Simultaneous in situ generation of hydrogen peroxide and Fenton reaction over Pd-Fe catalysts
Abstract
High mineralization degree of organic compounds can be achieved by a novel environmentally-friendly full heterogeneous Pd–Fe catalytic system, which involves in situ generation of hydrogen peroxide from formic acid and oxygen, and oxidation of organic compounds by Fenton process in a one-pot reaction.
Full text
This journal is cthe Owner Societies 2010 Phys. Chem. Chem. Phys., 2010, 12, 14673–14676 14673 Simultaneous in situ generation of hydrogen peroxide and Fenton reaction over Pd–Fe catalystsw Mohammad S. Yalfani, a Sandra Contreras,* a Jordi Llorca, b Montserrat Dominguez, b Jesus E. Sueiras a and Francesc Medina* a Received 13th July 2010, Accepted 17th September 2010 DOI: 10.1039/c0cp01157f High mineralization degree of organic compounds can be achieved by a novel environmentally-friendly full heterogeneous Pd–Fe catalytic system, which involves in situ generation of hydrogen peroxide from formic acid and oxygen, and oxidation of organic compounds by Fenton process in a one-pot reaction. The Fenton process is known as one of the most efficient advanced oxidation processes for the degradation of organic pollutants. 1 However, the overall performance of the process is influenced by its low mineralization capacity due to the formation of recalcitrant intermediates. 2 The conventional Fenton process (CFP) requires soluble ferrous ion and H 2 O 2 . Ferrous ion as a homogeneous catalyst requires further treatment due to the formation of sludge. H 2 O 2 is usually provided by bulk feeding, which does not yield high efficiency. Very recently, the Fenton process has shown good performance with catalytic in situ generated hydrogen peroxide. 3 In situ produced hydrogen peroxide can be consumed at an appreciable controlled rate prior to decomposition to H 2 O and O 2 , which leads to an improved performance of H 2 O 2 in the favorite reaction direction. 4 Here, we demonstrate for the first time that the Pd–Fe catalytic coupling is able to achieve a nearly total degree of mineralization for the Fenton reaction within a full heterogeneous catalytic system under very mild conditions. The catalytic system involves the simultaneous generation of hydrogen peroxide from formic acid and oxygen, the formation of hydroxyl radicals and the oxidation of organic compounds. Alumina-supported Pd–Fe catalysts were synthesized by two different procedures involving co- (denoted as Pd5FeCI) and successive impregnation (see experimental details in ESIw). The latter route was performed twice: in one case (denoted as Pd5Fe), palladium was deposited on alumina and then Fe impregnation was carried out, and in the other (denoted as FePd5), the Fe impregnation took place first and then the Pd was deposited. The Pd and Fe metal contents in the above three samples were 5 and 1 wt%, respectively. A monometallic Pd 5 wt%/g-Al 2 O 3 (denoted as Pd5Al) was also prepared as a reference catalyst. The palladium loading was chosen from the study of H 2 O 2 generation from formic acid and O 2 over alumina-supported Pd catalysts with different Pd loads. The results showed that the highest H 2 O 2 productivity at the initial time of the reaction which is more adequate for in situ applications was achieved using Pd5Al. 3,5 Our experiments indicate that this productivity was further enhanced in the presence of Fe (see Fig. 1 in ESIw). Phenol as a model pollutant was degraded by the Fenton reaction over Pd–Fe catalysts at ambient conditions using H 2 O 2 generated in situ from formic acid and O 2 . The results by the Pd–Fe catalysts are compared with the corresponding reaction using the Pd5Al catalyst in the presence of 10 ppm of Fe 2+ (homogeneous Fenton catalyst) and CFP using 300 ppm H 2 O 2 (the amount estimated to be produced in situ by formic acid and O 2 over Pd5Al within 6 h) 3 and 10 ppm of Fe 2+ (Table 1). The reaction rate coefficients (k obs ) for formic acid and phenol decompositions are calculated by fitting data to a pseudo-first-order kinetics during the first hour. Formic acid decomposition rates for all of the catalysts are within a very narrow range, which indicates that Fe does not interfere in formic acid decomposition by Pd. 6 Phenol degradation over the PdFeCI catalyst proceeds at a rate 2.4 times lower than with Pd5Al. The catalyst also shows lower mineralization activity. Although the Pd5Fe catalyst oxidizes phenol at a lower rate, its performance in mineralization is slightly better. However, the FePd5 catalyst competes with Pd5Al in phenol oxidation and shows outstanding pollutant compound mineralization ability, especially in comparison with CFP, which is unable to exceed 50%. 2c A higher H 2 O 2 feeding increases the rate at which phenol disappears, but it results in a lower degree of mineralization. 2b Over Pd5Al and Pd–Fe catalysts, formic acid is finished at 4 h, but the mineralization proceeds even in the absence of formic acid. This phenomenon can be attributed to the ability of the catalysts to mineralize intermediates. The stability of FePd5 was proved by adding 20 mM of formic acid as soon as the initial 40 mM was finished, i.e. at 4 h. Fig. 1a shows the phenol degradation profile of this reaction. This graph demonstrates that the second stage of the reaction proceeds at a rate similar to that of the initial phenol oxidation. This proves that the catalyst remains active after 4 h and that the system is capable of degrading even very low concentrations of pollutant. Most importantly, the achievement of a very high degree of mineralization suggests that such a system has the potential to completely remove all organic intermediates. FePd5 was the most appropriate Pd–Fe catalyst because no measurable leached Pd or Fe remained at the end of each run. Application of the later process was expanded for the degradation of 2,4-dichlorophenol (DCP, as representative of a Departament d’Enginyeria Quı´mica, Universitat Rovira i Virgili, Av. Paı¨sos Catalans, 26, 43007, Tarragona, Spain. E-mail: [email protected], [email protected]; Fax: +34 977559621; Tel: +34 977559680 b Institut de Te `cniques Energe `tiques i Centre de Recerca en Nanoenginyeria, Universitat Polite `cnica de Catalunya, Av. Diagonal, 647, 08028, Barcelona, Spain wElectronic supplementary information (ESI) available: Experimental details, H 2 O 2 generation graph, quantitative TPR data. See DOI: 10.1039/c0cp01157f COMMUNICATION www.rsc.org/pccp |Physical Chemistry Chemical Physics Downloaded by Universitat Politecnica de Catalunya on 28 December 2010 Published on 03 November 2010 on http://pubs.rsc.org | doi:10.1039/C0CP01157F View Online
14674 Phys. Chem. Chem. Phys., 2010, 12, 14673–14676 This journal is cthe Owner Societies 2010 chlorophenols) and clofibric acid (CFA, as representative of pharmaceutical compounds). The results are shown in Fig. 1b and c. In the case of DCP, the reaction is started with a high rate so that 95% of DCP is destructed within 2 h. Second addition of formic acid gives rise to proceeding the reaction with similar rate. By termination of formic acid decomposition of DCP is stopped. For CFA, similar trend is observed but the mineralization degree achieved is lower. The catalysts were characterized in order to explain the differences observed in catalytic activity. Fig. 2 contains TPR profiles of the samples, that shows for the Pd5Al sample only a desorption peak of b-PdH, which means an almost total reduction of PdO at ambient temperature. 7 In the presence of Fe, the disappearance of the b-PdH desorption peak is accompanied by the growth of peaks at areas A and B, which means that iron suppresses b-PdH formation. 8 In contrast, the reduction of Fe shifts to lower temperatures. In the TPR thermograms of the Pd5FeCI and Pd5Fe samples, the peak of area A shows much more H 2 consumption (8.4 and 7 times respectively) than the thermogram of the FePd5 sample (see Table S1 in ESIw). High merging for the Pd and Fe species is expected in the Pd5FeCI sample, which was synthesized by co-impregnation. It can be concluded that the peak appearing in area A corresponds to the simultaneous reduction of palladium and iron oxides, resulting in the generation of Fig. 1 Organic compounds degradation profiles over FePd5 performed in two steps: (a) phenol, (b) 2,4-dichlorophenol and (c) clofibric acid. After 4 h, an additional 20 mM (1 mmol) formic acid was added. The numbers in parentheses are the corresponding TOC percentages removed at that time. Table 1 Phenol degradation results by CFP and over Pd5Al and Pd–Fe catalysts Catalyst t/h Ph. conv. (%) TOC removed a (%) k obs(FA)b / min 1 k obs(Ph)c / min 1 Pd leached/ mg l 1 (%) Fe leached/ mg l 1 (%) Fe 2+ 10 mg l 1d 4 100 45 — 1.90 10 2 (R 2 = 0.9821) —— 6 100 47 Pd5Al + Fe 2+ 10 mg l 1 4 85.3 55 1.38 10 2 (R 2 = 0.9996) 1.71 10 2 (R 2 = 0.9950) 0— 6 86.3 66 Pd5FeCI 4 72.2 47 1.29 10 2 (R 2 = 0.9956) 7.00 10 3 (R 2 = 0.9945) 0 0.86 (4.3) 6 73.6 62 Pd5Fe 4 91.4 57 1.39 10 2 (R 2 = 0.9983) 1.04 10 2 (R 2 = 0.99926) 0 1.46 (7.3) 6 93.2 72 FePd5 4 91.2 68 1.33 10 2 (R 2 = 0.9905) 1.26 10 2 (R 2 = 0.9998) 0o0.1 6 92.1 78 a Total organic carbon. b,c Rate coefficients of formic acid and phenol decomposition for the first 1 h of reaction, respectively. d CFP using 300 ppm H 2 O 2 . Fig. 2 TPR thermograms of the samples: (a) Pd5Al, (b) FePd5, (c) Pd5Fe and (d) Pd5FeCI. Downloaded by Universitat Politecnica de Catalunya on 28 December 2010 Published on 03 November 2010 on http://pubs.rsc.org | doi:10.1039/C0CP01157F View Online
This journal is cthe Owner Societies 2010 Phys. Chem. Chem. Phys., 2010, 12, 14673–14676 14675 Pd–Fe alloy. 9,10 The remarkable narrowness of the peak can be attributed to the uniform and well-dispersed iron and palladium oxide particles that yielded to very fine Pd–Fe alloy particles. The second reduction in area B can be attributed to the partial iron oxide reduction still being affected by Pd. The Pd5Fe sample has a relatively high tendency towards Pd–Fe alloy formation. In contrast, for the FePd5 sample, owing to the existence of b-PdH, much of the Pd has not merged with the Fe, and thus least tendency to alloy formation is observed. In accordance with the TPR data, a HRTEM analysis of Pd5FeCI and Pd5Fe (Fig. 3A and B) revealed lattice fringes at 2.20 A ˚for both samples. This value is within the (111) lattice fringes of the PdFe and Pd 3 Fe alloys at 2.19 A ˚and 2.22 A ˚, respectively, and slightly below the value of the (111) crystallographic plane of metallic Pd (2.24 A ˚). In addition to alloy particles, individual metallic Pd particles dispersed on alumina crystallites are also detectable in these two samples, but no isolated Fe-containing phases are observed. In contrast, the HRTEM analysis of the FePd5 sample (Fig. 3C) indicates the presence of metallic Pd and Fe 2 O 3 , which is identified by lattice fringes at 1.84 A ˚and 2.21 A ˚ascribed to (024) and (113) crystallographic planes, respectively. In situ surface analysis by XPS during the reduction of the samples shows considerable reduction of PdO at 100 1C (470% in all cases) (see Table 2), whereas the amount of reduced-surface iron is much higher for FePd5 (18.4%) than for Pd5Fe or Pd5FeCI (0% and 6.5%, respectively). Interestingly, reduction at 200 1C increases the amount of Fe reduced by up to 25.4% for FePd5 and, at the same time, slightly decreases the amount of Pd reduced (from 75% to 72.9%), which suggests that the reduction of Fe 2 O 3 occurs via electron transfer between metallic Pd and Fe 2 O 3 particles. At this temperature, the amount of reduced-surface iron increases to a lower extent for Pd5Fe and Pd5FeCI samples (7.2 and 20.3%, respectively). Thus, the order of sequential impregnation during the preparation of samples plays an important role in the final characteristics of the surface, which may account for the different activity in the Fenton reaction. The binding energy recorded for the Fe (+d) p3/2 core level is very close to that of Fe 2 O 3 /Al 2 O 3 (710.8 eV). This indicates that ionic iron species on the surface of the samples are mostly Fe 3+ . 11 Also, on the surface of Pd–Fe alloy particles, Fe is mostly present as Fe 3+ , as was shown by Chen et al. 12 Therefore, according to the above characterizations, firstly, close proximity and high interaction between the Pd and Fe species is observed. High stability of both metals indicated by leaching results can be due to such interaction. Secondly, for the Pd5FeCI and Pd5Fe samples, much of the Fe participates in alloy formation, whereas a weak tendency towards alloy formation is observed for FePd5. In contrast, the main species found for this sample are metallic Pd and Fe 2 O 3 . Fig. 3 HRTEM images of the following samples: (A) Pd5FeCI, (B) Pd5Fe and (C) FePd5. Table 2 XPS quantitative results of the calcined and reduced Pd–Fe samples Sample Binding energy/eV Elements contributions (%) Pd(0)3d5/2 Pd(d + )3d5/2 Fe(0)2p3/2 Fe(d + )2p3/2 Pd(0) Pd n+ Fe(0) Fe n+ Pd5FeCI calc. — 335.8 — 710.6 0 100 0 100 Pd5FeCI red. 100 1C 335.0 336.4 706.3 711.4 80.9 19.1 6.5 93.5 Pd5FeCI red. 200 1C 334.8 335.9 705.8 711.0 75.1 24.9 20.3 79.7 Pd5Fe calc. — 336.6 — 710.5/715.7 0 100 0 100 Pd5Fe red. 100 1C 335.4 336.9 — 711.2/717.0 72.7 27.3 0 100 Pd5Fe red. 200 1C 335.4 336.7 705.7 710.6 77.5 22.5 7.2 92.8 FePd5 calc. — 336.1 — 710.7 0 100 0 100 FePd5 red. 100 1C 335.4 336.8 706.8 711.5 75 25 18.4 81.6 FePd5 red. 200 1C 335.2 336.4 706.3 710.8 72.9 27.1 25.4 74.6 Downloaded by Universitat Politecnica de Catalunya on 28 December 2010 Published on 03 November 2010 on http://pubs.rsc.org | doi:10.1039/C0CP01157F View Online
14676 Phys. Chem. Chem. Phys., 2010, 12, 14673–14676 This journal is cthe Owner Societies 2010 The preference of the Pd–Fe catalysts in mineralization with respect to the Pd5Al–ferrous ion coupling and CFP can be elucidated by a mechanistic model. In CFP, H 2 O 2 is decomposed into hydroxyl radicals by dissolved ferrous ions. In a homogeneous system using the Pd5Al–ferrous ion, the hydrogen peroxide generated should be released into the solution to reach a soluble ferrous ion for radical formation. Over Pd–Fe catalysts, the mechanism can take the form of a spillover effect (Scheme 1). 13 For surface species, the spillover effect mostly involves metallic Pd and Fe 2 O 3 . Based on that, formic acid decomposes to CO 2 and H 2 over metallic Pd, which is followed by reaction with O 2 , leading to H 2 O 2 formation. Then, surface chemisorbed H 2 O 2 diffuses onto the Fe 2 O 3 surface and, depending on the oxidation state of the Fe, is decomposed into OH or O 2 H radical. 14 In the last stage, the organic molecule approaches the radical and is oxidized to the oxidation products. Surface diffusion of activated H 2 O 2 may also take place via alumina support. No spillover of chemisorbed H 2 O 2 has been reported. It is important to say that the Pd–Fe alloy may not favor the Fenton reaction; a close conjunction of metallic Pd and Fe 2 O 3 particles would be more suitable. This conclusion is based on the better results obtained by the FePd5 catalyst. In summary, a nearly total mineralization of phenol was achieved by a Fenton reaction over a Pd–Fe catalytic system. H 2 O 2 was generated in situ by formic acid and O 2 at ambient conditions. Degradation of chlorophenols and pharmaceutical compounds was also tested which indicated extensive capacity of the catalytic system in degradation of other categories of organic pollutants. The catalysts showed outstanding ability in a multi-step process that included H 2 O 2 generation and the Fenton reaction. The catalysts are highly stable, as shown by the lack of Pd and Fe leaching, which represents a full heterogeneous Fenton process. These results suggest promising prospects for a one-pot full mineralization of organic pollutants. This work was funded by MICINN projects CTM2008- 02453 and CTQ2009-12520 and CIDEM project VALTEC 08- 1-0052. We also thank MICINN for the funding given to S.C. through the Ramo ´n y Cajal program. M.S.Y. acknowledges URV for the PhD grant. J.L. and F.M. acknowledge support from Catalan Government through the ICREA Academia awards. Notes and references 1 J. J. Pignatello, E. Oliveros and A. Mackay, Crit. Rev. Environ. Sci. Technol., 2006, 36, 1; E. Brillas, I. Sire ´s and M. Oturan, Chem. Rev., 2009, 109, 6570. 2(a) R. J. Bigda, Chem. Eng. Prog., 1995, 62; (b) R. Alnaizy and A. Akgerman, Adv. Environ. Res., 2000, 4, 233; (c) J. A. Zazo, J. A. Casas, A. F. Mahedano, M. A. Gilarranz and J. J. Rodriguez, Environ. Sci. Technol., 2005, 39, 9295. 3 M. S. Yalfani, S. Contreras, F. Medina and J. Sueiras, Appl. Catal. B: Environ., 2009, 89, 519. 4 S. Niwa, M. Eswaramoorthy, J. Nair, A. Raj, N. Ith, H. Shoji, T. Namba and F. Mizukami, Science, 2002, 295, 105; J. M. Campos-Martin, G. Blanco-Brieva and J. L. G. Fierro, Angew. Chem., Int. Ed., 2006, 45, 6962; J. J. Bravo-Sua ´rez, K. K. Bando, T. Akita, T. Fujitani and T. J. Oyama, Chem. Commun., 2008, 3272. 5 M. S. Yalfani, S. Contreras, F. Medina and J. Sueiras, Chem. Commun., 2008, 3885. 6 E. M. Cordi and J. L. Falconer, J. Catal., 1996, 162, 104. 7 F. Pinna, F. Menegazzo, M. Signoretto, P. Canton, G. Fagherazzi and N. Pernicone, Appl. Catal. A: Gen., 2001, 219, 195. 8 F. J. Berry, L. E. Smart, P. S. Sai Prasad, N. Lingaiah and P. Kanta Rao, Appl. Catal. A: Gen., 2000, 204, 191. 9 F. Pinna, M. Selva, M. Signoretto, G. Strukul, F. Boccuzzi, A. Benedetti, P. Canton and G. Fagherazzi, J. Catal., 1994, 150, 356. 10 G. Leitz, M. Nimz, J. Vo ¨lter, K. La ´za ´r and L. Guczi, Appl. Catal., 1988, 45, 71. 11 A. P. Grosvener, B. A. Kobe, M. C. Biesinger and N. S. McIntyre, Surf. Interface Anal., 2004, 36, 1564. 12 J. Chen, X. K. Sun, M. C. Yang, J. Xu, W. X. Chen, W. D. Wei and Z. Q. Hu, Appl. Surf. Sci., 1993, 72, 267. 13 W. C. Conner and J. L. Falconer, Chem. Rev., 1995, 95, 759. 14 S.-S. Lin and M. D. Gurol, Environ. Sci. Technol., 1998, 32, 1417. Scheme 1 Mechanism of the phenol degradation reaction via in situ generated H 2 O 2 including: (1) decomposition of formic acid to CO 2 and H 2 , (2) reaction of O 2 with surface H 2 to generate H 2 O 2 , (3) decomposition of chemisorbed H 2 O 2 into radicals, (4) oxidation of organic compounds by surface radicals. OC*: organic compound. Downloaded by Universitat Politecnica de Catalunya on 28 December 2010 Published on 03 November 2010 on http://pubs.rsc.org | doi:10.1039/C0CP01157F View Online