scieee AI-readable full text Open interactive document viewer

Towards sustainable solid-state supercapacitors: electroactive conducting polymers combined with biohydrogels

Pérez Madrigal, Maria del Mar,Estrany Coda, Francesc,Armelín Diggroc, Elaine Aparecida,Díaz Díaz, David,Alemán Llansó, Carlos

Abstract

Solid-state organic electrochemical supercapacitors (OESCs) have been fabricated using poly(3,4-ethylenedioxythiophene) (PEDOT) electrodes, a biohydrogel as electrolyte system, and polyaniline fibers as redox additive. The effectivity of sodium alginate, kappa-carrageenan, chitosan and gelatin hydrogels as electrolytic media has been evaluated considering different criteria. Results indicate that kappa-carrageenan-based hydrogel is the most suitable to perform as electrolyte due to the appropriate combination of properties: mechanical stability, ease of preparation, lack of water leaking, and good medium for the electrochemical response of PEDOT electrodes. Cyclic voltammetry and galvanostatic charge-discharge assays indicate that OESCs based on PEDOT electrodes and kappa-carrageenan hydrogel as electrolyte exhibits a good supercapacitor response in terms of specific capacitance, cycling stability, small leakage current and low self-discharging tendency. On the basis of these good properties, four OESC devices were assembled in series and used to power a red LED, confirming that, in addition to advantageous characteristics (e.g. elimination of liquid leaking and enhancement of the device compactness), the designed biohydrogel-containing OESC exhibits potential for practical applications. On the other hand, preliminary assays have been performed loading the kappa-carrageenan hydrogel with polyaniline nanofibers, which act as a redox additive. OESC devices prepared using such loaded biohydrogel have been found to be very promising and, therefore, future work is oriented towards the improvement of their design.

Full text

1 Towards sustainable solid-state supercapacitors: Electroactive conducting polymers combined with biohydrogels Maria M. Pérez-Madrigal,1,2,3 Francesc Estrany,3,4 Elaine Armelin,1,2,3 David Díaz Díaz,1,5,* and Carlos Alemán2,3,* 1 Institut für Organische Chemie Fakultät für Chemie und Pharmazie Universität Regensburg Universitätsstr. 31 , 93053 Regensburg , Germany 2 Departament d’Enginyeria Química, ETSEIB, Universitat Politècnica de Catalunya, Avda. Diagonal 647, Barcelona E-08028, Spain 3 Center for Research in Nano-Engineering, Universitat Politècnica de Catalunya, Campus Sud, Edifici C’, C/Pasqual i Vila s/n, Barcelona E-08028, Spain 4 Departament d’Enginyeria Química, Escola Universitària d’Enginyeria Tècnica Industrial de Barcelona, Universitat Politècnica de Catalunya, Comte d’Urgell 187, 08036 Barcelona, Spain 5 IQAC-CSIC, Jordi Girona 18-26, E-08034 Barcelona (Catalonia, Spain) * da[email protected]ensburg.de and carlos.al[email protected] 2 ABSTRACT Solid-state organic electrochemical supercapacitors (OESCs) have been fabricated using poly(3,4-ethylenedioxythiophene) (PEDOT) electrodes, a biohydrogel as electrolyte system, and polyaniline fibers as redox additive. The effectivity of sodium alginate, -carrageenan, chitosan and gelatin hydrogels as electrolytic media has been evaluated considering different criteria. Results indicate that -carrageenan-based hydrogel is the most suitable to perform as electrolyte due to the appropriate combination of properties: mechanical stability, ease of preparation, lack of water leaking, and good medium for the electrochemical response of PEDOT electrodes. Cyclic voltammetry and galvanostatic charge-discharge assays indicate that OESCs based on PEDOT electrodes and -carrageenan hydrogel as electrolyte exhibits a good supercapacitor response in terms of specific capacitance, cycling stability, small leakage current and low self-discharging tendency. On the basis of these good properties, four OESC devices were assembled in series and used to power a red LED, confirming that, in addition to advantageous characteristics (e.g. elimination of liquid leaking and enhancement of the device compactness), the designed biohydrogel-containing OESC exhibits potential for practical applications. On the other hand, preliminary assays have been performed loading the -carrageenan hydrogel with polyaniline nanofibers, which act as a redox additive. OESC devices prepared using such loaded biohydrogel have been found to be very promising and, therefore, future work is oriented towards the improvement of their design. Keywords: Biohydrogel; Biopolymer; Energy storage; Hydrogel electrolyte; Polyaniline; Polythiophene; Redox additive; Solid-state supercapacitor 3 INTRODUCTION Global concerns on green-chemistry and sustainable development have oriented research and technological developments towards more eco-friendly approaches. This is particularly important for energy-related issues due to both the depletion of fossil fuels and the negative environmental effects that they generate. Within this context, efforts are being made to (i) shift to renewable energy sources; and (ii) design highperformance energy storage devices (i.e. batteries and capacitors) using eco-friendly materials. Batteries display low-power densities although they have high-energy densities, whereas the opposite is true for conventional capacitors.1 In between, electrochemical capacitors, also called supercapacitors (ESCs), have recently been designed with advanced functionalities via environmentally-friendly processes. These systems exhibit high power and energy densities without compromising their cycling stability or other features.2-4 Furthermore, the development of nanostructured electrode materials and the better understanding of the energy-storage mechanisms have contributed to improve the performance of ESCs and to bridge the gap between electrochemical capacitors and batteries in terms of energy density.5-10 Depending on the energy-storage mechanism, electrode materials are divided in two different main groups. In the first one the capacitive behaviour solely relies on the electrostatic interactions (adsorption) between electrolytic ions and the electrode surface (i.e. electrical double-layer capacitance), while faradaic reactions contribute to the overall capacitance (i.e. pseudocapacitance) in the second group.11 Electroactive conducting polymers (ECPs) belong to the latter group and render promising electrodes in organic electrochemical supercapacitors (OESCs) due to their cost-effectiveness, lightweight and flexibility.12 In fact, ECPs display pseudocapacitance behavior as a result of: (i) the redox mechanism (i.e. charge is stored by electron transfer to the 4 polymer with ion pairing to stabilize the charge); and (ii) the double-layer behavior of doped ECPs, which allows resonance throughout the conjugated structure of the polymeric backbone. In a recent work, Mike and Lutkenhaus13 extensively reviewed the advances of ECPs in the energy storage field. Among ECPs, poly(3,4- ethylenedioxythiophene) (PEDOT) has been widely used for the fabrication of OESCs because of its outstanding capacitive performance, good electrical conductivity, high doping rate, stable charge-discharge response, easy of synthesis and advantages in cost.14-18 On the other hand, ECP-based hydrogels are receiving increasing attention,18,19 specially for their application as electrodes in OESCs devices.20-23 For example, multifunctional polyaniline (PAni) hydrogels, with high surface area and threedimensional porous nanostructure, displayed excellent electronic conductivity and electrochemical properties.22 As supercapacitors, such PAni hydrogels exhibited high specific capacitance and cycling stability. Similarly, the specific capacitance displayed by nanostructured conductive polypyrrole (PPy) hydrogels supported their application as supercapacitor electrodes.23 Eco-friendly innovative strategies have been undertaken to improve the performance of energy storage devices considering different strategies,24-30 as for example the design of both electrode materials and redox electrolytes24 using natural resources for electrode materials (e.g. PAni in sodium alginate)25 and aqueous-based solutions as electrolytic system (e.g. KOH, H2SO4 and Na2SO4).26 Regarding the electrolyte system, solid-state supercapacitors, which are formed not only by solid electrodes but also by a solid electrolyte system (SES), have attracted increasing attention because of their advantageous characteristics: high specific/volumetric energy density, flexibility, lightweight and easy of handling in comparison to conventional capacitors.31,32 Furthermore, 5 SES reduce or eliminate leakage of any liquid component and increase the device compactness. Polymeric materials used as SESs can be classified in three groups: (1) gel-based materials (e.g. polyacrylamide or agar); (2) polymers with dissolved salts (e.g. lithium perchlorate in polyethylene oxide); and (3) polyelectrolytes. Interestingly, recent studies focus on eco-friendly electrolytes for high-performance solid-state supercapacitors. For example, Buchtová et al.33 prepared an ionogel based on a chemically cross-linked polysaccharide matrix and a hydrophobic ionic liquid as a greener alternative to petrochemical-based polymeric SESs. Choudhury et al.34 reviewed that gel-polymer electrolytes frequently require using organic solvents during the gelation process, which is environmentally malignant. Hence, replacement of organic solvents with water in these electrolytic systems is highly desirable in terms of sustainability, also minimizing the device cost substantially. However, water-containing gel-polymer electrolytes – hydrogel-polymer electrolytes– limit the operating potential-window (i.e. ∼1.23 V only).34 Within this context, the performance of some ESCs has been improved using biohydrogels (e.g. sodium alginate, hydroxycellulose, gelatin and chitosan).34-38 For example, the electrochemical performance of the Si/C anode of Li-ion batteries was enhanced by applying a cross-linked alginate hydrogel binder.35 This work develops greener and more sustained energy storage devices by replacing conventional liquid electrolytic systems with biohydrogels in OESCs. If properly designed, biohydrogels are safe (i.e. non-toxic, non-flammable, and non-leakage), cheap and easy to prepare; they exhibit high-ionic conductivities and can be obtained from renewable sources. In spite of the advantageous outcome of biohydrogel-based systems as sustainable energy storage devices, caution is required since the electrolyte system plays a crucial role in determining the capacitor response. Thus, if not appropriately 6 conceived, the ion-diffusion rate in hydrogels may be poorer than that shown by liquid electrolytes, and thus limiting the final application of the energy storage device. In this work, Na-alginate, -carrageenan, chitosan and gelatin hydrogels (Scheme S1) have been combined with ECPs to fabricate OESC devices. More specifically, after a twostep selection process, the most appropriate biohydrogel constituted the electrolyte in a device containing PEDOT electrodes and PAni nanofibers (PAni-nfs) as redox additive. METHODS Materials. For the synthesis of PEDOT electrodes, 3,4-ethylenedioxythiophene (EDOT, 97%) was purchased from Sigma-Aldrich (483028); acetronitrile (Reag. Ph. Eur. for analysis, ACS) was purchased from Panreac (Spain); LiClO4 from Sigma- Aldrich (ACS reagent, ≥ 95.0%) was stored in an oven at 70 °C before use. For the synthesis of PAni nanofibers, aniline (ACS reagent ≥ 99.5%) and ammonium peroxodisulfate (ACS reagent ≥ 98.0%) were purchased from Sigma-Aldrich. The biopolymers used were all purchased from Sigma-Aldrich. Specifically, alginic acid sodium salt from brown algae-low viscosity (A2158, 100-300 cP, 2 % (25 °C)), κcarrageenan sulfated plant polysaccharide (22048, 5-25 mPa.s, 0.3% in H2O (25 ºC)), gelatin from porcine skin (gel strength 300, type A G2500), and chitosan medium molecular weight (448877, 200-800 cP, 1 wt. % in 1% acetic acid, 25 ºC). Other reagents used during the preparation of biohydrogel-based electrolytes included: sodium chloride coarse salt QP (Panreac Química S.L.U., Spain), potassium chloride GR (Merck), maleic anhydride (Fluka Analytical, puriss., ≥ 99.0% NT), formaldehyde solution (ACS reagent, 37 wt. % in H2O, contains 10-15% methanol as stabilizer, Sigma-Aldrich), acetic acid min. 99.5% (POCH), ethanol 96% v/v (USP, BP, 7 Ph.Eur. pure-pharma grade) and sodium hydroxide (pellets) both from Panreac Química S.L.U., Spain. Materials preparation. PEDOT electrodes were prepared by chroamperometry (CA) under a constant potential of 1.40 V and using LiClO4 as supporting electrolyte. Details about the preparation procedure are provided in the ESI. The polymerization charge was adjusted to 2.67 C (445 mC/cm2), which corresponded to a mass of polymerized PEDOT of 1.69  0.23 mg. A brief description of Na-alginate, -carrageenan, gelatin and chitosan as well as of the procedures used for the preparation of their hydrogels is provided in the ESI. Preparation of OESC energy storage devices. As a general procedure, OESC devices with biohydrogel-based electrolytes were prepared 24 hours before testing, and the electrolyte gelation proceeded with the electrodes placed in situ to achieve both a better contact between PEDOT and the hydrogel at the electrode/electrolyte interface, and to preserve the integrity of the ECP film (i.e. in some cases, as for example - carrageenan and gelatin, insertion of the PEDOT electrode after the gelation step would damage the ECP film due to the rigidity of the hydrogel). Moreover, to ensure a correct functioning of the biohydrogel as electrolyte, 0.1 M NaCl was mixed in the biopolymer solution prior to gelation. PEDOT electrodes were correctly fixed inside the OESC container (i.e. glass vial or plastic cup for devices with two- or three-electrode configuration, respectively, Scheme S2), leaving 1 cm of separation between them. Teflon® films were used to limit the area of PEDOT (6 cm2), and thus prevent the exposure of steel and its contacting with the hydrogel. Once the biopolymer solution was prepared (ESI), the container was filled with approximately 20-25 mL to fully cover the electrodes. Except for chitosan, all OESC devices were prepared following such steps, albeit slight differences arose during 8 the gelation step according to each procedure, namely regarding the gelation temperature (ESI). Due to the poor mechanical properties of chitosan hydrogel (see next section), for chitosan-containing devices, PEDOT electrodes and the reference electrode (when required) were inserted with extremely caution into the biohydrogel electrolyte after gelation. Finally, OESC devices were maintained at low temperature (4-6 °C, fridge) before their electrochemical characterization. In case of the three-electrode configuration, the reference electrode was not placed in the container before the gelation step, but a glass tube with open ends was used instead (Scheme S2b). 1-2 mL of phosphate buffered solution (PBS, pH 7.4) were introduced in the glass tube, and let to diffuse through the electrolyte hydrogel overnight to provide a good contact between the biohydrogel-based electrolyte and the reference electrode when introduced in the glass tube prior the electrochemical assays. Hereafter, the OESC devices with biohydrogel-based electrolyte using Na-alginate, -carrageenan, chitosan and gelatin will be referred as OESC-NaAlg, OESC-κC, OESC-Chi and OESC-Gel, respectively. Characterization. The Electronic Supporting Information (ESI) provides details of the equipment and conditions used for characterization by optical microscopy, UV-vis spectroscopy, scanning electron microscopy (SEM) and atomic force microscopy (AFM), as well as for electrical conductivity measurements. Electrochemical characterization. Electrochemical cells in three- and two-electrode configurations were assembled for electrochemical characterization: the former was suitable for the fast characterization of the electrode material (i.e. characterization of the PEDOT working electrode), whereas the latter was used to evaluate the supercapacitor performance of OESC devices under specific working conditions (i.e. the response of the whole cell). 9 Accordingly, the electrochemical response of PEDOT in different biohydrogel electrolytic media was first studied using a three-electrode cell configuration. The counter electrode (CE) was made of bare stainless steel, while an Ag|AgCl electrode containing saturated KCl aqueous solution (E0 = 0.222 V vs. standard hydrogen electrode at 25 °C) was used as reference electrode (RE). The electrochemical activity and stability (electroactivity and electrostability, respectively) of PEDOT in the different electrolytic media were determined by cyclic voltammetry (CV) after applying 50 consecutive oxidation-reduction cycles. The initial and final potential was -0.2 V, whereas the reversal potential was 1.0 V. All measurements were performed at room temperature using a scan rate of 50 mV/s. The electrostability was quantified as the loss of electroactivity (LEA; in %): (1) where ΔQ is the difference between the oxidation charge (in C) of the second (Q2) and the evaluated oxidation-reduction cycle (Q#). Data were obtained as the average of three samples for each system. Secondly, the performance of OESC devices (WE= CE= PEDOT) using different biohydrogel electrolytic media was evaluated in a two-electrode configuration. Galvanostatic charge-discharge (GCD) cycles were run between 0.0 and 0.8 V. Different current densities (i.e. charge and discharge rates, which are specified in units of current per electrode mass) were considered: 0.276, 0.692, 1.382, 2.764 or 5.529 A/g that corresponded to 0.467, 1.168, 2.336, 4.672 and 9.344 mA, respectively. All electrochemical experiments were run in triplicate and results presented in this work correspond to the averaged data. 2 Q QQ ·100 Q ΔQ LEA #2 II   16 PEDOT electrodes are expected to show greater surface area values. However, the scarce number of publications reporting this parameter obliges to take it under consideration. Mukkabla et al.51 have also reported the design of Bi2S3/GO composites enwrapped by a PEDOT coating as the anode in Li-ion batteries, Bi2S3/GO/PEDOT composite films being prepared by chemical polymerization. The BET specific surface areas of pristine Bi2S3, Bi2S3/GO and Bi2S3/GO/PEDOT were 12, 51 and 46 m2/g, respectively, while the pore volumes were 0.008, 0.034, and 0.035 cm3/g, respectively. Finally, although the study of Chao et al.54 does not involve the use of PEDOT, it deserves special consideration because of the morphology of the studied system. More specifically, porous SnS and SnS2 architectures were produced with a morphology that closely resembles the one displayed by the PEDOT electrodes designed in this work: a porous flower-like microstructure. BET analyses revealed that the surface areas of porous SnS and SnS2 structures are 66 m2/g and 33 m2/g, respectively.54 In summary, although the surface area of the PEDOT electrodes used in this work has not been determined due to the operational restrictions of the BET test, the revised literature described above allows us to suggest that this value would be found between 30 and 50 m2/g. Preparation and selection of biohydrogels as electrolyte system Figures S3a and S3b display images of the prepared hydrogels (bulk) and of the OESC-biohydrogel devices in a two-electrode configuration, respectively. Hydrogelbased electrolytes derived from Na-alginate and chitosan are opaque and exhibit poor mechanical integrity (i.e. they disintegrate when submitted to stress) in comparison to those obtained using -carrageenan and gelatin. In fact, the extremely poor mechanical integrity of chitosan required careful handling, limiting drastically its applicability as 17 biohydrogel-based electrolyte. In addition, water release was observed for Na-alginate and chitosan hydrogels, which also represented an important drawback. In contrast, - carrageenan and gelatin hydrogels are transparent and more robust, facilitating the assembly of PEDOT electrodes into the electrolyte. According to these results, chitosan hydrogels were discarded as electrolytic system. At this point, it should be clarified that the application of the biohydrogels as electrolytic media does not require careful evaluation of their mechanical properties but only visual inspection to ensure that these materials are robust enough to keep the electrodes at their positions. The morphology of -carrageenan, Na-alginate and gelatin hydrogels was characterized by SEM (Figure S4). Solid-state electrolytes are expected to present an open porous structure able to exploit at maximum the pseudocapacitance of PEDOT electrodes, favouring ion movement and transfer. Both -carrageenan and Na-alginate hydrogels accomplish this requirement, while gelatin exhibits a compact morphology in which the interconnected network of pores is absent. Selection of the sustainable OESC using biohydrogels as electrolyte system After discarding chitosan hydrogels as electrolyte due to its extremely poor mechanical integrity, the electrochemical response of PEDOT in each of the remaining three biohydrogels was investigated to determine their effectiveness as electrolytic media. Figures S5a-S5c display cyclic voltammograms recorded after several consecutive redox scans for -carrageenan, Na-alginate and gelatin electrolyte systems, respectively, using a three-electrode configuration. PBS was used as control electrolyte system (Figure S5d). These voltammograms have been used to evaluate the electroactivity of PEDOT (Figure 1a-1b), which corresponds to the similarity between the cathodic and anodic areas in the voltammograms (i.e. ratio between the reduction 18 and oxidation charges, Qred/Qox). The electroactivity increases with the number of redox cycles indicating that the ability to exchange charge reversibly improves and stabilizes after fifty consecutive oxidation-reduction cycles. Specifically, after the tenth cycle, the Qred/Qox ratio is higher than 0.90 for the three biohydrogel-based electrolytes (Figure 1b). Comparison of the current densities reached at the reversal potential (i.e. 1.0 V in Figures S5a-S5d) indicates that the amount of oxidized molecules is similar for - carrageenan, Na-alginate and PBS, whereas it is lower for gelatin-based electrolyte. Moreover, the electrochemical stability of PEDOT also changes with the electrolyte system (Figure 1c). After five-hundred redox cycles, the loss of electrochemical activity (LEA, Eqn 1) was slightly lower in -carrageenan (13%) than in Na-alginate and gelatin (18% and 16%, respectively). Moreover, the amount of charge stored by PEDOT electrodes varies depending on the electrolyte (Figure 1a): -carrageenan > Na-alginate > PBS > gelatin. Results indicate that the compact morphology of gelatin hydrogel hinders the access and escape of dopant ions during the oxidation and reduction processes of PEDOT, which reduces both the amount of charge stored and the current density. Furthermore, the response of PEDOT in both -carrageenan and Na-alginate hydrogel-based electrolytes is similar, indicating that the interconnecting network of both systems enables ion transport. Finally, the electrochemical performance of PEDOT in PBS electrolyte is worse in comparison to -carrageenan and Na-alginate based devices. More specifically, the electroactivity and LEA values obtained in PBS are lower and higher, respectively, than those reached using such two biohydrogels. These features indicate that the swelling and shrinkage of PEDOT electrodes during redox processes are enhanced in PBS electrolyte, inducing a faster and more severe mechanical degradation of the ECP that, in turn, affects its electrochemical properties. 19 Figures 1d and 1e show the variation of both the Coulombic efficiency (Eqn 4) and the SC (Eqn 2 and 3), respectively, against the current density for the three biopolymer hydrogel-based OESC systems. Data derive from the corresponding GCD curves (Figure S6). As it can be seen, the triangular shape of the GCD curves and SC values are better defined and higher, respectively, for OESC-κC than for OESC-NaAlg and OESC- Gel, independently of the current density used. In addition, after 25 charge-discharge processes, the SC determined for OESC-κC remained higher than 96% for all the considered current densities (Figure S6). For example, for the current density of 1.38 A/g, the SC only decreased 0.98%, evidencing excellent cycling stability. Overall, these results reflect that -carrageenan is the most suitable biohydrogel to perform as electrolyte due to the appropriate combination of properties: mechanical stability, ease of preparation, lack of water leaking, and good medium for the electrochemical response of PEDOT. Accordingly, investigations displayed in next sections are exclusively focused on OESC-κC devices (Figure 2). OESC-κC energy storage device: Capacitive performance Specific capacitance. The capacitive behavior of OESC-κC was investigated by CV and GCD curves (Figure 3). Results have been compared with those obtained for an OESC device with PBS as electrolytic medium (OESC-PBS), which has been used as a control (Figure S7). Cyclic voltammograms recorded for the OESC-κC device (Figure 3a) from 0.0 to 0.8 V display an almost ideal rectangular shape for scan rates up to 200 mV/s (Figure 3a), which is indicative of a good capacitive performance and low contact resistance. This effect is less pronounced for OECS-PBS (Figure S7a). Furthermore, the current density at the reversal and initial potential (i.e. anodic and cathodic current density, 20 respectively) varies linearly with the scan rate (Figure S8), evidencing that the electrochemical processes at OESC-C and OESC-PBS are not controlled by diffusion.55,56 On the other hand, except for the lowest scan rate, the SC values (Eqn 2 and 3) obtained for OESC-C are slightly higher than those determined for OESC-PBS (Figure 3b and Table S1). GCD curves for OESC-C devices exhibited a typical triangular shape with a small voltage drop at the beginning of the discharging step (Figure 3c). In general, PEDOT electrodes display symmetric charge-discharge curves that correspond to almost ideal capacitive properties: high coulombic efficiency and good reversibility.14,16,18 These features are observed for OESC- C devices, which results in SC values (Eqn 2 and 3) that range from 70 to 81 F/g for the second charge-discharge cycle (Figure 3d and Table S2). Although these SC values are similar to those obtained for the OESC-PBS device at low current densities (Figure S7), they tend to decrease for higher current densities, possibly due to slower ion movement and electrolyte diffusion in the biohydrogel-based electrolyte. In contrast, SC values for the OESC-PBS device do not present significant changes with the current density (Figure 3d). On the other hand, after 25 consecutive charge-discharge cycles, OESC-C devices displayed an excellent SC retention (i.e. higher than 92 %) for all tested current densities (Figure 3d). For example, the system was able to retain ca. 95 % of the highest SC value, which was obtained at 1.38 A/g (Table S2). As it was expected, the stability of the OESC-C device is slightly lower than that of the OESC-PBS one (Figure 3d and Table S2). This should be attributed to the degradative effects produced by consecutive charge-discharge cycles in the hydrogel structure. Overall, results displayed in this sub-section confirm that the OESC based on PEDOT electrodes and -carrageenan as electrolyte exhibits a good supercapacitor 21 response. The presence of the solid electrolyte does not affect negatively the PEDOT capacitive behavior, bringing advantageous characteristics to the final packaged cell for practical applications. Lifetime stability. Cyclability (i.e. from hundreds to thousands of cycles) is an important requirement for practical supercapacitor applications. In order to evaluate this property, as-prepared OESC-C devices were submitted to three-thousand consecutive GCD cycles at a constant current density of 1.38 A/g from 0 to 0.8 V, results being summarized in Figures 4a and 4b. After such amount of cycles, the SC decrease from 79.1 ± 0.4 F/g to 71.1 ± 2.2 F/g, which represents a variation of only 10% (i.e. 90% of retention). This slight reduction in the SC values for OESC-C has been associated to the swelling and shrinkage phenomena experienced by PEDOT during oxidation and reduction processes, respectively. Thus, consecutive doping-dedoping steps induce structural changes in PEDOT electrodes, which evolve from a porous morphology to a more compact one. The increasing compactness of PEDOT hinders the access and escape of dopant ions during the oxidation and reduction processes, respectively, until the equilibrium is reached. Moreover, to determine the lifetime stability of OESC-C, the same assay was repeated after one week of the device preparation. Figures 4c and 4d compare the results obtained for as as-prepared OESC-C devices (t0) with those obtained for devices prepared one week before (t1w). In this series of as prepared devices, the SC decrease from 85 ± 7 F/g to 80 ± 6 F/g after consecutive GCD cycles at a constant current density of 1.38 A/g from 0 to 0.8 V, which represents a variation of only 6% (i.e. 94% of retention). For the devices that were characterized one week after their preparation, the SC values corresponding to the second (80 ± 9 F/g) and five-hundredth (79 ± 8 F/g) 22 charge-discharge cycle differ by only 1 % (i.e. 99% of retention) and, more interestingly, they resemble to those determined for the as-prepared device after fivehundred cycles (79 ± 6 F/g), confirming that the structure of PEDOT is stabilized. In addition to this excellent cycling stability, OESC-C devices, when properly closed (Figure S9a), exhibit no water loss or evaporation, which further ensures its application. Leakage current and self-discharge response. The leakage current is the stable parasitic current expected when the capacitor is held indefinitely on charge at the rated voltage.57 OESC-C devices were charged to 0.8 V at 2.334 mA (i.e. 1.38 A/g), and kept at that potential for 5 minutes, while recording the current data through the OESC- C (i.e. leakage current). Figure 4e shows how the current quickly decreases to a minimum value of 51.2 A, staying at that value for the remaining time. This relatively small leakage current is associated to a good stability of OESC-C devices, which is crucial for energy storage applications. On the other hand, self-discharge is understood as the voltage drop on a charged capacitor after a set period of time. Such loss of charge, which may result in dysfunctional conditions, affect the electrochemical response of the capacitor by lowering the power and energy densities. Therefore, the rate of self-discharge has a major practical significance when assessing the performance and specifications of any energy storage device. Self-discharge is influenced by different factors, such as the chemistry and electrochemistry of the system, the purity of reagents and electrolyte and, mainly, the temperature.58 The self-discharging characteristics of OESC-C were determined by considering the following three-step test: (i) the OESC-C was charged to 0.8 V at 2.334 mA; (ii) it was kept at 1·10-11 mA for 10 min (self-discharging); and (iii) the device was discharged to 23 0.2 V at -1 mA. Figure 4f evidences how, for most of the cases, the voltage of OESC- C ended above 0.4 V after the set period of time. Although elucidation of the mechanisms and driving forces that control self-discharge is beyond the scope of this study, results validate the low self-discharging tendency of OESC-C devices, at least in the short term, ensuring specific practical applications. Practical application using a LED bulb. Four OESC-C devices were assembled in series (Figure 5a and Figure S9b-S9c) and subjected to the following GCD measurements: 10 charge-discharge cycles for 30 seconds at 1.38 A/g. Consequently, by assembling four devices the voltage window increases up to 4 V, while curves retain the symmetric shape, and thus the capacitance performance of individual OESC-C (Figure 5b). In a similar way, self-discharging curves for the assembled devices decrease from 4 V to ca. 1.5 V after 10 minutes (Figure 5c). To further confirm the suitability of OESC-C for practical applications, the assembled devices were used to power a red LED (lowest working potential 1.65-1.7 V, Figure 5d). For this purpose, the assembled system was charged to 4.0 V at 1.38 A/g and connected to the LED and two resistances in series (2  100 Ω), while recording the time the LED was lighted. For comparison purposes, this procedure was also applied to four assembled OESC-PBS devices, and repeated five times for each system (videos are provided in the Electronic Supporting Information). Results indicated that when using OESC-C the LED was lit for a longer time (35 ± 5 s) than in the case of control OESC-PBS (20 ± 4 s). Ragone plot. Energy (Emax; Eqn 5) and power (Pmax; Eqn 6) densities, which are important parameters for assessing the supercapacitor performance of energy storage 24 devices, are represented in Ragone plots (i.e. Emax against Pmax) to enable the comparison of different systems.59 Thus, these plots indicate how much energy is available (vertical axis) and how quickly it can be delivered (horizontal axis). The Ragone plot obtained for OESC-C and OESC-PBS (Figure 6) evidences that the two systems display similar energy density (6.1 ± 0.4 and 5.8 ± 1.0 Wh/kg, respectively), whereas the power density is higher for the former than for the latter (1.7 ± 0.5 and 0.8 ± 0.2·kW/kg, respectively). Considering that energy and power densities of supercapacitors for power applications are comprised in the interval between 1-9 Wh/kg and 1-10 kW/kg, respectively,60 the OESC-C system behaves as a good candidate for such application. It is of highly importance to remember that data in the Ragone plot (Figure 6) has to be considered carefully since it is based only on the total mass of active PEDOT electrodes, in accordance to the methodology described in previous works.57 However, as stated by Stoller and Ruoff,39 Pmax should be computed by considering the total mass of the device, which also includes dead components and the electrolyte. Improving the OESC-κC energy storage device Different strategies could be considered to obtain OESC-C devices with higher energy and power densities. On the one hand, a relatively simple strategy to enhance the power density is the design of supercapacitors with compact cell architectures (i.e. reducing the electrolyte volume) to decrease the total mass of the device. On the other hand, the energy density improves by increasing the SC of the device, which can be accomplished by properly modifying the electrode material to display larger specific surface area, higher conductivity, and better pore size distribution to favour ion diffusion. For example, the SC of a symmetrical pseudocapacitor improved substantially 25 after modifying the PEDOT-PSS electrodes with RuO2·xH2O.61 However, although these modifications are known to have satisfactory effects on the performance of the device, they are time-demanding and require additional synthetic routes to alter the properties of PEDOT electrodes.25 In addition to the previous two strategies, another interesting action to raise the SC is based on tailoring the electrolyte element. Thus, the introduction of redox additives into conventional aqueous electrolytes to induce electrochemical activity and reversibility has been described in recent studies.62-64 This modification contributes to the pseudocapacitance of the system through additional redox processes between the electrode and the added electrolyte. Similarly, the energy storage performance of solidstate supercapacitors has been improved adding redox additives to the polymeric electrolyte.55,65,66 Inspired by some of these strategies, the performance of the OESC-C energy storage device has been re-examined after the incorporation of PAni nanofibers (PAninfs) to the electrolyte system. The length and diameter of PAni-nfs, which were prepared using a previously described procedure (ESI),67-70 are 400 and 120 nm, respectively, as determined from SEM micrographs (Figure 7a). On the other hand, the doped state of the ECP was corroborated by examining polaronic bands in the UV-vis spectrum of PAni-nfs solution (Figure 7b).70 OESC-κC devices incorporating PAni-nfs in the hydrogel electrolyte (OESC- κC:PAni-nfs) were fabricated as is described in the Methods section. Specifically, PAninfs were introduced in the -carrageenan hydrogel before the gelation step, thus rendering a hydrogel-based electrolyte with redox additives. Figure 7c compares the unloaded and loaded -carrageenan hydrogels. 32 56. A. J. Bard and L. R. Faulkner, Electrochemical methods: Fundamentals and applications, John Wiley & Sons, New York, USA, 2nd edn, 2001. 57. Y. Xu, Z. Lin, X. Huang, Y. Liu, Y. Huang and X. Duan, ACS Nano, 2013, 7, 4042. 58. H. A. Andreas, J. Electrochem. Soc., 2015, 162, A5047. 59. T. Christen and M. W. Carlen, J. Power Sources, 2000, 91, 210. 60. J. Zang and X. Li, J. Mater. Chem., 2011, 21, 10965. 61. S. A. Hashmi, ACS Appl. Mater. Interfaces, 2013, 5, 3875. 62. H. Yu, L. Fan, J. Wu, Y. Lin, M. Huang, J. Lin and Z. Lan, RSC Adv., 2012 , 2, 6736. 63. S. Roldán, M. Granda, R. Menéndez, R. Santamaría and C. Blanco, J. Phys. Chem. C, 2011, 115, 17606. 64. S. T. Senthilkumar, R. K. Selvan, Y. S. Lee and J. S. Melo, J. Mater. Chem. A, 2013, 1, 1086. 65. J. Zhong, L.-Q. Fan, X. Wu, J.-H. Wu, G.-J. Liu, Ji.-M. Lin, M.-L. Huang and Y.- L. Wei, Electrochim. Acta, 2015, 166, 150. 66. G. Ma, M. Dong, K. Sun, E. Feng, H. Peng and Z. Lei, J. Mater. Chem. A, 2015, 3, 4035. 67. D. Li and R. B. Kaner, Chem. Commun., 2005, 3286. 68. J. Huang and R. B. Kaner, Angew. Chem. Int. Ed., 2004, 43, 5817; Angew. Chem., 2004, 116, 5941. 69. J. Huang and R. B. Kaner, Chem. Commun., 2006, 367. 33 CAPTIONS TO FIGURES Scheme 1. Preparation of OESC-κC:PAni-nfs devices. Figure 1. Cyclic voltammetry using a three-electrode configuration (Figure S5) have been used to determine the following electrochemical properties for PEDOT electrodes using different electrolyte systems: (a) variation of the stored charge, where Qox (left) and Qred (right) refer to oxidation and reduction charges; (b) electrochemical activity, which is defined by the Qred/Qox ratio; and (c) loss of electrochemical activity (LEA) against the number of consecutive redox cycles. Data are the average of three samples for each system. Galvanostatic charge-discharge assays using a two-electrode configuration (Figure S6) have been employed to evaluate the variation of (d) the Coulombic efficiency and (e) the specific capacitance (SC) against the applied current density for OESC devices with different biohydrogel-based electrolytes. Figure 2. Chemical structure and morphology (SEM micrographs) of OESC-C (middle) elements: -carrageenan hydrogel as electrolyte (left column) and PEDOT electrodes (right column). Figure 3. Electrochemical characterization (two-electrode configuration) of OESC- C devices, which present both CE and WE made of PEDOT and -carrageenan hydrogel as electrolyte. (a) Cyclic voltammograms recorded from 0.0 to 0.8 V after five consecutive redox cycles at scan rates of 10, 25, 50, 75, 100, 150 and 200 mV/s. (b) SC values derived from the cyclic voltammograms displayed in (a) (see Eqn 2 and 3). (c) GCD curves recorded from 0.0 to 0.8 V at different current densities. Solid lines correspond to the first charge-discharge cycle, while the dashed ones correspond to the twenty-fifth cycle. (d) SC values derived from the GCD curves displayed in (c) (see Eqn 2 and 3). SC values in (b) and (d) are compared with those obtained for the OESC-PBS 34 control device (Figure S7). In (d) empty symbols refer to the SC values determined for the twenty-fifth charge-discharge cycle. Figure 4. Cycling stability of OESC-C devices, which present both CE and WE made of PEDOT and -carrageenan hydrogel as electrolyte. (a) GCD curves recorded from 0 to 0.8 V at 1.38 A/g (two repetitions). Solid lines correspond to the second cycle, while the dashed ones correspond to the three-thousandth cycle. (b) SC values calculated with the data derived from (a). (c) GCD curves recorded from 0 to 0.8 V at 1.38 A/g for devices tested just as prepared (t0) and after one week of their preparation (t1w). Solid lines correspond to the first cycle, while the dashed ones correspond to the fivehundredth cycle. (d) SC values calculated with the data derived from (c). (e) Leakage current curve for OESC-C charged at 2.334 mA (i.e. 1.38 A/g) and kept at 0.8 V for 300 seconds. (f) Self-discharge curves for OESC-C devices. The procedure employed for these assays is described in the Methods section. Figure 5. (a) Four assembled OESC-C devices, which present both CE and WE made of PEDOT and -carrageenan hydrogel as electrolyte, connected in series to power a red LED (video displayed in the Electronic Supporting Information). (b) GCD curves recorded at 1.38 A/g (charging and discharging times of 30 seconds) for one and four assembled OESC-C devices (black and blue, respectively). (c) Self-discharge curves of four OESC-C devices connected in series. (d) LED powered using the system described in (a). Figure 6. Ragone plot (Emax vs Pmax) for OESC-C and OESC-PBS devices. Figure 7. (a) SEM image of PAni-nfs (100 kX). (b) UV-vis spectrum for a diluted solution of as-prepared PAni-nfs (1/100). (c) -Carrageenan hydrogel with (left) and without (right) PAni-nfs. (d) Cyclic voltammograms for PEDOT in three-electrode configuration recorded from -0.4 to 1.0 V at a scan rate of 50 mV/s using -carrageenan 35 hydrogel loaded with Pani-nfs as electrolyte media. (e) Four OESC-C:PAni-nfs assembled in series to light a red LED. (f) Charging-discharging processes for OESC- C (red squares) and OESC-C:PAni-nfs (blue circles) without (empty symbols) and with LED (filled symbols). 36 Scheme 1 25 mL 4 % w/v -Carrageenan 25 mL 0.5 g PAni-nfs in 0.01 M HCl 80 C 2% w/v κC 1% PAni-nfs (w/w) + 5 mL KCl 1 M 80 C (rpm) (rpm) (rpm) 37 Figure 1 Current density (A/g) 0.0 0.2 0.4 0.6 0.8 1.0 0.0 1.0 2.0 3.0 4.0 5.0 6.0 0.0 20.0 40.0 60.0 80.0 100.0 0.0 1.0 2.0 3.0 4.0 5.0 6.0 0.0 10.0 20.0 30.0 40.0 50.0 010 20 30 40 50 0.00 0.20 0.40 0.60 0.80 1.00 010 20 30 40 50 0.0 10.0 20.0 30.0 40.0 50.0 010 20 30 40 50 0.0 10.0 20.0 30.0 40.0 50.0 010 20 30 40 50 (a) Qox (mC/cm2) # Cycle Qred (mC/cm2) # Cycle 0.0 10.0 20.0 30.0 40.0 50.0 010 20 30 40 50 Control ᴋC Na-Alginate Gelatin PBS Na-alginate 0.0 10.0 20.0 30.0 40.0 50.0 010 20 30 40 50 Control ᴋC Na-Alginate Gelatin -carrageenan gelatin 0.0 10.0 20.0 30.0 40.0 50.0 010 20 30 40 50 Control ᴋC Na-Alginate Gelatin PBS Na-alginate 0.0 10.0 20.0 30.0 40.0 50.0 010 20 30 40 50 Control ᴋC Na-Alginate Gelatin -carrageenan gelatin (b) Qred/Qox (mC/cm2) # Cycle (c) LEA (%) # Cycle 0.0 10.0 20.0 30.0 40.0 50.0 010 20 30 40 50 Control ᴋC Na-Alginate Gelatin PBS Na-alginate 0.0 10.0 20.0 30.0 40.0 50.0 010 20 30 40 50 Control ᴋC Na-Alginate Gelatin -carrageenan gelatin 0.0 10.0 20.0 30.0 40.0 50.0 010 20 30 40 50 Control ᴋC Na-Alginate Gelatin PBS Na-alginate 0.0 10.0 20.0 30.0 40.0 50.0 010 20 30 40 50 Control ᴋC Na-Alginate Gelatin -carrageenan gelatin (d) Coulombic efficiency (e) SC (F/g) Current density (A/g) 0.0 10.0 20.0 30.0 40.0 50.0 010 20 30 40 50 Control ᴋC Na-Alginate Gelatin PBS Na-alginate 0.0 10.0 20.0 30.0 40.0 50.0 010 20 30 40 50 Control ᴋC Na-Alginate Gelatin -carrageenan gelatin 0.0 10.0 20.0 30.0 40.0 50.0 010 20 30 40 50 Control ᴋC Na-Alginate Gelatin PBS Na-alginate 0.0 10.0 20.0 30.0 40.0 50.0 010 20 30 40 50 Control ᴋC Na-Alginate Gelatin -carrageenan gelatin 38 Figure 2 PEDOT-Carrageenan 8 µm 800 nm 2 µm 400 nm 39 Figure 3 0.0 20.0 40.0 60.0 80.0 100.0 0.0 1.0 2.0 3.0 4.0 5.0 6.0 OESC-kC OESC-kC-25 OESC-PBS OESC-PBS-25 0.0 0.2 0.4 0.6 0.8 050 100 150 200 250 300 5.53 A/g 2.76 A/g 1.38 A/g 0.69 A/g 0.28 A/g 0.0 20.0 40.0 60.0 80.0 100.0 050 100 150 200 OESC-kC OESC-PBS (a) j (A/g) Cell voltage (V) -10.0 -6.0 -2.0 2.0 6.0 10.0 -0.1 0.1 0.3 0.5 0.7 0.9 200 10 (b) SC (F/g) Scan rate (mV/s) (c) Cell voltage (V) Time (s) (d) SC (F/g) Current density (A/g) 40 Figure 4 0 15 30 45 60 75 90 0.0 0.1 0.2 0.3 0.4 0.5 0.6 0.7 0.8 010 20 30 40 50 0.0 0.1 0.2 0.3 0.4 0.5 0.6 0.7 0.8 0 110 220 330 440 550 660 0.0 1.0 2.0 3.0 4.0 5.0 6.0 7.0 075 150 225 300 0 15 30 45 60 75 90 t0 t1w 0.0 0.1 0.2 0.3 0.4 0.5 0.6 0.7 0.8 010 20 30 40 50 (c) Cell voltage (V) Time (s) (d) SC (F/g) (e) Current (mA) Time (s) (f) Cell voltage (V) Time (s) t0 t1w 2nd cycle 500th cycle (a) Cell voltage (V) Time (s) (b) SC (F/g) 2nd cycle 3000th cycle 41 Figure 5 0.0 1.0 2.0 3.0 4.0 5.0 0 100 200 300 400 500 600 700 Cell voltage (V) -0.1 1.0 2.0 3.0 4.0 5.0 0 100 200 300 400 500 600 (a) Time (s) (b) (c) Time (s) (d) Cell voltage (V)