scieee AI-readable full text Open interactive document viewer

Experimental analysis of the size effect on the compressive behaviour of cylindrical samples core-drilled from existing brick masonry

Segura Domingo, Jorge,Pelà, Luca,Roca Fabregat, Pedro,Cabané Cañas, Albert

Abstract

This paper presents the results of an experimental programme about the evaluation of the size effect on the compressive behaviour of cylindrical samples of existing masonry. The study focuses on the in-situ coring and experimental testing of core specimens with 150 mm and 90 mm diameter. The 150 mm cylinder, recurrent in minor destructive evaluation of the compressive strength of existing masonry, includes four brick pieces, two mortar beds and one head joint. The 90 mm specimen includes one mortar bed and two segments of brick, and inflicts less damage on the inspected structural member due to its lower invasivity. The experimental research investigates the size effect on four different types of clay brick masonry. The first type was built in the laboratory using historical-like materials. The other three types of masonry belong to structural walls of existing historical buildings. The combination of experimental results from laboratory controlled materials and existing historical members shows that the size of the cylindrical specimen has regular effect on the compressive strength and the Young’s modulus. The consistent relationship found between the compressive strengths of the 150 mm and 90 mm core samples allows the use of the latter specimen for a more respectful inspection of existing structural masonry.

Full text

1 Experimental analysis of the size effect on the compressive behaviour of cylindrical samples core-drilled from existing brick masonry Jorge Seguraa,*, Luca Pelàa, Pere Rocaa, Albert Cabanéa a Department of Civil and Environmental Engineering, Universitat Politècnica de Catalunya (UPC- BarcelonaTech), 08034 Barcelona, Spain * Corresponding author. Department of Civil and Environmental Engineering, Universitat Politècnica de Catalunya (UPC-BarcelonaTech), Jordi Girona 1-3, 08034 Barcelona, Spain. E-mail address: jorge.seg[email protected] Abstract: This paper presents the results of an experimental programme about the evaluation of the size effect on the compressive behaviour of cylindrical samples of existing masonry. The study focuses on the in-situ coring and experimental testing of core specimens with 150 mm and 90 mm diameter. The 150 mm cylinder, recurrent in minor destructive evaluation of the compressive strength of existing masonry, includes four brick pieces, two mortar beds and one head joint. The 90 mm specimen includes one mortar bed and two segments of brick, and inflicts less damage on the inspected structural member due to its lower invasivity. The experimental research investigates the size effect on four different types of clay brick masonry. The first type was built in the laboratory using historicallike materials. The other three types of masonry belong to structural walls of existing historical buildings. The combination of experimental results from laboratory controlled materials and existing historical members shows that the size of the cylindrical specimen has regular effect on the compressive strength and the Young’s modulus. The consistent relationship found between the compressive strengths of the 150 mm and 90 mm core samples allows the use of the latter specimen for a more respectful inspection of existing structural masonry. 2 Keywords: MDT; core drilling; in-situ sampling; masonry; clay brick; lime mortar; compressive strength; Young’s modulus; size effect; historical buildings. Highlights: Compression tests on brick masonry cylinders of 150 mm and 90 mm are presented. Results from laboratory controlled and real historical materials are compared. The average ratio between the compressive strengths of 150 mm and 90 mm cores is 0.75. The average ratio between the Young’s moduli of 150 mm and 90 mm cores is 0.85. Testing 90 mm cylinders is found to be an alternative for inspecting existing masonry. Nomenclature CV coefficient of variation E Young’s modulus of masonry (generic) E150mm Young’s modulus of masonry obtained through tests on 150 mm cylinders E90mm Young’s modulus of masonry obtained through tests on 90 mm cylinders fb normalized compressive strength of bricks fc compressive strength of masonry (generic) fc,150mm compressive strength of masonry obtained through tests on 150 mm cylinders fc,90mm compressive strength of masonry obtained through tests on 90 mm cylinders fc* compressive strength of masonry derived from the proposed experimental approach fc,ACI estimation of the compressive strength of masonry with ACI expression fc,EC6 estimation of the compressive strength of masonry with Eurocode 6 expression fm,DPT compressive strength of mortar obtained through double punch tests MDT minor destructive testing technique Rc strengths ratio, computed as fc,150mm /fc,90mm RE Young’s moduli ratio, computed as E150mm/E90mm r2 coefficient of determination Δ % difference in percentage between experimental and empirical estimations 3 1 Introduction The use of masonry as building material is abundant all over the world, including many major examples of architectural heritage. Many of these buildings are in need of structural assessment because of structural damage or material decay experienced over the years. Additionally, their structural condition often requires careful evaluations due to the adaptation to new uses. The knowledge on the mechanical behaviour of this material and its most influent parameters, such as compressive strength and Young’s modulus, is of paramount importance for this kind of structural evaluations. The experimental determination of the mechanical properties of existing masonry is a challenging task. The in-situ sampling and subsequent testing of masonry specimens in the laboratory provide a suitable approach to the problem, since it is possible to obtain direct measurements of the mechanical parameters that describe the elastic and strength behaviour. However, the composite character of masonry requires laboratory tests on sufficiently large samples, able to represent the complexity of the material texture, and therefore including both units and mortar joints. Yet, the insitu sampling of large prismatic specimens of masonry, e.g. extracted from existing walls, may encounter important difficulties. In addition, sampling procedures should always be minimal in the case of historical buildings due to their cultural heritage value. A possible solution to the aforementioned limitations in the case of brickwork is offered by the minor destructive testing (MDT) technique consisting in extracting masonry core samples from the existing structure to be tested in the laboratory. This technique was proposed by the UIC Leaflet [1] on the inspection of brick masonry arch bridges, which suggests to core drill cylinders with a diameter of at least 150 mm including four brick segments, two mortar beds and one head joint. The cylindrical specimen is then tested under compression along the direction perpendicular to the mortar beds. Recent researches have shown that tests on such samples are able to reproduce the complex failure 4 mechanisms of brickwork in compression. The calibration of this technique by comparison with tests on other non-standard [2-4] and standard [5-7] masonry specimens has shown its ability to provide reliable estimations of the compressive strength of the material. Pelà et al. [6] investigated also the possibility of estimating the Young’s modulus of masonry by means of compression tests on this type of specimen. The use of cylindrical samples smaller than those suggested by the UIC Leaflet might constitute a possible alternative to reduce the damage inflicted to the building. This may reveal to be necessary in case of protected heritage constructions requiring minimum invasivity of the in-situ inspection. The use of smaller cylinders may provide also additional practical advantages, besides the reduction of damage grade during sampling. A larger amount of cylindrical cores could be extracted, allowing an increase of the statistical significance of the results. Also, finding convenient spots where to drill smaller cores is easier than for 150 mm diameter cylinders, especially in the case of plastered walls. Moreover, the reduced size of the cores makes the transport, storage and testing operations easier. A suitable cylindrical sample with dimensions smaller than the 150 mm diameter specimen of the UIC Leaflet should still include both the brick and mortar components in order to be able to represent realistically the composite character of the masonry material. The smallest core sample with these characteristics is composed of one diametric mortar joint and two cylindrical segments of brick. The diameter of this type of specimen should be around 90 mm and 100 mm in order to ensure a proper cutting of the two bricks without affecting the integrity of the interposed mortar joint. The use of cylinders with a diameter of 100 mm to determine the masonry compression parameters has been already investigated in [8, 9] with satisfactory results. Previous experimental and analytical studies available in the scientific literature have already addressed the size dependence on the strength of different types of brick masonry samples. The research by Carpinteri et al. [10] focused on size dependence on fracture properties, such as strength and toughness, by testing different samples under three-point bending. The authors highlighted the 5 important effect of constitutive heterogeneity on the size effect, especially when the specimen size is small. The numerical study by Lourenço [11] also showed the effect on tensile and compressive failures of the geometrical relationship between masonry units and the structural size. This paper presents an experimental research aimed at evaluating the size effect on the compressive strength and elasticity of cylindrical samples of existing brick masonry of 150 mm and 90 mm diameter. The adequacy of the 150 mm diameter masonry cores to assess the mechanical behaviour of masonry in compression has been already investigated and validated in [2-7]. This research pays special attention to the use of the smaller 90 mm diameter core samples, with the following specific objectives: (1) exploring the possibility to reproduce the mechanical behaviour of brick masonry in compression by means of tests carried out on them; (2) analysing the consistency and reliability of the results obtained and, specifically, investigating whether the scattering obtained is sufficiently moderate; (3) determining size-effect correlations for compressive strength and Young’s modulus based on the comparison with experimental results obtained from the 150 mm diameter cylinders. The comparison between the tests on the two types of cylindrical cores has been carried out for four different types of masonry, all of them made of solid clay bricks and lime mortar but characterized by different brick and mortar compressive strengths. The paper includes five sections. After an introduction about the purpose and objectives of the study, Section 2 presents the first experimental campaign performed on masonry walls built in the laboratory with historical-like materials. The extraction, preparation and testing of two sets of cylinders, with 90 mm and 150 mm diameter, were carried out in a laboratory controlled environment. Section 3 presents a second stage of the research, with three different experimental campaigns on different masonry typologies obtained from three real existing buildings. All field campaigns considered the in-situ sampling and subsequent laboratory testing of 90 mm and 150 mm cylindrical specimens. The results from the experimental programmes are discussed in Section 4, in terms of 6 failure modes, stability of experimental measurements, and size effect correlations of the compressive strengths and Young’s moduli of the 90 mm and 150 mm core samples. Section 4 presents also a comparison with predictive expressions from building codes. The paper ends with the concluding Section 5. 2 Experimental programme on masonry built in the laboratory The first stage of the research considered core samples extracted from masonry walls built in the laboratory with historical-like material components. The samples of this campaign were identified with code “MA”. The experimental programme was carried out at the Laboratory of Technology of Structures and Building Materials of the Technical University of Catalonia (UPC – BarcelonaTech). 2.1 Materials and construction of walls As stated before, the proposed MDT technique aims to study the compressive behaviour of existing brick masonry structures, with special focus on the case of historical buildings. Therefore, the masonry built in the laboratory was designed to represent as much as possible a typical historical masonry with solid clay bricks and low-strength lime mortar in joints. The bricks were handmade and presented rough surfaces and slightly variable dimensions. The nominal dimensions were 305 × 145 × 45 mm³. A set of bricks was polished and cut into pieces of dimensions 100 × 100 mm² to be tested in compression according to EN 772-1 [12]. Table 1 reports the normalized compressive strength (fb), obtained by multiplying the experimental value by the shape factor proposed by the standard. Two single-leaf walls with dimensions 1.6 × 0.8 × 0.145 m³ were built in the laboratory by using the aforementioned bricks (Fig. 1a). A qualified mason built the walls in running bond using a pure aerial lime mortar, classified as CL90 according to EN 459-1 [13]. The joint thickness varied between 15 mm and 20 mm. The walls were stored in laboratory conditions for more than one year 7 until the coring process. This long time was necessary for a sufficient hardening of the aerial lime mortar. At the time of the coring process for obtaining the masonry cylinders, some mortar joints were dismantled. These portions of mortar were cut into slabs with approximate dimensions of 50 × 50 mm². After regularization with a little amount of gypsum powder, these pieces were subjected to the double punch test (DPT) by following DIN 18555-9 [14]. More detailed information on DPT can be found in [15-17]. As can be seen in Table 1, the average compressive strength value measured by means of this test (fm,DPT) was equal to 1.61 MPa. It is worth mentioning that this compressive strength value for the aerial lime mortar was obtained after two years from the construction of the wall. The DPT technique, suitable for the mechanical characterisation of the mortar joints in existing buildings, was considered in campaign “MA” as well as in the three case studies that will be described in Section 3. The DPT results from the four campaigns will allow direct comparisons of the actual compressive strength of mortar inside the joints. Table 1. Experimental compressive strength of bricks (fb) and mortar joints (fm,DPT) in campaign “MA” executed on masonry built in the laboratory. “MA” fb fm_DPT Average (MPa) 17.44 1.61 Number of specimens 14 32 CV 8.3% 20.1% 2.2 Core drilling and preparation of masonry specimens Before the extraction of masonry cylindrical samples, a low vertical compression was applied to the walls with the aim of ascertaining their stability during the transportation inside the laboratory and the coring process. The extraction of the cores was done by horizontal drilling using the dry coring technology proposed, among others, in [4] and [6]. Two types of cylinders were extracted (Fig. 1b). First, 150 mm diameter core samples (actual diameter of 152.5 mm), including one vertical and two horizontal mortar 8 joints and four brick portions. Second, 90 mm diameter core samples (actual diameter of 92 mm), including a single diametric mortar joint and two brick portions. All the cores had an approximate depth of 145 mm. Six cylindrical specimens of each diameter were extracted from the walls. Additional cores were extracted and used for other parallel researches carried out by the authors [16]. Fig. 1. a) Masonry wall built in the laboratory for the campaign “MA”, and b) core drilling of 150 mm and 90 mm cylindrical samples. After extraction, two high strength mortar caps were casted on the cylindrical specimens (Fig. 2). These caps were used to create two flat surfaces allowing the application of an evenly distributed load. This approach was already proposed in [5-7] and differs from the UIC leaflet [1] where it is recommended to apply the load through steel concave loading plates and to make use of lead sheets in contact with the sample. The high strength mortar caps match the irregular curved perimeter of the cores and avoid any stress concentration during the tests. The widths of the caps were about 110 mm for the 150 mm cores, and about 70 mm for the 90 mm cores. These dimensions were chosen to maintain similar width to diameter ratios for the two different types of cylinder. 9 Fig. 2. Front and lateral views of regularized core samples of campaign “MA”: a) 150 mm cylinder and b) 90 mm cylinder. 2.3 Testing procedures Both 150 mm and 90 mm cores were tested in a general-purpose compression machine with load capacity of 3000 kN (Fig. 3) after two years from the construction of the walls. Thanks to the mortar caps, uniaxial compression could be applied perpendicularly to the horizontal joints. The tests were carried out in two consecutive stages. The first one was aimed to study the elastic behaviour of the material and consisted in the application of three loading/unloading cycles under load control. These cycles ranged from 5% to 20% of a supposed maximum load that had been estimated before the tests. In the lack of a specific standard for these tests, the first stage was planned taking as reference some standards on the measurement of the Young’s modulus for other materials [18-21], as well as former researches [6,22]. The Young’s modulus was calculated for the loading branch of the third cycle. The second stage aimed to investigate the nonlinear behaviour of the material and to measure its compressive strength. The cylinders were tested under displacement control, at a rate of 0.004 mm/s. The tests were stopped after registering part of the post-peak softening response. 16 The campaign with code “MD” involved a historical building in the district of Ciutat Vella (Fig. 7c). Built in the first half of the 19th century in Neoclassical style, this housing complex reflects the specific economical context of the time. The building stands out by the high-quality materials used, the stone masonry elements of the facades and the overall size of the construction. Brick masonry walls constitute the load bearing structure, which supports the floors made of timber beams with ceramic vaults in between. As in the former cases, the on-going renovation works motivated and allowed the extraction of the cylinders. Fig. 7. a) View of the building of the “Fabra i Coats” industrial complex in Barcelona studied in campaign “MB”, b) main façade of the residential building at Rambla de Catalunya Street in Barcelona studied in campaign “MC”, c) façade of the housing complex in the district of Ciutat Vella in Barcelona studied in campaign “MD”. During the visits to the three buildings, sets of bricks and fragments of mortar joints were extracted. Bricks had average dimensions of 291 × 140.5 × 52 mm³ in campaign “MB”, 294 × 145 × 17 49 mm³ in campaign “MC” and 294 × 145 × 45 mm³ in campaign “MD”. The three sets of bricks showed variability in grain size and colour. Brick pieces of 140 × 140 mm² and 100 × 100 mm² were cut respectively for campaign “MB” and campaigns “MC” and “MD”. These brick pieces and mortar fragments were prepared and tested in compression following the procedures described in Section 2.1 for campaign “MA”. Table 3 shows the corresponding results. The variability observed by visual inspection was also reflected in the compressive strength of bricks (fb), particularly in the case of campaign “MC”. Bricks of campaign “MD” were twice stronger than those of campaigns “MB” and “MA”, and three times stronger than the bricks of campaign “MC”. Table 3. Experimental compressive strengths of bricks (fb) and mortar (fm_DPT) of campaigns “MB”, “MC” and “MD”. “MB” fb fm_DPT “MC” fb fm_DPT “MD” fb fm_DPT Average (MPa) 18.80 0.62 Average (MPa) 10.74 1.52 Average (MPa) 35.45 3.1 No. of specimens 6 12 No. of specimens 12 28 No. of specimens 10 32 CV 12.4% 16.0% CV 28.0% 35.0% CV 14.8% 55.4% The masonry walls investigated in campaign “MB” were 600 mm thick, built in English bond with variable mortar joint thickness between 10 mm and 15 mm (Fig. 8a). The walls investigated in campaigns “MC” and “MD” were interior single leaf walls 145 mm thick built in running bond (Fig. 8c and e). The mortar joint thickness varied between 14 mm and 17 mm in the former and between 10 and 15 mm in the latter. The quality of workmanship was better in the types of masonry “MB” ad “MD” in terms of regularity and complete filling of mortar joints. Up to seven specimens of each cylinder type, 90 mm and 150 mm, were extracted in the three campaigns (Fig. 8b, d and f). Two additional specimens of 150 mm were extracted in campaign “MD”. The coring followed the same dry procedure mentioned in Section 2.2. It is worth to remark the advantages of this technique, as already reported in [6,16]. The total absence of water protected the integrity of the weak mortar joints and guaranteed the efficiency of the full process. Only two operators could easily handle the equipment and a half working day was enough to extract the required amount 18 of cores. The extraction of 90 mm cylinders was easier than for the 150 mm cores. Once the coredrilling machine was fixed to the masonry wall, the coring bit could be moved and the samples extracted along a circumferential path. Within a wall, finding an adequate spot to extract a 90 mm sample resulted easier than for a 150 mm core. Additionally, the specimens of campaign “MB”, which were extracted from 600 mm thick walls, were sawn to adjust their depth to the width of the constituent bricks (≈145 mm). 19 Fig. 8. a) Façade wall investigated in “Fabra i Coats” factory and b) in-situ core drilling for campaign “MB”, c) inner wall of the analysed building in Rambla Catalunya street and d) in-situ core drilling for campaign “MC”, e) inner wall of the building in Ciutat Vella and f) in-situ core drilling for campaign “MD”. The extracted specimens of the three campaigns were regularized with mortar caps and tested in compression, as described in Sections 2.2 and 2.3 for campaign “MA”. Fig. 9, Fig. 10 and Fig. 11 show the stress-strain curves of the tests for the three campaigns. The trends are similar to those discussed in Section 2 for the campaign “MA”. The cracking sequences, which are illustrated by the failure examples shown in Fig. 12, resulted very similarly to those of campaign “MA”. 20 Fig. 9. Compressive stress-strain curves of campaign “MB”: a) 150 mm samples and b) 90 mm samples. 21 Fig. 10. Compressive stress-strain curves of campaign “MC”: a) 150 mm samples and b) 90 mm samples. 22 Fig. 11. Compressive stress-strain curves of campaign “MD”: a) 150 mm samples and b) 90 mm samples. 23 Fig. 12. Modes of failure in the 150 mm (left) and 90 mm (right) core samples extracted from existing masonry buildings: a) and b) campaign “MB”, c) and d) campaign “MC”, e) and f) campaign “MD”. Table 4, Table 5 and Table 6 present the compressive strength and Young’s modulus results obtained from both types of cylindrical specimen for the campaigns “MB”, “MC” and “MD” respectively. The discussion of the results is included in Section 4.1. 24 Table 4. Compressive strengths (fc) and Young’s moduli (E) of 150 mm and 90 mm masonry cylinders of campaign “MB”. “MB” 150 mm cylinders “MB” 90 mm cylinders ID f c,150mm (MPa) E 150mm (MPa) ID f c,90mm (MPa) E 90mm (MPa) MB_3_0 9.13 -- MB_1_0 8.26 -- MB_3_3 6.53 2580 MB_1_1 13.22 3027 MB_3_5 7.45 1663 MB_1_3 7.14 2551 MB_3_6 5.60 2019 MB_1_6 8.51 -- MB_3_7 6.75 1992 MB_1_12 10.31 2430 MB_3_8 8.64 2902 MB_1_16 11.55 3727 MB_3_9 10.74 2665 MB_1_18 10.17 3719 Average 7.83 2304 Average 9.88 3091 CV 22.6% 20.9% CV 21.2% 20.0% Table 5. Compressive strengths (fc) and Young’s moduli (E) of 150 mm and 90 mm masonry cylinders of campaign “MC”. “MC” 150 mm cylinders “MC” 90 mm cylinders ID f c,150mm (MPa) E 150mm (MPa) ID f c,90mm (MPa) E 90mm (MPa) MC_3_1 6.76 1416 MC_1_1 7.06 1797 MC_3_2 4.94 1830 MC_1_2 7.81 1490 MC_3_3 5.44 1827 MC_1_3 7.44 1290 MC_3_4 5.20 1291 MC_1_4 6.82 1840 MC_3_5 5.47 -- MC_1_5 7.01 1956 MC_3_6 5.61 1688 MC_1_6 6.84 1906 MC_3_7 3.55 1360 MC_1_7 7.18 1495 Average 5.28 1569 Average 7.16 1682 CV 18.1% 15.4% CV 4.9% 15.1% Table 6. Compressive strengths (fc) and Young’s moduli (E) of 150 mm and 90 mm masonry cylinders of campaign “MD”. “MD” 150 mm cylinders “MD” 90 mm cylinders ID f c,150mm (MPa) E 150mm (MPa) ID f c,90mm (MPa) E 90mm (MPa) MD_3_1 11.91 4258 MD_1_1 16.67 5265 MD_3_2 7.68 3362 MD_1_2 10.36 3157 MD_3_3 8.14 1783 MD_1_3 10.04 2958 MD_3_4 9.73 3927 MD_1_4 13.72 3598 MD_3_5 11.18 2948 MD_1_5 11.66 3278 MD_3_6 7.80 4157 MD_1_6 14.86 3590 MD_3_7 8.05 3951 MD_1_7 12.02 4498 MD_3_8 13.26 3614 MD_3_9 6.75 3035 Average 9.39 3448 Average 12.76 3763 CV 23.9% 22.6% CV 19.1% 22.0% 25 4 Discussion 4.1 Comparison among the four experimental campaigns The experimental programme described in Section 2 consisted in testing samples extracted from masonry walls built in the laboratory. Useful remarks were drawn from the comparison between the results of the more novel MDT technique consisting in tests on 90 mm masonry cylinders with one mortar joint and the results of the relatively well-studied technique involving tests on 150 mm cylinders with two horizontal and one vertical mortar joints. Section 3 described three additional campaigns on samples extracted from real historical buildings that aimed to confirm the aforementioned findings for the case of real existing masonry. The comparison of the stress-strain curves depicted in Fig. 4, Fig. 9, Fig. 10 and Fig. 11 shows similar recognizable trends for the two types of specimen studied. The first branch observed in all the curves up to low values of stress is related to the specific testing protocol adopted in this research, which included the performance of initial loading/unloading cycles. Then, the curves can be generally divided into three sections: a linear branch, a non-linear behaviour before the peak stress and a softening response after the peak stress. Some differences are observed, however, in the stress-strain curves. Longer linear branches are generally observed in the case of the 150 mm specimens that, in some cases, develop up to almost the peak stress. For the 90 mm samples, usually higher values of the strain at peak stress are detected. These observations apply for the four types of masonry investigated. The examples of tested specimens shown in Fig. 12 for campaigns “MB”, “MC” and “MD” confirm the failure mechanisms reported for the masonry of campaign “MA”. The 56 cylinders tested in the context of this research failed in a very similar way. The failures were characterized by pseudovertical cracks appearing firstly on the bricks that caused eventually the detachment of the external parts, leaving a final sandglass shaped core. These features are in agreement with the findings described by former researches on 150 mm cores [2-6] and 100 mm cores [9]. 32 where 𝑓𝑓 𝑐𝑐 ∗ is the compressive strength of the masonry being inspected. Other references [2,4] include in the former relationship a correction factor because they consider the diametrical section to calculate the acting stresses and the load is applied differently as described in Section 2.2. Taking into account this latter remark, all the aforementioned references [2,4,5,7,23] propose equivalent expressions. Combining the former Equations 1 and 2, a new practical approach can be proposed consisting in the extraction and testing of 90 mm specimens and the estimation of the compressive strength of masonry through the application of the following expression (Eq. 3): 𝑓𝑓 𝑐𝑐 ∗≅0.75 𝑓𝑓 𝑐𝑐,90𝑚𝑚𝑚𝑚 (3) Table 7 presents the application of Equation 3 to the four types of masonry investigated herein. The estimations of the compressive strength are compared to the predictions provided by the application of other approaches. Among the available possibilities, one consists in testing the individual components, i.e. bricks and mortar, and applying empirical or analytical correlations to estimate the mechanical properties of the composite material from those of the components [30,34,35]. This approach faces several difficulties. One of them stems from the applicability of the equations available in literature. The expressions with an empirical basis, like those proposed by some available standards for the design of new masonry structures, are in principle only adequate for the new construction materials for which they were calibrated and show limitations in the applicability to historical masonry. Another major difficulty lays in the characterization of the existing mortar [17,36], which is hindered by the impossibility of extracting non-disturbed or normalized prismatic samples [37]. A possible solution to this difficulty is found in extracting joint fragments and testing them under double punch compression, as it is done in the present research and explained in Section 2.1. Table 7 includes the comparison between the experimental estimation of the compressive strength by Equation 3 and the predictions of two expressions available in building codes [38,39]. The term fc,ACI represents the compressive strength estimated by the unit strength method expression 33 proposed in the Commentary on the Specification for Masonry Structures ACI 530.1-02 [38]. This empirical expression correlates the strength of the masonry with the strength of the units. The term fc,EC6 indicates the value obtained with the expression proposed by Eurocode 6 [39]. In the latter, the characteristic compressive strength of the composite material is correlated with the average compressive strengths of both mortar and units. The values reported in Table 7 have been previously converted into mean value by multiplying by a factor equal to 1.2 as recommended in EN1052-1 [27]. The mortar strength introduced into the equation is the one obtained via the double punch tests. The columns on the right of the predictions express the difference in percentage terms (Δ %) with respect to the experimental estimation. Table 7. Experimental estimation of masonry compressive strength (fc*) vs. predictions from expressions of ACI [38] (fc,ACI ) and EC6 [39] (fc,EC6). Δ % expresses the difference in percentage of the predictions with respect to the experimental estimation. Masonry f c * (MPa) f c,ACI (MPa) Δ % f c,EC6 (MPa) Δ % "MA" - Lab 7.19 6.24 -13.2% 5.63 -21.7% "MB" - Fabra 7.41 6.52 -12.0% 4.46 -39.8% "MC" - Rambla 5.37 4.90 -8.8% 3.94 -26.6% “MD” C. Vella 9.57 9.84 2.8% 11.26 17.7% The expression proposed by the ACI Specification [38] provides similar values to the experimental estimations, with a close agreement of 2.8 % in the case of the masonry made with the strongest bricks (campaign “MD”). In the latter, the equation of the Eurocode 6 [39] provides a nonconservative estimation, while it yields more conservative estimations in the cases of campaigns “MA”, “MB” and “MC”. It is remarkable that the highest difference is found for campaign “MB”, which is the type of masonry with the poorest mortar. In the cases of low strength materials (campaigns “MA”, “MB” and “MC”), the expressions proposed by the building standards have provided more conservative values of the compressive strength compared with the experimental results. Under the assumption that the values obtained by means of the use of masonry cylinders are closer to the actual compressive strength of masonry, the 34 investigated technique can be regarded as a convenient tool for mechanical characterization. Since an accurate estimation of the mechanical properties helps to reduce uncertainties during the structural assessment, the design of possible interventions, such as retrofit or strengthening, can be less prominent and thus more respectful of the cultural value of existing heritage buildings. 5 Conclusions This paper has presented an experimental research on the characterization of the compressive mechanical properties of existing masonry. The laboratory testing of core samples extracted from masonry walls has been investigated as a MDT inspection technique. Two types of core, the already studied and validated three-joint cylinder with diameter of 150 mm and the proposed one-joint cylinder with diameter of 90 mm, have been tested and compared to study the effect associated to the reduction of size. The aim in reducing the cylinder’s size is to limit the damage caused to the structure during the sampling and allowing a more efficient extraction and testing. Tests on the two types of cylinder were investigated on masonry walls built in the laboratory with historical-like materials and then applied to three real case studies of historical buildings in Barcelona. The following conclusions can be drawn from the analysis of the results: - The dry procedure applied to drill the cores has proved to be a clean and efficient method for the extraction of cylindrical specimens in existing buildings. The extraction of 90 mm cylinders was comparatively easier than the extraction of 150 mm cylinders. - The experimental evidence confirms the adequacy of the 90 mm samples to reproduce the expected mechanical behaviour of masonry in compression. Similar failure mechanisms were found for the two cylinder types. It has been observed that tests on both cylinder types adequately represent the complex interaction between bricks and mortar that characterizes the masonry response in compression. 35 - The size of the core sample has been found to have significant effect on the compressive strength and the Young’s modulus. The comparison of the four experimental campaigns has shown that the tests on the two types of specimen provide consistent results and the same logical trends for the compressive strength and the Young’s modulus of masonry. The moderate scattering obtained in the tests can be fully explained by the variability found in the constituents’ material properties. - The comparison of the compressive strength results obtained from 150 mm and 90 mm specimens has provided an almost uniform relation for the four different experimental campaigns. A linear regression of the results has yielded a proportionality constant of 0.75. This coefficient may be considered applicable to masonry types similar to the ones investigated, i.e. made of solid clay bricks –with normalized compressive strengths from 10 to 35 MPa- and joints made of lime mortar –with compressive strengths from 0.60 to 3 MPa. - Testing small 90 mm diameter cores has proved to be an advantageous and promising technique for the evaluation of the resisting properties of masonry in compression. A suggested set of 6 specimens extracted from an existing structural member may provide a reliable estimation of the compressive strength and an acceptable estimation of the Young’s modulus. Acknowledgements The authors gratefully acknowledge the financial support from the Ministry of Economy and Competitiveness and from the Ministry of Science, Innovation and Universities of the Spanish Government, as well as that of the ERDF (European Regional Development Fund) through projects MULTIMAS (Multiscale techniques for the experimental and numerical analysis of the reliability of masonry structures, ref. num. BIA2015-63882-P) and SEVERUS (Multilevel evaluation of seismic vulnerability and risk mitigation of masonry buildings in resilient historical urban centres, ref. num. RTI2018-099589-B-I00). Support from Secretaria d’Universitats i Investigació de la Generalitat de 36 Catalunya through a predoctoral grant awarded to the first author is also gratefully acknowledged. The authors would like to thank Larisa García-Ramonda for her helpful contributions. References [1] UIC, Leaflet 778-3R: Recommendations for the inspection, assessment and maintenance of masonry arch bridges, 1995. [2] A. Brencich, E. Sterpi, Compressive Strength of Solid Clay Brick Masonry: Calibration of Experimental Tests and Theoretical Issues, in: P. B. Lourenço, C. Modena, P. Roca, S. Agrawal (Eds.), SAHC 2006 - Struct. Anal. Hist. Constr., Macmillan India Let., 2006: pp. 757-766. [3] A. Brencich, D. Sabia, Experimental identification of a multi-span masonry bridge: The Tanaro Bridge, Constr. Build. Mater. 22 (2008) 2087-2099. doi:10.1016/j.conbuildmat.2007.07.031. [4] P. Matysek, Compressive strength of brick masonry in existing buildings — research on samples cut from the structures, in: C. Modena, F. da Porto, M.R. Valluzzi (Eds.), Brick Block Mason. - Trends, Innov. Challenges, Taylor & Francis Group, 2016: pp. 1741-1747. [5] L. Pelà, P. Roca, A. Benedetti, Mechanical Characterization of Historical Masonry by Core Drilling and Testing of Cylindrical Samples, Int. J. Archit. Herit. (2016) 150817093153002. doi:10.1080/15583058.2015.1077906. [6] L. Pelà, E. Canella, A. Aprile, P. Roca, Compression test of masonry core samples extracted from existing brickwork, Constr. Build. Mater. 119 (2016) 230-240. doi:10.1016/j.conbuildmat.2016.05.057. [7] L. Pelà, E. Canella, K. Kasioumi, P. Roca, D. Marastoni, Complete experimental characterization of lime mortar and clay brick masonry, in: C. Modena, F. da Porto, M.R. Valluzzi (Eds.), Brick Block Mason. - Trends, Innov. Challenges, Taylor & Francis Group, 2016: pp. 1799-1806. [8] E. Sassoni, C. Mazzotti, G. Pagliai, Comparison between experimental methods for evaluating the compressive strength of existing masonry buildings, Constr. Build. Mater. 68 (2014) 206-219. doi:10.1016/j.conbuildmat.2014.06.070. [9] P. Matysek, T. Stryszewska, S. Kanka, Experimental research of masonry compressive strength in the Auschwitz II - Birkenau former death camp buildings, Eng. Fail. Anal. 68 (2016) 263-274. doi:10.1016/j.engfailanal.2016.06.007. 37 [10] A. Carpinteri, B. Chiaia, P. Bocca, Size dependence of strength and fracture properties of brick masonry walls, J. Eng. Mech. 123 (1997) 816-822. [11] P.B. Lourenço, Two aspects related to the analysis of masonry structures: size effect and parameter sensitivity. Report n 03.21.1.31.25, 1997. [12] European Committee for Standardization (CEN), EN 772-1:2011, Methods of Test for Masonry Units - Part 1: Determination of Compressive Strength, (2011). [13] European Committee for Standardization (CEN), EN 459-1 Building lime - Part 1: Definitions, specifications and conformity criteria, (2010). [14] Deutsches Institut für Normung (DIN), DIN 18555-9: Testing of mortar containing mineral binders - Part 9: Determining the compressive strength of hardened mortar, (1999). [15] D. Marastoni, L. Pelà, A. Benedetti, P. Roca, Combining Brazilian Tests on masonry cores and Double Punch Tests for the mechanical characterization of historical mortars, Constr. Build. Mater. 112 (2016) 112-127. doi:10.1016/j.conbuildmat.2016.02.168. [16] L. Pelà, K. Kasioumi, P. Roca, Experimental evaluation of the shear strength of aerial lime mortar brickwork by standard tests on triplets and non-standard tests on core samples, Eng. Struct. 136 (2017) 441-453. doi:10.1016/j.engstruct.2017.01.028. [17] L. Pelà, P. Roca, A. Aprile, Combined In-Situ and Laboratory Minor Destructive Testing of Historical Mortars, Int. J. Archit. Herit. 12 (2018) 334-349. doi:10.1080/15583058.2017.1323247. [18] European Committee for Standardization (CEN), EN 14580 Natural stone test methods. Determination of static elastic modulus, (2006). [19] American Society for Testing and Materials, ASTM E111 Standard Test Method for Young’s Modulus , Tangent Modulus , and Chord Modulus 1, (2010). [20] European Committee for Standardization (CEN), EN 12390-13 Testing hardened concrete - Part 13: Determination of secant modulus of elasticity in compression, (2013). [21] American Society for Testing and Materials, ASTM C 469-02 Standard Test Method for Static Modulus of Elasticity and Poisson’s Ratio of Concrete in Compression, (2002). 38 [22] A. Drougkas, P. Roca, C. Molins, Compressive strength and elasticity of pure lime mortar masonry, Mater. Struct. Constr. 49(3) (2016) 983-999. doi:DOI: 10.1617/s11527-015-0553-2. [23] S. Jafari, R. Esposito, J. Rots, Literature review on the assessment of masonry properties by tests on core samples, in: W.J. Quist, S.J.C. Granneman, R.P.J. van Hees (Ed.), 4th WTA Int. PhD Symp., Vlaanderen, 2017: p. 172-180. [24] A.W. Hendry, Structural Masonry, Macmillan Press Ltd, 1998. [25] M. Como, Statics of Historic Masonry Constructions, Springer, 2013. [26] J. Segura, L. Pelà, P. Roca, Monotonic and cyclic testing of clay brick and lime mortar masonry in compression, Constr. Build. Mater. 193 (2018) 453-466. doi:10.1016/j.conbuildmat.2018.10.198. [27] European Committee for Standardization (CEN), EN 1052-1 Methods of test for masonry - Part 1: Determination of compressive strength, (1999). [28] American Society for Testing and Materials, ASTM C1314-09 Standard Test Method for Compressive Strength of Masonry Prisms, (2009). [29] M. Tomazevic, Earthquake-resistant design of masonry buildings, Imperial College Press, 1999. doi:https://doi.org/10.1142/p055. [30] A. Drougkas, C. Molins, P. Roca, Numerical prediction of the behavior, strength and elasticity of masonry in compression, Eng. Struct. 90 (2015) 15-28. doi:10.1016/j.engstruct.2015.02.011. [31] G.N. Pande, J.X. Liang, J. Middleton, Equivalent elastic moduli for brick masonry, Comput. Geotech. 8 (1989) 243-265. doi:10.1016/0266-352X(89)90045-1. [32] A. Mohammed, T.G. Hughes, A. Mustapha, The effect of scale on the structural behaviour of masonry under compression, Constr. Build. Mater. 25 (2011) 303-307. doi:10.1016/j.conbuildmat.2010.06.025. [33] C.L. Knox, D. Dizhur, J.M. Ingham, Experimental study on scale effects in clay brick masonry prisms and wall panels investigating compression and shear related properties, Constr. Build. Mater. 163 (2018) 706-713. doi:10.1016/j.conbuildmat.2017.12.149. [34] D. Ferretti, E. Coïsson, D. Ugolotti, E. Lenticchia, Use of EC6-like equations to estimate the compressive strength of masonry made of solid clay bricks and lime mortar, in: C. Modena, F. da Porto, M.R. Valluzzi (Eds.), Brick Block Mason. - Trends, Innov. Challenges, Taylor & Francis Group, 2016: p. 1561-1570. 39 [35] D. Liberatore, A. Marotta, L. Sorrentino, Estimation of solid clay brick unreinforced masonry compressive strength based on mortar and unit mechanical parameters, in: Proceedings of 9th Int. Mason. Conf., Guimaraes, 2014: p. 1715-1722. [36] M. Drdácký, Non-Standard Testing of Mechanical Characteristics of Historic Mortars, Int. J. Archit. Herit. 5 (2011) 383-394. doi:10.1080/15583051003717788. [37] European Committee for Standardization (CEN), EN 1015-11 Methods of test for mortar for masonry - Part 11: Determination of flexural and compressive strength of hardened mortar, (1999). [38] ACI, ASCE, TMS, Commentary on Specification for Masonry Structures (ACI 530.1-02/ASCE 6-02/TMS 602- 02), (2004). [39] European Committee for Standardization (CEN), Eurocode 6: Design of masonry structures - Part 1: General rules for reinforced and unreinforced masonry structures, (2005).