Full text
1 Meet Jaydeepkumar Ozaa,b, Andreas Starkc, Efthymios Polatidisd, Pere Barriobero Vilae,f, Moslem Shahverdia,f, Christian Leinenbach*a,b a Empa, Swiss Federal Laboratories for Materials Science and Technology, Überlandstrasse 129, 8600 Dübendorf, Switzerland b Laboratory for Photonic Materials and Characterization, École Polytechnique Fédérale de Lausanne (EPFL), 1015 Lausanne, Switzerland c Institute of Materials Physics, Helmholtz Zentrum Hereon, Geesthacht, Germany d Laboratory of Technology and Strength of Materials, Department of Mechanical Engineering and Aeronautics, University of Patras, Patra, 26504, Greece e Department of Material Science and Engineering, Technical University of Catalonia-BarcelonaTech (UPC), Barcelona 08019, Spain f CIM UPC, Carrer de Llorens i Artigas 12, 08028 Barcelona, Spain, g School of Civil Engineering, University of Tehran, 16th Azar Street, Tehran, Iran Abstract Iron-based shape memory alloys (Fe-SMAs) are emerging materials with extensive application in civil structures owing to their unique properties, including the shape memory effect. However, it is crucial to understand the time dependent behavior of Fe-SMAs for their effective application as prestressing element. In particular, behavior at individual stress, the underlying mechanism, and the transformation kinetics have not been investigated yet. To address these important fundamental research gaps, in-situ compression creep and stress relaxation experiments with high-energy X-ray diffraction (HEXRD) of a Fe-17Mn-5Si-10Cr-4Ni-1(V,C) Fe-SMAs were conducted. The time-depend- ent behavior of the Fe-SMA was investigated at different stress levels with respect to the yield strength (YS) at room temperature. The experimental result showed that the material exhibits a creep strain of up to 1.84% and 56 MPa relaxed stress at test stress of 769 MPa (1.6 YS) within one hour of holding. Stacking fault probability and phase volume fraction quantification provide an understanding of the mechanisms based on different stress levels. The transformation kinetics traced from the characteristics of HEXRD peaks offer further insights on creep depending on the contribution of {hkl} families. The paper concludes with an evaluation of the existing models for predicting creep and stress relaxation of Fe-SMA. Keywords Fe-based shape memory alloy (Fe-SMA), high-energy X-ray diffraction (HEXRD), Creep, Stress relaxation, Phase transformation, Transformation kinetics.
2 1 Shape Memory Alloys (SMAs) are a unique class of materials characterized by the shape memory effect (SME) and pseudoelasticity (PE). The SME involves a shape recovery after deformation upon heating and cooling while, PE describes the recovery of a large non-linear strain upon loading and unloading. These distinctive properties are crucial for a wide range of technological applications, thus have attracted significant research attention. Ni-Ti based SMAs have been the centre of this attention due to their good SME and biocompatibility. Ni-Ti based SMAs are used in applications for sensors, actuators, stents, in aerospace, automotive and other medical fields [1]. SMAs high damping capacity and fatigue resistance also increased the curiosity of structural engineers to apply the SMAs as smart materials [2]. However, high cost limits their potential usage where the material is required in bulk, e.g., reinforcement in concrete. Over the past two decades, scientists at Empa (Swiss Federal Laboratories for Materials Science and Technology) Switzerland have been investigating SMAs for applying it as reinforcements in concrete [3-5]. Fe-SMA consists of two major phases with different crystal structures and properties. The high temperature phase is the Face Centered Cub -austenite, and the low temperature phase is the Hexagonal Close Packed -martensite. The shape memory effect in Fe-SMAs derives from the reversible phase transformation between austenite and martensite. Pre-straining and activation are two - stressing in concrete [6]. The application of Fe-SMA for pre-stressing in civil engineering applications is efficient as it does not require anchorage, ducts, and hydraulic jacks, unlike conventional prestressing techniques. Additionally, pre-stress force loss due to friction can be eliminated. Overall, the good mechanical properties of Fe-SMAs [6-8] and ease of fabrication make them one of the emerging materials for reinforcement applications [3]. The innovative reinforcement application based on Fe-SMA has been successfully implemented by the industry [9] for structural strengthening and retrofitting of buildings and infrastructures. As the typical life span of a reinforced concrete structure is in the range of 50-100 years the time-sensitive properties of the reinforcement, such as creep and stress relaxation, plays a crucial role in determining the service life of these structures. Creep is the time-dependent plastic deformation of a material at constant stress and temperature [10]. Interest and investigation of creep at low homologous temperatures (T/Tm <0.5) have been limited as most of the alloys undergo a negligible amount of creep in such conditions. Pure metals [11-14] and binary alloys [15-17] undergo low temperature creep. However, limited creep studies on phase transforming material exhibiting martensitic transformation have been reported. Reed et al. [18] investigated and reviewed the creep behavior of austenitic stainless steel at temperatures as low as 4 K to RT. Creep strain in the secondary stage with respect to the normalized stress between 304L, 304LN, and 310 SS at 20 K for 1200 minutes was compared. It was observed that
3 304L and 304LN show lower creep strain compared to 310 grade due to the high amount of metastable austenite, which transforms into BCC martensite that increases strain hardening and decreases creep strain. Harjo et al. [19] conducted creep studies on TRIP steel at 716 MPa and metastable 304 SS at 432 MPa using in-situ neutron diffraction at room temperature. The TRIP steel and 304 SS showed ~1% creep strain after 10 hours, but the volume fraction of austenite did not change. Whereas Tsuchida et al. [20] conducted a creep test (constant load) at 719 MPa for a holding time of 10 hours with ining the holding time increased from 3.3 to 5.5% during thirty seconds of holding, and it remained almost similar after that. Creep due to transformation is confined in the initial few seconds in the investigated TRIP steel. Thus, limited studies on various TRIP steels at different stress levels suggest that creep due to transformation is negligible or confined to a few seconds, depending on the composition. Whereas, transformation in 304L and 304LN leads to reduced creep. Therefore, contradicting conclusions in the literature with limited investigation also motivate the creep investigation of Fe- SMA. The stress relaxation test is a valuable method for understanding the time-dependent behavior of materials. During such tests, the reduction of stress in a material held at a constant strain and temperature is investigated. The relaxation data is used for designing bolts, gaskets, and springs as the tightness decreases with time [21]. Similarly, relaxation results can be utilized for designing the Fe-SMA prestressed concrete beam [22, 23] or assessing the long term structural performance [24, 25]. The amount of relaxation is necessary for determining the achievable pre-stress levels. Thus, stress relaxation of pre-stressed Fe-SMA plays a key role on the structural response of the reinforced structure. In contrast to the investigated transformation based steels, the first ex-situ study of Fe-SMA shows a pronounced amount of creep and stress relaxation during a fifteen minutes holding in a stepwise study [26]. The creep and relaxation experiments of Fe-SMA directed towards transformation induced pronounced creep. However, investigation by stepwise stress increment with a single specimen leads to only a cumulative sum of transformation at different stress levels. As the reinforcement is directly subjected to a single stress value (recovery stress) during application and the recovery stress varies depending on the activation temperature, it is important to understand the behavior at different stress levels decoupling the stress effect. The transformation kinetics and the quantification can help understand its contribution and impact towards time dependent properties. Thus, the objective of the study was to characterize the material over time at different stress levels. Ex-situ experiments would require various specimens to be tested and characterized before, between, and after the test to study the rapid transformation. Therefore, in-situ testing and characterization using synchrotron radiation have been applied to investigate the real-time behavior of Fe-SMA. The diffraction information was acquired during loading, holding, and unloading to understand the overall behavior with a focus on time dependent mechanical behavior at different stress levels.
4 2 2.1 The SMA that was investigated in the study has a composition of Fe-17Mn-5Si-10Cr-4Ni-1(V,C) stahl GmbH & Co KG, Austria and re-fer AG, Switzerland. These rods are fabricated sequentially by a hot rolling process in several steps to the targeted diameter, followed by air cooling. Rods were machined to 4.5 mm diameter and 9 mm height cylindrical samples by mechanical lath for the compression experiments, as shown in Figure 1 (d). Key features such as surface finish and flatness were prepared based on the tolerance specified in the ASTM E9-19 standard. A length-to-diameter ratio of two was chosen to prevent buckling during the experiments. Before and after the creep tests, cylindrical samples were cut from the middle using electrical discharge machining (EDM) for microstructure analysis. The samples were ground and polished with Hitachi IM 4000 ion milling machine was used as a final polishing step. It provides controlled surface removal useful for surface-sensitive EBSD analysis. A Zeiss GeminiSEM 460 scanning electron microscope along with Oxford instruments symmetry S2 EBSD detector was used for collecting microstructure information. The accelerating voltage during EBSD mapping was 20 kV. The step size of the EBSD map was less than one micron. The results were analyzed using AZtecCrystal. 2.2 Compression creep and stress relaxation tests with High Energy X-ray Diffraction (HEXRD) were conducted at the P07 beamline, experimental hutch 3, PETRA III, Deutsches Elektronen Synchrotron (DESY) Hamburg, Germany [27]. A simplistic schematic representing the experimental setup is shown in Figure 1 (a). Cylindrical specimens were placed in a modified Bähr DIL 805 A/D dilatometer, as shown in Figure 1 (b). A pushrod connected to a Linear Variable Differential Transformer (LVDT) was used to collect strain information during the testing. During creep tests, the samples were subjected to targeted load values with respect to the yield strength (0.7 YS = 337 MPa, 0.9 YS = 433 MPa, 1.3 YS = 625 MPa, 1.6 YS = 770 MPa). The samples were loaded at a strain rate of 8×10-3 s-1 to reach the target stresses as soon as possible to prevent creep/relaxation during the loading phase. Later, the strain increment with time was monitored by LVDT at a constant load for one hour. The loading protocol was the same for the stress relaxation experiments, and the stress drop with time was monitored by the load cell at a constant punch position of the punch for one hour. Ideally, stress relaxation is with constant strain, but the dilatometer with LVDT did not have any feedback system for maintaining constant strain, so the experiments were conducted with a constant punch position. The strain increment with time and stress
5 drop with time are termed creep strain and relaxed stress. Compression creep and stress relaxation tests were conducted at different stresses at room temperature (23°C) for a duration of one hour. The high energy X-rays of 0.124 Å wavelength (~100 keV) were incident on the specimen during the test, and the diffraction rings were captured using PerkinElmer XRD image-plate detector. The slit aperture size with (1 x 1 mm2) beam spot parameters were optimized to receive the best possible signal. The sample-to-detector distance was approximately 1430 mm. A LaB6 NIST SRM 660b standard specimen was measured for calibration of the diffraction setup. The diffraction rings were captured every 0.2 seconds in FAST mode for the first fifteen minutes. Later, the capture rate was switched to every two seconds in SLOW mode for the rest of the test period. Debye-Scherrer diffraction rings obtained during the test were converted into Cartesian coordinates (azimuthal angle - q (Å-1)) to obtain diffraction graphs (Intensity vs q (Å-1)). For the conversion, a 360° Azimuthal integral of the Debye rings was done using Fit2D software. The diffraction peaks were indexed using the crystallography open database (COD) in Xpert HighScore software and literature. To gain further insights into the time dependent behavior, peak properties such as integrated intensity and lattice strain along the loading and transverse deformation direction were evaluated by integrating specific regions ('cakes') of the diffraction rings. For loading direction, the chosen cakes were from 175-185° and 355-5°, whereas for transverse direction cakes from 85-95° and 265-275° were selected, as shown in Figure 1 (c). Both cake regions were averaged to have better statistics, and the findings are reported in section 3.4. Individual peaks were fitted by the PseudoVoigt function in Python using the lmfit [31] library to obtain integrated intensity and peak position. The normalization of integrated intensity is done by taking the initial value as a reference/unity. Peak positions were used to calculate the interplanar distance by Bragg's law, while lattice strain values were calculated using the interplanar distance of the lattice before the test ( ) and during the creep test at a specific time interval ( ). The lattice strain formula is as follows: Rietveld refinement was implemented on XRD spectra obtained from 360° azimuthal integral of diffraction rings. Phase reference files were uploaded in the GSAS II software [28]. The background was fitted using a Chebyshev polynomial of 9 orders. FCC and HCP phases were refined individually using spherical harmonics preferred orientation model with 8 and 6 orders. A generalized microstrain model was used to model the broadening of the peaks. Additionally, selective atom parameters and sample parameters with respect to the beam were refined considering the deformation with time. The stacking fault probability was calculated from the diffraction angle variation as per the Warren model [29]. (1)
6 (a) (b) (c) (d) Figure 1: (a) Schematic representation of the insitu synchrotron test setup, (b) Dilatometer setup used during the experiment, (c) 10° selective azimuthal integral parallel [0°] and perpendicular [90°] to the loading direction, (d) Cylindrical specimen before and after insitu creep of Fe-SMA.
7 3 3.1 Figure 2 shows SEM micrographs and EBSD phase maps of as received Fe-SMA before the creep test and after the creep test at 769 MPa for one hour and unloading. Grains with characteristic annealing twins are observed in Figure 2 (a). Additional figures with an overlay of special boundaries highlighting twins and IPF coloring implying no preferential orientation of the grains are shown in supplementary data (Figure 1). EBSD phase map (Figure 2 (c)) shows the FCC matrix (green color) (a) (b) (c) (d) Figure 2: Scanning electron micrographs of as received Fe-SMA (cross-section of the specimen) before the creep test and after the creep test at 769 MPa for one hour and unloading (a) & (b) Forward scatter detector (c) & (d) EBSD phase map overlay
8 phase. BCC phase is detected predominately near the grain boundaries. This BCC phase is assumed -ferrite phase due to ferrite stabilizer (like Cr, Si, or V) segregation near the grain boundaries [30]. This phase is also observed in austenitic stainless steel and shape memory alloys close to the composition of Fe-SMA used in this study [31, 32]. The detection -martensite in the undeformed state could be due to the internal stresses localized around the VC precipitate due to the difference in the thermal expansion coefficient of the matrix and precipitate [33]. The confidence index of the BCC and HCP phase is relatively low, so HEXRD with higher sensitivity provide much better statistics. Thus, the observation of these minor phases is discussed with HEXRD data in section 3.3. After the creep test, the microstructure reveals a notable distribution of martensite plates within the deformed grains (Figure 2 (b) and (d)). Typical martensite plates along the {111} planes are observed. However, it appears that the EBSD resolution during a step size of 0.4 µm can only detect thick martensite phase fraction (less than 1%) is observed through EBSD maps. Another reason for a lower martensite phase fraction could be the characteristic pseudoelastic behavior of Fe-SMA that leads to reverse transfor- -SMA used in this study is less than 1% [5]. Thus, martensitic transformation can be observed, but the detection of thin plates is limited with EBSD after the experiment.
9 3.2 In-situ creep experiments were conducted at four different stress levels (0.7 YS = 337 MPa, 0.9 YS = 433 MPa, 1.3 YS = 625 MPa, 1.6 YS = 770 MPa) with respect to the yield strength. The yield strength of Fe-SMA was calculated based on 0.1% offset, considering the smooth elastic-plastic transition due to nucleation of stacking faults and the onset of martensitic transformation prior to irrecoverable slip [33]. To understand the influence of stress-induced martensite on creep behavior of Fe- SMA, creep experiments were conducted at two stress levels below and at two stress levels above the yield strength. Additionally, it is also important to investigate creep above the yield strength as Fe- SMA is subjected to limited plastic deformation for stress-induced martensite formation during the pre-straining step for its application as a reinforcement in concrete. Subsequently, if the activation step does not fully transform the martensite to austenite to generate the recovery stress, the creep (a) (b) (c) Figure 3: (a) Compressive stress strain behavior during the creep test at 769 MPa (= 1.6 YS) for a holding period of 3600 seconds at 23°C. (b) Creep strain increment with time during the entire holding period. (c) Creep strain observed after onehour creep test at different stress levels with respect to the yield strength.
16 one hour) is observed by the dwell time of 1800 seconds. The creep strain and relaxed stress show a similar trend during the holding period. The variation of relaxation percentage at different initial states is shown in Figure 6 (c). 3.6 ion with time (a) (b) a function of stress during (a) creep and (b) stress relaxation for one hour. variation in integrated intensities, its evolution was tracked to gather insights into changes at various stress levels during the creep and stress relaxation experiments, as depicted in Figure 7. The austenite grain family trend over time at 1.6 YS and 1.3 YS is almost similar with variation in the magnitude of the reduction (Figure 7 (a)). This implies that the amount of transformation and plasticity effects over time reduce with the reduction in stress levels. Additionally, it can be observed that slow reduction of intensity at 0.9 YS, as it implies that limited plastification and phase transformation occur at this stress level. It is noted that the elastic/plastic transition zone in this material is extended, and some plasticity and/or phase transformation can already take place at stresses below the considered yield stress defined by the 0.1 offset method. In contrast, no reduction in the normalized integrated intensity at 0.7 YS is observed, and the creep strain is negligible during the holding period of one hour. This suggests that limited creep strain, dislocation plasticity and phase transformation occur at stress levels well below the yield strength. The stress relaxation increases with an increase in the stress level, as shown in Figure 6 (c). Similar levels during the stress relaxation experiments (Figure 7 (b)). The normalized integrated intensity of
17 owever, the magnitude of reduction is significantly less pronounced as compared to the creep experiment at that corresponding stress. Additionally, the variation 4 4.1 Figure 8: Stacking fault probability evolution during creep at different stress levels. Deformation in Fe-SMA is primarily induced by dislocation slip activity, stacking fault formation and subsequent transformation [39]. The stacking fault probability provides insights into stacking fault formation in the material. The stacking fault probability (SFP) was calculated by the variation of the diffraction angles using the Warren model [29]. (2) / hkl is the diffraction angle, which varies with time. The stacking fault probability of the four prominent austenite peaks (111) (200) (220) (311) was averaged. To better understand the trend, least-square based Savitky-Golay filter [40] was used on the data points shown with dashed lines. SFP variation with time at different creep stresses is shown in Figure 8. The dotted points are the data, and the dashed lines show the trend. An increasing SFP is observed with time for creep experiment at 1.3 YS and 1.6 YS, while almost zero SFP is observed at lower stress levels (0.7 YS and 0.9 YS). This indicates that stacking faults continue to form during creep at higher strain levels. Additionally, the SFP magnitude is higher in 1.3 YS as compared to 1.6 YS. Thus, it is hypothesized that more stacking faults are formed at that corresponding stress level.
18 The evolution of the peak intensities over time, as shown in Figure 7 (a) during the in-situ experiments, qualitatively suggests that phase transformation evolves during creep. However, to understand the correlation of the creep strain with the phase transformation, it is important to quantify the evolution of the martensite phase. The evolution of the phase volume fraction evaluated from the Rietveld refinement of selected diffraction spectra from creep and stress relaxation investigated at the highest stress level is shown in Figure 9. The results indicate that the austenite volume fraction decreases throughout the creep test, as shown in Figure 9 (a). The decrease in austenite is rapid during the initial thirty minutes, after which the rate of reduction slows down, as indicated by a change in the slope. This sharp reduction of austenite peak is accompanied by a sharp increase in martensite peak. Thus, the Rietveld refinement observation (a) (b) Figure 9: Phase volume fraction of the phases during the (a) creep test and (b) stress relaxation test at 769 MPa (1.6 YS). The phase quantification from the Rietveld refinement and weighted profile (Rwp) indicator for goodness of fit is summarized in Table 2 -martensite volume fraction is not 100% and 0% due to the stressinduced martensite formed during load application -martensite formation during the creep test at an engineering stress of 769 MPa for one hour is 9.79 %. Martensitic transformation is observed due to stacking fault formation on every second closely packed {111} plane. Possible displacement vectors for faulting on a {111} plane are 1/6 [-1-12], 1/6 [-12-1] or 1/6 [2-1-1]. If the displacement vectors of faulting are all the same, it is estimated that the maxi- 43]. In contrast, an unequal probability of the displacement vector will lead to lower shear. Assuming a heterogeneous displacement faulting vector, the strain due to martensitic transformation during creep of Fe-SMA might be
19 approximately half the maximum strain factor. Thus, the creep strain due to transformation at 769 MPa could be 1.71% (9.79 x 0.175). The additional creep strain can be due to dislocation plasticity and stacking faults formed that have not yet been transformed to martensite. The strain can vary depending on the grain orientation and limited partial deformation accommodation during transformation [26] mation is the dominating creep mechanism. Table 2: Phase volume fractions at different holding time during the creep test. Table 3: Creep strain and transformation correlation with the applied stress during creep at different stress levels Applied stress (x Y.S) Creep strain (%) Creep-induced martensite fraction (%) Creep strain (%) due to Transformation Stacking fault and slip activity 1.6 YS 1.84 9.79 1.71 0.13 1.3 YS 1.36 3.84 0.67 0.69 0.9 YS 0.14 - martensite intensity. 0.7 YS 0.03 The stacking fault probability and phase transformation give overall insights into the creep mechanism. The stacking fault probability is relatively high at 1.3 YS as compared to 1.6 YS, while the transformation is higher for creep at 1.6 YS. This implies that stacking fault contribution in the creep strain is higher at 1.3 YS. This can be observed if we assign the creep strain apart from the transformation, as shown in Table 3. The percentage distribution can vary depending on the peak fitting, so it has to be considered qualitatively. The phase volume fraction quantification was difficult for creep at 0.9 YS and 0.7 YS. However, we can infer the behavior from the SFP and integrated intensity plots from Figure 8 and Figure 7 (a). Creep at 0.7 YS does not result in a decrease in the integrated intensity of austenite peaks, implying deformation creep without transformation. On the other hand, creep at 0.9 YS leads to a reduction in integrated intensity and an increase in SFP, indicating more stacking faults and transformation. However, the intensity of the martensite peaks is too low for Rietveld refinement, making it challenging to quantify the extent of transformation. Time (sec) Creep strain (%) -FCC -HCP Weighted profile (Rwp) 0 0 54.62 45.38 5.72 1800 1.73 45.31 54.69 6.22 3600 1.84 44.83 55.17 6.25
20 The phase volume fraction variation during the stress relaxation test at 1.6 YS is shown in Figure 8 (b). A reduction of the amount of austenite over time can be observed, suggesting austenite-to-mar- tensite forward transformation. However, the variation is limited to one thousand seconds, and the magnitude of variation is ~1.21 %. Later, almost negligible variation is observed with time. It is important to mention that the stress relaxation tests were performed with a fixed crosshead position, not by controlling the strain of the compression sample, due to the limitations of the available setup at the beamline. This approach could result in the relaxation of the dilatometer component and a noisy signal. Therefore, to gain more insights, the behavior should be examined at a constant strain. Overall, creep strain depends on the magnitude of applied stress. Negligible creep is observed at stress levels well below the yield strength (0.7 YS) for the holding time of one hour. Significant creep is observed at stresses closer to the yield strength (0.9 YS), and pronounced creep is observed above the yield strength of Fe-SMA (1.3 and 1.6 YS). The creep strain is influenced by the initial stressfurther stacking fault generation and transformation. The contribution of stacking fault and transformation in creep strain is highly dependent on the creep stress. The higher the stress, the more stacking faults are generated during loading, and hence during creep, the transformation strain contribution is higher, and the SFP is lower. The stress relaxation also strongly depends on the creep stress. 4.2 Fe-SMA is foreseen as an emerging reinforcement material for extending the life of the existing structures. As the reinforcement service life range is between 50-100 years, it is crucial to understand the time dependent material characteristics. From our experiments, significant creep and stress relaxation was observed within the first 1800 seconds. Thus, it is crucial to model the time dependent behavior during the initial stage. Existing empirical models for creep and stress relaxation [41] have been applied to the acquired data, and possible implications are discussed. 4.2.1 Materials with high primary creep strain have been described by the power law function. (3) a and b are material constants with varying time (t). The time exponent b relates to the exhaustion rate of the creep. The exhaustion rate is linked with the reducing dislocation mobility with time due to increased dislocation density or dislocation distribution change. A smaller value of the exponent indicates faster exhaustion of the creep strain. Andrade [42] conducted creep experiments on lead, fused wire (lead and tin) and copper wires at 15°C and 162°C. In this work, the extension was divided
21 into three different categories. One was the immediate extension on loading, an initial flow that grad- Additionally, the experimental data with a specific time exponent (b = 1/3) fitted well, and the proposed relation was: However, the specific time exponent is not universal and varies for different materials. The logarithmic creep model considers the plastic strain during loading and strain increment with logarithmic function of time [43] (5) Power law creep, Andrade, and logarithmic creep are common models utilized to interpolate experimental data. These empirical models are also applied to the experimental creep data of Fe-SMA in this present work. The creep strain as a function of time is best fitted with the exhaustion log model at 0.7 YS, 1.3 YS, and 1.6 YS with R2 value greater than 0.97, except for creep at 0.9 YS. The fitted curves with experimental data for 0.9 YS and 1.6 YS are shown in Figure 10. The best fit parameter values of different models for the creep behavior, including the goodness of fit, are shown in Table 4. The fitted curves of other stress levels are added in the supplementary data (Figure 3). The exhaustion model shows a rapid creep that reduces with time. The behavior has been correlated with increasing dislocation density and reducing dislocation mobility with time. This can explain the creep behavior at 0.7 YS as we observe no reduction of integrated intensity with time, as shown in Figure 7 (a). However, it certainly does not explain the creep behavior of Fe-SMA at different stress levels. In the case, where the creep behavior is studied above the yield strength, stress-induced martensite is initiated at this stress level. Even during the holding period of constant load, the in-situ observation shows that the martensitic transformation dominates the rapid creep in the initial few minutes, and later, the transformation rate slows down, and it is accompanied by a reduced creep rate. However, the fitting of creep strain at 0.9 YS is well described by the simple power-law rather than the exhaustion log model. It is also evident in Figure 10 (b) that the exhaustion log model overpredicts the creep strain in the initial few seconds. This behavior can be explained by the normalized integrated intensity variation with time in Figure 7 (a). Here, the intensity reduction is not rapid in the initial few seconds, but it reduces significantly with time. Therefore, stress levels close to the yield strength (0.9 YS), where we do not expect a significant amount of stress-induced martensite also show martensitic transformation with time. Thus, long-term creep behavior evaluation at stress levels close to the yield strength will provide vital information. (4)
22 Overall, the creep data can be fitted with the existing creep models. However, the dominating creep mechanism at different stress levels cannot be accounted for. Therefore, a new single model considering the mechanism and stress parameters to describe the creep of Fe-SMA shall be considered. (a) (b) (c) (d) Figure 10: Room temperature creep behavior of Fe- SMA fitted with empirical models (a) & (b) at 0.9 YS stress (c) & (d) 1.6 YS stress. Table 4: Empirical model details and fitting parameters for creep behavior of Fe-SMA. Model Best fit parameters value R2 0.9 YS 1.6 YS 0.9 YS 1.6 YS Simple power-law a = 0.03, b = 0.2 a = 0.86, b = 0.1 0.99 0.95 (b) (d)
23 Andrade creep 0 0 0.98 0.82 Logarithmic exhaustion creep 0 = 1 = 0.03, t0 = 1 0 = 1 = 0.39, t0 = 1 0.81 0.99 4.2.2 Stress reduction with time can be observed in stress relaxation experiments. Crystal plasticity based models are used to relate the behavior. The flow stress required for dislocation motion during plastic i) due to obstacles with stress distribution over a large *) due to short-range obstacles [44]. i + * (6) The total strain in a material can be due to elastic and plastic contributions. total elastic plastic total = 0 elastic plastic = (7) Based on the Orowan equation [45], the time dependent behavior during stress relaxation is a function m), Burger's vector of dislocation (b), and average dislocation velocity plastic = m (8) m is the mobile dislocation density. (9) Log model 1 in equation (9) is obtained when we substitute the average dislocation density in the Arrhenius rate form [46] and plastic strain rate equation (7) in the Orowan equation (8). The Log m and i plastic deformation [47]. Thus, fo m was introm in the differential form. (10)
24 The above expression considers the variation o m constant. However, the relaxed stress output is similar to log model 1 for Fe-SMA and is not discussed further. (11) Varma et al. [48] developed a constitutive model (Equation 11 - Log model 2) with consideration for the evolution of transient stress and correct prediction of activation volume. The log model 1 has some limitations with modeling evolution of the mobile dislocation density and activation volume. Nevertheless, it fits the experimental data of 316L stainless steel well without major errors. Whereas log model 2 fitting was observed to be better than log model 1 [48]. (a) (b) (c) (d) Figure 11: Room temperature stress relaxation behavior of Fe-SMA fitted with empirical models at different stress levels (a) & (b) at 0.9 YS stress (c) & (d) 1.6 YS stress. (b) (d)
25 Table 5: Empirical model details and fitting parameters for stress relaxation behavior of Fe-SMA Model Best fit parameters value R2 0.9 YS 1.6 YS 0.9 YS 1.6 YS Log model 1 0.99 0.99 Log model 2 = 3.06, = 0.2, = 20, = 2.49, 0.75 0.99 0.99 Thus, the stress relaxation behavior of Fe-SMA at different stress levels was fitted using logarithmic empirical models in the literature [48-50]. For comparison with creep, stress relaxation behavior along with fitting at 0.9 YS and 1.6 YS is shown in Figure 11. Both the models fit well with R2 value of 0.99, as shown in Table 5. However, the empirical models underpredict the relaxation during the first 100 seconds and close to one hour. This can be due to different stress relaxation mechanisms as we observe phase transformation for a few hundred seconds. Log model 1 and 2 show almost similar relaxation trends at 0.9 YS with residual (deviation of the model output as compared to the experimental data) of 1.1 MPa. However, with increasing stress log model 2 tends to be closer to the behavior of Fe-SMA, where the residual for log model 2 is 3 MPa and log model 1 is 6 MPa. From the log model 2 fitted data, gesting mobile dislocation density increment along with strain hardening while is related to internal i ) as a function of dislocation annihilation and strain hardening. Both and value increases with increasing start stress values for stress relaxation. This implies that the mobile dislocation density and internal stress increase at higher stress. A higher amount of dislocation density and internal stress can be the reason of higher stress relaxation at higher stress levels. However, the deformation of Fe-SMA is dominated by stacking faults, and the stacking fault can be related to . The amount of stacking fault and subsequent transformation increases during loading. At the start of the relaxation, the stacking fault interaction is high along with phase transformation leading to higher relaxation. After a few hundred seconds, the interaction reduces, and the internal stress is redistributed leading to a reduction in relaxation rate. Overall, the empirical models fit well with the experimental data of Fe-SMA. However, the basis of the model varies, and the mechanism during stress relaxation of Fe-SMA seems to be difficult to interpret with this limited study.