Hafnium oxide/graphene/hafnium oxide-stacked nanostructures as resistive switching media
Abstract
Producción Científica
Full text
1Hafnium Oxide/Graphene/Hafnium Oxide-Stacked Nanostructures 2as Resistive Switching Media 3Tauno Kahro,*Aivar Tarre, Tanel Käämbre, Helle-Mai Piirsoo, Jekaterina Kozlova, Peeter Ritslaid, 4Aarne Kasikov, Taivo Jogiaas, Guillermo Vinuesa, Salvador Duenas, Helena Castán, Aile Tamm, 5and Kaupo Kukli Cite This: https://doi.org/10.1021/acsanm.1c00587 Read Online ACCESS Metrics & More Article Recommendations 6ABSTRACT: Thin HfO2films were grown by atomic layer deposition on chemical vapor-deposited large-area graphene. The 7graphene was transferred, prior to the deposition of the HfO2overlayer, to the HfO2bottom dielectric layer pregrown on the Si/TiN 8substrate. Either HfCl4or Hf[N(CH3)(C2H5)]4was used as the metal precursor for the bottom layer. The O2plasma-assisted 9process was applied for growing HfO2from Hf[N(CH3)(C2H5)]4also on the top of graphene. To improve graphene transfer, the 10 effects of the surface pretreatments of the as-grown and aged Si/TiN/HfO2substrates were studied and compared. The graphene 11 layer retained its integrity after the plasma processes. Studies on resistive switching on HfO2-graphene-HfO2nanostructures revealed 12 that the operational voltage ranges in the graphene-HfO2stacks were modified together with the ratios between high- and low- 13 resistance states. 14 KEYWORDS: graphene, atomic layer deposition, hafnium oxide, stacked nanostructures, resistive switching 15 ■INTRODUCTION 16 Metal oxide−graphene-based memristor switches have 17 emerged as attractive and promising devices due to the 18 possibility to downscale both switchable medium thickness and 19 effective electrode area, together with further integration of the 20 memory matrices with flexible substrates. 1,2 Graphene may be 21 used as an interfacial barrier layer controlling ionic transport 22 between metal oxide-based medium and the electrode metal. 23 The latter was proposed in a study by Lee et al., conducted on 24 Ta/graphene/Ta2O5stacks. 3 The performance models of 25 resistively switching devices have been presented and 26 schematized in numerous studies on material stacks constitut- 27 ing such devices, including those containing graphene. 1−3 28 Graphene has also been used in HfO2-based resistive switching 29 memory stacks as a complementary conducting layer between 30 HfO2and top metal electrodes, 4 or, as an interesting 31 alternative, in the form of the edge electrode in contact with 32 HfO2-based switching medium. 1 In the former study, 4 33 graphene layers were mounted between the HfO2surface 34 and top electrodes made of inert gold metal, in order to 35 provide an effective oxygen reservoir at the oxide−metal 36interface. 37 Graphene layers are most commonly formed using H2- 38 assisted pyrolysis of methane, CH4, via high-temperature 39 chemical vapor deposition (CVD) on catalytic metal (Cu and 40 Ni) substrates and thereafter transferred to the functional 41 insulator substrates. It is important to note that the transfer 42 procedure of CVD-grown graphene is commonly carried out at 43 room temperature, which allows one to rely on the safety of 44 the procedure in terms of its possible influence on the structure 45 and composition of substrate layers. At the same time, if 46another functional insulator layer is to be deposited from the Received: February 26, 2021 Accepted: May 3, 2021 Articlewww.acsanm.org © XXXX The Authors. Published by American Chemical Society A https://doi.org/10.1021/acsanm.1c00587 ACS Appl. Nano Mater. XXXX, XXX, XXX−XXX
47 vapor phase on the transferred graphene, then one has to 48 beware that the deposition process, which has often had to be 49 carried out at elevated temperatures and using aggressive 50 reactants, may, at first, distort or even destroy the integrity of 51 the graphene layers. In this connection and if the goal is to 52 build a functional device structure, such as a resistively 53 switching cell, in consecutive processes demanding elevation of 54 substrate temperatures and exploitation of, for example, 55 plasma-assisted deposition, it would be imperatively necessary 56 to thoroughly study the effect of such a sequence of processes 57 on the quality of the transferred graphene. 58 Direct growth of graphene on, for example, metal oxide 59 substrates remains a challenge, and advancing of wet chemical 60 transfer processes is still in order. Feasible deposition of dense 61 dielectric metal oxides on graphene has also been a well-known 62 issue along with the development of graphene-based junctions. 63 Application of various metal precursor chemistries, reactor 64 parameters, seed layers, and different graphene functionaliza- 65 tion procedures has been examined. 2,5−8 Atomic layer 66 deposition (ALD) has herewith been applied in the wafer- 67 scale fabrication of HfO2gate dielectrics for graphene channel 68 transistors, whereby the HfO2films were grown using 69 Hf[N(CH3)(C2H5)]4(TEMAHf) and H2O as precursors at 70 200 °C. 9 Later, it has been reported that HfO2films can be 71 grown by ALD from TEMAHf and H2O even at 120 °C on the 72 graphene transistor channel, providing better defined device 73 performance compared, for example, to the ALD-grown TiO2 74 and Al2O3gate dielectrics. 10 75 Application of TEMAHf in the ALD process 11 could 76 nowadays be regarded as a part of possibly the most feasible 77 route to HfO2films on graphene. 9,10,12−16 Other hafnium 78 alkylamides such as Hf[N(CH3)2]4 17,18 are also of interest 79 because application of alkylamide-based precursor chemistry 80 allows one to exploit rather low substrate temperatures in the 81 range of 100−200 °C. Low temperatures effectively assist in 82 increasing the nucleation density of films on carbon 83substrates. 14 84 Complementary procedures can be applied in order to create 85 and increase the density of nucleation sites on otherwise inert 86 graphene. Electron-beam irradiation has reported to be useful 87 on the graphene surface prior to ALD of HfO2at 90 °C from 88 Hf[N(CH3)2]4. 18 Ion-beam-assisted treatment has been 89 examined as a procedure assisting in removal of PMMA 90 residues after the graphene transfer procedures and before 91 ALD of HfO2at 200 °C. Atmospheric oxygen plasma 92 treatment of graphene has been described as a useful 93 procedure for increasing the nucleation density of thin ZrO2 94 films upon ALD at 150 °C from Zr[N(CH3)(C2H5)]4. 19 The 95 latter is worth noting because of the similarity between Zr and 96 Hf precursor chemistries and the crystalline structure of ZrO2 97and HfO2. 98 Carbon-free HfCl4can be exploited as the hafnium 99 precursor, providing crystal growth in HfO2films in the 100 deposition temperature range of 220−750 °C. 20 HfCl4is 101 resistant to thermal decomposition and can thus be applied in 102 a much wider substrate temperature range compared to the 103metal alkylamide precursors. The application of HfCl4for the Figure 1. Schematic representation of the preparation process of the stacked nanostructures. ACS Applied Nano Materials www.acsanm.org Article https://doi.org/10.1021/acsanm.1c00587 ACS Appl. Nano Mater. XXXX, XXX, XXX−XXX B
104 ALD of HfO2on the top of graphene has earlier required 105 prefunctionalization of graphene by growing the first HfO2 106 layers on graphene from HfCl4and H2O at a temperature as 107 low as 180 °C, 21 that is, at substrate temperatures reduced 108 below those otherwise considered as those optimized for the 109 given precursor system. Later, another study has been carried 110 out to comparatively investigate the growth of HfO2films on 111 graphene by ALD from Hf[N(CH3)(C2H5)]4and HfCl4at 250 112 °C. 22 In the latter study, the structural and electrical properties 113 of the oxide grown in chloride-based ALD were actually 114 claimed as superior, compared to those evaluated after the 115 alkylamide-based ALD. Nevertheless, it is worth noting that 116 the exploitation of the TEMAHf precursor may also allow 117 crystallization, that is, growth of HfO2with an ordered 118 structure at temperatures as low as 250 °C, when deposited 119 using O2plasma as the oxygen precursor. 23 120 HfO2-graphene-HfO2nanostructures with graphene embed- 121 ded between HfO2host layers have seldom been publicly 122 described to date. Few studies have employed either graphene 123 oxide nanodots 24 or graphene platelets (domains) 25 as electron 124 traps inside the HfO2insulator dielectric films, in order to 125 engineer charge trapping memory cells. 126 HfO2is an ionic metal oxide which inevitably contains its 127 metastable polymorphs and oxygen vacancies in its as- 128 deposited state. At the same time, HfO2essentially crystallizes 129 as dioxide, instead of suboxides. Besides inherent chemical 130 stability, ALD of HfO2has been scaled up well enough in 131 terms of the selection of precursor chemistry, reactor design, 132 and deposition temperatures for processes on noncarbon 133 substrates. HfO2is also a material partially accommodated to 134 contemporary nanoelectronics whereby hafnium alkylamides, 135 such as TEMAHf, are prospective chemicals, generally 136 providing dense nucleation and growth of uniform nanolayers. 137 In regard with the application of plasma-assisted growth, the 138 influence of plasma on graphene-based substrate structures is 139 yet to be described in the case of the present precursor 140 chemistry and pretreatments, which is also one of the goals of 141 the present study. 142 The present study is devoted to the examination of the 143 feasibility of graphene transfer routes from the catalyst copper 144 substrate onto HfO2films grown by ALD in either HfCl4or 145 Hf[N(CH3)(C2H5)]4-based process. The graphene layers were 146 afterward embedded between HfO2films, whereby the HfO2 147 layers covering the graphene were grown by ALD using 148 Hf[N(CH3)(C2H5)]4and O2plasma as precursors. Spectro- 149 scopic and microscopic studies were subsequently conducted 150 in order to evaluate possible affection of the plasma-assisted 151 ALD on graphene. The performance of the HfO2-graphene- 152 HfO2nanostructures as resistive switching media was 153 evaluated as a functional application of the engineered stacks. 154 ■EXPERIMENTAL SECTION 155 Sample Preparation. Graphene was grown on commercial 25 156 μm-thick polycrystalline copper foil (99.5%, Alfa Aesar) in an in- 157 house-built CVD reactor. The foil was annealed, prior to the graphene 158 deposition, at 1000 °C in Ar/H2(99.999%, Linde Gas) flow for 60 159 min and then additionally exposed to the mixture of 10% CH4 160 (99.999%, Linde Gas) in Ar at 1000 °C for 120 min. Then, the foil 161 was cooled down in Ar flow. 162 The graphene was transferred from copper foils onto reference Si/ 163 SiO2and Si/TiN/HfO2substrates using a wet transfer process. 164 Poly(methyl-methacrylate) (PMMA, with a molecular weight of 165 ∼996,000 g/mol, Sigma-Aldrich) was dissolved in chlorobenzene 166 (Sigma-Aldrich) and then spin-coated onto one side of the graphene/ 167 Cu/graphene structures with a thickness of around 120 nm, and the 168 graphene on the uncoated side was removed by plasma treatment. 169 The Cu foil was dissolved in 1 M (NH4)2S2O8solution overnight. To 170remove the residual etchant, the floating PMMA/graphene film was 171 soaked several times in deionized water baths and transferred onto 172 f1 differently treated substrates (Figure 1). The samples were dried in air 173 for 20 h and then heated on a hot plate at 100 °C for 1 h to improve 174 the contact between graphene and the substrate. The PMMA layer 175was removed by dissolving it in dichloromethane (Sigma-Aldrich). 176Finally, graphene samples were rinsed with 2-propanol. 177 For the deposition of HfO2films, two ALD routes were used, 178 distinctive on the basis of the precursor chemistry. HfCl4and 179TEMAHf were applied as metal precursors. HfCl4was, in the present 180 study, considered as a carbon-free precursor effectively providing 181 growth of HfO2films together with crystallization. O2plasma was 182 exploited as the oxygen precursor together with TEMAHf. For the 183 deposition of the first HfO2layer directly on the bottom TiN 184electrode as for the substrate to the subsequently transferred 185 graphene, both HfCl4and TEMAHf were used as the metal precursor 186 in separate experiments (Figure 1), whereas for the growth of the 187 HfO2film on the top of the graphene layer, only the TEMAHf-based 188 process was exploited. In order to form the base stack structure as a 189substrate for the further transfer of graphene domains, the HfO2films 190 were grown either at 300 °C, by applying 80 ALD cycles with HfCl4 191 and H2O as precursors (Figure 1, Sample I), or at 200 °C, by first 192 applying 120 pulses of H2O followed by 80 ALD cycles consisting of 193alternate TEMAHf and O2plasma pulses (Figure 1, Samples II−V). 194 HfO2films were deposited from HfCl4and H2O in an in-house- 195built hot-wall flow-type ALD reactor. 26 ALD of HfO2from 196 Hf[N(CH3)(C2H5)]4and remote O2plasma was carried out in a 197 commercial Picosun R-200 Advanced ALD system. The bottom 198 electrode substrates exploited were pieces of Si wafers that had been 199 coated with a conductive and crystalline 10 nm-thick TiN layer. TiN 200was grown by pulsed CVD using a batch TiCl4/NH3process 27,28 at 201 temperatures of 450−500 °C in an ASM A412 Large Batch 300 mm 202reactor at Fraunhofer IPMS-CNT. 203 Different surface treatment procedures were applied before 204completion of the switching stack devices. The description of 205 procedures together with their possible effects on structural quality 206 of graphene and metal oxide layers will fully be described below in 207 order to allow one to decide on the necessity to apply these upon 208construction of functional, switchable nanodevices. 209 The CVD-grown graphene transferred to an as-deposited ALD- 210HfO2tended to roll off, wrinkle, and break, not adhering to the metal 211 oxide layer. It is worth noting that the transfer process of the graphene 212 could be improved, resulting in an appreciably homogeneous and 213 reliable adhesion of the graphene domains on the HfO2film surface. 214 The adhesion was strengthened after storing the HfO2-covered 215substrates under laboratory air conditions over several days, sealed 216 against sticking of dust particles, but open to humidity. After storage 217 of HfO2in an air environment over 160 h, approximately, the 218 graphene transferred onto the HfO2surface was adhered appreciably, 219 without delamination, as observed in the case of Sample I(Figure 1). 220The observation implied the need for controlled pretreatment of the 221 as-deposited oxide surface. For this, various substrate treatments 222 before graphene transfer can be found in the literature. For Si/SiO2 223substrates, to increase hydrophilicity (for instance, to increase the 224 density of OH groups), HF dip or plasma treatment could be used. 29 225On the other hand, different substrate treatments will create the 226 number of charged defects and could have a negative effect of 227 fabricated graphene devices (for instance, mobility of charge carriers 228could decrease). 29,30 For ALD-grown dielectrics, plasma treatment 229 may reactivate the surfaces of objects. Therefore, milder surface 230 treatment techniques, such as water, alcohols, or heating prior to the 231 graphene transfer procedure, could be used to replace too aggressive 232treatments, as also shown in Figure 1, Samples II−V. 233 The growth of HfO2films on the top of graphene also required 234pretreatment of the substrate surface, as noted above. The top HfO2 235 layer was grown on transferred graphene using TEMAHf and O2 236plasma in all cases. For the graphene on HfO2grown from HfCl4and ACS Applied Nano Materials www.acsanm.org Article https://doi.org/10.1021/acsanm.1c00587 ACS Appl. Nano Mater. XXXX, XXX, XXX−XXX C
237 H2O (Sample I,Figure 1) prior to the growth of top HfO2, the surface 238 of graphene was preheated at 300 °C for 1 h to clean its surface from 239 possible residues and then exposed to 120 sequential H2O pulses 240 followed by 120 TEMAHf pulses at 200 °C. The latter treatment was, 241 at first, applied in order to prepare the graphene substrate by covering 242 it by a disordered oxide layer, assumptionally providing fast nucleation 243 of the functional HfO2film. Additionally, the purpose of the treatment 244 was to protect the graphene against the possible damaging effect of O2 245 plasma via pregrowth of a buffer layer by applying a water-assisted 246 procedure. All the samples were exposed to an additional sequence of 247 120 H2O pulses before the growth of the top HfO2layer, in order to 248 ensure the preoxidation of the buffer layer and protection of graphene. 249 The HfO2film on the top was, thereafter, formed by applying 80 250 HfO2cycles consisting of a sequence of 0.3−4.0 to 15.0−4.0 s for 251 TEMAHf pulse-purge-O2plasma pulse-purge, respectively, either at 252 200 °C (Sample I,Figure 1) or at 300 °C (Samples II−V,Figure 1). 253 Similar reference HfO2structures were prepared using two different 254 ALD chemistries but without graphene embedded in HfO2. 255 Characterization. Structural characterization of graphene-based 256 nanostructures was performed using a micro-Raman spectroscopic 257 system Renishaw inVia at an excitation wavelength of 514 nm, that is, 258 the excitation energy was 2.4 eV. The spectral resolution reached, 259 approximately, 1.5−2cm −1. The Si reference was used for calibration. 260 The surface morphology of the graphene and HfO2films was 261 evaluated by high-resolution scanning electron microscopy (HR- 262 SEM; FEI Helios NanoLab 600). The focused ion beam (FIB; FEI 263 Nanolab 600 dual-beam (SEM-FIB) system) in situ lift-offtechnique 264 was used to prepare thin samples for high-resolution transmission 265 electron microscopy (HR-TEM) study. TEM analysis was performed 266 in the scanning mode (STEM) at 200 kV using a Cs-probe-corrected 267 transmission electron microscope (FEI Titan Themis 200). The 268 thickness and crystal structure of the deposited HfO2films were 269 evaluated by X-ray reflectometry and by grazing incidence X-ray 270 diffractometry (GIXRD), respectively, using Cu Kαradiation 271 (SmartLaB, Rigaku). 272 The X-ray photoelectron spectroscopy (XPS) spectra were 273 collected at normal emission using a Gammadata/Scienta SES100 274 hemispherical analyzer and a Thermo VG ScientificXR3E2 275 nonmonochromatized dual anode X-ray source (Al Kα/Mg Kα). 276 The analyzer energy scale calibration was checked against the 4f7/2 277 line from cleaned gold foil at 84.0 eV binding energy. Relevant to 278 estimating elemental composition from XPS survey scans, the 279 constant (i.e., independent of photoelectron kinetic energy) analyzer 280 transmission function was checked against accessible core level lines 281 of clean Au, Ag, and Cu samples and additionally asserted by constant 282 magnification in spatial imaging (in the nonenergy-dispersive 283 direction) of a structured test sample through the electron optics 284 over the entire used kinetic energy range. The minor sample charging 285 was corrected for by adjusting the adventitious carbon (typically 286 present in ex situ-measured samples) C 1s peak to 284.8 eV. Spectral 287 components were fitted, and elemental content from survey spectra 288 was estimated using CasaXPS software, 31 used for the quasi-metallic 289 graphene sp2component appropriate asymmetric lineshapes 32 to 290 conservatively estimate the relative contributions from impurity 291 carbon species (sp3carbon- and oxygen-bonded). The overlayer 292 graphene C 1s analysis was further checked and refined using the 293 SPANCF package. 33,34 294 Optical measurements of the graphene nanostructures were 295 performed on spectroscopic ellipsometer GES-5E (Semilab Co) 296 using a microspot option where light is focused on a film surface via a 297 telescope. The converging angle of a beam was about 4°, and the spot 298 size was about 0.35 ×0.8 mm for 65°angle of incidence. Fitting was 299 performed using the program SEA and Tauc-Lorentz dispersion 300 model. Fit quality was characterized using a correlation function 301 between the measured and computed spectra R2. 302 For the electrical measurements, HfO2-graphene-HfO2stack 303 structures were supplied with titanium electrode electron beam 304 evaporated to thicknesses of 100−110 nm through a shadow mask at 305 230 °C. Backside contact to the measurement circuitry was provided 306 by the thermally evaporated aluminum layer with a thickness of 100 307 nm at room temperature. Electrical measurements were carried out in 308 a probe station. The Ti electrodes used in the measurement had either 309 a diameter of 50 μm (area 0.002 mm2) or 250 μm with an area of 0.05 310 mm2. The samples were electrically characterized in both dc and ac 311 regimes using a Keithley 4200 SCS semiconductor analyzer. The bias 312 voltage was applied to the top electrode, while the bottom electrode 313 was grounded. The forming procedure was carried out as a voltage 314 sweep with positive bias, and a current compliance in the order of 315 microamperes was applied to avoid irreversible breakdown of devices. 316 In general, the formation took place between 1.5 and 4 V. The 317 current−voltage curves were obtained by applying positive and 318 negative voltage sweeps, while the memory maps were measured by 319 applying increasing voltage pulses while maintaining a reading voltage 320of 0.1 V. 321 ■RESULTS AND DISCUSSION 322 Morphology and Structure. According to SEM analysis, 323 the as-transferred graphene was appreciably uniform and the 324 film coverage was, as estimated, more than 95%. It should be 325 mentioned that for the as-grown HfO2dielectrics, only boiling 326 in deionized water and then heating in a hot plate improve 327 graphene transfer, whereas 2-propanol-rinsed samples showed 328 more breaks and cracks. Furthermore, graphene layers on aged, 329 that is, openly stored, ALD dielectrics became similar, in terms 330 of continuity, to those on HfO2in Sample Iand implied no 331clear dependence on the selected pretreatments. 332 In the image of transferred graphene on the Si/TiN/HfO2 333 f2 substrate (Figure 2a), one can see wrinkles, which may have 334 resulted from the transferring process. The structure and 335 morphology of the bottom HfO2dielectric layer were similar in 336all cases regardless of the precursor used. The morphology Figure 2. SEM images of (a) Si/TiN/HfO2/graphene (Sample IV before the top HfO2layer) and (b) Si/TiN/HfO2/graphene/HfO2 nanostructures (Sample IV). ACS Applied Nano Materials www.acsanm.org Article https://doi.org/10.1021/acsanm.1c00587 ACS Appl. Nano Mater. XXXX, XXX, XXX−XXX D
337 and/or the film coverage of top-layer HfO2on Si/TiN/HfO2 338 and Si/TiN/HfO2/graphene substrates was also uniform. 339 The surfaces were uniformly covered by grain-like features 340 with an average size of about 20 nm, as evaluated (with ImageJ 341 software) on the bird-eye SEM images. However, some darker 342 areas, possibly “valleys”on the top layer of HfO2grown on 343 graphene, can be seen in Figure 2b, which may be due to the 344 morphological effect, that is, adhesion can vary between 345 graphene and the Si/TiN/HfO2substrate. 346 The HfO2films were grown to the thicknesses ranging from 347 7.5 to 9.0 nm on Si substrates, in accordance with the XRR 348 analysis. The thicknesses of HfO2films deposited both below 349 and on the top of the transferred graphene layers were 9 nm 350 (on Si/TiN substrates), as evaluated by spectroscopic 351 ellipsometry. Similar layer thicknesses were also seen in the f3 352 TEM images (Figure 3). 353 TEM measurements showed that the different layers from 354 the nanostructures are clearly distinguishable (Figure 3). The 355 result visually resembles that earlier observed in the case of 356 ZrO2-graphene-ZrO2stacks 35 and in Ta-graphene-Ta2O5 357 stacks. 3 The top layer of HfO2both on graphene and on the 358 bottom HfO2had a lower density as compared to the bottom 359 HfO2film on the Si/TiN substrate. However, the top layer 360 thickness was comparable to the bottom and both values were 361 in accordance with the results of XRR and ellipsometry. 362 Furthermore, the results showed that the HfO2films were at 363 least partially crystallized, that is, possessed certain short-range 364 ordering and nanocrystallinity. 365The HfO2films grown on Si and Si/TiN substrate surfaces 366were formed as strongly disordered, that is, layers containing 367crystallites with a size of approximately 2 nm as estimated on 368 f4the basis of GIXRD results (Figure 4) The diffractograms of 369the HfO2films grown from both TEMAHf and HfCl4 370precursors were similar. The results indicated that the first 371unambiguously identified reflections began to appear in the 372diffractograms from the films grown at 250 °C (not shown) 373and when using at least 500 growth cycles. In the latter, 374reference, the film was grown to a thickness of 50 nm, 375approximately, and the HfO2was crystallized in a dominantly 376monoclinic phase (card 34-0104), as revealed by reflections of 377moderate intensity but clearly apparent in the diffraction 378pattern. In the case of 80 growth cycles as used in the present 379work to deposit 7−9 nm-thick functional HfO2layers on TiN 380and on graphene, the growth of nanocrystals in the reference 381HfO2films was revealed only by weak and broad trace 382reflections at 28 and 30.3°, referring to the formation of 383metastable cubic polymorph of HfO2(card 96-900-9017) in 384addition to the stable monoclinic phase. In the reference films 385grown at 200 °C, implications of ordering became hardly 386detectable in the diffraction patterns. 387Raman Spectroscopy. The Raman spectra of graphene 388transferred on the reference Si/SiO2substrate showed two 389main bands at 1587 cm−1for G and at 2688 cm−1for 2D bands 390 f5(Figure 5). The positions of the bands slightly varied from 391sample to sample; therefore, the average values of each band 392position were used for further analysis. The 2D band had a 393narrow Lorentzian shape, which is one of the characteristic 394features of single-layer graphene. 36,37 The defect-related D 395band at 1350 cm−1and the D′band at 1620 cm−1were initially 396absent in the Raman spectra, but they appeared after 397deposition of the upper HfO2dielectric layer on graphene 398either with or without “buffer ALD”treatments. 399Positions of Raman bands characteristic of graphene varied 400on differently treated substrates, Figure 5, right panel. This 401shifting and widening of bands can be explained by strain 36 or 402more likely doping by charge transfer between graphene and 403the substrate, 38 which may be enhanced also by the inevitable 404presence of residual impurities. The position of the G band 405thus changes with (electron) doping. The frequency of the G 406band reaches its minimum value when the Fermi level is at the 407Dirac point. At room temperature, this value, ωG, has been 408estimated to be 1579.2 cm−1, 36,39 and the Raman shift has Figure 3. Cross-sectional high-resolution STEM bright-field image of the Si/TiN/HfO2/graphene/HfO2/Ti-electrode (Sample I, top) and Si/TiN/HfO2/HfO2/Ti-electrode (Sample Iwithout graphene, bottom) stack structures. Figure 4. GIXRD patterns of HfO2films grown at different deposition temperatures with 80 and 500 growth cycles, indicated by labels. Miller indexes corresponding to the reflections of monoclinic (M) and cubic (C) polymorphs of HfO2are also indicated by labels. ACS Applied Nano Materials www.acsanm.org Article https://doi.org/10.1021/acsanm.1c00587 ACS Appl. Nano Mater. XXXX, XXX, XXX−XXX E
409 increased with the concentrations of either holes or 410 electrons. 40 The G band width has been reported to decrease 411 symmetrically as the concentrations of electrons or holes 412 increase. 36 The position of the 2D band also depends on the 413 Fermi level, increasing with the hole concentration and 414 decreasing with the electron concentration. 36,40 In addition, 415 the integrated intensity of the 2D band has decreased as the 416 Fermi level increases. 31 417 Usually, CVD-grown graphene has been regarded as a 418 slightly p-type conductor (i.e., hole doped due to the presence 419 and charge transfer effect of oxygen and/or water). 40−43 In the 420 present study, after transferring the CVD-graphene onto 7.5− 421 9.0 nm-thick HfO2dielectric layers, downshifts of the positions 422 and widenings of the G and 2D bands could be detected and 423 measured, as shown in Figure 5. Similar behavior has recently 424 been reported in a study by Ben Maad et al., 41 where graphene 425 was transferred on HfO2films of different thicknesses, and 426 similar shifting and broadening of bands were measured, most 427 prominent in the case of thinnest (5 nm) HfO2films. The high 428 density of carriers transferred to graphene from such thin 429 dielectrics (10 nm or less) may be explained by the localization 430 of traps at the Si/SiO2/HfO2interface but still closer to the 431 graphene layer as compared to thicker dielectric layer/ 432 graphene structures. 41 433 In the present study, the Raman measurements revealed that 434 the positions of G and 2D bands reached the lowest values in 435 the case where no water or other additional treatments were 436 applied on the HfO2surface (deposited from HfCl4) before the 437 graphene transfer procedure (Figure 1, Sample I). It is thus 438 indeed likely that either the pretreatment procedures 439 conducted on the HfO2surface have covered the oxide with 440 layers of chemical groups which at least partially blocked the 441 charge transfer and accompanying the graphene doping 442 process or HfO2deposited from TEMAHf has a lower amount 443 of localized traps compared to the HfO2deposited from HfCl4. 444 The treatment procedures with boiled water or 2-propanol 445 on Si/TiN/HfO2substrates may have created a dense layer of 446 hydroxyl groups on the dielectric surface, and therefore, the 447 electron transfer (doping) from HfO2to graphene was at least 448 partially hindered. Under such conditions, the significance of 449 p-type doping may have increased somewhat, but still in lesser 450 extents than in the case of the stacks consisting of graphene 451 transferred to the Si/SiO2substrate. 44 It should be noted that, 452 in accordance with the Raman results, the effect of the selected 453surface treatments on graphene on aged (i.e., openly stored 454 under laboratory air conditions) HfO2dielectrics was weak, 455 also showing similar (p-type) trends with implications of 456doping effects. 457 After the deposition of the top HfO2layers on graphene, the 458 Raman signatures of graphene in the stacks became more 459uniform in terms of the positions and widths of G and 2D 460 bands. The largest shift (22 cm−1) in the location of bands has 461 occurred in the case of HfO2grown in plasma-assisted ALD 462 from TEMAHf on graphene transferred on HfO2grown from 463 HfCl4(Sample I,Figure 1). However, after the deposition of 464 the top HfO2layers, the positions of 2D bands increased rather 465 than being decreased in terms of the frequency, being 466 indicative of behavior opposite to the expected one, as the 467 shift should presumably imply the increasing concentration of 468 electrons and significance of n-doping. A possible explanation 469 is that the HfO2films grown from HfCl4on TiN (Sample I, 470Figure 1) were additionally heated at 300 °C for 1 h, together 471 with the transferred graphene layer. Upon heating at 300 °C, 472 before the deposition of the upper HfO2layer, the surface of 473 graphene was, probably, cleaned and more bonding sites for 474 OH groups after H2O treatment were provided, as proposed 475 earlier in the literature. 45 The OH groups could further prevent 476 electron doping from the upper-layer dielectric. 44 The result of 477 the lesser extent of electron doping was a shift of the 2D band 478 to higher frequencies, that is, higher significance of p-type 479 doping, because OH groups can uptake electrons from 480graphene or HfO2. In the cases of stacks, where the HfO2 481 films were grown from TEMAHf and exposed to 120 H2O 482 pulses (Samples II−V,Figure 1), no extra heating was 483 performed before 120 H2O pulses. When the top layer of 484 HfO2was deposited on graphene, similar Raman band shifts 485 were observed, implying some significance of p-type doping. 486 The shift from the initial positions, that is, from the positions 487 recorded before the deposition of the top HfO2film on 488 graphene, remained smaller than that in the case of Sample I 489(Figure 1). 490 To some extent, damaging graphene during the deposition 491 of metal oxide layers on the top of graphene can hardly be 492 avoided. In the present case, after the plasma-assisted ALD of 493 the upper HfO2film, the D and D′bands have emerged in the 494 graphene Raman spectrum (Figure 5). The presence of these, 495 generally defect-related, bands, D and D′can mean either 496physical damage 46 or the exhibition of sp3hybridization 43,47,48 497or be due to amorphous carbon complementarily formed on 498 graphene. 49 In addition, the observed broadening of the 499 Raman bands could also be a consequence of defects 50 or due 500 to higher amplitudes of charge fluctuations (“puddles”) 47 501 which could arise from charged impurities in the disordered 502 dielectric layer and polar adsorbates (OH groups) between 503graphene and dielectrics. 504 On the other hand, the (larger) broadenings and (up and 505 down) shifting of the bands could be an averaging effect over 506nanometer-scale strain variations. 51 507 Interestingly, some Raman spectra (Figure 5) showed 508narrow bands at 1556 and 2333 cm−1, which are probably 509indicative of O2and N2molecules, respectively. These species 510could have been trapped in the pores of the HfO2film during Figure 5. Representative Raman spectra of graphene-based stack structures in the case of differently stacked structures described by labels and normalized by the G band according to G band intensities where additional Raman bands at 1556 cm−1, labeled by #, and those at 2333 cm−1, labeled by *, indicate adsorbed oxygen and nitrogen molecules, respectively. The right panel represents Raman spectra normalized to the G band of the graphene-based stack structures in the energy range of 1570−1610 cm−1. ACS Applied Nano Materials www.acsanm.org Article https://doi.org/10.1021/acsanm.1c00587 ACS Appl. Nano Mater. XXXX, XXX, XXX−XXX F
511 the deposition process (O2from oxygen plasma and N2from 512 carrier gas) or, alternatively, adsorbed on the surface of stack 513 structures from the atmosphere. 52,53 514 X-ray Photoelectron Spectroscopy. The elemental 515 composition of reference HfO2ALD films, as-deposited and 516 graphene-coated, was estimated from XPS survey spectra (not 517 shown) and showed close agreement with stoichiometric 518 hafnium to oxygen content ratios, that is, corresponded to that 519 of HfO2, for the as-deposited oxide layers without the graphene 520 cover layer, whereas the relative oxygen content was found to 521 be somewhat in excess compared to that in the graphene- 522 coated samples. 523 However, the main purpose of the application of XPS was to 524 evaluate the presence of possible residual species associated 525 with the PMMA-assisted graphene transfer process, thus 526 probing the quality of the as-transferred graphene layer. XPS 527 can, thereby, provide additional information about surface 528 defects/impurities and have been used for the characterization 529 of nanographite/graphene structures in this regard before. 48 In 530 the present study, the C 1s spectrum from the HfO2film f6 531 covered by the transferred graphene (Figure 6, upper panel) 532 was fitted in the common manner using the asymmetric 533 Doniach−Sunjic (DS) line shape 32 for the (metallic) sp2 534 component characteristic of graphene and Gaussian−Lorent- 535 zian symmetric shapes for the other components, 54 after 536 subtracting Shirley background. The asymmetry of the DS line 537 was limited to a value of 0.14, which has earlier been found 538 valid for pristine graphene. 55−57 This was appropriate in order 539 to avoid underestimation of additional, possibly impurity- 540 originated shoulders, and asymmetric shape inadequately 541 dominating in the spectrum, even if some authors have 542 reported that the peak asymmetry can be enhanced in the 543presence of defects. 56 544 Herewith, the purity of graphene was estimated rather 545 conservatively from C 1s XPS analysis and that the residual 546 content found here can be plausibly seen as the upper limit 547 values for the impurities in the sample. The XPS results for the 548 C 1s spectrum (Figure 6, upper panel) indicated that the 549 relative content of what is identified as oxidized carbon 550 remained below 5−6% of the total signal, while the separate 551 (∼7.5%) sp3feature at least partly associated to dangling bonds 552 at edges of graphene patches. 57 The latter was partially 553 supported by the Raman measurements, described above, 554 which confirmed that the D band was, in practice, absent in the 555case of graphene not covered by the top HfO2layer. 556 It is worth noting that for the PMMA used in the 557 transferring process of the graphene layer to the oxide surface, 558 even the residue after subtracting the sp2component from the 559 C 1s spectrum bears no close resemblance to its C 1s spectrum 560 of PMMA, 58 suggesting that there are virtually no PMMA 561residues left on graphene in our experiments. 562 In Figure 6, bottom panel, one can see that the O 1s 563 photoelectron spectrum measured on a HfO2film, not coated 564 with transferred graphene, reveals a minor contribution from 565 hydroxyl groups (approximately 9% of the overall oxygen 566 signal), present on the HfO2film surface, and from adsorbed 567 hydrocarbons (6%). For the graphene-covered HfO2sample, 568 the spectral component referring to the presence of hydro- 569 carbons grew by around 1.5 times in relation to the main oxide 570 peak, which was consistent with the C 1s signal other than that 571 from the sp2-hybridized carbon signal originating from 572 graphene sheets. At the same time, the dominating lowest 573 binding energy component from the HfO2remained consistent 574 with the stoichiometric ratio between oxygen and hafnium in 575 the probed volume, as derived from the signal ratios for both 576 these samples in survey spectra (not shown). However, the 577 middle component at ∼531.5 eV binding energy, which 578 commonly originates in surface hydroxyl, 59 grew approximately 579 twice, plausibly originating from the hydroxylated metal oxide 580 surface under the graphene layer. This is also supported by an 581 observation, according to which excessive oxygen-bonded 582carbon was not present in the C 1s spectrum. 583 The Hf 4f spectra for both graphene-covered and bare HfO2 584 (not shown) could be well fitted by a single spin−orbit split 585 pair of Voigt profiles, hence indicating that the samples were 586 chemically homogeneous, as expected for these thick oxide 587 films. 60 The Hf 4f7/2 binding energy of 16.9 eV agrees with 588 several previous studies of HfO2films 60−62 even if the values 589 closer to 18 eV have also been considered. 63 However, such a 590 divergence of values may stem from the common but lately 591 criticized 64,65 practice of referencing binding energies to 592 adventitious carbon (often still the best available option), 593 which can be circumvented using different internal references, 594 viz., the Si 2p signal for very thin films on such a substrate, 65,66 595 whose use has previously visualized overcorrection using the 596 carbon reference, 60,66 and raised reconsiderations if the surface 597 carbon is, necessarily, in a sufficiently intimate contact to the 598 surface, providing charge equilibrium with the oxide surface 599beneath. Figure 6. High-resolution XPS scan of the C 1s core-level region with spectral component fit(symbolsdata, solid lineoverall fit envelope, and colored fieldsfit components) upper panel, and high-resolution XPS scan of theO1scorelevelpeakwith decomposed components, measured on the graphene-coated HfO2 film without the top HfO2layer bottom panel. ACS Applied Nano Materials www.acsanm.org Article https://doi.org/10.1021/acsanm.1c00587 ACS Appl. Nano Mater. XXXX, XXX, XXX−XXX G
600 Resistive Switching Behavior. In order to follow the 601 effect of the graphene layer on electrical properties, selected 602 stacks with graphene and without graphene were subjected to f7 603 resistive switching measurements. Figure 7 depicts the 604 switching behavior observed in both types of stacks, where 605 the first HfO2layer was grown using HfCl4and H2O, whereas 606 the second HfO2layer was grown using Hf[N(C2H5)(CH3)]2 607 and O2plasma (Sample I,Figure 1). One can see that the 608 switching performance was achieved and repeatable with and 609 without the graphene interlayer between bottom and top HfO2 610 films. The conventional resistive switching current−voltage 611 characteristics were measured along with linear voltage sweeps 612 and resulted in uniform switching with a defined high 613 resistivity state (HRS) and low resistivity state (LRS), although 614 the ratio between those states did not exceed 8, that is, did not 615 reach an order of magnitude. The resistive switching behavior 616 observed was bipolar and proceeded counterclockwise. This 617 means that switching from one resistive state to another 618 required a different polarity of the applied voltage. The 619 switching from the HRS to LRS, that is, the SET procedure, 620 occurred during sweeping positive voltage on the Ti electrode 621 in relation to the bottom TiN electrode and, correspondingly, 622 switching from the LRS to HRS, that is, the RESET process 623 took place during the negative voltage sequence. 624 The bottom and top HfO2layers were, as described above, 625 grown in different ALD processes using HfCl4and Hf[N- 626 (CH3)(C2H5)]4as precursors, respectively. The chloride-based 627 process results in films inevitably containing chlorine as the 628 residual impurity, 20 which was confirmed by XRF in this work 629 as well and remained in the range of 0.6 at. %, whereas the 630 alkylamide-based process results in films containing more 631 carbon. 67 In addition to chemically somewhat different 632 compositions of these films contributing the double-layer 633stack, the HfO2grown from the chloride precursor may form 634 as somewhat more intensely crystallized compared to that 635 formed in the alkylamide process. 20,67 Both structural and 636 chemical differences, that is, process-related discontinuity in 637 the complete stack, plausibly cause energetic barriers of 638 moderate height for charge carriers, in addition to the 639 interfaces between bottom and top oxide layers. This may be 640 a possible reason to the current jump (Figure 7a) during 641 switching events, which in the case of the SET process 642occurred at +0.6 V and in the case of RESET occurred at −0.7 643V. 644 In the case of the stacked nanostructures with the graphene 645 interlayer, the voltages for SET and RESET appeared 646 somewhat more symmetric and the “humps”were noticeably 647weakened (Figure 7a). Also decreased was the LRS/HRS ratio, 648which did not exceed 2.5 in the case of the embedded 649 graphene layer. It is possible that the introduction of naturally 650 conductive graphene with possibly accompanied doping, 651 together with increased defect densities, has significantly 652 decreased the effect of the barrier to the conducting pathways 653 (possibly filaments), suppressing both the stepwise switching 654 process and resistance state differences. Note that the 655 conduction currents through the graphene-containing stack 656 (Figure 7a) were increased by almost an order of magnitude, 657compared to those measured in the reference HfO2stack 658(Figure 7a). 659 In connection with the conventional resistive switching 660 measurements, one has to consider that rectangular voltage 661 pulses are applied on the electrodes, with the amplitude 662increasing along with the number of pulses in sequence. At the 663increasing voltage pulses, values of current are recorded, which 664 sequentially and cumulatively form the current−voltage curve 665 until the transition (switching) to the LRS. Upon back-and- 666 forth sweeping of the sequence of voltage pulses with gradually 667 and alternately increasing and decreasing amplitudes, the 668 envelope curves of the current−voltage dependences are 669 acquired (Figure 7a), showing typical resistive switching 670 behavior in such a medium. In order to better measure this 671 hysteresis, low reading voltage curves can be recorded, and this 672means that whenever we increase the applied voltage, the 673 current value is measured at the reading voltage, instead of at 674 the increased voltage value. Such hysteretic curves can be 675 termed hysterons, which demonstrate the nonvolatile effect of 676 the MIM device studied, and improve the distinction between 677 low and high conduction memory states, as was observed also 678 in the present study for the stack containing the graphene 679 interlayer (Figure 7b). In the latter case, currents were read at 680 voltage values of 0.1 V in between the sequential sampling bias 681voltage pulses. The value of the measured current was, 682dominantly, determined by the two resistance states achieved 683 alternately. Two clearly defined plateaus were reached and 684 passed through before and after the sequential SET and 685 RESET transitions (Figure 7b). Current−voltage loop with 686 remarkable squareness, alternatively defined as a current 687 memory map, was thus formed with the memory window 688 between the high and low current states (in the present case, 689 with a nominal LRS/HRS ratio of 1.5 only) distinctively 690separated by 45 μA. Figure 7. Current−voltage curves of the HfO2−HfO2reference double layers, as well as HfO2-graphene-HfO2stacks (a), and a current−voltage memory map from HfO2-graphene-HfO2stacks (b). The electrode area was 0.002 mm2. In both double layers and graphene-containing stacks, the first HfO2layer was grown in the chloride-based ALD process, and the top HfO2layer was grown from the alkylamide precursor (Sample I). ACS Applied Nano Materials www.acsanm.org Article https://doi.org/10.1021/acsanm.1c00587 ACS Appl. Nano Mater. XXXX, XXX, XXX−XXX H
691 The HfO2-graphene-HfO2stacks with HfO2films both 692 grown from the Hf[N(C2H5)(CH3)]4precursor demonstrated 693 resistive switching behavior defined somewhat better com- 694 pared to that observed in the stacks where the bottom HfO2 695 film was grown from HfCl4and H2O. The results are f8 696 exemplified by Figure 8, inset, depicting hysteretic switching 697 behavior of TiN/HfO2/graphene/HfO2/Ti nanostructures 698 (Sample IV), in which the bottom HfO2layer was heat- 699 treated without boiling in water before the graphene transfer 700 process. In Figure 8, inset, the current loops formed during 10 701 subsequential back-and-forth voltage sweeps are depicted. 702 The switching between two distinctive resistivity states took 703 place at approximately 0.5 and −0.6 V in the case of both SET 704 and RESET processes, respectively. The ratio between low- 705 and high-resistance states (LRS/HRS) reached an order of 706 magnitude, that is, 10, approximately, at 0.02 V. Notably, the 707 LRS/HRS ratio remained appreciably stable along with cycling 708 the switching voltages over several tens of times (Figure 8). 709 The latter result could be regarded as promising in terms of the 710 first retention characteristics. f9 711 In Figure 9, average resistive switching voltage curves are 712 depicted. These loops are representative for the samples with 713differently treated HfO2surfaces before the graphene transfer 714process. It is worth noting that the stacks behaved quite 715similarly in terms of the LRS/HRS ratio and switching voltage 716values, except the one which has been rinsed in 2-propanol 717followed by rinsing in water (Sample V)(Figure 9). This can 718be better demonstrated in the memory map comparison of 719 f10Figure 10. Plausibly, 2-propanol and water treatment has 720resulted in densification of a layer of the hydrocarbon species 721in addition to the graphene, giving rise to the electronic defect 722densities. The latter has, also plausibly, led to the narrower 723memory window expressed by both the current envelope curve 724(Figure 9) and current memory map (Figure 10) measured for 725Sample V(Figure 1), when compared to the rest of the 726samples. As the number of defects increased, the leakage 727current in the bulk increased. The applied energy was 728dispersed in the whole bulk, and thus, less energy was 729employed to form the conductive filaments, making them 730weaker (less conductive) than in the other cases. As a result, 731lower currents were obtained in the LRS state of Sample V. 732 ■CONCLUSIONS 733Chemical vapor-deposited graphene layers were successfully 734transferred between embedding layers of HfO2grown by ALD. 735The HfO2films grown as substrates to graphene were 736deposited from HfCl4and water or Hf[N(CH3)(C2H5)]4 737and O2plasma as precursors, whereby the HfO2films on 738graphene were grown only from Hf[N(CH3)(C2H5)]4and 739plasma. Different aging and rinsing treatments were applied 740prior to both graphene transfer procedures and HfO2ALD, in 741order to improve adhesion of graphene on the bottom HfO2 742layer and nucleation of top HfO2on graphene, respectively. 743Raman probing allowed one to decide that the structure of 744graphene was essentially retained after the plasma ALD 745process. However, also in accordance with Raman, defects 746were created in graphene during plasma ALD of HfO2, 747regardless of protective treatment procedures. Nevertheless, 748after deposition of the upper layer HfO2, the Raman spectra 749from the differently treated graphene nanostructures became 750uniformly similar. The HfO2dielectric layers grew homoge- 751neously and were nanocrystalline. 752Resistive switching measurements revealed that the HfO2- 753graphene-HfO2stacks consisting of HfO2layers both grown 754from hafnium alkylamide and O2plasma can demonstrate Figure 8. Retention characteristic, measured from the TiN/HfO2/ graphene/HfO2/Ti (Sample IV) stack, where HfO2layers were grown using TEMAHf and O2plasma. The inset shows 10 sequential current−voltage envelope curves. The electrode dot area was 0.05 mm2. The retention current values were registered at the voltage values of 0.1 V. Figure 9. Representative average current−voltage envelope curves measured from the TiN/HfO2/graphene/HfO2/Ti stack, where all the HfO2layers were grown using TEMAHf and O2plasma as precursors. The bottom HfO2surface treatment procedures are denoted by the labels presented in the legend in accordance with Figure 1. Figure 10. Current−voltage memory maps, measured from TiN/ HfO2/graphene/HfO2/Ti nanostructures, where all HfO2layers were grown using TEMAHf and O2plasma. The bottom HfO2surface treatment procedures are denoted by the labels within the legend in accordance with Figure 1. ACS Applied Nano Materials www.acsanm.org Article https://doi.org/10.1021/acsanm.1c00587 ACS Appl. Nano Mater. XXXX, XXX, XXX−XXX I