scieee AI-readable full text Open interactive document viewer

Modulating the Tg of poly(alkylene succinate)s by inserting bio-based aromatic units via ring-opening copolymerization

Morales Huerta, Juan Carlos,Martínez de Ilarduya Sáez de Asteasu, Domingo Antxon,Muñoz Guerra, Sebastián

Abstract

Two series of aliphatic-aromatic copolyesters derived from succinic and 2,5-furandicarboxylic acids, and di-O-2-(hydroxyethyl) resorcinol as diol substituent of either 1,4-butanediol or ethylene glycol, respectively, were obtained by ring opening polymerization(ROP) performed in bulk and catalyzed by Sn(Oct)2. Cyclic oligomers of furandicarboxylate of di-O-2-(hydroxyethyl) resorcinol were successfully synthesized by high-dilution condensation, and then copolymerized with cyclic oligomers of either butylene or ethylene succinate. The synthesized resorcinol-containing succinate-furanoatecopolyesters had Mw oscillating between 50,000 and 30,000 g·mol-1 depending on composition, and they all displayed a nearly random microstructure. They showed an excellent thermal stability with onset decomposition temperatures near 300 °C. They are amorphous with Tg increasing monotonically with the content in resorcinol in both series with values ranging from -30 or -13 °C for butylene and ethylene-based copolyesters, respectively, up to around 45 °C. The resorcinol-containing succinate-furanoate copolyesters showed appreciable hydrolytic degradation when incubated for a few weeks in water under physiological conditions, a behavior that was notably enhanced in the presence of lipases

Full text

polymers Article Modulating the Tgof Poly(alkylene succinate)s by Inserting Bio-Based Aromatic Units via Ring-Opening Copolymerization Juan Carlos Morales-Huerta, Antxon Martínez de Ilarduya ID and Sebastián Muñoz-Guerra * ID Departament d’Enginyeria Química, Universitat Politècnica de Catalunya, ETSEIB, Diagonal 647, 08028 Barcelona, Spain; [email protected] (J.C.M.-H.); [email protected] (A.M.d.I.) *Correspondence: [email protected]; Tel.: +34-93-401-6680 Received: 12 November 2017; Accepted: 6 December 2017; Published: 12 December 2017 Abstract: Two series of aliphatic-aromatic copolyesters derived from succinic and 2,5-furandicarboxylic acids, and di-O-2-(hydroxyethyl) resorcinol as diol substituent of either 1,4-butanediol or ethylene glycol, respectively, were obtained by ring opening polymerization(ROP) performed in bulk and catalyzed by Sn(Oct) 2 . Cyclic oligomers of furandicarboxylate of di-O-2-(hydroxyethyl) resorcinol were successfully synthesized by high-dilution condensation, and then copolymerized with cyclic oligomers of either butylene or ethylene succinate. The synthesized resorcinol-containing succinate-furanoatecopolyesters had M w oscillating between 50,000 and 30,000 g · mol −1 depending on composition, and they all displayed a nearly random microstructure. They showed an excellent thermal stability with onset decomposition temperatures near 300 ◦ C. They are amorphous with T g increasing monotonically with the content in resorcinol in both series with values ranging from − 30 or − 13 ◦ C for butylene and ethylene-based copolyesters, respectively, up to around 45 ◦ C. The resorcinol-containing succinate-furanoate copolyesters showed appreciable hydrolytic degradation when incubated for a few weeks in water under physiological conditions, a behavior that was notably enhanced in the presence of lipases. Keywords: bio-based copolyesters; poly(alkylene succinate)s; resorcinol; 2,5-furandicarboxylic acid; ED-ROP; furane-based polyesters 1. Introduction Poly(alkylene succinate)s area family of aliphatic polyesters that are distinguished by their easy accessibility from naturally occurring compounds and their noticeable biodegradability [ 1 , 2 ]. In fact, the US Department of Energy declared bio-based succinic acid as a high-potential chemical platform for compounds so far obtained from fossil feedstock, which is indeed the case of poly(succinate)s [ 3 ]. Also most alkanediols, and in particular 1,2-ethanediol and 1,4-butanediol, are compounds accessible from renewable resources [ 4 – 6 ]. Poly(alkylene succinate)s are highly crystalline polyesters with thermal and mechanical properties largely depending on the length of the alkylene moiety [ 7 , 8 ]. Poly(butylene succinate) (PBS) and poly(ethylene succinate) (PES), with melting temperatures of 115 and 100 ◦ C respectively, are by far the most well-known members of the family, the former being currently produced at industrial scale, and both of them showing excellent potential for packaging and biomedical applications [ 9 ]. Nonetheless, due to the high flexibility inherent to the aliphatic polyester chain, the glass transition temperatures of poly(alkylene succinate)s are too low, with values around − 30 and − 12 ◦ C for PBS and PES, respectively. Copolymerization including benzenedicarboxylic acids as comonomers has proven to be a highly effective method to increase the T g of the aliphatic polyesters [ 10 ]. This is not however a fully satisfactory approach since the sustainability of the Polymers 2017,9, 701; doi:10.3390/polym9120701 www.mdpi.com/journal/polymers Polymers 2017,9, 701 2 of 17 parent aliphatic polyester becomes largely reduced, and its biodegradability is almost lost when significant amounts of aromatic moieties are introduced in the polymer chain [ 11 ]. Copolymerization using bio-based 2,5-furandicarboxylic acid has represented a noteworthy step forward in this regard. Poly(butylene succinate-co-2,5-furandicarboxylate) copolyesters, abbreviated as co(PBS x BF y ), with T g within the ± 30 ◦ C range depending on composition, and retaining appreciable biodegradability, have been described by different authors [ 12 – 14 ]. Also Bikiaris et al. have recently reported on poly(ethylene succinate-co-2,5-furandicarboxylate)s, abbreviated as co(PES x EF y ), which display T g increasing monotonically up to near 80 ◦ C and whichare able to show perceptible biodegradability even for high contents in furanoate units [15]. In the present work, copolyesters of PES and PBS containing both 2,5-furandicarboxylate (F) and 1,3-benzenedioxyethylene (R) units, which derive from the 2,5-furandicarboxilic acid (FDCA) and resorcinol, respectively, are reported. FDCA is a well-known bio-based compound that is currently receiving enormous attention as a possible substitute of terephthalic and isophthalic acids in the industrial synthesis of aromatic polyesters [ 16 – 18 ]. Resorcinol (1,3-dihydroxybenzene) is a diphenol currently produced at industrial scale by alkaline fusion of 1,3-benzenedisulfonic acid but that may be also obtained from glucose by fermentation either via inositol [19,20] or via triacetic acid lactone [21]. This compound is extensively used in medicine as external antiseptic [ 22 ], and it is also consumed in large amounts in the industrial manufacture of formaldehyde resins [23]. The synthesis of linear polyesters using a resorcinol-based monomer was firstly reported by Vijayakumar et al. [ 24 ] and later by Gioia et al. [ 25 ]. These authors etherified resorcinol with ethylene carbonate todi-O-2-(hydroxyethyl) resorcinol (HER). This primary aliphatic diol allowed the avoidance ofthe polymerization restraints derived from the low reactivity of the aromatic hydroxyl groups. HER was made to react with both aromatic and aliphatic dicarboxylic acids, both saturated and unsaturated, to obtain an assortment of potentially sustainable amorphous polyesters. Resorcinol-containing polymers with M w up to near 55,000 g · mol −1 were reported by Goia et al. [ 25 ]. Additionally, several patents covering diverse aromatic copolyesters of resorcinol displaying high barrier properties have been also reported [ 26 , 27 ]. The ability of resorcinol to repress gas permeability in polymers is in line with the general behavior that is characteristic of 1,3-disubstituted aromatic compounds. The aim of the present paper was to obtain PES and PBS copolyesters with enhanced T g but without losing the potential sustainability of the parent homopolyesters. The hypothesis applied to the work was that the substitution of the alkylene unit by a resorcinol-derived unit in poly(alkylene succinate-co-furanoate) copolyesters may further increase the stiffness of the chain in a similar manner as aromatic diacids do. In order to favor the sustainability of the synthesis, the copolyesters have been prepared by ring-opening copolymerization in bulk following the methodology previously used by us for the synthesis of co(PBS x BF y ) copolyesters [ 14 ]. By this method solvents are avoided and generation of byproducts is minimized. Cyclic oligomers of furandicarboxylate of di-O-2-(hydroxyethyl) resorcinol required for ring opening polymerization (ROP) have been prepared for the first time and characterized following the same methodology reported by us for the synthesis of butylene furanoate oligomers. By this means, two series of succinate-furanoatecopolyesters, made from mixtures of either 1,4-butanediol or ethylene glycol, and di-O-2-(hydroxyethyl) resorcinol, have been obtained for a wide range of compositions. The thermal behavior and biodegradability of the two copolyesters series was comparatively evaluated between them and also taking as reference the poly(alkylene succinate-co-furanoate) series reported in the recent literature [14,15]. 2. Materials and Methods 2.1. Materials 2,5-Furandicarboxylic acid (FDCA, 98% purity) was purchased from Satachem (Shanghai, China). Di-O-2-(hydroxyethyl) resorcinol (HER) (99%) was obtained from TCI Chemicals (Tokyo, Polymers 2017,9, 701 3 of 17 Japan), thionyl chloride (SOCl 2 , 99%), 1,4-butanediol (BD, 99%), ethylene glycol (EG, 99%), di-azabicyclo[2.2.2]octane (DABCO, 99%), tin(II) ethylhexanoate (Sn(Oct) 2 , 99%) catalysts, and porcine pancreas lipase were purchased from Sigma-Aldrich Co. (St. Louis, MO, USA).Triethylamine (Et 3 N, 98%) and dimethyl succinate (DMS) were purchased from Panreac (Castellar del Vallés, Spain). Solvents used for reaction, isolation and purification were of high-purity grade and used as received, except dichloromethane (DCM), tetrahydrofurane (THF) and toluene that were dried on 3 Å-molecular sieves. DABCO catalyst was purified by sublimation. 2.2. Measurements 1 H and 13 C NMR spectra were recorded on a Bruker AMX-300 spectrometer (Bruker, Billerica, MA, USA) at 25 ◦ C, operating at 300.1 and 75.5 MHz, respectively. For NMR analysis, monomers, cyclic oligomers, intermediate compounds, and polymers were dissolved in deuterated chloroform (CDCl 3 ), and spectra were internally referenced to tetramethylsilane (TMS). About 10 and 50 mg of sample in 1 mL of solvent were used for 1 H and 13 C NMR, respectively. Sixty-four scans were recorded for 1H and between 1000 and 10,000 scans for 13C NMR. High-performance liquid chromatography (HPLC) analysis was performed at 25 ◦ C in a Waters apparatus equipped with a UV detector of Applied Biosystems(Foster City, CA, USA) operating at 254 nm wavelength, and a Scharlau Science column (Si60, 5 µ m; 250 × 4.6 mm, Scharlab, Sentmenat, Spain). Cyclic oligomers (1 mg) were dissolved in chloroform (1 mL) and eluted with hexane/1,4-dioxane 70/30 (v/v) at a flow rate of 1.0 mL·min−1. Matrix-assisted laser desorption/ionization time of flight (MALDI-TOF) mass spectra were recorded in a 4700 Proteomics Analyzer instrument (Applied Biosystems, Foster City, CA, USA) of the Proteomics Platform of Barcelona Science Park, University of Barcelona. Spectra acquisition was performed in the MS reflector positive-ion mode. About 0.1 mg of sample was dissolved in 50 µ L of DCM and 2 µ L of this solution were mixed with an equal volume of DCM solution of anthracene (10 mg · mL −1 ) and this mixture left to evaporate to dryness onto the stainless steel plate of the analyzer. The residue was then covered with 2 µ L of a solution of 2,5-dihydroxibenzoic acid in acetonitrile/H 2 O (1/1) containing 0.1% trifluoroacetic acid (TFA), and the mixture was left to dry prior to exposition to the laser beam. Molecular weight analysis was performedby GPC on a Waters equipment provided with RI and UV detectors. 100 µ L of 0.1% (w/v) sample solution were injected and chromatographed with a flow of 0.5 mL · min −1 of 1,1,1,3,3,3-hexafluoroisopropanol (HFIP). HR5E and HR2 Waters linear Styragel columns (7.8 mm × 300 mm, pore size 103–104 Å) packed with crosslinked polystyrene and protected with a pre-column were used. Average molecular weights and molecular dispersities were calculated against PMMA standards. The thermal behavior of cyclic compounds and polymers were examined by differential scanning calorimetry (DSC), using a (Perking-Elmer Pyris apparatus, Waltam, MA, USA). Thermograms were recorded on 3–6 mg samples in the − 80–200 ◦ C interval at heating or cooling rates of 10 ◦ C · min −1 under a nitrogen flow of 20 mL · min −1 . Indium and zinc were used as standards for temperature and enthalpy calibration, respectively. The glass transition temperature (T g ) was taken as the inflection point of the heating DSC traces recorded at 20 ◦ C · min −1 from quenched samples, and the melting temperature (T m ) was taken as the maximum of the endothermic peak appearing on heating traces. Thermogravimetric analysis was performed on a Mettler-Toledo TGA/DSC 1 Star System under a nitrogen flow of 20 mL · min −1 at a heating rate of 10 ◦ C · min −1 and within a temperature range of 30 to 600 ◦C. 2.3. Synthesis of Cyclic Oligomers Cyclic oligomers of butylene succinate and ethylene succinate, c(BS) n and c(ES) n respectively, were prepared by the high-dilution condensation (HDC) method [ 28 ] following the experimental procedures reported by us [ 14 , 29 ]. Cyclic oligo[di-O-2-(hydroxyethyl) resorcinol 2,5-furandicarboxylate]s, Polymers 2017,9, 701 4 of 17 abbreviated as c(RF) n , were synthesized from HER and 2,5-furandicarboxylic dichloride (FDCA-Cl 2 ) by applying the HDC methodology in a manner as we reportedfor the synthesisof cyclic oligo(butylene 2,5-furandicarboxylate)s with some minor modifications [ 30 ]. To 250 mL of THF placed in a three-necked round bottom flask at 0 ◦ C, 6.30 mmol (0.71 g) of DABCO were added under stirring. 2.55 mmol (0.48 g) of FDCA-Cl 2 and 2.55 mmol (0.5 g) of HER in 10 mL of THF were then drop-wise added simultaneously over a period of time of 40 min using separated addition funnels in order to maintain the reagents equimolarity. The reaction was finished by adding 1 mL of water followed by 5 mL of 1 M HCl. After stirring for 5 min, the reaction mixture was diluted with DCM and filtered. The filtrate was washed with 0.1 M HCl, dried on MgSO 4 , and evaporated to dryness to render a mixture of linear and cyclic oligomers. Linear oligomers were removed by chromatography through a short column of silica gel using a cold mixture of DCM/diethyl ether 90/10 (v/v) as eluent. Yield: 60%. 1 H NMR ( δ ppm, CDCl 3 , 300 MHz): 7.30–7.10 (m), 6.63 (dd), 6.54 (m), 4.67 (m), 4.56 (m), 4.46 (m), 4.26 (m). 13 C NMR ( δ ppm, CDCl 3 , 75.5 MHz): 161.6, 159.6, 157.8, 146.5, 130.0, 129.8, 118.9, 118.4, 111.7, 107.4, 107.2, 102.1, 69.2, 65.7, 65.6, 64.9, 63.7, 63.6. 2.4. Synthesis of Polyesters Polyesters and copolyesters were synthesized by ROP in bulk using Sn(Oct) 2 as catalyst. The general procedure was as follows: the mixture made of c(RF) n and either c(BS) n or c(ES) n at the definite molar ratio and containing 1 mol % of catalyst, was dissolved in CHCl 3 in a three-necked round bottom flask, and then evaporated to dryness and held under vacuum for 24 h. Reaction was then initiated by heating the mixture at the selected temperature and left it to proceed for the scheduled time under mechanical stirring and under a nitrogen flow. Aliquots were removed at scheduled times and analyzed by GPC in order to follow the evolution of molecular weight as the reaction proceeded. 2.5. Hydrolytic and Enzymatic Degradation Copolyesters coPBS 40 RF 60 ,coPBS 50 RF 50 ,coPBS 70 RF 30 ,coPES 40 RF 60 ,coPES 50 RF 50 and coPES 70 RF 30 as well as the parent homopolyesters PBS, PES and PRF were selected for the degradation study. Films with a thickness of ~200 µ m were prepared by casting from either HFIP or chloroform solution of the polymer at a concentration of 100 g · L −1 . Films were cut into 10 mm-diameter, 20–30 mg-weight disks and dried under vacuum to constant weight. For hydrolytic degradation assays, samples were immersed in vials containing 10 mL of sodium phosphate buffer, pH 7.4 at 37 ◦ C. Enzymatic degradation assays were carried out in the same buffer but with 10 mg of porcine pancreas lipase added. In this case, the buffer solution was replaced every 72 h in order to insurance enzyme activity. In both cases, disks were withdrawn from the incubation medium at scheduled times, washed carefully with distilled water, dried to constant weight, and analyzed by GPC. 3. Results and Discussion The synthetic route followed in this work for the preparation of coPBS x RF y and coPES x RF y copolyesters by ROP including the synthesis of the cyclic oligomers and their polymerization is depicted in Scheme 1. Polymers 2017,9, 701 5 of 17 Polymers 2017, 9, 701 5 of 17 Scheme 1. Route of synthesis leading to PBSRF and PESRF copolyesters. 3.1. Synthesis of Cyclic Oligomers The cyclic oligomers c (BS) n and c (ES) n were first synthesized by enzymatic cyclocondensation in solution of dimethyl succinate with either 1,4-butanediol or ethylene glycol, respectively, applying the general procedure previously described by us [30]. A summary of relevant features of these cyclic oligomers fractions is given in Table 1. It is worth noticing that both fractions are heterogeneous in cycle sizes and that no dimer is detected in the c (ES) n fraction. Table 1. Cyclic Oligomers Fractions used for ROP. Fraction Precursors Yield (%) a Composition (%-wt) b Thermal Properties Tm (°C) c °Td,5% (°C) d maxTd (°C) d c(BS)n DMS + BD 70 50/40/10 105 266 340/400 c(ES)n DMS + EG 70 0/45/55 100 200 300/400 c(RF)n FDCA-Cl2 + HER 60 28/57/15 158/166/185 263 415 a Yields for the oligomeric after the removal of the linear species (flashed). b Mixtures of dimer/trimer/tetramer species measured by HPLC. c Determined by DSC at 10 °C·min−1. d Decomposition temperatures (onset and maximum rate) determined by TGA. The c (RF) n fraction has been synthesized for the first time in this work from FDCA-Cl2 and HER in 60% yield after removing the linear oligomers by flash chromatography. The 1H and 13C NMR spectra of this purified oligomeric fraction were fully consistent with the expected cyclic chemical structure (Figure 1). Splitting displayed by some signals is due to magnetic environment OO O O O OO O OO OO O O C C CC O O O O OO O O n-1 O O O OOO OO n-1 n-1 O O Ox OOOOO OOOy OO O Ox OOOO OOOy OCl Cl O O FDCA-Cl2 OOH O HO MeO OMe O O DMS HO OH EG HO BD OH + + + c(RF)n c(BS)n c(ES)n CALB DABCO CALB 90 oC 90 oC 0 oC Sn(Oct)2 Sn(Oct)2 coPBSxRFy coPESxRFy HER Scheme 1. Route of synthesis leading to PBSRF and PESRF copolyesters. 3.1. Synthesis of Cyclic Oligomers The cyclic oligomers c(BS) n and c(ES) n were first synthesized by enzymatic cyclocondensation in solution of dimethyl succinate with either 1,4-butanediol or ethylene glycol, respectively, applying the general procedure previously described by us [ 30 ]. A summary of relevant features of these cyclic oligomers fractions is given in Table 1. It is worth noticing that both fractions are heterogeneous in cycle sizes and that no dimer is detected in the c(ES)nfraction. Table 1. Cyclic Oligomers Fractions used for ROP. Fraction Precursors Yield (%) aComposition (% wt) bThermal Properties Tm(◦C) c◦Td,5% (◦C) d maxTd(◦C) d c(BS)nDMS + BD 70 50/40/10 105 266 340/400 c(ES)nDMS + EG 70 0/45/55 100 200 300/400 c(RF)nFDCA-Cl2+ HER 60 28/57/15 158/166/185 263 415 a Yields for the oligomeric after the removal of the linear species (flashed). b Mixtures of dimer/trimer/tetramer species measured by HPLC. c Determined by DSC at 10 ◦ C · min −1 . d Decomposition temperatures (onset and maximum rate) determined by TGA. The c(RF) n fraction has been synthesized for the first time in this work from FDCA-Cl 2 and HER in 60% yield after removing the linear oligomers by flash chromatography. The 1 H and 13 C NMR spectra of this purified oligomeric fraction were fully consistent with the expected cyclic chemical Polymers 2017,9, 701 6 of 17 structure (Figure 1). Splitting displayed by some signals is due to magnetic environment differences between protons and carbons attached to the cyclic dimer and to other cyclic oligomers of higher size, which become distinguishable by NMR. Polymers 2017, 9, 701 6 of 17 differences between protons and carbons attached to the cyclic dimer and to other cyclic oligomers of higher size, which become distinguishable by NMR. Figure 1. 1H and 13C NMR spectra of c(RF)n. The composition of the c(RF)n fraction was determined by HPLC chromatography and MALDI-TOF spectroscopy, and results obtained therefrom are shown in Figure 2. Three peaks were observed in the HPLC chromatograms which correspond to dimer, trimer and tetramer species in an approximate molar ratio of 2/4/1, as it was ascertained in the MALDI-TOF spectra. According to these results, the content of this fraction in species of size higher than tetramer may be considered almost negligible. Figure 2. HPLC (a) and MALDI-TOF (b) of c(RF)n. As it is seen in Table 1, thermal properties of c (RF) n differ significantly from those of c (BS) n and c (ES) n . These resorcinol-containing cycles not only melt at higher temperature but also display multiple peaks probably arising from cyclic species of different size. On the other hand, c (RF) n shows much greater resistance to decomposition by heating than the alkylene succinate cycles, as it should be expected from their aromatic constitution. Furthermore, as it is shown in Figure 3, the TGA trace of c (RF) n only shows one single weight loss step at difference (ppm) 0.00.51.01.52.02.53.03.54.04.55.05.56.06.57.07.5 (ppm) 020406080100120140160 400 600 800 1000 1200 1400 1600 1800 2000 0 10 20 30 40 50 60 70 80 90 100 c(RF)4 c(RF)3 % Intensity mass (m/z) 318 c(RF)2 b) 010 20 30 40 50 60 70 80 c(RF)4 c(RF)3 time (min) c(RF)2 a) Figure 1. 1H and 13C NMR spectra of c(RF)n. The composition of the c(RF) n fraction was determined by HPLC chromatography and MALDI-TOF spectroscopy, and results obtained therefrom are shown in Figure 2. Three peaks were observed in the HPLC chromatograms which correspond to dimer, trimer and tetramer species in an approximate molar ratio of 2/4/1, as it was ascertained in the MALDI-TOF spectra. According to these results, the content of this fraction in species of size higher than tetramer may be considered almost negligible. Polymers 2017, 9, 701 6 of 17 differences between protons and carbons attached to the cyclic dimer and to other cyclic oligomers of higher size, which become distinguishable by NMR. Figure 1. 1H and 13C NMR spectra of c(RF)n. The composition of the c(RF)n fraction was determined by HPLC chromatography and MALDI-TOF spectroscopy, and results obtained therefrom are shown in Figure 2. Three peaks were observed in the HPLC chromatograms which correspond to dimer, trimer and tetramer species in an approximate molar ratio of 2/4/1, as it was ascertained in the MALDI-TOF spectra. According to these results, the content of this fraction in species of size higher than tetramer may be considered almost negligible. Figure 2. HPLC (a) and MALDI-TOF (b) of c(RF)n. As it is seen in Table 1, thermal properties of c (RF) n differ significantly from those of c (BS) n and c (ES) n . These resorcinol-containing cycles not only melt at higher temperature but also display multiple peaks probably arising from cyclic species of different size. On the other hand, c (RF) n shows much greater resistance to decomposition by heating than the alkylene succinate cycles, as it should be expected from their aromatic constitution. Furthermore, as it is shown in Figure 3, the TGA trace of c (RF) n only shows one single weight loss step at difference (ppm) 0.00.51.01.52.02.53.03.54.04.55.05.56.06.57.07.5 (ppm) 020406080100120140160 400 600 800 1000 1200 1400 1600 1800 2000 0 10 20 30 40 50 60 70 80 90 100 c(RF)4 c(RF)3 % Intensity mass (m/z) 318 c(RF)2 b) 010 20 30 40 50 60 70 80 c(RF)4 c(RF)3 time (min) c(RF)2 a) Figure 2. HPLC (a) and MALDI-TOF (b) of c(RF)n. As it is seen in Table 1, thermal properties of c(RF) n differ significantly from those of c(BS) n and c(ES) n . These resorcinol-containing cycles not only melt at higher temperature but also display Polymers 2017,9, 701 7 of 17 multiple peaks probably arising from cyclic species of different size. On the other hand, c(RF) n shows much greater resistance to decomposition by heating than the alkylene succinate cycles, as it should be expected from their aromatic constitution. Furthermore, as it is shown in Figure 3, the TGA trace of c(RF) n only shows one single weight loss step at difference with the two well separate falls that are observed for alkylene succinate cycles. This is a very reasonable result since the weight losses displayed by c(BS) n and c(ES) n at temperatures in the 300–350 ◦ C range are reported to be due to partial volatilization of the sample, a fact that is not expected to happen in the case of c(RF)n. Polymers 2017, 9, 701 7 of 17 with the two well separate falls that are observed for alkylene succinate cycles. This is a very reasonable result since the weight losses displayed by c (BS) n and c (ES) n at temperatures in the 300–350 °C range are reported to be due to partial volatilization of the sample, a fact that is not expected to happen in the case of c (RF) n . Figure 3. Compared TGA analysis of cyclic oligomers. (a) TGA traces; (b) Derivative curves showing temperatures at which degradation takes place at maximum rate. 3.2. Synthesis of Copolyesters The synthesis of the copolyesters was performed by ED-ROP (Entropically-Driven Ring Opening Polymerization) in bulk using Sn(Oct)2 as catalyst. Two copolyesters series, i.e., coPBSxRFy and coPESxRFy, were prepared frommixtures of either c(BS)n or c(ES)n and c(RF)n at molar ratios ranging between 10% and 90%, in addition to the homopolyesters PBS, PES and PRF. Reaction temperatures above 190 °C were used to insure melting of the cycles. Preliminary assays indicated that reaction noticeably speeded when temperature was raised from 190 to 200 °C but not significant change in rate was observed when temperature was further increased, a behavior that was shared by the two series (Figure 4). According to these results, this was the temperature of choice applied for the synthesis of the whole collection of copolyesters. The evolution of the molecular weight of the forming polymer as a function of reaction time for several selected compositions is represented for the two series in Figure 5. An asymptotic trend was followed in all cases showing a notable decay in reaction rate after five hours when weight-average molecular weight values up to ~40,000 and ~50,000 g·mol−1 for PBS and PES copolyesters, respectively, were attained. Lower values, around 28,000–30,000 g mol-1 were indeed achieved when higher contents of RF were used. Figure 4. Evolution ofMwalong reaction time in the ROP of equimolar mixtures of c(RF)n and either c(BS)n (a) or c(ES)n (b) forthree different temperatures. 0 1 2 3 4 5 0 5 10 15 20 25 30 35 40 45 50 220 °C 200 °C 190 °C Mw (kg mol-1) time (h) a) 0 1 2 3 4 5 0 5 10 15 20 25 30 35 40 45 50 220 °C 200 °C 190 °C Mw(kg mol-1) time(h) b) 100 200 300 400 500 600 -2.5 -2.0 -1.5 -1.0 -0.5 0.0 c(BS)n c(ES)n c(RF)n Derivative remaining weight (% oC-1) Temperature(°C) b) 100 200 300 400 500 600 0 20 40 60 80 100 c(BS)n c(ES)n c(RF)n Remaining Weight (%) Temperature(°C) a) Figure 3. Compared TGA analysis of cyclic oligomers. ( a ) TGA traces; ( b ) Derivative curves showing temperatures at which degradation takes place at maximum rate. 3.2. Synthesis of Copolyesters The synthesis of the copolyesters was performed by ED-ROP (Entropically-Driven Ring Opening Polymerization) in bulk using Sn(Oct) 2 as catalyst. Two copolyesters series, i.e., coPBS x RF y and coPES x RF y , were prepared frommixtures of either c(BS) n or c(ES) n and c(RF) n at molar ratios ranging between 10% and 90%, in addition to the homopolyesters PBS, PES and PRF. Reaction temperatures above 190 ◦ C were used to insure melting of the cycles. Preliminary assays indicated that reaction noticeably speeded when temperature was raised from 190 to 200 ◦ C but not significant change in rate was observed when temperature was further increased, a behavior that was shared by the two series (Figure 4). According to these results, this was the temperature of choice applied for the synthesis of the whole collection of copolyesters. The evolution of the molecular weight of the forming polymer as a function of reaction time for several selected compositions is represented for the two series in Figure 5. An asymptotic trend was followed in all cases showing a notable decay in reaction rate after five hours when weight-average molecular weight values up to ~40,000 and ~50,000 g · mol −1 for PBS and PES copolyesters, respectively, were attained. Lower values, around 28,000–30,000 g · mol −1 were indeed achieved when higher contents of RF were used. Interestingly, ROP proceeded faster as the content of the feed in c(RF) n diminished, which may be interpreted as due to the higher relative reactivity of the alkylene succinate cycles. An assay of polymerization in absence of catalyst showed not significant increase in molecular weight indicating that ROP was unable to proceed by exclusive action of heating. The NMR analysis of the copolyesters ascertained the chemical constitution expected for them. 1 H NMR spectra of coPBS 50 RF 50 and coPES 50 RF 50 are shown in Figure 6as representative examples and the whole spectra collection for the two series is accessible in the SI file (Figures S1 and S2). The comonomer content in the copolyesters determined from the information provided by 1 H NMR spectra revealed a good correlation with the composition used in the feed with deviations being always below 5%. The values obtained for every case are detailed in Table 2. Polymers 2017,9, 701 8 of 17 Polymers 2017, 9, 701 7 of 17 with the two well separate falls that are observed for alkylene succinate cycles. This is a very reasonable result since the weight losses displayed by c (BS) n and c (ES) n at temperatures in the 300–350 °C range are reported to be due to partial volatilization of the sample, a fact that is not expected to happen in the case of c (RF) n . Figure 3. Compared TGA analysis of cyclic oligomers. (a) TGA traces; (b) Derivative curves showing temperatures at which degradation takes place at maximum rate. 3.2. Synthesis of Copolyesters The synthesis of the copolyesters was performed by ED-ROP (Entropically-Driven Ring Opening Polymerization) in bulk using Sn(Oct)2 as catalyst. Two copolyesters series, i.e., coPBSxRFy and coPESxRFy, were prepared frommixtures of either c(BS)n or c(ES)n and c(RF)n at molar ratios ranging between 10% and 90%, in addition to the homopolyesters PBS, PES and PRF. Reaction temperatures above 190 °C were used to insure melting of the cycles. Preliminary assays indicated that reaction noticeably speeded when temperature was raised from 190 to 200 °C but not significant change in rate was observed when temperature was further increased, a behavior that was shared by the two series (Figure 4). According to these results, this was the temperature of choice applied for the synthesis of the whole collection of copolyesters. The evolution of the molecular weight of the forming polymer as a function of reaction time for several selected compositions is represented for the two series in Figure 5. An asymptotic trend was followed in all cases showing a notable decay in reaction rate after five hours when weight-average molecular weight values up to ~40,000 and ~50,000 g·mol−1 for PBS and PES copolyesters, respectively, were attained. Lower values, around 28,000–30,000 g mol-1 were indeed achieved when higher contents of RF were used. Figure 4. Evolution ofMwalong reaction time in the ROP of equimolar mixtures of c(RF)n and either c(BS)n (a) or c(ES)n (b) forthree different temperatures. 0 1 2 3 4 5 0 5 10 15 20 25 30 35 40 45 50 220 °C 200 °C 190 °C Mw (kg mol-1) time (h) a) 0 1 2 3 4 5 0 5 10 15 20 25 30 35 40 45 50 220 °C 200 °C 190 °C Mw(kg mol-1) time(h) b) 100 200 300 400 500 600 -2.5 -2.0 -1.5 -1.0 -0.5 0.0 c(BS)n c(ES)n c(RF)n Derivative remaining weight (% oC-1) Temperature(°C) b) 100 200 300 400 500 600 0 20 40 60 80 100 c(BS)n c(ES)n c(RF)n Remaining Weight (%) Temperature(°C) a) Figure 4. Evolution ofM w along reaction time in the ROP of equimolar mixtures of c(RF) n and either c(BS)n(a) or c(ES)n(b) forthree different temperatures. Polymers 2017, 9, 701 8 of 17 Interestingly, ROP proceeded faster as the content of the feed in c(RF)n diminished, which may be interpreted as due to the higher relative reactivity of the alkylene succinate cycles. An assay of polymerization in absence of catalyst showed not significant increase in molecular weight indicating that ROP was unable to proceed by exclusive action of heating. Figure 5. Evolution of Mw along reaction time in the ROP of mixtures of c(RF)n and either c(BS)n (a) or c(ES)n (b) for different feed compositions. The NMR analysis of the copolyesters ascertained the chemical constitution expected for them. 1H NMR spectra of coPBS50RF50 and coPES50RF50 are shown in Figure 6 as representative examples and the whole spectra collection for the two series is accessible in the SI file (Figures S1 and S2). The comonomer content in the copolyesters determined from the information provided by 1H NMR spectra revealed a good correlation with the composition used in the feed with deviations being always below 5%. The values obtained for every case are detailed in Table 2. Table 2. Resorcinol-containing Succinate-FuranoateCopolyesters Obtained by ROP. Opolyester Yield (%) GPC a Composition b x(BS or ES)/y(RF) Chain Microstructure c Mw (g·mol−1) Đ Feed Copolyester n(B/E)S n(B/E)F nRS nRF B PBS 90 50,000 1.9 100/- 100/- - - - - - coPBS90RF10 96 48,000 2.0 90/10 86/14 17.3 1.1 2.8 1.5 0.72 coPBS80RF20 95 46,000 1.8 80/20 78/22 7.2 1.2 3.8 1.4 0.89 coPBS70RF30 90 42,500 1.6 70/30 64/36 4.2 1.3 2.8 1.6 0.90 coPBS50RF50 80 37,200 2.0 50/50 49/51 2.3 1.9 2.1 1.9 0.96 coPBS40RF60 80 36,000 1.7 40/60 37/63 1.8 2.2 1.7 2.5 0.96 coPBS20RF80 85 32,200 1.8 20/80 21/79 1.5 3.2 1.3 3.9 0.92 PES 90 45,000 1.7 100/- 100/- - - - - - coPES90RF10 95 42,500 1.9 90/10 86/14 4.6 1.3 7.3 1.2 1.07 coPES80RF20 92 41,000 1.8 80/20 77/23 3.3 1.4 4.9 1.3 1.17 coPES70RF30 80 39,200 1.5 70/30 76/24 3.0 1.5 4.2 1.3 1.08 coPES50RF50 85 34,500 1.4 50/50 49/51 1.5 3.2 2.3 1.8 1.23 coPES40RF60 90 34,000 1.6 40/60 36/64 1.7 2.5 1.6 2.7 0.98 coPES20RF80 91 31,000 1.8 20/80 19/81 1.3 4.1 1.2 5.6 0.95 PRF 80 28,000 1.9 -/100 -/100 - - - - - a Molecular weight and dispersity measured by GPC. b Composition of the feed and the copolyester. c Number-average sequence length of the different sequences present in the copolyesters (see text) and randomness (B) determined by 13C NMR spectra using the equations reported by Devaux [31]. 0 1 2 3 4 5 0 10 20 30 40 50 60 70 80 PBS coPBS80RF20 coPBS50RF50 coPBS20RF80 PRF coPBS50RF50 (blank) Mw(kg mol-1) time(h) a) 0 1 2 3 4 5 0 10 20 30 40 50 60 70 80 PES coPES80RF20 coPES50RF50 coPES20RF80 PRF coPES50RF50(blank) Mw (kg mol-1) time (h) b) Figure 5. Evolution of M w along reaction time in the ROP of mixtures of c(RF) n and either c(BS) n ( a ) or c(ES)n(b) for different feed compositions. Table 2. Resorcinol-containing Succinate-FuranoateCopolyesters Obtained by ROP. Opolyester Yield (%) GPC aComposition bx(BS or ES)/y(RF) Chain Microstructure c Mw(g·mol−1)ĐFeed Copolyester n(B/E)S n(B/E)F nRS nRF B PBS 90 50,000 1.9 100/- 100/- - - - - - coPBS90RF10 96 48,000 2.0 90/10 86/14 17.3 1.1 2.8 1.5 0.72 coPBS80RF20 95 46,000 1.8 80/20 78/22 7.2 1.2 3.8 1.4 0.89 coPBS70RF30 90 42,500 1.6 70/30 64/36 4.2 1.3 2.8 1.6 0.90 coPBS50RF50 80 37,200 2.0 50/50 49/51 2.3 1.9 2.1 1.9 0.96 coPBS40RF60 80 36,000 1.7 40/60 37/63 1.8 2.2 1.7 2.5 0.96 coPBS20RF80 85 32,200 1.8 20/80 21/79 1.5 3.2 1.3 3.9 0.92 PES 90 45,000 1.7 100/- 100/- - - - - - coPES90RF10 95 42,500 1.9 90/10 86/14 4.6 1.3 7.3 1.2 1.07 coPES80RF20 92 41,000 1.8 80/20 77/23 3.3 1.4 4.9 1.3 1.17 coPES70RF30 80 39,200 1.5 70/30 76/24 3.0 1.5 4.2 1.3 1.08 coPES50RF50 85 34,500 1.4 50/50 49/51 1.5 3.2 2.3 1.8 1.23 coPES40RF60 90 34,000 1.6 40/60 36/64 1.7 2.5 1.6 2.7 0.98 coPES20RF80 91 31,000 1.8 20/80 19/81 1.3 4.1 1.2 5.6 0.95 PRF 80 28,000 1.9 -/100 -/100 - - - - - a Molecular weight and dispersity measured by GPC. b Composition of the feed and the copolyester. c Number-average sequence length of the different sequences present in the copolyesters (see text) and randomness (B) determined by 13C NMR spectra using the equations reported by Devaux [31]. Polymers 2017,9, 701 9 of 17 Polymers 2017, 9, 701 9 of 17 Figure 6. 1H NMR spectra of resorcinol-containing succinate-furanoatecopolyesters. (a) coPBS50RF50; (b) coPES50RF50. 3.3. Microstructure of the Copolyesters The number average sequence lengths (n) present in the copolyesters as well as their degrees of randomness (B) were determined by NMR. For this analysis we have applied the statistical model described by Devaux et al. [31] for polycondensates [S] = [B] or [S] = [E], and [F] = [R] and [BF] = [RS] or [EF] = [RS], for the two series. The number average sequence lengths (n) and the degree of randomness (B) were calculated using the following expressions: 𝑛𝐵𝑆 =[𝐵𝑆] [𝐵𝐹]+ 1, 𝑛𝐵𝐹 =[𝐵𝐹] [𝐵𝑆]+ 1, 𝑛𝑅𝑆 =[𝑅𝑆] [𝑅𝐹]+ 1, 𝑛𝑅𝐹 =[𝑅𝐹] [𝑅𝑆]+ 1 𝐵 = 1 𝑛𝐵𝑆 +1 𝑛𝑅𝐹 𝑛𝐸𝑆 =[𝐸𝑆] [𝐸𝐹]+ 1, 𝑛𝐸𝐹 =[𝐸𝐹] [𝐸𝑆]+ 1, 𝑛𝑅𝑆 =[𝑅𝑆] [𝑅𝐹]+ 1, 𝑛𝑅𝐹 =[𝑅𝐹] [𝑅𝑆]+ 1 𝐵 = 1 𝑛𝐸𝑆 +1 𝑛𝑅𝐹 where the dyads fractions were calculated from the integrals of the 13C NMR spectra, and assuming similar relaxation times for the same carbons in the different dyads. It was additionally assumed that in all triads the substitution on the left of a central unit does not influence the substitution on the right. The 13C NMR spectra of the coPBSxRFy series are shown in Figure 7 where it is seen that some of the signals split into four peaks due to the sensitivity of these carbons to sequence distribution at the level of triads. By deconvolution of these signals the content of the different dyads could be OO O OOO O ar br dr erfr OO beO OO O cr js kb bb 8 7 6 5 4 3 2 1 0 fr ar,be,br (ppm) er,dr js TMS CHCl3 cr coPES50RF50 b) a) ar,bb,br er,dr fr,cr js kb coPBS50RF50 CHCl3 TMS Figure 6. 1 H NMR spectra of resorcinol-containing succinate-furanoatecopolyesters. ( a )coPBS 50 RF 50 ; (b)coPES50RF50. 3.3. Microstructure of the Copolyesters The number average sequence lengths (n) present in the copolyesters as well as their degrees of randomness (B) were determined by NMR. For this analysis we have applied the statistical model described by Devaux et al. [31] for polycondensates [S] = [B] or [S] = [E], and [F] = [R] and [BF] = [RS] or [EF] = [RS], for the two series. The number average sequence lengths (n) and the degree of randomness (B) were calculated using the following expressions: nBS =[BS] [BF]+1, nBF =[BF] [BS]+1, nRS =[RS] [RF]+1, nRF =[RF] [RS]+1 B=1 nBS +1 nRF nES =[ES] [EF]+1, nEF =[EF] [ES]+1, nRS =[RS] [RF]+1, nRF =[RF] [RS]+1 B=1 nES +1 nRF where the dyads fractions were calculated from the integrals of the 13 C NMR spectra, and assuming similar relaxation times for the same carbons in the different dyads. It was additionally assumed that in all triads the substitution on the left of a central unit does not influence the substitution on the right. The 13 C NMR spectra of the coPBS x RF y series are shown in Figure 7where it is seen that some of the Polymers 2017,9, 701 16 of 17 References 1. Tsui, A.; Wright, Z.C.; Frank, C.W. Biodegradable polyesters from renewable resources. Annu. Rev. Chem. Biomol. 2013,4, 143–170. [CrossRef] [PubMed] 2. Zia, K.M.; Nooren, A.; Zuber, M.; Tabasum, S.; Mujahid, M. Recent developments and future prospects on bio-based polyesters derived from renewable resources: A review. Int. J. Biol. Macromol. 2015 ,82, 1028–1040. [CrossRef] [PubMed] 3. Bechthold, I.; Bretz, K.; Kabasci, S.; Kopitzky, R.; Springer, A. Succinic acid: A new platform chemical for bio-based polymers from renewable resources. Chem. Eng. Technol. 2008,31, 647–654. [CrossRef] 4. Werpy, T.; Petersen, G. Top Value Added Chemicals from Biomass Volume I: Results of Screening for Potential Candidates from Sugars and Synthesis Gas; Pacific Northwest National Laboratory (PNNL): Richland, WA, USA; National Renewable Energy Laboratory (NREL): Golden, CO, USA, 2004. Available online: http: //www.osti.gov/bridge (accessed on 12 October 2017). 5. Cooper, J.S.; Vigon, B. Life Cycle Engineering Guidelines; Chapter 5: New Design; EPA/600/R-01/101; National Risk Management Research Laboratory, Office of Research and Development: Cincinnati, OH, USA, 2001; pp. 51–52. 6. Wolf, O. (Ed.) Techno-Economic Feasibility of Large-Scale Production of Bio-Based Polymers in Europe; Technical Report EUR 22103 EN; Fraunhofer Institut: Munich, Germany, 2005. 7. Papageorgiou, G.Z.; Bikiaris, D.N. Crystallization and melting behavior of three biodegradable poly (alkylene succinates). A comparative study. Polymer 2005,46, 12081–12092. [CrossRef] 8. Bikiaris, D.N.; Achilias, D.S. Synthesis of poly(alkylene succinate) biodegradable polyesters, Part II: Mathematical modelling of the polycondensation reaction. Polymer 2008,49, 3677–3685. [CrossRef] 9. Gigli, M.; Fabbri, M.; Lotti, N.; Gamberini, R.; Rimini, B.; Munari, A. Poly(butylene succinate)-based polyesters. Eur. Polym. J. 2016,75, 431–460. [CrossRef] 10. Wojtczak, M.; Dutkiewicz, S.; Galeski, A.; Gutowska, A. Classification of aliphatic-butylene terephthalate copolyesters in relation to aliphatic/aromatic ratio. Polymer 2017,113, 119–134. [CrossRef] 11. Witt, U.; Muller, R.-J.; Deckwer, W.-D. Biodegradation of polyester copolymers containing aromatic compounds. J. Macromol. Sci. Pure Appl. Chem. 1995,A32, 851–856. [CrossRef] 12. Wu, L.; Mincheva, R.; Xu, Y.; Raquez, J.M.; Dubois, P. High Molecular Weight Poly(butylene succinate-co-butylene furandicarboxylate) Copolyesters: From Catalyzed Polycondensation Reaction to Thermomechanical Properties. Biomacromolecules 2012,13, 2973–2981. [CrossRef] [PubMed] 13. Jacquel, N.; Saint-Loup, R.; Pascault, J.P.; Rousseau, A.; Fenouillot, F. Synthesis and properties of poly(butylene succinate): Efficiency of different transesterification catalysts. Polymer 2015 ,59, 234–242. [CrossRef] 14. Morales-Huerta, J.C.; Ciulik, C.B.A.; Martínez de Ilarduya, A.; Muñoz-Guerra, S. Fully bio-based aromatic-aliphatic copolyesters: Poly(butylene furandicarboxylate-co-succinate)s obtained by ring opening polymerization. Polym. Chem. 2017,8, 748–760. [CrossRef] 15. Terzopoulou, Z.; Tsanaktsis, V.; Bikiaris, D.N.; Exarhopoulos, S.; Papageorgiou, D.G.; Papageorgiou, G.Z. Biobasedpoly(ethylene furanoate-co-ethylene succinate) copolyesters: Solid state structure, melting point depression and biodegradability. RSC Adv. 2016,6, 84003–84015. [CrossRef] 16. Gandini, A. Furans as offspring of sugars and polysaccharides and progenitors of a family of remarkable polymers: A review of recent progress. Polym. Chem. 2010,1, 245–251. [CrossRef] 17. Sousa, A.F.; Vilela, C.; Fonseca, A.C.; Matos, M.; Freire, C.S.; Gruter, G.J.M.; Coelho, J.F.J.; Silvestre, A.J.D. Biobased polyesters and other polymers from 2,5-furandicarboxylic acid: A tribute to furan excellency. Polym. Chem. 2015,6, 5961–5983. [CrossRef] 18. Papageorgiou, G.Z.; Papageorgiou, D.G.; Terzopoulou, Z.; Bikiaris, D.N. Production of bio-based 2,5-furan dicarboxylate polyesters: Recent progress and critical aspects in their synthesis and thermal properties. Eur. Polym. J. 2016,83, 202–229. [CrossRef] 19. Sanderson, K. US biofuels: A field in ferment. Nature 2006,444, 673–676. [CrossRef] [PubMed] 20. Rocha, L.; Marston, A.; Potterat, O.; Kaplan, M.A.C.; Hostettmann, K. More phloroglucinols from Hypericumbrasiliense. Phytochemistry 1996,42, 185–188. [CrossRef] 21. Hansen, C.A.; Frost, J.W. Deoxygenation of polyhydroxybenzenes: An alternative strategy for the benzene-free synthesis of aromatic chemicals. J. Am. Chem. Soc. 2002 ,124, 5926–5927. [CrossRef] [PubMed] Polymers 2017,9, 701 17 of 17 22. Durairaj, R.B. Resorcinol: Chemistry, Technology and Applications; Springer: Berlin, Germany, 2005. 23. Al-Muhtaseb, S.A.; Ritter, J.A. Preparation and properties of resorcinol-formaldehyde organic and carbon gels. Adv. Mat. 2003,15, 101–114. [CrossRef] 24. Vijayakumar, C.T.; Sivasamy, P.; Rajkumar, T. Synthesis and characterization of 1,3-bis (2-hydroxyethoxy) benzene based saturated and unsaturated polyesters. Eur. Polym. J. 2007,43, 3028–3035. [CrossRef] 25. Gioia, C.; Banella, M.B.; Vannini, M.; Celli, A.; Colonna, M.; Caretti, D. Resorcinol: A potentially bio-based building block for the preparation of sustainable polyesters. Eur. Polym. J. 2015,73, 38–49. [CrossRef] 26. Barbee, R.B.; Davis, B. Copolyesters from Ether-Containing Glycols and Acids. U.S. Patent 4518763, 21 May 1985. 27. Takahashi, K.; Nakamachi, K.; Niimi, H.; Hiraoka, S.; Sakai, M.; Tsuboi, H. Polyester Pellets and Proccess for Preparing the Same. Patent Application No. EP 0939095A2, 1 September 1999. 28. Brunelle, D.J.; Bradt, J.E.; Serth-Guzzo, J.; Takekoshi, T.; Evans, T.; Pearce, E.J.; Wilson, P. Semicrystalline polymers via ring-opening polymerization: Preparation and polymerization of alkylene phthalate cyclic oligomers. Macromolecules 1988,31, 4782–4790. [CrossRef] [PubMed] 29. Morales-Huerta, J.C.; Martínez de Ilarduya, A.; Muñoz-Guerra, S. A green strategy for the synthesis of poly(ethylene succinate) and its copolyesters via enzymatic ring opening polymerization. Eur. Polym. J. 2017 , 95, 514–519. [CrossRef] 30. Morales-Huerta, J.C.; Martínez de Ilarduya, A.; Muñoz-Guerra, S. Poly(alkylene 2,5-furandicarboxylate)s (PEF and PBF) by ring opening polymerization. Polymer 2016,87, 148–158. [CrossRef] 31. Devaux, J.; Godard, P.; Mercier, J.P. Bisphenol-A polycarbonate–poly(butylene terephthalate) transesterification. I. Theoretical study of the structure and of the degree of randomness in four-component copolycondensates. J. Polym. Sci. Polym. Phys. 1982,20, 1875–1880. [CrossRef] 32. Hodge, P. Entropically driven Ring-Opening Polymerization of strainless organic macrocycles. Chem. Rev. 2014,114, 2278–2312. [CrossRef] [PubMed] 33. Fox, T.G. Influence of diluent and of copolymer composition on the glass temperature of a polymer system. Bull. Am. Phys. Soc. 1956,1, 123–135. 34. Gordon, M.; Taylor, J.S. Ideal copolymers and the 2nd-ordertransitions of synthetic rubbers. 1. Non-crystalline copolymers. J. Appl. Chem. 1952,2, 493–500. [CrossRef] 35. Bikiaris, D.N.; Papageorgiou, G.Z.; Achilias, D.S. Synthesis and comparative biodegradability studies of three poly(alkylene succinate)s. Polym. Degrad. Stab. 2005,91, 31–43. [CrossRef] 36. Terzopoulou, Z.; Karakatsianopoulou, E.; Kasmi, N.; Tsanaktsis, V.; Nikolaidis, N.; Kostoglou, M.; Papageorgiou, G.Z.; Lambropoulou, D.A.; Bikiaris, D.N. Effect of catalyst type on molecular weight increase and coloration of poly(ethylene furanoate) biobased polyester during melt polycondensation. Polym. Chem. 2017,8, 6895–6908. [CrossRef] © 2017 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license (http://creativecommons.org/licenses/by/4.0/).