scieee AI-readable full text Open interactive document viewer

Stabilization of photovoltaic panels cell wastes in building material matrices

Fernández Carrasco, Lucía,Ferrer, Rober,Aponte Hernández, Diego Fernando,Martínez Ramírez, Sagrario

Abstract

This is a study about the hydration process of a mixture of Portland cement and solar photovoltaic cells waste. The nature of the hydration products of different compositions of these mixtures have been evaluated, at 20º C of temperature, by means of the analysis of samples throughout x- ray diffraction and infrared spectroscopy. The total porosity and mechanical strength development of those materials was also determined. It was revealed that the presence of solar cell residue –up to 5%- in the cement matrices do not induce to the develop of new hydration products different of those from the normal hydration of the Portland cement. However, the presence of the waste induces to a reduction of the mechanical strength and an increase in the total porosity is evidenced.

Full text

1st Spanish National Conference on Advances in Materials Recycling and Eco- Energy Madrid, 12-13 November 2009 S05-6 189 STABILIZATION OF PHOTOVOLTAIC PANELS CELL WASTES IN BUILDING MATERIAL MATRICES L. Fernández-Carrasco1, R. Ferrer2, D.F. Aponte2 and S. Martínez-Ramírez3 1 Escola Tècnica Superior d’Arquitectura del Vallès, Departament de Construccions Arquitectoniques I – Grup Lita (UPC). C/ Pere Serra, 1-15 -08173 Sant Cugat del Vallès. 2Escola Tècnica Superior d’Enginyers de Camins, Canals i Ports de Barcelona, Departament d’Enginyeria de la Construcció (UPC). c/ Jordi Girona, 1-3 – 08034 Barcelona. 3Instituto de Estructura de la Materia (CSIC), C/Serrano 121, 28006 Madrid. Abstract This is a study about the hydration process of a mixture of Portland cement and solar photovoltaic cells waste. The nature of the hydration products of different compositions of these mixtures have been evaluated, at 20º C of temperature, by means of the analysis of samples throughout xray diffraction and infrared spectroscopy. The total porosity and mechanical strength development of those materials was also determined. It was revealed that the presence of solar cell residue –up to 5%- in the cement matrices do not induce to the develop of new hydration products different of those from the normal hydration of the Portland cement. However, the presence of the waste induces to a reduction of the mechanical strength and an increase in the total porosity is evidenced. Keywords: solar photovoltaic cells, cement, hydration, microstructure, strength. INTRODUCTION Photovoltaic (PV) energy is a renewable, versatile technology that can be used for almost anything that requires electricity. In the past 20 yr, research and development has advanced PV and a new generation of low-cost products based on thin films of photoactive materials (e.g., amorphous silicon, copper indium diselenide, cadmium telluride, and film crystalline silicon) deposited on inexpensive substrates, increase the prospects of rapid commercialization [2-3]. An important factor and the key in the cycle of life of PV modules is decommissioning at the end of their use, expected to last about 30 yr. Moreover, there is a concern about disposing them because they may contain minor amounts of regulated materials (e.g., Cd, Pb and Se). Options to recycle manufacturing wastes and used solar cells are recently being investigated [4-5]. This research is an attempt to explore the possible reutilization of solar cell residues from PV panels in construction materials, which cannot only provide low cost cement and concrete but also, can help to decrease environmental hazards. In this context, an experimental study of the addition of residues from the manufacturing of PV solar cells to Portland cement has been developed in order to stabilizate/valorizate this waste in Portland cement matrices. EXPERIMENTAL Materials A Portland cement type I 52.5 R and a solar cell residue (SCR) obtained from the manufacturing of photovoltaic panels A-120P from ATERSA were used in this research as raw materials. A PHILIPS PW 2400 X-ray fluorescence spectrometer with a PW 2540 VTC sample changer was utilized to determine the chemical composition of the materials (see Table 1). The SCR presents 1.69% of AgO, 0.05% of PbO and 0.05% of Ni2O. Mineralogical composition of the raw materials was determined by an X-ray diffractometer (XRD) with a Siemens D500 instrument and an FTIR- Bomem MB-120 Fourier transform infrared spectrophotometer with a frequency range of 350 to 5000 cm-1 were used. 1st Spanish National Conference on Advances in Materials Recycling and Eco- Energy Madrid, 12-13 November 2009 S05-6 190 Table 1. Chemical Composition of raw materials Al2O3 CaO SiO2 Fe2O3 MgO K2O TiO2 CP 5.04 63.25 19.56 3.50 1.96 0.75 0.22 SCR 13.87 0.07 84.26 --- --- --- --- EXPERIMENTAL The solar cells residue was grinded using a Retsch disc mill. The grinded wastes were sieved trough a 0.063 mm sieve and only the particles of minor of 63 µm size were used for the study: the Figure 1 shows the received residue from Atersa and the grinded one. Figure 1. Solar cells residue In order to study the microstructure of these materials different pastes, with and without SCR, were elaborated. First of all, consistency tests were conducted in order to establish the appropriate ratio water/cement for pastes elaboration (UNE-EN 196–3). The initial composition of the studied mixtures is shown in Table 2. Table 2. Initial composition of the studied mixtures Notation % SCR PC 0 SCR0.3 0.3 SCR0.5 0.5 SCR1 1 SCR3 3 SCR5 5 SCR15 15 The pastes were placed in a curing chamber at 20 ± 1 ºC and RH=95 ± 2 % and were cured for up to 28 days, after that they were immersed in acetone in order to stop the hydration process of the pastes. The pastes mineralogy and microstructure of the matrices were studied by XRD and FTIR. In order to determine materials strength, mortars, with and without SCR, were prepared with a siliceous aggregate (UNE-EN 196-1). The selected studied SCR/Portland cement ratios were: 0.3, 0.5, 1, 3 and 5%; the binder/sand ratio was 3:1 and the water/cementitious material ratio was kept constant at 0.5. The specimens were cured at 20±1 ºC and 95 ± 2 % relative humidity (RH) for 28 days. The flexural and compressive strengths of the specimens were measured as specified in European standard UNE-EN 196-1. RESULTS Consistency and initial and final set tests The results of these tests are shown in Table 3. During the development of the tests it could be notice, mainly with major SCR content and at early ages of the reactions that some kind of expansion of the materials was happening. Table 3. The results of consistency and set tests % SCR Water/solid Initial set (min.) Final set (min.) 0 0.284 150 215 5 0.287 169 226 15 0.288 175 230 Strength and total porosity The representation of the mechanical strength of mortars at 28 days of curing time, as a function of SCR percentage is given in Figure 1. The addition of 0.3% SCR did not significantly modify the compressive strength of mortars, although a more important reduction of strength is observed for 0.5 % and higher of SCR. However, a minimum of compressive strength is achieved for mixtures with major SCR portion. Then, the presence of SCR induces to a substantial change in compressive strength compared to the specimens without admixtures. It may be deduced from the data in Table 4 that the total porosity values show an important increase with the presence of SCR in the mixtures and major for samples with 0.5 % content of SCR. However, it is remarkable that from 1 to 5% of SCR neither content nor significant influence are observed; it is interesting to remark that with 5% of SCR the total porosity of the sample is the same that for Portland cement. Table 4. Total porosity and Compressive strenth % SCR % Total porosity MPa Compressive Strength 0 14.9 55.4 0.3 16.0 50.5 0.5 16.8 43.6 1 16.5 34.2 3 15.5 30.3 5 14.9 32.4 1st Spanish National Conference on Advances in Materials Recycling and Eco- Energy Madrid, 12-13 November 2009 S05-6 191 Figure 1. Total porosity and compressive strength. Paste mineralogy and microstructure Infrared spectroscopy The Figure 2 shows the infrared spectrums of the pastes prepared with different dosages of SCR and cured during 28 days. The infrared spectrums of all the studied pastes had vibration bands at around 3645 cm-1 associated with the OH free frequency due to portlandite presence; minor relative intensity of this band was observed in samples with higher SCR content. The infrared spectrums of the samples had vibration bands at around 963- 975 cm-1, associated with the Si-O (ν3 (Si-O)) stretching vibration in the SiO4 tetrahedra comprising the C-S-H gel. The two bands appearing between 456 and 470 cm-1 were attributed to the O-Si-O (ν4 (O-Si-O)) deformation vibration. The aragonite and calcite ν3 [CO3]2- vibration bands appeared at 1490 and 1423 cm-1, respectively, while the ν2 [CO3]2- and ν4 [CO3]2- vibration bands for the carbonates were observed at 874 cm-1 indicating some minor carbonation of samples. The anti-symmetrical stretching frecuency of the sulphate ion (ν3 SO4) of ettringite is centred towards 1118 cm-1. Figure 2. Infrared spectrums of samples. X-ray diffraction (XRD) The figure 3 shows the XRD patterns for the pastes with and without admixture and cured during 28 days. Although, the identification of the C-S-H gel through XRD is particularly difficult, the presence of portlandite and a non reacted SCR can be clearly identified. Minor portion of ettringite is detected as SCR portion increase in the studied samples. Figure 3. X-ray diffraction of samples 0 10 20 30 40 50 60 0246 Strength\Totalporosity %SCR % MPa 1st Spanish National Conference on Advances in Materials Recycling and Eco- Energy Madrid, 12-13 November 2009 S05-6 192 DISCUSSION The studied hydration process shows that the incorporation of SCR to Portland cement matrices does not develop into different compounds of the normal hydration of Portland cement. However, it would be very interesting to make a next step in the investigation and try to follow the reactions not only at the macro and micro scale but also at the nano scale; it would be of great interest to know the probably incorporation of different elements from the SCR into the hydration products and a special effort should be done in the leaching of these matrices in order to avoid the release of hazardous compounds. In the relation to the physical properties of these materials, this behaviors could be assigned to the reaction at early ages of the aluminum from SCR with portlandite giving to a release of hydrogen that provoke a more porous structure and having consequences in the strength development of materials. However, the presence of 5% of SCR does not modify the total porosity but the mechanical strength decrease, then it would be good to make another microstructural studies as determination of pore size distribution and scanning electron microscopy in order to clarify this results. Then, it is obvious that non structural applications can be affronted with this type of mixtures but they still present good properties and probably will give solutions to potential ongoing new purposes. CONCLUSIONS The use of the SCR as a component of the cement matrix induces to: 1. A substantial change in compressive strength compared to the specimens without admixtures. A decrease of 31% is measured. 2. There is an influence in the set of the mixtures and provoke a retard of the initial and final set but still it is into the standards requirements. 3. The total porosity of mixtures is influenced and decreased up to 1% for samples with SRC and it is not modified for 5%. 4. With the experimental techniques used there were not detected compounds different of that of the normal ones observed in the Portland cement hydration. Major portion of ettringite and portlandite were detected in samples without SCR. REFERENCES [1] V. M. Fthenakis. “End-of-life management and recycling of PV modules” Energy Policy 28 (2000) 1051-1058. [2] V. Fthenakis, W. Wang, H. C. Kim “Life cycle inventory analysis of the production of metals used in photovoltaics” Renewable and Sustainable Energy Reviews 13 (2009) 493–517. [3] A. Sharma, C.R. Chen, Nguyen Vu Lan. “Solar-energy drying systems: A review” Renewable and Sustainable Energy Reviews 13 (2009) 1185–1210. [4] D. Appleyard. Light Cycle: Recycling PV materials. Renewable Energy World Magazine (2009). [5] E. Bombach, A. Muller, K. Wambach, I. Rover, Recycling of Solar cells and Modules-Recent Improvements. 20th European photovoltaic solar energy conference, Barcelona (2005).