scieee AI-readable full text Open interactive document viewer

Unsupervised classification of surface defects in wire rod production obtained by Eddy current sensors

Saludes Rodil, Sergio,Baeyens Lázaro, Enrique,Rodríguez Juan, Carlos

Abstract

Producción Científica

Full text

Sensors 2015,15, 10100-10117; doi:10.3390/s150510100 OPEN ACCESS sensors ISSN 1424-8220 www.mdpi.com/journal/sensors Article Unsupervised Classification of Surface Defects in Wire Rod Production Obtained by Eddy Current Sensors Sergio Saludes-Rodil 1,*, Enrique Baeyens 2and Carlos P. Rodríguez-Juan 3 1Centro Tecnológico CARTIF, Parque Tecnológico de Boecillo 205, 47151 Boecillo, Valladolid, Spain 2Instituto de las Tecnologías Avanzadas de la Producción, Universidad de Valladolid, Paseo del cauce 59, 47011 Valladolid, Spain; E-Mail: [email protected]a.es 3ISEND S.A., Parque Tecnológico de Boecillo, Luis Proust 10, 47151 Boecillo, Valladolid, Spain; E-Mail: [email protected] *Author to whom correspondence should be addressed; E-Mail: [email protected]; Tel.: +34-983-546-521; Fax: +34-983-546-504. Academic Editor: Vittorio M.N. Passaro Received: 5 March 2015 / Accepted: 22 April 2015 / Published: 29 April 2015 Abstract: An unsupervised approach to classify surface defects in wire rod manufacturing is developed in this paper. The defects are extracted from an eddy current signal and classified using a clustering technique that uses the dynamic time warping distance as the dissimilarity measure. The new approach has been successfully tested using industrial data. It is shown that it outperforms other classification alternatives, such as the modified Fourier descriptors. Keywords: dynamic time warping; cluster analysis; modified Fourier descriptors; unsupervised classification; wire rod manufacturing; eddy current inspection; nondestructive testing 1. Introduction Wire rods made using the hot rolling technique can present surface defects. Several techniques have been applied to detect the surface defects that appear during wire rod manufacturing. Approaches based on image processing have been proposed in [1,2]. Alternatively to computer vision-based techniques, the eddy current nondestructive technique is effectively used to detect surface defects [3]. The basic instrument for eddy current inspection is a coil fed with an alternating electric current. The complex impedance of the coil Z0changes in accordance with the eddy current redistribution due to material defects or inhomogeneities [4,5]. Sensors 2015,15 10101 Besides detection, defect classification is of industrial interest, and a great deal of research has been devoted to this issue. Many approaches are based on signal processing or shape characterization followed by a supervised classifier. This implies the use of labeled defect sets covering all possible defect types. A complete knowledge base that includes as many examples as possible of every type of possible defect is crucial to develop a good classification procedure. This is a serious drawback, because it is not always easy nor even possible in industrial practice to collect a number of examples large enough to build a useful knowledge base. There is an interest in developing automated eddy current-based inspection systems able to detect and classify defects. However, the lack of adequate defect collections in hot rolling industrial plants prevents the design of supervised defect classifiers. Motivated by this fact, we proposed an unsupervised classifier that can aid the plant operators to build their knowledge bases and classify and analyze the surface defects appearing in their products. The rest of the paper is organized as follows. In Section 2, the problem of the classification of surface defects obtained by eddy current supervision in the manufacturing of a wire rod is described and formulated. A revision of related work and the main contributions in our work are also included. In Section 3, several methods of unsupervised classification are explained, and the normalized dynamic time warping distance that will be used as a dissimilarity metric between defect sequences is also introduced. The results of an experiment using real data obtained during the production of the wire rod are reported in Section 4. Section 5contains the discussion of the results. Finally, some conclusions are given in Section 6. 2. Description of the Problem 2.1. Eddy Current Inspection in Wire Rod Manufacturing Wire rods are an intermediate steel product of approximately a round solid cross section that is wound into coils and transported in this form. It is primarily used for subsequent drawing and finishing by wire drawers and is ultimately used to manufacture a variety of products, including electric welded chains, cold-drawn bars, springs, nails, reinforcing wire mesh, chain link fence and many different types of wires. Bar and wire rods are produced by hot rolling, and surface defects can appear on rods during the manufacturing process. These defects can be detected by an eddy current inspection system. The layout of a wire rod mill and its inspection system are schematically represented in Figure 1. The eddy current probe is placed at the end of the mill process and operates when the wire is still hot, at around 927 ◦C, depending on the material. The probe used belongs to the differential class and was managed by an ISEND HOTanalyzer system. The authors would like to not disclose the operation details due to confidentiality reasons. The methods presented in this paper are independent of the probe operational parameters. The eddy current inspection system directly acquires impedance measurements from the product line. It isolates the recorded parts where the impedance of the coil probe experiences a change that corresponds to a surface defect. Sensors 2015,15 10102 The inspection signal is a sequence of measurements of the complex impedance: Z0(t) = x(t) + jy(t)(1) A surface defect is a finite subsequence of the complex impedance signal Z0(t). Billet Furnace Rolling mills Eddy current probe Loop lying head Signal Adaptation Rod Wire Figure 1. Layout of a wire rod mill with the eddy current inspection system. The industrial supervision system of Figure 1is continuously collecting measurements and produces a large amount of data that are not possible to analyze by a human operator without the aid of some automatic computer system. Our solution is motivated by the requirements of the operators in a real manufacturing plant and consists of an automatic system that analyzes the eddy current signal recorded during a production batch and extracts every subsequence of interest where the impedance changes. These subsequences are the collection Σof surface defects to be classified. The defect collection Σis classified offline using unsupervised classification methods, and the results are provided to the operators for their posterior analysis. Hence, our solution avoids a very tedious, unpractical and almost unfeasible human classification process and can be considered as an initial step towards an online unsupervised classification system. 2.2. Problem Formulation In order to formalize the problem, the impedance measurement at time tis assumed to belong to a metric space (F, d)where Fis the underlying set and dis the distance on that set. In our case, the set F can be either the complex plane Cor the Euclidean plane R2, which are mathematically equivalent. Let S(F)denote the set of every finite sequence on F. Hence, any defect is modeled as an element of S(F), and the collection of defects is given by: Σ = {xk∈S(F) : k= 1, . . . , K}(2) The problem of interest can be posed as follows: given a collection Σof unlabeled defects corresponding to an unknown number Kof defect types, determine the number Kand find a partition {Σk:k= 1, . . . , N}, such that each defect in the subset Σkbelongs to the same defect type. A partition {Σk:k= 1, . . . , K}of Σsatisfies that Σk⊂Σfor any k,Σj∩Σk=∅for j6=kand ∪K k=1Σk= Σ. The main difficulties in this problem are that the defects are unlabeled, and the different types of defects are unknown in advance. Besides, the sequences representing individual defects have different lengths, even for defects belonging to the same class. The features characterizing different defect classes are related to the shape and orientation of the polar graph of the complex impedance, but Sensors 2015,15 10103 they are independent of the length and scale. These difficulties motivate the use of unsupervised classification methods and the definition of a metric for sequences of different lengths that allows the right classification of defects. The unsupervised classification methods considered are the K-medoids clustering algorithm and the evolving self-organizing map algorithm. As a metric for the dissimilarity of defect sequences, the normalized dynamic time warping distance is used. 2.3. Related Work Classification algorithms for eddy current testing can be arranged into two main categories: 1. Signal processing based: Eddy current signals are processed in order to extract some characteristics from them, allowing differentiating among defect types, as in [6–11]. 2. Shape based: The shape of the eddy current signals in the impedance plane are processed to find out the contours or appearances associated with every type of defect, as in [12–15]. Signal processing-based techniques are the most commonly found in the literature. Every technique in this class processes the eddy current signals in order to obtain a finite set of numeric values that unequivocally characterizes every type of defect. Time-frequency transformation, like wavelet analysis, has been extensively used to process eddy current signals. In [6], several applications to detect defects in nuclear power generation components are reported. In [7], the wavelet analysis is used to enhance the eddy current signals prior to defect detection. Time domain methods have also been proposed [8]. The Hilbert transform [9] and the principal component analysis [10] are some of the techniques used to extract features from the eddy current signals. Furthermore, neural networks have been applied in [11]. Contrarily to signal processing based methods, there are other methods that rely on the shape that the impedance takes in the complex plane. Most of these methods are based on the modified Fourier descriptors [16], which are used to describe closed curves by a finite set of numerical features. This technique is briefly described in Section 3. Modified Fourier descriptors have been applied to classify eddy current signals in [12–15]. 2.4. Main Contributions The main contribution in this paper is an efficient unsupervised method for classifying surface defects in the manufacturing of wire rods using eddy current inspection. This method comprises two key elements. First, a new defect dissimilarity measure for eddy current signals is introduced. This measure uses the normalized dynamic time warping (DTW). Second, a clustering approach that uses the DTW distance is applied in an unsupervised way. The K-medoids clustering algorithm has been successfully tested. In addition, an evolving self-organizing map (ESOM) has been applied to obtain a set of defect prototypes that are later classified using the K-medoids clustering algorithm. A defect is classified by the cluster corresponding to the closest prototype in the DTW distance. The ESOM also uses the normalized DTW measure, and its goal is to obtain a parsimonious representation of the defects collection Σthat can be preserved from a production shift to the next one. The ESOM is evolving with any new defect, but the clustering process is accomplished only once for each shift. The techniques used in this paper are Sensors 2015,15 10104 not new; however, to the knowledge of the authors, they have not been previously used in conjunction to classify surface defects in wire rod manufacturing. The resultant approach has been demonstrated to be very effective and outperforms other alternatives based on modified Fourier descriptors that have been extensively used in feature extraction of signal obtained by eddy current inspection. 3. Methods 3.1. Modified Fourier Descriptors Let x∈S(C)be a finite sequence of complex numbers representing the impedances corresponding to a surface defect. Let N=|x|be the length of the sequence, then: x={xk:k= 1, . . . , N}(3) The sequence xcan be equivalently represented by the Fourier descriptors {fk:k=−N 2+1, . . . N 2}, which are the coefficients of the Fourier transform of x: xk= N 2 X `=−N 2+1 fkej2πk`/N (4) with: fk=1 N N X `=0 x`e−j2πk`/N (5) The defect shape in the impedance plane is completely described by the Fourier descriptors fk. However, they are sensitive to signal transformations, such as translation, scale change and reverse description. An alternative description is proposed in [16] to overcome this drawback. It consists of using nonlinear combinations of the Fourier descriptors: bk=f1+kf1−k f2 1 with k= 2,3,...,N 2−1(6) b1=f2|f1| f2 1 (7) These are the Grandlun’s modified Fourier descriptors. They contain information about shape and are invariant under translation and scale change. Only b1is sensitive to rotation, which provides information about the overall defect phase. The main disadvantage of Grandlun’s modified Fourier descriptors is that they are affected by reverse description, i.e., their value depends on the direction that the defect passes through the probe. To avoid this problem, a modified formulation is proposed in [13]: dk=fkf−k |f1f−1|with k= 1,2,...,N 2−1(8) The Oukhellou modified Fourier descriptors contain information about the shape of the defect and are invariant under translation, scale change and reverse description. Besides, they are also sensitive to rotation changes, so they provide information about the defect phase. Sensors 2015,15 10105 3.2. Dynamic Time Warping Dynamic time warping (DTW) [17,18] is a well-known technique to obtain the optimal alignment between two given time-dependent sequences under certain restrictions. Intuitively, the sequences are warped in a nonlinear fashion to match each other. Let x,y∈S(R2)be two sequences of length N=|x|and M=|y|, respectively, where dis the Euclidean distance in R2. In order to align these sequences using DTW, a matrix N-by-Mis constructed. The element (i, j)of this matrix contains the Euclidean distance d(xi, yj)between the two points xi∈x and yj∈y. A warping path wis a finite sequence of Kpairs of natural numbers w:= {wk∈N×N: k= 1,2, . . . , K}satisfying the following conditions: 1. Path length: the length of the warping path is bounded by : max{N, M} ≤ L≤N+M−1(9) 2. Boundary condition: the initial and final values of the warping path are given by : w1= (1,1) , wL= (N, M)(10) 3. Step size condition: the warping path cannot increase more than one in each dimension : wk+1 −wk∈ {(0,1),(1,0),(1,1)} k= 1, . . . , L −1(11) Let W(x,y)denote the set of all possible warping paths for two finite sequences xand yof elements of the set F. The distance D(w;x,y)of the sequences xand ywith respect to the warping path w∈W(x,y)is defined as: D(w;x,y) := |w| X `=1 dxw`,1, yw`,2(12) Furthermore, an optimal warping path for the sequences xand yis a warping path w∗∈W(x,y) having minimal distance for those sequences with respect to all possible warping paths. The DTW distance D∗(x,y)between the sequences xand yis then defined as the distance of those sequences with respect to an optimal warping path: D∗(x,y) = min {D(w;x,y) : w∈W(x,y)}(13) The optimal path is computed by applying dynamic programming to Equation (12) that defines the distance with respect to the warping path. The DTW distance is sensitive to the length of the sequences. Since the DTW distance is usually applied to sequences of different lengths, it can be normalized dividing by the length of the optimal warping path. The normalized DTW distance between two finite length sequences x,y∈S(F)is defined as: ∆(x,y) = K−1D∗(x,y)(14) where Kis the length of the optimal warping path, i.e.,K=|w|. An algorithm that computes the normalized DTW distance is given in Algorithm 1. Sensors 2015,15 10106 Algorithm 1. Normalized DTW distance. Let x,y∈ F be two finite sequences of lengths N=|x|and M=|y|, respectively. The normalized DTW distance ∆(x,y)is computed as follows: 1. Initialize δ(0,0) = 0,δ(n,0) =∞for n= 1, . . . , N and δ(0,m)=∞for m= 1, . . . , M and compute the terms of the DTW matrix, using the difference equation: δ(n,m)= min{δ(n−1,m), δ(n,m−1), δ(n−1,m−1)}+d(xn, xm) for (n, m)∈ {1, . . . , N}×{1, . . . , M}. 2. Initialize `= 0,v`= (N, M)and compute the sequence v∈N2as follows: while [v`6= (1,1)], repeat: `=`+ 1, v`∈arg min{δv:v∈ {v`−1−(1,0), v`−1−(0,1), v`−1−(1,1)}} end while loop then K=|v|and w∗={w`:w`=sK−`+1(v)}. 3. The normalized DTW distance between the sequences xand yis ∆(x,y) = K−1δ(N,M). 3.3. The K-Medoids Algorithm Clustering methods are used to classify a collection of objects Σinto different classes without human intervention. A well-known hard clustering method is the given by the K-medoids algorithm [19]. Each cluster is represented by a vector selected among the elements Σ, which is a set of sequences to be classified into Kgroups. The representative element of each class is called a medoid. Apart form its medoid, each cluster contains all sequences in Σthat are not used as medoids in other clusters and lie closer to its medoid than to the medoids representing the other clusters. An algorithm to perform K-medoids clustering is given in Algorithm 2. 3.4. The Evolving Self-Organizing Map The evolving self-organizing map (ESOM) [20,21] is used to obtain a parsimonious representation of a given set of elements Σin terms of a reduced number of prototype elements and certain relationships between them. The ESOM is an evolving version of the self-organizing map (SOM). The main differences are that no topological constraint is given a priori for the feature map and that prototype elements are not organized onto a lattice. The ESOM is represented by a graph, where each prototype element is a node or vertex, and the relationships are represented by edges of different weights. The ESOM provides a preserving topology representation of the input space in terms of a reduced number of defect prototypes. This representation contains the relevant information about the defect classes that is preserved among production shifts. Sensors 2015,15 10107 Algorithm 2. K-medoids algorithm. Let ∆(x,y)denote the distance between two elements x,y∈Σ. 1. Choose an arbitrary partition PK={Σk:k= 1, . . . , K}of Σand an arbitrary set of medoids Λ = {m(Σk)∈Σk:k= 1, . . . , K}. 2. For every Σk∈ PK, compute the elements that are wrongly classified, i.e., x∈Σksatisfying ∆(x, m(Σj)) <∆(x, m(Σk)) for Σj6= Σk. For these elements, update the partition as follows: Σ0 k= Σk− {x}and Σ0 j= Σj+{x}. The resultant partition is P0 K={Σ0 k:k= 1. . . . , K}. 3. Obtain the medoids set Λ0={m(Σ0 k):Σ0 k∈ P0 K}for the new partition P0 Kby solving the following Koptimization programs: m(Σ0 k)∈arg min{max{γk: ∆(x,y)≤γk,y∈Σ0 k}:x∈Σ0 k},Σ0 k∈ P0 K 4. If the medoids set does not change, i.e., if Λ0= Λ, then the clustering process is completed. Otherwise, do Λ=Λ0, and go to Step 2. The ESOM network starts without any vertex. During learning, the network is updated to capture the on-line incoming data, creating new nodes and edges when necessary. Edges are used to maintain the neighborhood relationships between close nodes. The connection strength is determined by the distance between connected nodes. If the distance is large, the edge weight is weak and it can be disregarded. In this way, the feature map can be split apart, and data structures, such as clusters and outliers can emerge. The ESOM network is characterized by a triplet: N= (V,E, s)(15) where V ⊂ S(R2)is the vertex set containing the prototype nodes, E ⊂ V × V is the edge set and s:E → Ris a function that provides the edge weights. For a set of defects Σ, the ESOM is obtained by applying an iterative algorithm with a set of parameters P={, σ, γ, τ}. The parameter controls the distance between different prototypes; γis the learning rate; σcontrols the spread of neighborhood; and τis used for the preservation of the weakest connections. Usually σ=[20]. The learning process can be summarized in Algorithm 3. Sensors 2015,15 10108 Algorithm 3. Evolving self-organizing map. 1. Start with k= 0,V=∅,E=∅. 2. Choose a new x∈Σand compute: Vm(x) = {y∈ V : ∆(x,y)< }(16) If Vm(x) = ∅go to 4. 3. Update: V0=V ∪ {x}(17) E0=E ∪ {(x,y1),(x,y2)}(18) where: ∆(x, y1) = min{y:y∈ V} (19) ∆(x, y2) = min{y:y6=y1,y∈ V} (20) and go to 5. 4. Let y∗be such that: ∆(x,y∗) = min{∆(x,y) : y∈ Vm}(21) and N(y∗) = {y: (y,y∗)∈ E}. Update: V0={φ(y) : y∈ V} (22) where: φ(y) = ((1 −α)y+αx y ∈ {y∗}∪N(y∗) yotherwise (23) and: α=γe−|∆(z,x)|2/2σ2(24) 5. Update the connection strengths as follows: s(yi,yj) = /∆(yi,yj)(25) for any (yi,yj)∈ V0× V0and i6=j. 6. Do k0=k+ 1; if mod (k0, τ)=0, remove the weakest connection. 7. Do k=k0,V=V0and E=E0, and go to 2. The distance between sequences ∆(x,y)is obtained using the DTW. Besides, since the sequences have different lengths, the sum operation in Equation (23) is not trivial, but it can be computed using the Sensors 2015,15 10115 in the ESOM network by a number of prototypes and their connections. Hence, a large database of defects need not be stored. 6. Conclusions An efficient new unsupervised method for classifying surface defects in wire rod manufacturing has been developed. The defects are obtained by an eddy current inspection system. The new method is based on the DTW distance, which is used to measure the dissimilarity between the defects and uses an evolving self-organizing map to obtain a representative set of defect prototypes for each production shift. These prototypes are later classified using a K-medoids clustering algorithm. The performance of the new method was demonstrated using a collection of real defects obtained in a manufacturing plant. This collection of defects was labeled by experts. The proposed method outperforms the classification methods based on modified Fourier descriptors that have also been applied to classify eddy current signals. The developed method was conceived of as a computer tool to be applied offline, after a production shift, and to help the plant operators to automatically discover and classify the possible surface defects in the manufactured product. The DTW properties allows the method to deal with possible changes in production speed and the different sizes of defects belonging to the same class. Acknowledgments This work has been partially supported by the Spanish Ministry of Economy and Competitiveness through the INNPACTO program, Project Code IPT–2012–0755–420000. The authors would like to thank Bruno Chedal Anglay and Karen Gallardo, who are with Global Steel Wire S.A., for granting access to data and providing technical support in labeling defects. Author Contributions Sergio Saludes-Rodil proposed the idea. Enrique Baeyens and Sergio Saludes-Rodil arranged the methods. Carlos P. Rodíguez-Juan gathered and prepared the data. All of the authors analyzed the results and revised the paper. Conflicts of Interest The authors declare no conflict of interest. References 1. Li, J.; Shi, J.; Chang, T. On-line seam detection in rolling processes using snake projection and discrete wavelet transform. J. Manuf. Sci. Technol. 2007,129, 926–933. 2. Yun, J.P.; Choi, D.; Jeon, Y.; Park, C.; Kim, S.W. Defect inspection system for steel wire rods produced by hot rolling process. Int. J. Adv. Manuf. Technol. 2014,70, 1625–1634. 3. Blitz, J. Electrical and Magnetic Methods of Non-Destructive Testing; Springer: Berlin/Heidelberg, Germany, 1997; Volume 3. Sensors 2015,15 10116 4. Rajesh, S.N.; Udpa, L.; Udpa, S.S. Numerical model based approach for estimating probability of detection in NDE applications. IEEE Trans. Magn. 1993,29, 1857–1860. 5. McMaster, R.C. Nondestructive Testing Handbook; American Society for Nondestructive Testing, Ronals Press: New York, NY, USA, 1959. 6. Grman, J.; Ravas, R.; Syrova, L. Application of wavelet transformation in eddy current testing of steam generator tubes. In Proceedings of the IEEE Instrumentation and Measurement Technology Conference, Budapest, Hungary, 21–23 May 2001. 7. Ma, X.; Peyton, A.J. Feature detection and monitoring of eddy current imaging data by means of wavelet based singularity analysis. NDT E Int. 2010,43, 687–694. 8. Udpa, L.; Ramuhalli, P.; Benson, J.; Udpa, S. Automated analysis of eddy current signals in steam generator tube inspection. In Proceedings of the 16th WCNDT 2004—World Conference on NDT, Montreal, Canada, 30 August–3 September 2004. 9. Chen, T.; Tian, G.Y.; Sophian, A.; Que, P.W. Feature extraction and selection for defect classification of pulsed eddy current NDT. NDT E Int. 2008,41, 467–476. 10. Sophian, A.; Tian, G.Y.; Taylor, D.; Rudlin, J. A feature extraction technique based on principal component analysis for pulsed eddy current NDT. NDT E Int. 2003,36, 37–41. 11. De Mesquita, R.N.; Ting, D.K.S.; Cabral, E.L.L.; Upadhyaya, B.R. Classification of steam generator tube defects for real-time applications using eddy current test data and Self-Organising Maps. Real-Time Syst. 2004,27, 49–70. 12. Lord, W.; Satish, S.R. Fourier Descriptor Classification of Differential Eddy Current Probe Impedance Plane Trajectories. In Review of Progress in Quantitative Nondestructive Evaluation; Springer-Verlag US: La Jolla, CA, USA, 1984; Volume 3A, pp. 589–603. 13. Oukhellou, L.; Aknin, P. Modified Fourier Descriptors: A new parametrisation of eddy current signatures applied to the rail defect classification. In Proceedings of the III International Workshop on Advances in Signal Processing for Non Destructive Evaluation of Materials, Québec City, Quebec, Canada, 5–8 August 1997. 14. Lingvall, F.; Stepinski, T. Automatic detecting and classifying defects during eddy current inspection of riveted lap-joints. NDT E Int. 2000,33, 47–55. 15. Smid, R.; Docekal, A.; Kreidl, M. Automated classification of eddy current signatures during manual inspection. NDT E Int. 2005,38, 462–470. 16. Granlund, G.H. Fourier Preprocessing for Hand Print Character Recognition. IEEE Trans. Comput. 1972,21, 192–201. 17. Sakoe, H.; Chiba, S. Dynamic Programming Algorithm Optimization for Spoken Word Recognition. IEEE Trans. Acoust. Speech Signal Process. 1978,ASSP-26, 43–49. 18. Ten Holt, G.A.; Reinders, M.J.T.; Hendriks, E.A. Multi-dimensional dynamic time warping for gesture recognition. In Proceedings of the Thirteen Annual Conference of the Advanced School for Computing and Imaging, Zeewolde, The Netherlands, 13–15 June 2007. 19. Theodoridis, S.; Koutrumbas, K. Pattern Recognition, 4th ed.; Academic Press: Waltham, MA, USA, 2009. Sensors 2015,15 10117 20. Deng, D.; Kasabov, N. Evolving Self-organizing Maps for On-line Learning, Data Analysis and Modelling; The Information Science Discussion Paper Series, University of Otago: Dunedin, New Zealand, 2000. 21. Deng, D.; Kasabov, N. On-line pattern analysis by evolving self-organizing maps. Neurocomputing 2003,51, 87–103. 22. Von Luxburg, U. A tutorial on spectral clustering. Stat. Comput. 2007,17, 395–416. 23. Rousseeuw, P.J. Silhouettes: A graphical aid to the interpretation and validation of cluster analysis. J. Comput. Appl. Math. 1987,20, 53–65. 24. Zahn, C.T. Graph-Theoretical Methods for Detecting and Describing Gestalt Clusters. IEEE Trans. Comput. 1971,C-20, 68–86. c 2015 by the authors; licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution license (http://creativecommons.org/licenses/by/4.0/).