scieee AI-readable full text Open interactive document viewer

Production of molecular weight fractionated hemicelluloses hydrolyzates from spent coffee grounds combining hydrothermal extraction and a multistep ultrafiltration/diafiltration

Ramos Andrés, Marta,Andrés Iglesias, Cristina,García Serna, Juan

Abstract

Producción Científica

Full text

Elsevier Editorial System(tm) for Bioresource Technology Manuscript Draft Manuscript Number: BITE-D-19-03822R3 Title: Production of molecular weight fractionated hemicelluloses hydrolyzates from spent coffee grounds combining hydrothermal extraction and a multistep ultrafiltration/diafiltration Article Type: Original research paper Keywords: coffee; polysaccharides; autohydrolysis; membrane; supercritical CO2 Corresponding Author: Professor Juan Garcia-Serna, Ph.D. Corresponding Author's Institution: University of Valladolid First Author: Marta Ramos-Andrés, MEng. Order of Authors: Marta Ramos-Andrés, MEng.; Cristina Andrés-Iglesias, PhD.; Juan Garcia-Serna, Ph.D. Abstract: Spent coffee grounds are a huge residual stream from instant coffee makers. The production of spent coffee oil and molecular weight fractionated hemicellulose hydrolysates via supercritical CO2 and a hydrothermal treatment followed by concentration, separation, and purification through cascade ultrafiltration/diafiltration (30-10-5 kDa) was studied. Hemicelluloses extraction yield reached 3.49 g/100 g of dry defatted spent coffee after 40 min at 160 ºC. The ultrafiltration system allowed concentrating up to 5-fold certain groups of hemicellulose, being most of them retained in the first membrane. Hemicellulose concentration and molecular weight of the feed exerted a great influence on the mass transfer through the membrane due to the formation of aggregates. However, purification through diafiltration allowed both to decrease byproducts retentions from 45.6% to 8.7%, increasing the molecular weight of each fraction. Six hemicellulose products were obtained with purities between 83.7 - 97.8 wt% and weight-average molecular weights between 1641 and 49733 Da. Research Data Related to this Submission -------------------------------------------------- Title: Data for: Production of molecular weight fractionated hemicelluloses hydrolysates from spent coffee grounds combining hydrothermal extraction and a multistep ultrafiltration/diafiltration Repository: Mendeley Data https://data.mendeley.com/datasets/dwsxfrmrzp/draft?a=5e97bdd7-9771-4586- 8748-c233cc4b5456 Manuscript Number: BITE-D-19-03822R1 Manuscript Title: Production of molecular weight fractionated hemicelluloses hydrolyzates from spent coffee grounds combining hydrothermal extraction and a multistep ultrafiltration/diafiltration Article Type: Original research paper Comments: We appreciate the editor’s helpful comments. The latest modifications have been marked in green in the manuscript. According to instructions on supplementary material, a sentence like "The ATR-FTIR spectra of spent coffee grounds oil and spent coffee grounds before and after extractions were determined (E-supplementary data of this work can be found in online version of the paper)." cannot be accepted. The part between brackets must simply be deleted. It was deleted as indicated. *Detailed Response to Reviewers Graphical Abstract (for review) HIGHLIGHTS  Spent Coffee Grounds supercritical CO2 defat and hydrothermal hydrolysis  Concentration of target groups of hemicelluloses up to 5-fold by ultrafiltration  Separation of hemicelluloses in three fractions by a cascade ultrafiltration system  Purification of fractionated hemicelluloses by diafiltration reusing water  Reduction of the concentration of not target hemicelluloses by diafiltration *Highlights (for review) 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 1 Production of molecular weight fractionated hemicelluloses 1 hydrolyzates from spent coffee grounds combining 2 hydrothermal extraction and a multistep 3 ultrafiltration/diafiltration 4 Marta Ramos-Andrés, Cristina Andrés-Iglesias and Juan García-Serna* 5 High Pressure Processes Group, BioEcoUVa Research Institute on Bioeconomy and 6 Department of Chemical Engineering and Environmental Technology, 7 EII Sede Mergelina, University of Valladolid, 47011, Valladolid, SPAIN 8 * Corresponding author, Tel.: +34983184934, e-mail: [email protected] 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 *Manuscript Click here to view linked References 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 2 Abstract 27 28 Spent coffee grounds are a huge residual stream from instant coffee makers. The 29 production of spent coffee oil and molecular weight fractionated hemicellulose 30 hydrolysates via supercritical CO2 and a hydrothermal treatment followed by 31 concentration, separation, and purification through cascade ultrafiltration/diafiltration 32 (30-10-5 kDa) was studied. Hemicelluloses extraction yield reached 3.49 g/100 g of dry 33 defatted spent coffee after 40 min at 160 ºC. The ultrafiltration system allowed 34 concentrating up to 5-fold certain groups of hemicellulose, being most of them retained 35 in the first membrane. Hemicellulose concentration and molecular weight of the feed 36 exerted a great influence on the mass transfer through the membrane due to the 37 formation of aggregates. However, purification through diafiltration allowed both to 38 decrease by-products retentions from 45.6% to 8.7%, increasing the molecular weight 39 of each fraction. Six hemicellulose products were obtained with purities between 83.7 – 40 97.8 wt% and weight-average molecular weights between 1641 and 49733 Da. 41 42 Keywords: coffee; polysaccharides; autohydrolysis; membrane; supercritical CO2 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 3 1. Introduction 58 Spent coffee grounds are one of the main organic wastes from the food industry the 59 opportunity of revalorization is huge. In both the preparation of a coffee beverage and 60 in the production of soluble coffee, the coffee is subjected to extraction with hot water 61 or steam for the release of several substances that are transferred to the liquid phase. 62 The solid residue of this process is known as spent coffee grounds. Worldwide, coffee is 63 the second-largest commodity, being a 50 % of its worldwide production destined for 64 the manufacture of soluble coffee which generates around 6 million tons of spent 65 coffee grounds per year (Ballesteros et al., 2014). This waste is currently burned to 66 produce energy (e.g. in cement production) or dumped in the landfills but these options 67 have disadvantages. Thus, incineration only recovers part of the energy and emit 68 polluting gases into the atmosphere, and the deposition in landfills means (1) occupying 69 a space with waste instead of using it for other purposes such as cultivation, (2) 70 emission of odors associated with fermentation processes, and (3) release into the 71 environment of substances of certain toxicity such as caffeine, tannins and polyphenols 72 (Melo et al., 2014). In this sense, due to environmental problems that affect our society, 73 it is necessary to look for alternative resources for the production of high value-added 74 products being these resources, renewable and non-polluting. In addition, it is desirable 75 that their use as biomass raw material (RM) does not compete with any other possible 76 application such as the food industry. 77 In recent years several studies have been focused on the valorization of spent coffee 78 grounds looking for alternative uses. Due to this, several compounds of interest have 79 been extracted, mainly coffee oil (Jin et al., 2018; Loyao et al., 2018), carbohydrates 80 (Getachew et al., 2018; Nguyen et al., 2019), and bioactive compounds (Pettinato et al., 81 2019; Shang et al., 2017). Coffee oil has applications as additive in cosmetic 82 formulations, in the manufacture of biodiesel and in the bioproduction of 83 polyhydroyalkanoates; coffee carbohydrates can be used as both, food and 84 pharmaceutical additives, and also as carbon source in biotechnology; bioactive 85 compounds have applications as supplements and in pharmacy due to their antioxidant, 86 antibacterial, antiviral, anti-inflammatory and anticarcinogenic properties (Campos-87 Vega et al., 2015; Zabaniotou and Kamaterou, 2018). The solid residue after the 88 extraction of these valuable compounds has also applications such as filler for polymers, 89 adsorbent, biochar, bio-oil, fuel, and compost (Kovalcik et al., 2018). 90 Among the mentioned compounds, the extraction of carbohydrates from spent coffee 91 grounds is of great interest as cellulose and hemicellulose constitute approximately 45% 92 of the weight of the RM (Campos-Vega et al., 2015). In spent coffee grounds, 93 hemicelluloses are heterogeneous carbohydrates generally formed by hexoses 94 (mannose, galactose, and glucose) and pentoses (arabinose) (Campos-Vega et al., 95 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 4 2015). Consequently, the types of hemicelluloses that may be mainly present are 96 glucomannan and galactoglucomannan. Galactomannans are high molecular weight 97 polysaccharides with a low level of branching, composed of a backbone of mannose 98 containing single galactose side groups. Depolymerization and debranching of 99 galactomannans occur during the roasting process increasing their solubility in water 100 (Ballesteros et al., 2017). It should be noted that about 70 wt% of the hemicelluloses 101 glucomannan and galactoglucomannan remain in the spent coffee grounds matrix after 102 the coffee brewing process or during soluble coffee production (Zabaniotou and 103 Kamaterou, 2018). 104 After the extraction, hemicelluloses can exhibit different configurations such as 105 monomeric, oligomeric, and polymeric with different degrees of polymerization. The 106 properties and, therefore, the industrial applications will be different depending on 107 their configuration and molecular weight distribution. In monomeric form, 108 hemicelluloses are known for their applications in the production of biochemicals, 109 biosugars, and energy (Baptista et al., 2018; Dutta and Chakraborty, 2018; Luo et al., 110 2019); in their oligomeric form, hemicelluloses are used as feed and pharmaceutical 111 additives (Samanta et al., 2015); and in their polymeric form, hemicelluloses have 112 applications in food packaging, hydrogels, and thermoplastics (Farhat et al., 2018; 113 García-Uriostegui et al., 2018; Liu et al., 2019). With regards to hemicelluloses extracted 114 from spent coffee, films formed from glucomannan have proven to have interesting 115 properties such as good gas barrier, flexibility, and mechanical strength, making them 116 suitable for food packaging (Fortunati et al., 2016). Hydrogels with drug-delivery 117 applications have also been developed from galactoglucomannan (Voepel et al., 2009). 118 In their oligomeric form, mannooligosaccharides from spent coffee have been produced 119 by hydrothermal treatment at 220 ºC, with further monosaccharides removal by carbon 120 chromatography (Takao et al., 2006). The major mannooligosaccharides were 121 mannobiose (19 %), mannotriose (27 %), mannotetraose (21 %) and mannopentose (17 122 %). These oligosaccharides had good effects reducing abdominal and subcutaneous fat 123 accumulation in humans when administered daily. The bioactivity of these 124 hemicelluloses, associated with their oligomeric form, was also studied by Getachew 125 and Chun (2017) through a reduction of molecular weight by hydrothermal treatment in 126 a semi-continuous reactor. Hemicelluloses from coffee were extracted by alkaline 127 treatment, being less than 5% of the total hemicelluloses in monomeric form. The 128 modified hemicelluloses obtained by hydrothermal treatment at 180 and 220 ºC 129 showed a much higher antioxidant capacity. 130 The high valuable hemicelluloses can be extracted by different extraction methods: 131 dilute acid extraction, hot water extraction, steam explosion extraction, alkali 132 extraction, dilute acid steam explosion extraction, organic solvents extraction, and 133 microwave-assisted extraction. Both dilute acid extraction and alkaline extraction are 134 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 5 among the most commonly used, as hemicelluloses can be extracted in both alkaline 135 and acid solutions (Fortunati et al., 2016). These extractions give rise to quite defined 136 hemicelluloses whose molecular weight range is not very wide, with polydispersity 137 values usually lower than 2. On the contrary, the extraction of hemicelluloses by 138 hydrothermal treatment can produce a wide variety of molecular weights in 139 hemicelluloses depending on the severity of the treatment. 140 The variety of molecular weights in the hemicelluloses that can be extracted by 141 hydrothermal treatment makes necessary a downstreaming process that allows both to 142 obtain hemicelluloses of adequate purity and to separate them depending on the 143 molecular weight. The most common downstream processes are precipitation with 144 ethanol and chromatography. However, following the philosophy of respect for the 145 environment, it is worth noting the use of ultrafiltration (UF) membranes. Although the 146 fractions of hemicelluloses obtained by membranes are more heterogeneous (Peng et 147 al., 2012), this separation process has multiple advantages, as low energy requirements, 148 mild operating conditions, no chemicals are required except for cleaning, and the 149 equipment has a simple and easily scalable design (Nayak and Bhushan, 2019). 150 Ultrafiltration/Diafiltration (UF/DF) has been used by several authors in different types 151 of biomass to obtain different hemicellulose fractions. Thuvander and Jönsson (2016) 152 used downstream processing of galactoglucomannan-type hemicelluloses from the 153 process water from a thermomechanical pulp mill with spruce as primary RM. The 154 process was carried out using a cascade system of prefiltration, microfiltration and UF. 155 The concentration was increased thanks to UF from 0.85-1.5 g/L to 25-52 g/L, using a 156 high feed volume reduction of up to 98%. Likewise, in a later study of the same authors, 157 they used diafiltration (DF) to purify the previously ultrafiltered hemicelluloses, but the 158 desired effect was not achieved since the percentage of retention of hemicelluloses and 159 lignin in the membrane was very similar, not achieving the separation between them 160 (Thuvander et al., 2016). Laine et al. (2015) carried out extraction by alkaline hydrolysis 161 with NaOH from both wood pulp and brewer’s spent grain. It was demonstrated that 162 their UF/DF system allows not only to separate and purify the hemicelluloses but also to 163 recover and recirculate part of the NaOH used in the extraction. 164 González-Muñoz et al. (2013) used a hemicelluloses concentration and DF system 165 composed of 5 membranes in cascade with molecular weight cut-off (MWCO) of 10, 5, 166 3, 1 and 0.3 kDa. With this system, they were able to separate and purify the 167 hemicelluloses obtained by hydrothermal treatment from Pinus pinaster wood. The 168 initial concentration of hemicelluloses in the autohydrolysis liquor was 17.92 g/L, 169 meanwhile, the concentration of the hemicellulose fractions obtained after the 170 downstream process was in the range 1.08-6.01 g/L. This decrease in concentration is 171 normal due to obtaining several fractions from a single feed. The purity was increased 172 from 69.4 wt% in the feed liquor to values between 80.5-90.3 wt% in the diafiltered 173 fractions, which also had different molecular weight distributions. 174 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 12 The yield of coffee oil reached by scCO2 was 14.04 % of the dry RM, which represents a 394 70.2 % of the extraction yield obtained by Soxhlet hexane extraction. Similar results 395 were obtained by Andrade et al. (2012) whose yield was 10.5 % (dry RM) using scCO2 396 extraction. On the other hand, their extractions with other methods such as ultrasound 397 and Soxhlet resulted in yields ranging between 9 and 15 %. Also, Couto et al. (2009) 398 performed a scCO2 extraction of coffee oil during 3 h that resulted in a yield up to 85% 399 compared to the yield reached through Soxhlet hexane extraction. The lower extraction 400 yield in the present work compared to Couto et al. could be due to a lower extraction 401 time (2 h in present work vs. 3 h). In addition, it should be noted that the amount of oil 402 present in the spent coffee grounds can vary depending on the type of coffee, roasting 403 conditions, and the brewing process (Andrade et al., 2012). 404 The main lipids in spent coffee grounds of this research were free fatty acids (58.00 wt% 405 ± 1.00) and triglycerides (32.00 wt% ± 2.00). In addition, the minor components 406 detected were: short-chain esters (0.50 wt% ± 0.10), long-chain esters (6.60 wt% ± 407 0.70), diglycerides (1.71 wt% ± 0.03) and monoglycerides (1.26 wt% ± 0.05). 408 Transformation of spent coffee oil into biodiesel has been studied through direct 409 transesterification into fatty acid methyl esters with short-chain alcohols such as 410 methanol by many research groups. However, this oil can contain high levels of free 411 fatty acids, which is a disadvantage in the transesterification process. The free fatty 412 acids can give rise to soap by-products during the alkali-catalyzed process because they 413 neutralize the catalyst, resulting in the formation of unwanted emulsions. In addition, 414 the presence of free fatty acids is responsible for the high degree of viscosity of the 415 spent coffee oil, which hinders the mixing during the reaction as well as reduces the 416 separation yield between the biodiesel and the glycerol formed. To overcome the 417 problem of free fatty acid, Al-Hamamre et al. (2012) implemented a two-stage 418 transesterification process including a first stage catalyzed by acid prior to the alkali-419 catalyzed stage. In certain cases, the biodiesel obtained through this double 420 transesterification process did not meet the NP EN 14214:2009 standards, so it has to 421 be cut either with other vegetable oils or with other biodiesel (Caetano et al., 2014). 422 Tuntiwiwattanapun et al. (2017) developed a process of direct transesterification of the 423 spent coffee, without the need to extract the oil, resulting in a biodiesel yield of 77 %. In 424 this process, methanol wash was carried out to reduce the content of free fatty acids, 425 and the influence of temperature, reaction time and particle size on the biodiesel yield 426 were studied. Methanol was separated by flash distillation, and biodiesel was recovered 427 from glycerol by adding hexane, which was later also removed by flash distillation. 428 Determination of fatty acids profile showed a content of 45.1 ± 0.3 % in saturated fatty 429 acids, 11.40 ± 0.04 % in monounsaturated fatty acids and 43.4 ± 0.3% in 430 polyunsaturated fatty acids. The major fatty acids were linoleic acid C18:2n-6 (42.1 ± 431 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 13 0.3%), palmitic acid C16:0 (33.6 ± 0.2%), oleic acid C18:1n-9 (10.47 ± 0.02%), stearic 432 acid C18:0 (7.27 ± 0.08%) and arachidic acid C20:0 (3.23 ± 0.02%), among others. 433 Campos-Vega et al. explained that spent coffee grounds can be divided into two types 434 of oil depending on the ratio between saturated and polyunsaturated fatty acids. Since 435 in this case, the unsaturated/saturated ratio is 1.11, this oil could be considered as less 436 atherogenic and thrombogenic than those with ratio <1 (Campos-Vega et al., 2015). 437 Furthermore, spent coffee grounds oil with a very similar composition to the one 438 obtained in this study (also extracted by scCO2) was used in the synthesis of 439 biodegradable polymers with high yield (0.77 g polyhydroxyalkanoates/kg spent coffee 440 grounds oil) (Obruca et al., 2014). 441 3.3. Extraction of hemicelluloses and by-products 442 The extraction yield was determined by dividing the mass of hemicelluloses extracted 443 by the total amount of carbohydrates in the RM (holocellulose). The accumulated yield 444 evolves slightly asymptotically over time, reaching a maximum value 9.96 wt% when the 445 extraction was carried out at 160°C (logRo = 3.37), and a maximum of 8.22 wt% at 140 446 °C (logRo = 2.78). This relatively low yield may be due to several factors: (1) the repellent 447 effect of the oil, which was not completely removed and may suppose an obstacle in 448 the extraction of hemicelluloses; and/or (2) spent coffee grounds could require a higher 449 temperature than the one used in the production of soluble coffee or in the coffee 450 brewing process so that the previously unextracted polysaccharides were extracted 451 now, as recently demonstrated by Pedras et al. (2019). L F Ballesteros et al. (2017) 452 extracted the hemicelluloses from spent coffee grounds through autohydrolysis without 453 previous extraction of oil, and their maximum accumulated yield was 5.72 wt% (logRo = 454 3.83). The hemicelluloses recovered at these conditions were arabinogalactans and 455 galactomannans. 456 Although the hemicelluloses extraction yield could have been higher if more lipids had 457 been removed, the extraction with scCO2 is the most appropriate option. The yield of oil 458 extraction was high in relation to the time (70 % in 2 h). In addition, as already 459 mentioned, some of the most important potential application of hemicelluloses are in 460 the food, cosmetics and pharmaceutical industries, so it is very important to avoid any 461 toxicity or smell of the product. Due to this, scCO2 has the great advantage of having 462 low toxicity and no-smell in relation to other solvents such as hexane. Furthermore, it 463 allows operating at low temperatures which reduce the risk of thermal degradation of 464 components present in the spent coffee grounds and has a low cost compared to other 465 solvents. 466 The cumulative extraction of hemicelluloses and by-products, taking the RM in the dry 467 base as reference, is shown in Fig 3a. The extraction of by-products was low and 468 remained approximately constant over time. The extracted hemicelluloses, therefore, 469 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 14 had a relatively high purity due to the low presence of sugars, aldehydes and 470 degradation products, which were probably mostly extracted in the soluble coffee 471 production process. Within the temperature range of this study, a higher extraction 472 temperature in spent coffee grounds results in slightly higher extraction of both 473 hemicelluloses and by-products. Mayanga-Torres et al. (2017) obtained an accumulated 474 yield of 8.8 g/100 g RM through autohydrolysis (175 ºC, 36 min, 22.5 MPa, logRo = 3.76), 475 also using a flow-through reactor system with a residence time of 9 min. In our study, 476 the residence time was 12 min and the maximum cumulative yield obtained was 3.49 477 g/100 g RM. This lower yield value can be attributed to milder conditions of both 478 pressure and temperature during extraction, as well as, lower presence of 479 carbohydrates in the spent coffee grounds. 480 Regarding the extracted by-products, the main ones were acids, followed by sugars and 481 aldehydes, as can be seen in Fig. 3b. Also, degradation products (furfural and 5-HMF) 482 are released during extraction with very low yields (up to 0.02 g/100 g). The higher 483 temperature (160 °C) led to a higher content of organic acids due to the hydrolysis of 484 high molecular weight hemicelluloses already extracted into lower molecular weight 485 hemicelluloses. The rest of the by-products were also in greater proportion when the 486 temperature was higher. 487 Previous studies showed that hydrothermal treatment could be tailored towards the 488 selective recovery of hemicelluloses and the reorganization of the remaining cellulose 489 and lignin fractions with improved morphological characteristics (Nitsos et al., 2016, 490 2013). In these studies the severity factor was in the range logRO = 1.90 – 4.69, where a 491 good correlation between hemicelluloses yield extraction and logRO was obtained. 492 However, it was demonstrated that at the same logRO values, hydrolyzates with 493 different composition and molecular weight can be obtained. In the present study, low 494 severity values were used: in the extraction at 140 ºC logRO = 2.02, 2.35, 2.65 and 2.78 495 were analyzed, while at 160 ºC logRO = 2.61, 2.94, 3.24 and 3.37 were analyzed. 496 According to these values and to the evolution in the extraction of hemicelluloses and 497 by-products (Fig. 3a), purity was always higher in the points studied at 140 ºC than 498 those at 160 ºC, even though the logRO was of a very similar order. At both 499 temperatures, the highest purity was obtained for the highest logRO (2.78 for 140 ºC 500 and 3.37 for 160 ºC). This higher purity could be attributed to the higher extraction 501 time, where the extraction by-products increased in much smaller magnitude than the 502 extraction of hemicelluloses. 503 3.4. Molecular weight distribution of extracted hemicelluloses 504 Fig. 4 shows the evolution of the molecular weight distribution of the hemicelluloses at 505 the outlet of the flow-through reactor. At the beginning of extraction (Fig. 4a) the 506 presence of hemicelluloses was higher in the 160 °C extract than in the 140 °C extract, 507 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 15 except for those hemicelluloses > 30 kDa. After 15 minutes of extraction (Fig. 4b), 508 hemicelluloses > 30kDa obtained at 160 °C (logRo = 2.94) were fully hydrolyzed to 509 hemicelluloses of lower molecular weights. On the other hand, the 140 °C extract (logRo 510 = 2.35) still maintained hemicelluloses > 30 kDa. At this time, the total concentration of 511 hemicelluloses decreased considerably in the 160 °C extract, meanwhile, it is still almost 512 constant in the 140° C extract comparing to time 0. After 40 min (Fig. 4c), 513 hemicelluloses > 30 kDa were also lost in the 140 °C extract (logRo = 2.78). 514 Hemicelluloses obtained at 140 °C suffered at this final time a more accentuated 515 decrease in their total concentration than those obtained at 160 °C (logRo = 3.37), which 516 may be explained by the fact that at 140 °C it is not possible to extract much more 517 hemicelluloses from the RM. 518 The distribution of oligosaccharides was similar in both experiments at 140 and 160 ºC, 519 being the diose and triose configuration the most abundant, followed in decreasing 520 order by tetraose, pentose, etc. The concentrations of monomers and oligosaccharides, 521 both decreasing over time, were always higher in extraction at 160 ºC than at 140 ºC. At 522 160 ºC the greatest decrease occurred after the first 15 min of extraction, while at 140 523 ºC the most abrupt decrease occurred at the end of extraction, after 40 min. This 524 difference may be due to a faster extraction/production of oligosaccharides at 160 ºC 525 than at 140 ºC. 526 Relating the molecular weight distribution (Fig. 4) with the logRO used, the evolution can 527 be studied depending on the extraction temperature. At 140 ºC, moving from 15 min 528 (logRO = 2.65) to 40 min (logRO = 2.78), the ratio monomers/total hemicelluloses 529 decreased, while at 160 ºC the ratio increased from 15 min (logRO = 3.24) to 40 min 530 (logRO = 3.37). This may be due to the more accentuated autohydrolysis process at a 531 higher temperature. The proportion of the oligomeric groups from diose to heptaose 532 increased with the increase of logRO at both temperatures, especially at 140 ºC, possibly 533 due to less rupture towards monomers or to a more accentuated decrease in the 534 concentration of hemicelluloses in polymeric form. Conversely, molecular weight 535 groups higher than heptaose decreased their proportion with the increase of logRO at 536 both temperatures, especially at 160 ºC. 537 538 3.5. Concentration, purification and separation by ultrafiltration/diafiltration 539 The three objectives of the downstream process were concentration, purification, and 540 separation of hemicelluloses. 541 3.5.1. Concentration 542 The increase in the concentration of certain groups of hemicelluloses was mainly 543 carried out at the UF stage. Feed volume reduction of 80 % was fixed in each 544 membrane, resulting in a maximum increase of the concentration of 5-fold respect to 545 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 16 the normalized concentration in the Feed stream. This increase in the concentration 546 respect to the normalized Feed concentration was called concentration factor, and it is 547 represented in Fig. 5. This factor was defined as the ratio of the RI detector intensity of 548 each group of hemicelluloses (mono, di, tri, etc.) in the UF and UF/DF streams 549 comparing with the Feed stream. At 140 ºC the weight-average molecular weight of the 550 Feed stream was 12763 Da (hemicellulose concentration: 358.1 mg/L), while at 160°C 551 was 6720 Da (hemicellulose concentration: 556.9 mg/L). This difference occurred due to 552 the fact that at a lower temperature (140 ºC) hemicelluloses were less autohydrolyzed. 553 Regarding the first membrane (30 kDa), in the 140 ºC extract hemicelluloses were more 554 retained than in the 160 ºC extract, as the concentration factor of all the groups 555 suffered a greater increase. This higher retention could be attributed to a higher 556 weight-average molecular weight of the Feed stream, which makes more difficult mass 557 transfer across the membrane. Hemicelluloses from the > 30 kDa group were almost 558 completely retained in the first membrane in both cases, as the concentration factor in 559 Ret-30 kDa-DF was almost 5, being 5 the maximum that can be reached with a VR = 80 560 %. 561 In the last two membranes (10 and 5 kDa), there was no considerable increase in 562 concentration compared with the Feed. This is due to the high retention in the first 563 membrane (30 kDa). In the case of 160°C due to the lower molecular weight of 564 hemicelluloses in this extract, the concentration in these retentates was higher than in 565 140°C extract, as more hemicelluloses were able to cross the first membrane. 566 3.5.2. Purification 567 After UF, it is usually necessary to purify the retentates due to the retention of some 568 hemicelluloses whose MW < MWCO. In the present work, the used of DF purified the 569 hemicelluloses retained not just by reducing the concentration of by-products but also 570 by enrichment in hemicelluloses of higher molecular weight, thus a higher weight-571 average molecular weight of the product. Fig. 5 shows the changes in the concentration 572 factor of the products after purification by DF, called UF/DF products. 573 In the first membrane (30 kDa), DF reduced the presence of all the hemicellulose groups 574 in the 140 ºC extract, being the more reduced the ones of lower molecular weight (from 575 mono to 1.6-5 kDa). In the 160 ºC extract, DF was able to reduce the presence of an 576 only certain group of hemicelluloses (from mono to 1.6-5 kDa), but not of the others. 577 This could be due to a higher hemicelluloses concentration of the 160 ºC Feed stream 578 (556.9 mg/L) compared to 140 ºC Feed stream (358.1 mg/L). Monomers, dimers, and 579 trimers may have been trapped on the feed side by other hemicelluloses. Regarding 580 intermediate size hemicelluloses (5-30 kDa), problems for crossing the UF membranes 581 agree with previous studies. In this sense, Strand et al. (2015) reported that the 582 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 17 substances more harmful for the UF capacity were intermediate size hemicelluloses. 583 Otherwise, the highest molecular weight hemicelluloses (>30 kDa) cannot cross the 584 membrane being retained easily, and the lowest molecular weight substances (by-585 products) can generally pass through it causing no problems of concentration 586 polarization and/or membrane fouling. 587 Regarding the last two membranes (10 and 5 kDa), in the 140 ºC extract part of the 588 hemicelluloses of 10-30 kDa group dragged in the DF of the first membrane (30 kDa) 589 were recovered in the DF of the second membrane (10 kDa), thanks to the reuse of the 590 DF water. However, in the DF of 160 ºC extract, there was no recovery of hemicelluloses 591 in the second membrane as hemicelluloses >10 kDa were not dragged during the DF of 592 the 30 kDa membrane. DF of the 10 kDa and 5 kDa retentates also allowed to decrease 593 the presence of hemicelluloses whose MW < MWCO. If a higher decrease were desired, 594 a higher number of diavolumes would be necessary. 595 One of the main goals of DF is to reduce the presence of by-products in the UF 596 retentates. This effect can be seen in Table 1. By-products were more retained in the 597 membrane when hemicelluloses had the highest weight-average molecular weight, and 598 the DF was more crucial to purify the retentates. This higher retention of by-products 599 may be due to the formation of certain aggregated by high molecular weight 600 hemicelluloses, which trap the by-products. The percentage of by-products removal 601 after DF was 56.3 % for 140 ºC extract, compared to 31.6 % for the 160 ºC extract, 602 whose molecular weight was lower (6720 Da vs. 12763 Da). Similarly, in the case of 603 lower molecular weight hemicelluloses, a higher percentage of by-products was 604 recovered directly in the permeate 49.0 % (160 ºC extract) against 31.2 % (140 ºC 605 extract). The maximum retention of by-products in the purified retentates was 8.7 %, so 606 the DF can be considered as a good method for purification. It should be noted that the 607 application of a greater number of diavolumes would further reduce this retention. The 608 increase in the purity of the products through the removal of by-products is shown in 609 section 3.6. 610 3.5.3. Separation 611 The third objective of this work was the hemicellulose separation depending on the 612 molecular weight. This purpose was achieved partially in the UF process and also in the 613 UF/DF process above mentioned. After DF results showed that the majority of the 614 target hemicelluloses (> 5 kDa) were recovered in the purified retentate. At 160 ºC, 615 hemicelluloses from the groups 5-10 kDa, 10-30 kDa and >30 kDa were recovered with 616 percentages of 78.9, 99.5 and 100%, respectively. In the case of 140 ºC, the recoveries 617 were lower with values of 57.4, 85.7 and 90.6 % of the groups 5-10 kDa, 10-30 kDa and 618 > 30 kDa, respectively. These lower recoveries could be attributed to mass transfer 619 difficulties associated with the high molecular weight of the Feed stream, and 620 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 18 therefore, these hemicelluloses trapped into the membrane were dragged to the DF 621 water. 622 On the contrary, certain hemicelluloses were not the target in this particular process, 623 thus the objective was to separate them from the purified retentates. These substances 624 were monomers, dimers and trimers, oligomers from tetra to penta, and hemicelluloses 625 between 1.6-5 kDa. At 160 ºC, the total removal percentage of these compounds was 626 57.2 % compared to 66.2 % in the case of 140 ºC. All these substances were eliminated 627 by the 5 kDa permeate and the DF waters. 628 3.6. Characterization of the products 629 Table 2 shows some parameters of the Feed streams, UF products, and UF/DF products: 630 weight-average molecular weight (MW), hemicelluloses concentration, by-products 631 concentration, and purity. Feed volume reduction of 80% allowed that most of the 632 hemicellulose concentrations were similar to or higher than the hemicellulose 633 concentration in Feed steam, despite the fact that hemicelluloses are only partially 634 retained by each of the membranes and are distributed in three retentates, one 635 permeate, and the DF water. 636 Cascade UF system allowed obtaining three differentiated fractions of hemicelluloses: 637 Ret-30 kDa, Ret-10 kDa, and Ret-5 kDa. These products differ considerably in their 638 weight-average molecular weight. In the 140 ºC extract, the MWs were 34965 Da (Ret-639 30 kDa), 2029 Da (Ret-10 kDa), and 1564 kDa (Ret-5 kDa). The UF products from the 160 640 ºC extract had MWs of 15265 Da (Ret-30 kDa), 3618 Da (Ret-10 kDa), and 1388 Da (Ret-641 5 kDa). 642 Purity has been determined as the relation between the concentration of 643 hemicelluloses in the solution and the total concentration of compounds detected by 644 HPLC (hemicelluloses, sugars, aldehydes, acids, furfural, and 5-HMF). The assumption 645 that the lignin that may be present did not contribute significantly to purity is justified 646 by the low severity used in the autohydrolysis and the very low percentage of acid-647 soluble lignin quantified in the raw material characterization. The purity of the three 648 products after UF was in the range 67.0 to 89.5 wt%, being the average purity of the 649 Feed liquors 79.8 wt%. 650 According to Table 2 and previous results, purification by DF allowed (1) to increase the 651 MW of the products, (2) to recover hemicelluloses dragged in the DF of the previous 652 membrane in the cascade, and (3) to diminish the presence of by-products increasing 653 the purity of the retentates. The purity of the products after UF/DF was in the range 654 83.7 to 97.8 wt%. 655 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 19 The reported data allow the formulation of UF material balances with Feed, Ret-30 kDa, 656 Ret-10 kDa, Ret-5 kDa, and Perm-5 kDa, taking into account that feed volume reduction 657 was 80 % (v/v) in each of the UF steps. Discrepancies can be attributed to 658 experimental/analytical errors and small retention of the compounds on the membrane 659 surface. 660 Molecular weight characterization of the feed liquors and the UF/DF products (Fig. 6) 661 shows the different molecular weight distributions obtained. Feed streams had a variety 662 of hemicelluloses, thus having a considerable polydispersion. Hemicelluloses between 663 1.6-5 kDa were the more common in both feed of 140 and 160 ºC extract with 664 percentages of 28.9 wt% and 31.9 wt%, respectively. The most abundant oligomer was 665 mannotriose with percentages of 8.9 wt% (140 ºC extract) and 9.3 wt% (160 ºC). 666 Comparing each of the products individually, the UF/DF of 140 ºC extract resulted in a 667 Ret-30 kDa-DF containing mainly > 30 kDa hemicelluloses (28.2 wt%), with a lower 668 proportion of monomers, dimers, trimers, oligomers and also 1.6-5 kDa hemicelluloses 669 than the Feed. This was thanks to the improved mass transfer across the membrane 670 during DF. The other two retentates (Ret-10 kDa-DF and Ret-5 kDa-DF) contained 671 mainly hemicelluloses between 1.6-5 kDa (25.8 wt% in both cases), with a similar or 672 higher proportion of oligomeric hemicelluloses than the Feed. The most abundant 673 oligomer of these two retentates was again mannotriose with percentages of 9.8 wt% 674 (Ret-10 kDa-DF) and 17.0 wt% (Ret-5 kDa-DF). In the case of 160 ºC extract, Ret-30 kDa-675 DF was rich in 1.6-5 kDa hemicelluloses (30.4 wt%). It is also worth noting: 1) the 676 increase in the proportion of hemicellulose of molecular weight higher than the group 677 1.6-5 kDa and 2) the decrease in the proportion of hemicelluloses of molecular weight 678 lower than 1.6-5 kDa, comparing both with the Feed. Ret-10 kDa-DF and Ret-5 kDa-DF 679 had their higher proportion in hemicelluloses between 1.6-5 kDa (30.2 and 20.6 wt%, 680 respectively), with mannotriose as the most abundant oligomer (9.3 wt% and 14.7 wt%, 681 respectively). 682 3.7. Structural characterization of the spent solids 683 The ATR-FTIR spectra of spent coffee grounds oil and spent coffee grounds before and 684 after extractions were determined. The broad bands in 3600-3000 cm-1 region are 685 attributed to the hydroxyl group of O-H stretching vibrations related to cellulosic 686 materials (Lazzari et al., 2018). The absorbance in this region increased after the 687 extraction of oil from spent coffee grounds. This increase shows that oil removal is a 688 good pre-treatment, as the polysaccharides appeared to be more concentrated and 689 accessible in the matrix of the raw material. The decrease in absorbance after 690 hemicellulose extraction was greater at a higher extraction temperature, indicating a 691 greater breakage of bonds due to hemicellulose extraction. The region between 3000-692 2800 cm-1 is related to C-H stretching vibration (Ballesteros et al., 2015). Two peaks 693 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 20 have high absorption in this range: 2920 cm-1 and 2845 cm-1. These bands are due to 694 the CH2 symmetrical and asymmetrical stretching, respectively (Lazzari et al., 2018). 695 Some authors have related these stretching with aliphatic bounds attributed to the 696 presence of caffeine and lipids (Li et al., 2014). This can be confirmed by the presence of 697 the same peaks in the spectrum of spent coffee grounds oil. Other authors have related 698 the peak at 2920 cm-1 with the presence of hydrogen bonds in cellulose. The peaks 699 between 1750 cm-1 and 1730 cm-1 represent ester moieties in the hemicellulose 700 fraction related to the bonds between lignin and polysaccharides (Ravindran et al., 701 2017). This peak appears after extraction of oil from spent coffee grounds, indicating 702 that the oil release made the ester groups more available in the matrix. These ester 703 groups are part of both the hemicellulose-lignin complexes and the oil. The region 704 1700-1500 cm-1 is related with carbonyl groups (C=O) asymmetrical and symmetrical 705 stretching vibrations, and the peaks at 1700 and 1650 cm-1 are highly associated to the 706 presence of caffeine and chlorogenic acid (Ballesteros et al., 2015). The presence of 707 caffeine in the spent coffee oil is again confirmed by the peak 1700 cm-1. Regarding the 708 second peak (1650 cm-1), the absorbance was constant after oil extraction by scCO2, 709 which could indicate that the chlorogenic acid remained in the defatted spent coffee 710 matrix. The band at 1369 cm-1 is attributed to the C-H deformation in cellulose and 711 hemicellulose (Traoré et al., 2016). The intensity of this band increased after oil 712 extraction, and decreased after hemicellulose extraction more markedly at a higher 713 extraction temperature. This decrease was due to the breakage of C-H bonds in the 714 hemicelluloses and between hemicelluloses and cellulose during extraction. The broad 715 region between 1200-920 cm-1 is related to the stretching vibration of C-O in C-O-H 716 bonds such as glycosidic bonds, attributed to polysaccharide sugars (Ballesteros et al., 717 2015). After oil extraction, the intensity of this band increased considerably, which can 718 be attributed to a greater presence of this type of bond without unions linkages with 719 the lipid phase in the matrix. There was a large decrease in absorbance in this region 720 after the extraction of the hemicelluloses so that the higher the extraction temperature 721 the higher the absorbance decrease. This decrease in intensity suggests the rupture of 722 hydrogen bonds between cellulose and hemicelluloses, as well as the hydrolysis of 723 polysaccharides. Within this region, the peak at 1035 cm-1 is related to the C-O, C=C, 724 and C-C-O stretching between polysaccharides and lignin (Ravindran et al., 2017). The 725 peaks at 935 cm-1, 869 cm-1 and 801 cm-1 can be attributed with glycosidic linkage in 726 cellulose and hemicellulose (Ballesteros et al., 2017; Feng Xu et al., 2013). The intensity 727 of these peaks decreased by a very similar degree at both temperatures, as the ruptures 728 of glycosidic bonds in hemicelluloses are of greater importance when they occur in the 729 liquid phase (autohydrolysis). 730 4. Conclusions 731 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 21 Spent coffee grounds where defatted using supercritical CO2 and hydrolyzed in 732 subcritical water at 140 and 160 ºC in a pilot plant. The hemicellulose hydrolyzates were 733 concentrated, purified and separated by means of multiple-step 734 ultrafiltration/diafiltration. The concentration of hemicelluloses occurred mainly in the 735 first membrane due to difficulties in the mass transfer by the formation of aggregates. 736 The separation and purification were improved by diafiltration, which considerably 737 reduced the retention of both by-products and not target hemicelluloses. Obtaining 738 purified hemicellulose fractions at pilot scale allows the production on a larger scale for 739 potential applications in food, pharmaceutical, and biopolymers industries. 740 741 Acknowledgments 742 The authors acknowledge the Spanish Economy and Competitiveness Ministry, Project 743 Reference: CTQ2015-64892-R (MINECO/FEDER) for funding. Marta Ramos-Andrés 744 would like to thank the Spanish Ministry of Education Culture and Sports, the training 745 program of university professors (reference FPU15/06366) for the research-training 746 contract. The authors wish also to thank PROSOL Productos Solubles S.A. for the raw 747 material and the advice. 748 References 749 1. Al-Hamamre, Z., Foerster, S., Hartmann, F., Kröger, M., Kaltschmitt, M., 2012. Oil 750 extracted from spent coffee grounds as a renewable source for fatty acid methyl 751 ester manufacturing. Fuel 96, 70–76. . Fuel 752 2. Andrade, K.S., Gonalvez, R.T., Maraschin, M., Ribeiro-Do-Valle, R.M., Martínez, J., 753 Ferreira, S.R.S., 2012. Supercritical fluid extraction from spent coffee grounds and 754 coffee husks: Antioxidant activity and effect of operational variables on extract 755 composition. Talanta 88, 544–552. . Talanta 756 3. Ballesteros, L.F., Cerqueira, M.A., Teixeira, J.A., Mussatto, S.I., 2015. Characterization 757 of polysaccharides extracted from spent coffee grounds by alkali pretreatment. 758 Carbohydr. Polym. 127, 347–354. . Carbohydr. Polym. 759 4. Ballesteros, L.F., Teixeira, J.A., Mussatto, S.I., 2017. Extraction of polysaccharides by 760 autohydrolysis of spent coffee grounds and evaluation of their antioxidant activity. 761 Carbohydr. Polym. 157, 258–266. . Carbohydr. Polym. 762 5. Ballesteros, L.F., Teixeira, J.A., Mussatto, S.I., 2014. Chemical, Functional, and 763 Structural Properties of Spent Coffee Grounds and Coffee Silverskin. Food 764 Bioprocess Technol. 7, 3493–3503. . Food Bioprocess Technol. 765 6. Baptista, S.L., Cunha, J.T., Romaní, A., Domingues, L., 2018. Xylitol production from 766 lignocellulosic whole slurry corn cob by engineered industrial Saccharomyces 767 cerevisiae PE-2. Bioresour. Technol. 267, 481–491. . Bioresour. Technol. 768 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 28 Fig. 2 976 977 978 979 980 981 982 983 984 985 986 987 988 989 990 991 992 993 994 995 996 997 998 999 1000 1001 1002 Feed Ret-30kDa Ret-30 kDa-DF Ret-10kDa H2O Perm-5kDa Ret-10 kDa-DF Ret-5kDa Ret-5kDa-DF DF water UF 30 kDa UF 10 kDa UF 5 kDa H2O H2O H2O H2O H2O DF 30 kDa DF 30 kDa DF 10 kDa DF 10 kDa DF 10 kDa DF 5 kDa DF 5 kDa DF 5 kDa 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 29 Fig. 3 1003 1004 1005 1006 1007 1008 1009 1010 1011 1012 1013 1014 1015 1016 1017 1018 1019 1020 1021 1022 1023 1024 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 30 Fig. 4 1025 1026 1027 1028 1029 1030 1031 1032 1033 1034 1035 1036 1037 1038 1039 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 31 Fig. 5 1040 1041 1042 1043 1044 1045 1046 1047 1048 1049 1050 1051 1052 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 32 Fig. 6 1053 1054 1055 1056 1057 1058 1059 1060 1061 1062 1063 1064 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 33 Tables 1065 1066 Table 1 1067 Recovery of by-products after UF and UF/DF 1068 UF by-products recoveries UF/DF by-products recoveries MW (Da) Perm-5 kDa Ret-30 kDa Ret-10 kDa Ret-5 kDa Ret-30 kDa-DF Ret-10 kDa-DF Ret-5 kDa-DF DF water* 140 ºC 12763 31.2 % 45.6 % 9.3 % 13.9 % 2.7 % 3.4 % 6.5 % 56.3 % 160 ºC 6720 49.0 % 19.1 % 16.5 % 15.4 % 3.1 % 7.5 % 8.7 % 31.6 % * recovery of by-products in the different DF waters was determined by material balance 1069 1070 1071 1072 1073 1074 1075 1076 1077 1078 1079 1080 1081 1082 1083 1084 1085 1086 1087 1088 1089 1090 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 61 62 63 64 65 34 Table 2 1091 Characterization of the UF and UF/DF products 1092 1093 140 ºC 160 ºC MW (Da) Hemicelluloses (mg/L) By-products (mg/L) Purity (wt%) MW (Da) Hemicelluloses (mg/L) By-products (mg/L) Purity (wt%) Feed 12785 358.1 118.0 75.2 % 6720 556.9* 103.9 84.3 % Ret-30 kDa 34965 457.4 225.7 67.0 % 15265 770.7 90.3 89.5 % Ret-30 kDa-DF 49733 382.7 13.3 96.6 % 23236 656.9 14.8 97.8 % Ret-10 kDa 2029 390.2 57.5 87.2 % 3618 561.4 97.5 85.2 % Ret-10 kDa-DF 4158 341.7 21.0 94.2 % 4043 494.4 44.6 91.7 % Ret-5 kDa 1564 368.1 107.5 77.4 % 1388 642.1 113.6 85.0 % Ret-5 kDa-DF 1641 256.7 49.9 83.7 % 1803 442.1 64.2 87.3 % Perm-5 kDa 1941 323.5 60.3 84.3 % 1596 439.1 90.6 82.9 % *determined by an average of the extract concentrations corresponding to the first 10 minutes of extraction 1094 1095 Electronic Annex Click here to download Electronic Annex: Appendix A. Supplementary information.docx