scieee AI-readable full text Open interactive document viewer

Microstructural and mechanical characterization of additively manufactured parts of maraging 18Ni300M steel with water and gas atomized powders feedstock

Peinado, Gabriel,Carvalho, Caue,Jardini, Andre,Souza, Eduardo,Ávila Díaz, Julián Arnaldo,Baptista, Carlos

Abstract

The demand for manufacturing components with complex geometries, good mechanical properties, and material efficiency has surged across various industries, encompassing aerospace, military, nuclear, and naval sectors. Laser powder bed fusion (LPBF), as an additive manufacturing (AM) process, has emerged as a promising method for producing ultra-high mechanical strength alloys, like maraging 300 steel (18Ni300M). However, in numerous studies in the literature concerning the effects of processing parameters on the properties of 18Ni300M steel parts fabricated through LPBF, limited attention has been given to the influence that powder atomization methods may exert on the final properties of these parts. This article investigated the effect of gas atomization (GA) and water atomization (WA) processes on the microstructure of 18Ni300M steel powders and the mechanical properties, microstructure, and chemical composition of LPBF-produced parts. The results revealed significant distinctions in the morphology, aggregation degree, and particle size distribution between the GA and WA powders, which directly influenced the microstructure and affected the amount of defects in LPBF-produced parts. Despite the similar mechanical response found in the WA and GA specimens in the elastic region, the samples produced with the WA batch presented a brittle behavior with a ductility of only 4.06%, whereas the GA parts had an elastoplastic behavior with an elongation of 11.52%. The bulks from the WA batch produced in the LPBF process were compromised due to powder contamination with oxygen, which increased gas porosity and effected fragile oxide particles visible on the fracture surface

Full text

Vol.:(0123456789) 1 3 The International Journal of Advanced Manufacturing Technology https://doi.org/10.1007/s00170-023-12686-2 ORIGINAL ARTICLE Microstructural andmechanical characterization ofadditively manufactured parts ofmaraging 18Ni300M steel withwater andgas atomized powders feedstock GabrielPeinado1· CauêCarvalho1· AndréJardini2· EduardoSouza2· JuliánArnaldoAvila3,4· CarlosBaptista1 Received: 30 August 2023 / Accepted: 13 November 2023 © The Author(s) 2023 Abstract The demand for manufacturing components with complex geometries, good mechanical properties, and material efficiency has surged across various industries, encompassing aerospace, military, nuclear, and naval sectors. Laser powder bed fusion (LPBF), as an additive manufacturing (AM) process, has emerged as a promising method for producing ultra-high mechanical strength alloys, like maraging 300 steel (18Ni300M). However, in numerous studies in the literature concerning the effects of processing parameters on the properties of 18Ni300M steel parts fabricated through LPBF, limited attention has been given to the influence that powder atomization methods may exert on the final properties of these parts. This article investigated the effect of gas atomization (GA) and water atomization (WA) processes on the microstructure of 18Ni300M steel powders and the mechanical properties, microstructure, and chemical composition of LPBF-produced parts. The results revealed significant distinctions in the morphology, aggregation degree, and particle size distribution between the GA and WA powders, which directly influenced the microstructure and affected the amount of defects in LPBF-produced parts. Despite the similar mechanical response found in the WA and GA specimens in the elastic region, the samples produced with the WA batch presented a brittle behavior with a ductility of only 4.06%, whereas the GA parts had an elastoplastic behavior with an elongation of 11.52%. The bulks from the WA batch produced in the LPBF process were compromised due to powder contamination with oxygen, which increased gas porosity and effected fragile oxide particles visible on the fracture surface. Keywords Maraging steel· Powder atomization· Additive manufacturing· Laser powder bed fusion· Microstructural characterization· Mechanical properties 1 Introduction Maraging steels belong to the group of ultra-high mechanical strength steels. Their properties are achieved due to an aging heat treatment that allows the formation of nanometric precipitates (e.g., Ni3Ti, Ni3Mo, Ni3(Ti, Mo), Fe7Mo6, Fe2Ti, Fe2Mo and Fe2(Ti, Mo)) distributed along a martensitic matrix [1], as well as the TRIP (transformation-induced plasticity) effect [2]. In academic and industrial fields, the maraging steel class that has attracted the most attention is the one presenting 18% (wt. pct.) of nickel and grade 300 (18Ni300M) due to the combination of its mechanical strength (YS = 300 ksi ≈ 2000MPa) and fracture toughness (KIc = 80MPa∙m0.5) [3]. For additive manufacturing purposes, besides the excellent mechanical properties of this alloy, its very low carbon content (< 300ppm) hindered the precipitation of brittle carbides at the grain boundaries and the nucleation of solidification cracking and retained austenite [3–5]. * Julián Arnaldo Avila julian.arnaldo.a[email protected] 1 Engineering School ofLorena, University ofSão Paulo (EEL/USP), Estrada Municipal Do Campinho, S/N, Lorena, SPZipCode:12602-810, Brazil 2 School ofChemical Engineering, State University ofCampinas, (FEQ/UNICAMP), Avenida Albert Einstein, 500, Campinas, SPZipCode:13083-852, Brazil 3 Research Group inStructures andMechanics ofMaterials (REMM), Department ofStrength ofMaterials andStructural Engineering, Universitat Politècnica de Catalunya (UPC), Diagonal 647, 08028Barcelona, Spain 4 School ofEngineering ofSão João da Boa Vista, São Paulo State University, Av. Profa. Isette Corrèa Fontão, 505, SãoJoãodaBoaVista13876-750, Brazil The International Journal of Advanced Manufacturing Technology 1 3 Currently, works involving 18Ni300M steel processed by LPBF are focused on optimizing its mechanical properties through the study of process or heat treatment parameters [1, 6–9]. However, the characteristics of the particulate material used during AM can be important in order to understand the properties of manufactured parts. Many variables are related to the production of high-density parts by LPBF [10–12], such as the spot size, laser power, hatch spacing, scan speed, and layer thickness. Regarding the powder feedstock, its chemical composition, permeability, flowability, particle size distribution, average size, morphology, aspect ratio, and solidity of the particles must be investigated since they directly affect the properties of the LPBF printed parts. When preparing powders for LPBF, two atomization methods are commonly employed: gas atomization (GA) and water atomization (WA), the latter being lower expensive than the former [13]. Both procedures begin with the melting of the metallic alloy, which flows through a funnel into the atomization chamber. Inside the chamber, a high-pressure stream of either water or inert gas (N2 or Ar) is used to promote the atomization and subsequent solidification of the metallic material. The solidified metal particles are then collected in the lower portion of the atomization chamber [14]. As far as morphology is concerned, the powder particles generated by the gas atomization process tend to be more spherical than those produced by water atomization [14] due to the gas’s lower thermal capacity than water, which allows for a longer solidification time for the liquid metal. However, both processes are susceptible to contamination with interstitial elements [14–16]. In a previous work [17], the impact of GA and WA processes on the powder morphology of H13 tool steel was investigated. It was found that GA produced spherical powder particles, while WA resulted in cylindrical, irregular, and often coarsened shapes. The authors used mathematical models, considering particle size, LPBF process parameters, and material properties to predict the behavior of powder particles in the melt pool. The shape characteristics of WA powder particles led them to reach significantly higher temperatures in the melt pool than when using GA particles (1760°C and 1018°C, respectively). This temperature difference during solidification caused a higher thermal gradient in WA particles, increasing the likelihood of thermal microcrack formation. The modeling results showed that a larger percentage of GA particles (83%) solidified upon reaching the melt pool. In comparison, a smaller percentage of WA particles (65%) entered the melt pool, with some remaining in a liquid (49%) or vapor state (16%). The study’s findings significantly affect additive manufacturing, especially for LPBF-processed parts. The higher temperature of the WA particles and their increased porosity may compromise part integrity and adhesion between layers, affecting final part quality. Additionally, chaotic liquid metal flow in WA particles can widen the melt pool and accentuate the segregation of substances like carbides and nitrides [17]. Deirmina etal. [18] investigated the mechanical properties of 18Ni300M additive manufactured parts processed from steel powders with different contents of N and O. The authors verified that the monotonic properties of the specimens were not significantly affected by the raw material. However, the fatigue strength of the samples processed with the powder containing lower oxygen content was approximately 20% higher [18]. Another attempt to compare WA and GA powder has been reported in 4130 steel [19], where the components processed with WA feedstock showed a loss of ductility. Nevertheless, after heat treatments, they were able to homogenize the mechanical properties with those from the GA feedstock. On the other hand, in the case of 316L stainless steel [20], the WA and GA feedstock delivered similar mechanical strength and elongation to fracture, but both had longer elongation than the cast counterpart, which was below 40%. Nothing related to the maraging steel atomized with different routes was found. The main objective of this work is to characterize two distinct batches of 18Ni300M steel particulate material and investigate their influence on the microstructure and mechanical properties of parts processed by LPBF. The GA and WA powder feedstocks presented spherical and semiregular particles, respectively. Both materials were processed using the same fabrication parameters and the same LPBF equipment, and the powder and as-built components were submitted to microstructural and mechanical characterization. Although the WA feedstock delivered samples with less elongation to fracture than the GA parts, and despite the oxygen contamination, some of their microstructural features and their mechanical response in the elastic region were similar, thus offering an alternative material with a cheaper atomization process. 2 Material andexperimental procedure 2.1 Material andadditive manufacturing The 18Ni300M steel powders used as raw material in the LPBF process were gas and water atomized by two companies. The two batches of powders would be designated GA (N2 gas atomized) and WA (water atomized) for identification purposes. The main morphometric difference between the particulate materials is the particle size range. According to the information provided by the companies, the batch GA presented at the end of the process an average particle size between 40 and 50µm. In comparison, the batch WA would contain particles between 40 and 100µm. In this investigation, roundness, aspect ratio, and solidity among the various existing morphometric parameters were studied due to their importance in describing powders intended for the LPBF process. In a nutshell, roundness The International Journal of Advanced Manufacturing Technology 1 3 indicates the similarity between the projected area of a particle and the area of an equivalent circle; in turn, the aspect ratio expresses the ratio between the largest axis and the smallest one existing in a particle and, finally, solidity is related to the projected area by the area of the convex envelope of a particle [21]. The microstructural analyses of the powders were carried out using scanning electron microscopy (SEM) in a HITACHI TM 3000 microscope. The freeware ImageJ, version 1.53t [22], was employed to determine particle size distribution and morphometric parameters. The 18Ni300M steel powders from the GA and WA batches were processed using LPBF technology in an EOS M280 manufacturing device in a nitrogen-protective atmosphere. The laser power varied between 180 and 200 W, while the layer thickness was kept constant at 30μm. The beam spot diameter ranged from 100 to 120μm. Specimens were processed for microstructural, chemical, and mechanical characterizations. 2.2 Microstructural andchemical analysis Samples were ground from 320 to 2400-grit SiC emery paper, then polished in silica suspension with 0.05μm particle size according to the ASTM E3 standard [23]. Etching was performed with 5% HNO3 mixed with ethanol for 15s. Melt pools were investigated in a LEICA optical microscope (OM), model DM 4000M, whereas the solidification structures formed during the LPBF process were assessed using SEM in a Tescan Mira 4 microscope. To investigate the anisotropy within sections of parts processed by LPBF, the samples were subjected to Vickers microhardness testing on three different faces relative to the build direction (Z), which are referred to as interlayer (XY), longitudinal (XZ), and transversal (YZ), in this study, according to ISO/ASTM 52900 terminology for additive manufacturing [24]. The Vickers microhardness measurements were carried out at 10 specific points, adhering to the ASTM E384-17 standard [25]. The chemical composition concerning the main alloy elements present in 18Ni300M (e.g., Ni, Co, Mo, Ti, Al, C, Mn, Si, and Fe in balance) of the AM bulks was determined through optical emission analyses using an RL-4460 Thermo Fisher instrument. The wet chemical analyses were conducted on printed parts from batches GA and WA, to primarily determine the oxygen and nitrogen content in the bulk material. Due to limitations in the optical emission technique, it was not feasible to identify these elements. The samples destined for microstructural and chemical analyses had a cubic geometry (10mm). X-ray diffraction analyses were conducted using a PANalytical Empyrean diffractometer with Mo radiation (λ = 0.7093Å), a current of 30mA, and a voltage of 40kV. The measurement range was set at 2θ = 15º to 60º with a step size of 0.02º and a counting time of 70s. Phase identification was achieved by indexing the diffraction patterns with the crystallographic data from the ICSD database, where martensite (α’) was indexed with entry 64,795 and austenite (γ) with entry 44,862 using the PowderCell software. The identified phases were quantified using the X’ Pert HighScore Plus software and a spreadsheet implemented with the Williamson-Hall method [26]. 2.3 Mechanical characterization Tensile tests were carried out on a MTS 810.23M machine under displacement control using an MTS extensometer model 632.26F-21 with a gauge length of 8.0mm and a crosshead speed of 0.5mm·min−1. The data acquisition rate was 4 points per second. The subsize specimens tested were based on references [27–29] and are shown in Fig.1 (a). The 3D model of the test specimen, along with the X, Y, and Z axes relative to the build direction, has been incorporated into Fig.1 (b). Average monotonic mechanical properties of the 18Ni300M steel, i.e., yield stress (YS), ultimate tensile strength (UTS), Young’s modulus (E), and percent elongation (ΔL) were determined from three tests for each batch, following ASTM E8/E8 M-1 standard [30]. One way to evaluate the influence of powder feedstock on the mechanical properties of 18Ni300M steel parts processed by LPBF is to employ work hardening models. Generally, the three known types of work hardening models are isotropic, kinematic, and combined hardening. The isotropic hardening represents the expansion of the elastic domain and is related to short-range interaction of dislocations; the kinematic hardening represents the translation of the yield surface in the stress space and is related to the straining process that involves long-range interactions with glissile dislocations [31]. Fig. 1 Tensile specimens processed by LPBF in the 18Ni300M, dimensions in mm, (a) geometry, and (b) the isometric view showing the orientation of the cartesian axis. Z direction coincides with the building direction The International Journal of Advanced Manufacturing Technology 1 3 The true stress–logarithmic plastic strain curves were plotted, and power-law models based on Hollomons’ equation were fitted to the experimental data. The best correlation between experimental data and the powermodel mentioned above was determined using the Levenberg–Marquardt least square method. The parameter that indicates the best fit is the lowest sum of the squares of the deviation (χ2). Fractographic analyses of 18Ni300M specimens were carried out using SEM in a Tescan Mira 4 microscope. Among the isotropic hardening models, Hollomon’s power law and its adaptations are the simplest and the most widely used for metallic materials, such as steels and aluminum alloys [31]. Hollomon’s power law is denoted by Eq.1, where σ and  εp are the true stress and logarithmic plastic strain, respectively, K is the strength coefficient, and n is the strain hardening exponent. In certain scenarios, accounting for pre-existing residual strain in the material, arising from forming processes or a high density of defects inherent in the manufacturing process, as observed in parts processed by AM [32], becomes necessary. A common way to address this situation is to use Swift’s work hardening model, which presented in Eq.2 [31]. in the given equation, σ ,  εp , K and n hold the same meaning as the parameters in Hollomon’s model, while  ε0 represents the pre-strain induced by material defects. (1) σ=K ⋅  ε p n (2) σ=K ⋅ (  ε p + ε0 )n 3 Results 3.1 Powder Figure2 depicts micrographs and particle size distribution of the 18Ni300M powders from GA and WA batches. Table1 and Fig.2 (e)-(f) show the morphometric parameters of GA and WA powders, respectively. Figure2 (a)-(d) shows that the particles of GA batch exhibit a higher level of uniformity than those in the WA batch. Both batches have agglomerated particles and smaller particles attached as “satellites” to the surface of larger ones. However, the particles in the WA batch display more irregularities, and satellites are more frequent, which indicates a less uniform particle distribution. As shown in Fig.2 (e) and (f), the GA batch has a normal particle size distribution between 20 and 40μm (normal distribution). This range is commonly used for LPBF processing of 18Ni300M steel powders [7–9, 18]. On the other hand, the WA batch has a bimodal particle size distribution, with two predominant ranges: between 20 and 40μm and between 60 and 100μm. The analysis of Fig.2 (e) and (f) and Table1 further supports the discussions presented by Pinkerton and Li [17] regarding the morphology of the GA and WA feedstocks, which were briefly mentioned in the literature review of this article. The bimodal distribution of particles in the WA batch affected the roundness and solidity. The irregularity of the particles impairs the projection of an irregular particle in a circle and the ratio between the area of a particle and the area projected by the convex envelope, as seen in the lower Fig. 2 Micrographs of the GA powder in the upper row and WA in the lower row: (a and c) low magnification and (b and d) high magnification SEM images and (e and f) particle size distribution The International Journal of Advanced Manufacturing Technology 1 3 values determined for these morphometric parameters of the WA batch. However, the greater asymmetry and smaller circularity of particles result in a higher aspect ratio (ratio between the major and minor axes) for the WA batch. 3.2 As‑built parts The bulks’ chemical composition determined through optical emission analyses and percentage differences (Δwt.%), per the MIL-S-46850D specification [8, 33], are presented in Table2. Moreover, the oxygen and nitrogen content (ppm) measured by wet chemical analyses in the LPBF-manufac- tured parts from both batches are also provided in Table2. The XY, XZ, and YZ sections of 18Ni300M parts printed by LPBF were reconstructed using optical micrographs covering an area of 900 × 1200μm. For a detailed analysis of the melt pools, the transverse section was examined using micrographs sized at 420 × 440μm using an OM. From these micrographs, the width of 10 randomly selected melt pools were measured and the results were presented in Table3. Additionally, the solidification microstructure of the YZ section was studied using micrographs obtained from an SEM (30 × 30μm). The results for the GA batch are presented in Fig.3 (a), (c), and (e), whereas the results for the WA batch are depicted in Fig.3 (b), (d), and (f). As outlined in the ASTM 962 standard [34], the density of the 18Ni300M parts was calculated following Archimedes’ principle. Four fields in XY section micrographs with an area of 900 × 1200μm were used to estimate pore surface fraction by quantitative stereology theory. Two representative fields for batches GA and WA are represented in Fig.4. Direction-dependent mechanical properties are common in 18Ni300M steel parts processed by LPBF, because of the material’s microstructural disparities inherited from additive manufacturing processing [35]. These differences become more significant when the material does not undergo a heat treatment that would homogenize it, as seen in the present study. To assess the mechanical anisotropy of XY, XZ, and YZ sections, Vickers microhardness of GA and WA batches of 18Ni300M steel samples was measured. The results are shown in Fig.5. The reconstruction of the XY, XZ, and YZ sections is shown in Fig.3 (a) and (b), revealing no significant differences between the bulk structures of the two batches of 18Ni300M steel, except for a higher concentration of defects in the material processed from the WA batch, which is clearly visible. Figure3 (c) and (d) display the melt pools of the YZ section. As expected, the concentration of pores (indicated by white arrows) within the pools and at their edges is more pronounced in the WA batch due to the bimodal distribution and lower circularity of the powder particles mentioned earlier. Additionally, the micrograph of Table 1 Morphometric parameters of 18Ni300M powder batches Graphic definition [21] ParameterGA batchWA batch Roundness0.68 0.40 Aspect ratio1.14 1.69 Solidity 0.92 0.87 Table 2 Chemical composition (wt. % and ppm) of 18Ni300M powders Batch Ni Co Mo Ti Al C Mn Si Fe N(ppm) O(ppm) GA 18.82 8.80 4.46 1.45 0.06 0.008 0.02 0.08 Bal 52.0 12.0 WA 18.53 9.58 4.50 0.81 0.10 0.011 0.03 0.05 Bal 129.5 4460.0 Δwt.% 1.5 8.9 0.9 44.1 66.7 37.5 50.0 37.5 – – – Table 3 Melt pool width and density analyses of 18Ni300M parts were conducted using Archimedes’ principle and quantitative stereology theory Batch Melt pool width (μm) Archimedes’ principle Quantitative stereology GA 56.8 ± 6.0 99.3% 99.7% WA 77.7 ± 8.9 99.0% 99.2% The International Journal of Advanced Manufacturing Technology 1 3 Fig. 3 (a) and (b) Reconstruction of the XY, XZ, and YZ sections of 18Ni300M parts printed by LPBF; (c) and (d) YZ section optical micrographs and (e) and (f) XY section electronic micrographs of 18Ni300M steel bulks Fig. 4 Quantification of the surface porosity fraction (highlighted in red) in the (a) GA and (b) WA batches of 18Ni300M steel The International Journal of Advanced Manufacturing Technology 1 3 the WA batch shows the presence of large inclusion particles (marked by black arrows) [32, 36]. In contrast, the GA micrograph exhibits a lack of fusion defect (pointed by a dashed arrow), which is characteristic of the LPBF process [4]. Upon analyzing Table3, it is evident that the average width of the melt pools found in the material processed from the WA batch is larger but still within the range reported in the literature (45–100μm) [4]. This result can be explained based on the findings of Pinkerton and Li, as mentioned earlier, since the flow of liquid metal becomes more disorganized as the morphological irregularity of the particles increases, which is consistent with the WA batch [17]. In Fig.3 (e) and (f), the microstructure resulting from solidification is highly similar between the two batches, aligning with findings from other studies in the literature that report a cellular solidification microstructure characterized by epitaxial grain growth from the boundaries of the melt pools [32, 37, 38]. On the other hand, the solidification microstructure of 18Ni300M steel from the GA batch as shown in Fig.3 (e) reveals three distinctive cellular substructures characteristic of the LPBF process: (1) thin, (2) coarse, and (3) elongated cells [39]. The LPBF process inherently high cooling rates (105K·s−1) [10] lead to the expected formation of a fine cellular microstructure after solidification. However, coalesced and elongated cells are formed due to heat dissipation from a new or adjacent layer. Typically, cell growth accompanies the segregation of alloying elements (in the case of the maraging steel grade 300, commonly-segregated elements are Ni, Ti, and Mo), as evidenced by the increased thickness of their walls [37]. The density results of 18Ni300M steel, as presented in Table3, exhibit similarity between the GA and WA batches and do not show significant differences across the measurement methods used, Archimedes’ principle and quantitative stereology. Moreover, the percentage values obtained from Archimedes’ method were calculated based on the theoretical density of the 18Ni300M steel processed through the conventional route (VIM and VAR) [34]. This finding suggests that the parts processed by LPBF from both GA and WA batches exhibit a low pore content compared to VIM and VAR maraging steel. Upon examining Table3, it is evident that the porosity percentage in both conditions tends to be very close (as indicated by the proximity of the densities), given that the pore size in the GA batch material is smaller. These pores appear homogeneously distributed compared to the WA batch material, where larger and more concentrated pores are present in specific regions. 3.3 Phase identification andquantification inthepowders andprinted parts of18Ni300M steel Figure6 displays the X-ray diffractograms showcasing the indexed and quantified phases for the powders and processed parts of 18Ni300M steel. 3.4 Tensile tests Engineering tensile curves of 18Ni300M are exhibited in Fig.7. Due to the similarity between the plots, only one of the three curves was displayed for each batch (GA and WA) of 18Ni300M steel. By comparison, the curve with the caption “Afkhami etal.” was obtained from a paper in which LPBF also processed 18Ni300M steel under conditions similar to the present article [40]. Moreover, the curve labeled as “VIM and VAR” was derived from tensile tests carried out by our research group under conditions similar to those applied to AM specimens, with a sample of 18Ni300M steel processed by the conventional route involving vacuum induction melting (VIM) and vacuum arc remelting (VAR). The monotonic properties of 18Ni300M steel were determined through tests on three samples from both GA and WA batches and the average values of these properties are presented in Table4. The monotonic properties obtained from engineering tensile curves exhibited in Fig.7 and summarized in Table4 indicate that 18Ni300M steel parts printed from the GA batch present higher ductility and strength than those manufactured from the WA batch. Upon analyzing the curves of both batches, it becomes evident that, after the YS point, samples processed with the GA batch undergo a substantial amount of plastic deformation until fracture. In contrast, the mechanical behavior of parts processed with the WA batch is brittle, with minimal plastic deformation leading to fracture. The high mechanical strength observed in both batches of 18Ni300M steel is attributed to the elevated dislocation Fig. 5 Vickers microhardness in XY, XZ, and YZ sections The International Journal of Advanced Manufacturing Technology 1 3 density reported in the martensitic structure of this alloy, which ranges from 1014 to 1015 m−2 [41]. Additionally, alloying elements such as O, N, Co, Al, Ti, and Mo in solid solution further contribute to the material’s hardening. The YS values found for the two batches cannot be directly compared to the literature values [42] (≈ 2000MPa) since the material is not undergoing aging treatment, resulting in a lower density of strengthening precipitates than required to achieve this ultra-high mechanical strength. Interestingly, when maraging 300 steel is thermally aged, the density of precipitates can reach 1023 m−3 [43]. In Fig.8 (a), true stress–strain curves for GA and WA batches of 18Ni300M are displayed. The material behavior at high strains (after yielding and before reaching ultimate tensile stress) was investigated, and the true stress – logarithmic plastic strain data were fitted to power equations based on Hollomon’s law, as shown in Fig.8 (b) and (c). True stress–logarithmic plastic strain modeling for 18Ni300M steel processed from the GA batch did not conform to Hollomon’s power law. For this reason, a modified equation for Hollomon’s law was proposed ( σ=K ⋅  ε ( n⋅  ε−m p ) p ), as shown in Fig.8 (b). Analyzing Fig.8 (a), it can be observed that the behavior of the two curves up to the beginning of hardening is similar indicated by a dashed line in the graph to restrict the deformation of  ε=0.005 . For this reason, the true stress–logarithmic plastic strain curve referring to the GA batch was modeled in two ranges: for  ε < 0.005, Hollomon’s power law was used, and for  ε > 0.005, a power equation derived from Swift’s hardening model was employed [31], as depicted in Fig.8 (d). The values for K, n, the constant m generated with the modified Hollomon’s power law, χ2, and the adjusted R-square, R2, for modeled curves of Fig.8 (b) and (c) are described in Table5. Figure8 (a) illustrates the true stress–strain curves of 18Ni300M steel, indicating a significantly more ductile behavior of the material processed from the GA batch than Fig. 6 X-ray diffractograms for powders and additively manufactured parts of 18Ni300M steel Fig. 7 Engineering tensile curves for 18Ni300M steel of the GA and WA batches compared to the VIM and VAR and an external reference (Afkami etal. [40]) Table 4 Mechanical properties of 18Ni300M steel Monotonic property GA batch WA batch Afkami etal. [40] VIM and VAR UTS (MPa) 1110.4 1021.9 1162 1055.6 YS (MPa) 986.5 939.2 1078 765.8 ΔL (%) 11.52 4.06 11.7 15.06 E (GPa) 157.8 148.3 174 122.5 The International Journal of Advanced Manufacturing Technology 1 3 the WA one. Additionally, in Fig.8 (b), it is evident that fitting the points corresponding to the GA batch curve after yielding and before the ultimate tensile stress with Hollomon’s equation was unsatisfactory, as indicated by the parameters χ2 = 59.85 and R2 = 0.971 from Table5. However, Hollomon’s model exhibited a good fit to the material manufactured from WA batch data, as shown in Fig.8 (c), and the parameters extracted from Table5 revealed χ2 = 0.20 and R2 = 0.999. A modified equation derived from Hollomon’s power law was proposed to find a more accurate mathematical model that describes the entire curve of the GA batch. Although the curve mathematically fitted the experimental data well, as evidenced by the statistical descriptors χ2 = 2.27 and R2 = 0.998, the parameters obtained with this model may not accurately describe the physical metallurgy of the work hardening in 18Ni300M steel processed from the GA powder. Hence, discussions regarding the mechanical and metallurgical behavior of this material under this condition (GA batch) will be based on Fig.8 (d) and the parameters determined from Hollomon’s and Swift’s laws applied in two plastic deformation intervals, as shown in Table6. The plastic deformation intervals selected for applying Hollomon’s and Swift’s models to the true stress–logarithmic plastic strain data of the GA batch were determined based on the similarity between the curves of GA and WA batches at the beginning of the plastic regime. (  ε < 0.005, this resemblance, in the true stress–strain curve, is highlighted by a dashed line.). Since Hollomon’s Fig. 8 (a) True stress–strain curves for 18Ni300M steel from GA and WA batches; (b) and (c) true stress–logarithmic plastic strain experimental data modeled by Hollomon’s law and a modified equation, and (d) Hollomon’s and Swift’s models fitting true stress Table 5 Work hardening and statistical parameters determined for 18Ni300M steel additive manufactured from GA and WA batches PL MPL PL MPL PL MPL PL MPL PL MPL Batch K (MPa) n m R2χ2 GA 1374.4 1181.5 0.0498 0.00329 – 0.339 0.971 0.998 59.85 2.27 WA 1499.9 0.0735 – 0.999 0.20 PL and MPL stand for Hollomon’s power law and Modified Hollomon’s power law