scieee AI-readable full text Open interactive document viewer

Influence of the characteristics of expandable graphite on the morphology, thermal properties, fire behaviour and compression performance of a rigid polyurethane foam

Acuña, Pablo,Li, Zhi,Santiago Calvo, Mercerdes,Villafañe González, Fernando,Rodríguez Pérez, Miguel Ángel,Wang, De-YI

Abstract

Producción Científica

Full text

polymers Article Influence of the Characteristics of Expandable Graphite on the Morphology, Thermal Properties, Fire Behaviour and Compression Performance of a Rigid Polyurethane Foam Pablo Acuña 1,4 , Zhi Li 1,5, Mercedes Santiago-Calvo 2, Fernando Villafañe 3, Miguel Ángel Rodríguez-Perez 2and De-Yi Wang 1,* 1IMDEA Materials Institute, C/Eric Kandel, 2, 28906 Getafe, Madrid, Spain; [email protected] (P.A.); [email protected] (Z.L.) 2Cellular Materials Laboratory (CellMat), Condensed Matter Physics Department, Faculty of Science, University of Valladolid, Campus Miguel Delibes, Paseo de Belén, 7, 47011 Valladolid, Spain; [email protected] (M.S.-C.); marr[email protected] (M.Á.R.-P.) 3GIR MIOMeT-IU Cinquima-Química Inorgánica, Faculty of Science, University of Valladolid, Campus Miguel Delibes, Paseo de Belén, 7, 47011 Valladolid, Spain; [email protected] 4Department of Materials Science and Engineering and Chemical Engineering, Carlos III University, Avda. de la Universidad, 30, 28911 Leganés, Madrid, Spain 5Universidad Politécnica de Madrid, E.T.S. de Ingenieros de Caminos, 28040 Madrid, Spain *Correspondence: [email protected]; Tel.: +34-91-549-3422 Received: 5 December 2018; Accepted: 10 January 2019; Published: 18 January 2019   Abstract: Three types of expandable graphite (EG) differing in particle size and expansion volume, are compared as flame retardant additives to rigid polyurethane foams (RPUFs). In this paper we discuss microstructure, thermal stability, fire behavior, and compression performance. We find that ell size distributions were less homogeneous and cell size was reduced. Furthermore, thermal conductivity increased along with EG loading. Thermogravimetric analysis (TGA) showed that EG only increased residue yield differently. The results indicate that a higher expansion of EG increased the limiting oxygen index (LOI) value, whereas a bigger particle size EG improved the rating of the vertical burning test (UL94). Results from the cone calorimeter test showed that a bigger particle size EG effectively reduced peak of heat release rate (pHRR). Furthermore, a higher expansion, led to a decrease in smoke production (TSP). The combination of both characteristics gives extraordinary results. The physical–mechanical characterization of the EG/RPUF foams revealed that their compression performance decreased slightly, mostly due to the effect of a bigger size EG. Keywords: polyurethane foam; expandable graphite; mechanical property; flame retardancy 1. Introduction Polyurethanes (PU) are a family of polymeric materials with a wide range of applications, including paints, adhesives, elastomers, and flexible or rigid foams [ 1 ]. Rigid polyurethane foams (RPUFs) are widely used in some industries like refrigeration, engineering, construction or electronics, since they are insulating materials with good mechanical properties [ 2 , 3 ]. However, RPUFs are also very flammable material, which is an important drawback for some of their final applications. Therefore, flame retardant additives are highly recommended in order to achieve a good flame retardant performance, to fulfil its practical demands [ 4 ]. Traditionally, halogenated flame retardants have been used, due to their superior smoke suppression and slowing flame spread characteristics. On PU foams, tris-(2-chlor-propyl)-phosphate (TCPP) was mainly used. However, environmental concerns related to Polymers 2019,11, 168; doi:10.3390/polym11010168 www.mdpi.com/journal/polymers Polymers 2019,11, 168 2 of 19 the emission of toxic gases from the combustion of halogenated flame retardants have led the European Union (EU) requiring the development of new halogen-free flame retardants [5]. Different halogen-free flame retardants have been added to RPUF. Phosphorous compounds, such as toluidine spirocyclic pentaerythritol bisphosphonate (TSPB), can achieve a 26.5% in the limiting oxygen index (LOI) test from a TSPB content of 30% on a RPUF [ 6 ]. Other phosphorus compounds, such as 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), and its derivatives, have produced good flame retardant performance, as well as better compressive strength [ 7 ]. Ammonium polyphosphate (APP) [ 8 ], dimethylmethylphosphonate (DMMP) [ 9 ], and ciclophosphazenes [ 10 ] have been also described as good solutions. Nevertheless, different inorganic flame retardants have shown even better results in terms of flame retardancy. Thus, the presence of aluminum trihydroxide (ATH) allows materials to reach a 72.5% in the LOI test. Although these results were obtained only with high loading of ~40 wt %, this seriously weakens the mechanical properties of the final foam [ 11 , 12 ]. Furthermore, expandable graphite (EG) is an inorganic flame retardant, which has received a lot of attention in recent years as a new halogen-free flame retardant [ 2 , 4 , 8 – 15 ]. EG is manufactured from flake graphite by treatment with strong acids like sulfuric or nitric acid, which are eventually intercalated into the graphite crystal structure, so that it expands or exfoliates when heated [ 16 ]. With the temperature increase, these intercalation compounds decompose into gaseous products, and produce a higher inter-graphene layer pressure. According to Camino et al. [ 17 ], the reaction of graphite with H 2 SO 4 is a redox process, which releases CO 2 , SO 2 , and water. Thus, the volume of the graphite can increase up to 300 times, thereby lowering its density and increasing the surface area by ca. 10-fold. Once in the polymer, EG forms a worm-like insulation carbonaceous protective layer in the condensed phase with the polymer, thus isolating the material from heat and precluding mass transfer to heat sources [18,19]. The release of water and other volatiles also helps suffocate the flames [20]. The effect of adding EG on the properties of a water blown RPUF has been previously evaluated by several authors. Xiang-Cheng Bian et al. [ 21 ] described that higher density foams show better flame retardancy behaviors compared to lower density foams. In addition, the study of the mechanical properties showed a correlation between density and compressive stress [ 22 ]. EG not only makes the foaming process harder, but also worsens the mechanical properties of foam [ 9 ]. On the other hand, the effect of particle size and EG’s rate of expansion, were only studied separately. The effect of particle size of EG on semi-rigid polyurethane foams indicated that bigger particle sizes of EG gave better LOI, horizontal burning test, mechanical properties performance [ 23 ], and therefore a significant improvement of the thermal stability [24]. The rate of expansion was studied by Lorenzetti [25], who showed that the rate of expansion had no significant influence on flame retardancy performance, playing only a limited role on the LOI test, and no effect on the cone calorimeter test. On the contrary, Xiao-Liang Zhang et al. [ 26 ] indicated that the efficiency of EG depends on its expandability; the more expandability, the better flame-retardant performance. Thus, no conclusion may be drawn about which parameter dominates the mechanism of EG in order to achieve a precise flame retardant behavior. The purpose of this research is to study the effect of several EGs with two different particle sizes; 300 and 500 µ m, as well as different expansion volumes; 250 and 350 cm 3 /g, on the properties of RPUFs. Both particle size and expansion volume were studied, taking into consideration the impact on the flame retardancy and thermal stability. Indeed, cellular structure, density, and compression properties of EG/RPUF composites were also reported and discussed based on the different particle sizes of EG. Besides, the divergence of some previously reported results, and the absence of systematic investigations regarding the optimization of EG performance, encouraged us to develop this study. We aimed to select the best characteristics of EG as a flame retardant additive for RPUFs, and to find a balance between its flame retardant and compression performance. In this paper, three types of EG (EG1, EG2, and EG3), with different contents (0, 6, 8, and 10 wt %) were used as flame retardant additives to RPUF. 10 flame retardant RPUFs were prepared. The influence of particle size, expansion volume, and filler content on foam properties are herein systematically discussed. Polymers 2019,11, 168 3 of 19 2. Experimental 2.1. Materials Polyurethane raw materials FOAM-IT! ™ 5 (PU) were provided by Smooth-On (FormX Spain, Barcelona, Spain): polyurethane raw materials were divided in two sides: A-side (referred to isocyanate), and B-side (referred to polyol, containing catalysts, surfactants, and water as blowing agent). For the RPUF, the manufacturer provided the following data: free rise density, 80 Kg/m 3 ; viscosity, 300 cps; and mixing ratio, 100/87 (A:B). Expandable graphite (EG), flame retardant GHL PX 95 N (Ash max. 5%, moisture 1%, volume expansion of 250 cm 3 /g, starting temperature 180–220 ◦ C, and 300 µ m particle size; EG1), GHL PX 98 HE (Ash max. 2%, moisture 1%, expansion volume of 350 cm 3 /g, starting temperature 180–220 ◦ C, and 300 µ m particle size; EG2), and GHL PX 99 32 350 (Ash max. 1%, moisture 1%, expansion volume of 350 cm 3 /g, starting temperature 150 ◦ C, and 500 µ m particle size; EG3), were kindly provided by Georg H. Luh, GmbH (Walluf, Germany). 2.2. Foam Preparation RPUFs with 0, 6, 8, and 10 wt% EG were prepared using the one-shot and free-rising methods. The B-side parts of the RPUFs and EG were firstly mixed in a plastic beaker for 2 minutes with a mechanical stirrer at 1000 rpm until uniform dispersions were obtained. Then, the correct amount of isocyanate (A-side) was added, and the mixture was stirred rapidly at 1200 rpm (for 30 s until the system became homogeneous) with a heidolph RZR-1 mechanical stirrer. The mixture was finally poured into a 250 mm × 250 mm × 60 mm open aluminum mold, where the RPUFs were raised in vertical direction at room temperature. After curing at room temperature for a minimum of 3 h, samples were cut according to the standards of the different test performed. RPUFs formulations are shown in Table 1below. Table 1. The formulae of rigid polyurethane foams samples (RPUFs). Samples EG content (wt %) PU 0 EG1-6 6 EG2-6 6 EG3-6 6 EG1-8 8 EG2-8 8 EG3-8 8 EG1-10 10 EG2-10 10 EG3-10 10 2.3. Characterization Foam density was measured as described by ASTM D1622/D1622M-14 [ 27 ]. Density was determined by dividing the weight of each sample by its corresponding volume. Three different cylindrical samples of 30 mm × 30 mm (diameter × height) for each material were measured. Their data and average standard deviations were reported. The percentage of open cells (OC %) was measured using a gas pycnometer Accupyc II 1340 from Micromeritics, according to ASTM D6226-10 [ 28 ]. Open cell content was measured for three cylindrical samples (with the same dimensions of those used for density measurements) from each material after measuring their densities. Their data and average standard deviations were reported. The cellular structure of the foam and SEM micrographs were determined by Scanning Electron Microscopy (SEM) with a JEOL JSM-820 microscope (JEOL, Tokyo, Japan). The cured foams were cut in order to ensure a smooth surface, which was examined by SEM after vacuum coating with a gold monolayer. SEM micrographs were obtained for the growth plane (z plane) of the foam. An image Polymers 2019,11, 168 4 of 19 analysis technique [ 29 ] of the SEM micrographs was used to determine the main characteristics of the cellular foam structure: cell size distribution, mean cell size ( Φ3D ), and anisotropy ratio (AR). The calculated statistical parameters for cell size distribution were: standard deviation (SD), normalized standard deviation (NSD), and asymmetry coefficient (AC). The experimental uncertainties for cell size were ~5% and the experimental uncertainties for the NSD and AC were ~8%. These experimental errors were obtained by the differences when measuring the same parameters again using other micrographs of the same samples, and repeating the whole process of image analysis. Thermal conductivity was determined at ca. 25 ◦ C using a transient plane source thermal constant analyzer, Hot-Disk TPS 2500S, according to ISO 22007-2:2008 method [ 30 ]. The measurements were performed using two cylindrical samples cut from the same materials of 30 mm × 30 mm (diameter × height). A disk-shaped TPS sensor (Hot Disk, Gothenburg, Sweden) with a diameter of 3.189 mm was used in all measurements, after being located in contact with the xy plane (perpendicular to growth plane) of the two samples [ 31 ]. Five measurements were obtained for each material. Their data and average standard deviations were reported. The thermal stability of the specimens (TGA) was studied by a Q50 thermogravimetric analyzer (TA instruments, New Castle, DE, USA), under nitrogen atmosphere, at a heating rate of 10 ◦ C/min from 30 to 700 ◦C using ca. 10 mg of each sample, placed in a platinum cup. The limited oxygen index (LOI) test was performed with an oxygen index test instrument (FTT, East Grinstead, UK) following the ASTM D2863-13 standard [ 32 ]. The size of the specimens measured was 130 mm ×10 mm ×10 mm (length ×width ×thickness). The UL94 vertical burning test was performed on an UL94 Horizontal/Vertical Flame Chamber (FTT, East Grinstead, UK) according to ASTM D3801-10 standard [ 33 ]. The height of burning flame was 20 mm. The size of the samples measured was 130 mm × 13 mm × 10 mm (length × width × thickness). Five specimens were tested for each sample. Their data and average standard deviations were reported. The cone calorimeter test was performed with a cone calorimeter instrument (FTT) following ISO 5660-1 standard [ 34 ] under an external flux of 50 kW/m 2 . The samples of 100 mm × 100 mm × 30 mm (length × width × thickness) were wrapped in aluminum foil, and exposed horizontally to the external flux. Measurements were made in duplicate. Their data and average standard deviations were reported. Compressive properties were tested with an INSTRON 566 instrument following ASTM D1621-00 standard [ 35 ]. A maximum of six specimens for each sample, with size 50 mm × 50 mm × 30 mm (length × width × thickness), were tested. The compressive constant rate was 3 mm/min. The properties were measured in the direction of foam growth. The average compressive strength and average standard deviations were reported. 3. Results and Discussion 3.1. Cellular Structure Analysis and Thermal Conductivity The main characteristics studied for the cellular foam structure were: open cell content (OC %), mean cell size ( Φ 3D), cell size distribution, anisotropy ratio (AR), density, and thermal conductivity. Furthermore, the statistical parameters for cell size distribution determined were: standard deviation (SD), normalized standard deviation (NSD), and asymmetry coefficient (AC). NSD (ratio between the SD and Φ 3D) is related to the width of cell size distribution, and therefore provides information about the homogeneity of the cell size distribution. Thus, homogeneous cell distributions present small values of NSD, whereas AC provides information about the shape of the distribution. All these parameters are collected in Table 2. Density is one of the most critical parameters of a RPUF, because it affects the distribution of the filler (EG) in the polymeric matrix, and so its impact on density determines its performance for many applications [ 15 , 23 ] such as the strength, modulus, and energy absorption ability of the foam [ 32 , 36 ]. Polymers 2019,11, 168 5 of 19 EG-filled RPUF showed higher density than those of neat foam. This may be related to the increase of the polyol viscosity when EG was incorporated into the RPUF matrix, along with the very high density of EG particles cooperated to the RPUF matrix (for example, 2.2 g/cm 3 for EG1 versus ac. 0.1 g/cm 3 for neat PU foam). However, the three different particle sizes of EG impacted the RPUF ´ s density differently. As an example, EG1 was the filler which produced a higher increase over this parameter. Thus, an increase on average of 8.0% was observed with the addition of EG1, of 4.8% with EG2, and of 4.9% with EG3. Considering the foams containing 10 wt % EG, the density grew by 9.4% for EG1 samples with respect to that of neat foam, by 6.9% for EG2, and by 5.9% for EG3. As a matter of fact, this phenomena was related to the impact of smaller EG particle size on the neat foam, by decreasing the average cell size due to a nucleating effect during the foam formation, as reported by Luo et al. [ 24 ]. One decisive parameter in RPUFs is open cell content (OC %), since closed cell structures were required for structural and thermal insulating applications. A slight increase in open cell content compared to that of reference foam (6.90%) was observed with the addition of EG particles. However, open cell content was similar for all different EG particles (between 9.1% and 9.9%), except for the foam containing EG3 at 6 wt %, which was the highest (10.8%), and for the foam containing EG1 at 8 wt % (7.8%), which had the lowest value for the EG-filled materials. This indicated that EG, as a filler, increased the OC %; mostly, bigger EG particles increased the OC % in a greater way. Cell size is a crucial factor influencing the properties of foams. The analysis of RPUF samples for SEM micrographs is shown in Figure 1. As previously described in other studies, EG particles have a nucleating effect during foam formation, decreasing the average cell size [ 4 , 37 ]. In particular, the addition of EG1 promoted the highest cell size reduction (34% for the sample with 6 wt % content), whereas the average cell size reduction reached 30% for EG1, 27% for EG2, and 13% for EG3. Therefore, the highest cell size reduction was obtained for EG particles with the lowest size (300 µ m), due to the aggregation between particles [24]. Larger particle size EG (EG3) enlarged the cell sizes (500 µm), which was probably located mainly in the struts, that is, the intersection of several cells. On the other hand, the lower particle size EG (EG1 and EG2; 300 µ m) were not located there due to the lower size compared with the neat foam (467 µ m) [ 23 ]. Instead, the anisotropy ratio (AR) of loaded EG/PU did not show significant changes with respect to that of neat PU. On the other hand, the histograms depicted in Figure 2provide valuable additional information about cell size distribution. The data indicated that the presence of EG particles modified cell size distribution, increasing the heterogeneity (NSD values rise) and asymmetry (AC values move away from zero). The distribution was more asymmetric with the highest particle size EG (EG3). The size of the EG particles used (300 or 500 µ m) was in the same order as the mean cell size of foam, which might be the main reason behind EG particles being located between cell walls and struts [ 37 ] (Figure 3), thus modifying cellular structure. One of the main applications of RPUF is their use as insulating material, due to their low thermal conductivity, which is well represented as the sum of gas phase, solid phase, and radiative conductivity [ 38 ]. Therefore, thermal conductivity of RPUF was herein measured in order to evaluate the effect of EG. Indeed, these thermal conductivity measurements were made once the foam reached a stationary state, that is, when the carbon dioxide inside the cells (generated during the foaming reaction) was completely substituted by atmospheric air (approximately two weeks after production) [ 38 ]. It is well known that particles in the RPUF formulation can act as nucleating agents, decreasing cell size and/or acting as infrared radiation blockers, which increases the extinction coefficient. Consequently, this implied a decrease in radiation contribution to thermal conductivity. However, thermal conductivity increased with the addition of increasing amounts of EG particles (Table 2), which could be explained considering the increase in conduction through the solid phase, due to the following reasons: the high density (around 100 kg/m 3 ) of PU formulations used in this study [ 39 , 40 ], the increase in foam density due to the EG addition [ 38 ], and the formation of a network for conducting interconnected EG particles throughout the insulating PU matrix for higher EG contents (above six wt %) [ 41 ]. Finally, the addition of EG particles slightly increased the open cell content in the foams, which contributed to increased thermal conductivity. Polymers 2019,11, 168 6 of 19 Table 2. Main characteristics of the cellular structure of EG/PU foams, density, and thermal conductivity values. SAMPLES Density (Kg/m3) Open Cell (%) Cell Size (µm) NSD AC AR Thermal Conductivity (mW/mK) PU 95.9 ±0.1 6.9 ±0.2 467 ±120 0.26 −0.26 1.14 48.9 ±0.1 EG1-6 100.9 ± 1.1 9.4 ±0.4 310 ±105 0.34 0.61 1.26 52.7 ±0.2 EG1-8 104.7 ± 1.7 7.8 ±0.6 339 ±132 0.39 0.57 1.23 53.0 ±0.2 EG1-10 104.9 ± 0.3 9.5 ±0.1 339 ±108 0.32 0.56 1.25 56.0 ±0.1 EG2-6 96.5 ±1.7 9.4 ±1.5 329 ±126 0.38 0.67 1.30 50.4 ±0.1 EG2-8 99.6 ±0.5 9.1 ±0.1 349 ±121 0.35 0.85 1.04 51.6 ±0.2 EG2-10 102.8 ±5 9.9 ±0.2 340 ±104 0.31 0.83 1.14 52.8 ±0.2 EG3-6 97.5 ±1.5 10.8 ±0.7 423 ±148 0.35 0.97 1.21 51.0 ±0.3 EG3-8 102.7 ± 0.6 9.3 ±1.2 383 ±181 0.47 1.12 1.12 52.0 ±0.2 EG3-10 101.6 ± 0.9 9.5 ±0.6 408 ±155 0.38 1.13 1.13 52.2 ±0.4 Polymers 2018, 10, x FOR PEER REVIEW 7 of 21 Figure 1. SEM micrographs of the growth plane of rigid polyurethane foam (RPUF) samples. Figure 1. SEM micrographs of the growth plane of rigid polyurethane foam (RPUF) samples. Polymers 2019,11, 168 7 of 19 Polymers 2018, 10, x FOR PEER REVIEW 8 of 21 0 200 400 600 800 1000 0.00 0.05 0.10 0.15 0.20 0.25 Relative Frequency Cell size (microns) PU EG1-6 EG1-8 EG1-10 a) 0 200 400 600 800 1000 0.00 0.05 0.10 0.15 0.20 0.25 b) Relative Frequency Cell size (microns) PU EG2-6 EG2-8 EG2-10 Polymers 2018, 10, x FOR PEER REVIEW 9 of 21 Figure 2. Cell size distribution for (a) EG1, (b) EG2, and (c) EG3 RPUF samples. Figure 3. SEM micrograph of EG3-10 sample in the RPUF matrix. 3.2. Thermogravimetric Analysis TGA is one of the most relevant analysis for evaluating thermal properties of RPUFs. Thermogravimetric analysis (TGA) and differential thermogravimetry (DTG) analysis of neat RPUF (PU) and EG-filled RPUF samples on N2 atmosphere are illustrated in Figure 4 (samples containing 10 wt % of EG) and S1, the data is collected in Table 3. The corresponding thermal parameters were: the initial decomposition temperature (T5 wt %, namely the temperature at 5% weight loss), the temperature at maximum weight loss rate (Tmax, denoted as the peak value from the DTG curves), and the remaining residue at the end of the test. Both unfilled and EG-filled RPUFs showed a similar degradation curve for each sample. The degradation process consisted of a 2-steps process [36,42]. The first step of degradation for the neat RPUF was between 150 and 250 °C with ca. 7% weight loss. This step may be associated to the evaporation of small molecules of unreacted isocyanate monomers [43]. The second step of degradation occurred between 250 and 620 °C, and it was mainly due to the formation of the original PU components (isocyanates and polyols), due to the break of urethane bonds in hard segments [37,43]. Isocyanate formed remains, but polyol segments also decomposed into aliphatic ether alcohol, olefins, and CO2. As the temperature increased, more complex products were formed, such as amino compounds and CO2 from former isocyanate were removed at ca. 350 °C. At higher temperatures (ca. 500 °C), other products derived from isocyanate groups (such as amines 0 200 400 600 800 1000 0.00 0.05 0.10 0.15 0.20 0.25 c) Relative Frequency Cell size (microns) PU EG3-6 EG3-8 EG3-10 Figure 2. Cell size distribution for (a) EG1, (b) EG2, and (c) EG3 RPUF samples. Polymers 2019,11, 168 8 of 19 Polymers 2018, 10, x FOR PEER REVIEW 9 of 21 Figure 2. Cell size distribution for (a) EG1, (b) EG2, and (c) EG3 RPUF samples. Figure 3. SEM micrograph of EG3-10 sample in the RPUF matrix. 3.2. Thermogravimetric Analysis TGA is one of the most relevant analysis for evaluating thermal properties of RPUFs. Thermogravimetric analysis (TGA) and differential thermogravimetry (DTG) analysis of neat RPUF (PU) and EG-filled RPUF samples on N2 atmosphere are illustrated in Figure 4 (samples containing 10 wt % of EG) and S1, the data is collected in Table 3. The corresponding thermal parameters were: the initial decomposition temperature (T5 wt %, namely the temperature at 5% weight loss), the temperature at maximum weight loss rate (Tmax, denoted as the peak value from the DTG curves), and the remaining residue at the end of the test. Both unfilled and EG-filled RPUFs showed a similar degradation curve for each sample. The degradation process consisted of a 2-steps process [36,42]. The first step of degradation for the neat RPUF was between 150 and 250 °C with ca. 7% weight loss. This step may be associated to the evaporation of small molecules of unreacted isocyanate monomers [43]. The second step of degradation occurred between 250 and 620 °C, and it was mainly due to the formation of the original PU components (isocyanates and polyols), due to the break of urethane bonds in hard segments [37,43]. Isocyanate formed remains, but polyol segments also decomposed into aliphatic ether alcohol, olefins, and CO2. As the temperature increased, more complex products were formed, such as amino compounds and CO2 from former isocyanate were removed at ca. 350 °C. At higher temperatures (ca. 500 °C), other products derived from isocyanate groups (such as amines 0 200 400 600 800 1000 0.00 0.05 0.10 0.15 0.20 0.25 c) Relative Frequency Cell size (microns) PU EG3-6 EG3-8 EG3-10 Figure 3. SEM micrograph of EG3-10 sample in the RPUF matrix. 3.2. Thermogravimetric Analysis TGA is one of the most relevant analysis for evaluating thermal properties of RPUFs. Thermogravimetric analysis (TGA) and differential thermogravimetry (DTG) analysis of neat RPUF (PU) and EG-filled RPUF samples on N 2 atmosphere are illustrated in Figure 4(samples containing 10 wt % of EG) and S1, the data is collected in Table 3. The corresponding thermal parameters were: the initial decomposition temperature (T 5 wt % , namely the temperature at 5% weight loss), the temperature at maximum weight loss rate (T max , denoted as the peak value from the DTG curves), and the remaining residue at the end of the test. Both unfilled and EG-filled RPUFs showed a similar degradation curve for each sample. The degradation process consisted of a 2-steps process [ 36 , 42 ]. The first step of degradation for the neat RPUF was between 150 and 250 ◦ C with ca. 7% weight loss. This step may be associated to the evaporation of small molecules of unreacted isocyanate monomers [ 43 ]. The second step of degradation occurred between 250 and 620 ◦ C, and it was mainly due to the formation of the original PU components (isocyanates and polyols), due to the break of urethane bonds in hard segments [ 37 , 43 ]. Isocyanate formed remains, but polyol segments also decomposed into aliphatic ether alcohol, olefins, and CO 2 . As the temperature increased, more complex products were formed, such as amino compounds and CO 2 from former isocyanate were removed at ca. 350 ◦ C. At higher temperatures (ca. 500 ◦ C), other products derived from isocyanate groups (such as amines or benzene alkyl) decomposed into volatile products like CO 2 , HCN or NO 2 , which were generated in the final stage of the degradation process [42]. For the EG-filled foams, the degradation started earlier. Some authors have attributed the earlier degradation temperature of foam to the oxidation and degradation of polymer matrix promoted by the residual acid inside the layers of EG [ 17 , 24 , 44 ]. In fact, the average of the first peak degradation temperature on the DTG curves for the EG1 samples (with lowest rate of expansion) was 194 ◦ C. For EG2 and EG3 samples (both EGs with the same rate of expansion), they increased to 202 and to 201 ◦ C, respectively. In other words, the higher rate of expansion, delayed the degradation starting point. For EG1, the average of the first step of degradation, not taking into account the loading, was in the range 121–223 ◦ C, whereas it was 132–233 ◦ C for EG2, and 136–228 ◦ C for the particles with higher size EG3. The increasing range could be explained considering the higher rate of expansion combined with a bigger particle size of EG particles, which delayed the degradation path mechanism once the acid has been volatized. The average of the maximum degradation temperature (T max ) for EG1 was 310 ◦ C, whereas it increased to 317 ◦ C for EG2, and was slightly reduced to 315 ◦ C for EG particles with higher size; EG3. Meanwhile, the residual char increased for all EG-filled RPUF with respect to neat PU. The residue wt % increased along with the EG loading to reach a maximum of 22.6 wt % for EG1. The char layer formed acted as a thermal barrier, protecting the foam from further decomposition and limiting the degradation of the polyurethane matrix. Higher rate of expansion did not improved the char residue, neither did a higher particle size. A turning point regarding particle size and rate of expansion was found for EG1 samples, and they were the best according to the char residue wt %. Polymers 2019,11, 168 9 of 19 According to Yi Li. et al. [ 37 ], bigger particle size of EG did not influence the T max , but in accordance with the high rate of expansion, more gases can be generated, resulting in less residual char. Although the rate of expansion increased the degradation temperature, only minor influences were observed. Considering the effect of EG in the foam, except for the residue wt %, there were no important impacts on the polyurethane degradation, as EG did not react with the polyurethane matrix [45]. Polymers 2018, 10, x FOR PEER REVIEW 11 of 21 Figure 4. (a) TGA and (b) DTG curves for RPUF samples containing EG1, EG2, and EG3 at 10 wt % loading. Table 3. TGA data for EG/PU samples. SAMPLE T 5 wt% (°C) T max (°C) Residue (wt %) PU 231 329 9.8 EG1-6 231 307 14.6 EG1-8 238 313 17.6 EG1-10 228 311 22.6 EG2-6 236 322 15.0 EG2-8 237 325 17.2 EG2-10 238 303 17.7 EG3-6 234 316 14.8 EG3-8 226 313 14.9 EG3-10 229 315 19.6 3.3. Fire Behaviors Figure 4. ( a ) TGA and ( b ) DTG curves for RPUF samples containing EG1, EG2, and EG3 at 10 wt % loading. Table 3. TGA data for EG/PU samples. SAMPLE T5 wt% (◦C) Tmax (◦C) Residue (wt %) PU 231 329 9.8 EG1-6 231 307 14.6 EG1-8 238 313 17.6 EG1-10 228 311 22.6 EG2-6 236 322 15.0 EG2-8 237 325 17.2 EG2-10 238 303 17.7 EG3-6 234 316 14.8 EG3-8 226 313 14.9 EG3-10 229 315 19.6 Polymers 2019,11, 168 16 of 19 tests showed that EG with the lowest particle size slightly diminished the compressive performance, whereas, a higher particle size led to a greater decrease. Although the increasing density had a positive influence on the compressive strength, the poor interaction between EG and the PU matrix leads to poor compression performance. Supplementary Materials: The following are available online at http://www.mdpi.com/2073-4360/11/1/168/ s1. Author Contributions: Conceptualization, D.-Y.W.; data curation, P.A.; formal analysis, P.A., M.S.-C., F.V., and M.Á.R.-P.; investigation, P.A.; project administration, D.-Y.W.; supervision, D.-Y.W.; writing–original draft, P.A., M.S.-C., F.V., and M.Á.R.-P. Funding: Financial support from the Spanish Ministry of Economy and Competitiveness (MINECO) and FEDER Program (NEOADFOAM/RTC-2015-3340-3, Ramón y Cajal fellowship/RYC-2012-10737) is gratefully acknowledged. Acknowledgments: Special thanks to Georg H. Luh, GmbH (Walluf, German company, which provided the essential expandable graphites (EGs) for this manuscript. Conflicts of Interest: The authors declare no conflict of interest. References 1. Shi, L.; Li, Z.-M.; Yang, M.-B.; Yin, B.; Zhou, Q.-M.; Tian, C.-R.; Wang, J.-H. Expandable Graphite for Halogen-Free Flame-Retardant of High-Density Rigid Polyurethane Foams. J. Polym. Plast. Technol. Eng. 2005,44, 1323–1327. [CrossRef] 2. Xi, W.; Qian, L.; Chen, Y.; Wang, J.; Liu, X. Addition flame-retardant behaviors of expandable graphite and [bis(2-hydroxyethyl)amino]-methyl-phosphonic acid dimethyl ester in rigid polyurethane foams. Polym. Degrad. Stab. 2015,122, 36–43. [CrossRef] 3. Zhang, L.; Zhang, M.; Zhou, Y.; Hu, L. The study of mechanical behavior and flame retardancy of castor oil phosphate-based rigid polyurethane foam composites containing expanded graphite and triethyl phosphate. Polym. Degrad. Stab. 2013,98, 2784–2794. [CrossRef] 4. Heinen, M.; Gervase, A.E.; Petzhold, C.L. Vegetable oil-based rigid polyurethanes and phosphorylated flame-retardants derived from epoxydized soybean oil. Polym. Degrad. Stab. 2014,108, 76–86. [CrossRef] 5. SCHER Opinion on the risk assessment report on tris(2-chloro-1-methylethyl) phosphate (TCPP); CAS no. 13674-84-5; Environmental Part: Brussels, Belgium, 20 September 2007. 6. Wu, D.; Zhao, P.; Liu, Y.; Liu, X.; Wang, X. Halogen Free flame retardant rigid polyurethane foam with a novel phosphorus–nitrogen intumescent flame retardant. J. Appl. Polym. Sci. 2014,131, 39581. [CrossRef] 7. Zhang, M.; Luo, Z.; Zhang, J.; Chen, S.; Zhou, Y. Effects of a novel phosphorus–nitrogen flame retardant on rosin-based rigid polyurethane foams. Polym. Degrad. Stab. 2015,120, 427–434. [CrossRef] 8. Liu, Y.; He, J.; Yang, R. Effects of Dimethyl Methylphosphonate, Aluminum Hydroxide, Ammonium Polyphosphate, and Expandable Graphite on the Flame Retardancy and Thermal Properties of Polyisocyanurate–Polyurethane Foams. Ind. Eng. Chem. Res. 2015,54, 5876–5884. [CrossRef] 9. Feng, F.; Qian, L. The flame retardant behaviors and synergistic effect of expandable graphite and dimethyl methylphosphonate in rigid polyurethane foams. Polym. Comp. 2014,35, 301–309. [CrossRef] 10. Qian, L.; Feng, F.; Tang, S. Bi-phase flame-retardant effect of hexa-phenoxy-cyclotriphosphazene on rigid polyurethane foams containing expandable graphite. Polymers 2014,55, 95–101. [CrossRef] 11. Wang, W.; He, K.; Dong, Q.; Fan, Y.; Zhu, N.; Xia, Y.; Li, H.; Wang, J.; Yuan, Z.; Wang, E.; et al. Influence of Aluminum Hydroxide and Expandable Graphite on the Flammability of Polyisocyanurate-Polyurethane Foams. Appl. Mech. Mater. 2013,368–370, 741–746. [CrossRef] 12. Jin, J.; Dong, Q.; Shu, Z.; Wang, W.; He, K. Flame Retardant Properties of Polyurethane/Expandable Praphite Composites. Procedia Eng. 2014,71, 304–309. [CrossRef] 13. Modesti, M.; Lorenzetti, A. Halogen-free flame retardants for polymeric foams. Polym. Degrad. Stab. 2002 ,78, 167–173. [CrossRef] 14. Modesti, M.; Lorenzetti, A.; Simioni, F.; Camino, G. Expandable graphite as an intumescent flame retardant in polyisocyanurate–polyurethane foams. Polym. Degrad. Stab. 2002,77, 195–202. [CrossRef] Polymers 2019,11, 168 17 of 19 15. Gao, L.; Zheng, G.; Zhou, Y.; Hu, L.; Feng, G.; Xie, Y. Synergistic effect of expandable graphite, melamine polyphosphate and layered double hydroxide on improving the fire behavior of rosin-based rigid polyurethane foam. Ind. Crops Prod. 2013,50, 638–647. [CrossRef] 16. Xiling, C.; Kemin, S.; Jihui, L.; Jinpeng, L. Preparation of lower-sulfur content and expandable graphite. Carbon 1996,34, 1599–1603. [CrossRef] 17. Camino, G.; Duquesne, S.; Delobel, R.; Eling, B.; Lindsay, C.; Roels, T. Mechanism of Expandable Graphite Fire Retardant Action in Polyurethanes. In Fire and Polymers: Materials and Solutions for Hazard Prevention; Nelson, G.L., Wilkie, C.A., Eds.; ACS Symposium Series 797; American Chemical Society: Washington, DC, USA, 2001; Volume 8, pp. 90–109. 18. Chen, X.; Zhuo, J.; Song, W.; Jiao, C.; Qian, Y.; Li, S. Flame retardant effects of organic inorganic hybrid intumescent flame retardant based on expandable graphite in silicone rubber composites. Polym. Adv. Technol. 2014,25, 1530–1537. [CrossRef] 19. Kirpluks, M.; Cabulis, U.; Zeltins, V.; Stiebra, L.; Avots, A. Rigid Polyurethane Foam Thermal Insulation Protected with Mineral Intumescent Mat. Autex Res. J. 2014,14, 259–269. [CrossRef] 20. Kura´nska, M.; Cabulis, U.; Augu´scik, M.; Prociak, A.; Ryszkowska, J.; Kirpluks, M. Bio-based polyurethane-polyisocyanurate composites with an intumescent flame retardant. Polym. Degrad. Stab. 2016,127, 11–19. [CrossRef] 21. Bian, X.; Tang, J.; Li, Z.; Lu, Z.; Lu, A. Dependence of flame-retardant properties on density of expandable graphite filled rigid polyurethane foam. J. Appl. Polym. Sci. 2007,104, 3347–3355. [CrossRef] 22. Thirumal, M.; Khastgir, D.; Singha, N.K.; Manjunath, B.S.; Naik, Y.P. Effect of foam density on the properties of water blown rigid polyurethane foam. J. Appl. Polym. Sci. 2008,108, 1810–1817. [CrossRef] 23. Thirumal, M.; Khastgir, D.; Singha, N.K.; Manjunath, B.S.; Naik, Y.P. Effect of expandable graphite on the properties of intumescent flame-retardant polyurethane foam. J. Appl. Polym. Sci. 2008 ,110, 2586–2594. [CrossRef] 24. Luo, W.; Li, Y.; Zou, H.; Liang, M. Study of different-sized sulfur-free expandable graphite on morphology and properties of water-blown semi-rigid polyurethane foams. RSC Adv. 2014,4, 37302–37310. [CrossRef] 25. Lorenzetti, A.; Dittrich, B.; Schartel, B.; Roso, M.; Modesti, M. Expandable graphite in polyurethane foams: The effect of expansion volume and intercalants on flame retardancy. J. Appl. Polym. Sci. 2017 ,134, 45173. [CrossRef] 26. Zhang, X.L.; Duan, H.J.; Yan, D.X.; Kang, L.Q.; Zhang, W.Q.; Tang, J.-H.; Li, Z.M. A facile strategy to fabricate microencapsulated expandable graphite as a flame-retardant for rigid polyurethane foams. J. Appl. Polym. Sci. 2015,132, 42364. [CrossRef] 27. ASTM D1622-08, Standard Test Method for Apparent Density of Rigid Cellular Plastics; ASTM International: West Conshohocken, PA, USA, 2008. 28. ASTM D6226-10, Standard Test Method for Open Cell Content of Rigid Cellular Plastics; ASTM International: West Conshohocken, PA, USA, 2010. 29. Pinto, J.; Solorzano, E.; Rodríguez-Pérez, M.A.; de Saja, J.A. Characterization of the cellular structure based on user-interactive image analysis procedures. J. Cell. Plast. 2013,49, 555–575. [CrossRef] 30. ISO 22007-2. Plastics-Determination of Thermal Conductivity and Thermal Diffusivity—Part 2: Transient Plane Heat Source (Hot Disc) Method; International Organization for Standardization (ISO): Geneva, Switzerland, 2008. 31. Almanza, O.; Rodríguez, M.A.; de Saja, J.A. Applicability of the transient plane source method to measure the thermal conductivity of low-density polyethylene foams. J. Polym. Sci. B 2004 ,42, 1226–1234. [CrossRef] 32. ASTM D2863-13, Standard Test Method for Measuring the Minimum Oxygen Concentration to Support Candle-Like Combustion of Plastics (Oxygen Index); ASTM International: West Conshohocken, PA, USA, 2013. 33. ASTM D3801-10, Standard Test Method for Measuring the Comparative Burning Characteristics of Solid Plastics in a Vertical Position; ASTM International: West Conshohocken, PA, USA, 2010. 34. ISO 5660-1: Reaction-to-Fire Tests. Heat Release, Smoke Production and Mass Loss Rate. Heat Release Rate (Cone Calorimeter Method) and Smoke Production Rate (Dynamic Measurement); International Organization for Standardization (ISO): Geneva, Switzerland, 2015. 35. ASTM D1621-00, Standard Test Method for Compressive Properties Of Rigid Cellular Plastics; ASTM International: West Conshohocken, PA, USA, 2000. Polymers 2019,11, 168 18 of 19 36. Chattopadhyay, D.K.; Webster, D.C. Thermal Stability and flame Retardancy of Polyurethanes. Prog. Polym. Sci. 2009,34, 1068–1133. [CrossRef] 37. Li, Y.; Zou, J.; Zhou, S.; Chen, Y.; Zou, H.; Liang, M.; Luo, W. Effect of expandable graphite particle size on the flame retardant, mechanical, and thermal properties of water-blown semi-rigid polyurethane foam. J. Appl. Polym. Sci. 2014,131, 39885. [CrossRef] 38. Estravís, S.; Tirado-Mediavilla, J.; Santiago-Calvo, M.; Ruiz-Herrero, J.L.; Villafañe, F.; Rodríguez-Pérez, M.A. Rigid polyurethane foams with infused nanoclays: Relationship between cellular structure and thermal conductivity. Eur. Polym. J. 2016,80, 1–15. [CrossRef] 39. Rodríguez-Pérez, M.A.; Alonso, O.; Alonso, J.; de Saja, J.A. Thermal conductivity of physically crosslinked closed cell polyolefin foams. Polym. Test. 1997,16, 287–298. [CrossRef] 40. Solórzano, E.; Rodríguez-Pérez, M.A.; Lázaro, J.; de Saja, J.A. Influence of Solid Phase Conductivity and Cellular Structure on the Heat Transfer Mechanisms of Cellular Materials: Diverse Case Studies. Adv. Eng. Mater. 2009,11, 818–824. [CrossRef] 41. Debelak, B.; Lafdi, K. Use of exfoliated graphite filler to enhance polymer physical properties. Carbon 2007, 45, 1727–1734. [CrossRef] 42. Chuang, F.S. Analysis of thermal degradation of diacetylene-containing polyurethane copolymers. Polym. Degrad. Stab. 2007,92, 1393–1407. [CrossRef] 43. Jiao, L.; Xiao, H.; Wang, Q.; Sun, J. Thermal degradation characteristics of rigid polyurethane foam and the volatile products analysis with TG-FTIR-MS. Polym. Degrad. Stab. 2013,98, 2687–2696. [CrossRef] 44. Chen, X.; Liu, Y.; Bai, S.; Wang, Q. Macromolecular Nitrogen-Phosphorous Compound/Expandable Graphite Synchronous Expansion Flame Retardant Polystyrene Foam. Polym. Plast. Technol. Eng. 2014 ,53, 1402–1407. [CrossRef] 45. Duquesne, S.; Le Bras, M.; Bourbigot, S.; Delobel, R.; Camino, G.; Eling, B.; Lindsay, C.; Roels, T. Thermal degradation of polyurethane and polyurethane/expandable graphite coatings. Polym. Degrad. Stab. 2001 ,74, 493–499. [CrossRef] 46. Kang, F.; Leng, Y.; Zhang, T. Influences of density and flake size on the mechanical properties of flexible graphite. Carbon 1998,36, 875–881. 47. Lefebvre, J.; Bastin, B.; Le Bras, M.; Duquesne, S.; Ritter, C.; Paleja, R.; Poutch, F. Flame spread of flexible polyurethane foam: Comprehensive study. Polym. Test. 2004,23, 281–290. [CrossRef] 48. Schartel, B.; Hull, T.R. Development of fire-retarded materials—Interpretation of cone calorimeter data. Fire Mater. 2007,31, 327–354. [CrossRef] 49. Wang, S.; Qian, L.; Xin, F. The synergistic flame-retardant behaviors of pentaerythritol phosphate and expandable graphite in rigid polyurethane foams. Polym. Compos. 2018,39, 329–336. [CrossRef] 50. Zhang, M.; Pan, H.; Zhang, L.; Hu, L.; Zho, Y. Study of the mechanical, thermal properties and flame retardancy of rigid polyurethane foams prepared from modified castor-oil-based polyols. Ind. Crops Prod. 2014,59, 135–143. [CrossRef] 51. Chen, X.; Yu, J.; Guo, S.; Luo, Z.; He, M. Flammability and Thermal Oxidative Degradation Kinetics of Magnesium Hydroxide and Expandable Graphite Flame Retarded Polypropylene Composites. J. Macromol. Sci. Pure 2008,45, 712–720. [CrossRef] 52. Chen, X.; Yu, J.; Lu, S.; Wu, H.; Guo, S.; Zuo, Z. Combustion Characteristics of Polypropylene/Magnesium Hydroxide/Expandable Graphite Composites. J. Macromol. Sci. Part B 2009,48, 1081–1092. [CrossRef] 53. Xiaolang, C.; Hong, W.; Zhu, L. Synergistic effects of expandable graphite with magnesium hydroxide on the flame retardancy and thermal properties of polypropylene. Polym. Eng. Sci. 2007,47, 1756–1760. 54. Du, L.; Zhang, Y.; Yuan, X.; Chen, J. Combustion Characteristics and Synergistic Effect of Halogen-Free Flame-Retarded EVA/Hydrotalcite Blends with Expandable Graphite and Fumed Silica. Polym. Plast. Technol. 2009,48, 1002–1007. [CrossRef] Polymers 2019,11, 168 19 of 19 55. Modesti, M.; Lorenzetti, A. Flame retardancy of polyisocyanurate–polyurethane foams: Use of different charring agents. Polym. Degrad. Stab. 2002,78, 341–347. [CrossRef] 56. Bian, X.; Tang, J.; Li, Z. Flame retardancy of hollow glass microsphere/rigid polyurethane foams in the presence of expandable graphite. J. Appl. Polym. Sci. 2008,109, 1935–1943. [CrossRef] © 2019 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license (http://creativecommons.org/licenses/by/4.0/).