scieee AI-readable full text Open interactive document viewer

Smart hybrid nanomaterials for biomimetic membranes

Lopes Rodrigues, Maximilien

Abstract

This thesis focuses on the preparation of nanomaterials made of proteins and polymers. Even though the technology has advanced in the last decades to design new devices at the atomic scale, researchers are still inspired by what Nature has produced and optimized for millions of years. Following this concept, this work uses proteins forming water-filled channels, called porins, which regulate the flow of ions and biomolecules in cellular life. Two proteins were studied: Omp2a and VDAC36. The first part of the dissertation is the thermomechanical properties study of the latest hybrid membrane developed by the IMEM group: an thin nanoperforated poly(lactic acid) (PLA) film with the Omp2a porin immobilized onto the surface . For this purpose, a new equipment based on the microcantilever technology was used. The SCAnning LAser analyzer (SCALA) characterizes the coated cantilevers which allows the following of the cantilever bending induced by the compression/expansion of the sample coating (i.e. proteins or polymers). In this study, the intermolecular reorganization of Omp2a aggregates was evidenced as well as the protein secondary structure stability against temperature. The same method was employed to study the impact of nanofeatures (perforations and drugs domains) on films of PLA. They affected the glass transition and the cold crystallization temperatures. The changes were dependent on the size and abundance of the nanofeatures, which can modulate the properties of future materials. Moreover, this work established a protocol for the study of biomolecules and polymers attached to microcantilevers, allowing an accurate study of the thermomechanical properties using very low amounts of sample. The second part of the thesis is the development of new hybrid nanomaterials composed of VDAC36, PLA and poly(3,4-ethylenedioxythiophene) (PEDOT). An efficient protocol was established for the production of VDAC36 and its subsequent refolding was achieved. The beta-barrel nature of the protein was revealed and its tendency to form oligomers was demonstrated. Finally, the size of the protein inner channel could be determined. The VDAC36 was added to the polymer material made of three alternating layers of PLA and PEDOT. The electrical properties of the material were modified by the addition of the protein: the overall resistance was reduced and the supercapacitive behaviour was enhanced. The description of the electrical equivalent circuit also revealed that the protein induced the diffusion of ions. To improve the material, the number of layers was increased and the conducting polymer was modified by incorporating a monomer bearing a dodecyl chain. The modifications were proved useful as the protein content and the electrical properties increased. Finally, the new hybrid material could provide an adaptive electrical response according to the concentration of biomolecules.

Full text

Smart hybrid nanomaterials for biomimetic membranes by Maximilien Lopes Rodrigues ADVERTIMENT La consulta d’aquesta tesi queda condicionada a l’acceptació de les següents condicions d'ús: La difusió d’aquesta tesi per mitjà del r e p o s i t o r i i n s t i t u c i o n a l UPCommons (http://upcommons.upc.edu/tesis) i el repositori cooperatiu TDX ( h t t p : / / w w w . t d x . c a t / ) ha estat autoritzada pels titulars dels drets de propietat intel·lectual únicament per a usos privats emmarcats en activitats d’investigació i docència. No s’autoritza la seva reproducció amb finalitats de lucre ni la seva difusió i posada a disposició des d’un lloc aliè al servei UPCommons o TDX. No s’autoritza la presentació del seu contingut en una finestra o marc aliè a UPCommons (framing). Aquesta reserva de drets afecta tant al resum de presentació de la tesi com als seus continguts. En la utilització o cita de parts de la tesi és obligat indicar el nom de la persona autora. ADVERTENCIA La consulta de esta tesis queda condicionada a la aceptación de las siguientes condiciones de uso: La difusión de esta tesis por medio del repositorio institucional UPCommons (http://upcommons.upc.edu/tesis) y el repositorio cooperativo TDR (http://www.tdx.cat/?localeattribute=es) ha sido autorizada por los titulares de los derechos de propiedad intelectual únicamente para usos privados enmarcados en actividades de investigación y docencia. No se autoriza su reproducción con finalidades de lucro ni su difusión y puesta a disposición desde un sitio ajeno al servicio UPCommons No se autoriza la presentación de su contenido en una ventana o marco ajeno a UPCommons (framing). Esta reserva de derechos afecta tanto al resumen de presentación de la tesis como a sus contenidos. En la utilización o cita de partes de la tesis es obligado indicar el nombre de la persona autora. WARNING On having consulted this thesis you’re accepting the following use conditions: Spreading this thesis by the i n s t i t u t i o n a l r e p o s i t o r y UPCommons (http://upcommons.upc.edu/tesis) and the cooperative repository TDX (http://www.tdx.cat/?localeattribute=en) has been authorized by the titular of the intellectual property rights only for private uses placed in investigation and teaching activities. Reproduction with lucrative aims is not authorized neither its spreading nor availability from a site foreign to the UPCommons service. Introducing its content in a window or frame foreign to the UPCommons service is not authorized (framing). These rights affect to the presentation summary of the thesis as well as to its contents. In the using or citation of parts of the thesis it’s obliged to indicate the name of the author. Smart hybrid nanomaterials for biomimetic membranes Presented by Maximilien Lopes Rodrigues Supervised by Prof. Carlos Alemán Prof. Catherine Michaux Thesis submitted to obtain the degree Doctor of Philosophy in Polymers and Biopolymers Universitat Politècnica de Catalunya Barcelona, 2019 Department of Chemical Engineering Innovation in Material and Molecular Engineering (IMEM) I Summary The development of nanoscopic devices has pushed forward the possibilities in the fields of filtration, biosensing and nanofluidics. Combined with adapted materials such as biocompatible polymers, those innovative tools represent a promising technology for future biomedical applications. The main topic of this thesis is the preparation of nanomaterials made of proteins and polymers. Even though the technology has advanced in the last decades to design new devices at the atomic scale, researchers are still inspired by what Nature has produced and optimized for millions of years. Following this concept, this work uses membrane proteins forming water-filled channels which regulate the flow of ions, nutrients and biomolecules in cells. They act as the gates of the membranes and determine if a molecule passes or not. More specifically, the proteins involved in this project are the porins Omp2a and VDAC36. Omp2a is a 16-stranded β-barrel from the gram-negative bacterium Brucella melitensis. On the other hand, VDAC36 is a slightly larger barrel composed of 19 β-strands and located in mitochondria of Solanum tuberosum, a plant model. The following manuscript is divided in two main parts: 1) the thermomechanical study of proteins and polymers and 2) the development of a new hybrid nanomembrane. The first part investigates the thermomechanical properties of the latest hybrid membrane developed by the IMEM group: an ultra-thin nanoperforated poly(lactic acid) (PLA) film loaded with Omp2a. For this purpose, a new equipment based on the microcantilever technology was employed: the SCAnning LAser analyzer (SCALA). SCALA analyses the surface of coated cantilevers by reflecting a laser beam on it. The sample (and the cantilever) placed in a thermocontrolled chamber is warmed up/cooled down with high precision. It allows following the cantilever bending induced by the compression/expansion of the sample coating (i.e. proteins or polymers in our case). Using the aforementioned method, the intermolecular reorganization of Omp2a aggregates was evidenced as well as the protein secondary structure stability against temperature. The same method was employed to study the impact of nanofeatures on ultra-thin films of PLA. Nanopores, nanoperforations and nanodomains composed of organic drugs were added to the films. Those nanofeatures, by their size, abundance and location, affected the apparent glass transition and the cold crystallization temperatures. Those results suggest that the properties of future nanomaterials can be modulated by such treatments. Moreover, this work established a protocol for the study of biomolecules and polymers attached to microcantilevers, allowing an accurate analysis of the thermomechanical properties using very low amounts of sample. II The second part of the thesis is the development of a new hybrid nanomaterials composed of VDAC36, PLA and poly(3,4-ethylenedioxythiophene) (PEDOT). Contrary to Omp2a, no protocol was already established for VDAC36 production. For this purpose, the expression of the protein in bacteria and the subsequent purification by chromatography were optimized. Membrane proteins require a specific environment (i.e. amphiphilic) to retain their structure and activity. For this reason, a refolding step is necessary to recover its native form. The refolding was achieved using a protocol based on the combination of a detergent and a di-alcohol. The recovery of the secondary and tertiary structure was assessed by circular dichroism and intrinsic fluorescence, respectively. The formation of dimers and tetramers was then evidenced by cross-linking. Interestingly, the tetramers were degraded into dimers by a reducing agent, suggesting the involvement of an intermolecular disulphide bond. The protein was then reconstituted into lipid vesicles (i.e. liposomes) and the size of the channel was determined by swelling assay. After that, the polymer material was prepared. The assembly of PLA and PEDOT nanofilms was achieved to take profit of the promising PEDOT electrochemical properties and the mechanical integrity and robustness of PLA. The PLA layers were prepared by spin-coating and nanoperforated by solvent etching. It allowed the PEDOT to grow by electropolymerization through the perforations and cover the entire surface of the PLA. The PEDOT layer was then covered by a new layer of nanoperforated PLA. The protein was finally immobilized on the surface by solvent evaporation. Fluorescence, FTIR and XPS evidenced its presence in the material and microscopy studies the correct superposition of each polymer layer. Electrochemical impedance spectroscopy was performed to thoroughly describe the electrical properties of the new 3-layered material. The addition of VDAC36 into the material induced a decrease in its electrical resistance and enhanced its supercapacitive properties. Moreover, the complete description of the electrical equivalent circuit demonstrated the ion diffusion process induced by addition of the protein. Based on the previous results, a similar membrane was prepared using a mixture of EDOT and a modified EDOT monomer, containing an α-dodecyl chain instead of the ethylenedioxy group. The modification aimed to mimic the protein natural membrane made of lipids. Indeed, VDAC36, like all porins, has a high content of hydrophobic residues and may require a suitable matrix to maximize its activity. The mixture of both monomers could indeed successfully provide a higher content of retained proteins. An impedance study revealed again that the resistance was decreased and the supercapacitive properties enhanced after addition of the proteins. Finally, the biomaterial could detect biomolecules such as ATP and provide a response depending on the concentration of the electrolyte. III Acknowledgement This thesis is the result of the work of many people and only words will not be enough to express how I am grateful to all of them. I want to start to thank my supervisors who all had the patience to overview my work until the very end. Thank you Catherine Michaux for your daily support and all your investment during the entire thesis. No matter what happened, you continuously offered help and energy to move forward. Thank you Eric Perpète for sharing your scientific and life experiences and pushing me in the right direction. You hosted me in the best lab of the University of Namur since the master degree. You made me part of a solid group and I am very grateful for that. Thank you David Zanuy for all the help you offered me and for always being available. You provided me company, history lessons and showed me your strong vision of how Science should be. Thank you Carlos Alemàn for your leadership and very hard work. You always had a clear vision of the whole thesis and constantly could adapt to make it whole, designing new exciting projects and managing the entire laboratory without any flaw. Without you, my life would have been very different in many aspects and I am very grateful we could complete this thesis all together. During those years, I had the chance to meet tons of people that marked my mind. Probably few of them will read those lines. A heartfelt “thank you” to all of them for just being present and make this chapter of my life a rich human experience. Manu. this name resonates like a forgotten legend. Thank you for all the time spent together in the lab or anywhere else. You were definitely a pillar for me in Namur. Your wisdom, advises, nonsense talks, motivation to play cards really made my days. Thank you for being you. I wish every group had its own Manu. In the CPB lab, I am grateful I had the chance to meet Guillaume, Thibaut, Raphael, Boris, Maes, Stéphanie, Anaïs, Amaury, Djora, Romain, Victor, Nicolas, Laurène, Lauriane, Delphine, Fabiola, Simon. Some of them contributed to this thesis by helping me a lot in the lab. I hope you keep good memories of the time spent there. Thank you to the members of the other labs in Namur for sharing good moments all together. Bench, Coco, Thomas, Junior, Arvind, Andrea, Simon etc. I also acknowledge the labs URBM and URBE for training me and sharing their equipment with us. At the UPC, I had the chance to meet a lot of other students from all around the world. Thank you very much Anna, Brenda and Didac for your huge help and the funny moments we had in the lab. Ina and Hamidreza E. who form the amazing Best Team ever. Angelica, Guillem, Georgina, Hamidreza K., Reza, Amirmajid, Maryam, Jordi T., Jordi S., Guillem, Sonia, Maricruz, Neudys, Ludka, Lucas, Vitor, Ali and Omid, I will always keep the memories we have built as friends. Thank you Nicolas and Alex, for our weekly meetings making those helmets flying! Thank you Pit, Guillaume, Maxime and the whole Maxi-foot team for all those memories. Thank you Cinthia for showing me your determination, pushing me to the best version of myself and giving me motivation for all my actions. Papa, maman et Nina, merci infiniment pour tout ce que vous avez toujours fait pour moi. Votre regard me donnera toujours la force de continuer. IV Table of contents Summary .............................................................................................................................................. I Acknowledgement ............................................................................................................................. III Table of contents .............................................................................................................................. IV List of figures ................................................................................................................................... VII List of tables .................................................................................................................................... XII List of abbreviations ....................................................................................................................... XIII List of symbols ................................................................................................................................ XV 1. Introduction ...............................................................................................................................1 1.1. Motivation of the research ..................................................................................................1 1.2. Proteins, structure and function ..........................................................................................3 1.3. Polymers .............................................................................................................................6 1.4. State-of-the-art ...................................................................................................................7 1.5. Objectives ......................................................................................................................... 11 1.6. Methodology .................................................................................................................... 12 1.7. Bibliography ..................................................................................................................... 15 2. Thermomechanical response of Omp2a ................................................................................ 21 2.1. Introduction ...................................................................................................................... 22 2.2. Methods ............................................................................................................................ 24 2.3. Results and discussion ...................................................................................................... 28 Secondary structure and diameter ............................................................................................. 28 Time resolved WAXD data on heating and cooling of lyophilized Omp2a.............................. 33 Protein immobilization onto the surface of silicon microcantilevers ........................................ 35 Thermomechanical response of protein functionalized microcantilevers ................................. 40 2.4. Conclusion ....................................................................................................................... 49 2.5. Bibliography ..................................................................................................................... 50 3. Effect of nanofeatures on the thermal transitions of PLA films ......................................... 55 3.1. Introduction ...................................................................................................................... 56 3.2. Methods ............................................................................................................................ 58 3.3. Results and discussion ...................................................................................................... 62 Thermomechanical response of PLA and PVA ultra-thin films ............................................... 62 Thermomechanical response of nanopored and nanoperforated PLA ultra-thin films .............. 64 Thermomechanical response of PLA-drug ultra-thin films....................................................... 69 V 3.4. Conclusion ....................................................................................................................... 76 3.5. Bibliography ..................................................................................................................... 77 4. Structural and functional characterization of VDAC36 ...................................................... 83 4.1. Introduction ...................................................................................................................... 84 4.2. Methods ............................................................................................................................ 85 4.3. Results and discussion ...................................................................................................... 88 Expression, purification and refolding ...................................................................................... 88 Structural studies of stVDAC36: secondary and tertiary structure ........................................... 92 Oligomerization studies by cross-linking .................................................................................. 95 Functional studies: pore-forming activity ................................................................................. 98 Functional studies: ATP binding to plant VDAC ................................................................... 101 4.4. Conclusion ..................................................................................................................... 103 4.5. Bibliography ................................................................................................................... 104 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 ............................. 111 5.1. Introduction .................................................................................................................... 112 5.2. Methods .......................................................................................................................... 114 5.3. Results and discussion .................................................................................................... 118 Preparation and characterization of the 3-layered film ........................................................... 118 Immobilization of the protein into the 3-layered film ............................................................. 121 Influence of the protein on the film electrical response .......................................................... 128 5.4. Conclusion ..................................................................................................................... 131 5.5. Bibliography ................................................................................................................... 132 VI 6. Enhanced biomimetic membrane made of PLA, PEDOT-P3DT and VDAC36 ............. 137 6.1. Introduction .................................................................................................................... 138 6.2. Methods .......................................................................................................................... 140 6.3. Results and discussion .................................................................................................... 143 Characterization of COP and PEDOT ..................................................................................... 143 Free-standing 5-layered membranes ....................................................................................... 146 Functionalization of 5-layered membranes ............................................................................. 150 EIS measurement of 5-pPLA/COP/por biosensor ................................................................... 154 6.4. Conclusion ..................................................................................................................... 160 6.5. Bibliography ................................................................................................................... 161 7. Conclusion ............................................................................................................................. 169 7.1. Specific conclusions................................................................................................... 171 XIII List of abbreviations AFM Atomic force microscopy ATP Adenosine triphosphate BSA Bovine serum albumin CD Circular dichroism CP Conducting polymer CPB Physical Chemistry of Biomolecules DFDNB 1,5-difluoro-2,4-dinitrobenzene DMA dimethyl adipimidate DMS dimethyl suberimidate DNA Deoxyribonucleic acid DOPC 1,2-dioleoyl-sn-glycero-3-phosphocholine DLS Dynamic light scattering EIS Electrochemical impedance spectroscopy FTIR Fourier-transform infrared spectroscopy HFIP Hexafluoroisopropanol IMEM Innovation Material and Molecular Engineering IPTG β-D-1-thiogalactopyranoside LB Lysogeny broth LYS Lysozyme MPD 2-methyl-2,4-pentanediol NADH Nicotinamide adenine dinucleotide hydrogen NM Nanomembrane OMP Outer membrane protein PBS Phosphate-buffered saline PCR Polymerase Chain Reaction PDB Protein data bank XIV PEDOT Poly(3,4-ethylenedioxythiophene) PEG Poly(ethyleneglycol) PLA Poly(lactic acid) PNMPy Poly(N-methyl-pyrrole) PSD Positive sensitive detector PSS Poly(styrene sulfonate) PVA Poly(vinyl alcohol) SCALA Scanning Laser Analyzer SDS Sodium dodecyl sulfate SEM Scanning electron microscopy TEM Transmission electron microscopy TRP Tryptophan TYR Tyrosine VDAC Voltage dependent anion channel VMD Visual Molecular Dynamics WAXD Wide angle X-ray diffraction XPS X-ray photoelectron spectroscopy XV List of symbols Deff Effective diameter  Contact angle f/f Resonance frequency shift  Resonance frequency k Spring rigidity M Effective mass E Young modulus S Displacement of the laser on the detector z Deflection of the cantilever  Surface stress Tg Glass transition temperature Tcc Cold crystallization temperature λmax Maximum absorption wavelength Dpore Diameter of the protein pore RS Electrolyte resistance Rp Resistance of the film CPE3L Capacitance of a 3-layered film CPEst Capacitance of steel W Warburg impedance 1. Introduction 1. Introduction 1 1. Introduction 1.1. Motivation of the research The term nanotechnology was coined by Professor Taniguchi in 1974, defining the emerging field as “the processing of separation, consolidation and deformation of materials by one atom or one molecule” [1]. A broader conception of the now ubiquitous term refers to all components purposefully constructed at the nanoscale (i.e. one billionth of a meter) to fulfil a specific function. For systems at this scale, the manipulation of atoms and molecules is an intrinsic component of endeavours towards the dream of maximum accuracy. Implicit to this achievement is the equal necessity of precision while constructing the materials and the ingenuity to navigate around technological limitations such as instrument resolution. Nevertheless, scientists and engineers have developed numerous applications for a broad range of fields such as water purification, electronics, medicine, drug development or energy among many others [2–4]. Controlling the organization of molecules and atoms is far from an easy task. To circumvent this obstacle, researchers developed innovative methods to achieve their goal. Three different approaches to achieve the preparation of nanodevices are briefly described here (Figure 1.1). The first one, lithography, is a clever method to design the surface of a nanomaterial, especially in electronics [5]. Practically, a light or electron beam is directed towards a stencil that makes a pattern on the silicon surface. In that way, the irradiated atoms have a different reactivity which causes them to interact with other chemicals. Another method is to literally move or deposit the atom(s) on the surface of the material. Dip-pen patterning is achieved by using the very precise tip of an atomic force microscope (AFM) that can interact with one single atom or drop of solution [6]. Alternatively, self-assembling, in which a disordered system spontaneously turns into an organized structure, is commonly exploited to design nanostructure [7]. Taking advantage of the natural selforganization of matter, it permits a three-dimensional building compared to the above mentioned approaches. In a similar concept, taking directly profit of what the nature has built during millions of years can prove itself to be very efficient. Indeed, biomimetics stimulated the engineers and scientists during the last decades to design numerous technologies [8–10]. Planes, cars, trains, boats, adhesive surfaces, water filtration devices, ventilation systems are all technologies present in our daily life that were improved by learning from the nature. Biomimetics evolved from a simple imitation to an integration and combination of natural structures for the development of functional materials (Figure 1.2). The strategy consists in surveying the naturally occurring biological structures associated with the properties to be achieved by the new synthetic materials [11]. In all organisms, the proteins are present to ensure the vital functions. 1. Introduction 2 Figure 1.1: Schematic representation of three methods for designing nanomaterials. From top to bottom: Lithography, dip pen patterning and self-assembling. In this framework, nanomaterials based on proteins offer countless potential nanosized devices such as nanoreactors [12], filtration devices [13], nanosensors [14], or drug delivery systems [15-16]. Many of these applications usually require channel shaped components which provide nanoscopic pathways for the passage of molecules. Appropriately, a family of proteins, called porins, can naturally form channels. They undoubtedly are serious candidates for the development of new applications and deserve particular attention from any learned person willing to develop nanodevices. The general purpose of the present thesis is to build new nanomaterials based on the integration of channel forming proteins. 1. Introduction 3 Figure 1.2: Schematic representation of biomimetics with the integration of biological elements (proteins) in synthetic nanomaterials. 1.2. Proteins, structure and function Proteins are biological macromolecules synthesized by cells to ensure all functions of the organism. Each protein is composed of a specific combination of amino acids named primary structure and coded by a specific gene in the DNA. There are 20 natural amino-acids differing by their lateral chain. The length of proteins usually ranges from 100 to 1000 amino acids. This long chain folds itself into secondary structural elements such as α-helices or β-sheets (Figure 1.3). Those elements arrange themselves into a 3D tertiary structure, which exhibits specific features and shape ensuring the proper activity of the protein [17]. The process during which the protein acquires its correct tertiary structure is called (re)folding. Protein’s structure is affected by the physicochemical conditions of the medium. If the latter fails to provide a suitable environment, the protein will lose its conformation and stay reversibly inactive. In some cases, multiples identical proteins gather to form an oligomer representing the quaternary structure. While the amino acids are covalently bonded, the tertiary structure is mainly stabilized by hydrogen bonds. Proteins have utility in a wide range of processes like structural purposes, performing and controlling chemical reactions or transporting ions and molecules [18]. Besides, proteins can be divided into two mains categories: soluble and membrane. The first category is composed of proteins soluble in water and, usually, they spontaneously adopt their active conformation. On the contrary, membrane proteins are not soluble in water. They are located in lipid bilayers that provide an amphiphilic environment that matches the hydrophobicity of the membrane protein. 1. Introduction 4 Figure 1.3: Structure of an amino acid and the peptide bond. Representation of the four levels of structures in proteins [17]. The function of transport is of particular interest in the design of nanoapplications. The type of transport in which this thesis is focused implies the move of molecules or ions across the biological membrane (lipid bilayer). The latter is impermeable to water or any hydrophilic molecule and protect the cell from its external environment [19]. To allow the passage of molecules from any side to the other, transport proteins are disseminated along the membrane. They act as the gates of the membrane and determine if a molecule passes or not. The solutes may be transported in two ways: actively and passively (Figure 1.4). The active way, performed by carrier proteins, is assimilated to a pump which transports the solutes from a low concentration to a high concentration environment. Because this is thermodynamically unfavourable, the process requires the use of energy, usually by ATP hydrolysis to modify the conformation of the protein. On the other hand, the passive transport does not use energy and solutes follow the concentration gradient. The proteins responsible of passive diffusion have a tertiary structure forming a channel [20]. Because of their location in the outer membrane of gram-negative bacteria or mitochondria, they are often referred as “outer membrane protein” (OMP). They generally adopt a barrel structure composed of anti-parallel βstrands, hence the name β-barrel (Figure 1.5) [21]. Some α-helices structure can also form channels, such as aquaporins [22]. 1. Introduction 11 1.5. Objectives The present thesis hypothesizes that the combination of rationally selected polymers with β-barrel proteins could lead to the development of bionanosensors. The electrical response of such nanodevices would depend on the solutes crossing the protein channel towards the responsive polymer. The main objective is to prepare a new nanomaterial including the protein VDAC36, a porin that forms a water-filled channel and presents a voltage-gating ability. The polymers retained as the material’s support are a well-known conducting polymer, PEDOT, and PLA. PEDOT provides the electrical conductivity necessary for accurate sensing while PLA offers the robustness needed for a stable free-standing material. By combining the assets of the three components, the project aims at developing an innovative responsive nanobiosensor. A side objective of this thesis is to understand better the features of the latest hybrid nanomaterial designed by the IMEM group. More specifically, it involves the study of the thermomechanical properties of the Omp2a porin and nanomodified poly(lactic acid) (PLA) films by using an innovative microcantilever technology. To achieve the first objective, the next steps were followed:  Produce and purify the VDAC36 protein  Refold the VDAC36 using the sodium dodecyl sulfate (SDS) - 2-methyl-2,4-pentanediol (MPD) method  Characterize VDAC36 and determine its pore size  Optimize the assembling of PEDOT and PLA  Insert VDAC36 into the polymer film  Characterize the film and verify the insertion of the protein  Study the electrical properties of the hybrid material by electrochemical impedance spectroscopy Likewise, to accomplish the second objective the next steps were followed:  Produce and purify the Omp2a protein  Refold the Omp2a using the SDS-MPD method  Study the effect of temperature on Omp2a using standard spectroscopic techniques  Develop and optimize the fixation of Omp2a and PLA on microcantilevers  Analyze the thermomechanical properties of Omp2a and PLA with the Scanning Laser Analyzer (SCALA) 1. Introduction 12 1.6. Methodology The present work involves the utilization of polymers and channel proteins and their combination for the preparation of hybrid nanofilms with enhanced ion transport activity. As a result of their structural relevance for the design of nanomaterials, the transport proteins Omp2a and VDAC proteins were selected. Omp2a is located in the gram-negative bacterium Brucella responsible of the Brucellosis, a zoonotic infection affecting mammals [37]. The protein is composed of 367 amino acids for a total molecular weight of 39 kDa and it assembles into a trimer. Previous functional studies revealed the transport function of the protein and further topology prediction showed its β-barrel structure [38]. The barrel is made of 16 antiparallel β-strands separated by short turns on the intracellular side and longs loops on the extracellular side. The third loop, the longest, folds inside the barrel to form an α-helix constricting the channel. The minimum diameter of the inner channel of 0.74 nm allows molecules such as sugar (e.g. maltotetraose) to pass through the pore [39]. The model we have developed shows that the loops carry an excess of negative charges while the inner part of the channel is mainly positively charged [24]. Moreover, two pathways have been identified for the ions transport. This supports the preferential diffusion of some ions observed after integration of Omp2a into poly(pyrrole) and poly(lactic acid) nanomembranes [34-36]. VDAC36, for voltage-dependent anion channel, is a plant pore-forming protein found in the outer mitochondrial membrane of Solanum tuberosum [40]. It contains 277 amino acids for a total weight of 30 kDa. The function of VDAC proteins is associated with the permeability of the mitochondria. Specifically, they regulate the diffusion of ions and metabolites such as nicotinamide adenine dinucleotide hydrogen (NADH) or adenosine triphosphate (ATP). VDAC proteins adopt a β-barrel structure composed of 19 antiparallel β-strands. This conformation forms an inner channel restricted by an α-helix at the N-terminal extremity that folds into the pore [41]. The strands are separated by short turns on both sides of the protein, making the pore more accessible than the one of Omp2a. The diameter of the channel is about 2.0 nm allowing large molecules to pass through it [42]. Interestingly, VDAC proteins have a gating ability. Depending the electric potential, the inner αhelix undergoes conformational changes and the channel can switch from an open to a closed-state or vice-versa [43]. This feature is very promising for the development of smart bionanomaterials with controlled diffusion. Regarding the matrix containing the channel proteins, PLA was chosen for its ability to be stable and free-standing as demonstrated in the previous works. Moreover, it is possible to obtain size- 1. Introduction 13 controlled nanoperforations across the film and to select its thickness and shape [44]. Another polymer, PEDOT, was also considered for this study. It is a CP with supercapacitive properties promising for the development of sensors with tuneable electric response [45]. Both PLA and PEDOT are non-cytotoxic and their synergetic combination could lead to electroactive free-standing nanomaterials with potential biomedical applications. The methodology followed to complete the study was divided into three tasks described below. Task 1: Protein production In order to perform the numerous analyses along this project, an appropriate quantity of protein is needed. When it comes to the production of transport proteins, as with all membrane proteins, the process is considered as challenging [46]. Indeed, their over-expression in bacteria often results in the formation of biologically inactive aggregates called inclusion bodies, which are incompetent elements for any meaningful structural or functional study [47]. Still, the over-expression in inclusion bodies can present several advantages compared to classical expression. First, it is less stressful for host bacteria and the produced proteins are less prone to degradation and high expression levels can be reached [48]. For those reasons, the selected proteins are produced in E. coli bacteria in inclusion bodies. Task 2: Purification and refolding of the protein The produced proteins are obtained in an inactive (i.e. unfolded) and impure form. They were therefore purified by fast protein liquid chromatography. The aforementioned requirement of membrane proteins to be surrounded by an amphiphilic medium to remain active makes their refolding difficult. Nevertheless, the CPB group for the University of Namur has demonstrated the reliability of an original protein refolding procedure, based on the synergistic association of the SDS anionic detergent with a diol-type organic cosolvent, the MPD [49-50]. This method has been extensively applied to various proteins such as β-barrel structures. The protocol simplicity and low economic costs make it a serious asset for the acquisition of active channel proteins. To characterize the proteins, diverse techniques are employed such as circular dichroism (CD), fluorescence, UV- vis absorbance to name a few. Functionality tests and oligomer formation studies are carried in order to understand better the channel properties and its tendency to aggregate. 1. Introduction 14 Task 3: Polymers preparation and protein integration The crucial step of this work is to prepare a suitable nanofilm that welcomes the active channel protein. PLA has proved itself to be able to host the protein but lacks the electroactivity that PEDOT provides. Stacking layers of PLA and PEDOT seems to be a smart option to combine the features of the two polymers. PLA nanomembranes are prepared by spin-coating a mixture of PLA and PVA. By selective solvent etching, the PVA is dissolved causing the formation of nanoperforations ready to receive the proteins. PEDOT is directly polymerized onto the underlying PLA layer. The process is repeated to create the final film. Then, the protein is immobilized in the PLA nanoperforations by deposition and solvent evaporation. The hybrid nanofilms are then characterized by an array of techniques (including electron and atomic force microscopies (SEM and AFM)) to assess their morphology at the nanoscale. The insertion of the protein is verified by X-ray photoelectron spectroscopy (XPS) and FTIR spectroscopy. Electrochemical impedance spectroscopy (EIS) is finally employed to study the response of the material with different solutes. 1. Introduction 15 1.7. Bibliography [1] A. Sandhu, “Who invented nano?,” Nat. Nanotechnol., 1, 2, 87–87, 2006. [2] S. A. Edwards, The nanotech pioneers : where are they taking us? Wiley-VCH, 2006. [3] J. Jeevanandam, A. Barhoum, Y. S. Chan, A. Dufresne, and M. K. Danquah, “Review on nanoparticles and nanostructured materials: history, sources, toxicity and regulations,” Beilstein J. Nanotechnol., 9, 1, 1050–1074, 2018. [4] V. Prakash Sharma, U. Sharma, M. Chattopadhyay, and V. N. Shukla, “Advance Applications of Nanomaterials: A Review,” Mater. Today Proc., 5, 2, 6376–6380, 2018. [5] J. E. E. Baglin, “Ion beam nanoscale fabrication and lithography—A review,” Appl. Surf. Sci., 258, 9, 4103–4111, 2012. [6] Y.-S. Choi, X. Wu, and D.-W. Lee, “Selective nano-patterning of graphene using a heated atomic force microscope tip,” Rev. Sci. Instrum., 85, 4, 045002, 2014. [7] H. Wang, L. Li, H.-W. An, B. Peng, and R. Zheng, “Self-Assembled Nanomaterials: Design Principle, Nanostructural Effect, Functional Mechanism as Antimicrobial or Detection Agent,” Mater. Horizons, 2019. [8] C. Sanchez, H. Arribart, and M. M. Giraud Guille, “Biomimetism and bioinspiration as tools for the design of innovative materials and systems,” Nat. Mater., 4, 4, 277–288, 2005. [9] J. Hwang, Y. Jeong, J. M. Park, K. H. Lee, J. W. Hong, and J. Choi, “Biomimetics: forecasting the future of science, engineering, and medicine,” Int. J. Nanomedicine, 10, 5701, 2015. [10] J. F. V Vincent, “Biomimetics — a review,” Proc. Inst. Mech. Eng. Part H J. Eng. Med., 223, 8, 919–939, 2009. [11] F. Baneyx, “Review of Biomimetic and Bioinspired Nanomaterials Biomimetic and Bioinspired Nanomaterials . Edited by Challa S. S. R.Kumar (Louisiana State University, Baton Rouge, LA). WILEY-VCH Verlag GmbH & Co KGaA : Weinheim . 2010 . xxii + 564 pp. $205.00. ISBN 978-3-527-32167-4 .,” J. Am. Chem. Soc., 133, 13, 5161–5161, 2011. [12] Dennis M. Vriezema, Marta Comellas Aragonès, Johannes A. A. W. Elemans, Jeroen J. L. M. Cornelissen, and Alan E. Rowan, and R. J. M. Nolte*, “Self-Assembled Nanoreactors,” 2005. [13] J. R. Werber, C. O. Osuji, and M. Elimelech, “Materials for next-generation desalination and water purification membranes,” Nat. Rev. Mater., 1, 5, 16018, 2016. [14] Y.-R. Kim, S. Jung, H. Ryu, Y.-E. Yoo, S. M. Kim, and T.-J. Jeon, “Synthetic biomimetic membranes and their sensor applications.,” Sensors (Basel)., 12, 7, 9530–50, 2012. [15] S. Majd, E. C. Yusko, Y. N. Billeh, M. X. Macrae, J. Yang, and M. Mayer, “Applications of biological pores in nanomedicine, sensing, and nanoelectronics,” Curr. Opin. Biotechnol., 21, 4, 439–476, 2010. [16] S. Mura, J. Nicolas, and P. Couvreur, “Stimuli-responsive nanocarriers for drug delivery,” Nat. Mater., 12, 11, 991–1003, 2013. [17] I. Rehman and S. Botelho, Biochemistry, Tertiary Structure, Protein. StatPearls Publishing, 2019. [18] C. A. Ouzounis, R. M. R. Coulson, A. J. Enright, V. Kunin, and J. B. Pereira-Leal, “Classification schemes for protein structure and function,” Nat. Rev. Genet., 4, 7, 508–519, 2003. [19] A. M. Seddon, P. Curnow, and P. J. Booth, “Membrane proteins, lipids and detergents: Not just a soap opera,” Biochim. Biophys. Acta - Biomembr., 1666, 1–2, 105–117, 2004. [20] J.-M. Pagès, C. E. James, and M. Winterhalter, “The porin and the permeating antibiotic: a selective diffusion barrier in Gram-negative bacteria.,” Nat. Rev. Microbiol., 6, 12, 893– 903, 2008. [21] V. a Feher, A. Randall, P. Baldi, R. M. Bush, L. M. de la Maza, and R. E. Amaro, “A 3- 1. Introduction 16 dimensional trimeric β-barrel model for Chlamydia MOMP contains conserved and novel elements of Gram-negative bacterial porins.,” PLoS One, 8, 7, e68934, 2013. [22] W. Xie, F. He, B. Wang, T.-S. Chung, K. Jeyaseelan, A. Armugam, and Y. W. Tong, “An aquaporin-based vesicle-embedded polymeric membrane for low energy water filtration,” J. Mater. Chem. A, 1, 26, 7592, 2013. [23] J. H. Kleinschmidt, “Folding and Stability of Monomeric β-Barrel Membrane Proteins,” in Protein-Lipid Interactions, Weinheim, FRG: Wiley-VCH Verlag GmbH & Co. KGaA, 2006, 27–56. [24] M. Lopes-Rodrigues, D. Zanuy, C. Alemán, C. Michaux, and E. A. Perpète, “3D structure of a Brucella melitensis porin: molecular modelling in lipid membranes,” J. Biomol. Struct. Dyn., 1–13, 2018. [25] F. Seidi, R. Jenjob, and D. Crespy, “Designing Smart Polymer Conjugates for Controlled Release of Payloads,” Chem. Rev., 118, 7, 3965–4036, 2018. [26] M. Kumar, J. E. O. Habel, Y. X. Shen, W. P. Meier, and T. Walz, “High-density reconstitution of functional water channels into vesicular and planar block copolymer membranes,” J. Am. Chem. Soc., 134, 45, 18631–18637, 2012. [27] S. Balme, J.-M. Janot, L. Berardo, F. Henn, D. Bonhenry, S. Kraszewski, F. Picaud, and C. Ramseyer, “New Bioinspired Membrane Made of a Biological Ion Channel Confined into the Cylindrical Nanopore of a Solid-State Polymer.,” Nano Lett., 11, 2, 712–716, 2011. [28] A. Güven, M. Fioroni, B. Hauer, and U. Schwaneberg, “Molecular understanding of sterically controlled compound release through an engineered channel protein (FhuA).,” J. Nanobiotechnology, 8, 14, 2010. [29] N. Muhammad, T. Dworeck, M. Fioroni, and U. Schwaneberg, “Engineering of the E. coli Outer Membrane Protein FhuA to overcome the Hydrophobic Mismatch in Thick Polymeric Membranes,” J. Nanobiotechnology, 9, 1, 8, 2011. [30] C. Nardin, J. Widmer, M. Winterhalter, and W. Meier, “Amphiphilic block copolymer nanocontainers as bioreactors,” Eur. Phys. J. E, 4, 4, 403–410, 2001. [31] A. Ranquin, W. Versées, W. Meier, J. Steyaert, and P. Van Gelder, “Therapeutic Nanoreactors: Combining Chemistry and Biology in a Novel Triblock Copolymer Drug Delivery System,” Nano Lett., 5, 11, 2220–2224, 2005. [32] A. Onoda, K. Fukumoto, M. Arlt, M. Bocola, U. Schwaneberg, and T. Hayashi, “A rhodium complex-linked β-barrel protein as a hybrid biocatalyst for phenylacetylene polymerization,” Chem. Commun., 48, 78, 9756, 2012. [33] N. Misra, J. A. Martinez, S.-C. J. Huang, Y. Wang, P. Stroeve, C. P. Grigoropoulos, and A. Noy, “Bioelectronic silicon nanowire devices using functional membrane proteins.,” Proc. Natl. Acad. Sci. U. S. A., 106, 33, 13780–4, 2009. [34] M. M. Pérez-Madrigal, L. J. del Valle, E. Armelin, C. Michaux, G. Roussel, E. A. Perpète, and C. Alemán, “Polypyrrole-Supported Membrane Proteins for Bio-Inspired Ion Channels,” ACS Appl. Mater. Interfaces, 7, 3, 1632–1643, 2015. [35] D. T. McQuade, A. E. Pullen, and T. M. Swager, “Conjugated polymer-based chemical sensors.,” Chem. Rev., 100, 7, 2537–74, 2000. [36] A. Puiggalí-jou, M. M. Pérez-madrigal, L. J. del Valle, E. Armelin, M. T. Casas, C. Michaux, E. A. Perpète, F. Estrany, C. Alemán, L. J. Valle, E. Armelin, M. T. Casas, C. Michaux, E. A. Perpète, F. Estrany, and C. Alemán, “Confinement of a β-barrel protein in nanoperforated free-standing nanomembranes for ion transport,” Nanoscale, 8, 38, 16922– 16935, 2016. [37] G. Pappas, P. Papadimitriou, N. Akritidis, L. Christou, and E. V Tsianos, “The new global map of human brucellosis,” 6, February, 91–99, 2006. [38] J. Y. Paquet, M. A. Diaz, S. Genevrois, M. Grayon, J. M. Verger, X. De Bolle, J. H. Lakey, J. J. Letesson, and A. Cloeckaert, “Molecular, antigenic, and functional analyses of Omp2b 1. Introduction 17 porin size variants of Brucella spp.,” J. Bacteriol., 183, 16, 4839–4847, 2001. [39] J. Y. Paquet, C. Vinals, J. Wouters, J. J. Letesson, and E. Depiereux, “Topology prediction of Brucella abortus Omp2b and Omp2a porins after critical assessment of transmembrane beta strands prediction by several secondary structure prediction methods.,” J. Biomol. Struct. Dyn., 17, October 2014, 747–757, 2000. [40] T. Salinas, S. El Farouk-Ameqrane, E. Ubrig, C. Sauter, A.-M. M. Duchêne, and L. Maréchal-Drouard, “Molecular basis for the differential interaction of plant mitochondrial VDAC proteins with tRNAs,” Nucleic Acids Res., 42, 15, 9937–9948, 2014. [41] S. Hiller, R. G. Garces, T. J. Malia, V. Y. Orekhov, M. Colombini, and G. Wagner, “Solution Structure of the Integral Human Membrane Protein VDAC-1 in Detergent Micelles,” Science (80-. )., 321, 5893, 1206–1210, 2008. [42] M. Colombini, “The VDAC channel: Molecular basis for selectivity,” Biochim. Biophys. Acta - Mol. Cell Res., 1863, 10, 2498–2502, 2016. [43] H. Rui, K. Il Lee, R. W. Pastor, and W. Im, “Molecular dynamics studies of ion permeation in VDAC,” Biophys. J., 100, 3, 602–610, 2011. [44] A. Puiggalí-Jou, J. Medina, L. J. del Valle, and C. Alemán, “Nanoperforations in poly(lactic acid) free-standing nanomembranes to promote interactions with cell filopodia,” Eur. Polym. J., 75, 552–564, 2016. [45] J. Bobacka, A. Lewenstam, and A. Ivaska, “Electrochemical impedance spectroscopy of oxidized poly(3,4-ethylenedioxythiophene) film electrodes in aqueous solutions,” J. Electroanal. Chem., 489, 1–2, 17–27, 2000. [46] F. Junge, B. Schneider, S. Reckel, D. Schwarz, V. Dötsch, and F. Bernhard, “Large-scale production of functional membrane proteins.,” Cell. Mol. Life Sci., 65, 11, 1729–55, 2008. [47] E. D. Clark, “Protein refolding for industrial processes.,” Curr. Opin. Biotechnol., 12, 2, 202–7, 2001. [48] R. Laage and D. Langosch, “Strategies for prokaryotic expression of eukaryotic membrane proteins.,” Traffic, 2, 2, 99–104, 2001. [49] C. Michaux, N. C. Pomroy, and G. G. Privé, “Refolding SDS-Denatured Proteins by the Addition of Amphipathic Cosolvents,” J. Mol. Biol., 375, 5, 1477–1488, 2008. [50] C. Michaux, G. Roussel, M. Lopes-Rodrigues, A. Matagne, and E. A. Perpète, “Unravelling the mechanisms of a protein refolding process based on the association of detergents and cosolvents,” J. Pept. Sci., March, 485–491, 2016. 2. Thermomechanical response of Omp2a 2. Thermomechanical response of Omp2a 27 and the automated two-dimensional scanning of a single layer beam by voice-coil actuators. The equipment has been implemented with a thermal chamber containing a thermoelectric cooler and a cartridge heater. These elements are capable of sweeping the chamber’s temperature from –50°C up to 220°C by flowing thermostatized N2 to the sample. A holder containing multiple thermometer probes is placed inside the chamber for a better mapping of the temperature. All measurements were performed in nitrogen environment. The temperature control was regulated by software created by the MecWins Company. Monocrystalline Si microcantilever chips containing arrays of eight cantilevers (Micromotive GmbH) were used for the measurements. Specifically, the nominal length, width, and thickness of the cantilevers were 500, 90±2 and 1 μm, respectively. Resonance frequency measurements were conducted in a nitrogen atmosphere at 25°C. The experimental setup is based on the shift induced in the resonance frequency by the added mass onto the cantilever through functionalization. The used platform consists in the automated two-dimensional scanning with a single laser (1 mW) beam by voice-coil actuators perpendicularly located. The cantilever array is illuminated by the laser beam and a two-dimensional linear position detector (PSD) is arranged to collect the reflected beams. Location and characterization of cantilever sensors is carried out using TRACKER, an algorithm based on the recognition of reflected intensity patterns. This capability of SCALA allows the user to characterize a single sensor or an array of them in a fully automated process. A change in the local slope at the cantilever surface results into a displacement of the reflected laser spot on the PSD, which is denoted S. S is used to obtain the cantilever profile along its longitudinal axis, z(x), by integrating:  cos 4 1 ')'( 2 1 )( 0 2 x D x dxxS D xz (1) where D is the distance between the cantilever and the PSD and β is the angle between the incident laser beam and the cantilever normal at its rest position. Coated cantilevers can be used as precise thermometers by exploiting the bimaterial effect, which refers to the measurable bending (i.e. differential stress) produced by temperature changes in substrates coated on one side by another material. Similarly, coated microcantilevers undergo a deflection as a result of temperature changes due to the thermal expansion coefficient difference between the coating material of the cantilever and the cantilever itself. 2. Thermomechanical response of Omp2a 28 2.3. Results and discussion The response of Omp2a to thermal stress has been compared with those of BSA and LYS. LYS exhibits an ellipsoidal shape in which both ordered (30% -helix, 27% turn and 13% -sheet secondary structures) and unordered (30%) regions coexist [27], while BSA structure is predominantly -helical with the remaining polypeptide occurring in turns and loops (i.e. no -sheet content) [28]. Omp2a has a cylindrical shape composed of β-strands separated by long unfolded loops [29]. Although the secondary structure of bacterial β-barrels is known to be sensitive to the polarity of the environment, they exhibit an increased thermal stability that has been typically attributed not only to the abundant -strands barrel but also to their oligomeric architectures [30– 33]. However, complete understanding of the thermal response of their supramolecular oligomeric architectures in synthetic environments, which is essential for the utilization of β-barrels in the fabrication of bioinspired nanodevices, is an unresolved question [34]. Before nanomechanical measurements, the effects of the heat shift on the secondary structure and aggregation tendency of the three proteins have been examined. Secondary structure and diameter Temperature-induced protein denaturation is frequently detected using FTIR spectroscopy and Circular Dichroism in various wavelength regimes. The vibrational spectrum in FTIR is selective in the absorption band frequency position, widths, and intensities in response to protein structural changes [35]. Specifically, the amide I band (1700 – 1600 cm-1), which convolutes the major structural domain elements of proteins, including -helix, -sheet, turn and random coil (unstructured), has been used to visualize the response of BSA, LYS and Omp2a to heating. Circular Dichroism monitors the secondary structure of proteins. In CD, folded proteins have typical spectra for each secondary structure: the -helix recognized by minima at 220 and 210 nm, while the -sheet has a minimum at 218 nm and a maximum at 195 nm [36]. These two structural motifs are detected in the spectra recorded for LYS and Omp2a at room temperature, whereas the spectrum of BSA mainly involves the helical motif. CD (Figure 2.1) and FTIR (Figure 2.2) spectra were recorded in heating runs from 5ºC to 90ºC and reflect an increment of the disordered motifs at temperatures higher than 55ºC for both BSA and LYS. Meanwhile, the content of ordered secondary structures, especially -helix, decreases. The unfolding temperature estimated from CD results is 67ºC and 65ºC for BSA and LYS, respectively. These results are fully consistent with those early reported in previous studies in aqueous solution [37-38]. Specifically, the studies concluded that the proteins lose a small part of helical structures in the -domain below 64ºC, undergoing irreversible (unless cooling start before reaching 75ºC) 2. Thermomechanical response of Omp2a 29 thermal unfolding of the secondary structures at a temperature close to 75°C. On the other hand, Omp2a only exhibits slight variations in its secondary structures, the amount of unstructured content remaining practically constant from 5°C to 90ºC. Moreover, the thermal behavior of the three proteins is reversible, as is evidenced from the analyses of the CD spectra recorded in cooling runs (Figure 2.3). Figure 2.1: CD spectra recorded for BSA, LYS and Omp2a proteins at temperatures ranging from 5°C to 90°C (heating runs). Measurements for BSA and LYS were performed using a carbonate buffer, whereas a dodecyl sulfate (SDS) – 2-methyl-2,4-pentanediol (MPD) buffer was used for Omp2a. 2. Thermomechanical response of Omp2a 30 Figure 2.2: FTIR spectra in the region of amide I of (A) BSA, (B) LYS and (C) Omp2a at 30 ºC and 100 ºC (left and right, respectively). The deconvolution of the amide I absorption band is displayed in all cases. 2. Thermomechanical response of Omp2a 31 Figure 2.3: Secondary structure content of BSA, LYS and Omp2a obtained by deconvolution of the CD spectra for heating and cooling runs. The FTIR and CD results of Omp2a prove that the efficient inter-strand hydrogen bond network preserves the protein secondary structure from thermal unfolding even outside the natural lipid environments. The heat-induced evolution of secondary structures in Omp2a has also been compared with conventional soluble proteins. The structural signatures of BSA and LYS significantly change beyond 55ºC, evidencing the loss of secondary structure [39], while the CD spectrum of Omp2a remains practically unaltered until 90°C. At high temperature both BSA and LYS underwent a drastic unfolding, as is reflected by the apparition of an intense deconvoluted peak at 1640 cm-1 in FTIR that has been associated to the unstructured protein. In contrast, the resemblance between all spectra recorded for Omp2a suggests that the -barrel structure is preserved even at high temperatures. The influence of the temperature in the shape and aggregation of the proteins was also assessed by Dynamic Light Scattering (DLS). Profiles displaying the variation of the particle effective diameter (Deff) with the temperature are included in Figure 2.4 (both heating and cooling runs). Bimodal distributions were found for BSA at all examined temperatures and, therefore, two Deff profiles are displayed in Figure 2.4. In the first mode, which corresponds to individual BSA molecules, Deff 2. Thermomechanical response of Omp2a 32 grows from 8.1  1.4 nm at 20°C to 10.7  1.4 nm at 60°C, evidencing that the unfolding process is accompanied by an increment of the molecular dimension. The lowest value, 8.1  1.4 nm at 20°C, which is consistent with the dimensions of the prolate ellipsoid shape proposed for the protein monomer [40], increases by 30% with the temperature, due to the unfolding. The Deff values of the second mode are approximately three times higher than the first one, indicating that BSA potentially forms trimers. In this case, Deff increases from 23  4 nm at 20°C to 46  2 nm at 60°C. However, the highest value at 20°C, 23  4 nm, grows more than twice when the temperature reaches 60°C. In this case, small aggregates (dimers or trimers) not only experience unfolding processes but also incorporate more protein molecules. Accordingly, it is concluded that BSA self-association is promoted by the temperature when already formed aggregates act as nuclei. Figure 2.4: Effective diameter measured by DLS at temperatures ranging from 20ºC to 60ºC (heating and cooling runs are displayed) for BSA, LYS and Omp2a. In contrast, LYS presents unimodal distributions, independently of the temperature, with similar Deff values (i.e. 4.3  0.2 nm and 4.3  0.5 nm at 20 and 60°C, respectively). Although these results suggest that LYS volume is not affected by the unfolding, what actually occurs is that unfolding is accompanied by a reduction of the protein hydration. The latter was proved in early X-ray scattering 2. Thermomechanical response of Omp2a 33 studies at 20°C and 80°C [37], which showed that the electron density of water in LYS crystals decreases with the crystallization temperature and, consequently, the radius of gyration remained practically invariant. Thus, it is hypothesized that changes in protein hydration offset the thermally induced protein motion. Similar observations have been found for other proteins [41], negative volume changes being detected in some cases [42]. The Deff of LYS, which remains at 4.3  0.2 nm for both 20 and 60°C, corresponds to the monomer diameter [40-43]. Thus, the contribution of aggregates, which are difficult to avoid completely even with dilute samples, was null in the case of LYS. These features combined with CD and FTIR data indicate that the unfolding is the only thermally-induced transition for LYS. Omp2a also presents a unimodal distribution, even though Deff increases from 6.1  0.2 nm at 20°C to 12.6  2.4 nm at 60°C. The former value has been associated to the trimeric state while the latter corresponds to bigger aggregates [1]. During the cooling run, Deff decreases from 21.6  5.1 nm at 60°C to 6.9  0.4 nm at 20°C. The thermal stability observed for Omp2a combined with the significant Deff variation indicates that the reversible aggregation of this β-barrel is notably affected by the temperature. DLS data reflect that Omp2a self-associates into the typical trimeric state found in the outer membranes of bacteria in the detergent buffer at room temperature. Thus, the Deff measured by transmission electron microscopy (TEM) for Omp2a trimers in dried samples was recently found to be 9.3  3.0 nm [1], which is consistent with the DLS value at 20°C aforementioned. However, the formation of bigger aggregates is detected by DLS when the temperature increases above 50°C, even though they are significantly smaller (Deff = 12.6  2.4 nm) than those also observed in dried samples at room temperature (Deff = 25.9  4.8 nm) by TEM. Thus, the van der Waals interactions between the side groups at the external side of the -barrel are promoted through both drying and heating. This feature points out the importance of improving the understanding of Omp2a self-association processes in non-native environments, as for example those used to fabricate bioinspired nanomaterials for ion transport. Overall, FTIR, CD and DLS results probe that LYS and BSA are suitable controls for the present microcantileveler deflection studies due to their different behavior not only with respect to Omp2a but also among them. Time resolved WAXD data on heating and cooling of lyophilized Omp2a Real time WAXD experiments were performed using synchrotron radiation to examine the evolution of the -strand structures in dried Omp2a during heating and cooling processes. Analyses were performed considering both Omp2a and blank samples, which were obtained by freeze drying the detergent buffer solution in presence and absence of protein, respectively. The one dimensional WAXD profile acquired for Omp2a at room temperature exhibits a sharp and intense peak at q = 2. Thermomechanical response of Omp2a 34 15.64 nm-1 (Figure 2.5), which corresponds to an inter-strand spacing of d = 4.02 Å [44-45]. This peak is absent in the spectra recorded for blank samples, the broad peak centered at q = 15.40 nm-1 being attributed to the salts from the buffer (Figure 2.5). The presence and absence of the reflection associated to the -strands in the Omp2a and blank samples, respectively, is clarified in the representative diffraction patterns showed in Figure 2.5d. Figure 2.5: (A) 1D scattering patterns of blank (salts from the buffer solution) and Omp2a samples as dry powder at room temperature. (B) 2D scattering patters of the blank and Omp2a dried samples at room temperature. (C) 1D scattering pattern of Omp2a when a temperature ramp (heating) is applied. (D) Intensity of the peak profile for the blank and the Omp2a samples at q= 15.6 nm-1 during the temperature ramp. Figure 2.5c displays a three-dimensional representation of the freeze dried Omp2a WAXD profiles in the -strand region (q = 15-16 nm-1) obtained by heating at a rate of 5°C/min from 25°C to 110°C. Figure 2.5d represents the variation in intensity of the peak at q = 15.6 nm-1 that occurs when heating both for Omp2a and blank samples. The variation with temperature of this narrow and intense peak has been used to monitor the effect of the different thermally-induced structural processes in inter-strand interactions. First, the intensity has a small increment at 50-55°C, which has been attributed to the reinforcement of neighboring intermolecular connections. According to DLS observations, which evidenced the transition from the trimeric form to bigger aggregates, this result has been interpreted as the formation of new hydrogen bonds between neighboring protein molecules. This hypothesis is also supported by the Omp2a trimer computational model [29]. After 2. Thermomechanical response of Omp2a 35 this, from 55°C to 75°C the intensity decreases slowly and, suddenly, grows again at 80°C. These changes suggest the restructuration of the newly formed aggregates during the heating process. Finally, the peak progressively broadened and becomes less intense at higher temperatures, evidencing that temperature has some effects in the local stability of the -strands. In spite of this, the peak maintains 47% of its initial intensity at 100°C, which is consistent with the overall stability of the -barrel structure observed by FTIR. WAXD experiments indicate that temperature affects the -sheet structure of Omp2a. This effect is focused in intermolecular interactions at temperatures lower than 80°C and in both inter- and intramolecular interactions at higher temperatures. However, the amount of -strands preserved at 110°C is still high enough to preserve the -barrel structure, which supports FTIR and CD results. Thus, WAXD results corroborate the conversion of trimers into bigger aggregates at 50-55°C, which after equilibration through local reorganizations remain relatively stable until 80°C. At higher temperatures, inter- and, probably, intramolecular -strands, are affected by the thermal stress, these interactions being roughly halved. This interpretation is consistent with the well-known high thermal stability of bacterial porins, which exhibit temperature induced unfolding above 100°C [30]. This unusual stability is consequence of their -barrel structural architecture composed of antiparallel -sheets, in which strands are connected by short turns on one side and long loops on the other. Thus, the energy required to breakdown the secondary and quaternary structure of bacterial porins is significantly higher than that necessary to unfold BSA and LYS. Also, yet porin aggregates are stable, a variety of transitions associated to changes in their size (i.e. to dimers, trimers or bigger aggregates) has been detected at temperatures significantly lower than their unfolding temperatures but comparable to the typical unfolding temperatures of conventional proteins [46–48], which is in agreement with the opposite behaviours of Omp2a and BSA. Protein immobilization onto the surface of silicon microcantilevers The microcantilever-based biosensing technology has been applied in this work to monitor the response of porins in synthetic environments against the temperature change. Analysis of the results has been carried out by comparing their thermal behavior with the proteins BSA and LYS. Among other features, this nanomechanical platform is characterized by the high sensitivity, label-free detection, and small sample consumption due to the size of the microcantilevers (ca. 1000 m2) [49]. For successful characterization, the first step is the functionalization of silicon microcantilevers to achieve a stable and irreversible protein–surface binding. 2. Thermomechanical response of Omp2a 36 In this work, a recently developed procedure to covalently bind peptides to silicon has been extrapolated and adapted to BSA, LYS and Omp2a proteins (Figure 2.6) [50]. This four-step protocol can be summarized as follows: 1) the microcantilever surface, previously hydroxylated with acids, is silanized with (3-glycodyloxypropyl)trimethoxysilane; 2) epoxy groups are opened with Nα,Nα-bis(carboxymethyl)-L-lysine hydrate (NTA-NH2) at basic pH; 3) the carboxylated surface derived from 2) is activated with a mixture of 1-[(3-dimethylamino)propyl]-3- ethylcarbodiimide methiodide (EDC) and N-hydroxysuccinimide (NHS); and 4) proteins are immobilized by incubating the activated surface in the corresponding protein solution. Before conducting any measurement, proteins not covalently bonded to the substrate were desorbed by washing with a phosphate buffer solution. Since the three proteins investigated contain a relatively large number of amine groups, corresponding to multiple lysine residues, in addition to the N- terminal amine, the study of protein-overhang interactions is limited by this immobilization procedure. Figure 2.6: Protein functionalization protocol for silicon substrates. Comparison of the characteristic XPS spectra in the N 1s, C 1s and O 1s regions of hydroxylated (non-functionalized) silicon and protein-functionalized substrates (Figure 2.7) chemically proves the success of the immobilization protocol. The presence of a peak in the C 1s region of the nonfunctionalized silicon spectrum has been attributed to the presence of organic contaminants from the environment. Whilst the latter makes more difficult the corroboration of the protein incorporation, the carbon content is significantly higher when silicon was functionalized with BSA, LYS and Omp2a (Table 2.1), showing a 4.5, 3.0 and 3.2 fold increase, respectively. Moreover, the apparition 2. Thermomechanical response of Omp2a 43 Figure 2.13: Relative displacement as a function of the temperature of a representative hydroxylated (nonfunctionalized) cantilever. The average displacement curve obtained for LYS (Figure 2.14), which was obtained using 16 different microcantilever sensors, reflects a behaviour very different from that obtained for nonfunctionalized cantilevers. The slope of the displacement curve in the region comprised from room temperature to 50°C is related to the deflection produced by the different thermal response of the two materials contained in the system (i.e. the silicon support and the attached proteins). More specifically, protein-functionalized cantilevers undergo a differential stress due to the thermal expansion coefficient difference between the protein and the microcantilever itself, giving rise to the cantilever deflection. After this, at 50°C the protein starts to unfold, causing a redistribution of the mass and reducing the contact between the protein and the substrate. This situation enhances the cantilever deflection, as it is reflected by the sustained increasing displacement of the profile. Figure 2.14: Thermomechanical response of cantivelevers functionalized with LYS proteins. Left: mean relative displacement as a function of the temperature and the corresponding standard error of the mean (thick light-grey lines), both calculated with the data of at least 7 different cantilevers. Right: cartoons representation of the folded  unfolded transitions. 2. Thermomechanical response of Omp2a 44 Thus, the melting temperature of LYS, as determined thermomechanically, is approximately 60°C, which is consistent with the CD data. At 70°C the slope of the displacement curve changes and the curve is similar to that observed for the hydroxylated silicon cantilevers (Figure 2.13). Thus, once LYS completes the conversion towards the unfolding state, the changes induced by the thermal dynamics of the random coil are not appearing in the deflection. At this stage the effects associated to the mass redistribution and the variation of the protein···surface interactions are negligible in average. Overall, the profile displayed for LYS should be considered as the fingerprint to recognize the thermomechanical response of conventional proteins, in which the folded  unfolded is the only occurring thermal transition. Figure 2.15 displays the average displacement curve achieved for BSA. From a qualitative point of view, the behaviour of the curve is similar to that described above for LYS until 100°C, even though the cantilever deflection is smaller for BSA. This has been attributed to the higher molecular weight of BSA and its tendency to aggregate, both reducing the differences in the stress distribution and the stress gradient between the protein and the substrate. Consequently, the impact of the bimetallic effects in the bending of the cantilever is relatively small before the protein denaturation at 60°C. Moreover, the effect of the redistribution of the mass during the unfolding process is also smaller than for LYS. As the effect of the unfolding on the cantilever displacement is expected to be directly proportional to the amount of protein molecules, these results suggest that such amount is lower for cantilevers functionalized with BSA than with LYS. Although this could be in apparent contradiction with the nanomechanical first mode resonance shift, which is 90 Hz lower for the latter (Figure 2.12), it is worth noting that the molecular weight of BSA is four times higher than that of LYS. Figure 2.15: Thermomechanical response of cantivelevers functionalized with BSA proteins. Left: mean relative displacement as a function of the temperature and the corresponding standard error of the mean (thick light-grey lines), both calculated with the data of at least 7 different cantilevers. Right: cartoons representation of the folded  unfolded transitions. 2. Thermomechanical response of Omp2a 45 In spite of this, the dynamics of the random coil causes a change in the cantilevers deflection. Thus, deflection downwards or upwards of the cantilever is mainly defined by the response of the protein within the studied temperature range and, as mentioned above, the deflection was relatively low before the unfolding. After this, the upward profile experiences an abrupt change at 110°C, which is not detected for LYS. Although this sudden drop in the displacement could be hypothesized as a disaggregation of the proteins, a simple thermogravimetric analysis evidenced that it corresponds to the evaporation of water molecules that were strongly interacting with the protein. Accordingly, in addition to the molecular unfolding, thermomechanical characterization of BSA reveals sharp dehydration process that, suddenly, produces a change of the deflection. The displacement profile recorded for Omp2a (Figure 2.16) exhibits unusual complexity. Although bimetallic effect initially affects the cantilever deflection, as in LYS and BSA, four regions can be distinguished above 40°C for Omp2a. In the first one, which extends from 40°C to 60°C, the variation of the displacement is practically null, suggesting that the redistribution of the molecular masses and the changes in the protein···substrate interactions are minimum (region I). This region has been associated with the alteration of intermolecular interactions before the transition from trimers to bigger aggregates, which is also consistent with WAXD observations. While initially they seem to become more intense, the step prior to the conversion into bigger aggregate is characterized by a weakening of interactions among neighbouring Omp2a molecules in trimers. This phase transition is evidenced by the increasing displacement (region II), which occurs in a relatively wide interval of temperatures (i.e. between 60°C and 77°C). After this (region III), the displacement undergoes small fluctuations, the average deflection increment along the whole region being very small. These fluctuations have been associated with local re-organizations in the newly formed aggregates. Above 105°C, the displacement drops sharply (region IV), suggesting that at such high temperatures the thermal stability of the -barrel is finally lost. Therefore, the downward deflection of the cantilevers is a consequence of the folded  unfolded transition that alters both the mass distribution and the Omp2a···substrate interactions. These observations are fully consistent with the WAXD results. 2. Thermomechanical response of Omp2a 46 Figure 2.16: Thermomechanical response of cantivelevers functionalized with Omp2a proteins. Left: mean relative displacement as a function of the temperature and the corresponding standard error of the mean (thick light-grey lines), both calculated with the data of at least 7 different cantilevers. Right: cartoons representation of the trimer  large aggregate and -barrel  unfolded transitions. In addition to the mass redistribution onto the cantilever surface, which causes changes in the resonance frequency, and to the bimetallic effect, the main mechanical effect in microcantilevers is the surfaces stress () that induces a nanoscale bending [2]. This effect, which occurs if only one of both cantilever sides are coated or, as in this work, functionalized, is quantified using the Stoney’s equation [54]:  (4) where L is the microcantilever effective length (450 m), T is the microcantilever thickness (1 m), E is the Young modulus of silicon (150 GPa),  is the Poisson ratio of silicon (0.17) and z is the deflection of the cantilever. The surface stress is frequently associated to intermolecular interactions between molecules anchored onto the cantilever surface, such as van der Waals forces, hydrogen bonds, electrostatic interactions, steric repulsions, etc. Ideally, protein-functionalized cantilevers should not exhibit any static surface stress if the functionalization was identical for both sides. However, in practice, the experimental set-ups used during the functionalization process do not result in two identical cantilever sides. As a consequence, the surface stress is not negligible for protein-functionalized cantivelers. At 120°C,  = 0.46  0.12, 0.31  0.05 and 0.30  0.15 mN/m for LYS, BSA and Omp2a, respectively (Figure 2.17). This is significantly higher than the value for hydroxylated non-functionalized cantilevers (e.g. at 120°C, = 0.08  0.012 mN/m). Moreover, the surface stress experiences a significant increment when the temperature is higher than 50°C for all functionalized cantivelers (Figure 2.17). 2. Thermomechanical response of Omp2a 47 Figure 2.17: Variation of the surface stress for hydroxylated (control) and protein-functionalized cantilevers against the temperature. Analyses of the displacement curves obtained for protein-functionalized cantilevers allowed distinguishing folded  unfolded conformational transitions from phase changes related with protein aggregates. Thus, the thermally-induced increment in the deflection of proteinfunctionalized cantilevers is not constant, as occurs for non-functionalized cantilevers. Proteins are much more sensitive than silicon to the temperature and, therefore, the general evolution of the displacement observed at relatively low temperatures (< 50°C) is mainly due to the differences in both stress distribution and stress gradient between the protein and the silicon substrate (i.e. the bimetallic effect). In such conditions, the bending of protein-functionalized cantilevers depends on the molecular weight and the presence of aggregates. Conventional proteins exhibit an abrupt change in the evolution of the curve, which is ascribed to their unfolding process. This folded  unfolded transition occurs at temperatures close to 50°C and 60°C for LYS and BSA, respectively, which are lower than those observed in water (60- 70°C). Consequently, in solution the folded structure of these soluble proteins is stabilized by intermolecular hydrogen bonds with surrounding water molecules, which are loss upon removal of the solvent. This instability induces a lower unfolding temperature. 2. Thermomechanical response of Omp2a 48 Once the denatured protein reaches a stable random coil, the dynamics of this state should not affect the thermomechanical response of the cantilever. This is true for LYS- and BSA-functionalized substrates, which show a behavior similar to that of non-functionalized cantilevers when the temperature exceeds 55 and 60°C, respectively. However, BSA-functionalized cantilevers display another transition at 110°C that has been ascribed to the evaporation of water molecules strongly interacting with protein molecules. The thermomechanical response of Omp2a is more complex than those of LYS and BSA because of both its intrinsic thermal stability and the tendency to form not only trimers but also larger aggregates. The thermal behavior of this porin is characterized by local re-organizations, which affect the strength of intermolecular interactions among neighbouring Omp2a molecules, inducing the transition from trimers to larger aggregates. The formation of such larger aggregates is consistent not only with DLS results but also with previous TEM investigations [1]. The latter phase transition is poorly defined, as reflects the continuous increase of the displacement in the temperature interval comprised between 60°C and 77°C. This feature should be attributed to the fact that the size and shape of the aggregates formed at such temperatures are constrained by the functionalization of the cantilever, which defines the tethering position of the protein molecules and gives variability to the transition. Such heterogeneity explains the undefined character of the transition that, in spite of the monodisperse and precise chemical nature of Omp2a molecules, occurs within a wide interval of temperatures rather than at a precise temperature. On the other hand, the thermal unfolding of Omp2a is detected at 105°C, this temperature representing the upper threshold in relation to the manipulation of stable protein aggregates. 2. Thermomechanical response of Omp2a 49 2.4. Conclusion In summary, thermomechanical measurements at the microscopic level on functionalized cantilevers have provided molecular insights that complement the information obtained from conventional characterization techniques on ensembles formed by a very large number of molecules. A serious limitation of conventional techniques is that they provide only a sample average response and are unable to give information on specific local features on or within the sample. Within this context, the unique thermomechanical response of Omp2a-functionalized cantilevers, which exhibits four well-defined regimes above 40°C, suggests practical approaches to improve the efficacy of smart biomimetic NMs with porins immobilized onto the surface or confined inside synthetic pores. Specifically, although the effectiveness of NMs is regulated by the amount of porin molecules active for the ion transport, controlling their orientation once immobilized onto the surface or inside nanopores is a challenge that has not been achieved yet. However, the identification of temperature intervals in which protein molecules experience local structural re-arrangements with an enhancement of intermolecular interactions, suggests that soft post-thermal treatments could be very advantageous to improve the efficacy of the NMs. Thus, this could be achieved by heating the proteins from their initial assembly state to denaturalization and, subsequently, cooling under controlled conditions to maximize favorable interactions. The amount of protein molecules contributing to the selective ion transport substrate could be substantially increased by enhancing the intermolecular interactions. 2. Thermomechanical response of Omp2a 50 2.5. Bibliography [1] A. Puiggalí-jou, M. M. Pérez-madrigal, L. J. del Valle, E. Armelin, M. T. Casas, C. Michaux, E. A. Perpète, F. Estrany, C. Alemán, L. J. Valle, E. Armelin, M. T. Casas, C. Michaux, E. A. Perpète, F. Estrany, and C. Alemán, “Confinement of a β-barrel protein in nanoperforated free-standing nanomembranes for ion transport,” Nanoscale, 8, 38, 16922– 16935, 2016. [2] J. Tamayo, P. M. Kosaka, J. J. Ruz, Á. San Paulo, and M. Calleja, “Biosensors based on nanomechanical systems,” Chem. Soc. Rev., 42, 3, 1287–1311, 2013. [3] M. Li, H. X. Tang, and M. L. Roukes, “Ultra-sensitive NEMS-based cantilevers for sensing, scanned probe and very high-frequency applications,” Nat. Nanotechnol., 2, 2, 114–120, 2007. [4] J. Chaste, A. Eichler, J. Moser, G. Ceballos, R. Rurali, and A. Bachtold, “A nanomechanical mass sensor with yoctogram resolution,” Nat. Nanotechnol., 7, 5, 301–304, 2012. [5] J. W. Ndieyira, M. Watari, A. D. Barrera, D. Zhou, M. Vögtli, M. Batchelor, M. A. Cooper, T. Strunz, M. A. Horton, C. Abell, T. Rayment, G. Aeppli, and R. A. McKendry, “Nanomechanical detection of antibiotic–mucopeptide binding in a model for superbug drug resistance,” Nat. Nanotechnol., 3, 11, 691–696, 2008. [6] P. M. Kosaka, J. Tamayo, J. J. Ruz, S. Puertas, E. Polo, V. Grazu, J. M. de la Fuente, and M. Calleja, “Tackling reproducibility in microcantilever biosensors: a statistical approach for sensitive and specific end-point detection of immunoreactions,” Analyst, 138, 3, 863– 872, 2013. [7] M. Soccio, G. Luongo, C. Esteves, A. Salvador-Matar, O. Ahumada, D. R. Rueda, M. C. García-Gutiérrez, N. Lotti, A. Munari, and T. A. Ezquerra, “Thermomechanical response of a semicrystalline polymer in the vicinity of the melting by using microcantilever technology,” Appl. Phys. Lett., 104, 25, 251904, 2014. [8] O. Ahumada, M. M. Pérez-Madrigal, J. Ramirez, D. Curcó, C. Esteves, A. Salvador-Matar, G. Luongo, E. Armelin, J. Puiggalí, and C. Alemán, “Sensitive thermal transitions of nanoscale polymer samples using the bimetallic effect: Application to ultra-thin polythiophene,” Rev. Sci. Instrum., 84, 5, 053904, 2013. [9] E. Rebollar, M. Sanz, C. Esteves, N. F. Martínez, Ó. Ahumada, and M. Castillejo, “Gold coating of micromechanical DNA biosensors by pulsed laser deposition,” J. Appl. Phys., 112, 8, 084330, 2012. [10] G.-G. Bumbu, M. Wolkenhauer, G. Kircher, J. S. Gutmann, and R. Berger, “Micromechanical Cantilever Technique: A Tool for Investigating the Swelling of Polymer Brushes,” Langmuir, 23, 4, 2203–2207, 2007. [11] M. del Rey, R. A. da Silva, D. Meneses, D. F. S. Petri, J. Tamayo, M. Calleja, and P. M. Kosaka, “Monitoring swelling and deswelling of thin polymer films by microcantilever sensors,” Sensors Actuators B Chem., 204, 602–610, 2014. [12] C. M. Domínguez, D. Ramos, J. I. Mendieta-Moreno, J. L. G. Fierro, J. Mendieta, J. Tamayo, and M. Calleja, “Effect of water-DNA interactions on elastic properties of DNA self-assembled monolayers,” Sci. Rep., 7, 1, 536, 2017. [13] O. Malvar, J. J. Ruz, P. M. Kosaka, C. M. Domínguez, E. Gil-Santos, M. Calleja, and J. Tamayo, “Mass and stiffness spectrometry of nanoparticles and whole intact bacteria by multimode nanomechanical resonators,” Nat. Commun., 7, 1, 13452, 2016. [14] A. K. Naik, M. S. Hanay, W. K. Hiebert, X. L. Feng, and M. L. Roukes, “Towards singlemolecule nanomechanical mass spectrometry,” Nat. Nanotechnol., 4, 7, 445–450, 2009. [15] Y. Shen, P. O. Saboe, I. T. Sines, M. Erbakan, and M. Kumar, “Biomimetic membranes: A review,” J. Memb. Sci., 454, 359–381, 2014. [16] M. Ali, S. Nasir, Q. H. Nguyen, J. K. Sahoo, M. N. Tahir, W. Tremel, and W. Ensinger, “Metal Ion Affinity-based Biomolecular Recognition and Conjugation inside Synthetic 2. Thermomechanical response of Omp2a 51 Polymer Nanopores Modified with Iron–Terpyridine Complexes,” J. Am. Chem. Soc., 133, 43, 17307–17314, 2011. [17] X. Hou, W. Guo, and L. Jiang, “Biomimetic smart nanopores and nanochannels,” Chem. Soc. Rev., 40, 5, 2385, 2011. [18] M. M. Pérez-Madrigal, L. J. del Valle, E. Armelin, C. Michaux, G. Roussel, E. A. Perpète, and C. Alemán, “Polypyrrole-Supported Membrane Proteins for Bio-Inspired Ion Channels,” ACS Appl. Mater. Interfaces, 7, 3, 1632–1643, 2015. [19] X. Zhang, W. Fu, C. G. Palivan, and W. Meier, “Natural channel protein inserts and functions in a completely artificial, solid-supported bilayer membrane.,” Nat. Sci. reports, 3, 1, 2196, 2013. [20] A. R. Hall, A. Scott, D. Rotem, K. K. Mehta, H. Bayley, and C. Dekker, “Hybrid pore formation by directed insertion of α-haemolysin into solid-state nanopores,” Nat. Nanotechnol., 5, 12, 874–877, 2010. [21] S. Balme, J.-M. Janot, L. Berardo, F. Henn, D. Bonhenry, S. Kraszewski, F. Picaud, and C. Ramseyer, “New Bioinspired Membrane Made of a Biological Ion Channel Confined into the Cylindrical Nanopore of a Solid-State Polymer.,” Nano Lett., 11, 2, 712–716, 2011. [22] G. Roussel, A. Matagne, X. De Bolle, E. A. a. Perpète, and C. Michaux, “Purification, refolding and characterization of the trimeric Omp2a outer membrane porin from Brucella melitensis,” Protein Expr. Purif., 83, 2, 198–204, 2012. [23] G. Roussel, E. A. Perpète, A. Matagne, E. Tinti, and C. Michaux, “Towards a universal method for protein refolding: The trimeric beta barrel membrane Omp2a as a test case,” Biotechnol. Bioeng., 110, 2, 417–423, 2013. [24] L. Whitmore and B. A. Wallace, “Protein secondary structure analyses from circular dichroism spectroscopy: Methods and reference databases,” Biopolymers, 89, 5, 392–400, 2008. [25] L. Lechuga Gomez, V. Alvarez-Sanchez, and F. J. Tamayo de Miguel, “System and method for detecting the displacement of a plurality of micro- and nanomechanical elements, such as micro-cantilevers,” 7,646,494 B2, 2010. [26] F. J. Tamayo de Miguel, J. Mertens, and M. Calleja-Gomez, “System and method for the inspection of micro and nanomechanical structures,” 7,978,344 B2, 2011. [27] M. S. Weiss, G. J. Palm, and R. Hilgenfeld, “Crystallization, structure solution and refinement of hen egg-white lysozyme at pH 8.0 in the presence of MPD,” Acta Crystallogr. Sect. D Biol. Crystallogr., 56, 8, 952–958, 2000. [28] K. A. Majorek, P. J. Porebski, A. Dayal, M. D. Zimmerman, K. Jablonska, A. J. Stewart, M. Chruszcz, and W. Minor, “Structural and immunologic characterization of bovine, horse, and rabbit serum albumins,” Mol. Immunol., 52, 3–4, 174–182, 2012. [29] M. Lopes-Rodrigues, D. Zanuy, C. Alemán, C. Michaux, and E. A. Perpète, “3D structure of a Brucella melitensis porin: molecular modelling in lipid membranes,” J. Biomol. Struct. Dyn., 1–13, 2018. [30] K. Zeth and M. Thein, “Porins in Prokaryotes and Eukaryotes: Common Themes and Variations,” Biochem. J., 431, 1, 13–22, 2010. [31] L. K. Tamm, H. Hong, and B. Liang, “Folding and assembly of β-barrel membrane proteins,” Biochim. Biophys. Acta - Biomembr., 1666, 1–2, 250–263, 2004. [32] C. P. Moon, N. R. Zaccai, P. J. Fleming, D. Gessmann, and K. G. Fleming, “Membrane protein thermodynamic stability may serve as the energy sink for sorting in the periplasm,” Proc. Natl. Acad. Sci., 110, 11, 4285–4290, 2013. [33] J. H. Kleinschmidt, “Folding and Stability of Monomeric β-Barrel Membrane Proteins,” in Protein-Lipid Interactions, Weinheim, FRG: Wiley-VCH Verlag GmbH & Co. KGaA, 2006, 27–56. [34] F. Rodríguez-Ropero, M. Fioroni, and T. Dworeck, Channel Proteins as Tools in Nanotechnology, Biology, B. Springer, 2014. 2. Thermomechanical response of Omp2a 52 [35] K. Murayama and M. Tomida, “Heat-Induced Secondary Structure and Conformation Change of Bovine Serum Albumin Investigated by Fourier Transform Infrared Spectroscopy,” Biochemistry, 43, 36, 11526–11532, 2004. [36] N. J. Greenfield, “Using circular dichroism collected as a function of temperature to determine the thermodynamics of protein unfolding and binding interactions,” Nat. Protoc., 1, 6, 2527–2535, 2007. [37] F. Meersman, C. Atilgan, A. J. Miles, R. Bader, W. Shang, A. Matagne, B. A. Wallace, and M. H. J. Koch, “Consistent Picture of the Reversible Thermal Unfolding of Hen Egg-White Lysozyme from Experiment and Molecular Dynamics,” Biophys. J., 99, 7, 2255–2263, 2010. [38] T. Knubovets, J. J. Osterhout, P. J. Connolly, and A. M. Klibanov, “Structure, thermostability, and conformational flexibility of hen egg-white lysozyme dissolved in glycerol,” Proc. Natl. Acad. Sci., 96, 4, 1262–1267, 1999. [39] P. Saha, C. Manna, J. Chakrabarti, and M. Ghosh, “Reversible thermal unfolding of a yfdX protein with chaperone-like activity,” Sci. Rep., 6, 1, 29541, 2016. [40] W. L. Stoppel, J. C. White, S. D. Horava, S. R. Bhatia, and S. C. Roberts, “Transport of biological molecules in surfactant–alginate composite hydrogels,” Acta Biomater., 7, 11, 3988–3998, 2011. [41] C. R. Chen and G. I. Makhatadze, “Molecular Determinants of Temperature Dependence of Protein Volume Change upon Unfolding,” J. Phys. Chem. B, 121, 35, 8300–8310, 2017. [42] T. V. Chalikian and K. J. Breslauer, “On volume changes accompanying conformational transitions of biopolymers,” Biopolymers, 39, 5, 619–626, 1998. [43] S. E. Hill, T. Miti, T. Richmond, and M. Muschol, “Spatial Extent of Charge Repulsion Regulates Assembly Pathways for Lysozyme Amyloid Fibrils,” PLoS One, 6, 4, e18171, 2011. [44] S. K. Maji, L. Wang, J. Greenwald, and R. Riek, “Structure-activity relationship of amyloid fibrils,” FEBS Lett., 583, 16, 2610–2617, 2009. [45] D. Eisenberg, “The discovery of the -helix and -sheet, the principal structural features of proteins,” Proc. Natl. Acad. Sci., 100, 20, 11207–11210, 2003. [46] S. Sukumaran, K. Hauser, E. Maier, R. Benz, and W. Mäntele, “Structure–function correlation of outer membrane protein porin fromParacoccus denitrificans,” Biopolymers, 82, 4, 344–348, 2006. [47] S. Sukumaran, C. Zscherp, and W. Mäntele, “Investigation of the thermal stability of porin from Paracoccus denitrificans by site-directed mutagenesis and Fourier transform infrared spectroscopy,” Biopolymers, 74, 1–2, 82–86, 2004. [48] T. F. Solov’eva, G. N. Likhatskaya, V. A. Khomenko, A. M. Stenkova, N. Y. Kim, O. Y. Portnyagina, O. D. Novikova, E. V. Trifonov, E. A. Nurminski, and M. P. Isaeva, “A Novel OmpY Porin From Yersinia Pseudotuberculosis : Structure, Channel-Forming Activity and Trimer Thermal Stability,” J. Biomol. Struct. Dyn., 28, 4, 517–533, 2011. [49] N. F. Martínez, P. M. Kosaka, J. Tamayo, J. Ramírez, O. Ahumada, J. Mertens, T. D. Hien, C. V. Rijn, and M. Calleja, “High throughput optical readout of dense arrays of nanomechanical systems for sensing applications,” Rev. Sci. Instrum., 81, 12, 125109, 2010. [50] A. Puiggalí-Jou, L. J. del Valle, C. Alemán, and M. M. Pérez-Madrigal, “Weighing biointeractions between fibrin(ogen) and clot-binding peptides using microcantilever sensors,” J. Pept. Sci., 23, 2, 162–171, 2017. [51] M. Alvarez and L. M. Lechuga, “Microcantilever-based platforms as biosensing tools,” Analyst, 135, 5, 827, 2010. [52] K. S. Hwang, K. Eom, J. H. Lee, D. W. Chun, B. H. Cha, D. S. Yoon, T. S. Kim, and J. H. Park, “Dominant surface stress driven by biomolecular interactions in the dynamical response of nanomechanical microcantilevers,” Appl. Phys. Lett., 89, 17, 173905, 2006. [53] J. R. Barnes, R. J. Stephenson, C. N. Woodburn, S. J. O’Shea, M. E. Welland, T. Rayment, 3. Effect of nanofeatures on the thermal transitions of PLA films 58 3.2. Methods Materials. PLA 2002D, a product of Natureworks, was kindly supplied by Nupik International (Polinyà, Spain). According to the manufacturer, this PLA has a D content of 1.5%, a residual monomer content of 0.3%, density of 1.24 g cm-3, glass transition temperature (Tg) of 55-60 °C, and melting temperature (Tm) of 155-170 °C. The number and weight average molecular weight and polydispersity index, as determined by gel permeation chromatography, is Mn= 98100 g/mol, Mw= 181000 g/mol and 1.85, respectively. PVA (87-89% hydrolysed) with Mw= 13000 – 23000 g/mol was purchased from Sigma-Aldrich. Curcumin (CUR) and stiripentol (STP) were purchased from Sigma-Aldrich. 1,1,1,3,3,3-Hexafluoroisopropanol (HFIP) was purchased from Apollo Scientific Limit (UK). Preparation of solutions and mixtures. For the fabrication of homogeneous PLA and PVA ultrathin films without drug loading, 10 mg/mL polymer solutions in HFIP were prepared. Nanopored and nanoperforated films were obtained by blending PLA and PVA. PLA-PVA blends with 80:20 and 90:10 PLA:PVA v/v ratios were prepared by mixing PLA (8 and 9 mg/mL, respectively) and PVA (2 and 1 mg/mL, respectively) HFIP solutions. On the other hand, drug-loaded films with 80:20 and 90:10 PLA:CUR and PLA:STP v/v ratios were obtained by mixing PLA (8 and 9 mg/mL) and drug (2 and 1 mg/mL) HFIP solutions. Preparation of ultra-thin films. 10 µL of PLA, PVA, PLA:PVA or PVA:drug solution was dropped onto a silicon microcantilevers chip, like that displayed in Figure 3.1a. The chip was fixed on a glass holder for spin-coating. The spin-coating was performed at 3500 rpm for 60 seconds in all cases. For the preparation of nanopored and nanoperforated PLA, samples coated with PLAPVA films were incubated in milli-Q water during 1 h for the dissolution of the PVA nanophases [18]. Spin-coating was performed with a spin-coater (WS-400BZ-6NPP/A1/AR1 Laurell Technologies Corporation). Typically, 6-9 ng films were obtained in all cases. Samples were dried under vacuum for 24 h before analysis. 3. Effect of nanofeatures on the thermal transitions of PLA films 59 Figure 3.1: Low- and high-magnification optical images of a silicon chip of 8 microcantilevers. (b) Experimental set-up for the thermal analyses conducted with SCALA Thermal analyses of microcantilevers. Deflection was measured by means of an equipment for the optical read-out of the microcantilevers named SCALA, (from MecWins) [25-26]. This technique combines the optical beam deflection method and the automated two-dimensional scanning of a single laser beam by voice-coil actuators. The equipment implements a thermal chamber with a thermoelectric cooler and cartridge heater. These elements are capable of sweeping the chamber’s temperature by flowing thermostatized N2 to the sample. A holder with multiple thermometer probes is placed inside the chamber for a better mapping of the temperature. All the measurements are performed in nitrogen environment to avoid the oxidation of the sample. Figure 3.1b schematizes the experimental set-up. The cantilever array is illuminated by the laser beam and a two-dimensional linear position detector (PSD) is arranged to collect the reflected beams. Location and characterization of cantilever sensors is carried out using TRACKER, an algorithm based on the recognition of reflected intensity patterns. This capability of SCALA allows the user to characterize a single sensor or an array of them in a fully automated process. A change in the local slope at the cantilever surface results into a displacement of the reflected laser spot on the PSD, which is denoted S (Figure 3.1b). S is used to obtain the cantilever profile along its longitudinal axis, z(x), by integrating: 3. Effect of nanofeatures on the thermal transitions of PLA films 60  cos 4 1 ')'( 2 1 )( 0 2 x D x dxxS D xz (1) where D is the distance between the cantilever and the PSD and  is the angle between the incident laser beam and the cantilever normal at its rest position. Coated cantilevers can be used as precise thermometers by exploiting the bimaterial effect [27], which refers to the measurable bending (i.e. differential stress) produced by temperature changes in substrates coated on one side by another material. Similarly, coated microcantilevers undergo a deflection, Δz (Figure 3.1b), as a result of temperature changes due to the thermal expansion coefficient difference between the coating material of the cantilever and the cantilever itself [11]. The temperature control was regulated by software created by the MecWins Company. The average deflection curves discussed in this work were obtained using 16 different microcantilevers. Monocrystalline Si microcantilever chips containing arrays of eight cantilevers (Micromotive GmbH) were used for thermomechanical measurements (Figure 3.1a). Specifically, the nominal length, width, and thickness of the cantilevers were 500, 90  2, and 1 μm, respectively. Profilometry. Film thickness measurements were carried out using a Dektak 150 stylus profilometer (Veeco, Plainview, NY). Different scratches were intentionally caused on the films and measured to allow statistical analysis of data. At least eighteen independent measurements were performed for three samples of each examined condition. Imaging of the films was conducted using the following optimized settings: tip radius= 12.5 m; stylus force= 3.0 mg; scan length= 1 mm; and speed= 100 µm/s. 3. Effect of nanofeatures on the thermal transitions of PLA films 61 Scanning electron microscopy (SEM). A Focus Ion Beam Zeiss Neon 40 instrument (Carl Zeiss, Germany) equipped with an energy dispersive X-ray (EDX) spectroscopy system and operating at 5 kV for characterization of the membranes was used. Films supported onto silicon sheets were mounted on a double-sided adhesive carbon disc and sputter-coated with an ultra-thin carbon layer (6-10 nm) to prevent sample charging problems. The diameter of the perforations was measured with the SmartTiff software from Carl Zeiss SMT Ltd. FTIR spectroscopy. FTIR spectra were recorded on a FTIR Jasco 4100 spectrophotometer. Samples were deposited on an attenuated total reflection accessory (Top-plate) with a diamond crystal (Specac model MKII Golden Gate Heated Single Reflection Diamond ATR). For each sample, 64 scans were performed between 4000 and 600 cm-1 with a resolution of 4 cm-1. 3. Effect of nanofeatures on the thermal transitions of PLA films 62 3.3. Results and discussion Thermomechanical response of PLA and PVA ultra-thin films Figure 3.2 show the ramp applied to the chips during the heating process (i.e. 1 ºC/min) and the thermal response of control non-coated cantilevers, which has been analysed by plotting the average deflection against the temperature. As it is expected, the deflection of uncoated cantilevers increases slowly and progressively with the temperature, as the deflection of rectangular bare cantilevers of length L grows linearly with the change of temperature (T), that is z  L2T [28]. However, the deflection is very small reaching a value of only -0.08 nm at 100 ºC indicating that changes discussed below for polymer-coated cantilevers are induced by the bimaterial effect (i.e. different thermal expansion/contraction behaviour of the polymer and the silicon cantilever). In this work, all thermal analyses with SCALA have been conducted from room temperature (25 ºC) up to 100 ºC. The latter is not only the denaturation temperature of the proteins typically used to prepare PLA nanomembranes for biofiltration but also a reasonable temperature to apply thermal treatments to drug-loaded PLA devices without causing melt [18]. Figure 3.2: Mean deflection curves (obtained using 16 microcantilevers) measured for bare microcantilevers. In the deflection curve, the standard error of the mean is indicated by thick light-gray lines. The ramp of temperature is displayed in the inset. PLA ultra-thin films were prepared by spin-coating a HFIP polymer solution onto previously cleaned bare microcantilevers chip. The thickness and roughness of the resulting films was 1546 nm and 2.50.5 nm, respectively, indicating that they are also ultra-flat. This is evidenced in Figure 3.3a, which shows a representative SEM micrograph. Figure 3.4 shows the average deflection curve obtained for PLA, which is very different from that obtained for bare cantilevers. Thus, PLA-coated cantilevers undergo a differential stress due to the thermal expansion coefficient difference between the polymer and the silicon from the microcantilever, giving rise to significant net positive (upward) 3. Effect of nanofeatures on the thermal transitions of PLA films 63 deflection. This implies a contraction of the PLA volume, resulting from the reduction of the configurational entropy of PLA chains, which causes the reduction of the compressive forces on the silicon side of the cantilever. Figure 3.3: SEM micrographs of (a) PLA and (b) PVA. Figure 3.4: Mean deflection curves (obtained using 16 microcantilevers) measured for microcantilevers coated with PLA. In the deflection curve, the standard error of the mean is indicated by thick light-gray lines. Cartoons in schematize the tensile surface stress due to the attraction between PLA molecules, which leads to positive (upward) deflection. The PLA deflection profile shows a subtle change in the slope that has been associated to the Tg, determined to be 51 ºC from the intersection of the tangents to the curves. This value is slightly lower that the Tg supplied by the manufacturer, which has been attributed to a small amount HFIP solvent molecules remaining after the spin-coating process. Thus, the ultra-thin nature of the film and the small weight of the sample (8 ng) favour the plasticiser behaviour of residual HFIP solvent. After the Tg, a second change in the slope is detected at 71 ºC, associated to the crystallization of amorphous domains during heating from room temperature. This phenomenon, called cold crystallization, is observed for PLA and the cold crystallization temperature (Tcc) typically ranges from 70º to 165 º depending on the molecular weight and previous processing of the sample [29–33]. 3. Effect of nanofeatures on the thermal transitions of PLA films 64 Since nanoperforated PLA ultra-thin films were prepared by blending PLA and PVA and by removing PVA domains via water etching, we decided to complete this section studying the thermomechanical response of PVA ultra-thin films. A representative SEM micrograph of such films, which exhibited thickness and roughness of 18117 nm and 1.80.4 nm, respectively, is displayed in Figure 3.3b. The average deflection curve of PVA is shown in Figure 3.5. Unlike PLA, net negative (downward) deflection is observed, which has been attributed to increased repulsive forces on the silicon-coated surface of the microcantilevers. The interaction between PVA chains decreases with increasing temperature, whereas the opposite effect was detected for PLA. Figure 3.5: Mean deflection curves (obtained using 16 microcantilevers) measured for microcantilevers coated with PVA ultra-thin films. In the deflection curve, the standard error of the mean is indicated by thick light-gray lines. Cartoons schematize the compressive surface stress due to the repulsion between PVA molecules, which leads to negative downward deflection. The complex deflection profile recorded for PVA shows an abrupt change in the slope starting at 56ºC, following a straight line until 66 ºC. This sharp change in the negative deflection tendency has been associated to the loss of mass produced by the detachment of superficially adsorbed water molecules. PVA is indeed a hydrophilic polymer that tends to capture water molecules at the surface. The vapour pressure of water being low, unbound of the superficially adsorbed molecules is expected at the indicated temperature interval. After this, the slope experiences a slight change that allows to determine the Tg = 87 ºC. This value is in agreement with the Tg values provided in the literature [34–36]. Thermomechanical response of nanopored and nanoperforated PLA ultra-thin films PLA-PVA layers were deposited onto silicon microcantilevers by spin-coating 90:10 and 80:20 PLA:PVA mixtures in HFIP. As PLA and PVA are immiscible polymers, spin-coating promoted the segregation of both polymers and the subsequent formation of nanofeatures [17]. They consisted in 3. Effect of nanofeatures on the thermal transitions of PLA films 65 spherical PVA nanodomains homogeneously distributed in the resulting PLA film. According to previous work, PVA nanofeatures can be used to create nanopores or nanoperforations in PLA ultrathin films by removing them via selective water etching [17-18]. More specifically, PVA nanofeatures transform into nanoperforations when their diameter is similar to the entire film thickness, while they create nanopores when the diameter is smaller. Moreover, both thickness and diameter depend not only on the operational conditions used for the spin-coating (see Methods section) but also on the substrate (i.e. silicon cantilevers in this case). It is worth noting that the use of an approach based on the combination of phase separation by spin-coating and selective solvent etching is expected to cause significant stress at the pore-air and/or perforation-air interfaces. Hereafter, solvent etched PLA ultra-thin films derived from spin-coated 90:10 and 80:20 PLA:PVA mixtures are denoted 90-PLA and 80-PLA, respectively. Figure 3.6: SEM micrographs of nanopored 90-PLA and nanoperforated 80-PLA. Examples of nanoperforations and nanopores are marked in (d) by red and blue circles, respectively. The thickness of 90-PLA and 80-PLA films is 14011 and 1199 nm, respectively, whereas the average diameter of the created nanofeatures is 7418 and 9629 nm, respectively. According to such thickness / diameter ratios, the topography of these PLA nanofilms may involve nanopores and nanoperforations. Representative SEM micrographs of 90-PLA films are displayed in Figure 3.6. The surface of such nanofilms exhibits abundant nanopores of very different sizes, but in all cases smaller than 100 nm and homogeneously distributed. In contrast, the surface of 80-PLA films can be described as distribution of both nanopores and nanoperforations, even though the former are more abundant than the latter. According to previous studies on nanoperforated PLA ultra-thin 3. Effect of nanofeatures on the thermal transitions of PLA films 66 films, nanopores and nanoperforations are distinguishable in Figure 3.6. Thus, nanoperforations correspond to nanofeatures with diameters around 120 nm (some examples are marked with red boxes in Figure 3.6), while the diameter of nanopores is much lower, 45 nm (some examples are marked with blue boxes in Figure 3.6). Obviously, nanofeatures affect the roughness of the films, which increases from 2.50.5 nm for neat PLA to 9012 and 12620 nm for 90-PLA and 80-PLA, respectively. More complete structural characterization of the nanoperforations was described in previous studies [17-18] and is not within the scope of this work, aiming to study the influence of nanopores and nanoperforations in the thermomechanical response of PLA nanosheets. Figure 3.7: Mean deflection curves of nanopored 90-PLA ultra-thin films. Cartoons sketch of the rearrangement of the PLA molecules at the interface of the pores and perforations, which were affected by the PVA etching. Initially, molecules are stressed by repulsive interactions (red pores / perforations; negative deflection) but, after a temperature threshold, they are relaxed by attractive interactions (green pores; positive deflection). The thermomechanical response of nanopored 90-PLA is completely different from that discussed above for the homogeneous PLA films (Figure 3.7). Two different regimes are clearly identified. The first is defined by the downward profile with negative deflection in the 32-to-48 ºC temperature interval, while the second corresponds to the subsequent ascending profile with positive deflection. This transition from one regime to the other has been interpreted as a rearrangement of the PLA molecules at the pores, which were probably stressed at the PLA–PVA interface before the water etching process. Once the PVA is removed, the increasing temperature ramp allows relaxing such interfacial molecules, changing repulsive interactions (negative deflection) into attractive ones (positive deflection). In the second regime, two changes in the slope are detected at 58 and 70 ºC, which have been associated with the Tg and Tcc, respectively. It is worth noting that the Tg of 90- PLA is 7 ºC higher that that found for compact PLA ultra-thin films (Tg= 51 ºC). According to previous observations, this shift is induced by the effect of film-air interface in the interactions among polymer chains [14]. Thus, the influence of the bulk and the film-air interface in nanopored 3. Effect of nanofeatures on the thermal transitions of PLA films 67 90-PLA films decreases and increases, respectively, in comparison to compact and homogeneous PLA, which was reported to increase the Tg. This phenomenon is consistent with the downward deflection at the lower temperature region (Figure 3.7), reflecting that both the surface stress and the thermal properties are affected by the interactions at the interface. On the other hand, the cold crystallization process in PLA ultra-thin films remains unaffected by the presence of nanopores, suggesting that the mobility of relaxed polymers molecules is preserved. The thermomechanical response of 80-PLA films is completely dominated by nanofeatures (Figure 3.8). In these films, the diameter of nanopores is not only larger than in 90-PLA but also is close to the thickness of the film. Nanofeatures therefore consist in a mixture of nanopores and nanoperforations. Both elements favour the effects associated to the film-air interface in detriment of those of bulk PLA. Thus, the most striking feature of the profile obtained for 80-PLA is the continuous negative deflection indicating that repulsive interactions dominate attractive interactions throughout the whole temperature interval. Three changes in the slope of the deflection profile are detected. The first at 49 ºC has been associated to the relaxation of the PLA molecules located at the film-air interface. However, the size and depth of nanopores are significantly higher in 80-PLA than in 90-PLA. The extent of this relaxation is therefore lower in the former than in the latter, which explains the continuous negative deflection displayed in Figure 3.8. After this, two thermal transitions associated to the Tg and Tcc are detected at 63 ºC and 78 ºC, respectively. Again, these results indicate that the presence of nanofeatures induces a shift in the transition temperatures towards higher values. Moreover, this effect becomes more pronounced when the stress of the PLA molecules located at the interface of the pores and perforations predominate over the film-air interface associated to the 2D nature of the ultra-thin film. Figure 3.8: Mean deflection curves of nanoperforated 80-PLA ultra-thin films. Cartoons sketch of the rearrangement of the PLA molecules at the interface of the pores and perforations, which were affected by the PVA etching. Initially, molecules are stressed by repulsive interactions (red pores / perforations; negative 3. Effect of nanofeatures on the thermal transitions of PLA films 74 distribution of the peaks in the physical mixtures is nearly identical to those of neat STP and PLA, which is attributable to the lack of drug···polymer interactions. Figure 3.15: FTIR spectra of STP, PLA and PLA/STP(10). Results from SCALA studies on PLA/STP(10) and PLA/STP(20) are in Figure 3.16. The Tg and Tcc determined for PLA/STP(10) (i.e. 61 ºC and 89 ºC, respectively) are higher than those obtained for neat PLA. The increment in the Tg, which is of 10 ºC, is very similar to that obtained for PLA/CUR(10). Again, this has been attributed to the rigidity of PLA chains confined in ultra-thin films, which is induced by the STP nanoaggregates. Comparison between PLA/STP(10) and PLA/CUR(10) suggests that the influence of the size of STP aggregates is offset by their abundance, which is significantly lower than for CUR-loaded films. Besides, the increment in the Tcc with respect to neat PLA (18 ºC) is lower than that observed in PLA/CUR(10). This has been associated to the fact that the amount of PLA chains affected by the drug in the cold crystallization process is mainly influenced by the density of nanodomains. 3. Effect of nanofeatures on the thermal transitions of PLA films 75 Figure 3.16: Mean deflection curves measured for microcantilever coated with PLA/STP(10) and PLA/STP(20). On the other hand, the Tg and Tcc obtained for PLA/STP(20) (i.e. 54 ºC and 83 ºC, respectively) are intermediate between those of neat PLA and PLA/CUR(20). This observation suggests that, in this case, STP aggregates are not acting as a plasticizer. Thus, the increment in the size and the reduction in the density of drug nanodomains with respect to PLA/CUR(20) indicate that the effects on the rigidity of the PLA chains predominates over those on the mobility (i.e. the plasticising effect). In summary, results obtained for drug loaded PLA ultra-thin films demonstrate the sensitivity of the SCALA methodology, which allows identifying features in the nanometer-length scale that are usually undetectable by conventional calorimetric methods based on bulk samples. 3. Effect of nanofeatures on the thermal transitions of PLA films 76 3.4. Conclusion SCALA microcantilevers technology has been used to investigate the influence of nanofeatures in the thermal response of PLA ultra-thin films. By comparing with conventional DSC analyses, the Tg and Tcc derived from the deflection profiles recorded for cantilevers coated with homogeneous and compact PLA and PVA ultra-thin films are very similar to those of the bulk polymers. Moreover, such deflection profiles provide information not only about the variation with the temperature of attractive and repulsive interactions between PLA and PVA chains, respectively, but also about the unbound of the water molecules from the surface of the latter polymer. Incorporation of physical nanofeatures, as for example nanopores, nanoperforations and segregated CUR or STP nanodomains, to ultra-thin films causes stress in the polymer molecules located at the PLA-air and PLA-drug interfaces, altering the thermal response. In the case of nanopored and nanoperforated PLA, such stress is probably due to the methodology applied to generate nanofeatures (i.e. phase separation through spin-coating followed by selective solvent etching), resulting in a significant increment of both the Tg and the Tcc with respect to homogeneous and compact PLA ultra-thin films. The thermal response of drug-loaded PLA films depends on the size and abundance of the nanodomains, which affect enhancing or reducing the strength of polymer···polymer interactions and increasing the mobility of polymer chains. Consequently, the Tg can increase or decrease with respect to neat PLA, while the Tcc increases in all cases. In summary, the used microcantileverbased technology has provided important microscopic information about the influence of nanofeatures on the thermal response of PLA, unreachable using conventional calorimetric methods, which was never reported before. 3. Effect of nanofeatures on the thermal transitions of PLA films 77 3.5. Bibliography [1] F. Zhou, W. Shu, M. E. Welland, and W. T. S. Huck, “Highly Reversible and Multi-Stage Cantilever Actuation Driven by Polyelectrolyte Brushes,” J. Am. Chem. Soc., 128, 16, 5326–5327, 2006. [2] T. Chen, D. P. Chang, T. Liu, R. Desikan, R. Datar, T. Thundat, R. Berger, and S. Zauscher, “Glucose-responsive polymer brushes for microcantilever sensing,” J. Mater. Chem., 20, 17, 3391, 2010. [3] S. Lenz, S. K. Nett, M. Memesa, R. F. Roskamp, A. Timmann, S. V. Roth, R. Berger, and J. S. Gutmann, “Thermal Response of Surface Grafted Two-Dimensional Polystyrene (PS)/Polyvinylmethylether (PVME) Blend Films,” Macromolecules, 43, 2, 1108–1116, 2010. [4] G. M. A. Alves, S. B. Goswami, R. D. Mansano, and A. Boisen, “Using microcantilever sensors to measure poly(lactic-co-glycolic acid) plasticization by moisture uptake,” Polym. Test., 65, 407–413, 2018. [5] C. Bradley, N. Jalili, S. K. Nett, L. Chu, R. Förch, J. S. Gutmann, and R. Berger, “Response Characteristics of Thermoresponsive Polymers Using Nanomechanical Cantilever Sensors,” Macromol. Chem. Phys., 210, 16, 1339–1345, 2009. [6] J. Zhao, R. Berger, and J. S. Gutmann, “Thermal contributions to the bending of bimaterial cantilever sensors,” Appl. Phys. Lett., 89, 3, 033110, 2006. [7] R. Muñoz, F. Aguilar-Sandoval, L. Bellon, and F. Melo, “Detecting protein folding by thermal fluctuations of microcantilevers,” PLoS One, 12, 12, e0189979, 2017. [8] M. Lopes-Rodrigues, A. Puiggalí-Jou, D. Martí-Balleste, L. J. Del Valle, C. Michaux, E. A. Perpète, and C. Alemán, “Thermomechanical Response of a Representative Porin for Biomimetics,” ACS Omega, 3, 7, 7856–7867, 2018. [9] A. Cagliani, P. Kosaka, J. Tamayo, and Z. J. Davis, “Monitoring the hydration of DNA selfassembled monolayers using an extensional nanomechanical resonator,” Lab Chip, 12, 11, 2069, 2012. [10] N. Jung and S. Jeon, “Nanomechanical Thermal Analysis with Silicon Cantilevers of the Mechanical Properties of Poly(vinyl acetate) near the Glass Transition Temperature,” Macromolecules, 41, 24, 9819–9822, 2008. [11] N. Jung, H. Seo, D. Lee, C. Y. Ryu, and S. Jeon, “Nanomechanical Thermal Analysis of the Glass Transition of Polystyrene Using Silicon Cantilevers,” Macromolecules, 41, 19, 6873– 6875, 2008. [12] M. Yun, N. Jung, C. Yim, and S. Jeon, “Nanomechanical thermal analysis of the effects of physical aging on glass transitions in PS/PMMA blend and PS-PMMA diblock copolymers,” Polymer (Guildf)., 52, 18, 4136–4140, 2011. [13] S. A. Manzoor Bukhari, M. F. Khan, A. Goswami, R. McGee, and T. Thundat, “Thermomechanical analysis of picograms of polymers using a suspended microchannel cantilever,” RSC Adv., 7, 14, 8415–8420, 2017. [14] O. Ahumada, M. M. Pérez-Madrigal, J. Ramirez, D. Curcó, C. Esteves, A. Salvador-Matar, G. Luongo, E. Armelin, J. Puiggalí, and C. Alemán, “Sensitive thermal transitions of nanoscale polymer samples using the bimetallic effect: Application to ultra-thin polythiophene,” Rev. Sci. Instrum., 84, 5, 053904, 2013. [15] M. Soccio, G. Luongo, C. Esteves, A. Salvador-Matar, O. Ahumada, D. R. Rueda, M. C. García-Gutiérrez, N. Lotti, A. Munari, and T. A. Ezquerra, “Thermomechanical response of a semicrystalline polymer in the vicinity of the melting by using microcantilever technology,” Appl. Phys. Lett., 104, 25, 251904, 2014. [16] M. Karl, P. E. Larsen, V. P. Rangacharya, E. Te Hwu, J. Rantanen, A. Boisen, and T. Rades, “Ultrasensitive Microstring Resonators for Solid State Thermomechanical Analysis of Small and Large Molecules,” J. Am. Chem. Soc., 140, 50, 17522–17531, 2018. 3. Effect of nanofeatures on the thermal transitions of PLA films 78 [17] A. Puiggalí-Jou, J. Medina, L. J. del Valle, and C. Alemán, “Nanoperforations in poly(lactic acid) free-standing nanomembranes to promote interactions with cell filopodia,” Eur. Polym. J., 75, 552–564, 2016. [18] A. Puiggalí-jou, M. M. Pérez-madrigal, L. J. del Valle, E. Armelin, M. T. Casas, C. Michaux, E. A. Perpète, F. Estrany, C. Alemán, L. J. Valle, E. Armelin, M. T. Casas, C. Michaux, E. A. Perpète, F. Estrany, and C. Alemán, “Confinement of a β-barrel protein in nanoperforated free-standing nanomembranes for ion transport,” Nanoscale, 8, 38, 16922– 16935, 2016. [19] B. Dorj, J.-E. Won, O. Purevdorj, K. D. Patel, J.-H. Kim, E.-J. Lee, and H.-W. Kim, “A novel therapeutic design of microporous-structured biopolymer scaffolds for drug loading and delivery,” Acta Biomater., 10, 3, 1238–1250, 2014. [20] J. M. Anderson and M. S. Shive, “Biodegradation and biocompatibility of PLA and PLGA microspheres,” Adv. Drug Deliv. Rev., 64, 72–82, 2012. [21] J. Delmote, L. Teruel-Biosca, J. L. Gómez Ribelles, and G. Gallego Ferrer, “Emulsion based microencapsulation of proteins in poly(L-lactic acid) films and membranes for the controlled release of drugs,” Polym. Degrad. Stab., 146, 24–33, 2017. [22] A. Gao, F. Liu, Z. Xiong, and Q. Yang, “Tunable adhesion of superoleophilic/superhydrophobic poly (lactic acid) membrane for controlled-release of oil soluble drugs,” J. Colloid Interface Sci., 505, 49–58, 2017. [23] J. Pang, Y. Luan, F. Li, X. Cai, J. Du, and Z. Li, “Ibuprofen-loaded poly(lactic-co-glycolic acid) films for controlled drug release,” Int. J. Nanomedicine, 6, 659, 2011. [24] A. Puiggalí-Jou, A. Cejudo, L. J. del Valle, and C. Alemán, “Smart Drug Delivery from Electrospun Fibers through Electroresponsive Polymeric Nanoparticles,” ACS Appl. Bio Mater., 1, 5, 1594–1605, 2018. [25] L. Lechuga Gomez, V. Alvarez-Sanchez, and F. J. Tamayo de Miguel, “System and method for detecting the displacement of a plurality of micro- and nanomechanical elements, such as micro-cantilevers,” 7,646,494 B2, 2010. [26] F. J. Tamayo de Miguel, J. Mertens, and M. Calleja-Gomez, “System and method for the inspection of micro and nanomechanical structures,” 7,978,344 B2, 2011. [27] R. Berger, C. Gerber, J. K. Gimzewski, E. Meyer, and H. J. Güntherodt, “Thermal analysis using a micromechanical calorimeter,” Appl. Phys. Lett., 69, 1, 40–42, 1996. [28] J. R. Barnes, R. J. Stephenson, C. N. Woodburn, S. J. O’Shea, M. E. Welland, T. Rayment, J. K. Gimzewski, and C. Gerber, “A femtojoule calorimeter using micromechanical sensors,” Rev. Sci. Instrum., 65, 12, 3793–3798, 1994. [29] E. S. Trofimchuk, A. V. Efimov, T. E. Grokhovskaya, N. I. Nikonorova, M. A. Moskvina, N. G. Sedush, P. V. Dorovatovskii, O. A. Ivanova, E. G. Rukhlya, A. L. Volynskii, and S. N. Chvalun, “Cold Crystallization of Glassy Polylactide during Solvent Crazing,” ACS Appl. Mater. Interfaces, 9, 39, 34325–34336, 2017. [30] C. Zhou, H. Li, W. Zhang, J. Li, S. Huang, Y. Meng, J. de Claville Christiansen, D. Yu, Z. Wu, and S. Jiang, “Thermal strain-induced cold crystallization of amorphous poly(lactic acid),” CrystEngComm, 18, 18, 3237–3246, 2016. [31] R. Androsch, H. M. N. Iqbal, and C. Schick, “Non-isothermal crystal nucleation of poly (llactic acid),” Polymer (Guildf)., 81, 151–158, 2015. [32] R. Androsch and M. L. Di Lorenzo, “Crystal Nucleation in Glassy Poly( l -lactic acid),” Macromolecules, 46, 15, 6048–6056, 2013. [33] Pengju Pan, Weihua Kai, Bo Zhu, and Tungalag Dong, and Y. Inoue*, “Polymorphous Crystallization and Multiple Melting Behavior of Poly(l-lactide): Molecular Weight Dependence,” 2007. [34] J. Rault, R. Gref, Z. H. Ping, Q. T. Nguyen, and J. Néel, “Glass transition temperature regulation effect in a poly(vinyl alcohol)—water system,” Polymer (Guildf)., 36, 8, 1655– 1661, 1995. 3. Effect of nanofeatures on the thermal transitions of PLA films 79 [35] E. Fathi, N. Atyabi, M. Imani, and Z. Alinejad, “Physically crosslinked polyvinyl alcohol– dextran blend xerogels: Morphology and thermal behavior,” Carbohydr. Polym., 84, 1, 145– 152, 2011. [36] A. Stavropoulou, K. G. Papadokostaki, and M. Sanopoulou, “Thermal properties of poly(vinyl alcohol)-solute blends studied by TMDSC,” J. Appl. Polym. Sci., 93, 3, 1151– 1156, 2004. [37] D. Karunagaran, R. Rashmi, and T. Kumar, “Induction of Apoptosis by Curcumin and Its Implications for Cancer Therapy,” Curr. Cancer Drug Targets, 5, 2, 117–129, 2005. [38] C.-H. Hsu and A.-L. Cheng, “Clinical studies with curcumin,” in The Molecular Targets and Therapeutic Uses of Curcumin in Health and Disease, Boston, MA: Springer US, 2007, 471–480. [39] B. B. Aggarwal and B. Sung, “Pharmacological basis for the role of curcumin in chronic diseases: an age-old spice with modern targets,” Trends Pharmacol. Sci., 30, 2, 85–94, 2009. [40] P. Anand, S. G. Thomas, A. B. Kunnumakkara, C. Sundaram, K. B. Harikumar, B. Sung, S. T. Tharakan, K. Misra, I. K. Priyadarsini, K. N. Rajasekharan, and B. B. Aggarwal, “Biological activities of curcumin and its analogues (Congeners) made by man and Mother Nature,” Biochem. Pharmacol., 76, 11, 1590–1611, 2008. [41] D. Chopra, L. Ray, A. Dwivedi, S. K. Tiwari, J. Singh, K. P. Singh, H. N. Kushwaha, S. Jahan, A. Pandey, S. K. Gupta, R. K. Chaturvedi, A. B. Pant, R. S. Ray, and K. C. Gupta, “Photoprotective efficiency of PLGA-curcumin nanoparticles versus curcumin through the involvement of ERK/AKT pathway under ambient UV-R exposure in HaCaT cell line,” Biomaterials, 84, 25–41, 2016. [42] A. Puiggalí-Jou, P. Micheletti, F. Estrany, L. J. del Valle, and C. Alemán, “Electrostimulated Release of Neutral Drugs from Polythiophene Nanoparticles: Smart Regulation of Drug-Polymer Interactions,” Adv. Healthc. Mater., 6, 18, 1700453, 2017. [43] Y. Chen, J. Lin, Y. Wan, Y. Fei, H. Wang, and W. Gao, “Preparation and blood compatibility of electrospun PLA/curcumin composite membranes,” Fibers Polym., 13, 10, 1254–1258, 2012. [44] T. T. T. Nguyen, C. Ghosh, S.-G. Hwang, L. D. Tran, and J. S. Park, “Characteristics of curcumin-loaded poly (lactic acid) nanofibers for wound healing,” J. Mater. Sci., 48, 20, 7125–7133, 2013. [45] J. L. Fisher, “The anti-convulsant stiripentol acts directly on the GABAA receptor as a positive allosteric modulator,” Neuropharmacology, 56, 1, 190–197, 2009. [46] I. S. S. Sharifah, A. A. B. Qairol, H. N. Azlina, and M. K. N. Khairusshima, “Thermal, Structural and Mechanical Properties of Melt Drawn Cur-loaded Poly(lactic acid) Fibers,” Procedia Eng., 184, 544–551, 2017. [47] G. Perumal, S. Pappuru, D. Chakraborty, A. Maya Nandkumar, D. K. Chand, and M. Doble, “Synthesis and characterization of curcumin loaded PLA—Hyperbranched polyglycerol electrospun blend for wound dressing applications,” Mater. Sci. Eng. C, 76, 1196–1204, 2017. 4. Structural and functional characterization of VDAC36 83 4. Structural and functional characterization of VDAC36 Abstract Forming water-filled channel in the mitochondria outer membrane and diffusing essential metabolites such as NADH and ATP, the VDAC (voltage-dependent anion channel) protein family plays a central role in all eukaryotic cells. Little is known about the structural and functional properties of plant VDACs in comparison with their mammalian homologues. In the present contribution, one of the two VDACs isoforms of Solanum tuberosum, stVDAC36, has been successfully overexpressed and refolded by an in-house method. Circular dichroism and intrinsic fluorescence could give information on its secondary and tertiary structure. Cross-linking and molecular modelling studies could evidence the presence of dimers and tetramers, and suggest the formation of a potential intermolecular disulphide bond between two stVDAC36 monomers. The pore-forming activity was also assessed by liposome swelling assays, highlighting a pore diameter between 2.0 and 2.7 nm. Finally, insights about the ATP binding inside the pore are pointed out by docking studies and electrostatic calculations. 4. Structural and functional characterization of VDAC36 90 Figure 4.3: Far UV circular dichroism spectra of stVDAC36. After purification, the protein was placed in different refolding buffers composed of 20 mM phosphate pH 8 and 66 mM NaCl, and different concentrations of sodium dodecylsulfate (SDS) and 2-methyl-2,4-pentanediol (MPD). A) The protein is unfolded regardless the concentration of detergent. B) Spectra show a β-barrel signal after addition of MPD. By adding an increasing amount of MPD, the CD spectra change to finally reach a signal corresponding to β-sheets and more particularly to a β-barrel structure (Figure 4.3B) [24–26]. With a MPD concentration of 0.5 M, the minimum at 208 nm is still present and it is concluded that this concentration is not sufficient to achieve the protein refolding. The CD spectrum corresponding to 30 mM SDS and 1 M MPD does not have the minimum at 208 nm and represents the transition between the unfolded state and the β-barrel structure. A suitable environment for the refolding is reached for the ratio 60 mM SDS and 1.5 M MPD and a β-barrel CD spectrum is obtained. Interestingly, the same ratio was also required to obtain the highest refolding yield for Omp2a, a bacterial porin also forming β-barrel [12]. This is a new evidence of the effectiveness of the SDSMPD refolding method. 91 Figure 4.4: Steady-state intrinsic fluorescence spectra of stVDAC36 in buffers composed of 20 mM phosphate pH 8 and 66 mM NaCl, and with different concentrations of SDS and MPD. The λmax is shifted from 309 to 320 nm upon addition of MPD into the refolding buffer. The tryptophan (Trp) fluorescence is a common method to study the refolding of proteins and complements the CD analysis. More specifically it provides insights into the polarity of the Trp vicinity, thereby indicating the orientation of the residue (e.g. pointing towards the hydrophilic inner channel or the lipid membrane). In the SDS buffers, the stVDAC36 λmax is at 309 nm with a decreasing intensity when the SDS concentration increases (Figure 4.4). This trend was also observed for peptides denatured in SDS [27]. With the addition of MPD, a bathochromic shift is observed to a λmax of 320 nm, corresponding to a more polar environment. This result supports the recovery of the β-barrel conformation by addition of the MPD, as demonstrated by the CD analysis. This red-shift between the SDS-unfolded and the native state was also pointed out for peptides [28]. The increasing of the fluorescence intensity indicates that the Trp residue is less hindered after refolding. To sum up, the fluorescence results are in accordance with the information gathered from the CD analysis and support the evidences of the successful stVDAC36 refolding by the SDS/MPD method. The latter has proven itself a reliable and fast method for the refolding of membrane proteins. 4. Structural and functional characterization of VDAC36 92 Structural studies of stVDAC36: secondary and tertiary structure The CD data were analyzed in order to extract the percentage of each secondary structure and to understand better the conformational changes underwent by the protein during its refolding (Table 4.1). Table 4.1: Secondary structure content of stVDAC36 in different refolding conditions. Percentages were obtained by deconvolution of circular dichroism spectra. % α-helices β-strands Turns Unordered 3.5 mM SDS 43 21 10 26 10 mM SDS 32 14 16 38 30 mM SDS 29 17 16 38 60 mM SDS 29 19 16 36 10 mM SDS + 0.5 M MPD 6 45 10 39 30 mM SDS + 1 M MPD 4 52 9 35 60 mM SDS + 1.5M MPD 1 68 9 22 Theoretical model 5 64 10 21 The β-strands content is higher for a SDS concentration of 3.5 mM than for the higher concentrations. This particularity can be related with the micelles formation. Indeed, above 3.5 mM the SDS could form micelles that alter the properties of the medium, hence modifying the detergentprotein interactions. Another interesting phenomenon is that SDS promotes the formation of helixlike structures [29], as illustrated by the high α-helix content for the conditions without MPD. With the alcohol, the micelles organization is perturbed and the protein accessible surface for detergents is reduced [30]. Consequently, the α-helix content drops significantly. The turn content remains almost unchanged, independently of the SDS/MPD ratio. With 0.5 M and 1 M of MPD, the unordered structure contents are similar to that of the denatured protein whereas the β-strands formation is largely intensified by MPD. Finally, concentrations of 60 mM SDS and 1.5 M MPD give the highest amount of β-structures and the smallest of unordered structures, which perfectly matches the structural data found in the Protein Data Bank (PDB) for other VDAC proteins. Membrane proteins remain a challenge for crystallographic studies and no plant VDAC structure has been resolved yet making stVDAC36 structure still undescribed. To answer the need for atomic structural information, molecular modelling has become a cost and time effective alternative. A 3D model of the protein was therefore built by threading, based on the VDAC2 structure from zebrafish 93 (PDB: 4BUM) [31]. As observed in experimental VDAC structures [32], the resulting stVDAC36 model is composed of 19 β-strands separated by short loops on the cellular side and turns on the intermembrane space. The β-strands contribute the most to the secondary content with a percentage of 64% (Table 4.1), accordingly to the previously described CD spectra. The stVDAC36 model presents two girdles of aromatic residues similarly to other β-barrels like porins [33]. The N- terminal chain folds inside the barrel into an α-helix that forms a bottleneck restricting the size of the channel (Figure 4.5). The resulting pore diameter (Dpore) is 1.56 nm, while the diameter of the channel with the α-helix outside the barrel is 2.16 nm. The Dpore calculated from the model are in accordance with the literature [34–36]. It is important to note that the open state of VDAC proteins is dependent of the solute trying to cross the channel. Small ions such as sodium or chloride will see the protein as an open gate wherever the α-helix is located. On the contrary, bulkier molecules may not be able to pass through the channel when the α-helix restrains the pore. Figure 4.5: Cartoon representation of the stVDAC36 model built by threading. Secondary structure is displayed with the following colors: β-strands (yellow), α-helix (red), turns (cyan) and loops (loop). A) Side views with the maximum diameter of the channel in blue. B) Side view without the N-terminus α-helix. C) Top view of the stVDAC36 model with the residues constituting the inner channel. The colors correspond to the nature of the amino acids as follow: polar (green), apolar (gray), positive (blue) and negative (red). D) Top view of the stVDAC36 model without the N-terminus α-helix. The fifty-five residues facing the inside of the channel and participating in the properties of the inner pore were identified in the model. The channel is composed of 34% polar (neutral), 19% 4. Structural and functional characterization of VDAC36 94 apolar, 9% aromatic, 21% positively charged, 17% negatively charged. Such proportions designate the channel as a polar environment with an almost neutral overall charge (i.e. +2). stVDAC36 does not have any particular distribution of the residues inside the pore. Indeed, the repartition is balanced with an alternation of positively and negatively charged residues all over the circumference of the channel (Figure 4.5C). With the α-helix removal, the pore is composed of 45% polar (neutral), 29% apolar, 3% aromatic, 13% positively charged and 10% negatively charged residues. The pore remains mainly polar and the charges distribution across the channel is modified. The translocation of charges was previously observed to explain the anion selectivity of VDAC proteins and supports the validity of our model [37]. 95 Oligomerization studies by cross-linking Some VDAC proteins have already been investigated in structural and functional studies but their oligomeric state is still uncertain. In previous works, monomers, dimers, trimers, tetramers and even hexamers have been mentioned for this protein family [38–40]. VDAC proteins retain their activity both in monomer and in oligomer state, making difficult to establish any solid structure-property correlation. Meanwhile, evidencing the nature of the stVDAC36 oligomeric states would help understanding the structural organization of the mitochondria outer membrane and its components as well as the role of oligomerization in biological processes [40–42]. Indeed, a correlation between VDAC oligomerization and apoptosis has previously been reported [4]. In that context, crosslinking is the method of choice to characterize the quaternary structure of proteins. Three homobifunctional and irreversible cross-linkers were selected with different spacer arm length: DMS (11.0 Å), DMA (8.6 Å) and DFDNB (3.0 Å). DMS and DMA have an amine-reactive imidoester groups and react with the N-terminal α-amines and lysine ε-amines at pH 7-10. They have the advantages to not change the charge of the protein thus retaining native structure and do not overreact with other nucleophilic groups. However, they present the risk to form a wide range of poorly defined oligomers and large aggregates of polymerized proteins. DFDNB contains active fluorine atoms reacting with amines but it is less selective than both DMS and DMA. This drawback can be partially countered by using very low concentrations of cross-linkers and a short incubation time. The tests were carried out with/without the β-mercaptoethanol reducing agent and resolved by SDSPAGE (Figure 4.6). The optimal refolding buffer, i.e. giving the highest β-sheets content, was selected for those experiments (60 mM SDS, 1.5 M MPD, 20 mM phosphate pH 8, 66 mM NaCl). Without β-mercaptoethanol, both DMA and DMS give strong bands at ~120 kDa, potentially evidencing the presence of tetramers. Interestingly, the intensity of this band is stronger than the one corresponding to the monomer. Large oligomers (> 250 kDa) could also be observed at the top of the gels. With DFDNB, weaker bands appear at about 30 and 90 kDa for monomer and trimers, respectively and the majority of the protein has aggregated. When adding the reducing agent, stVDAC36 monomers remain at the same apparent molecular weight of 30 kDa but the band at ~120 kDa was worn away. This result suggests that βmercaptoethanol can prevent the formation of stable tetramers even though it does not alter the abundance of large aggregates. Interestingly a weak band appears at ~60 kDa, hypothetically resulting from the degradation of the tetramers into dimers. The cross-linking experiments suggest that stVDAC36 can form dimers, trimers and tetramers, the latter being predominant but sensible to 4. Structural and functional characterization of VDAC36 96 chemical conditions. Trimers are associated to the weakest band which suggests a less probable state, and they are therefore not retained for the following discussion. Figure 4.6: SDS-PAGE of stVDAC36 after incubation with three cross-linkers of different space arm length: dimethyl suberimidate (DMS, 11.0 Å), dimethyl adipimidate (DMA, 8.6 Å) and 1,5-difluoro-2,4- dinitrobenzene (DFDNB, 3.0 Å). The buffer is composed of phosphate pH 8, 66 mM NaCl, 60 mM SDS and 1.5 M MPD. The effect of a reducing agent in the loading buffer was studied: A) no β-mercaptoethanol, B) with β-mercaptoethanol. The effect of the reducing agent brings us to consider the involvement of cysteine residues in the oligomerization process. A single cysteine residue is present in stVDAC36 and is, according to the model, located on the external part of the β-barrel, therefore available for intermolecular disulphide bridge. Studies on mammalian VDAC showed the involvement of cysteine in the oligomerization but this was only demonstrated for proteins with high content of Cys residues (up to nine) [43]. On the other hand, it was proved that cysteines in human VDAC2 mainly exist in their reduced form in the mitochondrial outer membrane and are more likely to stabilize the barrel with their apolar environment [44]. Actually, the number of cysteines is variable across the mammalian isoforms and their role still need to be elucidated. In the case of plants, no study has been yet performed on the role of cysteines. This first study would therefore give hypotheses on the relation between cysteines and oligomerization. A dimer model with a disulphide bond formed by Cys158 was constructed using our stVDAC36 model (Figure 4.7). The zebrafish VDAC2, which served as a template for the stVDAC36 model, was proved to form dimer and also possesses a single Cys residue but not participating in the oligomerization [31]. The position of the Cys residue could be one reason of the different dimer 97 configuration: in stVDAC36 is at the top of the β-barrel on the cytoplasmic side while it is located at middle height of the barrel in zebrafish VDAC2. Figure 4.7: Cartoon representation of the dimer of stVDAC36 model with the intermolecular disulphide bond formed by Cys158. Secondary structure is displayed with the following colors: β-strands (yellow), α-helix (red), turns (cyan) and loops (loop). A) Side view. B) Top view. 4. Structural and functional characterization of VDAC36 98 Functional studies: pore-forming activity Phosphatidylcholine lipids represent the main constituent of the mitochondria outer membrane where VDAC proteins are located [45]. The purified stVDAC36 was therefore reconstituted into large unilamellar vesicles (LUV) of 1,2-dioleoyl-sn-glycero-3-phosphocholine (DOPC). The vesicles were prepared by extrusion to control their size. DLS measurements indicated a hydrodynamic diameter of 148.4 ± 15.8 nm. The liposomes were also observed by TEM and showed an average diameter of 202.84 ± 31.35 nm (Figure 4.9). Micrographs were similar to the ones reported in literature [46]. The apparent bigger size of the liposomes by TEM is explained by the flattening of the vesicles after deposition onto the surface. The equation gives the maximum diameter that a spherical object of diameter d can have after flattening [47]. Considering the latter equation, both DLS and TEM provided consistent sizes of the DOPC liposomes. Figure 4.8: TEM images of negative stained DOPC liposomes prepared by extrusion. Prior to functional assays, structural studies of stVDAC36 were conducted by CD to verify the conformational state of the protein after reconstitution. The spectrum of the proteoliposome is very similar to the refolded one (Figure 4.3), indicating a β-barrel structure. The calculated β-sheet content is 59% confirming the correct folding of the protein. However, a bathochromic shift is observed compared to the spectrum of the SDS-MPD refolding buffer sample. This effect was attributed to the differences in the physical properties of the amphiphilic environments SDS-MPD and DOPC liposomes [48]. 99 Liposome swelling assays were then performed in test solutions containing substrates of different sizes. This method using sugars or polyethylene glycol (PEG) as diffusing solutes demonstrated its relevance to determinate the pore radius of membrane protein [49–52]. The selected solutes were classified according to their diameter (Table 4.2) considering that they adopt a spherical shape in water [49-51–57]. This approximation becomes less accurate as the size of the solute, especially PEG, increases. Table 4.2: Size of the solutes used for the liposome swelling assay. The rate was calculated as the difference between the initial and last absorbance values (after 300 seconds). Solute Glycine Glucose Saccharose Raffinose Stachyose PEG1000 PEG1500 PEG2000 PEG3500 PEG6000 PEG8000 Size (nm) 0.3 0.6 0.9 1.1 1.4 1.7 1.8 2.0 2.7 3.7 4.5 Rate of diffusion (%) 40.0 36.0 34.3 28.2 25.4 18.8 13.6 6.4 0.0 0.0 0.0 Liposomes without protein were added to the test solutions as negative controls, and no change in absorbance was observed. The swelling is more important with smaller solutes as previously reported for reconstituted pore-forming proteins [58]. No swelling was observed for PEG with a molecular weight equal or above 3500 Da (Figure 4.9). The assay demonstrated the ability of the reconstituted stVDAC36 to form a channel and diffuse solutes with a molecular weight below 3500 Da. The results also give an indirect determination of the pore size between 2.0 and 2.7 nm of diameter. Figure 4.9: Liposome swelling assay of stVDAC36 reconstituted in DOPC liposomes. The absorbance was recorded at 450 nm after dilution of the proteo-liposomes into the test solutions containing glycine, saccharides or poly(ethyleneglycol) (PEG) of various sizes. Those results are in agreement with the model and also with other VDAC from other organisms [35–37]. The discrepancies may be explained by the elliptical shape of the VDAC pore and the 4. Structural and functional characterization of VDAC36 106 Acta - Mol. Cell Res., 1863, 10, 2498–2502, 2016. [38] V. Betaneli, E. P. Petrov, and P. Schwille, “The role of lipids in VDAC oligomerization.,” Biophys. J., 102, 3, 523–31, 2012. [39] B. W. Hoogenboom, K. Suda, A. Engel, and D. Fotiadis, “The Supramolecular Assemblies of Voltage-dependent Anion Channels in the Native Membrane,” J. Mol. Biol., 370, 2, 246– 255, 2007. [40] R. Zalk, A. Israelson, E. S. Garty, H. Azoulay-Zohar, and V. Shoshan-Barmatz, “Oligomeric states of the voltage-dependent anion channel and cytochrome c release from mitochondria.,” Biochem. J., 386, Pt 1, 73–83, 2005. [41] J. Krause, R. Hay, C. Kowollik, and D. Brdiczka, “Cross-linking analysis of yeast mitochondrial outer membrane.,” Biochim. Biophys. Acta, 860, 3, 690–8, 1986. [42] S. Peng, E. Blachly-Dyson, M. Colombini, and M. Forte, “Determination of the number of polypeptide subunits in a functional VDAC channel from Saccharomyces cerevisiae.,” J. Bioenerg. Biomembr., 24, 1, 27–31, 1992. [43] V. De Pinto, S. Reina, A. Gupta, A. Messina, and R. Mahalakshmi, “Role of cysteines in mammalian VDAC isoforms’ function,” Biochim. Biophys. Acta - Bioenerg., 1857, 8, 1219– 1227, 2016. [44] S. R. Maurya and R. Mahalakshmi, “Cysteine Residues Impact the Stability and Micelle Interaction Dynamics of the Human Mitochondrial β-Barrel Anion Channel hVDAC-2,” PLoS One, 9, 3, e92183, 2014. [45] A. I. P. . de Kroon, D. Dolis, A. Mayer, R. Lill, and B. de Kruijff, “Phospholipid composition of highly purified mitochondrial outer membranes of rat liver and Neurospora crassa. Is cardiolipin present in the mitochondrial outer membrane?,” Biochim. Biophys. Acta - Biomembr., 1325, 1, 108–116, 1997. [46] P. Walsh, G. Vanderlee, J. Yau, J. Campeau, V. L. Sim, C. M. Yip, and S. Sharpe, “The mechanism of membrane disruption by cytotoxic amyloid oligomers formed by prion protein(106-126) is dependent on bilayer composition.,” J. Biol. Chem., 289, 15, 10419–30, 2014. [47] U. Baxa, “Imaging of Liposomes by Transmission Electron Microscopy,” in Characterization of Nanoparticles Intended for Drug Delivery, Humana Press, New York, NY, 2018, 73–88. [48] A. J. Miles and B. A. Wallace, “Circular dichroism spectroscopy of membrane proteins,” Chem. Soc. Rev., 45, 18, 4859–4872, 2016. [49] A. Godbole, R. Mitra, A. K. Dubey, P. S. Reddy, and M. K. Mathew, “Bacterial expression, purification and characterization of a rice voltage-dependent, anion-selective channel isoform, OsVDAC4,” J. Membr. Biol., 244, 2, 67–80, 2011. [50] F. Jacob-Dubuisson, “Channel Formation by FhaC, the Outer Membrane Protein Involved in the Secretion of the Bordetella pertussis Filamentous Hemagglutinin,” J. Biol. Chem., 274, 53, 37731–37735, 1999. [51] H. Nikaido and E. Y. Rosenberg, “Porin channels in Escherichia coli: studies with liposomes reconstituted from purified proteins.,” J. Bacteriol., 153, 1, 241–52, 1983. [52] J. W. F. Robertson, C. G. Rodrigues, V. M. Stanford, K. A. Rubinson, O. V. Krasilnikov, and J. J. Kasianowicz, “Single-molecule mass spectrometry in solution using a solitary nanopore,” Proc. Natl. Acad. Sci., 104, 20, 8207–8211, 2007. [53] C. M. Tam and A. Y. Tremblay, “Membrane pore characterization—comparison between single and multicomponent solute probe techniques,” J. Memb. Sci., 57, 2–3, 271–287, 1991. [54] S. G. Schultz and A. K. Solomon, “Determination of the effective hydrodynamic radii of small molecules by viscometry.,” J. Gen. Physiol., 44, 6, 1189–99, 1961. [55] C. J. Fee and J. M. Van Alstine, “Prediction of the Viscosity Radius and the Size Exclusion Chromatography Behavior of PEGylated Proteins,” Bioconjug. Chem., 15, 6, 1304–1313, 107 2004. [56] S. Kuga, “Pore size distribution analysis of gel substances by size exclusion chromatography,” J. Chromatogr. A, 206, 3, 449–461, 1981. [57] Z. Ma, D. N. LeBard, S. M. Loverde, K. A. Sharp, M. L. Klein, D. E. Discher, and T. H. Finkel, “TCR Triggering by pMHC Ligands Tethered on Surfaces via Poly(Ethylene Glycol) Depends on Polymer Length,” PLoS One, 9, 11, e112292, 2014. [58] R. H. Senaratne, H. Mobasheri, P. Jenner, E. J. A. Lea, and K. G. Papavinasasundaram, “Expression of a Gene for a Porin-Like Protein of the OmpA Family from Mycobacterium tuberculosis H37Rv Expression of a Gene for a Porin-Like Protein of the OmpA Family from Mycobacterium tuberculosis H37Rv,” 180, 14, 3541–3547, 1998. [59] D. A. Koppel, K. W. Kinnally, P. Masters, M. Forte, E. Blachly-Dyson, and C. A. Mannella, “Bacterial expression and characterization of the mitochondrial outer membrane channel. Effects of n-terminal modifications.,” J. Biol. Chem., 273, 22, 13794–800, 1998. [60] C. Guardiani, M. A. Scorciapino, G. F. Amodeo, J. Grdadolnik, G. Pappalardo, V. De Pinto, M. Ceccarelli, and M. Casu, “The N-Terminal Peptides of the Three Human Isoforms of the Mitochondrial Voltage-Dependent Anion Channel Have Different Helical Propensities,” Biochemistry, 54, 36, 5646–5656, 2015. [61] H. Saidani, E.-M. Krammer, M. Prevost, and F. Homble, “Plant VDAC Selectivity and Voltage-Dependence are Uncoupled,” Biophys. J., 106, 2, 791a, 2014. [62] M. A. Aksoyoglu, R. Podgornik, S. M. Bezrukov, P. A. Gurnev, M. Muthukumar, and V. A. Parsegian, “Size-dependent forced PEG partitioning into channels: VDAC, OmpC, and αhemolysin.,” Proc. Natl. Acad. Sci. U. S. A., 113, 32, 9003–8, 2016. [63] O. P. Choudhary, R. Ujwal, W. Kowallis, R. Coalson, J. Abramson, and M. Grabe, “The Electrostatics of VDAC: Implications for Selectivity and Gating,” J. Mol. Biol., 396, 3, 580–592, 2010. [64] S. R. Shuvo, F. G. Ferens, and D. A. Court, “The N-terminus of VDAC: Structure, mutational analysis, and a potential role in regulating barrel shape,” Biochim. Biophys. Acta - Biomembr., 1858, 6, 1350–1361, 2016. [65] T. Rostovtseva and M. Colombini, “VDAC channels mediate and gate the flow of ATP: implications for the regulation of mitochondrial function,” Biophys. J., 72, 5, 1954–1962, 1997. [66] R. Ujwal, D. Cascio, J.-P. Colletier, S. Faham, J. Zhang, L. Toro, P. Ping, and J. Abramson, “The crystal structure of mouse VDAC1 at 2.3 A resolution reveals mechanistic insights into metabolite gating,” Proc. Natl. Acad. Sci., 105, 46, 17742–17747, 2008. [67] O. P. Choudhary, A. Paz, J. L. Adelman, J.-P. Colletier, J. Abramson, and M. Grabe, “Structure-guided simulations illuminate the mechanism of ATP transport through VDAC1,” Nat. Struct. Mol. Biol., 21, 7, 626–632, 2014. 5. Biomimetic hybrid membrane made of PLA, PEDOT and VDAC36 111 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 Summary Hybrid free-standing biomimetic materials are developed by integrating the VDAC36 β-barrel protein into robust and flexible three-layered polymer nanomembranes. The first and third layers are prepared by spin-coating a mixture of poly(lactic acid) (PLA) and poly(vinyl alcohol) (PVA). PVA nanofeatures are transformed into controlled nanoperforations by solvent-etching. The two nanoperforated PLA layers are separated by an electroactive layer, which is successfully electropolymerized by introducing a conducting sacrificial substrate below the first PLA nanosheet. Finally, the nanomaterial is consolidated by immobilizing the VDAC36 protein, active as an ion channel, into the nanoperforations of the upper layer. The integration of the protein causes a significant reduction of the material electrical resistance, which decreases from 21.9 to 3.9 k·cm2. Electrochemical impedance spectroscopy studies reveal that the hybrid material behaves as a supercapacitor. The combination of polymers and proteins is promising for the development of new devices in bioelectronics. 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 112 5.1. Introduction Hybrid biomimetic membranes take advantage, on the one hand, of biomolecules having gained excellence on their specificity and efficiency during billions of years, and, on the other hand, of artificial materials loading the purified biological molecules as well as providing technological properties, such as robustness, scalability and suitable nanofeatures to confine the biomolecules. Molecular sensing, water purification and desalination, drug delivery and DNA sequencing are some striking applications of these 2D devices. Porins are a class of outer membrane proteins (OMPs), which consist of -barrel channels located in gram-negative bacteria and mitochondria [1]. -Barrels are typically employed for the fabrication of hybrid biomimetic membranes [2–6], even though other biomolecules and materials have also attracted interest [7–13]. From the perspective of the employed materials, the approaches used to modify artificial membranes, which can be free-standing or tethered onto solid supports, with biomolecules are those based on the use of amphiphilic copolymers and nanostructured polymers. In a recent study, the latter approach was used to embed an OMP, named Omp2a [14], in a supported conducting polymer (CP) membrane made of poly(N-methylpyrrole) (PNMPy) [5]. Electrochemical impedance spectroscopy (EIS) showed that PNMPy/Omp2a preferentially promotes the passive transport of K+ in solutions with relatively high ionic concentrations. The PNMPy membrane was electrochemically synthesized onto a rigid stainless steel electrode, which represents a serious inconvenient for possible future applications. Later, self-standing poly(lactic acid) (PLA) nanomembranes were used as support for the Omp2a protein [6]. These membranes, which were prepared by spin-coating an immiscible mixture of poly(vinyl alcohol) (PVA) and PLA [15], showed nanoperforations (diameter: 5122 nm) resulting from the combination of nanophase segregation processes and selective solvent etching. EIS assays evidenced that, with respect to protein-free nanoperforated PLA (npPLA) nanomembranes, the protein, confined around and inside the nanoperforations, enhanced the conductivity and selectivity against some ions [16]. 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 113 In this work we present a new approach to synergistically combine the advantages of supported and free-standing hybrid biomimetic membranes based on CPs, biodegradable PLA and OMPs. This approach is based on a smart strategy that merges the processing of npPLA nanosheets, the anodic polymerization of poly(3,4-ethylenedioxythiopene) (PEDOT), and the functionality of Voltage Dependent Anion Channels (VDACs), porins found in the outer mitochondrial membrane of all eukaryotic cells [17]. The function of VDACs is associated with the permeability of the mitochondria, regulating the diffusion of ions and metabolites [18-19]. Specifically, this work focus on the use of VDAC from Solanum tuberosum, a plant (potato) model organism, hereafter named VDAC36 [20]. Results show that npPLA/PEDOT/npPLA/VDAC free-standing membranes are biomimetic, exhibit low electrical resistance, and behave as a supercapacitor. 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 114 5.2. Methods Materials. Poly(3,4-ethylenedioxythiophene):poly(styrenesulfonate) (PEDOT:PSS) 1.3 wt. % dispersion in H2O, 3,4-ethylenedioxythiophene (EDOT), PVA 87-89% hydrolyzed and lithium perchlorate (LiClO4) were purchased from Sigma-Aldrich (USA). PLA 2002D, a product of Natureworks, was kindly supplied by Nupik International (Polinyà, Spain). According to the manufacturer, this PLA has a D content of 4.25%, a residual monomer content of 0.3%, density of 1.24 g/cm3, glass transition temperature (Tg) of 58 oC, and melting temperature (Tm) of 153 oC. Acetonitrile and hexafluoroisopropanol (HFIP) were purchased from Panreac Quimica S.A.U. (Spain). Spin-coating. Spin-coating was performed using the conditions described in the main text with a spin-coater (WS-400BZ-6NPP/A1/AR1 Laurell Technologies Corporation). The PEDOT:PSS sacrificial layer was obtained by spin-coating a commercial water dispersion (1.3 wt. %) at a speed of 800 rpm for 1 min. Nanoperforated PLA (npPLA) layers were obtained by blending PLA and PVA with a ratio of 90:10 v/v (PLA:PVA), prepared by mixing PLA (10 mg/mL) and PVA (10 mg/mL) HFIP solutions. The spin-coating of the PLA:PVA mixture was conducted at 1200 rpm for 1 min. The resulting PLA:PVA nanomembrane was transformed into npPLA by eliminating the PVA phase. For this purpose, selective solvent etching was carried out by dropping milli-Q water on the surface for 1 h without agitation at 20 ºC. Anodic polymerization. Anodic polymerizations were performed using a VersaStat II potentiostatgalvanostat connected to a computer controlled through a Metrohm Autolab Nova program. Electrochemical experiments were conducted in a three-electrode two-compartment cell under nitrogen atmosphere (99.995% in purity) at 20 ºC. The anodic compartment was filled with 40 mL of a 10 mM EDOT solution in acetonitrile containing 0.1 M LiClO4 as supporting electrolyte, while the cathodic compartment was filled with 10 mL of the same electrolyte solution. Steel AISI 316L sheets, previously washed with acetone and ethanol, were employed as working (coated with a PEDOT:PSS layer) and counter (bare) electrodes. The reference electrode was an Ag|AgCl electrode containing a KCl saturated aqueous solution (Eº = 0.222 V at 25 ºC), which was connected to the working compartment through a salt bridge containing the electrolyte solution. All anodic polymerizations were conducted by chronoamperometry under a constant potential of +1.40 V and adjusting the polymerization charge to 90 mC. Expression, purification and immobilization of the VDAC36 protein. Escherichia coli BL21 (DE3) bacteria were transformed to produce 6 His-tagged VDAC36 proteins in inclusion bodies. 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 115 Bacteria were then lysed and centrifuged to obtain the final pellet corresponding to the non-purified unfolded proteins. VDAC36 was then purified by Ni2+ affinity column. VDAC36 was eluted and the buffer was exchanged to 20 mM phosphate pH 8, 60 mM sodium dodecyl sulfate (SDS) and 1.5 M 2-methyl-2,4-pentanediol (MPD) with a PD10 desalting column. The supported npPLA/PEDOT/npPLA 3-layered film was used to immobilize the protein. For this purpose, samples were placed on a 24-well plate and incubated with 1000 µL of a protein solution, which contained 0.85 mg/mL VDAC36, 60 mM SDS and 1.5 M MPD, for 12 h at 20 ºC. The resulting npPLA/PEDOT/npPLA/VDAC samples were rinsed three times with milliQ water to remove residues. Blank film was obtained using the same procedure (i.e. 60 mM SDS and 1.5 M MPD) but without VDAC36. Profilometry. Film thickness measurements were carried out using a Dektak 150 stylus profilometer (Veeco, Plainview, NY). Different scratches were intentionally caused on the films and measured to allow statistical analysis of data. At least eighteen independent measurements were performed for three samples of each examined condition. Imaging of the films was conducted using the following optimized settings: tip radius = 2.5 m; stylus force = 3.0 mg; scan length = 1 mm; and speed = 50 µm/s. Scanning electron microscopy. Detailed inspection of films and layers was conducted by scanning electron microscopy (SEM). A Focus Ion Beam Zeiss Neon 40 instrument (Carl Zeiss, Germany) equipped with an energy dispersive X-ray (EDX) spectroscopy system and operating at 1 kV was used. Films supported onto steel sheets were mounted on a double-sided adhesive carbon disc and sputter-coated with an ultra-thin carbon layer (6-10 nm) to prevent sample charging problems. The diameter of the perforations was measured with the SmartTiff software from Carl Zeiss SMT Ltd. Fluorescence microscopy. Imaging was performed using an Axio Observer Z1 fluorescence microscope (Carl Zeiss) confocal laser scanning microscope with a 60x oil objective. The excitation wavelength was set to 280 nm and the emission was collected at 303 and 354 nm, for tyrosine (Tyr) and tryptophan (Trp) residues, respectively. Atomic force microscopy. AFM images of PLA nanomembranes before and after application of selective solvent etching were obtained with a Molecular Imaging PicoSPM using a NanoScope IV controller under ambient conditions. The tapping mode AFM was operated at constant deflection (i.e. vertical constant force with triangular shaped gold-coated silicon nitride). The row scanning 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 122 Figure 5.4: SEM micrographs with increasing magnification (bottom to top) of npPLA/PEDOT/npPLA/VDAC (left column) and npPLA/PEDOT/npPLA (right column) 3-layered films. The different elements of the film (i.e. npPLA of the upper layer, PEDOT clusters emerging from the intermediate layer and SDS crystals) are marked in red, while representative nanoperforations of the upper npPLA layer are marked in blue. 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 123 Figure 5.5: Confocal microscopy images of (a) npPLA/PEDOT/npPLA and (b) npPLA/PEDOT/npPLA/VDAC. The panels at the first and second columns correspond to the fluorescence images, the panel at the right displays the merged images. Scale bar: 10 µm. The latter observation was corroborated by AFM. Comparison of topographic and phase AFM images recorded for npPLA/PEDOT/npPLA films before and after incubation with VDAC36 (Figure 5.6) shows that the protein was not only confined inside and around the nanopores of the outer npPLA layer but also adsorbed onto its electrochemically inactive surface. Although only the protein immobilized in the pores is expected to contribute to ion transport, regulation of the adsorption process to avoid the immobilization onto the surface is, unfortunately, a very difficult task. 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 124 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 125 Figure 5.6: 2D topographic and phase contrast AFM images (left and right, respectively) for (a) npPLA/PEDOT/npPLA and (b) npPLA/PEDOT/npPLA/VDAC: 5x5 µm² (top), 1x1 µm² (middle) and 0.25x0.25 µm² (bottom) windows. Comparison of the images recorded for the 3-layered film reflects the apparition of small protuberances after incubation in the protein solution. These protuberances, which have been attributed to protein aggregates, are located onto the film surface and inside and around the nanopores of the outer npPLA layer. Further characterization by XPS, contact angle measures, FTIR spectroscopy and CD unambiguously confirmed the immobilization of the protein. The atomic compositions of npPLA/PEDOT/npPLA and npPLA/PEDOT/npPLA/VDAC, as obtained by XPS, are compared in 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 126 Table 5.1. The penetration of X-ray radiation using the conditions described in Methods section (ESI) is expected to be 10 nm, even though in this case the penetration is unknown due to the nanoperforations at the upper layer. The content of N 1s, which is undetectable for npPLA/PEDOT/npPLA, is 0.19% for npPLA/PEDOT/npPLA/VDAC. This feature, together with the increment of O 1s content, supports the presence of the porin. 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 127 Table 5.1: Atomic percent composition obtained by XPS for the studied 3-layered films. C 1s N 1s O 1s S 2p npPLA/PEDOT/npPLA 72.01 0.00 27.88 0.11 npPLA/PEDOT/npPLA/VDAC 70.87 0.19 28.88 0.06 The contact angles () measured in water (Figure 5.7) also provided indirect evidences of the successful immobilization of VDAC36. The wettability of npPLA/PEDOT/npPLA (=61°7°) significantly increased upon the incorporation of the protein (=41°10°), which has been attributed to the effect of the hydrophilic residues found in the loops connecting the β-strands of the protein or inside the central pore. Figure 5.7: Contact angle of the 3-layered films. Detachment of 3-layered films from steel substrates was achieved by selective elimination of the thin sacrificial layer. Although PEDOT:PSS is not soluble in water, it forms a colloidal dispersion. After immersion into milli-Q water for 12 h, films were detached from the steel substrate and easily recovered with fine-point tweezers. The resulting free-standing films, which do not deteriorate during such process, are 1.05 m in thickness and shows excellent conformability (Figure 5.8). 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 128 Figure 5.8: Photographs showing the robustness and conformability of free standing npPLA/PEDOT/npPLA/VDAC films. Figure 5.9 compares the FTIR spectra from 890 to 1790 cm-1 of several films after detachment. Although the side chain bands of charged amino residues at 1631 and 1755 cm-1 are not identified because of the overlapping with the bands associated to the thiophene ring (C=C and C–C stretching) of PEDOT [23], it is possible, from the typical amide band, to unambiguously conclude that VDAC36 has been successfully immobilized. Indeed, the amide III and II vibrational modes of the protein, which arise from the coupling between the N−H in-plane bending and C−N stretching modes, are clearly recognizable at 1230 and 1514 cm-1, respectively. Figure 5.9: FTIR spectra of 3-layered free standing films. 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 129 The immobilized protein not only remained at the free-standing 3-layered film, as proved by FTIR spectroscopy (Figure 5.9) but also preserved its -barrel structure. Figure 5.10 compares the CD spectra recorded for VDAC36 in five different scenarios: (i) unfolded (negative control); (ii) refolded in SDS-MPD; (iii) after immobilization onto the supported 3-layered film; and (iv) after detachment of the free-standing film. All spectra, with the exception of the unfolded protein, exhibit a broad minimum at 218-220 nm that is typically associated with β-stranded proteins [24]. The spectrum of the unfolded protein reflects structural modifications associated with the conformational lost. Figure 5.10: CD spectra for the VDAC36 protein: unfolded, refolded, after immobilization onto supported 3- layered films and after detachment of the 3-layered film from the steel substrate. Influence of the protein on the film electrical response EIS studies were conducted on npPLA/PEDOT/npPLA and npPLA/PEDOT/npPLA/VDAC to monitor the changes in resistance and capacitance caused by the 3-layered configuration containing both npPLA and CP with respect to simple membranes with only one of such components. The ion transport was evaluated by measuring the impedance for frequencies ranging from 10-2 to 105 Hz, using a 0.5 M NaCl solution and steel electrodes. Figure 5.11 displays the recorded Nyquist and Bode plots. The EECs used to fit the experimental data and the corresponding parameters are sketched in Figure 5.12, where RS is the electrolyte resistance and Rp represents the ability of the films to impede ion transport at the interface between the electrolyte and the membrane (i.e. the resistance of the film). The EECs also include double layer capacitances from both the 3-layered film and the steel electrode (CPE3L and CPEst, respectively) and a Warburg impedance element (W), corresponding to the diffusion of water molecules. In the case of npPLA/PEDOT/npPLA/VDAC, 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 130 both Rp and CPE3L include the overall contribution of the VDAC36-integrated interface. Both CPE3L and CPEst were modelled using a constant phase element (CPE). Figure 5.11: (a) Nyquist and (b) Bode plots in a 0.5 M NaCl aqueous solution. Symbols correspond to experimental data, while lines are fitted curves according to EEC. The Rp of the 3-layered film functionalized with VDAC36 is one order of magnitude lower than that of the film without protein (i.e. 3.9 and 21.9 k·cm2, respectively) using a 0.5 M NaCl solution. Interestingly, the resistance of the npPLA/PEDOT/npNA/VDAC membrane is very similar to that observed for the PPy/Omp2a membrane (1.3 k·cm2) [5], though the amount of CP contained was significantly higher and was not self-supported. Similarly, the resistance reported for Omp2a protein supported onto lipid bilayers, which exhibited much less mechanical strength than polymeric nanomembranes, was of 3.7 kΩ·cm2 [16]. 5. Biomimetic hybrid membranes made of PLA, PEDOT and VDAC36 131 Figure 5.12: Electrical equivalent circuit (EEC) elements used for fitting experimental data recorded for npPLA/PEDOT/npPLA and npPLA/PEDOT/npPLA/VDAC. These results confirm that npPLA/PEDOT/npNA/VDAC membranes behave as smart biomimetic membranes fulfilling the self-standing and mechanical integrity requirements of many applications in different areas of the biomedical field, such as nanofluidics, biosensing and energy conversion. In addition to the heterogeneous characteristics of the electrode surface (i.e. roughness, porosity, reactivity), the CPE impedance is related to non-uniform diffusion across the interface. Accordingly, CPE is expressed as [Q·(jω)n]-1, representing an ideal capacitor (n = 1), a pure resistor (n = 0) or a diffusion process (n = 0.5). For films without and with VDAC36, the value of n obtained for the CPE associated to CPE3L is 0.769 and 0.927, reflecting that the protein significantly improves the capacitive behaviour of the film. The well-known supercapacitive (i.e. electrochemically capacitive) response of PEDOT is typically attributed to its ability to promote series of fast and reversible redox reactions [25-26]. However, our results show that the integration of the protein enhances this behaviour. This change is justified by the addition of the bounded Warburg diffusion impedance (T) element, which is characteristic of films that contain a fixed amount of electroactive material (i.e. films of finite thickness). The addition of T, which is usually related to the diffusion resistance of ions in doped electrodes of batteries and supercapacitors [27– 29], indicates that VDAC36 induces a fast transfer and subsequent adsorption of electrolytes on the surface of the membrane. This leads to an increased CPE3L, as demonstrated by the EEC parameters (Figure 5.12), indicating that npPLA/PEDOT/npPLA/VDAC membranes are potential candidates for the fabrication of bio-supercapacitors.