scieee AI-readable full text Open interactive document viewer

Design of a cathodic protection of offshore structures

Taskiran, Bahat

Abstract

Based on the standpoint of the environment, corrosion is an environmental occurrence that is required to maintain the natural balance. From the engineer’s standpoint, this natural balance is observed as a damaging natural attack on a metal by an electrochemical reaction. This natural attack has various types such as uniform, crevice or pitting corrosion and it results in severe material loss, which contributes to lost production and increased maintenance, repair, and replacement costs, as well as restoration costs. Hence, prevention of corrosion is quite significant for metal to be applied in an offshore platform.

Full text

1 Design of Cathodic Protection of Offshore Structures/Màster Treball Final de Master Facultat de Nàutica de Barcelona Universitat Politècnica de Catalunya Written by: Bahat Taskiran Supervisors: Assoc. Prof. Dr. Özgür Özgüç Asoc. Prof. Dr. Sergio Ivan Velasquez Correa Master Barcelona, data 2 Disseny de Protecció Catòdica d'Estructures Offshore/Màster Treball Final de Master Facultat de Nàutica de Barcelona Universitat Politècnica de Catalunya Treball realitzat per: Bahat Taskiran Dirigit per: Assoc. Prof. Dr. Özgür Özgüç Asoc. Prof. Dr. Sergio Ivan Velasquez Correa Master Barcelona, data Departament de CIÈNCIA I ENGINYERIA NÀUTIQUES 3 Versió Data Modificacions 1 [Data] Creació del document Revisió... Escrit per: Revisat i aprovat per: Autor/a: Tutor/a: Data: Data: Revisat i aprovat per: Co-Tutor/a: Data: 4 To my mother, father and sister... 5 6 Resum Basat en el punt de vista del medi ambient, la corrosió és un esdeveniment ambiental que cal per mantenir l'equilibri natural. Des del punt de vista de lenginyer, aquest equilibri natural sobserva com un atac natural perjudicial a un metall per una reacció electroquímica. Aquest atac natural té diversos tipus, com la corrosió uniforme, per esquerdes o per picades, i dóna com a resultat una pèrdua de material severa, fet que contribueix a la pèrdua de producció ia l'augment dels costos de manteniment, reparació i reemplaçament, així com els costos de restauració. Per tant, la prevenció de la corrosió és molt important per al metall que s'aplicarà a una plataforma marina. El mètode més típic per prevenir la corrosió de les superfícies d'acer de les estructures a alta mar és utilitzar un sistema de protecció catòdica i un revestiment eficaç. Els mètodes de protecció catòdica funcionen convertint les àrees actives d'una superfície metàl·lica en àrees passives, col·locant-les així al càtode d'una cel·la electroquímica. Mentre s'apliquen aquests mètodes de protecció, també es pot fer servir un recobriment. La intenció del recobriment és regular una via electrolítica posant una barrera entre la superfície metàl·lica i la solució corrosiva. Abans de discutir els detalls del disseny, en aquesta investigació s'esmenten tant la protecció catòdica de corrent impresa com la protecció catòdica d'ànode de sacrifici, així com la combinació de CP amb recobriment. El mètode de l'ànode de sacrifici (SACP) s'aplica amb un metall que té un potencial menor que el metall de l'estructura que cal protegir. Per tant, els ànodes de sacrifici provoquen una corrosió del metall més ràpida que la que té l'estructura metàl·lica i brinden protecció contra la corrosió. Mentre que, com que el mètode de corrent impres (ICCP) produeix el seu corrent per mitjà d'una font externa, no hi ha necessitat d'ànode de sacrifici com s'aplica a SACP. Sobre aquesta base, tots dos mètodes de protecció catòdica tenen diferents requisits i criteris de disseny. Aquestes diferències entre SACP i ICCP s'esmenten en aquesta investigació en termes d'instal·lació del sistema, efectes ambientals, combinació amb recobriment i requisits d'acer i ànode. Durant l'aplicació d'aquestes proteccions, tota la vida d'aquesta protecció per a l'estructura en qüestió es denomina Vida Anticipada. Encara que és difícil complir completament la vida prevista, el càlcul del disseny s'ha de fer d'acord amb aquesta vida útil i els paràmetres requerits (p. ex., massa de l'ànode, tipus d'ànode, sortida de corrent, etc.) s'han d'obtenir correctament . Si no, la distribució d'ànodes podria no ser eficient per desplegar tota l'àrea a protegir. Com a exemple de càlcul de disseny per a una àrea submergida d'un sistema, es va considerar el disseny de SACP per a una estructura hipotètica de parc eòlic ubicada a les Illes Canàries i es va seguir la recomanació de disseny DNV-RP-B401 com a guia en aquesta investigació. Els paràmetres inicials dels càlculs de disseny (per exemple, salinitat, massa inicial, temperatura, etc.) es van obtenir de fonts governamentals i projectes anteriors a les Illes Canàries. La intenció principal d‟aquest càlcul és explicar el procés de disseny de protecció catòdica utilitzant la recomanació DNV i determinar les diferències entre estructures recobertes i no recobertes en termes de requisits d‟ànode. Segons els resultats, l'ús d'un ànode d'alumini independent, que té un factor d'utilització més gran en comparació amb altres tipus d'ànodes, a més del recobriment de Categoria III basat en la guia DNV, condueix a una menor quantitat de massa d'ànode. Per tant, el consum d'ànodes i les despeses es minimitzaran i hi ha una distribució d'ànodes més adequada a través de les distàncies més llargues a causa de la caiguda més baixa d'IR. 7 ABSTRACT Based on the standpoint of the environment, corrosion is an environmental occurrence that is required to maintain the natural balance. From the engineer’s standpoint, this natural balance is observed as a damaging natural attack on a metal by an electrochemical reaction. This natural attack has various types such as uniform, crevice or pitting corrosion and it results in severe material loss, which contributes to lost production and increased maintenance, repair, and replacement costs, as well as restoration costs. Hence, prevention of corrosion is quite significant for metal to be applied in an offshore platform. The most typical method of preventing corrosion from steel surfaces of offshore structures is to use a cathodic protection system and effective coating. The Cathodic Protection methods work by converting active areas on a metal surface into passive areas, thus putting them into the cathode of an electrochemical cell. While applying these protection methods, a coating may also be employed. The intention of coating is to regulate an electrolytic pathway by putting a barrier between the metallic surface and the corrosive solution. Before discussing the design details, both Impressed Current Cathodic Protection and Sacrificial Anode Cathodic Protection, as well as the combination of CP with coating are mentioned in this research. The sacrificial anode method (SACP) is applied with a metal having a lower potential than the structure metal to be protected. Thus, sacrificial anodes result in quicker corrosion on metal than structure metal has and protect against corrosion. Whereas, as Imthe pressed current method (ICCP) produces its current by means of an external source, there is no need for sacrificial anode as it is applied in SACP. On this basis, both cathodic protection methods have different requirements and design criteria. These differences between SACP and ICCP are mentioned in this research in terms of installation of the system, steel and anode requirements, combination with coating, and environmental effects. While applying these protections, the entire life of this protection for the structure concerned is cal as “Anticipated Life”. Although it’s difficult to completely meet the anticipated life, design calculation must be done in accordance with this design life and required parameters ( e.g. anode mass, anode type, current output, etc.) must be obtained correctly. Otherwise, anode distribution might not be efficient to deploy the entire area to be protected. As an example of design calculation for a submerged area of a system, SACP design was considered for a hypothetical wind farm structure located in Canary Island and DNV-RP-B401 design recommendation was followed as guidance in this research. Initial parameters of design calculations (e.g. salinity, initial mass, temperature, etc.) were obtained by governmental sources and previous projects across Canary Island. The main intention of this calculation is to explain the design process of cathodic protection using DNV recommendation and determine the differences between coated and uncoated structures in terms of anode requirement. According to results, the use of stand-off aluminum anode which has a greater utilization factor compared to other anode types in addition Category III coating based on DNV guidance leads to a lower amount of anode mass. Thus, anode consumption and expenses will minimize and a more suitable anode distribution exists through the longer distances due to lower IR drop. Keywords: “Corrosion Control”, “Sacrificial Anode Cathodic Protection”, “Cathodic Protection Design Criteria”, “Impressed Current”, “Anode Calculation” 8 Table of contents ACKNOWLEDGEMENTS......................................................................................................................4 ABSTRACT...........................................................................................................................................6 LIST OF FIGURES........................................................................................................................11 LIST OF TABLES......................................................................................................................................13 CHAPTER 1. CORROSION………………………………………………………………………………………………………...16 1.1. INTRODUCTION TO CORROSION..................................................................................................16 1.2. CONTROL OF CORROSION..........................................................................................................18 1.3. POLARIZATION.........................................................................................................................19 1.3.1. Concentrated Polarization...........................................................................................19 1.3.2. Activated Polarization.................................................................................................19 1.4. CORROSION RATES...................................................................................................................22 1.5. CORROSION TYPES.................................................................................................................24 1.5.1. Uniform Corrosion......................................................................................................24 1.5.2. Galvanic Corrosion......................................................................................................24 1.5.3. Crevice Corrosion..................................................................................................................26 1.5.4. Pitting Corrosion.........................................................................................................26 1.5.5. Microbial Induced Corrosion.................................................................................................28 1.5.6. Environmental Cracking...............................................................................................30 1.6. OFFSHORE CORROSION AREAS................................................................................................31 1.6.1. Athmosperic Zone........................................................................................................32 1.6.2. Splash Zone.................................................................................................................32 1.6.3. Submerged Zone..........................................................................................................33 1.7. MATERIALS AND CORROSION BEHAVIOUR OF MATERIALS................................................33 1.7.1. Stainless Steel..............................................................................................................35 1.7.2. Carbon Steel................................................................................................................36 1.7.3. Cast Irons....................................................................................................................37 1.7.4. Alloy Steel...................................................................................................................37 CHAPTER 2. CATHODIC PROTECTION…………………………………………………………………………………..…39 2.1. PRINCIPLES OF CATHODIC PROTECTION..............................................................................39 2.1.1. Positive Effects of Using Cathodic Protection..................................................................42 2.1.2. Significant Points To Be Considered in Cathodic Protection..............................................44 2.1.2.1. Hydrogen Evolution of Cathodic Protection....................................................45 2.1.2.2. Potential of Components..............................................................................45 9 2.2 TYPES OF CATHODIC PROTECTION..................................................................................................46 2.2.1. Sacrificial Anode Cathodic Protection.............................................................................46 2.2.2. Impressed Current Cathodic Protection..........................................................................48 2.3. COATING.....................................................................................................................................49 2.3.1. Coating Types..............................................................................................................50 2.3.1.1. Inhibitor Coating..........................................................................................51 2.3.1.2. Barrier Coating.............................................................................................51 2.3.1.3. Sacrificial Coating........................................................................................51 2.3.2. Coating Selection.........................................................................................................51 2.3.3. Difficult Regions to be Coated.......................................................................................52 2.4. COMBINATION OF COATING AND CATHODIC PROTECTION..............................................................52 2.5. COMPARISON OF ICCP AND SACP..................................................................................................53 CHAPTER 3. DESIGN CALCULATIONS AND PROCEDURES OF CATHODIC PROTECTION……………….54 3.1. GENERAL……………………………………………………………………………………………………………………………54 3.2. DESIGN CALCULATIONS……………………………………………………………………………………………………………54 3.2.1. Surface Area……………………………………………………………………………………………………………54 3.2.2. Current Demand…………………………..…………………………………………………………………………54 3.2.3. Anode Mass…………………………………………………………………………………………………………….55 3.2.4. Anode Number………………………………………………………………………………………………………..56 3.2.5. Anode Resistance………………………………………………………………………………………………….…57 3.2.6. Anode Current Output…………………………………………………………………………………………………………58 3.3. DESIGN PARAMETERS USED IN CALCULATIONS…… …………...………………………………………………..59 3.3.1. Design Life……………………..……………………………………………………………………………………….59 3.3.2 Design Current Density…………………… ………………………………………………………………………..59 3.3.3 Anode Utilization Factor…………………………………………………………………………………………….60 3.3.4 Coating Breakdown Factor…………………………………………………………………………………………60 3.3.5 Current Drain Design Parameter……… ………………………………………………………………………..61 CHAPTER 4. MAINTENANCE AND RETROFIT OF CATHODIC PROTECTION…………………………………..62 4.1. ANODE MANUFACTURING ……………………………………………………………………………………………………….62 4.1.1. Requirements…….....……………………………………………………………………………………………….62 4.1.2. Manufacturing Procedure…………………………………………………………………………………………62 4.1.3. Coating………………………………………………………………………………………………………………..…62 4.1.4. Pre-Production Quality (PQT)…………………………………………………………………………………….62 4.1.5. Quality Control of Anode……………………………………………………………………………………….…63 4.1.6. Inspection and Testing…………………………………………………………………………………………..…63 4.2. MAINTENANCE AND OPERATIONS…………………………………………………………………………………………….64 4.2.1.Rectifier Ground-Bed Transformer Failure in ICCP…………………………………………………………64 4.2.2. Sacrificial Anode Cathodic Protection Failures……………………………………………………………..64 16 CHAPTER 1 1) CORROSION 1.1. Introduction to Corrosion Corrosion is the degradation of a metal as a result of chemical or electrochemical reactions occurring in its surroundings. Furthermore, corrosion is an electron transfer process that is a charged metal ion is formed while an uncharged metal atom loses one or more electrons as follows; This process must first be examined at a microscopic level in order to fully comprehend it. A corrosion cell made up of four components is required for the chemical reaction to take place. Potential corrosion can be defined as follows; 1) A cathode side where electrons are gattered. 2) An anode side where electrons are given off and leading to loss of metal. 3) A metallic circuit that is created by the structure. 4) An electrolyte area where anode and cathode are interacted with each other by submerging. 17 Figure 1. - Corrosion cell explaining the relations of the four key components of an active cell [5] The four components as it seems above are a circuit in which allows corrosion to take place due to potential difference and tendency of electron transfer from anode to cathode side through the metallic path. As a result of this reaction anode system expose corrosion. Metals tend to manage electricity. If the environment where metals are to be placed is also good conductive, then corrosion will occur through electrochemical factors. It should be noted that corrosion only occurs when metals interact with its environment. For more information, metal or alloy must be unstable with its environment. Hence, changing the environment of the metal could be an efficient way of corrosion prevention. However, the offshore environment can not be changed based on its electrochemical factor. The only way of prevention is using more suitable materials and applying for protection. For example, wrought iron would be suitable for the urban environment but the use of wrought iron will cause corrosion offshore due to the effects of the salt of the ocean. Corrosion and corrosion prevention costs are around 5.0 percent of a country's gross national product, resulting in a huge economic factor to companies. The entire cost of corrosion in the oil and gas industry is projected to be $1.372 billion per year. Compared to old projects, current Offshore Projects are projected in a hazardous environment including more factors that leads to corrosion impact. Component life must be improved due to the rising difficulty of maintaining components in more remote and demanding environments. Components with improved corrosion 18 resistance are now required because they extend service life and decrease the need for costly maintenance. The most efficient time to prevent corrosion is during the design phase. As a result, the designer must have a thorough understanding of corrosion concepts as well as specialized knowledge of the environment and materials relevant to their field of design. The use of proper design eliminates the need for costly retrofits. Following that, the commissioning and operation of plants should be done with corrosion protection in mind. [3] 1.2. Control Of Corrosion In this part, corrosion was defined briefly as the interaction between metal and its offshore environment, and factors leading to corrosion will be mentioned separately in the later sections, such as the amount of attack concerning metal’s thickness, types of corrosion ( Pitting, Crevice) and corroded area of surface, in order to discuss those in accordance with corrosion control. It’s obvious that corrosion rate is a vitally important factor in which regulates the life duration of structure. Even if the corrosion rate has a tolerated amount, engineers have to consider that it also depends on the thickness of the metal, the interaction of metal and environment, etc. In other words, all the factors must be reviewed in order to obtain control of corrosion. By using special metals for the structure, corrosion control can be thought of as a reaction regulator, which means, the mechanical and physical features of the metal can be provided in the whole life duration of the structure. While applying this process, the life of this structure is called “ Anticipated Life” and it should be noted that this is not the absolute time of the process. On the other hand, though engineers can be told according to planned time that operation should last, it can be corroded much earlier or some extra services can be required. There is no restriction for the cost, however, although structures can be designed to be 10-years of anticipated life, it’s completely impossible to design a facility that maintenance is not required during 10 years. Hence, spending more money in order to achieve more protection may lead to spending unnecessary money. Due to the fact that corrosion is an interaction between metal and its environment, these two factors must take place to control. Hence, control could be provided by selecting suitable metals or alloys rather than selecting all other materials or acting of the metals against non-metal materials. The other factors are, control of corrosion can be provided by the resistant materials or the materials that decrease the risks of the environment by means of applying corrosion inhibitors, changing the chemical reactions, avoiding sea pollution, shifting the temperature or velocity etc. The selection of metal and alloy can be changed according to companies and their work but the resistance of metals against corrosion can not be neglected. Also, the availability of the metal is significant and companies should find a factory that would also be able to manufacture the same metal next years. For instance, although 18%Cr – 8% Ni stainless steel are more expensive than 17% Cr stainless steel, the former are being manufactured more than the latter and it’s also problematic to weld the second one, hence the first one is more useable. Concerning to cost, this manufacturing and also delivering costs should be considered. It should not be considered that finding metal as cheap as it can, will be a good choice to avoid unnecessary expenses. For example, using platinum can be seen as unnecessary expenses but applying for certain parts of the structure will be a profitable investment. Even so, mild steel which 19 can be found easily and has enough corrosion resistance is more preferable to platinum for the offshore structures, just in case cathodic protection or an effective coating can be designed [15]. 1.3. Polarization Polarization is the process that turning a material’s normal potential into more positive or more negative through an external source. When an anode and a cathode are electrically coupled, the anode's lower standard potential acts as an external driving force, causing the cathodes to transfer, or polarize, towards a more negative potential. It may be considered that materials with more negative energy have more tendency to corrode, however, the amount of negative energy does not have a direct relationship in this way. To give an example, the negative energy potential of Aluminum is -1.662V which makes it a quite active metal, however, kinetic energy during the reaction or its corrosion rate is not as high as its potential. This is why it’s not used in the structural parts in which more dangerous or corrosion might spread around fast. For more information, to give an opposite example of Aluminum, copper (Cu) can be reviewed. Although Cu has a higher potential compared to Aluminum (+0.337 V), it corrodes higher than Aluminum does. In short, corrosion rates are not only dependent on potential, there are many various reasons which may affect the rate of corrosion, as mentioned in the corrosion Rates title. Hence, polarization is the combination of such relationships among current and potential that is dependent on many factors in the way of linear or non-linear. Polarization can be either cathodic or anodic, and it can be modulated by concentration or activation as mentioned below. 1) Concentrated Polarization: If there is enough component to undergo a reaction, the corrosion process can be limited by this amount and chemical reaction can be concentrated based on these components. As the components start consuming and transfer is slow, this polarization is also known as Overpotential Diffusion. For more information, the rate of ion diffusion on the metallic surface affects the increase of reaction rate. This ion rate is limiting current in other words and can be shown as 𝑖𝐿. In this equation 1 below, the relation of polarization response can be described. 𝜂𝐶= 2.303 𝑅𝑇 𝑛𝐹 log (1 − 𝑖 𝑖𝐿) (1.3.1) 𝑊ℎ𝑒𝑟𝑒; 𝜂𝐶∶ 𝑝𝑜𝑙𝑎𝑟𝑖𝑧𝑒𝑑 𝑝𝑜𝑡𝑒𝑛𝑡𝑖𝑎𝑙 i: current 𝑖𝐿: limited ion diffusion 2) Activated Polarization: The potential difference above the equilibration value required to produce currents based on the energy activation of a redox reaction is known as activation polarization. The activation energy is necessary for electrons to be transported from electrodes to the analyte. Furthermore, the characteristics that are part of generally all 20 electrochemical reactions and are inherent to kinetics are referred to as activation polarization. The reaction of hydrogen gas can be a good example of this. This is a straightforward reaction, and the pace at which hydrogen ions are transformed into hydrogen gas depends on several variables, including the rate at which electrons are transferred into hydrogen ions. This reaction is also called hydrogen overpotential. In order to start the chemical reaction, the required activation energy for polarization must be achieved. According to this reaction activated polarization can be described by equation 2 shown below. 𝜂𝐴= 𝛽𝑙𝑜𝑔 𝑖 𝑖𝑂 (1.3.1.) Where; 𝜂𝐴∶ 𝑝𝑜𝑙𝑎𝑟𝑖𝑧𝑒𝑑 𝑝𝑜𝑡𝑎𝑛𝑡𝑖𝑎𝑙 𝑖𝑂∶ 𝑒𝑙𝑒𝑐𝑡𝑟𝑖𝑐 𝑐𝑢𝑟𝑟𝑒𝑛𝑡 𝑡𝑜 𝑏𝑒 𝑎𝑐𝑡𝑖𝑣𝑎𝑡𝑒𝑑 Both activated and concentrated polarization equations contain the constant terms for each metal in which can be presented and the slope of the curve can be obtained. This slope is named as Tafel Slope which is known very well among the corrosion science community. This slope is conventional in order to evaluate corrosion behavior and obtain a relationship between polarization resistance. The essential principle of this process is to obtain the first reading of potential by measuring without current that is interacted with working electrolyte or metal of interest. Then the working electrolyte starts polarizing by means of galvanostatically, potentiodynamically, or potentiostatically and becomes more negative or positive. Finally, the current response can be obtained by this polarization and then an essential diagram of metal can be obtained. The other useable way of polarization is monitoring the corrosion to evaluate corrosion rate. This technique is called Linear polarization resistance and by applying this technique a plot can be achieved which includes the potential applied and its current response. Hence, it can be noted that polarization resistance is the slope of the curve which is obtained by the proportion of potential and current response. To give a before and after example for polarization resistance Figure 2 and Figure 3 are below. In these figures, it changes of carbon – steel rebar can be noted by the slope which is turning into almost a straight line by the time. By following this slope, the parts in which severe corrosion occurred can be observed. 21 Figure 2.The diagram of Carbon – Steel Rebar before corrosion [14] Concerning to Figure 2, ions are allowed to move into immersed electrolyte employing working electrode. Hence, it becomes enough to generate a big current by a potentiostat (in the way of potentiodynamically polarizing), thus indicating a low polarization resistance is a symbol of a high corrosion rate. Figure 3. The diagram of Carbon – Steel Rebar after corrosion [14] 22 It can be noted that there is an extreme change in the range of -77.0mV to -425.0mV, which means severe corrosion is occurred. 1.4. Corrosion Rates (𝒊𝒂) The corrosion rate is defined as the quantity of corrosion that occurred at the surface area over a given length of time. This rate can be obtained by measuring the before and after weight of metals exposed to a corrosive environment. The general method of corrosion rate is the result of applying driving force (L) and anodic resistance (R). The driving force is the difference between Corrosion Potential (𝐸𝑐𝑜𝑟𝑟) and Equilibrium Potential (𝐸𝑒𝑞). Also, the driving force can be referred to as the forces pushing anodic reaction of corrosion equation and so, it is contrasted with the anodic resistance (R). Hence, formulation of corrosion rate is the ratio of L and R, which is 𝑖𝑎 = L ⁄R formally. [21] Corrosion rate also can be obtained by electrochemical methods. To be able to employ the electrochemical methods, Faraday’s law can be used to turn electrochemical into gravimetric parameters. 𝐼.𝑡 𝐹 = ∆𝑊 𝑊𝑚/𝑍 Where; I = Electric current t = Time F = Constant value of Faraday ( 96500 coulombs) ∆𝑊 = Weight difference of metal Z = Valency of electrons By this equation, current can be obtained which is also known as “ corrosion density” or “Icorr” and this corrosion is assumed to be uniform corrosion in which will be referred to below at "corrosion types" part. That is allowed if there is a homogeneous attack and current obtained from the result must only be related with the surface exposed to the corrosion, hence it’s written by 𝜇A/𝑐𝑚2. It must be noted that electrochemical methods are the methods that are difficult to apply due to the high value of the Faraday constant and also low rates of corrosion can be taken into account which is not reached with the same methods used in electrochemical ones. 23 Figure 4. Structure behavior against seawater attack [14] The corrosion density produces instant values while the method is used. When it is recorded on a regular basis and compared to a specific period in order to determine the evolution of the corrosion process, it is turned into corrosion rate. Despite the rate and density are the different parameters, they take into account the same purposes practically. Current values of corrosion density can be considered as a comparative factor between offshore structures. To give an example, Figure 4 showed above, refers to the act of a structure interacting with the seawater attack. The corrosion density is low at first, then increases extremely based on the behavior of steel. There are many types of water and it is obvious that each has different quality in terms of corrosion. Offshore platforms, such as Oil and Gas Platforms are exposed to the most hazardous corrosion type coming from sea salt and immersion. Rates are driven by many factors. These are chemical factors, salinity, duration of wetness and temperature. As the ambient temperature increases corrosion rates increase as well. It was noted that a 10-degree difference in the weather affects corrosion 2.3 times faster due to more dissolution of the iron-carbon alloy. Concerning to chemical factors, it is noted that amount of chloride and sulfur dioxide increases while the system is corroding. The corrosion rates of metal artifacts exposed to the outside (bronze, copper, marble, and steel) are found to be proportional to the sulfur dioxide concentration. These types of factors are mostly based on the top part of the structure (Atmospheric zone) where the structure does not interact with the sea. The bottom part of the structure interacted with seawater has more corrosive media compared to the above part such as water velocity, pH and various dissolved salts coming from salinity. This complex form of marine environment makes the bottom part more significant and leads to all kinds of corrosion types. 24 1.5. Corrosion Types There are different types of corrosion, which a metal can be affected in offshore platforms as well as zones that different types of corrosion may occur. These types can be listed as Uniform Corrosion, Galvanic Corrosion, Crevice Corrosion, Pitting Corrosion, Microbial Induced Corrosion. Figure 5. Types of Corrosion 1.5.1 Uniform Corrosion: Uniform corrosion is also known as general corrosion. This corrosion is the consistent loss of metal over an entire surface. Although it is shown like the most dangerous corrosion type by its appearance, it’s quite easy to predict before it happens. Therefore, this corrosion is possibly the most well-known of all corrosion types by engineers. To get more comprehensive, engineers of NACE (National Association of Corrosion Engineers) have created a unit to be able to measure the corrosion rate (1 mil =0.001 in). Table 1 shows how the various rates of corrosion can be classified to correspond to the acceptable usage of materials. Table 1. Classification of Corrosion Rate by its performance. [6] 1.5.2. Galvanic Corrosion: Galvanic Corrosion is the most common corrosion process occurred in offshore platforms. The deterioration shows itself as a continuous layer of corrosion that covered the entire damaged surface area. When two dissimilar metals, such as stainless steel (SS) fitting and a regular carbon 25 steel (CS) nut are electrically linked in the same electrolyte, galvanic corrosion occurs. Furthermore, galvanic corrosion can be detected by the electrical current defined earlier. As previously stated, metals having soiled components can form an electrical circuit in which electrons can move from one location on a metal surface to another, leading to corrosion. As a result, purified metals that contain positive potential compared to active metals have more resistance against corrosion and this difference in potential can be classified by Galvanic series. Table 2 shows the list of common metals regarding their potential. Table 2. Potential differences [6] Noble metals are metals that can be used in their natural state after being recovered from the soil. Whereas, active metals require more energy to be able to use in a convenient form. This is a significant corrosion concept that is frequently encountered in the engineering field. To give an example, consider a positive metal such as platinum in which will be connected with a negative metal such as Magnesium. Electron reaction will start from negative metal (due to having higher energy) to active. As it can be seen in galvanic table above, negative metals tend to become more anode than positive metals. In this situation, magnesium is an anode whilst platinum is a cathode. The corrosion rate of the chemical reaction also depends on the distance between anode and cathode metals. In this case, platinum is too far away from magnesium, hence faster corrosion will be occurred. This rate also depends on the size of the surface area. When this ratio is combined with appropriate conditions, the rate of galvanic corrosion between two metals can be determined. For example, the rate of small anodes against large cathodes will be higher. Hence, corrosion is considered minimal until the anode area exceeds the cathode area. As a result, a small ratio of anode/cathode will cause more deterioration of the anode, therefore small places are being affected by this corrosion such as sharp points and edges of structures. [6] 32 of seawater on a regular basis, owing to varying water levels caused by tidal movement. These areas can be classified separately and requirements must be known properly before Cathodic Design. These three-part can be classified as Athmosperic Zone, Splash Zone ad Submerged Zone. 1.6.1. Atmospheric Zone The atmospheric zone is the above part of the structure and this part is neither wetted nor impacted by the ascent of tidal waves. As it’s not interacted with the sea, this zone does not include electrolytes. To be able to prevent corrosion, a convenient coating can be considered. In other words, as an electrolyte does not interact with this zone cathodic design is not required. The structure's design aims to keep the exposed steel surface area in this zone to a minimum. To be able to minimize the exposed steel surface can be done by tubular members. Clean welds having good profiles that merge into the parent metal prevent any crevice type corrosions, and steel structures can be boxed in to achieve the same aim. Another way of building a structure with a reduced potential to corrode is replacing steel with corrosion-resistant materials and nonmetals whenever available. It should be noted that dissimilar metals are to be joined is not recommended while designing, however, providing a solution between joints can be a convenient way. This method eliminates the risk of damaging design features that tend to corrosion by their nature. 1.6.2. Splash Zone The area of an offshore structure that is periodically in and out of water owing to the impact of waves or tides is known as the splash zone. Waves, wind and daily tidal variations can an cause increase in corrosion on exposed metal surfaces by alternating soaking and drying. The height of the splash zone can be considered as the vertical distance between the upper part and lower part based on its high and low tide. According to Det Norske Veritas, the astronomical tidal range plus a wave height with a 0.01 chance of exceeding it. The top limit of the splash zone is calculated by assuming that 65 percent of the wave height is above the highest astronomical tide (HAT), and the lower limit is calculated by assuming that 35 percent of the wave height is below the lowest astronomical tide (LAT). [11] Splash zone can be considered as the parts such as pipeline field joints and riser systems. As the sea level varies constantly, cathodic protection is not a convenient way of preventing corrosion for this place. Cathodic protection is used for the parts that are fully submerged. Paints and zinc coatings can be used to protect portions above the "splash zone" that are solely exposed to the atmosphere, but they must be reapplied as needed. Also, Thermal Sprayed Aluminum coating is widely specified for the protection of the splash zone. To be able to provide sufficient prevention metal must be isolated by coating and some materials can be suitable such as rubber or polyurethane. Also, the coating is to be designed must avoid the structure from electrolytic corrosion. The other requirements can be listed as having good thermal isolation, flexibility, impact resistance and bio-fouling resistant. 33 1.6.3. Submerged Zone The submerged zone is the part that is located completed into the seawater and below the splash zone. As the interaction between electrolyte environments, cathodic protection can be considered. To be able to protect this part, a well-designed cathodic design and high-performance coating system can be combined. As it does in the atmospheric zone, in order to reduce the risk of corrosion at the tight corners and crevices which are difficult to cover by using coating, tubular structures are preferable. From the design stress-reduction point of view, fatigue stress should be decreased and if necessary, the design should also relieve the tension exerted on welded members. All kinds of piles such as structure and skirt piles, as well as centralizers, must be considered to be a part of the Cathodic Protection system while designing. These members are welded to the jacket legs in order to connect, and their whole surface area must be taken into account while calculating the total polarization amount. The rest of the part must be welded conveniently in order to bound electrically through the structure to provide cathodic protection. The structures that are not welded can be taken into account as one structure with the rest of the structure after electrical bonding for calculating polarization current and determining anode mass and amount. Even if they are in the submerged zone, the part of the submerged system that closes to mudline has a very low corrosion rate compared to the above part due to the fact that non-oxygen environment or the turbulence interacted with steel, however, these parts must be included in the whole Cathodic Protection system as well. Concerning to chain members, chains are structural elements that span the splash and submerged zones, and they are frequently designed with double the corrosion allowance as the rate of corrosion. As explained in Splash Zone, Cathodic Protection is not a well-protected system for the splash part, whereas this part must include a high corrosion allowance. Hence, engineers should make every effort to maintain the chain's lie inside the effective radius range of the Cathodic Protection current, offering some protection to the chains. The protection of galvanized steel is not as same as chains, and its wire ropes are protected from water by a polyurethane coating loaded with grease on the outside. The galvanized wires are sufficiently protected from corrosion by this wrapping. A good wire rope design, on the other hand, will contain a sacrificial zinc wire as secondary protection within the rope composition. 1.7. Materials and Corrosion Behaviour of Materials Due to the risk of the offshore environment, materials used for the structures should be selected carefully. Although the accidents recorded in the oil and gas industry is not critically high, materials degradation could lead to a costly and dangerous situation with serious consequences for human life and the environment. Crystal structures of the materials are distinct features for each material which can be described by its unite cell. This cell consists of a body in which atoms are set up. There are three types of body that is observed in general; the body-centered cubic, face-centered cubic and hexagonal-close packed cubic. 34 Figure 10.1 Body-Centered Cubic Figure 10.2 Face-Centered Cubic Figure 10.3 Hexagonal – Close Packed Cubic Although structure crystals of each metal are presented in the same condition, some of them can be changed based on their environment. For instance, titanium has a Hexagonal – Close Packed Cubic form in general but its structure crystal can be oriented as Body – Centered Cubic form in the environment where the temperature is higher than room temperature. This situation is called allotropes. Structure crystals of metals are bonded to each other in different ways, called grains, and this connection of grains are known as grain boundaries. The acting of the metals against corrosion is highly related to these grain boundaries and a high amount of grain boundary decreases 35 the corrosion resistance of a metal. In order to increase corrosion resistance, other elements can be oriented with pure metals and this interactionis called alloy solution. Before metal and its alloys are decided, their structure crystals, mechanical features and phase diagram should be investigated. Metals can be classified as it can be seen below in Table.3 Body-Centered Cubic Chromium, iron, vanadium, molybdenum Face-Centered Cubic Silver, aluminum, copper, gold, nickel Hexagonal–Close Packed Cubic Titanium, zinc, magnesium, cobalt Table 3. Classification of metals in terms of Structure Crystal Form Some of the metals shown above are suitable for the offshore environment but the addition of alloy may be required for resistance. These are also not only suitable for up-stream, mid and downstream. Most common materials can be listed as Stainless Steel, Carbon Steel, Cast irons and Alloy steel, Also Copper Alloys, Nickel Alloys and Titanium Alloys are known as corrosion-resistant alloys (CRA). CRAs are generally applied for the places where the corrosion rate is high. 1.7.1. Stainless Steel As it can be noted by its name, stainless steel is a combination of 2 metals in order to provide more resistance. The first metal of stainless steel is iron, exposed to corrosion when its interacted with seawater. In order to provide corrosion resistance, chromium is added as second metal. Although stainless steel has built-in corrosion resistance, it can and will be corroded under certain conditions. The rate of its corrosion resistance depends on the amount of chromium present. The minimum limit amount of chromium that should be added to iron is 10.5 percent. Also, nickel and molybdenum can be introduced into it to increase mechanical resistance. This chromium interacts fast with the oxygen in the air, forming a thin oxide coating on the surface of the steel. As a result, it serves as a protective barrier. The chromium oxide acts as a passive coating, keeping the iron in the alloy safe from the environment's air and water. Thus corrosion resistance of stainless is provided. High maintenance is not required for stainless steel and it’s one of the most common materials around the offshore industry due to its low maintenance and resistance to oxidation. Austenitic, ferritic, martensitic, and duplex stainless steels are the four main varieties of stainless steel. Austenitic stainless steel is the most common in the industry, accounting for more than 70% of total stainless steel production. It includes maximum of 0.15% carbon and at least 16% chromium which makes it very strong against corrosion. Based on their strength, ferritic can be listed as second, rather than martensitic. Also, concerning to pitting or localized corrosion, duplex stainless steel can be selected to achieve high corrosion resistance. Apart from these varieties, there are also some components that may be observed. (Table 4) [16] 36 Table 4.Other components in Stainless Stells [16] 1.7.2. Carbon Steel Carbon Steel is also frequently used in Offshore Industry, especially in Oil and Gas Industry, because of its availability, convenience and low price. However, as structure are not well protected because of its inefficient corrosion resistance, there is a limit of applying Carbon steel. For more information, its basically suitable for the corrosion where happens in pipe due to producing oil and gas, but by the addition of sand corrosion, resistance can not be efficient. [17] The main metal of carbon steel is also iron and concerning to crystal structure, iron is a Body- Centered Cubic. The amount of carbon added to iron is 2.5%. In order to provide efficient resistance, some components can be selected based on the phase of the corrosive area. These are Ferrite, Cementite, Pearlite, Martensite, Austenite and Bainite. The most common carbon steel is Ferrite. As Ferrite is easy to deform due to its low amount of carbon, some other alloys can be added such as silicon. Cementite and Martensite are preferable for hard steel such as dual-phase steel, therefore not preferable for low carbon steels. Pearlite and Bainite are combinations of ferrite and cementite but generally, Pearlite is desirable. And finally, austenite is not suitable with every steel but low carbon steels and dual-phase steels. For more information on the type of Carbon Steel, Table 4 is shown below. 37 Table 5. Types of Carbon Steel [16] 1.7.3. Cast Irons Cast iron is the combination of iron, silicon and carbon alloys with greater than 2% carbon content [18]. As cast irons are highly fluid, its commonly useable to unite the materials. Based on tensile stress and hardness, it can be classified into malleable, gray, ductile and white. If Cast Iron contains a sufficient amount of alloy, corrosion resistance can be as much as Stainless Steel has. Silicon, copper, nickel or molybdenum can be added in order to provide this corrosion resistance. Table 6. Types of Cast Irons [16] 1.7.4. Alloy Steels Alloy steels is the steels that interacted with some elements in order to increase the mechanical features, such as corrosion resistance, hardenability and strength. The amount of these alloys can be changed between 1% to 50% in accordance with steel’s requirement. Based on this requirement, 38 alloys steel can be defined into two groups; low alloy and high alloy steels. In the offshore industry, alloy steels are defined as low alloy steels. According to Smith and Hashemi, the low alloy limit is 4%, on the other hand, Degarmo defines it as 8%. [19] Previous materials defined above also include alloy materials but it should not be considered that those are also alloy steels. In order to be defined as alloy steel, steel should be alloyed with molybdenum, silicon, chromium, nickel, boron and vanadium. The most common alloying elements and their effects on steel are shown in Table 6. [16] Table 7. Alloying Elements and Their Effects [16] 39 Chapter 2 CATHODIC PROTECTION 2.1. Principle of Cathodic Protection Corrosion was implied at the previous sections as a reactions consisting of two sides in which electrons are gathered in cathodic side and given off in anodic side. Before referring to Cathodic Protection, cathodic and anodic side of corrosion must be defined in detail. To begin with, a interaction between iron and aqueous environment leads to a reaction. As a result of this chemical or electrochemical reaction between iron and aqueous environment, equation 4.1. occurs. 2𝐹𝑒 + 𝑂2+ 𝐻2𝑂 → 2𝐹𝑒(𝑂𝐻)2 (4.1.) Due to oxidation, this output (2𝐹𝑒(𝑂𝐻)2) then turns into magnetite (𝐹𝑒3𝑂4) or FeOOH (hydrated ferric oxide), which means it’s corroded. This is the general corrosion reaction of iron which leads to an electron transfer process that is a charged metal ion is formed while an uncharged metal atom loses electrons as shown separately in Equation 4.2. and 4.3. 2𝐹𝑒 → 2𝐹𝑒2+ + 4𝑒− ( 4.2.) 𝑂2+ 2𝐻2𝑂 + 4𝑒− → 4𝑂𝐻− (4.3.) Positively charged ferrous ions have a tendency to dissolve in electrolyte solutions, thus electron gathers at the end of the metal as the result of a certain electric potential difference. As a result, an oxidation reaction occurs which is also known as an anodic reaction as Equation 4.2. and this end place of the metal is the anodic area. 40 In addition, electrons interact with hydrogen ions and hence, hydrogen is formed as it can be seen in Equation 4.3. This is known as cathodic reaction and this end place of the solution is the cathodic area. As a result, electrons that occurred in the anodic reaction[2] are employed in the cathodic reaction[3] and there is no deficiency in terms of electrons availability (If both cathodic and anodic sides work similarly). Thus metal becomes its electrode potential, which is also known as corrosion potential (𝐸𝑐𝑜𝑟𝑟). Figure 8 shows the relationship between anodic and cathodic reactions and how the electrons released from the anodic reaction are consumed in a cathodic reaction. Figure 11. Basic corrosion process that electrons released in Anodic Reaction are taken by Cathodic Reaction and leads to a metal consumption. [20] It can be easily noted what might happen if this reaction happens in terms of the anodic side and cathodic side. For more information, as electrons are taken from the metallic surface, it can be expected that Equation 4.2. would be faster in order to change the lost electrons. Whereas, Equation 4.3. would be slower due to the deficiency of electrons. As a result amount of metal consumption would be higher. Hence, in order to keep electrons on a metallic surface, additional electrons should be used and thus, the anodic reaction can be controlled. As anodic reactions are being controlled, the cathodic reaction will be higher in order to consume the electrons. As a result metal consumption would be slower. This technique is known as Cathodic Protection. Figure 8 shows the consumption of additional electrons rather than the electrons released from an anodic reaction. By this solution, the cathodic reaction would be able to get its required electron (2 electrons) without using an anodic reaction in order to achieve its partial cathodic protection. Also, it can be noted in Figure 9 that by getting 2 electrons from the external source, one of the anodic reactions that occurred in Figure 8 is prevented. 41 Figure 12. Partial Cathodic Protection in which 2 electrons are taken from an external source rather than iron atoms.[20] As a result, in order to achieve full cathodic protection, the surface should be purified from 𝑂𝐻−which means 4 electrons released from external source is required. Figure 10 shows the fully protected surface where the accumulation of 𝑂𝐻− does not exist due to control of anodic reaction. Figure 13. Fully protected metallic surface by cathodic protection [20] When an immersed metal and solution starts interacting, there will be a phase where the energy of the ion is larger through smaller from either direction. However, only the cations with charged positively will be able to pass into the solution, which means negatively charged anions can not pass. Hence, there will be an accumulation of positive ions. Equilibrium is the phase when chemical driving force (L) equals the electrical force of the reaction and the potential differences between metal and the solution is known as “equilibrium potential difference”. [22] 48 Figure 18.2. Stand off anode [30] Stand off shaped anodes are commonly suitable for large anodes such as subsea templates. This type of anodes places the anode in a steel sled and secures it to the steel structure with a specific clamp. This method is simple to set up and less expensive to retrofit an existing structure. Bracelet anodes were once largely utilized for pipelines, but they are now found on upper zone of platform legs, where they offer a high current-output-to-weight ratio while reducing drag. Anode shape can be selected during the theoretical stage according to forces applied during the installation, during the pile installation, or wave effects. Stand off type anodes may be considered more carefully compared to other anode types, in order to get more efficiency. Inside of anode design must be fit for anode weights and against the forces that may take place during the lifespan such as wave or storm damages, materials, or forces. Concerning to material selection, BS4360 grade 40A, 43A or 50C, or API 5L grades B, X42, or X52 can be utilized. As well as, NACE standarts must be followed and must meet the minimum limit S BS1706 [30]. 2.2.2. Impressed Current Cathodic Protection Unlike sacrificial anode systems where current is driven by the total potential difference between anode material and structure, the impressed current system ( ICCP) produces current by means of its own external source. During the lifespan of the CP, the electrical current output produced by the external source is adjusted in order to achieve and sustain an efficient potential level for protection over the structure to be applied. This system is commonly employed for the structures in which require high power demands, such as water storage tanks, or for the places are to be different 49 current requirements. For this applications in which changeable conditions lead to a changing in current density, automatic potential control rectifiers is preferable in order to sustain adequate potential. The requirements of ICCP can be listed as [31] ; - DC Power Source - External - Circuit, connections, current cables - System for monitoring - Dielectric cover where is placed between cathode and anode in order to increase current distribution. - Structure to be applied - Reference electrodes The most popular ICCP systems anodes are high silicon-cast iron, magnetite, graphite and platinized materials such as titanium or niobium. The current of ICCP system anodes can be up to 100 V and high current densities can be obtained. The benefit of this high current is protecting larger areas from a single anode compared to SACP and being able to control remotely due to an adequate amount of voltage. Table 8 shows the properties of impressed current anodes. Table 9. Properties of Impressed Current Anodes 2.3. Coatings The intention of coating is to regulate an electrolytic pathway by putting a barrier between the applied metallic surface and the corrosive solution. If all the metallic surfaces can be well-coated with a substance that is completely waterproof and free of defects, all attacks from outside could be prevented. However, unfortunately, none of the coating and meticulous applications will guarantee an endlessly perfect coating. The error of coating starts with small flaws and increases by time. Table 10 shows the failure of coatings on offshore structures by the time. 50 Table 10. Coating degradations of Offshore Structures. [33] Concerning to coated and uncoated structure, it can be predicted that coated structure have fewer leaks over its lifespan but the first leak can be observed in coated structure due to the corrosion activation oriented from protected area through unprotected area. Furthermore, to be able to prevent this leak, a replacement will be required for this area. A new metal may have a tendency to become active metal (anodic) in terms of corrosive environment and coated structure may even have a worse situation by increasing of corrosion rate. In order to avoid this case, if complete cathodic protection will not be employed with coating, at least, limited cathodic protection installations with sacrificial anodes, often known as "hot spot" protection, can be a cost-effective alternative in this case. For the areas affected by stray current, it is crucial to apply an effective coating to the line in the part of the pickup current in order to boost resistance and decrease the total current that will lead to the structure's metal consumption when it discharges somewhere else. In this case, defining of current pickup is comparatively easy. The effect of coating on cathodic protection can be easily observed in terms of the current required for protection. The decrease might be as high as 99.8% for a very good coating to as low as 50% for a severely bad, old, flawed coating [34]. To be able to obtain efficient protection, material selection is also important for decreasing. 2.3.1. Coating Types Coatings generally contain three components; solvent, binder and pigment. But it can be changed in some examples. For instance, a coating that includes 100% solids does not have a solvent component. By using these materials, three types of coating can be obtained; 51 2.3.1.1. Inhibitor Coating A protective barrier is placed to a metallic surface in the form of a solid, film, or fluid to eliminate corrosion. These barrier coatings have chemical or physical qualities that avoid external stimuli from causing corrosion reactivity and/or material breakdown. 2.3.1.2. Barrier Coating A barrier coating creates an insulating and physical barrier, preventing corrosive materials, such as the electrolyte, from coming into contact with the substrate. 2.3.1.3. Sacrificial Coating As applied in Sacrificial CP, sacrificial coatings are a type of selfless coating made of a metal, typically zinc, that corrodes more quickly than steel. In essence, this approach hijacks the corrosion process and directs it in a non-harmful direction for the asset the coating is supposed to preserve. It should be noted that some types of materials used in coating applications are no longer available due to some significant reasons. For instance, chromate-based and coal tar anamel are no longer useable due to environmental risk and health-based problems. These materials are also more effective than other materials, hence, the current coating is not able to provide a better lifespan as it used to be. Therefore, cathodic protection takes place a significant role while applying with coatings. In addition, cathodic protection is not relatively useable for the structure regions where a high flow rate occurs. Therefore, the need for cathodic protection should be evaluated based on its location. 2.3.2. Coating Selection Coating applications can be selected in terms of exposure status or environmental risks. On the other hand, having a variety of coating products to supply by manufacturers results in an accessible market. For the narrow or limited regions, brushable or rollable products are preferable over traditional spray or airless spray solutions. The use of coating on pipeline or flat structure surfaces can be applied faster but some additional materials are required. General considerations while selecting coating are; In case of atmospheric exposure; Alkyd-based materials or waterborne acrylics can be selected for good condition. For the best protection, zinc-based primer, polyurethane topcoat or galvanizing can be selected. In case of submerged regions; Epoxy, urethanes, polysiloxane or vinyl ester (restricted by Environmental Protection Agency’s (EPA)) can be employed for efficient protection. 52 In case of buried exposure AWWA C222 Polyurethane would be the best solution. Also, fusion bonded epoxy can be applied. For a general coating selection, surface tolerant epoxy or moisture-cured urethane can be applied. This selection would provide efficient protection by sticking the edge of the flaw region. 2.3.3. Difficult regions to be coated Unmaintained regions such as nailed connections, crevices, clinged structures or back-to-back plates might be faced with coating breakdown sooner. Although variety of coating types exist, most of them can be cracked easily as being crosslinked. Flexible caulking can be utilized to assist coating material but frequent maintenance might be required [35]. 2.4. Combination of Coating and Cathodic Protection - As mentioned previously, coating highly decreases the current demand for cathodic protection, hence also decreases the needed anode weight. Structures with weightsensitive and long lifespans may lead to high costs during the corrosion process. In order to absorb a high amount of current demand and also stray current CP should be combined with coatings. - Coating is also should be applied for the bare metal regions of the structures in which is expected to be high current. This is more relatively for deep-water applications where calcareous deposits may take a long time to build. - For complicated and large systems such as multi-well oil&gas production systems, the coating should be applied extensively in order to control long-term current demand and provide an efficient current distribution. - Coating may not be compitable for the immersed structure regions due to need of highly review for the fatigue cracks such as critical welded points of an immersed structure. - Although metalic coating is suitable for the aluminum or zinc-based materials by applying for sacrificial cathodic protection, it’s not as suitable as organic coatings in terms of controlling the current demand of CP. Hence, zinc-rich materials are considered compitable for the combination of coating and CP due to either the way of its cathodic disownment or insufficient electrical resistivity, which results in high cathodic protection current demand. 53 2.5. COMPARISON OF ICCP SYSTEMS AND SACRIFICIAL ANODE SYSTEM Use of Sacrificial Anodes Method or Impressed Current Method can be classified as it seem detaily in Table 11. Comparison SACP ICCP Table 11. Comparison between SACP and ICCP 54 CHAPTER 3 3. DESIGN CALCULATIONS AND PROCEDURES OF CATHODIC PROTECTION 3.1. General If the area to be protected is large complex to calculate, the system can be subdivided based on zones or such as buried and submerged zones and detailed design should be maintained for each zone. After dividing each zones, anode types and relevant devices should be planned in accordance with forces applied on installed anodes during the operation. Furthermore, the coating to be selected should also be planned by following the coating categories, allowing for prior calculation of current demand by using the current densities and related total anode net mass needed for CP. 3.2. Design Calculations 3.2.1. Surface Area Calculation Each zone should be measured separately without coating systems and also if any part of the system was affected by any condition (e.g. temperature), this part should also be measured separately, otherwise current demand will be a false result. 3.2.2. Current Demand In order to obtain efficient polarizing capacity for the system and also provide adequate cathodic protection throughout its lifespan, current demand should be calculated for each zone’s surface area by using the current densities (initial, mean and final) and coating breakdown factor. Current demand can be calculated by using the formula shown below; 𝐼𝑐= 𝐴𝑐∗ 𝑖𝑐∗ 𝑓 𝑐 (10.3.1.) 55 Where; 𝐼𝑐 : Current Demand (A) 𝐴𝑐 : Surface Area to be protected (A/𝑚2) 𝑓 𝑐 : Coating breakdown factor 𝑖𝑐 : Current density The coating breakdown factor for uncoated systems is assumed to be 1, which means there is no insulation by coating. This factor is explained detailly in the coating breakdown factor part. The other way of finding the total current requirement, also for uncoated systems, it can be estimated by using Table 12; Table 12. Current requirements for uncoated systems 3.2.3. ANODE MASS CALCULATION After determining of current demand and anode selection, total anode mass calculation would be possible to obtain. In order to obtain total anode mass, (𝑀𝑎), to be needed for lifespan, the formula is used as follows; 56 Where; 𝐼𝑐𝑚 : Current demand with mean current density 𝑡𝑓: Design life u: Anode utilization factor 𝜖 : Electrochemical capacity of design 3.2.4. ANODE NUMBER CALCULATION Based on the anode selection, total anode number (N), the mass of anode (𝑀𝑎) and anode dimension should be obtained in order to meet the conditions for initial and final current (𝐼𝑐𝑖 and 𝐼𝑐𝑓) outputs and also anode current capacity (𝐶𝑎). Concerning to initial and final current outputs, individual current output (𝐼𝑎) is measured by means of Ohm’s Law. Where; ∈𝑎°: Circuit design potential of anode selected (V) 𝑅𝑎 : Resistance of anode (Ohm) 𝐼𝑎 : Individual current output (are to be calculated for initial and final current separately) ∈𝑐°: Potential of protective design Concerning to anode current capacity, the formula is; 𝐶𝑎 = 𝑀𝑎*𝜀* u Where; 𝑀𝑎 : Total anode mass 57 u: Anode utilization factor 𝜖 : Electrochemical capacity of design In order to make sure whether the calculation is correct or not, following formula can be used; Where; 𝐶𝑎𝑡𝑜𝑡 : Total amount of anode current capacity 𝐼𝑐𝑓,𝐼𝑐𝑚, 𝐼𝑐𝑖 : Current demands based on each current densities 𝐼𝑎𝑖 𝑎𝑛𝑑 𝐼𝑎𝑓 : Individual current outputs for initial and final current densities 3.2.5. CALCULATIONS OF ANODE RESISTANCE Anode resistance, 𝑅𝑎 (ohm), is calculated based on anode type as it can be seen in Table 13. While using these formulas, specific environmental parameters are required. (e.g. salinity,temperature,sediment factors etc.) Table 13. Anode resistance formulas for each anode type [37]. 64 fractional testing for an anode, prior and the next 3 anodes (minimum) must be tested individually to ensure that testing for the following anodes is suitable [37]. 4.2. MAINTENANCE and OPERATIONS After the installation of CP system, some certain operations are followed in order to prevent current or next failure. The failure that occurred in the CP system is not always visible or solvable remotely. For instance, if there is a potential fall on the pipeline system through the soil, corrosion damages the pipeline slowly and out of sight (except special equipment to provide visibility). Furthermore, no one can notice this failure until a leak takes place and when it’s realized it may be too late for the system concerned in terms of lifespan. As in the example of pipeline potential fall to the soil, there are other failure signals based on offshore structures concerned. These failures may pay more attention to the maintenance workers during the operation applying regularly and workers come up with a solution for the system before it’s too late. This maintenance should be guided by operators or manufacturers. Some common failures for SACP and ICCP systems are mentioned below. 4.2.1. Rectifier Ground-Bed Transformer Failure in ICCP It should be noted that this failure can be seen in any part of the system although that area is being protected. In ICCP applications, the following components of the system should be taken into account in order to prevent failures [38]. - The power supply - Cable connections in the whole system; to prevent low connection and provide more protection. - Complete rectifier components such as circuit breaker, transformer, or stacks. - The ground bed of the system; anodes may have a problem for any reason which leads to an increase of total resistance. Thus a change may occur in soil content. - Coating; breakdown may occur in the coating over time and results in an increase of system demand. 4.2.2. Sacrificial Anode System Failures As sacrificial anode systems include various drainage points, there may be some failures in small regions of the system. Hence, it should be noted that even small regions must be controlled by operators to ensure that the whole network is running properly. In SACP applications, the following topics should be taken into account in order to prevent failures. 65 - Mechanical damage control to the connections. - Dry soil may affect the current output negatively, thus a failure may occur in the structure or anodes. - As in ICCP failure, coating breakdown may also result in an increase in system demand for the SACP system. This failure mostly will be revealed by the failure of current output as in ICCP systems. Although this failure is not always visible, it can be under control if it is measured by means of a shunt or an ammeter can be installed [38]. 66 Chapter 5 Experimental work and analyses The main intention of this thesis is to explain the design of cathodic protection for the offshore structures and make design calculations for each coated and uncoated cathodic protection thus, providing a discussion in accordance with its anode size. Designing sacrificial for the external surface of a hypothetical construction to be placed in 30 meters of water off the coast of the Canary Islands is a recommended practice. The reason for selecting the Canary Islands is the Spanish Wind Energy Association, Asociación Empresarial Eólica (AEE), which aims at least 3 GW of offshore wind turbines that can be built in Spain by 2030 and the most considered place is the Canary Islands. These calculations will be measured based on DNV RP B401 recommendations as applied in the previous sections. The flow of the design calculations is as follows in Figure 16. Figure 19. The flow of design calculation [45] Monopile foundations are the most often utilized wind turbine foundation due to their ease of construction compared to other foundation types. Although most of the offshore wind turbines are 67 anchored to the seafloor up to 50-meter depth (except floating wind turbines which is connected to the sea bed with mooring lines), 40-meter and lower depths are the most convenient levels in terms of technical advantages and monopile foundation provides a better condition at this level. Hence, monopile foundation is decided for wind farm foundation concerned. Both internal and external sections of the monopile structures can be affected by corrosion. Concerning to external part, the coating should be applied for the splash and atmospheric zones whereas CP is applied for the submerged zone of the wind turbine as mentioned in previous sections. The internal part of the system also interacts with corrosion and corrosion control should also take into account. In order to prevent, if the internal part is confined from the air entrance corrosion control can be achieved however, prevention of entire amount of air is impossible for these systems, hence, CP or a coating system may provide a better manner for prevention. According to previous experiences, the use of SACP for internal protection increases the acid level of the water concerned [39]. Furthermore, when SACP is implemented for the internal part, an important change in hydrogen level is not observed except increasing of hydrogen sulfide level [40]. For maintenance, changing of 5% water from J-Tube parts is compulsory every day [41]. As internal cathodic protection would be costly and can’t be monitored well due to the restricted area of the internal surface, a coating may not be employed. For this experiment, internal parts have been left uncoated. Figure 20. Internal J Tubes for daily seawater changing [45] 68 For the external part, it has been noted that a high amount of anode needed for protection interacts with each other which results in protection for the submerged part since anodes are being stacked. Hence instead of using a high amount of anode, coating is the alternative way to provide protection as the current demand is reduced. For anode type selection, stand – off anode can be employed. Based on coating quality which is categorized by DNV B401 recommendation, up to 80% insulation can be achieved by using Category 3 coating for stand – off anode aluminum anode mass [42]. Flash mounted anode will also be applied in order to classify the difference between stand-off anode and flash mounted. As common standards will be followed, both anode shapes will be considered to be 100 kg weight [30]. Calculation Procedure of DNV B401 In order to follow the flow of the Sacrificial Anode calculations surface area of the external part, environmental parameters, current demand, anode mass, steel type, total current output and anode resistance should be obtained (Figure 17). Structural and Environmental Parameters Related parameters for the monopiles are; Outer diameter: 8 m Wall thickness: 120 mm Total length: 90.5 m ( 50 m buried zone, 40 m column of seawater, 0.5 m mean water line (MWL)) A transition piece (TP) connects the monopile part to the upper part. This piece starts from below sea level and stretches through the intertidal and splash zone as it can be seen in Figure 18. For design calculations, this part can be neglected. 69 Figure 21. Zones of Monopile Foundation The structure will be located 20 km away from the Southeast of the Gran Canaria Island’s coast. According to Puertos del Estado, a Spanish government’s port agency, water temperature for the bottom part ranges from 15 to 25 degrees [44]. The other seawater parameters are salinity and dissolved oxygen of approximately 34,32 and 5,63 mg/L [44]. The Sedimental current of the southeast part of Canary Island is 30-40 cm 𝑠−1 [43]. Finally, the average wave height is 1.25 to 2.7 meters [44]. In general, a modern wind turbine of acceptable quality will typically last 20 years, however, this can be extended to 25 years or beyond depending on environmental circumstances and proper maintenance practices. However, as the structure ages, the maintenance expenses will rise. In this lifespan, as tidal and splash zones are exposed to coverence of the transition piece, severe corrosion rates occur due to occasionally drying and wetting conditions and oxygen concentration. If cathodic protection is applied for this zone, it will be inefficient due to deficiency of submerged seawater, hence, the coating is utilized for this region. Barrier coating will be designed for this region and it also meets the design life of the structure by lasting about 20 years. Calculations and Results Calculations of Surface Area : To begin with, the surface area of the external part which is consists of buried, submerged and splash zones was measured first. In order to obtain the CP current demand, the steel surface area to be protected was multiplied by the initial, mean and current densities needed to accomplish the 70 polarization and keep the potential more negative value than -0.800 V based on silver/silver chloride electrode. As the coating breakdown factor takes into account the coated places, current demand is minimized. Concerning to anode mass needed for the whole design lifespan, mean current density is employed. On the other hand, the initial current density is employed to stimulate quick calcareous deposit formation which will get minimized the system current demand over its anticipated lifespan. And finally, the final current density is employed when the calcareous part and connected fouling are partially removed by means of waves or other conditions. To sum up, all densities are required in order to obtain CP’s current demand [45]. As temperature varies between 15 to 25 degrees, subtropical conditions of current densities for seawater exposed bare metal surfaces are used (Table 16). Table 17. Current densities based on Canary Island conditions. Zone Length (m) Surface Area (𝒎𝟐) Mean Water Line 0,5 113,098 Submerged 40 1105,84 Buried 50 1357,17 Table 18. Calculations of Surface Area to be protected In order to obtain current demand, the formula is used as follows; 𝐼𝑐= 𝐴𝑐∗ 𝑖𝑐∗ 𝑓 𝑐 Surface areas (𝐴𝑐) are found in table 18. Also, the suggested current densities for the subtropical environment are provided in table 17. As design current densities are dependent on regional depth and temperature, each region will be found separately. For the buried region, the current density is 0.020 A/𝑚2[37]. The use of coating decreases the current demand. This reduction depends on the category of coating and DNV – RP – 401 guidance will be followed in this calculation. According to DNV, the categories are; Sub-Tropical (12-20°C) Depth (m) Initial Mean Final 0-30 m 0,170 0,080 0,110 30-100 m 0,140 0,070 0,090 71 Category 1: Primer coat which is 50 μm nominal DFT (dry film thickness). Category 2: Primer coat and one layer of coating for top, 150–250 μm nominal DFT. Category 3: Primer coat and two layers of coating for top, 300 μm nominal DFT. Category 4: Primer coat and three layers of coating for top, 450 μm nominal DFT. For the uncoated regions, the coating breakdown factor is assumed to be 1. For coated regions, 𝑘1 and 𝑘2 values stated in Table 16 are employed separately for each initial, mean and final part. And finally, values are calculated by the formulas below; 𝑓𝐶 (initial) = 𝑘1+ 𝑘2∗ 𝑡 𝑓𝐶(𝑚𝑒𝑎𝑛) = 𝑘1+ 𝑘2∗ 𝑡/2 𝑓𝐶 (final) = 𝑘1+ 𝑘2∗ 𝑡 The results of each category for a 25-year design lifespan are shown in table 19. As the coating breakdown factor can’t be greater than 1, the values greater than 1 were shown as 1. After obtaining each coating breakdown factor, current demand is obtained as it seen in Table 20 and the total current demand for CP can be found by summing up each zone’s result (Table 21). Depth (m) Coating Breakdowns Uncoated Category 1 Category 2 Category 3 0 – 30 m Initial 1 1 0,8 0,395 Mean 1 1 0,425 0,2075 Final 1 1 0,8 0,395 30+ m Inıtial 1 1 0,55 0,32 Mean 1 0,725 0,3 0,17 Final 1 1 0,55 0,32 Table 19. Results of each Coating Breakdown Factor categorized According to results in Table 19, Category I has the lowest reduction compared to Category II and Category III. It must be noted that Category II and III provide a better convenience in terms of current demand. Current demand results for each zones are provided in Table 20 by using the coating breakdown factor. As the inputs to be used for calculation will be different at 30 meters and more depths, calculations for the submerged zone is divided into 2 calculation. 72 Depth (m) Zone Uncoated Cat I Cat II Cat III 0-0,5 MWL Initial 19,22 19,22 15,38 7,59 Mean 90,47 90,47 38,45 18,77 Final 12,44 12,44 9,95 4,91 0,5-30 Submerged Initial 145,27 145,27 116,21 57,38 Mean 683,60 683,60 290,53 141,85 Final 94,00 94,00 75,20 37,12 30-40,5 Submerged Initial 49,14 49,14 27,09 15,76 Mean 24,62 18,85 7,38 4,18 Final 31,66 31,66 17,41 10,13 40,5-90,5 Buried Initial 190,00 190,00 104,50 60,80 Mean 95,00 68,87 28,50 16,15 Final 122,14 122,14 67,18 39,08 Table 20. Current Demand results for each zone Totals Uncoated Cat I Cat II Cat III Initial 403,63 403,63 263,18 141,53 Mean 893,69 861,79 364,86 180,95 Final 260,24 260,24 169,74 91,24 Table 21. Total Current Demands Mass of Anode Calculation As it stated before, anode mass is calculated by the formula below; 73 Where; 𝐼𝑐𝑚 : Current demand with mean current density 𝑡𝑓: Design life u: Anode utilization factor 𝜖: Electrochemical capacity of design Current demand with mean current demand and design lifespan parameters are already known. 8760 is the total hours of an entire year. The reason why mean current demand is employed in anode mass formula is final and initial current demands do not stand in a constant value. Concerning to anode type, aluminum was selected due to its economic aspect and electrochemical efficiency of having less weight requirement compared to zinc or magnesium. However, these factors shouldn’t be the only reasons for anode selection. For instance, stand off aluminum anode may provide a suitable condition in terms of weight or electrochemical efficiency but these conditions may also affect the wave loading of the structure in a negative manner throughout its design lifespan. The utilization factor of stand off and flush mounted anodes are 0.90 and 0.85 as it can be seen in Table 15 with the DNV recommendations. According to DNV recommendation in Annex A, the electrochemical capacity of design, 𝜖, recommended value is dependent on zone to be calculated and these values are preferable up to 30° average yearly degrees. Based on this recommendation, the Aluminum based electrochemical capacity for seawater is 2000 Ah/kg and for the sediment zone is 1500 Ah/kg [37]. The result of anode mass calculations are provided in Table 22 below; Uncoated Cat I Cat II Cat III Stand-off 108732,2 104851,1 44391,3 22015,5 Flush mounted 115128,3 111018,8 47002,5 23310,6 Table 22. Anode mass calculations 80 in Aluminum mobility [54]. Therefore, aluminum is not only a good selection in terms of its electrochemical capacity and low weight, it’s also would be a better selection in terms of less pollution compared to the zinc anode. While coastal waters generally have an aluminum concentration of 0.5–0.68 g/, zinc concentration is as high as 4 μg/L and more. The best locations to exploit the off-shore wind source in Canary Island, regarding to Martin Mederos et al. (2011), González et al. (2017), and Schallenberg-Rodrguez and Garca Montesdeoca (2018), are the area between Tenerife Island and the west-northwest coast side, as well as the south and southeast parts of the island. Concerning to permission, the implementation of offshore wind farms are supported by Asociación Empresarial Eólica (AEE) and a CP design for 4 assembled wind structure can be considered in this experiment. If an uncoated structure that has 108 tonnes of anode mass based on DNV calculations is planned for per structure, the total amount of aluminum consumed in the system will be 532 tonnes for each structure. By using Coating III, it could be reduced to 88 tonnes. Conclusion Sacrificial cathodic protection design calculations of hypothetical offshore wind system located in Canary Island is obtained by means of DNV guidance. Relevant initial parameters (seawater parameters, initial mass, length, thickness, etc.) have been obtained from related offshore website sources and previous researches about CP design calculation. On this basis, it can be observed that initial parameters are required for designing cathodic protection of an offshore system and getting a valid result is available. The intention of these calculations is to determine the differences between coated and uncoated structure in terms of anode and mass requirement. According to the results, it’s obvious that the use of Coating II or Coating III would provide severe benefits in terms of current demand reduction, anode requirement and total mass of anode. This beneficial effect will minimize anode consumption and expense, as well as aluminum emissions, and will lead to a more suitable anode distribution in order to provide that Cathodic Protection is deployed across longer distances due to lower IR drop. As a result, corrosion risk can be lowered by using coating in combination with cathodic protection and design calculations prove this approach. Although the coating is quite an effective method, other factors should also be taken into account. For example, stand-off anode has a better result in the use of design calculation but considerations may be given in order to provide better resistance. Also concerning to environmental factors, materials that decrease the risks of the environment by means of applying corrosion inhibitors, changing the chemical reactions, avoiding sea pollution, shifting the temperature or velocity, etc. can be taken into account. Finally, one of the most important factors is anode distribution. Therefore, providing a better distribution and combining the different zones to reach every place is the major point of cathodic protection design. 81 References 1. Metallurgical Failure Analysis Techniques and Case Studies Chapter 9 – Corrosion, Kannadi Palankeezhe Balan 2. Corrosion Impact of Offshore Platforms, Structures, and Vessels By FranK Byron 3. Comprehensive Chemical Kinetics Volume 28, 1989, Pages 233-279 4. Atmospheric and Marine Corrosion: Influential Environmental Factors and Models 5. NACE International Basic Corrosion Course Handbook. Houston, TX: National Association of Corrosion Engineers, 2000. 6. Corrosion Protection Systems in Offshore Structures by Ivanov 7. Kennell, Glyn F.; Evitts, Richard W.; Heppner, Kevin L. (2008). "A critical crevice solution and IR drop crevice corrosion model". Corrosion Science. 50 (6): 1716– 1725. 8. "Different Types of Corrosion – Crevice Corrosion” www.corrosionclinic.com. Retrieved 2021-05-24. 9. Von Wolzlgenkuhr Cah and Van Der Vlugt LS; The Graphitisation of Cast Iron as an Electrochemical Process in Anaerobic Soils; Water 18; pp147-165 (1934); (Translation in Corrosion 17 pp293-299 (1961)). 10. D.A. Jones, Principles and Prevention of Corrosion, New Jersey: Prentice Hall, 1996. 11. S.A. Bradford, Corrosion Control, New York: Van Nostrand Reinhold, 1993. 12. Ramesh Singh, in Corrosion Control for Offshore Structures, 2014 13. Lye, Rolf E. "Splash Zone Protection: A Norwegian Operator's View." Paper presented at the CORROSION 2001, Houston, Texas, March 2001. 14. Desing of Cathodic Protection Using BEM for the components of the pilot ocean energy system, VDM Verlag Dr. Müller (2012) 15. L L Shreir Corrosion: Corrosion Control Pg: 2-4 16. Corrosion Control in the Oil and Gas Industry,Sankara Papavinasam, October 2013 17. Faisal Mutahhar, ... Kenneth P. Roberts, in Trends in Oil and Gas Corrosion Research and Technologies, 2017 18. Campbell, F.C. (2008). Elements of Metallurgy and Engineering Alloys Materials Park, Ohio: ASM International. p. 453. ISBN 978-0-87170-867-0 19. MATERIALS AND PROCESS IN MANUFACTURING - E. Paul DeGarmo, J T. Black Ronald A. Kohser, Pg 112 20. Principles of Cathodic Protection - V. Ashworth volume 2, pp 10:3–10:28,2010 21. Construction and Building Materials - P. Schiessl, Pg 391-402 22. Encyclopedia of Electrochemical Power Sources - S. Panero , November 2009 23. Cathodic protection and cathodic prevention – Pletro Pedeferri, 1996 24. C.A. Zaffe and C.E. Sims, Hydrogen, Flakes and Shatter cracks (1940) II(5) 145–151. 25. M. Szczepanski, The Brittleness of Steel, John Wiley & Sons, Inc. pp. 188. 26. S. Klisowski and W. H. Hartt, Quali®cation of Cathodic Protection for Corrosion Control of Pretensioned Tendons in Concrete, in `Corrosion of Reinforcement in Concrete Construction', edited by C. L. Page, P. B. Bamforth and J. W. Figgs (The Royal Society of Chemistry, Cambridge, 1996), pp. 354-68. 82 27. C. L. Page, Interfacial Eects on Electrochemical Protection Methods Applied to Steel in Chloride Containing Concrete, in `Rehabilitation of Concrete Structures', edited by D. W. S. Ho and F. Collins (RILEM/CCSIRO/ ACRA, Melbourne, 1992), pp. 179-87. 28. D.J. Eyres M.Sc., F.R.I.N.A., G.J. Bruce M.B.A, F.R.I.N.A., MSNAME., in Ship Construction (Seventh Edition), 2012 29. Branko N. Popov, Swaminatha P. Kumaraguru, in Handbook of Environmental Degradation of Materials (Second Edition), 2012 30. Mohamed A. El-Reedy Ph.D., in Offshore Structures, 2012 31. GUIDANCE NOTES ON CATHODIC PROTECTION OF OFFSHORE STRUCTURES, American Bureau of Shipping 32. T.M. Zhang and W.M. Zhao, J. Chin. Soci. Corros. Prot., 34 (2014) 315. 33. L.L. Sheir, R.A. Jarman, and G.T. Burstein; “Corrosion”, Volume 2: “Corrosion Control”, 3rd edition, Butterworth Heinemann, ISBN 0-7506-1077-8, PP 10.3 – 10.28 34. Corrosion Basics—An Introduction, Second Edition, Pierre R. Roberge, ed. (Houston, TX: NACE International, 2006), pp. 178-179. 35. Canal Operation and Maintenance Coatings and Cathodic Protection - U.S. Department of the Interior Bureau of Reclamation Office 36. YongBai QiangBai - Subsea Engineering Handbook (Second Edition) 2019, Pages 731-767 37. DNV - Recommended practice RP B401 Cathodic Protection Design 2010 38. Pipeline Corrosion and Cathodic Protection: A Practical Manual for Corrosion – Marshall Parker, Pages 125-129 39. Maher, M.M., Swain, G., 2019. Corrosion control and ecosystems enhancement for offshore monopiles. Mater. Perform. 58, 28–33. 40. Delwiche, A., Lydon, P., Tavares, I., 2017. Concerns over utilizing aluminium alloy anodes in sealed environments. NACE - International Corrosion Conference Series. 41. Delwiche, A., Tavares, I., 2017. Retrofit strategy using aluminium anodes for the internal sections of windturbine monopiles. NACE - International Corrosion ConferenceSeries. 42. Sarhadi, A., Abrahamsen, A.B., Stolpe, M., 2018. Optimal design of galvanic corrosion protection systems for offshore wind turbine support structures. Corrosion 74, 829–841 43. Variation of the tidal properties around Gran Canaria - Antonio MARTINEZ , Esther PEREZ, Miguel BRUNO. 44. Ministerio de Transportes Movilidad Y Agenda Urbana - https://www.puertos.es/en-us/oceanografia/Pages/portus.aspx 45. Conceptual Sacrificial Anode Cathodic Protection Design for offshore wind monopiles – Caglar Erdogan - Geoffrey Swain 46. Lichtenstein, L., 2015. DNV GL standard harmonization Recommended Practice on corrosion protection of offshore wind farms. Proc. Int. Offshore Polar Eng. Conf. 2015-Janua 659–663. 47. Optimising the location of anodes in cathodic protection systems to smooth potential distribution – E. Santana Diaz, R. Adey. 83 48. SIMULATION OF GALVANIC CORROSION USING BOUNDARY ELEMENT METHOD - Z Shamsu, A.A Mohammed, N.U Saidin, 2011 49. Ramesh Singh, in Corrosion Control for Offshore Structures, 2014 50. Wyatt, B.S., Preston, J., Jacob, W.R., Cathodic protection of offshore renewable energy infrastructure - Part 1. Inst. Corros. pages 19–24 - 2020. 51. Materials selection for XL wind turbine support structures: A corrosion-fatigue perspective – Victor Igwermezie, Ali Mehmanparast, 2018 52. Fatigue design of offshore steel monopile wind substructures - F. Brennan and I. Tavares, 2014 53. Cathodic protection by zinc sacrificial anodes: Impact on marine sedimentmetallic contamination - C. Rousseau, F.Baraud, L.Leleyter, O.Gil, 2009 54. The impact of aluminium sacrificial anodes on the marine environment: A case study C. Gabelle , F. Baraud , L. Biree , S. Gouali , H. Hamdoun , C. Rousseau , E. van Veen , L. Leleyter (2012) 55. https://www.corrosionclinic.com/types_of_corrosion/pitting_corrosion.htm 56. Comparative study on the effect of NaNO 2 in corrosion inhibition of micro-alloyed and API-5L X65 steels in E20 simulated FGE, Olufunmilayo Oluwabukola Joseph (2017)