scieee AI-readable full text Open interactive document viewer

Influence of end groups in hyperbranched polyesters used as modifiers in the characteristics of epoxy thermosets cured by adipic dihydrazide

Tomuta, Adrian Marius,Ramis Juan, Xavier,Flor López, Sílvia de la,Serra Albet, Maria Àngels

Abstract

Mixtures of diglycidylether of bisphenol A (DGEBA) resin and different ratios of aliphatic-aromatic hyperbranched polyester (HBP) were cured by a latent curing agent, adipic dihydrazide (AH). The HBPs prepared have hydroxyl groups or 10-undecenoyl or allyl groups as chain ends. The curing mixtures were investigated by differential scanning calorimetry (DSC) to study the curing process and to evaluate the kinetic parameters of the different formulations. These studies suggest that HBPs decrease the curing rate of epoxy/AH in the case of vinyl terminated HPB, whereas OH terminated HBP accelerates the first stages and delays the lasts. The thermosets obtained showed an improvement in microhardness and impact strength without any reduction of the Tg and thermal parameters. Microparticle phase separation was observed with the undecenoyl HBP derivatives or when a 10% of allyl HBP derivative was in the formulation.

Full text

1. Introduction Epoxy resins are widely used in several applications: adhesives, coatings, castings, electric laminates, encapsulation of semiconductor devices, matrix materials for composites, structural components and engineering [1, 2], because of their good characteristics such as adhesion and chemical resistance. However, due to their high cross-link density they are inherently brittle, which limits their applicability. With the aim to increase their toughness different types of modifiers have been added to epoxy formulations such as rubber, thermoplastic and core-shell particles. The addition of liquid rubbers and thermoplastics was one of the first attempts to improve toughness, but usually this method has a detrimental effect on the thermomechanical characteristics of the thermosets and the processability of the formulation [3], which is a drawback for coatings applications [4, 5]. To solve the limitations related to processability, hyperbranched polymers (HBPs) were introduced as toughness modifiers [6–8]. The advantage is that their highly branched structure prevents entanglement, reducing the viscosity of the formulation in comparison to the use of their linear analogues. Moreover, the great number of terminal groups has a significant effect on the reactivity, can increase the compatibility with the resin and helps to maintain thermomechanical characteristics [9, 10]. Based on their unique properties, HBPs have been applied not only as tougheners for ther- 595 Influence of end groups in hyperbranched polyesters used as modifiers in the characteristics of epoxy thermosets cured by adipic dihydrazide A. M. Tomuta1, X. Ramis2, S. de la Flor3, A. Serra1* 1Department of Analytical and Organic Chemistry, Universitat Rovira i Virgili, C/Marcel!lí Domingo s/n, 43007 Tarragona, Spain 2Laboratory of Thermodynamics, ETSEIB, Universitat Politècnica de Catalunya, Diagonal 647, 08028 Barcelona, Spain 3Department of Mechanical Engineering, Universitat Rovira i Virgili, C/ Països Catalans 26, 43007 Tarragona, Spain Received 24 January 2013; accepted in revised form 27 March 2013 Abstract. Mixtures of diglycidylether of bisphenol A (DGEBA) resin and different ratios of aliphatic-aromatic hyperbranched polyester (HBP) were cured by a latent curing agent, adipic dihydrazide (AH). The HBPs prepared have hydroxyl groups or 10-undecenoyl or allyl groups as chain ends. The curing mixtures were investigated by differential scanning calorimetry (DSC) to study the curing process and to evaluate the kinetic parameters of the different formulations. These studies suggest that HBPs decrease the curing rate of epoxy/AH in the case of vinyl terminated HPB, whereas OH terminated HBP accelerates the first stages and delays the lasts. The thermosets obtained showed an improvement in microhardness and impact strength without any reduction of the Tgand thermal parameters. Microparticle phase separation was observed with the undecenoyl HBP derivatives or when a 10% of allyl HBP derivative was in the formulation. Keywords: thermosetting resins, toughness, hyperbranched polymers, latency, dihydrazides eXPRESS Polymer Letters Vol.7, No.7 (2013) 595–606 Available online at www.expresspolymlett.com DOI: 10.3144/expresspolymlett.2013.57 *Corresponding author, e-mail: [email protected] © BME-PT mosets but also in cross-linking or adhesive agents [11], compatibilizers [12], dispersers [13], processing aids, and rheology modifiers [14, 15]. One of the most effective methods of inhibiting crack growth after impact is the addition of a second phase that induces the formation of particles that absorb the impact energy and deflect the crack [5]. Usually, the particles are generated from a homogeneous solution composed of the resin, curing agent and modifiers, which on curing causes a reactioninduced phase separation (RIPS) to take place. The phase separated morphology is highly dependent on the kinetics of curing and on the dynamics of the phase separation process. The synthesis and characterization of aromaticaliphatic hyperbranched polyesters modified with long and short vinylic chains and their use as modifiers of DGEBA thermosets cured with hexahydro- 4-methylphthalic anhydride was reported by us [16]. The addition of these modifiers led to significantly increased rates of cure. However, the materials obtained were homogeneous and the increase in impact strength was only modest. In addition, the HBPs led to a plasticization and to a considerable decrease in the Tg. In a previous paper we demonstrated the latent character of a series of dihydrazides in the thermal curing of DGEBA [17]. Several dihydrazides were synthesized and used as stoichiometric curing agents of epoxy resins. From the dihydrazides synthesized, AH was the one that leads to curing at the lowest temperature (maximum of the curing exotherm at 165°C) and led to materials with good characteristics. However, dihydrazides possess a high crystalline character and they are difficult to disperse or dissolve, because on melting (at 181–184°C) the curing process is extremely fast. In the present work, the influence of the addition of aromatic-aliphatic hyperbranched polyesters modified with long and short vinylic chains (see Figure 1) to the epoxy formulation has been studied with two different aims: to increase toughness and help to disperse AH in the DGEBA resin. In addition, it was expected from the fast curing process caused by the dihydrazides at the appropriate temperature that could induce phase separated morphologies, when the HBP structure cannot be covalently incorporated to the epoxy matrix, because of its solubility and the end group characteristics. Tomuta et al. – eXPRESS Polymer Letters Vol.7, No.7 (2013) 595–606 596 Figure 1. Structure of the HBP modifiers added to the formulations 2. Experimental 2.1. Materials 4,4-Bis(4-hydroxyphenyl) valeric acid, N,N"-dicy- clohexylcarbodiimide (DCC), triethyl amine, allyl bromide, 10-undecenoyl chloride, diethyl adipate and hydrazine hydrate were purchased from Sigma Aldrich (St. Louis, MO, USA) and used without further purification. Diglycidyl ether of Bisphenol A (DGEBA) Epikote Resin 828 was provided by Momentive Speciality Chemicals Inc. (Barbastro, Spain) with an epoxy equivalent of 184 g/eq and was dried in vacuum before use. All the organic solvents were purchased from Scharlab and purified by standard procedures. 4-(N,N-dimethylamino) pyridinium p-toluenesulfonate (DPTS) was prepared as described in the literature [18]. 2.2. Synthesis of adipic dihydrazide (AH) 50.5 g (0.25 mol) of the diethyl adipate were dissolved in 200 mL of absolute ethanol and 0.9 mol of hydrazine hydrate (90%) were added drop by drop. Once the addition was complete the heating was turned on and the mixture was kept 6 h at reflux. During this time a white precipitate was formed, which was filtered through a Buchner funnel and then washed twice with cold ethanol. The white powder was dried in the vacuum oven at 50°C. The obtained yield was higher than 90%. m.p. 181–4°C (recrystallized from ethanol). 1HNMR (DMSO-d6, # in ppm): 8.93 s (2H, –NH–); 4.14 s (4H, –NH2); 1.97 t (4H, –CH2–) 1.41 m (4H, –CH2–); 13C NMR (DMSO-d6, # in ppm): 171.49 (–CONH–); 33.27 (–CH2–); 24.99 (–CH2–). FTIR-ATR (cm–1): 3310, 3288, 3197, 1626, 1529, 1376, 1273, 1166, 1033, 690. 2.3. Hyperbranched polyester synthesis (HBP-OH) The HBP-OH (Figure 1) was synthesized according to a previously described procedure [19] from 4,4- bis(4-hydroxyphenyl) valeric acid as AB2 monomer. The 1H and 13CNMR data are in accordance with those published [20]. Mn: 8700 g/mol, Mw: 12300 g/mol. Tg121°C (by DSC). The amount of hydroxyl groups was determined according to ISO 2554-1974 standards. The number of hydroxyl groups per molecule found by titration was 36 [16]. 2.4. Derivatization of HBP-OH with 10-undecenoyl chain ends (HBP-Und) The derivatization was done from HBP-OH (Figure 1) synthesized previously by reacting with 10- undecenoyl chloride in the presence of triethylamine, as previously described [16]. The product was dried in a vacuum oven at 50°C overnight and a pale brown viscous liquid was obtained. Yield: 94% Tg18°C (by DSC). 1HNMR (400 MHz, CDCl3), # (ppm): 1.26 m (–CH2–); 1.41 m (–CH3); 1.68 m (–CH2–); 2.06 m (–CH2–); 2.34 m (–CH2–); 2.55 m (–CH2–); 5.10 dd (CH2=); 5.87 m (=CH–); 7.11 m (CH Ar). 13CNMR (100.6 MHz, CDCl3), # (ppm): 24.7 (–CH2–); 27.6 (–CH2–); 28.9 (–CH2–); 33.6 (–CH2–); 34.3 (–CH2–) 36.2 (–CH2–); 45.4 (=C=);113.9 (CH2=); 121.2 (Ar) ; 128.2 (Ar); 139.0 (=CH–); 145.6 (Ar); 148.6 (Ar);172.3 (C=O). 2.5. Derivatization of HBP-OH with allyl chain ends (HBP-Allyl) The derivatization was performed by nucleophylic substitution on allyl bromide by the phenolate end groups, formed by treating HBP-OH (Figure 1) with K2CO3in a mixture of THF and acetone, as previously reported [16]. HBP-Allyl was obtained by precipitating the THF solution on water. The polymer was dried in a vacuum oven at 50°C overnight and a white powder was obtained. Yield: 90%. Tg 81°C (by DSC). 1HNMR (400 MHz, CDCl3), # (ppm): 1.65 s (–CH3–); 2.36 m (–CH2–); 2.53 (–CH2–); 4.53 s (–CH2–); 5.35 dd (CH2=); 6.07 m (=CH–); 6.8–7.2 m (CH Ar). 13CNMR (100.6 MHz, CDCl3), # (ppm): 28.0 (–CH2–); 30.6 (–CH2); 36.6 (–CH2–); 45.1 (=C=); 68.9 (–CH2–); 114.3 (Ar); 117,9 (CH2=) ; 128.4 (Ar); 133.5 (=CH–); 141.2 (Ar); 156.9 (Ar); 172.5 (C=O). 2.6. Preparation of the curing mixtures The neat DGEBA/AH formulation was prepared by adding the stoichiometric amounts of each reactant to a mortar and homogenizing them by mechanical mixing while heating at 90°C. For the preparation of the formulations with the HBP modifiers, first of all the corresponding proportion was dissolved in DGEBA by adding a little amount of THF. The sol- Tomuta et al. – eXPRESS Polymer Letters Vol.7, No.7 (2013) 595–606 597 vent was then eliminated in vacuum at 50°C overnight and then the stoichiometric amount of AH was added and homogenized by mixing in a mortar while heating at 90°C. The proportions of HBPs added were a 5 and 10% w/w in reference to DGEBA. AH was added in a molar proportion to DGEBA of 1:2. 2.7. Measurements The 400 MHz 1HNMR and 100.6 MHz 13C NMR spectra were obtained with a Varian Gemini 400 spectrometer with Fourier Transformed (Palo Alto, California USA). 1HNMR spectra were acquired in 1min and 16 scans with a 1.0 s relaxation delay (D1). 13CNMR spectra were obtained using a D1 of 0.5 s and an acquisition time of 0.2 s. A total of 500 accumulations were recorded. CDCl3was used as a solvent and tetramethylsilane (TMS) as internal standard. Calorimetric analyses were carried out on a Mettler DSC-821e calorimeter (Greifensee, Switzerland). Samples of approximately 10 mg were cured in aluminium pans in a nitrogen atmosphere. Non-isother- mal experiments were performed from 0 to 225°C at heating rates of 2, 5, 10, and 15°C/min to determine the reaction heat and the kinetic parameters. In the non-isothermal curing process, the degree of conversion at a given temperature Twas calculated as the quotient between the heat released up to T and the total reaction heat associated with the complete conversion of all reactive groups. The precision of the given enthalpies is ±3%. The Tgs of the cured materials were determined with a second scan at 20°C/min after dynamic curing by the mid-point method and the error is estimated to be approximately ±1°C. The Tgs of the pure HBPs were determined by a similar procedure. Dynamic mechanical thermal analysis (DMTA) was carried out with a TA Instruments DMTA 2980 analyzer (New Castle, USA). The samples were cured isothermally in a mould at 190°C for 1 h and then post-cured for 0.5 h at 200°C. Before the samples were prepared, they were degassed in a vacuum oven at 50°C for 3 h. Single cantilever bending at 1Hz was performed at 3°C/min from 30 to 220°C on prismatic rectangular samples (1.5$20$5 mm3). Thermogravimetric analysis was carried out with a Mettler-Toledo TGA/SDTA 851e thermobalance (Greifensee, Switzerland). Cured samples with an approximate mass of 5 mg were heated from 30 to 800°C at a heating rate of 10°C/min in a nitrogen atmosphere. Impact tests were performed at room temperature by means of a Zwick 5110 impact tester (Altamonte Springs, USA) according to ASTM D 4508-05 using rectangular samples (25$12$2.5 mm3). The pendulum employed had a kinetic energy of 1 J. For each material, 9 determinations were made. The impact strength (IS) was calculated from the energy absorbed by the sample upon fracture according to Equation (1): (1) where Eand E0are the energy loss of the pendulum with and without sample respectively, and Sis the cross-section of the samples. The fracture area of impacted samples was metalized with gold and observed with a scanning electron microscope (SEM) Jeol JSM 6400 (Tokyo, Japan). The kinetic triplet (pre-exponential factor, activation energy, and the kinetic model) of the curing was determined using integral isoconversional nonisothermal kinetic analysis, Kissinger-Akahira- Sunose equation, combined with the Coats-Redfern procedure. Details of the kinetic methodology are given in previous studies [21]. Microhardness was measured with a Wilson Wolpert (Micro-Knoop 401MAV) device (Massachusetts, USA) following the ASTM D1474-98 (2008) standard procedure. For each material 10 determinations were made with a confidence level of 95%. The Knoop microhardness (HKN) was calculated from Equation (2): (2) where Lis the load applied to the indenter (0.025 kg), Ap is the projected area of indentation in mm2, lis the measured length of long diagonal of indentation in mm, and Cpis the indenter constant (7.028·10–2) relating l2to Ap. The values were obtained from 10 determinations with the calculated precision (95% of confidence level). HKN 5L Ap 5L l2Cp IS 5E2E0 S IS 5E2E0 S HKN 5L Ap 5L l2Cp Tomuta et al. – eXPRESS Polymer Letters Vol.7, No.7 (2013) 595–606 598 3. Results and discussion 3.1. Calorimetric study of the curing process and the thermosets obtained In the preparation of epoxy thermosets, the selection of the curing agent is crucial to obtaining good thermoset properties but especially when a HBP modifier is added to the formulation, because of the role played by the chemistry of the curing agent in the possible reaction of the terminal groups in the HBP structure. A number of authors used primary amines as curing agents, which did not allow the covalent incorporation of hydroxyl terminated HBPs to the epoxy matrix and thus microphase separation in the final material could be observed [22, 23]. In the present study, the addition of a 5 or 10% in weight of HBP-OH and its derivatives with allyl and 10- undecenoyl chain ends should not react with dihydrazides and phase separation could also be expected. However, not only the chemistry of the terminal groups but also the structure of the HBP and the curing rate can influence the phase separation process. In a previous paper, we reported the study of the curing process of DGEBA with some dihydrazides and concluded that the stoichiometric proportion is 2mol of DGEBA per each mol of dihydrazide. The structure of the network formed was confirmed by FTIR analysis and is represented in Figure 2. The curing could be catalyzed by acidic and basic catalysts but the latent character was reduced, and therefore some effects on the curing evolution can be expected on adding HBP modifiers. We studied the curing process by non-isothermal scanning calorimetry. The calorimetric curves collected in Figure 3 show the curing exotherms for all the formulations studied. The plot of conversion against temperature for all the studied formulations is represented in Figure 4 and the calorimetric data are collected in Table 1. In this plot, we can observe Tomuta et al. – eXPRESS Polymer Letters Vol.7, No.7 (2013) 595–606 599 Figure 2. Structure of the network formed by reaction of the epoxy resin and the adipic dihydrazide Figure 3. Calorimetric curves for the formulations studied obtained in DSC scans at 10°C/min under N2 Figure 4. Conversion against temperature of the dynamic curing at 10°C/min of all the formulations studied that the latent character of the curing of the neat formulation is slightly reduced on adding the HBP modifiers. The effect on the latency seems to be more noticeable on adding HBP-OH, which catalyzes the first stages of the curing process. However, a delay is observed at higher conversions. The catalytic effect is increased with the proportion of HBP-OH in the formulation. This can be explained by the presence of phenolic groups, which can facilitate the nucleophylic attack of the nitrogen on the epoxy ring by the formation of hydrogen bonds, as is described for epoxy-amine formulations [24]. Since during curing of epoxy resins with active NH2moieties OH groups are always formed, the effect of the phenolic groups of the HBP is not as noticeable when the conversion reaches a certain extent. Moreover, the viscosity of the reactive mixture increases and can delay the curing process. The addition of HBP-Und and HBP-Allyl leads to a significant reduction of the curing rate, and higher temperatures are needed to cure these formulations. However, there is not a clear dependence of the curing rate with the amount of modifier. In a previous study in epoxy-anhydride thermosets with both modified HBPs an acceleration of the curing was observed in spite of the higher viscosities of the formulations. This acceleration was attributed to the presence of carboxylic groups in the focal point of the HBPs, which can catalyze the curing process [16]. In the present case using dihydrazides, the dilution effect on adding the modifiers and the increase in the viscosity seem to greatly influence the curing rate in comparison to the acidic catalysis produced by carboxylic groups [17]. From the values in Table 1 we can observe that the curing enthalpy of the formulations containing HBP modifiers is somewhat lower than that measured for the neat formulation, but in all cases the curing was complete, as identified by the complete disappearance of the band at 910 cm–1 in the FTIR of the final thermosets. It should be stressed that the Tgmeasured for the modified thermosets does not decrease significantly, and even increases in the case of adding HBP-OH to the formulation. If we consider the Tgs of the different hyperbranched Tg HBP and the Tgof the neat material and apply these values and the corresponding proportions (w) in the Fox equation [25] (Equation (3)) we can predict the Tgvalues of the homogenously blended modified thermosets: (3) As can be seen in Table 1, only the thermoset with a 5% of Allyl-HBP has an experimental value of Tg similar to that predicted by this equation, whereas the addition of the other vinylic modified HBPs does not significantly influence the Tgdetermined for the neat material. This result can be explained by a phase separation of the HBPs due to the incompatibility produced during the curing reaction, which will be further confirmed by SEM. Since the initial solution was fully compatible, the separation of the particles is originated by a reaction-induced phase separation process (RIPS), which is highly dependent on the kinetics of curing and on the dynamics of the phase separation process. It should be pointed out, that the same HBP-Allyl and HBP-Und were 1 Tg 5w Tg HBP 112w Tg neat 1 Tg 5w Tg HBP 112w Tg neat Tomuta et al. – eXPRESS Polymer Letters Vol.7, No.7 (2013) 595–606 600 Table 1. Calorimetric data and kinetic parameters obtained in the curing of all the formulations aTemperature of the maximum of the curing exotherm registered at 10°C/min. bEnthalpy of the curing exotherm registered at 10°C/min. cTgdetermined after curing in a dynamic scan registered at 20°C/min. dTgcalculated by the Fox equation. eValues of activation energy at 50% of conversion, evaluated by the isoconversional non-isothermal procedure. fPre-exponential factors calculated for autocatalytic model (n= 2.1, m= 0.9) with g(%) = [(1–%)%–1]–0.9(0.9)–1. gValues of rate constants at 170°C using the Arrhenius equation at 50% conversion. Thermoset Tmaxa [°C] !hb [J/g] !hb [kJ/eq] Tgc [°C] TgFoxd [°C] Eae [kJ/mol] lnAf [s–1] k170°Cg [min–1] Neat 165 408 96 128 128 170 49.2 21.3 HBP-OH-5% 170 352 90 130 128 114 33.0 7.1 HBP-OH-10% 167 331 89 138 127 99 29.0 7.3 HBP-Und-5% 172 355 91 127 121 117 33.4 5.0 HBP-Und-10% 176 327 88 123 113 117 33.1 4.5 HBP-Allyl-5% 180 273 70 123 125 161 45.3 4.7 HBP-Allyl-10% 177 285 78 128 121 127 35.7 3.0 used as modifiers of DGEBA/anhydride thermosets, leading to completely homogeneous materials [16]. The higher curing rate when dihydrazides are used as curing agents and the highly polar structure of the network produced with this agent could both be responsible for the phase separation process, since these HBPs cannot be chemically incorporated into the epoxy network and have non-polar characteristics, especially in case of HBP-Und, as a result of the presence of the long aliphatic chains. Thus, the addition of a 5% of HBP-Allyl to the formulation leads to a homogeneous material because of its higher compatibility, due to its shorter aliphatic structure. On adding HBP-OH to the formulation, the Tgof the final thermosets is even higher than that predicted by the Fox equation. This unexpected result in fully homogeneous materials can be rationalized by the reduction in free volume due to the hydrogen bonding established between the OH groups of HBP and the epoxy-dihydrazide network [26]. In Table 1, the kinetic parameters calculated for the curing of the different formulations are collected. The kinetics of these systems was studied by the non-isothermal isoconversional procedure, as explained in the experimental part and in a previous article [21]. Figure 5 shows the evolution of the activation energy against conversion for the formulations studied. As is shown in the Figure 5, the activation energy remains, during curing, nearly constant for all formulations. This result suggests that the reaction mechanism is the same in the whole range of curing and only a single kinetic model is needed to describe the curing. In many reaction processes the values of activation energy, due to the compensation effect between the activation energy and the pre-exponen- tial factor [27], do not reflect exactly the reaction rate and it is better to discuss the rate constants calculated using the Arrhenius equation and the aforementioned kinetic parameters. To calculate the frequency factors, we selected the kinetic model that best fits the experimental data, which for all formulations was the autocatalytic kinetic model with n= 2.1 and m= 0.9. This kinetic model is consistent with the accelerative effect of the hydroxyl groups generated during curing. The calculated values of the rate constants (Table 1) illustrate the order of reactivity on curing at a conversion of 0.5 and agree with the experimental conversion-temperature curves. In this conversion, all the HBP modifiers show a delaying effect on the curing rate, as can be also observed in Figure 4. However, this effect is not produced at the beginning of curing in the case of the formulations containing HBP-OH, where hydroxyl terminal groups accelerate the curing. 3.2. Characterization of the materials by TGA and DMTA Table 2 and Figure 6 present the thermogravimetric data and the derivatives of the TGA curves, respectively. The thermosets obtained show a higher resistance to thermal degradation than the neat material, since the ester groups introduced are aromatic and therefore there is no &-elimination process that finally leads to the formation of little fragments that can be lost on heating. There is also no effect on the temperature of the maximum degradation rate, but the shape of the curves changes on modifying the mate- Tomuta et al. – eXPRESS Polymer Letters Vol.7, No.7 (2013) 595–606 601 Table 2. Thermogravimetric data for all the thermosets obtained aTemperature of the 5% of weight loss in N2atmosphere. bThe temperature of the peaks of the derivative on the thermogram registered in N2atmosphere. cChar yield after a dynamic scan until 600°C in N2atmosphere. Thermoset T5%a [°C] Tmaxb [°C] Char yieldc [%] Neat 287 337–390 12.2 OH-5% 292 344–407 13.2 OH-10% 290 352–398 14.1 Und-5% 293 355–404 14.5 Und-10% 291 356–402 14.6 Allyl-5% 297 360–400 13.7 Allyl-10% 296 350–410 13.8 Figure 5. Apparent activation energies against conversion of all the formulations studied rials. As we can see, all the degradation curves are bimodal, indicating two different degradative processes. In case of the neat material, the peak at lower temperature is more pronounced than the one occurring at higher temperature, whereas in case of the material containing a 10% of HBP-Und the contrary trend is observed. This can be related to the lower proportion of OH groups in the latter. Figures 7 and 8 show the curves of the storage modulus and tan!, respectively, for all the thermosets prepared obtained by DMTA. In Figure 7 we can see that the modulus in the rubbery state is similar for the neat and HBP-OH formulations, which seems to indicate that the crosslinking density, either covalently or by hydrogen bonding, is quite similar. On the contrary, the presence of HBP-Ally and HBP- Und leads to a reduction of the modulus. From Figure 8, it can be seen that the temperature of the maximum of the tan!peak is quite similar for all the thermosets studied, but the values are higher than those obtained by DSC, because of the differences in the frequency applied in DMTA technique. It should be noted that the materials containing a 10% of HBP-Allyl or HBP-Und show a much broader curve indicating their lower homogeneity. 3.3. Mechanical and morphological characterization Microhardness measurements are very useful in rating coatings on rigid substrates as a measure of the resistance that one body offers against penetration by another under static loads. These measurements were carried out with a Knoop microindenter and the results are shown in Figure 9. As can be seen, the addition of all the HBP modifiers does not reduce this parameter but even increases it, which is advantageous in the performance of the coatings. The best formulation in terms Tomuta et al. – eXPRESS Polymer Letters Vol.7, No.7 (2013) 595–606 602 Figure 6. Derivatives of the TGA curves in N2atmosphere for the thermosets obtained Figure 7. Evolution of storage modulus against temperature at 1 Hz for all the thermosets obtained Figure 8. Evolution of tan!against temperature at 1 Hz for all the thermosets obtained Figure 9. Microhardness values of the thermosets prepared. The increase in microhardness respect to the neat formulation is also indicated. of microhardness enhancement is the one containing a 10% of HBP-Allyl. The results of the impact tests are collected in Figure 10 for all the materials prepared. The values correspond to the energy absorbed by the material during crack propagation. It is possible to prove that the modification of DGEBA/AH thermosets with all the HBPs synthesized improves this value, as it was reported in previous publications on epoxy/ amine or anhydride systems [28]. As we can see, all the modified thermosets present a higher value than the neat material. The highest values were obtained with a 10% of HBP-Und or a 5% of HBP-Allyl. In reference to the impact strength values, it should be pointed out that the neat system is tougher than the DGEBA/MHHPA neat material studied in a previous publication (2.4 to 3.9 kJ/m2) [16]. This illustrates the important role of the curing agent in the characteristics of the thermosets. Moreover, the addition of HBP-Und and HBP-Allyl to DGEBA/dihydrazide materials results in a greater improvement of the toughness characteristics in comparison with DGEBA/MHHPA thermosets. The SEM micrographs of the impacted fracture surfaces are collected in Figure 11. These show a fracture surface with cracks and river-line structures in different planes in the neat material in accordance with the impact strength measured. In agreement with our earlier interpretations, on comparing the experimental Tgs which are higher than those predicted by the Fox equation, materials containing a 5% of HBP-Und or a 10% of both vinylic modifiers show a clear phase separation of the HBP from the epoxy matrix. Usually, particle phase separated materials have enhanced toughness characteristics [5, 29]. However, the thermoset containing a 10% of HBP-OH shows a notable improvement in impact strength, quite similar to phase separated materials, but it presents a homogeneous appearance with a patterned roughness. This type of morphology was previously observed by us in materials obtained with 1-methylimidazole, which cured very fast as is also the case here [30]. The Tgmeasured for this thermoset does not indicate plasticization, related to ductility, that dictate its toughness characteristics [31]. However, the rougher surface appearance observed in the fractographs containing HBP-OH blends, suggests that the impact specimens experienced more plastic deformation during fracture in comparison with the unmodified epoxy network. As we can see, materials with a 5 or a 10% in weight of HBP-Allyl show very different fracture morphologies. Whereas the first one, present a homogeneous appearance with unidirectional cracks, riverline structures and striations, the second present nanoparticles (of about 300 nm) distributed in the surface, which leads to high expanded cracks. In both materials containing HBP-Und a microphase separation is observed which stops or deflects the crack propagation. In both cases, the size of the particles has a broad distribution, and more particles with a bigger size (average about 1.5 µm) can be observed for the material containing a larger proportion of modifier. In Figure 12, a more detailed micrograph of the fracture surface for the material containing a 10% of HBP-Und is shown. As we can see, when the crack reaches the particle, it terminates and the energy is dissipated around the particle of HBP. This indicates that there is no interfacial adhesion between epoxy network and HBP-Und as expected as a result of the loss of hydrogen bonding by derivatization of phenolic groups. Some authors reported that the improvement in the interfacial adhesion of epoxy resin and HBP particles contributes to an improvement of the facture behaviour of epoxy resin/HBP blends [27]. According to that argument, the nano/ microphase separation reached in the present study does not very effectively enhance the toughness, as was expected. HBP-OH modifiers do not separate because of the compatibility with the epoxy matrix. However, the improvement in toughness is achieved in all the materials obtained in the present work without any decrease of Tgor deterioration of the Tomuta et al. – eXPRESS Polymer Letters Vol.7, No.7 (2013) 595–606 603 Figure 10. Impact strength values of the thermosets prepared