scieee AI-readable full text Open interactive document viewer

In situ high-energy synchrotron X-ray diffraction reveals the role of texture on the activation of slip and twinning during deformation of laser powder bed fusion Ti–6Al–4V

Vallejos, Juan Manuel,Barriobero Vila, Pere,Gussone, Joachim,Haubrich, Jan,Kelm, Klemens,Stark, A,Schell, N.,Requena, Guillermo

Abstract

The deformation behavior of Ti–6Al–4V processed by laser powder bed fusion (LPBF) is investigated by in situ high-energy synchrotron X-ray diffraction (HEXRD) during uniaxial compression. The initial microstructure of the alloy consists of a fine lamellar a¿+¿ß microstructure where a lamellae are separated by thin continuous ß layers within prior ß grains. The anisotropy of the alloy is studied in the deformation direction using samples that are built at the angles of 0°, 45°, and 90° with respect to the LPBF base plate. The sample oriented at 0° presents higher strength–ductility trade-off compared with the conditions oriented at 45° and 90°. The in situ HEXRD experiments continuously reveal the microstructure response during deformation and that the textures for each orientation are associated with a different activation sequence of deformation mechanisms.

Full text

1 In situ high energy synchrotron X-ray diffraction reveals the role of texture on the activation of slip and twinning during deformation of laser powder bed fusion Ti-6Al-4V Juan Manuel Vallejos, Pere Barriobero-Vila, Joachim Gussone, Jan Haubrich, Andreas Stark, Norbert Schell, Guillermo Requena Dr. Juan Manuel Vallejos Instituto de Física Rosario, Bv. 27 de febrero 210 bis, 2000 Rosario, Argentina Universidad Nacional del Nordeste, Facultad de Ingeniería, Las Heras 727, 3500 Resistencia, Argentina Dr. Pere Barriobero-Vila, Dr. Joachim Gussone, Dr. Jan Haubrich, Prof. Guillermo Requena Institute of Materials Research, German Aerospace Center (DLR), Linder Höhe, 51147 Cologne, Germany. Prof. Guillermo Requena Metallic Structures and Materials Systems for Aerospace Engineering, RWTH Aachen University, 52062 Aachen, Germany. Dr. Andreas Stark, Dr. Norbert Schell Helmholtz-Zentrum Geesthacht, Max-Planck-Straße 1, 21502 Geesthacht, Germany. Keywords: high energy synchrotron X-ray diffraction, titanium alloys, twinning-induced plasticity, additive manufacturing, texture, laser powder bed fusion The deformation behaviour of Ti-6Al-4V processed by laser powder bed fusion (LPBF) is investigated by in situ high energy synchrotron X-ray diffraction (HEXRD) during uniaxial compression. The initial microstructure of the alloy consists of a fine lamellar α + β microstructure where α lamellae are separated by thin continuous β layers within prior β grains. The anisotropy of the alloy is studied in the deformation direction using samples built at angles of 0°, 45° and 90° with respect to the LPBF base plate. The sample oriented at 0° presents higher strength-ductility trade-off compared to the conditions oriented at 45° and 90°. The in situ HEXRD experiments continuously reveal the microstructure response during deformation and that the textures for each orientation are associated with a different activation sequence of deformation mechanisms. 1. Introduction 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 2 Ti–6Al–4V is the most studied and commercially used Ti-based alloy, occupying more than half of the market share of titanium products. [1,2] The microstructure of this alloy can be tuned by thermomechanical treatments to obtain a wide range of mechanical properties. [3] Also, the excellent corrosion resistance that can be achieved explains the use of Ti–6Al–4V in a wide range of applications, fundamentally in aerospace and biomedical industry. [1] The traditional manufacturing chain used for Ti–6Al–4V comprises thermomechanical processing followed by machining. [4] This usually leads to high machining costs and large amounts of material loss. The latter can be reduced by metal additive manufacturing (AM), which is especially attractive for decreasing the production costs of components made of Tibased alloys. [5] AM allows the fabrication of near net-shape metallic components with complex geometries such as load-optimized structures of minimal weight. During laser powder bed fusion (LPBF), Ti-based alloys undergo a thermal history consisting of a steep and directional temperature gradient along the building direction. This leads to coarse and columnar prior-β grains strongly textured in the <100> β orientation along the building direction. [6-9] In addition, the high cooling rates (at the order of 10 3 °C s -1 ) produced in LPBF thermal cycles result in the β → α' (hcp) martensitic transformation. [6,10-14] As a consequence, a microstructure dominated by acicular α' with Burgers orientation relationship and distributed within prior β grains is usually obtained in as-built LPBF condition. The microstructural defects that arise from LPBF (e.g. porosity), and the dominating brittle nature of α' martensite are generally considered the cause of poor ductility in as-built LPBF Ti–6Al–4V. [15] Compared to samples with fully martensitic α' microstructure, lamellar α + β microstructures can improve the ductility in Ti–6Al–4V. [10,12,15] To this end, decomposing the metastable α' phase into stable α and β phases has been the goal of several studies. [6,7,9,16-18] Opposing this, it has also been shown that a ductile mechanical response can be achieved in fully α' or dual α + α' microstructures. [19,20] This behaviour was attributed to a higher compatibility, i.e. slip transfer across grain boundaries, between hcp α and α' grains than in 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 3 the case of the hcp/bcc α/β interfaces. Moreover, Zheng et al. suggested that the α/β interface plays a key role in the nucleation and propagation of α twins during deformation of Ti–6Al– 4V. [21] The deformation modes that can be activated during deformation of LPBF Ti-6Al-4V is a complex issue. In addition to the microstructural features mentioned above, they depend on crystallographic texture, i.e. on the load direction. [22-25] In this work, in situ high energy synchrotron X-ray diffraction (HEXRD) is carried out during compressive deformation to determine the sequence of activation of deformation mechanisms and its correspondence with the texture obtained in Ti-6Al-4V manufactured by LPBF. The deformation modes of LPBF Ti-6Al-4V are investigated for conditions deformed at 0°, 45° and 90° with respect to the LPBF building platform. The in situ time-resolved experiments using HEXRD allow for continuous tracking of the deformation mechanisms. 2. Experimental section 2.1. Laser powder bed fusion LPBF of a Ti–6Al–4V (wt.%) grade 23 powder alloy was carried out in argon 5.0 atmosphere using a SLM280HL machine (SLM Solutions Group AG, Lübbeck, Germany). The temperature of the build platform was set to 200 °C. The powder alloy was produced by gas atomization and consisted of spherical particles of a size distribution D 10 = 22 µm, D 50 = 34 µm and D 90 = 46 µm, measured by the standard method ASTM B822. Cubic samples of 10×10×10 mm 3 were built using a chess scanning strategy. The laser pattern for the bulk material consists of chess domains, where the scanning vectors between these domains present a relative rotation of 90°. [26] The LPBF processing parameters are summarized in Table 1. The volume energy density was calculated using Equation 1. The LPBF strategy aimed at applying an intensified intrinsic heat treatment (IHT) to promote decomposition of α' 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 4 martensite into stable α and β phases. [7] This microstructure is sought to increase the ductility of Ti–6Al–4V. [10,12,15] . For compression testing, LPBF cubic samples were machined into cylindrical specimens of 5.5 mm length and 3.5 mm diameter. In order to study the anisotropy of the alloy, the cylindrical samples were machined with the compression axis at 0°, 45° and 90° with respect to the base plate plane of the LPBF machine (hereinafter 0deg, 45deg and 90deg conditions, respectively). A schematic image of the compression directions of the samples with respect to the building platform is shown in Figure 1. Table 1. LPBF parameters used for the processing of the samples. Laser power P [W] Scanning velocity v [mm/s] Hatch distance h [µm] Focal offset distance F [mm] Layer thickness d [µm] Volume energy density Ev [J/mm3] 250 1000 40 0 30 208   =  ·· [/  ] (1) Where E v is the volume energy density; v is the scanning velocity; h is the hatch distance; and d is the layer thickness. 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 5 Figure 1. The samples investigated were manufactured in build directions of 0° (0deg), 45° (45deg) and 90°(90deg) with respect to the base plate of the LPBF machine. 2.2. In situ high energy synchrotron X-ray diffraction during uniaxial compression In situ high energy synchrotron X-ray diffraction (HEXRD) during uniaxial compression was performed in transmission mode (sample thickness = 3.5 mm) at the beamline P07-HEMS of PETRA III (Deutsches Elektronen-Synchrotron, DESY, Hamburg, Germany). [27] The energy of the X-ray beam and the wavelength used were 100 keV and 0.124 nm, respectively; the slit-aperture size of the beam 1×1 mm 2 . The incident X-ray beam was positioned at the centre of the samples before and during deformation. A PerkinElmer XRD 1621 detector acquired the Debye-Scherrer rings during deformation at intervals of 0.5 s/image. The compression tests were carried out at room temperature using a modified dilatometer Bähr 805A/D equipped with a deformation unit. [28,29] The cylindrical samples were compressed at a strain rate of 0.002 s −1 . No buckling of the samples was observed during deformation. The effect of the dilatometer stiffness on the phase’s macrostrains is assumed to be negligible. An illustrative diagram of the experimental setup is shown in Figure 2a. 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 6 Figure 2. a. In situ high energy synchrotron X-ray diffraction during uniaxial compression: experimental setup. b. Debye–Scherrer rings unrolled and converted into Cartesian coordinates (Azimuthal angle ψ, 2θ). c. Example of the evolution as a function of strain for a single {h k l} reflection shown in the selected inset (green dashed line) of Figure 2b. d. Normalized colour-coded 2D image corresponding to the evolution of a {h k l} Bragg reflection intensity for the Azimuthal range 0-360° as a function of strain during uniaxial compression. 2.3. Data processing In order to investigate the evolution of the diffraction images obtained in situ by HEXRD during deformation, the acquired Debye–Scherrer rings were unrolled and converted into 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 7 Cartesian coordinates (Azimuth angle ψ, 2θ), as shown in Figure 2b. Then, the unrolled {h k l} reflexion was cut from the diffraction image, as indicated by the green dotted-line rectangle in Figure 2b. Using the software ImageJ, the intensity sum of Bragg reflections was projected on the ψ - ε plane. [30] This step is shown in Figure 2c. Finally, a normalized colour-coded 2D image is plotted, corresponding to the evolution of {h k l} Bragg reflection intensity for the Azimuthal range 0-360° as a function of strain during uniaxial compression (Figure 2d). The software Maud was employed for Rietveld and texture analyses of the diffraction patterns. [31] An extended Williams-Imhof-Matthies-Vinel algorithm (E-WIMV) integrated in MAUD was used for texture analysis. [31,32] The moment pole stress was employed as a stress model for the Rietveld refinement of the images acquired under compression. [33,34] The instrumental parameters of the HEXRD setup were obtained from a LaB 6 powder standard. The Schmid factors of the α phase were calculated using the software MTEX and the crystal lattice parameters were obtained from Rietveld refinements. [35] Sections of 20° (± 10° with respect to the load) direction were taken from the Debye–Scherrer rings (Figure 2a) to calculate the lattice strains during deformation according to Equation 2. [36] The 2θ variations of individual {h k l} reflections in the load direction were considered for this analysis. Similarly, the calculation of the full width at half maximum (FWHM) were determined for cake portions of 20° in the load direction by single peak fitting (pseudo-Voigt approximation).   =   (2) where ε hkl is the lattice strain of a {h k l} plane family; d 0hkl and d hkl are the plane spacings for the {h k l} family before and during deformation, respectively. 2.4. Microstructure characterization 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 8 Scanning electron microscopy (SEM) in backscattered electron mode (BSE) was used to characterize the microstructure of the samples in the as-built condition. The SEM studies were performed employing a FEI Helios-Nanolab600i microscope (Thermofisher, Waltham, MA, USA). The specimens were prepared by grinding and polishing using a TegraPol machine with 3 µm diamond and SiO 2 suspension. 3. Results Figure 3a and b show the initial microstructure of the LPBF as-built condition. Prior-β grain boundaries are highlighted by dashed lines in Figure 3a. Figure 3b shows that the microstructure is characterized by a partial decomposition of α into α + β. Layers of β can be observed in light grey (see arrows). The lamellar microstructure is composed of fine β layers decorating the α + α grains. These results correlate well with previous investigations reporting this effect using high energy density during LPBF. [7,26] Regions with α and α phases may be expected as a consequence of incomplete martensite decomposition. Since these similar hcp phases cannot be reliably distinguished using HEXRD, they will be referred to as α hereinafter. Figure 3c shows the inverse pole figures of α for 0deg, 45deg and 90deg in the compression direction. In 0deg orientation, the maximum intensities are located close to the basal and prismatic planes. On the other hand, in the specimen at 45deg the maximum intensities are mainly found on the right side of the stereographic triangle, i.e. close to the (101 0)α and (21 1 0)α planes, as well as close to the basal plane. In contrast, for 90deg, the planes near (21 1 2)α are those found most closely aligned to the load direction. 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 9 Figure 3. a. SEM-BSE image of the as-built LPBF condition. The prior-β grains are highlighted by dashed lines. b. SEM-BSE image with major magnification, where β layers are indicated by arrows. c. Inverse pole figures of α for 0deg, 45deg and 90deg orientations in the compression direction. The building direction is vertical for 0deg, 45° from the compression direction for 45deg and coincident with the compression direction for 90deg condition. The true stress - strain curves obtained from the room temperature compression tests are plotted in Figure 4a. The 0deg orientation shows higher ductility and strength than the other two conditions. In order to analyse the work hardening behaviour of the three studied conditions, the evolution of the strain hardening rate (SHR) is shown as dot-line curves as a function of true strain (Figure 4a). It can be observed that the SHR for the 0deg condition is higher than for 45deg and 90deg during the entire deformation. Figure 4b shows the ultimate strength and deformation at break for the three studied orientations. The strength-ductility trade-off is maximum for 0deg. On the opposite, the 45deg condition presents the lowest ductility and strength. 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 16 oriented perpendicular to the compression axis, and its extension is therefore required to accommodate deformation. The directional dependence of twinning for hcp crystals can be observed in the SF corresponding to twinning systems in Figure 8b. The compression twinning system presents maximum SF when the compression direction is perpendicular to the basal plane, and decreases as the c-axis moves away from the load direction. In contrast, the SF of tensile twinning systems has a maximum when the c-axis is perpendicular to the compression direction. It should be noted that the CRSS for the basal and prismatic slip systems in Ti–6Al–4V are very similar to each other, and they are much lower than that for the pyramidal system. [44] This implies that for a grain with a high SF for the pyramidal slip system, the other two slip systems can be activated first because their CRSS is smaller. By comparing the initial texture presented in the IPF of Figure 8c with the SF in Figure 8a-b, the 0deg orientation presents a texture with the majority of the grains prone to activate several deformation systems: {112 2}α compression and {112 1}α tensile twinning as well as prismatic and pyramidal slip. This texture distribution with favourably-oriented grains for twinning or slip activation explains the mechanical behaviour of this condition at beginning of the compression test. The initial orientation of grains in this condition, prone to trigger both tensile and compression twinning modes, indicates that both processes may take place during deformation. This agrees with Figure 5a, where several sudden intensity changes can be seen for this condition, although it is not possible to identify a defined angle of rotation. This could indicate that more than one twinning system is activated. It is also possible that these twinning systems are being activated sequentially, as it is widely reported for pure Ti and α-Ti alloys. [42,44-47] The initial texture in the 45deg orientation is very favourable for activating the prismatic slip system, as it can be observed in the IPF shown in Figure 8c. Although some grains are well oriented to activate {112 2}α compression and {112 1}α tensile twinning systems, the 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 17 prismatic slip system is associated with a low CRSS. Thus, it is plausible that the latter dominates over the twinning deformation modes. [44] The deformation mechanisms that can be activated at the beginning of compression for the 90deg condition are slip in the basal system as well as pyramidal slip and {112 1}α tensile twinning, as observed by comparing Figure 8a, b and c. The initial texture, strongly oriented close to the {21 1 2} plane, indicates that the initial deformation mechanism that governs at the onset of plastic range is slip in the basal plane system. This can be seen in the rapid broadening of the {0002}α reflection during the initial stage of plastic deformation, as it was shown in Figure 6. The grains favourably-oriented for {112 1}α tensile twinning may be responsible for the strain-induced twinning activity, higher than in the 45deg condition but lower than in the 0deg condition, as it was shown in Figures 5-7. Compression twinning is initially restricted in this condition because there are not many grains with the c-axis oriented in the load direction at the beginning of compression. 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 18 Figure 8. Schmid factors as a function of crystallographic orientation for: a. basal, prismatic and pyramidal slip systems; b. {112 2}α, {112 1}α and {101 2}α twinning systems under compression. c. Inverse pole figures of α showing the initial texture for the three investigated conditions. 4.2. Texture evolution during compression A sequential texture development is generally observed in materials where twinning makes a major contribution to plastic deformation. [47] This is related to the reorientation of domains within grains during the nucleation and growth of twins. As can be seen in Figure 5a, the 0deg condition seems to show the most remarkable texture variation. The IPF at different strain levels are shown in Figure 9a to better understand the evolution of texture during compression. The texture changes considerably during deformation in the 0deg orientation. The most remarkable variation is the decrease in intensity near the direction of the {101 0}α 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 19 plane. These orientations have high SF for both tensile twinning modes, {112 1}α and {101 2}α, as it was shown in Figure 8. This is associated with the intensity increase at the base of stereographic triangle, between {21 1 2}α and {21 1 0}α, , as indicated by the arrow in Figure 9a. This figure shows that this increment in intensity can be related to the activation of {112 1}α tensile twinning in crystals oriented near {101 0}α, with a shift of about 35° and <21 1 0> as the rotation axis. The calculated angle of rotation ω is 34°, very close to the theoretical angle, and the axis of rotation r is <2.9 1.7     1.2     0.5>, only 8° away from the <21 1 0> theoretical axis. Although a slight increase in intensity can be observed near the {101 1}α orientation at  = 0.11, no rotations compatible with twinning systems were found for this reflection. This may be due to a sequential combination of different twinning systems, which modifies the rotation of the twin with respect to the matrix. [42] The stress-strain curve for this condition shows a strength-ductility trade-off higher than the other two orientations. We suggest that this is related to the combined activation of slip and strain-induced twinning, which also produces a high strain hardening rate. Less significant texture changes than in the previous case were observed in the 45deg condition (Figure 9b). This is compatible with slip as the dominant mode of plastic deformation. A slight increase in intensity near {21 1 2}α orientation is compatible with the formation of {112 1}α tensile twinning in grains oriented close to {1010}α. The rotation between parent and twin is represented by an angle of rotation ω of 42° (7° away from the theoretical one) and an axis of rotation r <2.9 1.5     1.4     0.1> (1.5° of difference with the <21 1 0> theoretical axis). In the 45deg condition, the tendency to activate the prismatic slip system in detriment of the other deformation modes, fundamentally the twinning systems, seems responsible for the low elongation at break and SHR achieved. The initial texture of the 90deg condition, with most of the grains oriented far from the {0001}α basal plane, restricts the activation of compression twinning (Figure 9c). However, 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 20 many crystals are prone to activate basal slip and {112 1}α tensile twinning. These two mechanisms govern plastic deformation in this condition. Similar rotations to those shown in the two previous cases were found. These are compatible with {112 1}α tensile twinning in grains oriented close to {101 0}α orientation. The texture evolution has similarities to that observed in Figure 9a for the 0deg condition: an intensity decrease can be observed close to the {101 0}α plane, i.e. a region that corresponds to a high SF for {112 1}α tensile twinning (Figure 8b). The 90deg condition shows a lower amount of domains oriented close to the {101 0}α plane than the 0deg condition (compare the IPF in Fig. 10a and c). Therefore, a lower strain-induced twinning activity can be expected for the 90deg condition, which may be responsible for the higher strength-ductility trade-off of 0deg. Despite the fact that the three studied conditions present an initial texture with grains prone to activate the two tensile twinning systems, only {112 1}α twinning seems to be active during compression. In pure Ti, the governing twinning mode is {101 2}. [42] However, as the content of Al increases, this deformation mechanism is abruptly restricted. [48] This was attributed to a higher stacking fault energy and yield stress with increasing Al. [48] In this sense, the 6 wt% of Al in Ti–6Al–4V may be responsible for the difference in the activation of twinning mechanisms compared to pure Ti. For pure Ti, it is commonly known that twinning plays a fundamental role during plastic deformation. However, there are limited reports of twinning in Ti–6Al–4V. [21-22,49,50] This study points to twinning as an important deformation mode for this alloy when produced by LPBF. In this sense, a favourable initial texture is fundamental for the activation and propagation of {112 1}α tensile twinning. 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 21 Figure 9. Inverse pole figures at representative strain levels showing the texture evolution during uniaxial compression for: a. 0deg; b. 45deg; c. 90deg conditions. As a summary, Figure 10a-c shows the dominant deformation mechanisms observed for each deformation stage in the 0deg, 45deg and 90deg conditions, respectively. For the 0deg orientation, a combination of three mechanisms govern the plastic deformation: basal and prismatic slip and {112 2}α tensile twinning. The relatively larger amount of domains oriented close to {101 0}α compared to the 90deg condition and the coexistence of the three deformation modes throughout the entire range of plastic deformation makes it possible to achieve a higher strength ductility trade-off in this condition. Moreover, the occurrence of more than one twinning mode in a sequential and combined way in the 0deg orientation is 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 22 possible because not all rotations were identified with a particular twinning system. [42] Despite the fact that this condition presents favourable grains to activate compression twinning, this mode of deformation could not be clearly observed in Figure 9a. Therefore, it is not included in Figure 10a as a dominant mechanism of deformation, although it could assist in the plastic deformation of the alloy in this orientation. On the other hand, slip in the basal system dominates the initial plastic deformation in the 90deg orientation, followed by a combination of slip and {112 1}α tensile twinning, fundamentally in ε ~ 0.05-0.1. Basal slip is considered to be the dominant mechanism in the second stage of deformation, while twinning assists it to accommodate compression deformation. This assumption is based on the fact that this condition showed less signs of twinning than in the previous case and that the initial texture is well oriented to activate slip in the basal plane. In this condition, a deformation at break of  ~ 0.2 is reached. The mechanism that dominates the plastic deformation in the 45deg orientation is slip in the α prismatic system. Twinning plays a secondary role and as a consequence, the deformation at break and the ultimate strength are lower than in the previous cases. 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 23 Figure 10. Plastic deformation mechanisms dominating in each deformation stage indicated on the true stressstrain curves of: a. 0deg; b. 45deg; c. 90deg conditions. 5. Conclusions 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 24 In this work, the deformation mechanisms under compression of Ti-6Al-4V processed by laser powder bed fusion (LPBF) were investigated in situ using high energy synchrotron X- ray diffraction (HEXRD). To this purpose, samples oriented at 0°, 45° and 90° with respect to the LPBF build plate were investigated. These are three conditions with different initial textures of the α phase with respect to the load direction. In situ compression tests were performed during HEXRD to monitor the evolution of the microstructure during deformation. The following conclusions can be drawn:  A microstructure derived from the partial decomposition of α' into α grains and β layers was obtained within prior β grains by LPBF as a consequence of the intensified intrinsic heat treatment applied during LPBF. The prior β grains have predominantly columnar shapes, while some globular grains were also observed.  The highest ultimate strength and deformation at break was obtained in the 0deg condition. On the contrary, the lower strength-ductility trade-off was observed for the 45deg condition. The higher deformation at break obtained in the 0deg and 90deg conditions is a consequence of the substantial contribution of {112 1}α tensile twinning to the plastic deformation of the alloy.  The initial texture plays an important role in the resulting strength-ductility trade-off. An initial texture favourable for {112 1}α tensile twinning, with several grains oriented near {101 0}α orientation, produces a sequential and synergistic activation of slip and twinning deformation modes that lead to an improved mechanical response. On the other hand, an initial texture for which prismatic slip dominates deformation, with grains oriented near {101 0}α and {21 1 0}α orientations, restricts the mechanical performance of LPBF Ti-6Al-4V.  A fast evolution of texture was observed in the conditions where twinning produced a substantial contribution to plastic deformation, i.e. 0deg and 90 deg. The texture 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 25 evolution in this conditions shows sudden grain rotations, compatible with {112 1}α tensile twinning. On the other hand, the texture during compression in the 45deg build orientation show minor changes, as expected from a condition in which slip in prismatic system dominates plastic deformation. Also, the rotations in this condition are compatible with {112 1}α tensile twinning. The results obtained in this work show that there are still windows of opportunity to adjust the strength-ductility trade-off of LPBF Ti-6Al-4V by tuning initial texture and exploiting the combined effects of slip and twinning. Acknowledgements The Deutsches Elektronen-Synchrotron (DESY) is acknowledged for the provision of synchrotron radiation facilities in the framework of the proposal I-20191042. References [1] C. Leyens, M. Peters, Titanium and Titanium Alloys: Fundamentals and Applications, Wiley-VCH, Weinheim, Germany 2003. [2] C. Cui, B. Hu, L. Zhao, S. Liu, Materials & Design 2011, 32, 1684. [3] G. Lütjering, Mater. Sci. Eng. A 1998, 243, 32. [4] G. Lütjering, J.C. Williams, Titanium, Springer, New York, USA 2007. [5] R. Huang, M. Riddle, D. Graziano, J. Warren, S. Das, S. Nimbalkar, J. Cresko, E. Masanet, Journal of Cleaner Production 2016, 135, 1559. [6] T. Vilaro, C. Colin, J.D. Bartout, Met. Mat. Trans. A Phys. Metallurgy 2011, 42A, 3190. [7] P. Barriobero-Vila, J. Gussone, J. Haubrich, S. Sandlöbes, J. Da Silva, P. Cloetens, N. Schell, G. Requena, Materials 2017, 10, 268. 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65