisted on 11 shear tests of FRP RC beams, 5 of them with and 6 without GFRP stirrups. The beams presented different longitudinal GFRP reinforcement ratios and different transversal GFRP reinforcement ratios. 15
In relation to the failure mode of the tests with stirrups, beam L05-1 failed in shear by stirrup rupture at the bottom bent zone with a maximum measured strain at mid-height of the beam of 55% the bare-bar rupture strain. Beam L05-2 failed in flexure, even though shear failure was imminent. Beam L20-1 failed by sliding along a large diagonal crack, showing the rupture of the stirrups at failure. Beam L20-2 failed in flexure by concrete crushing with the rupture of some stirrups. One of the conclusions was that with multiple layers of longitudinal bars, the stirrups rupture did not occur at the bent location (as in beam L05-1) but near the end of the lap-splice (L20-2). Figure 4: failure in stirrups at the bent zone of L05-1 (Bentz et al. 2010) Figure 5: Flexural compression failure in constant moment region of L20-2(Bentz et al. 2010) o (Niewels 2008) (Niewels 2008) carried out an experimental program with 4 concrete beams with FRP flexural and shear reinforcement tested in shear in two phases. The variables of the tests were the type of longitudinal bars and stirrups and the amount of transversal reinforcement. The beams with stirrups failed in the shear compression zone due to overstress in shear and compression. Stirrups strains above 10‰ were measured. However, the stirrups did not fail due to concentration of stresses at the bent zone. 16
The tension in the FRP reinforcement should be limited to control the depth of shear cracks and maintain the integrity of the concrete, and to prevent failure in the bent zone of the transversal reinforcement. , 0.004 frp v fv fb f Ef= ≤ (2.7) Where, Efv is the modulus of elasticity of the transversal FRP reinforcement and ffb represents the strength of bent portion of FRP bar. , 0.05 0.30 b fb frp u b r ff d = ⋅+ ⋅ (2.8) Where rb and db represents the internal radius, respectively equivalent diameter of the bent, and ffrp,u the ultimate tensile strength of the transversal FRP stirrup. 2.3.2 (CNR-DT 204/2006) The total shear resistance of the reinforced concrete element with FRP stirrups can be calculated with the following formula: ( ) , , , max min ; Rd Rd c Rd frp Rd c V VVV= + (2.9) Where, VRdc,max is the concrete contribution corresponding to failure due to crushing of the diagonal compression concrete strut in the web. The contribution of the concrete resistance to shear can be calculated with the equation: () 1 3 , 1.3 1.2 40 fl Rd c rd d fl w s E V k bd E τρ = ⋅ ⋅ ⋅⋅ +⋅ ⋅⋅ 2.10 Where, Es is the modulus of elasticity of the steel, and τrd is the design shear stress calculated with: ,0.05 0.25 rd ctk f τ = ⋅ (2.11) Where fctk,0.05 is the characteristic concrete tensile strength (5%fractile). 23
fl fl w A bd ρ =⋅ (2.12) kd is a coefficient that can take the following values o kd = 1.0 in members where more than 50% of the reinforcement is interrupted; o other cases kd=1.6-d ≥ 1.0 The resistance to shear provided by the transversal FRP reinforcement: ,, , frp v frp v Rd frp Afd Vs ⋅⋅ = (2.13) ,,frp v frp u f ff φ γ = (2.14) Where ffrp,v is the reduce tensile strength of the transversal reinforcement and γfφ is a partial factor to account for bending effect equal to: o 2 when no specific experimental tests are performed o ffu/ffbd Where, ffu is the strength of an FRP bar and ffbd the design strength of the bending area of the FRP. The maximum shear force absorbed by the diagonal compression concrete strut in the web is determined as: , max 0.5 0.9 Rd c c w V fb d ν = ⋅⋅ ⋅ ⋅ ⋅ (2.15) 0.7 200 0.5 c f ν =−≥ (2.16) 2.3.3 (JSCE 1997) The total shear resistance of the reinforced concrete element with FRP stirrups can be calculated as: ,,Rd Rd c Rd frp VV V = + (2.17) 24
The shear resistance of concrete is: Where: 1 3 0.2 0.72 vcd c ff =⋅≤ N/mm2 (2.19) 1 4 1000 1.5 dd β = ≤ (2.20) 1 3 1000 1.5 ff p s E E ρ β ⋅ =⋅≤ (2.21) 1 n β = (No axial forces) (2.22) The shear resistance of the transversal FRP reinforcement is: , ,, , frp v frp v frp v Rd frp AE Vz s ε ⋅⋅ = ⋅ (2.23) 1 10 4 , ,, 10 0.3 frp frp frp v c frp v frp v E hfE ρ ερ − − ⋅ = ⋅⋅ ⋅ ⋅ (2.24) Where, εfrp,v is the design deformation of the transversal FRP reinforcement and h the height of the beam. 2.3.4 (CSA S806-12) The total shear resistance of the reinforced concrete element with FRP stirrups can be calculated with the following formula, where the left term represents the resistance of the compressed strut. ,, 0.22 cwv Rd Rd c Rd frp V V V fbd= + ≤ ⋅⋅⋅ (2.25) ,Rd c d p n vcd w V f bd βββ = ⋅ ⋅⋅ ⋅⋅ (2.18) 25
The shear resistance of concrete is given by: ( ) 1 3 , 0.05 Rd c c m r c w v V kk f bd λφ = ⋅⋅ ⋅ ⋅ ⋅ ⋅ ⋅ (2.26) , 0.11 0.2 cw Rdc cw fbdV fbd⋅ ⋅⋅≤ ≤ ⋅ ⋅⋅ (2.27) Where: λ is concrete density factor , equal to 1.0 for normal concrete. φc is the concrete resistance factor 2 60 c f N mm ≤ , is the compressive concrete strength. 0.9 v dd= ⋅ (2.28) ( ) 1 2 m k VdM= ⋅ (2.29) ( ) 1 3 1 rr kE ρ =+⋅ (2.30) o If a/d < 2.5, VRd,c shall be multiplied by ka 2.5 a k VdM = ⋅⋅ , 1.0 2.5 a k≤≤ (2.31) o If d>300 mm and At<At,min, VRd,c shall be multiplied by ks 750 1.0 450 s kd = ≤ + (2.32) The shear resistance of the transversal FRP reinforcement is: ,, , cot frp v frp v v Rd frp Afd Vs θ ⋅ ⋅⋅ = (2.33) ( ) 30 7000 x θε =+⋅ (2.34) 0.5 2 x ff Md V N EA ε ++ ⋅ =⋅⋅ (2.35) ( ) 2 , ,, , min 0.005 ; 0.4 ;1200 frp v frp v frp bend frp u f E f f N mm=⋅=⋅ (2.36) 26
2.3.5 Proposal by (Fico et al. 2008) In consistency with the experimental results of (Nagasaka et al. 1933) where the average stress of FRP stirrups was only half of the breaking strength of bent portions, (Fico et al. 2008) suggested a limit strain value,εf,lim ,for the stirrups contribution depending on the fiber type, that can be observed in Table 6. In addition, a limit of the transverse stirrups ratio of 1% was recommended for more reliable predictions. Type of fiber ε f,lim CFRP 0.0035 AFRP 0.0070 GFRP 0.0085 Table 6: Limit strain value(Fico et al. 2008) The shear resistance of the reinforce concrete element with transversal stirrups is calculated according to (CNR-DT 204/2006): ( ) , , , max min ; Rd Rd c Rd frp Rd c V VVV = + (2.9) Where VRd,c , VRd,frp and VRdc,max are the same as in(CNR-DT 204/2006) guideline. The formulation proposed by the (CNR-DT 204/2006) guideline for the contribution of the shear transversal FRP reinforcement VRd,frp is modified to take into account the strain limitation for each type of fiber. , ,, ,, , ,, frp v frp v u frp v b Rd frp frp v u A f df Vsf ⋅⋅ = ⋅ (2.37) , , , ,limfrp v b frp v frp fE ε = ⋅ (2.38) Equation (2.37) can be rewritten as: , ,lim , , frp v f frp v Rd frp A Ed Vs ε ⋅⋅⋅ = ⋅ (2.39) 27
2.3.6 Proposal by (Nehdi et al. 2007) The total shear resistance of the reinforced concrete element with FRP stirrups is given by: ,,Rd Rd c Rd frp VV V= + The shear resistance of concrete depends on the a/d relation, where a is the shear span. o For a/d > 2.5: 0.3 , 2.1 f c Rd ct s E fd VaE ρ ⋅⋅ = ⋅ (2.40) o For a/d < 2.5: 0.3 , 2.5 2.1 f c Rd ct s E fd d VaE a ρ ⋅⋅ =⋅⋅ (2.41) The shear resistance of the transversal FRP reinforcement: ( ) 0.5 , , ,, 0.5 Rd frp frp v frp v u w V A f bd= ⋅ ⋅ ⋅⋅ (2.42) 2.3.7 Proposal by (Hegger et al. 2009) (Hegger et al. 2009) developed a shear design equation where the concrete shear strength contribution is based on Eurocode and the contribution of FRP shear reinforcement depends on a strain limit obtained from existing experimental work. The total shear resistance of the reinforced concrete element with FRP stirrups: ,,Rd Rd c Rd frp VV V= + The shear resistance of concrete: 1 3 ,0.205 100 r Rd c f ck w s E V k f bd E β κρ = ⋅⋅ ⋅⋅ ⋅⋅ ⋅ ⋅ ⋅ (2.43) 28
, , 1 10 frp v f frp v c E kE ρ =−⋅ ⋅ (2.44) 3da β = ⋅ (2.45) 1 200 d κ = + (2.46) Where: β factor that increases the shear strength of the concrete near the supports. The shear resistance of the transversal FRP reinforcement: ,, , cot 1 min ; cot tan frp v frp v Rd frp w c cm Afz V bz f s θαθθ ⋅ ⋅⋅ = ⋅⋅ ⋅ ⋅ + (2.47) 0.9zd= (2.48) ( ) , , , , ,lim min 0.4 ; frp v frp u frp v frp v f fE ε =⋅⋅ (2.49) ( ) 0 , ,lim , , 00 3 0.015 frp v frp v frp v c EE ερ =+⋅ (2.50) Where: αc =0.2 ϴ is the truss angle ffrp,u is the ultimate tensile strength of FRP ffrp,v is the design value of the tensile strength of FRP reinforcement 29
3 Non-linear shear-sensitive fiber beam model The present work used the program CONSHEAR to analyze the behaviour of the beams tested by (Kurth 2012). CONSHEAR (Ferreira 2013) is a computer program for the nonlinear analysis of reinforced and prestressed concrete frame structures by means of the fiber beam element approach and accounting for axial force-shear-bending interaction. The numerical model implemented in CONSHEAR is based on a previous model founded on the Finite Element Method (FEM) and on the Bernoulli’s beam theory that is implemented in the computer program CONS (Marı 2000). In general, its main characteristics are: the Timoshenko beam theory is assumed at the element level; a hybrid sectional formulation, in which input variables comprises both kinematical and force quantities, links the plane section theory with the assumption of a constant shear stress flow. The multiaxial constitutive behaviour of concrete is assumed through a smeared crack approach with full rotating cracks; compression weakening (softening) and tensile tension stiffening effects are included. Longitudinal reinforcement is simulated through the use of steel filaments while transversal reinforcement is considered smeared in the concrete fibers. In the following, a brief insight into the fundamental of the numerical model that is implemented into the computer code CONSHEAR is offered. 3.1.1 Structural scheme In numerical simulations by means of the FEM using 1D fiber beam models the structure is divided into elements interconnected by nodes and the material nonlinearities are introduced at each control section that is discretized into longitudinal fiber as observed in Figure 8. 30
Figure 8: General characteristics of the fiber beam models (Ferreira 2013) 3.1.2 Finite element A 2-noded Timoshenko finite element with linear shape functions is used in the model. For the 2D case, the displacement field is a function of two displacements, axial u and vertical w, and a rotation θy. In the Timoshenko beam theory it is assumed that undeformed plane sections perpendicular to the beam axis remain plane but not necessarily normal to the longitudinal axis after deformation. An average rotation of the section due to distortion is considered in order to maintain valid the plane section assumption. Figure 9: Fiber beam model in CONSHEAR: a) general characteristics b) finite element for the 2D case (Ferreira 2013) 31
3.1.3 Sectional level The cross-section is discretized into two types of fibers, as presented in Figure 3: the non-shear resistant ones, submitted to 1D axial stresses only, and the shear resistant fibers, submitted to a multiaxial stress-strain state. Axial force and bending moment are resisted by the entire crosssection; shear forces and interaction with normal forces are only considered in the shear resistant fibers. This fiber subdivision is an input of the model related to the shape of the cross section: for rectangular, T-shape and I-shape, the fibers that pertain to the web (disregarding the bottom cover area) are considered shear resistant. Particularly for the T-shape and I-shapes cross sections, if there is strong evidence that compressive flanges contribute to the shear-resistance mechanism, an effective area of the flange beff determined according to (Zararis et al. 2006) can be considered as 2D fibers. Figure 10: Assumptions of the model at the section level (Ferreira 2013) 3.1.4 Material models Cracked concrete is assumed as a homogeneous material with orthotropic behaviour (Figure 11(a)). The constitutive model is formulated in terms of average principal strains ε12= [ε1 ε2] T and stresses σ12= [σ1 σ2] T between the undamaged and cracked areas. . In this formulation 32
4.1.4 Experimental setup for shear tests The experimental setup is illustrated in Figure 17. Two shear tests were performed per specimen with different load and support positions. The first part of the experiment is a 4 -point bending test; the failure was produced on the right side where the weaker shear reinforcement (or no shear reinforcement) is located. The second part of the experiment was a 3-point bending test. Here, failure occurred in the left part of the beam that was higher transversally reinforced. Figure 17: Experimental set-up of shear tests (Kurth 2012) The load was applied to about 50% of the loading cell capacity and controlled with 5 kN / min and 10 kN / min and the displacement controlled at 0.5 mm / min and 1.0 mm / min. The tests were stopped four to seven times, at constant load or constant deformation, to carry out crack width measurements. The following sensors were used to record the experimental data and its position can be seen in Figure 14. o Concrete longitudinal strains in compression (strain gages = DMS) B1 ... B14 o longitudinal strains in concrete in the tension / compression zone (transducer) D1 ... D3 o reinforcement slip on the beam ends (sensor) E1 and E2 39
o Strains in concrete in the shear field (transducer Rosette) R1 ... R6 o shear crack width (sensor) S1 S2 ... o displacements (displacement transducer) W1 W5 ... o strains in the longitudinal reinforcement (DMS) LG1 ... LG7 o stains in the shear reinforcement (DMS) SG1 ... SG30 The basic arrangement of the metrological devices for concrete are in Figure 18 and for reinforcement are in Figure 19 Figure 18: Metrology of concrete (Kurth 2012) 40
Figure 19: Metrology of reinforcement (Kurth 2012) 4.1.5 Failure modes Stirrup failure The specimens with lower shear reinforcement ratios (ρw = 0.45 and 0.75%) and medium shear reinforcement ratios (ρw=1.26%) and for high concrete strengths (fcm = 75.7 and 82.0 N / mm²) presented failure of the transversal reinforcement, due to a combined shear-tensile stress locally present in the region of the main shear crack(Figure 20). Figure 20: Cracking at failure in experimental S4AH-0.8-7 (rw = 0.75%, fcm =42.2 N/mm2 (Kurth 2012) 41
Figure 21 shows the damaged stirrups types A and B after the failure in the test S4AH-0.8-7 and S6BN-0.8-11. In contrast, the reinforcement type C presented a local failure in the connections as the FRP rod was pulled out of the polymer concrete anchor head (Figure 22 ). S4AH-0.8-7 ( ρ w = 0,75 %,fcm = 42,2 N/mm²) S6BN-0.8-11 ( ρ w = 0,75 %, fcm = 30,4 N/mm²) Figure 21: Damaged stirrups (Type A and B) after failure in experiments with a shear reinforcement degrees ρw of 0.75% (Kurth 2012) Longitudinal cracked DHB (double headed bolt) Extract of the polymer anchor head Figure 22: Damaged double headed bolt (type C) after failure while trying S12CH-0.7-23 (ρw = 0.75%, fcm = 73.1 N / mm²)(Kurth 2012) 42
Diagonal compression failure In the experiments with high shear reinforcement ratios, from ρw = 2.22% rto ρw = 2.26%, and medium shear reinforcement degrees (ρw = 1.26%) with the lower concrete strengths (fcm≤ 73.1 N/mm²) failure occurred by crushing of concrete in the web (diagonal compression shear failure) Figure 23: Cracking at failure in experimental S6BN-2.3-12 (ρw = 2.26%, fcm = 30.7 N / mm²)(Kurth 2012) Figure 24: Cracking at failure in experimental S2AN-2.3-4 (ρw = 2.26%, fcm = 33.5 N / mm²)(Kurth 2012) When compression struts fail different failure images were observed. In Experiments S2AN-2.3- 4 and 2.3-8-S6BN-2.3-12 was almost completely blown off the concrete cover in the web area at failure of the concrete strut (Figure 24). 43
In Table 9 are presented, for each specimen, the different types of failure along with the transversal reinforcement ratio ρw , concrete strength fcm , average shear crack angle at failure βr and the ultimate shear force Vu. Test ρw [%] f cm [N/mm2] β r [ᵒ] V u [kN] Failure type S1AN-1.3-2 1,20 38,4 40 427 diagonal tension failure S2AN-0.8-3 0,75 34,1 30 332 stirrup failure S2AN-2.3-4 2,26 33,5 36 486 diagonal tension failure S3AH-1.3-6 1,26 82,0 31 571 stirrup failure S4AN-0.8-7 0,75 42,2 32 326 stirrup failure S4AH-2.3-8 2,26 42,6 34 544 diagonal tension failure S5BN-1.3-10 1,26 42,8 37 439 diagonal tension failure S6BN-0.8-11 0,75 30,4 33 302 stirrup failure S6BN-2.3-12 2,26 30,7 37 448 diagonal tension failure S7BH-1.3-14 1,26 75,7 31 626 stirrup failure S8BH-0.8-15 0,75 72,7 27 439 stirrup failure S8BH-2.3-16 2,26 69,9 33 581 diagonal tension failure S9CN-1.3-18 1,26 37,7 36 410 diagonal tension failure S10CN-0.7-19 0,75 32,0 23 304 failure of DHB head S10CN-2.2-20 2,22 33,6 34 484 diagonal tension failure S11CH-0.4-21 0,45 67,6 28 374 failure of DHB head S11CH-1.3-22 1,26 71,0 33 621 diagonal tension failure S12CH-0.7-23 0,75 73,1 32 441 failure of DHB head S12CH-2.2-24 2,22 73,9 36 742 diagonal tension failure Table 9: Types of failure for the experimental beams 44
In the present work, 5 beams were considered to be simulated with CONSHEAR S2AN-0.8-3, S4AH-0.8-7, S6BN-0.8-11, S8BH-0.8-15, S10CN-0.7-19 - that are loaded in 2-point bending configuration, in the first phase of testing This choice was motivated by the fact that the second test is influenced by the damage brought from the first test, which could only be well captured by a phased analysis, which is out of the aims of this work. Also, experimental data from test 1 are more reliable to be compared with the numerical results, as they are less influenced by the previous testing and consequent damage. Table 10 lists the characteristics of the beams under study. The dimensions are the same for all the beams, 3 beams (S2AN-0.8-3, S6BN-0.8-11 and S10CN-0.7-19) are reinforced with 6ø32 mm FRP, having the longitudinal ratio ρl of 8.5% and 2 with 8ø32 (S4AH-0.8-7 and S8BH-0.8-15) having the longitudinal ratio ρl of 11.5%. For transversal reinforcement there are 3 types of stirrups used with 2 different diameters ø12 (S2AN-0.8-3, S4AH-0.8-7, S6BN-0.8-11, S8BH-0.8- 15) and ø16 (S10CN-0.7-19). 45
Table 10: Beam dimensions, concrete properties, longitudinal reinforcement, and transversal reinforcement(Kurth 2012) Trial Type reinf b [mm] bw [mm] h [mm] Ec [N/mm 2] fcm [N/mm 2] fctm [N/mm2] Φ/s [mm] ρw [%] Efw [N/mm 2] f fw,exp [N/mm 2] εu, t ρl [%] Efl [N/mm 2] ffl [N/mm 2] εu, l S2AN - 0.8-3 A , l 400 100 650 25600 34 2,70 Ø12/ 300 0,75 56200 382 0.0068 8,52 59000 1000 0.017 S4AH - 0.8-7 A , l 400 100 650 25500 42 2,31 Ø12/ 300 0,75 56200 382 0.0068 11,57 59000 1000 0.017 S6BN - 0.8-11 B , ll 400 100 650 24600 30 2,32 Ø12/ 300 0,75 57000 770 0.0135 8,44 62600 1000 0.016 S8BH - 0.8-15 B , ll 400 100 650 33400 73 3,56 Ø12/ 300 0,75 57000 770 0.0135 11,47 62600 1000 0.016 S10CN - 0.7-19 C , ll 400 100 650 23200 32 2,20 Ø16/ 270 0,74 63400 611 0.0096 8,44 62600 1000 0.016 46
4.2 Numerical model The first objective of the numerical analysis is the validation of the computer program for the case of FRP RC beams by comparing the numerical results with the experimental data captured in local points by the sensors.After validating the model, the second objective is to perform a deeper analysis of the structural behaviour of the beams. The following sensors were considered to perform the comparison with the numerical outputs: for the concrete strain compression (B4-right side of the beam);, displacement transducer (W3- middle of the beam); strain in the longitudinal reinforcement (LG1, LG2, LG3 ,LG4 ,LG5 ,LG6 ,LG7); strain in the shear reinforcement ( SG17…SG26- right side of the beam) and shear crack width (S1 – right side of the beam) . This was all the data available in the original reference by (Kurth 2012) . Since the numerical model is based on the finite element method, it is necessary to discretize the beam to be analyzed into a mesh. As shown in Figure 27, the beam was simulated using 28 bar type elements of equal length, generating 29 nodes. Nodes 3 and 27 correspond to the simply supported points, while the node 15 coincides with the center-beam section. In turn, the cross section has been divided into 8 trapeziums that are discretized into filaments as observed in Figure 25(Ferreira 2013). Longitudinal rebars were modeled in their real position in the cross-section. Furthermore in Figure 26, it is considered a shear resistant zone that is composed of the web and the effective width of the flange (beff=340mm) which was calculated using the formulas in (Zararis et al. 2006). Figure 25: Discretization of the cross section Figure 26: Shear resistant zone 47
Figure 27: Discretization of the beam The model with CONSHEAR is the same for all the beams since they have the same length L=7 m and same cross-section dimensions b=400mm, bw=100mm, h=650mm. The difference between the beams are only related with the reinforcement configurations, as can be observed in Figure 28 for longitudinal reinforcement and in Figure 29 for transversal reinforcement. The specimens S2AN-0.8-3 and S4AH-0.8-7 have the same transversal reinforcement (ø12 FRP at a pace of 300 mm) on the right side of the beam and a tensile strength of ffw= 382 N/mm2 .The difference between them is the longitudinal reinforcement- S2AN-0.8-3 has 6 ø32 while S4AH- 0.8-7 has 8 ø32 both have an elastic modulus of Efl= 5900 N/mm2.Also the concrete characteristics differ; S2AN-0.8-3 has a compressive strength of fcm=34 N/mm2 and S4AH-0.8-7 of fcm=42 N/mm2 . The specimens S6BN-0.8-11 and S8BH-0.8-15 are reinforced transversally with ø12 FRP at a pace of 300 mm with a tensile strength of ffw= 770 N/mm2. Longitudinally S6BN-0.8-11 is reinforced with 6 ø32 and S8BH-0.8-15 with 8 ø32, both with elastic modulus of Efl=62600 N/mm2.The compressive strength of concrete is of fcm=30 N/mm2 for S6BN-0.8-11 and of fcm=73 N/mm2 for S8BH-0.8-15. Beam test S10CN-0.7-19 is reinforced transversally with ø16 FRP at a pace of 270 mm with a tensile strength of ffw=611 N/mm2; the longitudinal reinforcement is of 6ø32 with an elastic modulus of Efl=62600 N/mm2; the strength of concrete is fcm=32 N/mm2. The specimen S6BN-0.8-11 is compared in detail with the experimental results and discussed deeply in the following section, as it presents the best fitting with the experimental data. The results of the other simulated beams are treated with less detail and presented in a separate section at the end of the present chapter. 48
Other sources of damage in the experimental testing that can contribute to the difference are the possible damage due to shrinkage, creep and transportation. This would diminish the contribution of concrete resistance, thus making the load be absorbed more by the FRP stirrups. 4.3.1.4 Longitudinal strains in concrete Figure 37 presents the concrete strains in the mid span of the beam for different load levels. Figure 37: Experimental and numerical results of concrete deformation for test S6BN-0.8-11 As can be seen, the predicted results show a great similarity with the experimental ones. Only a small difference is seen in the load level (V=100kN). The experimental deformations are of 1.25‰ (1.25 * 10-3) in the bottom part (tension) for shear value V=100 kN, and our numerical results in the bottom part are 1.6‰ (1.6*10-3). This is, again, due to the possibility that the beam was precracked, causing a decrease in tensile strength of the concrete. For higher load levels, the fitting is very good. 0 10 20 30 40 50 60 70 -4 -2 0246 h [cm] ε [‰ ] S6BN-0.8-11 V= 100 kN numerical V= 100 kN experimental V= 200 kN numerical V= 200 kN experimental V= 250 kN numerical V= 250 kN experimental V= 302 kN numerical V= 302 kN experimental 55
4.3.1.5 Transversal strain in the concrete web Transversal strains in the concrete web measured by the strain rossette are compared with the numerical results in Figure 32. Figure 38: Shear-strain of concrete numerical and experimental results for test S6BN-0.8-11 The numerical approach overestimates the start of concrete cracking with about 100 kN. This is again due to our model being stiffer. Even though it can be observed that the model represents the experimental data, being capable of capturing the start of the diagonal cracking that corresponds to the load level for which the strains increase abruptly. Again, experimental measurements in this location (web of the beam) are very vulnerable to the effects of cracking. 4.3.1.6 Crack patterns The crack development on the two beams was numerically predicted by the use of the discrete representation algorithm presented in chapter 3.1.5. Table 11 represents the development of cracking with increasing load predicted by the model and the comparison with the experimental observations for the ultimate load state. Numerical predictions, in terms of crack propagation and inclinations, show a fairly good agreement with the experimental evidence. It is interesting to 0 50 100 150 200 250 300 350 400 450 -2.00 -1.50 -1.00 -0.50 0.00 0.50 V[kN] ε [‰ ] S6BN-0.8-11 numerical experiemntal 56
observe that the cracks develop more in the shear critical zone (right span of the beam). The beam reached an ultimate shear force V=302kN and has a stirrup failure. Cracking patterns Shear force V=100kN V=200kN V=250kN V=302kN Experimental results Table 11: Cracking patterns at different load levels for test S6BN-0.8-11 57
Figure 39 represents the crack width in the shear critical area with increase load (experimental and numerical results). Figure 39: Cracking width for test S6BN-0.8-11 In relation to experimental results, Crack 1 and 2 represent the average crack width results measured experimentally with fiber optical sensors. The numerical results (as it is based on the smeared cracked approach and is not possible to monitor one single crack) correspond to average crack widths of different scanned areas; x distance measured in m from the left support of the beam until the left support (Figure 40) Figure 40: Location of measured cracks 0 50 100 150 200 250 300 350 0.00 0.50 1.00 1.50 2.00 2.50 V[kN] w[mm] S6BN-0.8-11 x= 5.6 x= 5.485 x= 5.397 x= 5.338 x= 5.276 5.287 x= 5.3 crack 2 crack 1 58
Experimentally (Kurth 2012) obtained an average crack width of 1.2mm and a maximum crack width of 2mm which is similar with our numerical results that show a maximum crack width of 2.4mm at the ultimate shear force, and an average crack width of 1.5mm. In the shear critical zone the biggest crack width forms. It can be observed that the numerical results are consistent with the experimental observations, for all levels of damage. It is difficult to compare the results because, in reality the discrete crack was measured with an optical sensor (ARAMIS), and the numerical results are obtained with a model based on the smeared crack approach that considers an average distribution of the crack in the element. Even though, the results present agree with the experimental ones in terms of order of magnitude and tendencies. 4.3.1.7 Other numerical results Figure 41 presents the strains in transversal reinforcement for different heights in the cross section. Figure 41: Strain in the stirrups for different positions of the sensors test S6BN-0.8-11 0 50 100 150 200 250 300 350 400 450 -2.00 0.00 2.00 4.00 6.00 8.00 10.00 V[kN] ε [‰ ] bent up down 59
The up and down sensors corresponds to the ones described in (Kurth 2012) Figure 33 (SG19 and SG20) which are situated at the middle of the stirrup, and the sensor in the bent zone is added by us to measure the strains in the failure zone of the stirrup. As can be observed the strain in the bent zone is bigger 9.21‰ compared to 7.91 ‰ down, and 6.73‰ up, that is because the stirrups are more loaded when there is more damage, which is the bottom of the beam. When the cracking propagates to the top, the stirrups start to carry load. Figure 42 represents the flow of strains in transversal reinforcement along the shear critical cross section for a load level of V= 302 kN. Figure 42: Strains in stirrup height at the bent zone for testS6BN-0.8-11 The same can be seen here. The bottom parts of the stirrups are more loaded than the top parts, and this is because we have more damage at the bottom and the top part in under compression, so the stirrups do not need to work. 0.00 0.10 0.20 0.30 0.40 0.50 0.60 0.70 -2.00 0.00 2.00 4.00 6.00 8.00 h[m] ε [‰ ] S6BN-0.8-11 numerical 60
4.3.2 Other tests beams The results of the other test beams S2AN-0.8-3, S4AH-0.8-7, S8BH-0.8-15 and S10CN-0.7-19 are presented together in the following. This results present different tendencies and issues as the ones discussed in detail before; so no discussion is made specifically for these cases. 4.3.2.1 Load vs displacement Figure 43: Experimental and numerical deflection in the center of the beam for tests S2AN-0.8-3, S4AH-0.8-7, S8BH-0.8-15 and S10CN-0.7-19 0 50 100 150 200 250 300 350 400 0 20 40 60 80 V [kN] displacement [mm] S2AN-0.8-3 experimental numerical 0 50 100 150 200 250 300 350 0 20 40 60 V [kN] displacement [mm] S4AH-0.8-7 experimental numerical 0 100 200 300 400 500 0 20 40 60 80 V [kN] displacement [mm] S8BH-0.8-15 experimental numerical 0 100 200 300 400 500 600 0 20 40 60 80 V [kN] displacement [mm] S10CN-0.7-19 experimental numerical 61
4.3.2.2 Strains in the FRP longitudinal reinforcement Figure 44: Experimental and numerical results of strains in the FRP longitudinal reinforcmenet for tests S2AN-0.8-3, S4AH-0.8-7, S8BH-0.8-15 and S10CN-0.7-19 -2 0 2 4 6 8 0123456 ε [‰ ] L [m] S2AN-0.8-3 V= 100 kN numerical V= 100 kN experimental V= 200 kN numerical V= 200 kN experimental V= 300 kN numerical V= 300 kN experimental V= 326 kN numerical V= 326 kN experimental -1 0 1 2 3 4 5 0123456 ε [‰ ] L [m] S4AH-0.8-7 V= 100 kN numerical V= 100 kN experimental V= 200 kN numerical V= 200 kN experimental V= 300 kN numerical V= 300 kN experimental V= 326 kN numerical V= 326 kN experimental -1 0 1 2 3 4 5 6 0123456 ε [‰ ] L[m] S8BH-0.8-15 V= 100 kN numerical V= 100 kN experimental V= 250 kN numerical V= 250 kN experimental V= 400 kN numerical V= 400 kN experimental V= 439 kN numerical V= 439 kN experimental -1 0 1 2 3 4 5 0123456 ε [‰ ] L [m] S10CN-0.7-19 V= 100 kN numerical V= 100 kN experimental V= 200 kN numerical V= 200 kN experimental V= 250 kN numerical V= 250 kN experimental V= 304 kN numerical V= 304 kN experimental 62
4.3.2.3 Strains in the FRP transversal reinforcement -2 0 2 4 6 8 10 12 0 0.2 0.4 0.6 0.8 1 1.2 1.4 1.6 ε [‰ ] L [m] S2AN-0.8-3 V= 100 kN numerical down V= 100 kN down V= 100 kN numerical up V= 100 kN up V= 200 kN numerical down V= 200 kN down V= 200 kN numerical up V= 200 kN up V= 250 kN numerical down V= 250 kN down V= 250 kN numerical up V= 250 kN up V= 302 kN numerical down V= 302 kN down V= 302 kN numerical up V= 302 kN up -2 0 2 4 6 8 10 12 14 16 0 0.2 0.4 0.6 0.8 1 1.2 1.4 1.6 ε [‰ ] L [m] S4AH-0.8-7 V= 100 kN numerical down V= 100 kN down V= 100 kN numerical up V= 100 kN up V= 200 kN numerical down V= 200 kN down V= 200 kN numerical up V= 200 kN up V= 300 kN numerical down V= 300 kN down V= 300 kN numerical up V= 300 kN up V= 326 kN numerical down V= 326 kN down V= 326 kN numerical up V= 326 kN up 63
Figure 45: Experimental and numerical results of strains in stirrups along the length of the beam for tests S2AN-0.8-3, S4AH-0.8-7, S8BH-0.8-15 and S10CN-0.7-19 -2 0 2 4 6 8 10 12 14 16 0 0.2 0.4 0.6 0.8 1 1.2 1.4 1.6 ε [‰ ] L [m] S8BH-0.8-15 V= 100 kN numerical down V= 100 kN down V= 100 kN numerical up V= 100 kN up V= 200 kN numerical down V= 200 kN down V= 200 kN numerical up V= 200 kN up V= 250 kN numerical down -1 0 1 2 3 4 5 6 7 8 9 0 0.5 1 1.5 2 ε [‰ ] L [m] S10CN-0.7-19 V= 100 kN numerical down V= 100 kN down V= 100 kN numerical up V= 100 kN up V= 200 kN numerical down V= 200 kN down V= 200 kN numerical up V= 200 kN up V= 250 kN numerical down 64
Ferreira, D. et al., 2013. Nonlinear analysis of RC beams using a hybrid shear-flexural fibre beam model. Engineering Computations, 31(7), pp.1444–1483. Ferreira, D.C.S., 2013. Computer Program CONSHEAR Nonlinear analysis of concrete structures critical to shear. , (April). Fico, R., Prota, A. & Manfredi, G., 2008. Assessment of Eurocode-like design equations for the shear capacity of FRP RC members. Composites Part B: Engineering, 39(5), pp.792–806. Hegger, J., Kurth, M. & Niewels, J., 2009. Shear Analysis of Concrete Members With Fiber- Reinforced Polymers ( Frp ) As Internal Reinforcement. Concrete, (July), pp.13–16. JSCE, 1997. Recommendations for design and construction of concrete streuctures using continuous fiber reinforcing materials. Japan Society of Civil Engineers., C, p.325. Kurth, M., 2012. Kurth RWTH Disse Querkrafttragverhalten Faservebundkunststoffe 2012-12. Marı, A.R., 2000. Numerical simulation of the segmental construction of three dimensional concrete frames. Engineering Structures, 22(6), pp.585–596. Nagasaka, T., Fukuyama, H. & Tanigaki, M., 1933. Shear performance of concrete beams reinforced with FRP sitrups. 1993. Detroit, Michigan. Nehdi, M., El Chabib, H. & Saïd, a. A., 2007. Proposed Shear Design Equations for FRP-Reinforced Concrete Beams Based on Genetic Algorithms Approach. Journal of Materials in Civil Engineering, 19(12), pp.1033–1042. Niewels, J., 2008. Zum Tragverhalten von Betonbauteilen mit Faserverbundkunststoff- Bewehrung. Thesis. Pilakoutas, K., 2000. Failure Analysis of Industrial Composite Materials, E. E. Gdoutos, K. Pilakoutas, and C. A. Rodopoulos, eds., McGraw-Hill,. Composites in Concrete Construction, (London), pp.449–497. Shehata, E., Morphy, R. & Rizkalla, S., 2000. Fibre reinforced polymer shear reinforcement for concrete members: behaviour and design guidelines. Canadian Journal of Civil Engineering, 27(5), pp.859–872. Spadea, S., 2010. Comportamento di elmenti di calcestruzzo armato con barre di materiale compositeo fibroinforzato. University of Salerno, Fisciano, Italy. Zararis, I.P., Karaveziroglou, M.K. & Zararis, P.D., 2006. Shear strength of reinforced concrete T- beams. ACI Structural Journal, 103(5), pp.693–700. 71
Zhao, W., Maruyama, K. & Suzuki, H., 1995. Shear behaviour of concrete beams reinforced with FRP rods as longitudinal and shear reinforcement. In: Proceedings of the 2nd international RILEM symposium non-metallic (FRP) reinforcement for concrete structures (FRPRCS-2); 1995. p. 352e9. 72