Numerical simulations of corners in RC frames using Strut-and-Tie Method and CDP model XIII International Conference on Computational Plasticity. Fundamentals and Applications COMPLAS XIII E. Oñate, D.R.J. Owen, D. Peric and M. Chiumenti (Eds) NUMERICAL SIMULATIONS OF CORNERS IN RC FRAMES USING STRUT-AND-TIE METHOD AND CDP MODEL M. SZCZECINA*, A. WINNICKI† * Kielce University of Technology, Faculty of Civil Engineering and Architecture al. Tysiąclecia Państwa Polskiego 7, 25-314 Kielce, Poland e-mail:
[email protected] † Cracow University of Technology, Faculty of Civil Engineering Warszawska Street 24, 31-155 Cracow, Poland
[email protected] Key words: frame corners, opening bending moment, Strut-and-Tie method, FEM, Abaqus, Concrete Damaged Plasticity model. Abstract. Corners of reinforced concrete frames under opening bending moment should be always considered in complex stress conditions. A proper reinforcement of these corners demands some special methods instead of traditional algorithms. In this paper two chosen method are described, namely Strut-and-Tie (S&T) and FEM using Abaqus software. The second method uses Concrete Damaged Plasticity model, implemented in Abaqus code. The corners taken into consideration differ from each other in a reinforcement pattern. Moreover, two different cases of section heights are analyzed: same and different heights of elements joining in a corner. Calculations in S&T method allow to establish proper reinforcement and corner efficiency factor. Then the corners are modeled in Abaqus using CDP and results of crack patterns, efficiency factor, yielding, non-linear behavior and history of load are gained. An extra scientific problem described in this paper is a proper choice of CDP parameters. 1 INTRODUCTION Corners under opening bending moment are very common case in structural design. They appear in single and multi storey frames, underground water tanks, retain walls and foundations. In the Figure 1 a corner under opening bending moment with sample crack pattern is presented. Figure 1: Corner under opening bending moment (crack pattern after [1]) 608
M. Szczecina, A. Winnicki Depending on the type of structure this corner can be considered in plane stress or plane strain state. The first case refers to single or multi storey frames and the second state is characteristic for tanks and retaining walls. Both these cases are useful for structural designers and are considered in this paper. The choice of these corners for analysis is due to the fact that they are under complex stress conditions and a proper choice of their reinforcement requires some special methods. One of these methods is S&T, which is well described in Eurocode 2 [2] and FIB bulletins. However, S&T method for corners under opening bending moment is developed only for corner with the same section heights of beam and column. There is no guidance for corners with different section heights. Moreover, S&T allows only to calculate a required reinforcement and to check if maximal compression stress is not higher than admissible. The second method used by the authors is FEM, performed in Abaqus [3]. This method allows to recreate full history of load and yielding, including crack pattern and propagation. The reinforcement calculated in S&T is an input for FEM model and results gained in Abaqus allow to confirm which reinforcement pattern is worth recommendation. 2 INPUT DATA FOR FRAME CORNERS The corners taken for analysis have some common properties, which are listed below. All corners are made of concrete C40/50 and reinforced with steel B500SP. Here are the material constants: - concrete: fck =40 MPa, fcd =34.30 MPa, Ecm=35 GPa, ν=0.167, - steel: fyk = 500 MPa, fyd = 434.8 MPa, Es=200 GPa, ν=0.3. Each corner is loaded with an opening bending moment M=30 kNm modeled as a pair of forces of magnitude: - 250 kN for the section height 200mm and the distance between the forces is 120mm, - 71.43 kN for the section height 500mm and the distance between the forces is 420mm. The geometry of corners for both cases is presented in the Figure 2. For the time being analysis is restricted to corners with the same section heights. In future authors plan to extend analysis for the case of different section heights. The reinforcement patterns taken into consideration are introduced in the Figure 3. Figure 2: Dimensions of corners 609
M. Szczecina, A. Winnicki Figure 3: Reinforcement patterns for corners The stress-strain curve for concrete in uniaxial compression is approximated by piecewise linearization of σ−ε curve given in EC2 [2]. The coordinates of assumed points are listed in the Table 1. For description of concrete in uniaxial tension a linear σ−ε relation is assumed in postcritical state for given fracture energy Gf. Table 1: Compresive behavior of concrete Yield stress [MPa] Inelastic strain [ o / oo ] 13.70 0.00 29.30 0.95 34.30 1.75 33.70 2.25 The Abaqus user should also input some other important CDP model parameters. The authors of this paper analyze how the choice of these parameters affects the results of calculations. All these parameters are listed in the Table 2. Table 2: CDP parameters range Fracture energy G f [Nm - 1 ]: 146.5, 500, 1000 Dilation angle [degrees]: 0, 5, 15, 30 Relaxation time [s]: 0.0001 Eccentricity: 0.1 fb0/fc0: 1.16 K: 0.667 610
M. Szczecina, A. Winnicki For steel rebars elastic-idealplastic relation in uniaxial σ−ε state is assumed (Figure 4). Figure 4: Reinforcing steel behavior 3 CONCRETE DAMAGED PLASTICITY MODEL One of the concrete models available in Abaqus software is the so-called Concrete Damaged Plasticity. The theoretical framework of the model has been defined by Lubliner, Onate, Oller and Oliver [4]. A fundamental of this model is the assumption that there are two mechanisms of concrete damage: tensile cracking and compressive crushing. The amount of plastic deformation is controlled by the equivalent plastic strain in tension and compression. There are two damage parameters namely, dt and dc, where the subscript t denotes tension and c denotes compression of the concrete. These parameters are functions of plastic strain and take a value from 0 (in virgin state) to 1 (a total loss of capacity). Due to these parameters the reduction of the material stiffness is defined according to the formula [5]: 1 (1) where D is a material stiffness operator, Do is the stiffness operator in elastic range and d denotes one of these two parameters, dt or dc, depending on whether the material is in a compression or tension. Abaqus allows piecewise linearization of σ−ε curve both in compression and tension according to values specified by user. Values used by authors are described in section 2. The program allows also to specify fracture energy Gf. An important procedure that improves the convergence of the nonlinear problem is a regularization. One of the ways to carry it out is the use of visco-plastic model which takes into account the viscous properties of concrete. This possibility exists in Concrete Damaged Plasticity model in Abaqus and assumes Duvaut-Lions' viscoplastic model [6]. This regularization is expressed using formula: 1 (2) where denotes the viscoplastic strain of concrete and is the plastic strain of the concrete without taking into account the viscosity, µ is the relaxation time (in Abaqus called the viscosity parameter). In addition, in an analogous manner the degradation parameter of stiffness is regularized according to formula: 611
M. Szczecina, A. Winnicki 1 (3) where d is one of two degradation parameters dc or dt and is the degradation parameter taking into account both viscoplasticity and viscous damage. The final relationship between stress and strain taking into account both viscoplasticity and viscous damage has form: 1 : (4) where : denotes a scalar product of tensors. The flow potential is defined by the hyperbolic function being asymptotic to the Drucker- Prager cone [5]. The yield function implemented in CDP model is specified according to Lubliner et al. [4] with later modifications by Lee and Fenves [7]. The plastic flow is nonassociated and therefore an Abaqus user should define dilation angle separately. For a full definition of CDP model in Abaqus one should input the following parameters: - compressive behavior of concrete including compression damage condition, - tension behavior of concrete (optionally fracture energy) including tension damage condition, - dilation angle ψ in the p-q plane, - flow potential eccentricity ε, - the ratio fb0/fc0 of biaxial compressive yield stress to uniaxial compressive yield stress, - the ratio K of the second stress invariant on the tensile meridian to that on the compressive meridian for the yield function, - the viscosity parameter (if viscous regularization is used). 4 CALIBRATION OF CDP MODEL PARAMETERS The calibration of CDP model parameters is performed in Abaqus software as a uniaxial and biaxial compression of a concrete specimen. Results of the calculations are compared with the well-known laboratory tests of Kupfer [8]. The specimen has the same properties and dimensions as Kupfer's ones (20x20x5 cm). The FEM analysis is performed in threedimensional strain state. Finite elements are modeled as 3D cubic elements (Figure 5). Figure 5: 3D view of a concrete specimen One of the boundary condition of this model is a linear displacement of a top surface of the specimen (for uniaxial compression) or linear displacement of both top and lateral surface (for 612
M. Szczecina, A. Winnicki biaxial compression). The biaxial compression tests are divided into two separate cases: when compression for both directions is equal (1:1) and when compression for one direction is two times higher (1:0.5). Results of calculations are presented in the form of plots of linear strains and volumetric strain versus stress. A tested parameter is dilation angle, which varies from 0 through 5, 15 till 30 degrees. In the Figures 6 and 7 linear and volumetric strains versus leading stress σ11 for uniaxial compression are shown. The Figures 8 and 9 present the same relationship for biaxial (σ11:σ22=1:1) compression and Figures 10 and 11 for σ11:σ22=1:0.5. Stress values are given in non-dimensional form scaled relative to uniaxial compressive strength fc. Each graph contains also curves gained in tests by Kupfer [8]. For uniaxial compression the compressive behavior of concrete is defined according to Kupfer's results. The point is to find for which dilation angle the σ−ε curve for biaxial compression is the most similar to laboratory tests. Figure 6: Linear strains versus σ 11 for uniaxial compression -1,2 -1 -0,8 -0,6 -0,4 -0,2 0 -0,0032 -0,0022 -0,0012 -0,0002 0,0008 0,0018 ε 11 and e22=e33 vs σ22/fc, uniaxial test e11 dil. 30 e11 dil. 15 e11 dil. 5 e11 dil. 0 e11 Kupfer e33 dil. 30 e33 dil. 15 e33 dil. 5 e33 dil. 0 e33 Kupfer 613
M. Szczecina, A. Winnicki Figure 7: Volumetric strain versus σ 11 for uniaxial compression Figure 8: Linear strains versus σ 11 for 1:1 biaxial compression -0,001 -0,0008 -0,0006 -0,0004 -0,0002 0 0,0002 0,0004 0,0006 0,0008 0,001 -0,003 -0,0025 -0,002 -0,0015 -0,001 -0,0005 0 ε vvs ε11, uniaxial test ev dil. 30 ev dil. 15 ev dil. 5 ev dil. 0 Kupfer -1,4 -1,2 -1 -0,8 -0,6 -0,4 -0,2 0 -0,004 -0,002 0 0,002 0,004 0,006 0,008 0,01 ε 11 and e33 vs σ22/fc , biaxial test, 1:1 e11 dil. 30 e11 dil. 15 e11 dil. 5 e11 dil. 0 e11 Kupfer e33 dil. 30 e33 dil. 15 e33 dil. 5 e33 dil. 0 e33 Kupfer 614
M. Szczecina, A. Winnicki Figure 9: Volumetric strain versus ε 11 for 1:1 biaxial compression Figure 10: Linear strains versus σ 11 for 1:0.5 biaxial compression -0,0025 -0,002 -0,0015 -0,001 -0,0005 0 0,0005 0,001 0,0015 0,002 0,0025 -0,003 -0,0025 -0,002 -0,0015 -0,001 -0,0005 0 ε vvs ε22, biaxial test, 1:1 ev dil. 30 ev dil. 15 ev dil. 5 ev dil. 0 Kupfer -1,4 -1,2 -1 -0,8 -0,6 -0,4 -0,2 0 -0,0044 -0,0024 -0,0004 0,0016 0,0036 ε 11 and ε33 vs σ22/fc, biaxial test, 1:0.5 e11 dil. 30 e11 dil. 15 e11 dil. 5 e11 dil. 0 Kupfer e33 dil. 30 e33 dil. 15 e33 dil. 5 e33 dil. 0 e33 Kupfer 615
M. Szczecina, A. Winnicki Figure 11: Volumetric strain versus σ 11 for 1:0.5 biaxial compression The results of this calibration show that for biaxial compression (1:1) the most compatible with Kupfer's tests is the curve for dilation angle 15 degrees. For the other cases the dilation of 5 degrees seems to be rational. Using dilation angle of 30 degrees, Abaqus user should be aware that positive volumetric strains in concrete can appear. 5 STRUT-AND-TIE AND ABAQUS ANALYSIS All the chosen reinforcement details are at first analyzed with Strut-and-Tie method. Thanks to these calculations a required reinforcement and a corner efficiency factor are established. The corner efficiency factor is a ratio of permissible stress in struts to compressive stress calculated for each strut for the external moment equal to 30 kNm. All the results are listed in the Table 3. Table 3: Results gained with Strut-and-Tie method N o Reinforcement detail Efficiency factor Provided reinforcement 1. 0.83 Main reinforcement: 4 bars each φ 20mm 2. 0.76 Main reinforcement: 4 bars each φ 20mm Diagonal bar: 2 bars each φ 12mm -0,0025 -0,002 -0,0015 -0,001 -0,0005 0 0,0005 0,001 0,0015 -0,0035 -0,003 -0,0025 -0,002 -0,0015 -0,001 -0,0005 0 ε vvs ε22, biaxial test, 1:0.5 ev dil. 30 ev dil. 15 ev dil. 5 ev dil. 0 616