Full text
MASTER THESIS Master Structural and Construction Engineering Title Quality improvement of the recycled aggregates through surface treatment 706-TFM-233 Author Alexandra Descarrega Tutor Marilda Barra and Enric Vázquez Intensification Construction Engineering Date 10/10/2011
2 First of all, I want to offer my sincere gratefulnesses to my tutors Marilda Barra and Enric Vazquez for giving me the opportunity to develop this work, and the support and coffee moments of the rest of the department. To the Professor Anette Muller and all her team of Bauhaus's university, for their help and for making my stay in Weimar an experience that I will never forget. To my parents and sister and, especially to Jordi, for his understanding and support given to me during all time.
3 Resum L’estudi aquí presentat pretén millorar les qualitats dels àrids reciclats mitjançant un tractament superficial. La metodologia desenvolupada ha posat en pràctica diferents mètodes d’impregnació utilitzant àrids reciclats de diferent procedència i productes d’impregnació altament putzolànics. Avaluats cadascun dels mètodes d’impregnació estudiats, l’assaig dinàmic de doble impregnació ha estat el més efectiu, obtenint així resultats satisfactoris. Aquest assaig realitzat engloba dos tipus d’impregnacions, primer una impregnació amb hidròxid càlcic i després una impregnació amb la sílice col·loïdal, un material altament reactiu amb partícules entre 10 i 20 nm, totalment amorf. Aquesta tècnica d’impregnació prèviament citada, millora de forma clara les propietats mecàniques dels àrids reciclats de formigó. Aquest increment de resistència, mesurat mitjançant l’assaig crushing factor, ha sigut conseqüència directa del desenvolupament de la reacció putzolànica i de la funció de la sílice col·loïdal com a filler. A més, amb el fi de comparar la els resultat obtinguts, també s’han realitzat assajos paral·lels amb àrids naturals procedents de cantera. PARAULES CLAU: àrid reciclat, residus de construcció i demolició, putzolànics, sílice col·loïdal, impregnació
4 Abstract The study here presented aims to improve the recycled aggregates quality through surface treatment. The developed methodology has put into practice different impregnation methods using recycled aggregates of various origins and highly pozzolanic impregnation products. After evaluating each of the studied impregnation methods, the rotating double impregnation test has been the most effective, providing with the most successful results. This test included two types of impregnations: a calcium hydroxide impregnation first and afterwards, a colloidal silica impregnation. The colloidal silica is a highly reactive material with a particle size between 10 and 20 nm, totally amorphous. The impregnation technique aforementioned clearly improves the mechanical properties of the recycled concrete aggregates. This increase of resistance, evaluated through the crushing factor test, has been a direct consequence of the pozzolanic reaction developed, and the function of colloidal silica as filler. In addition, in order to compare the results obtained, parallel tests with natural aggregates from quarry were also carried out. KEYWORDS: recycled aggregates, construction and demolition waste, pozzolanics, colloidal silica, carbonation, impregnation
5 Index Chapter 1. Introduction and aims ................................................................................... 10 1.1 Introduction .................................................................................................................... 10 1.2 Aims of the research ...................................................................................................... 12 1.2.1 Objectives ................................................................................................................. 12 1.2.2 Significance .............................................................................................................. 12 Chapter 2. State of the art 14 2.1 Recycled aggregate ....................................................................................................... 14 2.1.1 Background of recycling aggregates in Europe ....................................................... 14 2.1.1.1 Public perception and costs ............................................................................. 17 2.1.2 Types ........................................................................................................................ 18 2.1.3 Production ................................................................................................................ 18 2.1.3.1 Types of plants ................................................................................................. 20 2.1.4 Properties ................................................................................................................. 23 2.1.4.1 Particle size distribution ................................................................................... 23 2.1.4.2 Shape and superficial texture .......................................................................... 24 2.1.4.3 Water absorption and Density ......................................................................... 24 2.1.4.4 Determination of resistance to fragmentation .................................................. 25 2.1.4.5 Determination of Crushing Factor .................................................................... 25 2.1.4.6 Chemical properties and Durability .................................................................. 25 2.1.4.7 Adhered mortar ................................................................................................ 27 2.1.4.8 Content of soft particles ................................................................................... 27 2.1.4.9 Contaminants and impurities ........................................................................... 27 2.1.4.10 Leaching ........................................................................................................ 28 2.2 Reduction of the emission of carbon dioxide ............................................................. 29 2.2.1 Global Warming ....................................................................................................... 29 2.2.1.1 Cement production ........................................................................................... 30
6 2.2.2 Carbon dioxide sequestration .................................................................................. 31 2.2.3 Recycled aggregates, a path to carbon dioxide reduction ....................................... 33 2.3 Quality improvement of the recycled aggregates ....................................................... 34 2.3.1 The carbonation ....................................................................................................... 34 2.3.1.1 Mechanism of carbonation ............................................................................... 34 2.3.1.2 Dependency of CSH carbonation rate on CO 2 pressure ................................. 35 2.3.1.3 Mineralogical changes due to carbonation ...................................................... 35 2.3.1.4 Models of carbonation ...................................................................................... 36 2.3.2 Surface improvement of recycled aggregates ......................................................... 38 2.3.2.1 Types of treatments ......................................................................................... 38 2.3.2.2 Interface ........................................................................................................... 40 2.3.2.3 Hydration reactions .......................................................................................... 40 2.3.3 Methods of measure ................................................................................................ 41 Chapter 3. Methodology and experimental program .............................................. 43 3.1 Used materials ................................................................................................................ 44 3.1.1 Origin materials of the recycled aggregates ............................................................ 44 3.1.2 Studied recycled aggregates ................................................................................... 44 3.1.3 Impregnation products ............................................................................................. 48 3.2 Methods used to characterize the materials object of the study .............................. 51 3.2.1 Characterization of the recycled aggregates studied in this research ..................... 51 3.2.1.1 Pore Size Distribution through Mercury intrusion porosimetry ....................... 51 3.2.1.2 Chemical Analysis through X-Ray Fluorescence Spectrometry ...................... 51 3.2.1.3 Mineralogical Analysis through X-Ray Diffraction and Scanning Electron Microscopy ................................................................................................................... 51 3.2.1.4 Water absorption and densities ....................................................................... 51 3.2.1.5 Crushing factor ................................................................................................. 52 3.2.2 Characterization of the impregnation products ........................................................ 53 3.2.2.1 Chemical Analysis through X-Ray Fluorescence Spectrometry ...................... 53 3.2.2.2 Mineralogical Analysis through X-Ray Diffraction and Scanning Electron Microscopy ................................................................................................................... 53 3.2.2.3 Particle size distribution through the laser diffraction analysis ........................ 53 3.3 Results of the methods used to characterize the materials object of the study ..... 54 3.3.1 Characterization of the produced recycled aggregates object of this study ............ 54 3.3.1.1 Recycled concrete aggregate from Weimar (RCAW) ...................................... 54
7 3.3.1.2 Recycled concrete aggregate from Barcelona (RCAB) ................................... 56 3.3.1.3 Recycled ceramic brick aggregate (RCBA) ..................................................... 57 3.3.1.4 Recycled calcium silica brick aggregate (RCSBA) .......................................... 57 3.3.1.5 Recycled light brick aggregate (RLBA) ............................................................ 57 3.3.2 Characterization of the impregnation products ........................................................ 58 3.3.2.1 Sheet microsilica .............................................................................................. 58 3.3.2.2 Spherical microsilica ........................................................................................ 61 3.3.2.3 Nanosilica ........................................................................................................ 64 3.3.2.4 Colloidal silica .................................................................................................. 66 3.3.2.5 Calcium hydroxide ........................................................................................... 67 3.4 Thecniques used to improve the surface qualities of the recycled aggregates ........... 68 3.4.1 Methods used to improve the surface qualities of the recycled aggregates ............ 68 3.4.1.1 Vacuum impregnation ...................................................................................... 68 3.4.1.2 Rotating impregnation ...................................................................................... 69 3.4.1.3 Cycic dry and wet impregnation ....................................................................... 70 3.4.1.4 Rotating double impregnation .......................................................................... 72 3.4.2 Methods used to evaluate the success of the surface treatment ............................ 72 3.4.2.1 Pore Size Distribution through Mercury intrusion ............................................ 72 3.4.2.2 Chemical Analysis through X-Ray Fluorescence Spectrometry ...................... 72 3.4.2.3 Mineralogical Analysis through X-Ray Diffraction and Scanning Electron Microscopy .................................................................................................................. 73 3.4.2.4 Water absorption and densities ....................................................................... 73 3.4.2.5 Crushing factor ................................................................................................. 73 3.4.3 Results obtained from the methods used to evaluate the success of the surface treatment ........................................................................................................................... 73 3.4.3.1 Vacuum impregnation ...................................................................................... 73 3.4.3.2 Rotating impregnation ...................................................................................... 79 3.4.3.3 Cyclic dry and wet impregnation ...................................................................... 80 3.4.3.4 Rotating double impregnation .......................................................................... 81 Chapter 4. Discussion .......................................................................................................... 86 4.1 Analysis of the developed procedures ........................................................................ 86 4.2 Efficiency of the surface treatments on the recycled aggregates with colloidal silica dispersion .................................................................................................................... 88 4.3 Study of costs ................................................................................................................. 90
8 Chapter 5. Conclusions ....................................................................................................... 92 Chapter 6. Bibliography ..................................................................................................... 95
9
Chapter 2. State of the art 16 Graph 2.2. Recycling Rates of mineral wastes (European Quality Association for Recycling, 2006) We can see that Netherlands is the country with the highest percentage of recycled aggregates, but it is France and Germany the countries which have the biggest amount of recycled aggregates against the total amount of mineral waste. These results are a direct consequence of the economy growth of every Country. The most recent data obtained from the EQAR-Congress (May 2011), of the conference given by Sr. Gunther Wolff confirm that, Germany, Belgium, the Netherlands and Denmark have recycling rates higher than 80%, against Spain, Portugal, Cyprus, Hungary, Poland or Greece with rates lower than 20%. Studying in detail the aggregates from Construction and Demolition in Spain, according to the last publication for the GERD (Asociación española de gestores de residuos de construcción y demolición), in Nov. 2010, in Spain between 30 and 40 millions tons of Construction and Demolition Waste (CDW) are generated every year. Currently in Spain there are 156 plants for the recycling of CDW, most of which are located in Catalunya and Madrid. The current rate of recycling in Spain is between 15% and 20% of the total production, as compared to the European average production of 45%, although some Countries such as Netherlands or Germany achieve rates closer to 80%. The aforementioned 15% of CDW recycled is transformed in different products. About 35% of it is commercialized as recycled product (bases and subbases of roads, drainages, sands and gravels, fill, soil base, etc.); another 40% of it is destined to fillings and restorations; the remaining 15% from the mix fraction is recovered and sorted as a plastics, woods, metal materials, etc.; and the rest of the waste is discarded and disposed of.[2] 0% 10% 20% 30% 40% 50% 60% 70% 80% 90% 100% Recycling Rates of mineral wastes Recycling rates of mineral wastes
Chapter 2. State of the art Graph 2.3. Construction and 2.1.1.1 Public perception and costs Still today, i n the eyes of the and demolition waste are seen as Besides technical consideration affecting the general acceptance of its wider use, which include public confidence, costs and liability. The use of recycled concrete can also be local conditions. It depends on several - Proxi mity and quantity of available natural - Reliability of supply, quality and quantity of capacity of recycling facility) - Public perceptions regarding the quality - Governme nt procurement incentives - St andards and regulations requiring different compared to primary material - Taxes and levies on natural aggregates The cost of sending waste to landfi selling concrete waste from a construction site to a recycler materials in a new construction on the same site can also be materials. A study carried out by that in Europe there are some recycled aggregates. In some countries where there 85% Construction and Demolition Waste in Spain CDW No Recycled CDW Recycled Construction and Demolition Waste recycled dates ( Proyecto Public perception and costs n the eyes of the population recycled aggregates derived from are seen as of inferior quality. Besides technical consideration s and the environmental benefits , there are other affecting the general acceptance of its wider use, which include public confidence, costs and concrete can also be cost-effective , depending on the on several factors: mity and quantity of available natural aggregates Reliability of supply, quality and quantity of CDW (availability of materials and of recycling facility) Public perceptions regarding the quality of recycled products nt procurement incentives andards and regulations requiring different treatment for recycled aggregate to primary material Taxes and levies on natural aggregates and on landfill cost of sending waste to landfi ll can often be grea ter than the cost of sorting and selling concrete waste from a construction site to a recycler . The cost of using demolition materials in a new construction on the same site can also be lower to that of using carried out by the World Business Council for Sustainable Development show that in Europe there are some different situations regarding profit margin between natural and recycled aggregates. In some countries where there is a lack of natural aggregates 15% Construction and Demolition Waste in Spain CDW No Recycled CDW Recycled 35% 40% 10% Recycled CDW in Spain Recycled aggregates Fillings and restorations Mixed fraction Debris 17 Proyecto GEAR) derived from construction , there are other issues affecting the general acceptance of its wider use, which include public confidence, costs and , depending on the situation and CDW (availability of materials and treatment for recycled aggregate ter than the cost of sorting and The cost of using demolition lower to that of using new Development show profit margin between natural and a lack of natural aggregates , recycling 15% 10% Recycled CDW in Spain Recycled aggregates Fillings and restorations
Chapter 2. State of the art 18 aggregates become an attractive alternative. But on the other hand, where there is abundance of quarries, the commercialization of recycled aggregates is more complicated. 2.1.2 Types The recycled aggregates have two basic classification criteria, on the one hand the particle size distribution on the other, the material composition. The composition allows us to determine the percentage of the weight for each of the different materials that are usually contained in the recycled aggregates. In particular, the materials most commonly found are the stone without adhered mortar, concrete, ceramic materials, asphalt, and other minority but damaging materials (waste, gypsum, organic mattered), which can not to exceed the 1%. According the classification done by El Proyecto GEAR, the recycled aggregates can be classified in five groups: TYPE DESCRIPTION QUANTITY OF ELEMENTS (% of total weight) Ru (Stony products) Rc (Concrete and mortar) Rb (Ceramic) Ra (Asphalt) X (Others) Ar H Recycled concrete aggregate ≥ 90% ≤ 10% ≤ 5% ≤ 1% ArM H Mix recycled concrete aggregate ≥ 70% ≤ 30% ≤ 5% ≤ 1% ArM C Mix recycled ceramic aggregate < 70% > 30 % ≤ 5% ≤ 1% ArM A Mix recycled asphalt aggregate - - 5% - 30% ≤ 1% MI Inert material - - - ≤ 5% Table 2.1. Recycled aggregates classification (Proyecto GEAR) 2.1.3 Production The processes for the production of recycled aggregates are carried out in plants of treatment which are similar to the plants of crushing of natural aggregates. These include five stages in the recycling process of construction and demolition waste and they done in the following order: 1. Coarse separation 2. Crushing 3. Separation of ferrous elements 4. Screening 5. Removal of impurities by air separation During the coarse separation the debris is chopped smaller so as to go smoothly into the crusher inlet. The crushing can be also performed by squeezing, impacting and grinding.
Chapter 2. State of the art 19 To obtain a decreasingly sized product three different crushing stages, take place primary crushing, secondary crushing and milling. Particle size distribution classes are determined during the screening operation. If necessary, impurities like wood, plastic and paper can be removed. Air separation technique is more convenient than the washing separation which is more expensive. The process ends with the storage of the products. It is difficult to take a scheme of a plant of CDW recycling as a reference, since every plant is a fruit of the needs of every zone where it is implanted, and adapted to give the maximum of performance, bearing in mind CDW material that comes to it. These plants of CDW recycling to obtain aggregates are already mobile, semimobile or fixed. They use basically an equipment of pre-screening, one o more of crushing, one for the magnetic separation and one by the sifted end. As it has already been mentioned, the recycling aggregates production has two differentiated parts to obtain good and clean aggregates. The first step is the sorting in the construction work or outside the recycling plant and afterwards its material is treated in the recycling plant. Below there are some photos that show the different types of recycled materials storage around the recycling plant. Fig.2.1. Recycled ceramic aggregates Fig.2.2. Recycled concrete aggregates
Chapter 2. State of the art 20 Fig.2.3. Mix recycled aggregates 2.1.3.1 Types of plants Stationary general plants Stationary plants of treatment manage very heterogeneous waste kinds. The heterogeneity of the CDW forces to equip the plant with machinery of great hardiness and oversized for the nominal capacity foreseen in other applications. When a location is chosen to build a CDW's plant, it is necessary to estimate not only the quantity of CDW's generated in the radius of influence of the plant, but also the production of recycled material that can be in use in the construction around it. Stationary plants are permanent installations equipped with conveyor belt, several sifts and frequently two different types of crushing machines. Stationary laboratory plants On the other hand, the stationary laboratory plants. Photographs can be seen below of two of the biggest real size laboratories to produce recycled aggregates in Europe, both located in Germany. The criterion to choose the type of machine of processing can be summarised as follows: - Resistance of the material - Hardness of the material - Quantity of material - Principal properties of the material - Size and form wished finals - Wished purity - Heat reached during the process
Chapter 2. State of the art 21 First, there is the recycling laboratory of the Bauhaus University, situated in Weimar (Germany). This laboratory belongs to the university, and they have several processing machines to study and develop projects and researchers to go to the recycling construction and demolition sites. Fig.2.4. Recycling Laboratory in Bauhaus University (Weimar) Below there is a diagram with all types of machines to process the CDW. Example of Jaw crusher Example of Impact crusher Example of Roll crusher Fig.2.5. Processing machine for coarse crushing Coarse crushing 1. Jaw crusher 2. Impact crusher 3. Roll crusher 4. Hammer crusher
Chapter 2. State of the art 22 Example of Ball mills Example of Other mills Fig.2.6. Processing machine for fine crushing Fig.2.7. Processing machine for classified And here can be seen the Verfahrenstechnik für rohstoffe UVR-FIA situated in Freiberg (Germany), a private company that studies the mineral/material processing, developing projects for the universities and researching for other companies. This three-storey laboratory is divided in two sections so they can carry out dry and wet processes and at the same time. In the ground floor there are the sorting machines, in the first floor the crushing machines and in the third floor there is the entrance of the material and the expulsion of the dust. Fig.2.8. UVR-FIA Laboratory in Freiberg Fine crushing 1. Ball mills 2. Impact mills 3. Vibrating mills 4. Hammer mills 5. Mortar mills 6. Other mills Classified 1. Vibration and vibrating screens 2. Sifter
Chapter 2. State of the art 23 Mobile Plants The mobile plants have the advantage of being able to be temporarily placed in the center of waste generation, hence maximizing the availability to fully load. The mobile plants are mobile or semi-mobile machines sized for the road transport. These machines are less expensive and easier to handle than the fixed ones, even though they are also less efficient. Fig.2.9. Mobile plant, single machine It is possible to use them inside the demolition site thus avoiding excessive handling of the debris and considerably reducing the cost of transport. A mobile plant for construction and demolition waste recycling is made basically of a crusher with a magnetic separator and a vibrating screen for the particle size distribution classification. These machines are positioned next to each other to make up a recycling station. The crusher and the screen are usually separated. Nowadays, it is possible to find a single machine with crusher, magnetic separator and screen. 2.1.4 Properties The European rules, established by the European Committee for Standardization (CEN), define the recycled aggregates as an aggregate resulting from the treatment of the inorganic material previously used in a construction process. These materials have differential characteristics when compared to the natural aggregates. DIFERENTIAL CHARACTERISITCS Minor density that natural and artificial aggregates Pozzolanic properties Major draining capacity Control of the productive process and the quality of the product Price more competitive Table 2.2. Differential characteristics of recycled aggregates (Proyecto GEAR) 2.1.4.1 Particle size distribution The particle size distribution of the recycled aggregate mainly depends of the crushing process. According to the ache M-11 [3], the finesse modulus in recycled aggregates only presents a few differences with that of the natural aggregate, depending basically of the crushing process and the quality of the original concrete. The values oscillate around 6,8 for sizes of 20 and 25 mm.
Chapter 2. State of the art 24 2.1.4.2 Shape and superficial texture The mortar that remains adhered to the recycling aggregates causes its texture to be rougher and porous than the one of natural aggregates. On the other hand, the shape coefficient is similar at the natural aggregates, lower at the limit 0,20 established by the EHE. And the slab rate, lower than the natural aggregates and the EHE value, is around 7-9%. 2.1.4.3 Water absorption and Density The water absorption is defined as the absorption rates of water by aggregate. It is determined by measuring the increase in mass of an oven dried sample when immersed in water for 24 hours. The ratio of the increase in mass of the sample, expressed as a percentage, is termed of absorption as the standard procedure is prescribed in standard UNE-EN 1097-6. The absorption rate not only affects the bond between the aggregate and cement paste but also the specific gravity of the aggregate. When the water absorption of the aggregate is higher, it will decrease the workability of fresh concretes. The water absorption is the physical property of recycled aggregate which shows more difference with the natural aggregate. The habitual rates of absorption are comprised between 4-10%, in a lot of cases failing the limit of 7% established by the annex 15 of the EHE. The absorption rate produces the effect of having to control the mix proportions of water content and to maintain water-cement ratio constant. That means, in concrete design, the higher absorption raises the issues of workability and water demand. The density or specific gravity of an aggregate is defined as the ratio of the mass of solid in a given volume of sample to the mass of an equal volume of water at the same temperature. The specific gravity is clustered under three different conditions namely bulk, apparent and saturated specific gravity. The bulk specific gravity is where the specific gravity of the aggregate is determined under the natural environment. The apparent specific gravity is determined after the aggregate is oven dried for 24 hours. The saturated specific gravity is determined when the aggregate is under the saturated condition. The specific gravity of an aggregate gives valuable information on its quality and properties and it is seen that the higher the specific gravity of an aggregate, the harder and stronger it will be. The density of the recycled aggregates is lower than the one of natural aggregates, because of the fact that the cement paste remains stuck at the grains and because there are some impurities of lower density, as asphalt or bricks. According of some studies developed, the possible densities range between 2,07-2,65 kg/dm3, for the aggregates to be considered within rates of normal density. A density higher than 2,00 kg/dm3, such as the standard UNE-EN 1097-6, is the established rate for the aggregates to make concrete. The main factors to influence the density or absorption of recycled aggregates are the size of the sample, the technical processing used on the aggregates production, the contamination degree of the aggregate and the properties of the concrete of origin. The fine fraction presents a lower density and a higher absorption than the coarse fractions, due to the fine fractions containing a higher amount of cement paste. On the other hand, concrete of lower w/c produces aggregates of higher quality, with higher density and a lower water absorption rate.
Chapter 2. State of the art 25 To summarize, we can say that we the crusher process carried out with successive stages of crushing helps remove more content of cement and therefore, the water absorption decreases and the density is increased, thus reaching values similar to those of the natural aggregates. 2.1.4.4 Determination of resistance to fragmentation According to the standard UNE-EN 1097-2, to determine the resistance to fragmentation of aggregates, there are two available methods:, the Coefficient of the Angeles test and the Aggregate Impact Value test. Currently in Spain the reference test is the Los Angeles Coefficient. It is the difference between the original mass of the aggregate and its mass after being submitted to an abrasive load and then rejecting the material that goes through the sieve 1,6 UNE expressed as a percentage of its initial mass. The value expected for the recycled aggregate can be placed within a very wide range, of 25-42 %, depending basically on the size of particles and on the quality of the original concrete. Generally the Los Angeles Coefficient increases in the fractions of smaller size. The EHE establishes a maximum value of 40% to be able to apply it to make new concrete 2.1.4.5 Determination of Crushing Value In aggregate crushing value test, the aggregate is subjected to 400 KN compression load in a cylindrical mold. The crushing value is defined by the percentage of loss in mass on 2.50 mm size of test. Bigger percentage of aggregate crushing value means the aggregate is inferior in quality. The standard BS 882:1992 corresponding with the Spanish standard UNE 83- 112-89, states that the aggregate with a crushing value lower than 25% can be used in heavy duty floor; a crushing value higher than 30% means the aggregate can be used in concrete for wearing surfaces; and when higher than 45% it can be used for other concrete purposes. The experimental result shows the crushing value of natural aggregate is 16.33 % and recycled aggregate is about 30.00 % meaning that natural aggregate is better than recycled aggregate, as was to be expected, but the difference is not very significant. 2.1.4.6 Chemical properties and Durability Chloride content The recycled aggregates can contain an appreciable amount of chlorides, mainly if the raw material is a concrete from maritime building works, bridges or pavements exposed to the thaw salt. It could be necessary to also identify the total chlorides contents in the aggregate, due to the possibility that the combined chlorides can be reactive and damage the bars. The chloride content of recycled aggregates is a matter of concern if the material is going to be used in reinforced concrete. Chloride concentration just after mixing is situated around to the 0,001-0,005%, for concretes not exposed to the aforementioned conditions. The presence of important amounts of chloride destroys a passive layer of reinforcing bars and induces corrosion of the reinforcing bars and a risk of an alkali-silica reaction is possible.
Chapter 2. State of the art 32 RESERVOIR CARBON (GT) ESTIMATES CARBON AS FRACTION OF TOTAL MASS Ocean 38.430 0,00003 Land biota 705 0,34199 Land 2890 0,00012 Sediments 77.800.000 0,00039 Carbonate sediments 65.300.000 0,00032 Organic matter sediments 12.500.000 0,00006 Table 2.3. The distribution of carbon on earth (Bob Field in 2008) The main CO 2 sequestration technologies can be divided in categories: - Mineral CO 2 sequestration - Terrestrial biosphere - Ocean storage - Oil and gas reservoirs - Deep saline formations The main drawback of these techniques, besides the limited applicability of some, is the temporary character of the storage, and the final effects of this technique. For example, the CO 2 stored in the ocean will return to the atmosphere in about a hundred to a thousand of years, and it furthermore changes the pH of the water, affecting the environment. On the other hand, storing CO 2 in oil and gas reservoirs needs continuous monitoring for an infinite length of time. An alternative technology to store carbon dioxide permanently and safely is carbon dioxide sequestration by mineral carbonation. The main advantage of this technique is that products form mineral carbonates are known to be stable over geological time periods. The basic idea of mineral carbonation is to mimic the weathering, a natural process, where the calcium or magnesium from silicate minerals is bound with CO 2 dissolved in water, forming environmentally benign and stable calcium/magnesium carbonates. Rock watering involves dissolution of atmospheric CO2 into water and reaction with minerals. The weathering process can be viewed as an acid-base reaction in which an acid (H 2 CO 3 /CO 2 ) is neutralized by a solid base (mineral). Another method for CO 2 sequestration is the use of waste cement as a calcium source for carbonate formation. Actually some researchers working in the fields related to cementbased materials are exploring possibilities to develop economical, practical, and environmentally friendly technologies for CO 2 reduction and sequestration in cement-based materials. Waste cement is a calcium-rich waste product containing calcium in the form of calcium silicate hydrate (CSH) and calcium hydroxide, portlandite (Ca(OH) 2 ). The construction and demolition waste represents a potentially large source of alkalinity. Rain or irrigation water reacting with crushed concrete would provide a source of Ca(OH) 2 to be use in conditioning shallow terrestrial or deep geologic reservoir pore water to enhance formation of carbonate minerals.
Chapter 2. State of the art 33 Cement-based materials absorb CO 2 through a process known as carbonation reaction with alkalis in the cement-based materials that results in CO 2 sequestration in these materials. About 19% of the carbon dioxide produced during the manufacture of cement is reabsorbed by the concrete over its lifecycle [7]. Carbon dioxide mineralization is the process of reacting carbon dioxide to form a solid by-product. It occurs either in the natural process off carbonation or by some specifically designed process. The normal process of carbonation is very slow, about one mm/year. The carbonation is known to occur in concrete, but is usually limited to exterior surface exposed to carbon dioxide and humidity in the air. This accelerated carbon dioxide surface absorption phenomenon may be important for determining novel and effective carbon sequestration process using recycled concrete. The carbonation reaction, the reverse process of calcination, is diffusion limited and dependant on many variables such as relative humidity, pH, concrete mix, concrete age, and pore structure. The reaction is mainly limited by the diffusion rate of carbon dioxide into the interior of the concrete mass. 2.2.3 Recycled aggregates, a path to carbon dioxide reduction A study developed in Australia concludes that the reprocessing construction and demolition waste into recycled aggregates ushers important environmental advantages. The environmental gains are attached below: - Reduced resource consumption - Diversion of waste materials from landfill - Reduced quarrying - Reduced greenhouse gas emissions Recycled aggregates can diminish the used energy in addition to reducing the emissions caused by transportation, basically where the material is reused in a closer area to the site of reprocessing. The energy used to produce recycled aggregates is 21MJ/tonne and the resulting emissions are around 4 kg CO 2 . This could represent up to 46% fewer emissions than an equivalent quarry product. [7] A Sustainable Aggregates CO 2 Estimator tool has been developed to calculate the emission and the economic implications between recycled and natural aggregates.
Chapter 2. State of the art 34 2.3 QUALITY IMPROVEMENT OF THE RECYCLED AGGREGATES The main problems of using Recycled Concrete Aggregates (RCAs) basically in concretes are: higher porosity and hence higher water absorption, lower mechanical strengths, residual impurities on the surface of the RCAs creating weaker bond between cement paste and aggregate, etc. Despite all the problematic lied above, several mechanisms are exposed to improve the quality of these recycled aggregates, being able to achieve a more generalized use in the construction industry. The improvements in long-term durability were associated with a reduction of the pH for the pore solution, and substantial conversion of calcium hydroxide, anhydrous material and CSH gel to calcium carbonate and silica gel. Improved mechanical properties and dimensional stability were attributed to substantial reductions in total porosity and modifications in micro-pore structure respectively. Processing could be aimed at producing a matrix material with minimal amounts of calcium hydroxide, anhydrous material and CSH gel along with a controlled pore structure [8]. Next the carbonation and the surface improvements are studied. 2.3.1 The carbonation 2.3.1.1 Mechanism of carbonation The carbonation process is in theory very simple but quite complex in reality. Basically calcium hydroxide (CaOH) in contact with carbon dioxide (CO 2 ) forms calcium carbonate (CaCO 3 ). Carbonation is a reaction where carbon dioxide gas or carbonate ions must pass through a carbonated surface into the material to reach fresh concrete. This is a diffusion process either by carbon dioxide gas or by carbonate ions, which in turn is controlled by the water saturation of the capillary system. Its reaction is a diffusion limited and dependant on many variables such as relative humidity, pH, concrete mix, concrete age, and pore structure (surface area). The water is not consumed but it is necessary so that the reaction takes place. A 60% of degree of drying (DOD) gives the greatest amount of conversion to calcium carbonate and silica gel [9]. When the calcium hydroxide is exposed to dissolved carbon dioxide under high pH conditions, the carbon dioxide will react with the calcium hydroxide rather quickly to form the more stable calcium carbonate. Variations in pH, concentrations, temperatures, and other factor will all impact this reaction rate. The calcium carbonate bonds are considered to be a combination of the three different crystals of calcium carbonate: vaterite, aragonite and calcite. Argonite presence is important since its formation is related with the presence of CSH with low Ca/Si content produced by decalcification of the primary CSH or by the CSH formed in the surroundings of a silica fume grains. Once exposed the basic concept of what means the reaction of carbonatión, below, we will showing more detailed conclusions reached so far by researches carried out by different centres of investigation.
Chapter 2. State of the art 35 2.3.1.2 Dependency of CSH carbonation rate on CO 2 pressure Currently, there are some published studies about different types of carbonation, such as natural carbonation, carbonation at atmospheric pressure with different content of CO 2 , and supercritical carbonation, carbonation at high CO 2 pressures. The microstructure of cement pastes carbonated using supercritical carbonation (SCCO 2 ) is different than that of air-carbonated pastes. SCCO 2 of cementicious materials increases strength and reduces permeability. Moreover the samples treated under supercritical conditions during 2h were carbonated to a larger extent than those naturally carbonated for 200 days [10]. The solubility strongly depends on the CO 2 pressure, the solubility of calcium ions at P CO2 = 3,0 MPa is 3 times that at P CO2 = 0,1 MPa [11]. For the purpose of improving the hydration resistance by carbonation treatment, it is recommended that the CaO materials should either have less appreciable apparent porosity or a limited carbonation ratio for the high-porosity CaO material. Carbon dioxide accelerated concrete curing involves many concurrent microstructural and chemical changes. The chemical changes occurring during natural concrete weathering are comparable to those that happen when using CO 2 accelerated concrete curing. See below the reactions which represent the chemical changes that occur during the carbonation reaction. ( ) 2 2 2 3 CO g H O H CO + → 2 3 3 H CO HCO H − + → + Dissolution of CO 2 in water 2 3 3 HCO CO H − − + → + ( ) ( ) 2 2 2 2 2 2 2 x x y CaO SiO nH O yH CaO SiO nH O yCa yH O + + ⋅ ⋅ ⋅ + → ⋅ ⋅ + + 2 2 ( ) 2 Ca OH Ca OH + − → + 2 2 3 3 Ca CO CaCO + − + → Precipitation of calcium carbonate 2.3.1.3 Mineralogical changes due to carbonation The sequence of mineralogical change during the carbonation is a complex process involving the mass of CO 2 that has reacted with cement hydrates as well as the partial pressure as CO 2 at the selected point. Calcite does not develop immediately, the amount of calcite increases progressively with increasing amount of CO 2 . We also have to know that an increase in surface areas, as recycled concrete cement mortars, may have the potential to sequestrate additional carbon dioxide compared to the carbonation reaction. The graph attached below shows clearly the sequence of the different zones in the carbonation of hydrated cement paste at 25ºC at saturated relative humidity [12]. Calcium dissolution from cement and portlandite
Chapter 2. State of the art 36 Fig.2.10. Carbonation of hydrated cement paste at 25ºC at saturated relative humidity The paste before carbonation is basically made of CSH, portlandite and monosulfoaluminate, but at the end of the carbonation test, it obtains mainly calcite and silica amorphous. The results of this graph have other explanation, according to some authors. Castellote also declares that shen carbonating at 10% and 100% of CO 2 , the CSH gel completely disappears, a polymerized Ca-modified silica gel is formed, as a result of the decalsification of the CSH, to point at ccarbonation up to a 3% of CO 2 , results in a microestructure much more similar to natural carbonation at aproximatly 0,03% CO2. However, Haselbach exposes that, under right conditions, all the calcium within the paste in the calcium hydroxide form can be carbonated, but there are varying predictions on how much carbonation can take place in the CSH. Legerblad predicts that in fact all the calcium can be carbonated given enough time and the proper conditions, but Engelsen, estimates a percentage of 75% [13, 14]. After all the different theories exposed above, it can be concluded that investigation is still unable to provide clear answers to the question of what is the maximum carbonation possible. On the other hand, the carbonation causes volume changes. The carbonation of portlandite is expansive and gives a value of 11% expansion [12], but this does not mean that it should appreciate a dimensional change in the cement pasta. The paste contains considerable porosity and, provided that crystallization of product phases occurs in pores, no physical expansion need occur. 2.3.1.4 Models of carbonation The classic elementary models based in the carbonation are located on the CO2 ingress front (having continuous diffusion), which provides the well-known and practical analytical solution proportional to t , taken together with the mass balance of CO2, and considering CO2 as an ideal gas [14].
Chapter 2. State of the art 37 2 2 2 co co c D P t xQ R T ⋅ ⋅ ⋅ =⋅ ⋅ With: X c : carbonation depth (m) D CO2 : coefficient of CO 2 diffusion in carbonated zones (m 2 /s) P CO2 : pressure of CO 2 at the concrete surface (Pa) t: time (s) Q: quantity of carbonatable calcium (mol/m 3 of material) R: constant of perfect gases (J/mol/K) T: temperature (K) A study of University of Toulouse of published in 2010, proposes an elementary model was proposed, in with the quantity of carbonated calcium had two sources: - The calcium of the portlandite, the ettringite and the aluminates. This calcium is completely carbonatable whatever the CO2 partial pressure. - The calcium of CSH. An approximate solution of the carbonation front ingress kinetics was then proposed. Only three parameters were involved in the solution and enabled it to comply with all the experimental results [15]. 2 0 0 0 0 2 ( ) 2 1 2 1 1 co cn n p atm atm D P t x t C P P R T C Q P n P ϕ β ⋅ ⋅ ⋅ = ⋅ ⋅ ⋅ + ⋅ ⋅ ⋅ ⋅ + + With: X c : carbonation depth (m) D 0 CO2 : coefficient of CO 2 diffusion in carbonated zones for atmospheric pressure (m 2 /s) P 0 : P CO2 (0,t) = pressure of CO 2 (Pa) t: time (s) R: constant of perfect gases (J/mol/K) T: temperature (K) β: supplementary sealing of porosity due the CSH carbonation (independent of the material) C2: number of moles of calcium in CSH for the material considered (mol/l for cement paste) n: chemical affinity of CSH towards the CO 2 pressure condition(independent of the material) P atm : atmospheric pressure (Pa) φp: fraction of paste in the concrete (l of cement paste/ l of concrete or mortar) Q1: number of moles of calcium initially contained in the hydroxides We need to point out that the problem of this model is that it doesn’t consider different moistures and different temperatures to be applied to natural conditions.
Chapter 2. State of the art 38 Fick’s law The carbonation reaction is diffusion limited and dependant on many variables such as relative humidity, pH, and concrete mix. Concrete age and pore structure. The carbonation process of concrete is principally a diffusion phenomenon. The penetration rate of carbon dioxide depends mainly on the concrete quality and the exposure condition. Based on both Fick’s first and second laws of linear diffusion equations, the threedimensional equation of conservation of mass is expressed. Concrete will carbonate whenever carbon dioxide and some water are available. The speed of carbonation depends on how fast the carbon dioxide and/or the carbonate ions can move into the concrete and react with the cement paste. In some cases, like under ground and when submerged in water, the accessibility of carbonate gas and ions may be the rate limiting factor. In a normal case scenario, however, gas is available and we can assume a constant amount at the concrete surface. 2.3.2 Surface improvement of recycled aggregates It is a fact that the recycled aggregates have some limitations: they are significantly more permeable than the natural aggregates, as proved by Roumiana Zaharieva [16]; they have micro cracks, as a consequence of the crushing process; they are covered with loose particles, which prevent a good bonding between the new cement matrix and the recycled aggregates; and they also have high porosity with the consequences that involves. The improvements of the surface across superficial treatments have a clear goal, which is to diminish the limitations of the recycled aggregates and improve its qualities. It is possible to improve the properties of recycled aggregates by suitable organic or inorganic treatment systems. We will now proceed to present the types of surface improvement studied until now. Nowadays there are some types of recycled aggregates surface treatments in study. 2.3.2.1 Types of treatments Many studies attempt to improve the quality of recycled aggregates from concrete. Masaro Tsujino [17] tried the mineral oil and silane type improving agents. He concluded that the silane type diminishes the strength of new concrete, whereas the mineral oil results looked promising, but still need more investigation. J. J. Kim [18] presented the results of an experimental study of surface treated recycled aggregates with the three different types of pozzolanic materials: sodium silicate, colloidal silica and silica fume by surface adsorption treatment for closing the open pores. A different approach was taken by Katz [19], who investigated the problem of recycled aggregate that is covered with loose particles that may prevent good bonding between the new cement matrix and the recycled aggregates. The old cement paste that remained on the natural aggregate was porous and cracked, giving place to the bad properties of the recycled aggregates. Katz proposed two methods to improve the quality of RAC, the impregnation with a solution of silica fume and the ultrasonic cleaning off the recycled aggregates. The silica fume improves the properties of cement made from recycled concrete in two ways: by improving the interface between the RCA and new cement matrix and by strengthening the structure of the old paste that is still adhered to the RCA, which has cracked
Chapter 2. State of the art 39 during the crushing process. In other words silica acts as a microfiller, filling the transition zone between the aggregates surface and the bulk of cement matrix, followed by pozzolanic reaction at the same place, resulting in fine and discontinuous pore structure [20]. So far no research has been conducted that combines the carbonation with any surface treatment of those that are exposed later. In spite of that, future lines of investigation are necessary, as there are still many different ways to continue. After reviewing the literature on the subject, it can be seen that nowadays silica products are the type of surface improving products with better expectations to be applied in the waste aggregates to achieve good results. Currently it is possible to find some silica products in the market, with products differing basically in their particle size. Nanotechnology (NT) is neither a new science nor a new technology; it helps scientists to develop composites with improved and desired characteristics. The size of the particles in the composites is crucial as, at the length scale of a manometer, the properties of many materials could be quite different from their bulk state. Applications of NT are in vary divergent fields and are already employed to enhance properties of many construction materials such as concrete, steel, glass, etc. Nano materials can modify the molecular structure of hydrated cement paste and thereby enhance many properties. In this study the the acuous silica dispersion will be used to enhance the properties of recycled aggregates. Nano Silica (NS) can contribute to efficient 'Particle Packing' in concretes by densifying the micro and nanostructure leading to improved mechanical and durability properties. NS can control degradation (through blocking of water entry on account of pore refinement) of the fundamental binder system of hydrated cement i.e., C-S-H gel caused usually due to calcium leaching out when immersed in water. NS improves the behaviour of freshly mixed cement concretes by imparting segregation resistance and by enhancing both workability/mouldability and cohesion of the matrix [21]. Particles of several sizes in a concrete mix cause a good filler effect, so that the net void volume generated is minimised and thereby an optimum mix with desirable properties is obtained. The actual packing in a multi-size particulate mix depends upon the difference between maximum and minimum sizes of particles in the mix; addition of nanoparticles increases its effect substantially. Treatment of RCA with Nano silica is one of the options available to benefit the RCA. The NS used is usually in the form of stable dispersions of nanometre size silica particles and this dispersion is generally in water. NS range has very high surface area of up to 750 m2/gram of silica solids, bearing in mind that the surface area of Portland cement ranges from 0.25 to 0,40 m2/gram.
Chapter 2. State of the art 40 2.3.2.2 Interface Karen L. Scrivener [22] has studied the interstitial transition zone that is created by the packing of the anhydrous cement grains, which produces a region of high porosity in the first 15–20 mm. Quantitative characterisation of the interfacial transition zone (ITZ) between aggregate and cement paste in concrete, confirms that it forms due to the packing of cement grains against the larger aggregate particles. This initial packing leads to a more porous zone of about 15 to 20 µm in width. The deposition of hydration products, especially calcium hydroxide tends to fill this zone, but even in mature pastes the ITZ still has a significantly higher porosity. Fig.2.13. Model of interface zone (Zimbelman, 1985),[22] Modification of the interfacial transition zone between the aggregates and the bulk matrix of concrete by using silica is a common technique applied nowadays to improve concrete properties. Impregnation of the recycled aggregate with a silica solution introduces silica particles into the cracked and loose layer of this aggregate. During concrete hardening, this layer improves the interfacial transition zone, as noted above, through the filler effect. In addition, further pozzolanic reaction between silica and the portlandite strengthen the weak structure of RA to form an improved zone, which extends from the natural aggregate through the residues as the old cement paste turns into the new cement matrix. The stronger effect of the silica treatment at an early age indicates that the filler effect of silica fume is more dominant in improving the RA than the pozzolanic reaction, which is known to develop more slowly [19]. 2.3.2.3 Hydration reactions The main reaction carried out in the silica solution surface improvement is the pozzolanic reaction. The SiO2, the principal compound in silica solutions, is a pozzolana that provokes a pozzolanic reaction.
Chapter 2. State of the art 41 A pozzolana is a sort of material that contains fundamentally silicon or silicon and aluminium, which gives it an acid character and, therefore, a great affinity for the lime (trend to combine with the lime in water presence to temperature sets). In addition, the pozzolana is basically compound with vitreous phase, being the crystalline phase very small, which gives place a material of high reactivity. The pozzolana for itself has a very small cementing value. Nevertheless, finely ground in the presence of moisture, it reacts with the calcium hydroxide to ambient temperature, giving place to the new one formation of stable compounds, slightly soluble in water and possessing cementing characteristics, capable of developing resistance for hydraulic hardening. Following, the pozzolanic reaction can be seen: Cement hydration: 2( ) Cement H O CSH A CH others + → + + Pozzolanic reaction: ( ) Pozzolan CH CSH B others + → + The main characteristics of pozzolanic reactions are: - It is a slow reaction, as opposed to the cement hydration reaction, which is fast, and gives off heat. The pozzolanic reaction also develops slow resistance. - It is a reaction that consumes calcium hydroxide instead of calcium, important fact for the durability. - The products from the reaction fill the free capillary spaces after cement hydration. 2.3.3 Methods of measure As it has previously been commented, the carbonation and the surface treatments are the methods still under study to improve the qualities of the recycled concrete aggregates. But, to achieve good results and to establish general models to understand the carbonation and the pozzolanic reactions, it is very important to know the measurement methods. On the one hand, to determine carbonation profiles in concrete some measurement methods can be used: the Gammadenssimetry, Thermogravimetric analysis and Chemical analysis, the Si Magic Angle Spinning-Nuclear Magnetic Resonance (Si M.A.S.-N.M.R.), and the X-Ray Diffraction (XRD), [10,24]. On the other hand, to determine the success of the surface treatments is necessary to use the Mercury intrusion porosimentry, chemical analysis trough X-ray fluorescence, and mineralogical analysis trough X-ray diffraction and Scanning Electronic Microscope.
Chapter 3. Methodology and experimental program 48 Fig.3.7. Recycled ceramic brick aggregate (RCBA) Fig.3.8. Recycled calcium silica brick aggregate (RCSBA) Fig.3.9. Recycled light brick aggregate (RLBA) 3.1.3 Impregnation products Silica products The silica used in this study, except for the solid one, is presented in a stable water dispersion of silica. All the impregnation products used are vitreous siliceous materials, also known as pozzolan materials. Four different silica impregnation products were used: sheet microsilica, spherical microsilica, nanosilica and colloidal silica. Below you can see a comparative table that shows differences between the four types of silica products.
Chapter 3. Methodology and experimental program 49 Watery Suspension of Silica Sheet microsilica CENTRILIT NC (Fig. 3.10.) Spherical microsilica CENTRILIT FUME SX (Fig. 3.11.) Nanosilica NANOSILICA (Fig. 3.12.) Colloidal Silica ISOSIL AN 3 NF (Fig. 3.13.) Solid content of active material 50±1,5% 50±1% 100% 30% Color White Grey White Translucent Particle size (nm) 1.050 290 123 10-20 Consistency Liquid Liquid Solid Liquid Character - - - Anionic PH at 25ºC - - - 9,5-10 Surface specifies - - - 210-220 Viscosity - - - 5±2 (m.pas 20ªC) Dispersion density (g/cm 3 ) 1,43±0,02 1,38 - 1,20-1,21 Solid density (g/cm 3 ) - - 2,64 - % Na 2 O - - - ≤0,3% Table.3.3. Properties of silica products The above impregnation products are very fine pozzolanic material. They are composed of amorphous silica, which is an oxide of silicon that can occur naturally or be syntethically produced. It is characterized by the absence of crystalline structure, and has no peaks in its X- ray diffraction pattern. Of these types of silica, the spherical microsilica is the most common; it is composed of ultra-fine solid spherical particles of amorphous silica, each approximately 100 times smaller than cement grain. Below you can see some photographs of each of the different silica products utilized. Fig.3.10. Sheet microsilica Fig. 3.11. Spherical microsilica Fig.3.12. Nanosilica Fig.3.13. Colloidal silica
Chapter 3. Methodology and experimental program 50 Calcium hydroxide The calcium hydroxide is also traditionally called slaked lime or hydrated lime. The calcium hydroxide used in this study, was presented in a solid state; it is composed of fine solid particles of crystalline silica, 10 times smaller than cement grain. Fig.3.14. Calcium hydroxide
Chapter 3. Methodology and experimental program 51 3.2 METHODS USED TO CHARACTERIZE THE MATERIALS OBJECT OF THE STUDY 3.2.1 Characterization of the recycled aggregates studied in this research The characterization of the previously mentioned materials was conducted using the following tests. 3.2.1.1 Pore Size Distribution through Mercury intrusion porosimetry Mercury porosimetry characterize a material’s porosity by applying various levels of pressure to a sample immersed in mercury. The pressure required to intrude mercury into the pores is inversely proportional to the size of the pores. AutoPore IV 9500 V1.06 was the device used to carry out this test. The mercury intrusión porosimetry was used to determine the sizes of the pores in the untreated and the treated recycled concrete aggregates. 3.2.1.2 Chemical Analysis through X-Ray Fluorescence Spectrometry (XRF) Chemical analysis is conducted for a wide range of purposes, from material identification and characterization, to quality control monitoring. We determined the chemical analysis using the data collected by the instrumental technique of X-Ray Fluorescence Spectroscopy. The aim of this chemical analysis was determining the chemical composition of the material, before and after surface treatment. 3.2.1.3 Mineralogical Analysis through X-Ray Diffraction (XRD) and Scanning Electron Microscopy (SEM) The mineralogical analysis is the study of materials to determine mineral composition and mineral structure. This analysis can be used to identify mineral species, and understand their characteristics and properties. We combined both techniques for mineralogical evaluation, the X-Ray Diffraction and the Scanning Electron Microscopy. XRD uses a powder sample whereas the SEM uses a raw material. DRX was used to analyze the evolution of the pozzolanic reaction after the surface treatment of the recycled concrete aggregates. The Scanning Electron Microscopy provided us with the microscopic information. 3.2.1.4 Water absorption and densities The density and the water absorption is determined according to the standard UNE-EN 1097-6 2000: Tests for mechanical and physical properties of aggregates - Part 6: Determination of particle density and water absorption. Simultaneously we have also obtained the bulk and particle density with Pulverpyknometer Geopyk and Heliumvergleichspyknometer respectively.
Chapter 3. Methodology and experimental program The bulk density was determined using the density according to the principle of displacement of piece materials. Fig.3.15 . Bulk density with Pulverpyknometer Geopy And on the other hand, the Helium was used as a measuring gas. Fig.3.16. Particle 3.2.1 .5 Crushing factor The crushin g value was Aggregates for concrete. Crushing The crushing factor is an indicative value of compression resistance. The aggregates ar e put inside a mould and, after the mould is filled, a compression load is progressively applied Methodology and experimental program The bulk density was determined using the GEO Pyc 1360, for the determination of density according to the principle of displacement of piece materials. 5 . Bulk density with Pulverpyknometer Geopyk And on the other hand, the particle densit y was determined by the Ultrapyk Helium was used as a measuring gas. Particle density with Heliumvergleichspyknometer .5 Crushing factor g value was determined according to the standard UNE 83 Aggregates for concrete. Crushing factor determination. Fig. 3.17.Crushing factor The crushing factor is an indicative value of compression resistance. The aggregates e put inside a mould and, after the mould is filled, a compression load is progressively applied 52 GEO Pyc 1360, for the determination of bulk y was determined by the Ultrapyk nometer 1000. according to the standard UNE 83 -112-89: The crushing factor is an indicative value of compression resistance. The aggregates e put inside a mould and, after the mould is filled, a compression load is progressively applied
Chapter 3. Methodology and experimental program 53 at a speed of 40 kN/min and up to a maximum of 400kN. Then, at the end, the resulting material is sieved to separate the coarse fraction from the finer one. Fig.3.18. Material obtained from the crushing test 3.2.2 Characterization of the impregnation products The characterization of impregnation products has been carried out using the following tests: 3.2.2.1Chemical Analysis through X-Ray Fluorescence Spectrometry (XRF) This method was used to determine the chemical composition of each impregnation product, thus obtaining information on their pozzolanic capacity. 3.2.2.2 Mineralogical Analysis through X-Ray Diffraction (XRD) and Scanning Electron Microscopy (SEM) The higher level of amorphous phases means a material is more reactive. Christaline phases make materials more stable and unlikely to react. The Scanning Electron Microscopy, on the other hand, was used to determine the particle size and shape. The localised chemical information (EDX) obtained through the SEM we can relate the studied particles with their chemical composition. 3.2.2.3 Particle size distribution through the laser diffraction analysis The specification sheet of three out of the four types of impregnation products (sheet microsilica, spherical microsilica and noanosilica) did not provide us with the particle size information. Since that data was necessary for the research, the particle size was determined using the Coulter LS 230, placed for the determination of bulk density according to the principle of displacement of piece materials.
Chapter 3. Methodology and experimental program 54 3.3 RESULTS OF THE METHODS USED TO CHARACTERIZE THE MATERIALS OBJECT OF THE STUDY 3.3.1 Characterization of the produced recycled aggregates object of this study Recycled aggregates were characterized by using X-Ray Fluorescence Spectrometry, X-Ray Diffraction, Scanning Electron Microscopy, Mercury Intrusión Porosimetry, density and absorption, and the crushing factor. 3.3.1.1 Recycled concrete aggregate from Weimar (RCAW) RCAW BEFORE IMPREGANTION, X-RAY FLUORESCENCE SPECTROMETRY Compound Concentration (%) MgO 0,24 Al 2 O 3 2,46 SiO 2 75,01 SO 3 0,56 K 2 O 1,02 CaO 10,98 TiO 2 0,10 Fe 2 O 3 0,93 SrO 0,04 BaO 0,27 PtO 2 0,07 Table.3.4. Chemical Analysis through X-Ray Fluorescence Spectrometry (XRF) of the Recycled concrete aggregate from Weimar Fig. 3.19. Mineralogical and Chemical Analysis through Scanning Electron Microscopy (SEM) and localised chemical information (EDX) of the Recycled concrete aggregate from Weimar
Chapter 3. Methodology and experimental program 55 Graph 3.1. Mineralogical Analysis through X-Ray Diffraction (XRD) of the Recycled concrete aggregate from Weimar BULK DENSITY PARTICLE DENSITY POROSITY WATER ABSORPTION 2,21 g/cm 2 2,67 g/cm 2 17,26% 6,18% Table.3.5. Water absorption, densities and porosity of the Recycled concrete aggregate from Weimar According to the above data, the recycled concrete aggregates from Weimar are characterized by a high SiO 2 content, basically from the quartz origin aggregates; besides we also can detect the presence of Microcline and Larnite, two anhydrous compounds. The porosity is 17, 26% with a water absorption of the 6,18%. On the other hand, in reference to the below graph, the pore volume distribution, we can see that the main range of porosity is placed between 0,01 and 0,1 µm. OC.ANTESIMP 72-0156 (C) - Portlandite, syn - Ca(OH)2 33-0302 (*) - Larnite, syn - Ca2SiO4 19-0932 (I) - Microcline, intermediate - KAlSi3O8 05-0586 (*) - Calcite, syn - CaCO3 46-1045 (*) - Quartz, syn - SiO2 Operations: Import OC.ANTESIMP - File: a1_287_0287_OC.ANTESIMP.raw - Type: 2Th/Th locked - Start: 4.014 ° - End: 80.001 ° - Step: 0.017 ° - Step time: 50.2 s - Temp.: 25 °C (Room) - Time Started: 0 s - 2-Theta: 4.014 ° - T Lin (Counts) 0 1000 2000 3000 4000 2-Theta - Scale 20.3 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39
Chapter 3. Methodology and experimental program 56 Graph 3.2. Cumulated pore volume distribution through Mercury Intrusion Porosimetry of the Recycled concrete aggregate from Weimar 3.3.1.2 Recycled concrete aggregate from Barcelona (RCAB) Graph 3.3. Mineralogical Analysis through X-Ray Diffraction (XRD) of the untreated recycled concrete aggregates from Barcelona 0% 20% 40% 60% 80% 100% 120% 0,001 0,01 0,1 1 10 100 1000 pore volume / % pore radius / µm Cumulated pore volume RCAW before impregnation 49-0442 (*) - Calcium Silicate - Ca3SiO5 - Y: 2.17 % - d x by: 1. - WL: 1.5406 - Monoclinic - 46-1045 (*) - Quartz, syn - SiO2 - Y: 3.05 % - d x by: 1. - WL: 1.5406 - Hexagonal - I/Ic PDF 3.4 - 05-0586 (*) - Calcite, syn - CaCO3 - Y: 73.31 % - d x by: 1. - WL: 1.5406 - Rhombohedral - I/Ic PDF 2. - 44-1481 (*) - Portlandite, syn - Ca(OH)2 - Y: 6.07 % - d x by: 1. - WL: 1.5406 - Hexagonal - I/Ic PDF 2.9 - Operations: Displacement 0.000 | Displacement 0.000 | Import DRX_C_0 - File: a1_287_0332_DRX_C_0.raw - Type: 2Th/Th locked - Start: 4.013 ° - End: 80.000 ° - Step: 0.017 ° - Step time: 80. s - Temp.: 25 °C (Room) - Time Started: 0 s - 2-Theta: 4.013 ° - Theta: 2.007 ° - Lin (Counts) 0 1000 2000 3000 4000 2-Theta - Scale 17 20 30 40 50 60
Chapter 3. Methodology and experimental program 57 BULK DENSITY POROSITY WATER ABSORPTION CRUSHING FACTOR 2,31 g/cm 2 9,57 % 5,99 % 30 ≈ 31 Table.3.6. Water absorption, porosity, water absorption and crushing factor of the Recycled concrete aggregate from Barcelona The recycled concrete aggregate from Barcelona has a high content of calcite, basically from the limestone origin aggregates. On the other hand, in the diffractogram we can find high volume of portlandite due to the fact that this is not very old concrete, and we also find anhydrous silicates. This concrete has 9,57% of porosity and a water absorption value of 5,99%. For this concrete we also tested the crushing factor, with is between 30 and 31. 3.3.1.3 Recycled ceramic brick aggregate (RCBA) BULK DENSITY PARTICLE DENSITY POROSITY WATER ABSORPTION 1,54 g/cm 2 2,92 g/cm 2 47,33% 28,94% Table.3.7. Water absorption, densities and porosity of the Recycled ceramic brick aggregate In the table above we can see the physical properties of the recycled ceramic brick aggregates, with a porosity of 47,33% with a water absorption of 29,94%. 3.3.1.4 Recycled calcium silica brick aggregate (RCSBA) BULK DENSITY PARTICLE DENSITY POROSITY WATER ABSORPTION 1,85 g/cm 2 2,70 g/cm 2 31,61% 15,12% Table.3.8. Water absorption, densities and porosity of the Recycled calcium silica brick aggregate This other type of brick, the calcium silica one, has a lower porosity than the ceramic one, with a water absorption of 15,12%. 3.3.1.5 Recycled light brick aggregate (RLBA) BULK DENSITY PARTICLE DENSITY POROSITY WATER ABSORPTION 1,04 g/cm 2 2,58 g/cm 2 59,93% 60,81% Table.3.9. Water absorption, densities and porosity of the Recycled light brick aggregate
Chapter 3. Methodology and experimental program 64 3.3.2.3 Nanosilica NANOSILICA, X-RAY FLUORESCENCE SPECTROMETRY Compound Concentration (%) Al 2 O 3 0,416 SiO 2 97,177 SO 3 0,118 K 2 O 0,143 CaO 1,863 BaO 0,283 Table.3.12. Chemical Analysis through X-Ray Fluorescence Spectrometry (XRF) of the Nanosilica Fig. 3.23. Mineralogical and Chemical Analysis through Scanning Electron Microscopy (SEM) and localised chemical information (EDX) of a particle of Nanosilica.
Chapter 3. Methodology and experimental program 65 The nanosilica is a pure amorphous pozzolana with no appreciable crystal in the diffractogram and with 97,18 % of silicon oxide, this high level of silicon making it highly reactive. As we can see in the photography, fig 3.22, the shape of the particles is rounded but not uniform, with an average particle size of 123 nm, according to the diagram of particle size distribution. Graph 3.8. Mineralogical Analysis through X-Ray Diffraction (XRD) of the Nanosilica Graph 3.9. Pore size distribution through the laser diffraction analysis of the Nanosilica Operations: Y Scale Add -83 | Import DRX_nano - File: a1_287_0331_DRX_nano.raw - Type: 2Th/Th locked - Start: 4.013 ° - End: 80.000 ° - Step: 0.017 ° - Step time: 80. s - Temp.: 25 °C (Room) - Time Started: 0 s - 2-Theta: 4.013 ° - Theta: 2.007 ° Lin (Counts) 0 100 200 300 400 2-Theta - Scale 5 10 20 30 40 50 60 70 80
Chapter 3. Methodology and experimental program 66 3.3.2.4 Colloidal silica NANOSILICA, X-RAY FLUORESCENCE SPECTROMETRY Compound Concentration (%) Na 2 O 1,044 MgO 0,237 Al 2 O 3 0,508 SiO 2 95,311 SO 3 0,426 CaO 1,474 Fe 2 O 3 0,382 BaO 0,391 PtO 2 0,090 Cl 0,138 Table.3.13. Chemical Analysis through X-Ray Fluorescence Spectrometry (XRF) of the Colloidal silica Fig. 3.24. Mineralogical and Chemical Analysis through Scanning Electron Microscopy (SEM) and localised chemical information (EDX) of a particle of Colloidal Silica.
Chapter 3. Methodology and experimental program 67 Graph 3.10. Mineralogical Analysis through X-Ray Diffraction (XRD) of the Colloidal Silica The Colloidal Silica is also a pure amorphous pozzolana without any crystal phases. The chemical analysis present an 95,31% of silicon oxide, and the localised chemical information (EDX) also shows a high peak of Si. The shape of the particles, according to the electron microscope photos, is spherical with a particle size of 10-20nm, according to the specification sheet. 3.3.2.5 Calcium hydroxide The Calcium hydroxide (Ca(OH)2) is a white and crystalline water-soluble powder which reacts with pozzolan materials. According to the specification sheet, the particle size is 1000 nm of average, and particles have a 96% of purity. Graph 3.11. Mineralogical Analysis through X-Ray Diffraction (XRD) of the Calcium hydroxide The X-ray diffraction show a clear picks of calcium hydroxide and a smaller crystals of calcite. The diffraction corroborate the dates from the specification sheet. Operations: Y Scale Add -125 | Import DRX_colloidal - File: a1_287_0329_DRX_colloidal.raw - Type: 2Th/Th locked - Start: 4.013 ° - End: 80.000 ° - Step: 0.017 ° - Step time: 80. s - Temp.: 25 °C (Room) - Time Started: 0 s - 2-Theta: 4.013 ° - Theta: Lin (Counts) 0 100 200 300 400 500 2-Theta - Scale 5 10 20 30 40 50 60 70 80 cal 05-0586 (*) - Calcite, syn - CaCO3 - S-Q 12.5 % 04-0733 (I) - Portlandite, syn - Ca(OH)2 - S-Q 87.5 % Operations: Import Type: 2Th/Th unlocked - Start: 3.976 ° - End: 69.976 ° - Step: 0.050 ° - Step time: 3. s Lin (Counts) 0 100 200 300 400 500 600 700 2-Theta - Scale 4 10 20 30 40 50 60
Chapter 3. Methodology and experimental program 68 3.4 TECHNIQUES USED TO IMPROVE THE SURFACE QUALITIES OF THE RECYCLED AGGREGATES 3.4.1 Methods used to improve the surface qualities of the recycled aggregates 3.4.1.1 Vacuum impregnation This is a method developed in the Bauhaus University in Weimar. As previously stated, four different types of recycled aggregates have been used: recycled concrete aggregate from Weimar (RCAW), recycled ceramic brick aggregate (RCBA, recycled calcium silica brick aggregate (RCSBA), and the recycled light brick aggregate (RLBA). These were chosen because each of them has a different porous distribution. Firstly, we dried the samples in the oven at 105ºC. Afterwards, the dried samples were submitted to different conditions, to obtain the best impregnation. The concrete was tested under different conditions of pressures and type of silica dispersion. Diagram 3.2. Vacuum impregnation method The samples, after a three hour desiccation period inside the recipient fig. 3.25., are soaked in the silica dispersion (50% solid content) during 20 hours at constant pressure. The pressure tested is 0, 250, 500, and 750 MPa, and also at atmospheric pressure. To develop the different vacuums, we used a container with hermetic closing connected to a vacuum pump. The regulation of the pressure was done manually, fact that explains the small variability of the vacuum pressures at which the samples were submitted. After impregnation, the cleaning of the samples was done through a brushing process, to allow the water absorption calculation. RCAW RCBA RCSBA RLBA Crushing process CONCRETE Dried 105ºC SHEET MS SPHERICAL MS Dissecation 3h Samples cleaning Vacuum impr. 24 hours
Chapter 3. Methodology and experimental program 69 A) Oven B) Vacuum recipient Fig.3.25. Impregnation procedure C) Vacuum impregn. machine 3.4.1.2 Rotating Impregnation To prevent the formation of the superficial skin that forms during the vacuum impregnation, a rotating impregnation is tried instead. In a rotating test, the samples are struck by themselves helping the prevention of the superficial skin formation. For this test, the aforementiond five different types of recycled aggregates were used: RCAW, RCAB, RCBA, RCSBA, and RLBA. Before the actual test, a trial was done. Two botles with the same samples and the same silica dispersion, were stored: one of them in a static period and the other one in a dynamic period by a rotating machine. After 24h, we obtained what the next photograps show. A) Dynamic test B) Static test Fig.3.26. Dynamic and static impregnation test The bottle that was kept static for 24h gave a bad result, all the samples had the silica stuck to the surface and, the silica was less fluid than before the start of the test. On the other hand, the bottle kept un a dynamic period for 24h gave a good result, the silica was as liquid as before the start of the test, and the samples did not have the skin. After this advance, the experimental campaign continued with dynamics impreganations at atmospheric pression.
Chapter 3. Methodology and experimental program 70 Fig.3.27. Rotating machine from Weimar Fig.3.28. Rotating machine from Barcelona The following diagram explains the experimental campaing carried out. The rotating impregnation with Spherical microsilica and nanosilica at atmospheric presures of the RCAW, RCBA, RCSBA and RLBA was developed in Weimar. Diagram 3.3. Rotating impregnation method The impregnation of the recycled aggregates RCAW, RCBA, RCSBA and RLBA with spherical microsilica and nanosilica took place over a 24 hour period using a rotating machine, as shown in diagram 3.3. After the impregnation, samples were cleaned using 1l bottles full of water in which the samples were submerged for 30 minutes in a rotating machine. Once clean, we could procede to calculate the water absorption of the samples. 3.4.1.3 Cyclic dry and wet impregnation Parallel to colloidal silica impregnation, a cyclical impregnation test was carried out, with the recycled concrete aggregate from Barcelona samples. The aim was to determine whether a cyclical dry and wet processes could lower the water absorption rate of the material. The purpose of this test was to corroborate if, by means of the repetition of the impregnation test, it was possible to perceive, across the water absorptions, the entry of solid content of the microsilica in dispersion inside of the concrete samples tested. The next a diagram shows the experimental procedure developed in this next step. Crushing process CONCRETE Dried 105ºC Samples cleaning NANOSILICA SPHERICAL MS RCAW RCBA RCSBA RLBA Rotating impr. 24 hours
Chapter 3. Methodology and experimental program 71 Diagram 3.4. Cyclic impregnation test at atmospheric pressure As we can see in diagram above, the test consisted in the combination of the silica impregnation in the rotating machine for 30 minutes, in the bottles shown in photograph A, and then a short cleaning of 15 minutes, also in the rotating machine in the bottles shown in photograph C. Once the impregnation with spherical microsilica and nanosilica is complete, samples are dried until they reach a constant weight. We can then measure the water and the silica absorptions. A) Impregnation bottles B) Rotating machine C) Cleaning bottles D) Samples E) Balance Fig. 3.29. Cyclic impregnation test 14 CYCLES CYCLIC MS IMPREGN. TEST Rotating impr. 30 min Different solid content Spherical MS / Nanosilica Rotating cleaning 15 min Drying 105ºC Static impr. 30 min Water Drying 105ºC
Chapter 3. Methodology and experimental program 72 3.4.1.4 Rotating double impregnation Diagram 3.5. Calcium hydroxide and Colloidal Silica Impregnation method at atmospheric pressure In agreement with the graph above, the calcium hydroxide and colloidal silica impregnation test was developed in two steps. After the samples drying, a first impregnation was done during 30 minutes with calcium hydroxide, in order to facilitate the development of the later pozzolanic reaction motivated by the addition of silicon oxide of the colloidal silica. After the calcium hydroxide impregnation, we proceeded to carry out the colloidal silica impregnation in a rotating machine during 24h, according to M.Tsuji [25]. After the impregnation, the aggregates were sieved, separing the colloidal silica. Later, the aggregates were stored in the humid chamber in constant themperature and moisture. After 10 days and after one month, the crushing value test was done and the reasults were compared with the values of the granite and the limestone crushing test. The granite and the limestone are main aggregates used to produce concrete. 3.4.2 Methods used to evaluate the success of the surface treatment 3.4.2.1 Pore Size Distribution through Mercury intrusion porosimetry Mercury porosimetry characterize a material’s porosity by applying various levels of pressure to a sample immersed in mercury. AutoPore IV 9500 V1.06 was the device used to carry out this test. To evaluate the success of the surface treatment, the mercury intrusion porosimetry was used to determine the sizes of the pores in the treated recycled concrete aggregates. 3.4.2.2 Chemical Analysis through X-Ray Fluorescence Spectrometry (XRF) The data collected by the instrumental technique of X-Ray Fluorescence Spectroscopy give as the chemical characterization of the material. Crushing process CONCRETE Dried 105ºC Rotating impr. 30 min Calcium hidroxide Drying 105ºC Silica colloidal Wet room 1 mounth Wet room 10days Rotating impr. 24 hours RCAB
Chapter 3. Methodology and experimental program 73 The aim of this chemical analysis was determining the chemical composition of the material, after surface treatment. 3.4.2.3 Mineralogical Analysis through X-Ray Diffraction (XRD) and Scanning Electron Microscopy (SEM) The mineralogical analysis is the study of materials to determine mineral composition and mineral structure. We combined the X-Ray Diffraction and the Scanning Electron Microscopy techniques. DRX was used to analyze the evolution of the pozzolanic reaction after the surface treatment of the recycled concrete aggregates. The Scanning Electron Microscopy provided us with the microscopic information. 3.4.2.4 Water absorption and densities We have determined the density and the water absorption according to the standard UNE-EN 1097-6 2000 after the impregnation test. Simultaneously we have also obtained the bulk and particle density with Pulverpyknometer Geopyk and Heliumvergleichspyknometer respectively. 3.4.2.5 Crushing factor The crushing value was determined according to the standard UNE 83-112-89: Aggregates for concrete. Crushing factor determination. The crushing factor was used to analyze the evolution of the resistance after the surface treatment of the recycled concrete aggregates. 3.4.3 Results obtained from the methods used to evaluate the success of the surface treatment 3.4.3.1 Vacuum impregnation To check the efficiency of the impregnation test under vacuum we used the following tests: ore size distribution through Mercury intrusion porosimetry, Chemical Analysis through X- Ray Fluorescence Spectrometry (XRF), Mineralogical Analysis through X-Ray Diffraction (XRD) and Water absorption and densities. The results for these tests were compared with the data obtained for these same tests from untreated samples.
Chapter 3. Methodology and experimental program 80 solid content of active material, does not prove to decrease the water absorption in the tested samples. At this point of the research, it was decided to conduct a mercury intrusion porosimetry (MIP) to determine the pore size distribution after surface treatment in RCAW and then compare the results with the ones of the untreated RCAW. The pore diameters that can be measured by MIP vary from 0.001 µm to 1000 µm according to the pressure used. Graph 3.15. Cumulated pore volume distribution through Mercury Intrusion Porosimetry of the RCAW after rotating impregnation method Above, the pore volume distribution shows a clear inflection point at pore radius 0,07 µm for the RCAW after spherical microsilica impregnation. Between 0,001 and 0,07 µm, in the aggregates treated with spherical microsilica, the volume of pores increases; against between 0,07 and 1000 µm, where the volume pores decrease in reference of the untreated aggregates. This means that the spherical microsilica impregnation makes finer some of the pores of the treated aggregates. On the other hand, the pore volume distribution for the RCAW after nanosilica impregnation does not show any variation compared to the untreated aggregates. 3.4.3.3 Cyclic dry and wet impregnation A follow up of the water and spherical microsilica absorption by the RCAB was carried out to test the efficiency of cyclic dry and wet impregnation. The results obtained after these 14 cycles, show a progressive decrease of absorption: the initial absorption of 5% was reduced in around 0,45%. This result implies that repeated 0% 20% 40% 60% 80% 100% 120% 0,001 0,01 0,1 1 10 100 1000 pore volume / % pore radius / µm Cumulated pore volume RCAW before impregantion RCAW after spherical microsilica impregnation RCAW after nanosilica impregnation"
Chapter 3. Methodology and experimental program 81 cycles of dry and wet impregnation allow that a higher quantity of impregnation product can penetrate the surface, as opposed to just one cycle. Graph 3.16. Water absorption during the cycling impregnation test 3.4.3.4 Rotating double impregnation As it is known, the main goals of the rotating double impregnation are two: on the one hand we aim for the filler function; and on the other hand, we want the aggregate densification trough a pozzolanic reaction. The evaluation of this method, the calcium hydroxide and colloidal silica impregnation, was done using the following methods: Mineralogical Analysis, Water absorption and densities, and the crushing factor. The results for the treated and untreated material were then compared. Below, the mineralogical study of the RCAB. The study shows the spectrums before impregnation, at 10 days of hydration, and at one month of hydration. In the diffractogram of the concrete without any impregnation, we find portlandite, calcite proceeding of some remains of limestone aggregates, and two anhydrous silicates. On the graph 3.17, the diffractograms of the samples before impregnation are compared, after 10 days of hydration, and after 1 month of hydration. The results can be summarised as follows: - The level of portlandite decreases when the time of hydration is increased. After one month of hydration the amount of portlandite diminishes considerably from the volume existing 4,30% 4,40% 4,50% 4,60% 4,70% 4,80% 4,90% 5,00% 5,10% 5,20% Percentage of absorption Cycles Cycling MS Spherical Impregnation IMPREG. MS WA.MS IMPREG.NS WA.NS Lineal (IMPREG. MS) Lineal (WA.MS) Lineal (IMPREG.NS) Lineal (WA.NS)
Chapter 3. Methodology and experimental program 82 before the impregnation. However, at 10 days of hydration the peak of the portlandite increases regarding the initial amounts due to the calcium hydroxide impregnation. - The Calcite, the quartz and the calcium silicate, remain constant in all the phases. The mineralogical results prove that the pozzolanic reaction has been carried out. Graph 3.17. Comparative Mineralogical Analysis through X-Ray Diffraction (XRD) of the treated recycled concrete aggregates from Barcelona with colloidal silica impregnation at different period of hydration Besides the mineralogical analysis of the RCAB, we carried out the crushing test for treated materials at different hydration periods, and then the results of the treated material were compared to the results obtained for the untreated one. We decided to use that specific test because we could compare our results with a benchmark, since other papers have already been published on the matter [21, 25]. To establish a comparison background, the same tests were done for limestone and granite aggregates, and then the results compared to the ones obtained for the recycled aggregates, treated and untreated. The table below shows the differences between the crushing factor values of the recycled concrete aggregates and the granite and limestone aggregates under the same conditions. The table shows the comparison between the results of the test for the RCAB untreated; the RCAB impregnated with calcium hydroxide and colloidal silica at 10 days of hydration; the RCAB impregnated with calcium hydroxide and colloidal silica at 1 month of hydration; the untreated granite aggregates; and the untreated limestone aggregates. DRX_C_0 49-0442 (*) - Calcium Silicate - Ca3SiO5 - Y: 2.17 % - d x by: 1. - WL: 1.5406 - Monoclinic - 46-1045 (*) - Quartz, syn - SiO2 - Y: 3.05 % - d x by: 1. - WL: 1.5406 - Hexagonal - I/Ic PDF 3.4 - 05-0586 (*) - Calcite, syn - CaCO3 - Y: 73.31 % - d x by: 1. - WL: 1.5406 - Rhombohedral - I/Ic PDF 44-1481 (*) - Portlandite, syn - Ca(OH)2 - Y: 6.07 % - d x by: 1. - WL: 1.5406 - Hexagonal - I/Ic PD Operations: Y Scale Add 83 | Y Scale Add 208 | Y Scale Add 125 | Y Scale Add 1 | Displacement 0.0 DRX_C_30 - File: a1_287_0334_DRX_C_30.raw - Type: 2Th/Th locked - Start: 4.013 ° - End: 80.00 Operations: X Offset 0.000 | Y Scale Add 42 | Y Scale Add -83 | Displacement 0.000 | Displacement - DRX_C_10 - File: a1_287_0333_DRX_C_10.raw - Type: 2Th/Th locked - Start: 4.013 ° - End: 80.00 Operations: Displacement 0.000 | Displacement 0.000 | Import DRX_C_0 - File: a1_287_0332_DRX_C_0.raw - Type: 2Th/Th locked - Start: 4.013 ° - End: 80.000 ° Lin (Counts) 0 100 200 300 400 500 600 700 800 900 1000 1100 1200 1300 1400 1500 1600 1700 1800 1900 2000 2100 2200 2300 2-Theta - Scale 18 20 30 40 50
Chapter 3. Methodology and experimental program 83 TEST CRUSHING VALUE RCAB untreated 30 ≈ 31 RCAB impregnated at 10 days of hydration 28,7 ≈ 29 RCAB impregnated at 1 month of hydration 27,5 ≈ 28,5 Untreated limestone aggregates 23 ≈ 24 Untreated granite aggregates 12 ≈ 13 Table.3.20. Crushing value before and after calcium hydroxide and colloidal silica impregnation The granite aggregates have the smallest crushing value, unlike the untreated recycled aggregates which have the highest value. The higher the value of the crushing test, the worst is the resistance of these aggregates. On the other hand, the following graph represents the young modulus obtained from the crushing value test. To make the graph, we used the data from the hydraulic press; the strength, the time and the piston stroke. Graph 3.18. Young modulus 0,00 5,00 10,00 15,00 20,00 25,00 0,00% 5,00% 10,00% 15,00% 20,00% 25,00% Tension (MPa) Deformation (%) Young modulus trough crushing value RCAB untreated (90,18 Mpa) RCAB impregnated at 10 days of hydration (93,06 Mpa) RCAB impregnated at 1 month of hydration (96,64 Mpa) Untreated limestone aggregates (102,45 Mpa) Untreated granite aggregates (128,85 Mpa)
Chapter 3. Methodology and experimental program 84 The previous graph shows that resistance increases as the samples increase the hydration period in the humid chamber. In order to corroborate the results of the crushing test, we proceeded to carry out the density saturated superficially dry and water absorption tests. Graph.3.19. Density saturated superficially dry and Water absorption before and after colloidal silica impregnation As can be seen in the above graph, the density follows a pattern of increasing at the same time that the period of hydration increases. On the other hand, the water absorption tends to diminish proportionally with the density increase. Regarding the results obtained in the density saturated superficially dry and water absorption, it is important to mention that they constitute approximate values and with low precision. Bearing this fact in mind, we took the results obtained only as a trend or pattern, which have to be studied more thoroughly. 2,00% 2,10% 2,20% 2,30% 2,40% 2,50% 2,60% 2,70% 2,80% 2,90% 2,56 2,57 2,57 2,57 2,57 2,57 2,58 2,58 Before impr. 10 days hydration 30 days hydration g/cm3 Density saturated superficially dry and Water absorption Density saturated superficially dry Water absorption
Chapter 4. Discussion 85
Chapter 4. Discussion 86 Chapter 4 Discussion 4.1 ANALYSIS OF THE DEVELOPED PROCEDURES The results obtained in this study indicate an improvement in the quality of the recycled aggregates. After the experimental research using four types of silica products, the most effective impregnation has been the one that uses the calcium hydroxide and the colloidal silica dispersion. The research starts with an exhaustive study of the bibliography, and then proceeds to study the possible ways of improving the quality of recycled aggregates. At this moment, the accelerated carbonation and the surface treatments are the main ways in study to improve the properties of the recycled aggregates. The main problems of recycled aggregates can be summarised as: higher porosity, and hence higher water absorption, lower mechanical strengths, and the tendency for the impurities to stick to the surface, creating bad bonds between cement paste and aggregate when new concrete is produced. This study has tried to raise the quality of the recycled aggregates through the surface treatments, specifically by using the silica impregnation tests. The experimental program has been developed over time, in parallel with the results obtained. To develop the study, we used different kinds of recycled aggregates and different types of impregnation products. On the one hand, five different kinds of recycled aggregates have been used: recycled concrete aggregate from Weimar (RCAW), recycled concrete aggregate from Barcelona (RCAB), recycled ceramic brick aggregate (RCBA), recycled calcium silica brick aggregate (RCSBA), and recycled light brick aggregate (RLBA). On the other hand, we used four types of impregnation products: sheet microsilica (CENTRILIT NC), spherical microsilica (CENTRILIT FUME SX), nanosilica, and colloidal silica (ISOSIL AN 3 NF). To improve the surface qualities of the recycled aggregates, different methods of impregnation were used: - The vacuum impregnation. This impregnation consists on submerging the samples in the impregnation product dispersion under low pressures during 20 hours.
Chapter 4. Discussion 87 - The rotating impregnation. This method is based on a dynamic impregnation by using a rotating machine. The impregnation takes place under atmospheric pressure during 20 hours. - The cyclic dry and wet impregnation. This technique consists on repeating the same silica impregnation several times. This impregnation was made using a rotating machine for 30 minutes. - The rotating double impregnation. This impregnation was carried out in two steps. A first impregnation was done with calcium hydroxide during 30 minutes, after which we proceeded to carry out the colloidal silica impregnation during 24 hours, both of them using a rotating machine. After the impregnations, the samples are stored in a humid chamber to facilitate the pozzolanic reaction. All of the above methods were evaluated in order to know the success of the surface treatment. For that, different tests were used: mercury intrusion porosimetry, X-ray fluorescence spectrometry, X-ray diffraction, scanning electron microscopy, water absorption and densities and crushing factor. The results obtained from the methods to evaluate the success of the surface treatment are shown below: - Vacuum impregnation. According to the chemical analyses we can see that the amount of SiO 2 remains the same before and after impregnation; the volume of portlandite has not suffered any variation either, meaning that the pozzolanic reaction has not taken place; the water absorption and porosity of treated samples did not present a clear decrease when compared to the untreated ones. For all these reasons, we can say that we obtained unsuccessful results. - Rotating impregnation. The water absorption and the mercury porosimetry were carried out to check the method developed. According to all the data gathered, no decrease of the water absorption in the tested samples could be proved. Neither could any appreciable decrease of the pore volume trough the mercury intrusion porosimetry test. - Cyclic dry and wet impregnation. The results obtained after 14 cycles show a progressive decrease of absorption: the initial absorption of 5% was reduced in around 0,45%. - Rotating double impregnation. The X-ray diffraction results show that the level of portlandite decreases when the time of hydration is increased, proving that the pozzolanic reaction took place. The density and the water absorption were also studied, the results of these tests not pointing out a clear decrease of the water absorption or an increase of the density of the treated samples. On the other hand, besides the mineralogical analysis, we carried out the crushing factor, which shows a clear resistance increase of the treated recycled concrete aggregates.
Chapter 4. Discussion 88 4.2 EFFICIENCY OF THE SURFACE TREATMENTS ON THE RECYCLED AGGREGATES WITH CALCIUM HYDROXIDE AND COLLOIDAL SILICA DISPERSION According to the previous chapters, it is the colloidal cilica dispersion that has the finer particle size; on the other end, the sheet microsilica has the bigger one. Colloidal Silica is approximately 1000 times smaller than the cement grain size, as opposed to the sheet microsilica, which is only around 10 times smaller than the cement grain size. In the following paragraphs we can see the main reasons for having obtained good results with the colloidal silica product. The hydrated cement contains solid components and voids. The main solid components are Calcium Silicate Hydrate (CSH), Calcium Hydroxide (CH) and Calcium Sulfoaluminates (CS). CSH takes up about 50 to 60% the total volume, CH to between 20 to 25% of the volume, and CS takes up about 15 to 20%. On the other hand, the total voids in the concrete can be classified into four types: the spacing between CSH sheets take up about 1nm, the capillary voids take up about 10 to 1000 nm, the entrained air voids occupy about 100 µm to 1 mm, and the entrapped air voids occupy about 1 to 10mm. The colloidal silica dispersion used has a particle size of 10 to 20 nm. That means that this colloidal silica can go through the capillary voids up to the entrapped air voids, and at the same time that it can fill some of them. See diagram 3.9. In this project, the colloidal silica dispersion carries out two functions, on the one hand it acts as a filler, filling some voids and improving the hardened cement graded. And on the other hand it works as a pozzolanic material high reactive. The pozzolanic function is the main work of the colloidal silica dispersion. The basis of the pozzolanic reaction is an acid-base reaction between the CH (Portlandite) and silicic acid, obtaining CSH. Due to the puzzolanic reaction, the CSH increases its volume, and consequently the capillary voids and CH products decrease. As well as its role in reducing the capillary voids the pozzolanic reaction is also developed in the interstitial zone were the calcium hydroxide is more abundant. As it was already detailed in the bibliography review [23], the interstitial transition zone is a critical zone both of the recycled concrete aggregates and of the recycled concrete production. As it has already been mentioned in the previous section, the results obtained using the colloidal silica were evaluated trough the X-ray diffraction, water absorption and densities, crushing factor. According to the interpreted diffractograms we can see that the level of portlandite decreases when the time of hydration is increased. After one month of hydration the amount of portlandite diminishes considerably from the volume existing before the impregnation. However, at 10 days of hydration the peak of the portlandite increases regarding the initial amounts due to the calcium hydroxide impregnation. The mineralogical results prove that the pozzolanic reaction has taken place. On the other hand, the crushing factor indicates the facility of the aggregates to be crushed. As shown in section 3.4.3.4, recycled concrete aggregates before any impregnation have a value of around 30, and after the colloidal silica impregnation this value decreases, until it reaches a value of 29 ten days after hydration, and around 28 one month after hydration. These results mean that the function of colloidal silica as filler and pozzolanic activator have taken place. To understand the results obtained from the crushing factor of the recycled concrete aggregates studied, they will be framed in the context of the two types of natural aggregates used in Catalonia for concrete, the limestone and the granitic stone.
Chapter 4. Discussion Diagram The crushing value of the recycled concrete aggregates after impregnation is four points higher than the crushing value of the limestone. best value: 13, 15 points below the value of recycled concrete aggregates. This result shows the small difference between the treated recycled concrete aggregat aggregates often used in concrete Furthermore, dry surface tests were carried out to test the water absorption and the density of saturated particles. The results of these tests do not point out a clear decrease of the water absorptio n or an increase of the density of the treated samples. The fine silica particles cannot fill all the inside the porous structure makes the pores smaller, thus increasing the capillary property. In addition, ano ther factor that influences the results of all the tests conducted is the temperature of drying. The crushing value, the water absorption and the densities tests, were all tested with samples dried at 110 ± 5 ºC. because the dehydration of it occurs below 100 ºC. [26] Diagram 4.1. Particle size, Nano-engineering concrete value of the recycled concrete aggregates after impregnation is four points higher than the crushing value of the limestone. T he granite aggregates have the best value: 13, 15 points below the value of recycled concrete aggregates. This result shows the small difference between the treated recycled concrete aggregat es and the limestone often used in concrete . Furthermore, dry surface tests were carried out to test the water absorption and the density of saturated particles. The results of these tests do not point out a clear decrease of the n or an increase of the density of the treated samples. The fine silica particles cannot fill all the mortar voids. The solid material deposited inside the porous structure makes the pores smaller, thus increasing the capillary property. ther factor that influences the results of all the tests conducted is the temperature of drying. The crushing value, the water absorption and the densities tests, were all tested with samples dried at 110 ± 5 ºC. At this temperature the ettringite disappea because the dehydration of it occurs below 100 ºC. [26] 89 value of the recycled concrete aggregates after impregnation is 28, only he granite aggregates have the best value: 13, 15 points below the value of recycled concrete aggregates. This result shows es and the limestone Furthermore, dry surface tests were carried out to test the water absorption and the density of saturated particles. The results of these tests do not point out a clear decrease of the voids. The solid material deposited inside the porous structure makes the pores smaller, thus increasing the capillary property. ther factor that influences the results of all the tests conducted is the temperature of drying. The crushing value, the water absorption and the densities tests, were all At this temperature the ettringite disappea rs completely
Chapter 6. Bibliography 96 [14]. Haselbach Liv. M, Shuguo Ma. Potential for carbon adsorption on concrete: Surface XPS analyses. University of South Carolina (March 2008) [15]. Hyvert N, Sellier A. Dependency of C-S-H carbonation rate on co2 pressure to explain transition from accelerated tests to natural carbonation. University of Toulouse (April 2009) [16] Zaharieva R, Buyle-Bodin F. Assessment of the surface permeation properties of recycled aggregates concrete. University of Architecture, Sofia (Jan. 2002) [17] Tsujino M, Noguchi T. Study on the application of low-quality recycled coarse aggregate to concrete structure by surface modification treatment. University of Tokyo (2006) [18] Kim J. J, Youn S. H, Cho M. J, Shin H. T, Yoon J. B, Hwang K. H, and Lee D. S. The recycled aggregates with surface treatment by pozzolanics. Nat’l University,Korea (2005) [19] Katz A. Treatments for the improvement of recycled aggregates. Technion-Israel Institute of Technology (2004) [20] Kalaiarasu S. M, Subramanian K. Properties of recycled aggregate concrete with silica fume. Coimbatore Institute of Technology, India (2006) [21] Kutcharlapati S; Sarkar A. K, Rajamane N P. Nanosilica improves recycled concrete aggregates. Centre for Advanced Concrete Research, SRM University, Katankulathur (Jan. 2011) [22] Scrivener K.L, Crumbie A.K, Laugesen P. The interfacial transition zone (itz) Between cement paste and aggregate in concrete. E. Polytechnique Lausane, Swit. (2004) [23] Zimbelmann R. A contribution to the problem of cement-aggregate bond. Otto-Graf-Institut. Stuttgart, Germany (1985) [24] Villain G, Thiery M. Measurement methods of carbonation profiles in concrete thermogravimetry, chemical analysis and gammadensimetry. Laboratory central, Paris (Apr. 2007) [25] Tsuji M, Sawamoto T. Technical method to improve properties of recycled aggregates concrete. University of Tokyo [26] Alonso C, Fernández L. Dehydration and rehydration processes of cement paste exposed to high temperature environments. Institute of Construction “Eduardo Torroja” (C.S.I.C.), Madrid (2004)