scieee AI-readable full text Open interactive document viewer

Biofunctionalization of REDV elastin-like recombinamers improves endothelialization on CoCr alloy surfaces for cardiovascular applications

Castellanos, Maria Isabel,Grau, Anna,Rodriguez Cabello, Jose Carlos,Gil Mur, Francisco Javier,Manero Planella, José María,Pegueroles Neyra, Marta

Abstract

To improve cardiovascular implant success, metal-based stents are designated to modulate endothelial cells adhesion and migration in order to prevent restenosis and late thrombosis diseases. Biomimetic coatings with extra-cellular matrix adhesive biomolecules onto stents surfaces are a strategy to recover a healthy endothelium. However, the appropriate bioactive sequences to selective promote growth of endothelium and the biomolecules surface immobilization strategy remains to be elucidated. In this study, biofunctionalization of cobalt chromium, CoCr, alloy surfaces with elastin-like recombinamers, ELR, genetically modified with an REDV sequence, was performed to enhance metal surfaces endothelialization. Moreover, physical adsorption and covalent bonding were used as biomolecules binding strategies onto CoCr alloy. Surfaces were activated with plasma and etched with sodium hydroxide previous to silanization with 3-chloropropyltriethoxysilane and functionalized with the ELR. CoCr alloy surfaces were successfully biofunctionalized and the use of an ELR with an REDV sequence, allows conferring bioactivity to the biomaterials surface, demonstrating a higher cell adhesion and spreading of HUVEC cells on the different CoCr surfaces. This effect is emphasized as increases the amount of immobilized biomolecules and directly related to the immobilization technique, covalent bonding, and the increase of surface charge electronegativity. Our strategy of REDV elastin-like recombinamers immobilization onto CoCr alloy surfaces via covalent bonding through organosilanes provides a bioactive surface that promotes endothelial cell adhesion and spreading. (C) 2015 Elsevier B.V. All rights reserved.

Full text

Elsevier Editorial System(tm) for Colloids and Surfaces B: Biointerfaces Manuscript Draft Manuscript Number: COLSUB-D-14-01450R1 Title: Biofunctionalization of REDV elastin-like recombinamers improves endothelialization on CoCr alloy surfaces for cardiovascular applications Article Type: Full Length Article Keywords: CoCr alloy, Surface functionalization, Elastin-like recombinamers, Biomimetic materials, Endothelialization Corresponding Author: Dr. Marta Pegueroles, Corresponding Author's Institution: Technical University of Catalonia First Author: Maria Isabel Castellanos Order of Authors: Maria Isabel Castellanos; Anne-Sophie Zenses; Anna Grau; Jose Carlos Rodríguez- Cabello; Francisco Javier Gil; José María Manero; Marta Pegueroles Manuscript Region of Origin: SPAIN Abstract: To improve cardiovascular implant success, metal-based stents are designated to modulate endothelial cells adhesion and migration in order to prevent restenosis and late thrombosis diseases. Biomimetic coatings with extra-cellular matrix adhesive biomolecules onto stents surfaces are a strategy to recover a healthy endothelium. However, the appropriate bioactive sequences to selective promote growth of endothelium and the biomolecules surface immobilization strategy remains to be elucidated. In this study, biofunctionalization of cobalt chromium, CoCr, alloy surfaces with elastin-like recombinamers, ELR, genetically modified with an REDV sequence, was performed to enhance metal surfaces endothelialization. Moreover, physical adsorption and covalent bonding were used as biomolecules binding strategies onto CoCr alloy. Surfaces were activated with plasma and etched with sodium hydroxide previous to silanization with 3-chloropropyltriethoxysilane and functionalized with the ELR. CoCr alloy surfaces were successfully biofunctionalized and the use of an ELR with an REDV sequence, allows conferring bioactivity to the biomaterials surface, demonstrating a higher cell adhesion and spreading of HUVEC cells on the different CoCr surfaces. This effect is emphasized as increases the amount of immobilized biomolecules and directly related to the immobilization technique, covalent bonding, and the increase of surface charge electronegativity. Our strategy of REDV elastin-like recombinamers immobilization onto CoCr alloy surfaces via covalent bonding through organosilanes provides a bioactive surface that promotes endothelial cell adhesion and spreading. Response to Reviewers: Responses to reviewer’s comments: We are grateful to reviewers for the critical comments and useful suggestions that have helped us to improve our paper. As indicated in the responses that follow, we have taken all these comments and suggestions into account in the revised version of our paper. Answers to the Reviewers’ comments are written in blue. The main text is revised according to these answers and written in red. To reviewer #1 CoCr alloy surface Surface activation Surface silanization NaOH etching Covalently immobilised ELR Elastin-like recombinamer, ELR ELR *Graphical Abstract (for review) Highlights  We immobilized an elastin-like recombinamer, ELR, on CoCr, alloy through physisorption and covalent bonding.  The ELR combines a bioactive motif specific for endothelial cell adhesion.  The ELR immobilization is enhanced with silanization and surface charge.  The ELR coated surfaces displayed an improved HUVEC cell adhesion and spreading. *Highlights (for review) 1 Title: Biofunctionalization of REDV elastin-like recombinamers improves endothelialization on CoCr alloy surfaces for cardiovascular applications Authors: Maria Isabel Castellanos1,2,3, Anne-Sophie Zenses1,3, Anna Grau1,3, Jose Carlos Rodríguez- Cabello2,4, Francisco Javier Gil1,2,3, Jose María Manero1,2,3, Marta Pegueroles1,2,3,*. Affiliations: 1 Biomaterials, Biomechanics and Tissue Engineering Group, Department of Materials Science and Metallurgy, Technical University of Catalonia (UPC), Av. Diagonal 647, 08028 Barcelona, Spain 2 Biomedical Research Networking Centre in Bioengineering, Biomaterials and Nanomedicine (CIBER-BBN), Maria de Luna 11, Ed. CEEI, 50118 Zaragoza, Spain 3 Centre for Research in NanoEngineering (CRNE), UPC, C/Pascual i Vila 15, 08028 Barcelona, Spain 4 GIR BIOFORGE (Group for Advanced Materials and Nanobiotechnology), Universidad de Valladolid (UVA), Valladolid 47011, Spain. Corr. Author: * Marta Pegueroles, PhD [email protected] Biomaterials, Biomechanics and Tissue Engineering Group Department of Materials Science and Metallurgy Technical University of Catalonia (UPC) Av. Diagonal 647 08028 Barcelona Spain. Tel: +34 934054154 Fax: +34 934016706 Maria Isabel Castellanos: mar[email protected] Anne-Sophie Zenses: a[email protected] Anna Grau: [email protected] Jose Carlos Rodríguez-Cabello: [email protected] Francisco Javier Gil: francesc.xavi[email protected] Jose María Manero: [email protected] Marta Pegueroles: [email protected] *Revised Manuscript Click here to view linked References 2 Abstract To improve cardiovascular implant success, metal-based stents are designated to modulate endothelial cells adhesion and migration in order to prevent restenosis and late thrombosis diseases. Biomimetic coatings with extra-cellular matrix adhesive biomolecules onto stents surfaces are a strategy to recover a healthy endothelium. However, the appropriate bioactive sequences to selective promote growth of endothelium and the biomolecules surface immobilization strategy remains to be elucidated. In this study, biofunctionalization of cobalt chromium, CoCr, alloy surfaces with elastin-like recombinamers, ELR, genetically modified with an REDV sequence, was performed to enhance metal surfaces endothelialization. Moreover, physical adsorption and covalent bonding were used as biomolecules binding strategies onto CoCr alloy. Surfaces were activated with plasma and etched with sodium hydroxide previous to silanization with 3-chloropropyltriethoxysilane and functionalized with the ELR. CoCr alloy surfaces were successfully biofunctionalized and the use of an ELR with an REDV sequence, allows conferring bioactivity to the biomaterials surface, demonstrating a higher cell adhesion and spreading of HUVEC cells on the different CoCr surfaces. This effect is emphasized as increases the amount of immobilized biomolecules and directly related to the immobilization technique, covalent bonding, and the increase of surface charge electronegativity. Our strategy of REDV elastin-like recombinamers immobilization onto CoCr alloy surfaces via covalent bonding through organosilanes provides a bioactive surface that promotes endothelial cell adhesion and spreading. Keywords CoCr alloy; Surface functionalization; Elastin-like recombinamers; Biomimetic materials; Endothelialization. 3 1. Introduction 1 Coronary angioplasty and stent insertion is the major surgery to solve cardiovascular disease [1,2]. However, in-stent 2 restenosis (ISR), stents thrombosis (ST) and incomplete stent endothelialization remain the principal mechanisms for 3 the failure of the bare-metal stents (BMS) and drug-eluting stents (DES) after implantation [3]. Interestingly, ISR, is 4 developed in 20%-30% of lesions treated with BMS and in <10% when treated with DES. ISR consists of artery 5 narrowing within the stented segment due to neointimal hyperplastia and over-proliferation of vascular smooth 6 muscle cells (SMCs) [4–6]. Despite the decrease in the ISR rate, DES, delays the formation of healthy endothelium 7 due to the delivery of antiproliferative drugs and suffers from late ST increasing the patients time anti-platelet therapy 8 [7]. The native and healthy endothelium is an active organ that maintains vessel integrity and modulates vascular 9 tone, consisting of a monolayer of endothelial cells, thereby reducing the potential for thrombosis and restenosis. 10 Several studies have demonstrated that stent surface endothelialization is a well-known methodology to inhibit the 11 restenosis and thrombosis [7–9]. 12 Control of cell-material interactions, and thus cell behaviour, may first be achieved by preventing nonspecific protein 13 adsorption and undesirable cell adhesion and, second, by exposing specific cell ligands or bioactive molecules to 14 optimize the adhesion, migration and/or proliferation of desired cells. Biofunctionalization with cell adhesive 15 molecules onto metallic surfaces is a well-established process to control and guide cellular response [10,11]. 16 Different biomolecules are used such as the immobilization of extracellular matrix (ECM) proteins, where the 17 maintenance of the native form enhances their biological function but they present immunological problems, they are 18 difficult to purify and to control their functionalization [6,12]. Another strategy is the use of short peptides, which are 19 non-immunogenic and easy to control their surface immobilization, but, they cannot carry on some functionalities 20 that natural proteins can [13,14]. The use of recombinant proteins such as elastin like-elastin recombinamers (ELR) 21 can avoid the mentioned problems and highlight the indicated advantages. ELR are oligomeric macromolecules based 22 on the repetition of the (VPGXG) motif from elastin, in which X is any amino acid except L-proline [15]. The 23 composition is strictly defined by engineering design and enable the introduction of peptide sequences to extend their 24 properties, they are produced as recombinant proteins mimicking the basic properties of elastin and exhibiting mono-25 dispersity and a high control over amino acid sequence [16,17]. The recombinant nature of ELRs allows to include 26 bioactive domains such as endothelial cell attachment sequence arginine–(glutamic acid)– (aspartic acid)–valine 27 (REDV) [7,16], which mediates endothelial cell adhesion and spreading on fibronectin via its α4β1 receptor [18,19] 28 over smooth muscle cells and platelets [20]. 29 CoCr alloy is a biocompatible material widely used as in coronary stents due to its non-toxicity, elasticity, plasticity, 30 corrosion resistance addition to maintaining the radiopacity and radial strength [21,22]. However, these materials are 31 bioinert, thus leading in some cases to long endothelialization processes that can be overcome with biochemical 32 surface modification through the immobilization of an ELR with an REDV sequence [7,10,11] onto metallic stents 33 surface. 34 Immobilization of cell adhesive motifs onto metallic surfaces can be enhanced by the surface activation through 35 physicochemical surface modification to promote a physical adsorption and/or covalent bonding. Surface properties 36 such as surface hydrophilicity/hydrophobicity, roughness, texture, chemical composition, electrical charge and 37 morphology play an important role on surface functionalization and then, on cell response [23]. 38 The aim of the present work was to obtain a new family of biofunctionalized CoCr alloy surfaces with REDV elastin-39 like recombinamers using two different surface activation treatments (plasma and NaOH etching) and two anchoring 40 mechanisms (physisorption and covalent immobilization), and evaluate the immobilized ELR and the in vitro 41 HUVEC cell adhesion response. 42 43 44 4 1 2. Materials and Methods 2 2.1 Materials 3 2.1.1 Metallic surfaces 4 CoCr alloy (Co-20Cr-14.6W-10.8Ni-2.5Fe-1.5Mn, ASTM F90) (Technalloy Company) discs of 8,5 mm diameter 5 and 2 mm thick were abraded subsequently with 240, 400, 600, 800 and 1200 grit silicon carbide abrasive paper and 6 finally polished with a water suspension of 1 µm and 0.05 µm alumina powder. Prior to the surface treatments, all 7 samples were ultrasonically cleaned with ethanol, distilled water and acetone for 5 min each. 8 2.1.2 Elastin-like recombinamers (ELRs) 9 Elastin-like recombinamers (ELRs) were provided and synthesized by the BIOFORGE group at the University of 10 Valladolid, Spain. The elastin-like recombinamers are governed by (VPGXG) n module in which X is any amino acid 11 except L-proline and that include other amino-acidic sequences following already optimized protocols [15–17]. ELR 12 with an REDV sequence, Arg-Glu-Asp-Val, for endothelial cell adhesion was designed with the following sequence 13 [17]: 14 REDV: ((VPGIG)2(VPGKG)(VPGIG)2EEQIGHIPREDVDYHLYP(VPGIG)2(VPGKG)(VPGIG)2(VGVAPG)3 )10 15 2.1.3 Cells 16 Human umbilical vein endothelial cells, HUVEC´s (Lonza Group Ldt, Basel, Switzerland,) were grown in endothelial 17 cell basal medium (EBM®) medium, with 5% FBS, 0.1% GA-100, 0.1% rhEGF (growth factor), 0.4% BBE and 18 0.1% Hydrocortisone (Lonza, Cologne, Germany) at 37°C in a 5% CO2/ 95% air atmosphere and at 100% humidity. 19 The culture medium was changed every 2 days. For the experiments, cell culture flasks Nunc, (Thermo Scientific, 20 Roskilde, Denmark) were pre-coated with 1µg/ml fibronectin solution in PBS 1X, FN, and cells were harvested at 21 70–90% confluence by trypsin/EDTA (Sigma-Aldrich, Missouri, United States), centrifuged and re-suspended in a 22 serum-free medium before being plated at 2 x 104 HUVEC cells per sample. 23 HUVEC cell passage between 4 and 8 was used for all the experiments [24,25]. 24 25 2.2 Surface functionalization 26 Bioactivity of the polished CoCr surfaces (CT) was achieved by means of ELRs covalent functionalization through 27 the following steps: (1) surface activation, (2) silanization and (3) immobilization of ELRs. First, the surface 28 activation treatments applied to the samples were as follows: 29 PL: Oxygen plasma surface treatment with a Plasma Cleaner (Sterilizer PDC-002, Harrick Scientific Corporation, 30 United States) for 5 min at high power setting. 31 NA: Basic etching with 5 M NaOH solution during 2 h at RT. Next, samples were cleaned twice in distilled water 32 during 30 min. 33 Then, as a second step, each of the previous series were silanized immediately by immersing the substrate in a 34 solution of 10 ml of anhydrous toluene, 1 ml (0.05 M) of N,N - diisopropylethylamine (DIEA) and 2 ml (0.5 M) of 3-35 chloropropyltriethoxysilane (CPTES) (Sigma-Aldrich, Missouri, United States) per disk under nitrogen atmosphere 36 for 1 h at 90 °C under stirring. The nomenclature used throughout the text for control, plasma and sodium hydroxide 37 treated surfaces silanized with CPTES was CT-CP, PL-CP and NA-CP, respectively. After reaction, the discs were 38 ultrasonically rinsed with cyclohexane, isopropanol, distilled water, and acetone, for 15 min each and were finally 39 dried with nitrogen. The CPTES-modified substrates were stored under vacuum in argon atmosphere. 40 Finally, ELR was immobilised on the CoCr surface by two different methods: (1) physical adsorption on the control, 41 plasma and sodium hydroxide treated surfaces (the samples were coded as CT-REDV, PL-REDV, NA-REDV); and 42 (2) covalent immobilisation through a CPTES silanization process of the previously control, plasma and sodium 43 hydroxide treated surfaces (the samples were coded CT-CP-REDV, PL-CP-REDV, NA-CP-REDV). Activated and 44 silanized samples were incubated overnight at room temperature and at a biopolymer concentration of 500 µg/ml of 45 5 dissolved elastin-like recombinamers with an REDV sequence in ultrapure Milli-Q water and the pH adjusted to 13.0 1 with Na2CO3 O/N at RT to ensure that all the amines were deprotonated to facilitate nucleophilic attack. Afterwards, 2 the solution was removed and samples thoroughly washed with water and dried in a stream of nitrogen and 3 immediately analyzed as described below. 4 In summary, the following groups of surfaces were studied: a) CoCr surfaces (CT, PL, NA); b) CPTES grafted 5 surfaces (CT-CP, PL-CP, NA-CP); c) elastin-like recombinamer physisorbed surfaces (CT-REDV, PL-REDV, NA-6 REDV) and; d) elastin-like recombinamer silanized surfaces (CT-CP-REDV, PL-CP-REDV, NA-CP-REDV). 7 2.3 Surface characterization 8 2.3.1 Surface roughness 9 Surface roughness measurements were performed with white light interferometry (Optical interferometer 10 VeecoWyko 9300NT, Veeco Instruments, USA). Type of measurement VSI (Vertical Scanning Interferometry). 11 Three samples of each treatment series were analysed and three measurements of roughness were carried out. Data 12 analysis was performed with Wyko Vision 4.10 software (Veeco Instruments). Curvature and tilt were eliminated 13 from every surface analysis with a Gaussian filter. The average roughness (Ra), arithmetic average of the absolute 14 values of the profile height deviations from the mean plane, and the surface index area (SIA), ratio between real and 15 nominal area, were quantified from the topographical images. 16 2.3.2 Wettability and surface free energy 17 The wettability studies were performed using the sessile drop method with a contact angle video based system 18 (Contact Angle System OCA15plus, Dataphysics, Germany) and analysed with the SCA20 software (Dataphysics, 19 Germany). For each measure, 3 µl of distilled water (miliQ) and 3 µl of diiodomethane were used [26]. Contact 20 angles for SFE calculations were measured at room temperature and the drop deposited on the surface after the same 21 cleaning procedures and treatments. 22 For each sample, fifteen drops were analysed. The surface free energies (SFE) of the different treatments were 23 calculated using the Owens and Wendt approach (OW) adaptation of Young´s equation [27,28]: 24 γ γ  γ  (1) 25 γ.1  cosθ 2. γ . γ /  2. γ . γ / (2) 26 where γ is the dispersive part of liquid surface tension, γ  is the dispersive part of the solid SFE, γ  is the polar part 27 of liquid surface tension and γ  is the polar part of the solid SFE. 28 2.3.3 Surface chemical characterization 29 The chemical analysis of the surface, before and after activation, silanization procedures and ELRs attachment, was 30 investigated by X-ray photoelectron spectroscopy (XPS) (SPECS Surface Nano Analysis GmbH, Berlin, Germany), 31 equipped with an Al anode XR50 source operating at 150 W and a Phoibos 150 MCD-9 detector. 32 The elements present on the surface were qualitatively evaluated by low-resolution survey spectra, whereas high-33 resolution of some determined elements (C 1s, N 1s, O 1s, Cr 2p, Co 2p, Si 2s, Cl 2p) were recorded with pass energy 34 of 35 eV at 0,1 eV steps at a pressure below 5x10-9 mbar. The positions of the peaks were referred to the C 1s signal 35 at 284.8 eV. CasaXPS spectrum software (Casa Software Ltd., UK); was used to analyse the different spectra and 36 perform the XPS peak deconvolution of survey and high resolution. Two samples were studied for each surface 37 condition. 38 2.3.4 Surface Charge 39 A streaming potential instrument (Surpass Electrokinetic Analyzer, Anton Paar, Austria) with an adjustable gap cell 40 was used to determine apparent ζ-potential of the activated, silanized and functionalized surfaces. The ‘titration unit’ 41 allows automatically performed series of measurements at a varied-pH solution. A 1 mM KCl solution was used as 42 electrolyte. The pressure ramp was run up to a maximum pressure of 500 mbar. The electrolyte solution was adjusted 43 to a starting pH = 9.0 using 0.1M KOH. The automatic titration was performed down to pH=3.0 adding 0.1 M HCl. 44 6 Through the VisioLab software (Anton Paar, Austria), it was determined the value of the isoelectric point (IEP) and 1 the surface charge at pH 7.4. For each surface condition, three measurements were performed. 2 3 2.4 ELRs biofunctionalized adlayer characterization 4 The quantification and characterization of the attached elastin like recombinamers layer were characterized by atomic 5 force microscopy (AFM), FITC fluorescence quantification, XPS analysis and quartz-crystal microbalance with 6 monitoring dissipation (QCM-D). 7 Topographical changes due to ELR’s adsorption onto the different treated surfaces were analyzed using AFM 8 (Multimode, NanoScope V Controller, Veeco, Digital Instruments, USA) associated with the software WSxM, in 9 tapping mode using silicon cantilevers under ambient conditions. 10 2.4.1 FITC–ELR preparation and adsorption quantification 11 FITC-labelled REDV elastin-like recombinamer solution (FITC-REDV) 1 ml of 1 mg/ml, has been prepared 12 following the Pierce® FITC Labelling Kit (Thermo Fisher Scientific, USA). The final protein concentration was 13 estimated by measuring the absorbance at 280 nm and 494 nm (UV Mini 1240 spectrophotometer, Shimadzu), and 14 the protein was then stored at 4 ⁰C. 15 500 µg/ml FITC-labelled REDV was adsorbed on the different CoCr treated series during overnight at room 16 temperature. Stability tests were performed on physisorbed and silanized surfaces by adsorbing FITC-REDV on the 17 different treated surfaces and then, sonication in PBS 1X during 1 h. The samples were then rinsed three times with 18 PBS 1X. The adsorbed FITC-labelled protein was eluted with 500 µl of 0.2 M NaOH for 2h. The fluorescent intensity 19 of the extracts was measured with a spectrofluorophotometer (Infinite M200 Pro, Tecan, Switzerland). The excitation 20 and emission wavelengths were set at 488 and 530 nm, respectively. Fluorescent measurements of the attached ELR 21 have been performed prior and after sonication. 22 2.4.2 Quartz crystal microbalance with monitoring dissipation (QCM-D) 23 A quartz crystal microbalance consists of a piezoelectric quartz crystal sensor that is excited to oscillation at its 24 fundamental resonant frequency, f. The equipment is used to measure very small masses added on the surface of the 25 sensor because an increase in mass (∆m) bound to the quartz surface causes the crystal oscillation frequency to 26 decrease, obtaining a negative shift of the resonance frequency (-∆f). The Sauerbrey relation concludes that the 27 change in resonance frequency is proportional to the change in the adsorbed mass if the adsorbed layer is much 28 smaller than the mass of the crystal [29]. The Voigt model settles for a viscoelastic or thick layer for which ∆f is not 29 directly proportional to ∆m, i.e. the effectively coupled mass depends on how the oscillatory motion of the crystal 30 propagates into and through the viscoelastic adlayer [30]. In addition to that, most surface-adsorbed protein layers are 31 hydrated, so they are not only highly viscous and cause significant energy dissipation, but also add mass to the 32 adsorbed protein layer. In those cases the dissipation factor, D, simultaneously calculated with f when using the QCM 33 must also be taken into consideration.. The dissipation factor is inversely proportional to the Q-factor of the oscillator 34 [30], which is a nondimensional parameter that compares the time constant for decay of an oscillating physical 35 system's amplitude to its oscillation period as defined by: 36 Equation 1 stored dissipated E2 E Q 1 D⋅π⋅ == 37 where Edissipated is the energy dissipated during one period of oscillation, and Estored is the energy stored in the 38 oscillating system. 39 Co-20Cr-15W-10Ni-1.5Mn (QSX999) sensors were purchased at Q-Sense (Sweden). The fundamental mode of the 40 sensors was at 4.95 MHz. Prior to use, the sensors were cleaned as follows: (1) 10 min sonication with ethanol (96 %, 41 Panreac); (2) 10 min sonication with acetone (99.5 %, Panreac); (3) 10 min sonication with MilliQ ultrapure water; 42 and (4) 10 min UV/ ozone chamber (BioForce Nanosciences, Ames, USA). The QCM-D (D300, Q-Sense, Sweden) 43 13 efficient alternative to enhance rapid endothelialization. Herein, we have successfully immobilised REDV on the 1 metallic surfaces through physisorption or covalent bonding by using traditional organosilane chemistry. The 2 successful biomolecule adlayer was thoroughly quantified and characterized. Previously to functionalization, metallic 3 surfaces were effectively activated to increase the amount of hydroxyls and then, enhancing silanization and, finally, 4 improving ELR immobilization. Covalent bonding coatings of the ELR have shown higher amount and stability than 5 the physisorbed ELR coatings. The results demonstrate that the silanization process was not completely effective 6 since a mixture of covalent and physisorption behaviour was observed, the use of big biomolecules with different 7 anchor groups causes covalent and weak bonding between the biomolecule and the surface. Both immobilization 8 process and surface electrostatic forces influence the amount of immobilized ELR onto the surface. Most importantly, 9 early HUVEC cell adhesion response was directly related to the amount of immobilized ELR on the surfaces. Thus, 10 coating CoCr surfaces with REDV is a promising strategy to enhance rapid endothelialization and improve the long-11 term efficacy of cardiovascular stents. 12 13 Acknowledgments 14 Authors acknowledge the Spanish Government for financial support through project MAT 2012-30706, co-funded by 15 the EU through European Regional Development Funds, and the Agency for Administration of University and 16 Research Grants of the Government of Catalonia (2014 SGR 1333). We acknowledge financial support from the EU 17 through the European regional development fund (ERDF), from the MINECO (MAT2013-41723-R y MAT2013-18 42473-R, PRI-PIBAR- 2011-1403, and MAT2012-38043), the JCyL (projects VA049A11, VA152A12, and 19 VA155A12), the CIBER-BBN, the JCyL, and the Instituto de Salud Carlos III under the Network Center of 20 Regenerative Medicine and Cellular Therapy of Castilla and Leon. M.I.C. would like to thank the Generalitat de 21 Catalunya for funding through a FI Scholarship. The authors acknowledge Montse Dominguez and Romain Schieber 22 for their useful technical assistance regarding the XPS and AFM analysis. 23 24 25 14 References 1 [1] J.C. Palmaz, Intravascular stents in the last and the next 10 years, J Endovasc Ther 11 Suppl (2004) 200–2 206. 3 [2] A. Tan, Y. Farhatnia, A. de Mel, J. Rajadas, M.S. Alavijeh, A.M. Seifalian, Inception to actualization: next 4 generation coronary stent coatings incorporating nanotechnology, J. Biotechnol. 164 (2013) 151–70. 5 [3] R. Busch, A. Strohbach, S. Rethfeldt, S. Walz, M. Busch, S. Petersen, S. Felix, K. Stemberg, New stent 6 surface materials: the impact of polymer-dependent interactions of human endothelial cells, smooth muscle 7 cells, and platelets, Acta Biomater. 10 (2014) 688–700. 8 [4] P. Wenaweser, C. Rey, F.R. Eberli, M. Togni, D. Tüller, S. Locher, A. Remondino, C. Seiler, O.M. Hess, B. 9 Meier, S. Windecker, Stent thrombosis following bare-metal stent implantation: success of emergency 10 percutaneous coronary intervention and predictors of adverse outcome, Eur. Heart. J. 26 (2005) 1180–7. 11 [5] T. Simard, B. Hibbert, F.D. Ramirez, M. Froeschl, Y.-X. Chen, E.R. O’Brien, The evolution of coronary 12 stents: a brief review, Can. J. Cardiol. 30 (2014) 35–45. 13 [6] F. Nazneen, G. Herzog, D.W. Arrigan, N. Caplice, P. Benvenuto, P. Galvin, M. Thompson, Surface 14 chemical and physical modification in stent technology for the treatment of coronary artery disease, J. 15 Biomed. Mater. Res. B Appl. Biomater. 100 (2012) 1989–2014. 16 [7] Y. Wei, Y. Ji, L.-L. Xiao, Q. Lin, J. Xu, K. Ren, J. Ji, Surface engineering of cardiovascular stent with 17 endothelial cell selectivity for in vivo re-endothelialisation, Biomaterials 34 (2013) 2588–99. 18 [8] T. Inoue, K. Croce, T. Morooka, M. Sakuma, K. Node, D.I. Simon, Vascular inflammation and repair 19 implications for re-endothelialization, restenosis, and stent thrombosis, JACC Cardiovasc. Interv. 4 (2011) 20 1057–66. 21 [9] L.G. Melo, M. Gnecchi, A.S. Pachori, D. Kong, K. Wang, X. Liu, R.E. Pratt, V.J. Dzau, Endothelium-22 targeted gene and cell-based therapies for cardiovascular disease, Arterioscler. Thromb. Vasc. Biol. 24 23 (2004) 1761–74. 24 [10] A. de Mel, G. Jell, M. Stevens, A. Seifalian, Biofunctionalization of biomaterials for accelerated in situ 25 endothelialization: a review, Biomacromolecules 9 (2008) 2969–79. 26 [11] K. Zhang, T. Liu, J. Li, J. Chen, Surface modification of implanted cardiovascular metal stents: From 27 antithrombosis and antirestenosis to endothelialization, J. Biomed. Mater. Res. A 102 (2014) 588–609. 28 [12] H. Chen, L. Yuan, W. Song, Z. Wu, D. Li, Biocompatible polymer materials: Role of protein–surface 29 interactions, Prog. Polym. Sci. 33 (2008) 1059–87. 30 [13] M.H. Fittkau, P. Zilla, D. Bezuidenhout, M.P. Lutolf, P. Human, J.A. Hubbell, N. Davies, The selective 31 modulation of endothelial cell mobility on RGD peptide containing surfaces by YIGSR peptides, 32 Biomaterials 26 (2005) 167–74. 33 [14] D.F. Williams, The role of short synthetic adhesion peptides in regenerative medicine; the debate, 34 Biomaterials 32 (2011) 4195–7. 35 [15] A. Girotti, A. Fernández‐Colino. Elastin‐like recombinamers: Biosynthetic strategies and biotechnological 36 applications, Biotechnol. J. 6 (2011) 1174–86. 37 [16] R.R. Costa, C.A. Custódio, A.M. Testera, F.J. Arias, J.C. Rodríguez-Cabello, N.M. Alves, J.F. Mano, 38 Stimuli-responsive thin Coatings Using Elastin-Like Polymers for Biomedical Applications, Adv Funct 39 Mater 2009;19:3210–8. 40 [17] J.C. Rodríguez-Cabello, L. Martín, Emerging applications of multifunctional elastin-like recombinamers, 41 Nanomedicine 6 (2011) 111–22. 42 [18] E. Monchaux, P. Vermette, Bioactive microarrays immobilized on low-fouling surfaces to study specific 43 endothelial cell adhesion, Biomacromolecules 8 (2007) 3668–73. 44 15 [19] S.P. Massia, J.A. Hubbell, Vascular endothelial cell adhesion and spreading promoted by the peptide REDV 1 of the IIICS region of plasma fibronectin is mediated by integrin alpha 4 beta 1, J. Biol. Chem. 267 (1992) 2 14019–26. 3 [20] H. Ceylan, A.B. Tekinay, M.O. Guler, Selective adhesion and growth of vascular endothelial cells on 4 bioactive peptide nanofiber functionalized stainless steel surface, Biomaterials 32 (2011) 8797–805. 5 [21] D. Kereiakes, Usefulness of a cobalt chromium coronary stent alloy, Am. J. Cardiol. 92 (2003) 463–6. 6 [22] T. Hanawa, An overview of biofunctionalization of metals in Japan, J. R. Soc. Interface. 6 Suppl 3 (2009) 7 S361–9. 8 [23] Y. Oshida, A. Hashem, T. Nishihara, M.V. Yapchulay, Fractal dimension analysis of mandibular bones: 9 toward a morphological compatibility of implants, Biomed. Mater. Eng. 4 (1994) 397–407. 10 [24] B.C. Heng, P.P. Bezerra, Q.R. Meng, D.W. Chin, L.B. Koh, H. Li, H. Zhang, P.R. Preiser, F.Y. Boey, S.S. 11 Venkatraman, Adhesion, proliferation, and gene expression profile of human umbilical vein endothelial cells 12 cultured on bilayered polyelectrolyte coatings composed of glycosaminoglycans, Biointerphases 5 (2010) 13 53–62. 14 [25] A. Andukuri, W.P. Minor, M. Kushwaha, J.M. Anderson, H.-W. Jun, Effect of endothelium mimicking self-15 assembled nanomatrices on cell adhesion and spreading of human endothelial cells and smooth muscle cells, 16 Nanomedicine 6 (2010) 289–97. 17 [26] S.J. Marshall, S.C. Bayne, R. Baier, A.P. Tomsia, G.W. Marshall, A review of adhesion science, Dent. 18 Mater. 26 (2010) e11–6. 19 [27] A.W. Neumann, R.J. Good, C.J. Hope, M. Sejpal, An equation-of-state approach to determine surface 20 tensions of low-energy solids from contact angles, J. Colloid. Interface Sci. 49 (1974) 291–304. 21 [28] A. Rudawska, E. Jacniacka, Analysis for determining surface free energy uncertainty by the Owen–Wendt 22 method, Int. J. Adhes. Adhes. 29 (2009) 451–7. 23 [29] A.G. Hemmersam, M. Foss, J. Chevallier, F. Besenbacher, Adsorption of fibrinogen on tantalum oxide, 24 titanium oxide and gold studied by the QCM-D technique. Colloids Surf. B Biointerfaces 43 (2005) 208-25 215. 26 [30] F. Höök, B. Kasemo, T. Nylander, C. Fant, K. Sott, H. Elwing, Variations in coupled water, viscoelastic 27 properties, and film thickness of a Mefp-1 protein film during adsorption and cross-linking: a quartz crystal 28 microbalance with dissipation monitoring, ellipsometry, and surface plasmon resonance study, Anal. Chem. 29 73 (2001) 5796–804. 30 [31] M.C. Biesinger, B.P. Payne, A.P. Grosvenor, L.W.M. Lau, A.R. Gerson, R.S.C. Smart, Resolving surface 31 chemical states in XPS analysis of first row transition metals, oxides and hydroxides: Cr, Mn, Fe, Co and Ni, 32 Appl. Surf. Sci. 257 (2011) 2717–30. 33 [32] B.V. Crist, A Review of XPS Data-Banks 1 (2007) 1–52. 34 [33] S. Surviliene, The use of XPS for study of the surface layers of Cr–Co alloy electrodeposited from Cr(III) 35 formate–urea baths, Solid State Ionics 179 (2008) 222–7. 36 [34] G. Mani, M. Feldman, S. Oh, Surface modification of cobalt-chromium-tungsten-nickel alloy using 37 octadecyltrichlorosilanes, Appl. Surf. Sci. 255 (2009) 5961–70. 38 [35] T. Hanawa, S. Hiromoto, K. Asami, Characterization of the surface oxide of a Co ± Cr ± Mo alloy after 39 being located in quasi-biological environments using XPS, Appl. Surf. Sci. 183 (2001) 68–75. 40 [36] I. Milos, D. Du, P. Panjan, Chromium Nitride by XPS. Surf. Sci. 5 (1998) 138–44. 41 [37] I. Milošev, The effect of biomolecules on the behaviour of CoCrMo alloy in various simulated physiological 42 solutions, Electrochim. Acta 78 (2012) 259–73. 43 [38] S. Liu, D.M. Rose, J. Han, M.H. Ginsberg, Alpha4 integrins in cardiovascular development and diseases, 44 Trends Cardiovasc. Med. 10 (2000) 253–7. 45 16 [39] E. Salvagni, G. Berguig, E. Engel, J.C. Rodriguez-Cabello, G. Coullerez, M. Textor, J.A. Planell, F.J. Gil, C. 1 Aparicio, A bioactive elastin-like recombinamer reduces unspecific protein adsorption and enhances cell 2 response on titanium surfaces, Colloids Surf. B Biointerfaces 114 (2014) 225–33. 3 [40] Y.Noda, S. Noro, T. Akutagawa, T. Nakamura, Gold nanoparticle assemblies stabilized by 4 bis(phthalocyaninato)lanthanide(III) complexes through van der Waals interactions. Scientific Reports 4 5 (2014) 3758. 6 [41] Y. Chen, X. Zheng, H. Ji, C. Ding, Effect of Ti–OH formation on bioactivity of vacuum plasma sprayed 7 titanium coating after chemical treatment, Surf. Coatings Technol. 202 (2007) 494–8. 8 [42] H. Tamura, A. Tanaka, K. Mita, R. Furuichi, Surface Hydroxyl Site Densities on Metal Oxides as a Measure 9 for the Ion-Exchange Capacity, J. Colloid. Interface. Sci. 209 (1999) 225–31. 10 [43] X. Chen, P. Sevilla, C. Aparicio, Surface biofunctionalization by covalent co-immobilization of 11 oligopeptides, Colloids Surf. B Biointerfaces 107 (2013) 189–97. 12 [44] T. Hanawa, A comprehensive review of techniques for biofunctionalization of titanium, J. Periodontal 13 Implant. Sci. 41 (2011) 263–72. 14 [45] V. Paredes, E. Salvagni, E. Rodriguez, Assessment and comparison of surface chemical composition and 15 oxide layer modification upon two different activation methods on a CoCrMo alloy, J. Mater. Sci. Mater. 16 Med. 43 (2013) 1–10. 17 [46] X. Liu, P. Chu, C. Ding, Surface modification of titanium, titanium alloys, and related materials for 18 biomedical applications, Mater. Sci. Eng. R. Reports 47 (2004) 49–121. 19 [47] C. Aparicio, J.M. Manero, F. Conde, M. Pegueroles, J.A. Planell, M Vallet-Regí, F.J. Gil, Acceleration of 20 apatite nucleation on microrough bioactive titanium for bone-replacing implants, J. Biomed. Mater. Res. Part 21 A 82 (2007) 521–9. 22 [48] S.L. Walker, S. Bhattacharjee, E.M. V. Hoek., M. Elimelech, A novel asymmetric clamping cell for 23 measuring streaming potential of flat surfaces, Langmuir 18 (2002) 2193–8. 24 [49] G.A. Parks, The isoelectric points of solid oxides, solid hydroxides, and aqueous hydroxo complex systems, 25 Chem. Rev. 65 (1965) 177-198. 26 [50] L. Kozlowski, Calculation of protein isoelectric point (2012) Retrieved from http://isoelectric.ovh.org/. 27 [51] T. Hanawa, An overview of biofunctionalization of metals in Japan, J. R. Soc. Interface 6 Suppl. 3 (2009) 28 S361–9. 29 [52] M. Godoy-Gallardo, C. Mas-Moruno, M.C. Fernández-Calderón, C. Pérez-Giraldo, J.M. Manero, F. 30 Albericio, F.J. Gil, D. Rodríguez, Covalent immobilization of hLf1-11 peptide on a titanium surface reduces 31 bacterial adhesion and biofilm formation, Acta Biomater. 10 (2014) 3522-34. 32 [53] M. González, E. Salvagni, J.C. Rodríguez-Cabello, E. Rupérez, F.J. Gil, J. Peña, J.M. Manero, A low elastic 33 modulus Ti-Nb-Hf alloy bioactivated with an elastin-like protein-based polymer enhances osteoblast cell 34 adhesion and spreading, J. Biomed. Mater. Res. A 101 (2013) 819–26. 35 [54] M. Pegueroles, C. Aparicio, M. Bosio, E. Engel, F.J. Gil, J.A. Planell, G. Altankov, Spatial organization of 36 osteoblast fibronectin matrix on titanium surfaces: effects of roughness, chemical heterogeneity and surface 37 energy, Acta Biomater. 6 (2010) 291–301. 38 [55] C.N. Elias, Y. Oshida, J.H.C. Lima, C.A. Muller, Relationship between surface properties (roughness, 39 wettability and morphology) of titanium and dental implant removal torque, J. Mech. Behav. Biomed. 40 Mater. 1 (2008) 234–42. 41 [56] A. Rezania, R. Johnson, A.R. Lefkow, K.E. Healy, Bioactivation of Metal Oxide Surfaces. 1. Surface 42 Characterization and Cell Response, Langmuir 15 (1999) 6931–9. 43 17 [57] F. Höök, J. Vörös, M. Rodahl, R. Kurrat, A comparative study of protein adsorption on titanium oxide 1 surfaces using in situ ellipsometry, optical waveguide lightmode spectroscopy, and quartz crystal 2 microbalance/dissipation, Colloids Surfaces B 24 (2002) 155–70. 3 [58] Q. Lin, X. Ding, F. Qiu, X. Song, G. Fu, J. Ji, In situ endothelialization of intravascular stents coated with an 4 anti-CD34 antibody functionalized heparin-collagen multilayer, Biomaterials 31 (2010) 4017–25. 5 [59] D.C. Hansen, Biological Interactions at metal surfaces, JOM 63 (2011) 22-23. 6 [60] J. Schneider, L.C. Ciacchi, A Classical Potential to Model the Adsorption of Biological Molecules on 7 Oxidized Titanium Surfaces, J. Chem. Theory Comput. 7 (2011) 473–84. 8 [61] B.G. Keselowsky, D.M. Collard, A.J. García, Surface chemistry modulates focal adhesion composition and 9 signaling through changes in integrin binding, Biomaterials 25 (2004) 5947–54. 10 [62] E. Potthoff, D. Franco, V. D’Alessandro, C. Starck, V. Falk, T. Zambelli, J.A. Vorholt, D. Poulikakos, A. 11 Ferrari, Toward a rational design of surface textures promoting endothelialization, Nano. Lett. 14(2014) 12 1069–79. 13 [63] R. Barbucci, D. Pasqui, A. Wirsen, S. Affrossman, A. Curtis, C. Tetta, Micro and nano-structured surfaces, 14 J. Mater. Sci. Mater. Med. 14 (2003) 721–5. 15 [64] S.J. Liliensiek, J.A. Wood, J. Yong, R. Auerbach, P.F. Nealey, C.J. Murphy, Modulation of human vascular 16 endothelial cell behaviors by nanotopographic cues, Biomaterials 31 (2010) 5418–26. 17 [65] M. Pegueroles, F.J. Gil, J.A. Planell, C. Aparicio, The influence of blasting and sterilization on static and 18 time-related wettability and surface-energy properties of titanium surfaces, Surf. Coatings Technol. 202 19 (2008) 3470–9. 20 [66] L. Ponsonnet, K. Reybier, N. Jaffrezic, V. Comte, C. Lagneau, M. Lissac, C. Martelet, Relationship between 21 surface properties (roughness, wettability) of titanium and titanium alloys and cell behaviour, Mater Sci. 22 Eng. C 23 (2003) 551–60. 23 [67] K. Cai, M. Frant, J. Bossert, G. Hildebrand, K. Liefeith, K.D. Jandt, Surface functionalized titanium thin 24 films: zeta-potential, protein adsorption and cell proliferation, Colloids Surf. B Biointerfaces 50 (2006) 1–8. 25 [68] E.D. Kaufman, J. Belyea, M.C. Johnson, Z.M. Nicholson, J.L. Ricks, P.K. Shah, M. Bayless, T. Pettersson, 26 Z. Feldoto, E. Blomberg, P. Claesson, S. Franzen, Probing protein adsorption onto mercaptoundecanoic acid 27 stabilized gold nanoparticles and surfaces by quartz crystal microbalance and -potential measurements, 28 Langmuir 23 (2007) 6053–62. 29 30 31 18 Figures Legends 1 2 Fig. 1. Wettability studies of activated and silanized CoCr surfaces: a) water contact angle. The * symbol indicates 3 CA mean-values with non-statistically-significant differences respect to CT; b) surface free energy (SFE) and their 4 different components (dispersive and polar). The #, *, & symbols join SFE and dispersive mean-values with non-5 statisticallysignificant differences. CT: polished CoCr. PL: polished CoCr treated with oxygen plasma. NA: 6 polished CoCr, etched with NaOH. CT-CP: CT followed by CPTES silanization. PL-CP: PL followed by CPTES 7 silanization. NA-CP: NA followed by CPTES silanization 8 9 Fig. 2. XPS high resolution spectra of C 1s (a) and O 1s (b) obtained at the modified CoCr surfaces after each 10 reaction step. Polished CoCr samples (CT) were used as control. CT: polished CoCr. PL: polished CoCr treated with 11 oxygen plasma. NA: polished CoCr, etched with NaOH. CT-REDV: CT with elastin-like recombinamer (ELR) 12 (physisorbed). PL-REDV: PL with ELR (physisorbed). NA-REDV: NA with ELR (physisorbed). CT-CP-REDV: CT 13 followed by CPTES silanization with ELR (covalent immobilization). PL-CP-REDV: PL followed by CPTES 14 silanization with ELR (covalent immobilization. NA-CP-REDV: NA followed by CPTES silanization with ELR 15 (covalent immobilization). 16 17 Fig. 3. AFM images and roughness parameters of ELR attachment on CoCr treated surfaces. Bar: 200 nm (for 18 acronyms definition, see captions Fig.1 and Fig.2). 19 20 Fig. 4. ∆D versus ∆f plot and adlayer parameters for the adsorption of RGD elastin-like polymer (500 µg/ml) on 21 CoCr alloy coated sensors obtained by QCM-D. Calculations were performed after 4 h of adsorption time using the 22 Voigt model. REDV: CoCr QCM-D sensor with ELR (physisorption). CP-REDV: CoCr QCM-D sensor followed by 23 CPTES silanization with ELR (covalent immobilization). 24 25 Fig. 5. FITC-REDV stability test results on different treated CoCr surfaces before and after 1h of ultrasonic 26 solicitations in PBS 1X at RT. Fluorescent measurement were performed after FITC ELR desorption with NaOH 0,2 27 M during 2h. The ¨, #, *, symbols join fluorescent intensities with non-statistically-significant differences (for 28 acronyms definition, see captions Fig.1 and Fig.2). 29 30 Fig. 6. a) Fluorescent images of the HUVEC cells cultured for 4 h on CT, CT-REDV, PL-CP-REDV and NA-REDV 31 surfaces in serum-free medium. Bars: 100 µm; b) quantification of the cell number, total area occupied by cells, 32 aspect ratio and maximum diameter for the HUVEC cultured for 4 h on treated CoCr samples. Each area was 33 analysed by FIJI ImageJ software was 869.7 µm × 689.07 µm (for acronyms definition, see captions Fig.1 and Fig.2). 34 35 36 1 Table 1. XPS characterisation percentage of atomic composition at the different modified CoCr surfaces (for acronyms definition, see captions Fig.1 and Fig.2). Surfaces C 1s O 1s N 1s Co 2p Cr 2p Ni 2p W 4d Cl 2p Si 2s CT 39.1 ± 2.0 37.7 ± 1.5 0.9 ± 0.3 9.0 ± 1.0 11.1 ± 0.1 1.0 ± 0.3 1.0 ± 0.0 0.0 ± 0.0 0.0 ± 0.0 PL 20.3 ± 0.2 54.3 ± 1.9 0.4 ± 0.1 15.2 ± 1.1 6.3 ± 1.0 2.5 ± 0.4 0.9 ± 0.1 0.0 ± 0.0 0.0 ± 0.0 NA 37.3 ± 5.8 42.4 ± 2.5 4.5 ± 0.1 6.7 ± 1.0 7.0 ± 0.5 0.8 ± 0.2 1.0 ± 0.7 0.0 ± 0.0 0.0 ± 0.0 CT-CP 31.3 ± 2.0 47.6 ± 0.8 0.5 ± 0.1 9.4 ± 1.0 7.7 ± 1.1 1.5 ± 0.5 0.7 ± 0.1 0.4 ± 0.1 0.9 ± 0.1 PL-CP 31.4 ± 3.1 44.6 ± 2.6 2.4 ± 1.3 9.0 ± 0.8 8.5 ± 1.1 1.7 ± 1.0 1.1 ± 0.4 0.4 ± 0.5 0.7 ± 0.5 NA-CP 28.0 ± 0.9 51.3 ± 2.6 0.3 ± 0.2 10.8 ± 1.0 5.3 ± 0.5 2.3 ± 0.6 0.9 ± 0.3 0.2 ± 0.2 0.8 ± 0.2 CT-REDV 52.0 ± 1.0 29.4 ± 1.5 8.6 ± 0.5 3.5 ± 0.3 4.9 ± 0.8 0.7 ± 0.0 0.8 ± 0.2 0.0 ± 0.0 0.0 ± 0.0 PL-REDV 55.8 ± 6.0 26.4 ± 4.1 12.4 ± 0.6 2.4 ± 1.3 2.1 ± 0.8 0.6 ± 0.2 0.4 ± 0.1 0.0 ± 0.0 0.0 ± 0.0 NA-REDV 50.1 ± 1.6 30.6 ± 0.7 9.0 ± 1.2 3.3 ± 0.2 5.3 ± 0.2 0.9 ± 0.1 0.7 ± 0.2 0.0 ± 0.0 0.0 ± 0.0 CT-CP-REDV 53.5 ± 2.6 27.6 ± 3.0 11.4 ± 1.0 2.2 ± 0.8 3.2 ± 0.6 0.4 ± 0.1 0.7 ± 0.1 0.2 ± 0.2 0.4 ± 0.1 PL-CP-REDV 52.1 ± 1.8 24.8 ± 1.1 11.7 ± 1.3 1.6 ± 0.4 2.4 ± 0.5 0.2 ± 0.0 0.5 ± 0.0 0.0 ± 0.0 0.6 ± 0.1 NA-CP-REDV 52.1 ± 1.8 30.3 ± 0.9 10.4 ± 0.4 2.0 ± 0.4 4.0 ± 0.3 0.2 ± 0.0 0.4 ± 0.0 0.1 ± 0.1 0.5 ± 0.4 Table 1 1 Table 2. Isoelectric point (IEP) and apparent zeta-potential (), at pH 7.4, of modified CoCr surfaces (for acronyms definition, see captions Fig.1 and Fig.2). Surfaces IEP  at pH = 7,4 (mV) CT 3.5 ± 0.01 -26.4 ± 0.70 PL 3.8 ± 0.01 -27.1 ± 2.47 NA 4.1± 0.02 -31.1 ± 2.31 CT-CP 3.8 ± 0.01 -30.5 ± 4.38 PL-CP 3.7 ± 0.01 -38.4 ± 4.78 NA-CP 4.6 ± 0.01 -34.9 ± 3.61 CT-REDV 3.9 ± 0.00 -25.3 ± 2.63 PL-REDV 5.0 ± 0.04 -31.1 ± 0.54 NA-REDV 4.6 ± 0.04 -29.1 ± 4.19 CT-CP-REDV 4.7 ± 0.05 -24.7 ± 1.57 PL-CP-REDV 3.8 ± 0.00 -35.5 ± 5.35 NA-CP-REDV 4.5 ± 0.02 -26.7 ± 0.83 Table 2 Fig. 1 b) Intensity (a.u.) a) Intensity (a.u.) Fig.2