1 Biocompatible 3D Printed Yttria-Stabilized Zirconia parts using Direct Ink Writing Irene Buj-Corral1,*, Hector Sanz-Fraile2, Aitor Tejo-Otero1, Elena Xuriguera3, Jorge Otero 2,4 1 Department of Mechanical Engineering, School of Engineering of Barcelona (ETSEIB), Universitat Politècnica de Catalunya, Av. Diagonal, 647, 08028 Barcelona, Spain 2Unit of Biophysics and Bioengineering. School of Medicine and Health Sciences. Universitat de Barcelona. Barcelona. Spain. 3 Department of Materials Science and Physical Chemistry, Universitat de Barcelona, Carrer Martí i Franquès 1, 08028 Barcelona, Spain 4 CIBER de Enfermedades Respiratorias, Madrid, Spain *Corresponding author:
[email protected] Abstract Metals such as titanium alloys or Cr-Co alloys have been the most widely used materials in biomedical applications that require high mechanical properties, such as implantology. However, a major disadvantage of these materials is related to the release of ion metals to the body. As an alternative, prostheses made of ceramic materials produce less debris and have better durability. The aim of the present work is to culture human bone-marrow-derived mesenchymal stem cells (hBM-MSCs) on 3D printed rough yttria-stabilized zirconia parts to study their biocompatibility. For that, surface roughness and biocompatibility tests are carried out, and it was confirmed that 3 mol % yttria-stabilized zirconia is a promising material due to its high biocompatibility. 1. Introduction Metals have been the most widely used materials in biomedical applications that require excellent mechanical properties, such as implantology. However, a major disadvantage of these materials is related to the release of ion metals. These may cause inflammatory and hypersensitivity reactions 1. Additionally, a failure in medical implants such as hip or knee would lead to the removal of the device and the need to implant a new one. As an alternative, research in the use of ceramics is growing in popularity. Prostheses made from ceramic materials produce less debris and have better durability than those made from metals or plastics 2.
2 Amongst the different ceramics used in prosthetics (such as hydroxyapatite 3, or alumina 4,5), zirconia 4 offers several advantages: (1) reduction in the wear rate of implants 6 and the risk of toxicity 7; (2) excellent biocompatibility 8 and corrosion resistance 9; (3) outstanding mechanical properties for the manufacture of prostheses 8. Zirconia has a monoclinic structure at room temperature. As temperature increases, it changes to tetragonal and later to cubic. The transition between monoclinic and tetragonal leads to an important volume change. For this reason, yttria is often added to zirconia to stabilize it with a mix of tetragonal and cubic structures at room temperature 10. Among the different parameters that can affect the performance of the ceramics is related to their surface roughness, for example in terms of fracture toughness. One of the most employed AM techniques for ceramics is Direct Ink Writing (DIW), an extrusion technique in which a ceramic paste is extruded and subsequently deposited layer-by-layer11. Different ceramic materials can be printed with DIW, for example, kaolinite clay ceramics12, zirconia13, zirconia-toughened alumina14 or hydroxiapatite15. Yttria-stabilized zirconia (YSZ) is a biocompatible ceramic with high mechanical properties. It also has the advantage that it can be 3D printed in order to manufacture complex shapes such as prostheses or dental implants 16,17. Nevertheless, to the author’s knowledge, few in vitro studies are known for proving the biocompatibility of 3D printed YSZ 18,19. On the other hand, the surface finish of ceramics is known to affect their mechanical properties 20 and also influence their biocompatibility21. In addition, surface roughness is related to bacterial growth in dental implants22. The aim of the present research study is to culture human bone-marrow-derived mesenchymal stem cells (hBM-MSCs) on 3D printed yttria-stabilized zirconia parts with different surface roughness values to assess their suitability. 2. Materials and Methods 2.1. Zirconia parts preparation for cell culture Zirconia pastes were prepared in a mixer. Mixing time was 2 min and rotational speed was 2000 min-1. Vacuum pressure was used to enable both dispersions of materials and removal of bubbles (ARV-310P Thinky Corporation, Tokyo, Japan). Yttria-stabilized zirconia (YSZ) with a 3 mol% concentration (HSY-3B, Daiichi Kigenso Kagaku Kogyo Co., Ltd., Japan) and a 0.5 % wt dispersant (Dolapix PC75, Zschimmer & Schwarz, Germany) were mixed to a Pluronic F-127
3 (Sigma-Aldrich, UK) stock solution of 25 wt% concentration. The final solid percentage was 40 v%. The d50 value of the ceramic powder ranged between 0.7 and 1.5 μm. Disk-shaped samples of diameter 10 mm and height 4 mm were printed and subsequently sintered at 1550 °C, with a heating rate of 5 °C/min. The final dimensions of the disks were around 8.5 mm in diameter and 3 mm in height. A linear infill pattern of raster angle 0° was used, with different infill values of 80% and 95% respectively. Three replicates were considered for each experiment. A customized 3D printer was used, Dual Paste Extruder, from CIM-UPC (Figure 1). Nozzle diameter was 0.58 mm, layer height was 0.3 mm, printing speed was 5 mm/s and the extrusion multiplier was 100%. 2.2. Surface roughness characterization According to 23, the different roughness parameters can be divided into six groups: (1) amplitude, (2) spatial, (3) hybrid, (4) functional, (5) feature, and (6) other 3D parameters. In the present study, not only areal an arithmetical mean studied, but also skewness (Ssk) and kurtosis (Sku). Sa (Equation 1) is the average value of the heights, expressed as an absolute value, regarding the central plane 13. Ssk (Equation 2) corresponds to the symmetry of the heights concerning the central plane. A positive Ssk value indicates the predominance of peaks, while a negative value corresponds to the predominance of valleys 24. Kurtosis parameter Sku (Equation 3) is related to the peakedness of the surface. Sharp peaks and valleys correspond to Sku >3, while rounded peaks and valleys are related to Sku <3 24. Both parameters are related to the friction control of surfaces 25. A Smartproof 5 confocal microscope (Zeiss, Oberkochen, Germany) was used to measure areal roughness, with a 20X magnification lens. Optical equipment was used, to prevent damage to Figure 1. Printing head of the Dual Paste extruder from CIM-UPC Nozzle 3D Printed Scaffold Piston X-Y platform Motor Material with the syringe
4 the samples and/or to the tip of a contact roughness meter 26. The uncertainty of the microscope in the vertical direction is ± (0.1 µm + 0.008 × L), whereas in the horizontal direction it is ± (0.1 µm + 0.012 × L). Areal parameters were determined according to ISO 25178 standard 27. 𝑆𝑆𝑎𝑎=1 𝐴𝐴 �|𝑍𝑍 (𝑥𝑥,𝑦𝑦)| 𝑑𝑑𝑥𝑥𝑑𝑑𝑦𝑦 𝐴𝐴 (1) 𝑆𝑆𝑘𝑘𝑘𝑘 =1 𝐴𝐴𝑞𝑞 4 � |𝑍𝑍 (𝑥𝑥,𝑦𝑦)|3 𝑑𝑑𝑥𝑥𝑑𝑑𝑦𝑦 𝐴𝐴 (2) 𝑆𝑆𝑠𝑠𝑘𝑘 =1 𝐴𝐴 �|𝑍𝑍 (𝑥𝑥,𝑦𝑦)| 𝑑𝑑𝑥𝑥𝑑𝑑𝑦𝑦 𝐴𝐴 (3) where A is the measured area and Z (x, y) is a function that corresponds to the surface topography. Roughness was measured on the upper surface of the disks, within an area of 0.5 x 0.5 mm. 2.3. BM-MSCs culture hBM-MSCs are widely used in regenerative medicine and they are a widely accepted model to test the biocompatibility of new scaffold developments 28. hBM-MSCs were expanded and cultured following the manufacturer’s instructions (ATCC, VA). The medium was replaced every 2 days and cells were split from T-75 flasks at reaching 80% confluence. Cells in passage 5 were used for this study. 3D printed zirconia scaffolds were sterilized by high pressure and vapor using an autoclave (Tomy SX-700E) before seeding the cells, and half of them were coated with type I collagen at a concentration of 0.1 mg/mL (Merck, US). Cells were seeded with a density of 4·104 cells/cm2 and cultured for 24h and 72h. At the endpoint, samples were stained for DNA (NucBlue) to identify cell nuclei and imaged with a confocal microscope with a monitored X-Y stage (Nikon TI-HUBC, Japan) with a 10x objective. 3. Results and Discussion 3.1. Surface Roughness Table 1 shows the average values of areal arithmetic mean, skewness, and kurtosis of both 80% and 95% porosity experiments. Overall, both porosities show a smooth roughness, no sharp or rounded valley or as well as the presence of high peaks or deep valleys. Figure 2 shows the surface topography of the 3D-printed parts.
5 Table 1. Surface roughness of the upper surface of the yttria-stabilized zirconia samples. Sa [µm] Ssk Sku 80% porosity 0.30±0.026 -0.002±0.48 10.35±8.37 95% porosity 0.69±0.007 -0.137±0.048 5.03±0.41 The surface topographies show that the different printed lines were fused, showing no holes among them. In Figure 2a, several parallel crests are observed, corresponding to the deposition of material along parallel lines in the linear structure. In Figure 2b only some crests are observed, showing that, due to an excess of material, the paste has mixed. As for Sa values in Table 1, higher roughness values are observed for 95 % infill (Figure 2b) than for 80 % infill (Figure 2a). This suggests that, for high infill value of 95 % there is an excess of material that leads to higher crests. A slightly negative value for Ssk was reported for 95 % infill (Figure 2b), showing higher valleys than peaks. As for Sku, the high value of 10.35 was obtained for 80 % infill, corresponding to sharp peaks and valleys, with a lower value of 5.03 for 95 % infill. In both cases, Sku was higher than 3, which corresponds to a normal distribution of heights. Shao et al. 29 reported surface roughness close to 8 μm for zirconia. For implants, Sa values below or equal to 1 µm are considered to be smooth, while values above 1 µm are rough 30. Therefore, the samples in the present study are smooth and, therefore, it is not necessary to undertake a subsequent polishing operation. Additionally, the surface roughness obtained in lateral walls of (b) (a) Figure 2. Surface topography of YSZ parts printed with: (a) 80% infill, (b) 95% infill
6 yttria-stabilized zirconia pastes depends on print speed. The lower speed, the smoother the surface is 31. In the present work, however, the roughness was measured on the upper surface of the printed parts to assess its influence on cell compatibility. 3.2. In vitro biocompatibility assessment As can be observed in Figure 3, hBM-MSCs were able to attach to the 3D printed zirconia scaffolds and showed good viability after 3 days of culture (no differences were observed between 24h and 72h of culture). It is noticeable that no differences were observed between uncoated and coated samples (type I collagen), showing that the bare material is biocompatible enough to allow direct cell culture on top without the need for functionalization, so unspecific adhesions formed by MSCs on bare scaffolds are enough for them to proliferate. Collagen has been proven to enhance biocompatibility mainly on metallic substrates such as titanium32 or magnesium alloys33 but it might not be so effective on ceramic substrates. On the other hand, although a higher proliferation might be observed in the higher infill scaffolds, the difference is not significant enough to extract conclusions about the most appropriate infill parameter. The surface properties of the scaffolds directly affect cellular behavior. A too smooth or too rough scaffold could cause the cells not to adhere or to modify their behaviour. For example, in soft hydrogels osteodifferentiation increased with surface roughness, being important from Rq values around 0.38 μm, while in stiff hydrogels higher osteodifferentiation was observed for intermediate roughness values34. In this work, the areal average roughness Sa measured in the Figure 3. Fluorescent images (DAPI, cell nuclei) of hBM-MSCs cultured for 24h or 72h on zirconia scaffolds (80% or 95% of porosity) with and without type I collagen coating.
7 above scaffolds, between 0.30±.026 μm and 0.69±0.0 μm, led to a good cell proliferation behavior as shown in Figure 3. Thus, it seems that scaffolds’ roughness makes them suitable for MSCs culture. 4. Conclusions In the present work, 3D-printed yttria-stabilized zirconia parts are presented to be used as a novel material in implantology. It was found that the physical properties of the material, such as the surface topography, make the material a suitable candidate for prosthetics. The culture on top of the developed scaffolds of hBM-MSCs showed high viability. Interestingly, there was no difference between bare parts and those coated with an extracellular matrix protein to increase adhesion, so the 3D printed scaffolds could be used without further processing. This opens a door in the field of personalized medicine, as scaffolds could be directly printed with the needed shape before the intervention in the patient. Further research in vivo, by implanting the developed scaffolds in animals, would be needed to evaluate the scaffolds presented herein, but in vitro results suggest that biocompatibility would not be a limiting factor in those experiments. Acknowledgments This work was co-financed by the European Union Regional Development Fund within the framework of the ERDF Operational Program of Catalonia 2014–2020 with a grant of 50% of total cost eligible, project BASE3D, grant number 001-P-001646. Authors would like to thank Alejandro Domínguez and Daniel Vidal for their help with the experimental tests. References 1. Czarnek K, Terpilowska S, Siwicki AK. Selected aspects of the action of cobalt ions in the human body. Cent Eur J Immunol 2015; 40: 236–242. 2. Lerouge S, Huk O, Yahia L, et al. Characterization of in vivo wear debris from ceramicceramic total hip arthroplasties. J Biomed Mater Res 1996; 32: 627–633.
8 3. Hamdi DA, Jiang ZT, No K, et al. Biocompatibility study of multi-layered hydroxyapatite coatings synthesized on Ti-6Al-4V alloys by RF magnetron sputtering for prostheticorthopaedic implant applications. Appl Surf Sci 2019; 463: 292–299. 4. De Aza AH, Chevalier J, Fantozzi G, et al. Crack growth resistance of zirconia toughened alumina ceramics for joint prostheses. Key Eng Mater 2001; 23: 1535–1538. 5. Zeng P. Biocompatible alumina ceramic for total hip replacements. 2008. Epub ahead of print 2008. DOI: 10.1179/174328408X287682. 6. Jiang L, Liao Y, Wan Q, et al. Effects of sintering temperature and particle size on the translucency of zirconium dioxide dental ceramic. J Mater Sci Mater Med 2011; 22: 2429– 2435. 7. Bearden LJ, Cooke FW. Growth inhibition of cultured fibroblasts by cobalt and nickel. J Biomed Mater Res 1980; 14: 289–309. 8. Gautam C, Joyner J, Gautam A, et al. Zirconia based dental ceramics: structure, mechanical properties, biocompatibility and applications. Dalt Trans 2016; 45: 19194– 19215. 9. Bergman M, Bergman B, Söremark R. Tissue accumulation of nickel released due to electrochemical corrosion of non-precious dental casting alloys. J Oral Rehabil 1980; 7: 325–330. 10. Hayashi H, Saitou T, Maruyama N, et al. Thermal expansion coefficient of yttria stabilized zirconia for various yttria contents. Solid State Ionics. Epub ahead of print 2005. DOI: 10.1016/j.ssi.2004.08.021. 11. Lewis JA. Direct ink writing of 3D functional materials. Adv Funct Mater 2006; 16: 2193– 2204. 12. Revelo CF, Colorado HA. 3D printing of kaolinite clay ceramics using the Direct Ink Writing (DIW) technique. Ceram Int. Epub ahead of print 2018. DOI: 10.1016/j.ceramint.2017.12.219. 13. Buj-Corral I, Domínguez-Fernández A, Gómez-Gejo A. Effect of printing parameters on dimensional error and surface roughness obtained in direct ink writing (DIW) processes. Materials (Basel); 13. Epub ahead of print 2020. DOI: 10.3390/ma13092157. 14. Stanciuc AM, Sprecher CM, Adrien J, et al. Robocast zirconia-toughened alumina
9 scaffolds: Processing, structural characterisation and interaction with human primary osteoblasts. J Eur Ceram Soc. Epub ahead of print 2018. DOI: 10.1016/j.jeurceramsoc.2017.08.031. 15. Cesarano J, Dellinger JG, Saavedra MP, et al. Customization of load-bearing hydroxyapatite lattice scaffolds. Int J Appl Ceram Technol 2005; 2: 212–220. 16. Pieralli S, Kohal RJ, Jung RE, et al. Clinical Outcomes of Zirconia Dental Implants: A Systematic Review. J Dent Res 2017; 96: 38–46. 17. Pieralli S, Kohal RJ, Lopez Hernandez E, et al. Osseointegration of zirconia dental implants in animal investigations: A systematic review and meta-analysis. Dent Mater 2018; 34: 171–182. 18. Hodásová L, Sans J, Molina BG, et al. Polymer infiltrated ceramic networks with biocompatible adhesive and 3D-printed highly porous scaffolds. Addit Manuf; 39. Epub ahead of print 2021. DOI: 10.1016/j.addma.2021.101850. 19. Chen F, Zhu H, Wu JM, et al. Preparation and biological evaluation of ZrO2 all-ceramic teeth by DLP technology. Ceram Int 2020; 46: 11268–11274. 20. Shukla PP, Lawrence J, Wu H. Fracture toughness of a zirconia engineering ceramic and the effects thereon of surface processing with fibre laser radiation. Proc Inst Mech Eng Part B J Eng Manuf. Epub ahead of print 2010. DOI: 10.1243/09544054JEM1887. 21. Li M, Zhang L, Zhang C, et al. Effect of Y2O3 on the physical properties and biocompatibility of β–SiAlON ceramics. Ceram Int 2020; 46: 23427–23432. 22. Rashid H. The effect of surface roughness on ceramics used in dentistry: A review of literature. European Journal of Dentistry. Epub ahead of print 2014. DOI: 10.4103/1305- 7456.143646. 23. Deltombe R, Kubiak KJ, Bigerelle M. How to select the most relevant 3D roughness parameters of a surface. Scanning 2014; 36: 150–160. 24. LLC MM. 3D S Parameters - Height (Amplitude) Parameters. 25. Sedlaček M, Gregorčič P, Podgornik B. Use of the Roughness Parameters S sk and S ku to Control Friction—A Method for Designing Surface Texturing. Tribol Trans 2017; 60: 260– 266. 26. Oonishi H, Wakitani S, Murata N, et al. Clinical experience with ceramics in total hip