! !! ! ! Surface!characterization!and!cell! instructive!properties!of!superficially! modified!dental!zirconia!! ! Doctoral!Program!of!Materials!Science!and!Engineering!! ! Joaquim!Minguela!Díaz! Carles!Mas-Moruno,!supervisor! Joan!Josep!Roa!Rovira,!supervisor! ! Thesis!as!a!compendium!of!publications! ! Biomaterials,!Biomechanics!and!Tissue!Engineering!Research!Group! Center!for!Structural!Integrity,!Reliability!and!Micromechanics!of! Materials! Universitat!Politècnica!de!Catalunya!-!BarcelonaTech! ! Barcelona,!May!2021!
Preface'' ! I! Preface! ! The!Ph.D.!Thesis!is!presented!as!a!compendium!of!three!original!papers.!All!the! work! included! in! these! papers! has! been! carried! out! at!the! Departament) de) Ciència) i) Enginyeria) de) Materials) at! the) Universitat) Politècnica) de) Catalunya) -) BarcelonaTech,! under! the! supervision! of! Dr.! Carles! Mas! Moruno! and! Dr.! Joan! Josep! Roa! Rovira.! Part! of! the! work,! in! particular! the! evaluation! of! residual! stresses! and! the! laser-patterning,! were! carried! out! during! my! research! stage! conducted!at!the!Chair!of!Functional!Materials!(FuWe)!group!at!the!Universität! des!Saarlandes!(Saarbrücken,!Germany).! ! This! PhD.! Thesis! has! been! supported! by! a! Predoctoral! fellowship! from! the! Barcelona)Research)Center)in)Multiscale)Science)and)Engineering.! ! Joaquim!Minguela! ! Barcelona,!2021!
Abstract'' ! III! Abstract! ! Tetragonal! polycrystalline! zirconia! doped! with! 3! mol%! yttria! (3Y-TZP)! has! become! one! of! the! most! popular! dental! ceramics.! Thanks! to! its! outstanding! mechanical!properties!(including!high!hardness,!toughness!and!wear!resistance),! biocompatibility! and! white! color,! it! is! now! commonly! employed! to! produce! components!such!as!crowns,!implants,!abutments,!bridges!or!posts!and!cores.! ! In! the! case! of! dental! implants,! which! are! directly! screwed! into! the! jawbone,! implant’s! surfaces! can! be! modified! through! different! physical! or! chemical! techniques! to! ensure! a! rapid! and! proper! osteointegration.! In! the! first! case,! surface!topography!is!known!to!play!a!critical!role!in!cell-material!interactions! and! to! influence! several! cell! functions! such! as! adhesion,! proliferation! or! differentiation.! In! the! second! case,! specific! chemical! cues! such! as! integrinbinding! peptidic! molecules! from! bone! extracellular! matrix! can! affect! cell! behavior!with!a!high!degree!of!specificity.!The!combination!of!both!strategies! may!provide!a!powerful!tool!to!obtain!an!improved!bone-to-implant!contact!and! ensure!long!lasting!implants.! ! In! this! Ph.D.! Thesis! a! dual! approach! employing! surface!topographical! modification! and! peptidic! biofunctionalization! on! dental! zirconia! is! explored,! with!the!aim!of!providing!a!flexible!tool!to!improve!tissue!integration!of!ceramic! restorations.!! ! Regarding! surface!topographical! modifications,! two! different! strategies!are! investigated:!grinding!and!laser-micropatterning.!Both!of!them!can!generate!not! only!rough!surfaces!at!the!micro-!and!submicrometric!length!scale!but!also!other! features! such! as! grooves,! which! may! guide! cell! growth.! However,! these! two! techniques! are! based! on! different! principles.! While! in! grinding!technique! the! material!is!removed!by!a!mechanical!process,!laser!patterning!is!based!on!the! thermal!effects!of!absorbed!photons.!!
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! IV! ! However,!these!methods! are! not!exempt!from!introducing!a!certain!degree!of! surface!damage,!which!can!be!detrimental!for!the!final!application.!In!addition,! 3Y-TZP! is! susceptible! of! a! spontaneous! surface! phase! transformation! from! tetragonal!(t-)!to!monoclinic! (m-)! phase! under! two!different! scenarios.! One! is! known! as! transformation! toughening! and! it! is! a! stress-assisted! mechanism! accompanied!by!a!volume!increase!(∼!4%)!activated!by!the!near!tip!crack!stress! field,!which!increase!crack!propagation!resistance.!On!the!other!hand,!a!second! scenario!exists!known!as!low!temperature!degradation!(LTD).!In!this!case,!aging! by! progressive! t) →) m! transformation! at! the! surface! is! triggered! by! water! molecules.! In! this! particular! case,! this! mechanism! induces! roughening! and! micro-cracking,!which!can!drastically!reduce!the!mechanical!properties!and!in! particular!the!wear!resistance!by!generating!pull-out!of!3Y-TZP!grains.!In!this! regard,!some!surface!treatments!can!affect!the!LTD!resistance!of!the!material,!or! even!induce!this!phase!transformation.!For!these!reasons,!a!particular!emphasis! is! placed! on! the! changes! in! the! surface! and! subsurface! introduced! by! both! methods.! Damage,! microstructure,! phase! transformation! and! residual! stresses! are!characterized,!as!well!as!its!effects!on!LTD!and!mechanical!properties.!! ! On!the!other!hand,!peptidic!biofunctionalization!is!carried!out!by!using!a!peptidic! platform! that! incorporates! the! cell-adhesive! RGD! and! the! osteogenic! DWIVA! motives.! This! strategy! is! combined! with! the! best! performing! topographymodifying! treatment.! On! this! surface! that! integrates! the! stimuli! provided! by! topography! and! the! peptides,! cell! adhesion,! cell! migration! and! osteogenic! properties!are!characterized!in!detail.! ! The! results! of! this! Ph.D.! Thesis! may! serve! as! a! further! step! in! the! journey! of! developing!zirconia-based!ceramic!materials!to!become!a!reference!material!in! prosthodontics.!The!dual!functionalization!presented!here!is!a!powerful!tool!to! improve!the!tissue!integration!and!healing! success!of!3Y-TZP!dental!implants.! Importantly,! both! the! topography! and! the! peptidic! platform! can! be! easily! modified!and!designed!to!fulfill!different!requirements!(osteogenic,!angiogenic,! antibacterial,!etc.).!!!
Resum'' ! V! Resum! ! La!zircònia!policristal·lina!tetragonal! dopada!amb!un!3%! d’ítria! (3Y-TZP)!s’ha! convertit! en! una! de! les! ceràmiques! dentals! més! populars.! Gràcies! a! les! seves! excel·lents!propietats!mecàniques!(inclosa!l’alta!duresa,!tenacitat!i!resistència!al! desgast),! la! biocompatibilitat! i! el! color! blanc,! ara! s’utilitza! habitualment! per! produir!components!com!corones,!implants!o!ponts.! ! En!el!cas!d’implants!dentals,!que!es!cargolen!directament!a!l’os!de!la!mandíbula,! les! superfícies! de! l’implant! es! poden! modificar! mitjançant! diferents! tècniques! físiques!o!químiques!per!garantir!una!osteointegració!ràpida!i!adequada.!En!el! primer! cas,! se! sap! que! la! topografia! superficial! té! un! paper! crític! en! les! interaccions!cèl·lula-material!i!que!influeix!en!diverses!funcions!cel·lulars!com! ara! l’adhesió,! la! proliferació! o! la! diferenciació.! En! el! segon! cas,! els! estímuls! químics!específics!com!els!que!indueixen!les!molècules!peptídiques!de!la!matriu! extracel·lular! òssia! poden! afectar! el! comportament! cel·lular! amb! un! alt! grau! d’especificitat.!La!combinació!d’ambdues!estratègies!pot!proporcionar!una!eina! poderosa!per!obtenir!una!millor!interacció!entre!l’os!i!l’implant!i!garantir!una! vida!llarga!als!implants.!! ! En!aquesta!tesis!doctoral!s'explora!una!estratègia!dual!que!utilitza!la!modificació! superficial!de! la! topografia!i! la! biofuncionalització! peptídica! sobre! zircònia! dental,!amb!l'objectiu!de!proporcionar!una!eina!flexible!per!millorar!la!integració! amb!els!teixits!de!les!restauracions!ceràmiques.!! ! Pel! que! fa! a! les! modificacions! superficials! de! la! topografia,! s’estudien! dues! estratègies!diferents:!rectificat!i!micro-patrons!làser.!Tots!dos!poden!generar!no! només!superfícies!rugoses!a!l’escala!micro-!i!submicromètrica,!sinó!també!altres! característiques!com!ara!canals/solcs,!que!poden!guiar!el!creixement!cel·lular.! Tot!i!això,!aquestes!dues!tècniques!es!basen!en!principis!diferents.!Mentre!que!en!
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! VI! la! tècnica! de! rectificat! el! material! s’elimina! mitjançant! un! procés! mecànic,! el! patró!làser!es!basa!en!els!efectes!tèrmics!dels!fotons!absorbits.! ! No!obstant!això,!aquests!mètodes!no!estan!exempts!d’introduir!un!cert!grau!de! dany!a!la!superfície,!que!pot!ser!perjudicial!per!a!l’aplicació!final.!A!més,!la!3Y- TZP! és! susceptible! d’una! transformació! espontània! de! fase! des! de! la! fase! tetragonal!(t-)!a!la!monoclínica!(m-)!sota!dos!escenaris!diferents.!Un!es!coneix! com! a! augment) de) tenacitat) per) transformació) de) fase! (“transformation! toughening”,!en!anglès)!i!és!un!mecanisme!activat!per!esforços!acompanyat!d’un! augment! de! volum! (∼! 4%).! Aquest! procés! està! activat! pel! camp! d’esforços! proper! a! una! esquerda,! augmentant!la! resistència! a! la! propagació! de! les! esquerdes.!D’altra!banda,!existeix!un!segon!escenari!conegut!com!degradació!a! baixa!temperatura!(“low!temperature!degradation”,!en!anglès).!En!aquest!cas,!la! progressiva! transformació! de! t! →! m! a! la! superfície! és! provocada!per! les! molècules!d'aigua.!Aquest! mecanisme!indueix!rugositat!i! micro-esquerdes!a!la! superfície,! que! poden! reduir! dràsticament! les! propietats! mecàniques! i,! en! particular,! la! resistència! al! desgast.! En! aquest! sentit,! alguns! tractaments! superficials!poden!afectar!la!resistència!a!la!degradació!del!material!o!fins!i!tot! induir!aquesta!transformació!de!fase.!Per!aquestes!raons,!es!fa!un!èmfasi!especial! en!els!canvis!en!la!superfície!introduïts!per!tots!dos!mètodes.!Es!caracteritzen!els! danys,!la!microestructura,!la!transformació!de!fase!i!les!tensions!residuals,!així! com! els! seus! efectes! sobre! les! propietats! mecàniques! i! la! degradació! a! baixa! temperatura.! !! D’altra! banda,! la! biofuncionalització! peptídica! es! realitza! mitjançant! una! plataforma!peptídica!que!incorpora!el!motiu!adhesiu!RGD!i!el!motiu!osteogènic! DWIVA.! Aquesta! estratègia! es! combina! amb! el! tractament! modificador! de! la! topografia!amb!el!millor!rendiment!(rectificat!o!micro-patrons!làser).!En!aquesta! superfície!on!s’integren!els!estímuls!proporcionats!per!la!topografia!i!els!pèptids,! s’estudia!l’adhesió!cel·lular,!la!migració!cel·lular!i!les!propietats!osteogèniques.!! ! Els!resultats!d’aquesta!tesis!doctoral!es!poden!considerar!com!un!pas!més!en!el! desenvolupament!de!materials!ceràmics!amb!base!de!zircònia!per!convertir-se!
Resum'' ! VII! en! un! material! de! referència! en! prostodòncia.! La! doble! funcionalització! presentada! aquí! és! una! potent! eina! per! millorar! la! integració! del! teixit! i! la! capacitat!de!curació!dels!implants!dentals!de!3Y-TZP.!És!important!destacar!que! tant! la! topografia! com! la! plataforma! peptídica! es! poden! modificar! i! dissenyar! específicament!per!complir!altres!requisits!(osteogènic,!angiogènic,!antibacterià,! etc.).
Glossary'of'acronyms'' ! XV! Glossary!of! acronyms! ! ! ! 3Y-TZP!3!mol%!yttria!stabilized!tetragonal!zirconia!polycrystal! ALP!Alkaline!phosphatase! BIC!Bone-implant!contact! BMP-2!Bone!morphogenetic!protein!2! BMSC!Bone!marrow!stromal!cells! c-!Cubic! CAD!Computer-aided!design! CAM!Computer-aided!manufacturing! Ce-TZP!Ceria!stabilized!tetragonal!zirconia!polycrystal! CLSM!Confocal!laser!scanning!microscopy! CN!Coordination!number! DAPI!4′,6-diamidino-2-phenylindole! DLIP!Direct!laser!interference!patterning! DNA!Deoxyribonucleic!acid! DWIVA!Asp-Trp-Ile-Val-Ala!tetrapeptide! ECM!Extracellular!matrix! FBR!Foreign!body!response! FIB!Focused!ion!beam! FPD!Fixed!partial!denture! FSZ!Fully!stabilized!zirconia! GAG!Glycosaminoglycans! HA!Hydroxyapatite! IGF-1!Insulin-like!growth!factor!1! IR!Infrared! L-DOPA!L-3,4-dihydroxyphenylalanine!
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! XVI! LTD!Low!temperature!degradation! M!Multidirectional! m-!Monoclinic! m →'t!Monoclinic!to!tetragonal!phase!transformation! MC3T3!Mouse!osteoblast-like!cells! Mg-PSZ!Magnesia!doped!partially!stabilized!zirconia! MSC!Mesenchymal!stem!cell! PBS!Phosphate-buffered!saline! PCL!Polycaprolactone! PEG!Polyethylene!glycol! PFA!Paraformaldehyde! PLGA!Poly(D,L-lactic-co-glycolic!acid)! PMA!Polymethacrylic!acid! PSZ!Partially!stabilized!zirconia! PVA!Poly(vinyl!alcohol)! Ra!Average!roughness! RGD!Arg-Gly-Asp!tripeptide! Sa!Surface!average!roughness! SaOS-2!Human!sarcoma!osteogenic!cell! SBF!Simulated!body!fluid! SEM!Scanning!electron!microscopy! SOFC!Solid!oxide!fuel!cell! t-!Tetragonal! t →!m!Tetragonal!to!monoclinic!phase!transformation! TBC!Thermal!barrier!coating! TEM!Transmission!electron!microscopy! TGF-β!Transforming!growth!factor!β!!! THR!Total!hip!replacement! TZP!Tetragonal!zirconia!polycrystal! U!Unidirectional! UV!Ultraviolet! Vm!Monoclinic!volume!fraction!! XRD!X-ray!diffraction!
Glossary'of'acronyms'' ! XVII! Y-TZP!Yttria!stabilized!tetragonal!zirconia!polycrystal! ZTA!Zirconia!toughened!alumina!
! ! Chapter!1! Introduction! ! ! !
Introduction' ! 3! 1!Introduction!! 1.1 Zirconia:!an!overview! 1.1.1 Brief!history!of!zirconia! ! Zirconia! (ZrO2)! was! first! extracted! in! 1787! from! jacinth,! a! variety! of! zircon! (ZrSiO4)!used!as!a!gemstone,!by!the!German!chemist!Martin!Heinrich!Klaproth! (1743! -! 1817).! During! the! following! 150! years! after! its! discovery,! no! technological! uses! were! found! for! ZrO2,! except! for! certain! niche! applications,! such! as! the! production! of! bricks! for! high! temperature! applications! and! its! employment! in! glasses! of! high! index! of! refraction! [1].! This! apparent! lack! of! technical!uses!was!mainly!due!to!the!impossibility!of!producing!solid!and!dense! parts!after!sintering.!! ! Pure!ZrO2!is!a!polymorphic!material!and!can!be!found!in!three!main!crystalline! arrangements:! monoclinic! (m),) tetragonal! (t)! and! cubic! (c),! as! displayed! in! Figure'1![2].!At!room!temperature!it!presents!a!m-structure!and!transforms!into! t-!when!heating!above!1170°C.! If!further!heated,! it!transforms!into!c-phase!at! 2370°C.! After! the! sintering! process,! the! t-phase-containing! material! is! cooled! down!and!reversibly!transforms!again!into!m-phase.!Such!transformation!is!of! martensitic! nature! and! is! accompanied! by! a! 4! %! of! volume! expansion,! which! cannot!be!accommodated!by!the!bulk!material!and!leads!to!extensive!cracking.!! ! ! Figure!1)The)three)polymorphs)of)ZrO2.)a))Monoclinic,)b))tetragonal)and)c))cubic.) Red)atoms)correspond)to)zirconium,)while)blue)atoms)correspond)to)oxygen)[2].) !
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 4! It!was!not!until!1929!that!Ruff!et)al.!showed!that!c-phase!could!be!stabilized!at! room!temperature!by!the!addition!of! oxides,! such! as! magnesium!oxide!(MgO)! and! calcium! oxide! (CaO)! [3,4],! avoiding! the! detrimental! t →! m) phase! transformation.! Through! this! method,! both! c-!and! t-phases! were! retained! at! room!temperature!in!a!metastable!form.!A!material!known!as!partially-stabilized! zirconia!(PSZ)!was!produced,!consisting!on!a!dispersion!of!fine!m-/t-!precipitates! in! a! c-matrix.! However,! the! key! discovery! for! the! production! of! high-strength! zirconia!was!made!in!1975!and!published!in!the!work!Ceramic)steel?)by!Garvie!et) al.) [5].! Garvie! and! his! coworkers! found! that! the! presence! of! metastable! tprecipitates!in!PSZ!improved!drastically!the!mechanical!properties.!It!was!stated! that! the! increase! in! strength! was! mainly! due! to! the! energy! absorption! of! the! stress-induced!t →!m)phase)transformation.!This!mechanism!is!now!known!as! “transformation!toughening”!and!relies!on!the!phase!expansion!of!the!m-phase.! Stresses!at!the!tip!of!an!advancing!crack!can!destabilize!the!metastable!t-phase! and!trigger!the!t →!m)phase!transformation.!The!volume!change!associated!to!the! m-phase!creates!a!compressive!field!that!opposes!to!the!opening!of!the!crack,! strengthening! the! material! [2],! as! illustrated! in! Figure' 2.! In! order! to! take! advantage! of! this! mechanism,! efforts! on! the! successive! years! were! put! on! creating!fully!t-!phase!materials,!known!as!tetragonal!zirconia!polycrystals!(TZP)! [6],!and!first!developed!by!Rieth!et)al.)[7]!and!by!Gupta!et)al.)[8].! !
Introduction' ! 5! ! Figure! 2)Transformation)toughening)mechanism.)Stresses)at)the)tip)of)the)crack) trigger)the)t-)to)m-phase)transformation.)The)volume)increase)of)the)transformed) material)closes)the)crack,)hampering)its)propagation)[9].) 1.1.2 Classification! ! According! to! its! stabilization! degree,! several! types! of! microstructures! can! be! obtained:! ! - Fully'stabilized'zirconia'(FSZ):!such!materials!are!constituted!by!only!czirconia.! They! are! obtained! by! employing! a! high! concentration! of! stabilizers.! Their! applications! include,! among! others,! the! production! of! refractory!materials,!solid!oxide!fuel!cells!(SOFCs)!or!oxygen!sensors.! - Partially' stabilized' zirconia' (PSZ):!they!are!constituted!by!a!c-matrix! with!a!dispersion!of!nano-sized!t-precipitates.!They!can!be!obtained!by! doping!with!MgO!(as!shown!in!Figure'3a!)!or!CaO.! - Tetragonal' zirconia' polycrystals' (TZP):!they!consist!in!a!stabilized!tphase!material,!which!can!contain!a!certain!amount!of!c-phase,!depending! on! the! stabilizer! concentration.! They! possess! high! strength! and! toughness.!The!most!common!stabilizers!to!obtain!such!microstructures! are!yttrium!oxide!or!yttria!(Y2O3,!see!Figure'3b)!and!cerium!oxide!or!ceria!! (CeO2).!
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 12! change.! As! depicted! in! Figure' 8' the! first! step! consists! in! the! nucleation! of! a! martensite!plate,!with!a!shear!component!of!~0.16!and!a!volumetric!change!of! ~0.045![2].!If!constraint!in!a!bulk!material!(i.e.!not!in!the!surface),!the!stresses! derived!from!the!shear!component!induce!the!formation!of!a!second!variant!with! an! opposed! shear! strain,! cancelling! the! shear! effects! of! the! first! variant.! This! phase!transformation!process!is!autocatalytic!and!proceeds!with!the!formation! of!twin!related!variants.!The!result!is!a!shear!component!near!to!zero,!and!a!net! volume!change!around!~0.045.!! ! ! Figure! 8)t →)m)phase)transformation)process.)a))t-)material.)b))Transformation) starts) and) a) m-) lath) nucleates.) c)) Stresses) originated) in) the) surrounding) matrix) promote) the) formation) of) a) second) twin-related) variant,) with) an) opposed) shear) component.)d))Transformation)further)proceeds)[2].) ! As!described!by!Lange![19],!from!a!thermodynamical!point!of!view!the!condition! for!transformation!can!be!written!as:! ! ! 𝛥𝐺!!!=𝛥𝐺!+𝛥𝑈!" +𝛥𝑈!! Eq.)1) ! where! 𝛥𝐺!!!!is! the! change! in! total! free! energy! of! the! t →! m) phase! transformation.! When! it! becomes! negative,! t-! particles! are! unstable! and! may! transform.!𝛥𝐺!!is!the!difference!in!chemical!free!energy!between!the!t-!and!m-) phases.!Below!the!To(t/m)!temperature,!𝛥𝐺!<0!(see!Figure' 7).!It!depends!on! both! temperature! and! stabilizer! content.! Thus,! in! order! to! have! a! t-!particle! 𝛥𝐺!<𝛥𝑈!" +𝛥𝑈!.!The!term!𝛥𝑈!"!is >0!and!corresponds!to!the!elastic!strain!
Introduction' ! 13! energy!associated!to!the!phase!change!of!the!particle.!It!depends!on!the!stiffness! of! the! matrix,! size! and! shape! of! the! particle! and! surrounding! stresses.! In! this! sense,! hydrostatic! tensile! stresses! reduce! the! value! of! this! variable,! favoring! transformation.! On! the! contrary,! compressive! stresses! increase! its! value,! stabilizing! the! t-!particle.! Finally,!𝛥𝑈!!is! also!>0!and! refers! to! the! change! in! energy!associated!to!the!surface!of!the!particle,!such!as!crack!generation.! ! With!the!above!considerations,!transformation!toughening!can!be!explained,!as! follows.! In! the! front! of! an! advancing! crack,! shear! and! tensile! stresses! reduce! 𝛥𝑈!"!enough!so!that!𝛥𝐺!!!!becomes!negative!and!t-!particles!become!unstable.! The!t →!m)transformation!is!triggered!and!the!volume!expansion!of!the!material! at! the! crack! tip! produces! a! compressive! stress! field,! opposing! to! crack! propagation.! This! mechanism! has! been! presented! in! section! 1.1.1!and! is! depicted! in! Figure' 2.! Thus,! transformation! toughening! is! able! to! reduce! the! stress!intensity!factor!at!the!crack!tip![18,20],!increasing!fracture!toughness:! ! ! ! 𝐾!"#$ =𝐾!−𝐾!"!! Eq.)2) ! where!𝐾!!is! the! stress! intensity! factor! applied! by! external! forces;!𝐾!"!!is! the! stress! shielding! effect! due! to! the! transformation! toughening! mechanism;! and! 𝐾!"#$!is!the!real!stress!intensity!factor!at!the!crack!tip.!! ! 1.1.6 Low-temperature!degradation! ! As!explained!previously!in!section1.1.5,!one!of!the!consequences!of!the!t-phase! metastability! is! the! transformation! toughening! mechanism.! However,! it! also! constitutes! the!basis! of! a! deleterious! process,! known! as! low-temperature! degradation!(LTD),!ageing!or!hydrothermal!degradation.! ! This! process! was! first! reported! in! 1981! by! Kobayashi! [21]!and! has! been! described!by!other!authors![22–28].!In!humid!environments,!a!progressive!and!
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 14! uncontrolled!transformation!of! the! grains!in!the!surface! from! the!t-!to!the!m-! phase!is!triggered.!This!transformation!is!associated!to!the!generation!of!microcracks!and!can!advance!inside!the!material!until!the!catastrophic!failure!of!the! specimen.!Yoshimura![22]!described!its!main!features!as:! ! - The! degradation! occurs! significantly! at! temperatures! between! 200! and! 300°C! in! air.! However,! it! must! be! noted! that! it! can! also! occur! at! body! temperature!after!prolonged!periods!of!time,!with!a!special!relevance!in! biomedical!implants![29].! - Degradation!starts!in!the!surface!and!progresses!to!the!bulk.! - The! volume! change! associated! to! the! t →! m) phase)transformation! produces!macro-!and!micro-cracking.! - Water!and!water!vapor!accelerate!the!t →!m)phase!transformation.! - By!increasing!dopant!concentration!or!by!reducing!grain!size,!the!process! can!be!delayed.! ! The!exact!mechanisms!by!which!water!molecules!can!destabilize!the!t-phase!are! still!debated,!but!there!is!a!consensus!about!the!important!role!played!by!oxygen! vacancies.! In! humid! environments,! water–derived! species! (OH-)! occupy! the! oxygen!vacancies!of!the!surface,!reducing!its!number!and!introducing!stresses!in! the!lattice![30,31].!Schubert!and!Frey![32]!found!a!contraction!in!the!lattice!after! LTD,!which!introduced!tensile!stresses!of!around!300-500!MPa,!destabilizing!the! t-phase.!According!to!the!authors,!the!introduction!of!OH-!was!the!responsible!of! this! contraction,! with! oxygen! atoms! occupying! the! vacancies! and! hydrogen! atoms! located! at! interstitial! sites.! However,! more! recently,! Duong! et) al.![33]! found! that! moisture! diffusion! occurs! by! parallel! but! independent! H+!and! O2-! diffusion.! What! is! clear,! is! that! diffusion! of! such! species! can! destabilize! the! tphase!on!the!surface!and!that!this!process!can!continue!inside!the!bulk!material.! The!series!of!events!are!as!follow!(see'Figure'9):! ! - First,!an)m-phase!lath!nucleates!at!the!surface!of!the!most!unstable!grain! (i.e.!larger!grains,!grains!with!lower!Y2O3!content,!etc.)!and!it!propagates!
Introduction' ! 15! inside!the!grain!by!self-accommodated!variants,!as!described!in'Figure'8.! This!initial!stage!is!shown!in'Figure'9a.! - Martensite! (m-)! plates! reaching! the! grain! boundaries! generate! microcracks!as!well!as!stresses!at!the!neighboring!grains,!favoring!the!creation! of!new!plates!on!the!surrounding!grains!(see!Figure'9b).!This!is!known!as! autocatalytic!propagation![27].!In!addition,!the!net!volume!increase!of!the! transformed! particles! generates! additional! stresses! and! micro-cracks.! Thus,!m-phase!does!not!appear!homogeneously!throughout!the!surface,! but! nucleates! in! specific! grains! and! propagate,! by! a! nucleation-and- growth!mechanism.!! - Water!can!penetrate!through!micro-cracks,!promoting!the!degradation!of! deeper!layers!in!combination!with!the!autocatalytic!propagation.!Pull-out! of!superficial!grains!can!be!observed.!Transformation!advances!to!deeper! layers!weakening!the!material,!until!final!failure!happens!as!depicted!in! Figure'9c.! ! ! ! Figure!9)Schematic)representation)of)the)LTD)process.)a))m-phase)nucleates)on)the) surface.)b))Once)the)surface)is)transformed,)the)process)extends)to)deeper)layers.)At) this)point,)micro-cracks)and)grain)uplifts)due)to)volume)expansion)are)observed)on) the)surface.)c)) Transformation) propagates)inside)the) bulk.) The)surface)is) totally) transformed) and) extensive) grain) pull-out) can) be) observed) as) well) as) microcracking.) Water) can) penetrate) inside) the) material,) assisting) degradation.) Mechanical)properties)of)the)surface)get)severely)affected)[27].) !
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 16! The!main!features!of!the!subsurface!damage!after!LTD!have!been!characterized! in! detail.! Jiménez-Piqué! et) al.) [34])studied! the! network! of! micro-cracks! after! degradation.!They!found!that!the!cracks!were!mostly!parallel!to!the!surface!and! that!they!displayed!a!density!gradient!from!the!surface.!A!3D!focused!Ion!beam! (FIB)! tomography! reconstruction! is! displayed! in! Figure' 10a,! where! a! small! volume!of!the!degraded!layer!is!shown.!The!crack!network!(in!purple)!induced! during!the!LTD!process!is!clearly!evident.! ! In!addition,!Jiménez-Piqué!et)al.)concluded!that!the!decrease!in!elastic!modulus! of!the!degraded!layer!was!not!due!to!the!increase!in!m-content,!but!rather!to!the! presence!of!the!micro-cracks,!which!can!be!observed!in!Figure'10b.! ! ! Figure!10)a))Three)perspectives)of)the)reconstructed)network)of)micro-cracks)(in) purple))under)the)surface)after)LTD) process.)Yellow)material)corresponds)to)the) protective)platinum)layer)deposited)onto)the)surface.)Red)dots)correspond)to)pores.) b))A)FIB)cross-section)showing)the)crack)network)[34].) !
Introduction' ! 17! LTD! is! of! especial! relevance! in! the! biomedical! field,! where! the! lifespan! of! implants!can!be!reduced!due!to!the!moisture!of!the!biological!environment![29].! In! 2001! a! series! of! failures! in! 3Y-TZP! hip! replacements! (i.e.! femoral! heads),! resulted!in!drastic!decrease!in!the!use!of!3Y-TZP!for!orthopedic!applications![24].! Although! the! failures! were! mainly! related! to! an! increase! in! porosity! due! to! a! change!in!the!sintering!process,!an!increase!in!the!t →!m)phase)transformation! was! identified! in! the! porous! regions,! playing! a! secondary! role! in! the! deterioration! of! properties! [35].! Since! then,! efforts! have! been! made! to! understand,! control! and! avoid! LTD.! In! order! to! evaluate! the! behavior! of! a! ceramic!component!after!LTD,!accelerated!tests!can!be!carried!in!water!steam.!In! this! regard,! the! degradation! process! kinetics! can! be! described! by! the! Mehl- Avrami-Johnson!equation![36],!as!follows:! ) 𝑓 !=1−𝑒𝑥𝑝[−(𝑏𝑡)!]! Eq.)3) ! where!𝑓 !!is! the! monoclinic! volume! fraction,! t! is! the! degradation! time,! b)is! an! activation! energy! term! (𝑏=𝑏! 𝑒𝑥𝑝 [−! !"])! and! n!an! exponent! related! to! the! nucleation!and!growth!conditions.!At!higher!temperatures,!reaction!kinetics!are! faster.! Thus,! by! performing! experiments! at! such! temperatures,! the! relevant! parameters! can! be! extracted,! and! kinetics! extrapolated! at! room! temperature.! Ageing!kinetics!of!3Y-TZP!are!typically!determined!in!water!steam!at!134°C!and! 2!bar!of!pressure,!with!1!hour!of!degradation!corresponding!to!3-4!years!in)vivo.! However,!as!the!particular!microstructural!features!of!each!material!affect!the! degradation!kinetics,!for!accurate!results!the!correct!determination!of!b!and!n) should!be!carried!out![23,37].! ! ! ! ! !
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 18! 1.2 Zirconia!in!restorative!dentistry! 1.2.1 Brief!history!of!dental!zirconia! ! The! loss!of! teeth,! particularly! anterior! teeth,! creates! not! only! a! functional! impairment,!but!also!psychological!and!social!problems,!due!to!its!aesthetic!role.! Before!the!advent!of!modern!artificial!implants,!it!was!common!to!use!natural! materials! to! replace! missing! teeth,! such! as! teeth! from! human! donors,! carved! animal!teeth,!ivory,!wood!or!bone.!These!solutions!were!unstable!in!human!oral! environment,! presenting! several! disadvantages,! including! change! in! color! and! unpleasant! odor.! In! 1774,! the! Parisian! apothecary! Alexis! Duchâteau! and! the! dentist!Nicholas!Dubois!de!Chémant!made!the!first!successful!porcelain!denture.! Since!then!and!during!the!following!two!centuries,!a!continuous!improvement! was!made!in!ceramic!dental!materials![38,39].!! ! The!first!paper!regarding!a!biomedical!application!for!zirconia!was!published!in! 1969!by!Helmer!and!Driskell![40],!and!it!was!not!until!1988!when!Christel!et)al.) suggested!the!use!of!zirconia!to!produce!femoral!heads!for!total!hip!replacement! (THR)![41].!Unfortunately,!as!noted!above,!after!a!LTD-related!failure!of!around! 400! zirconia! ball! heads! in! 2001,! the! use! of! zirconia! in! the! biomedical! field! suffered!a!drastic!decrease![24].!However,!thanks!to!the!developments!made!in! the!90s,!the!dental!community!showed!a!special!interest!in!the!material!due!to!its! excellent! mechanical! properties! (strength,! hardness,! wear! resistance! and! fracture!toughness),!biocompatibility!and!its!good!aesthetic!appearance.!These! properties,!which!make!it!suitable!in!dental!restorations,!depend!on:!grain!size,! presence! of! an! intergranulary! glassy! phase,! stability! of! the! t-phase,! porosity,! elastic!modulus!and!thermal!expansion!mismatch!between!components.!In!this! sense,! Y-TZP! was! introduced! to! produce! several! restorations,! including! fixed! partial!dentures!(FPD),!implants,!abutments,!post!and!cores,!etc.!Thus,!during!the! last! twenty! years! TZP-based! ceramics! have! attracted! an! increasing! attention! from!the!dental!community,!with!several!products!in!the!market!and!an!evolving! composition! and! processing! techniques! to! match! market! needs! [42,43]!(see! Table'2).!! !
Introduction' ! 19! Table!2)Listing)of)some)representative)TZP)formulations)in)the)dental)market)[44].) Classification' Generation' Material'name' Manufacturer' Composition' ! ! Y-TZP! 1! Lava!Frame! 3M!ESPE! 3Y-TZP! Zenostar!MO! Wieland!Dental! 3Y-TZP! 2! Lava!Plus! 3M!ESPE! 3Y-TZP! Zenostar!T! Wieland!Dental! 3Y-TZP! 3! Lava!Esthetic! 3M!ESPE! 5Y-PSZ! Zenostar!MT! Wieland!dental! 4Y-PSZ! Y-TZP/!Al2O3! -! ZirTough! Kuraray- Noritake! Y-TZP/4! mass%!Al2O3! Ce-TZP/!Al2O3! -! NANOZR! Panasonic! 70!vol.%!10Ce- TZP/30! vol.%! Al2O3! ! ! Although! most! of! the! commercial! products! are! based! on! Y-TZP,! Ce-TZP/Al2O3! composites!are!also!available.!During!the!short!live!of!zirconia!in!the!dental!field,! three!generations!of!materials!in!terms!of!composition!and!powder!processing! have!been!developed.!After!a!first!generation!of!Y-TZP!materials!(containing!0.25! wt%!alumina,!as!a!sintering!aid)!with!excellent!mechanical!properties,!a!second! generation! of! zirconia! was! developed,! with! lower! Al2O3! content!and! higher! sintering!temperatures!in!order!to!improve!translucency.!A!third!generation!has! recently!been!developed!with!a!higher!Y2O3!content!(4-5!mol%),!which!improved! translucency! by! increasing! its! c-phase! content,! at! the! expense! of! mechanical! properties![43,44].!As!the!interest!in!such!materials!grow,!new!formulations!and! processing! techniques! will! arise,! with! the! aim! at! obtaining! high! strength,! translucent!and!LTD-resistant!materials.! ! 1.2.2 Applications!in!dentistry! ! Several! dental! components! are! produced! nowadays! with! Y-TZP,! including! crowns,! fixed! partial! dentures,! posts! and! cores,! implants! and! abutments.! The! manufacturing! process! is! based! on! computer-aided! design/computer-aided!
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 20! manufacturing!(CAD/CAM)!technology,!allowing!to!produce!both!prefabricated! and!custom-made!components.!Regarding!the!latter!type!and!depending!on!the! component,! a! personalized! computer! design! can! be! made! based! on! three! dimensional!(3D)!scans!of!the!patient’s!defect.!Two!approaches!can!be!followed! on!the!manufacturing!process:!hard!and!soft!machining![43,45–47].!! ! • In!hard!machining,!a!fully!sintered!Y-TZP!block!is!milled!down!to!the!final! shape! with! diamond! tools.! Such! approach! involves! high! tool! wear! and! costs,!is!time-consuming!and!requires!robust!milling!systems.!! • On!the!other!hand,!soft!machining!is!the!most!common!technique,!and!is! based! on! the! milling! of! pre-sintered! blocks! of! zirconia! with! tungsten! carbide!burs.!At!this!point,!binders!of!the!original!powders!have!already! been! burnt! and! the! Y-TZP! block! is! minimally! hardened! by! the! presintering!treatment.!The!machined!part!is!enlarged!by!a!20-25%!relative! to!its!final!dimensions,!as!during!the!final!sintering!step!it!suffers!a!linear! shrinkage,!which!may!involve!the!need!of!final!shape!corrections!after!the! heat!treatment.!! ! Regardless! of! the! manufacturing! process,! the! final! material! must! meet! some! general!requirements,!which!are!listed!in!Table'3.! ! Table!3)Engineering)guides)for)manufacturing)zirconia-based)ceramics)for)dental) applications)[37].) Property' Unit' Requirement' Density! %!of!theoretical!density! >!99%! Stabilizer!content:!Y2O3! mol%! 3!<!x!<!8! Grain!size! μm! GS!<!0.3! Residual!stress! MPa! σ!<!300!(tensile)! Monoclinic!content! !!!!!!Initial! !!!!!!After!aging!test!(134°C,!2!bar!H2O,!1!h)! Volume!fraction!to!total!zirconia! ! Negligible! Negligible! Strength!in!4-point!bending! !!!!!!Initial! !!!!!!After!aging! MPa! ! 600! 600!
Introduction' ! 21! ! !The! following! paragraphs! include! a! description! of! the! different! dental! prostheses!that!can!be!produced!of!zirconia-based!ceramic!materials:! ! Crowns:! crowns! are! used! when! teeth! present! functional!or! aesthetic! defects! in! size,! shape,! color! or! function.! They! consist! on! a! “cap”! that! covers! the! tooth.! They! can! also! be! placed! on! the! top! of! an! implantabutment!system!in!order!to!replace!a!tooth.!As!zirconia!presents!a!white! color!and!opacity!that!does!not!fully!match!the!natural!look!of!a!tooth,! they! can! be! stained! before! sintering! and! veneered! with! feldspathic! porcelain.! In! posterior! crowns,! however,! due! to! the! lower! aesthetic! requirements! and! the! higher! loads! monolithic! crowns! can! be! placed,! avoiding! the! use! of! veneers,! which! can! suffer! from! chipping.! Surface! mechanical! pre-treatments! such! as! grinding! or! sandblasting! may! be! applied!to!the!surfaces!in!order!to!improve!adhesion!of!the!veneer!and/or! the!adhesion!of!the!crown!to!the!underlying!structures.!Other!alternatives! to! zirconia! are! full! metallic! crowns! (with! low! aesthetics)! or! porcelain! fused!to!metal.! ! Fixed! partial! dentures:'fixed! partial! dentures! (FPDs)! are! meant! to! replace!several!missing!teeth!and!are!permanently!fixed!to!adjacent!teeth! or!implants.! Its! structure!(see! Figure' 11)! is! similar! to! a! “bridge”! lying! over! two! “pillars”.! The! “pillars”! can! be! the! adjacent! teeth! or! dental! implants!(abutments).!The!“bridge”!consists!on!the!retainers!(that!unite! the! bridge! to! the! underlying! teeth! or! abutment),! the! pontic! (the! suspended!part!of!the!bridge)!and!the!connector!(that!unites!retainer!and! pontic)![48].!When!a!force!from!biting!is!applied!to!the!pontic,!the!load!is! transmitted!to!the!connector,!retainer!and!finally!to!the!abutment!and!the! surrounding! bone! structure.! Similarly! to! crowns,! chipping! of! the! veneering!is!the!major!problem!that!may!occur!over!time![45].)
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 28! ! Figure! 14)Representation)of)the)initial)cell)adhesion)to)a)surface)immersed)in)a) biological)fluid.)The)chemical)properties)of)the)surface)determine)the)composition) of)the)adsorbed) layer) and)the)conformation) of) the)adhered) proteins.) When) cells) reach)the)surface)they)bind)to)specific)ligands)found)in)this)layer)of)biomolecules) [60].) ! The!chemical!properties!of!the!surface!affect!both!the!composition!of!the!layer! and!the!conformation!(and!thus,!the!functionality)!of!the!adhered!proteins.!The! situation!is!generally!different!in)vitro!than!in)vivo,!due!to!the!distinct!chemical! composition!of!cell!culture!media!and!physiological!fluids.!While!cells!cultured!in) vitro)depend! mainly! on! cell! adhesive! proteins! from! the! serum! to! adhere! (e.g.! fibronectin!and!vitronectin),!in)vivo!they!are!also!accompanied!by!other!proteins! such!as!fibrinogen!or!albumin.!One! of!the!main! contributions!to!cell!adhesion! from!these!molecules!comes!from!the!presence!of!the!arginine-glycine-aspartic! acid!(RGD)!amino!acid!sequence![61].!Cells!can!bind!to!this!sequence!through! integrin! receptors! establishing! stable! bonds! that! evolve! into! focal! complexes! (see! Figure' 15).! Focal! complexes! are! bound! intracellularly! to! actin! filaments,! participating! in! cytoskeleton! organization! and! mechanotransduction,! and! are! involved! in! the! capacity! of! the! cell! to! adhere,! spread,! divide! and! migrate.! In!
Introduction' ! 29! addition,! the! layer! of! adhered! proteins! may! provide! binding! sites! for! growth! factors,!promoting!cell!differentiation,!as!observed!in!fibronectin![62].!! ! ! Figure! 15) Model) of) the) proteins) composition) and) position) in) a) focal) adhesion.) Integrins)(in)red))can)attach)to)the)RGD)sequence)in)the)extracellular)matrix.)Once) bound) they) gather) together) in) large) complexes) called) focal) adhesions.) These) complexes) are) bound) to) the) actin) filaments) (in) blue)) through) a) series) of) intracellular)proteins)[63].) ! From!the!physical' point' of' view,!two!main! contributions! can! be! found! from! surface!properties:!topography!and!stiffness.!Surface!topography!can!modify!cell! behavior! in! terms! of! adhesion,! spreading,! migration,! differentiation,! and! gene! expression![64–69].!The!effects!of!topography!depend!on!cell!type!but!also!on! the! scale! of! the! features! respect! cell! size! [55]!(see! Figure' 16).! For! macrotopographical!features,!much!larger!than!cells,!the!increase!in!surface!roughness! favors!a!better!bone-surface!interlocking,!ensuring!mechanical!stability![70].!On! the!other!hand,!at!the!micro-!(1!-!10!μm)!and!sub-micrometric!length!scale!(100! nm!-!1!μm),!both!in)vivo)and!in)vitro)studies!show!improved!results!by!comparing! micro-rough! versus! flat! implants.! In! fact,! most! of! the! dental! implants! in! the! market!take!advantage!of!these!observations,!presenting!an!Ra!ranged!between! 1-2!μm![70].!In!this!regard,!in)vivo)studies!reported!higher!bone-implant!contact! and! higher! torques! needed! to! remove! roughened! screws! as! compared! to! flat!
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 30! ones! [71,72].! This! may! be! attributed! on! the! one! hand! to! an! enhanced! micromechanical! retention! [73]!and! on! the! other!hand! to! a! higher! number! and! activation! of! platelets! on! rougher! surfaces!(producing! the! fibrin! clots! that! facilitate! cell! migration! to! the! surface)! [74,75].! In) vitro,) higher! osteoblast! differentiation!and!local!factor! production! has! been!observed!for!micro-rough! surfaces![76,77],!although!the!exact!mechanisms!are!still!under!debate.!! ! In!recent!years,!the!importance!of!controlling!nano-topography!(<!100!nm)!has! also!been!highlighted.!Integrin!receptors!interact!with!ligands!at!the!nanometric! length!scale!and!the!spacing,!density,!and!distribution!of!adhesive!nano-sites!has! been! shown! to! highly! affect! integrin! clustering! and,! thus,! the! adhesion! and! spreading!quality![78].!Nano-features!can!affect!not!only!cell!adhesion![79,80],! but! also! improve! osteogenesis! [81–83].! In! fact,! Dalby! et)al.![68]! found! that! a! certain! degree! of! nano-feature! disorder! could! influence! stem! cell! phenotype,! indicating! that! organization! of! the! topography! is! as! important! as! its! size! and! shape.! Due! to! the! fact! that! bone! presents! a! hierarchical! structure! at! different! length!scales!(i.e.!from!macro-!to!nano-),!the!mimicking!of!such!combination!has! been!addressed,!with!improved!results!respect!to!the!use!of!only!micro-!or!nano-! features![84].! ! !
Introduction' ! 31! ! Figure!16)Representation)of)the)influence)of)topography)at)different)length)scales.) At)the)macro-scale,)mechanical)bone-surface)interlocking)ensures)primary)stability) of)the)implant.)At)the)micro-scale,)roughness)introduces)micro-mechanical)stability) as) well) as) provides) mechanical) cues) to) cells) that) influence) adhesion,) spreading,) proliferation,)migration)and)differentiation.)At)the)nano-scale,)interactions)at)the) integrin)level)affect)focal)adhesion)and)cytoskeleton)organization,)which)triggers) cell)signaling)from)the)mechanotransduction)machinery)[55].) ! As!mentioned!before,!stiffness!is!another!physical!property!that!can!affect!cell! behavior.!Indeed,!the!stiffness!of!the!substrate!where!cells!are!growing!can!guide! stem! cell! differentiation! into! specific! lineages! [85,86].! Cells! can! sense! forces! exerted! by! the! matrix! through! the! actin! structures! linked! to! focal! adhesions.! These! forces!result! in! intra-cellular! signaling! that! can! affect! gene! expression.! Interestingly,!this!process!is!independent!from!the!stimulation!by!soluble!factors,! but!presents!synergism!with!it.!Thus,!the!stiffness!of!a!biomaterial!must!be!in! concordance! to! the! tissue! it! replaces.! In! the! case! of! bone,! rigid! materials! are! preferred;! in! the! case! of! other! tissues! such! as! muscle,! softer! materials! are! required![86].!! ! In!this!regard,!Figure' 17!displays!how!substrates!with!different!stiffness!affect! the!morphology!of!MSCs.!When!MSCs!were!grown!on!substrates!with!a!stiffness!
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 32! resembling! brain! tissue,! muscle! or! the! crosslinked! collagen! in! osteoids,! differentiation!was!guided!to!the!lineage!of!each!corresponding!tissue:!neurons,! myoblasts!or!osteoblasts,!respectively.!! ! ! Figure!17)Human)MSCs)cultured)on)substrates)with)different)stiffness:))0.1-1)kPa) (brain)stiffness),)8-17)kPa)(muscle)stiffness))and)25-40)kPa)(stiffness)of)crosslinked) collagen) of) osteoids).) After) 96) hours) of) culture,) cell) morphology) was) completely) different) in) the) substrates:) branched) neuron-like) cells) in) the) softer) substrates,) spindle) myoblast-like) cells) in) the) intermediate) stiffness) substrate,) and) polygonal) cells)in)the)stiffest)one.)Scale)bar)is)20)μm)[86].) Mineralized!bone,! as!well!as!materials! intended!to!replace!bone! (e.g.!zirconia,! titanium),! present! a! higher! stiffness! than! the! one! employed! in! the! study! of! Figure' 17.!Thus,!on!such!surfaces,!MSCs!tend!to!differentiate!into!osteoblasts.! The!Young’s!modulus!of!cortical!bone,!titanium!and!Y-TZP!are!listed!in!Table'4.! !
Introduction' ! 33! Table!4)Young’s)modulus)of)typical)materials)for)dental)implants,)as)compared)to) bone.) Material' Young’s'Modulus'(GPa)' Cortical!Bone! 20! Ti6Al4V! 110! 3Y-TZP! 210! ! ! It!can!be!observed!that!the!Young’s!modulus!of!both!titanium!alloys!and!zirconia! ceramics! are! much! higher! than! the! one! of! human! bone.! This! difference! of! stiffness!is!responsible!of!a!mechanism!known!as!“stress!shielding”![87].!In!the! surgery!of!long!bones,!such!as!the!femur,!the!higher!stiffness!of!the!prosthetic! elements!can!“shield”!the!surrounding!bone!from!experiencing!the!desired!levels! of!stress.!If!the!bone!does!not!experience!a!certain!level!of!mechanical!stresses!it! gets! progressively! resorbed,! which! compromise! the! bone-implant! function.! However,! in! the! dental! field! the! “stress! shielding”! effect! on! the! implant-jaw! system! has! not! been! confirmed.! In! fact,! recent! studies! based! on! numerical! simulations!have!highlighted!the!benefits!of!using!stiff!materials![88].!! ! Given!the!broad!range!of!stimuli!that!the!surface!deliver!to!cells,!both!physical! and! chemical! modifications! are! performed! to! implants! in! order! to! favor! osteointegration.! Such! modifications! may! be! oriented! to! provide! a! better! mechanical! retention,! such! as! macro-roughening! of! the! surface,! or! may! be! designed! to! improve! interactions! at! the! material-cell! level! such! as! facilitating! adhesion,!migration!or!cell!differentiation.!! ! ! ! ! ! !
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 34! 1.4 Surface!modification!of!zirconia!based!ceramics! 1.4.1 Topographical!modifications! 1.4.1.1 Relevant+techniques+in+zirconia+dental+prostheses+ ! Commercial! dental! implants! are! generally! roughened! to! promote! faster! and! better!implant-bone!integration,!obtaining!improved!bone-implant!contact!(BIC)! and! removal! torques,! in) vivo.! Modifications! are! mostly! addressed! to! increase! both!surface!area!and!macro-/micro-!mechanical!retention.!However,!the!effect! of! micro-! and! nano-topography! on! bone-like! cells,! although! probably! present! and!beneficial,!is!not!specifically!targeted!in!such!modifications.!Thus,!most!of! the! employed! techniques! are! directed! towards! a! general! increase! in! surface! roughness!at!different!length!scales,!but!not!towards!the!creation!of!particular! topographies!that!trigger!specific!cell!functions.! ! The! most! common! techniques! employed! in! Y-TZP! implants! include! machining/grinding,!sandblasting,!chemical!etching!and!laser!patterning![89,90].! Other! methods! employed! on! titanium! implants! such! as! anodization! are! not! suitable! because! of! the! lack! of! electrical! conductivity!of! zirconia.! While! sandblasting! and! chemical! etching! produce! random! topographical!features,! grinding! can! produce! directional! (although! also! random)! patterns.! The! three! latter! modifications! (i.e.! grinding,! sandblasting! and! etching)! are! the! most! common!and!are!employed!in!several!commercial!implants.!! ! Among! the! techniques! that! allow! creating! specific! pre-designed! topographies,! laser! patterning! stands! out! due! to! the! possibility! of! creating! features! at! the! micron-!and!submicron-!level![91,92].!Although!its!commercial!use!is!still!limited! (e.g.!Z!systems,!Oensingen,!Switzerland)!due!to!its!lower!processing!speeds!and! the!cost!of!the!involved!technology,!research!on!this!subject!in!recent!years!has! highlighted! the! potential! of! the! technique.! In! this! regard,! alternative! methods! able!to!create!defined!topographies,!such!as!lithographic-based!techniques,!are! also! highly! relevant! in! the! research! field! due! to! their!high! resolution! and! flexibility!but!lack!the!processing!speeds!needed!for!commercial!use.!
Introduction' ! 35! One! aspect! that! must! be! noted! is! that,! in! general,! such! techniques! not! only! modify! surface! topography,! but! are! also! accompanied! by! microstructural! changes! and! micro-damage! that! may! influence! LTD! behavior! and! mechanical! properties! [93,94].! The! changes! introduced! might! be! beneficial! or! not,! and! therefore,!detailed!characterization!of!the!surface!and!its!properties!are!required! after!such!modifications.!A!brief!description!of!the!cited!superficial!treatments!is! outlined!below:! ! Grinding:)a!surface!finishing!method!similar!to!polishing,!which!involves! coarser!abrasive!media.!The!surface!of!the!material!is!in!contact!with!a! rotating! grinding! wheel,! which! consists! on! abrasive! particles! (usually! diamond)!embedded!in!a!matrix,!as!depicted!in!Figure' 18.!The!contact! between!these!sharp!particles!and!the!material!creates!a!combination!of! plastic!flow!and!brittle!fracture!(i.e.!micro-cracks,!decohesion,!etc.).!In!this! sense,! material! removal! takes! place! by! chipping! and! the! confluence! of! cracks! from! adjacent! penetration! sites! [95].! If! the! depth! of! cut! of! the! grinding! wheel! is! sufficiently! low,! a! ductile! regime! can! be! achieved,! reducing! surface! damage! [96].! This! technique! can! be! used! both! as! a! surface!finishing!procedure!or!to!adjust!the!final!shape!of!a!component.!! ! ! Figure! 18)SEM)micrographs)of)a))surface)of)a)bur.)Embedded)diamond)particles) can) be) observed) [97])and) b)) 3Y-TZP) surface) after) grinding.) The) tracks) left) by) abrasive)particles)are)evident.) !
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 36! Sandblasting:)this!technique!consists!on!the!projection!of!a!hard-ceramic! particles! jet! onto! the! surface,! generating! plastic! deformation! and! removing!chunks!of!material!(see!Figure'19a).!It!has!been!widely!used!in! dentistry!to!not!only!achieve!a!better!osteointegration!of!implants![98],! but! also! to! enhance!the! bonding! between! dental! crowns! and! luting! cement! or! between! the! crown! and! the! veneering! porcelain,! due! to! an! increase! in! surface! area! and! wettability! [99,100].! The! mechanism! by! which!a!particle!from!the!jet!is!able!to!erode!the!material!is!based!on!the! particular! interaction! particle-surface,! which! is! similar! in! nature! to! a! quasi-static!indentation![101].!The!high!stresses!around!the!collision!zone! create!lateral!and!radial!cracks!that!can!propagate!and!lead!to!material! pull! out! with! successive! impacts.! Lateral! cracks! are! responsible! for! material!chipping!while!radial!cracks!penetrate!through!the!material!and! are!responsible!for!a!reduction!in!strength.!Depending!on!the!particles’! size,! speed,! and! impact! angle! different! values! of! roughness! can! be! achieved.! As! some! remnant! particles! may! be! strongly! attached! to! the! surface!after!the!treatment,!a!biocompatible!material!must!be!chosen!for! the! particles! used.! In! this! regard,! materials! such! as! alumina! (Al2O3),! titanium! dioxide! (TiO2)! or! calcium! phosphates! are! suitable! for! this! purpose![98].!) ) Chemical! etching:)this!surface!treatment!consists!on!the! dissolution!of! the!material’s!surface!by!an!alkali!or!an!acid!etchant,!creating!a!roughness! at!the!micro-!and!the!nanometric!length!scale.!Although!Y-TZP!presents!a! very! high! chemical! inertness,! it! has! been! successfully! etched! with:! hydrofluoric! acid!(HF),! hypophosphorous! acid! (H3PO2),! potassium! hydroxide!(KOH)!and!sodium!hydroxide!(NaOH);!being!HF!the!agent!with! the!fastest!etching!rate![102–104].!) Chemical!etching!is!frequently!used!in!combination!with!sandblasting!in! order!to!superimpose!nano-roughness!to!a!previously!micro-roughened! substrate![102],!as!shown!in!Figure'19b.! )
Introduction' ! 37! ! Figure!19)SEM)micrographs)of)a))sandblasted)Y-TZP)and)b))sandblasted)and)alkali) etched)Y-TZP.)The)introduction)of)nano-roughness)to)sandblasted)specimens)can)be) clearly)observed)[105].) ! Laser! Patterning:)this!technique!consists! on! the! creation! of! a! surface! pattern!by!selectively!removing!material!with!a!laser!beam!(see!Figure' 20).! High! density! optical! energy! is! required! to! melt,! dissociate! (break! chemical!bonds),!vaporize!and!expulse!material!from!the!interaction!zone! [106].! Several! types! of! lasers,! working! modes! and! techniques! may! be! used,! creating! different! types! of! laser-material! interaction! [107]!that! allow! producing! a! wide! range! of! patterns! and! topographies,! including! features! at! the! micron-! and! submicron-! length! scale! [108].! It! is! a! noncontact! technique,! which! avoids! surface! contamination! as! well! as! tool! wear,!which!is!especially!relevant!when!machining!hard!ceramics.! ! !
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 44! ! Figure! 23) Cells) growing) on) a) ground) 3Y-TZP) surface.) Alignment) of) cell) bodies) along)the)grooves)is)observed.)In)red,)cell)cytoskeleton;)in)blue,)cell)nucleus.)The) image)was)obtained)in)the)experimental)work)of)this)thesis.) ! 1.4.1.3 Laser+micro-patterning+ ! Laser!applications!are!of!interest!for!a!variety!of!fields!including!the!scientific,! industrial,!medical! or! military.! They! can! be! used!to!transmit! information! (e.g.! telecommunications),!gather!information!(e.g.!measuring!devices)!or!as!a!tool!to! modify! matter! (e.g.! laser! marking,! cutting,! welding,! etc.),! among! others.! Depending!on!the!properties!of!the!laser!beam,!such!as!wavelength!or!intensity,! the!mechanisms!by!which!it!interacts!with!matter!can!change,!affecting!surface! chemistry,! topography! or! phase! composition! in! different! ways! [136].! In! particular,! when! short! pulses! of! high! energy! are! employed,! localized! melting,! vaporization! or! ablation! are! possible,! which! has! been! of! especial! interest! in! surface!engineering.!!In!this!field,!laser!techniques!have!been!employed!to!create! micro-patterns! on! the! surface! of! metallic! [137],! ceramic! ! and! polymeric! components![138]!by!selectively!removing!material.!! ! In!order!to!create!such!patterns!different!techniques!can!be!employed,!including! direct!laser!writing,!projection!patterning!or!direct!laser!interference!patterning!
Introduction' ! 45! (DLIP)![136].!The!latter!technique,!DLIP,!allows!producing!surface!patterns!by! the!inhomogeneous!energy!distribution!produced!by!the!interference!of!two!or! more!laser!beams.!When!coherent!and!linearly!polarized!beams!are!allowed!to! interfere! on! a! surface,! the! particular! intensity! distribution! depends! on! the! wavelength,!number!of!beams!and!their!relative!angles![139,140].!If!beams!are! energetic!enough,!their!interaction!with!the!surface!produces!material!removal! and!a!surface!pattern!is!created![92,141–144].!Different!patterns!depending!on! the!number!of!beams!are!shown!in!Figure'24.! ! ! ! Figure! 24)Different)intensity)distribution)patterns)with)two)(left),)three)(center)) and) four) (right)) beams.) On) the) top) the) intensity) distribution) is) shown.) On) the) bottom,)the)corresponding)beam)geometry)[142].) ! Several!studies!have!successfully!attempted!to!create!micro-patterns!on!Y-TZP,! and! the! majority! focused! on! linear! structures! [91,92,145–152],! achieving! features!at!the!micron!scale.!The!most!common!approaches!involve!the!use!of! laser! equipment! providing! pulses! at! the! nanosecond! (mostly! Nd:YAG! at! a! wavelength! of! 1064! nm,! or! 532/355/266! nm! by! second! and! third-harmonic! generation)!or!femtosecond!time-scale!(in!general!Ti:sapphire!at!a!wavelength! around!800!nm).!Although!both!time!regimes!are!suitable!to!micro-structure!Y-
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 46! TZP,! the! nature! of! laser-material! interaction! is! different,! and! therefore! the! produced! topography,! surface! damage! and! microstructural! changes! are! also! different.! The! mechanisms! underlying! this! effect! are! related! to! energy! absorption,! relaxation! and! the! time-scale! of! the! pulses! involved,! and! are! explained!below![107,136,153].! ! Laser!radiation!is!absorbed!by!the!electrons!of!the!target!material.!In!Y-TZP!(and! most!of!dielectrics),!the!large!gap!between!the!valence!and!the!conduction!bands! (≈4-5!eV![154,155])!restricts!the!linear!absorption!of!photons!to!wavelengths!in! the!ultraviolet!(UV)!or!shorter.!However,!at!high!intensities!such!as!in!the!case!of! short! pulsed-lasers,! non-linear! optical! processes! take! place! and! multi-photon! absorption!is!possible.!By!this!effect,!several!photons!with!energy!lower!than!the! band!gap!can!be!absorbed!at!the!same!time,!and!thus,!lasers!emitting!at!longer! wavelengths!can!be!employed!(visible!and!infrared!(IR)).!! ! The!incident!energy!from!photons!is!thus!transferred!to!free!electrons,!which!are! in!an!excited!state.!The!time!needed!to!transfer!this!energy! to! the! lattice! and! reach!an!electron-lattice! thermal!equilibrium!is!in!the!order!of!10-12!s.!At!this! point,!the!duration!of!the!pulse!is!critical.!If!laser!pulses!at!the!nanosecond!(10-9! s)!regime!are!delivered,!electrons!have!enough!time!to!transfer!their!energy!to! the!lattice!through!electron-lattice!collisions,!and!the!main!energy!loss!is!heat! conduction!into!the!solid![107].!This!way,!material!removal!takes!place!mainly! by!thermal!mechanisms!(melting,!vaporization,!etc.)!However,!if!the!laser!pulses! are!at!the!femtosecond!regime!(10-15!s),!there!is!insufficient!time!to!transfer!the! energy! to! the! lattice! and! electrons! are! heated! at! high! temperature! almost! instantaneously.!Material!removal!is!thus!carried!out!by!non-thermal!processes,! i.e.!ablation!(electrostatic!ablation,!Coulomb!explosion,!photolysis,!etc.)![153].!! ! In! practice,! in! each! time! regime! several! mechanisms! can! take! place! simultaneously,! although! one! of! them! is! predominant.! In! Y-TZP,! melting! and! vaporization!are!the!main!responsible!for!material!removal!in!the!nanosecond! regime,!while!ablation!is! observed! in! the! femtosecond.!Thus,!different!surface! features!are!observed!after!treatments!in!one!or!another!regime.!!
Introduction' ! 47! Surface)and)microstructural)changes) ! Materials!patterned!with!nanosecond!lasers!present!a!surface!layer!with!evident! signs!of!melting!and!resolidification.!Several!defects!can!be!observed,!with!the! presence!of!cracks!(due!to!thermal!shock),!pores!and!droplets![92,152].!Stresses! generated! by! such! cracks! trigger! the! t →! m) phase! transformation[152,156].! Slight!texture!in!the!t-phase!has!been!also!measured!and!due!to!resolidification! some!microstructural!changes!have!been!observed,!such!as!recrystallization!and! columnar! grain! growth! in! the! recast! layer! [156].! In! contrast,! femtosecond! treated! surfaces! present! a! difference! appearance,! with! features! indicating! ablation!instead!of!melting.!Scarce!efforts!have!been!dedicated!to!the!study!of!the! surface!changes!on!Y-TZP!after!patterning!with!femtosecond!lasers.!Some!subsuperficial!micro-cracks!and!pores!were!observed!by!Stanciuc!et)al.)[148])after! patterning,! as! well! as! ripple! formation! under! certain! conditions! [148,157].! In! addition,! very! small! amounts! of! phase! transformation! were! found! [91,149].! Characteristic!features!of!laser-modified!surfaces!in!both!regimes!are!shown!in! Figure'25.! ! ! Figure! 25) SEM) micrographs) of) the) surface) features) of) laser-modified) Y-TZP.) a)) Surface)appearance)after)modification)with)a)nanosecond)regime)laser.)A)layer)of) resolidified)material)is)visible,)with)the)presence)of)droplets)and)cracks)[152].)Scale) bar) is) 5) μm.) b)) A) pit) produced) with) a) femtosecond) regime) laser.) Ripples) are) observed)on)the)bottom)of)the)pit)[148].)Scale)bar)is)15)μm.) !
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 48! Mechanical)properties)and)low)temperature)degradation) ! Although! of! particular! relevance,! just! a! few! works! have! studied! mechanical! properties!and!LTD!resistance!after!such!treatments.!Daniel!et)al.)[158]!observed! an!increase!in!mechanical!properties!in!the!nanosecond!regime,!which!attributed! to! compressive! residual! stresses! and! a! reduced! grain! size.! However,! more! recently,! both! Pereira! et) al.) [152]!and! Roitero! et) al.) [159])found! a! reduced! strength! but! a! slightly! increased! Weibull! modulus.! In! particular,! Roitero! and! coworkers! attributed! the! reduced! strength! to! the! enlargement! of! pre-existing! defects!(i.e.!pores)!close!to!the!surface.!! ! Pereira! et) al.) [152]!found! a! worsening! of! the! LTD! resistance! after! laser! patterning!in!the!nanosecond!pulse!regime,!which!could!be!improved!in!some! cases!by!a!thermal!treatment.!Roitero!et)al.)[94])obtained!similar!results.!They! found! an! overall! decreased! LTD! resistance! after! laser! patterning.! Although! compressive!residual!stresses!favored!slower!phase!transformation!kinetics,!the! presence! of! a! higher! initial! m-phase! content! (due! to! the! laser-patterning! process)! decreased! the! overall! ageing! resistance.! However,! after! a! thermal! treatment!at!1200°C!degradation!was!improved!respect!as-sintered!specimens.! Such!improvements!were!related!to!the!reversible)m)→)t)phase!transformation,! the!presence!of!texture!induced!by!the!laser!treatment,!as!well!as!the!generation! of!a!micro-cracked!network!on!the!surface!(due!to!the!laser!treatment),!which! could!potentially!hinder!autocatalytic!phase!transformation.! ! Cellular)response) ! Laser! machined! micro-patterns! on! zirconia-based! materials! can! modulate! cell! morphology.!Different!topographies!have!been!produced!such!as!pits![148]!and! linear!structures![149–151,160,161].!While!pits!can!just!affect!cell!morphology! (i.e.! size,! aspect! ratio,! circularity,! etc.),! linear! structures! can! also! promote! cell! alignment!(see!Figure'26).!Several!studies!have!shown!improved!response!from! cells!of!the!bone!lineage!when!growing!on!linearly!patterned!zirconia!substrates.! These!enhancements! include! improved! osteogenic! differentiation! from! human!
Introduction' ! 49! bone! marrow! stromal! cells! (BMSCs)! [149],! as! well! as! increased! ALP,! mineralization! and! osteogenic! gene! upregulation! in! osteoblast-like! cells! [150,160,161].!In!this!regard,!it!has!been!shown!that!grooved!patterns!can!guide! stem!cell!differentiation,!depending!on!the!particular!geometry!of!the!grooves! [162].! ! In)vivo,)micro-grooves! can! also! improve! implant! performance.! For! instance,! it! has!been!shown!that!laser-ablated!microgrooves!on!the!implant!collar!can!affect! epithelial,! fibroblastic! and! osteoblastic! migratory! patterns,! influencing! the! orientation!of!the!connective!tissue!fibers!respect!the!implant!surface![163].!The! correct!orientation!of!such!fibers!hinders!the!apical!migration!of!the!junctional! epithelium,!avoiding!crestal!bone!loss.!Laser!patterned!implant!collars!can!limit! the! epithelial! downgrowth,! improve! soft! and! bone! tissue! attachment,! and! influence!bone!remodeling!so!that!improved!bone!quality!is!found!adjacent!to! the!implant![164].! ! ! Figure! 26) Cells) growing) inside) a) laser-patterned) groove) on) Y-TZP.) Cell) body) extensions)can)be)observed)toward)the)micro-grooved)walls)[160].) !
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 50! 1.4.2 Chemical!modifications!-!coatings! 1.4.2.1 Biofunctional+coatings:+an+overview+ ! The!surface!of!biomaterials!can!be!chemically!modified!in!order!to!add!certain! biological!properties.!One!possibility!is!to!alter!the! chemical! properties! of! the! surface! itself.! For! example,! surfaces! can! be!treated! with! UV! light! in! order! to! enhance!their!wettability![165].!However,!these!strategies!depend!largely!on!the! material!employed!(i.e.!expected!performance!cannot!be!directly!extrapolated!to! different!materials)!and!offer!a!relatively!narrow!range!of!possibilities.!Another! option!consists!on!surface!coatings![166,167],!which!can!be!designed!to!present! specific!biological!cues!and!are!easier!to!apply!to!different!substrate!materials.! Coatings!can! be!grouped!into! inorganic!or!organic,! depending!on!the! material! from!which!they!are!produced.!Some!of!the!possibilities!offered!by!this!strategy! are!detailed!below.! ! Inorganic)coatings) ) The!most!common!inorganic!coatings!in!bone!tissue!engineering!are!based!on! ceramic! inorganic! materials,! including! calcium) phosphates) (CaP)![168]!and! bioactive)glasses![169].!While!CaP!cements!are!a!family!of!materials!with!similar! composition!to!bone!and!teeth,!bioactive!glasses!are!based!on!mixtures!of!the! oxides!SiO2–CaO–MgO–Na2O–K2O–P2O5.!These!coatings!promote!the!deposition! of!a!thin!layer!of!biological!apatite!on!the!surface,!which!facilitates!the!adhesion! and!differentiation!of!host!cells.!They!present!a!very!good!osteoconduction!and! can!even!promote!osteogenesis![170,171].!Coatings!can!be!produced!by!several! techniques!(e.g.!plasma!spraying!or!electrodeposition![168,169])!and!have!been! mainly! applied! to! titanium! substrates! but! can! also! be! employed! on! zirconia! [172,173].!However,!the!control!of!composition!and!structure!of!the!produced! apatite!is!complex!and!the!mechanical!properties!of!thick!coatings!may!present!a! poor!performance![174,175].!An!alternative!to!such!coatings!is!the!deposition!of! apatite!through!a!biomimetic!process.!In!this!method!a!bone-like!apatite!layer!is! formed!on!the!surface!of!a!material!after!immersion!in!a!simulated!body!fluid!
Introduction' ! 51! (SBF),! as! shown! in!Figure' 27.! The! deposited! layer! consists! on! amorphous! or! poorly! crystalline! ion-substituted! calcium! orthophosphates.! The! method! proposed! by! Kokubo! and! coworkers! [176,177],! which! entails! a! previous! thermochemical!treatment,!is!a!good!example!of!this!approach!and!can!be!used! on!zirconia![178]!as!well!as!on!various!metals,!including!titanium.! ! ! Figure!27)SEM)micrographs)of)the)surfaces)of)10Ce-TZP/Al2O3)composites)which) were)either)a))untreated)or)b))treated)with)5M)H3PO4),)and)subsequently)immersed) in) SBF) for) 7) days.) The) surface) treated) with) H3PO4)is) fully) covered) by) a) layer) of) nucleated)apatite)[178].)) ! Organic)coatings) ) These! coatings! are! based! on! the! immobilization! of! polymers! on! the! surface,! either!from!a!synthetic!or!a!natural!origin.!They!are!highly!versatile!as,!to!some! extent,!can!be!tuned!to!modify!their!properties!in!terms!of!density,!morphology,! thickness,!hydrophobicity,!degradability,!etc.!They!may!be!aimed!at!mimicking! the!extracellular!environment!(i.e.!the!ECM),!trigger!specific!cell!functions,!act!as! drug! delivery! systems,! etc.! They! can! be! classified! into! synthetic!and! natural) coatings,)as!schematized!in!Figure'28.)
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 52! ! Figure! 28) Classification) of) organic) coatings) according) to) the) origin) of) the) polymers)employed.) ! Synthetic' coatings! are! produced! from! human-made,! artificially! synthesized! polymers.!They!can!be!degradable!or!non-degradable!and!are!mainly!employed! to! alter! some! chemical! properties,! such! as! the! hydrophilic/hydrophobic! behavior,!or!act!as!drug!delivery!systems.!They!are!highly!tunable,!their!physical! properties!can!be!modified!depending!on!the!specific!application,!and!present! low! immunogenicity! risks.! However,! their! ability! to! deliver! specific! biological! cues! is! limited.! Degradable! polymers! are! usually! employed! as! drug-delivery! agents! and! include! poly(D,L-lactic-co-glycolic! acid)! (PLGA)! [179]!or! polycaprolactone! (PCL)! [180].! Non-degradable! polymers! include! poly(vinyl! alcohol)!(PVA),!polymethacrylic!acid!(PMA)![181],!or!polyethylene!glycol!(PEG)! [182].!! ! In!contrast!to!synthetic!coatings,!natural'coatings!are!produced!from!molecules! derived!from!living!organisms.!They!can!be!sourced!from!a!natural!origin!or!be! produced! synthetically,! inspired! by! nature.!They! can! provide! cell-specific! interactions! and! are! highly! biocompatible! and! non-toxic.! However,! their! synthesis!is!often!more!complex!and!when!sourced!from!natural!origins,!both! their! composition! and! conformation! cannot! be! entirely! controlled.! Natural! coatings! include! a! wide! range! of! molecules! including! polysaccharides! (e.g.! glycosaminoglycans! (GAGs),! chitosan,! alginate,! pectin! etc.),! proteins! derived! from! the! ECM!(e.g.! collagen! type! I,! fibronectin,! vitronectin,!etc.)! and! peptides.!
Introduction' ! 53! While!polysaccharides!do!not!generally!possess!cell!specific!properties,!they!can! provide!biocompatible!and!stable!structures!to!support!other!molecules,!or!favor! protein!adsorption!and!interaction!with!ECM!molecules![183–186].!On!the!other! side,! ECM-derived! proteins! can! present! specific! sites! with! biologic! activity,! including!the!presence!of!cell!binding!motives! or! the! ability! to! entrap! growth! factors![62,187].!ECM!proteins!are!complex!molecules!that!can!possess!multiple! functions,!interact!with!other!proteins!and!present!unmasked!functions!that!can! be!activated!in!the!right!moment!by!the!right!biological!environment![188].!In! the! last! decades,! recombinant! DNA! technologies! offer! also! the! possibility! to! produce! chimeric! proteins! that! gather! multiple! biological! functions! [189].! However,!there!is!a!concern!with!the!disease!transmission!and!immunogenicity! problems!derived!from!the!use!of!such!proteins,!as!they!are!either!derived!from!a! natural!source!or!produced!by!recombinant!technologies!in!organisms!such!as! bacteria! or! yeast! [190].! In! addition,! the! relatively! large! size! of! proteins! may! entail! stability! issues! in! varying! conditions! of! pH! and! temperature.! Another! approach! that! circumvents! such! problems! consists! on! the! use! of! synthetic! peptides,! short! sequences! of! amino! acids.! They! can! be! derived! from! natural! sources!(e.g.!ECM,!soluble!factors,!etc.)!or!engineered!for!specific!purposes,!and! can! be! easily! synthesized! by! liquid! or! solid-phase! chemistry.! Peptides! can! present!very!different!biological!properties![191–193]!and!due!to!their!smaller! size! are! more! stable! than! proteins! and! can! be! grafted! at! high! surface! concentrations.!In!addition,!multifunctional!coatings!can!be!obtained!if!different! peptides!are!combined![194–196].! ! The! use! of! organic! coatings! on! zirconia! has! been! scarcely! investigated.! The! available!studies!include!the!use!of!polydopamine!coatings![197,198],!as!well!as! surface!functionalization!with!proteins!and!peptides.!In!this!regard,!there!is!one! study!involving!the!functionalization!with!the!insulin-like!growth!factor!1!(IGF- 1)![199]!and!some!additional!works!regarding!the!feasibility!of!the!RGD!peptidic! functionalization![200–202].!Such!studies!are!mainly!focused!on!improving!the! cell!adhesive!properties!of!the!zirconia!surfaces.! !
! Chapter!2! Aim!and! structure!of!the! thesis
Aim'and'structure'of'the'thesis' ! 63! 2!Aim!and!structure!of!the!thesis! 2.1 Aim!of!the!thesis! ! Since! the! first! dental! implants! developed! by!Brånemark! [222],! titanium! has! become!the!“gold!standard“!in!oral!implantology.!Over!time,!the!original!designs! as! well! as! the! surface! properties! have! been!extensively! modified! in! order! to! accelerate!healing!time![223].!Roughened!surfaces!and!hydroxyapatite!coatings! were! introduced! in! the! 1980’s.! In! this! sense,! roughened! implants! have! been! obtained!by!employing!techniques!such!as!sandblasting,!chemical!etching,!laser! structuring!and/or!anodic!oxidation.!On!the!other!hand,!inorganic!coatings!have! also!been!explored,!including!the!well-known!hydroxyapatite,!and!others!such!as! carbon,!bioactive!glass,!titanium!dioxide!films!and!fluoride!surface!treatments.! More!recently,!the!release!of!drugs!(e.g.!bisphosphonates!and!statins),!antibiotics! (e.g.! tetracycline)! and! growth! factors! (e.g.! bone! morphogenetic! proteins! and! transforming! growth! factor! β1)! have! been! introduced,! as! well! as! the! study! of! organic!coatings!including!synthetic!peptides!and!recombinant!proteins.!! ! In! contrast! to! the! long! and! successful! history! of! titanium,! zirconia-based! ceramics! began! their! journey! in! prosthetic! dentistry! in! the! early! 2000’s,! after! suffering!an!unexpected!setback!in!the!hip!replacement!field.!The!technological! challenges!to!surface!modify!a!hard!ceramic!coupled!with!the!critical!changes!in! the! LTD! behavior,! further! slowed! the! introduction! of! these! materials! in! the! biomedical!field.!Nowadays,!zirconia!is!the!preferred!choice!to!produce!several! dental!parts,!but!its!application!as!an!implant!is!still!reduced.!Yet,!some!of!the! improvements! performed! on! titanium! implants! have! also! been! employed! in! zirconia!including!grinding,!sandblasting,!chemical!etching,!laser!patterning!and! hydroxyapatite!coatings.! ! In!this!context,!the!present!Ph.D.!Thesis!will!investigate!topography-modifying! treatments! in! 3Y-TZP! able! to! improve! the! implant-tissue! integration.! The! induced!surface! damage,! phase! transformation! and! changes! in! LTD! resistance! will! be! evaluated,! as! well! as! its! biological! effects! on! cell! cultures.! The! most! promising! surface! treatment! will! be! further! functionalized! with! a! peptidic!
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 64! platform!to!enhance!its!osteogenic!and!cell!adhesive!properties.!Thus,!the!main! goal!of!this!Ph.D.!Thesis!is!to!combine!two!surface!treatments!on!3Y-TZP!able!to! improve! its! tissue! integration! potential,! one! of! physical! and! one! of! chemical! nature.!Throughout!this!Ph.D.!Thesis!it!will!be!shown!that,!similarly!to!titanium,! zirconia–based! ceramics! can! be! surface-modified! with! advanced! and! highly! tunable! methods,! avoiding! extensive! surface! damage! or! LTD! worsening,! and! importantly,!with!industrial!applicability.! ! Two! surface! treatments! were! chosen:! grinding/polishing! and! laser! micropatterning.!Both!of!them!can!increase!the!average!roughness!(Ra)!at!the!micro-! and!sub-micrometric!length!scale!as!well!as!introduce!directional!features!that! can! guide! cell! growth.! However,! the! surface! modifications! are! achieved! by! different!principles,!entirely!mechanically!in!the!case!of!grinding/polishing!and! thermally! in! the! case! of! laser! micro-patterning.! Hence,! differently! affected! microstructures!(i.e.!grain!refinement,!micro-cracks,!phase!transformation,!etc.)! and!surface!damage!are!expected.!Both!present!their!advantages!and!drawbacks.! While! grinding/polishing!is! faster! and! cheaper,! laser! micro-patterning! can! produce!more!reproducible!and!homogeneous!structures.!As!described!before,! the! one! displaying! the! best! outcome! will! be! further! functionalized! with! an! osteogenic!and!cell!adhesive!peptidic!platform,!including!the!RGD! and!DWIVA! sequences.! ! ! ! ! ! ! ! ! ! ! !
Aim'and'structure'of'the'thesis' ! 65! 2.2 Structure!of!the!thesis! ! The!content!of!this!Ph.D.!Thesis!is!presented!as!a!compendium!of!publications:! ! - In! Paper) I) the! changes! on! the! surface! and! the! subsurface! after! grinding/polishing!3Y-TZP!will!be!evaluated.!In!particular,!topographical! changes,! the! presence! of! surface! damage,! changes! in! microstructure,! phase! transformation! and! residual! stresses! will! be! discussed.! For! this! purpose,! different! treatments! in! terms! of! grinding! severity! and! directionality!will!be!compared.!Results!are!published!in!“J.!Minguela,!S.! Slawik,! F.! Mücklich,! M.P.! Ginebra,! L.! Llanes,! C.! Mas-Moruno,! J.J.! Roa,! Evolution) of) microstructure) and) residual) stresses) in) gradually) ground/polished)3Y-TZP,!J.!Eur.!Ceram.!Soc.!40!(2020)!1582–1591”.! ! - In!Paper)II)the!influence!of!grinding/polishing)on!mechanical!properties,! LTD! resistance! and! cell! behavior! will! be! analyzed.! The! properties! observed!will!be!explained!on!the!basis!of!the!surface!changes!reported!in! Paper)I.!Results!are!published!in!“J.!Minguela,!M.P.!Ginebra,!L.!Llanes,!C.! Mas-Moruno,! J.J.! Roa,! Influence) of) grinding/polishing) on) the) mechanical,) phase)stability)and)cell)adhesion)properties)of)yttria-stabilized)zirconia,!J.! Eur.!Ceram.!Soc.!40!(2020)!4304–4314”.! ! - In! Paper) III!3Y-TZP! will! be! micro-patterned! with! a! femtosecond! laser.! Surface!damage,!microstructure,!phase!transformation,!residual!stresses! and! LTD! resistance! will! be! analyzed.! The! surface! will! also! be! functionalized!with!a!dual!RGD/DWIVA!peptidic!platform.!The!rationale! for! selecting! laser! patterning! over! grinding! for! functionalization! is! detailed!in!Annex)A.!The!effects!on! cell!behavior!derived! from!both!the! topography!and!the!biomolecule!will!be!discussed.!Results!are!published! in!“J.!Minguela,!D.W.!Müller,!F.!Mücklich,!L.!Llanes,!M.P.!Ginebra,!J.J.!Roa,!C.! Mas-Moruno,! Peptidic) biofunctionalization) of) laser) patterned) dental) zirconia:) a) biochemical-topographical) approach,! Mat.! Sci.! Eng.! C! 125! (2021)!112096”.!
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 66! ! - In!Annex)A)the!rationale!and!the!experimental!procedure!for!selecting!an! optimal!topography-modification!technique!will!de!detailed.!A!technique! is! selected! between! grinding! and! laser! micro-patterning,! to! be! further! functionalized!with!the!biomolecule!in!Paper)III.!! !
! Chapter!3! Summary!of!the! main!results!
Summary'of'the'main'results' ! 69! 3!Summary!of!the!main!results! 3.1 Effects!of!the!topographical!modification!techniques! ! Two! main! surface! treatments! able! to! modify! topography! at! different! length! scales!were!studied:!grinding/polishing!and!laser-patterning.! ! Grinding/polishing' ! In!Papers)I!and!II!the!main!subsurface!changes!after!grinding/polishing! were! characterized! by! means! of! advanced! characterization! techniques! (i.e.! field! emission! scanning! electron! microscopy;! focused! ion! beam;! confocal! micro-Raman! spectroscopy,! etc.).! The! surface! properties! were! also!investigated!and!correlated!to!the!observed!subsurface!changes.!For! this! purpose,! gradually! ground/polished! specimens! were! produced,! yielding!four!different!topographies!of!increasing!roughness!(grades!1–4)! and!two!different!textures!(unidirectionally,!U,!and!multidirectionally,!M).! ! Regarding! Paper)I,! it! was! found! that! several! changes! take! place! on! the! subsurface! after! grinding/polishing,! which! are! correlated! with! the! severity!of!the!abrasion.!A!layer!of!recrystallized!nano-grains!was!found! on!the!ground!surfaces.!The!thickness!of!this!layer!increased!in!agreement! with!the!abrasion!severity!employed.!Even!in!mildly!polished!specimens! (1-M/U),! a! partially! recrystallized! layer! could! be! observed.! The! t) →) m! stress-induced!phase!transformation!took!place,!following!the!same!trend! as! displayed! by! surface! recrystallization.! As! expected,! due! to! the! expansive!nature!of!the!t)→)m)phase!transformation,!a!layer!of!residual! compressive! stresses! could! be! detected,! reaching! 1.4! GPa! in! the! most! severely!ground!surfaces.!Simple!mathematical!equations!relating!surface! average! roughness! (Sa),! monoclinic! volume! fraction! (Vm)! and! residual! surface!stresses!could!be!obtained.!Although!the!observed!changes!after! grinding/polishing! can! be! beneficial! for! the! mechanical! properties! and! the! LTD! resistance! of! the! surface,! damage! in! the! form! of! flakes! was! observed!in!the!most!severely!abraded!specimens!(4-M/U),!associated!to!
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 76! As! for! the! peptidic! platform,! improved! cell! attachment,! well-developed! cytoskeletons!and!larger!cell!area!were!observed,!but!no!effects!regarding!cell! migration!were!detected.!! ! Although!some!osteogenic!potential!was!found!in!10L!specimens!(i.e.!the!ones! grooved!with!a!periodicity!of!10!μm),!the!largest!effects!were!observed!from!the! biomolecule,!which!favored!upregulation!of!several!genes!related!to!osteoblastic! differentiation!in!all!the!surfaces.! ! Hence,! the! combination! of! topographical! features! and! the! peptidic! platform! provided!a!powerful!tool!to!tune!and!enhance!cellular!responses,!which!indicate! potential! to! improve! tissue! integration.! As! schematized! in! Figure' 34,! while! topographical! features! could! guide! cellular! growth,! the! biomolecule! improved! cell!attachment!and!osteogenic!properties.! !
Summary'of'the'main'results' ! 77! ! Figure! 34)Scheme)of)the)main)results)obtained)from)the)characterization)of)cell) response)on)laser)treated)and)functionalized)specimens.)CTRL)samples)correspond) to)mirror-like)polished)specimens)employed)as)a)flat)topography)reference.)
! Chapter!4! Paper!I! ! Evolution!of!microstructure!and!residual! stresses! in! gradually! ground/polished! 3Y-TZP! ! Available'at:' https://www.sciencedirect.com/science/article/abs/pii/S 0955221919307289'
! ! Contents lists available at ScienceDirect Journal of the European Ceramic Society journal homepage: www.elsevier.com/locate/jeurceramsoc Original Article Evolution of microstructure and residual stresses in gradually ground/ polished 3Y-TZP J. Minguela a,b,c , S. Slawik d , F. Mücklich d , M.P. Ginebra a,c,e , L. Llanes b,c , C. Mas-Moruno a,c, *, J.J. Roa b,c, * a Biomaterials, Biomechanics and Tissue Engineering Group (BBT), Department of Materials Science and Metallurgical Engineering, Universitat Politècnica de Catalunya, 08019 Barcelona, Spain b Center for Structural Integrity, Reliability and Micromechanics of Materials (CIEFMA), Department of Materials Science and Metallurgical Engineering, Universitat Politècnica de Catalunya, 08019 Barcelona, Spain c Barcelona Research Center in Multiscale Science and Engineering, Universitat Politècnica de Catalunya, 08019 Barcelona, Spain d Functional Materials, Department of Materials Science and Engineering, Saarland University, 66123 Saarbruecken, Germany e Institute for Bioengineering of Catalonia (IBEC), Barcelona Institute of Technology (BIST), 08028 Barcelona, Spain ARTICLE INFO Keywords: Zirconia Grinding Microstructure Phase transformation Residual stresses ABSTRACT A comprehensive study of progressively ground/polished 3Y-TZP was performed with the aim of better understanding the mechanisms driving the microstructural modifications observed after such procedures, and identifying the processing parameters leading to optimal microstructures (i.e. ageing-protective and damagefree). Gradually ground/polished surfaces were produced, yielding four different topographies of increasing roughness (grades 1–4) and two different textures (unidirectionally, U, and multidirectionally, M). Phase transformation, microstructure and residual stresses were investigated by means of advanced characterization techniques. It was found that low-roughness mildly ground/polished specimens (i.e. 2-M/U) presented a nanometric layer with the ageing-related protective features generally associated with coarsely ground specimens. A lower limit for grain refinement in terms of surface abrasion was also found, in which partial recrystallization took place (i.e. 1-M/U). A mathematical relation was established between average surface roughness (S a ), monoclinic volume fraction (V m ) and surface compressive residual stresses, demonstrating that if the processing parameters are controlled, both V m and residual stresses can be predicted by the measurement of S a . 1. Introduction Polycrystalline tetragonal zirconia doped with 3 mol.% yttria (usually referred to as either 3Y-TZP or 3Y-ZrO 2 ) has been widely used as a structural ceramic due to its outstanding mechanical properties [1]. For instance, in the case of prosthodontics, several components are produced using zirconia-based materials such as implants, abutments, crowns, bridges and endodontic posts and cores [2–4]. During the manufacture process, several shaping and surface finishing steps are commonly involved, including computer-aided design/computer-aided manufacturing (CAD/CAM) machining, drilling, cutting, grinding or polishing. All of them are known to introduce surface defects as well as microstructural and crystallographic changes [5–8]. Grinding processes are routinely used as finishing steps; and thus, microstructural changes after such surface treatments have been studied in detail. In this regard, a close inspection of ground specimens by Muñoz-Tabares et al. [5] revealed three different microstructural layers just below the surface: 1) a first zone of recrystallized nano-grains in the range of 10–20 nm; 2) a plastically deformed zone; and 3) a layer where abundant stress-induced tetragonal (t) to monoclinic (m) transformation (t→m) took place, generating residual compressive stresses. As a result of its ability to generate such changes, grinding has attracted researchers interest as a means of modifying surface properties. Both mechanical behaviour [9,10] and ageing resistance [11,12] can be modified through the introduction of compressive stresses (as well as detrimental cracks and flaws), but also in response to the presence of nano-grains and the reduction in domain size by ferroelastic switching [7,13,14]. In particular, the addition of a thin layer of residual compressive stresses can improve mechanical properties and is able to stabilize the t-phase, hindering the nucleation and propagation of the m-phase in the so-called hydrothermal degradation process [15], also known as ageing or low-temperature degradation [16]. In this aspect, https://doi.org/10.1016/j.jeurceramsoc.2019.10.057 Received 30 July 2019; Received in revised form 21 October 2019; Accepted 29 October 2019 ⁎ Corresponding authors at: Barcelona Research Center in Multiscale Science and Engineering, Universitat Politècnica de Catalunya, 08019 Barcelona, Spain. E-mail addresses: [email protected] (C. Mas-Moruno), [email protected] (J.J. Roa). -RXUQDORIWKH(XURSHDQ&HUDPLF6RFLHW\² $YDLODEOHRQOLQH1RYHPEHU (OVHYLHU/WG$OOULJKWVUHVHUYHG 7
! ! the presence of a nanograined layer on the surface has also proven to be beneficial, displaying a protective effect due to the reduced grain size [17,18]. As a consequence of the intense changes introduced after severe grinding, most of the published data are related to the effects produced by this harsh condition. However, microstructural effects obtained using softer procedures are commonly neglected; and thus, structural information of intermediate surface states is lost. Hence, a comprehensive study including milder polishing/ grinding procedures would be of relevance, because i) the characterization of intermediate stages can expand the current knowledge about the mechanisms driving microstructural modifications, and ii) the screening of different and progressive surface states can serve to identify and optimize the processing parameters leading to the best microstructured surfaces (i.e. in terms of ageing resistance and surface damage). Within this context, in the present work a comprehensive characterization study was carried out, including surface conditions that range from mirror-like polished to coarsely ground. Special emphasis was put on intermediate conditions, with the main goal of studying the changes and evolution from a free of defects bulk-like material into a severely affected surface, in terms of microstructure, phase transformation and residual stresses. 2. Experimental procedure 2.1. Specimen preparation Specimens were produced from zirconia powders stabilized with 3 mol.% yttria (TZ-3YSB-E, Tosoh, Japan). The powders were shaped by uniaxial pressing at 50 MPa, followed by cold isostatic pressing at 288 MPa. The green bodies were then sintered in air at 1450 °C for two hours with heating and cooling rates of 3 °C/min (LHT 02/17, Nabertherm). By this method, 15 mm diameter disc-shaped specimens were obtained. In order to characterize the starting material, specimens were mirror-like polished and grain size, density, hardness and indentation fracture toughness were measured. Grain size was evaluated by thermally etching the samples, and subsequent examination of them by Field Emission Scanning Electron Microscopy (FESEM, Carl Zeiss Neon 40). Five images per sample in three different specimens were taken in order to have statistical significance and the linear interception method was used. Density was characterized by the Archimedes method in distilled water. Finally, hardness was obtained from 1 kgf Vickers indentations and fracture toughness was calculated with the method proposed by Niihara et al. [19] using 30 kgf indentations. Four indentations per specimen in three different specimens were used for both measurements. The properties of the starting material are summarized in Table 1. 2.2. Superficial modification: grinding/polishing treatments Different surface finish conditions were obtained by polishing the samples in a Buehler Ecomet4 automatic polishing machine, coupled with an Automet2 power head. Four different roughness grades and two different patterns were produced: multidirectional (M) and unidirectional (U) grooves. Besides, one mirror-like polished specimen (MP) was used as a reference. Table 2 shows the codes for the different specimens tested as well as the different parameters employed to superficially modify each sample. 2.3. Surface characterization Surface roughness of the obtained topographies was measured by white light interferometry (WLI, Veeco Wyko 9300 N T). FESEM was employed in order to observe general appearance, topographical features and surface damage right after treatment. Aiming to get detailed information of the sub-surface, cross-sections were prepared by means of Focused Ion Beam (FIB, Carl Zeiss Neon 40) using a Ga + source. Prior to FIB milling, a protective thin platinum layer was deposited on the region of interest. Current as well as acceleration voltage were continuously decreased down to a final polishing stage at 500 pA and 30 kV. Crystalline phases were determined by X-Ray Diffraction (XRD) and confocal micro-Raman Spectroscopy. XRD (D8-Advance, Bruker) was carried on both Bragg-Brentano symmetric geometry configuration (k α- 1 Johansson Typ monochromator in the primary side, parallel plate collimator with a LynxEye detector in the secondary side) and grazing incidence angle at ω= 1° (Goebel mirror in the primary side, parallel plate collimator with scintillation detector in the secondary side). The analysis was performed from 26°≤2θ≤37° on a diffractometer using Cu K α radiation (40 kV and 40 mA) with 0.02° step size and 1 s/step. For Bragg-Brentano symmetric configuration the penetration depth of the incident X-rays (i.e. the thickness of the sample, where 90% of the information recorded in a diffractogram is gathered) at 2θ= 30° is around 5 μm according to the Lambert-Beer’s law, while on the grazing incidence angle experiment it is reduced to around 300 nm. The volume fraction of the monoclinic phase (V m ) was calculated with the equation proposed by Toraya et al. [20], as follows: =+ ++ V II II I 1.311[ (1 ¯11) (111)] 1.311[ (1 ¯11) (111)] (101) mmm mm t (1) where I m and I t correspond to the intensities of the monoclinic and tetragonal peaks, respectively. In-depth m-phase distribution was characterized with confocal micro-Raman spectroscopy (inVia Qontor, Renishaw) with a Nd:YAG laser (wavelength 532 nm, integration time 0.1 s). Phase maps under the surface were obtained. To do that the discs were cut in half, as depicted in Fig. 7e, and the cross-sections were mirror-like polished. Volume fraction of m-phase was quantified by using the equation proposed by Katagiri et al. [21]: =+ ++ V II III2.2 mmm tmm 181 190 147 181 190 (2) where I m and I t correspond to the integrated intensities of the monoclinic and tetragonal bands, respectively. Numbers indicate Raman shift in cm −1 . In order to reveal the microstructure and be able to study the surface recrystallization effect, some specimens were thermally etched (1100 °C for 1 h, with heating and cooling rates of 12 °C/min) and subsequently observed by FESEM. Surface residual stresses were calculated with the sin 2 ψmethod by XRD analysis (Empyrean, PANalytical) using Cu K α radiation (40 kV and 40 mA). An X-ray lens with cross aperture (primary side) and parallel plate collimator with 0D proportional counter detector (secondary side) were employed. The tetragonal (101) t peak found at 2θ= 30.2° was used for the stress calculations, at Chi angles from -60° to +60° in 13 steps. The use of a peak at low 2θwas necessary to obtain an X-Ray penetration depth similar to the thickness of the stressed layer. The loss of sensitivity at small 2θangles was reduced by using parallel plate collimators on the secondary side [22]. As the stress measurements performed in the (101) t may be influenced by surrounding peaks, such as the (111) r , some of the spectra were deconvoluted with the PANalytical HighScore Plus software, in order to Table 1 Summary of the main microstructural and mechanical properties of the starting 3Y-TZP material. Grain size (μm) 0.32 ± 0.12 Density (g·cm −3 ) 6.08 ± 0.01 Hardness (GPa) 13.46 ± 0.34 Indentation fracture toughness (MPa·√m) 5.09 ± 0.02 J. Minguela, et al. -RXUQDORIWKH(XURSHDQ&HUDPLF6RFLHW\²
! ! ' obtain more accurate values. Given the high amount of recorded spectra, this methodology was only performed in selected samples. In order to characterize the anisotropy of the stress state, measurements were done along three different directions on the surface (Φ= 0°, 45° and 90°). For samples with unidirectional scratches, Φ= 0° and Φ= 90° correspond to a direction parallel and perpendicular to the grooves, respectively. For samples with multidirectional grooves, the angles were chosen arbitrarily. Stress analysis was performed by using the PANalytical X’Pert Stress plus software. The X-ray elastic constants (XECs) used for such calculations were S 1 = -1.58 TPa −1 and S 1 2 2 = 6.50 TPa −1 [23]. A piezo-spectroscopic technique was also employed in order to obtain cross-sectional macro-stress maps of the t-phase. This technique has already been used by other authors for the assessment of stresses in zirconia-based materials [24–26]. Stresses can change the frequency of vibrational modes and induce shifts in Raman bands. These Raman shifts can be related to hydrostatic stress through the following equation: =⟨⟩ω ∆ 3Πσ tt (3) where ω∆ is the Raman band shift in − cm 1 , ⟨ ⟩σtis the average hydrostatic stress in the tetragonal phase in GPa and Π t is the uniaxial piezospectroscopic coefficient for the chosen tetragonal band in − cm / GP a 1 . In order to know the piezo-spectroscopic coefficient, a calibration process is necessary. In this work, piezo-spectroscopic coefficients determined by Pezzotti and Porporati in 3Y-TZP have been used [25] for the tband found around 146 − cm 1 . Raman band positions were obtained by fitting the data to Gaussian curves with commercially available software (WiRE 4.4, Renishaw). Residual stresses were calculated from the spectroscopic data obtained in cross-sections. 3. Results and discussion The overlapping of individual abrasions during grinding/polishing procedures, progressively eroded the surface resulting in a characteristic grooved topography. Fig. 1 shows the FESEM micrographs of the studied surfaces after grinding/polishing. The average surface roughness (S a ) obtained by WLI is summarized at the top and the bottom of the micrographs for the M and U specimens, respectively. A clear linear pattern is observed in all the images. By choosing the adequate abrasive and polishing dynamics, the obtained topographical features were finely tailored, including different surface roughness and patterning texture. While M conditions presented multidirectionally oriented scratches, U conditions were constituted by almost parallel grooves. From 1 to 4, an increase in roughness with deeper valleys and higher peaks was noticed, in accordance with the use of rougher abrasive particles. Likewise, for the roughest condition, more evident and extended signs of damage were present. For conditions 1 to 3, the lack of visible surface cracks, smooth and homogeneous tracks without chipping, and the presence of serrated and irregular edges, which indicated that extruded material at the sides of the grooves (ploughing) had been detached, pointed out to ductile material removal mechanisms. At sufficiently low cutting depths, plastic flow is more energetically favourable than brittle fracture, and is the responsible for material removal even in intrinsically fragile materials [27]. Hence, a surface free of defects from brittle fracture events was obtained. Despite brittle regime was not reached in any of the studied specimens, in the case of the rougher structures (i.e. 4-M/U) additional damage mechanisms (e.g. flaking, material detachment and micro-cracks) were activated, as depicted in Fig. 2. On such specimens, due to the higher friction between the abrading particles and the surface, extensive damage in the form of micro-cracking was observed along some of the grooves. Fig. 2 presents a magnified FESEM micrograph showing this kind of surface defects, related to ductile flaking [28]. This created a track of aligned semicircular flakes, such as the ones observed in Fig. 2a. Material detachment also occurred in some of the most damaged grooves, revealing the sub-surface grainy microstructure (Fig. 2b, zones marked as A, B, C and D). The effects of abrasion in such procedures are not only limited to topographical modifications and surface damage, but are also able to introduce crystalline phase transformations, lattice distortions and texture [5]. As shown in Fig. 3a, where the results of XRD experiments in Bragg-Brentano symmetric geometry are displayed, several crystallographic changes were identified after modifying the surface. While MP and 1-M spectra overlapped almost entirely, 2-M, 3-M and 4-M presented important alterations, progressively intensified with the severity of the applied abrasion. As the diamond particles erode the material, the accompanying shearing and tensile stresses in the subsurface destabilize the metastable tphase, which undergoes a martensitic transformation into mone [29]. Accordingly, the most evident change in spectra after grinding was the increase in the content of mphase at the surface, as shown in Figs. 3b and d, which increased almost linearly to a maximum of V m = 7% in 4-M. Furthermore, in the left side of the (101) t a tail was observed, increasing in intensity from 2-M to 4- M. This peak was first proposed to be associated with a rhombohedral phase (r-phase) [30], arising from the transformation of cubic grains (c →r) under high stresses, or from the transformation of the tetragonal phase (t→r), as suggested by other authors [31,32]. It has also been associated with lattice distortions produced after grinding [33]. One of the known mechanisms of zirconia to accommodate stresses Table 2 Summary of the codes and grinding/polishing parameters of the superficially modified specimens. J. Minguela, et al. -RXUQDORIWKH(XURSHDQ&HUDPLF6RFLHW\²
! ! 84! ' ' ' ' is the ferroelastic switching of domains [7,13]. Under high biaxial stresses such as the ones produced during grinding, the c-axis of the t phase reorients perpendicularly to the surface [5,34,35]. This domain reorientation promotes the onset of texture (i.e. a preferential crystallographic orientation), as revealed by the changes of the (002) t / (200) t intensity relation [7]. Figs. 3c and 3e display the relation between these two peaks, showing that similarly to the increase in m-phase, as the abrasion gets more severe, an increase in texture is noticed. Regarding surface directionality, M and U specimens showed no significant differences (results not shown) and hence just diffractograms for the M specimens are presented. The high strain introduced after surface mechanical treatments can produce changes in microstructure, which are able to affect material’s properties such as the hydrothermal degradation behaviour [17]. As shown in Fig. 4a, three distinctive microstructural regions were observed under the surface of 3Y-TZP after grinding (labelled as regions 1, 2 and 3), in a 4-M cross-sectioned specimen. These microstructural features are in agreement with previous studies [6,35] and are described in detail by Muñoz-Tabares et al. [5]. As reported in [5], in-situ recrystallization occurs in the first nanometres (in a layer of about 300 nm), where a refined microstructure is observed. Due to the high strain, progressive misorientation of dislocation cells lead to the formation of new nano-sized grains, in the range of 10–20 nm (region 1). Below (region 2), plastically deformed grains in a direction parallel to the surface are observed, followed by a third layer of bulk-like grains in which monoclinic laths are identified (region 3). Two monoclinic laths found in this region are shown in the inset of Fig. 4a. It should be noted that, in the present work, shallow micro-cracks extending parallel to the surface were observed in the first region, linked to the flakes observed in Fig. 2. The steep difference in properties between the nano-sized and the plastically deformed layer and the fact that flaking is intrinsically parallel to the surface, may avoid its propagation to deeper regions. Although microstructure after grinding and other procedures involving intense abrasion have been thoroughly studied [5,6,8,35,36] changes after mild procedures such as polishing are quite unknown. Fig. 4b shows the microstructure of 2-M specimens, polished with a 30 μm diamond slurry, as detailed in Table 2. Less intense microstructural modifications were present in this case, and just two defined zones were observed: a very shallow first layer of nano-sized grains, with a thickness smaller than 100 nm; and a second layer of bulk-like Fig. 1. FESEM micrographs of the different topographies obtained. Multidirectional (M) patterns are displayed in the first row, while unidirectional (U) patterns are presented in the second. From left to right, increasing levels of roughness, 1–4 (more information available in Table 2). On the top and bottom, average surface roughness (S a ) in nm is available for the M and U patterns, respectively. Fig. 2. Different modes of surface damage for the specimens 4-M/U. a) Flakes left by a particle sliding from left to right in 4-M. Dotted lines delimit the edge of the groove and b) damage in 4-U. The dotted square outlines an area with flaking. Labels A, B, C and D identify zones with material detachment. J. Minguela, et al. -RXUQDORIWKH(XURSHDQ&HUDPLF6RFLHW\²
! material where no deformed grains and no monoclinic twins were observed. As illustrated in Fig. 4c, a magnification of the first micron under the surface presented no signs of plastically deformed grains with a sudden transition between an extremely shallow refined layer and the bulk-like material. A nano-sized grain layer, as the ones observed in Fig. 4, can successfully protect zirconia-based materials from ageing [17]. Grinding has been used for such purpose [11], but for many applications surface roughness or micro-damage produced after these treatments may not be acceptable. The present results evidence that softer procedures, leading to lower levels of surface damage and roughness, may also introduce some of the protective features generally associated with coarsely ground zirconia. In order to have a better insight about grain refinement, M specimens were thermally etched. Thermal etching is carried out in polished surfaces and involves a mass transport away from grain boundaries, so that grooves develop and boundaries become visible [37]. Fig. 5 shows the surface microstructure after thermally etching the specimens at 1100 °C for 1 h. MP specimen presented a grain size distribution around 300 nm, in agreement with values reported by other authors working with similar conditions (Fig. 5a) [5,38]. Instead, 2-M, 3-M and 4-M (Figs. 5c, d and e), displayed a layer of recrystallized nano-grains covering the surface, in accordance with the presence of a superficial nano-sized grain layer (Fig. 4). As reported by other authors after high resolution TEM observations, the dynamically recrystallized grains present a size in the order of 20 nm [5], but grow during the annealing process depending on the chosen etching temperature [35]. In the case of 1-M (Fig. 5b), however, an intermediate behaviour was observed, with a combination of both bulk-like and nano-sized grains. As shown in the magnification of Fig. 5f, the surface presented a bimodal distribution with large grains in the order of 300–400 nm (left side of the micrograph) and small ones below 100 nm (right side of the micrograph). Accordingly, the surface of 1-M seemed to be in the limit of strain required for nano-structuring, with just some of the grains accumulating enough strain to fully recrystallize. The experiments carried out suggest that under the used conditions (i.e. load, speed, polishing equipment, etc.) a polishing procedure providing a surface roughness as low as S a = 16 ± 1 nm is able to initiate the recrystallization process, highlighting the extreme sensitivity of 3Y-TZP to be surface modified. As it has been shown by different techniques (e.g. XRD, FESEM and FIB/FESEM), important structural changes occurred on the very first nm of the surface upon grinding. Due to the reduced thickness of the affected layer, the evaluation of crystalline phases on an even smaller scale seems necessary. For such purpose, XRD in grazing incidence of 1° was performed in a superficial layer of around 300 nm. Results for M specimens are displayed in Fig. 6a. If compared to Fig. 3, MP and 1-M spectra were still similar to each other, although in this case both of them showed a slight hump on the left side of (101) t , a little amount of m-phase (Fig. 6b), as well as higher (002) t /(200) t ratio (Fig. 6c). For the rest of specimens, a significant increase in mphase and texture was appreciated. For these conditions, 2-M, 3-M and 4-M, (101) t was shifted around 0.5° to lower angles, giving way either to the (111) r , or to a peak produced by the distortion of the tetragonal lattice [33]. Content of m- Fig. 3. Results of the XRD experiments in Bragg-Brentano symmetric geometry, n = 3. a) XRD spectra of representative specimens, b) and c) magnifications of the (1 ¯11) m peak and the (002) t /(200) t tetragonal doublet, respectively. d) m-phase volume fraction. Dashed area corresponds to the detection limit of the technique, V m = 1%. e) (002) t /(200) t intensity relation. Fig. 4. Sub-superficial microstructure of a) 4-M and b) 2-M specimen. c) Magnification of a region in 2-M. Dashed lines in a) and b) delimit the different regions. Inset in a) identify two monoclinic laths (see white arrows). Note that a very shallow layer of nano-grains is discerned in c), without any sign of plastic deformation. J. Minguela, et al. -RXUQDORIWKH(XURSHDQ&HUDPLF6RFLHW\²
! ! Contents lists available at ScienceDirect Journal of the European Ceramic Society journal homepage: www.elsevier.com/locate/jeurceramsoc Original Article Influence of grinding/polishing on the mechanical, phase stability and cell adhesion properties of yttria-stabilized zirconia J. Minguela a,b,c , M.P. Ginebra a,c,d , L. Llanes b,c , C. Mas-Moruno a,c, *, J.J. Roa b,c, * a Biomaterials, Biomechanics and Tissue Engineering Group (BBT), Department of Materials Science and Engineering, Universitat Politècnica de Catalunya - BarcelonaTECH, 08019 Barcelona, Spain b Center for Structural Integrity, Micromechanics and Reliability of Materials (CIEFMA), Department of Materials Science and Engineering, Universitat Politècnica de Catalunya - BarcelonaTECH, 08019 Barcelona, Spain c Barcelona Research Center in Multiscale Science and Engineering, Universitat Politècnica de Catalunya - BarcelonaTECH, 08019 Barcelona, Spain d Institute for Bioengineering of Catalonia (IBEC), Barcelona Institute of Technology (BIST), 08028 Barcelona, Spain ARTICLE INFO Keywords: Zirconia Grinding Mechanical properties Hydrothermal degradation Cell adhesion ABSTRACT The changes in mechanical properties, hydrothermal degradation and cell adhesion were studied in 3Y-TZP under two different superficial modification patterns (uni- and multidirectional) with a surface roughness ranging from 16 to 603 nm. In this sense, mechanical properties (i.e. hardness, indentation fracture toughness and scratch) and accelerated tests in water steam were measured to evaluate the influence of the surface treatments on the superficially modified layer. Moreover, a detailed characterization through micro-Raman spectroscopy and X-Ray diffraction was performed. Finally, SaOS-2 osteoblasts were used for the evaluation of the cell adhesion behaviour on the surfaces. Overall, ground/polished specimens increased the mechanical properties and ageing resistance of mirror-like polished specimens, although resistance to degradation was maximum at intermediate conditions (S a ≈40−180 nm). The studied surfaces allowed cell attachment, but promoted contact guidance (i.e. cell alignment) only on unidirectionally ground surfaces above Sa = 150 nm. 1. Introduction Zirconia-based materials have gained increasing attention during the last years in restorative dentistry, and are now used to produce several prosthetic elements, such as crowns, bridges, endodontic posts and cores, abutments and dental implants [1,2]. Among the different zirconia compositions available, yttria-doped zirconia (Y-TZP) is still the most commonly used solution, although other compositions such as ceria-doped or zirconia-alumina composites are also employed in order to improve zirconia’s ageing resistance [1–5](alsoknownashydrothermaldegradation or low-temperature degradation [6]), at the expense of certain mechanical properties [7,8]. The superior properties of zirconia, which include high strength, toughness, hardness and wear resistance; and especially its whitish colour resembling natural teeth, have been decisive for the development of new advanced ceramic solutions in dentistry [9]. Due to the harsh environment of the oral cavity, dental materials present many challenges from the mechanical [10] and chemical [11] point of view. On the one hand, cyclic contact loads from chewing as well as sliding loads from food and teeth abrasion can introduce flaws on the surface, which may compromise the long-term reliability of the prosthesis. On the other hand, after long periods in contact with moisture, yttria-stabilized zirconia may be affected by hydrothermal degradation [12,13]. When kept for a long time in a humid environment, a martensitic phase transformation from the metastable tetragonal (t) phase to the monoclinic (m) one takes place spontaneously on the surface. This transformation is associated with an m-volume expansion of around 4 % that generates micro-cracks through which water can penetrate into the material and further degrade it until the final failure. However, many restorative elements (e.g. dental implants) should not only preserve its structural integrity for several years, but also display a proper biological interaction [14] both in the short and long term. In the particular case of dental implants, the surface plays a key role, interacting with bone and guiding the biological response towards a proper osseointegration and mechanical stability. Since it is indeed the surface that provides the features that will largely decide the success of an implant, the ability of modifying and fine-tuning its properties has been a subject of study. Extensive research has been carried out to investigate the changes in microstructure, https://doi.org/10.1016/j.jeurceramsoc.2020.03.049 Received 9 December 2019; Received in revised form 20 March 2020; Accepted 24 March 2020 ⁎ Corresponding authors at: Barcelona Research Center in Multiscale Science and Engineering, Universitat Politècnica de Catalunya - BarcelonaTECH, 08019 Barcelona, Spain. E-mail addresses: [email protected] (C. Mas-Moruno), [email protected] (J.J. Roa). -RXUQDORIWKH(XURSHDQ&HUDPLF6RFLHW\² $YDLODEOHRQOLQH$SULO (OVHYLHU/WG$OOULJKWVUHVHUYHG 7
! ! mechanical properties and/or hydrothermal degradation of Y-TZP materials after surface treatments such as sandblasting [15,16], grinding [17–19], chemical etching [20,21] or laser patterning [22,23]. As a surface-modifying technique, grinding/polishing is known to affect the properties of Y-TZP. Several changes are introduced on the surface and subsurface depending on the severity of the treatment such as increased roughness, microstructural modifications, residual stresses, cracks, etc. as detailed by Muñoz-Tabares et al. [17]. The consequences of such changes inevitably leave their imprint on the material’s properties, mainly in terms of mechanical and hydrothermal degradation behaviour. In the first case, the layer of residual compressive stresses originating from the expansive stress-induced t→mtransformation enhances the mechanical properties of the surface, as long as the introduced damage is controlled [15,17,24–27]Inthesecondcase,hydrothermaldegradationcanbedelayed by certain microstructural features associated with grinding procedures [18,28–30]suchasthereductioningrainsizeinthedynamically recrystallized surface [31], the t-phase stabilizing effect of the residual compressive layer [32,33], and the reduction in domain size by ferroelastic switching, as shown by Jue et al. [34]. On the other hand, the changes in surface topography introduced by such procedures may be used as a tool to improve biological response. In this regard, grinding as well as sandblasting and chemical etching have been used, mostly in titanium surfaces, as a means to improve osseointegration [35,36]. Both eukaryotic and prokaryotic cells can be affected by the topographical cues of the substrate in which they are adhered [37,38]. In particular, osseointegration of biomedical implants can be enhanced by increasing surface roughness, both in the macroscale because of a better bone-surface interlocking [39,40], and in the micro- and nanoscale because of the beneficial influence of roughness in osteoblasts activity [41–43], displaying higher levels of adhesion and extracellular matrix deposition [44]. Although the individual mechanisms able to affect surface properties after grinding are known, predicting the outcome of their combined effects after a specific treatment is still challenging. Most of the available studies are based on the comparison of a few grinding treatments, relying solely on the m-phase content to explain the observed differences, without providing a detailed characterization of the surface. As a result, different studies report contradictory outcomes from apparently similar treatments, as it is the unique combination in terms of microstructure, surface defects and residual stresses after each treatment what dictates the final properties of the material. Therefore, it is of paramount importance to study how increasingly severe treatments affect surface properties, and to relate such properties with the microstructural features of the surface. This will allow: i) to understand and rationalize differences found among conflicting studies, and ii) to gather the necessary knowledge in order to smartly design surface microstructure and obtain materials with the desired mechanical, ageing and cell instructive properties. For this reason, in the present work a series of gradually ground/polished 3Y-TZP surfaces were prepared. The chosen material resembled low-translucency 3Y-TZP, mainly employed in veneered restorations as well as dental implants and abutments. Mechanical properties, ageing resistance and cell adhesion performance were studied and related to the particular features of each surface [45]. Within this context, the hypotheses under examination are: - Grinding/polishing are able to modify surface properties. -Different abrasion degrees can lead to different surface properties. - The increase in surface properties is not necessarily in direct correlation with the abrasion severity employed. 2. Experimental procedure 2.1. Sample preparation Specimens were produced from zirconia powders stabilized with 3 mol% yttria (TZ-3YSB-E, Tosoh). Powders were cold isostatically pressed at 288 MPa and sintered at 1450 °C for 2 h, with constant heating and cooling rates of 3 °C/min. Disc-shaped specimens of 15 mm diameter and 2 mm thickness were obtained by this procedure. Grain size determined by the linear interception method was found to be 0.32 ± 0.12 μm and density was above 99 % of the theoretical one. 2.2. Grinding/Polishing treatments Specimens were gradually ground/polished (Ecomet4, Buehler) in order to obtain progressive levels of surface roughness and abrasion severity. Four different roughness grades (1–4) and two different directionalities were obtained: aligned (unidirectional, U) and random grooves (multidirectional, M). A mirror-like polished surface (labelled as MP) was also included in all the experiments as a reference. Further details about the procedure and the codes used to identify the specimens can be found in [45]. The main microstructural and crystallographic features, residual stresses and surface damage of the studied specimens are summarized in Table 1 [45]. 2.3. Surface characterization Roughness parameters were obtained by White Light Interferometry (WLI, Wyko 9300 N T, Veeco). Measurements were performed in regions of 150μm×150 μm by stitching four images taken at a magnification of 50×. Surface parameters were obtained with the Veeco’s Vision®software. Tilt was corrected and a filter was used in the flattest conditions in order to separate roughness from waviness. For this purpose, a Robust Gaussian short wavelength pass filter with a spatial cut-offat 0.01 mm was selected. A description of the roughness parameters studied in this work can be found in Refs. [46–48]. Wettability of the surfaces was determined by static contact angle (CA, OCA15 Plus, Dataphysics) with the sessile drop method [49]. Measurements were done at room temperature with ultrapure Milli-Q water (3 μL drop volume) and contact angle determined by Laplace- Young fitting with SCA 20®software (Dataphysics). For both WLI and CA, values shown are the mean of three different measurements in three different specimens. 2.4. Mechanical characterization In order to determine the Vickers hardness (HV) and indentation fracture toughness (K Ic ), four indentations per specimen in three different samples were made on the surfaces, at 10 kgf and 30 kgf. 10 kgf indentations were used for Vickers hardness calculations, while the cracks originated at the corners of 30 kgf indentations were measured to calculate apparent indentation fracture toughness with the equation proposed by Niihara et al. [50]. The orientation of indentations was arbitrary, regardless of the groove’s direction. However, to determine the presence of anisotropic properties after grinding, 30 kgf indentations were performed again in 4-U samples, in order to induce cracks running parallel or perpendicular to the grooves. Indentation size and crack length were determined by Field Emission Scanning Electron Microscopy (FESEM, Carl Zeiss Neon 40) imaging. Scratch tests [51] were carried out on a CMS Revetest using a Rockwell C diamond tip (200 μm radius), increasing the load linearly from 0 N to 200 N, with a scratch length of 5 mm and an advancing speed of 1 mm/min. Three scratches were done per specimen, with one specimen per condition. After the tests, specimens were observed under FESEM. Some of the specimens were also cut transverse to the scratches, near the end of the tracks, in order to observe the sub-superficial damage induced at one particular load. The cross-sections were polished and observed with a Confocal Laser Scanning Microscope (CLSM, Lext OLS3100 Olympus). J. Minguela, et al. -RXUQDORIWKH(XURSHDQ&HUDPLF6RFLHW\²
! ! 2.5. Hydrothermal degradation Accelerated degradation tests in water steam were performed at 134 °C and 2 bars of pressure (Micro8, Selecta) [52]. Monoclinic phase (mphase) was quantified by X-Ray Diffraction (XRD, D8-Advance, Bruker) in Bragg-Brentano symmetric geometry using Cu K α radiation (40 kV and 40 mA) with 0.02° step size, 1 s/step and a 2θrange of 26°≤2θ≤37°. In order to study t→mtransformation kinetics, XRD spectra were collected at different degradation times (at 0, 2.5, 5, 10, 15, 20, 30, 40 and 50 h). Monoclinic content was calculated with the equation proposed by Toraya et al. [53]. For each condition and time point, the monoclinic fraction of three different specimens was averaged. Samples degraded for 50 h, which correspond to the last time point used, were cut and the cross-section was mirror-polished. CLSM was employed to observe the extent of the transformed layer. m-phase maps in the cross-sections were also obtained using Confocal micro-Raman spectroscopy (Cm-RS, inVia Qontor, Renishaw) with a Nd:YAG laser (wavelength 532 nm, integration time 0.1 s). m-phase was quantified by using the equation proposed by Katagiri et al. [54]. 2.6. Cell adhesion study Human sarcoma osteogenic (SaOS-2) cells (ATCC) at passage 15–17 were cultured in Mc Coy’s 5A medium supplemented with 10 % (v/v) foetal bovine serum (FBS), 2 % (v/v) 4-(2-hydroxyethyl)-1-piper- azineethanesulfonic acid (HEPES), 1 % (w/v) sodium pyruvate, 50 μg/ mL streptomycin, 50 U/ mL penicillin, and 1 % (w/v) L-glutamine. Cells were maintained at 37 °C in a humidified atmosphere containing 5 % (v/v) CO 2 , changing culture medium every three days. This cell line represents a well established cellular model to study osteoblast-like responses on biomaterials [55,56]. After reaching 80 % confluence, cells were trypsinized (Trypsin-EDTA) and seeded at a concentration of 10,000 cells/specimen in the same medium used for cell culture. Cells were allowed to attach and spread for 24 h and then they were gently washed with PBS, fixed with paraformaldehyde (PFA, 4 % w/v in PBS) for 30 min and permeabilized with 0.05 % (w/v) Triton X-100 in PBS for 20 min. Actin fibers were stained by incubating with TRITC-con- jugated phalloidin (1:300, in permeabilizing buffer) for 1 h and nuclei were stained using 4′,6-diamidino-2- phenylindole (DAPI) (1:1000, in PBS-glycine 20 mM) for 2 min, both in the dark. Between all steps, samples were rinsed three times with PBS-glycine for 5 min. All reagents were purchased from Sigma–Aldrich, unless otherwise noted. Specimens were mounted in Mowiol 4–88, examined under a fluorescence CLSM (CLSM, LSM 800, Carl Zeiss) and images were processed using Fiji/Image-J package [57] to calculate cell-shape parameters. Assays were done with triplicates, and repeated twice. 2.7. Statistical analysis Values in all graphs are displayed as mean ± standard deviation. Statistical comparison of values was based on ANOVA using Tukey’s test for pair-wise comparisons (p < 0.05). Differences were also analysed with the non-parametric Mann-Whitney test. The software used for statistical analysis was Minitab®18.1. 3. Results and discussion 3.1. Topographical characterization As depicted in the WLI images of Fig. 1, during specimen preparation the use of distinct grit sizes and polishing dynamics allowed to obtain a range of topographies, combining different roughnesses and directionalities. As coarser abrasives were used, an increase in roughness was observed (i.e. specimens from 1 to 4). As plotted in Fig. 2aand visually depicted in Fig. 2e, S a increased by a factor larger than or equal to three between consecutive roughness grades, and no significant differences were present between M and U specimens. An evident textured directional pattern was present in U specimens, while grooves in Table 1 Summary of the microstructure, phase composition, residual stresses and surface damage of the specimens used in the present work [45]. U T and U P indicate residual stresses measured transverse or parallel to the grinding grooves (in unidirectionally ground specimens). J. Minguela, et al. -RXUQDORIWKH(XURSHDQ&HUDPLF6RFLHW\²
! ! M samples showed a random arrangement. This texture was further confirmed by S tr (Fig. 2b), indicating a stronger anisotropy in all U specimens. A gradual increase in surface area was also noticed, which according to S dr (Fig. 2c) increased to about 20 % in the case of 4-M/U. Although grinding/polishing introduced evident topographical modifications on the surfaces, contact angles (Fig. 2d) remained almost constant between 60° and 70°. This may be attributed to the relatively narrow S a range of the studied surfaces, with similar differences as found by other authors in this material [58]. 3.2. Mechanical characterization The interaction between abrasive particles and the surface is not only limited to topographical modifications. As the diamond abrasives erode the surface, shearing and tensile stresses induce a t→mtransformation, reaching several microns deep [17,45]. The volume expansion of the mphase induces a compressive stress state on the surface that can exceed the GPa, which may affect its mechanical properties [17,59]. 10 kgf HV test results are presented in Fig. 3a, in which no significant differences were observed. However, in the case of K Ic aclearincreasingtrendwas detected. Fig. 3bshowstheresultsofK Ic for M and U specimens, both presenting the same behaviour. As rougher abrasives were used (i.e. higher compressive state on the surface, as shown in Table 1), statistically higher values were obtained. 4-M/U specimens showed an increase of 1.5 MPa·√mascomparedtoMP,whichrepresentsanimprovementof around 30 %. In order to study if the anisotropic stress state found in unidirectionally ground specimens (see Table 1)canresultinanisotropic mechanical properties, further indentations were done in 4-U specimens, this time aligning the originated cracks in two different directions: parallel and perpendicular to the grooves. According to results presented in Fig. 3c, despite the high variability in crack length measurements, a significantly increased K Ic parallel to the grinding grooves was detected. As depicted in Fig. 3d, the higher stresses perpendicular to the grinding direction were able to hamper crack propagation along the grooves. In order to evaluate the effects of this stressed layer on flaw development after a sliding contact, scratch tests were carried out in M specimens and surface damage was evaluated by FESEM. Micrographs in Fig. 4a correspond to the last part of the scratch tracks, showing the region under applied loads between 120−200 N. Images of the polished cross-sections near the end of the tracks, under loads above 180 N, are displayed in Fig. 4c and 4d. From the top view it is observed that lateral cracks formed along the tracks at high loads, except for specimen Fig. 1. WLI topographical images of the specimens after surface modification. From left to right, increasing levels of roughness, 1 to 4. Multidirectional (M) patterns are displayed on the top, while unidirectional (U) patterns are displayed on the bottom. Fig. 2. Roughness parameters, contact angle and surface profile in ground/polished specimens. a) Arithmetic average height (S a ), b) Texture aspect ratio (S tr ), c) Developed interfacial area ratio (S dr ), d) Contact angle and e) Surface profile of heights. J. Minguela, et al. -RXUQDORIWKH(XURSHDQ&HUDPLF6RFLHW\²
! ! 4-M in which no cracks were visible. A magnification of the final section in 4-M is presented in Fig. 4b. Yet, once the cross-sections were evaluated, all the specimens presented sub-surface lateral cracks, generated at the centre of the track (where stresses are maximum) and propagating laterally up to the surface. As shown in Fig. 4d, MP specimen presented two symmetric lateral cracks at each side of the track. In the case of 4-M, cracks were also observed, with less symmetry and irregular length. While in MP they were wide and reached the surface open, allowing for a clear identification in the top view, cracks in 4-M were narrow and their intersection with the surface was difficult to detect. Such differences between crack morphology may be related to two different factors found in coarsely ground specimens. On one hand, the presence of a shallow layer of compressive stresses on the surface (around 6−7μm thickness [45]). It may avoid crack opening in a similar fashion as observed in the K Ic experiments. On the other hand, possibly to a lower extent, the highly distorted microstructure under the first micron. It may deflect or hinder crack propagation, as observed in severe plastically deformed materials [60]. The obtained results demonstrate that the changes undergone after grinding/polishing procedures are able to improve surface mechanical properties, in particular crack propagation after contact damage events, by improving apparent fracture toughness. A close relation thus exists between surface mechanical response and the layer of residual stresses. 3.3. Hydrothermal degradation Fig. 5 plots the transformation kinetics of both M (Fig. 5a) and U (Fig. 5b) specimens after degradation in water steam. Degradation kinetics showed that unlike the grinding directionality, whose influence was minor, the severity of the abrasion (i.e. grit size) critically influenced the degradation behaviour. All the ground/polished specimens exhibited an improved resistance to hydrothermal degradation, as compared to MP specimens. However, both too soft and too aggressive treatments failed to provide protection against degradation over time. In contrast, 2-M/U and 3-M/U, presenting intermediate roughness, displayed an excellent resistance to degradation. The former in particular showed no signs of increase in the monoclinic content even after 50 h in water steam, which corresponds to roughly 150 years in vivo [52], much longer than the expected lifetime of any biomedical implant. Fig. 6 shows CLSM images and am-phase mapping of the cross-sections in all M specimens as well as in MP after 50 h of degradation. MP specimens presented the maximum transformation depth, with a homogeneous fully degraded layer of about 10−11 μm. Meanwhile, both 2-M and 3-M were free of degradation. Specimens 1-M and 4-M presented partial transformation of the surface, with a similar degree of transformation but a different distribution of the monoclinic material. On one hand, transformation in 4-M was very heterogeneous and seemed to be nucleated around specific spots, leaving Fig. 3. Mechanical surface properties of the studied specimens. a) Vickers hardness, b) Apparent indentation fracture toughness, c) Apparent indentation fracture toughness in 4-U specimens along two different directions: perpendicular and parallel to the grinding grooves. d) Schematic representation of the influence of residual surface stresses on indentation crack length. Red arrows depict the intensity and direction of the residual stresses. Anisotropic stress states in unidirectionally ground specimens led to anisotropic mechanical behaviour. Groups identified by the same letter are not statistically different (p > 0.05). (For interpretation of the references to colour in the Figure, the reader is referred to the web version of this article). J. Minguela, et al. -RXUQDORIWKH(XURSHDQ&HUDPLF6RFLHW\²
! ! other surface regions with lower amounts of m-phase. On the other hand, 1-M presented a layer-like structure with maximum transformation in the surface region, decreasing with depth. Nevertheless, both 1-M and 4-M displayed lower transformation depths as compared to MP. Several of the microstructural features observed after grinding/ polishing procedures are known to have a protective effect against Fig. 4. a) FESEM micrographs of the tracks left after scratch tests in M specimens. Note that no cracks were visible on the surface of 4-M. Dashed line in MP indicates how specimens were cross-sectioned to obtain figures c) and d). b) Magnification of the last section of the track in a 4-M specimen. c) and d) CLSM cross sectional images of the last section of the scratch at loads above 180 N in 4-M and MP specimens, respectively. Lateral cracks could be observed in both specimens, presenting different morphologies. Fig. 5. Degradation kinetics in water steam. The evolution of the monoclinic volume fraction is plotted against degradation time. a) M specimens and b) U specimens. No degradation was observed in 2-M/U specimens and just a slight increase in the monoclinic content could be appreciated in 3-M/U specimens. The 20 % V m left to reach a full m-phase material in MP specimens, corresponded to non-transformable cubic (c) phase. J. Minguela, et al. -RXUQDORIWKH(XURSHDQ&HUDPLF6RFLHW\²
! ! ageing. Reduction in grain size after surface recrystallization [31], as well as in domain size due to ferroelastic switching [34], and presence of a layer of residual compressive stresses [33] are known to delay low temperature degradation through different mechanisms. The behaviour shown by the studied specimens can be explained in terms of the presence of such features, as summarized in Table 1. Both 2-M/U and 3-M/ U, presenting an excellent resistance, displayed a recrystallized surface of nano-grains, a certain amount of domain switching (i.e. texture as shown by (002) t /(200) t XRD intensity relation), as well as a layer of residual compressive stresses [45]. 3-M/U was ground with resinbonded and relatively large diamond particles, presenting an affected layer of several microns deep. 2-M/U was polished with smaller diamond particles in water-based slurries, involving a milder process that reduced the affected region to a very shallow but intense layer, in the first micron of material. However, both of them were able to effectively protect the surface. In fact, similar degradation resistance in softly polished specimens have been recently reported [30] with 15 μm diamond polishing. As the grinding/polishing varied from this optimal finishing, degradation started to occur. While 1-M/U seemed not to present enough protective features, 4-M/U showed a deterioration of the achieved protection. Regarding the former, XRD spectra performed in a previous study [45], showed to be very similar to the one in the mirror-polished (MP) with almost no changes even in grazing incidence measurements, lacking the protection of surface texture and the residual stresses following the t→mtransformation. However, 1-M/U’s surface was found to present partial recrystallization, which seemed to have a positive effect, as degradation was clearly improved respect to MP. In fact, ageing in this specimen presented a degradation similar to 4-M/U, in which a very severe grinding had been applied. It is important to highlight that a surface finishing as smooth as the one in 1- M/U, with a S a =16 nm, was able to introduce the microstructural changes needed for the delay of ageing. The key point to enhance ageing resistance through microstructural tailoring, is thus not to introduce large changes, but just the adequate ones. This could be observed in the case of 4-M/U, where degradation was higher than in 2-M/U and 3-M/U, even though the former exhibited the largest microstructural changes. The decrease in performance for this specimen was related to surface damage. As evidenced in Fig. 7a and 7b, where the surfaces of 3-M and 4-M specimens are shown right after grinding (i.e. not degraded), regions with extensive damage in the form of micro-cracks could be observed in 4-M. This is different to the scenario found in the rest of the specimens, where ductile material removal mechanisms took place exclusively. In order to study whether the worsening of the degradation behaviour was indeed related to such surface state, a superficial m-phase map was obtained in one of the 4-M specimens degraded for 50 h. Fig. 7c shows the obtained phase map along with an optical micrograph of the corresponding region. While most of the surface presented damaged material (labelled as A), a damage-free track with a whitish surface crossed the measured region almost horizontally (labelled as B). Phase mapping clearly revealed that the entire surface was degraded except for the damage-free track, which was totally resistant to degradation. In fact, one damaged track crossed the non-transformed region, acting as a nucleating zone for the m-phase (labelled as C). As shown in our previous study [45], as the diamond particle size increases, material removal mechanisms tend to change from ductile to brittle, favouring the presence of damaged regions and allowing water to bypass the protective layer. Thus, if microstructural tuning through grinding procedures is to be performed for ageing-protective reasons, a balance must be achieved between the introduction of beneficial features and the prevention of surface microdamage. 3.4. Cell adhesion study Surface topography of biomaterials is known to affect cell behaviour [61]. Indeed, it is well accepted that roughness can influence (positively or not) the adhesion, proliferation and differentiation of osteoblastic cells [42,43,62,63]. However, the majority of works have generally focused on titanium and studies on other materials, e.g. Y-TZP, are needed. Fig. 8 displays the results obtained in the cell adhesion assays. As shown in Fig. 8a, the number of adherent SaOS-2 was very similar on all Fig. 6. Cross-sections of the degraded specimens after 50 h in water steam. On the left, CLSM images. On the right, m-phase distribution determined by confocal micro-Raman spectroscopy. Note that for each condition, CLSM and phase images were taken from the same specimen but probing different regions. J. Minguela, et al. -RXUQDORIWKH(XURSHDQ&HUDPLF6RFLHW\²
! ! the studied surfaces, without statistically significant differences as a function of the surface topography. In detail, neither an increase in surface roughness (i.e. Sa values) nor the presence of a pattern texture (M/U) seemed to influence cell attachment. In contrast, cell morphology and orientation were dependent on the topography. This effect can be observed in Fig. 8b and 8c, where for both 3-U and 4-U, a slight decrease in cell area (statistically significant for 4-U) and an increase in the aspect ratio (statistically significant for 3-U and 4-U), i.e. a more elongated cell shape, were observed. As depicted in Fig. 8d the morphological changes in 3-U and 4-U were related to a strong alignment in the direction of the grinding grooves, which was only detected on these two surfaces. For the rest of the specimens no alignment was observed, displaying similar morphological features as those found in the mirrorlike polished MP specimen. These results indicate that roughness alone does not directly affect cell area or their aspect ratio, but in combination with oriented patterns is able to favour cell alignment above a certain roughness level, changing cell morphology. Previous data already reported such effect on ground titanium surfaces [64,65], as well as in other materials [66]. The ability to induce cell alignment has been a subject of interest for many researchers, as a means of affecting cell behaviour. In fact, it has been shown to trigger cytoskeleton reorganization, and to affect extracellular matrix remodelling, cell migration, membrane protein relocation and gene expression [67]. Herein we propose the existence of a threshold larger or equal to Sa =150 nm to effectively induce cell alignment on unidirectionally ground Y-TZP. Fig. 8e and 8f show two fluorescence CLSM images of stained cells in Fig. 7. FESEM micrograph of the surface in a) 3-M and b) 4-M specimens right after grinding (i.e. not degraded). Extensive damage could be seen in 4-M surface, with the presence of micro-cracks and flaking, while 3-M presented a smoother damage-free surface, with evident signs of plastic material removal mechanisms. c) Insight on the degradation behaviour of 4-M specimens. On the left, optical microscopy image of a 4-M specimen surface degraded for 50 h. On the right, m-phase mapping of the outlined region through confocal micro-Raman spectroscopy. Labels A indicate large regions were micro-damage was observed on the ground tracks. Label B identifies a track (in whitish colour) with no damage, where mainly ductile removal mechanisms took place. Label C shows a damaged track crossing the damage-free region. J. Minguela, et al. -RXUQDORIWKH(XURSHDQ&HUDPLF6RFLHW\²
! ! specimens 3-M and 3-U. An alignment in 3-U in the direction of grinding is clearly noticed, while cells are randomly spread onto 3-M surfaces. 4. Conclusions Microstructural and crystallographic changes after surface grinding/polishing were able to greatly affect both mechanical properties and hydrothermal degradation resistance of 3Y-TZP. Furthermore, topographical changes (i.e. unidirectional grooves) efficiently promoted osteoblasts alignment. Although the increase in properties showed a significant direct correlation with abrasion severity, surface damage introduced in the coarsest grinding worsened ageing resistance. In particular, it was observed that: •The layer of compressive residual stresses as a result of the t→m transformation resulted in an increase in apparent fracture toughness, which hindered the propagation of superficial cracks, as well as the opening of subsurface cracks reaching the surface, the latter as observed in scratch tests. The studied mechanical properties improved with grinding. •In order to protect 3Y-TZP from ageing, it was shown that coarse grinding is not only unnecessary, but can be counterproductive. Instead, intermediate conditions (in terms of grit size), including both grinding and rough polishing, could protect the surface from degradation, even in damage-free specimens with a roughness as low as S a =45 nm. In this regard, zirconia showed to be highly responsive to surface mechanical treatments. Even specimens polished until a surface roughness of S a= 16 nm displayed an important degree of surface protection. •All the topographical modifications performed allowed cell attachment and presented contact guidance when unidirectionally ground above a certain roughness level. Declaration of Competing Interest The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper. Acknowledgements This work was supported by the Ministerio de Ciencia, Innovación y Universidades (MAT2017-83905-R, MINECO/FEDER), the Generalitat de Catalunya (2017 SGR-933 and SGR-1165) and the CREATe-Network Project, Horizon 2020 Program of the European Commission (RISE Project Nr. 644013). J. Minguela has been supported by a predoctoral fellowship from the Barcelona Research Center in Multiscale Science and Engineering of the UPC. M-P. Ginebra acknowledges the ICREA Academia Award from the Generalitat de Catalunya. C. Mas-Moruno thanks the Spanish Government for a Ramon y Cajal grant. J.J. Roa acknowledges the Serra Hunter programme from the Generalitat de Catalunya. References [1] H.J. Conrad, W.J. Seong, I.J. Pesun, Current ceramic materials and systems with clinical recommendations: a systematic review, J. Prosthet. Dent. 98 (2007) 389–404. [2] T. Miyazaki, T. Nakamura, H. Matsumura, S. Ban, T. Kobayashi, Current status of zirconia restoration, J. Prosthodont. Res. 57 (2013) 236–261. [3] J.R. Kelly, I. Denry, Stabilized zirconia as a structural ceramic: an overview, Dent. Mater. 24 (2008) 289–298. [4] I. Denry, J.R. Kelly, State of the art of zirconia for dental applications, Dent. Mater. Fig. 8. SaOS-2 adhesion results after 24 h of incubation in FBS-supplemented medium. a) Cellular adhesion (cells/cm 2 ), b) cell area (μm 2 ) and c) cell aspect ratio. d) Angular histogram of cell orientation. Each bar of the histogram represents the relative cell number aligned to a specific angle on the surface. In U specimens 90° corresponds to the grinding direction. e) and f) Fluorescence CLSM images of the cells cultured on specimens 3-M and 3-U, respectively. Actin filaments are stained with TRITC-conjugated phalloidin (red), and cell nuclei with DAPI (blue). White arrow in f) points to the grinding direction. Groups identified by the same letter are not statistically different (p > 0.05). (For interpretation of the references to colour in the Figure, the reader is referred to the web version of this article). J. Minguela, et al. -RXUQDORIWKH(XURSHDQ&HUDPLF6RFLHW\²
! ! Materials Science & Engineering C 125 (2021) 112096 2 year survival rate of 98.4% (95% CI 91.6, 99.9) [3], long-term studies are still needed. In the case of titanium, for instance, implant survival rates at 10 years are close to 95% [4]. Moreover, it should be taken into account that it is estimated that 5.5–6 million implants are placed each year only in Europe [5]. Therefore, even if the percentage of dental implant failure is low, in absolute values a large number of patients need a revision surgery every year, and the consequences are often catastrophic. The reasons for failure are varied and still not completely understood. They are often related to the initial foreign body response, but also to other events disbalancing the osteointegration process, including peri-implantitis, non-optimal implant design, traumatic handling, new loading conditions after losing adjacent teeth, and general health aspects [6]. In particular, further improvement of osteointegration at the implant surface is still necessary as [7]: - In healthy subjects the osteointegration of a dental implant is a slow process. An early or immediate loading is not possible, which has negative effects in terms of patient morbidity and healthcare costs. - The placement of implants is counter indicated in clinically compromised patients, where impaired osteointegration is observed. Such conditions include diabetes mellitus, osteoporosis, radiotherapy in neck and head or smoking addiction [8,9]. For these reasons, surface modification (e.g. topographical or biochemical) of implants has been widely employed in order to enhance bone formation at the material-tissue interface and achieve a proper biological seal at the gum level [10,11]. Surface topography can improve tissue integration in several ways. Firstly, surface roughness favors cell adhesion [12] and allows for better mechanical interlocking when in contact with bone [13]. Secondly, surface texture can influence cell behavior. For example, grooved surfaces can display contact guidance and favor cell migration, which is of special interest in applications where tissue growth over a surface must be guided [14,15], including dental implants [16–18]. In addition, both micro-[19,20] and nano- [11,21] topographical features can modify gene expression through cellular mechanotransduction. Indeed, changes in the organization of the cytoskeleton can trigger signaling pathways that (up)regulate the expression of genes involved in osteodifferentiation. It is the case of linear patterns, in which different groove/ ridge combinations can guide human mesenchymal stem cell (hMSC) differentiation into several lineages, including the osteogenic one [22–24]. However, due to its particular properties, surface modification of Y- TZP remains challenging as compared to other materials used in dentistry such as titanium. Y-TZP is a relatively hard and brittle-like material [25]; thus, its surface can only withstand limited amounts of plastic deformation before presenting surface damage [26,27]. Accordingly, milder treatments must be employed if excessive crack formation, chipping or stress-induced phase transformation (from tetragonal to monoclinic phase, t → m) are to be avoided. Consequently, relatively low values of surface average roughness (R a ) are obtained. Due to its chemical inertness, etching is only limited to a few aggressive reagents [28], and other methods such as anodization are not possible due to the lack of electronic conductivity. The effect of such treatments on the hydrothermal degradation of Y-TZP has to be taken in particular consideration. After extended exposure to water, some Y-TZP formulations can undergo a spontaneous phase transformation from t- to the more stable m-phase, which is associated with crack formation and weakening [29,30]. Excessive surface damage can facilitate this process [31,32], and as a consequence suitable methods for surface modification are limited, especially in biomedical applications. Among the methods that have been successfully employed to superficially modify the topography of Y-TZP there are mechanical, chemical and thermal-based techniques, including sandblasting, grinding [26], chemical etching [28] and laser micro-patterning [33]. Of particular interest is laser patterning, which stands out as an efficient means of producing detailed and reproducible topographies at different length scales (e.g. grooves [34], pits [35], grits [36] or other textures) with relatively fast processing speed. Besides, as a non-contact technique it presents additional advantages, such as the absence of tool wear and surface contamination. Y-TZP surface has been successfully structured with lasers working on different regimes and employing different techniques [33,34,37–39]. In particular, direct laser interference patterning (DLIP) represents a promising technique for industrial use thanks to its ability to produce periodical patterns (mostly grooves, although other patterns are possible) in a single step, with higher processing speeds as compared to other techniques (e.g. laser writing or lithographic techniques) and resolutions at the micron- and sub-micron level [40–43]. Notably, it is possible to engrave such patterns in complex 3D structures, such as the body of threaded dental implants [44]. Just a few works are available about DLIP structuring of Y-TZP surfaces [24,32,33,41,43,45–47] and its influence on damage and hydrothermal degradation, which are only known in the nanosecond pulse duration regime [32,41,46], but not in the femtosecond one. Likewise, cellular behavior on Y-TZP grooved substrates has been scarcely characterized, whether produced by DLIP or direct writing. The available information agrees in that the grooved topographies (as it has been widely characterized in other materials [19,48]) can influence cell morphology, and that differentiation into the osteogenic lineage may be enhanced [24,36,49–51]. Alternatively, biochemical surface modifications may also be used in order to improve the osteointegrative potential of biomedical surfaces. Such modifications are generally based on the extracellular matrix (ECM) of bone, either its mineral inorganic part (e.g. calcium phosphate coatings) or its organic components (e.g. collagen, fibronectin, etc.) [11,52]. Of particular relevance are those organic molecules able to trigger receptor-specific cell functions, especially proteins [53], growth factors [54,55], peptides and related analogues [56,57]. In the particular case of peptidic molecules, several works have explored the functionalization of dental materials to enhance their surface properties and bioactivity [58]. These works include the use of antibacterial peptides [59,60], peptides that can reinforce epithelial sealing [61] and peptides that are osteogenic [62] or can improve the bone healing process [63], among others. The main advantage of using synthetic peptides lies on their specificity, reduced size, and higher stability against enzymatic degradation and environmental changes such as pH or temperature. Although the most well-known peptide in tissue engineering is the RGD sequence [64], with a predominant role in cell-adhesion, other peptides have shown potential to improve bone healing and osteointegration [65]. In this regard, several peptide sequences have been found to present osteoinductive properties [66], such as those derived from the bone morphogenetic protein 2 (BMP-2) [67,68]. BMP-2 induces osteoblastic differentiation by binding to type I and type II BMP receptors (BMPRs). Lee et al. [69] studied a BMP-2 derived peptide (DWIVA) and found an increased osteoblastic differentiation of human bone marrow stromal cells through Smad signal transduction. Subsequently, it was recently demonstrated that combining this peptide with the RGD motif synergistically promoted integrin and BMPR signaling, inhibiting myotube formation on C2C12 cells and activating their transdifferentiation into the osteogenic lineage [70]. Notably, this study showed that the combination RGD-DWIVA in a geometrically controlled manner increased cell adhesion and promoted BMP-dependent signaling in a larger extent as compared to the presence of RGD or DWIVA only. Within this context, the aim of the present work was to study the combination of topographical and biochemical modifications on Y-TZP biomaterials, and evaluate their effects at the surface level and its biological influence on hMSCs. Grooved laser patterns were created with two different periodicities: one with features of only a few microns, much below the cell body size, 3 μ m; the other one with larger grooves, in a closer range to the cell size, 10 μ m. DLIP technique was employed in order to ensure both periodicity and high processing speeds with J. Minguela et al.
! ! Materials Science & Engineering C 125 (2021) 112096 3 industrial applicability. The femtosecond regime was chosen because previous studies reported extended surface damage [46] and limitations in terms of pattern depth for the nanosecond regime [33]. A detailed topographical and microstructural characterization of the modified surfaces was carried out to analyze surface damage and changes in surface properties. To the best knowledge of the authors, these effects have not been investigated for such treatment. Additionally, the patterned surfaces were also functionalized with a dual peptidic platform [71], including the RGD and the BMP-2-derived DWIVA sequences [70], to further tune hMSC behavior. Interestingly, the biofunctionalization of Y-TZP has been scarce and limited to cell adhesive peptides [72–74]. Studies expanding the potential of peptidic functionalization to other areas (e.g. osteogenesis) are missing, and to date no studies combining topographical and biochemical modifications on this material can be found. Thus, the main objective of this study was to investigate for the first time the combination of ultrashort pulsed direct laser interference patterning (USP-DLIP) and chemical functionalization on Y-TZP and explore the potential synergisms between topographical and biochemical cues (Fig. 1). Such combined approach may improve the tissue integrative properties and osteogenic potential of Y-TZP surfaces and provide new insights for the design of long-term functional dental implants. 2. Experimental procedure 2.1. Material processing 2.1.1. Sample preparation Disc-shaped samples of 15 mm diameter were produced from zirconia powders stabilized with 3 mol% yttria (TZ-3YSB-E, Tosoh). Briefly, powders were cold isostatically pressed at 288 MPa and sintered at 1450 ◦C for 2 h (constant heating and cooling rates of 3 ◦C/min) obtaining a material with a grain size of 0.32 ±0.12 μ m and a density above 99% of the theoretical one. All the samples were mirror-like polished using suspensions of diamond particles with decreasing particle size (30 μ m – 6 μ m – 3 μ m) with a final polishing step using an alumina suspension of 0.02 μ m particle size. Some samples were not further modified to be used as reference specimens, labeled as CTRL. Further details about sample preparation and characterization can be found elsewhere [75]. After polishing, samples were cleaned in an ultrasonic bath in 6-minute washes, as follows: cyclohexane (x 2), acetone (x 2), deionized water (x 2), ethanol (x 2) and acetone (x 2). Finally, samples were dried in a N 2 stream. 2.1.2. Laser patterning In order to obtain surface patterns, DLIP was employed. In this technique, an inhomogeneous fluence distribution is produced on the surface due to the interference of two or more laser beams, originating a periodical pattern [15,76]. The particular geometry of the patterns depends on the number of interfering beams as well as the optical setup. Surface patterning was carried out by using a Ti:Sapphire laser source emitting ultrashort pulses of 100 fs at Full Width Half Maximum (FWHM) with a centered wavelength λ of 800 nm. A detailed description of the optical setup employed in this work can be found in [43]. Briefly, an aperture defines the working beam diameter while a wave plate adjusts the polarization angle of the laser beam perpendicular to the generated pattern orientation in the first section of the optical setup. Further on, the femtosecond pulsed seed beam is divided by a Diffractive Optical Element (DOE), while the individual coherent beams are finally overlapped on the sample surface by means of a lens system. The beamoverlap induces a line-like interference pattern. The periodicity Π is defined by Π=λ 2tan(θ 2)(1) where θ is the incidence angle between the individual beams [43]. An alteration of Π can be achieved by changing the distance between DOE and the focusing lens system. The sample was mounted on a (x,y) motorized stage. In order to fully structure specimen surfaces, laser pulses were synchronized with the motorized stage. An optimization process was carried out adjusting laser power, stage speed and pulse overlapping in relation to the DOE-lens system spacing until homogeneous linear patterns were obtained of either 3 or 10 μ m periodicity. Such laser-treated specimens were labeled as 3L and 10L, respectively. Samples were subsequently cleaned and dried as described above. Fig. 1. Scheme of the rationale behind this study. Two different strategies were employed in order to improve the tissue integration potential of zirconia surfaces, one of topographical and one of biochemical nature. The main known effects on human cells from each strategy are detailed on the figure. J. Minguela et al.
! ! Materials Science & Engineering C 125 (2021) 112096 4 2.2. Biofunctionalization process 2.2.1. Biomolecule synthesis The coating molecule (labeled as P) was produced using standard solid-phase peptide synthesis protocols and characterized as described elsewhere [70]. As shown in Fig. 2, the peptidic platform contains the bioactive sequences RGDS and DWIVA, and two units of L-3,4-dihy- droxyphenylalanine (L-DOPA) as surface anchoring points. An analogue with 5(6)-carboxyfluorescein was also synthesized to perform characterization studies with fluorescent methods. 2.2.2. Surface functionalization Samples were coated overnight with a 150 μ L drop at 100 μ M of the peptidic platform (P) solution. As previously indicated, some samples were functionalized with the fluorescently labeled platform, for characterization purposes. Next, samples were rinsed thrice with deionized water and dried in a N 2 stream. Specimens functionalized with the peptide were labeled as CTRL-P, 3L-P and 10L-P. A summary with all the specimens and labels used in this work can be found in Table 1. 2.3. Surface characterization 2.3.1. Surface changes induced by the laser treatment Changes in surface topography were visualized by Field Emission Scanning Electron Microscopy (FESEM, Carl Zeiss Neon 40). Roughness parameters and surface profiles were obtained using a Confocal Laser Scanning Microscope (CLSM, Olympus Lext OLS3100). For such purpose, three specimens were evaluated per surface condition, and three images of 96 μ m ×128 μ m were taken on each specimen. Crystalline phases were determined by X-Ray Diffraction (XRD, Bruker D8-Advance) in Bragg-Brentano symmetric geometry configuration. The analysis was performed from 26◦≤2θ ≤37◦on a diffractometer using Cu K α radiation (40 kV and 40 mA) with 0.02◦step size and 1 s/step. The volume fraction (V m ) of the monoclinic phase (m) was calculated with the equation proposed by Toraya et al. [77]. The residual stress state of the surfaces was characterized with the sin 2 ψ method [78] by XRD analysis (Empyrean, PANalytical) using Cu K α radiation (40 kV and 40 mA). With the same methodology employed in a previous study [75], the tetragonal (101) t peak found at 2θ =30.2◦was used for the stress calculations, at Chi angles from −60◦to +60◦in 13 steps. Measurements were performed along three directions on the surface: Φ =0◦, 45◦and 90◦, in order to identify possible stress anisotropies. In this case, Φ =0◦and Φ =90◦corresponded to a direction parallel and perpendicular to the grooved patterns, respectively. Analysis was performed by using the PANalytical X’Pert Stress plus software. Crystalline phases were determined in triplicates, while residual stresses were determined in duplicates. In order to characterize the microstructure resulting from the laser modification, thin lamellas of the subsurface were obtained by Focused Ion Beam (FIB, FEI Helios Nanolab Dualbeam 600) and deposited on a copper grid. The lamellas were then observed under Scanning Transmission Electron Microscopy (STEM, Carl Zeiss Neon 40) to reveal the subsurface microstructure. Hydrothermal degradation resistance (also known as ageing or lowtemperature degradation (LTD)) of the specimens after surface patterning was investigated. More information about this phenomenon can be found in Ref. [29]. In such process, the t → m transformation, of expansive nature, spontaneously takes place on the surface in the Fig. 2. Chemical structure of the biomolecule. The RGDS and the DWIVA sequences are highlighted in different colors, as well as the L-DOPA based anchoring unit. In the fluorescently labeled biomolecule, 5(6)-carboxyfluorescein was bound to the N-terminus of DWIVA. (For interpretation of the references to color in this figure legend, the reader is referred to the web version of this article.) Table 1 Labels and description of the studied surface conditions. Label Description CTRL Mirror-like polished. Used as a flat topography reference. 3L Laser patterned with a periodicity of 3 μ m. 10L Laser patterned with a periodicity of 10 μ m. CTRL-P CTRL specimens functionalized with the peptidic platform. 3L-P 3L specimens functionalized with the peptidic platform. 10L-P 10L specimens functionalized with the peptidic platform. J. Minguela et al.
! ! Materials Science & Engineering C 125 (2021) 112096 5 presence of moisture. It is associated with the onset of micro-cracks and is able to progress autocatalytically to the bulk material [79]. LTD is of great concern, especially in the biomedical field, where it has been responsible for the catastrophic failure of medical prostheses. In order to evaluate the resistance to LTD of Y-TZP materials, accelerated tests can be carried out in water steam, as reported elsewhere [29,80]. Hence, specimens were degraded in an autoclave at 134 ◦C and 2 bars of pressure (Selecta Micro8) for 30 h. V m was determined by XRD at several timepoints, and the m-phase content was plotted against degradation time. Three specimens per condition were used. 2.3.2. Attachment of the biomolecule The presence of the peptides on the surface after biofunctionalization was verified through the changes in the surface nitrogen content. This was evaluated by using X-Ray Photoelectron Spectroscopy (XPS) and determining the percentage of the N1s signal. XPS spectra were acquired with a non-monochromatic Al anode X50 source, operating at 150 W at a pressure below 7.5 ×10 −9 mbar. A Phoibos 150 MCD-9 detector (SPECS Surface Nano Analysis GmbH) was employed. To record high-resolution spectra, detector pass energy was fixed at 20 eV with 0.05 eV steps. The obtained spectra were analyzed using Casa XPS software. All binding energies were referenced to the signal of C1s. Measurements were acquired in duplicates. To further study the attachment of the biomolecule and its distribution, a fluorescently-labeled version of the peptide was employed. Surfaces functionalized with such peptides were observed under fluorescence CLSM (Carl Zeiss LSM 800). Three images were taken on each specimen, and three different specimens were studied per condition. The data obtained was analyzed using Fiji/ImageJ. Finally, the peptide surface density was determined following the method reported in [70]. For such purpose, samples coated with the fluorescently-labeled peptides were used in duplicates. After functionalization, the peptidic platforms were detached off the surfaces with 500 μ L of an aqueous solution of NaOH 1 M for 12 min at 70 ◦C. The supernatants were collected. In parallel, a standard curve of the same fluorescent peptide was prepared in NaOH 1 M, with concentrations ranging from 0 nM to 2500 nM. 50 μ L of both the supernatants and each concentration of the standard curve were pipetted into a black 96-well plate. The fluorescence (λ excitation =485 nm, λ emission =528 nm) was read in a multimode reader (Synergy HTX multimode reader, Bio- Tek). The standard curve was finally used to determine the surface density of the peptide. 2.4. Biological characterization 2.4.1. Cell culture Bone-marrow derived hMSCs were purchased from ATCC and cultured in Advanced Dulbecco’s Modified Eagle’s Medium (DMEM) supplemented with 10% (v/v) fetal bovine serum (FBS), 50 U/mL penicillin, 50 μ g/mL streptomycin and 1% (w/v) L-glutamine. Cells were maintained at 37 ◦C, in a humidified atmosphere containing 5% (v/v) CO 2 , changing culture medium three times per week. Cells were detached with trypsin-EDTA and replated on a new flask after reaching 80% confluence. All reagents were purchased from Sigma–Aldrich, unless otherwise specified. Before conducting all cellular experiments, samples were disinfected for 15 min in 70% (v/v) ethanol and subsequently washed thrice with phosphate-buffered saline (PBS). Experiments were carried out in 24- well plates, as sample size closely matched this diameter. 2.4.2. Cell adhesion In the cell adhesion assay, hMSCs at passage 6 were seeded at a concentration of 5000 cells/well in serum-free medium and incubated at 37 ◦C and 5% (v/v) CO 2 containing atmosphere. After 6 h, medium was aspired and non-adherent cells removed by carefully washing with PBS. Cells were fixed with paraformaldehyde (PFA, 4% w/v in PBS) for 30 min and permeabilized with 0.05% (w/v) Triton X-100 in PBS for 20 min. Actin fibers were stained by incubating with TRITC-conjugated phalloidin (1:300, in permeabilizing buffer) for 1 h and nuclei were stained using 4′,6-diamidino-2- phenylindole (DAPI) (1:1000, in PBS- glycine 20 mM) for 2 min, both in the dark. Between all steps, samples were rinsed three times with PBS-glycine for 5 min. Specimens were mounted in Mowiol 4–88, examined under a fluorescence CLSM (Carl Zeiss LSM 800) and images were processed using Fiji/Image-J package [81] to calculate cell-shape parameters. The experiment was performed using triplicates. Once all images were obtained, the samples were immersed in PBS at room temperature for two days, while gently shaking. The mounting medium was dissolved and the coverslips removed. Cells were then dehydrated through immersion in increasing concentrations of ethanol and observed under FESEM. Cell adhesion after one day was also evaluated with the Alamar Blue assay (Invitrogen, ThermoFisher Scientific). In this case, hMSCs at passage 4 were employed, seeding an initial concentration of 5000 cells/ well in serum-free medium. Cells were maintained as described before. After 6 h, non-adherent cells were rinsed and carefully aspired, and complete medium (i.e. FBS supplemented) was added. After one day, cell number was determined with the Alamar Blue assay. Briefly, medium was replaced by 10% (v/v) Alamar Blue reagent in complete medium for 2 h. After the time was reached, the fluorescence of the reagent was measured following the manufacturer’s instructions in a multimode reader (Synergy HTX multimode reader, BioTek), and compared to a standard curve relating cell number and fluorescence intensity. Three biological and three technical replicates were used. 2.4.3. Cell migration In order to study cell migration, silicon culture-inserts (Ibidi) were placed on the surface of the samples. 20,000 hMSCs at passage 5 were seeded in each insert in complete medium, following the volumes recommended by the manufacturer. Cells were left to attach for 24 h, and the inserts were then removed, leaving a confluent layer with a squared shape of approximately 7 ×7 mm at the center of the samples. Nonadherent cells were rinsed and fresh medium was added. At this point, some specimens were carefully washed with PBS, fixed with PFA (4% w/ v in PBS) for 30 min and stored at 4 ◦C in PBS. These specimens were used as a reference, in order to determine the initial cell layer shape and size just after removing the inserts. The rest of the specimens were incubated for an additional 72 h. During this period, cells started migrating to the rest of the surface. After the time was finished, the specimens were washed with PBS and fixed with PFA. Cells were permeabilized with 0.05% (w/v) Triton X-100 in PBS for 20 min and stained in a 0.5% (w/v) toluidine blue solution for 10 min. Samples were rinsed until the excess dye was removed and dried in a N 2 stream. The stained samples were visualized under a stereomicroscope system (Olympus SZX16) and images analyzed with Fiji/Image-J package. The cell layer size and shape of all specimens was measured, and compared to the reference specimens. An explanatory scheme of this experiment can be found in Fig. 10a. Each condition was evaluated by triplicate. 2.4.4. Cell differentiation 15,000 cells/well of hMSCs at passage 4 were seeded in all the cell differentiation experiments. Cells were seeded in serum-free medium for 6 h, and non-adherent cells were then carefully aspired and medium replaced by a complete one. The genetic expression of several genes related to hMSC differentiation was analyzed. After an incubation time of 7 days, total RNA was extracted and purified using the RNeasy Mini Kit (Qiagen). RNA was quantified using a Take3 Micro-Volume Plate (BioTek) and a Synergy HTX multimode reader (BioTek). Equal RNA amounts for each sample were retrotranscribed to cDNA using the Maxima First Strand cDNA Synthesis Kit (ThermoFisher Scientific). RT-qPCR were performed using the PowerUp SYBR Green Master Mix (Applied Biosystems) and specific J. Minguela et al.
! ! Materials Science & Engineering C 125 (2021) 112096 6 primers (see Table 2) in a MIC qPCR cycler (Bio Molecular Systems). The genes tested were: runt-related transcription factor 2 (RUNX2), alkaline phosphatase (ALP), collagen type I (COL-1) and osterix (OSX). Three biological and three technical replicates were tested for each condition studied. The fold change of gene expression was obtained after normalizing the values to CTRL specimens and to the housekeeping gene GAPDH. Detailed calculations have been described elsewhere [82]. Alkaline phosphatase (ALP) activity, a marker associated with the early stages of osteogenesis, was also investigated. After an incubation period of 14 days, cells were rinsed with PBS, lysed with 500 μ L of mammalian protein extraction reagent (mPER, ThermoFisher Scientific) and ALP activity measured as indicated by the manufacturer. A colorimetric assay based on the conversion of p-nitrophenyl phosphate (pNPP) into p-nitrophenol (pNP) was employed (SensoLyte® pNPP Alkaline Phosphatase Assay Kit, AnaSpec Inc.). The results were expressed as nanograms of ALP and normalized by the number of cells on each surface. The number of cells was measured prior to protein extraction on the same day, by employing the Alamar Blue assay. Three biological and three technical replicates were used. 2.4.5. Statistical analysis Values in graphs are displayed as mean ±standard deviation. Statistical differences were assessed by ANOVA using Tukey’s test for pairwise comparisons (p <0.05). Differences were further analyzed and confirmed with the non-parametric Mann-Whitney test. The software employed was Minitab® 18.1. 3. Results and discussion 3.1. Laser patterning As displayed in Fig. 3, CLSM was used to obtain the most relevant topographical parameters after laser modification. By adjusting the optical setup, periodicity could be controlled and set at the desired values: 3.03 ±0.16 μ m (3L) and 9.92 ±0.36 μ m (10L). Such periodicities were chosen with respect to cell size. One periodicity was set to only have a few microns, much below the cell body size (3L), and the other one was set to obtain larger grooves, closer to the range of the cell (i.e. 10L). In contrast to previous results obtained with nanosecond lasers [33], the use of DLIP in the femtosecond regime presented less limitations in terms of pattern depth, which in the present case were 3.04 ± 0.48 μ m in 10L, and 0.99 ±0.19 μ m in 3L. Accordingly, the measured surface average roughness (S a ) was found to be 1030 ±110 nm in 10L and 370 ±20 nm in 3L. The roughness before sample patterning is represented by the CTRL specimens, which was initially 20 ±10 nm. The possibility of producing grooves with larger depths without losing pattern definition is important, as different depths can have different effects on cell behavior [83,84]. In addition, surfaces with larger S a values are known to present better osteointegration in vivo [85,86] . The large differences in terms of the achievable depths between DLIP in both regimes (i.e. nano- and femto-) owes to changes in the nature of laser-material interaction. In the nanosecond regime, material removal is produced by a combination of ablation and melting. In this regime, pulse duration is higher than the electron-phonon relaxation time. Electrons transfer the absorbed energy to the lattice and a thermal equilibrium is reached, leading to heat conduction to the surrounding material [87]. As a consequence, after nanosecond pulsed DLIP irradiation, material is selectively molten in the regions of maximum fluence and pushed to cold areas due to thermocapillarity (i.e. Marangoni effect [88]), producing a grooved topography. Roitero et al. [33] found that, by this method, a trade-off exists between pattern depth and quality. That is, higher depth was accompanied by lower pattern definition. However, in the femtosecond regime, due to the ultrashort pulse duration below the electron-phonon relaxation time [89], material removal is mainly driven by evaporative ablation. In this regime, electrons are heated almost instantly to high temperatures before an energy transfer to the lattice takes place. This results in cold ablation (i.e. direct vaporization and ion break-off), minimizing thermal damage [87,90]. In brief, the transition from melting to ablation (from nano- to femtosecond regime) in DLIP structuring of zirconia allowed to obtain both higher depth and pattern definition, demonstrating the clear advantage of using ultrashort pulses. This can be observed in Fig. 4 where FESEM micrographs of the laser modified surface are presented. As displayed in these images, groove edges were clearly defined, presenting a sharp transition between ablated and non-ablated regions. However, the nano-topography on the valleys differed between both specimens. While 3L presented an array of periodic line-like substructures, 10L presented a more stochastic nano-topography (see magnifications in Fig. 4). Similar sub-structures have been observed when employing different pulse energy or pulse number in the same materials and lasers [35]. Interestingly, although the ripples observed in the bottom of 3L valleys were similar to the feature characteristics of laser-induced periodic substructures (LIPSS) [91], their orientation was aligned parallel to the linear polarization angle of the beam and thus appeared to follow a different formation mechanism compared to classic LIPSS. The formation of such ripples has also been identified in other materials patterned in similar conditions, and its nature is still not clear [43]. In addition to nano-topography, more evident signs of micromelting were present in 3L as compared to 10L, as evidenced by the presence of droplets and recast material. A closer inspection of 10L surfaces is presented in Fig. 5 along STEM micrographs of different sub-surface regions. Fig. 5a presents a general view of 10L surface. Fig. 5b and d correspond to the magnification of two areas: the valleys and the top of the grooves, respectively. Micrographs clearly displayed that material on the top of the grooves remained unaltered, without the presence of any feature indicating microstructural modifications after laser irradiation. However, a sharp transition was observed between this region and the ablated valleys. Most dielectric materials, such as Y-TZP, present a too wide bandgap to absorb single photons at the wavelengths employed. However, at sufficiently high photon intensity, nonlinear absorption processes become predominant and significant multiphoton absorption can take place. The free excited electrons that are generated can then gain enough kinetic energy (through single photon absorption) to excite further electrons into the conduction band, leading to an electron avalanche ionization [92]. This process is generally accepted as the main mechanism of photon absorption by semiconductors and insulators and explains the ability of ultrashort-pulsed lasers to ablate such materials [93]. In the case of the present work, once a threshold of incoming photon intensity was surpassed, nonlinear absorption mechanisms dominated and ablation started, explaining the sudden transition between the nonablated and the ablated regions. Hence, below the ablation threshold no changes were produced either in the surface (Fig. 5d) or in the subsurface (Fig. 5e). However, once the ablation threshold was surpassed, material was clearly ablated. Apart from evaporative ablation, which was the main material removal mechanism, topography of the valleys suggested that a slight melting was produced, as observed in Fig. 5b. A large number of cavities could be observed, presumably due to the Table 2 Sequences of the primers employed. Primer Sequence (5′-3′) RUNX2 F AAATGCCTCCGCTGTTATGAA R GCTCCGGCCCACAAATCT ALP F ATCTTTGGTCTGGCTCCCATG R TTTCCCGTTCACCGTCCAC COL-1 F AGGTCCCCCTGGAAAGAA R AATCCTCGAGCACCCTGA OSX F TGCTTGAGGAGGAAGTTCAC R AGGTCACTGCCCACAGAGTA J. Minguela et al.
! ! Materials Science & Engineering C 125 (2021) 112096 7 occurrence of localized boiling, creating an intricate nano-topography. Although most of the pores seemed to be connected to the surface, STEM images revealed some pores below the surface, always in the first 500 nm of material (Fig. 5c). Nano-cracks originated on this layer as well, as a result of the high temperature gradients after material resolidification. Stress-induced t → m phase transformation can take place around cracks in the laser-affected layer of Y-TZP [46]. In fact, it was observed that a subtle t → m phase transformation took place in both 3L and 10L after laser modification, where traces of the m-phase remained lower than V m =3% (and above the detection limits of the equipment V m > 1%). No other changes were detected after laser modification. The corresponding XRD spectra of the 2θ region between 26◦and 37◦is presented in Fig. 6a. Although the m-phase content found was low, the superficial nucleation of m-phase coupled to the presence of small cracks may affect hydrothermal degradation resistance of Y-TZP surfaces. For this reason, accelerated degradation tests were carried out in water steam [32,80]. Degradation kinetics of CTRL, 3L and 10L surfaces are displayed in Fig. 6b. In order to revert the detrimental consequences of m-phase after laser patterning and to relief possible residual stresses, a thermal treatment can be applied. As an example, 10L specimens were selected and heated up to 1200 ◦C for 1 h with a cooling and heating rate of 5 ◦C/min. These specimens were labeled as 10L-TT and included in the degradation experiment. It can be noticed that both 3L and 10L behaved worse than the CTRL specimens, displaying an earlier increase in the m-phase content. As explained, the nano-cracks, through which water can easily penetrate the material, coupled with a pre-existing amount of m-phase and the increase in surface area after laser treatment, may explain such performance. However, the thermal treatment (TT) reverted the negative consequences of the laser modification, and even improved significantly the behavior respect to CTRL specimens. The recovery of properties after the TT is explained by the total reversion m → t of the m-phase traces and the release of residual stresses [32,94]. However, the increase in the resistance respect CTRL specimens is more difficult to rationalize, and may be explained by the changes in nano-topography of the surface. The size of the protrusions originated on the valleys in 10L samples (see Fig. 5b) are below the average grain size (300 nm). This may have the same effect as reducing the grain size of the first layer of grains, which could hinder m-phase nucleation [95]. As shown in the image included in Fig. 6b, after the laser treatment the surface changed its color into a reddish/brownish one. Many other authors have already reported the color change in zirconia after laser modification [38,46,51,96], which is generally associated with the formation of color centers [46,96]. As it can be observed on the image, the whitish color was recovered after the thermal treatment. Fig. 6c plots the residual stresses found in 10L and CTRL specimens. The presence of residual stresses due to the thermal effects of the laser can influence mechanical properties and LTD [97]. The laser treatment Fig. 3. From left to right: 3D reconstruction of the micro-patterned surfaces and roughness profiles. P and D indicate pattern periodicity and depth, respectively. J. Minguela et al.
! ! Materials Science & Engineering C 125 (2021) 112096 8 introduced slightly tensile stresses along the pattern and slightly compressive ones perpendicularly, as compared to CTRL. Compressive stresses can stabilize the t-phase and delay LTD. In this case, the values found were relatively low, of similar magnitude to those that can be found on mildly polished surfaces [75]. On the other hand, tensile stresses can facilitate the degradation process [31]. Their relative impact on the LTD behavior of the surface is complex and depends on several factors, including stabilizer content, grain size, alumina content, etc. However, the tensile stresses obtained lie below the limit recommended to avoid LTD ( σ <300 MPa) [98]. In the light of the obtained results, a thermal treatment (TT) should be carried out after laser patterning. The main benefits are listed below: - Although LTD degradation cannot be totally hindered in 3Y-TZP, these materials are designed to delay its detrimental effects beyond the expected lifespan of the prostheses. An earlier degradation increases the probabilities of a premature mechanical failure. As shown, LTD resistance can be worsened after laser patterning, but a TT can effectively revert its negative consequences. - From the aesthetic point of view, preserving the surface color of the prostheses is of particular interest for the final application. One of the advantages of using zirconia instead of titanium lies in its whitish and more natural appearance. Laser patterning changes the surface color, but this process can be reverted after a TT. - Residual stresses can affect LTD. In particular, tensile stresses can worsen the degradation resistance. A TT can relieve the residual stresses introduced by the laser patterning process [31]. 3.2. Surface functionalization In order to improve the biological effects of the surface patterns, specimens were biofunctionalized with a dual platform combining a well-known cell-adhesive peptide (RGD) and an osteoinductive peptide (DWIVA). The presence of the peptides after functionalization was determined by different methods. Fig. 7a shows the images obtained by fluorescence CLSM of the surfaces after functionalizing with a fluorescent version of the platform. All the functionalized samples presented a certain degree of fluorescence, with a higher intensity in the laser treated specimens as compared to the flat CTRL-P. The peptide was detached from these surfaces with NaOH and the fluorescence of the supernatant measured and compared to a standard curve relating fluorescence intensity against platform concentration. Fig. 7b plots the obtained peptide concentration on the surface of the samples. Similar to Fig. 7a, the presence of the platform was confirmed in the functionalized specimens and a higher amount was found in the laser-modified surfaces, with 10L presenting the highest content. Finally, the surface chemical composition of the functionalized specimens was studied by XPS (non-fluorescent platform). Fig. 7c shows the atomic percentage of nitrogen (N1s signal) on the surface (as compared to the total content of Zr, Y and O), which is directly related to the presence of peptide bonds and amino acid side chains of the peptidic backbone. Results were in agreement with the trend obtained in the quantification experiment (Fig. 7b). All the functionalized samples displayed a clear increase in the nitrogen content, which was maximum in the laser-patterned samples. These experiments clearly showed that the anchoring molecule used in the peptidic platform was effective in attaching the biomolecule to the Fig. 4. FESEM micrographs of the studied surfaces of a) CTRL, b) 3L and c) 10L specimens. Black particles in CTRL specimens correspond to Al 2 O 3 inclusions present in the Y-TZP feedstock. J. Minguela et al.
! ! Materials Science & Engineering C 125 (2021) 112096 9 surface of zirconia. L-DOPA is one of the main components of the adhesive proteins employed by marine mussels to anchor surfaces in seawater [99]. It can strongly bind to both organic and inorganic substrates [100] and its properties have been exploited, among other applications, to coat biomedical surfaces including zirconia [74,101]. The higher surface concentration of the platform observed in the lasermodified specimens can be explained by the increase in surface area, which was due not only to the grooves but also to the nano-topographies observed on the bottom of the valleys. In this regard, while the primary pattern (i.e. the grooves) increased the surface area in both 3L and 10L by a factor close to 1.6 with respect to a flat surface (Wenzel’s roughness factor for a rectangular profile), the nanotopography in 10L presented more intricate features (see Fig. 4), further increasing surface area as compared to 3L. Accordingly, the highest values of peptide attachment were found in 10L. The presence of peptides entrapped inside the nanotopographies (nano-pores) cannot be discarded and may have also increased the values obtained during the peptide quantification. 3.3. Cell response on the patterned/biofunctionalized surfaces 3.3.1. Cell-adhesion Fig. 8 presents the results obtained in the cell-adhesion assay, evaluating cell morphology 6 h after cell seeding. The behavior observed was determined by the combined effects of the two modifications studied: surface patterns and the biomolecule. The effects of laser patterning on cell morphology were studied by comparing CTRL, 3L and 10L. As shown in Fig. 8a, cells cultured on the patterned surfaces underwent a drastic shape change. Cell body stretched along the grooves and thinned in the perpendicular direction, displaying a large increase in aspect ratio (Fig. 8e), as compared to the round-shaped cells growing in CTRL. Apart from the morphological changes, the most evident effect of laser patterns was the alignment of cells along the grooves, with more than 90% of the cells aligned at ±15◦ of the pattern direction in both 3L and 10L (Fig. 8f). Regarding cell number, no significant differences were found (Fig. 8b). In summary, topography greatly affected cell morphology due to a significant contact guidance. FESEM micrographs of both 3L and 10L are shown in Fig. 9c to f. The alignment effect is obvious on the images. A cell body extension growing on a ridge can be observed in Fig. 9e. Cells could also establish contact with the nano-topography, as evidenced in Fig. 9f, where filopodia extending from the cell body (right part of the image) anchored to the lateral side of a valley (left part of the image). On the other hand, the effects of the biomolecule were also studied, as well as its combination with surface patterns. In the case of flat specimens, CTRL-P displayed important differences with respect to its non-functionalized equivalent, CTRL. When free of the biochemical stimuli of the peptides, CTRL specimens displayed relatively small, starshape cell bodies, with evident cell projections (see magnification attached to Fig. 8a CTRL and Fig. 9a). On such surfaces, non-specific cell-material interactions were expected, with an establishment of weak bonds based on electrostatic interactions, hydrogen bonding, etc. Under such conditions, a poorly developed cell cytoskeleton and a reduced cell area were observed. In contrast, biofunctionalized surfaces displayed a two-fold increase in surface area (Fig. 8d), with polygonal cell bodies displaying well-developed bundles of actin filaments (see magnification attached to Fig. 8a CTRL-P and Fig. 9b). In the latter condition, due to the cell-adhesion properties of the biomolecule employed, a higher number of cells attached to the surface (Fig. 8b). This improvement in the number of cells on the functionalized specimens is in well agreement with the literature [56,64,70] and was corroborated by an adhesion assay with Alamar Blue. Following an incubation time of 24 h after cell seeding, the functionalized specimen presented a higher number of adhered cells, as shown in Fig. 8c. In contrast to flat specimens, the combination of the peptidic Fig. 5. Surface features of 10L specimens. a) General micrograph view of 10L surface, b) magnification of the valley nano-topography with the presence of nanopores and nano-cracks, c) STEM micrograph of the valley subsurface, d) magnification of the top of the grooves where no signs of surface modification are observed and e) STEM micrograph of the subsurface in the top of the grooves. J. Minguela et al.
! ! Materials Science & Engineering C 125 (2021) 112096 10 Fig. 6. Results of the XRD experiments. a) XRD spectra of the studied specimens. Just minor changes were observed with small traces of m-phase in the laser treated specimens. In the magnification below, x/y axis relation has been modified to clearly show the presence of m-phase traces. b) Degradation kinetics in water steam. The increase in m-phase content is plotted against degradation time. A picture depicting the recovery of the white color of 10L after thermal treatment is included. c) Residual surface stresses in 10L and CTRL specimens measured by XRD. In 10L, 0◦correspond to a direction parallel to the grooves. Positive and negative values correspond to tensile and compressive stresses respectively. Fig. 7. Characterization of the presence of peptides on the surfaces. a) Fluorescence CLSM of the specimens functionalized with the fluorescently-labeled peptidic platforms. b) Results of the peptide quantification by detachment of the fluorescently-labeled peptidic platforms. c) Atomic percentage of nitrogen (N1s signal) on the surfaces (non-fluorescent platform was used). J. Minguela et al.
! ! Materials Science & Engineering C 125 (2021) 112096 11 platform with the laser-patterned surfaces did not display such drastic differences. Cell morphology of non-functionalized 3L and 10L specimens did not differ significantly from that exhibited by the functionalized versions 3L-P and 10L-P, in both cases presenting an elongated spindle-shape. In this case, the effect of the topography prevailed markedly over the biochemical cues. As expected, although standard deviation was high, the main trend showed higher cell number in all functionalized specimens as compared to their non-functionalized equivalents (Fig. 8b and c). As in CTRL specimens, but to a lower extent, the effect of RGD resulted in a higher cell area (Fig. 8d). In this case, a lower degree of thinning perpendicularly to the grooves was observed, as compared to 3L and 10L. This translated into a lower aspect ratio, which still was much higher respect to CTRL and CTRL-P (Fig. 8e). In terms of cell alignment, the peptidic platform did not introduce significant changes, displaying both 3L-P and 10L-P an alignment degree around 90% (Fig. 8f). Overall, laser pattering mainly affected cell-shape and alignment, without significant changes in cell number. Once the surfaces were biofunctionalized, large changes were observed in flat CTRL specimens, mainly in terms of a higher cell body area and a well-developed cell cytoskeleton. In laser-patterned surfaces such changes were reduced. No differences in cytoskeleton organization or alignment were observed Fig. 8. hMSCs adhesion results after 6 h in serum free medium. a) Representative images of the studied specimens under fluorescence CLSM. Actin filaments were stained with TRITC-conjugated phalloidin (red), and cell nuclei with DAPI (blue). b) Cellular adhesion (cells/cm 2 ), c) cellular adhesion by the AlamarBlue assay 24 h after cell seeding (cells/cm 2 ), d) cell area ( μ m 2 ), e) cell aspect ratio and f) cell alignment (%). Cell alignment was defined as the percentage of cells aligned along a direction ±15◦respect to the pattern direction. Red bars correspond to the non-functionalized specimens while blue bars represent specimens functionalized with the peptidic platform. * indicates statistical differences between functionalized and non-functionalized specimens with the same topography (e.g. 10L vs. 10L-P). # indicates statistical differences between 10L or 3L with respect to CTRL, analyzing only the effect of topography, without functionalization (p <0.05). (For interpretation of the references to color in this figure legend, the reader is referred to the web version of this article.) J. Minguela et al.
! ! Chapter!7! Main!conclusions! and!relevance!of! the!findings
Main'conclusions'and'relevance'of'the'findings' ! 127! 7!Main!conclusions!and!relevance!of!the!findings! ! The!main!conclusions!of!the!work!gathered!in!this!thesis!will!be!summarized!and! discussed!below,!highlighting!the!relevance!of!the!most!remarkable!findings.! ! Grinding/polishing' ' Grinding/polishing!procedures! not! only! affect! surface! roughness,! but! also! microstructure!and!phase!composition!of!3Y-TZP.!The!stresses!generated!by!the! abrading! particles! trigger! the! m-phase! transformation.! In! turn,! the! expansive! nature! of! this! phase! transformation! generates! a! residual! compressive! surface! layer.!In!the!light!of!the!results!obtained,!surface!roughness,!monoclinic!volume! fraction!(Vm)!and!the!value!of!residual!stresses!can!be!mathematically!related.! This!observation!is!not!trivial.!If!the!manufacturing!conditions!of!zirconia!parts! are!controlled,!the!residual!stress!state!and!m-phase!content!of!the!ground!parts! can! be! deduced! by! using! a! simple! profilometer.! This! procedure! is! relatively! cheap,!simple,!readily!available!and!fast,!and!avoids!the!use!of!more!expensive! and!complex!equipment,!such!as!X-ray!diffractometers!or!Raman!spectrometers.!! ! On!the!other!hand,!severe!microstructural!changes!are!found!on!the!surface!of! ground! and! polished! specimens.! The! main! changes! are! due! to! surface! grain! recrystallization.!Although!it!is!a!phenomenon!that!has!been!previously!reported! in!this!material,!the!work!conducted!along!this!Ph.D.!Thesis!demonstrates!that! recrystallization!takes!place!in!a!wide!range!of!grinding/polishing!procedures,! and!not!only!on!coarsely!ground!surfaces.!Even!after!relatively!mild!procedures,! surface! recrystallization! can! be! observed.! In! this! regard,! the! transition! from! bulk-like! to! recrystallized! surfaces! was! identified! in! polished! surfaces! with! a! roughness! as! low! as! Sa! =! 16! ±! 1! nm,! in! which! partial! recrystallization! was! observed.! The! consequences! of! these! findings! are! very! important.! LTD! experiments! showed! that! mildly! polished! surfaces! can! present! excellent! protective! features.! Surfaces! with! low! roughness! (Sa!<! 50! nm)! had! the! same! protective!properties!as!ground!specimens,!showing!an!excellent!resistance!even! after!50!hours!in!water!steam!(equivalent!to!more!than!150!years!in)vivo).!In!this!
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 128! regard,! even! the! specimens! polished! to! a! Sa! =! 16! nm! displayed! a! significant! degree!of!protection!respect!to!mirror-like!polished!specimens!(Sa!=!5!nm).!After! 20! hours! in! water! steam! (equivalent! to! 60! years! in) vivo)! they! presented! a! monoclinic!content!of!Vm!<!10!%,!while!mirror-like!polished!surfaces!presented! already! a! severely! degraded! surface! with! Vm! =! 60! %.! These! results! must! be! highlighted,!as!most!of!the!literature!available!has!overlooked!such!effects.!! ! As!also!reported!previously!by!other!authors,!if!too!coarse!grinding!is!employed,! the!resistance!to!LTD!can!be!worsened.!Although!other!works!have!related!the! worsening! of! properties! to! surface! damage,! no! evidences! were! given! on! this! relation.! In! the! present! Ph.D.! Thesis,! a! clear! relation! is! found! between! degradation! of! the! surface! and! damage! in! the! form! of! flakes,! which! were! associated!to!subsurface!micro-cracks.!! ! From!these!observations,!it!can!be!concluded!that!3Y-TZP!is!highly!susceptible!to! changes!after!surface!mechanical!treatments.!A!special!emphasis!must!be!placed! on!this!sentence,!as!small!changes!on!the!surface!can!have!catastrophic!effects!on! the! performance! of! 3Y-TZP!final! parts.! Recent! history! of! zirconia! has! sadly! evidenced!this!fact.! ! Finally,! regarding! mechanical! properties,! the! layer! of! residual! compressive! stresses!generated!after!grinding!can!improve!contact!damage!properties.! ! Laser'patterning' ' DLIP! technique! can! be! employed! to! micro-pattern! ceramic! materials! in! the! femtosecond! pulse! regime,! such! as! 3Y-TZP.! Although! one! recent! work! has! employed! this! technique! and! this! time! regime! successfully! (with! a! five-fold! longer!pulse!duration),!it!is!the!first!time!that!such!a!good!pattern!definition!is! achieved,!and!that!grooves!with!a!periodicity!as!low!as!3!μm!are!ablated.!The! results! obtained! in! this! Ph.D.! thesis! also! highlight! the! potential! industrial! application!of!this!technique,!which!allows!creating!homogeneous!and!defined!
Main'conclusions'and'relevance'of'the'findings' ! 129! features! of! only! a! few! microns! in! 3Y-TZP! materials.! No! other! technique! with! equivalent!processing!speed!has!yet!achieved!these!results.! ! The!effects!in!the!subsurface!of!DLIP!laser-patterned!3Y-TZP!in!the!nanosecond! regime! have! been! recently! studied.! However,! no! clues! on! the! effects! in! the! femtosecond! regime! existed! until! now.! In! contrast! to! the! nanosecond! time! regime,!where!extensive!melting!of!the!surface!is!produced,!the!material!removal! mechanism! in! the! femtosecond! regime! is! mainly! governed! by! ablation.! While! material!in!the!top!of!the!peaks!remains!unaltered,!material!on!the!bottom!of!the! valleys!is! ablated,! producing! a! stochastic!grainy! nano-topography.! Surface! damage!in!the!form!of!nano-cracks!and!nano-pores!can!be!found!on!the!valleys,! but!limited!to!a!layer!of!500!nm!below!the!surface.!Just!traces!of!m-!phase!can!be! detected!after!these!procedures!and!very!low!residual!stresses!are!generated,!in! the!range!of!the!ones!found!in!mirror-like!polished!specimens.!LTD!is!slightly! worsened,!but!after!a!thermal!treatment!it!can!be!reverted,!even!improving!the! LTD!resistance!of!the!base!material.! ! Femtosecond!regime!DLIP!shows!a! clear! potential! to! be!employed!in!creating! micro-! and! nano-topographies! on! biomedical! surfaces,! where! surface! damage! must!be!reduced!and!features!of!only!a!few!micrometers!are!required.! ! Biological'effects'of'the'topographies'and'surface'functionalization' ! Grooved!topographies!have!been!obtained!by!two!methods:!grinding/polishing! and!laser!micro-patterning.!None!of!the!surfaces!showed!a!significant!increase!in! cell! attachment,! although! when! the! grooves! were! parallel,! contact! guidance! could! be! observed.! In! the! case! of! ground/polished!surfaces,! this! was! only! observed!in!surfaces!above!a!certain!roughness!threshold!(Sa)>!150!nm)!and!just! in!the!smaller!SaOS-2,!but!not!in!the!larger!MSCs.!The!roughness!degree!that!can! be!achieved!by!grinding!without!producing!excessive!surface!damage!is!limited.! Thus,!the!topographical!features!obtained!with!this!method!may!not!be!enough! to! efficiently! guide! the! growth! of! larger! cells.! This! problem! can! be! solved! by!
!Surface'characterization'and'cell'instructive'properties'of'superficially'modified'dental'zirconia'' ! 130! producing!the!grooves!by! laser!micro-patterning,!where!the!cost!of!producing! deeper!features!is!less!detrimental!in!terms!of!surface!damage.! ! Laser! grooved! surfaces! can! guide! cellular! growth,! inducing! cell! alignment,! elongation!and!cell!migration!along!the!pattern.!In!the!perpendicular!direction,! however,!migration!is!limited.!This!effect!has!been!already!used!in)vivo)in!dog! models! where! micro-textured! collars! showed! reduced! epithelial! downgrowth! and!greater!bone!attachment.! ! Regarding! the! peptidic! platform! employed,! the! L-DOPA-based! anchoring! molecule! can! successfully! attach! to! 3Y-TZP.! The! effects! from! the! dual! RGDDWIVA! platform! are! kept! once! the! molecule! attaches! to! the! surface.! Functionalized! surfaces! present! more! cells,! better! spread! and! with! welldeveloped!cytoskeletons.!The!molecule!introduces!osteogenic!properties!to!the! surfaces! by! upregulating! several! osteogenesis-related! genes.! Importantly,! the! effects!derived!from!the!topography!are!not!masked!by!the!biomolecule,!and!are! also! kept! in! functionalized! specimens.! Thus,! by! combining! the! laser! micropatterns! and! the! peptidic! platform! cell! growth! can! be! guided,! and! improved! adhesion!and!osteogenic!cues!are!provided.! ! The!combination!of!surface!topography!and!biofunctionalization!carried!out!in! this!Ph.D.!Thesis!show!that!the!effects!from!both!strategies!are!compatible!and! can!be!combined! to! tailor!the!surface!properties.! Of!note,!such!dual!approach! was!never!investigated!before!on!3Y-TZP.!!By!studying!other!topographies!and! employing! other! peptides,! more! properties! can! be! introduced! to! 3Y-TZP! surfaces,!depending!on!the!specific!application.!This!dual!functionalization!can! thus! become! a! powerful! tool! to! improve! the! tissue! integration! and! healing! success!of!3Y-TZP!dental!implants.! !
! ! References
References'' ! 133! ! [1]!R.B.! Heimann,! H.D.! Lehmann,! Bioceramics! –! A! Historical! Perspective,! in:! Bioceram.! Coatings!Med.!Implant.,!Wiley,!2015:!pp.!1–10.! [2]!R.H.J.!Hannink,!P.M.!Kelly,!B.C.!Muddle,!Transformation!toughening!in!zirconia-containing! ceramics,!J.!Am.!Ceram.!Soc.!83!(2000)!461–487.! [3]!O.! Ruff,! F.! Ebert,! Beiträge! zur! Keramik! hochfeuerfester! Stoffe.!l.! Die! Formen! des! Zirkondioxyds,!Zeitschrift!Für!Anorg.!Und!Allg.!Chemie!180!(1929)!19–41.! [4]!O.!Ruff,!F.!Ebert,!E.!Stephan,!Beiträge!zur!Keramik!hochfeuerfester!Stoffe!II.!Das!System! ZrO2-CaO,!Zeitschrift!Für!Anorg.!Und!Allg.!Chemie!180!(1929)!215–224.! [5]!R.C.!Garvie,!R.H.!Hannink,!R.T.!Pascoe,!Ceramic!steel?,!Nature!258!(1975)!703–704.! [6]!I.! Nettleship,! R.! Stevens,! Tetragonal! zirconia! polycrystal! (TZP)-A! review,! Int.! J.! High! Technol.!Ceram.!3!(1987)!1–32.! [7]!P.H.!Rieth,!J.S.!Reed,!A.W.!Naumann,!Fabrication!and!flexural!strength!of!ultrafine-!grained! yttria-stabilized!zirconia,!Am.!Ceram.!Soc.!Bull!55!(1976)!717–721.! [8]!T.K.!Gupta,!J.H.!Bechtold,!R.C.!Kuznicki,!L.H.!Cadoff,!B.R.!Rossing,!Stabilization!of!tetragonal! phase!in!polycrystalline!zirconia,!J.!Mater.!Sci.!12!(1977)!2421–2426.! [9]!S.!Ban,!Reliability!and!properties!of!core!materials!for!all-ceramic!dental!restorations,!Jpn.! Dent.!Sci.!Rev.!44!(2008)!3–21.! [10]!J.R.!Kelly,!I.!Denry,!Stabilized!zirconia!as!a!structural!ceramic:!An!overview,!Dent.!Mater.! 24!(2008)!289–298.! [11]!J.!Chevalier,!L.!Gremillard,!Ceramics!for!medical!applications:!A!picture!for!the!next!20! years,!J.!Eur.!Ceram.!Soc.!29!(2009)!1245–1255.! [12]!I.!Birkby,!R.!Stevens,!Applications!of!Zirconia!Ceramics,!Key!Eng.!Mater.!122–124!(1996)! 527–552.! [13]!C.!Piconi,!G.!Maccauro,!F.!Muratori,!E.!Brach!Del!Prever,!Alumina!and!zirconia!ceramics!in! joint!replacements.,!J.!Appl.!Biomater.!Biomech.!1!(2003)!19–32.! [14]!M.! Peters,! B.! Saruhan-Brings,! U.! Schulz,! Advanced! Coatings! for! Blades! of! Future! Aero! Engines,!in:!Proc.!CEAS!2009!Eur.!Air!Sp.!Conf.,!Manchester,!UK,!2009:!pp.!1–9.! [15]!J.E.! Shigley,! A.! Gilbertson,! S.! Eaton-Magaña,! Characterization! of! colorless! coated! cubic! zirconia!(Diamantine),!Gems!Gemol.!48!(2012)!18–30.! [16]!S.! Shukla,! S.!Seal,! Mechanisms! of! room! temperature! metastable! tetragonal! phase! stabilisation!in!zirconia,!Int.!Mater.!Rev.!50!(2005)!45–64.! [17]!University! of! Cambridge,! DoITPoMS! TLP! Library.! Available! at:https://www.doitpoms.ac.uk/tlplib/fuel-cells/sofc_electrolyte.php! (accessed! November!24,!2020).! [18]!J.! Chevalier,! L.! Gremillard,! A.! V.! Virkar,! D.R.! Clarke,! The! tetragonal-monoclinic! transformation! in! zirconia:! Lessons! learned! and! future! trends,! J.! Am.! Ceram.! Soc.! 92! (2009)!1901–1920.! [19]!F.F.! Lange,! Transformation! toughening! -! Part! 1! Size! effects! associated! with! the!