Atomic layer deposited nanolaminates of zirconium oxide and manganese oxide from manganese(III)acetylacetonate and ozone
Abstract
Producción Científica
Full text
Nanotechnology ACCEPTED MANUSCRIPT • OPEN ACCESS Atomic layer deposited nanolaminates of zirconium oxide and manganese oxide from manganese(III)acetylacetonate and ozone To cite this article before publication: Kristjan Kalam et al 2021 Nanotechnology in press https://doi.org/10.1088/1361-6528/abfee9 Manuscript version: Accepted Manuscript Accepted Manuscript is “the version of the article accepted for publication including all changes made as a result of the peer review process, and which may also include the addition to the article by IOP Publishing of a header, an article ID, a cover sheet and/or an ‘Accepted Manuscript’ watermark, but excluding any other editing, typesetting or other changes made by IOP Publishing and/or its licensors” This Accepted Manuscript is © 2021 The Author(s). Published by IOP Publishing Ltd.. As the Version of Record of this article is going to be / has been published on a gold open access basis under a CC BY 3.0 licence, this Accepted Manuscript is available for reuse under a CC BY 3.0 licence immediately. Everyone is permitted to use all or part of the original content in this article, provided that they adhere to all the terms of the licence https://creativecommons.org/licences/by/3.0 Although reasonable endeavours have been taken to obtain all necessary permissions from third parties to include their copyrighted content within this article, their full citation and copyright line may not be present in this Accepted Manuscript version. Before using any content from this article, please refer to the Version of Record on IOPscience once published for full citation and copyright details, as permissions may be required. All third party content is fully copyright protected and is not published on a gold open access basis under a CC BY licence, unless that is specifically stated in the figure caption in the Version of Record. View the article online for updates and enhancements. This content was downloaded from IP address 157.88.111.111 on 12/05/2021 at 10:17
1 Atomic layer deposited nanolaminates of zirconium oxide and manganese oxide from manganese(III)acetylacetonate and ozone. Kristjan Kalam*1, Raul Rammula1, Peeter Ritslaid1, Tanel Käämbre1, Joosep Link2, Raivo Stern2, Guillermo Vinuesa3, Salvador Dueñas3, Helena Castán3, Aile Tamm1, Kaupo Kukli1. 1Institute of Physics, University of Tartu, W. Ostwald 1, 50411 Tartu, Estonia. 2National Institute of Chemical Physics and Biophysics, Akadeemia tee 23, 12618 Tallinn, Estonia. 3Department of Electronics, University of Valladolid, Paseo Belén 15, 47011 Valladolid, Spain. * Corresponding author, e-mail: [email protected] Abstract Atomic layer deposition method was used to grow thin films consisting of ZrO2 and MnOx layers. Magnetic and electric properties were studied of films deposited at 300 ºC. Some deposition characteristics of the manganese(III)acetylacetonate and ozone process were investigated, such as the dependence of growth rate on the deposition temperature and film crystallinity. All films were partly crystalline in their as-deposited state. Zirconium oxide contained cubic and tetragonal phases of ZrO2, while the manganese oxide was shown to consist of cubic Mn2O3 and tetragonal Mn3O4 phases. All the films exhibited nonlinear saturative magnetization with hysteresis, as well as resistive switching characteristics. Keywords: Atomic layer deposition, thin films, magnetic materials, resistive switching Introduction Zirconium and manganese oxide thin films have many applications, for example ZrO2 can be used as an optical coating [1, 2], waveguide [3, 4], gas sensor [5, 6], gate dielectric in a transistor [7], functional layer of a resistive switching memory [8] and a ferroelectric memory [9, 10]. Mn-doped zirconia has also been reported to be a magnetic material [11-12]. Magnetic polarization has been achieved and studied also in Fe, Co and Ni doped zirconia [13], Ca and Mg doped [14], Ag doped [15] and even in un-doped zirconia [16-17]. MnO2 has been used as Page 1 of 27 AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
2 a catalyst [18] and an electrode [19]. MnO has been used as electrode material [20]. Mn2O3 has been used for water splitting devices [21]. Oxides of zirconium and magnesium have been prepared via reactive sputtering [22-23], pulsed laser deposition [1, 14, 24], electron beam evaporation [25-26], chemical vapour deposition [27-28] and spray pyrolysis [29-30]. Zirconium oxide films generally form, in atomic layer deposition (ALD) processes, possessing dioxide (ZrO2) stoichiometry and exhibiting crystal structure characteristic of ZrO2 polymorphs, regardless of the precursor chemistry used. For instance, ZrO2 films have been grown by ALD using, e.g., (CpMe)2ZrMe2 or (CpMe)2Zr(OMe)Me (Cp = C5H5, Me = CH3) as Zr precursors, and O3 as the oxidant at 300 or 350 °C [31]. Growth of ZrO2 films from CpZr(NMe2)3 and H2O was investigated in real time at substrate temperatures ranging from 120 to 350 °C [32]. ZrO2 growth has also been carried out using ZrCl4 and H2O as precursors [33] and a similar process has also been monitored in real time [34]. Furthermore, zirconia has been deposited from Zr[N(C2H5)(CH3)]4 and H2O [9, 35]. At the same time, in the case of manganese oxide, the stoichiometry can vary, concurrently with the lattice, due to three different valences of manganese. Thus, MnO2 has been atomic layer deposited from Mn(thd)3 (thd = 2,2,6,6–tetramethyl-3,5 heptanedione) and O3 [21, 36], MnO has also been atomic layer deposited using Mn(EtCp)2, and H2O [20], Mn(thd)3 and NH3 plasma [21], manganese(III)acetylacetonate, further denoted as Mn(acac)3, and H2O [37]. Mn2O3 has been obtained in the films, after annealing the as-deposited MnO2 or MnO [21]. This study is devoted to ALD of laminated thin films consisting of ZrO2 and manganese oxide. The purpose was to firstly investigate the process of depositing manganese oxide from (Mn(acac)3) and ozone, O3, and, thereafter, study the memory effects in nanolaminated zirconia and manganese oxide. Specifically, possible ferromagnetic, ferroelectric and resistive switching properties of such thin films were probed. Experimental details The films studied in this work were grown in a low-pressure flow-type ALD reactor [38]. Mn(acac)3 (97%, ACROS Organics) was used as the manganese precursor and evaporated at Page 2 of 27AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
3 183 ºC. Zirconium precursor, ZrCl4 (99.9 %, Aldrich), was evaporated at 157 oC. Both metal precursors were evaporated from a glass boat inside the reactor at a pressure of 220 Pa. Nitrogen, N2 (99.999%, Eesti AGA AS), was applied as the carrier and purging gas. Ozone was produced from O2 (99.999%, AGA) using BMT Messtechnik 802 N generator. The ozone concentration at the reactor inlet, was 245–250 g/m3 in the experiments. The estimated ozone flow rate from the generator was about 68 scc/m, while the carrier gas flow rate was kept at about 220 scc/m. One ALD cycle of a binary oxide consists of four sequential pulses. For producing a layer of ZrO2, the sequence was ZrCl4 pulse – N2 purge – O3 pulse – N2 purge. In the case of depositing a manganese oxide layer, the metal precursor was Mn(acac)3, while purging with N2 and oxidizing with O3 was similar to the ZrO2 scheme. Pulse times for depositing both metals were 5-2-2-5 s for the sequence given above. Various layered structures were deposited, for example, 100 cycles of manganese oxide followed by a 100 cycles of zirconia, more details are given in Table I. ZrO2-MnOx films were grown on cleansed and etched Si(100) [39] substrate surfaces as well as on surfaces of conductive TiN layers. The TiN bottom electrode layers were pre-deposited on Si(100) wafers with a resistivity of 0.014–0.020 Ωcm, i.e., on Si boron-doped to the concentrations up to 5×1018–1×1019/cm3. TiN was grown by pulsed chemical vapour deposition using a batch TiCl4/NH3 process [40-41] at temperatures of 450–500 °C in an ASM A412 Large Batch 300 mm reactor at Fraunhofer IPMS-CNT. The films, which were deposited on TiN substrates for electrical measurements, were also supplied with Ti electrodes (area 0.204 mm2) electron-beam evaporated on top of the films. The structure to conduct electrical measurements was, from top to bottom, Ti/ZrO2–MnOx/TiN/Si/Al. Spectroscopic ellipsometer (SE), model GES5-E, was used for the measurements of the films thicknesses. Ellipsometric data was modelled in the range of 1.3-5.0 eV using the Tauc- Lorentz dispersion model. X-ray fluorescence (XRF) spectrometer Rigaku ZSX 400 and program ZSX Version 5.55 were used to measure the elemental composition of the films. Measurements were performed with a semi-quantitative (standardless analysis) program (SQX). SQX is a program to obtain concentrations of elements by theoretical calculation using the fundamental parameter (FP) method and internal sensitivity library. The X-ray photoelectron spectra (XPS) were collected at normal emission using a Gammadata/Scienta SES100 hemispherical analyser and a Thermo VG Scientific XR3E2 non-monochromatic dual anode X-ray source (Al-Kα / Mg-Kα). The analyser energy scale Page 3 of 27 AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
4 calibration was checked against the 4f7/2 line from cleaned gold foil at 84.0 eV binding energy. Relevant to estimating elemental composition from XPS survey scans, the constant (i.e., independent of photoelectron kinetic energy) analyser transmission function was checked against accessible core level lines of clean Au, Ag and Cu samples, and additionally asserted by constant magnification in spatial imaging (in the non-energy-dispersive direction) of a structured test sample through the electron optics over the entire used kinetic energy range). Spectral components were fitted, and elemental content from survey spectra was estimated using CasaXPS software [42]. XPS was exploited, in the first place, to detect the presence of carbon, complementarily to XRF, and study the differences of the carbon bonding in the films grown at two different temperatures, 250 and 300 °C, i.e. that providing the most uniform films in terms of thickness, and that probably enabling higher degree of structural ordering, respectively. No preclean or surface etching was conducted before XPS measurements, since deposition of metal electrodes was in order after the deposition of oxide films, and that could not be carried out in a continuous process without exposure to the laboratory air. Nevertheless, since the probing and analysis depth of XPS extends through topmost 4-5 nm of a film, the method allowed one to acquire data adequately, sufficient for the description of bonding between elements constituting the solid layers. Different roles for carbon impurities were expected due to the lower rate of surface exchange reactions at lower temperatures. The crystal structure was evaluated by grazing incidence X-ray diffractometry (GIXRD), using an X-ray diffractometer SmartLab Rigaku with CuKα radiation, which corresponds to an X-ray wavelength of 0.15406 nm. Resistive switching measurements were carried out by means of a semiconductor analyzer Keithley 4200SCS, with samples put in a light-tight probe station. The DC voltage was applied to the top electrode, leaving the bottom one grounded. The current-voltage curves were measured by applying voltage sweeps while incremental voltage pulses were applied in order to obtain the memory maps seen in Fig. 12. The resistive switching measurements appropriate for recording common current-voltage hystereses as well as those enabling admittance memory mapping have been described in a number of earlier studies, e.g., those devoted to HfO2 [43] and ZrO2-Al2O3 [44] based media. The aforementioned semiconductor analyzer can also be used to perform the Double Swing Quiescent Current (DSQC) technique [45], a novel method which would allow one to detect the polarization curves of thin film samples implying ferroelectric behaviour. Page 4 of 27AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
5 Magnetic measurements were performed using Vibrating Sample Magnetometer (VSM) option of the Physical Property Measurement System 14T Quantum Design by scanning the magnetic field from -0.5 to 0.5 T parallel to the film surface at 300 K and -3.5 to 3.5 T at 5 K. Results and discussion Film growth and composition Data regarding the composition of films is given in Table I. Since the zirconium precursor contains chloride and the manganese precursor contains carbon, amounts of these elements were measured as well. Table I. Thicknesses and manganese contents for studied samples with given process descriptions. Deposition temperature was 300 °C. Process description Thickness, nm Mn/(Mn+Zr) Cl, at. % C, at. % 200 x (ZrCl4+O3) 26 0 0.7 - 200 x (Mn(acac)3+O3) 50 1 - 33 100 x (Mn(acac)3+O3) + 100 x (ZrCl4+O3) 20+16 (MnOx + ZrO2) 0.6 0.6 11 50 x (Mn(acac)3+O3) + 50 x (ZrCl4+O3) 7+7 (MnOx + ZrO2) 0.6 0.4 28 50 x (Mn(acac)3+O3) + 50 x (ZrCl4+O3) + 50 x (Mn(acac)3+O3) + 50 x (ZrCl4+O3) + 50 x (Mn(acac)3+O3) 7+7+7+7+7 (MnOx + ZrO2 + MnOx + ZrO2 + MnOx) 0.7 1.3 11 Certain issues became related to the uniformity of the film thickness along the gas flow direction in the flow-type reactor used in the experiments. For ZrCl4 as the Zr precursor in ALD, it is known, that this particular precursor does not decompose thermally even at elevated temperatures. Even at the substrate temperature of 500 oC, the thickness of ZrO2 films grown from ZrCl4 and H2O may not deviate more than 12-15 %, measured along the substrate length [46]. Formation of certain thickness profile in chloride based ALD processes is probably inevitable in such flow-type reactors, possibly caused by the effect of secondary surface reactions, i.e., „poisoning“ of the surface by reaction products, that is HCl [47]. However, in the case of organic and oxygen-containing ligands to metals in the precursors Page 5 of 27 AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
6 like acetylacetonates, the thermal decomposition of the precursor can start in the gas phase during its transport in the reactor towards substrates, and, in this case at already slightly above 300 oC, the oxide layer may, thus, deposit with higher rate, and preferentially, to the regions closer to the leading edge of the substrate. This has, evidently, became a considerable issue in the case of the manganese oxide process, as can be seen in the Figure 1. 4 5 6 7 8 9 10 0 20 40 60 80 100 120 140 160 330 C 350 C 250 C 275 C Film thickness, nm Distance from the leading edge of substrate, cm 300 C Figure 1. Manganese oxide film thicknesses using 200 ALD cycles at various deposition temperatures. The XPS studies on elemental composition of the surface region of the films deposited at two different deposition temperatures 300 and 250 °C from XPS survey spectra revealed O:Mn content ratio approximately 1.4 for the film grown at 300 °C, similarly to the value obtained by XRF. For the film grown at 250 °C, this content ratio increased up to 2.5 and, considering the probability of formation of surface carbonate instead of oxide, increasing with decreasing substrate temperature due to incomplete reactions, the results obtained from the film grown at 250 °C could be interpreted via 3-4 nm thick surface layers dominantly consisting of MnCO3 (Fig. 2). Page 6 of 27AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
7 Figure 2. XPS results indicating the difference in contributions of residual carbon to the composition of manganese oxide films deposited at 250 and 300 °C. The Mn 2p spectrum (Fig. 3), although at least partially demonstrating formation of solid manganese oxide in the present study, is generally not convenient to use for the identification of the Mn charge state due to the underlying (2p1-3d final state) multiplet and nontrivial spectral structure, but the main peak maxima positions suggest 2+ and/or 3+ Mn charge states, and the satellite peak (Fig. 3) at binding energies ~5 eV higher than the main lines (in the 250 °C deposited sample spectrum) can be regarded as that typical of Mn2+ [48]. The films grown at 250 °C remained highly disordered. Multiphase structure started to form and become detected by X-ray diffraction studies or films deposited at 300 °C. The main diffraction maxima were attributed to tetragonal Mn3O4, while Mn2O3 was identified as an additional phase (Fig. 6), as will be described below. Both GIXRD and Mn 2p XPS implied that the phase composition of the MnOx films grown in the present study, especially at lowered temperatures, are complicated to define unambiguously (some further insight is provided from Mn 3s XPS, below). Besides, although manganese can take on all charge states from +7 to -3, the most abundant (and stable) oxides have charge states +2, +3 and +4, and the formula Mn3O4 can sometimes be written as MnO·Mn2O3, although such physical mixture picture would imply exchange interactions such that the magnetic properties would be that of an antiferromagnet (even at low temperatures), different from what we observe (below). Page 7 of 27 AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
8 Figure 3. XPS results decribing the bonding of manganese cations in manganese oxide films deposited at 250 and 300 °C. Figure 4 depicts oxygen 1s spectra obtained from the same reference films grown at temperatures of 250 and 300 °C. The XPS spectrum for O 1s acquired from the film grown at 300 °C demonstrated a dominant sharp peak at 529.9 eV, which is a value typical of bulk manganese oxides [49-51]. In addition, a shoulder structure was resolved and centred around 531.5 eV, which has been related to the presence of (surface) hydroxyl groups [52], accompanied by a smaller amount of C-O bonded impurity with the component peak above 532 eV and a trace peak above 533 eV. The latter could be associated to physisorbed water vapour. However, the signals detected in the spectral region in the range of 531-534 eV would also accommodate and reveal double-bonded carbon of carbonates [53-54] and/or ketonate ligands [55], likely arising from the residues of the metal precursor also exploited in the present study, amply present in the film grown at 250 °C. Page 8 of 27AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
15 020 40 60 80 100 120 140 0,0 2,0x10-5 4,0x10-5 6,0x10-5 8,0x10-5 1,0x10-4 Si-MnOx-ZrO2 laminates Moment, emu Temperature, K ALD cycle scheme: 100 + 100 50 + 50 50 + 50 + 50 + 50 + 50 MnOx 200 cycles Figure 10. Magnetic moment - temperature dependence for MnOx-ZrO2 and MnOx films. All films exhibited resistive switching (RS) characteristics (Fig. 11). This means that, under electrical stimulus, these samples change their resistance state and retain its value even when the power is turned off (non-volatile effect). It has earlier been established that the physics associated with RS involves the movement of both ions and electrons [66]. Furthermore, these devices require an electroforming step [67], an initial electrical stress necessary to activate the switching property. After this process, the characteristic RS current-voltage (I-V) curves can be obtained. Bivalued curves which present two distinctive conduction states referred to as the high-resistance (HRS) and the low-resistance (LRS). The pure (non-laminated) MnOx and ZrO2 samples presented the widest functional windows (Fig. 11-a and 11-b), along with the 50 x MnOx + 50 x ZrO2 (50+50 sample/film), which was the thinnest film as grown. The window narrowed as the number of cycles increased, as we can see when comparing the 50+50 and the 100 x MnOx + 100 x ZrO2 samples (100+100 sample/film) (Fig. 11-c). This is also shown in Figure 12, in which the memory maps [68] drawn from the same films are depicted. This fact can be explained taking into account that the number of ALD cycles determines the thickness of the film (14 nm versus 36 nm, in this case). The 100+100 film also demonstrated the narrowest window together with the multilayer film, which consisted of five sequential layers in stack. In addition to the thickness values (36 nm and 35 nm respectively), this might be due to the existence of several interfaces between the constituent layers, which could hinder the formation of the conductive filament. Page 15 of 27 AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
16 Figure 11. Current – Voltage cycles of pure ZrO2 (a), and MnOx (b) samples, and average current-voltage loops of all the films on a linear scale (c) and on a logarithmic scale (d). The non-laminated ZrO2 film had the lowest SET and RESET voltages (Fig. 11-a). However, this film was also the one with the highest current values for both LRS and HRS states (see also Fig. 12-a), showing, at the same time, the steepest SET and RESET transitions. At first glance, this could be seen as an advantage, as these transitions are also the fastest of all the samples. Nevertheless, this steep transition implies that ZrO2 samples alone may not perform well in multilevel applications, and the high current values may simply make it the least suitable for non-volatile-memory applications, as the power consumption would remain high. The results for non-laminated ZrO2 results are in a good accordance with the ones presented earlier by Ossorio et al. [69]. Page 16 of 27AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
17 Figure 12. Memory maps (a) and normalized memory maps (b) of the different samples. These maps are obtained by reading the current at 0.1 V after applying a previous programming voltage. The normalized values are obtained by considering the LRS as a value of 1.0. The non-laminated MnOx sample the lowest current values for both high and low resistance states (Figs. 11-b, 11-c), which provide similar resistance values to those determined by Zhang et al. [70] when applying Ohm’s law to the current values obtained for both HRS and LRS in the memory map that can be seen in Figure 12. The memory maps are an image of the state of the RRAM cell after a previous stress stimulus, and are obtained by measuring some representative magnitude of the state at voltages low enough so that the measurement process itself does not alter the state of the device [68, 71]. The low current values, along with a notably wide functional window (Fig. 12-b), make the MnOx film the most adequate for memory applications. Additionally, this sample presented smooth SET and RESET transitions, thus showing multilevel capabilities, which have been Page 17 of 27 AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
18 demonstrated to be useful for neuromorphic applications, i.e., artificial neural networks, as they might behave as electronic synapses [72]. The latter is also true for the MnOx-ZrO2 mixed samples, which all presented smooth SET and RESET transitions, as well as lower HRS and LRS currents when comparing them to the nonlaminated ZrO2 film. Thus, MnOx-ZrO2 films might become further investigated and suited to multilevel applications, as implied especially by the 100+100 sample film, which demonstrated the smoothest transitions. On the other hand, these stacks possessed rather narrow functional windows and, consequently, may not regarded as the most appropriate for memory applications, with the exception of the 50+50 sample, which really exhibited high ratio between HRS and LRS as well as appreciably low current values. Summary ZrO2 and manganese oxide films, as well as their layered structures, were deposited by ALD, using ZrCl4, Mn(acac)3 and ozone. XPS results confirmed significant contribution from carbon containing species in the manganese oxide film deposited at 250 °C, allowing one to consider even the formation and presence of MnCO3. At the same time, in the film deposited at 300 °C, essentially weaker role for residual carbon, and formation of Mn3O4 was detected and determined by both XPS and GIXRD. Therefore, 300 °C was chosen for the deposition temperature for nanolaminates. Non-laminated ZrO2 was found to form in its cubic and tetragonal polymorphs, whereas non-laminated manganese oxide possessed cubic Mn2O3 and tetragonal Mn3O4 phases. All the films were found to behave as ferromagnetic-like materials. At the same time, hysteretic charge polarization – electric field behaviour was not registered, and also the Double Swing Quiescent Current method measurements did not imply any ferroelectric behaviour. Manganese oxide films demonstrated both saturation magnetization and coercivity values by two orders of magnitude higher at 5 K, compared to the values measured at 300 K. In ZrO2-MnOx films and nanolaminates, the polarization values at the aforementioned temperatures reached differed by about ten times. Manganese oxide lost its high magnetization value at 40-45 K. All films exhibited excellent resistive switching characteristics with almost no difference between their commutation values. However, there appeared remarkable differences in the current values linked to both high and low resistance states, with the non-laminated ZrO2 sample film showing the highest ratios between these states. The non-laminated MnOx film Page 18 of 27AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
19 possessed the lowest ratio, while in the different ZrO2-MnOx samples the ratio between high and low resistance states varied. Both non-laminated samples present great functional windows between each resistance state. Nevertheless, the mixed ZrO2-MnOx films have very different windows between these states, with the 50 x MnOx + 50 x ZrO2 showing a great functional window, while the 100 x MnOx + 100 x ZrO2 and the multilayer film show the narrowest windows. This is explained by the variation in thickness and the fact that the multiple interfaces between the layer could hinder the formation of the filament. These results prove the potential interest of the MnOx and ZrO2/MnOx-based MIM structures in both nonvolatile memories and neuromorphic applications. Acknowledgements The present study was partially funded by the European Regional Development Fund projects “Emerging orders in quantum and nanomaterials” (TK134), "Advanced materials and hightechnology devices for sustainable energetics, sensorics and nanoelectronics“ (TK141), Spanish Ministry of Economy and Competitiveness (TEC2017-84321-C4-2-R) with support of Feder funds and Estonian Research Agency (PRG4, PRG753). References 1. Gottmann J and Kreutz E W 1999 Pulsed laser deposition of alumina and zirconia thin films on polymers and glass as optical and protective coatings Surface and Coatings Technology 116-119 1189-1194. https://doi.org/10.1016/S0257-8972(99)00191-7 2. Edlou S M, Smajkiewicz A, Al-Jumaily G A 1993 Optical properties and environmental stability of oxide coatings deposited by reactive sputtering Appl. Opt. 32 5601-5605. https://doi.org/10.1364/AO.32.005601 3. Sorek Y, Zevin M, Reisfeld R, Hurvits T and Ruschin S 1997 Zirconia and Zirconia−ORMOSIL Planar Waveguides Prepared at Room Temperature Chem. Mater. 9 670–676. https://doi.org/10.1021/cm960135x 4. Jasieniak J, Pacifico J, Signorini R, Chiasera A, Ferrari M, Martucci A and Mulvaney P 2007 Luminescence and Amplified Stimulated Emission in CdSe–ZnS‐Nanocrystal‐Doped Page 19 of 27 AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
20 TiO2 and ZrO2 Waveguides Advanced Functional Materials 17 1654-1662. https://doi.org/10.1002/adfm.200600955 5. Okamoto H, Obayashi H and Kudo T 1980 Carbon monoxide gas sensor made of stabilized zirconia Solid State Ionics 1 319-326. https://doi.org/10.1016/0167-2738(80)90012-0 6. Miura N, Nakatou M and Zhuiykov S 2003 Impedancemetric gas sensor based on zirconia solid electrolyte and oxide sensing electrode for detecting total NOx at high temperature Sensors and Actuators B: Chemical 93 221-228. https://doi.org/10.1016/S0925- 4005(03)00196-5 7. Houssa M, Afanasiev V V, Stesmans A and Heyns M M 2000 Variation in the fixed charge density of SiOx/ZrO2 gate dielectric stacks during postdeposition oxidation Appl. Phys. Lett. 77 1885-1887. https://doi.org/10.1063/1.1310635 8. Lin C Y, Wang S Y, Lee D Y and Tseng T Y 2008 Electrical properties and fatigue behaviors of ZrO2 resistive switching thin films Journal of The Electrochemical Society 155 H615-H619. https://doi.org/10.1149/1.2946430 9. Müller J, Böscke T S, Schröder U, Mueller S, Bräuhaus D, Böttger U, Frey L and Mikolajick T 2012 Ferroelectricity in Simple Binary ZrO2 and HfO2 Nano Letters 12 4318- 4323. https://doi.org/10.1021/nl302049k 10. Weeks S L, Pal A, Narasimhan V K, Littau K A and Chiang T 2017 Engineering of Ferroelectric HfO2−ZrO2 Nanolaminates ACS Appl. Mater. Interfaces 9 13440–13447. https://doi.org/10.1021/acsami.7b00776 11. Jia X, Yang W, Qin M and Li J 2009 Structure and magnetism in Mn-doped zirconia: Density-functional theory studies Journal of Magnetism and Magnetic Materials 321 2354- 2358. https://doi.org/10.1016/j.jmmm.2009.02.132 12. Dimri M C, Kooskora H, Pahapill J, Joon E, Heinmaa I, Subbi J and Stern R 2011 Search for ferromagnetism in manganese-stabilized zirconia Physica Status Solidi A - Applications and Materials Science 208 172-179. https://doi.org/10.1002/pssa.201026304 13. Hong N H, Kanoun M B, Goumri-Said S, Song J H, Chikoidze E, Dumont Y, Ruyter A and Kurisu M 2013 The origin of magnetism in transition metal-doped ZrO2 thin films: experiment and theory Journal of Physics: Condensed Matter 25 436003. https://doi.org/10.1088/0953-8984/25/43/436003 Page 20 of 27AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
21 14. Dimri M C, Khanduri H, Kooskora H, Kodu M, Jaaniso R, Heinmaa I, Mere A, Krustok J and Stern R 2012 Room-temperature ferromagnetism in Ca and Mg stabilized cubic zirconia Journal of Physics D - Applied Physics 45 475003. https://doi.org/10.1088/0022- 3727/45/47/475003 15. Chouhan L, Bouzerar G and Srivastava S K 2020 d(0) Ferromagnetism in Ag-doped monoclinic ZrO2 compounds Vacuum 182 109716. https://doi.org/10.1016/j.vacuum.2020.109716 16. Ning S, Zhan P, Xie Q, Li Z and Zhang Z 2013 Room-temperature ferromagnetism in undoped ZrO2 thin films Journal of Physics D: Applied Physics 46 445004. https://doi.org/10.1088/0022-3727/46/44/445004 17. Pattanaik S, Mishra D K, Sharma M K and Chatterjee R 2020 Experimental evidences of ferromagnetism in undoped monoclinic zirconia Inorganic Chemistry Communications 118 108042. https://doi.org/1016/j.inoche.2020.108042 18. Oyama S T 2000 Chemical and catalytic properties of ozone Catalysis Reviews 42 279- 322. https://doi.org/10.1081/CR-100100263 19. Torresi S C and Gorenstrein A 1992 Electrochromic behaviour of manganese dioxide electrodes in slightly alkaline solutions Electrochimica acta 37 2015-2019. https://doi.org/10.1016/0013-4686(92)87117-I 20. Strandwitz N C, Comstock D J, Grimm R L, Nichols-Nielander A C, Elam J and Lewis N S 2013 Photoelectrochemical behavior of n-type Si (100) electrodes coated with thin films of manganese oxide grown by atomic layer deposition The Journal of Physical Chemistry C 117 4931-4936. https://doi.org/10.1021/jp311207x 21. Mattelaer F, Bosserez T, Rongé J, Martens J A, Dendooven J and Detavernier C 2016 Manganese oxide films with controlled oxidation state for water splitting devices through a combination of atomic layer deposition and post-deposition annealing RSC advances 6 98337- 98343. https://doi.org/10.1039/C6RA19188F 22. Gao P, Meng L J, Dos Santos M P, Teixeira V and Andritschky M 2000 Characterisation of ZrO2 films prepared by rf reactive sputtering at different O2 concentrations in the sputtering gases Vacuum 56 143-148. https://doi.org/10.1016/S0040-6090(00)01395-X Page 21 of 27 AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
22 23. Landorf R W and Licht S J 1972 Sputtered Manganese Dioxide as Counterelectrodes in Thin Film Capacitors Journal of The Electrochemical Society 119 430. https://doi.org/10.1149/1.2404223 24. Neubeck W, Ranno L, Hunt M B, Vettier C and Givord D 1999 Epitaxial MnO thin films grown by pulsed laser deposition Applied surface science 138 195-198. https://doi.org/10.1016/S0169-4332(98)00421-8 25. Shen Y, Shao S, Yu H, Fan Z, He H and Shao J 2007 Influences of oxygen partial pressure on structure and related properties of ZrO2 thin films prepared by electron beam evaporation deposition Applied surface science 254 552-556. https://doi.org/10.1016/j.apsusc.2007.06.029 26. Seike T and Nagai J 1991 Electrochromism of 3d transition metal oxides Solar energy materials 22 107-117. https://doi.org/10.1016/0165-1633(91)90010-I 27. Jeon T S, White J M, Kwong D L 2001 Thermal stability of ultrathin ZrO2 films prepared by chemical vapor deposition on Si (100) Applied Physics Letters 78 368-370. https://doi.org/10.1063/1.1339994 28. Rizzi G A, Zanoni R, Di Siro S, Perriello L and Granozzi G 2000 Epitaxial growth of MnO nanoparticles on Pt (111) by reactive deposition of Mn2(CO)10 Surface science 462 187- 194. https://doi.org/10.1016/S0039-6028(00)00608-7 29. Perednis D, Wilhelm O, Pratsinis S E and Gauckler L J 2005 Morphology and deposition of thin yttria-stabilized zirconia films using spray pyrolysis Thin solid films 474 84-95. https://doi.org/10.1016/j.tsf.2004.08.014 30. Valletta R M and Pliskin W A 1967 Preparation and characterization of manganese oxide thin films Journal of The Electrochemical Society 114 944. https://doi.org/10.1149/1.2426786 31. Kukli K, Niinistö J, Tamm A, Lu J, Ritala M, Leskelä M and Putkonen M 2007 Atomic layer deposition of ZrO2 and HfO2 on deep trenched and planar silicon Microelectronic engineering 84 2010-2013. https://doi.org/10.1016/j.mee.2007.04.035 32. Aarik L, Alles H, Aidla A, Kahro T, Kukli K, Niinistö J and Mändar H Influence of process parameters on atomic layer deposition of ZrO2 thin films from CpZr(NMe2)3 and H2O Thin Solid Films 565 37-44. https://doi.org/10.1016/j.tsf.2014.06.052 Page 22 of 27AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
23 33. Kim H, McIntyre P C and Saraswat K C 2004 Microstructural evolution of ZrO2–HfO2 nanolaminate structures grown by atomic layer deposition Journal of materials research 19 643-650. https://doi.org/10.1557/jmr.2004.19.2.643 34. Tamm A, Kozlova J, Aarik L, Aidla A, Lu J, Kiisler A A, Kasikov A, Ritslaid P, Mändar H, Hultman L, Sammelselg V, Kukli K and Aarik J 2014 Atomic layer deposition of ZrO2 for graphene‐based multilayer structures: In situ and ex situ characterization of growth process physica status solidi (a) 211 397-402. https://doi.org/10.1002/pssa.201330106 35. Lin Y C, McGuire F and Franklin A D 2018 Realizing ferroelectric Hf0.5Zr0.5O2 with elemental capping layers Journal of Vacuum Science & Technology B, Nanotechnology and Microelectronics: Materials, Processing, Measurement, and Phenomena 36 011204. https://doi.org/10.1116/1.5002558 36. Nilsen O, Fjellvåg H and Kjekshus A 2003 Growth of manganese oxide thin films by atomic layer deposition Thin Solid Films 444 44-51. https://doi.org/10.1016/S0040- 6090(03)01101-5 37. Ghods A, Zhou C and Ferguson I T 2020 Structural and optical properties of (Zn, Mn) O thin films prepared by atomic layer deposition Journal of Vacuum Science & Technology A: Vacuum, Surfaces, and Films 38 042408. https://doi.org/10.1116/6.0000141 38. Arroval T, Aarik L, Rammula R, Kruusla V and Aarik J 2016 Effect of substrateenhanced and inhibited growth on atomic layer deposition and properties of aluminum– titanium oxide films Thin Solid Films 600 119–125. http://dx.doi.org/10.1016/j.tsf.2016.01.024 39. Kalam K, Seemen H, Ritslaid P, Rähn M, Tamm A, Kukli K, Kasikov A, Link J, Stern R, Dueñas S and Castán H 2018 Atomic layer deposition and properties of ZrO2/Fe2O3 thin films Beilstein Journal of Nanotechnology 9 119-128. http://dx.doi.org/10.3762/bjnano.9.14 40. Granneman E, Fischer P, Pierreux D, Terhorst H and Zagwijn P 2007 Batch ALD: Characteristics, comparison with single wafer ALD, and examples Surface and coatings technology 201 8899-8907. https://doi.org/10.1016/j.surfcoat.2007.05.009 41. Zagwijn P M, Verweij W, Pierreux D, Adjeroud N, Bankras R, Oosterlaken E, Snijders G J, Van den Hout M, Fischer P, Wilhelm R and Knapp M 2008 Novel Batch Titanium Nitride CVD Process for Advanced Metal Electrodes ECS Transactions 13 459. https://doi.org/10.1149/1.2911530 Page 23 of 27 AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript
24 42. Fairley N 2018 CasaXPS: Processing Software for XPS, AES, SIMS and More (Casa Software Ltd., 2018) [online] http://www.casaxps.com/. [Google Scholar] 43. Castán H, Dueñas S, García H, Ossorio O G, Domínguez L A, Sahelices B, Miranda E, González M B and Campabadal F 2018 Analysis and control of the intermediate memory states of RRAM devices by means of admittance parameters Journal of Applied Physics 124 152101. https://doi.org/10.1063/1.5024836 44. Castán H, Dueñas S, Kukli K, Kemell M, Ritala M and Leskelä M 2018 Study of the influence of the dielectric composition of Al/Ti/ZrO2:Al2O3/TiN/Si/Al structures on the resistive switching behavior for memory applications ECS Transactions 85 143-148. https://doi.org/10.1149/08508.0143ecst 45. Dueñas S, Castán H, Ossorio O G, Vinuesa G, García H, Kukli K and Leskelä K 2020 Double Swing Quiescent-Current: An Experimental Detection Method of Ferroelectricity in Very Leaky Dielectric Films ECS Transactions 97 3-6. https://doi.org/10.1149/09701.0003ecst 46. Ritala M and Leskelä M 1994 Zirconium dioxide thin films deposited by ALE using zirconium tetrachloride as precursor Applied Surface Science 75 333-340. https://doi.org/10.1016/0169-4332(94)90180-5 47. Siimon H and Aarik J 1997 Thickness profiles of thin films caused by secondary reactions in flow-type atomic layer deposition reactors Journal of Physics D: Applied Physics 30 1725. https://doi.org/10.1088/0022-3727/30/12/006 48. Bocquet A E, Mizokawa T, Morikawa K, Fujimori A, Barman S R, Maiti K, Sarma D D, Tokura Y and Onoda M 1996 Electronic structure of early 3d-transition-metal oxides by analysis of the 2p core-level photoemission spectra Phys. Rev. B 53 1161. https://doi.org/10.1103/PhysRevB.53.1161 49. NIST X-ray Photoelectron Spectroscopy Database, NIST Standard Reference Database Number 20, National Institute of Standards and Technology, Gaithersburg MD, 20899 (2000), https://doi.org/10.18434/T4T88K, (retrieved Nov. 22, 2020). 50. Stranick M A 1999 MnO2 by XPS Surface Science Spectra 6 31. https://doi.org/10.1116/1.1247888 Page 24 of 27AUTHOR SUBMITTED MANUSCRIPT - NANO-128626.R2 1 2 3 4 5 6 7 8 9 10 11 12 13 14 15 16 17 18 19 20 21 22 23 24 25 26 27 28 29 30 31 32 33 34 35 36 37 38 39 40 41 42 43 44 45 46 47 48 49 50 51 52 53 54 55 56 57 58 59 60 Accepted Manuscript