scieee AI-readable full text Open interactive document viewer

Diagonal tension performance of concrete panels reinforced with hooked end steel fibers

Carrillo León, Julián,Murcia Delso, Juan,Massone, Leonardo M.

Abstract

The increase in strength of Steel Fiber Reinforced Concrete (SFRC) depends mainly on factors such as the dosage, aspect ratio and number of hooked ends of the fibers. Previous studies proposed models to estimate the flexural and shear strength of SFRC beams, but the shear behavior of SFRC panels has not been extensively studied. The study includes diagonal tension tests on concrete panels to assess the shear performance of SFRC. The experimental program comprises 19 square concrete panels having 600 mm side and 75 mm thickness, including three nominal dosages of steel fibers (20, 40 and 60 kg/m3) and three different number of hooked ends (1, 1.5 and 2). The study proposes models to predict the shear strength and deformation capacity, stiffness degradation and toughness of SFRC panels with different number of hooked ends when subjected to diagonal tension. The models include four characteristic limit states of diagonal cracking, maximum residual strength, code-based acceptable degradation, and maximum deformation.

Full text

1 Diagonal tension performance of concrete panels reinforced with hooked end steel fibers Julian Carrillo a,1 , Juan Murcia-Delso b , Leonardo M. Massone c (1) Professor, Department of Civil Engineering, Universidad Militar Nueva Granada, UMNG, Bogotá, Colombia, [email protected] (2) Associate Professor, Department of Civil Engineering, Polytechnic University of Catalonia, Barcelona, Spain, [email protected] (3) Professor, Department of Civil Engineering, University of Chile, [email protected] Abstract The increase in strength of Steel Fiber Reinforced Concrete (SFRC) depends mainly on factors such as the dosage, aspect ratio and number of hooked ends of the fibers. Previous studies proposed models to estimate the flexural and shear strength of SFRC beams, but the shear behavior of SFRC panels has not been extensively studied. The study includes diagonal tension tests on concrete panels to assess the shear performance of SFRC. The experimental program comprises 19 square concrete panels having 600 mm side and 75 mm thickness, including three nominal dosages of steel fibers (20, 40 and 60 kg/m 3 ) and three different number of hooked ends (1, 1.5 and 2). The study proposes models to predict the shear strength and deformation capacity, stiffness degradation and toughness of SFRC panels with different number of hooked ends when subjected to diagonal tension. The models include four characteristic limit states of diagonal cracking, maximum residual strength, code-based acceptable degradation, and maximum deformation. Keywords: shear strength, concrete panels, steel fibers, failure modes, stiffness degradation, energy dissipation, diagonal tension. 1 Corresponding author. Tel.: +57 1 6500000 Ext. 1705; fax: + 57 1 6370557. Cra. 11 #101-80, [email protected] 2 1 Introduction Researchers and structural engineers are constantly seeking solutions to reduce the material damage and human losses caused by earthquakes. The construction companies also require improvements in the efficiency of the construction process of buildings. The use of steel fibers as structural reinforcement of concrete is an alternative that has been investigated in recent times to provide a solution to the two previous needs. Different researchers have demonstrated the mechanical and economic benefits of steel fiber reinforced concrete (SFRC). Steel fibers improve the tensile behavior and toughness of concrete by providing post-cracking strength, increasing toughness, and preventing brittle failure of concrete [1, 2]. Lafraugh and Moustafa [3] indicated that the impact strength of SFRC is increased both in direct impact tests and in the case of explosives, where the number of detached fragments is reduced. San Bartolomé et al. [4] demonstrated that SFRC panels with fiber dosages (D f ) higher than 30 kg/m 3 can increase the shear strength of the panels after cracking. Carrillo et al. [5] argued that steel fibers as concrete reinforcement facilitates the construction process, favor the industrialization of housing, and reduce construction time and costs. For example, the handling of steel fibers in the field is easier, so the use of steel fibers is more profitable because of the savings in labor and the reduction or elimination of material waste. The costs for transportation and storage of steel fibers is lower than those associated to electro-welded wire mesh or rebars. Fernandez [6] also stated that the use of steel fibers aided at decreasing construction costs for industrialized buildings and reduces conventional reinforcement in areas such as door and window lintels. The use of SFRC is also extended to other infrastructures such as pavement, precast elements, tunnels [7], among others. The interaction between the shear strength provided by fibers, concrete and conventional steel reinforcement can be assessed using information measured during testing of panels. Athanasopoulou [8] indicates that limited information is available about this interaction. In addition, closed-form equations for predicting the shear capacity of SFRC panels are not reported in the available literature. Most of the shear strength prediction models for SFRC elements have been proposed for beam-type elements or based on element formulations that use panel models (e.g., FSAM [9]) with uniaxial material properties (e.g., [10]). Chasioti and Vecchio [11] performed bi-axial tests on SFRC and concluded that the fibers as reinforcement increase the shear strength of concrete. Kim et al. [12] proposed a shear behavior model for any concrete member but excluded the effect of cyclic loads, as the case of 3 diagonal tension tests. These predictive models are mainly based on the truss analogy which is commonly used to predict the shear capacity in conventionally reinforced concrete elements. The contribution of the fibers in the truss analogy-based models is included independently or together with the contribution of the concrete. A review of the literature evidences that previous models for determining deformation of concrete panels focus on concrete reinforced conventionally at the web with deformed bars or electro-welded wire mesh [13, 14, 15]. However, no models are reported to predict the deformation capacity of FRC panels. On the other hand, the models proposed to estimate the contribution of fibers to the maximum residual shear strength are empirical and depend on the geometry of the beam [1, 2, 15, 16, 17, 18], the tensile and compressive mechanical characteristics of the concrete [1, 2, 15, 18, 19, 20], the maximum aggregate size [21], the reinforcement index, i.e., fiber volume (V f ) times fiber aspect ratio (l f /d f ) (RI = V f ×l f /d f ) [2, 16, 21, 22, 23], and the maximum pull-out strength between the fibers and the concrete matrix (τ) [22]. Different authors have proposed values of shear stress τ depending on the geometry and material of the fibers [2, 3, 16, 24, 25, 26]. Most of the studies reported the hooked end fibers as the fibers with the highest values of τ [16, 25, 26]. In addition, Zanjani et al. [27] observed that the anchorage between fibers and concrete increases with the number of hooked ends (N) of the fibers. Carrillo et al. [2831] observed that hooked end fibers improve residual tensile strength of the concrete when assessed using three-point bending test (3PBT), four-point bending tests (4PBT) and double punch test (DPT). Such residual tensile strength contributed by the fibers depends on the RI, number of hooked ends and tensile strength of fibers [2831]. Ashour et al. [16], Li et al. [15] and Shin et al. [17] argued that fibers increase their contribution to the maximum residual shear strength of beams when the ratio between the shear span (a) and the effective depth of reinforcement (d) is greater than 2.5. The strong connection between beam geometry and fiber contribution to shear strength makes difficult to expand the use of strength models proposed to beams to other types of elements such as panels or walls. To increase confidence in the use of steel fibers in concrete as structural reinforcement, this study experimentally evaluates the shear performance of SFRC panels by means of diagonal tension test with quasistatic cyclic loads. The experimental program includes diagonal tension tests on 19 square panels of 600 mm side and 75 mm thickness; two of them made of plain concrete and 17 made of concrete reinforced with three values of fiber dosages (D f ) and three different values of number of hooked ends (N). The properties of fresh concrete 4 were determined from slump, unit mass and air content tests. The mechanical properties of the concrete were determined by compressive strength and modulus of elasticity tests. The response measured in the panels was evaluated in terms of force-displacement envelopes, failure modes, shear stress-strain hysteresis curves and envelopes, stiffness degradation and energy dissipation. In the study, a dimensional analysis of the results measured in diagonal tension tests on SFRC panels is performed in order to determine the most influential variables in the shear performance of SFRC with different values of N. According to the evaluation of the predictive models and data analysis performed, a model to predict the shear strengths and strains of concrete panels reinforced with hooked end steel fibers is proposed. The model characterizes the performance at four key limit states describing the backbone shear stress-strain curve, namely, at diagonal cracking, maximum residual shear strength, loss of lateral resistance and maximum drift limit. 2 Experimental program The experimental program comprised tests on 17 square panels of 600 mm side and 75 mm thickness, made of concrete reinforced with three nominal dosages D f-nom of steel fibers (20 kg/m 3 , 40 kg/m 3 and 60 kg/m 3 ) and with three different values N (1, 1.5 and 2). The nomenclature used in this study is AN-B-#, where A indicates the number of hooked ends (1N, 1.5N or 2N), B represents D f-nom of fibers in the SFRC mixture (20 kg/m 3 , 40 kg/m 3 or 60 kg/m 3 ) and # represents the specimen number; for example, a mixture identified as 2N-40-1 represents the specimen 1 made of concrete reinforced with double (N = 2) hooked end fibers and D f-nom of 40 kg/m 3 . Two plain concrete panels were also tested, and they are identified as PC. One of the specimens of 1N-60 mix, was excluded from the results because one of the panels presented an unsatisfactory local failure mode. 2.1 Concrete characteristics The concrete used for the investigation had a nominal compressive strength of 24 MPa, a nominal maximum aggregate size of 12.7 mm (1/2 in.) and a slump of 25 cm (10 in.). The basic mechanical properties of the concrete were determined by compressive strength, modulus of elasticity and Poisson's ratio tests in accordance with ASTM standards. The shear behavior of SFRC was measured by diagonal tension tests on concrete panels based on ASTM E-519 [32]. Table 1 summarizes the characteristics of the concrete and the fibers used for manufacturing the 19 panels. Table 1 includes the average values of maximum compressive strength (f c ), modulus of elasticity (E c ) and 5 Poisson's ratio (ν) measured for the concrete. The coefficient of variation is also shown in Table 1 in parentheses. Carrillo et al. [2831] reported and discussed the properties of fresh concrete (slump, air content and unit mass) and the mechanical properties when assessed using three-point bending test (3PBT), four-point bending tests (4PBT) and double punch test (DPT), respectively. Table 1. Main characteristics of SFRC mixtures ID Concret e Fiber content f c , MPa E c , MPa ν D f , kg/m 3 V f , % PC 24.1 22895 0.21 0.0 0.00 (10.5%) (5.4%) (1.2%) 1N-20 24.5 21757 0.19 20.5 0.26 (0.8%) (5.3%) (10.3%) (3.6%) 1N-40 27.1 21314 0.19 41.1 0.52 (1.3%) (7.0%) (14.5%) (0.2%) 1N-60 24.6 21603 0.20 65 .0 0.83 (6.6%) (4.0%) (5.6%) (2.3%) 1.5N-20 26.7 21798 0.20 18.9 0.24 - (5.6%) (14.0%) (0.5%) 1.5N-40 23.0 19971 0.20 38.7 0.49 (0.2%) (4.5%) (10.2%) (4 .0 %) 1.5N-60 21.3 19424 0.18 58.6 0.75 (1.3%) (3.7%) (10.8%) (3.2%) 2N-20 24.1 21107 0.19 20 .0 0.26 (1.6%) (7.3%) - (2.9%) 2N-40 28.0 21542 0.20 39.2 0.50 (6.0%) (2.5%) (5.5%) (0.5%) 2N-60 28.1 20161 0.19 58.2 0.74 (2.9%) (8.6%) (5.6%) (3.3%) 2.2 Fiber characteristics Hooked end steel fibers were used in the study; i.e., 1, 1.5 and 2 hooks at the ends as shown in Table 2. The characteristics of the fibers specified by the manufacturer are also given in Table 2. Fibers with 1 hooked end have the traditional hook and its behavior depends on gradual sliding, which produces tensile stresses in the steel. The fibers with 1.5 hooked end show an improved anchorage and its behavior is similar to that of 1 hooked end fibers, but the tensile strength of fibers with 1.5 hooked end is 29% higher than that of the 1 hooked end fibers. The 2 hooked end fibers provide greater anchorage with concrete compared to 1- and 1.5- hooked end fibers. The improved anchorage of the 2 hooked end fibers allows the fracture be generated in the fiber body before sliding into its anchorage with the concrete [33]. 6 The ACI 318-19 code [34] indicates that D f greater than or equal to 60 kg/m 3 is acceptable to replace conventional steel stirrup shear reinforcing in beams. In this study, D f was defined in terms of the minimum dosage indicated in ACI 318-19 [34]; that is, D f-nom of 60 kg/m 3 , 40 kg/m 3 and 20 kg/m 3 were used, which are equivalent to 1, 2/3 and 1/3 of the minimum dosage defined in this code. These D f are equivalent to nominal fiber volume (V fnom ) of 0.25%, 0.51% and 0.76%, respectively. The fiber volume (V f ) represents the percentage of fibers within a total volume of concrete. This value of V f is computed as the ratio, in percentage, between D f and the density of its material, in this case, steel (7850 kg/m 3 ). The fibers were mixed on site inside the mixer. To ensure that the fibers were evenly distributed in the concrete matrix, the fiber addition rate was 1.7 kg/min and the mixing time was 5 minutes. The measured fiber dosage (D f ) and corresponding fiber volume (V f ) are also given in Table 1. Table 2. Fiber characteristics Shape Hooked end , N 1 1.5 2 Length , l f , mm 60 60 60 Diameter , d f , mm 0.90 0.90 0.90 Aspect ratio , l f /d f 65 65 65 Tensile strength , MPa 1160 1500 2300 Reference 3D 65/60 BG 4D 65/60 BG 5D 65/60 BG 2.3 Test setup and instrumentation Diagonal tension tests on panels were performed using a quasi-static cyclic loading protocol in accordance with ASTM E519 [32]. The diagonal tension test setup is shown in Fig. 1. Load application was performed by means of an MTS hydraulic actuator with a load capacity of 500 kN and a maximum stroke of 254 mm. The specimens were instrumented in order to measure the vertical and horizontal displacements of the panels, as shown in Fig. 1. The sensors used to measure the displacements were TML displacement transducers, type CDP-100, with a stroke capacity of 100 mm. The sampling frequency was 5 Hz. The corners of each specimen were reinforced with carbon fiber reinforced polymer (CFRP) to avoid local failure by crushing due to the concentration of compressive stresses. The corners were also confined with 3 mm thick steel plates with a tensile strength of 365 MPa. 7 Figure 1. Diagonal tension in panels: (a) test setup, (b) scheme with measures. Fig. 2 shows the loading protocol performed during the diagonal tension tests on panels, which was based on the protocol used by Almeida et al. [35] and Carrillo et al. [36] for concrete panels reinforced with conventional steel wires and externally reinforced with CFRP strips, respectively. The displacement amplitude was gradually increased until the ultimate strength state of the panels was achieved and therefore, the number of displacement cycles in the loading protocol in Fig. 2 depends on the displacement capacity of each panel. Fig. 2 shows that the first three displacement peaks with amplitudes of 0.02mm, 0.04mm and 0.08mm were defined in order to record the behavior associated to the elastic zone of the material. The next three displacement peaks with amplitude of 0.16mm, 0.24mm and 0.32mm were planned to record the residual performance of the panels immediately after diagonal cracking. The protocol implemented for the subsequent cycles was similar to that proposed by Almeida et al. [35] and Carrillo et al. [36]. The tests were displacement-controlled using the records from the actuator at a constant rate of 0.01 mm/s. During the tests, the width of the main cracks was recorded as the test reached each displacement peak. Details of the experimental program are reported by Silva (2019) [37]. Figure 2. Loading protocol. 0.0 0.8 1.6 2.4 0 2 4 6 8 10 12 14 16 18 20 22 24 26 28 Displacement, mm Cycles 1 2 3 4 5 6 78 9 10 11 12 13 14 0.02 0.04 0.08 0.16 0.24 0.32 0.40 0.60 0.80 1.00 1.20 1.60 2.00 Steel plates (b) Transducer (a) 8 3 Results and discussion 3.1 Force-displacement envelopes and cracking patterns The global response of the panels is analyzed in terms of the vertical force (P) versus horizontal displacement (ΔH) measured during the diagonal tension tests. The envelopes of the P-ΔH curves of the 19 panels are presented in Fig. 3. All panels presented a very stiff response prior to cracking. The two panels made of plain concrete exhibited brittle failures upon cracking at a load of approximately 250 kN, as shown in Fig 3a. The SFRC panels cracked at loads between 250 and 300 kN, and presented less brittle post-cracking responses. The residual resistance of the SFRC panels increased with the fiber dosage (D f ,), as shown in Fig. 3b-d. Only panels with D f =60 kg/m 3 exhibited some degree of hardening after cracking. The residual resistance of cracked SFRC panels was also improved with the number of fiber anchorages, as depicted from Fig. 3b-d. Figure 3. Vertical force vs. horizontal displacement envelopes: (a) PC (b) SFRC with 1 hooked end fibers, (c) SFRC with 1.5 hooked end fibers, (d) SFRC with 2 hooked end fibers Fig. 4 shows the crack patterns associated with the final damage state observed in the diagonal tension tests. The panels exhibited three different types of failure mechanisms or structural degradation by diagonal tension, 9 which are described in Table 3. The table shows that the single-crack failure mechanism (Type A) was the most common. The plain concrete (PC) panels exhibited a brittle and explosive failure mode, where the onset of a single crack in the main diagonal of the panels predominates. On the other hand, more than two cracks were generated in the diagonal of the panels with D f-nom of 60 kg/m 3 , due to the fact that the content of steel fibers allows the energy to be dissipated in a more distributed manner in the center of the specimen. This behavior was also observed in the concrete panels reinforced with 2 hooked end steel fibers, where more than two cracks were generated in the diagonal of the panels with D f-nom greater than or equal to 40 kg/m 3 due to the improvement of the anchorage at the hooked end of the fibers. Figure 4. Cracking patterns of diagonal tension tests in panels: (a) PC, (b) 1N-20 (1), (c) 1N-40, (d) 1N-60, (e) 1.5N-20 (2), (f) 1.5N-20, (g) 1.5N-40, (h) 1.5N-60, (i) 2N-20 (1), (j) 2N-20 (2), (k) 2N-40, (l) 2N-60. 3.2 Shear stress-strain curves Shear stress and strain were determined in accordance with the procedure established by ASTM E519 [32]. The shear stresses and associated strains were computed with Eqs. (1) and Eq. (2), respectively. Type A Type A Type B Type C Type A Type A Type B Type C Type A Type A Type C Type C (a) ( b ) ( c ) ( d ) ( e ) ( f ) ( g ) ( h ) ( i ) ( j ) ( k ) ( l ) 16 Figure 10. Coefficients C a and C b in terms of N : (a) C a , (b) C b . Table 4. Values of A and B for computing the coefficients of the proposed models Parameter Coefficient x Mean values Characteristic values A B A B v f C a N 0.013 0.002 0.01 0 v fu C b N 0.006 0.008 0.004 0.006 γ f C c N - 0.14 0.42 - 0.17 0.4 γ ad C d N 0.00004 - 0.00002 0.00002 0 k i C e RI 0.0009 0.005 0.0006 0 T f C f N - 80 300 - 96 280 T ad C g N 0.39 1.35 0.34 1.15 Fig. 11 shows the shear strain values measured during diagonal tension tests on SFRC panels, as a function of the RI. Fig. 11a shows that the strains at diagonal cracking (γ cr ) keep constant as D f and N increase, since, as explained above, there is no significant influence of the steel fibers in the elastic zone before the first cracking. Fig. 11c shows that the strain γ ad increases as D f and N increase because the fibers reduce the strength degradation after v f . This increase in the strains γ ad is also reflected in an increase of ductility and toughness in the SFRC panels. In contrast, Fig. 11b shows that the strain γ f decreases with D f and N. This decrease in γ f is related to the fact that, strain hardening with shorter plateau is generated in SFRC panels with higher D f and stiffness (K). As D f and N increase, the strains in the plateau get smaller and, therefore, the maximum residual strength is reached with smaller strains γ f . Figs. 11b and 11c show that the obtained trends are associated to very high correlation as r vary between 0.77 and 0.96 [39]. Based on the measured results, this study proposes Eqs. (8), (9) and (10) to determine the strains γ cr , γ f and γ ad in SFRC panels, respectively. The functional form of Eq. (8) is similar to that proposed by Carrillo and Alcocer [40] for low-rise concrete walls. Eq. (9) is not applicable to PC because of the absence of shear residual behavior. 0.00 0.02 0.04 0.06 1.0 1.5 2.0 2.5 C a N (a) r= 0.70 0.00 0.01 0.02 0.03 1.0 1.5 2.0 2.5 C b N (b) r= 0.66 17 Figure 11. Shear strains for diagonal tension of SFRC panels: (a) γ cr , (b) γ f , (c) γ ad . γ cr = v cr K e  H 100  (8) γ f = C c  RI  -1.7 (9) γ ad = C d  RI  (10) where K e is the cracked elastic stiffness and is determined using Eq. (11). Carrillo and Alcocer [40] proposed an equation to calculate the stiffness for low-rise concrete walls including flexural and shear strain components. However, diagonal tension behavior of panels fails in including bending stresses, therefore, Eq. (11) considers the shear component of the cracked elastic stiffness only. K e = c 2 G c A p H (11) where G c is the shear modulus of concrete, A p is the area of the main diagonal of the panel computed as the base area times 1/0.707, H is the side of the panel, and c 2 is a cracking coefficient. A cracking coefficient c 2 equal to 0.125 is proposed to estimate the stiffness of the cracked SFRC. A linear function is also used to calculate the coefficients C c and C d (see Eqs. (9) and (10)). Fig. 12 shows that the values of C c and C d depend on N. As shown in Fig. 12a, the value of C c decreases as N increases. Number of hooks N increases the confinement in the concrete matrix, and, at the maximum residual shear strength (γ f , v f ), such confinement is related to a reduction of strains γ f . In Fig. 12b, the value of C d increases as N increases because the fibers reduce the stiffness degradation by a softening behavior. The ductility of the SFRC panel increases with N, so the value of C d increases at the point (γ ad , v ad ), as shown in Fig. 12b. The values of C c and C d were determined by linear regression analysis, as shown in Figs. 12a and 12b. In this study, the parameters given in Table 4 are used in a linear function to calculate the C c and C d parameters. 0.0000 0.0002 0.0004 0.0006 0 20 40 60 γ cr , mm/mm RI 1N 1.5N 2N (a) X= 0.00029 CV = 21.6% 0.000 0.002 0.003 0.005 0 20 40 60 γ f , mm/mm RI 1N 1.5N 2N (b) r= 0.77 r= 0.78 r= 0.81 r= 0.96 r= 0.90 r= 0.85 0.000 0.002 0.004 0.007 0 20 40 60 γ ad , mm/mm RI 1N 1.5N 2N (c) 18 Figure 12. Parameters for estimating γ f and γ ad in terms of N : (a) C c , (b) C d . 4.2 Stiffness degradation To evaluate the stiffness degradation of the panels, the ratio between the post-cracking stiffness and the stiffness associated with the elastic zone (k i /k e ) is assessed in terms of the shear strain of each of the SFRC panels with 1, 1.5 and 2 hooked end steel fibers. The post-cracking stiffness was computed as the stiffness of the forcedisplacement envelope. Fig. 13 shows the stiffness degradation of each of the SFRC panels with D f-nom of 20 kg/m 3 , 40 kg/ m 3 and 60 kg/m 3 , and with 1, 1.5 and 2 hooked end steel fibers. In general, the cyclic effect of loading and unloading during the tests causes micro-cracking throughout the concrete matrix. Stiffness degradation can be caused by several factors such as shear cracking and slippage of steel fibers. Fig. 13 shows that stiffness degradation decreases as D f and N increase. However, the effect of D f on stiffness degradation is greater than that of N. Fig. 13d also shows the model proposed in this study to estimate the stiffness degradation in SFRC panels with different D f . Figure 13. Stiffness degradation for D f-nom : (a) 20 kg/m 3 , (b) 40 kg/m 3 , (c) 60 kg/m 3 , (d) predictive model. Based on the trends of the measured stiffness degradation (see Fig. 13d), Eq. (12) is proposed in this study to determine the stiffness degradation as a function of fiber volume (V f ) and fiber aspect ratio (l f /d f ). Fig. 13 shows that the trends of the stiffness degradation are associated to a very high correlations as r varies between 0.82 and 0.94. 0.0 0.2 0.4 0.6 1.0 1.5 2.0 2.5 Cc N (a) r= 0.91 0.00000 0.00006 0.00012 0.00018 1.0 1.5 2.0 2.5 C d N (b) r= 0.81 0.00 0.33 0.67 1.00 0.0000 0.0015 0.0030 0.0045 k i / k e Strain, mm/mm 1N-20 1.5N-20 2N-20 (a) 0.0 0.3 0.7 1.0 0.0000 0.0015 0.0030 0.0045 Strain, mm/mm 1N-40 1.5N-40 2N-40 (b) 0.00 0.33 0.67 1.00 0.0000 0.0015 0.0030 0.0045 Strain, mm/mm 1N-60 1.5N-60 2N-60 (c) 0.00 0.33 0.67 1.00 0.0000 0.0015 0.0030 0.0045 Strain, mm/mm (d) 20 kg/m 3 40 kg/m 3 60 kg/m 3 r= 0.82 r= 0.94 r= 0.83 19 k i = (C e (100 γ) -0.7 )k e (12) where k i is the stiffness for a given value of strain, k e is the stiffness in the elastic zone and is computed using Eq. (11), γ is the shear strain of the panel, and C e is a regression coefficient. Fig. 14 shows the relationship between RI and the coefficient C e . Fig. 14 shows that the value of C e increases 67% (0.05/0.03) when RI increases from 16 to 49. The latter values correspond to D f-nom of 20 and 60 kg/m 3 , respectively, for l f /d f of 65. In this study, a linear function is proposed to calculate the value of C e . The constants were determined by linear regression analysis, as shown in Fig. 14, and their values are presented in Table 4. Figure 14. Coefficient C e for estimating the shear stiffness k i in SFRC panels. 4.3 Energy dissipation Energy dissipation is an important property in structures subjected to seismic events since it allows reducing the stress demand through damping. Energy dissipation in the panel tests is quantified here by means of the toughness or energy absorption in shear (area under the shear stress-strain curve). Fig. 15 shows the ratio between the cumulative toughness (T i ) and the toughness at cracking (T cr ) for each of the SFRC panels with D f-nom of 20 kg/m 3 , 40 kg/m 3 and 60 kg/m 3 and with 1, 1.5 and 2 hooked end steel fibers. Figure 15. Energy dissipation in panels with different N : (a) 1, (b) 1.5, (c) 2, (d) average trends. 0.00 0.03 0.06 0.09 0 20 40 60 C e RI r= 0.84 0 10 20 30 0.0000 0.0015 0.0030 0.0045 T i /T cr Strain, mm/mm 1N-20 1N-40 1N-60 (a) 0 10 20 30 0.0000 0.0015 0.0030 0.0045 Strain, mm/mm 1.5N-20 1.5N-40 1.5N-60 (b) 0 10 20 30 0.0000 0.0015 0.0030 0.0045 Strain, mm/mm 2N-20 2N-40 2N-60 (c) 0 10 20 30 0.0000 0.0015 0.0030 0.0045 Strain, mm/mm (d) 20 kg/m 3 40 kg/m 3 60 kg/m 3 20 Fig. 15 shows that the energy dissipation or accumulated toughness increases as D f and N increase. A model is proposed in this study to determine the toughness up to the limit state of code-based acceptable degradation (γ ad , v ad ), which is defined for the time when the maximum shear strength degrades 20%. Fig. 16 shows the toughness at diagonal cracking (T cr ), at the maximum strength (T f ) and at the code-based acceptable degradation (T ad ) in terms of N and RI for each of the tested panels. Figure 16. Toughness in terms of N and RI : (a) T cr , (b) T f , (c) T ad . Fig. 16a shows that T cr /v cr keeps constant at approximately 3.5 since the contribution of steel fibers just begins at diagonal cracking. Fig. 16b shows that T f decreases with the RI because the strains associated with maximum residual strength also decrease (γ f ) (see Fig. 11b). Table 5 summarizes the increase of T ad (ΔT ad ) when D f or N is increased. Table 5 and Fig. 16c show that T ad in SFRC panels increases as D f and N increase. The ΔT ad values in Table 5 refer to the increase of energy in percentage as the D f-nom (20kg/m 3 , 40kg/m 3 and 60kg/m 3 ) or N (1, 1.5 and 2) increases. Table 5. Increase of T ad in SFRC panels in terms of D f and N D f N N D f-nom , kg/m 3 T ad , Joule ΔT ad D f - nom , kg/m 3 N T ad , Joule ΔT ad 1 20 23 - 20 1 23 - 40 29 29% 1.5 63 181% 60 213 634% 2 71 13% 1.5 20 63 - 40 1 29 - 40 80 26% 1.5 80 175% 60 382 379% 2 187 134% 2 20 71 - 60 1 213 - 40 187 162% 1.5 382 79% 60 480 157% 2 480 26% 0.0 2.5 5.0 7.5 0 20 40 60 T cr / v cr RI PC 1N 1.5N 2N (a) X= 3.5 CV = 14.7% 0 60 120 180 0 20 40 60 T f , J RI 1N 1.5N 2N (b) r= 0.94 r= 0.94 r= 0.88 0 170 340 510 0 20 40 60 T ad , J RI 1N 1.5N 2N PC (c) r= 0.75 r= 0.91 r= 0.83 21 Figs. 17a and 17b show the trend of T f /T cr and T ad /T cr ratios of PC and SFRC panels with different N (1, 1.5 and 2) in terms of RI. It is observed in Fig. 17a that the T f /T cr ratio decreases as the RI and N increase. On the other hand, it is observed in Fig. 17b that the T ad /T cr ratio increases as the RI and N increase. The r coefficients shown in Fig. 17 ranged between high and very high correlation (0.77 - 0.99) [39]. Based on the trends of T f /T cr and T ad /T cr ratios, this study proposes Eqs. (13) and (14) to determine the energy dissipation at the maximum residual strength (T f ) and code-based acceptable degradation (T ad ) as a function of the RI and the coefficients C f and C g . Figure 17. Energy dissipation in SFRC panels: (a) T ad /T cr , (b) T f /T cr . T f =   ×  × . (13) T ad = 0.01×  ×  (14) Fig. 18a and 18b show the linear trends of the parameters C f and C g . These parameters characterize the influence of N on the energy dissipations T f and T ad , respectively (see Eqs. (13) and (14)). The trends of the C f and C g in Figs. 18a and 18b are highly correlated as r are 0.74 and 0.77, respectively. As shown in Fig. 18, linear equations are proposed in this study to predict parameters C f and C g (see Table 4). Figure 18. Coefficients for estimating the shear toughness T f and T ad of SFRC panels: (a) C f , (b) C g . 0 5 10 15 0 20 40 60 T f /T cr RI 1N 1.5N 2N (a) r= 0.95 r= 0.77 r= 0.98 0 20 40 60 0 20 40 60 T ad /T cr RI 1N 1.5N 2N PC (b) r= 0.91 r= 0.86 r= 0.99 0 100 200 300 1.0 1.5 2.0 2.5 C f N (a) r= 0.74 1.0 1.7 2.4 3.1 1.0 1.5 2.0 2.5 C g N (b) r= 0.77 22 5 Statistical analysis of the proposed models To statistically evaluate the accuracy of the models proposed in this study, box and whisker plots of the ratio between the computed and measured parameters of strength, strain, stiffness and shear energy dissipation in SFRC panels are presented in Fig. 19. The figure shows the median (med), quartiles 1 and 3, and the maximum and minimum values (max, min) of the ratios between the computed and measured parameters. The quartiles 1 and 3 are the maximum and minimum limit of the boxes presented in Fig. 19. The figure also shows the over prediction (Op), computed as the percentage of values higher than 1.05. Figure 19. Box and whisker plots of the models proposed in this study: (a) shear strength, (b) shear strain, (c) stiffness, (d) toughness. Fig. 19 shows that the average coefficients between the computed and measured values of strength (v co /v me ), strain (γ co /γ me ), stiffness (k co /k me ) and toughness (T co /T me ) are always close but lower than 1, which indicates an accurate and conservative estimation. Fig. 19 also shows that the over predictions of the proposed models vary between 9.5% to 44.4% (X = 28.7%). The shear strength predictive model in Fig. 19a presents the lowest variation when compared with the models for estimating γ, k and T (Figs. 19b, 19c and 19d, respectively) because the ratio 0 1 2 3 v co / v me v cr min med Op = 9.5% Op = 35.3% Op = 11.8% max v f v ad v fu Op = 35.7% (a) 0 1 2 3 ɣ co /ɣ me ɣ cr ɣ f ɣ ad (b) Op = 33.3% Op = 29.4% Op = 33.3% 0 1 2 3 k co / k me k i Op = 32.7% (c) 0 1 2 3 T co /T me T f Op = 20.0% T ad Op = 44.4% (d) 23 v co /v me is lower than 1.57. The ratios γ co /γ me in Fig. 19b are lower than 1.51 for the parameters γ f and γ ad and up to 2.3 for the parameter γ cr . The maximum ratio T co /T me in Fig. 19d is 1.36 for the parameter T f and 2.38 for the parameter T ad . 6 Conclusions The influence of fiber dosage (D f ) and number of hooked ends (N) of steel fibers on shear strength, shear strain, crack width, stiffness degradation and energy dissipation on SFRC panels is assessed using quasi-static cyclic diagonal tension tests. The parameters were evaluated at diagonal cracking, maximum residual strength, codebased acceptable degradation, and maximum deformation limit states. Plain concrete (PC) panels showed brittle and explosive diagonal tension failure; in contrast, SFRC panels evidenced more ductile responses and less spalling. As D f increased, the SFRC panels presented failure modes with a greater number of cracks, presenting more than 2 cracks with D f-nom of 60 kg/m 3 . Only the SFRC panels with D f-nom of 60 kg/m 3 presented strain hardening, regardless of N. The crack widths of the SFRC panels in the diagonal tension tests varied between 0.2 and 3.0 mm with shear strains up to 0.45%. This crack width in the panels decreases as N and D f increase because the fibers improve the anchorage in the concrete matrix and limit the crack opening. This study proposes a set of equations to estimate the shear stress-strain response of SFRC with different D f and N. The shear stress and strain at the cracking point (ν cr and γ cr , respectively) tend to be constant regardless of N and the reinforcement index (RI = V f × l f /d f ), because the contribution of fibers to the concrete is only evident after cracking. The shear stress at the points of maximum residual strength (ν f ), code-based acceptable degradation (ν u ) and deformation limit of 0.01% (ν fu ) increase with N and RI. The maximum residual strength (ν f ) only exceeds the cracking point strength (ν cr ) in SFRC panels with D f-nom of 60 kg/m 3 , because strain hardening does not occur at lower D f . The strain at the point of maximum residual strength (γ f ) tends to decrease with N and the RI because the confinement in the concrete matrix increases and the plateau is shortened. On the other hand, the strain at the point of code-based acceptable degradation (γ ad ) increases with N and D f due to the strain capacity contributed by the fibers after cracking. Based on these results observed in this study, a model is proposed to estimate the shear stresses ν cr , ν f , ν u and ν fu , as well as the shear strains γ cr , γ f and γ ad . 24 The panel tests also evidenced that stiffness degradation decreased with an increase of D f . The study proposes a model to estimate the stiffness degradation of SFRC panels for a given value of strain and RI. In the results of diagonal tension tests on panels, a uniform dependence between shear stiffness and N was not observed, therefore, the proposed model does not include N within its equations to determine the stiffness degradation. Test results also showed that the addition of fibers contributes to increase the material toughness at the point of codebased acceptable degradation (T ad ), where it reaches values up to 30 times higher than the toughness at the cracking point (T cr ) for SFRC panels with 2 hooked ends and D f-nom of 60 kg/m 3 . On the other hand, the toughness at the point of maximum residual strength (T f ) decreases with N and D f because the strain γ f also decreases. This study proposes a model to estimate the toughness up to the point of maximum residual strength (T f ) and point of codebased acceptable degradation (T ad ) based on the toughness at the cracking point (T cr ), N and RI. Based on the findings of this study, it is recommended to use a minimum D f of 60 kg/m 3 in SFRC panels to achieve a strain hardening response and significant energy dissipation capacity. The new models proposed to predict the shear response of SFRC panels (including shear strength, stress-strain curves, stiffness and toughness) can be used to assess the performance of SFRC elements subjected to similar loading conditions and prone to diagonal tension failures, such as walls or coupling beams. The models are applicable to SFRC panels with D f between 19kg/m 3 and 65kg/m 3 and 1, 1.5 or 2 hooked ends. Additional experimental studies and developments on numerical modeling are recommended to improve the ability to predict the shear response of SFRC panels and increase the confidence of practitioners to use SFRC components. Acknowledgements The authors thank to Vicerrectoría de Investigaciones of UMNG for the financial support of the EXT-INV-3575 project. The authors also would like to thank Research Assistants Juan D. Vargas and Diego Silva at Universidad Militar Nueva Granada (UMNG) for data and figure processing. The authors also thank the companies Cemex- Colombia and Proalco-Bekaert-Colombia for supplying the concrete and steel fibers, respectively. All data that support the findings of this study are available from the corresponding author upon reasonable request. The views expressed in this paper are solely those of the authors and do not necessarily reflects the views of the sponsors. 25 References [1] Sharma A. (1986). Shear strength of steel fiber reinforced concrete beams. ACI J., 83:624–8. [2] Narayanan R, Darwish I. (1987). Use of steel fibers as shear reinforcement. ACI Structural, 84:216–27. [3] Lafraugh R., Moustafa S. (1975). Experimental investigation of the use of Steel fibers for shear reinforcement. Technical report. Concrete Technology Associates. Tacoma, USA. [4] San Bartolomé A., Muñoz A., Madalengoitia F. (2007). Shear strength behavior of concrete panels reinforced with welded-wire mesh, deformed bars, or Steel fibers. Pontificia Universidad Católica del Perú, Lima, Peru. (in Spanish) [5] Carrillo J., Pincheira J., Alcocer S. (2017). Behavior of low-rise, steel fiber-reinforced concrete thin walls under shake table excitations. Engineering Structures, 138:146-158, doi: 10.1016/j.engstruct.2017.02.017. [6] Fernández M. (1982). Steel fiber reinforced concretes, Informes de la construcción, 34(342):5-17 (in Spanish) [7] Massone, L. M., Nazar, F. (2018). Analytical and experimental evaluation of the use of fibers as partial reinforcement in shotcrete for tunnels in Chile. Tunnelling and Underground Space Technology, 77:13-25, doi: 10.1016/j.tust.2018.03.027. [8] Athanasopoulou A. (2010). Shear strength and drift capacity of reinforced concrete and high-performance fiber reinforced concrete low-rise walls subjected to displacement reversals. PhD Thesis, University of Michigan. [9] Orakcal, K., Massone, L. M., Ulugtekin, D. (2019). A hysteretic constitutive model for reinforced concrete panel elements. International J. of Concrete Structures and Materials, 13:51, doi: 10.1186/s40069-019-0365- 9. [10] Kang T.H.-K., Kim W., Massone L. M., Galleguillos T.A (2012). Shear-flexure coupling behavior of steel fiber-reinforced concrete beams. ACI Structural, 109(4):435–444. [11] Chasioti S., Vecchio F. (2017). Shear Behavior and Crack Control Characteristics of Hybrid Steel Fiber- Reinforced Concrete Panels. ACI Structural, 114-S18 : 209 – 220.