Full text
1 The importance of surface adsorbates in solution-processed thermoelectric materials: the case of SnSe Yu Liu,# Mariano Calcabrini # Yuan Yu, Aziz Genç, Cheng Chang, Tommaso Costanzo, Tobias Kleinhanns, Seungho Lee, Jordi Llorca, Oana Cojocaru-Mirédin, Maria Ibáñez* Dr. Y. Liu, M. Calcabrini, Dr. C. Chang, Dr. T. Constanzo, T. Kleinhanns, S. Lee, Prof. Maria Ibáñez IST Austria, Am Campus 1 3400 Klosterneuburg, Austria. E-mail: [email protected] # These authors contributed equally to this work. Dr. Y. Yu, Prof. O. Cojocaru-Mirédin RWTH Aachen, I. Physikalisches Institut (IA), Sommerfeldstraße 14 52074 Aachen, Germany. Prof. A. Genç Department of Materials Science and Engineering, Faculty of Engineering, Izmir Institute of Technology İzmir 35430, Turkey Prof. J. Lorca Institute of Energy Technologies, Department of Chemical Engineering and Barcelona Research Center in Multiscale Science and Engineering, Universitat Politècnica de Catalunya 08019 Barcelona, Spain. Keywords: SnSe, sodium, solution-processed, grain boundary, energy filtering, liquid-phase sintering, thermoelectrics Abstract: Solution synthesis of nanoparticles (NP) emerged as an alternative to prepare powders for thermoelectric materials with less demanding processing conditions than conventional melting and mechanical alloying. However, when NPs are synthesized in solution, their nucleation and growth occur in the presence of reaction regulating compounds that interact with the NP surface, yielding NPs with specific surface adsorbates. In surfactantassisted colloidal synthesis, surface adsorbates are known and linked to detrimental effects due to their insulating nature. Conversely, in the so-called surfactant-free syntheses, their presence and impact on the final material have been greatly overlooked. Here, we demonstrate that ionic adsorbates are unavoidable in surfactant-free synthesis and play a crucial role in the material microstructure evolution and thermoelectric properties. In particular, we study polycrystalline SnSe produce from NPs synthesized in polar solvents. This work shows that the common use of sodium salts as precursors yields unavoidably significant quantities of sodium in the final material. Based on the fundamentals of colloidal science, we explain that Na is an inevitable impurity as Na ions are electrostatically adsorbed at the NP surface to preserve charge neutrality. In the sintered pellets, Na+ is present within the matrix as dopants, in dislocations,
2 precipitates, and forming grain boundary complexions. The interfaces created between SnSe and Na-rich phases lead to energy filtering effects, enhancing the Seebeck coefficient. These results can be extended to other colloidal syntheses in polar media and highlight the importance of considering all the possible unintentional impurities to establish proper structure-property relationships and control material properties in solution-processed thermoelectric materials. 1. Introduction Thermoelectric devices reversibly convert heat into electricity both for power harvesting and for active cooling and heating. The efficiency of a thermoelectric device is determined by the temperature-dependent properties of the materials that constitute it. These are summarized in the thermoelectric figure of merit of each material, zT = S2 σ κ-1 T, that combines Seebeck coefficient (S), electrical conductivity (σ), thermal conductivity (κ) and absolute temperature (T).[1] The materials used in conventional thermoelectric devices are dense, polycrystalline inorganic semiconductors. Commonly, the processing of such materials has two steps: preparation of the semiconductor in powder form and the consolidation of the powder into a dense sample. The most common route to prepare powders among the thermoelectric community is through melting or mechanical alloying.[2] Alternatively, solution methods to produce micro- and nanoparticle (NP)-based powders with much less demanding conditions (e.g. lower reagent purity, lower temperatures, shorter reaction times) have been explored to reduce the powder production costs.[1,3] Furthermore, solution methods provide opportunities to produce powders with controlled features, such as average crystalline size, shape, composition, and crystal phase, to tune the consolidation process modifying the final material properties.[4,5] The synthesis of NPs in solution also enables an exquisite control over surface properties, such as faceting and surface composition at the atomic level.[6] Lastly, solutionbased methods allow extended device fabrication versatility, including flexible, conformable, and rigid modules with customized geometries.[7,8]
3 To date, solution-based syntheses lead to several bulk materials with state-of-the-art performances, as is the case of PbS,[5] Bi0.5Sb1.5Te3[9], and SnSe,[3] proving the potential of the strategy. Unlike solid-state processed powders, when dealing with NPs synthesized in solution, one should pay special attention to the role of surface species. In a non-vacuum environment, surfaces are usually covered by adsorbates.[10] For solids prepared from solution-processed NPs, the composition, chemical stability, and bonding nature of surface species play a role in the sintering process, and reaction byproducts can determine the final properties of the consolidated material. Surface species are carefully considered in surfactant-assisted colloidal synthesis because of the insulating nature of the generally used long-chain aliphatic surfactants[11] and the consequent detrimental effects on thermoelectric performance.[12] In such cases, the surfactants have to be removed to enhance the electrical conductivity. The most common strategy to do so is thermal decomposition, but this results in the presence of residual carbon in the final solid.[13– 15] Alternatively, surfactants can be exchanged with volatile compounds[16] or even inorganic species[17] that can further tune material properties.[15,18,19] In other synthetic methods, however, surface adsorbates are usually neglected. This is the case for the so-called surfactant-free methods,[3,20–32] the most widely used to produce thermoelectric powders. The vast majority of these reports do not include surface treatments since the NPs are considered "naked".[30,33,34] This is a miss conception as depending on the NP composition and surface termination, different species are adsorbed at the NP surface. Such surface adsorbates need to be identified to understand their role in the thermoelectric properties. Despite this, to the best of our knowledge, no reports have considered the role of adsorbates in surfactant-free solutionprocessed thermoelectric materials. Here, we study the effect of surface adsorbates in polycrystalline SnSe produced from solutionsynthesized NPs. SnSe highest zT obtained so far in p-type SnSe is ~2.6 at 923 K along the b
4 axis in SnSe single crystals;[40] and ~2.8 at 773 K along the out-of-plane direction in Br-doped n-type SnSe single crystal.[41] The superb performance of these materials is linked to the strong anharmonicity of the Sn-Se bonds that translates into ultralow thermal conductivities,[42,43] and to its multiple bands that can be accessed by doping to optimize its electronic properties.[35] However, the high cost, tedious production of single crystals, and their poor mechanical properties limit the large-scale use of SnSe in thermoelectric devices. Therefore, different strategies to produce polycrystalline SnSe with comparable performance are being explored,[44– 48] including solution processing methods.[3,20,49–53,21–23,25–28,32] In this work, we identify the surface species resulting in the aqueous synthesis of SnSe NPs, and demonstrate their effects on the sintering process and the thermoelectric properties. 2. Material synthesis: from SnSe powder to bulk SnSe The table below shows the most common reactants to synthesize SnSe in solution that yield state-of-the-art performances (Table 1). SnSe NPs are usually prepared in polar media (water or ethylene glycol, EG) using SnCl2 and Se, SeO2, or Na2SeO3 as precursors. Additionally, to ensure precursor solubility in the media, redox agents and acids or bases are used, generally, these are Na+ salts, as highlighted in Table 1. In all these reactions, soluble Sn2+ and Se2- species precipitate, forming SnSe NPs. Herein, we selected the simplest and most cost-effective synthetic method (i.e. normal pressure and water as solvent) as a prototypical reaction and used a slightly modified synthesis reported by Gregory et al.[31] Table 1. Summary of the state-of-art thermoelectric performance of p-type doped polycrystalline SnSe from solution-processed methods: including precursors, solvents, reaction temperature (T), reaction time (t), sintering conditions, and peak zT values (zTmax). Material Precursors, solvent zTmax Sn0.96Ga0.04Se[20] SnCl2·2H2O, GaCl3, NaOH, Se, H2O 2.2 (873 K) Sn0.98Pb0.01Zn0.01Se[27] SnCl2·2H2O, PbCl2, ZnCl2, NaOH, Se, H2O 2.2 (873 K) Sn0.95Se[50] SnCl2·2H2O, NaOH, Se, H2O 2.1 (873 K) Sn0.97Ge0.03Se[3] SnCl2·2H2O, GeI4, NaOH, Se, H2O 2.1 (873 k) Sn0.99Pb0.01Se-Se QDs[51] SnCl2·2H2O, PbCl2, NaOH, Se, H2O 2.0 (873 K)
5 Sn0.96Pb0.01Cd0.03Se[22] SnCl2·2H2O, PbCl2, CdCl2, NaOH, Se, H2O 1.9 (873 K) Sn0.948Cd0.023Se[52] SnCl2·2H2O, CdCl2, Na2SeO3, NaOH, EG 1.7 (823 K) SnSe-4%InSey[54] SnCl2·2H2O, InCl3·4H2O, Na2SeO3, NaOH, EG 1.7 (823 K) SnSe-1%PbSe[23] SnCl2·2H2O, PbCl2, NaOH, Se, H2O 1.7 (873 K) NaOH-Sn1−xSe[28] SnCl2, Na2SeO3, NaOH, EG 1.5 (823 K) Sn0.882Cu0.118Se[32] SnCl2·2H2O, CuCl2, Na2SeO3, NaOH, EG 1.41 (823 K) SnSe-15%Te NWs[49] SnCl2·2H2O, NaBH4, NaOH, Se, H2O 1.4 (790 K) Sn0.98Se[50] SnCl2·2H2O, Na2SeO3, NaOH, EG 1.36 (823 K) SnSe0.90Te0.1[55] SnCl2·2H2O, Na2SeO3, Na2TeO3, NaOH, EG 1.1 (800 K) Sn0.99Cu0.01Se[26] SnCl2·2H2O, CuCl, NaOH, Se, H2O 1.2 (873 K) SnSe0.9S0.1[21] SnCl2·2H2O, Na2S, NaBH4, NaOH, Se, H2O 1.16 (923 K) In the chosen synthetic procedure, NaBH4 is first dissolved in water, and Se powder is slowly added to form HSe-. In parallel, NaOH and SnCl2·2H2O are dissolved in water and the solution is heated to its boiling point. At this temperature, the freshly prepared Se-solution is rapidly injected. Upon injection, the reaction mixture turns black, indicating NP formation. After that, the reaction mixture is kept under reflux for additional 2 h. The as-synthetized NPs are purified by precipitation/redispersion with water and ethanol and then dried under vacuum overnight at room temperature. Afterwards, NP powder is annealed in forming gas (95% N2 + 5% H2) to remove oxides.[44] Finally, the annealed powders are sintered into cylindrical pellets using a spark plasma sintering system. Throughout the process, X-ray diffraction (XRD) is used to verify that the product is pure phase orthorhombic SnSe (Figure 1). From NP synthesis to the pellet formation, the experimental details can be found in the methods section.
6 Figure 1. A) Scheme of the processing steps of SnSe pellets. B) XRD patterns of initial SnSe NPs, annealed NPs, and sintered pellet along the out-of-plane direction, including the reference PDF 00-048-1224. C) Corresponding representative SEM micrographs of the material in the different processing steps. The inset shows a dense SnSe cylindrical pellet. 3. NP properties To have a comprehensive understanding of the sintered material and its formation, we first analyzed the NPs in detail. Scanning electron microscopy (SEM) and transmission electron microscopy (TEM) showed that the NPs have a rectangular shape with an average lateral size of ca. 150 nm (Figure 1C and 2A). High-resolution TEM (HRTEM) analysis confirmed the SnSe orthorhombic structure (space group Pnma) with lattice parameters a=11.5156 Å, b=4.1571 Å, and c=4.4302 Å observed by XRD. We further performed energy-dispersive X- ray spectroscopy (EDS) analysis to study the composition of the particles and found that the SnSe NPs are slightly Se-rich (Figure S1). Moreover, EDS revealed that the particles contained Na, while neither Cl (from SnCl2) nor B (from the excess BH4-) were detected, indicating that the washing effectively removes byproducts and excess reagents (Figure 2B). X-ray photoemission spectroscopy (XPS, Figure S3) analysis suggests that most of the Na is at the NP surface, yet we cannot discard its partial presence within the SnSe NPs. In the Se 3d XPS region, four peaks can be deconvoluted. These correspond to the 3d3/2 and 3d5/2 emission peaks Pellet Annealed NPs Purified NPs PDF 00-048-1224 2 (deg) 20 30 40 50 60 Drying Annealing // ⊥ H2O / EtOH 30 40 10 20 50 ~14 g per batch 93% yield NP synthesis NP purification Consolidation P P SPS Se Precursor Slicing Purified NPs Annealed NPs Pellet BC A SnCl2NaOH Sn precursor Ar Ar SnSe NPs T 1 μm1 μm1 μm A
7 of Se in two different oxidation states. Se2-, from SnSe, is observed at low binding energies while at higher energies, more oxidized Se species are present, with an oxidation state closer to 0.[21],[57] We speculate that these species are polyselenides (Sex2-), formed by partial oxidation of the NP surface during washing, as has been observed for Cu2Se NPs.[58–60] During the synthesis, Na+ is a spectator ion that compensates the charge of the reactive ions (OH-, BH4-, HSe-, etc.) but does not react in any way. However, its presence in the washed NPs indicates that Na+ are adsorbed at the surface. To understand the nature of the adsorption, we performed electrophoretic mobility measurements and determined that SnSe NPs are negatively charged (zeta-potential = -22 ± 5 Mv, Figure 2C) consistent with the Se-rich surface as determined by EDS (Figure S1). These results indicate that, in solution, the NPs are surrounded by a layer (Stern layer) of strongly bound cations (Na+) and a second layer of loosely bound ions (diffuse layer) composed mostly of cations (Na+) and some anions (OH-, HSe-) (Figure 2C). During washing, most of the anions are washed away (final pH = 10), but cations remain to ensure charge neutrality, explaining the presence of Na+ in the surface of the NPs (Na-SnSe, Figure 2D).
8 Figure 2. A) Bright-field TEM micrograph of several faceted SnSe NPs, HRTEM micrograph of the rectangular nanoparticle indicated with a blue square, and its corresponding power spectrum (FFT); B) STEM-EDS elemental mapping of Sn (blue), Se (red) and Na (green) for SnSe NPs; C) Schematic representation of the electrical double layer of aSnSe NP in solution; D) Schematic representation of a precipitated NP with Na+ ions adsorbed to preserve charge neutrality. 4. Pellets microstructure Compositional analysis with optic emission spectroscopy (ICP-OES, Figure SX) and EDS revealed that the pellets have ca. 2 at% Na content. Beyond the solubility limit, such large Na content is indirect proof that, independently of Na entering the lattice during the NPs synthesis, Na+ is adsorbed at the NP surface to maintain charge neutrality. We studied pellet’s microstructure with atom probe tomography (APT, Figure 3) and HRTEM (Figure 4) to determine the distribution of Na in the sintered material. Figure 3 shows the 3D distribution of Na in the pellets illustrated by the 2.0 at% Na isoconcentration surfaces; these surfaces are
9 analogous to contour plots such as altitude in a terrain and highlight the areas where the concentration of Na is ≥2 at%.[61] Na in the pellets is distributed in four different environments: i) within the grains; ii) at dislocations; iii) forming grain boundary complexions,[21] and iv) in nanoprecipitates (Figure 3). Figure 3. APT of a Na-containing SnSe pellet. A) 3D distribution of Na+ showing multiple dislocations highlighted by the Na-2.0 at. % isocomposition surface; B) 1D composition profile across a grain dislocation; C) 3D distribution of Na+ in the same pellet showing Na-rich precipitates; D) 1D composition profile across a precipitate. The characterizations prove that Na is an involuntary impurity of the NPs, and therefore of the final material when present in the reaction mixture. Hence, to evaluate the effect of Na in the processing and the transport properties of the material, we developed a new synthetic route to obtain Na-free SnSe NPs. In our synthesis, we replaced Na+ for a cation that decomposes during the annealing step. In particular, we used tetramethylammonium salts: Me4NBH4 and Me4NOH, instead of NaBH4 and NaOH. Following the same synthetic and purification process, we obtained pure phase Me4N-SnSe NPs with comparable characteristics (size and shape) to the ones produced with Na+ salts, Na-SnSe NPs (Figure S2). XPS characterization of Me4N- 015 30 45 60 75 0 1 2 48 51 54 Sn Se Na Composition (at. %) Distance (nm) 50 nm 2.0 at% Na Precipitates Dislocation C A 2.0 at% Na Dislocation array Dislocation 50 nm B Grain boundary Homogeneously distributed within the grain 010 20 30 40 0 3 6 9 40 45 50 55 Sn Se Na Composition (at. %) Distance (nm) D
16 the highest reported value.[90–92] We believe this is correlated to the fact that the synthetic methods used all Na salts to produce SnSe NPs. Hence, when n-type dopants are introduced, the presence of Na+, up to now unknown, establishes a pinning problem (coexistence of both types of dopants). 7. Experimental Section SnSe NPs synthesis: SnSe NPs were prepared following a procedure previously reported by Han et al.[31] with slight modifications. In a typical synthesis, NaBH4 (160 mmol, 98%, Fisher Scientific) was first dissolved in 400 ml deionized water, and then Se powder (80 mmol, 100 mesh, ≥99.5%, Sigma-Aldrich) was slowly added into the solution. Stirring should be avoided during this step due to the strong evolution of hydrogen gas. Once the bubbling finished, stirring was resumed under Ar flow until the solution became transparent indicating the complete reduction of Se. In parallel, NaOH (750 mmol, 98% Fisher Scientific) and SnCl2٠2 H2O (72 mmol, 98%, Fisher Scientific) were mixed with 360 ml of deionized water. The mixture was stirred at room temperature under Ar flow until complete dissolution. At this point, the solution was heated under reflux to its boiling point (ca. 101.3 °C). The freshly prepared selenide solution was rapidly injected into the boiling Sn (II) solution, and the temperature dropped to ~70 °C. Upon injection, the reaction mixture turned black indicating the NP formation. The temperature was allowed to recover to 101.3 °C and maintained at this temperature for 2 h. To purify the as-synthetized NPs, the mixture was decanted, and the transparent supernatant was carefully discarded. The remaining crude mixture (ca. 120 ml) was transferred into 3 centrifuge tubes. The NPs were purified by 3 precipitation/re-dispersion cycles with deionized water and ethanol alternatively. In the first cycle, the fresh deionized water was added into the crude solution by centrifugation at 6000 rpm for 1 min. Then, ethanol was used to redisperse the particles and the solution was centrifuged at 8000 rpm for 5 min. In the second cycle, deionized water was added to solubilize the remaining impurities and NPs
17 were precipitated by centrifugation at 9000 rpm for 5 min, Afterward, ethanol was employed to re-disperse and precipitate the particles by centrifugation at 8000 rpm for 5 min. These same steps were repeated for a third purification cycle. Washed NPs were dried under vacuum overnight at room temperature and kept in the glovebox for further use. Me4N-SnSe NPs: SnSe NPs without Na+ were produced following the above procedure keeping the molar ratios and using (CH3)4NOH٠5 H2O (tetramethylammonium hydroxide pentahydrate, 98%, Sigma-Aldrich) and (CH3)4NBH4 (tetramethylammonium borohydride, 95%, Sigma-Aldrich) instead of the corresponding Na-reagents. Bulk nanomaterial sintering: Dried SnSe NPs were annealed at 500 °C for 1 h under a forming gas (95% N2 + 5% H2) flow inside a tube furnace with the heating rate of around 10 °C/min. Then, the annealed powder finely grounded with an agate mortar and loaded into a graphite die in a glovebox before being pressed into cylinders (Ø 8.6 mm×12 mm). The process was carried out under vacuum, in an AGUS PECS Spark Plasma Sintering (SPS) System - Model SPS 210Sx applying a pressure of 45 MPa and at temperature of 500 °C for 5 min. The relative densities of the compacted pellets were measured by the Archimedes’ method and found to be above 92% of the theoretical value in all samples. From these cylinders, round shape pellets and rectangular bars were cut in two normal directions, i.e. parallel to the pressing direction and within the cylinder plane. Structural and chemical characterization: X-ray diffraction (XRD, 2θ: 20° to 60°; scanning rate: 5°/min) analyses were carried out on a Bruker AXS D8 ADVANCE X-ray diffractometer with Cu–Kα radiation (λ= 1.5406 Å). Size and morphology of initial NPs, annealed nanopowders, sintered pellets were examined by field-emission scanning electron microscopy (SEM) on an Auriga Zeiss operated at 5.0 kV. Composition was investigated by using an Oxford energy dispersive X-ray spectrometer (EDX) attached to the Zeiss Auriga SEM at 15.0
18 kV. Zeta potential and Zeta Deviations were measured with a Malvern Panalytical Zetasizer Nano (λ = 633 nm) in samples diluted in water (~0.1 mg/ml , pH = 6.5-7.0). The results are the average of 4 measurements with standard deviation <1 and were determined using the Smoluchowski approximation. HRTEM and STEM studies were conducted using a FEI Tecnai F20 field emission gun microscope operated at 200 kV with a point-to-point resolution of 0.19 nm. Before TEM studies, we prepared a cross-section by cutting it with a diamond saw. The piece obtained was afterward thinned to electron transparency by Focus Ion Beam (FIB) FEI Helios Dual Beam Nanolab. XPS was carried out on a Specs system equipped with a Mg anode XR50 source operating at 250 W and a Phoibos 150 MCD-9 detector (Specs GmbH). The pressure in the analysis chamber was kept below 10-7 Pa. Data processing was performed with the CasaXPS program (Casa Software Ltd.).Needle-shaped APT specimens were prepared by a standard “lift-out” method in a SEM/FIB dual-beam focused ion beam microscope (Helios NanoLab 650, FEI). APT measurements were performed on a local electrode atom probe (LEAP4000X Si, Cameca) by applying 10-ps, 5-pJ ultraviolet (wavelength=355 nm) laser pulses. The pulse repetition rate is 200 kHz, and the detection rate is set as 1 ion per 100 pulses on average. The measurement base temperature of specimen is 30 K to minimize surface migration. The ion flight path is 160 mm in our system. The detection efficiency of this LEAP is 50% owing to the open area of the microchannel plates. APT data were processed with the commercial software package IVAS 3.8.0. Thermoelectric characterization: Seebeck coefficients were measured by using a static DC method. Electrical resistivity data was obtained by a standard four-probe method. Seebeck coefficient and electrical resistivity were measured simultaneously in an LSR-3 LINSEIS system between room temperature and 833 K, under He atmosphere. 3 up and down
19 measurements were taken. Taking into account the system accuracy and the measurement precision, we estimate an error of ca. 4 % in the measurement of the electrical conductivity and Seebeck coefficient, respectively. The thermal conductivity was calculated by κ = λ Cp ρ, where λ is the thermal diffusivity, Cp is the heat capacity, and ρ is the mass density of the specimen. An LFA 1000 LINSEIS was used to determine the thermal diffusivities (λ) of the samples by the Laser Flash method with an estimated error of ca. 2.4 %. The constant pressure heat capacity (Cp) was estimated from empirical formula by the Dulong–Petit limit (3R law), and the density (ρ) values were measured using the Archimedes’ method. To avoid cluttering the plots, error bars were not included in the figures. Room temperature Hall charge carrier concentrations (nH) were measured with the Van der Pauw method using a magnetic field of 0.6 T (ezHEMS, NanoMagnetics). Values provided correspond to the average of 6 measurements, from which an error of ca. 15% was estimated. Supporting Information Supporting Information is available from the Wiley Online Library. Acknowledgements This work was financially supported by IST. AustriaYL acknowledges funding from the European Union’s Horizon 2020 research and innovation program under the Marie Sklodowska-Curie grant agreement No. 754411. M.C. has received funding from the European Union’s Horizon 2020 research and innovation programme under the Marie Skłodowska-Curie Grant Agreement No. 665385. SIEMENS CHENG..MEINER Received: ((will be filled in by the editorial staff)) Revised: ((will be filled in by the editorial staff)) Published online: ((will be filled in by the editorial staff)) References [1] S. Ortega, M. Ibáñez, Y. Liu, Y. Zhang, M. V Kovalenko, D. Cadavid, A. Cabot, Chem. Soc. Rev. 2017, 46, 3510. [2] A. Zevalkink, D. M. Smiadak, J. L. Blackburn, A. J. Ferguson, M. L. Chabinyc, O. Delaire, J. Wang, K. Kovnir, J. Martin, L. T. Schelhas, T. D. Sparks, S. D. Kang, M. T. Dylla, G. J. Snyder, B. R. Ortiz, E. S. Toberer, Appl. Phys. Rev. 2018, 5, 21303.
20 [3] S. Chandra, K. Biswas, 2019, 141, 6141. [4] M. Ibáñez, R. Zamani, W. Li, D. Cadavid, S. Gorsse, N. A. Katcho, A. Shavel, A. M. López, J. Ramon Morante, J. Arbiol, A. Cabot, Chem. Mater. 2012, 24, 4615. [5] M. Ibáñez, Z. Luo, A. Genç, L. Piveteau, S. Ortega, D. Cadavid, O. Dobrozhan, Y. Liu, M. Nachtegaal, M. Zebarjadi, J. Arbiol, M. V Kovalenko, A. Cabot, Nat. Commun. 2016, 7, 10766. [6] Z. Hens, J. De Roo, J. Am. Chem. Soc. 2020, 142, 15627. [7] S. H. Park, S. Jo, B. Kwon, F. Kim, H. W. Ban, J. E. Lee, D. H. Gu, S. H. Lee, Y. Hwang, J.-S. Kim, D.-B. Hyun, S. Lee, K. J. Choi, W. Jo, J. S. Son, Nat. Commun. 2016, 7, 13403. [8] S. Jo, S. Choo, F. Kim, S. H. Heo, J. S. Son, Adv. Mater. 2019, 31, 1804930. [9] Y. Liu, Y. Zhang, S. Ortega, M. Ibáñez, K. Ho Lim, A. Grau-Carbonell, S. Martí- Sánchez, K. Ming Ng, J. Arbiol, M. V. Kovalenko, D. Cadavid, A. Cabot, Nano Lett. 2018, 18, 2557. [10] In Surf. Chem. Colloid. Nanocrystals, The Royal Society Of Chemistry, 2021, pp. 1– 46. [11] A. Heuer-Jungemann, N. Feliu, I. Bakaimi, M. Hamaly, A. Alkilany, I. Chakraborty, A. Masood, M. F. Casula, A. Kostopoulou, E. Oh, K. Susumu, M. H. Stewart, I. L. Medintz, E. Stratakis, W. J. Parak, A. G. Kanaras, Chem. Rev. 2019, 119, 4819. [12] M. Ibáñez, R. Zamani, S. Gorsse, J. Fan, S. Ortega, D. Cadavid, J. Ramon Morante, J. Arbiol, A. Cabot, ACS Nano 2013, 7, 2573. [13] M. Cargnello, C. Chen, B. T. Diroll, V. V. T. Doan-Nguyen, R. J. Gorte, C. B. Murray, J. Am. Chem. Soc. 2015, 137, 6906. [14] P. Mohapatra, S. Shaw, D. Mendivelso-Perez, J. M. Bobbitt, T. F. Silva, F. Naab, B. Yuan, X. Tian, E. A. Smith, L. Cademartiri, Nat. Commun. 2017, 8, 2038. [15] M. Ibáñez, R. J. Korkosz, Z. Luo, P. Riba, D. Cadavid, S. Ortega, A. Cabot, M. G. Kanatzidis, J. Am. Chem. Soc. 2015, 137, 4046. [16] M. Scheele, N. Oeschler, K. Meier, A. Kornowski, C. Klinke, H. Weller, Adv. Funct. Mater. 2009, 19, 3476. [17] M. Ibáñez, A. Genç, R. Hasler, Y. Liu, O. Dobrozhan, O. Nazarenko, M. De La Mata, J. Arbiol, A. Cabot, M. V. Kovalenko, ACS Nano 2019, 13, 6572. [18] M. Ibáñez, R. Hasler, A. Genç, Y. Liu, B. Kuster, M. Schuster, O. Dobrozhan, D. Cadavid, J. Arbiol, A. Cabot, M. V. Kovalenko, J. Am. Chem. Soc. 2019, 141, 8025. [19] J. S. Son, H. Zhang, J. Jang, B. Poudel, A. Waring, L. Nally, D. V. Talapin, Angew. Chemie - Int. Ed. 2014, 53, 7466. [20] X. Lou, S. Li, X. Chen, Q. Zhang, H. Deng, J. Zhang, D. Li, X. Zhang, Y. Zhang, H. Zeng, G. Tang, ACS Nano 2021, 0, DOI 10.1021/acsnano.1c01469. [21] G. Han, S. R. Popuri, H. F. Greer, R. Zhang, L. Ferre-Llin, J. W. G. Bos, W. Zhou, M. J. Reece, D. J. Paul, A. R. Knox, D. H. Gregory, Chem. Sci. 2018, 9, 3828. [22] S. Li, X. Lou, X. Li, J. Zhang, D. Li, H. Deng, J. Liu, G. Tang, Chem. Mater. 2020, 32, 9761.
21 [23] G. Tang, W. Wei, J. Zhang, Y. Li, X. Wang, G. Xu, C. Chang, Z. Wang, Y. Du, L. D. D. Zhao, 2016, 138, 13647. [24] M. Li, Y. Liu, Y. Zhang, X. Han, T. Zhang, Y. Zuo, C. Xie, K. Xiao, J. Arbiol, J. Llorca, M. Ibáñez, J. Liu, A. Cabot, ACS Nano n.d., 15, 4967. [25] W. Wei, C. Chang, T. Yang, J. Liu, H. Tang, J. Zhang, Y. Li, F. Xu, Z. Zhang, J.-F. F. Li, G. Tang, J. Am. Chem. Soc. 2018, 140, 499. [26] Y. Gong, C. Chang, W. Wei, J. Liu, W. Xiong, S. Chai, D. Li, J. Zhang, G. Tang, Scr. Mater. 2018, 147, 74. [27] J. Liu, P. Wang, M. Wang, R. Xu, J. Zhang, J. Liu, D. Li, N. Liang, Y. Du, G. Chen, G. Tang, Nano Energy 2018, 53, 683. [28] X. Shi, W. Liu, A. Wu, V. T. Nguyen, H. Gao, Q. Sun, R. Moshwan, J. Zou, Z. Chen, InfoMat 2020, 2, 1201. [29] X. Shi, Z. G. Chen, W. Liu, L. Yang, M. Hong, R. Moshwan, L. Huang, J. Zou, Energy Storage Mater. 2018, 10, 130. [30] Y. Min, J. W. Roh, H. Yang, M. Park, S. Il Kim, S. Hwang, S. M. Lee, K. H. Lee, U. Jeong, Adv. Mater. 2013, 25, 1425. [31] G. Han, S. R. Popuri, H. F. Greer, J. W. G. Bos, W. Zhou, A. R. Knox, A. Montecucco, J. Siviter, E. A. Man, M. MacAuley, D. J. Paul, W. G. Li, M. C. Paul, M. Gao, T. Sweet, R. Freer, F. Azough, H. Baig, N. Sellami, T. K. Mallick, D. H. Gregory, Angew. Chemie - Int. Ed. 2016, 55, 6433. [32] X. Shi, K. Zheng, M. Hong, W. Liu, R. Moshwan, Y. Wang, X. Qu, Z. G. Chen, J. Zou, Chem. Sci. 2018, 9, 7376. [33] H. Wang, X. Liu, B. Zhang, L. Huang, M. Yang, X. Zhang, H. Zhang, G. Wang, X. Zhou, G. Han, Chem. Eng. J. 2020, 393, 124763. [34] C. Han, Z. Li, G. Q. (Max) Lu, S. Xue Dou, Nano Energy 2015, 15, 193. [35] L.-D. Zhao, C. Chang, G. Tan, M. G. Kanatzidis, Energy Environ. Sci. 2016, 9, 3044. [36] Z. G. Chen, X. Shi, L. D. Zhao, J. Zou, High-Performance SnSe Thermoelectric Materials: Progress and Future Challenge, Elsevier Ltd, 2018. [37] A. Banik, S. Roychowdhury, K. Biswas, Chem. Commun. 2018, 54, 6573. [38] W. Shi, M. Gao, J. Wei, J. Gao, C. Fan, E. Ashalley, H. Li, Z. Wang, Adv. Sci. 2018, 5, 1700602. [39] X.-L. L. Shi, X. Tao, J. Zou, Z.-G. G. Chen, Adv. Sci. 2020, n/a, 1902923. [40] L. D. Zhao, S. H. Lo, Y. Zhang, H. Sun, G. Tan, C. Uher, C. Wolverton, V. P. Dravid, M. G. Kanatzidis, Nature 2014, 508, 373. [41] C. Chang, M. Wu, D. He, Y. Pei, C. F. Wu, X. Wu, H. Yu, F. Zhu, K. Wang, Y. Chen, L. Huang, J. F. Li, J. He, L. D. Zhao, Science (80-. ). 2018, 360, 778. [42] R. Guo, X. Wang, Y. Kuang, B. Huang, Phys. Rev. B 2015, 92, 115202. [43] Y. Xiao, C. Chang, Y. Pei, D. Wu, K. Peng, X. Zhou, S. Gong, J. He, Y. Zhang, Z. Zeng, L.-D. Zhao, Phys. Rev. B 2016, 94, 125203. [44] Y. K. Lee, Z. Luo, S. P. Cho, M. G. Kanatzidis, I. Chung, Joule 2019, 3, 719. [45] Y. Luo, S. Cai, X. Hua, H. Chen, Q. Liang, C. Du, Y. Zheng, J. Shen, J. Xu, C.
22 Wolverton, V. P. Dravid, Q. Yan, M. G. Kanatzidis, Adv. Energy Mater. 2019, 9, 1803072. [46] Z.-H. Ge, D. Song, X. Chong, F. Zheng, L. Jin, X. Qian, L. Zheng, R. E. Dunin- Borkowski, P. Qin, J. Feng, L.-D. Zhao, J. Am. Chem. Soc. 2017, 139, 9714. [47] T. R. Wei, G. Tan, X. Zhang, C. F. Wu, J. F. Li, V. P. Dravid, G. J. Snyder, M. G. Kanatzidis, J. Am. Chem. Soc. 2016, 138, 8875. [48] E. K. Chere, Q. Zhang, K. Dahal, F. Cao, J. Mao, Z. Ren, J. Mater. Chem. A 2016, 4, 1848. [49] M. Li, Y. Liu, Y. Zhang, Y. Zuo, J. Li, K. H. H. Lim, D. Cadavid, K. M. M. Ng, A. Cabot, Dalton. Trans. 2019, 48, 3641. [50] X. Shi, Z. G. Chen, W. Liu, L. Yang, M. Hong, R. Moshwan, L. Huang, J. Zou, Energy Storage Mater. 2018, 10, 130. [51] R. Xu, L. Huang, J. Zhang, D. Li, J. Liu, J. Liu, J. Fang, M. Wang, G. Tang, J. Mater. Chem. A 2019, 7, 15757. [52] X. Shi, A. Wu, T. Feng, K. Zheng, W. Liu, Q. Sun, M. Hong, S. T. Pantelides, Z.-G. Chen, J. Zou, Adv. Energy Mater. 2019, 9, 1803242. [53] X. Liu, J. Xiao, H. Peng, X. Hong, K. Chan, J. K. Nørskov, Nat. Commun. 2017, 8, 1. [54] X. Shi, A. Wu, W. Liu, R. Moshwan, Y. Wang, Z.-G. G. G. Chen, J. Zou, ACS Nano 2018, 12, 11417. [55] M. Hong, Z. G. Chen, L. Yang, T. C. Chasapis, S. D. Kang, Y. Zou, G. J. Auchterlonie, M. G. Kanatzidis, G. J. Snyder, J. Zou, J. Mater. Chem. A 2017, 5, 10713. [56] M. Yarema, O. Yarema, W. M. M. Lin, S. Volk, N. Yazdani, D. Bozyigit, V. Wood, Chem. Mater. 2017, 29, 796. [57] K. Nakano, T. Sato, M. Tazaki, M. Takagi, 2000, DOI 10.1021/la990688x. [58] S. C. Riha, D. C. Johnson, A. L. Prieto, J. Am. Chem. Soc. 2011, 133, 1383. [59] D. Zhu, A. Tang, Q. Kong, B. Zeng, C. Yang, F. Teng, J. Phys. Chem. C 2017, 121, DOI 10.1021/acs.jpcc.7b03826. [60] D. Zhu, L. Wang, Z. Liu, A. Tang, Appl. Surf. Sci. 2020, 509, 145327. [61] O. C. Hellman, J. A. Vandenbroucke, J. Rüsing, D. Isheim, D. N. Seidman, Microsc. Microanal. 2000, 6, 437. [62] H. Konno, Y. Yamamoto, Bull. Chem. Soc. Jpn. 1987, 60, 2561. [63] J. Sangster, A. D. D. Pelton, The Na-Se (Sodium-Selenium) System, ASM International, 1997. [64] S.-J. L. Kang, Sintering: Densification, Grain Growth, and Microstructure, Butterworth-Heinemann, Oxford, 2005. [65] C. M. Sutter-Fella, J. A. Stückelberger, H. Hagendorfer, F. La Mattina, L. Kranz, S. Nishiwaki, A. R. Uhl, Y. E. Romanyuk, A. N. Tiwari, Chem. Mater. 2014, 26, 1420. [66] D. Braunger, D. Hariskos, G. Bilger, U. Rau, H. W. Schock, Thin Solid Films 2000, 361, 161. [67] M. Johnson, S. V. Baryshev, E. Thimsen, M. Manno, X. Zhang, I. V. Veryovkin, C.
23 Leighton, E. S. Aydil, Energy Environ. Sci. 2014, 7, 1931. [68] W. K. Musker, J. Am. Chem. Soc. 1964, 86, 960. [69] P. M. Anderson, J. P. Hirth, J. Lothe, Theory of Dislocations, Cambridge University Press, Cambridge, 2017. [70] K. V Ravi, Metall. Trans. 1972, 3, 1311. [71] Z. Chen, B. Ge, W. Li, S. Lin, J. Shen, Y. Chang, R. Hanus, G. J. Snyder, Y. Pei, Nat. Commun. 2017, 8, 13828. [72] Z. Chen, Z. Jian, W. Li, Y. Chang, B. Ge, R. Hanus, J. Yang, Y. Chen, M. Huang, G. J. Snyder, Y. Pei, Adv. Mater. 2017, 29, 1606768. [73] M. Legros, G. Dehm, E. Arzt, T. J. Balk, Science (80-. ). 2008, 319, 1646 LP. [74] Y. Yu, S. Zhang, A. M. Mio, B. Gault, A. Sheskin, C. Scheu, D. Raabe, F. Zu, M. Wuttig, Y. Amouyal, O. Cojocaru-Mirédin, ACS Appl. Mater. Interfaces 2018, 10, 3609. [75] S. A. Yamini, T. Ikeda, A. Lalonde, Y. Pei, S. X. Dou, G. J. Snyder, J. Mater. Chem. A 2013, 1, 8725. [76] J. He, I. D. Blum, H.-Q. Wang, S. N. Girard, J. Doak, L.-D. Zhao, J.-C. Zheng, G. Casillas, C. Wolverton, M. Jose-Yacaman, D. N. Seidman, M. G. Kanatzidis, V. P. Dravid, Nano Lett. 2012, 12, 5979. [77] S. A. Yamini, D. R. G. Mitchell, Z. M. Gibbs, R. Santos, V. Patterson, S. Li, Y. Z. Pei, S. X. Dou, G. Jeffrey Snyder, Adv. Energy Mater. 2015, 5, 1501047. [78] Y. K. Lee, K. Ahn, J. Cha, C. Zhou, H. S. Kim, G. Choi, S. I. Chae, J. H. Park, S. P. Cho, S. H. Park, Y. E. Sung, W. B. Lee, T. Hyeon, I. Chung, J. Am. Chem. Soc. 2017, 139, 10887. [79] Y. Zhou, W. Li, M. Wu, L.-D. Zhao, J. He, S.-H. Wei, L. Huang, Phys. Rev. B 2018, 97, 245202. [80] G. Shi, E. Kioupakis, J. Appl. Phys. 2015, 117, 065103. [81] L. Huang, G. Han, B. Zhang, D. H. Gregory, J. Mater. Chem. C 2019, 7, 7572. [82] L. D. Zhao, G. Tan, S. Hao, J. He, Y. Pei, H. Chi, H. Wang, S. Gong, H. Xu, V. P. Dravid, C. Uher, G. J. Snyder, C. Wolverton, M. G. Kanatzidis, Science (80-. ). 2016, 351, 141. [83] J. B. Li, V. Chawla, B. M. Clemens, Adv. Mater. 2012, 24, 720. [84] Y. Yan, C. S. Jiang, R. Noufi, S. H. Wei, H. R. Moutinho, M. M. Al-Jassim, Phys. Rev. Lett. 2007, 99, 235504. [85] C. S. Jiang, R. Noufi, J. A. AbuShama, K. Ramanathan, H. R. Moutinho, J. Pankow, M. M. Al-Jassim, Appl. Phys. Lett. 2004, 84, 3477. [86] C. Gayner, Y. Amouyal, Adv. Funct. Mater. 2019, DOI 10.1002/adfm.201901789. [87] J. Martin, L. Wang, L. Chen, G. S. Nolas, Phys. Rev. B 2009, 79, 115311. [88] T. R. Wei, G. Tan, C. F. Wu, C. Chang, L. D. Zhao, J. F. Li, G. J. Snyder, M. G. Kanatzidis, Appl. Phys. Lett. 2017, 110, 053901. [89] X. Shi, X. Tao, J. Zou, Z. Chen, Adv. Sci. 2020, 7, 1902923.
24 [90] X.-L. Shi, K. Zheng, W.-D. Liu, Y. Wang, Y.-Z. Yang, Z.-G. Chen, J. Zou, Adv. Energy Mater. 2018, 8, 1800775. [91] S. Chandra, A. Banik, K. Biswas, ACS Energy Lett. 2018, 3, 1153. [92] Z.-H. Ge, Y. Qiu, Y.-X. Chen, X. Chong, J. Feng, Z.-K. Liu, J. He, Adv. Funct. Mater. 2019, 29, 1902893.