scieee AI-readable full text Open interactive document viewer

A straightforward method to prepare supported Au clusters by mechanochemistry and its application in photocatalysis

Chen, Yufen,Soler Turu, Lluís,Xie, Chenyang,Vendrell Villafruela, Xavier,Serafin, Jaroslaw,Crespo Artiaga, Daniel,Llorca Piqué, Jordi

Abstract

Reducing the metal particle size on semiconductor-based materials from a few nanometers down to well-dispersed clusters or single atoms has been demonstrated to be an effective strategy to enhance the photocatalytic performance. However, designing a simple and fast synthesis procedure has consistently been a challenge. In this work, gold clusters have been easily synthesized and dispersed onto TiO2 surface by one-step ball milling from TiO2 and gold acetate. The Au clusters strongly interact with TiO2 and the resulting material exhibits outstanding photocatalytic performances on the generation of hydrogen under UV and visible light, which double those obtained on conventional Au/TiO2 photocatalysts containing Au nanoparticles. We have studied the effect of various preparation parameters and characterized the samples by a variety of microscopic and spectroscopic techniques. The particular architecture accomplished by ball milling results in efficient charge separation, low charge transfer resistance and high photocurrent response. This mechanochemical method not only provides a facile and cost-effective alternative to the conventional methods of fabricating Au/TiO2 catalysts, but also opens a promising avenue for developing other ultrasmall metal clusters onto different supports.

Full text

1 A straightforward method to prepare supported Au clusters by mechanochemistry and its application in photocatalysis Yufen Chen,1,2 Lluís Soler, 1,2,* Chenyang Xie 1,3 Xavier Vendrell,1,2 Jarosław Serafin,1,2 Daniel Crespo1,3 and Jordi Llorca1,2* 1 Institute of Energy Technologies and Barcelona Research Center in Multiscale Science and Engineering, Universitat Politècnica de Catalunya. Eduard Maristany 16, EEBE, 08019 Barcelona, Spain. 2 Department of Chemical Engineering, Universitat Politècnica de Catalunya. Eduard Maristany 16, EEBE, 08019 Barcelona, Spain. 3 Department of Physics. Universitat Politècnica de Catalunya, EEBE, Eduard Maristany 16, 08019 Barcelona, Spain. *Email. lluis.s[email protected]du *Email. [email protected] KEYWORDS: mechanochemistry, gold, titanium dioxide, hydrogen production, heterogeneous photocatalysis. HIGHLIGHTS • Au clusters are produced by one-step ball milling from TiO2 and Au acetate • Mechanochemically synthesized Au/TiO2 exhibits superior photocatalytic activity • Ball milling results in efficient charge separation and photocurrent response • Ball milling can provide highly active metal-semiconductor photocatalysts 2 ABSTRACT Reducing the metal particle size on semiconductor-based materials from a few nanometers down to well-dispersed clusters or single atoms has been demonstrated to be an effective strategy to enhance the photocatalytic performance. However, designing a simple and fast synthesis procedure has consistently been a challenge. In this work, gold clusters have been easily synthesized and dispersed onto TiO2 surface by one-step ball milling from TiO2 and gold acetate. The Au clusters strongly interact with TiO2 and the resulting material exhibits outstanding photocatalytic performances on the generation of hydrogen under UV and visible light, which double those obtained on conventional Au/TiO2 photocatalysts containing Au nanoparticles. We have studied the effect of various preparation parameters and characterized the samples by a variety of microscopic and spectroscopic techniques. The particular architecture accomplished by ball milling results in efficient charge separation, low charge transfer resistance and high photocurrent response. This mechanochemical method not only provides a facile and cost-effective alternative to the conventional methods of fabricating Au/TiO2 catalysts, but also opens a promising avenue for developing other ultrasmall metal clusters onto different supports. 3 1. INTRODUCTION Small metal species (nanoparticles, metal clusters, single atoms) exhibit unique chemical properties that differ from those of its corresponding bulk metal [1–3]. Such small metallic forms are gaining interest in heterogeneous photocatalysis. Whereas there are numerous studies demonstrating the influence of reducing the size of the supported metal to increase the photocatalytic performance [4,5], conceiving a facile one-step synthesis of well dispersed ultrasmall metal supported species has consistently been a challenge [6,7]. Ball milling is a well-known solventless method for decreasing the size of particles that presents several advantages such as simplicity, versatility and scalability [8]. In addition to decreasing the particle size, ball milling can be also employed to perform chemical transformations induced by mechanical forces by the so-called mechanochemistry [9,10]. Moreover, mechanochemical synthesis enables the use of insoluble reagents. Actually, mechanochemistry has been recently rediscovered as a promising method to produce highly active heterogeneous catalysts, which are not available by conventional synthesis routes [10–15]. For instance, mechanochemistry has recently been used to enhance the catalytic performance in the abatement of pollutants generated during the combustion of fossil fuels, such as the oxidation of soot over ceriabased catalysts [16,17], the oxidation of CO over different metal supported oxides [18,19], or the oxidation of CH4 over Pd/CeO2 catalysts [20,21]. Mechanochemistry has also been proven an as efficient approach to prepare active photocatalysts such as N- doped and S-doped TiO2 [22–26], photoactive semiconductor mixtures of Fe2O3-TiO2 and MoS2-TiO2 [27–30] and magnetically separable TiO2 [31]. Recently, the preparation 4 of Au/TiO2 for hydrogen (H2) photoproduction from gold complexes and manual grinding has been reported [32,33]. However, many questions remain open to shed light on how the mechanochemical action aids to enhance the photocatalytic process. Mechanochemistry is probably the simplest, fastest and environmentally-friendly method for preparing catalysts [34,35], but its use in the preparation of supported small metal species is scarce [19,20]. Moreover, the manufacture of heterogeneous catalysts integrating one or more co-catalysts over oxide supports typically involves several steps in liquid phase that could compromise the scalability and control of their industrial production. [36–38]. Here, we report for the first time the preparation of Au/TiO2 by mechanochemical action from commercial TiO2 and Au (III) acetate. We have carefully investigated the effect of the parameters influencing the mechanochemical action: milling time, milling frequency, ball to powder ratio and concentration of reactants. We show that the photocatalytic properties for H2 photogeneration of the resulting material, which contains an ultra-dispersion of Au clusters are much better than those of Au/TiO2 prepared by conventional wet methods, both under UV and visible light. This approach may be equally useful for other reactions. 2. EXPERIMENTAL 2.1 Materials Gold (III) acetate (Alfa Aesar, 99.9%), commercial TiO2 P90 (Degussa, ca. 90 m2 g- 1), commercial TiO2 P25 (Evonik, ca. 80% anatase and 20% rutile, purity>99.55%), gold (III) chloride hydrate (99.999%, trace metal basis) and glacial acetic acid were purchased from Sigma-Aldrich. Absolute ethanol was purchased from Scharlau. Milli-Q water (H2O) was routinely used. All reagents were used without further purification. 5 2.2 Preparation of Au/TiO2 P90 by mechanochemical synthesis In a typical synthesis of mechanically mixed Au/TiO2 photocatalyst to obtain a nominal Au loading of 1 wt%, gold (III) acetate (0.0057 g) and commercial TiO2 P90 (0.29 g) were added to a stainless-steel vessel (10 mL) along with one stainless-steel ball (15 mm diameter, 13.54 g weight), resulting in a ball to powder ratio (BPR) value of 45. The vessel was placed in a high-speed vibrating ball miller (Retsch, Mixer Mill MM200), and the mixture was ground for 10 min at a vibrational frequency of 15 Hz (unless otherwise stated). After milling, the powder was denoted as Au/P90-BM and used without any further treatment. 2.3 Synthesis of Au/TiO2 P90 by incipient wetness impregnation As a reference photocatalyst, the same nominal Au loading (1 wt%) was obtained by incipient wetness impregnation on the same TiO2 P90 support (0.052g) from a solution of 0.001 g of gold acetate dissolved in 5 mL of glacial acetic acid. The resulting impregnated powder was dried in an oven at 50 °C for 3 h. Afterwards, the sample was calcined at 300 °C for 3 h and labelled as Au/P90-IWI. 2.4 Synthesis of other reference photocatalysts samples To investigate the effects of raw materials and TiO2 surface area on H2 production rate, a set of reference photocatalysts were also synthesized using TiO2 P25 and HAuCl4 instead of TiO2 P90 and gold acetate, respectively. The photocatalysts were prepared with the same Au loading (1 wt%) and mechanochemical procedure (15 Hz, 10 min, BPR = 45). The samples obtained were denoted as Au/P25-BM and HAuCl4/P90-BM, respectively. A reference catalyst (Au/P90-PM) was prepared by grinding gold acetate and TiO2 P90 manually in a pestle and mortar for 10 min. TiO2 P90 without any 6 treatment and after ball milling (15 Hz, 10 min, BPR = 45) were also used as reference samples and were denoted as Pure P90 and P90-BM, respectively. 2.5 Characterization of the photocatalysts X-ray diffraction (XRD) analysis was performed in a Bruker D8 diffractometer with Cu Kα radiation (λ=1.5418 Å, 40 mA, 40 kV). Data were recorded in the 2θ range of 20-80° with a step size of 0.02° and a dwell time of 1 s per step. Crystallite sizes of samples were calculated using the Scherrer equation. High resolution transmission electron microscopy (HRTEM) and high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) were carried out on a FEI Tecnai F20 electron microscope equipped with a field emission electron gun and operated at an accelerating voltage of 200 kV. The point-to-point resolution was 0.19 nm. Scanning electron microscopy (SEM) images were performed on a Zeiss Neon40 Crossbeam Station instrument at 5.0 kV equipped with a field emission source. The free software Fiji was used to measure the particle size of the samples. UV-vis reflectance spectroscopy was measured on a Shimadzu UV3600 UV-vis/NIR apparatus. BaSO4 was used as a reference standard. The spectra were recorded at room temperature in air within the range of 300-800 nm. The acquired diffuse reflectance spectra were converted to absorbance through the standard Kubelka-Munk function. The band gap energies (Eg) of the prepared samples were estimated from the UV-vis spectra by Tauc plots of [F(R) hv]1/2 vs hv. X-ray photoelectron spectroscopy (XPS) was recorded on a SPECS system equipped with a Phoibos 150 MCD-9 detector and an Al anode XR50 source operating at 150 W. CasaXPS program (Casa Software Ltd., UK) was used to evaluate the XPS data (Shirley type background). Raman spectroscopy was carried out on a confocal Raman spectrometer (Renishaw in Via Qontor) equipped with a Leica DM2700M microscope over the range of 50 to 800 cm−1. A laser excitation source of 532 nm and a 7 grating of 2400 lines mm−1 were used. A power of the laser of 1 mW cm-2 was kept at all samples. Brunauer-Emmett-Teller (BET) surface area measurements were performed on QUADRASORBevo Gas Sorption Surface Area and Pore Size Analyzer by N2 sorption at 77 K. Before the N2 sorption isotherm measurements, all samples were outgassed at 110 °C for 12 hours. 2.6 Electrochemical and photoelectrochemical measurements The photoelectrochemical properties were measured on a Bio-logic Sp-200 (Bio- Logic Science Instruments, France) potentiostat/galvanostat in a three-electrode cell (volume 100 mL) with 25 mL of 0.5 M Na2SO4 electrolyte (pH=7.0) at room temperature. The catalyst loaded onto fluorine doped tin oxide (FTO) glass was used as the working electrode. The preparation process is as follows: after washing the FTO glass with ethanol and acetone three times, 15 mg of photocatalyst was dispersed in 15 mL of ethanol under ultrasounds for 30 min and the mixture was dripped onto the FTO glass by spin-coating and dried at room temperature. An Ag/AgCl (3.5 M) electrode (+0.205 V vs. NHE at 25 °C) was used as reference electrode and a spiral Pt (~ 3.6 cm²) wire was used as a counter electrode. The specimens were stabilized under open circuit condition for 1 hour before the measurements. The stable, quasi-steady state potential reached at the end of the stabilization period is denoted as open circuit potential (OCP). Transient photocurrent responses with time were recorded at a bias potential of 10 mV versus OCP during repeated on/off UV light cycles with interval of 20 s. Electrochemical impedance spectroscopy (EIS) experiments were performed at 10 mV amplitude relative to OCP over the frequency range of 1 MHz to 10 mHz. The resistance values of each sample were obtained from the intercepts on the real, Z’, impedance axis from the resultant Nyquist plots performed under UV radiation or dark conditions. Mott-Schottky (M-S) plots were performed at a frequency of 1 kHz and 8 amplitude of 10 mV from -0.8 V to 0.5 V with 20 potential steps. The capacitance and flat-band potential, Vfb, of Pure P90, Au/P90-IWI and Au/P90-BM can be defined by the horizontal intercept of the tangent line of (M-S) plots using the following equation (1): 𝐶𝐶−2 =2 𝑁𝑁𝐷𝐷𝜀𝜀𝜀𝜀0𝑒𝑒 �𝑉𝑉 −𝑉𝑉𝑓𝑓𝑓𝑓 −𝑘𝑘𝑘𝑘 𝑒𝑒� (1) where C is the space charge capacitance in the semiconductor, ND is the electron carrier density, e is elementary charge (1.60 × 10−19 C), ε0 is the Vacuum permittivity (8.85 × 10−12 F m−1), ε is the relative permittivity of TiO2 (55) [39], V is the applied potential, Vfb is the flat band potential, T is the absolute temperature, and k is the Boltzmann constant (1.38 × 10-23 m2 kg s-2 K-1). The effective density of states in conduction band, NC, can be estimated by equation (2), 𝑁𝑁𝐶𝐶= 2(2𝜋𝜋𝑚𝑚𝑑𝑑𝑑𝑑𝑘𝑘𝑘𝑘 ℎ2)3 2 (2) where mde is the density-of-state effective mass for electrons of nano-crystalline anatase TiO2 (9.1 × 10-30 kg), h is Planck constant. The estimated NC value is 7.7 × 1020 cm−3. For a n-type semiconductor, if the value of ND ˂ NC, it can be seen as a nondegenerate semiconductor [40]. Thus, for all prepared photocatalysts in this work, the Boltzmann statistics can be applied to get the bottom of the conduction band ECB (3): 𝐸𝐸𝐶𝐶𝐶𝐶 −𝐸𝐸𝐹𝐹=𝑘𝑘𝑘𝑘𝑘𝑘𝑘𝑘(𝑁𝑁𝐶𝐶 𝑁𝑁𝐷𝐷) (3) where EF is the Fermi level position (EF =Vfb). 2.7. Photocatalytic experiments The photogeneration of hydrogen was tested at atmospheric pressure with a tubular glass photoreactor (from SACOPA, S.A.U.) in a continuous mode as explained elsewhere [41–43]. 2.0 mg (unless otherwise stated) of the selected photocatalyst was dispersed in ethanol by ultrasonication and dripped onto a circular cellulose paper (Albet, thickness 0.18 mm, pore size 35-40 μm, 80 g m-2) and dried at 50 °C for 1 h. An 9 argon gas stream (20 mL min-1) was bubbled through a Drechsel bottle, which contained a liquid mixture of 87.5 g H2O and 9.92 g EtOH to obtain a water:ethanol vapor mixture of 9:1 (molar ratio). An external hot air blower controlled the temperature of the photoreactor and the temperature of the photocatalyst was monitored directly with a K-type thermocouple in contact with the sample. Gas products were analyzed on-line every 4 min with a micro gas chromatograph (GC, Agilent 490) equipped with MS 5 Å, Plot U and Stabilwax columns. The photoreactor was equipped with either a UV light source or a UV-visible light source aligned to a synthetic quartz glass cylindrical lens. The UV light source contained four LEDs emitting at 365 ± 5 nm. A light irradiation of 87 ± 0.5 mW cm−2 was measured directly with a UVA radiation monitor (from Solar Light Co., model PMA 2110, spectral response of 320-400 nm) and a radiometer (model PMA2200, Solar Light Co.). The UV-visible light source contained two LEDs emitting at 372 ± 5 nm and two LEDs emitting visible light (correlated color temperature (CCT) 6099 K, color rendering index (CRI) 74). The UV irradiance of the UV-visible light source was 14 ± 0.5 mW cm−2. The apparent quantum yield (AQY) was calculated by the following equation (4): AQY = 2nH2 np×100 = nNA ET/EP×100 = nNA (𝑃𝑃𝑃𝑃𝑃𝑃)/ (ℎ𝑐𝑐 𝜆𝜆)×100 (4) where nH2 refers to the number of molecules of generated H2. np refers to the incident photons reaching the catalyst. The number of H2 molecules can be calculated by nH2 = nNA, where n is hydrogen moles evolved during the time of light exposure (t), and NA is the Avogadro constant. The np can be calculated by np = ET/Ep, where ET and Ep are the total energy reaching the catalyst and the energy of a photon, respectively. In the equation ET = PSt, the terms P (W m-2), S (m2) and t (s) refer to the power density of incident monochromatic light, the irradiation area and the duration of the incident light exposure, respectively. In the equation Ep = hc/λ, where h, c and λ (m) are the Planck's 16 Fig. 2. XRD patterns (a) and Raman spectra (b) of A: Pure P90, B: Au/P90-IWI fresh, C: Au/P90-IWI after reaction, D: Au/P90-BM fresh, E: Au/P90-BM after reaction. Insets show expanded regions of XRD and Raman spectra. The horizontal dashed lines in the expanded Raman spectra indicate the full width at half maximum (FWHM) measured values. (c-e) HRTEM images of fresh Au/P90-BM (c,d) and Au/P90-IWI (e) 17 photocatalysts. (f-i) HAADF-STEM images of Au/P90-BM (f) fresh and (g) after reaction, and Au/P90-IWI (h) fresh and (i) after reaction. The inset histograms show the size distribution of Au nanoparticles. (j) Au 4f region of the XPS spectra of A: fresh Au/P90-IWI, B: Au/P90-IWI after reaction, C: fresh Au/P90-BM, D: Au/P90-BM after reaction. (k) Tauc plots of (F(R∞)E)1/2 versus E (eV) for Pure P90, Au/P90-IWI and Au/P90-BM, including a linear fit (dashed lines) to determine the band gap energy (Eg). All photocatalysts showed the characteristic Raman-active modes of anatase TiO2 (Fig. 2b) at 144.4, 196.15, 400.4, 514.9, and 637.5 cm−1 [54], whereas rutile phase was not observed due to its poor scattering efficiency. There is a slight peak broadening and shift of the main peak of Au/P90-BM (FWHM=12.2 cm−1) with respect to Pure P90 (FWHM=10.9 cm−1) and Au/P90-IWI (FWHM=10.9 cm−1) (Fig. 2b), which suggests that the addition of Au introduced some defects during the ball milling process [55]. Representative HRTEM images for fresh Au/P90-BM are presented in Figs. 2c and 2d. The Fourier Transform (FT) images shown in the insets of Fig. 2c show spots corresponding to the crystal planes of metallic Au, anatase and rutile. In addition to these large Au nanoparticles, a large number of ultrasmall Au entities (as highlighted by the yellow circles in Fig. 2d, with a size distribution between 0.1-0.5 nm), well dispersed over the surface of fresh Au/P90-BM, were also revealed by HRTEM. Noticeably, these ultrasmall Au entities, or Au clusters, were not present in the fresh Au/P90-IWI sample (see Fig. 2e). The samples Au/P90-BM and Au/P90-IWI were also carefully examined before and after the photoreaction by HAADF-STEM (Fig. 2f-i). The existence of Au nanoparticles (white spots in Z-contrast) was confirmed in all samples. However, whereas only large particles (15-20 nm) could be clearly identified in the fresh Au/P90-BM sample (Fig. 18 2f), an impressive amount of smaller Au particles (5-10 nm) appeared after the photoreaction (Fig. 2g, pointed by arrows). This clear appearance of small Au nanoparticles is likely due to the agglomeration of the Au clusters identified by HRTEM (Fig. 2d) during the photoreaction process. In contrast, HAADF-STEM observations demonstrate that there is no significant change of Au particle size for the sample Au/P90-IWI before and after photoreaction, and both are around 8 ± 2 nm (Figs. 2h and 2i). The XPS analysis of the Au 4f region (Fig. 2j) in Au/P90-IWI reveals the presence of metallic Au (Au0) at Au 4f7/2 of 82.7-83.1 eV [56], both in the fresh and used samples. But in Au/P90-BM, the Au 4f spectra changed radically before and after the photoreaction. The fresh sample is dominated by a signal at 83.6 eV, which can be assigned to gold clusters (labelled as Au0*), in addition to a minor signal corresponding to Au0 at 82.3 eV. After the photoreaction, the signal of the gold clusters Au0* totally disappeared. The loss of Au0* can be accounted for the agglomeration of Au clusters into larger nanoparticles after photoreaction, which is perfectly consistent with the HRTEM and HAADF-STEM results. In addition to this, the Au/Ti surface atomic ratios calculated by XPS (Table S3) clearly indicate that, for the same Au loading (1 wt%), the Au/Ti surface atomic ratio of fresh Au/P90-BM is almost 4-fold that of the other samples (1.92 vs. 0.47), which is a strong evidence of the better dispersion of Au in the fresh sample prepared by ball milling due to the presence of the Au clusters on it. Also, the strong decrease of the Au/Ti atomic ratio after photoreaction in the Au/P90-BM sample (from 1.92 to 0.45) is consistent with an aggregation process of the Au clusters during the photocatalytic test. The Ti 2p spectra (Fig. S7) displays only two components centered at binding energies of 458.5 eV and 464.3 eV, which are assigned to the Ti 2p3/2 and Ti 2p1/2 components of Ti4+ in TiO2 [57]. No peaks related with Ti3+ 19 components could be distinguished in any case. Scheme 1 summarizes the changes of the Au species in Au/P90-BM and Au/P90-IWI during the photoreaction process. From the characterization data and taking into account that the H2 photoproduction is much higher in Au/P90-BM with respect to Au/P90-IWI and the deactivation observed for Au/P90-BM during photoreaction (Fig. 1d) is due to the progressive transformation of the Au clusters into Au nanoparticles, it can be safely concluded that the photoactivity of the Au clusters-TiO2 interface obtained by ball milling is much higher than that of Au nanoparticles-TiO2. This is an important finding of this work. Nevertheless, the photostability of Au clusters over TiO2 surface is not maintained during long time photocatalytic H2 production experiments (Fig. S5) under the photocatalytic conditions tested in this work. The combination of UV exposure, a continuous stream of vaporized ethanol that act as sacrificial electron donor and the transfer of photogenerated electrons from TiO2 to Au species, originate a reducing environment that facilitates a dynamic restructuring phenomenon of Au clusters evolving into Au nanoparticles. Actually, it has been already reported that ultrasmall Au species are at a thermodynamic unstable state and tend to agglomerate under light irradiation or thermal changes [7]. Scheme 1. Illustrative representation of changes of Au species during the studied photoreaction of hydrogen generation. 20 The band gap energy values (Eg) of Pure P90, Au/P90-IWI and Au/P90-BM were calculated by using Tauc plots (Fig. 2k) from the UV-vis spectra (Fig. S2a) and are 3.18 eV, 3.05 eV and 2.97 eV, respectively. The values are all in the range of experimental error (3.08 ± 0.11 eV), indicating that ball milling had little influence on the band gap energy of the TiO2 support. In contrast, charge transfer strongly differs between Au/P90-IWI and Au/P90-BM as determined by electrochemical impedance spectroscopy (EIS). The Nyquist plot (see Fig. 3a) shows a partial high frequency arc in all cases corresponding to the charge transfer resistance. The obtained resistance values were significantly sensitive to the preparation method of the sample. As expected, Au/P90-IWI and Au/P90-BM resistance values were lower than those of pure P90 sample due to the addition of Au nanoparticles, which facilitate the electron transfer. More interestingly, the mechanochemically prepared Au/P90-BM shows a lower resistance than the conventionally prepared Au/P90-IWI, which indicates a better electron transfer and more efficient charge separation [58–60]. A similar trend is observed under dark conditions (Fig. S8a), although, as expected, the resistance values of all the samples were much higher compared with those obtained under UV light conditions. 21 Fig. 3. Nyquist plots under UV irradiation (a), Mott-Schottky plots (b, dark conditions) and transient photocurrent response (c, λ=365 nm) of Pure P90, Au/P90-IWI and Au/P90-BM. 22 Table 1. Electron carrier density (ND), flat band potential (Vfb), conduction band (ECB) and valence band (EVB) calculated for Pure P90, Au/P90-IWI and Au/P90-BM. Pure P90 Au/P90-IWI Au/P90-BM Dark UV Dark UV Dark UV N D (cm-3)a 9.0×1019 9.8×1019 9.9×1019 1.0×1020 9.2×1019 9.0×1019 V fb (V vs. AgCl)b -0.66 -0.65 -0.64 -0.63 -0.50 -0.47 V fb (V vs. NHE) -0.46 -0.45 -0.44 -0.43 -0.30 -0.27 E CB - E F (V vs. NHE)c 0.055 0.053 0.053 0.052 0.055 0.055 E CB (V vs. NHE) -0.52 -0.50 -0.49 -0.48 -0.36 -0.33 E VB (V vs. NHE)d 2.67 2.68 2.56 2.57 2.62 2.65 acalculated from Equation (1) bmeasured from M-S plots in Fig. 3b ccalculated from Equation (3) dcalculated by EVB = Eg + ECB Mott-Schottky (M-S) analysis was measured at the frequency of 1 kHz both under dark and UV light conditions (Fig. 3b and Fig. S8b). All samples show positive slopes in the M-S plots, as expected for n-type semiconductors. In addition, the intercept of the tangent lines of Au/P90-BM under dark and UV light appears at higher potential than that of Pure P90 and Au/P90-IWI, which indicates a higher flat band position (Vfb) in the ball milled sample. The shift in the Vfb (see Table 1) of TiO2 by the addition of Au is related to the Schottky junction formed at the Au/TiO2 interface and causes a decrease of the band bending and a positive shift on Vfb [61]. This is particularly evident for the Au/P90-BM sample, probably due to the presence of the Au clusters, which interact strongly with the titania support. The conduction band (ECB) is calculated to be about 52 23 mV to 55 mV above the Fermi level (EF) for all photocatalysts (Equation 3). Thus, the position of the bottom of the conduction band in Pure P90, Au/P90-IWI and Au/P90- BM can be determined, which are around -0.52 V, -0.49 V, and -0.36 V (vs. NHE, dark conditions), respectively. Combining with the band gap energy (Eg) values obtained from Tauc plots (Fig. 2k), the top of the valence band (EVB) in each sample is estimated to be 2.67 V, 2.56 V, and 2.62 V (vs. NHE, dark conditions), respectively [60]. The detailed results are shown in Table 1. The calculated electron carrier density (ND) values in all three photocatalysts are in the range of (9.5 ± 0.5) × 1019 cm−3 both in dark and UV light conditions, which means that the carrier density might not be the decisive factor for the photocatalytic activity improvement of TiO2 after the surface decoration with Au. In order to study the electron-hole pair formation and electron transfer efficiency [62], transient photocurrent measurements were carried out on Pure P90, Au/P90-IWI and Au/P90-BM (Fig. 3c). Au/P90-BM shows an outstanding, intense photocurrent among all the performed cycles. This result implies that photogenerated electrons and holes in Au/P90-BM moved faster than in Au/P90-IWI and Pure P90, which in turn restricted the recombination process effectively, leading to a more active photocatalyst (Scheme 2). As illustrated in Fig. 3c, the photocurrent recorded in Au/P90-BM progressively decreased over the successive cycles, which again is a direct consequence of the agglomeration of the Au clusters into Au nanoparticles. Therefore, the enhanced photocurrent response provoked by Au clusters explains the improved photocatalytic H2 production rate in Au/P90-BM, which was not observed for the sample Au/P90-IWI containing solely Au NPs. 24 Scheme 2. Illustrative representation of the photocatalytic mechanism of Au/P90-BM. ECB and EVB correspond to the energy band structures of the Au/P90-BM sample, where the bending of TiO2 energy bands and the electronic equilibrium of the Fermi level occurs due to the Au/TiO2 Schottky junction. The photogenerated electron transport pathways between Au clusters and TiO2 are depicted by arrows (the black vertical arrow represents the photoexcitation process of electron–hole pairs; the red dash arrow illustrates the restricted recombination of electron-hole pairs; e- and h+ in the blue and orange cycles correspond to a photogenerated electron and hole, respectively). Diagonal arrows represent charge carriers transport from the bulk to the surface, where the photocatalytic H2 generation takes place. SPR denotes the localized surface plasmon resonance phenomena on expanding the Au/P90-BM sample photo-response under visible light. All these observations explained the particular photocatalytic activity of the Au clusters on TiO2 prepared by mechanochemical force. Additionally, they also 25 demonstrated a dynamic restructuring phenomenon of Au clusters evolving into Au nanoparticles under the photocatalytic conditions tested, which has been crucial for determining the actual nature of active Au species. 4. CONCLUSIONS We have demonstrated a fast, simple and clean way to efficiently fabricate Au/TiO2 photocatalyst by one-step ball milling at room temperature directly from commercial TiO2 and gold acetate. The photocatalyst contains Au clusters well dispersed on the surface of TiO2 and exhibits an activity that doubles that of a conventional Au/TiO2 photocatalyst containing Au nanoparticles in the photoproduction of hydrogen under UV light. The mechanochemically manufactured Au/TiO2 is also more efficient under UV-visible light than when the photocatalytic process is carried out with conventional Au/TiO2. The strong interaction between the Au clusters and TiO2 accomplished by the ball milling method results in efficient charge separation, low charge transfer resistance and high photocurrent response. However, Au clusters agglomerate over time under the photocatalytic conditions tested and they transform into Au nanoparticles, which are less active. We have studied in detail this transformation with various microscopic and spectroscopic techniques and have clearly demonstrated the superior photocatalytic performance of the Au clusters. The mechanochemical approach for the production of heterogeneous supported catalysts provides a new perspective that might pave the way to the design of highly active metal-semiconductor catalytic systems with enhanced photocatalytic activity, which can be further explored for other catalytic applications. 32 [35] S. De, R. Luque, M. Ojeda, C. Xu, A.M. Balu, Mechanochemical synthesis of advanced nanomaterials for catalytic applications, Chem. Commun. 51 (2015) 6698–6713. doi:10.1039/c4cc09876e. [36] M.Q. Yang, Y. Zhang, N. Zhang, Z.R. Tang, Y.J. Xu, Visible-light-driven oxidation of primary C-H bonds over CdS with dual co-catalysts graphene and TiO2, Sci. Rep. 3 (2013) 3314. doi:10.1038/srep03314. [37] W. Ren, Z. Ai, F. Jia, L. Zhang, X. Fan, Z. Zou, Low temperature preparation and visible light photocatalytic activity of mesoporous carbon-doped crystalline TiO2, Appl. Catal. B Environ. 69 (2007) 138–144. doi:10.1016/j.apcatb.2006.06.015. [38] G.L. Martinez, M. Benito, I. Mata, L. Soler, E. Molins, J. Llorca, Preparation and photocatalytic activity of Au/TiO2 lyogels for hydrogen production, Sustain. Energy Fuels. 2 (2018) 2284–2295. doi:10.1039/C8SE00293B. [39] E. Thimsen, A.B.F. Martinson, J.W. Elam, M.J. Pellin, Energy levels, electronic properties, and rectification in ultrathin p-NiO films synthesized by atomic layer deposition, J. Phys. Chem. C. 116 (2012) 16830–16840. doi:10.1021/jp302008k. [40] Y. Liu, F. Le Formal, F. Boudoire, L. Yao, K. Sivula, N. Guijarro, Insights into the interfacial carrier behaviour of copper ferrite (CuFe2O4) photoanodes for solar water oxidation, J. Mater. Chem. A. 7 (2019) 1669–1677. doi:10.1039/c8ta11160j. [41] A. May-Masnou, L. Soler, M. Torras, P. Salles, J. Llorca, A. Roig, Fast and Simple Microwave Synthesis of TiO2/Au Nanoparticles for Gas-Phase 33 Photocatalytic Hydrogen Generation, Front. Chem. 6 (2018) 110. doi:10.3389/fchem.2018.00110. [42] L. Martínez, L. Soler, I. Angurell, J. Llorca, Effect of TiO2 nanoshape on the photoproduction of hydrogen from water-ethanol mixtures over Au3Cu/TiO2 prepared with preformed Au-Cu alloy nanoparticles, Appl. Catal. B Environ. 248 (2019) 504–514. doi:10.1016/j.apcatb.2019.02.053. [43] C. Xing, Y. Liu, Y. Zhang, J. Liu, T. Zhang, P. Tang, J. Arbiol, L. Soler, K. Sivula, N. Guijarro, X. Wang, J. Li, R. Du, Y. Zuo, A. Cabot, J. Llorca, Porous NiTiO3/TiO2 Nanostructures for Photocatatalytic Hydrogen Evolution, J. Mater. Chem. A. 7 (2019) 17053–17059. doi:10.1039/C9TA04763H. [44] E. Taboada, I. Angurell, J. Llorca, Dynamic photocatalytic hydrogen production from ethanol–water mixtures in an optical fiber honeycomb reactor loaded with Au/TiO2, J. Catal. 309 (2014) 460–467. doi:10.1016/j.jcat.2013.10.025. [45] V. Kumaravel, S. Mathew, J. Bartlett, S.C. Pillai, Photocatalytic hydrogen production using metal doped TiO2: A review of recent advances, Appl. Catal. B Environ. 244 (2019) 1021–1064. doi:10.1016/j.apcatb.2018.11.080. [46] A. Gołabiewska, A. Malankowska, M. Jarek, W. Lisowski, G. Nowaczyk, S. Jurga, A. Zaleska-Medynska, The effect of gold shape and size on the properties and visible light-induced photoactivity of Au-TiO2, Appl. Catal. B Environ. 196 (2016) 27–40. doi:10.1016/j.apcatb.2016.05.013. [47] Y. Zhang, S. He, W. Guo, Y. Hu, J. Huang, J.R. Mulcahy, W.D. Wei, Surface- Plasmon-Driven Hot Electron Photochemistry, Chem. Rev. 118 (2018) 2927– 34 2954. doi:10.1021/acs.chemrev.7b00430. [48] M. Murdoch, G.I.N. Waterhouse, M.A. Nadeem, J.B. Metson, M.A. Keane, R.F. Howe, J. Llorca, H. Idriss, The effect of gold loading and particle size on photocatalytic hydrogen production from ethanol over Au/TiO2 nanoparticles, Nat. Chem. 3 (2011) 489–492. doi:10.1038/NCHEM.1048. [49] P. Dzik, T. Svoboda, J. Kaštyl, M. Veselý, Modification of photocatalyst morphology by ball milling and its impact on the physicochemical properties of wet coated layers, Catal. Today. 328 (2019) 65–70. doi:10.1016/j.cattod.2019.01.051. [50] J. Miao, R. Zhang, L. Zhang, Photocatalytic degradations of three dyes with different chemical structures using ball-milled TiO2, Mater. Res. Bull. 97 (2018) 109–114. doi:10.1016/j.materresbull.2017.08.032. [51] J.O. Carneiro, S. Azevedo, F. Fernandes, E. Freitas, M. Pereira, C.J. Tavares, S. Lanceros-Méndez, V. Teixeira, Synthesis of iron-doped TiO2 nanoparticles by ball-milling process: the influence of process parameters on the structural, optical, magnetic, and photocatalytic properties, J. Mater. Sci. 49 (2014) 7476– 7488. doi:10.1007/s10853-014-8453-3. [52] C. De Leitenburg, A. Trovarelli, F. Zamar, S. Maschio, G. Dolcetti, J. Llorca, A novel and simple route to catalysts with a high oxygen storage capacity: The direct room-temperature synthesis of CeO2-ZrO2 solid solutions, J. Chem. Soc. Chem. Commun. (1995) 2181–2182. doi:10.1039/C39950002181. [53] A. Trovarelli, F. Zamar, J. Llorca, C. de Leitenburg, G. Dolcetti, J.T. Kiss, 35 Nanophase Fluorite-Structured CeO2–ZrO2 Catalysts Prepared by High-Energy Mechanical Milling, J. Catal. 169 (1997) 490–502. doi:10.1006/jcat.1997.1705. [54] W. Ouyang, M.J. Muñoz-Batista, A. Kubacka, R. Luque, M. Fernández-García, Enhancing photocatalytic performance of TiO2 in H2 evolution via Ru co-catalyst deposition, Appl. Catal. B Environ. 238 (2018) 434–443. doi:10.1016/j.apcatb.2018.07.046. [55] A.S. Bolokang, F.R. Cummings, B.P. Dhonge, H.M.I. Abdallah, T. Moyo, H.C. Swart, C.J. Arendse, T.F.G. Muller, D.E. Motaung, Characteristics of the mechanical milling on the room temperature ferromagnetism and sensing properties of TiO2 nanoparticles, Appl. Surf. Sci. 331 (2015) 362–372. doi:10.1016/j.apsusc.2015.01.055. [56] Z.G. Sun, X.S. Li, J.L. Liu, Y.C. Li, B. Zhu, A.M. Zhu, A promising visible-light photocatalyst: H2 plasma-activated amorphous-TiO2-supported Au nanoparticles, J. Catal. 375 (2019) 380–388. doi:10.1016/j.jcat.2019.05.027. [57] W. Zhou, W. Li, J.Q. Wang, Y. Qu, Y. Yang, Y. Xie, K. Zhang, L. Wang, H. Fu, D. Zhao, Ordered mesoporous black TiO2 as highly efficient hydrogen evolution photocatalyst, J. Am. Chem. Soc. 136 (2014) 9280–9283. doi:10.1021/ja504802q. [58] Y. Choi, H. Il Kim, G.H. Moon, S. Jo, W. Choi, Boosting up the Low Catalytic Activity of Silver for H2 Production on Ag/TiO2 Photocatalyst: Thiocyanate as a Selective Modifier, ACS Catal. 6 (2016) 821–828. doi:10.1021/acscatal.5b02376. [59] H. Ren, T. Dittrich, H. Ma, J.N. Hart, S. Fengler, S. Chen, Y. Li, Y. Wang, F. 36 Cao, M. Schieda, Y.H. Ng, Z. Xie, X. Bo, P. Koshy, L.R. Sheppard, C. Zhao, C.C. Sorrell, Manipulation of Charge Transport by Metallic V13O16 Decorated on Bismuth Vanadate Photoelectrochemical Catalyst, Adv. Mater. 31 (2019) 1–9. doi:10.1002/adma.201807204. [60] Z. Ai, Y. Shao, B. Chang, B. Huang, Y. Wu, X. Hao, Effective orientation control of photogenerated carrier separation via rational design of a Ti3C2(TiO2)@CdS/MoS2 photocatalytic system, Appl. Catal. B Environ. 242 (2019) 202–208. doi:10.1016/j.apcatb.2018.09.101. [61] P. Yilmaz, A.M. Lacerda, I. Larrosa, S. Dunn, Photoelectrocatalysis of Rhodamine B and Solar Hydrogen Production by TiO2 and Pd/TiO2 Catalyst Systems, Electrochim. Acta. 231 (2017) 641–649. doi:10.1016/j.electacta.2017.02.035. [62] W. Gao, J. Lu, S. Zhang, X. Zhang, Z. Wang, W. Qin, J. Wang, W. Zhou, H. Liu, Y. Sang, Suppressing Photoinduced Charge Recombination via the Lorentz Force in a Photocatalytic System, Adv. Sci. 6 (2019) 1901244–1901250. doi:10.1002/advs.201901244.