Full text
Functionalization of a Ti-based Alloy with Synthesized Recombinant Fibronectin Fragments to Improve Cellular Response Carolina Herranz Díez PhD Thesis Doctoral program of Biomedical Engineering Supervised by Dr. JM. Manero Planella Dr. Jordi Guillem Martí Department of Materials Science and Metallurgical Engineering Universitat Politècnica de Catalunya · Barcelona Tech (UPC) July 2014
Cuando me planteé realizar un doctorado, nunca pensé que el tiempo podría pasar tan rápido y tan lento a la vez. Tras cuatro años de trabajo me encuentro escribiendo las últimas líneas. Esta tesis es el producto del trabajo realizado durante estos cuatros años y no habría sido posible sin la colaboración y dedicación de muchas otras personas. En primer lugar, querría dar las gracias a mis directores de tesis, el Dr. José María Manero y el Dr. Jordi Guillem. También me gustaría darle las gracias a los miembros del grupo de Biomaterials, Biomechanics and Tissue Engineering (BBT) del Departamento de Ciencia de los Materiales e Ingeniería Metalúrgica de la ETSEIB porque cada uno de ellos ha participado de una forma u otra en esta tesis. Mención especial merecen Sara Gallinetti y Maria Godoy, sin ellas nada hubiera sido igual. Otro pilar importante en la consecución de esta tesis ha sido el Instituto de Bioingeniería de Cataluña (IBEC) que me abrió sus puertas y puso a mi alcance todos sus recursos. No puedo olvidarme de los investigadores de otros centros o departamentos que se prestaron a colaborar. Gracias al Dr. Benjamin Thierry y a la Dra. Lorena Diéguez del Ian Work Research Institute; a la Dra. Christine Selhuber-Unkel de la Universidad de Kiel; al Dr. Jeremy Schaffer de Fort Wayne Metals Corporation y al Dr. Emilio Jiménez y al Dr. Joan Josep Roa del Departamento de Ciencia de los Materiales e Ingeniería Metalúrgica de la UPC. Gracias a mis padres y a mi hermano por haber estado siempre apoyándome y gracias también a Gonzalo por embarcarse conmigo en esta aventura sin dudarlo ni un segundo.
I ABSTRACT According to a study of the European Commission, approximately one million hips are replaced by prostheses worldwide every year. The interaction of the human body with foreign materials that are subjected to alternating mechanical load in a highly corrosive environment still provides challenges. The main factors affecting prosthesis failure are stress shielding effect and poor osseointegration. In this thesis the problem of prosthesis failure has been approached from the material and from the osseointegration point of view trying to give a global solution to the problem. Niobium and hafnium, which are demonstrated to be totally biocompatible, were used to design a Ti-based alloy. The effect of the alloying elements regarding microstructure and elastic modulus was studied and the best composition was deeply characterized in terms of microstructure, elastic modulus, corrosion resistance and superficial energy. Recombinant fragments of fibronectin were synthesised spanning the cell attachment site and the heparin binding domain which are important for cell viability. These motifs were used to functionalise the surface of the TiNbHf alloy. Two tethering methods were studied: physisorption and silanisation. Silanisation was not used before to immobilise fibronectin recombinant fragments onto metallic substrates and in this thesis, its good performance was demonstrated. In vitro studies were made with each fragment and with different combinations of the fragments, which showed the importance of the heparin binding domain to obtain a cell response equivalent to that of fibronectin in terms of cell adhesion, proliferation and differentiation. Key words: stress shielding effect, titanium alloy, osseointegration, fibronectin, recombinant protein, biofunctionalisation, in vitro cell culture.
II RESUMEN De acuerdo con un estudio de la Comisión Europea, aproximadamente un millón de caderas son remplazadas por prótesis en el mundo anualmente. La interacción del cuerpo humano con materiales externos sujetos a una carga mecánica alternante en un medio altamente corrosivo todavía presenta ciertos desafíos. Los factores que contribuyen principalmente al fallo de una prótesis son el apantallamiento de cargas y la pobre osteointegracion. En la presente tesis el problema de la fallida de prótesis ha sido abordado desde el punto de vista del material y de la osteointegracion en un intento de dar una solución global al problema El niobio y el hafnio, cuya total biocompatibilidad ha sido demostrada, se han utilizado para diseñar una aleación de titanio. El efecto de dichos aleantes respecto a la microestructura y el módulo elástico ha sido estudiado y la mejor composición ha sido profundamente caracterizada en términos de microestructura, módulo elástico, resistencia a la corrosión y energía superficial. Fragmentos recombinados de fibronectina han sido sintetizados abarcando la zona de adhesión celular y la unión de heparina, las cuales son esenciales para la viabilidad celular. Dichos motivos han sido utilizados para funcionalizar la superficie de la aleación TiNbHf. Dos métodos de unión diferentes han sido estudiados: fisisorción y silanización. La silanización es un método que no se ha utilizado hasta el momento para inmovilizar fragmentos de fibronectina sobre superficies metálicas y en la presente tesis su idoneidad ha sido demostrada. Finalmente, estudios celulares in vitro se han llevado a cabo con cada fragmento y con diferentes combinaciones de ambos, lo cual ha mostrado la importancia de la zona de unión de heparina para obtener una respuesta celular equivalente a la obtenida con la molécula de fibronectina en cuanto a adhesión celular, proliferación y diferenciación.
III THESIS OBJECTIVES The main objective of this thesis is on one hand, study the ternary system TiNbHf as a potential substitute for the alloys used in total hip replacement and on the other hand, synthesise a fibronectin recombinant fragments spanning the III8-10 and III 12-14 domains to improve osseointegration. The specific objectives of the present thesis are: 1. To design a titanium alloy based on optimization of molecular orbital calculations of electronic structures towards low modulus of elasticity and the potential for super elasticity and study the effect of niobium and hafnium alloying elements in terms of microstructure and elastic modulus. 2. To select the appropriate TINbHf composition, fabricate a bar and characterise its microstructure, determine its elastic modulus, determine its corrosion resistance and study its superficial energy. 3. To fabricate, by recombinant protein techniques, the fibronectin fragments FNIII8-10 (CAS) and FNIII12-14 (HBII) and characterise the fuctionalisation of the TiNBHf alloy with such fragments. 4. To study cell response to the biofunctionalised material in terms of adhesion force and cell adhesion, proliferation and differentiation.
IV CONFERENCE CONTRIBUTIONS C. Herranz, J. Schaffer, T. Trifonov, J. Portillo, S. Estrade, Ll. Yedra, J. Mendoza, FX Gil, J.M. Manero. “Microstructural characterization of a potential superelastic Nickelfree titanium alloy”. III Microscopy at the Frontiers of Science Conference, September 2013, Tarragona, Spain (Poster Presentation). C. Herranz, J. Schaffer, J.M. Manero. “Potential Superelastic nickel-free titanium alloy”. 2013 Shape Memory and Superelastic Technology Conference, May 2013, Prague, Czech Republic (Poster Presentation) C. Herranz, M. González, J. Guillem-Martí, J. Peña,J.C Rodríguez-Cabello, F.J. Gil, J.M. Manero. “New nickel-free titanium alloys design and functionalization for implantology”. XXXIII Iberian Society de Biomechanics and Biomaterials Conference, November 2010, Valencia, Spain (Oral Presentation).
V ABSTRACT .................................................................................................................................... I RESUMEN ..................................................................................................................................... II THESIS OBJECTIVES ................................................................................................................. III CONFERENCE CONTRIBUTIONS .............................................................................................. IV I Introduction .......................................................................................................................... 1 Chapter 1 Introduction ................................................................................................................ 3 1. Bone ....................................................................................................................... 5 1.1 Bone composition ................................................................................................ 5 1.2 Bone mechanics................................................................................................... 7 1.2.1 Creep and stress relaxation ........................................................................... 7 1.2.3 Viscoelasticity .............................................................................................. 8 1.3 Bone cytology ..................................................................................................... 8 1.3.1 Mesenchymal Stem Cells (MSC) ................................................................. 8 1.3.2 Osteoblasts .................................................................................................... 9 1.3.3 Osteoclasts .................................................................................................. 10 1.3.4 Osteocytes ................................................................................................... 10 1.4 Bone remodelling process ................................................................................. 11 1.4.1 Cell processes during bone remodelling ..................................................... 11 1.4.2 Bone functional adaptation ......................................................................... 13 1.5 Bone diseases .................................................................................................... 14 2. Materials used for bone replacement ................................................................... 16 2.1 Biomaterials ...................................................................................................... 16 2.1.1 Definition .................................................................................................... 16 2.1.3 Use of biomaterials ..................................................................................... 16 2.2 Metals used as biomaterials for prosthesis ........................................................ 18 2.2.1 Introduction ................................................................................................ 18 2.2.2 Stainless Steels. .......................................................................................... 18
XII 3. CHAPTER 5: Recombinant fragments fabrication .............................................. 207 4. CHAPTER 6: Optimization of the biofunctionalisation process ......................... 208 5. CHAPTER 7: Cell response to the biofunctionalised surfaces ............................. 210 6.Bibliography .......................................................................................................... 215 V Conclusions ..................................................................................................................... 219 Chapter 9 Conclusions ............................................................................................................ 221 VI Ongoing Research ........................................................................................................... 225 Chapter 10 Effect of the cold work in the microstructure and mechanical properties of the Ti-25Nb-21Hf alloy .................................................................................................................... 227 1. Introduction ........................................................................................................... 229 2. Materials and methods .......................................................................................... 230 2.1 Sample fabrication........................................................................................... 230 2.2 Other samples tested........................................................................................ 231 2.3 Wire tensile testing .......................................................................................... 231 2.4 Rotary beam fatigue testing............................................................................. 231 2.5 Transmission electron microscopy (TEM) assay ............................................ 233 2.5.1 Focused ion beam (FIB) milling technique .............................................. 233 3. Results ................................................................................................................... 235 3.1 Tensile testing ................................................................................................. 235 3.1.1 Effect of the cold-work on the elastic modulus ........................................ 235 3.1.1 Effect of the heat treatment on the elastic modulus.................................. 237 3.1.3 Cyclic tensile testing ................................................................................. 238 3.2 Microstructure studies ..................................................................................... 239 3.3 Rotary beam fatigue testing............................................................................. 240 4. Discussion ............................................................................................................. 242 5. Conclusion ............................................................................................................ 243 6. Bibliography ......................................................................................................... 244
XIII Chapter 11 CASHB Fragment Fabrication ............................................................................. 245 1. Introduction ........................................................................................................... 247 2. Materials and methods .......................................................................................... 247 2.1 RNA extraction and reverse transcription ....................................................... 247 2.2 Primers design ................................................................................................. 247 2.3 PCR amplification ........................................................................................... 249 2.4 Fragments clonning procedure ........................................................................ 249 2.5 DNA fragments digestion................................................................................ 249 2.6 Plasmid and fused DNA ligation ..................................................................... 251 3. Results ................................................................................................................... 251 3.1 Amplification of the FN fragments ................................................................. 251 3.2 Plasmid-fused DNA ligation ........................................................................... 252 3.3 Fragment sequencing....................................................................................... 253 3.4 CASHBII fragment expression and purification ............................................. 256 5. Conclusion ............................................................................................................ 258 6. Bibliography ......................................................................................................... 260
1
1 I Introduction
2
3 Chapter 1 Introduction 1. Bone ...................................................................................................................................... 5 1.1 Bone composition ................................................................................................... 5 1.2 Bone mechanics ...................................................................................................... 7 1.3 Bone cytology ......................................................................................................... 8 1.4 Bone remodelling process ..................................................................................... 11 1.5 Bone diseases ........................................................................................................ 14 2. Materials used for bone replacement ............................................................................... 16 2.1 Biomaterials .......................................................................................................... 16 2.2 Metals used as biomaterials for prosthesis ........................................................... 18 2.3 Titanium as a biomaterial ..................................................................................... 23 2.4 Titanium alloys ..................................................................................................... 23 3. Problems derived from the interaction prosthesis-body .................................................... 26 3.1 Host response ........................................................................................................ 26 3.2 Toxicity and Allergy ............................................................................................. 29 3.3 Stress shielding effect ........................................................................................... 31 3.4 Poor osseointegration ............................................................................................ 33 4. Mimicking extracellular matrix .............................................................................................. 34 4.1 Extracellular matrix .............................................................................................. 34 4.2 Biofunctionalisation of surfaces ........................................................................... 41 4.3 Motifs for biofunctionalisation ............................................................................. 45 5. Bibliography ........................................................................................................................... 47
4
5 1. BONE Bone plays an important role in the human body giving support, protecting soft tissues and participating in mineral metabolism. Bones are the framework were soft organs are supported and anchored. Bones are also a reservoir for minerals that are released to the blood stream and distributed to other parts of the body and the responsible of production of blood cells. 1.1 Bone composition Bone is composed of 70% mineral (mostly hydroxiapatite), 22% organic matrix and 8% water, approximately. The organic matrix is composed of collagen in a 95% and the remaining 5% is composed of osteocalcin, osteonectin, proteoglycans, bone morphogenetic protein, proteolipids and phosphoproteins. Bone structural properties such as strain, strength, etc. are influenced by the different components of bone. Each component of bone contributes in a different way to bone structural properties. Depending on the percentage of each part the physical properties (strain, strength, etc.) can be modified. Depending on the shape of the bones they are classified in long, short, flat and irregular but all of them are formed for two basic osseous tissue: • Cortical bone: is compact, dense and forms the outer surface of bones, contributing 80% of the weight of a human skeleton (Fig.1). • Trabecular bone: is a porous lattice of bony struts called trabeculae (Fig.2). It has low density and strength but very high surface area, that fills the inner cavity of bones. The external layer of cancellous bone contains redbone marrow where the production of blood cells (known as haematopoiesis) takes place.
6 Fig.1 Microscopic structure of compact bone. A) Section of compact bone illustrating the osteons and the irrigation system. In the magnified section the osteocytes and the lamella are shown. B) Photomicrograph of a cross-sectional view of one osteon and portions of others. (90x). Adapted from 1. Fig.2 Long bone structure. A) Description of the parts of the long bone with a longitudinal cut showing the cortical and the trabecular bone. B) View of the trabecular and cortical bone present in the epiphysis. C) Cross section of the diaphysis showing the main components. Adapted from (1)
7 1.2 Bone mechanics Bone is a dynamic tissue that changes morphology depending on the stresses applied and their direction; this is translated in different mechanical properties depending on the area of bone we are focusing on. We can say bone is an anisotropic material with special characteristics. For this reason bone mechanics may be studied with two different perspectives: the material one and the structural. As a material, tensile and compression tests can be performed obtaining the results showed in Table 1. Bone type Direction and type of load Apparent density (g/cm2) Ultimate strength (MPa) Modulus of elasticity (106 MPa) Cortical (midfemur) Longitudinal tension 1.85 133 17 Longitudinal compression 1.85 193 17 Longitudinal shear 1.85 68 3.000 Transverse tension 1.85 51 11.500 Transverse compression 1.85 33 11.500 Travecular (vertebral body) Compression 0.31 6 76 Table 1. Values of some mechanical parameters when testing bone under different conditions. Adapted from 2 1.2.1 Creep and stress relaxation Collagen biochemistry of bone may change among different bone regions and there are also microcracks that make bone to deform over time when a constant loading is applied 3–5. This phenomenon is known as creep. Together with creep another phenomenon takes place, the stress relaxation. That means the diminishment of the stress necessary to
14 Recent theories have added a new vision to Wolff’s law keeping in mind that loading in bone remodelling process is important. It seems that all the scientists involved in such investigations agreed with the fact that is not the stress but the strain the key factor for the initiation of the process 20. Another important idea of the new conception of Wolff’s law is that the organisms possess the ability to adapt their structure to new living conditions. In Figure 5(a) the strict Wolff model for bone remodelling is represented. Under Wolff vision, bone was ruled by mathematical equations. On the other hand, in Figure 5(b) it is showed a schematic representation of the modern vision of bone remodelling. The model is very simplified, because it does not take into account the age, the shape or the living conditions. Fig.5 a) Wolff mathematical model of bone remodelling. b) Representation of the modern theory of bone remodelling. Adapted from 19. 1.5 Bone diseases The organism is always looking for homeostasis, and so does bone by means of remodelling. But there are some situations in which bone is not able to maintain the homeostasis by itself, and requires a replacement. Bone can be affected by different diseases or conditions that have as a result pain, malfunction, structural degeneration or a combination of them and the only way to alleviate them is replacement of the affected part. The disease can be caused by
15 bacteria, virus, fungus, autoimmunity, sclerosis, neoplasia, bone section missing or age related degeneration 21,22 The options to replace/repair bone are: • Allografts: the material used for the replacement is from another patient. The risks associated to this substitute are infection, rejection and loosening of stiffness due to sterilization. • Autografts: the material used is from the same patient, but from a different site (such as the pelvis). Despite reducing the chances of rejections, there is a limited amount of material available and more pain and risk of infection because of the two surgeries needed. • Synthetic materials: are materials developed in a laboratory which allows bone to regrow and fill the space or substitute the bone.. When dealing with age related degeneration, the solution is not as easy as in the replacement of missing parts case and it is necessary to replace the damage tissue with an alternative structure able to provide a degree of function equivalent to that of the damage tissue and also able to take the role of the affected tissue. Two of the most common age-related diseases of bone are arthritis and osteoporosis. The arthritis degrades joint’s cartilage and thus, the bones at joint rub against each other resulting in pain and decreased mobility. The osteoporosis is a phenomenon that makes bones brittle and it is also translated in a loss of bone mass. This brittleness and loosening of bone mass make bones prone to fracture 22. In these situations, it is impossible to repair the bone and the joints and a replacement is needed.
16 2. MATERIALS USED FOR BONE REPLACEMENT 2.1 Biomaterials 2.1.1 Definition There are many different definitions for a biomaterial: “Any substance (other than a drug), synthetic or natural, that can be used as a system or part of a system that treats, augments, or replaces any tissue, organ, or function of the body; especially, material suitable for use in prostheses that will be in contact with living tissue”. Miller-Keane Encyclopaedia and Dictionary of Medicine, Nursing, and Allied Health, Seventh Edition. © 2003 by Saunders, an imprint of Elsevier, Inc. All rights reserved. “Any synthetic material or device–eg implant or prosthesis-intended to treat, enhance or replace an aging or malfunctioning–or cosmetically unacceptable—native tissue, organ or function in the body. Cf Bioengineering, Breast implants, Hybrid artificial pancreas, Shiley valve, Teflon, Total hip replacement 2. A biomaterial used for its structural, not biological, properties–eg, collagen in cosmetics, carbohydrates modified by biotechnology to be used as lubricants for biomedical applications or as bulking agents in food manufacture” McGraw-Hill Concise Dictionary of Modern Medicine. © 2002 by The McGraw- Hill Companies, Inc. “A synthetic or semi synthetic material used in a biologic system to construct an implantable prosthesis and chosen for its biocompatibility.” Farlex Partner Medical Dictionary © Farlex 2012 “A systematically and pharmacologically inert substance designed for implantation within or incorporation with living systems”. Clemson University Advisory Board for Biomaterials Despite of the different definitions, there is one common characteristic: a biomaterial is a material that doesn’t belong to the body and is used to replace a specific function or a part of the body in a safe and physiologically acceptable way. 2.1.3 Use of biomaterials Biomaterials have been used for humans since more than 2000 years ago. Ancient civilizations as Aztecs used gold and silver to repair trephination defects, wood and
17 animal bones for dental substitution or fibres and tendons for sutures. During history man tried to replace damage parts with other devices made with gold, silver, iron, wood, etc. But they were unsuccessful because of the use of incorrect materials and infection after implantation due to no aseptically procedures. In the 1860’s the aseptic surgery technique was developed and since then there were an improvement in implanting devices. Thus, the use of stainless steel and engineered materials for biomedical applications increased. Many different materials are currently used as biomaterials: metals, ceramics, polymers, glasses and composite materials. These materials are not used as raw materials, depending on where they are going to be placed or the needed feature, they are moulded or machined and in a form of coatings, fibres, films or foams. The biomaterials are also used to replace many different parts in the body. In Figure 6 the different biomaterials, their principal properties and some of the medical devices made with them are shown 23,24. Fig.6 Different biomaterials with the pro's and con's and their applications in medicine. Ceramics very biocompatible brittle, not resilient, weak in tension DENTAL AND ORHTOPEDIC IMPLANTS Metals Strong, tough, ductile may corrode, dense, difficult to make JOINT REPLACEMENT, DENTAL ROOT IMPLANTS, PACER AND SUTURE WIRE, BONE PLATES AND SCREWS Polymers resileient, esasy to fabricate not strong, deforms with time, may degrade SUTURE, BLOOD VESSELS, LENSES, STURES, HIP SOCKET, EAR, NOSE Composites strong, tailor-made difficult to make BONE CEMENT, DENTAL RESIN Biomaterials
18 2.2 Metals used as biomaterials for prosthesis 2.2.1 Introduction As it was stated in point 2.1.3, with the development of the aseptic surgery technique in the 1860’s, there were an improvement in implanting devices and many efforts were done to improve the materials properties and their biocompatibility. 1900: Lane of England designed a fracture plate using steel. This fracture plate was improved by Sherman of Pittsburgh by eliminating sharp corners and adding vanadium to enhance toughness and ductility. 1924: Zierold discover Stellite (Co-Cr-based alloy) as the most inert material for implantation. 1929: Two new stainless steels were developed, 18-8 (18 w/o Cr, 8 w/o Ni) and 18- 8sMo (2-4 w/o Mo). They present high corrosion resistance, in particular the 18-8sMo to saline environments. 1932: A 19 w/o Cr, 9 w/ o Ni alloy named Vitallium was used for medical practice because of his light weight and resistance to corrosion. 1939: Tantalum was used in neurological and plastic surgery. Their poor mechanical properties and difficulties in processing devices with it made the material not suitable for orthopaedics. Late 1940’s: Initial commercial development of Ti as implant material. Late 1970’s: The use of Ti6Al4V in prosthesis grow quickly because of the high strength, light weight, formability and corrosion resistance. The alloys also presented good tissue tolerance. 2.2.2 Stainless Steels. Stainless steels were the first material used as a biomaterial. During history this material has been improved to be used as an implantable material. The first stainless steel used for implantation was 18-8 (18 w/o Cr, 8 w/o Ni). The addition of chromium enhanced the corrosion resistance 25. Another stainless steel used is the 18-8sMo (2-4 w/o Mo). The addition of molybdenum improved corrosion resistance to salt water 26. This
19 characteristic is very important because the body acts as a saline environment. The corrosion resistance to chloride solution of the alloy was enhanced by reducing carbon content to a 0.03 w/o. The 18-8 and 18-8sMo materials are the AISI 316 and 316L, respectively. They are the most widely used stainless steel for implants. The ASTM (American Society of Testing and Materials) recommends type 316L for implant fabrication. In table 2 the composition of the main stainless steel used for biomedical devices is shown. ELEMENT COMPOSITION (w/o) Carbon 0.03 max Manganese 2.00 max Phosphorus 0.025 max Sulfur 0.010 max Silicon 0.75 max Chromium 17.00-19.00 Nickel 13.00-15.00 Molybdenum 2.25-3.00 Nitrogen 0.10 max Copper 0.50 max Fe Balance Table 2. Composition in w/o of the AISI 316L stainless steel used for biomedical applications according to the ASTM 24. The elements with more presence in the alloy are chromium, nickel and molybdenum. Chromium is a reactive element, but if it is passivated is able to give high corrosion resistance. Nickel is used to stabilize the austenitic phase and enhances corrosion resistance. And molybdenum increases resistance to pitting corrosion in a saline environment. Despite of their good corrosion properties, stainless steel may corrode inside the body if they are exposed to high stress and/or hypoxia. For these reasons, the stainless steel is used for temporary devices such as fracture plates, screws and hip nails.
20 2.2.3. Co- Based Alloys There are two basic types of Co-based alloys: • CoCrMo: used to cast a product. Used in dentistry and in artificial joints. • CoNiCrMo: wrought by forging. Used for making stems of prosthesis subjected to high loads such as knee or hip joints. The ASTM recommends four types of Co-Based alloys for surgical implant applications. Co28Cr6Mo Castable Co20Cr15W10Ni Wrought Co28Cr6Mo Wrought Co35Ni20Cr10Mo Element Min Max Min Max Min Max Min Max Cr 27.2 30.00 19.00 21.00 26.0 30.0 19.0 21.0 Mo 5.0 7.0 - - 5.0 7.0 9.0 10.5 Ni - 2.5 9.0 11.0 - 1.0 33.0 37.0 Fe - 0.75 - 3.0 - 0.75 9.0 10.5 C - 0.35 0.05 0.15 - 0.35 - 0.025 Si - 1.0 - 1.0 - 1.0 - 0.15 Mn - 1.0 - 2.0 - 1.0 - 0.15 W - 0.2 14.0 16.0 - - P - 0.02 - 0.04 - - - 0.015 S - 0.01 - 0.03 - - - 0.01 N - 0.25 - - - 0.25 - - Al - 0.3 - - - - - Bo - 0.01 - - - - - 0.015 Ti - 1.0 Co Balance Table 3. Chemical composition of the Co-based alloys approved by the ASMT for biomedical applications 24. Although the ASMT recognizes this four Co-based alloys as good biomaterials, just two of them are mainly used in implant fabrications: CoCrMo and CoNiCrMo. Cobalt and chromium form a solid solution and the addition of molybdenum produce finer grains increasing strength after casting or forging. CoNiCrMo has a high degree of corrosion resistance to saline environment. However, implants of CoNiCrMo can only be fabricated by hot forging due to difficulties of cold working. Both alloys have similar abrasive wear properties although the CoNiCrMo is not suitable for joint prosthesis because it shows low frictional properties with itself and with other materials. Some studies suggest that this ions release due to friction might be harmful for the body 27.
21 The CoCr alloys were used in cast stem prosthesis but the stiffness of the alloy make the bone around the implant to resorb and there were also many stem fractures due to fatigue. Therefore, these alloys should be used for applications that require a long service life without fracture or stress fatigue. 2.2.4 Ti and Ti-Based Alloys In the late 1930s, the tolerance of titanium in cat femurs was discovered and since then, titanium has been used for implant fabrication. It was found that titanium had some advantages over stainless steel and Co-based alloys: it was lighter and had better mechanic-chemical properties. When compared to other metals used for medical devices, titanium and Ti-based alloys have lower elastic modulus, high strength and reduced ductility. However, the poor shear strength make titanium and Ti-based alloy not able to fabricate bone screws, plates, etc. The unalloyed titanium used for implant applications is classified in four grades depending on the impurities that it contains. Oxygen impurities are important because they play an important role in the ductility and the strength. The main Ti-based alloys used for implant fabrication are listed in the table below. Element Ti6Al4V Ti8Al17Nb Ti13Nb13Zr Ti12Mo6Zr2Fe N 0.05 0.05 0.05 0.05 C 0.08 0.08 0.08 0.05 H 0.0121 0.009 0.012 0.020 Fe 0.25 0.25 0.25 1.5-2.5 O 0.13 0.20 0.15 0.08-0.28 Al 5.5-6.5 5.5-6.5 - 5.5-6.75 V 3.5-4.5 - - - Ta 0.5 - - Zr - 12.5-14.0 5.0-7.0 Nb 6.5-7.5 12.5-14.0 - Mo - - 10.0-13.0 Ti Balance Table 4. Chemical composition of the Ti-based alloys approved by the ASMT for biomedical applications 24. Depending on the alloying elements, the properties of the alloys can be controlled. Aluminium is an α-stabilizer that increases the transformation temperature from α to β phase. On the other hand, V, Nb, Mn, Co, Ta, Cr and Cu are β-stabilizers that stabilize the beta-cubic phase and decrease the α-β transition temperature. Since oxygen
22 embrittles the alloy, the synthesis requires an inert atmosphere for high temperature processing or be forged below 925ºC. 2.2.5 Other metals Ni-Ti alloys: NiTi presents a special characteristic named shape memory effect (SME). This means that the material is able to return to its original shape when is deformed by heating above the transformation temperature or by releasing the load. The equiatomic NiTi alloy presents SME near room temperature. This special feature of Ni-Ti alloys makes them useful in applications such as stents and arrow intraortic balloon catheter amongst others. In the former application the transformation temperature feature plays a key role expanding the stent when placed into the arteries due to body temperature. In the latter application, the deformation capacity because of the loads exerted is crucial to allow movement through the meandering paths into the hart chamber. NiTi have been used in medicine since the late sixties 21. In addition to SME, NiTi alloy also exhibits ductility, high biocompatibility, superplasticity and high damping properties. All this make NiTi an attractive material for stents, tailored compressive fixation of bone fragments, vena cava filters, intracranial aneurysm clips, orthodontic dental arch wires, etc. Despite these promising features and applications, there is an increasing concern about Ni allergy 28–30. Tantalum: As titanium, this metal forms an oxide layer that makes them biocompatible 26,31 and prevents further oxygen penetration. Tantalum presents poor mechanical properties and high density. Is because of that, the uses of tantalum are restricted to wire sutures and arterial stents. Moreover, studies are being done with porous tantalum as bone graft substitute for the femoral head 32,33.
23 2.3 Titanium as a biomaterial 2.3.1 History Titanium was discovered in 1791 by William Gregor. In the 1940s Bothe et al. and Leventhal conducted animal experiments with stainless steel, CrCoMb and Ti to test their bioactivity. Titanium showed the best results. Since then the use of Ti as implant material increased. Titanium is the most widely used metal for medical devices. In the mid-1950s titanium started to be used in low-stress implants as heart valves. In the 1970s titanium was introduced for orthopaedic applications as an alternative of the CoCr. The lower elastic modulus, the elasticity and the good biocompatibility of titanium made him the perfect material for prosthesis 21,24,26. 2.3.2 What makes titanium biocompatible? Many materials oxidize in contact with liquids, such as body fluids. The zone in contact with the fluid is oxidized in a process called ionization. The bond between the oxidized layer and the non-oxidized layer gets weaker inducing the detachment of atoms. Atoms are released to the body fluids where they attach to proteins modifying them 21. This triggers the activation of defensive mechanism of the immune system and the metal is rejected. Titanium doesn’t present this behaviour; the bond between the oxidized layer and the non-oxidized one is stronger than in other metals. This peculiarity, avoid massive release of ions to the body minimizing the immune system response. This special feature of Ti makes the difference with the other metals used as biomaterials. 2.4 Titanium alloys In an attempt to improve the Young’s modulus, strength/ductility balance, fatigue strength, fracture toughness and wear resistance, titanium was alloyed with other elements. Table 5 show some of the titanium alloys developed for medical applications.
30 Fig.7 Toxicity of some pure metals regarding the growth of two different types of cells when in contact with them. Adapted from 35. 3.2.1 Allergy However, not all the ions are toxic. The ions released through sweat and other body fluids to the body may act as allergens. Allergy to metal ions is of high concern in Europe during the last decades. In figure 8 the percentage of allergy for some common metals is represented. One of the allergies that have increased more is the allergy to Ni. As it can be seen in figure 8 during the last years the increase has been dramatic. About the 20% of young females and 4% of young males suffer from it 26.
31 Fig.8 Percentage of allergy caused for each metal and the evolution of Ni allergy in population. Adapted from 26. There are few reports stating the effects of Ni release and their consequences, but above certain concentrations Ni triggers severe local tissue irritation, necrosis and toxic reactions 26,28,30. Studies made with NiTi dental implants, reported that the amount of ions released to the body are very low, and thus, the organism is capable to resorb it 29. Although Ni dental implants allergy has not been demonstrated in a clear way, Ni should be treated as a potential allergen and thus, be avoided in future biomaterials. 3.3 Stress shielding effect The properties of the materials used to bone replacement don’t match those of bone. In Fig 9, the elastic moduli of the different alloys used for bone replacement are shown. It is easy to see that all of them have greater elastic modulus than bone.
32 Fig.9 Modulus of elasticity of the most common biomedical alloys. Adapted from 44. Because of this higher modulus, the implant takes some of the loads that should be going to the bone. This phenomenon is called stress shielding effect. In replacement prosthesis, the stem is introduced into the bone canal and as the stem is stiffer, it shares the load and carrying capacity of bone. According to bone remodelling process explained in point 1.4, bone remodels depending on the loads applied. If fewer loads are applied, bone suffers a resorption, adapting itself to the new loads demand. In Fig. 10 b, the zone of bone with more stress demand is darker than the one at which the implant shares the loads. The consequence of the stress shielding effect is a reduction of bone density around the implant which leads to implant loosening. To avoid this non desirable effect, alloys with elastic modulus lower than the currently used ones are being developed and investigated 28.
33 Fig.10 Scheme of the loads transferred to bone and bone behavior during stress shielding effect. Adapted from 28. 3.4 Poor osseointegration The success of an implant depends on the degree of osseointegration. This concept was first introduced by Professor Per-Ingvar Branemark in the 1950's when he discovered the ability of bone to grow on titanium. Osseointegration is defined as "the formation of a direct interface between an implant and bone, without intervening soft tissue" 45. In a poor osseintegration scenario, the implant is not integrated with the surrounding bone and results in loosening of the implant with the consequent revision surgery. Revision surgery is not desirable for three reasons: a) is expensive; b) causes pain to the patient; c) the ratio of success is low 46. An appropriate surface chemistry, roughness and topography of the implant are of paramount importance to achieve good osseointegration. Implant should be designed with the aim to avoid fibrin adhesion, blood vessel growth and micromotions. Micromotions are understood as relative movements between the implant and the bone with which it has direct contact.
34 4. MIMICKING EXTRACELLULAR MATRIX The extracellular component of bone is very important for the bone remodelling process. Bone healing related to implants involves many cellular and extracellular biological events taking place at bone-implant interface that end when the implant is covered with newly formed bone. This phenomenon is called osseointegration. The biological events that take give rise to osseointegration are similar to those of bone healing process at least in terms of initial host response. The process is regulated by growth and differentiation factors released by the activated blood cells at bone-implant interface. After one day of implantation, osteoblasts and mesenchymal stem cells migrate and attach to the implant surface. These cells release bone-related proteins and create a noncollagenous matrix layer on the implant material that regulates cells adhesion and binding of minerals 28. The early deposition of bone on the implant surface is called peri-implant trabecular bone and ensures the biological fixation of the implant. 4.1 Extracellular matrix The extracellular matrix (ECM) is secreted by cells to create a proper environment where grow and communicate between them. This environment is formed by proteins, minerals, sugars and fluids. Once the cells are settled on the ECM, they can by themselves make new ECM according to their necessities or remodel the one is already made 47. 4.1.1 Functions The ECM is a non-cellular component of all tissues and organs, gives physical support for the cellular constituents and initiates biochemical and biomechanical cues needed for tissue morphogenesis, differentiation and homeostasis. Bone ECM gives tissue's chemical and mechanical properties, regulates bone cells and is a reservoir for ions 48. Tensile and compressive strength and also elasticity, depends
35 on the ECM. Protection is mediated by the ECM as well. The ECM has a buffering action that maintains extracellular homeostasis and water retention. The morphological organization and the physiological function of the tissue are also directed by the ECM. It binds growth factors (GFs) and interacts with cell-surface receptors to elicit signal transduction and regulate gene transcription. On the ECM one can find specific protein sequences recognized by cell membrane receptors such as integrins, discoidin domain receptors and syndecans that mediate cell adhesion. Adhesion plays an important role in cytoskeletal coupling to the ECM and in cell migration through the ECM. 4.1.2 Composition Bone ECM is formed of osteoid. The osteoid is an organic phase which constitutes approximately the 20% of bone mass and a mineral phase. In bone ECM there are growth factors and bone morphogenic proteins (BMP). In table 6, there is a scheme on which the type of molecule of the ECM and its role in ECM function is represented. Table 6. Scheme of the constituents of the ECM and their functions 49.
36 4.1.2.1 Collagen Amongst structural ECM proteins, collagen is the most abundant one. In mammalians there are up to 28 triple helical proteins called collagens. Collagens are present in many parts of the body and they are important for a many different functions such as tissue scaffolding, cell adhesion, cell migration, cancer, angiogenesis, tissue morphogenesis and tissue repair. Collagen associates with elastin to recover its coiled structure after being stretched. The stretching properties of elastin are limited by tight association with collagen fibrils. The way collagen fibrils are aligned is determined by connective tissue cells. They apply tension on the matrix organizing collagen fibrils into sheets and cables. In a tissue there is a mix of different types of collagen, although one type usually predominates. The different types of collagens are classified by function and domain homology 48,50. Mainly there are two big groups of collagens: heterotrimerics and homotrimerics. The former are collagens with two identical α chains and a third chain that differs; the latter have three identical α chains. The collagen predominant in bone is collagen type I which is heterotrimeric and fibrilforming. This type of collagen has an important role in tissue. It is the principal tensile element of tendon, cartilage, bone and skin. As can be seen in Fig. 11, collagen type I is formed by three polypeptide α chains linked by hydrogen bonds, exhibiting an extended polyproline-II conformation, a right-handed supercoil and a one-residue stagger between adjacent chains 51. Fibroblasts, condroblasts and osteoblasts synthesise collagen type I.
37 Fig.11 Image of the collagen structure. Adapted from 51. The integrin recognition adhesion sequences of collagen are located in the triple helical domain. The adhesion sequence for collagen is the peptide -Phe-O-Gly-Arg (GFOGER), where the O is hydroxyproline which signals the A-domain α1 integrins 51. 4.1.3.2 Fibronectin Fibronectin (FN) is a protein found in plasma and other body fluids and is a part of the ECM as well. FN mediates many different cellular interactions with the ECM and is necessary in cell adhesion, migration, growth and differentiation 52. Most of cell types express FN. Fibronectin is composed of two equal subunits of approximately 250kDa linked covalently near the C-terminus by a pair of disulphide bonds. There are three domain types of repeating units that form each monomer. The repeats are named type I, II and III. Fibronectin molecule presents in the domain I and III an heparin fixation zone (Heparin binding) and also in the domain III a zone for cell adhesion (See Fig.12).
38 Fig.12 Simplified molecule of Fibronectin. Each domain of FN is represented and the main characteristic of each domain. Adapted from 53. FN can be a ligand for a dozen members of the cell-surface heterodimeric receptors that link the ECM with the intracellular cytoskeleton which are called integrins (see Fig.13). Integrins bind to the FN Arg-Gly-Asp (RGD) sequence, which is located in the FN repeat III10. RGD is the most common sequence for cell adhesion through integrin signalling. However, it is not a specific sequence since it is recognized for several integrin types signalling only some aspects of cell behaviour (Dee et al). The presence of additional sequences is required for specifically recognition by concrete integrin types. For instance, FN presents a PHSRN (Pro–His–Ser–Arg–As) sequence belonging to the III9 domain 53. The PHSRN is necessary to bond RGD to the integrin α5β1 which increase its affinity forty-fold compared to RGD alone 54,55. RGD and PHSRN together give a stable adhesion to the integrin α5β1. Fibronectin also interact with heparan sulfate proteoglycans (HSPGs) via the heparin binding domains 49. HSPGs take part in the focal adhesions and stress fibres formation. When syndecan-4 (a membrane HSPG) binds to FN, interacts with integrins and induces the formation of focal adhesions and stress fibres. The syndecan-4 and syndecan-1 also play a role in the regulation of the activation of the αvβ3 and αvβ5. The extracellular domain of the proteoglycan interacts with the β-integrin subunit 53.
39 Some studies have shown that i) the FN heparin binding domain enhances cell adhesion and proliferation of osteoblasts and ii) the RGD-containing central cell-binding domain of FN together with the Heparin binding domain of FN enhances cell adhesive and spreading activities 56. 4.1.4 Adhesion process To make adhesion possible, cell membrane integrins must recognize a concrete amino . Briefly the mechanism of how RGD binds to integrins can be explained as follows (see Fig.13): the interface between the α and β subunits is the area of RGD recognition. The R residue must fit into a cleft located in the α subunit, whilst the D coordinates a cation bound in a von Willebrand factor domain in the β subunit. The process of integrin adhesion is very important for cell survival. Integrins are important for cellular processes establishing the unions between the ECM and the cytoskeleton. This linking acts as a mechanotransductor that regulate cell adhesion and spreading 54,57. Fig.13 Integrin domain structure. Adapted from 54. 4.1.4.1 Integrins The interactions between cells and cell-extracellular matrix are essential to cell motility, proliferation, differentiation, regulation of gene expression and cell viability. Integrins are composed of two units: the α and the β unit. There are 11 variations of α and 6 of β (see Fig.14). This makes a great variety of integrins, and thus cells are able to recognize different adhesion proteins (ligands) and different adhesion motifs 58.
46 4.3.3 Recombinant proteins Despite the efforts made to mimic ECM and its synergy sites with short chains of peptides, the bond is not as stable as with the full ECM proteins. This is because of two reasons: i) the high sensitivity of integrin's bond to conformation and orientation of the bonding motifs, ii) the less integrin specificity of the short peptides. The recombinant protein technique 57,71 arises as a potential solution to the weak points of peptides. When dealing with recombinant proteins the signalling zone of the ECM protein of interest can be spanned and thus, their properties and functions 76. With these type of motifs, the antigenicity of the full ECM proteins is reduced and the domains that may trigger undesirable cell responses as well. Another strong point of recombinant proteins is that some characteristics as protein immobilization, orientation or activity may be modulated by modification of some amino acids without affecting their integrin bond effectiveness. Moreover, there is the possibility of combine sequences, join different fragments, etc.
47 5. BIBLIOGRAPHY 1. Marieb, E. N. Human anatomy and physiology. 995, 60 (The Benjamin/Cummings, 1989). 2. Raisz, L. G., Rodan, G. A. & Bilezikian, J. P. Principles of bone biology. 2, 1696 (Academic Press, 2002). 3. Kopperdahl, D. L., Roberts, A. D. & Keaveny, T. M. Localized damage in vertebral bone is most detrimental in regions of high strain energy density. J. Biomech. Eng. 121, 622–8 (1999). 4. Nagaraja, S., Couse, T. L. & Guldberg, R. E. Trabecular bone microdamage and microstructural stresses under uniaxial compression. J. Biomech. 38, 707–16 (2005). 5. Taylor, D. A crack growth model for the simulation of fatigue in bone. Int. J. Fatigue 25, 387–395 (2003). 6. Ruimerman, R., Hilbers, P., van Rietbergen, B. & Huiskes, R. A theoretical framework for strain-related trabecular bone maintenance and adaptation. J. Biomech. 38, 931–41 (2005). 7. Schaffler, M. Fatigue and repair in bone. Int. J. Fatigue 22, 839–846 (2000). 8. Knothe Tate, M. L., Adamson, J. R., Tami, A. E. & Bauer, T. W. The osteocyte. Int. J. Biochem. Cell Biol. 36, 1–8 (2004). 9. Deans, R. J. & Moseley, A. B. Mesenchymal stem cells: Biology and potential clinical uses. Exp. Hematol. 28, 875–884 (2000). 10. Caplan, A. I. & Bruder, S. P. Mesenchymal stem cells: building blocks for molecular medicine in the 21st century. Trends Mol. Med. 7, 259–264 (2001). 11. Maxson, S., Lopez, E. A., Yoo, D., Danilkovitch-Miagkova, A. & LeRoux, M. A. Concise Review: Role of Mesenchymal Stem Cells in Wound Repair. Stem Cells Transl. Med. 1, 142–149 (2012). 12. Manolagas, S. C. Birth and Death of Bone Cells: Basic Regulatory Mechanisms and Implications for the Pathogenesis and Treatment of Osteoporosis. Endocr. Rev. 21, 115–137 (2000).
48 13. Crockett, J. C., Rogers, M. J., Coxon, F. P., Hocking, L. J. & Helfrich, M. H. Bone remodelling at a glance. J. Cell Sci. 124, 991–998 (2011). 14. Hill, P. A. Bone remodelling. J. Orthod. 25, 101–107 (1998). 15. Noble, B. S. & Reeve, J. Osteocyte function, osteocyte death and bone fracture resistance. Mol. Cell. Endocrinol. 159, 7–13 (2000). 16. Fernández-Tresguerres Hernández-Gil, I., Alobera Gracia, M. A., del Canto Pingarrón, M. & Blanco Jerez, L. Physiological bases of bone regeneration I. Histology and physiology of bone tissue. Med Oral Patol Oral Cir Bucal. 11, E–147–E–151 (2006). 17. Fernández-Tresguerres Hernández-Gil, I., Alobera Gracia, M. Á., del Canto Pingarrón, M. & Blanco Jerez, L. Physiological bases of bone regeneration II. The remodeling process. Med Oral Patol Oral Cir Bucal. 11, E–151–E–157 (2006). 18. Van Oers, R. F. M., Ruimerman, R., Tanck, E., Hilbers, P. A. J. & Huiskes, R. A unified theory for osteonal and hemi-osteonal remodeling. Bone 42, 250–9 (2008). 19. Wolff, J. The Classic: On the Inner Architecture of Bones and its Importance for Bone Growth. Clin. Orthop. Relat. Res. 468, 1132–1528 (2010). 20. Ruff, C., Holt, B. & Trinkaus, E. Who’s afraid of the big bad Wolff?: ?Wolff's law? and bone functional adaptation. Am. J. Phys. Anthropol. 129, 484–498 (2006). 21. Titanium in medicine :material science, surface science, engineering, biological responses, and medical applications. (Springer, 2001). 22. Cambridge, U. of. Structure of bone and implant materials. Bone replacement. at <http://www.doitpoms.ac.uk/tlplib/bones/bone-replacement.php> 23. University of Washington. An introduction to biomaterials. (2004). at <http://www.uweb.engr.washington.edu/research/tutorials/introbiomat.html> 24. Park, J. B. & Lakes, R. S. Biomaterials :an introduction. 3, 561 (Springer, 2007). 25. Ratner, B. D. Biomaterials science :an introduction to materials in medicine. 2, 851 (Elsevier Academic, 2004).
49 26. Niinomi, M. Recent Metallic Materials for Biomedical Applications. Metall. Mater. Trans. A 33, 477 (2002). 27. Swierenga, S. H. H., Gilman, J. P. W. & McLean, J. R. Cancer risk from inorganics. Cancer Metastasis Rev. 6, 113–154 (1987). 28. Geetha, M., Singh, A. K., Asokamani, R. & Gogia, A. K. Ti based biomaterials, the ultimate choice for orthopaedic implants – A review. Prog. Mater. Sci. 54, 397–425 (2009). 29. Uo, M., Watari, F., Yokoyama, A., Matsuno, H. & Kawasaki, T. Dissolution of nickel and tissue response observed by X-ray scanning analytical microscopy. Biomaterials 20, 747–755 (1999). 30. Yang, K. & Ren, Y. Nickel-free austenitic stainless steels for medical applications. Sci. Technol. Adavanced Mater. 11, 1–13 (2010). 31. Matsuno, H., Yokoyama, A., Watari, F., Uo, M. & Kawasaki, T. Biocompatibility and osteogenesis of refractory metal implants, titanium, hafnium, niobium, tantalum and rhenium. Biomaterials 22, 1253–1262 (2001). 32. Cohen, R. A porous tantalum trabecular metal: basic science. Am. J. Orthop. (Belle Mead. NJ). 31, 216–217 (2002). 33. Levine, B. R., Sporer, S., Poggie, R. A., Della Valle, C. J. & Jacobs, J. J. Experimental and clinical performance of porous tantalum in orthopedic surgery. Biomaterials 27, 4671–4681 (2006). 34. Wang, K. The use of titanium for medical applications in the USA. Int. Symp. Metall. Technol. Titan. Alloy. 213, 134–137 (1996). 35. YUMOTO, S. et al. ALUMINUM NEUROTOXICITY IN THE RAT BRAIN. Int. J. PIXE 02, 493–504 (1992). 36. Amick, D. D. Characterization of TiNbHf alloys for potential medical dental applications. (1993). 37. Hao, Y. L. et al. Super-elastic titanium alloy with unstable plastic deformation. 87, (2005).
50 38. Guo, S. & DiPietro, L. A. Factors Affecting Wound Healing. J. Dent. Res. 89, 219–229 (2010). 39. Anderson, J. M., Rodriguez, A. & Chang, D. T. Foreign body reaction to biomaterials. Innate Adapt. Immune Responses Tissue Eng. 20, 86–100 (2008). 40. Anderson, J. M. Biological responses to materials. Annu. Rev. Mater. Res. 31, 81–110 (2001). 41. The recombinant protein handbook. Protein amplification and simple purification. 42. Barbara Rolfe, J. et al. Regenerative Medicine and Tissue Engineering - Cells and Biomaterials. (InTech, 2011). doi:10.5772/837 43. Puleo, D. A. & Bizios, R. Biological Interactions on Materials Surfaces. (Springer, 2009). doi:10.1007/978-0-387-98161-1-7 44. Setcos, J. C., Babaei-Mahani, A., Silvio, L. Di, Mjör, I. A. & Wilson, N. H. F. The safety of nickel containing dental alloys. Dent. Mater. 22, 1163–1168 (2006). 45. Ridzwan, M. I. Z., Shuib, S., Hassan, A. Y., Shokri, A. A. & Mohamad Ibrahim, M. N. Problem of Stress Shielding and Improvement to the Hip Implant Designs: A Review. J. Med. Sci. 7, 460 (2007). 46. Miller, B. F., Keane, C. B., Klajn, D. S. & Boxaca, M. Diccionario enciclopédico de enfermería. 5a, 1524 (Panamericana, 1996). 47. Mavrogenis, A. F., Dimitriou, R., Parvizi, J. & Babis, G. C. Biology of implant osseointegration. J. Musculoskelet. Neuronal Interact. 9, 61–71 (2009). 48. Cassimeris Lingappa, Vishwanath R., Plopper, George.,Lewin, Benjamin.,, L. Lewin’s cells. (Jones and Bartlett Publishers, 2011). 49. Shekaran, A. & García, A. J. Extracellular matrix-mimetic adhesive biomaterials for bone repair. J. Biomed. Mater. Res. Part A 96A, 261–272 (2011). 50. Alberts, B. & Walter, P. Molecular biology of the cell. 4th, 1,36,49,1463 (Garland, 2002).
51 51. Kadler, K. E., Baldock, C., Bella, J. & Boot-Handford, R. P. Collagens at a glance. J. Cell Sci. 120, 1955–1958 (2007). 52. Humphries, J. D., Byron, A. & Humphries, M. J. Integrin ligands at a glance. J. Cell Sci. 119, 3901–3903 (2006). 53. Pankov, R. & Yamada, K. M. Fibronectin at a glance. J. Cell Sci. 115, 3861– 3863 (2002). 54. Sechler, J. L., Corbett, S. A. & Schwarzbauer, J. E. Modulatory Roles for Integrin Activation and the Synergy Site of Fibronectin during Matrix Assembly. Mol. Biol. Cell 8, 2563–2573 (1997). 55. Wierzbicka-Patynowski, I. & Schwarzbauer, J. E. The ins and outs of fibronectin matrix assembly. J. Cell Sci. 116, 3269–3276 (2003). 56. Sarrazin, S., Lamanna, W. C. & Esko, J. D. Heparan Sulfate Proteoglycans. Cold spring Harb. Perspect. Biol. 3, (2011). 57. García, A. J., Schwarzbauer, J. E. & Boettiger, D. Distinct Activation States of α5β1 Integrin Show Differential Binding to RGD and Synergy Domains of Fibronectin†. Biochemistry 41, 9063–9069 (2002). 58. Geiger, B., Spatz, J. P. & Bershadsky, A. D. Environmental sensing through focal adhesions. Nat. Rev. Mol. Cell Biol. 10, 21–33 (2009). 59. Ruoslahti, E. Integrins. J. Clin. Invest. 87, 1–5 (1990). 60. Petit, V. & Thiery, J.-P. Focal adhesions: Structure and dynamics. Biol. Cell 92, 477–494 (2000). 61. Hlady, V. & Buijs, J. Protein adsorption on solid surfaces. Curr. Opin. Biotechnol. 7, 72–77 (1996). 62. Rabe, M., Verdes, D. & Seeger, S. Understanding protein adsorption phenomena at solid surfaces. Adv. Colloid Interface Sci. 162, 87–106 (2011). 63. Nakanishi, K., Sakiyama, T. & Imamura, K. On the adsorption of proteins on solid surfaces, a common but very complicated phenomenon. J. Biosci. Bioeng. 91, 233–244 (2001).
52 64. Cai, K. et al. Surface functionalized titanium thin films: Zeta-potential, protein adsorption and cell proliferation. Colloids Surfaces B Biointerfaces 50, 1–8 (2006). 65. Xiao, S.-J., Textor, M., Spencer, N. D. & Sigrist, H. Covalent Attachment of Cell-Adhesive, (Arg-Gly-Asp)-Containing Peptides to Titanium Surfaces. Am. Chem. Soc. 14, 5507–5516 (1998). 66. Zhu, M., Lerum, M. Z. & Chen, W. How To Prepare Reproducible, Homogeneous, and Hydrolytically Stable Aminosilane-Derived Layers on Silica . Langmuir 28, 416–423 (2011). 67. Hanawa, T. An overview of biofunctionalization of metals in Japan. J. R. Soc. Interface 6, S361–S369 (2009). 68. Morra, M. Biomchemical Modification of Titanium Surfaces: Peptides and ECM Proteins. Eur. Cells Mater. 12, 1–15 (2006). 69. LeBaron, R. G. & Athanasiou, K. A. Extracellular Matrix Cell Adhesion Peptides: Functional applications in Orthopedic Materials. Tissue Eng. 6, 85–103 (2000). 70. Kim, H.-E., Kim, H.-W. & Jang, J.-H. Identification and characterization of a novel heparin-binding peptide for promoting osteoblast adhesion and proliferation by screening an Escherichia coli cell surface display peptide library. J. Pept. 15, 43 (2008). 71. García, A. J. & Reyes, C. D. Bio-adhesive Surfaces to Promote Osteoblast Differentiationand Bone Formation. J. Dent. Res. 84, 407 (2005). 72. Arnold, M. et al. Activation of Integrin Function by Nanopatterned Adhesive Interfaces. ChemPhysChem 5, 383–388 (2004). 73. Cavalcanti-Adam, E. A. et al. Cell Spreading and Focal Adhesion Dynamics Are Regulated by Spacing of Integrin Ligands. Biophys. J. 92, 2964–2974 (2007). 74. Keselowsky, B. G., Collard, D. M. & García, A. J. Integrin binding specificity regulates biomaterial surface chemistry effects on cell differentiation. Proc. Natl. Acad. Sci. U. S. A. 102, 5953–5957 (2005).
53 75. Deber, C. M., Madison, V. & Blout, E. R. Why cyclic peptides? Complementary approaches to conformations. Acc. Chem. Res. 9, 106–113 (1976). 76. Sørensen, H. P. & Mortensen, K. K. Advanced genetic strategies for recombinant protein expression in Escherichia coli. J. Biotechnol. 115, 113–128 (2005). 77. Gonzalez, M., Peña, J., Manero, J. M., Arciniegas, M. & Gil, F. J. Desing and Characterization of New Ti-Nb-Hf alloys. J. Mater. Eng. Perform. 18, 490 (2009).
54
55 II Materials and Methods
62 2. MECHANICAL AND MICROSTRUCTURAL CHARACTERIZATION OF THE ALLOY 2.1 Nanoindentation Nanoindentation6 is a simple technique on which the forces applied are in the order of nano Newtons (nN) and the depth penetrations are in the order of nanometres. This technique is based on contact mechanics. The main objective of this kind of text is obtaining the elastic modulus and the hardness of a given material with unknown properties. One of the advantages of this technique is that it is a non-destructive assay and small samples are needed reducing costs. The typical test consists on apply a stress on the indenter which is in contact with the sample surface. The load and the depth of indentation are recorded whilst the load goes from an initial value of zero to a maxim value and then returns to zero. Depth indentation and indenter geometry give a direct measure of the contact angle at full loading. From this measurement, mean contact pressure can be obtained and therefore, material hardness. An estimation of the material elastic modulus can be obtained analysing the initial portion of the elastic response during unloading. There is a great variety of indenter’s geometry, although the spherical tip and the Berkovich tip are the most used for nanoindentation. The determination of the contact area, the hardness and the elastic modulus is based on the Hertz elastic contact theory (Eq. 2.1). P= ∗∙√∙ℎ Eq. 2.1 The most studied case and thus, the better know is the contact between a rigid sphere and a flat surface (Fig.18). According to Fisher-Cripps6 approach, the maximum depth or total indentation (ht) is obtained at maximum load (Pmax). When this load is removed completely from the surface, a residual depth remains (hr). If maximum load is applied again, the loading is elastic until a distance (he) equal to the difference between the total indentation depth (ht) and the residual depth (hr). During the loading process
63 may be an elastic response at the beginning followed by an elastic-plastic deformation at high loads. R is the radius of curvature combined with the indenter radius (Ri) and the radius of the residual indentation (Rr). This radius is higher than the indenter radius due to the deformation that takes place on it. ∗ (Eq. 2.2) represents de effective modulus of the system, which combines the elastic properties of the indenter and of the sample under study taking into account the indenter’s deformation. Fig.18 (a) Representation of the contact between a rigid spherical indenter and a flat surface. (b) Loading-displacement curve for an elastic-plastic sample loaded with an spherical indenter. Adapted from (14) ∗ ′ Eq. 2.2 E and ν are the elastic modulus and the Poisson’s coefficient of the material under study; E’ and ν’ are the elastic constants of the indenter. For a diamond indenter the values are 1140 GPa and 0.07, respectively. The mean pressure contact is often called “indentation stress” and the relationship between contact area and contact radius (Eq. 2.3), “indentation deformation”. 2ℎ ! Eq. 2.3
64 This relationship leads us to think in a response of similar nature than that obtained by means of a classic tensile test and compression test. In both cases a linear response is given for a totally elastic condition. Despite this, with nanoindentation it is possible to obtain data regarding the elastic-plastic properties of the material that cannot be obtained with the conventional tensile tests. Depending on the parameters under study, different types of assay could be done. To perform the experiments, 1mm thick slide of material was cut and mirror polished. To determine the existence of phase transformation during loading and unloading process, 5 cycles of loading-unloading at an indentation depth of 300nm were done. To determine the elastic modulus and the hardness, 10 cycles of loading-unloading at an indentation depth of 2000nm were done. In this case, the first 100nm of the loading curve were taken and the resultant curve was fit with the Hertz curve. 2.2 Tensile testing The tensile testing is the most commonly used method to determine different mechanical properties such as the Elastic modulus, the ultimate strength, elastic deformation, etc. One of the advantages of this test is its standardization that permits to achieve the most reliable results. During the test, a cylindrical specimen is pulled for both sides until the sample changes its shape or fractures (Fig. 19). Fig.19 a) Image of the INSTRON 8500 DIGITAL CONTROL model 1342 used for testing. b) Evolution of the specimen test during tensile test7.
65 Six samples were machined according to the ASMT E8M-04 standard (Fig. 20). The tests were performed in an 8500 Digital Control testing machine model 1342 (Instron, Norwood, MA, USA). The specimens were pulled at 1.5•10-4s-1, according to the ASMT standard. Fig.20 Dimensions of the tensile test specimen according to the ASMT E8M-04. 2.3 Optical microscopy The determination of the grain size was carried out by means of a routine based on the ASTM E112 96 Standard Test Methods. The results were analyzed with Omnimet software (Buheler Company, Lake Bluff, IL, USA). The alloy was cut into a 1mm thick slice and mechanically polished with colloidal silica suspension achieving a mirror polished surface. The etching of the samples was carried out using Kroll’s reactive which composition is HF (48%), and HNO3 (65%) in an aqueous solution. A GX51 microscope (Olympus Corporation, Orangeburg, NY, USA) was used to study the microstructure of the material. Images were taken in a digital format and processed to eliminate the artifacts due to spots, corrosion points or polishing gridding pores, since these artifacts may lead to an error during the routine. To process the images the grain borders were drawn, then the background color was determined as well as the area to process. The outside frame was cleared out and the border grain eliminated. After that, the bit plane was thickened, filled and featured.
66 2.4 Transmission electron microscopy (TEM) This technique is based on Bragg’s Law. The source of light is an electron beam generated by a heated tungsten filament. The beam is exposed to a high voltage and accelerated. Beam’s current density spans a range between 100 and 200 keV. The beam passes through an ultrathin material sample. When trespassing, the electron beam interacts with the sample. Some of the electrons are absorbed and others are dispersed, loosing velocity and changing the trajectory. To visualize the electron beam after it passed through the sample, a magnetic lens is used. With the lens, the beam is focused, magnified and projected on a fluorescence display. The dark field images are generated from the diffracted electrons and the bright field images are obtained from the electrons that have passed through the sample. The samples to be studied must be transparent to the electron beam, between 10 and 500 nm thick, in order to obtain valid results. TEM technique allows the possibility to obtain the diffraction patterns of selected areas of the sample. The existing diffraction patterns and the net parameters of the structures, permit to index the diagrams obtained. In other words, TEM allows us to know the crystallography of the material under study. The microscope used was a JEM 1200 EXII (JEOL, Tokyo, Japan) (Fig.21) with a beam power of 120 kV and a calibrated chamber constant of λL=2.606 mm·nm. The chamber constant was calculated by TlCl powders (CsCl type, a=0.3841 nm).
67 Fig.21 a) Microscope JEOL 1200 EXII used in the assay. b)Electropolishing equipment Tenupol-3 by Struers. c) Sample after the electropolishing ready to be used in the TEM. The alloy was cut into a 1 mm thick slice and mechanically polished with a 240 paper grid achieving a 100 µm thickness. Afterwards, 3mm diameter discs were die-cast with a Model 659 Disc Punch (Gatan, Inc. Pleasanton, CA, USA). Once the discs were cut, they were polished by the jet-polishing method with a Tenupol-3 equipment (Struers, Denmark) at 10ºC and at a voltage of 40 V. The electrolyte used was composed by 40% 2-butoxyethanol, 40% methanol and 10% mL perchloric acid in an aqueous solution. The jet polishing technique enables de polishing of metal disks simultaneously from both sides and automatically stops the polishing operation when perforation occurs. 2.5 X-Ray diffraction The non-destructive X-Ray diffraction technique was used to determine alloy’s crystallography. When a laser beam comes into contact with a crystalline material, the beam diffraction takes place. By means of Bragg’s Law (nλ=2dsen (θ) the X-Ray diffraction wave length and the interatomic distance are related with the incidence angle of the diffracted beam (Fig. 22). a b c
68 Fig.22 Scheme of the X-ray beam diffraction on a crystalline material and the relation with the interatomic distance. Adapted from http://tap.iop.org Fig.23 Equipment used in the X-ray diffraction assays. Difractometer D8 Advance from Brueker. The alloy was cut into a 1mm thick sheet of and polished for one side with a 1200grit paper. It is important that the samples have parallel sides for the proper running of the technique. The samples were analyzed using a Difractometer D8 Advance (Bruker) equipment (Fig. 23). A Cu Kα (λ=1.542Å) radiation was applied because the wave length is similar to the distance between planes in the crystalline net. Measurements were taken with a step size of 0.05º and with an intensity normalized to the time of counting (counts per second). The Power Diffraction File (PDF) data base was used to identify and to index the phases present in the alloy. In the PDF the diffraction patterns of known materials are compiled and the crystalline structure, reticular parameters and diffraction plains are
69 detailed. The indexation of the phases is done by direct comparison between the PDF’s spectra and the ones obtained experimentally. Due to the novelty of the alloy there are no diffraction patterns available. The patterns used where those from Ti (α and β), Nb and a quenched TiNb alloy with up to 12% content of Nb. 3. PHYSICO-CHEMICAL CHARACTERIZATION OF THE ALLOY Some studies suggest that the type, quantity and conformation of the adsorbed proteins on a material, are influenced by the underlying substrate8–10. In other words, surface energy, roughness and chemistry are involved in the proteins adsorbed and thus, in the subsequent cell adhesion. In this section, the different methods used to determine the physic-chemical properties of the developed alloy are described. 3.5 Contact angle The solid surface tension of a given material can be determined by different methods, but one of the most extended ones is the contact angle. The strong points of this method are the simplicity, the small volume of liquid needed and an accuracy of approximately ±2º. But it also possess weak points as the small angles are difficult to measure, the measurement relies on the consistency of the operator to assign the tangent line and impurities onto the surface of the sample can alter the measurements11,12. The technique is based on Young’s equation. Young described in 1805 the contact angle of a liquid drop on an ideal solid surface by the mechanical equilibrium of the drop under the action of three interfacial tensions: • γlv: liquid–vapor γ • sv: solid–vapor • γsl: solid–liquid
70 Θγ is the so called Young’s contact angle (Fig.24) Fig.24 Representation of the angles formed between a liquid drop and a solid surface. Adapted from12 According to this, there is a correlation between the contact angle and the interfacial tensions (Eq. 1.1), but only two parameters can be measured; the contact angle and the liquid-vapor phase tension. γlv cos θγ= γsvγsl Eq.3.1 There are different methods that correlates contact angles with the surface energy of the sample11. In this thesis, the Owens and Wendt approach was used. According to Owens and Wendt, dispersion and hydrogen bonding forces may operate on a surface and the surface tension is being composed of two components: dispersive surface tension (γd) and surface tension due to hydrogen and dipole-dipole interactions (γh). γ= γd +γh Eq.3.2 Taking into account the forces that operate at the surface they postulated: γsl= γs+ γl - 2 "#$"%$-2 "#&"%& Eq.3.3 If equation 1.3 is combined with equation 1.1, the following relationship is obtained: γl (1+ cos θγ) = 2 "#$"%$-2 "#&"%& Eq. 3.4 In equation 1.4 there are two unknown parameters: "#$ and"' ℎ, thus be having one equation with two unknown quantities. Is because of that, two different liquids should be used to make the contact angle measurements for the same surface. Having the
71 contact angle of the same material for different liquids, two simultaneous equations could be solved. The equipment used to perform the assays was an Oca 15+ (Dataphysics, Filderstadt, Germany) (Fig. 25). It is provided with a horizontal stage to place the samples, an illumination source and a telescope with an incorporated protractor and a camera to take photographs of the drop profile. Fig.25 Contact angle measurement equipment Oca15+ from Dataphysics (www.dataphysics.de). The materials tested were Ti cp, Ti6Al4V and the developed alloy in the thesis. All of them were cut into 2 mm thick discs and were mirror polished. Measurements were done in triplicate using three discs for each material type.. All measurements were made the same day and under the same conditions. The liquids used for the measurements were MilliQ water and Diiodomethane (Sigma-Aldrich, Germany). Droplets of 3 µl were dispensed at a speed of 1 µl/s. Results were analyzed using the SCA20 Software (Dataphysics). 3.6 Zeta Potential The electric surface properties of the material are the result of the chemistry and the ion distribution at the diffuse interface between substrate and solution. The ζ-potential, the scientific term for electrokinetic potential, is widely used for quantification of the magnitude of the electrical charge at the double layer. . The technique used for ζ-potential quantification is based on the charge displacement in an electric double layer caused by an external force shifting the liquid phase tangentially
78 order to set the RT reaction. Retrotranscription was performed at 42ºC during 15 min and was inhibited at 95ºC for 3 min. The obtained cDNA was stored at -20ºC. 4.3 Primers design The DNA sequences used to amplify the FNIII 8-10 and the FNIII 12-14 of Homo sapiens fibronectin were obtained from the nucleotide NCBI database (www.ncbi.nlm.nih.gov/). Primers were selected from the Universal ProbeLibrary by Roche (www.roche-applied-science.com) and ordered to Invitrogen. For each fragment, CAS or HB II, the primer, the reading frame, the target, the added of the starting frame and the riding frame are given. A cleavage site was added to both fragments. The cleavage site was cut by the restriction enzyme forming the sticky ends, thus the DNA sequence was inserted in the plasmid. With the aim to allow the restriction enzyme to attach and cut the target, two nucleotides were added. It is important not to lose the reading frame of the protein of interest after any of the previous DNA sequence modifications. In Fig. 29 and Fig. 30 the final sequence obtained for each CAS primer and HB II primers after the nucleotides addition is shown, respectively. Fig.29 Primers D1 and D3 corresponding to the CAS sequence with the starting frame add, the cleavage site and the reading frame add.
79 Fig.30 Primers D1 and D3 corresponding to the HB II sequence with the starting frame add, the cleavage site and the reading frame add. 4.4 PCR amplification The polymerase chain reaction (PCR) is a biochemical technology in molecular biology to amplify a single or a few copies of a piece of DNA across several orders of magnitude, generating thousands to millions of copies of a particular DNA sequence. Fig.31 Equipment to conduct the polymerase chain reaction. The AmpliTaq Gold® 360 Master Mix (Invitrogen) was used. The kit contains thermostable polymerase, nucleotides, etc at the proper concentration and an enhancer called 360GC Enhancer. Basically PCR consists in three steps: denaturation, annealing and extension.
80 Denaturation is a process that must not take more than 30 seconds and is initiated at a temperature of 95ºC. During this step, the DNA is opened and rendered in a single strand. Anealling is the process on which the two primers bind the appropriate complementary strand. The temperature for this step varies depending on the size of the primer and its nucleotide sequence. The annealing temperature can go as high as 72°C. There is a temperature, called melting temperature, at which the 50% of the primer stops to attach the DNA, but it is not the temperature at which the primer is actually totally attached to DNA. In our case, the annealing temperature for each fragment was chosen regarding the melting temperature of the corresponding primer. For the CAS the annealing temperature was 70ºC and for the HB II, 67ºC. Once the annealing is completed the extension starts. The primers act as a mold to start the extension process. During the extension phase, the fragment corresponding to the target is amplified. The reaction took place at 72ºC because it is the optimal working temperature of the Taq polymerase. Three identical reactions were prepared for the PCR amplification. Each reaction was prepared mixing 25 µl of AmpliTaq Gold 360 Master Mix, 1 µl of each primer needed and 1 µl of DNA in aqueous solution. The PCR cycle was conducted following the supplier’s advice. In Tab. 9 the cycles, times and temperatures of the process are shown. During the cycling phase, the first 5 cycles were done at 65ºC to amplify the DNA fragment without the restriction target, the following cycles were done at 70ºC and the target and the DNA were both amplified.
81 State Step Temperature Time Holding AmpliTaq Gold 360 Master Mix polymerase activation 95ªC 10 min Cycling (40 cycles) Denaturation 95ºC 30 s Annealing 65ºC 30 s Extend 72ºC 60s/kb Denaturation 95ºC 30 s Annealing 70ºC 30 s Extend 72ºC 60s/kb Holding Final extend 72ºC 7 min Holding Final hold 4ºC ∞ Table 9. Table with the cycles, times and temperatures of the PCR cycle for each step or the reaction. 4.4.1 Verification of the PCR amplification The amplification of the different fragments was verified by electrophoresis. The electrophoresis permits to separate DNA molecules by weight. This method is based on the dynamics of proteolytic solutions22. The negative charge of the sugar-phosphate backbone of DNA is the cause of its migration towards the anode when a voltage is applied. The mobility of the DNA depends on molecule’s size; longer molecules migrate more slowly because they experience more resistance within the gel. Because the size of the molecule affects its mobility, smaller fragments end up nearer to the anode than longer ones in a given period23. Electrophoresis was carried out in an acrylamide gel. These types of gels are formed by hydrogen bridges when they are in a cold aquose solution. The pore size depends on the acrylamide concentration and is inversely proportional to gel concentration. Molecules pass through the pores, thus it is of paramount importance to know the type of molecule to analyze. For low molecular weight molecules it is needed a high concentrated gel, whilst for high molecular weight molecules a low concentrated gel is needed. The device used was a mini-PROTEAN 3by Bio-Rad. The gel was at a concentration of 6% and was composed by acrylamide, TBE5X (0.445 M Tris-borate, 0.01 M EDTA at pH 8.2), distilled H2O, TEMED and APS 10%. The
82 APS is the polymerizing agent and the TEMED is the reaction catalyst. A comb with wells was placed and the gel was set up for 30 min. . The 10 µl of the PCR result were mixed with 1.1 ul of Blue Juice Gel Loading Buffer. This buffer contains bromophenol blue in order to monitor the electrophoresis. The dye has a slight negative charge in a moderated pH migrating in the same direction but faster than DNA. The 100 bp DNA Ladder (Invitrogen) was used to identify the approximate size of the sample fragments. This molecular-weight size marker consists in 15 fragments from 100 to 1500 bp in multiples of 100 bp and an additional fragment of 2072 bp. The 600 bp band is 2 to 3 times more intense than the rest of the bands with the aim to give internal orientation. The ladder is not for quantification. Fig.32 Set up for the electrophoresis assay. The samples and the ladder were loaded into separate gel wells and electrophoresis was run at 150V in a Mini-Protean® 3 Cell (Bio-Rad) with no time set up. The gel was stained with A dilution of 5µl SYBR® Safe DNA Gel Stain (Invitrogen) in 50 µl of TBE 1x and visualized with Gel DocTM XR+ Molecular Imager (Bio-Rad, California, USA). Power supply Power supplyPower supply Power supply Electrophoresis Cuvette Electrophoresis Cuvette Electrophoresis Cuvette Electrophoresis Cuvette Gel + samples Gel + samplesGel + samples Gel + samples
83 4.4.2 Purification of the PCR amplification During the amplification process the DNA as well as the primers was amplified. The components of the PCR such as primers, dNTPS, enzymes, salts, etc. must be eliminated, if not the plasmid might insert them and avoid the correct replication of the DNA. The QIAquick PCR Purification kit (Qiagen) was used to carry on the purification. The kit combines the technology of spin columns with the properties of the selective union to a silica membrane specifically designed for that purpose. The kit also has specific buffers optimized for an efficient recovery of DNA and elimination of contaminants. The DNA is absorbed by the membrane at high salt concentration whilst the contaminants pass through de column. The impurities are eliminated and the pure DNA is eluted in Tris buffer or water. 140 µl of the PCR product were mixed with 700 µl of PB buffer from the kit and added to the columns provided with the kit. The mixture was centrifuged and washed oncolumn several times following the manufacturer’s instructions. Finally, 30 µl of EB buffer (10 mM Tris·Cl, pH 8.5) was added to the column and incubated for 1min at room temperature and centrifuged. The resulting 30 µl were the purified PCR product. 5. FRAGMENTS CLONNING PROCEDURE 5.1 E.coli transformation 5.1.1 E. coli strains used On this thesis two different strains of E.coli were used: • MAX Efficiency® DH5α™ Competent Cells • One Shot® BL21 Chemically Competent E. coli, both from Invitrogen. The MAX Efficiency® DH5α™ Competent Cells were used as libraries to amplify the inserted DNA.
84 The One Shot® BL21 Chemically Competent E. coli were used to express the proteins. This strain is deficient in proteases, reducing the degradation of the heterologous proteins expressed. 5.1.2 Plasmid The cloning was carried out using plasmids, also called vectors. A plasmid is a synthetic small circular double helix molecule of DNA derived from larger plasmids that are formed naturally in bacterial cells24. Plasmids replicate independently of bacterial chromosomes. This means that are unnecessary for bacteria, but they might provide selective advantages. These intrinsic characteristics of plasmids make them an important tool in molecular biology, especially in genetic engineering. One application is recombinant proteins production. Since the plasmid replicates independently of the bacterial DNA, it is possible to obtain numerous copies of the DNA recombined molecule. The plasmid used in this thesis was a pGEX-6P-1 (GE Healthcare, New Jersey, USA) (Fig.33). This plasmid has an ampicillin resistance marker, which confers resistance to 100 µg/ml ampicillin. Expression is under the control of the tac promoter, which is induced by the lactose analog isopropyl b-D thiogalactoside (IPTG). The plasmid is also engineered with an internal lacIq gene. The lacIq gene product is a repressor protein that binds to the operator region of the tac promoter, preventing expression until induction by IPTG (Isopropyl β-D-1-thiogalactopyranoside), thus maintaining tight control over expression of the insert. In addition to offering chemically inducible, highlevel expression, the plasmid allows mild elution conditions for release of fusion proteins from the affinity medium. Thus, effects on antigenicity and functional activity of the protein are minimized. The pGEX-P1-6 encodes the recognition sequence for site-specific cleavage by PreScission Protease, between the GST domain and the multiple cloning site. Cleavage of pGEX-6P GST fusion proteins occurs between the Gln and Gly residues of the recognition sequence Leu-Glu-Val-Leu-Phe-Gln-Gly-Pro. Low temperature (5°C) digestion minimizes the degradation of the protein of interest. Because PreScission Protease has been engineered with a GST tag, it can also be removed from the cleavage mixture simultaneously with the GST portion of the fusion protein. The pGEX-6P
85 plasmid permits convenient site-specific cleavage and simultaneous purification on Glutathione Sepharose. The pGEX-6P series provides all three translational reading frames linked between the GST coding region and the multiple cloning sites. Fig.33 Map of the p-GEX-P6-1 glutathione S-transferase fusion plasmid showing the reading frames and main features. Adapted from www.gelifesciences.com
86 5.1.3 Plasmid and DNA digestion In order to the plasmids to be used as a vector in the ligation it is important to cut the circular sequence with a restriction nuclease obtaining thus, a linear DNA molecule. This process is called digestion. The same process is used for DNA. The DNA is cut with the same restriction enzyme in order to obtain the desired fragments for cloning. The plasmid was digested by mixing 1ug of plasmid with 1 µl of SalI, 1 µl of NotI, 7 µl of NE Buffer 3, 0.7 µl of BSA. The mixture was incubated at 37ºC for 2h. The DNA was digested adding to the 30 µl purified PCR, 1 µl of SalI, 1 µl of NotI, 7 µl of NE Buffer 3, 0.7 µl of BSA. The mixture was incubated at 37ºC for 2h. After plasmid and DNA digestion, purification is needed with the aim to eliminate the fragments cut during digestion. The purification process was the same described in section 4.4.2. The aim of this purification is to eliminate the small target fragments which might be ligated again avoiding the fragment and plasmid ligation; the restriction enzymes, the buffer, etc. 5.1.4 Plasmid and DNA ligation Once the DNA and the plasmid were purified, the ligation between them was carried out. In Tab. 10 the combinations of the different reaction mixture for ligation are shown. COMBINATION 1 COMBINATION 2 COMBINATION 3 2 µl plasmid 3 µl plasmid 3 µl plasmid 2µl DNA 2 µl DNA 3 µl DNA 3 µl ligase buff er 3 µl ligase buffer 3 µl ligase buffer 1 µl ligase 1 µl ligase 1 µl ligase 22 µl H2O RNAse free 21 µl H2O RNAse free 20 µl H2O RNAse free Table 10. Quantities of each element that participate in the ligation for three different conditions.
87 When DNA and the plasmid get into contact they anneal through the sticky ends. After that, the DNA fragment and the plasmid are linked covalently by means of the T4 DNA Ligase (Roche, Manheim, Germany). The different combinations were left at 4ºC over night to alloy the reaction to took place. After that, all of them were mixed resulting in one reaction. Fig.34 Scheme of the annealing mechanism between the plasmid and the DNA fragment. 5.1.5 Transformation of the E.coli with the result of the Plasmid and DNA ligation Transformation is the incorporation of exogenous genetic material (e.g. plasmid with an inserted DNA fragment) into bacteria. Transformation is a basic technique used in molecular biology. It consists of two phases: • Union of the extracellular DNA with the cell. • Insertion of the extracellular DNA into cytoplasm. Some bacteria made this process naturally, although it is not frequent. To carry on the process in an artificial way, or in a forced way, a thermal shock was used. When the bacteria (E. coli in this case), gets into contact with the DNA (in this case, ligations), the DNA binds to lipopolysaccharides receptors on the cellular surface. The application of a heat shock is conducted, the sample changes from 0ºC to 42ºC and a release of cell surface lipids takes place. This transport of lipids opens pores on the cell membrane and the DNA pass through the pores to the cytoplasm. After that, the sample is cooled to a 0ºC making the open pores of cell membrane to disappear (26).
94 with nitrogen. All chemicals purchased from Sigma-Aldrich. FN fragments were prepared at a 100 µg/ml concentration diluted in PBS pH 7.4 (Invitrogen). A 100 µl drop of each fragment was placed on each sample and incubated overnight at room temperature. 7.2 Covalent binding. Silanisation In the present work, the silanisation method was done in solution and toluene was used as the anhydrous solvent. The crosslinker used was N-Succinimidyl 3- maleimidopropionate. Discs 2mm thick of the TiNbHf alloy were mirror polished and silanised according to the following procedure: Samples were cleaned with O2 plasma for 5min at a 12 MHz frequency in a Expanded Plasma Cleaner PDC-002 (Harrick Scientific Corporation, New York, USA). The aim was to promote and increase the formation of –OH groups on the material surface. Next samples were immersed in a solution of 0.08M APTES (Aminopropyl-triethoxysilane, Sigma-Aldrich) in toluene (Sigma-Aldrich) at 70ºC for 1h under agitation in an inert atmosphere. After silanisation, the samples were sonicated in toluene for 5 minutes and cleaned with toluene (3x), acetone (1x), isopropanol (3x), distilled water (3x), ethanol (3x) and acetone (3x) afterwards. Subsequently aminosilanised samples were immersed in a 7.5 mM solution of N-succinimidyl-3-maleimidopropionate in DMF (N, N- dimethylformamide Sigma-Aldrich) for 1h under agitation at room temperature. The cross-linked samples were rinsed in DMF (3x), acetone (1x), distilled water (10x), ethanol (3x) and acetone (3x) and dried with nitrogen. Straightforward, 100 µl drop of the desired motif of functionalisation was placed on the samples and incubated for 1h at room temperature. 7.3 Protein adhesion characterization 7.3.1 Optical Waveguide Lightmode Spectroscopy System (OWLS) The OWLS is a labelling-free technique used to investigate the interaction at the solid/liquid interface. With OWLS, the adsorption, binding and adhesion processes can
95 be studied. The technique is based on the coupling of a polarized light by a diffraction grating into the waveguide layer. To carry on the experiments a sensor is needed (Fig. 35). The sensor is a glass substrate, made by the SOL-GEL technology, with a waveguide layer of thickness 200nm and with a refraction index 1.8. The waveguide layer is grated with a periodicity of 2400 lines/mm. Fig.35 Sensor used for OWLS experiment. Extracted from www.microvacuum.com The sensing principle is based on the incoupling phenomenon (see Fig.36). The incoupling is a resonance phenomenon, that occurs at a precise angle of incidence which depends on the refractive index of the medium covering the surface of the waveguide. In the OWLS system, a He-Ne laser is used as the source of light and the incoupling occurs at two-well defined angles of incidence: one for the transverse electric (TE) and the other for the transverse magnetic (TM) polarization mode of the laser. These angles depend on the refractive indices of the medium covering the surface of the waveguide. Fig.36 Representation of the OWLS equipment sensing principle. Extracted from www.microvacuum.com
96 In Fig. 37 a scheme of the optical system is showed. A He-Ne laser beam pass through a shutter, is reflected on a prism and arrives to the sensor surface at a certain angle. The sensor is placed into a holder and positioned on a rotator. The stepping motor controls the rotator angle at any time and the two photodiodes at the edges of the waveguide measure light intensity. Both the stepping motor and the photodiodes are controlled by a computer. Fig.37 Representation of the optical set up of the OWLS system. Extracted from www.microvacuum.com In the present work a OWLSTM 120 Optical Waveguide Lightmode Spectroscopy System Biosense 2.6 Software (Micro Vacuum Ltd. Budapest, Hungary) was used. Adsorption mode was selected from the different solid-liquid interface phenomenon that OWLS is able to measure. In Fig. 22 scheme of the process is shown. To determine the amount of material adsorbed it was assumed that the adsorbed layer depended linearly on the concentration of the adsorbed material and a dynamic measurement was needed. Briefly, the procedure is as follows: the incoupling angles (TE and TM) for electric and magnetic modes are evaluated from the measured lightmode spectra. The effective refractive indices (N(TE), N(TM)) of the waveguide structure are calculated on the basis of incoupling condition. Once the effective refractive indices are calculated and assuming that the optical parameters of the waveguide layer (nF, dF), the substrate (nS) and the covering medium (nC) are known
97 (Fig. 38), the refractive index (nA) and the thickness (dA) of the added layer can be calculated. The chips used had a waveguide layer coated with a TiO2 10nm thin film which was the coating with closer characteristics to the TiNbHf alloy. Each chip was cleaned in an ultrasound bath with cyclohexane (3x), isopropanol (3x), H2O (3x), ethanol (3x) and acetone (3X) and was dried with N2. The chips used to determine the adsorbed amount of protein by a covalent bonding were silanised as explained in point 7.2. In this case, the biofunctionalisation motifs were CAS and HB II recombinant fragments of FN. To conduct the adsorption measurements, the optical parameters of the chip were measured after injecting PBS on the flow cell. Taking these parameters of reference to make the calculation, the dynamic measurement started. This measurement was made with the buffer solution to achieve a base line. When the drift dNTM/dt is less that 10-8 s- 1, the base line was considered stable and the protein fragment of study was injected in the flow cell with a syringe. The dynamic measurement of the protein adhesion was monitored for 1h. After 1h PBS was injected in the flow cell and the non-adsorbed protein onto the chip surface was eliminated. Fig.38 Scheme of the principle detection in an adhesion process. The refractive index changes by the binding of the analyte molecules. Extracted from www.microvacuum.com 7.3.3 Atomic Force Microscope (AFM) The AFM basic principle is that a prove and a sample can interact and the forces involved in this interaction can be translated into images.
98 The AFM uses a cantilever that act as a spring. When the cantilever is close to the surface suffer from the interaction forces which can be attractive or repulsive. This attraction or repulsion produces the deflection of the cantilever. To detect the cantilever's deflection and translate it into an electrical signal a laser beam is used (see Fig.39). The laser beam is reflected from the back of the cantilever onto a photodetector. Depending on the cantilever deflection, the angle of the laser beam reflected changes, and the beam spot is reflected in a different area of the photodetector. The signals from the four quadrants of the photodetector are compared to calculate the deflection signal. The electronic signals given by the photoelectrode are translated into images by means of software. Fig.39 Scheme of the cantilever deflection photodetection. AFM is a technique widely used when working with biological samples because there is no need of staining or coating the sample of study and the samples do not need to conduct electricity and they can be imaged in physiological conditions as well. This technique gives 3D topographical information of the samples as well as mechanical properties of adhesion. In this thesis, the AFM technique was used to determine the topographical distribution of the protein under study in a TiNbHf samples and the adhesion force of cells when in contact with the protein functionalized TiNbHf samples. The equipment used was a NanoWizar®III (JPK Instruments, Berlin, Germany) (Fig. 40).
99 Fig.40 NanoWizar®III from JPK Instruments set up. 7.3.3.1 Surface imaging The AFM was used to map the spatial distribution of the proteins either adsorbed or covalently bonded to the substrates. AFM cantilever can interact with the surface in a contact imaging mode or in tapping mode. In the contact mode the scanning forces applied on the adsorbed protein layer might re-distribute the protein outside of at the edges of the scanning area 27. To avoid this, the tapping mode was used. In the tapping mode the tip of the cantilever makes repulsive contact with the surface of the sample at the lowest point of the oscillation (Fig.41) Fig.41 Representation of the contact and tapping mode of the cantilever during surface imaging. Adapted from NanoWizard® AFM Handbook. JPK Instruments. The samples used in the assay were biofunctionalised with the CAS fragment as stated in point 7.1 for the physisorbed ones; and as in 7.2, for the silanised ones. All the experiments were conducted in PBS at 37ºC in an attempt to reproduce physiological conditions. Three images of each sample were taken and they were analyzed with the JPK SPM data processing software (JPK Instruments, Germany)
100 7.3.3.2 Cell adhesion force analysis The single molecule force spectroscopy is used to perform mechanical assays with single molecules. These experiments can be done at ambient conditions or in a fluid and at a controlled temperature. Basically, the experiment is based on a tip in contact with the sample that is retracted from it. The cantilever is still attached to the sample due to some kind of adhesion and the cantilever is deflected downwards, but at some point the cantilever's force is able to overcome the adhesion and break free. In the AFM force analysis conducted a cell was attached to a functionalized cantilever. In Fig.42 a visual description of the process and an image of the curve obtained is shown. Fig.42 A) Visualization of a cell adhered to a cantilever being attached and retracted from a surface. B) Representation of a Force-Distance curve of the events taking places during cell attachment and retraction. Adapted from www.jpk.com The tests were made with samples biofunctionalised with lRGD, cRGD and the CAS fragment as stated in point 7.2 immersed in culture medium at 37ºC. The cells used were rat mesenchymal stem cells (rMSC). The cells were cultured in Advanced DMEM supplemented with 10% FBS (foetal bovine serum), antibiotics (50 U/ml penicillin and 50 µg/ml streptomycin), 2 mM L-glutamine and 20 mM HEPES buffer solution. All the chemicals were purchased from Gibco®. The cantilevers were incubated in 0.5mg/ml BSA-biotin (Sigma-Aldrich, Germany) at room temperature overnight. After incubation, cantilevers were washed with PBS 1X three times and then, incubated in 0.5 mg/ml streptavidin (Sigma-Aldrich, Germany) at
101 room temperature for 10 min. After incubation, cantilevers were washed with PBS 1X three times. Immediately after, cantilevers were incubated in 0.2 mg/ml biotinconcanavalin A (Sigma-Aldrich, Germany) at room temperature for 10 min. The samples were placed in a petri dish specific for the AFM equipment and immersed in culture medium Advanced DMEM without FBS. To avoid cell adhesion to the petri dish a layer of Polyethylene glycol was made on the surface at which the samples were attached. 10ul of cells were introduced into the petri dish and a unique cell was immobilised on the cantilever. To achieve the cell immobilisation the cantilever was attached to the cell with a force of few nano Newtons and inducing contact for a few seconds. Once the cell was immobilised, it was placed on the sample with a load varying between 300 and 800 pN. Cell was left for 5 seconds intereacting with the surface and straightforward was moved away with a retracting speed of 3um/s. Six different cells were tested in each sample and 20 adhesion assays were made with each cell. All curves were analyzed with the JPK SPM data processing software (JPK Instruments, Germany) 8. CELLULAR ASSAYS 8.1 General considerations 8.1.1 Cell type In this thesis, the aim of the cell culture is to determine if cells are able to adhere, spread and differentiate in a device for bone applications. There are two cells involved in bone formation: mesenchymal stem cells and osteoblasts. The cell type used in this thesis was rat mesenchymal stem cells (rMSCs). Primary cell culture reflects in a more accurate way the process that takes part when an implant is inserted in the body. The cells were obtained from Sprague-Dawley rats in a process developed by Institute of Bioengineering of Catalonia (IBEC).
102 8.1.2 Culture medium Advanced DMEM (Gibco®, Invitrogen) was used for rMSCs culture. Advanced DMEM (Dulbecco's Modified Eagle Medium) is a widely used basal medium that allows the culture of mammalian cells with reduced Fetal Bovine Serum (FBS) supplementation. This medium contains high glucose, essential amino acids, sodium pyruvate and phenol red, thus it has to be supplemented with FBS, antibiotics, L- glutamine and the organic buffer HEPES (all from Invitrogen). In table 11 the formulation of the medium used in the assays is shown. COMPONENT % IN THE TOTAL VOLUME penicillin/streptomycin 1% L - glutamine 1% HEPES 2% FBS 10% Advanced DMEM 86% Table 11. Formulation of the supplemented Advanced DMEM used in the cell assays. 8.1.3 Cell culture maintenance rMSC cells were maintained in Advanced DMEM supplemented with 10% FBS (fetal bovine serum, Invitrogen), 20 mM HEPES Buffer solution (Invitrogen), antibiotics ( 50 U/ml penicillin and 50 µg/ml streptomycin, Invitrogen), 2 mM L-glutamine(Invitrogen) in an incubator with 5% CO2 and 95% relative humidity at 37ºC. Cell medium was changed every 2 days to maintain the proper levels of nutrients, growth factors and hormones for cell growth as well as for the pH and the osmotic pressure of the culture. Cells were kept at an optimal density for continued growth and to stimulate further proliferation. When cells reach confluence, cell proliferation is greatly reduced or ceases. Confluent cells were detached and seeded in a new flask. Cells were detached using TrypLE™ Express (Invitrogen). TrypLE™ Express is composed of cell dissociation enzymes with similar kinetics and cleavage specificities to trypsin. Detached cells were centrifuged, resuspended in medium and seeded.
103 8.2 Adhesion assay Cell adhesion assay was done to test the ability of the protein fragments developed to trigger or to enhance cell adhesion. The number of cells adhered were measured by a lactate dehydrogenase (LDH) assay and the morphology, cytoskeletal assembly and focal contacts by means of immune fluorescence. 8.2.1 Lactate dehydrogenase LDH assay The LDH assay is a non-radioactive colorimetric assay based on the measurement of the lactate dehydrogenase activity released from the cytosol of damaged cells. Lactate dehydrogenase (LDH) catalyses the interconversion of pyruvate and lactate. The LDH activity is determined by a coupled enzymatic reaction, whereby the tetrazolium salt INT is reduced to formazan. An increase in the number of cells results in an increase of LDH enzyme activity in the culture supernatant after lysis. This increase in the amount of enzyme activity in the supernatant directly correlates to the amount of formazan formed during a limited time period. The Cytotoxicity Detection Kit PLUS (LDH) from Roche was used. The kit is provided with a catalyst, a dye solution and a stop solution. The procedure to perform the assay was as follows: Samples were prepared as stated in point 7.2 and seeded with 25000 cells/well. After 5h incubation 300 µl of Mammalian Protein Extraction Reagent (M-PER) purchased from Thermo Scientific were added to the samples. The LDH kit reaction mixture was prepared following the manufacturer guidelines. 100 µl of each sample and the calibration curve were added to a 96 well plate. 100 µl of the LDH kit reaction mixture were added to the wells with the M-PER solution and incubated protected from light for 10-15min. After the incubation time, 50 µl of the LDH Kit stop solution were added to each well and the absorbance was read in a multiwell plaque reader at a λ=492nm. 8.2.3 Immunofluorescence Immunofluorescence is a technique based on the specificity of the interaction antigenantibody. The technique is applied directly on the cells and is capable of identify the
110
111 Chapter3 Effect of the alloying elements in the Ti-24.8Nb-16.2Hf-1Zr alloy 1. Design of the alloy composition ......................................................................................... 113 1.1 Effect of the alloying elements on the alloy’s quantum parameters ................... 114 1.2 Alloys composition verification .......................................................................... 117 2. Influence of the composition in the microstructure.......................................................... 119 2.1 Effect of Nb in the microstructure ...................................................................... 119 2.1.1 Optical microscopy results ........................................................................... 119 2.1.2 XRD results .................................................................................................. 120 2.1.3 TEM results .................................................................................................. 121 2.2 Effect of Hf in the microstructure ....................................................................... 122 2.2.1 Optical microscopy results ........................................................................... 122 2.2.2 XRD results .................................................................................................. 123 2.2.3 TEM results .................................................................................................. 123 3. Influence of the composition in the thermoelastic phase transformation induced by stress ........................................................................................................................................ 124 3.1 Effect of niobium in the thermoelastic phase transformation ............................. 125 3.1 Effect of hafnium in the thermoelastic phase transformation ............................. 126 4. Influence of the composition in the Elastic Modulus........................................................ 126 4.1 Effect of niobium in the elastic modulus ............................................................ 127 4.2 Effect of hafnium in the elastic modulus ............................................................ 128 5. Alloy’s Selection criteria ..................................................................................................... 130 6. Bibliography ......................................................................................................................... 133
112
113 1. DESIGN OF THE ALLOY COMPOSITION The basis alloy, Ti-24.8Nb-16.2Hf-1Zr 1, was located in the area of shape memory and low modulus according with the Arciniegas’ map2. Our aim was to remain in this area and to lower the elastic modulus without losing the β-phase properties of the alloy: high templability, high mechanical strength and conformability, plus low elastic modulus. Zirconium was eliminated because of its low proportion in the alloy (1%). The low amount of Zr in the base alloy made it more an impurity than a β-stabilizer affecting mechanical properties. Niobium and Hafnium were maintained because of their properties. • Niobium play two roles in the alloy: on one hand is a β-stabilizer, and on the other hand gives high corrosion resistance 3,4. • Hafnium has the excellent oxidation resistance, corrosion resistance in a wide variety of media, and high stability of oxides, nitrides, carbides and other compounds and also acts as a beta stabilizer 3. • The osteogenic and biocompatibility properties of both Nb and Hf 5. The percentage in mass of each element was varied forming 12 different ternary alloys according to the values shown in Table 12. ALLOY Nb (w%) Hf (w%) Ti (w%) 1 20 16 Balance 2 22 16 Balance 3 23 16 Balance 4 26 16 Balance 5 27 16 Balance 6 29 16 Balance 7 25 10 Balance 8 25 12 Balance 9 25 15 Balance 10 25 17 Balance 11 25 19 Balance 12 25 21 Balance Table 12. Variations in the composition of the ternary alloy Ti-25Nb-16Hf.
114 1.1 Effect of the alloying elements on the alloy’s quantum parameters Each alloying element has its own quantum parameters (Table 13). The value of the quantum parameters of the alloy is influenced by the quantum parameter of each alloying element and the amount of each element in the alloy. Element BO (eV) OE (eV) e/a Ti 0.641 0.15454 4 Nb 0.6207 0,14741 5 Hf 0.6698 0.14857 4 Table 13. Quantum parameters BO and OE and e/a relation for each alloying element. The quantum parameters calculated were the bond order (BO), the orbital free energy (OE) and the electron atom ratio (e/a). These values were calculated according to the following equations: = ∑(BO)i Eq. 3.1 = ∑(OE)i Eq. 3.2 // = ∑(e/a)i Eq. 3.3
115 The values obtained for each alloy are shown in Table 14. Alloy Formulation BO (eV) OE (eV) e/a 1 Ti-20Nb-16.2Hf 0.60992 0.15311 4.1314 2 Ti-22Nb-16.2Hf 0.61021 0.15300 4.1463 3 Ti-23Nb-16.2Hf 0.61036 0.15294 4.1539 4 Ti-26Nb-16.2Hf 0.61082 0.15277 4.1773 5 Ti-27Nb-16.2Hf 0.61098 0.15271 4.1853 6 Ti-29Nb-16.2Hf 0.61130 0.15258 4.2017 7 Ti-24.8Nb-10Hf 0.60891 0.15312 4.1584 8 Ti-24.8Nb-12Hf 0.60945 0.15303 4.1613 9 Ti-24.8Nb-15Hf 0.61029 0.15290 4.1654 10 Ti-24.8Nb-17Hf 0.61087 0.15280 4.1692 11 Ti-24.8Nb-19Hf 0.61148 0.15270 4.1725 12 Ti-24.8Nb-21Hf 0.61212 0.15260 4.1760 Table 14. Values of BO and OE corresponding to each alloy composition. As the wt % Nb increases, the BO and the e/a values increased whilst the the OE values decreased. The same behaviour was observed when the wt % Hf increased. When the wt % Nb was increased from 20 to 29, the BO was in the range 0.60992≤BO ≤ 0.61130; the OE was in the range 0.15311≤OE≤ 0.15258 and the e/a was in the range 4.1314 ≤ e/a ≤ 4.2017. When the wt % Hf was increased from 10 to 21, the BO was in the range 0.60891≤BO ≤ 0.61212; the OE was in the range 0.15312≤OE≤ 0.15260 and the e/a was in the range 4.1584≤ e/a ≤ 4.1760. The OE values did not vary significantly depending on the addition of Nb of Hf, whilst the values that were affected more significantly were the e/a values. Although all of the values correspond to values comprising the low elastic These quantum parameters were located in the Arciniegas' properties map (Fig. 43). The alloys are located in the region of shape memory and low modulus properties.
116 Fig.43 Alloys location in the properties map developed by Arciniegas. According to Fig.43, all the alloys are located in the shared properties region, except for the alloys of composition Ti-29Nb-16.2Hf and Ti-24.8Nb-21Hf which are located in the region of low elastic modulus, but so close to the shared properties region. These two alloys are also the only ones in the β-region. As long as the Nb and Hf are β-stabilisers and both have a high percentage in these alloys (29% and 21%) formulation, it makes sense the resulting microstructure was dominated by the β-phase. The values of the parameter e/a obtained in each alloy range from 4.13 to 4.20. There are just two alloys that do not fulfill the requirements to present ultra-low elastic modulus, high strength, superelastic-like elastic deformability and superplastic-like cold
117 workability without work hardening at room temperature. These alloys are the ones containing 20% wt and 22% wt of niobium. The rest of alloys are potential candidates to accomplish with those special properties. 1.2 Alloys composition verification Buttons of the designed alloys were fabricated in an arc melting furnace from Ti cp bars, Nb foil 99,8% purity and Hf shavings 99,7%. Once they were melted, the composition was verified by quantitave analysis using Energy Dispersive X-ray Spectroscopy (EDS). In Table 15 the values of experimental and theoretical chemical composition for each alloy are shown. The experimental values obtained are close to the theoretical values, with a slight deviation.
118 Alloy formulation %w Element Nb Hf Ti Exp. Theor. Exp. Theor. Exp. Theor. Ti-23Nb-16.2Hf 22.98 ±0.21 23 15.62 ±0.18 16.2 61.4 ±0.24 57.8 Ti-22Nb-16.2Hf 19.82 ±0.2 22 19.91 ±0.24 16.2 60.27 ±0.18 61.8 Ti-20Nb-16.2Hf 20.53 ±0.2 20 16.02 ±0.18 16.2 63.45 ±0.24 63.8 Ti-24.8Nb-17Hf 23.69 ±0.045 24.8 18.39 ±0.17 17 57.92 ±0.2 58.2 Ti-24.8Nb-19Hf 24.126 ±0.46 24.8 19.46 ±1.81 19 56.41 ±1.37 56.2 Ti-24.8Nb-21Hf 21.41 ±0.65 24.8 21.50 ±0.28 21 57.09 ±0.63 51.2 Ti-26Nb-16.2Hf 25.91 ±0.15 26 16.35 ±0.085 16.2 57.73 ±0.21 57.8 Ti-27Nb-16.2Hf 26.73 ±0.45 27 16.62 ±0.09 16.2 56.62 ±0.35 56.8 Ti-29Nb-16.2Hf 28.56 ±0.035 29 16.85 ±0.22 16.2 54.58 ±0.19 54.8 Ti-24.8Nb-15Hf 23.56 ±0.42 24.8 15.8 ±0.11 15 60.64 ±0.25 60.2 Ti-24.8Nb-12Hf 23.76 ±0.15 24.8 13.15 ±0.28 12 63.08 ±0.39 63.2 Ti-24.8Nb-10Hf 22.32 ±0.49 24.8 9.11 ±0.39 10 68.58 ±0.76 65.2 Table 15. Values of the EDS analysis for each material composition and their standard deviations.
119 2. INFLUENCE OF THE COMPOSITION IN THE MICROSTRUCTURE Diffraction database was used to identifying and indexing the phases present in the alloy. Due to the novelty of the alloy there are no diffraction patterns available. The patterns used where those from Ti (α and β), Nb and a quenched TiNb alloy with up to 12% content of Nb. Despite this, it was possible to relate each experimental peak with the close one on the reported spectra. 2.1 Effect of Nb in the microstructure 2.1.1 Optical microscopy results Previous studies report a needle-shaped α phases in a β-dominated matrix in Ti-Nb alloys6 and a dependence of the β-phase presence on the Nb content. High content of Nb favors the β-phase7. This microstructure is observed when the alloy is in an equilibrium state. In our case, the alloy is quenched and thus, not in equilibrium conditions. In Fig. 44 the micrographies obtained by optical microscopy for alloys with Nb content from 20% w.t. to 29% w.t. are shown. The microstructure is formed by martensitic plates. As the Nb content increases, the martensite plates become more organized until the microstructure is mainly beta with some isolated with some martensite. This martensite distribution might be due to the α’’ proportion with respect to the α’. Niobium is a beta stabilizer, therefore is logic that increasing niobium content makes the microstructure more beta. Nevertheless, this behaviour is not seen in the alloy with a 27% w.t. of Nb (Fig.44 e). This might be due to during polishing the martensite plaques were induced.
126 3.1 Effect of hafnium in the thermoelastic phase transformation In the manner of the Ti-(20-29)Nb-16.2Hf group alloys (Fig. 50), the Ti-24.8Nb(10- 21)Hf group alloys (Fig. 51) also present the characteristic loops of hysteresis of phase transformation induced by stress. As the Hf amount increases, the loops are becoming wider, except for the 15% w.t. Hf (Fig. 51 c). For this alloy, the same behavior as for the 23-27% w.t. Nb (Fig. 50 c and e) alloys is observed. This behaviour is similar to that of the austenitic NiTi13. The alloys with 17% w.t. Hf (Fig. 51 d) and 19% w.t. Hf (Fig. 51 e) pop-in’s show popin’s. As was said before, these events are indicators of plastic deformation. Fig.51 Nanoindentation curves obtained for 5 cycles of loading-unloading at an indentation depth of 300nm for the alloys Ti-24.8Nb-10Hf (a), Ti-24.8Nb-12Hf (b), Ti-24.8Nb-15Hf (c), Ti-24.8Nb-17Hf (d), Ti-24.8Nb-19Hf (e) and Ti-24.8Nb-21Hf (f) 4. INFLUENCE OF THE COMPOSITION IN THE ELASTIC MODULUS To know the elastic modulus of the alloys the P-h curves at 2000 nm depth were used. The first is 100 nm of each curve was approximated to the Hertz’s Equation. The slope of the curve determined the elastic modulus.
127 Nine nanoindentations were done on each sample and the obtained moduli and the average for each curve were calculated. . 4.1 Effect of niobium in the elastic modulus According to Table 16, the modulus values for the Ti-(20-29)Nb-16.2 alloys group span from 38 to 77 GPa. In all the cases we are dealing with low elastic modulus alloys. The elastic modulus values obtained show that for values of Nb percentage above 22% wt the modulus increases drastically, but for values above 27%wt Nb the value of the elastic modulus decreases again (Fig.52). As was shown in section 2.1, the increase in Nb content is translated in a β-phase microstructure. Elastic Modulus (GPa) % wt Nb 20 22 23 26 27 29 Average 41,71 38,29 77,40 74,17 74,00 68,42 SD 5,62 9,01 2,51 4,58 7,30 2,31 Max 50,00 57,00 80,00 79,00 86,00 72,00 Min 36,00 32,00 75,00 69,00 68,00 65,00 Table 16. Modulus of elasticity according to the %wt of Nb on each alloy, with the maximum and minimum values obtained. Fig.52 Graphic variation of the modulus of elasticity according to the %wt of Nb on each alloy, with the maximum and minimum values obtained.
128 Looking at the P-h curves for the first 100nm fitted to Hertz Equation (Fig.53), differences in slopes between the elastic and plastic zone can be observed. The change in the slope is an indicative of the transition from the plastic deformation to the elastic deformation. The change from the elastic to the plastic behaviour, according to the curves, takes place for a 2 nN average applied force and with an approximately 34 nm penetration depth. This trend was seen for all the alloys except for the 23% wt Nb in which the force to pass from the elastic to plastic regime was 12 nN and the penetration depth 80 nm (Fig. 53c). In other words, the 23% wt Nb alloy can be deformed with higher loads keeping its elastic behavior. Fig.53 Nanoindentation curves obtained for the first 100nm for the alloys Ti-20Nb-16.2Hf (a), Ti- 22Nb-16.2Hf (b), Ti-23Nb-16.2Hf (c), Ti-26Nb-16.2Hf (d), Ti-27Nb-16.2Hf (e) and Ti-29Nb-16.2Hf (f) and with the Hertz’s Equation fitting. The change in the slope determines the transition from elastic to plastic deformation. 4.2 Effect of hafnium in the elastic modulus Previous studies about the effect of Hf on the elastic modulus14–16 reported low influence or an increase of the modulus with the addition of Hf.
129 According to Table 17, the obtained moduli are in a range of 45-77 GPa, that means there is a variation of modulus depending on the Hf amount in the alloy despite no trend is seen between Hf quantity and modulus (Fig. 54) Elastic Modulus (Gpa) % wt Hf 10 12 15 17 19 21 Average 45,11 77,40 57,20 50,83 76,00 51,57 SD 3,74 6,58 1,10 2,41 8,91 5,62 Max 49,00 87,00 58,00 52,25 85,00 59,00 Min 38,75 70,00 56,00 46,00 60,00 42,00 Table 17. Modulus of elasticity according to the %wt of Hf on each alloy, with the maximum and minimum values obtained. Fig.54 Graphic variation of the modulus of elasticity according to the %wt of Hf on each alloy, with the maximum and minimum values obtained. The change from the elastic to the plastic behavior, according to the curves, took place for a 40 nN average applied force, but the penetration depth was not as constant as in the Nb alloys. For the Hf alloys it ranged from 1.5 to 5.4 nm. This trend was seen for all the alloys except for the 21% wt Hf in which the force to pass from the elastic to plastic regime was 7.5 nN and the penetration depth 79 nm.
130 Fig.55 Nanoindentation curves obtained for the first 100nm for the alloys Ti-24.8Nb-10Hf (a), Ti- 24.8Nb-12Hf (b), Ti-24.8Nb-15Hf (c), Ti-24.8Nb-17Hf (d), Ti-24.8Nb-19Hf (e) and Ti-24.8Nb-21Hf (f) and with the Hertz’s Equation fitting. The change in the slope determines the transition from elastic to plastic deformation. 5. ALLOY’S SELECTION CRITERIA Amongst the 12 alloys fabricated and studied, just one was chosen to work with and make further assays. The criteria for determine the parameters to be considered in the material selection were: Quantum parameters as close as possible to the ones described for Gum Metal17,18 High elastic deformation regime Low elastic modulus The quantum parameters of interest were Bo=2.87 eV, Md=2.45 eV and e/a=4.24. The BO and OE calculated values can be easily translated into Bo and Md values to compare the values. In Table 18 the values of Bo, Md and e/a for each alloy are displayed. There are two alloy compositions that showed quantum parameters close to the ones desired: 29% wt Nb and 21% wt Hf.
131 Formulation Bo (eV) Md (eV) e/a GUM METAL 2.87 2.45 4.24 Ti-20Nb-16.2Hf 2.848 2.473 4.1314 Ti-22Nb-16.2Hf 2.853 2.473 4.1463 Ti-23Nb-16.2Hf 2.855 2.473 4.1539 Ti-26Nb-16.2Hf 2.863 2.473 4.1773 Ti-27Nb-16.2Hf 2.865 2.473 4.1853 Ti-29Nb-16.2Hf 2.871 2.473 4.2017 Ti-24.8Nb-10Hf 2.849 2.460 4.1584 Ti-24.8Nb-12Hf 2.852 2.464 4.1613 Ti-24.8Nb-15Hf 2.858 2.470 4.1654 Ti-24.8Nb-17Hf 2.861 2.475 4.1692 Ti-24.8Nb-19Hf 2.865 2.479 4.1725 Ti-24.8Nb-21Hf 2.869 2.483 4.1760 Table 18. Values of the quantum parameters Bo, Md and e/a corresponding to each alloy composition. The alloy elasticity is important for further processing. If the elastic regime is high the material could be easily machined. In Fig.56 the different elastic-plastic behaviour of the alloys is shown. Comparing woth alloys it is clear that the elastic región of the 21 %wt Hf is higher than the one of the 29 %wt Nb.
132 Fig.56 Nanoindentation curves obtained for the first 100nm for the alloys Ti-29Nb-16Hf and Ti-25Nb- 21Hf with the Hertz’s Equation fitting. The change in the slope determines the transition from elastic to plastic deformation. The elastic modulus obtained by nanoindentation for the 29 %wt Nb has a value of 68.42 GPa which is higher than the modulus obtained for the 21 %wt Hf with value 51.57 GPa. According to the values of quantum parameters, elastic behaviour and elastic modulus, the chosen alloy to work with was the Ti-25Nb-21Hf.
133 6. BIBLIOGRAPHY 1. Gonzalez, M., Peña, J., Manero, J. M., Arciniegas, M. & Gil, F. J. Desing and Characterization of New Ti-Nb-Hf alloys. J. Mater. Eng. Perform. 18, 490 (2009). 2. Arciniegas, M., Peña, J., Manero, J. M., Paniagua, J. C. & Gil, F. J. Quantum parameters for guiding the design of Ti alloys with shape memory and/or low elastic modulus. Philos. Mag. 88, 2529 (2008). 3. Amick, D. D. Characterization of TiNbHf alloys for potential medical dental applications. (1993). 4. Geetha, M., Singh, A. K., Asokamani, R. & Gogia, A. K. Ti based biomaterials, the ultimate choice for orthopaedic implants – A review. Prog. Mater. Sci. 54, 397–425 (2009). 5. Matsuno, H., Yokoyama, A., Watari, F., Uo, M. & Kawasaki, T. Biocompatibility and osteogenesis of refractory metal implants, titanium, hafnium, niobium, tantalum and rhenium. Biomaterials 22, 1253–1262 (2001). 6. Hon, Y. H. & Wang Y.N, J. Y. and P. Composition/Phase Structure and Properties of Titanium-Niobium Alloys. Mater. Trans. 44, 2384 (2003). 7. Li, S., Hao, Y., Yang, R., Cui, Y. & Niinomi, M. Effect of Nb on Microstructural Characteristics of Ti-Nb-Ta-Zr Alloy for Biomedical Applications. Mater. Trans. 42, 2964–2969 (2002). 8. Nobuhito, S., Niinomi, M., Toshikazu, A., Takashi, S. & Tadahiko, F. Effects os Alloying Elements on Elastic Modulus of Ti-Nb-Ta-Zr System Alloy for Biomedical Applications. Mater. Sci. Forum 449-452, 1269–1272 (2004). 9. De Fontaine, D., Paton, N. . & Williams, J. . The omega phase transformation in titanium alloys as an example of displacement controlled reactions. Acta Metall. 19, 1153–1162 (1971). 10. Sukedai, E., Hashimoto, H. & Tomita, M. Investigation of omega-phase in Ti– Mo alloys by high resolution electron microscopy, image processing and darkfield methods. Philos. Mag. A 64, 1201–1208 (1991). 11. Bradby, J. E., Williams, J. S. & Wong-Leung, J. Nanoindentation-induced deformation of Ge. Appl. Phys. Lett. 80, 2651 (2002). 12. Oliver, W. C. & Pharr, G. M. An improved technique for determining hardness and elastic modulus using load and displacement sensing indentation experiments. Mater. Reserch Soc. 7, 1564 (1992). 13. González, M., Peña, J., Manero, J. M., Arciniegas, M. & Gil, F. J. Optimization of the Ti-16.2Hf-24.8Nb-1Zr Alloy by Cold Working. 18, 506 (2009).
134 14. Zhou, Y.-L., Niinomi, M. & Akahori, T. Changes in mechanical properties of Ti alloys in relation to alloying additions of Ta and Hf. 14th Int. Conf. Strength Mater. 483-484, 153–156 (2008). 15. Zhou, Y.-L., Niinomi, M. & Akahori, T. Dynamic Young’s Modulus andMchanical Properites of Ti-Hf alloys. Mater. Trans. 45, 1549 (2004). 16. Hon, Y. H., Wang, J. Y. & Pan, Y. N. Influence of hafnium content on mechanical behaviors of Ti–40Nb–xHf alloys. Mater. Lett. 58, 3182–3186 (2004). 17. Saito, T. et al. Multifunctional Alloys Obtained via a Dislocation-Free Plastic Deformation Mechanism. 300, 464 (2003). 18. Hao, Y. L. et al. Super-elastic titanium alloy with unstable plastic deformation. 87, (2005).
135 Chapter 4 Ti-25Nb-21Hf Alloy Characterization 1. Alloy’s microstructure ......................................................................................................... 137 1.1 Optical microscopy and grain size ...................................................................... 137 1.2 X-ray diffraction (XRD) ..................................................................................... 138 1.3 Transmission electron microscopy (TEM) ......................................................... 139 2. Determination of the elastic modulus ................................................................................ 140 2.1 Elastic modulus by means of nanoindentation.................................................... 140 2.2 Elastic modulus by means of tensile test ............................................................ 141 3. Alloy’s corrosion resistance ............................................................................................... 143 3.1 Open circuit potential .......................................................................................... 143 3.2 Cyclic voltametry ................................................................................................ 144 4. Alloy’s superficial energy.................................................................................................... 146 4.1 Contact angle measurements and SFE calculation ............................................. 146 4.2 Zeta potential results ........................................................................................... 148 5. Bibliography ......................................................................................................................... 150
238 Fig.109 Effect of the heat treatments in the elastic modulus of the different wires. 3.1.3 Cyclic tensile testing Fig.110 shows cyclic uniaxial tension tests that were performed at body temperature (37 ºC) and at 150 ºC on Ti25Nb21Hf wires after 99% cw. When the Ti25Nb21Hf specimens were tested at body temperature, no evidence of reversibly performing was seen in either of the cycles. Although for tests conducted at 150ºC, when the magnitude of the external loading returned to zero in the three first cycles, the strain recovered fully returned to the initial level. This elastic behaviour was not seen in further cycles. Fig.110 Graphic of the loading-unloading curves at different strain rates of the TiNbHf alloy at 37ºC and 150ºC
239 When the loading-unloading curves obtained for the Ti25Nb21Hf alloy at 150 ºC were compared with those of NiTi-SEA (Fig.111), it was seen that the behaviour of the Ti25Nb21Hf wire could be related in a certain way with NiTi behaviour. Fig.111 Comparison of the superelastic behaviour of the alloy Ti25Nb21Hf at 150ºC and the shape memory alloy NiTi at 25ºC. 3.2 Microstructure studies Fig. 112 shows the microstructures obtained for the alloys at different % cw and heattreated at 650ºC for 1 and 3 s. In all %cw conditions, the 3s heat treatment, lead to a microstructure composed by nanograined regions whilst the 1s heat treatment lead to a microstructure with a mixture of clearly defined grains and grains with not clearly defined boundaries. In all the cases, the bright field images confirmed the presence of austenite β (BCC), orthorhombic martensite α´´, ω-phase and an amorphous phase.
240 Fig.112 Microstructures obtained for the Ti25Nb21Hf cold worked at 75% heat treated at 650ºC for 1s (a) and for 3 s (d); cold worked at 95% heat trated at 650ºC for 1s b) and for 3s (e); cold worked at 99% heat trated at 650ºC for 1s (c) and for 3s (f). 3.3 Rotary beam fatigue testing Fig. 113 shows the results obtained for rotary beam fatigue testing. In air and at room temperature, the Ti25Nb21Hf alloy showed better fatigue response than NiTi and 316L. In air and at room temperature, Ti25Nb21Hf alloy was capable to perform at higher strain values until failure than the other two materials under study. The performed assays in PBS at body temperature showed fatigue strain amplitudes in excess of 0.5% at a greater cycle life than 107 cycles.
241 Fig.113 Results of the rotary beam fatigue testing at room temperature (25 ºC) in air for the Ti25Nb21Hf alloy, NiTi and 316L and in PBS and at body temperature (37 ºC) for the Ti25Nb21Hf alloy. The cumulative distribution at 1% alternating strain for superelastic NiTi compared to Ti25Nb21Hf alloy is shown in Fig.114. According to the graphic, the Ti25Nb21Hf alloy would last more cycles than NiTi until failure. Fig.114 Cumulative distribution at 1% alternating strain for superelastic NiTi compared to Ti25Nb21Hf alloy. 0 0.4 0.8 1.2 1.6 1E+4 1E+5 1E+6 1E+7 Strain (%) Cycles to failure Ti25Nb21Hf Air Ti25Nb21Hf PBS Nitinol, Af = 15°C Cold-drawn 316L 0.0 0.3 0.5 0.8 1.0 4 5 6 7 8 CDF, P(n <= N) Cycles to failure Nitinol TiHfNb
242 4. DISCUSSION During tensile testing was seen that higher percentages of cold work give raise to higher values of modulus as observed in other studies 10, but in all the cases the modulus obtained for the Ti25Nb21Hf alloy was between 50 GPa and 59 GPa. Since the modulus of elasticity obtained from the bar was close to 86GPa, then cold work induces an approximately 40% modulus reduction. In addition, the elastic modulus after cold work are close to the NiTi elastic modulus, although the elastic and plastic strain values are far from the ones seen in NiTi. The thermal treatment had also had an effect on the elastic modulus values. An increase in the heat-treatment duration is translated in higher values of elastic modulus. This behaviour concurs with the results obtained by Wang et al. 11 on which a TiNbTaZr alloy rolled by 99% cold reduction ratios in thickness was treated at 873 K and 1223 K for 1.2 ks. During cyclic tensile testing a modulus of elasticity lower than 60 GPa and axial recoverable strain greater than 3% were observed with stress hysteresis resembling a reversible stress-induced martensitic transformation at a test temperature of 150°C. Similar behaviour was observed in a Ti–35Nb–2Ta–3Zr alloy 11, but in this case the strain recovery did not fully returned to the initial level. A study by Miyazaki et al. 7 also reported shape memory effect and superelastic behavior in the Ti–22Nb–0.5O (at.%) alloy and Ti–22Nb–(1.0–2.0)O (at.%) alloys, respectively. TEM studies revealed a microstructure composed of austenite β-phase (BCC), orthorhombic martensite α´´, ω-phase and amorphous phase. The bright field images were the typical ones of nano-grained microstructures. The strong crystalline reflections belong to the austenite phase whereas the weak martensite reflections indicate that only a small amount of martensite is retained. This results agree with the results reported by Xie et al. 4 except for the fact that they did not observed ω-phase. The presence of the ω-phase in our specimens might be explained owing to low β-phase stability that promoted ω-phase formation during cold working, as was reported by Tane et al. 10 when studying the Ti–Nb–Ta–Zr–O alloy. In this study was also found that 90% cold working induced an increase in the Young’s modulus attributable to α″ martensite phase (0.09% O) and ω phase (0.09, 0.30, and 0.47% O) formation in the β phase matrix. This
243 could explain the fact that the modulus of the wires increased as the % of cold work increased too. The fatigue testing revealed that the Ti25Nb21Hf alloy had better life expectancy than NiTi and 316L. Moreover, when the fatigue was tested in PBS at body temperature, negligible saline impact on fatigue results was observed. 5. CONCLUSION The novel TiNbHf alloy presents superelasticity and phase transformation and there is no saline impact on fatigue results. These properties along with the fact that all components are biocompatible make TiNbHf alloy a potential product for nickel-free service as a superelastic material for medical device applications. TiNbHF alloy could be used in orthodontic wires for dental purposes, in intravascular stents, as bone fracture fixtures,staples for foot surgery etc. A thorough study of the effect of the cold work on the microstructure should be done. It would be convenient to determine grain size triggered by the different grades of cold work done in the wires as well as have an indexation of the rings observed in the bright field images. A texture analysis would be also of interest. Apart from the extensive microstructural characterization, further efforts should be directed to improve heat-treatment (variation of the temperature, combination of heattreatments, etc.) and alloy composition improvement (addition of other elements) to achieve superelasticity at low temperatures and eliminate ω-phase. The addition of other alloying elements should be taken into account as well.
244 6. BIBLIOGRAPHY 1. Wang, G.-F., Feng, X.-Q., Yu, S.-W. & Nan, C.-W. Interface effects on effective elastic moduli of nanocrystalline materials. Mater. Sci. Eng. A 363, 1–8 (2003). 2. Meyers, M. A., Mishra, A. & Benson, D. J. Mechanical properties of nanocrystalline materials. Prog. Mater. Sci. 51, 427–556 (2006). 3. Raducanu, D. et al. Mechanical and corrosion resistance of a new nanostructured Ti-Zr-Ta-Nb alloy. J. Mech. Behav. Biomed. Mater. 4, 1421–30 (2011). 4. Xie, K. Y. et al. Nanocrystalline β-Ti alloy with high hardness, low Young’s modulus and excellent in vitro biocompatibility for biomedical applications. Mater. Sci. Eng. C. Mater. Biol. Appl. 33, 3530–6 (2013). 5. Hou, F. Q., Li, S. J., Hao, Y. L. & Yang, R. Nonlinear elastic deformation behaviour of Ti–30Nb–12Zr alloys. Scr. Mater. 63, 54–57 (2010). 6. Hao, Y. L., Li, S. J., Sun, S. Y., Zheng, C. Y. & Yang, R. Elastic deformation behaviour of Ti-24Nb-4Zr-7.9Sn for biomedical applications. Acta Biomater. 3, 277–86 (2007). 7. Miyazaki, S., Kim, H. Y. & Hosoda, H. Development and characterization of Nifree Ti-base shape memory and superelastic alloys. Mater. Sci. Eng. A 438-440, 18–24 (2006). 8. Callister, W. D. & Rethwisch, D. G. Materials science and engineering. 8th, (John Wiley & Sons, 2011). 9. Giannuzzi, L. A. & Stevie, F. A. A review of focused ion beam milling techniques for TEM specimen preparation. Micron 30, 197–204 (1999). 10. Tane, M. et al. Low Young’s modulus in Ti–Nb–Ta–Zr–O alloys: Cold working and oxygen effects. Acta Mater. 59, 6975–6988 (2011). 11. Wang, L., Lu, W., Qin, J., Zhang, F. & Zhang, D. The characterization of shape memory effect for low elastic modulus biomedical β-type titanium alloy. Mater. Charact. 61, 535–541 (2010).
245 Chapter 11 CASHB Fragment Fabrication 1. Introduction .......................................................................................................................... 247 2. Materials and methods ........................................................................................................ 247 2.1 RNA extraction and reverse transcription .......................................................... 247 2.2 Primers design ..................................................................................................... 247 2.3 PCR amplification ............................................................................................... 249 2.4 Fragments clonning procedure ............................................................................ 249 2.5 DNA fragments digestion ................................................................................... 249 2.6 Plasmid and fused DNA ligation ........................................................................ 251 3. Results .................................................................................................................................. 251 3.1 Amplification of the FN fragments ..................................................................... 251 3.2 Plasmid-fused DNA ligation ............................................................................... 252 3.3 Fragment sequencing .......................................................................................... 253 3.4 CASHBII fragment expression and purification................................................. 256 5. Conclusion ........................................................................................................................... 258 6. Bibliography ......................................................................................................................... 260
246
247 1. INTRODUCTION One of the aims of this thesis was to synthesise fibronectin recombinant fragments to improve cell interaction and thus, biomaterial's integration. The recombinant protein technique 1,2 arises as a potential solution to the weak points of peptides. When dealing with recombinant proteins the signalling zone of the ECM protein of interest can be spanned and thus, their properties and functions 3. Another strong point of recombinant proteins is that some characteristics as protein immobilization, orientation or activity may be modulated by modification of some amino acids without affecting their function. Moreover, there is the possibility to combine sequences, join different fragments, etc. As was seen in Chapter 7, the CAS and HBII fragments improved the activity of the linear and cyclic RGD peptides; as well as triggered a similar response to FN where they were combined. Previous works which worked with fibronectin fragments used fragments separatelly4–9 or the sequence spanning from the FNIII8-14 10. In the present thesis two fragments of fibronectin were synthesized, the CAS and the HBII, and combined in an attempt to mimic fibronectin cell response. No evidence of research work regarding the union of both fragments was found. Thus, owing to the good results obtained with the fragments combination, and to go a step further, the fusion of both fragments was proposed. 2. MATERIALS AND METHODS 2.1 RNA extraction and reverse transcription Since the fragments used were the CAS and the HBII, the RNA extraction and reverse transcription was done as explained in Chapter 2, section 4.1. 2.2 Primers design The DNA sequences used to amplify the FNIII 8-10 and the FNIII 12-14 of Homo sapiens fibronectin were obtained from the nucleotide NCBI database (www.ncbi.nlm.nih.gov/). For each fragment, CAS or HB II, the primer, the reading
254 in the 5’ direction and in the 3’ direction. To check the sequence in the 3’ direction the DNA sequence obtained was transformed into the complementary form and was read in the reverse direction. First of all the primers were identified, then the targets and finally the DNA fragment sequence. Since the amplification process can introduce mutations, the nucleotides obtained were compared with the original ones. If there has been any change in the DNA sequence, this could lead to an amino acid substitution or to a truncated protein. Sometimes this mutation leads to no error in transcription because there is more than one amino acid that codifies the same protein as could be seen in Table 3 of Chapter 5. The underlined zones correspond to the primers’ sequence. The primer, the reading direction, the target, the added of the starting guideline and of the riding guideline are detailed in Fig.1. The d1 primer is marked in red; the d2rv primer is marked in green; the d2 primer is marked in orange; the d3 primer is marked in purple and the restriction enzyme targets in blue. The CASHBII sequence is underlined in grey and the mutations are in black. The sequence for the pGEX 5’ direction was: AATCGGATCTGGAAGTTCTGTTCCAGGGGCCCCTGGGATCCCCGGAATTCCCGGGTCGACAAGTTCCTCC TCCCACTGACCTGCGATTCACCAACATTGGTCCAGACACCATGCGTGTCACCTGGGCTCCACCCCCATCC ATTGATTTAACCAACTTCCTGGTGCGTTACTCACCTGTGAAAAATGAGGAAGATGTTGCAGAGTTGTCAA TTTCTCCTTCAGACAATGCAGTGGTCTTAACAAATCTCCTGCCTGGTACAGAATATGTAGTGAGTGTCTC CAGTGTCTACGAACAACATGAGAGCACACCTCTTAGAGGAAGACAGAAAACAGGTCTTGATTCCCCAACT GGCATTGACTTTTCTGATATTACTGCCAACTCTTTTACTGTGCACTGGATTGCTCCTCGAGCCACCATCA CTGGCTACAGGATCCGCCATCATCCCGAGCACTTCAGTGGGAGACCTCGAGAAGATCGGGTGCCCCACTC TCGGAATTCCATCACCCTCACCAACCTCACTCCAGGCACAGAGTATGTGGTCAGCATCGTTGCTCTTAAT GGCAGAGAGGAAAGTCCCTTATTGATTGGCCAACAATCAACAGTTTCTGATGTTCCGAGTTGCTCTTAAT GGCAGAGAGGAAAGTCCCTTATTGATTGGCCAACAATCAACAGTTTCTGATGTTCCGAGGGACCTGGAAG TTGTTGCTGCGACCCCCACCAGCCTACTGATCAGCTGGGATGCTCCTGCTGTCACAGTGAGATATTACAG GATCACTTACGGAGAAACAGGAGGAAATAGCCCTGTCCAGGAGTTCACTGTGCCTGGGAGCAAGTCTACA GCTACCATCAGCGGCCTTAAACCTGGAGTTGATTATACCATCACTGTGTATGCTGTCACTGGCCGTGGAG ACAGCCCCGCAAGCAGCAAGCCAATTTCCATTAAGCTTGCTATTCCTGCACCAACTGACCTGAAGTTCAC TCAGGTCACACCCACAAGCCTGAGCGCCCAGTGGACACCACCCAATGTTCAGCTCACTGGATATCGAGTG CGGGTGACCCCCANGGANAAAACGGGACCAATGAAAAAAATCAACCTTGCTCCTGANAGCTCATCCGGGG NTGTNTCANGGACTTATGGGGGNCNNCNAAANNNGAANNNGAGNGTNTATNCTCTTAAGGAAACTTNGAA AAGCAAAACANCTCAGGGGGTTGTCNCCNCTTTGNANAANGTCCCCCCCCAAAAAGGGNCNTGNNNANAA ATNCTTTTGNAAACCCCCTCCCCTTTNNTGGGNAAACAAAAAGGAAAAAANCCNNGGNTTCCAAGTTGAG
255 GCCNTCCCCCCCAGGGGCAAACCCTTTCNAAAACCCTNNNCGANNTNAAANCNCCCCCCCNGGNTTAAAN NGGNCGGNANAAAAAATCNNGNNCCTGGGAAAGGGG The sequence for the pGEX 3’ direction was: CCTGNNNCGAAACGCGCGAGGCAGATCGTCAGTCAGTCACGATGGCGGCCGCTGTCTTTTTCCTTCCAAT CAGGGGCTCGCTCTTCTGATTATTCTTCAGGGCAATGACATAAATTGTATATTCGGTTCCCGGTTCCAGG CCAGTAATAGTAGCCTCTGTGACACCAGGGCGGGGCCGAGGGACCACTTCTCTGGGAGGAGACCCAGGCT TCTCATACTTGATGATGTAGCCGGTAATCCTGGCACGTGGCGGCTGCCATGATACCAGCAAGGAATTGGG TGTGGTGGCCAGGAAACGCAGGTTGGATGGTGCATCAATGGCAGTGGAGGCGTCGATGACCACAGGGGAG CTCCGAGCATTGTCATTCAAGGTGTACAGGTAGATCTTGTAGTCAGTGCCTGGTTGTAAACCTGTGATGG TGTAGCTTCTGACATCTGGCTTGATGGTTCTCTGGATTGGAGTCTGGCCATTGGCTGGAACGGCATCAAC TTGGAAGCCAGTGATCGTCTCAGTCTTGGTTCTCCAGCTAATGGTGATGGTGGTCTCAGTAGCATCTGTC ACACGAGCCCTTCTTGGTGGGCTGACATTCTCCAGAGTGGTGACAACACCCTGAGCTGGTCTGCTTGTCA AAGTGTCCTTAAGAGCATAGACACTCACTTCATATTTGGTGGCCACCATAAGTCCTGATACAACCACGGA TGAGCTGTCAGGAGCAAGGTTGATTTCTTATTGGTCCGTCTTCTCCTTGGGGGTCACCCGCACTCGATAT CCAGTGAGCTGAACATTGGGTGGTGTCCACTGGGCGCTCAGGCTTGTGGGTGTGACCTGAGTGAACTTCA GGTCAGTTGGTGCAGGAATAGCAAGCTTAATGGAAATTGGCTTGCTGCTTGCGGGGCTGTCTCCACGGCC AGTGACAGCATACACAGTGATGGTATAATCAACTCCAGGTTTAAGGCCNCTGATGGTANCTGTAAACTTG CTCCNAGGCACAGTGAACTCCTGGANAGGGCTATTTCCCCCTGTTTCCCCGNAANTGATCCTGNAAAATC TCACTGGGAANANCAGGANCATCCCANCTGATCANNAGGCTGGNGGGGGTCCNAACAANANTTCCAGGTC CCTCGGAAANATCAAAAACTGTTAATTGTNGGCCANCCAAAAGGNACTTNCCTCTTGCCATAAAAAAAAN AAGCNAACCAAANCNTTTNCCNNGAANNAGTTTNNAANGGNAAAAANTCCAAAAGGGGGNNCCCATTTNT CAAGNTNCCNNNAAAGNCCCGNAAAAAGGNAACCTNANCCNGNNGGGGCCNGAAAAACCCNGCNAAAAAA AANTGGNAAAAAAAAAAAANCCCNGGGAAAAAC The results obtained showed one nucleotide change during the RT-PCR for the CASHBII in the pGEx 5' direction and another in the 3' direction. In the pGEX 5' direction, a G codon base was mutated into an A codon base, but this mutation did not affect the translation, because according to the codon chart both GAA and GAG translate the same amino acid: Glutamate. In the pGEX 3' direction, a T codon base was mutated into an A codon base, but as occurred in the pGEX 5' direction, the mutation did not affect the translation because both ACA and ACT translate the same amino acid: Tyrosine. It is important to highlight the fact that the sequencing technique has a limitation in the number of bases read, so it was not possible to read the whole sequence CASHBII in only one direction. Despite this it is clear that in the pGEX5' direction the CAS
256 sequence was first, then the D2rv primer, the D2 primer (corresponding to the HBII sequence) and the first nucleotides of the HBII sequences. Taking a look to the pGEX3' direction, the D3 primer corresponding to the HBII fragment is present, then the HBII sequence joint with the D2 primer and the D2rv primer (corresponding to the CAS sequence) and finally the first nucleotides of the CAS fragment. This was an evidence of the fragments fusion. 3.4 CASHBII fragment expression and purification The CASHBII sequence has a molecular weight of approximately 65kDa. After purification, the chromatograms showed no evidence of a peak related to protein elution. For this reason, a SDS-PAGE was done prior to purification. After bacterial culture and protein induction, the culture was sonicated to extract the expressed proteins by E.coli. As one of the problems of the lack of CASHBII fragment expression might be insolubility, the pellet was also studied. Fig.119 shows the result of the SDS-PAGE done with the supernatant and the pellet. As can be seen, there is no evidence of a band at 65kDa, which is the molecular weight of the CASHBII fragment neither in the supernatant bands nor in the pellet bands. Fig.119 SDS-PAGE of the CASHBII fragment. Bans correspond to proteins obtained after sonication in the supernatant and in the pellet. The ladder used was Precision Plus Protein™ Dual Color Standards from BioRad.
257 According to The Recombinant Protein Handbook from Amersham Pharmacia Biotech, if no protein is detected in bacterial sonicate it might be needed an optimization of the culture conditions to improve yield. Then, the effect of cell strain, medium composition, incubation temperature and induction conditions should be studied. Exact conditions will vary for each fusion protein expressed. This led us to study the expression of the fragment at different culture temperatures and with different concentrations of the promoter IPTG. The culture was done at 25ºC and 30ºC. As can be seen in Fig.120, no bands corresponding to the CASHBII fragment were detected. Fig.120 SDS-PAGE of the CASHBII fragment. Bans correspond to proteins obtained after sonication (S) in the supernatant and in the pellet (P) when cultured at 25ºC and 30ºC and at IPTG concentration of 1mM. The ladder used was Precision Plus Protein™ Dual Color Standards from BioRad. Fig.121 shows the results obtained after induce the protein with IPTG at 1mM, 0,5mM, 0,2mM and 0,1mM. According to the bands obtained, these IPTG concentrations did not trigger the proper expression of the CASHBII fragment.
258 Fig.121 SDS-PAGE of the CASHBII fragment. Bans correspond to proteins obtained after sonication (S) in the supernatant and in the pellet (P) protein was induced at different IPTG concentrations and at 37ºC. The ladder used was Precision Plus Protein™ Dual Color Standards from BioRad. 5. CONCLUSION Both the CAS and HBII fragments were fused successfully according to sequencing and the plasmids were able to insert the fused fragment. Despite this, the expression of the fragment was not successful. Different culture temperatures and inducer concentrations were studied without achieve protein expression. Further studies should be done regarding alterations of the growth conditions to achieve protein expression such as try another growth temperatures within the range of +20° to +30°C to improve solubility, decrease IPTG concentration to <0.1 mM to alter induction level, alter time of induction, induce for a shorter period of time or induce at a higher cell density for a short period of time. The disruption procedure (sonication) should be also checked. Cell disruption is seen by partial clearing of the suspension or by microscopic examination. Addition of lysozyme (0.1 volume of a 10 mg/ml lysozyme solution in 25 mM Tris™-HCl, pH 8.0) prior to sonication may improve results. Avoid frothing as this may denature the fusion protein. Check for expression by immunoblotting would be another useful tool. Some fusion proteins may be masked on an SDS-polyacrylamide gel by a bacterial protein of
259 approximately the same molecular weight. Immunoblotting can be used to identify fusion proteins in these cases. Ultimately, the E.coli strain and/or the plasmid could be changed.
260 6. BIBLIOGRAPHY 1. García, A. J., Schwarzbauer, J. E. & Boettiger, D. Distinct Activation States of α5β1 Integrin Show Differential Binding to RGD and Synergy Domains of Fibronectin†. Biochemistry 41, 9063–9069 (2002). 2. García, A. J. & Reyes, C. D. Bio-adhesive Surfaces to Promote Osteoblast Differentiationand Bone Formation. J. Dent. Res. 84, 407 (2005). 3. Sørensen, H. P. & Mortensen, K. K. Advanced genetic strategies for recombinant protein expression in Escherichia coli. J. Biotechnol. 115, 113–128 (2005). 4. Petrie, T. A., Capadona, J. R., Reyes, C. D. & García, A. J. Integrin specificity and enhanced cellular activities associated with surfaces presenting a recombinant fibronectin fragment compared to RGD supports. Biomaterials 27, 5459–5470 (2006). 5. Petrie, T. A. et al. The effect of integrin-specific bioactive coatings on tissue healing and implant osseointegration. Biomaterials 29, 2849–57 (2008). 6. Petrie, T. A., Reyes, C. D., Burns, K. L. & García, A. J. Simple application of fibronectin-mimetic coating enhances osseointegration of titanium implants. J. Cell. Mol. Med. 13, 2602–2612 (2009). 7. Rico, P., González-García, C., Petrie, T. A., García, A. J. & Salmerón-Sánchez, M. Molecular assembly and biological activity of a recombinant fragment of fibronectin (FNIII7–10) on poly(ethyl acrylate). Colloids Surfaces B Biointerfaces 78, 310–316 (2010). 8. Woods, A., Couchman, J. R., Johansson, S. & Höök, M. Adhesion and cytoskeletal organisation of fibroblasts in response to fibronectin fragments. EMBO J. 5, 665–70 (1986). 9. Dalton, B. A., McFarland, C. D., Underwood, P. A. & Steele, J. G. Role of the heparin binding domain of fibronectin in attachment and spreading of human bonederived cells. J. Cell Sci. 108, 2083–2092 (1995). 10. Kim, J.-H., Park, S.-O., Jang, H.-J. & Jang, J.-H. Importance of the heparinbinding domain of fibronectin for enhancing cell adhesion activity of the recombinant fibronectin. Biotechnol. Lett. 28, 1409–13 (2006).
261