scieee AI-readable full text Open interactive document viewer

Pt3Zr alloy as a protective coating against oxidation and hydrogen attack on Zr-based components in nuclear reactors

Arellano, Juan Salvador,Molina Martín, Luis Miguel,López Santodomingo, María José,Alonso Martín, Julio Alfonso

Abstract

Producción Científica

Full text

Full Length Article Pt 3 Zr alloy as a protective coating against oxidation and hydrogen attack on Zr-based components in nuclear reactors J.S. Arellano a , L.M. Molina b,* , M.J. L´ opez b , J.A. Alonso b,c a ´ Area de Física At´ omica Molecular Aplicada (FAMA), CBI, Universidad Aut´ onoma Metropolitana-Azcapotzalco, Av. San Pablo 420, Col. Nueva El Rosario, Ciudad de M´ exico, 02128, M´ exico b Departamento de Física Te´ orica, At´ omica y ´ Optica, Universidad de Valladolid, 47011 Valladolid, Spain c Donostia International Physics Center (DIPC), 20018 San Sebasti´ an, Spain ABSTRACT The adsorption of intact and dissociated water molecules on the surfaces of the Pt 3 Zr alloy and pure Zr have been investigated by means of density functional theory simulations. In each case, a varying amount of water molecules was placed on the surface until saturation coverage was reached. For both surfaces, all the energy barriers for the partial and complete decomposition of water were calculated. The partial dissociation of H 2 O into OH and H, and the complete dissociation into O and two H atoms are significantly more difficult on Pt 3 Zr surfaces, as compared to pure Zr surfaces: the dissociative adsorption energies are smaller and the activation barriers for dissociation are larger in Pt 3 Zr. In addition, the recombination of H atoms into H 2 molecules and desorption of those molecules is easier on the Pt 3 Zr surfaces. The results suggest that the use of the Pt 3 Zr alloy as a protective coating in Zr-based metallic components used in nuclear reactors can indeed improve their performance, since the alloyed Pt 3 Zr layers are much more resistant towards oxidation and H attack than pure Zr in the presence of hot water vapor. 1. Introduction Some issues discussed intensively in the literature on nuclear reactors are the oxidation, corrosion and hydrogen diffusion through the surfaces of the vessels and other metallic parts of the nuclear reactors [1,2]. Those problems can give rise to different types of accidents, and even more, to explosions in some nuclear reactors. A very important problem is the corrosion by hot water of the Zr alloys that are used for nuclear fuel cladding [2,3]. Those zirconium alloys were developed, since the 1950 s, not only for their use as nuclear fuel cladding, but also to form part of other nuclear reactor components. They possess important advantages, such as good mechanical properties, low thermal neutron capture cross-section, and corrosion resistance in high temperature water. However, in spite of the advances, the contact of water with the surface of the cladding layer of the nuclear fuel rods is still the main cause of corrosion, and as a consequence hydrogen could enter and diffuse into the alloy [2]. There are evidences that corrosion has a strong dependence on the particular composition of the zirconium alloys. In other words, small changes in the composition and the microstructure of the alloy can lead to significant differences in the resistance to corrosion [4]. The basic corrosion reaction at the surface of the Zr-based alloys is Zr +2 H 2 O (gas) → ZrO 2 +2 H 2 , which involves formation of a surface layer of zirconium oxide. The main problem is caused by the hydrogen formed during the oxidation reaction, which can diffuse through the oxide layer and enter inside the alloy, weakening its strength. As a conclusion, water corrosion of zirconium alloy nuclear fuel cladding and the inherent hydrogen pickup into the alloy are potentially limiting factors for the operation of nuclear fuel to high burnup and more extreme conditions. The mechanisms for the oxidation of the surface of Zr metal have been intensively studied [5–10]. Under standard conditions, a layer of ZrO 2 oxide forms on top of the Zr surface, and the presence of this layer does not prevent the diffusion of hydrogen into Zr bulk. The mobility of hydrogen atoms and the increase of their concentration within Zr metal and Zr alloys has also been extensively studied in experimental and theoretical works [11–13]. Two interesting ways of improving the durability of the standard Zr alloys used as cladding for nuclear fuels are either changing their composition, or coating them with thin films of other alloys more resistant to water vapor attack [14–16]. Addition of various dopants can reduce the tendency of the surface towards water adsorption and oxidation. Following this idea, we considered interesting the investigation of the surface properties of the Pt 3 Zr alloy, which belongs to the class of so-called ‘superalloys’, characterized by a high degree of chemical ordering and strong stability. At the 3–1 stoichiometry, the very stable compound Pt 3 Zr forms, which has the highest melting point (2250 ◦C) across the Pt-Zr phase diagram [17]. Such high stability and * Corresponding author. E-mail address: [email protected] (L.M. Molina). Contents lists available at ScienceDirect Computational Materials Science journal homepage: www.elsevier.com/locate/commatsci https://doi.org/10.1016/j.commatsci.2024.113313 Received 21 March 2024; Received in revised form 18 August 2024; Accepted 19 August 2024 Computational Materials Science 245 (2024) 113313 Available online 27 August 2024 0927-0256/© 2024 The Author(s). Published by Elsevier B.V. This is an open access article under the CC BY-NC-ND license ( http://creativecommons.org/licenses/bync-nd/4.0/ ). melting point make this material very interesting for its potential use as coating of the zirconium alloys employed in nuclear reactors. Some experimental and theoretical work has been done on the surface and bulk properties of this alloy. Pan et al. [18] studied the electronic structure of this compound and the energetics of oxygen insertion into the bulk of the alloy. Experiments by Li et al. [19] examined the structure and adhesion properties of thin films of zirconium oxide grown on top of the Pt 3 Zr alloy. A study by Antlanger et al. [20] investigated pure and oxidized Pt 3 Zr (0001) surfaces by scanning tunneling microscopy (STM), Auger electron spectroscopy, and density functional theory (DFT). The experimental work of Lackner et al. [21] analyzed the interaction of water with thin layers of ZrO 2 grown on top of the Pt 3 Zr alloy. DFT simulations by Ruiz Puigdollers et al. [22] focussed on the reducibility of those thin ZrO 2 layers and their interaction with hydrogen. In this manuscript, we report the results of an extensive comparison, using the density functional formalism [23], of the interaction of water with pure Zr and Pt 3 Zr surfaces. In each case, we analyze the interaction of water with those surfaces at various water coverages, and with the water molecules either intact, partially dissociated into H atoms and hydroxyl OH groups, or completely dissociated into O and H atoms. The activation barriers for dissociation were calculated. Also, we have Fig. 1. Top and side views of the lowest energy structures for adsorption of one to six water molecules at the Pt 3 Zr surface. In each case, the total adsorption binding energy Emolec[nH2O]of the n molecules is given. One low lying configuration is also given in the cases of one and five adsorbed molecules. Gray spheres: Pt atoms. Blue spheres: Zr atoms. Red spheres: O atoms. Yellow spheres: H atoms. J.S. Arellano et al. Computational Materials Science 245 (2024) 113313 2 simulated the adsorption of several oxygen atoms at each of the two surfaces, to gain some understanding on the initial processes leading towards surface oxidation. The results show that the Pt 3 Zr surface is indeed much less reactive than the pure Zr surface. Therefore, we expect that coating Zr-based alloys with thin layers of Pt 3 Zr can significantly improve the durability of these materials as nuclear fuel cladding. 2. Computational details Electronic structure calculations were performed using Density Functional Theory (DFT) [23] and the gradient-corrected GGA-PBE exchange–correlation functional [24]. The Projected Augmented Wave (PAW) technique was used, as implemented in the GPAW code [25]. This method is based on the use of a real space three-dimensional grid (with a uniform grid spacing of 0.2 Å in our case) to sample the electronic wave functions. Scalar-relativistic pseudopotentials were employed to describe the interaction between core and valence electrons. For the H, O, Pt and Zr atoms, 1, 6, 10 and 12 valence electrons are considered, respectively. In the case of Zr, including 4s and 4p electrons as valence electrons is necessary in order to prevent errors due to corepolarization. The simulations of adsorption of water on the pure Zr and Pt 3 Zr surfaces were performed using a slab model with a thickness of four atomic layers. The atoms in the bottom two layers were kept fixed at their positions in the bulk, and the two upper layers were freely relaxed under the presence of the adsorbates. To ensure that the wave functions decay to very small values at the z-direction boundary of the unit cell, a vacuum space of 14 Å was taken in the z direction on top of the slab. To be able to simulate a sizable coverage of intact and dissociated water molecules, a large lateral (in the x and y directions) unit cell of size 9.97 Å ×11.52 Å was employed for the Pt 3 Zr surface. In the case of pure Zr, Table 1 Average adsorption energies per molecule, Eav molec[nH2O],for adsorption of n =1 – 6 water molecules (per unit cell) on the Pt 3 Zr surface, and adsorption energy of each newly added molecule, Elast molec[nH2O]. All energies in eV. n1 2 3 4 5 6 Eav molec[nH2O]0.946 0.905 0.914 0.908 0.867 0.839 Elast molec[nH2O]0.946 0.864 0.932 0.889 0.705 0.777 Fig. 2. Top and side views of the relaxed structures for several adsorption configurations of a single water molecule dissociated into OH and H at the Pt 3 Zr surface. In each case, the adsorption energy Ediss[OH +H](see eq. (5)) is given.- Gray spheres: Pt atoms. Blue spheres: Zr atoms. Red spheres: O atoms. Yellow spheres: H atoms. J.S. Arellano et al. Computational Materials Science 245 (2024) 113313 3 the size of the unit cell size in the x and y directions was 11.22 Å ×12.96 Å. In both cases, those unit cells consist of 16 surface sites. Such large unit cells allow us simulating both the adsorption of isolated water molecules, and the co-adsorption of several water molecules, hydroxyls, etc., with the intention of studying the saturation coverage for each adsorbed species. A Monkhorst-Pack sampling of 2 ×2 k-points was found sufficient to obtain binding energies converged within 0.01 eV. Geometries were relaxed using the Broyden–Fletcher–Goldfarb–Shanno (BFGS) algorithm [26], until the maximum force on any atom was smaller than 0.015 eV/Å. This procedure results in total energies converged within 0.001 eV. Energy barriers for water dissociation were calculated using a constrained minimization method, involving several simulations where the reaction coordinate (the O–H bond distance) was restricted at monotonously increasing values, while allowing the rest of the system to freely relax [27]. For each of the two surfaces (pure Zr and the Pt 3 Zr alloy) we simulate the adsorption of a varying number of water molecules, either intact, partially dissociated into H and OH, or completely dissociated into co-adsorbed O and H atoms. For each of those cases, water molecules are successively adsorbed until signs of saturation coverage appear. This will happen when the binding energy of the last adsorbed molecule shows a sizable decrease. The dependence of the results with respect to the number of substrate layers used in the calculations has been analyzed by performing selected calculations with three, four, five and six layers in the substrate, with the positions of the atoms of the two bottom layers fixed in all cases. Table S1 of the Supplementary Material shows that the convergence of the molecular (H 2 O) and dissociative (OH+H) adsorption energies with the number of substrate layers is fast, and that using four layers is quite enough to get accurate results. Other workers have used substrates with three or four layers to study the behavior of gases on the surface of transition metals [28–30]. 3. Results and discussion 3.1. Water on the Pt 3 Zr surface We first discuss the adsorption of water on the Pt 3 Zr(0001) surface, at increasing coverage. All possible adsorption sites were explored, and the structures were relaxed. Fig. 1 shows top and side views of the lowest energy structures for the adsorption of up to six intact (non-dissociated) water molecules in the unit cell. The total binding energies for molecular adsorption of n non-dissociated water molecules Emolec[nH2O] = nE[H2Ogas] + E[surface] − E[nH2Oon surface](1) obtained by subtracting the total energy of the system with n adsorbed molecules from the sum of the energies of n water molecules in the gas phase and the energy of the clean surface, are also given in Fig. 1. The positive values of Emolec[nH2O]indicate that the process is exothermic. Fig. 3. Top and side views of the relaxed structures for several adsorption configurations of two water molecules dissociated into OH and H at the Pt 3 Zr surface. In each case, the total adsorption energy Ediss[2(OH +H) ] (with respect to two gas phase H 2 O molecules) is given.- Gray spheres: Pt atoms. Blue spheres: Zr atoms. Red spheres: O atoms. Yellow spheres: H atoms. J.S. Arellano et al. Computational Materials Science 245 (2024) 113313 4 Table 1 gives the average adsorption energies per molecule, Eav molec[nH2O] = Emolec[nH2O]/n(2) and the incremental binding energy, that is, the adsorption energy of the last adsorbed molecule (this is the energy released upon adsorption of the last water molecule on the surface) Elast molec[nH2O] = E[H2Ogas] + E[(n−1)H2Oon surface] −E[nH2Oon surface].(3) The adsorption energy of the last adsorbed molecule can alternatively be calculated as the difference Elast molec[nH2O] = Emolec[nH2O] − Emolec[(n−1)H2O].(4) A single water molecule adsorbs on top of a Zr atom, with the molecular plane almost parallel to the surface and the oxygen atom attached to Zr (see Fig. 1). The adsorption binding energy is 0.95 eV, revealing that the interaction between O and Zr is strong. When the water molecule is initially placed on top of a Pt atom, the O-Pt interaction becomes Fig. 4. Top and side views of the relaxed structures for several adsorption configurations of three (panels a to f) and four (panels g to i) water molecules dissociated into OH groups and H atoms at the Pt 3 Zr surface. In each case, the total dissociative adsorption energies Ediss[3(OH +H) ] and Ediss[4(OH +H) ], with respect to three and four gas phase H 2 O molecules, respectively, are given.- Gray spheres: Pt atoms. Blue spheres: Zr atoms. Red spheres: O atoms. Yellow spheres: H atoms. J.S. Arellano et al. Computational Materials Science 245 (2024) 113313 5 unfavorable, and the water molecule rotates until it forms a weak H-Pt bond (panel 1b). This configuration is much less stable, with a binding energy of 0.17 eV. Therefore, for multiple H 2 O adsorption, it makes sense to occupy all available surface Zr sites. The total adsorption energy increases linearly with the number of adsorbed molecules, at a rate of approximately 0.9 eV per H 2 O molecule, for adsorption from one up to four water molecules. This is not surprising, since the mutual distance between adsorbed water molecules is relatively large, making the adsorption of each additional molecule independent from the previous ones. Since we use a 2 ×2 unit cell, the four Zr surface sites become Table 2 Average adsorption energy per molecule, Eav diss[n(OH +H) ] for the dissociative adsorption of n =1 – 4 water molecules into OH and H on the Pt 3 Zr surface, and dissociative adsorption energy of each newly added water molecule, Elast diss[n(OH +H) ]. All energies in eV. Starting at n =4, the favorable sites for H adsorption saturate, and the dissociative adsorption energy of the last water molecule decreases appreciably. n1 2 3 4 Eav diss[n(OH +H) ] 1.475 1.466 1.487 1.378 Elast diss[n(OH +H) ] 1.475 1.457 1.530 1.050 Fig. 5. Top and side views of the relaxed structures for several adsorption configurations with one (conformers a, b, c, d), two (conformers e, f, g, h), and three (conformers i, j, k) water molecules (per unit cell) fully dissociated into O and H atoms at the Pt 3 Zr surface. In each case, the total dissociative adsorption energy Ediss[n(O+H+H) ] with respect to n gas phase molecules (n =1, 2, 3) is given.- Gray spheres: Pt atoms. Blue spheres: Zr atoms. Red spheres: O atoms. Yellow spheres: H atoms. Table 3 Average adsorption energy per molecule, Eav diss[n(O+H+H) ] for the dissociative adsorption of n =1 – 3 water molecules into O and two H atoms on the Pt 3 Zr surface, and dissociative adsorption energy of each newly added water molecule, Elast diss[n(O+H+H) ]. All energies in eV. n1 2 3 Eav diss[n(O+H+H) ] 1.329 1.096 0.793 Elast diss[n(O+H+H) ] 1.329 0.864 0.185 J.S. Arellano et al. Computational Materials Science 245 (2024) 113313 6 saturated after the adsorption of four H 2 O molecules. So, the fifth H 2 O molecule is adsorbed on top of a Pt atom. Although some stability is gained by forming hydrogen bonds with neighbor water molecules, the impossibility of forming an O-Zr bond causes a drop in the adsorption binding energy, from 0.90 eV for the fourth molecule to 0.70 eV for the fifth one. The sixth water molecule also binds in a similar conformation, involving hydrogen bonds with co-adsorbed water molecules. The dissociative adsorption of water molecules into OH and H at the Pt 3 Zr surface has been studied next. Similar to equations (1), (2), and (3), total dissociative adsorption energies of n water molecules per unit cell Ediss[n(OH +H) ] = E[nH2Ogas] + E[surface] − E[n(OH +O)on surface] (5) average dissociative adsorption energies Eav diss[n(OH +H) ] = Ediss[n(OH +H) ]/n(6) and the dissociative adsorption energy of the last water molecule Elast diss[n(OH +H) ] = E[H2Ogas] + E[(n −1)(OH +H)on surface] − E[n(OH +H)on surface] (7) can be defined. The structures for several optimized configurations of Fig. 6. Top and side views of the relaxed structures for adsorption of one, two and three oxygen atoms at the Pt 3 Zr surface. The lowest energy configuration and a low-lying structure are shown in each case. The total adsorption energies of the n oxygen atoms, Eads[nO], defined in eq. (11), are given.- Gray spheres: Pt atoms. Blue spheres: Zr atoms. Red spheres: O atoms. Yellow spheres: H atoms. Table 4 Desorption energies Edesorp[nH2]required to recombine the H atoms into H 2 molecules and desorb those molecules from a Pt 3 Zr surface covered with n fully dissociated water molecules (n =1–3) on the oxidized nO-Pt 3 Zr surface. Energies in eV. n1 2 3 Edesorp[nH2]1.313 2.286 2.628 Eav desorp[nH2]1.313 1.143 0.876 J.S. Arellano et al. Computational Materials Science 245 (2024) 113313 7 one dissociated molecule are shown in Fig. 2. As expected, the OH group has a strong preference to bind on top of the Zr atoms, forming a strong O-Zr bond with bond-length of 1.91 Å. The corresponding dissociative adsorption energies Ediss[OH +H]are also given in Fig. 2. It should be noticed that the reference is formed by a gas water molecule and the pristine surface. In the most stable configuration (conformer a in Fig. 2) the dissociative adsorption energy is 1.475 eV, around 0.5 eV higher than the adsorption energy of intact H 2 O. In this dissociated configuration, the H atom binds at a Pt-Pt bridge site, at distances 1.80 and 1.81 Å from the two Pt atoms. When the H atom sits at other Pt-Pt bridge sites (conformer b), or at hollow sites between three Pt atoms (conformers c and e), the dissociative adsorption energies decrease by 0.1-–0.3 eV. The possibility of placing the H atom at a location below the surface was also explored. In conformer f the H atom is embedded slightly below the surface, 0.45 Å below the most external layer of Pt atoms, and that configuration is less stable than conformer a by 0.7 eV. Fig. 3 shows several configurations for the co-adsorption of two dissociated water molecules at the Pt 3 Zr surface. The most stable configuration occurs when each dissociated molecule is adsorbed in the same conformation as in the most stable case of a single dissociated H 2 O molecule (see Fig. 2a). The total dissociative adsorption energy of the two molecules, Ediss[2(OH +H) ] = 2.932 eV, almost coincides with twice the dissociative adsorption energy of a single molecule (Ediss[OH +H] = 1.475 eV), because the distance between the co-adsorbed molecules is relatively large. This means that, at this stage, coverage is still sparse and there are no competitive co-adsorption effects. Again, attaching the H atoms to other Pt-Pt bridge sites (see conformers 3b and 3c) results in a reduction of the total adsorption energy by 0.1-–0.2 eV. It is interesting to compare configurations 3d and 3e. In these, the H atoms occupy different types of hollow sites between three Pt atoms, and configuration 3d is clearly preferred over 3e. In the first case, the hollow site has a Zr atom right below it in the second layer, whereas in the second case the hollow site has an empty space below in the second layer. The results for three and four dissociated H 2 O molecules are shown in Fig. 4. For three molecules (configurations a to f), there is just enough room on the surface to place the three H atoms at the most favorable binding sites, and therefore the total adsorption energy Ediss[3(OH +H) ] is approximately equal to three times the dissociative adsorption energy of a single molecule. Starting at four water molecules (configurations g-i), saturation effects begin to appear. In the most stable conformation, the dissociative adsorption energy of the fourth water molecule is Elast diss[4(OH +H) ] = 1.0 eV, while for the third molecule Elast diss[3(OH +H) ] it was around 1.4 eV (see Table 2). Finally, the complete dissociative adsorption of water molecules into O and two H atoms on the surface of Pt 3 Zr has been investigated, and the geometries for several adsorption configurations are shown on Fig. 5 for one (conformers a, b, c, d), two (conformers e, f, g, h), and three (conformers i, j, k) molecules. Those conformers include the lowest energy configuration and several low-lying structures. As expected, H atoms prefer to bind at Pt-Pt bridge sites as in the case of OH+H. Oxygen atoms occupy hollow sites between two Pt atoms and a Zr atom. The adsorption energies for full dissociation of the water molecules are defined Ediss[n(O+H+H)] =E[nH2Ogas]+E[surface]− E[n(O+H+H)onsurface] (8) Eav diss[n(O+H+H) ] = Ediss[n(O+H+H) ]/n(9) Elast diss[n(O+H+H) ] = E[H2Ogas] + E[(n−1)(O+H+H)on surface] −E[n(O+H+H)on surface] (10) For a single water molecule per unit cell, the dissociated adsorption energy, Ediss[O+H+H] = 1.329 eV, is a bit smaller than the adsorption energy corresponding to the dissociation into OH and H, Ediss[OH +O] = 1.475 eV. This means that splitting the adsorbed OH group into O and H atoms on the Pt 3 Zr surface has an energy cost of 0.15 eV. Configuration d in Fig. 5 reveals that the stability drops drastically when the O atom does not make contact with a surface Zr atom. In fact, that structure becomes thermodynamically unstable. Table 3 shows the evolution of the dissociative adsorption energies with the number of adsorbed water molecules. Strong competitive effects begin to appear at n =2, with Ediss and Elast diss decreasing markedly. This means that the presence of coadsorbed H atoms causes a lowering in the ability of the Pt 3 Zr surface to catalyze the dissociation of additional water molecules. For completeness, Fig. 6 shows the structures corresponding to adsorption of oxygen atoms at the Pt 3 Zr surface. The lowest energy configuration and a low-lying structure are given for one, two and three Fig. 7. Intermediate steps and reaction barriers for the dissociation of H 2 O into adsorbed O and H atoms at the Pt 3 Zr surface. Zero energy corresponds to the Pt 3 Zr surface and a free H 2 O molecule. J.S. Arellano et al. Computational Materials Science 245 (2024) 113313 8 oxygen adatoms per unit cell. The most favorable adsorption positions are on hollow sites, and the O atoms show two bonding modes: either bonding to a single Zr atom, or bonding to a Zr and to a Pt atom. At this small coverage the interaction between O adatoms is small, and the total adsorption energy Eads[nO] = n1 2E[O2] + E[surface] − E[nO on surface](11) which is included in Fig. 6, increases almost linearly with the number of O atoms. In a Pt 3 Zr surface covered with n fully dissociated water molecules (O+H+H) per cell, the energy required to recombine all the H atoms into H 2 molecules and desorb the n H 2 molecules can be calculated using the energies of the oxidized nO-Pt 3 Zr surface and the n(O+H+H)-Pt 3 Zr surface: Edesorp[nH2] = nE[H2gas] + E[nO on surface] − E[(nO +2nH)on surface].(12) Table 4 shows those desorption energies for n =1–3. At low coverage (n =1), Edesorp[H2] = 1.313 eV. With increasing coverage of oxygen and hydrogen species (n =2, 3), the total desorption energy of the n hydrogen molecules increases less than linearly with n. The average desorption energy Eav desorp[nH2] = Edesorp[nH2]/n decreases below 1 eV for increasing n. Overall, the calculations predict that when water is adsorbed, the surface of the Pt 3 Zr alloy will be preferentially saturated with hydroxyl OH groups bonded to the Zr surface atoms, and H atoms bonded to the Pt Fig. 8. Lowest energy structures (and a low-lying structure in some cases) for multiple adsorption of water molecules (n =1–5) at the Zr surface. In each case, the total adsorption energy E molec[nH2O]of the n H 2 O molecules is given. Blue spheres: Zr atoms. Red spheres: O atoms. Yellow spheres: H atoms. Table 5 Average adsorption energies per molecule, Eav molec[nH2O], for adsorption of n =1 – 8 water molecules on the surface of Zr, and adsorption energy of each newly added molecule, Elast molec[nH2O]. All energies in eV. n1 2 3 4 5 6 7 8 Eav molec[nH2O]0.712 0.710 0.703 0.700 0.703 0.702 0.691 0.696 Elast molec[nH2O]0.712 0.708 0.690 0.691 0.712 0.699 0.629 0.728 J.S. Arellano et al. Computational Materials Science 245 (2024) 113313 9 dissociation are significantly smaller. Full dissociation into O+H+H is energetically preferred on the Zr surface. Embedding of atomic H below the Pt 3 Zr surface is unfavorable with respect to staying above the surface, but this is easier on pure Zr. The energies required for the recombination of H atoms into H 2 molecules and desorption of those molecules from the Zr surface are larger, by a factor of two, compared to the same process on the Pt 3 Zr surface. In summary, the results reported in - this work provide evidence Fig. 15. a) Bader charges (in e units) at selected atoms for water dissociated into - OH and - H at the pure Zr surface (a), and the Pt 3 Zr surface (b). c) Comparison of electronic densities of states (DOS) for the case of a single water molecule dissociated into OH and H at the Pt 3 Zr and pure Zr surfaces. d) Three dimensional surfaces with constant value of the one-electron wave functions for oxygen and hydrogen states at the Pt 3 Zr surface. Blue and red contours indicate, respectively, regions of positive and negative phase of the wave functions. e) The same for the pure Zr surface. J.S. Arellano et al. Computational Materials Science 245 (2024) 113313 16 for the significantly larger reactivity of the Zr surface with water, as compared to the Pt 3 Zr surface. The decomposition of water molecules into H and OH (or O+H+H), and the penetration of H into the bulk are more difficult on Pt 3 Zr. The recombination of H atoms into H 2 and desorption of the H 2 molecules from the surface is easier on Pt 3 Zr. Thus, Pt 3 Zr could provide a good protective coating of different Zr parts of nuclear reactors, that would diminish the oxidation and the diffusion of hydrogen into the bulk of the walls, and the corresponding weakening of their strength. CRediT authorship contribution statement J.S. Arellano: Writing – review & editing, Writing – original draft, Visualization, Investigation, Formal analysis, Conceptualization. L.M. Molina: Writing – review & editing, Writing – original draft, Visualization, Investigation, Formal analysis, Conceptualization. M.J. L´ opez: Writing – review & editing, Writing – original draft, Investigation, Formal analysis, Conceptualization. J.A. Alonso: Writing – review & editing, Writing – original draft, Investigation, Formal analysis, Conceptualization. Declaration of competing interest The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper. Data availability Data will be made available on request. Acknowledgements Work supported by Ministerio de Ciencia e Innovaci´ on of Spain (Grants PID2019-104924RB-I00 funded by MCIN/AEI/ 10.13039/ 501100011033, and PID2022-138340OB-I00 funded by MCIN/AEI/ 10.13039/501100011033 and FSE+), and the University of Valladolid (GIR Nanostructure Physics). J.S.A. gratefully acknowledges the computing time provided at the LSVP at UAM-Iztapalapa, and J.A.A acknowledges the hospitality of DIPC. Appendix A. Supplementary data Supplementary data to this article can be found online at https://doi. org/10.1016/j.commatsci.2024.113313. References [1] F. Cattant, D. Crusset, D. F´ eron, Corrosion issues in nuclear industry today, Mater. Today 11 (2008) 32–37. [2] A.T. Motta, A. Couet, R.J. Comstock, Corrosion of zirconium alloys used for nuclear fuel cladding, Ann. Rev. Mater. Res. 45 (2015) 311–343. [3] B. Cox, Some thoughts on the mechanisms of in-reactor corrosion of zirconium alloys, J. Nuclear Materials 336 (2005) 331–368. [4] P. Rudling, Zr alloy corrosion and hydrogen pickup, ANT International, Molnlycke, Sweden, 2013. [5] I. Bespalov, M. Datler, S. Buhr, W. Drachsel, G. Rupprechter, Y. Suchorski, Initial stages of oxide formation on the Zr surface at low oxygen pressure: An in situ FIM and XPS study, Ultramicroscopy 159 (2015) 147–151. [6] J.L. Vandegrift, P.M. Price, J.P. Stroud, C.J. Parga, I.J. Van Rooyen, B.J. Jaques, D. P. Butt, Oxidation behavior of zirconium, zircaloy-3, zircaloy-4, Zr-1Nb, and Zr- 2.5Nb in air and oxygen, Nuclear Materials and Energy 20 (2019) 100692–100699. [7] T.W. Chiang, A. Chernatynskiy, M.J. Noordhoek, S.B. Sinnott, S.R. Phillpot, Anisotropy in oxidation of zirconium surfaces from density functional theory calculations, Comput. Mater. Sci. 98 (2015) 112–116. [8] Y.M. Wang, Y.S. Li, K.A.R. Mitchell, A LEED crystallographic analysis for the half monolayer structure formed by O at the Zr(0001) surface, Surf. Sci. 342 (1995) 272–280. [9] F.H. Wang, S.Y. Liu, J.X. Shang, Y.S. Zhou, Z. Li, J. Yang, Oxygen adsorption on Zr (0001) surfaces: Density functional calculations and a multiple-layer adsorption model, Surf. Sci. 602 (2008) 2212–2216. [10] K. Griffiths, C.S. Zhang, P.R. Norton, The autocatalytic decomposition of water on Zr(0001), Surf. Sci. 384 (1997) 70–80. [11] R.K. Siripurapu, B. Szpunar, J.A. Szpunar, Molecular dynamics study of hydrogen in α -zirconium, Int. J. Nuclear Energy (2014) 912369. [12] A. Zieli´ nski, S. Sobieszczyk, Hydrogen-enhanced degradation and oxide effects in zirconium alloys for nuclear applications, Int. J. Hydrogen Energy 36 (2011) 8619–8629. [13] B. Ensor, A.M. Lucente, M.J. Frederick, J. Sutliff, A.T. Motta, The role of hydrogen in zirconium alloy corrosion, J. Nuclear Materials 496 (2017) 301–312. [14] K. Hor´ akov´ a, S. Cichoˇ n, J. Lanˇ cok, I. Kratochvílov´ a, L. Fekete, P. Sajdl, A. Krausov´ a, J. Mac´ ak, V. Ch´ ab, Corrosion protection of zirconium surface based on Heusler alloy, Pure Appl. Chem. 89 (2017) 553–563. [15] C. Anghel, G. Hultquist, M. Limb¨ ack, P. Szakalos, Effects of Pt surface coverage on oxidation of Zr and other materials, J. ASTM Internat. 5 (2008) N2. [16] J. Zhang, Y. Shen, H. Wang, Q. An, Bi-doped zirconium alloys with enhanced water oxidation resistance, J. Phys. Chem. C 124 (2020) 23116–23125. [17] J.K. Stalick, R.M. Waterstrat, The zirconium–platinum phase diagram, J. Alloys Comp. 430 (2007) 123–131. [18] Y. Pan, S. Wang, L. Jia, X. Zhang, First-principles study of a new structure and oxidation mechanism of Pt 3 Zr, RSC Adv. 7 (2017) 54772–54778. [19] H. Li, J. Choi, W. Mayr-Schm¨ olzer, C. Weilach, C. Rameshan, F. Mittendorfer, J. Redinger, M. Schmid, G. Rupprechter, Growth of an ultrathin zirconia film on Pt 3 Zr examined by high-resolution X–ray photoelectron spectroscopy, temperatureprogrammed desorption, scanning tunneling microscopy, and density functional theory, J. Phys. Chem. C 119 (2015) 2462–2470. [20] M. Antlanger, W. Mayr-Schm¨ olzer, J. Pavelec, F. Mittendorfer, J. Redinger, P. Varga, U. Diebold, M. Schmid, Pt 3 Zr(0001): A substrate for growing wellordered ultrathin zirconia films by oxidation, Phys. Rev. B 86 (2012) 035451. [21] P. Lackner, J. Hulva, E.M. K¨ ock, W. Mayr-Schm¨ olzer, J. Choi, S. Penner, U. Diebold, F. Mittendorfer, J. Redinger, B. Kl¨ otzer, G.S. Parkinson, M. Schmid, Water adsorption at zirconia: from the ZrO 2 (111)/Pt 3 Zr(0001) model system to powder samples, J. Mater. Chem. A 6 (2018) 17587–17601. [22] A. Ruiz Puigdollers, G. Pacchioni, Reducibility of ZrO 2 /Pt 3 Zr and ZrO 2 /Pt 2D films compared to bulk zirconia: a DFT+U study of oxygen removal and H 2 adsorption, Nanoscale 9 (2017) 6866–6876. [23] W. Kohn, L.J. Sham, Self-consistent equations including exchange and correlation effects, Phys. Rev. 140 (1965) A1133–A1138. [24] J.P. Perdew, K. Burke, M. Ernzerhof, Generalized gradient approximation made simple, Phys. Rev. Lett. 77 (1996) 3865–3868. [25] J. Enkovaara, C. Rostgaard, J.J. Mortensen, J. Chen, M. Dulak, L. Ferrighi, J. Gavnholt, C. Glinsvad, V. Haikola, H.A. Hansen, et al., Electronic structure calculations with GPAW: a real-space implementation of the projector augmentedwave method, J. Phys. Condens. Matter. 22 (2010) 253202. [26] D.C. Liu, J. Nocedal, On the limited memory BFGS method for large scale optimization, Math. Program. 45 (1989) 503–528. [27] A. Alavi, P. Hu, T. Deutsch, P.L. Silvestrelli, J. Hutter, CO oxidation on Pt(111): an Ab initio density functional theory study, Phys. Rev. Lett. 80 (1998) 3650–3653. [28] L. Kristinsd´ ottir, E. Skúlason, A systematic DFT study of hydrogen diffusion on transition metal surfaces, Surf. Sci. 606 (2012) 1400–1404. [29] S.M. Sharada, R.K.B. Karlsson, Y. Maimaiti, J. Voss, T. Bligaard, Adsorption on transition metal surfaces: Transferability and accuracy of DFT using the ADS41 dataset, Phys. Rev. B 100 (2019) 035439. [30] P. Ferrin, S. Kandoi, A.U. Nilekar, M. Mavrikakis, Hydrogen adsorption, absorption and diffusion on and in transition metal surfaces: A DFT study, Surf. Sci. 606 (2012) 679–689. [31] Shuang-Xi Wang, Ping Zhang, Peng Zhang, Jian Zhao, Shu-Shen Li, Adsorption and dissociation of H 2 O on Zr (0 0 0 1) with density-functional theory studies, J. Nuclear Materials 424 (212) 51–56. [32] R.F.W. Bader, Atoms in Molecules - A Quantum Theory, Oxford University Press, Oxford, 1990. [33] W. Tang, E. Sanville, G. Henkelman, A grid-based Bader analysis algorithm without lattice bias, J. Phys.: Cond. Mater. 21 (2009) 084204. [34] J.A. Alonso, L.A. Girifalco, Electronegativity scale for metals, Phys. Rev B 19 (1979) 3889–3895. [35] W. Metiri, K. Cheikh, Ab initio study of structural, electronic, thermo-elastic and optical properties of Pt 3 Zr intermetallic compound, Chin. Phys. B 29 (2020) 047101. [36] Z. Li, K. Xiong, Y. Sun, C. Jin, S. Zhang, J. He, Y. Mao, First-principles study of mechanical and thermodynamic properties of intermetallic Pt3M (M =Al, Hf, Zr Co, Y, Sc), Comput. Condensed Matter 23 (2020) e00462. [37] Y. Pan, Experimental and theoretical investigation of origin of mechanical properties and facture mechanism of Pt 3 Zr high-temperature material, JOM 72 (2020) 2419–2425. J.S. Arellano et al. Computational Materials Science 245 (2024) 113313 17