Full text
DETERMINATION OF THE STATE OF HEALTH OF LI-ION BATTERIES: THE IRREVERSIBLE ENTROPY PRODUCTION APPROACH. Thesis submitted in partial fulfillment of the requirements for the PhD Degree issued by the Universitat Politècnica de Catalunya, in its Electronic Engineering Program. Author: Victòria Júlia Ovejas Benedicto Advisor: Àngel Cuadras Tomàs November 2017
i Contents Abstract In recent years, the demand of batteries has increased with the growth of portable applications. It is widely known, though, that the performance of batteries decreases with time and use. This loss of performance is measured by the State-of-Health (SoH) of the cells. However, there is no consensus in defining this parameter. Experimental, theoretical or even heuristic approaches can be found in literature and commercial systems, but usually, they only work for particular conditions and some of them are not linked to the degradation suffered by the cells themselves. The aim of this study is to find a parameter directly related to the degradation suffered by the cells. For this purpose, we investigate the irreversible entropy production in Li-ion cells because irreversible entropy is related to energy dissipation and thus, to irreversibilities due to system or energy degradation. In order to evaluate the degradation of the cells and its correspondence to irreversible entropy generation, we studied different Li-ion chemistries (NMC, LFP and LCO). Cells were cycled at different discharge rates (close to and far from equilibrium) and evaluated at different SoHs. Therefore, capacity fade and impedance rise (the most commonly used techniques in SoH determination) were characterized and related to irreversible entropy generation. In addition, postmortem analysis was carried out to achieve a deeper knowledge of the causes and effects of degradation. As a result of this study, we introduced a new parameter for system degradation characterization, the Relative-Entropy-Production (REP), defined as the irreversible entropy generation ratio between the actual state and the initial state. In particular, we found irreversible entropy production evaluated at low discharge rates was higher as more degraded were the NMC cells. In the case of LFP cells, irreversible entropy production decreased during initial cycles but then increased towards the EoL. This behavior coincided with a capacity increase during initial cycles. In addition, we found a relationship between irreversible entropy generation and the phase transformations taking place during the discharge processes in all the evaluated cells. It was associated to the fact that materials undergoing phase transformations expand and contract yielding to cracks and other structural modifications, which produce degradation and thus irreversible entropy. REP and irreversible entropy production are found to be promising magnitudes to characterize battery aging. Even though much research has still to be carried out, the idea is to define, in the future, a threshold in REP or irreversible entropy production that the cells can stand before considering their EoL is reached. Keywords: Li-ion, SoH, irreversible entropy, degradation, damage, battery, impedance, capacity fade, post-mortem.
iii Contents Acknowledgements First, I want to acknowledge to my thesis advisor, Àngel Cuadras, the technical and emotional support that he gave me during these years. I really appreciate he was always available for helping me and that he encouraged me for doing research stays abroad. I think this part was very important in the fulfillment of this work. During the research stays, which took place at Hawaii Natural Energy Institute (HNEI) in Hawaii (USA) and at the Institute for Power Electronics and Electrical Drives (ISEA) in Aachen (Germany), I learned many useful definitions and characterization techniques. For this reason, I am very grateful to Professors Bor Yann Liaw and Dirk Uwe Sauer for hosting me in their institutions. In addition, I would like to acknowledge everyone who helped me during these periods, especially Rita Graff who carried out some of the laboratory tests during my research stay in Aachen. The financial support that made this possible was provided by the Institut de Recerca en Energia de Catalunya (IREC) during the first stages of the dissertation and to the financial support of FPU contract given by MCU during the last four years. In particular, I would like to mention Professor Joan Ramon Morante from IREC for the trust he placed in the project on its first stages. During the completion of this study, we also participated in various projects (TEC2015-63899-C3-1-R, TEC2011-27397 and MAT2010-21510), which also contributed to the finantial support of this work. Moreover, I also want to acknowledge Ikerlan for helping us in cycling the cells when our facilities did not allow it. Finally, I want to highlight that it was very nice to share this experience with other PhD students, which became very good friends after that. We supported one another and we always put a touch of humor in everything we did. And last, but not least, I want to acknowledge to my loved ones the support and patience they have shown during this time, especially during the darkest episodes of this thesis. Thank you for everything to everyone.
v Contents List of acronyms and symbols BoC Beginning-of-Charge BoD Beginning-of-Discharge BoL Beginning-of-Life CT Charge Transfer EoC End-of-Charge EoD End-of-Discharge EoL End-of-Life I Current ICP Inductively Coupled Plasma NE Negative electrode SoC State-of-Charge SoH State-of-Health MT Mass Transfer OCV Open-circuit voltage PE Positive electrode RCV Rest cell voltage REP Relative-Entropy-Production Vcell Cell voltage Z Impedance
vii Contents Table of contents Abstract......................................................................................................................................................... i Acknowledgements ................................................................................................................................... iii List of acronyms and symbols ................................................................................................................. v Index of figures ......................................................................................................................................... xi Index of tables ........................................................................................................................................ xxv Chapter 1 General introduction ....................................................................................................... 29 1.1. Introduction to batteries ..................................................................................................... 29 1.1.1. Battery chemistries .......................................................................................................... 30 1.1.2. Packaging styles ............................................................................................................... 33 1.2. Lithium-ion cells................................................................................................................... 36 1.2.1. Redox reactions ............................................................................................................... 39 1.2.2. Contributions to overpotential in Li-ion batteries ..................................................... 40 1.2.3. Aging mechanisms .......................................................................................................... 46 1.3. SoC and SoH determination methods .............................................................................. 50 1.3.1. SoC definition .................................................................................................................. 50 1.3.2. SoH definition .................................................................................................................. 52 1.4. Motivation and objectives................................................................................................... 53 Chapter 2 Capacity fade .................................................................................................................... 55 2.1. Introduction .......................................................................................................................... 55 2.2. Materials and methods ........................................................................................................ 56 2.2.1. Battery cycling .................................................................................................................. 57 2.2.2. Initial characterization .................................................................................................... 59 2.2.3. Experimental SoC definition ......................................................................................... 61 2.2.4. Capacity measurements .................................................................................................. 63 2.3. Results and discussions ....................................................................................................... 63 2.3.1. Cell-to-cell variations ...................................................................................................... 63 2.3.2. LGC2 cells (NMC) .......................................................................................................... 65 2.3.3. LFP cells ........................................................................................................................... 66 2.3.4. LCO cells .......................................................................................................................... 70 2.4. Conclusions ........................................................................................................................... 70 Chapter 3 Impedance measurements .............................................................................................. 71 3.1. Introduction .......................................................................................................................... 71 3.1.1. Impedance Measurements ............................................................................................. 72 3.1.2. Electrochemical Impedance Spectroscopy (EIS) ....................................................... 73 3.1.3. Impedance from pulses .................................................................................................. 75 3.1.4. Parameters measured in Li-ion batteries by EIS ........................................................ 76 3.2. Materials and methods ........................................................................................................ 77
xiv Fig. 3.21. Ohmic resistance (top – left), charge-transfer resistance (top – right) and total resistance calculated as the addition of ohmic and charge-transfer resistances (bottom) evolution with SoC of four EVbat cells (LFP) that were set to different degradation levels. ...... 89 Fig. 3.22. (left) Absolute and relative (right) increases of ohmic and charge-transfer resistances of the EVbat cells (LFP) from cycles 50th (EVbat_1) to 200th (EVbat_3). ................................ 90 Fig. 3.23. Impedance evolution at SoC = 100 % of four EVbat cells (LFP) which were previously cycled 50, 100, 200 and 400 times. ........................................................................................ 90 Fig. 3.24. Ohmic (top-left), charge-transfer (top-right) and total (bottom) resistances of EVbat cells (LFP) at SoC = 100 % previously set to different degradation levels. ............................ 91 Fig. 3.25. Impedance evolution of the Fresh Microbattery with SoC. On the right side, serial and polarization resistances evolution with SoC. ....................................................................... 92 Fig. 3.26. Impedance evolution of the Old Microbattery with SoC (SoC 1 means totally charged and SoC 6 totally discharged). On the right side, serial and polarization resistances evolution with SoC. ................................................................................................................................... 92 Fig. 3.27. Absolute (left) and relative (right) increases of ohmic and charge-transfer resistances from BoL (Fresh Microbattery) to EoL (Old Microbattery). Old Microbattery was cycled 150 times until the capacity dropped 20 % of the initial capacity. .......................................... 93 Fig. 3.28. Inferred real and imaginary parts of impedance of a supercapacitor of 1 F and 5.5V from constant current charging voltage and from pulsed current charging in comparison to measured impedance. .............................................................................................................. 93 Fig. 3.29. Current response to a pulsed signal of 5 V and 1 ms (inset) averaged for 10 samples. ...... 94 Fig. 3.30. Comparison between impedance of a supercapacitor of 1 F and 5.5 V measured using a potentiostat and injecting a pulsed signal. The SNR (bottom part) indicated that below 15 dB, no fitting was possible. ............................................................................................... 94 Fig. 3.31. Comparison between impedance of Microbattery LCO cell measured using a potentiostat and injecting a current pulse of 1 A during 1 s and doing FFT transformations of current and voltage profiles. ................................................................................................................. 95 Fig. 3.32. Capacity evolution of a VIC cell measured at C/25 (top) and 2C (middle) showing the different tendencies found during the aging test. Charge-transfer and mass-transfer resistances evolution with aging measured at SoC = 100 % (bottom). Dashed lines represent the ranges in which different behaviors were appreciated............................ 101 Fig. 4.1. Thermodynamic systems classified depending on how they interact with the environment. ................................................................................................................................................. 110 Fig. 4.2. Schematic of Carnot heat engine [124]. ..................................................................................... 112 Fig. 4.3. Pseudo-OCV evolution during cycle life of LGC2074 cell (left) and LGC2075 cell (right) calculated from charge/discharge curves at C/25. .......................................................... 124
xv Contents Fig. 4.4. Comparison of charge and discharge OCV curves of LGC2 cells (NMC) at BoL and EoL measured by GITT and ps-OCV. ...................................................................................... 125 Fig. 4.5. Discharge OCV curves at BoL and EoL of LGC2075 cell (NMC) obtained from GITT measurements. ....................................................................................................................... 125 Fig. 4.6. Hysteresis voltage at BoL and EoL calculated as the difference in OCV during charge and discharge measured by using the GITT technique. ......................................................... 126 Fig. 4.7. Incremental capacity curves during charge process at a C/25 rate upon cycling of LGC2074 cell (NMC). It has to be noticed that resistive contributions has been subtracted prior to the analysis......................................................................................................................... 127 Fig. 4.8. Evolution of the overpotential at C/25 obtained from the ps-OCV curve of two NMC cells (LGC2074 cell to the left and LGC2075 to the right) during their cycle life. ............. 128 Fig. 4.9. (left) OCV evolution with cycle aging and (right) overpotential evolution at C/25 with cycle aging of the Li/NMC half-cell. ........................................................................................... 129 Fig. 4.10. (left) OCV evolution with cycle aging and (right) overpotential evolution at C/25 with cycle aging of the Li/Graphite half-cell. ..................................................................................... 129 Fig. 4.11. Overpotential generated at the PE and NE electrodes measured in half-cell configurations discharged at a C/25 rate (NMC/Li and graphite/Li) at BoL (left) and EoL (right). PE and NE overpotentials were added without taking into account the matching of the electrodes in order to obtain a rough approximation of the overpotential generated at the full-cell. ............................................................................................................................. 130 Fig. 4.12. Overpotential generated in a NMC cell at a 3C/2 discharge rate at different aging stages. ................................................................................................................................................. 130 Fig. 4.13. Comparison of the overpotential generated at C/25 calculated from the discharge GITT OCV (line + markers) and the ps-OCV (solid line) at BoL (left) and at the EoL (right). ................................................................................................................................................. 131 Fig. 4.14. Error in overpotential at C/25 introduced when using ps-OCV instead of GITT OCV during discharge at BoL and EoL ...................................................................................... 131 Fig. 4.15. Apparent resistance calculated from the overvoltage curves while discharging a NMC cell at C/25 (left) and at 3C/2 (right) rates. ............................................................................. 132 Fig. 4.16. Overpotential contributions at BoL (left) and EoL (right) while discharging the NMC cell at a C/25 rate at ambient temperature. Calculations were made with discharge GITT OCV. ....................................................................................................................................... 133 Fig. 4.17. Overpotential contributions at BoL (left) and EoL (right) while discharging the NMC cell at a 3C/2 rate at ambient temperature. ............................................................................. 133 Fig. 4.18. Derivative of the OCV with respect to temperature of a LGC2 cell (NMC) at BoL (black filled squares) and at the EoL (red unfilled circles). ........................................................ 134
xvi Fig. 4.19. Evolution of the irreversible entropy generation rate obtained from the ps-OCV curve at C/25 of two NMC cells (LGC2074 cell to the left and LGC2075 to the right) during their cycle life. ........................................................................................................................ 135 Fig. 4.20. Irreversible entropy production in a NMC cell at BoL and EoL when discharged at a C/25 rate at ambient temperature. It was obtained from the OCV curves obtained from the GITT measurements. ........................................................................................................... 135 Fig. 4.21. diS/dt contributions at BoL (left) and EoL (right) while discharging the NMC cell at a C/25 rate at ambient temperature. The results were obtained from the discharge GITT OCV curves. ..................................................................................................................................... 136 Fig. 4.22. (left) Absolute and (right) relative diS/dt contributions to total diS/dt at BoL (solid lines + filled symbols) and at the EoL (dashed lines + empty symbols) when discharging the NMC cells at a C/25 rate at ambient temperature. ......................................................... 136 Fig. 4.23. Irreversible entropy production in a NMC cell at a 3C/2 discharge rate at different aging stages. ...................................................................................................................................... 137 Fig. 4.24. diS/dt contributions at BoL (left) and EoL (right) while discharging the NMC cell at a 3C/2 rate at ambient temperature. ............................................................................................... 137 Fig. 4.25. (left) absolute and (right) relative diS/dt contributions to total diS at BoL (solid lines + filled symbols) and at the EoL (dashed lines + empty symbols) when discharging the NMC at a 3C/2 rate at ambient temperature. ............................................................................. 138 Fig. 4.26. Irreversible heat generation rate (topleft), reversible heat generation rate (topright), and total heat generation rate (bottom) at BoL and EoL of LGC2075 cell (NMC) discharged at a rate of C/25. ................................................................................................................... 139 Fig. 4.27. Evolution of irreversible heat generation rate (top-left), reversible heat generation rate (topright) and total heat generation rate (bottom) with cycles in the particular case of LGC2074 cell (NMC) represented for every SoC during a discharge process at 3C/2 rate. .......................................................................................................................................... 140 Fig. 4.28. Ps-OCV dependence on temperature for a LGC2 cell at BoL (left) and at the EoL (right). ................................................................................................................................................. 141 Fig. 4.29. Overpotential evolution with temperature at C/25 of a NMC cell at BoL (solid lines) and at the EoL (dashed lines). .................................................................................................... 141 Fig. 4.30. Evolution of the irreversible entropy generation rate with temperature at C/25 of a NMC cell at BoL (solid lines) and at the EoL (dashed lines). ................................................... 142 Fig. 4.31. Irreversible heat generation rate (topleft), reversible heat generation rate (topright), and total heat generation rate (bottom) at BoL (solid lines) and EoL (dashed lines) of a LGC2 cell (NMC) discharged at a rate of C/25 at different temperatures (5 ºC, 15 ºC and 32ºC). ............................................................................................................................... 143
xvii Contents Fig. 4.32. Pseudo-OCV evolution during cycle life of VIC01 cell (left) and VIC02 cell (right) calculated from charge/discharge voltage curves at C/25. ............................................ 144 Fig. 4.33. (left) Cell voltage of a VIC cell (LFP) under different charge/discharge rates. (right) ps- OCV curves of a VIC cell (LFP) obtained at different charge/discharge rates. ........ 144 Fig. 4.34. Comparison of charge and discharge OCV curves of VIC cells (LFP) at BoL (left) and EoL (right) measured by GITT and ps-OCV. .......................................................................... 145 Fig. 4.35. Discharge OCV curves at BoL and EoL of a VIC cell (LFP) obtained from GITT measurements at ambient temperature. ............................................................................. 145 Fig. 4.36. Hysteresis voltage of a VIC cell (LFP) calculated as the difference between charging and discharging GITT OCV curves at BoL and EoL. ........................................................... 146 Fig. 4.37. Incremental capacity analysis of a VIC cell (LFP) at different SoH at a C/25 discharge rate. On the left, IC curves. On the right: evolution of the area of peaks. .......................... 146 Fig. 4.38. Overpotential of a VIC cell (LFP) generated during a discharge at a C/25 rate and calculated from the ps-OCV at room temperature. ........................................................................... 147 Fig. 4.39. Overpotential generated in a VIC cell (LFP) at a 2C discharge rate evaluated at BoL (solid line) and EoL (dashed line). ................................................................................................ 148 Fig. 4.40. (left) Cell voltage of a VIC cell (LFP) at a discharge rate of C/25 and discharge OCV obtained from GITT measurements at BoL and EoL. (right) Comparison of the overpotential generated at a discharge rate of C/25 calculated from the discharge GITT OCV (line + markers) and the ps-OCV (lines) at BoL and EoL. ................................. 148 Fig. 4.41. Error in overpotential introduced when using ps-OCV instead of discharge GITT OCV at BoL and EoL. ........................................................................................................................ 149 Fig. 4.42. Comparison of the overpotential generated in a VIC cell (LFP) at 2C discharge rate calculated from the discharge GITT OCV and ps-OCV. .............................................. 149 Fig. 4.43. Apparent resistance of a VIC cell (LFP) at a discharge rate of C/25 represented at BoL and EoL. It was calculated from OCV values coming from GITT tests. ........................... 150 Fig. 4.44. Apparent resistance of a VIC cell (LFP) at a discharge rate of 2C represented at BoL and EoL. It was calculated from OCV values coming from GITT tests. ........................... 150 Fig. 4.45. Different contributions to overpotential of a VIC cell (LFP) at BoL subjected to a discharge at a rate of C/25 (left) and 2C (right). ............................................................................... 151 Fig. 4.46. Entropic coefficient of a VIC cell (LFP) at BoL and EoL. ................................................. 152 Fig. 4.47. Irreversible entropy generation rate of a VIC cell (LFP) produced during discharge at a rate of C/25 and obtained from ps-OCV curves. ................................................................... 152 Fig. 4.48. Irreversible entropy generation rate of a VIC cell (LFP) produced during discharge at a rate of C/25 and obtained from GITT OCV curves. ............................................................ 153
xviii Fig. 4.49. (left) Absolute and (right) relative diS/dt contributions at BoL while discharging the VIC cell at a C/25 rate at ambient temperature. The results were obtained from the discharge GITT OCV curves. .............................................................................................................. 153 Fig. 4.50. Irreversible entropy generation rate of a VIC cell (LFP) produced during discharge at a rate of 2C and obtained from GITT OCV curves. ................................................................. 154 Fig. 4.51. (left) Absolute and (right) relative contributions to total diS/dt at BoL when discharging a VIC cell at a 2C rate. ............................................................................................................ 154 Fig. 4.52. Irreversible heat generation rate (topleft), reversible heat generation rate (topright), and total heat generation rate (bottom) at BoL and EoL of a VIC cell (LFP) discharged at a rate of C/25. .......................................................................................................................... 155 Fig. 4.53. Irreversible heat generation rate (topleft), reversible heat generation rate (topright), and total heat generation rate (bottom) at BoL and EoL of a VIC cell (LFP) discharged at a rate of 2C. ............................................................................................................................... 156 Fig. 4.54. OCV curves of different EVbat cells (LFP) subjected to a different number of cycles (50, 100, 200, and 400). ................................................................................................................ 157 Fig. 4.55. (left) IC curves at a C/25 discharge rate of different EVbat cells (LFP) subjected to a different number of cycles (50, 100, 200, and 400). (right) Evolution of the area of peaks (1) and (2). .............................................................................................................................. 157 Fig. 4.56. Overpotential generated at a C/8 discharge rate of different EVbat cells (LFP) previously subjected to a different number of cycles (50, 100, 200, and 400, respectively). ........ 158 Fig. 4.57. Different contributions to overpotential generated in EVbat cells when discharged at a C/8 rate at four different SoHs (50 cycles, 100 cycles, 200 cycles and 400 cycles). ........... 159 Fig. 4.58. Irreversible entropy generation rate during discharge at C/8 of different EVbat cells (LFP) previously subjected to a different number of cycles (50, 100, 200, and 400). ........... 160 Fig. 4.59. Different contributions to irreversible entropy generation rate during discharge at C/8 of different EVbat cells (LFP) previously subjected to a different number of cycles (50, 100, 200, and 400). ................................................................................................................ 161 Fig. 4.60. (left) Absolute and (right) relative contribution to diS/dt of the ohmic term, activation polarization and concentration polarization of EVbat cells (LFP) discharged at a C/8 rate and previously subjected to 50, 100, 200 and 400 cycles, respectively. ................ 162 Fig. 4.61. OCV curves of two LCO cells at different SoH levels. ........................................................ 163 Fig. 4.62. Overpotential generated for two LCO cells at different SoH levels at a discharging rate of 1C. ........................................................................................................................................... 163 Fig. 4.63. Different contributions to overpotential generated in LCO cells when discharged at a 1C rate at BoL (left) and EoL (right). ...................................................................................... 164 Fig. 4.64. Derivative of the OCV with respect to temperature (entropic coefficient) of two LCO cells at different SoH levels. ......................................................................................................... 165
xix Contents Fig. 4.65. Generation rate of irreversible entropy of a LCO cell at BoL (left) and EoL (right) when discharged at 1C. ................................................................................................................... 165 Fig. 4.66. (left) Absolute and (right) relative contributions to the generation rate of irreversible entropy of two LCO cells at different degradation levels (BoL and EoL) when discharged at 1C. ................................................................................................................... 166 Fig. 4.67. Irreversible (top-left) and reversible (top-right) heat generated in the discharge process of two LCO cells at different SoH levels at a rate of 1C. Total generation of heat corresponds to the addition of reversible and irreversible effects (bottom). .............. 166 Fig. 4.68. Schematic representation of the energy transfers when converting chemical energy to electrical energy and the related useful work extracted from a battery. ....................... 167 Fig. 4.69. Hysteresis found in LFP (filled symbols) and NMC (empty symbols) cells at BoL and EoL at room temperature. ............................................................................................................ 169 Fig. 4.70. Increase in overpotential at a C/25 discharge rate, from BoL to EoL of NMC and LFP cells at room temperature. ................................................................................................... 172 Fig. 4.71. Increase in overpotential from BoL to EoL at discharge rates between 1C and 2C of NMC, LFP and LCO cells at ambient temperature. .................................................................... 172 Fig. 4.72. Energy exchange in a closed system (green arrows). Output energy (work) is related to input energy through the efficiency. The arrows in red, blue and purple indicate entropy production (i.e. energy degradation). Energy losses and entropy production are divided between heat flow towards the environment and system aging. The former is divided between reversible heat and irreversible heat (friction, Joule effect, transport, chargetransfer effects…). The later can be due to the input energy or generated spontaneously in non-equilibrium systems. ................................................................................................ 177 Fig. 4.73. diS evolution with cycle aging of NMC/graphite cells discharged at C/25 calculated from ps-OCV (left) and discharge GITT OCV (right). Effects coming from PE and NE were distinguished (labeled as PE and NE) thanks to half-cell measurements. ................... 178 Fig. 5.1. Cell-opening procedure. a) Remove the plastic cover. b) Open the can with a can-opener. c) Cut the current collector of the positive electrode and remove the top of the cell. d) Remove the can completely. e) Keep the jellyroll. f) Unroll the jellyroll and separate the electrodes and the separator. ............................................................................................... 187 Fig. 5.2. Weighting and samples preparation. a) Thickness measurement of the electrode and current collector. b) Punching the electrode for taking samples. c) Sample taken for building half-cells. d) Rinsing the samples in a solvent. e) Keeping the samples in a labeled box. f) Sample attached to a metallic support ready for XRD analysis. ................................ 188 Fig. 5.3. Unrolled electrode divided by sections. Rectangular and circular samples of different sizes were taken along the electrodes. ......................................................................................... 188
xx Fig. 5.4. Main steps in the process of building half-cells in a coin cell format where metallic lithium, fresh electrolyte and a new separator were added. .......................................................... 189 Fig. 5.5. Diagram of the different steps followed during the ICP-OES analysis [179]. .................... 192 Fig. 5.6. Example of metal dissolution and migration of Manganese and further deposition on SEI surface [180]. .......................................................................................................................... 193 Fig. 5.7. Visual inspection of the negative electrode (top) and image taken with the laser microscope (bottom) of a fresh cell (LGC2079), on the left and an aged cell (LGC2074), on the right. ........................................................................................................................................ 195 Fig. 5.8. Laser microscope image of the positive electrode of LGC2 cells (NMC) of a fresh cell (left) and an aged one (right)......................................................................................................... 195 Fig. 5.9. Visual inspection of the negative electrode (top) and image taken with the laser microscope (bottom) of a fresh cell (VIC05), on the left and an aged cell (VIC01), on the right. 196 Fig. 5.10. Laser microscope image of the positive electrode of VIC cells (LFP) of a fresh cell (left) and an aged one (right)......................................................................................................... 197 Fig. 5.11. Cell voltage versus delivered capacity of graphite/Li half-cells from samples taken at negative electrodes of fresh and aged NMC cells. ........................................................... 198 Fig. 5.12. (left) Incremental capacity of fresh and aged graphite/Li half-cells. Peaks (labeled from I to V) are associated to phase transitions of the electrodes. (right) Capacity associated to each one of the peaks obtained from the integration of peaks. .................................... 199 Fig. 5.13. Cell voltage versus delivered capacity of half-cells from samples taken at positive electrodes of fresh and aged NMC cells............................................................................................... 200 Fig. 5.14. Incremental capacity of NMC/Li half-cells from samples taken from fresh and aged positive electrodes. ................................................................................................................ 200 Fig. 5.15. Impedance contribution of Negative (NE) and Positive (PE) electrodes to the total impedance of the full cell at fully charged state. As an example, inner parts of a fresh cell were represented. ........................................................................................................... 201 Fig. 5.16. Impedance of half-cells at SoC = 100 % build with samples of the positive electrode of LGC2 (NMC) cells. From left to right, internal part of the jelly roll, central part and external part. Black filled squares represent the fresh cell and red empty circles the aged one. .......................................................................................................................................... 202 Fig. 5.17. Impedance variation during lithium insertion to the positive electrode. The maximum voltage represents when the full cell is fully charged and every decrease in voltage represents a 20 % of charge extracted until the cell was fully discharged. To the left, data coming from the fresh cell and, to the right, from the aged cell. Notice the different scales. ...................................................................................................................................... 203 Fig. 5.18. Impedance variation during lithium extraction from the negative electrode. The minimum voltage represents when the full cell is fully charged and every increase of voltage
xxi Contents represents a 20 % of charge extracted until the cell was fully discharged. To the left, data coming from the fresh cell and, to the right, from the aged cell. Notice the different scales. ...................................................................................................................................... 203 Fig. 5.19. Impedance comparison of a fresh and aged negative electrodes measured in a graphite/Li coin cell configuration in a fully delithiated state. ........................................................... 204 Fig. 5.20. Impedance of half-cells at SoC = 100 % build with samples of the negative electrode of LGC2 (NMC) cells. From left to right, more internal part of the jelly roll, central part and more external part. Black filled squares represent the fresh cell and red empty circles the aged one. .......................................................................................................................... 204 Fig. 5.21. Particle size distribution of the negative electrode of LGC2077 fresh cell (NMC). Mean size of the particles was 6.0812 m. .......................................................................................... 211 Fig. 5.22. Pore size distribution of the negative electrode of LGC2077 fresh cell (NMC). Accessible porosity was 32.27 %. ........................................................................................................... 211 Fig. 5.23. Particle size distribution of the positive electrode of LGC2077 fresh cell (NMC). Mean size of the particles was 5.7213 m. .......................................................................................... 212 Fig. 5.24. Pore size distribution of the positive electrode of LGC2077 fresh cell (NMC). Accessible porosity was 27.20 %. ........................................................................................................... 212 Fig. 5.25. XRD patterns of fresh and aged negative electrodes of LGC2 cells (NMC). ................... 213 Fig. 5.26. XRD patterns of fresh and aged positive electrodes of LGC2 cells (NMC). ................... 213 Fig. 5.27. XRD patterns of fresh and aged negative electrodes of VIC cells (LFP). ......................... 214 Fig. 5.28. XRD patterns of fresh and aged positive electrodes of VIC cells (LFP)........................... 214 Fig. 5.29. Metallic depositions at the negative electrode, which were stuck to the separator. ......... 216 Fig. 5.30. Pressure patterns exerted to the negative electrode by the positive current collector tab during cycling. ........................................................................................................................ 217 Fig. 5.31. Sample harvested from the positive electrode of an aged NMC cell. Pressure lines were clearly observed and there was an evident detachment of the active material from the current collector, especially at those pressure lines. ........................................................ 220 Fig. 6.1. Impedance evolution of a NMC cell at SoC = 100 % during the aging test. Different effects are associated to the positive and negative electrodes thanks to the half-cell measurements carried out during the post-mortem analysis. ........................................ 233 Fig. 6.2. Evolution of ohmic resistance (left) and charge-transfer resistance estimated from the real part of impedance that was covered by the measured semicircles (right) during the aging test. The line at the charge-transfer resistance graph indicates the cycle from which the charge-transfer resistance started increasing faster. ......................................................... 235 Fig. 6.3. Relative increases of R and RCT of three NMC cells during the aging process and the associated degradation mechanisms. .................................................................................. 235
xxii Fig. 6.4. Capacity fade of three NMC cells cycled under the same conditions evaluated at C/25 discharge rate. ........................................................................................................................ 235 Fig. 6.5. Capacity fade of three NMC cells cycled under the same conditions evaluated at 3C/2 discharge rate. ........................................................................................................................ 236 Fig. 6.6. Absolute increase in ohmic and charge-transfer resistances of a NMC cell from BoL to EoL with respect to the SoC. ....................................................................................................... 236 Fig. 6.7. Ps-OCV evolution of a NMC cell during the aging test at room temperature. The vertical lines represent the two easiest identifiable solid-solution phases to the eye. .............. 237 Fig. 6.8. Evolution of the irreversible entropy production in a NMC cell at a C/25 discharge rate during the aging test carried out at room temperature. It was obtained from ps-OCV (left) curves and discharge GITT OCV (right). The vertical lines represent the two easiest identifiable solid-solution phases from the OCV curves. .................................. 238 Fig. 6.9. Evolution of the irreversible entropy production in a NMC cell at a 3C/2 discharge rate during the aging test carried out at room temperature. It was obtained from ps-OCV (left) curves. The vertical lines represent the two easiest identifiable solid-solution phases from the OCV curves. ............................................................................................. 238 Fig. 6.10. Relative-Entropy-Production of a NMC cell at a C/25 discharge rate during the aging test carried out at room temperature (left) and REP of the various contributions to entropy production (right). It was obtained from discharge GITT OCV curves. The vertical lines represent the two easiest identifiable solid-solution phases from the OCV curves. .. 239 Fig. 6.11. Comparison of the Relative-Entropy-Production in a NMC cell at a 3C/2 discharge rate during the aging test carried out at room temperature calculated from ps-OCV and GITT OCV (left) and REP of the various contributions to entropy production calculated from ps-OCV (right). Vertical lines represent the two easiest identifiable solid-solution phases from the OCV curves. ................................................................... 240 Fig. 6.12. Relative-Entropy-Production in a NMC cell at a 3C/2 discharge rate during the aging test carried out at room temperature (left) and REP during the aging test at various SoCs (right). Vertical lines represent the two easiest identifiable solid-solution phases from the OCV curves. .................................................................................................................... 240 Fig. 6.13. Comparison of the Relative-Entropy-Production in a NMC cell at C/25 and 3C/2 (obtained from ps-OCV and GITT OCV curves) discharge rate during the aging test carried out at room temperature. ............................................................................................................ 241 Fig. 6.14. Capacity fade of two VIC cells (LFP) evaluated at C/25 (top-left) and 2C (top-right) discharge rates and ohmic resistance (bottom-left) and joint contribution of chargetransfer and mass-transfer resistances evolution with aging (bottom-right). Vertical lines represent the cycles from which impedance and capacity changed their tendencies. 242
xxiii Contents Fig. 6.15. Discharge GITT OCV evolution with aging. Vertical lines represent the two-phase domains (PCx) and the single-phase domains. ................................................................................. 243 Fig. 6.16. Evolution of the irreversible entropy production in a VIC cell (LFP) evaluated at a C/25 discharge rate from ps-OCV. .............................................................................................. 243 Fig. 6.17. Evolution of the irreversible entropy production in a VIC cell (LFP) evaluated at a C/25 discharge rate from discharge GITT OCV. Vertical lines represent phase changes (PCx) at BoL (left) and at EoL (right)........................................................................................... 243 Fig. 6.18. Evolution of the irreversible entropy production in a VIC cell (LFP) evaluated at a 2C discharge rate. Black vertical lines represent intervals corresponding to solid solutions at BoL and red ones at the EoL. The arrows represent the shifting they suffered from BoL to EoL ............................................................................................................................ 244 Fig. 6.19. Relative-Entropy-Production calculated from ps-OCV curves (not accounting for hysteresis) at a C/25 discharge rate (top-left) and particular values at SoC = 50 % (bottom). Increase in hysteresis during the aging test (right). Notice that in this case, REP has been calculated for the irreversible entropy production at each cycle at this particular SoC. ....................................................................................................................... 245 Fig. 6.20. Relative-Entropy-Production calculated from discharge GITT OCV curves at a C/25 discharge rate. Vertical lines represent the end of the plateaus and the starting point of the solid solutions at BoL (black solid line) and EoL (red dashed line). ..................... 246 Fig. 6.21. Relative-Entropy-Production at a 2C discharge rate. ............................................................ 246 Fig. 6.22. Comparison of the Relative-Entropy-Production in a VIC cell at C/25 and 2C discharge rate during the aging test carried out at room temperature. .......................................... 246 Fig. 6.23. Capacity fade of three EVbat cells (LFP) evaluated at a 2.5 C discharge rate. ................. 247 Fig. 6.24. Ohmic (top-left), charge-transfer (top-right), ohmic + charge-transfer (bottom-left) and ohmic + charge-transfer + mass-transfer (bottom-right) resistances of an EVbat cell. Mass-transfer resistance was only measured until the lowest measured frequency at the EIS, independently of the frequency at which the cell was working. Therefore, the absolute value of RMT does not correspond with the actual one. ................................. 248 Fig. 6.25. OCV evolution with aging of three EVbat cells at room temperature. Vertical lines represent the two easiest identifiable plateaus (phase transformations). The arrow indicates the shifting of the end of the plateau at the EoL. ........................................... 248 Fig. 6.26. Irreversible entropy production of three EVbat cells evaluated at a discharge rate of C/8. Vertical lines represent the end of phase transformations (in black at BoL and in red at the EoL). ................................................................................................................................ 249 Fig. 6.27. Relative-Entropy-Production of three EVbat cells evaluated at a discharge rate of C/8. Vertical lines represent the end of phase transformations (in black at BoL and in red at the EoL). ................................................................................................................................ 250
Chapter 1 30 Fig. 1.1. Main parts and schematic behavior of an electrochemical cell [3]. Cells can be classified in two different groups: primary and secondary cells. Primary cells are not rechargeable since the electrochemical reaction cannot be reversed whereas secondary ones can be recharged as they are able to regenerate the chemical reactants by reversing the electrochemical reaction. The general advantages of primary cells are good shelf life, high energy density at low to moderate discharge rates, little or no maintenance, and ease of use [1]. Conversely, secondary cells have the evident advantage that can be reused once totally discharged. Moreover, they show a high power density, high discharge rate, flat discharge curves, and good performance at low-temperature. As a drawback, the energy densities of secondary cells are generally lower than those of primary cells [1]. 1.1.1. Battery chemistries Lead-acid or Pb-acid batteries were developed by Gaston Planté in 1859. They were constructed by using coiled lead strips separated by linen cloth and immersed in sulfuric acid. By initially passing a dc current between the two lead strips, an oxide grew on the one on the positive side, forming a layer of lead dioxide. This caused the development of a voltage between them, and it was soon found that charge could be passed reversibly through this configuration, so that it could act to store electrical energy [4]. Lead-acid batteries are still very popular nowadays. Despite they offer low energy and power densities, they have high capacity retention, good cycle life, they perform reliably over a wide temperature range and they are relatively cheap and easy to manufacture [1]. Currently, they are designed in many different configurations depending on the application. They are used in both mobile (as an automotive starter battery for instance) and stationary applications, ranging from very low capacities to very high. Some of the stationary applications are telecommunications systems, electric
31 General Introduction utilities for operating power distribution controls, emergency and standby power systems, uninterruptible power systems (UPS), and in railroads, signaling and car power systems [1]. The most common application of lead-acid batteries and the one in widest use is the automotive SLI (Starting- Lighting-Ignition). The only rechargeable battery until 1899 was lead acid. Then, NiCd broke into the market. NiCd offered several advantages over lead acid but the materials were expensive. In 1932, the active materials were placed inside a porous nickel-plated electrode giving some advances to the nickelbased batteries. In 1947, the modern sealed NiCd battery, which was able to absorb the gas generated during charge, was developed. For a long time, NiCd was the preferred chemistry for two-way radios, emergency medical equipment, professional video cameras and power tools. In the late 1980s, sixty percent more capacity was achieved by adding more active material but it increased internal resistance and reduced cycle life. Some advantages of NiCd batteries are high cycle life if properly maintained. NiCd is the only battery that can be ultra-fast charged with little stress, has good load performance, can be stored in a discharged state if priming before use, is simple to store and transport, has a good low-temperature performance, and is the cheapest one in terms of cost per cycle. Some limitations of this chemistry are relatively low specific energy, the memory effect that causes a loss of capacity if not given a periodic full discharge cycle, toxicity of cadmium (main drawback), high self-discharge, and low cell voltage of 1.20 V. NiCd batteries are still a standard in the airline industry, but they need proper care to attain longevity. Although NiCd batteries were used for portable devices for more than fifty years, NiMH mostly replaced them in the 1900s because of the cadmium toxicity. Nowadays, NiMH cells have thirty to forty percent higher specific energy than the standard NiCd. Compared to NiCd, NiMH is more delicate and trickier to charge. Nickel-cadmium cells show one of the highest self-discharges with twenty percent in the first 24 hours after charge and ten percent per month thereafter. In detriment of the specific energy, self-discharge and corrosion of the alloy are lowered by modifying the hydride materials. Thereafter, the community continued seeking for lighter options, capable of giving higher energy densities. Then, lithium was found to be a good candidate because it is the lightest of all metals, has the greatest electrochemical potential and offers the largest energy density per kg [5]. Therefore, lithium metal negative electrodes were of high interest. However, during the 1980s, it was discovered that changes produced on them during cycling resulted in potential fire danger. Due to the underlying instability of lithium metal, the scientific community moved to non-metallic lithium battery employing lithium ions instead [5]. However, although Li-ions are intrinsically safe, they are slightly lower in energy density. Due to the need of shifting towards non-metallic lithium electrodes, in 1991, Sony started producing and commercializing the first Li-ion battery.
Chapter 1 32 Li-ion cells offered many advantages over their predecessors. As previously mentioned, lithium is the lightest of metals what makes Li-ion cells superior in the specific energy they can deliver (Table 1.1). In addition, they release 2 or 3 times more energy density than Nickel-based cells. Moreover, there is no memory effect in Li-ion cells, so they do not require a scheduled cycling to prolong their lifetime and the self-discharge is less than half compared to NiCd or NiMH (Table 1.1). In fact, the evolution of battery chemistries yielded every time to cells capable of providing at the same time, higher specific powers and higher specific energies (Fig. 1.2). Table 1.1. Characteristics of secondary batteries [1]. Parameter Leadacid NiCd NiMH Li-ion Nominal cell voltage, V 2.0 1.2 1.2 4.1 Specific energy, Wh/Kg 35 35 75 150 Energy density, Wh/L 70 100 240 400 Charge retention at 20ºC (shelf life), months 6-9 3-6 3-6 9-12 Calendar life, years 3-8 4-6 4-6 5+ Operating temperature, ºC -40 to 60 -20 to 45 -20 to 45 -20 to 60 Relative cost per watthour (initial unit cost to consumer) 10 15 25 45 Fig. 1.2. Specific capacity versus specific energy for different battery chemistries [6].
33 General Introduction 1.1.2. Packaging styles Nowadays, cells are manufactured in different configuration types. They are classified into cylindrical, prismatic, coin cells or pouch cells. In the 1700s and 1800s, batteries were developed for first time in Europe and they were mostly encased in glass jars [7]. Because of size limitations, they shifted to sealed wooden containers and composite materials. In the 1890s, battery manufacturing shifted to the United States. The first standard commercial cell for consumer use was produced by the National Carbon Company in 1896. It was the zinc-carbon Columbia Dry Cell Battery producing 1.5 V and measuring 6 inches in length [7]. With the increase of portable devices, the growing use of sealed cylindrical cells lead to standard sizes. The alphabet nomenclature, which is still in use, was formalized in 1917 by the National Institute of Standards and Technology [8]. The standards for most rechargeable batteries were previously standardized in 1906 by the International Electrochemical Commission (Table 1.2). Table 1.2. Historic and current battery sizes [8]. Size Dimensions History F cell 33 x 91 mm Introduced in 1896 for lanterns; later used for radios; only available in nickel-cadmium today. E cell N/A Introduced ca. 1905 to power box lanterns and hobby applications. Discontinued ca. 1980. D cell 34.2 x 61.5mm Introduced in 1898 for flashlights and radios; still current. C cell 25.5 x 50mm Introduced ca. 1900 to attain smaller form factor. Sub-C 22.2 x 42.9mm 16.1mL Cordless tool battery. Other sizes are ½, 4/5 and 5/4 sub-C lengths. Mostly NiCd. B cell 20.1 x 56.8mm Introduced in 1900 for portable lighting, including bicycle lights in Europe; discontinued in in North America in 2001. A cell 17 x 50mm Only available as a NiCd or NiMH cell; also available in 2/3 and 4/5 size. Popular in old laptops and hobby batteries. AA cell 14.5 x 50mm Introduced in 1907 as penlight battery for pocket lights and spy tool in WWI; added to ANSI standard in 1947. AAA cell 10.5 x 44.5mm Developed in 1954 to reduce size for Kodak and Polaroid cameras. Added to ANSI standard in 1959. AAAA cell 8.3 x 42.5mm Offshoot of 9V, since 1990s; used for laser pointers, LED penlights, computer styli, headphone amplifiers. 4.5V battery 67 x 62 x 22mm Three cells form a flat pack; short terminal strip is positive, long strip is negative; common in Europe, Russia. 9V battery 48.5 x 26.5 x 17.5mm Introduced in 1956 for transistor radios; contains six prismatic or AAAA cells. Added to ANSI standard in 1959. 18650 18 x 65mm 16.5mL Developed in the mid-1990s for lithium-ion; commonly used in laptops, e-bikes, including Tesla EV cars.
Chapter 1 34 26650 26 x 65mm 34.5mL Larger Li-ion. Some measure 26x70mm sold as 26700. Common chemistry is LiFeO4 for UPS, hobby, automotive. 14500 14 x 50mm Li-ion similar in size to AA. Cylindrical cells consist on many long layers including both electrodes and separator layers rolled up forming the jellyroll, which is placed, inside a metallic tubular can (Fig. 1.3). Current is passed to the external circuit through conductive tabs. Usually, negative tab is connected to the metallic can while the positive tab is connected to one of the ends of the cell. They continue being one of the most widely used packaging styles for primary and secondary batteries. Their advantages are ease of manufacture and good mechanical stability. The tubular cylinder can withstand high internal pressures without deforming [7]. As drawbacks, one has to consider the inefficient use of space and the contribution of the metallic can to the total weight. In terms of safety, most cylindrical cells feature a pressure relief mechanism, and the simplest one consists on a membrane seal that ruptures under high pressure. Fig. 1.3. Cylindrical cell on the left [9] and transversal cutting of a cylindrical cell on the right [6]. Coin cells or button cells (Fig. 1.4) appeared in the 1980s as a compact solution for portable devices. They are small, easy to stack and inexpensive to build. However, the rechargeable ones have to be recharged very slowly, being a very time-consuming process. Moreover, they can be swollen if charged too rapidly and they have no safety vent. Nowadays, coin cells are mostly used as primary batteries in medical implants, watches, hearing aids, car keys and memory backups [7]. Fig. 1.4. Coin cells on the left and transversal cutting of a coin cell on the right [7].
35 General Introduction Prismatic cells were introduced in the early 1900s due to the need of thinner cells. There are no universal sizes so each manufacturer designs its own battery depending on the needs [7]. They are made of various layers one on the top of the other or wound and flattened in a pseudo-prismatic jelly roll, making a best usage of the space (Fig. 1.5). Prismatic cells are designed to allow some swelling. They are also found in large capacity formats packaged into welded aluminum housings. As main drawbacks, prismatic cells are more expensive to manufacture, they have a less efficient thermal management and their cycle life is usually shorter than that of cylindrical cells [7]. Fig. 1.5. Prismatic cell on the left [10] and transversal cutting of a prismatic cell on the right [7]. In 1995, pouch cells were the most revolutionary cells with a packaging efficiency around 90 – 95 %. Instead of using a metallic or rigid housing, they offered a completely new design where conductive foil-tabs were welded to the electrodes and brought to the outside in a fully sealed way (Fig. 1.6) [7]. Because of the particular design, they are light and cost-effective to manufacture. As they do not have hard cases, they are allowed to swell. Small batteries are swollen easily than larger ones and, in some cases, they increase in volume around 8 - 10 % in approximately 500 cycles. Consequently, stacking cells one on the top of the other is not recommended for these type of cells. It is safer when laying them flat and leaving some space between each other taking into account the possible change in volume. Cycle life of pouch cells can be fast shortened when exposed to humidity and high temperatures [7]. In addition, pouch cells are usually manufactured by adding an extra gasbag that is filled by gassing in the first cycles and then is removed from the final product. Thus, gassing is not expected to occur in following cycles.
Chapter 1 36 Fig. 1.6. Pouch cell on the left [7] and pouch cell structure on the right [11]. 1.2. Lithium-ion cells Li-ion cells have a negative electrode whose active material is carbon, in which lithium ions can be intercalated/deintercalated during charge/discharge processes. The positive active material of liion cells is a lithiated metallic oxide intercalation compound in which lithium ions can also be inserted and extracted. Common positive electrodes are made of LiCoO2 (LCO), LiNiO2 and LiMn2O4 (LMO) (Table 1.3). These materials are stable in air, have a high nominal voltage and the lithium insertion reaction has good reversibility [1]. LiCoO2 was used by the first system commercialized based in lithium-ion technology. This material is the easiest to prepare, holds its structure during cycling, and offers good electrical performance. LiNiO2 is less expensive than LiCoO2, is more stable at higher temperatures, and has a lower self-discharge rate. However, commercial interest in LiNiO2 has waned as its instability has been shown to contribute to safety issues. Conversely, LiMn2O4 materials are more abundant, inexpensive, and nontoxic [1]. Regarding to the structure, LiCoO2 and LiNiO2 have a layered structure where the cobalt or nickel would reside within oxygen octahedral, and the lithium atoms would reside in the space between the oxygen layers [1]. However, LiMn2O4 spinel materials have a three-dimensional lattice or tunneled structure where octahedral and tetrahedral structures share their faces. The insertion and extraction reactions of these three lithiated metal oxides are: 𝐿𝑖𝐶𝑜𝑂2⇌𝐿𝑖1−𝑥𝐶𝑜𝑂2+𝑥𝐿𝑖++𝑥𝑒 𝐿𝑖𝑁𝑖𝑂2⇌𝐿𝑖1−𝑥𝑁𝑖𝑂2+𝑥𝐿𝑖++𝑥𝑒 𝐿𝑖𝑀𝑛2𝑂4⇌𝐿𝑖1−𝑥𝑀𝑛2𝑂4+𝑥𝐿𝑖++𝑥𝑒 In some cases, the full capacity density of some particular materials cannot be achieved as it is the case of LiCoO2 and LiNiO2 cathodes. Their reversible value of x is equal or lower than 0.5 while for LiMn2O4 it is equal or greater than 0.85. Therefore, theoretical capacity of LiCoO2 and LiNiO2 (274 mAh/g) can never be achieved if reversibility wants to be preserved. Therefore, practically, all three cathodes have approximately the same capacity density of 135 mAh/g (Table 1.3).
37 General Introduction The search for improved layered oxide materials containing low-cost transition metals lead to other positive electrode, which combine the abovementioned metals, such as Li(NiMnCo)O2 (or NMC) cells [12]. It is made of a nickel-manganese-cobalt combination and its negative electrode is made of graphite. NMC positive electrodes bring together the high energy density of LiCoO2 and the rate capability of LiMn2O4 and they can be tailored to serve as energy cells or power cells. Moreover, they require less cobalt than LiCoO2 making them cheaper and safer. They also have improved electrochemical properties and better structural, chemical, and thermal stability than LiCoO2 cells [12]. As it is typical of many layered compounds, the voltage profile of NMC versus Li/Li+ is gradually sloping. Below 4.3 V versus Li/Li +, NMC cells, provide higher capacity densities, typically around 160 mAh/g than LCO (capacities around 140 mAh/g). In 1997, Goodenough and coworkers reported on the electrochemical properties of a new class of cathode materials known as the phospho-olivines, which adopt the orthorhombic or olivine structure. LiFePO4 (LFP) is an example of these cathode materials [12]. In a LFP cell with a theoretical specific capacity of 170 mAh/g, the insertion and extraction of lithium from the positive electrode proceeds at about 3.45 V [12] (Table 1.3). The voltage profile of these cells is flat so the potential is independent of the composition of x in LixFePO4, what indicates that a two-phase reaction occurs. The two relevant phases are LiFePO4 (triphylite) and FePO4, also known as heterosite [12]. 𝐿𝑖𝐹𝑒𝑃𝑂4(𝑡𝑟𝑖𝑝ℎ𝑦𝑙𝑖𝑡𝑒)↔𝐹𝑒𝑃𝑂4(ℎ𝑒𝑡𝑒𝑟𝑜𝑠𝑖𝑡𝑒)+𝑒−+𝐿𝑖+ The active material particles are commonly coated by carbon because it ameliorates the low electronic conductivity of both the triphylite and heterosite phases and results in better rate performance [12]. Even though LFP cells offer lower energy density than LCO and NMC cells, they are inherently safer due to their better thermal and chemical stability, offer longer cycle life, and deliver higher power densities [12].
Chapter 1 38 Table 1.3. Characteristics of typical positive electrodes of li-ion cells [12]. Cathode material Structure Potential versus Li/Li+, V Specific capacity, mAh/g LiCoO2 (LCO) Layered 3.9 140 LiNi1/3Co1/3Mn1/3O2 (NMC) Layered 3.8 160-170 LiMn2O4 and variants (LMO) Spinel 4.1 100-120 LiFePO4 (LFP) Olivine 3.45 150-170 Summarizing, for the same price, LFP cells are superior in specific power, safety and life span (Fig. 1.7). Nevertheless, LMO and NMC cells exhibit similar characteristics except in terms of specific energy, performance and life span, in which NMC perform better. In addition, concerning to LCO, their characteristics are below the other represented chemistries except in their specific energy (better than LFP and equal to NMC) and performance. Fig. 1.7. Comparison of the characteristics of the most common Li-ion chemistries. Data were extracted from [13]. Specific energy Specific power Safety Performance Life span Cost LCO LMO NMC LFP
39 General Introduction 1.2.1. Redox reactions During charge and discharge, lithium ions move back and forward between positive and negative electrodes (Fig. 1.8). The process consists on an electrochemical redox (reduction-oxidation) reaction where half-cell reactions occur at each electrode at the same time. A redox reaction is a chemical reaction in which the oxidation states of the atoms are changed due to the transport of electrons between the chemical species. In particular, lithium salts that compose the electrolyte are the responsible of the transport of lithium-ion through the liquid electrolyte [14]. Those lithium-salts (i.e. LiPF6) dissolve and they separate into a lithium cation (Li+), which is surrounded by solvent molecules, and the corresponding anion (PF6). The ionic conductivity in the electrolyte is provided by these anions and cations. Two forces drive the lithium-ion transport: migration (transport induced by electric field) and diffusion (induced by concentration gradients) [14]. The reactions at the electrodes and the overall reaction are Positive electrode 𝐿𝑖𝑀𝑂2 ⇌𝐿𝑖1−𝑥𝑀𝑂2+𝑥𝐿𝑖++𝑥𝑒 Negative electrode 𝐶+𝑥𝐿𝑖++𝑥𝑒 ⇌𝐿𝑖𝑥𝐶 Overall reaction 𝐿𝑖𝑀𝑂2+ 𝐶 ⇌𝐿𝑖𝑥𝐶+𝐿𝑖1−𝑥𝑀𝑂2 Where LiMO2 represents the lithiated metal oxide intercalation compound. From left to right, the reactions are taking place during charge and from right to left during discharge process [1]. When the cell is at chemical equilibrium, the rates of the forward reaction and the backward reaction are the same. In that case, no net flow of current is present and there is no change in products concentration. When one of those reactions is faster, there is a net flow of current through the external circuit. This process can be defined in various steps: 1. Transport of the ions from one electrode to the other through the electrolyte. 2. Conduction of the electrons through the electrode in order to reach the reacting particle. 3. Chemical reaction at the particle surface. 4. Transfer of the electroactive species from the bulk of the solution to the particle surface. 5. Diffusion at the solid phase.
Chapter 1 46 Table 1.4. Limiting cases of Butler-Volmer formulation. Limiting case Mass transfer? Equation Linear behavior (very small ) No 𝑖=−𝑖𝑜·𝑛·𝐹 𝑅·𝑇·𝜂𝑎𝑐𝑡 (1.5) Yes 𝑖=( 1 1𝑖𝑜 ⁄+1𝑖𝑙,𝑐 ⁄−1𝑖𝑙,𝑎 ⁄)·𝑛·𝐹 𝑅·𝑇·𝜂 (1.6) Tafel behavior (large ) No ln𝑖=𝛼·𝑛·𝐹 𝑅·𝑇 ·𝜂+ln 𝑖0 (1.7) Yes ln𝑖=ln𝑖𝑜+(1−𝑖 𝑖𝑙,𝑐)·exp(−𝛼·𝑛·𝐹 𝑅·𝑇 ·𝜂) (1.8) 1.2.3. Aging mechanisms Li-ion batteries performance degrade when cycled (cycle aging) or when stored, even if they are not in use (calendar aging) [27–31]. The degradation level depends on many factors cycling or storage conditions as temperature, State-of-Charge (which will be explained in following subsections) or charge and discharge rates (history) [29,32,33]. In literature, aging is usually expressed in terms of capacity fade or power fade [34,35]. It is well known that Li-ion batteries are complex systems to understand and the aging mechanisms are even more complicated [35]. Moreover, capacity fade and power fade originate for various causes and their interactions. Therefore, these processes usually occur at similar timescales and cannot be evaluated separately [35]. In addition, beside degradation mechanisms are complex and they are coupled between them, they are also dependent on the chemistry, design and the manufacturing process [15]. All the elements that compose a cell (electrodes, binder, electrolyte, separator, and current collectors) are affected by aging [36–38]. The most common causes of aging affecting the negative electrode are SEI (Solid-Electrolyte Interface) growth and dissolution, current collector corrosion, binder decomposition, volume changes or lithium plating [35,38]. The main causes and effects of aging at the negative electrode are summarized in Table 1.5.
47 General Introduction Table 1.5. Main aging mechanisms at the negative electrode side. Cause Effect Aging mechanism Result in Changes in volume* Contact loss of active material particles LAM Capacity fade Changes in porosity Overpotentials Impedance rise Solvent co-intercalation and gas evolution Cracking of active material particles LAM (graphite exfolitation) LLI Capacity fade Lithium plating Lithium deposits and formation of dendrites LLI Capacity fade Impedance rise SEI layer growth Decrease of accessible surface Impedance rise Changes in porosity Impedance rise Consumption of Li LLI Capacity fade SEI layer decomposition Capacity fade Impedance rise Binder decomposition* Contact loss LLI Capacity fade Impedance rise Current collector corrosion Contact loss Binder dissolution Overpotentials Inhomogeneous distribution of I and V Impedance rise * Discrepancies were found in [35] and [38] in which the effects were related to either capacity fade or impedance rise. SEI is a layer that forms at the surface of the graphite because of the high reactivity of the electrolyte when they get in contact. It happens because electrolyte is unstable at the graphite electrode potential operating window. The formation and growth of SEI produces an increase of the electronic resistance what increases the potential operating window at which the electrolyte is, making it more stable and ceasing its growth progressively. SEI is basically composed by precipitates from reduced decomposition of solvents, salts, lithium ions, and other impurities within the electrolyte [39]. Part of the electrolyte and a large amount of lithium ions are consumed by SEI formation in the first cycles, which produce an irreversible capacity loss. Usually, extra lithium is added when manufacturing the cells taking into account the amount required for this initial SEI formation. When lithium ions reach the negative electrode faster than at the rate at which they can be accommodated into the layered structure of the graphite (during charge process), they are deposited
Chapter 1 48 at the surface of the electrode as metallic lithium. This implies that this lithium is not going to be available anymore for charging/discharging the cell thus producing an irreversible loss of capacity. Moreover, the lithium plating is rarely homogenous but it forms a dendritic structure that can produce internal short-circuits. Clearly, it has to be avoided for safety reasons. Low temperature operation favors lithium plating because the reaction rates slow down, thus more lithium ions stay at the surface of the electrode. The problem can be reduced by adding more graphite to the cell and therefore achieving a higher surface area of the negative electrode compared to the positive one, but there is always a trade-off between avoiding lithium plating and the extra lithium consumed in SEI formation that it produces. An illustrative representation of the main aging mechanisms acting at the negative electrode is given in Fig. 1.14. Fig. 1.14. Degradation mechanisms at the negative electrode of a li-ion cell [29]. Regarding the positive electrode, there is also the formation of a surface layer but it is less detrimental than the SEI to the battery performance. Unlike the SEI, the surface layer at the positive electrode thickness does not change significantly during aging. Its formation is attributed to the precipitation of undesired reaction products that blocks the pores of the existing layer. This makes the porosity, conductivity, and diffusion coefficient to change during aging process. Consequently, it produces an increase of impedance, a reduction of the active material that can be reached and therefore, it either reduces the cell capacity [15]. Main degradation mechanisms at the PE are due to lithium insertion/extraction and phase transitions that produce morphological changes as structural disordering or crystal distortion [35]. Aging is also attributed to metal dissolution, which produces the loss of active material and reduces the capacity of the cell and a surface layer, which makes the impedance to rise cell [35]. Moreover, binder and current collector corrosion also contribute to the degradation of the cell (Table 1.6). Unfortunately, the mechanisms of capacity fade are still not completely understood nowadays [35].
49 General Introduction Therefore, different assumptions are made in literature [29,35,38,40]. In Table 1.6, we summarized the different contributions found in literature. In addition, a graphical representation of those effects was plotted in Fig. 1.15. Table 1.6. Main aging mechanisms at the positive electrode side cell [35]. Cause Aging mechanism Result Li+ insertion/extraction Morphological changes: Structural disordering Change in surface porosity Capacity fade Impedance rise Phase transitions Morphological changes: Mechanical stress and strain Crystal distortion Capacity fade Metal dissolution Precipitation of new phases Loss of active material Surface layer formation Capacity fade Impedance rise Electrolyte decomposition Gas evolution Surface layer formation Impedance rise Binder decomposition Loss of contact Impedance rise Current collector corrossion Loss of contact Impedance rise Fig. 1.15. Aging mechanisms at the positive electrode of a Li-ion cell [35]. The reactions that do not contribute to the extraction or injection of energy from or to the cell, which are undesired reactions, are usually termed as side reactions. These reactions may cause aging in both the positive and negative electrodes. Even though the SEI at the carbon-based electrode is
Chapter 1 50 beneficial and essential for proper cell operation, it is considered as a side reaction because it consumes available lithium and reduces the amount of electrolyte in the cell. Aging mechanisms not only occur when charging or discharging the cells, there are also some reactions taking place when the cell is kept under open-circuit conditions. Especially when the battery is left to open-circuit conditions at high SoCs, a local redox process occurs at the positive electrode without any external electron transfer. It is known as self-discharge process and it is caused by the decomposition of the electrolyte [1]. 1.3. SoC and SoH determination methods 1.3.1. SoC definition In thermodynamic terms, SoC is defined as a state function of the battery [41]. It implies that it has to be defined when all the species in the system are in equilibrium (at constant temperature and pressure). In these conditions, the composition of the active material of the electrode and the concentration of the active species in that composition are unique (i.e. x in LixMyOz is fixed). Thus, the electrode potential at this composition and conditions will be unique versus a reference electrode [41]. In this case, SoC can be defined as a function of the lithium content in the active material [41]. Batteries comprise two electrodes each of them staying at specific potential and having different concentrations, when evaluated at equilibrium. Therefore, the OCV, which is measured at equilibrium, can be related to SoC because it expresses the difference in Li-ion concentration in the electrodes [41]. Therefore, a particular SoC can be associated to a particular OCV value for a particular cell at a certain temperature and degradation level. Moreover, SoC can also be calculated as the ratio between injected or remaining charge in the cell and the actual capacity of the cell (1.9) [41]. 𝑆𝑜𝐶 (%)= 𝑄𝑖𝑛𝑗𝑒𝑐𝑡𝑒𝑑 𝑄𝑎𝑐𝑡𝑢𝑎𝑙 ·100 (1.9) SoC measurement methods can be classified into experimental measurements, adaptive systems or hybrid methods combining both of them [42]. Experimental measurements mainly include voltage, current (Coulomb counting method), resistance or impedance measurements. Nevertheless, adaptive systems, such as Neural Networks or Kalman Filter algorithms, are designed to automatically adjust the SoC for different discharging conditions [42]. Hybrid methods are also considered in order to take advantage of the benefits of both estimation techniques. Some of the most common used experimental methods are summarized in this section. Coulomb Counting is the most used method for determining the SoC in practical applications [41,43,44]. It consists in estimating the remaining capacity under a giving test conditions from the delivered and nominal capacities. Delivered capacity is estimated by measuring and integrating the
51 General Introduction current I(t) that goes in and out from the cell. Therefore, it is related to the nominal capacity of the cell (Qnominal) and subsequently subtracted from the initial SoC (SoCinitial) (1.10). 𝑆𝑜𝐶(𝑡)=𝑆𝑜𝐶𝑖𝑛𝑖𝑡𝑖𝑎𝑙−∫𝐼(𝑡) 𝑡 0 𝑄𝑛𝑜𝑚𝑖𝑛𝑎𝑙·100 (1.10) This is a simple method because current and time can be directly measured (Table 1.7). The accuracy of this method basically depends on the precise measurement of current and an accurate estimation of the initial SoC [43]. Moreover, when it is performed for long period discharges, the measurement errors accumulate and can be a source of high inaccuracies. Thus, regular recalibration is required when using this method [45]. The self-discharge and the coulombic efficiency also affect the capacity measurement [43,44]. In addition, nominal capacity is defined by the manufacturer for a certain working conditions. Thus, it is not a realistic value of the actual capacity of the cells. Nominal capacity does not account for the cell-to-cell variability generated during the manufacturing process, for the capacity fade due to aging [41] or the temperature and discharge current [42,45]. Therefore, in order to improve the accuracy of the method, maximum capacity of the cells under certain conditions are used in equation (1.10) instead of nominal capacity [41,45]. More precise estimations have been proposed in literature in order to reduce the effects coming from these errors [41]. Moreover, this method is commonly used in combination with other supporting methods [45]. SoC estimation from OCV was very useful for lead-acid batteries because there is a linear relationship between OCV and SoC [42,44]. However, although the OCV curves of Li-ion batteries are characteristic of their chemical composition, they do not follow a linear relationship with the SoC. Moreover, they are composed of plateaus and transition between those plateaus. At the plateaus (refer to subsection 1.2.2), the OCV is almost constant (in some cases it varies less than 5 mV) for a large range of the SoC. For example, LFP cells have a unique plateau that almost covers the full range of SoC [41]. Therefore, this method would not be suitable to these cells by only measuring one OCV point during the battery operation (Table 1.7). SoC has also been estimated from impedance or resistance measurements [41–43]. The main drawback of using impedance to determine SoC is that additional equipment is required in order to carry out the impedance measurement (Table 1.7). Therefore, it makes it impractical and expensive. On the other hand, resistance is simple to obtain but it is inaccurate and difficult to interpret because equivalent electrical models are required. If the models are simple, they are inaccurate, and increasing the complexity of the models leads to an increase of computational effort.
Chapter 1 52 Table 1.7. Pros and cons of various experimental methods employed in determining the SoC [46]. Method Pros Cons Initial parameters Coulomb Counting Easy to implement Accurate if initial SoC value, current measurement and efficiency are precise. Initial SoC dependency Needs accurate value of self-discharge rate and coulombic efficiency. High accuracy in current measurement Not suitable for cells under very dynamic conditions Current Capacity Coulombic efficiency Self-discharge rate Initial SoC value OCV Easy to implement Accurate (depending on the chemistry) Needs some rest time Not suitable for some batteries as LFP Rest time Voltage Resistance or impedance Resistance: easy to implement Resistance: not so accurate Impedance: hard and costly Resistance Previous knowledge of impedance 1.3.2. SoH definition SoH is generally defined as the ability of a cell in delivering a specific performance in comparison with a fresh cell [32,33,47–50]. However, this specific performance varies from study to study because there is no consensus in what SoH is and how has to be determined [46,51]. Some of the battery parameters currently employed in SoH determination are capacity, internal resistance, ac impedance, self-discharge rate or power density [46]. The unit of SoH is percent and 100 % represents a fresh cell [46,51]. There is no consensus either in defining the SoH at the EoL of the cells. In various studies it is defined as a percentage of the initial performance and in others it is defined as 0 % at the EoL [33,50]. Thus, it implies that various equations to estimate SoH can be found in literature [33,49]. The most common approximations relate the SoH to the capacity fade or resistance rise. In particular, in [49] it is defined as the ratio between the initial capacity and the capacity at time t (1.11). However, in [33] it is defined separately in terms of capacity fade (SoHC) and resistance rise (SoHR) at the ith cycle (equations (1.12) and (1.13)). As it can be appreciated, they previously defined a threshold for
53 General Introduction EoL as the 80 % of the initial capacity and the double of the initial resistance. Thus, EoL was defined at SoH equal to 0 %. 𝑆𝑜𝐻(𝑡)=𝑑𝑖𝑠𝑐ℎ𝑎𝑟𝑔𝑒 𝑐𝑎𝑝𝑎𝑐𝑖𝑡𝑦 (𝑡) 𝑑𝑖𝑠𝑐ℎ𝑎𝑟𝑔𝑒 𝑐𝑎𝑝𝑎𝑐𝑖𝑡𝑦 (𝑡=0) (1.11) 𝑆𝑜𝐻𝐶(𝑖)=(1−𝐶0−𝐶(𝑖) 𝐶0·1 0.2)·100 (1.12) 𝑆𝑜𝐻𝑅(𝑖)=(1−𝑅(𝑖)−𝑅0 𝑅0·1 0.2)·100 (1.13) In particular, in electric vehicle (EV) applications, SoH is usually defined as the ratio between current capacity and initial capacity. EV cells are discarded when their SoH decreases to the 80 % [46,51,52]. SoH is usually predicted from empirical models [31]. These models can be more or less accurate, depending on the computational efforts required to simulate them. Thus, there is always a trade-off between computational complexity and accuracy in portable applications [46,47,51,52]. As it was stated in subchapter 1.2.3, it is well known that Li-ion batteries are complex systems to understand and the aging mechanisms are even more complicated. Moreover, capacity fade and power fade originate for various causes and their interactions. Therefore, it makes difficult to standardize a SoH definition valid for all the cells and applications. 1.4. Motivation and objectives The hypothesis of this dissertation was to demonstrate that the joint contribution of impedance and entropy of a cell is a valid parameter to discriminate the contributions of SoC and SoH. However, at the beginning of this study, we focused on measuring impedance but it was difficult to separate the various contributions related to cell degradation. A deep knowledge of batteries and electrochemistry are required for interpreting impedance data. Moreover, the various effects found at the impedance spectra show similar time constants what make them even more difficult to be distinguished and interpreted. Nevertheless, during this time, we focused in getting a better understanding of entropy and we realized that irreversible entropy production could stand by itself. It means that this term is directly related to the degradation suffered by the cells. Therefore, we shifted our motivation to find a relationship between the degradation of the cells and their irreversible entropy generation. The following chapters contain the introduction, a materials and methods section, the experimental results, the corresponding discussions and the conclusions. In Chapter 2 the results and
Chapter 1 54 discussions sections were presented together. The main contents of the chapters are summarized as follows: Chapter 1 A general introduction to bateries including some of the chemistries and packaging styles was developed. Then, a more specific description of Li-ion cells in particular was made. Their chemical and electrical behavior together with the main aging mechanisms they suffer were exposed. At the last part, State-of-Charge (SoC) and State-of-Health were defined. Chapter 2 In this chapter, the capacity fade of the diferent evaluated cells and the evolution of their voltatge responses during the aging tests were exposed. Chapter 3 Impedance measurements were carried out in this chapter. In particular, the evolution of impedance of the diferent cells during the cycling tests were tracked versus SoC and SoH. Moreover, impedance was estimated from digital signal processing of charging voltatge/current profiles and from pulses. Chapter 4 In this chapter, energy and entropy relations were evaluated. In particular, OCV, hysteresis, overpotential, reversible and irreversible entropies production and heat generations were considered. Moreover, incremental capacity analysis was carried out in order to estimate the main aging mechanisms taking place. Chapter 5 Post-mortem analysis was carried out in this chapter. The employed techniques were weighting, visual inspection, preparation of half-cells, capacity and impedance of half-cells, ICP analysis, porosimetry and XRD. Chapter 6 In this chapter, general discussions were carried out. All the results and discussions obtained from previous chapters were discussed in a global manner. Chapter 7 General conclusions were listed in this chapter. Moreover, future work and research lines derived from this study were also included.
Chapter 2 Capacity fade In this chapter, the evaluated cells are subjected to prolonged cycling in order to let them at differents SoHs for further analyses in following chapters. Moreover, the main parameters of those cells are described. In the results section, voltage profiles and capacity evolution with cycling are represented. 2.1. Introduction Cell degradation can be evaluated from either the decrease in capacity or the decrease in power capabilities. In this chapter, the evolution of capacity during cycling is investigated. Power fade in terms of impedance rise is analyzed in Chapter 3. The available capacity of the cells is directly related to the amount of active material, the available lithium for cycling and the remaining electrolyte but, at the same time, it depends on other parameters such as the charge or discharge rate, temperature or cut-off conditions [53,54]. At high rates (those that cannot be considered as close-to-equilibrium measurements); the electrochemical reactions do not have time to be completed before reaching the cut-off conditions. This is because high overpotentials are required to drive the reactions what makes the cut-off voltage limit to be reached before all the capacity could be fully exploited (refer to Fig. 1.11). In that case, the kinetic effects would be limiting the cell performance. The capacity threshold of a cell before being discarded depends on the intended application. For example, electric vehicles are one of the more demanding applications, whose batteries are discarded when their capacities decrease down to 80 % of the nominal capacity. In contrast, some other
Chapter 2 62 applied to the cell, all the ions accumulate at the electrode surface but have no time to react. Thus, they go back to the other electrode when the current is interrupted. As the SoC is defined inside the active material particles, some relaxing time has to be left after interrupting the current in order to wait for the particles at the surface to go back to the other electrode. If the SoC at the electrode surface were evaluated instead of inside the electrode particles, it would be correct to indicate SoC = 0 % or SoC = 100 % on it. 𝑆𝑜𝐶 (%)= 𝑄𝑖𝑛𝑗𝑒𝑐𝑡𝑒𝑑 𝑄𝑎𝑐𝑡𝑢𝑎𝑙_𝐿𝑜𝑤𝑅𝑎𝑡𝑒𝑠·100 (2.1) Summarizing, SoC is independent of aging because it does not depend on capacity but on normalized capacity to the actual capacity. What changes at moderate/high rates is the deliverable portion of capacity, thus the SoC at which the cells can be charged or discharged. 2.2.3.1. Practical SoC estimation As mentioned previously, when the cells are charged and discharged at very low rates, thermodynamic properties of the cells can be extracted because kinetics effects are minimized. Therefore, the OCV curve corresponding to the full SoC range (from 0 % to 100 %) can be obtained and stored in a look-up table for further comparisons. Then, if the measurements are carried out at higher rates, the SoC can be obtained by measuring the OCV at the EoC or EoD (after a resting period) and comparing it to the corresponding OCV-SoC look-up table obtained at thermodynamic rates. Periodically, while cycling the cells, a four hours resting period was left, in our case, in order to update the SoC at which we were charging/discharging the cells at the current SoH. Four hours were selected because it was the protocol followed in Hawaii (USA) during the research stay. We learnt from them how to estimate the SoC in that particular way. Four hours resting period offered a good trade-off between time and accuracy. Rest cell voltage after the four hours resting period was considered as the OCV, and consequently SoC was obtained from this data. An example of how SoC was determined was plotted in Fig. 2.2. In that example, a C/25 charge/discharge was carried out and it was assumed that the cell was completely charged and discharged, reaching a SoC of 100 % and 0 %, respectively. Therefore, the OCV curve was estimated as the average of charge and discharge curves at a rate of C/25. However, when charged and discharged at a constant current of C/5 rate, the 95 % of the cell was charged (from 0 % to 95 % SoC), and then remnant capacity was carried out in order to set the cell at 100 % SoC. During discharge, almost 99 % could be discharged at this constant current (from 100 % to 1 % SoC). At 1C, even less charge was injected or extracted. In particular, only the 80 % of the capacity was charged (starting from fully discharged state) and 98 % was obtained during discharge (starting from fully charged state). These values were only valid for
63 Capacity Fade this particular cell at this particular SoH and they were shown here as an example of the applied method used to determine the SoC. This particular method was employed for NMC cells and VIC cells (LFP). 100 80 60 40 20 0 3,0 3,2 3,4 3,6 3,8 4,0 4,2 4,4 Discharge RCV at 1C Discharge RCV at C/5 Discharge RCV at C/25 Charge RCV at 1C Charge RCV at C/5 OCV (V) SoC (%) OCV EoD RCV EoC RCV Charge RCV at C/25 Fig. 2.2. Example of SoC calculation at 3 different charge/discharge rates (C/25, C/5 and 1C) for a NMC cell at a particular SoH. End-of-Discharge Rest Cell Voltage (EoD RCV) and End-of-Charge Rest Cell Voltage (EoC RCV) after 4 h relaxation period was compared to the OCV-SoC curve obtained at low rates (C/25 in that case). 2.2.4. Capacity measurements We measured all capacities by Coulomb counting method. Available capacity depends on the chosen charge/discharge rate, which produces a higher or lower polarization. This polarization allows or prevents the full completion of the electrochemical reactions prior to reach the cut-off voltage. Temperature was also considered because the kinetics of reactions is temperature dependent, that is, the amount of charge stored or delivered by a cell depends on its temperature. 2.3. Results and discussions 2.3.1. Cell-to-cell variations Initial cell-to-cell variations were estimated in order to validate the repeatability of the results among these particular cells. This initial study was carried out for LGC2 cells (Table 2.6) and VIC cells (Table 2.7). In general, a higher variability was found for VIC cells. The small deviation in weights suggested that the manufacturing process was quite consistent. Variations in charge-transfer resistance between cells contributes to disparities in the capacity of the cells. Similar values were found at BoC but variabilities in charge-transfer resistance at BoD were larger in VIC cells. Finally, capacity ration represents the amount of active material in the cells. It was also higher in the case of VIC cells but both stayed below 1 %. Thus, from these results, we assumed the analyses carried out to one VIC or LGC2 cell would be extrapolable to other cells of the same batch.
Chapter 2 64 Table 2.6. Cell-to-cell variations of three LGC2 cells (NMC) at BoL. LGC2 cells Mean value and standard deviation Standard deviation in % Weight 46.2924 g ± 0.04387 g ± 0.095 % Charge-transfer resistance BoC 74.32 mΩ ± 5.01 mΩ ± 6.74 % Charge-transfer resistance BoD 64.37 mΩ ± 3.92 mΩ ± 6.1 % Capacity ration 27.447 ± 0.0576 mAh.%SoC-1 ± 0.21 % Table 2.7. Cell-to-cell variations of three VIC cells (LFP) at BoL. VIC cells Mean value and standard deviation Standard deviation in % Weight 14.93188 g ± 0.06557 g ± 0.44 % Charge-transfer resistance BoC 0.219 Ω ± 0.014 Ω ± 6.5 % Charge-transfer resistance BoD 0.116 Ω ± 0.0172 Ω ± 14.83 % Capacity ration 4.503 ± 0.0332 mAh.%SoC-1 ± 0.74 % During the initial characterization of the cells, rate capabilities of LGC2 and VIC cells were compared (Fig. 2.3). As it can be appreciated, LGC2 cells maintained the same voltage shape (including the plateaus measured at C/25) at a rate of C/5. Conversely, VIC cells maintained the plateaus during charge but at least the one at the EoD disappeared at C/5. Thus, LGC2 cells showed better rate capabilities than VIC cells. Fig. 2.3. Rate capability of a NMC cell (left) and a VIC cell (right) evaluated at C/25, C/5 and 1C at BoL and room temperature. 0,0 0,5 1,0 1,5 2,0 2,5 3,0 3,0 3,2 3,4 3,6 3,8 4,0 4,2 Capacity (Ah) C/25 C/5 1C Voltage (V) 0,00 0,05 0,10 0,15 0,20 0,25 0,30 0,35 0,40 0,45 2,0 2,2 2,4 2,6 2,8 3,0 3,2 3,4 3,6 C/25 C/5 1C Voltage (V) Capacity (Ah) 2,0 2,5 3,0 3,5
65 Capacity Fade 2.3.2. LGC2 cells (NMC) In the voltage profiles of a LGC2 cell (NMC) at different SoHs when discharged at C/25 and 3C/2 rates, the ohmic drop at the beginning of discharge was not as pronounced at C/25 rate as it was at a 3C/2 rate (Fig. 2.4). Furthermore, the available capacity at low rates was also decreased during the aging test because the plateaus dropped faster to lower voltages in the aged cells. At high rates, the cell voltage decreased faster from the very beginning of discharge as more aged were the cells, due to the worsening of kinetics, what produced a decrease in the extracted charge with aging at the same cut-off conditions. 0,0 0,5 1,0 1,5 2,0 2,5 3,0 3,0 3,2 3,4 3,6 3,8 4,0 4,2 4,4 cycle 6 cycle 30 cycle 107 cycle 322 Cell Voltage (V) Extracted charge at C/25 (Ah) 0.0 0.5 1.0 1.5 2.0 2.5 3.0 3.0 3.2 3.4 3.6 3.8 4.0 4.2 4.4 cycle 9 cycle 125 cycle 250 cycle 322 Cell Voltage (V) Extracted charge at 3C/2 (Ah) Fig. 2.4. Voltage profiles of a LGC2 cell versus delivered capacity at a C/25 (left) and 3C/2 (right) discharge rates. Nominal capacity is 2.8 Ah. The capacity evolution of the NMC cells evaluated at 3C/2 and C/25, showed a linear decrease at both high and low discharge rates (Fig. 2.5 and Fig. 2.6). However, at 3C/2, three different tendencies in capacity fade were found during the aging test. Moreover, all three evaluated cells revealed similar trend, indicating a good repeatability among them. The expected cycle life by the manufacturer was 300 cycles when charging and discharging at a C/2 rate. Even though discharge was done at 3C/2 instead of C/2, the cells maintained the 80 % of the nominal capacity even after 275 - 325 cycles. If the application would require lower currents, as C/25, the cells would be still capable to deliver more than 85 % of the nominal capacity after 325 cycles (Fig. 2.6).
Chapter 2 66 050 100 150 200 250 300 350 400 2,0 2,1 2,2 2,3 2,4 2,5 2,6 2,7 2,8 2,9 3 2 - 0.14 %·cycle-1 slope1: - 3.83 mAh·cycle-1 - 0.058 %·cycle-1 slope3: - 1.62 mAh·cycle-1 - 0.076 %·cycle-1 Capacity (Ah) # cycle LGC2074 LGC2075 LGC2076 slope2: - 2.12 mAh·cycle-1 172 76 80 84 88 92 96 100 Normalized capacity (%) Fig. 2.5. Capacity evolution of the NMC cells evaluated at a 3C/2 discharge rate (in Ah on the left and as a percentage of the nominal capacity on the right). Three different slopes in capacity fade were found, which were labeled and quantified. Some points have been skipped for clearer representation. 050 100 150 200 250 300 350 400 2,0 2,1 2,2 2,3 2,4 2,5 2,6 2,7 2,8 2,9 Capacity (Ah) # cycle LGC2074 LGC2075 LGC2076 slope: - 1.25 mAh·cycle-1 - 0.045 %·cycle-1 72 76 80 84 88 92 96 100 Normalized capacity (%) Fig. 2.6. Capacity evolution of the NMC cells evaluated at a C/25 discharge rate (in Ah on the left and as a percentage of the nominal capacity on the right). 2.3.3. LFP cells 2.3.3.1. VIC cells Concerning the voltage profiles of a VIC cell at different SOH levels evaluated at a C/25 discharge rate, the capacity decreased as more cycles were carried out to the cells (Fig. 2.7). The drop in voltage found around 0.15 Ah at BoL, corresponding to the transition between plateaus, was shifted to near 0.08 Ah at the EoL, what produced the highesto capacity fade at this rate.
67 Capacity Fade 0,0 0,1 0,2 0,3 0,4 0,5 1,9 2,0 2,1 3,0 3,1 3,2 3,3 3,4 cycle 6 cycle 33 cycle 201 cycle 503 cycle 717 cycle 930 cycle 1037 Cell Voltage (V) Extracted charge at C/25 (Ah) Fig. 2.7. Voltage profiles of a VIC cell (LFP) versus delivered capacity at a C/25 discharge rate at different aging levels. Discontinuity is due to the break for the sake of clarity in the representation. The capacity evolution of VIC cells evaluated at a 2C discharge rate showed three tendencies that could be approximated as linear with different slopes: in the first 50 cycles, the capacity increased. In the following 250 cycles, capacity decreased and did it faster than from that cycle until the end of the test (Fig. 2.8). However, the capacity did not go below the 70 % of the nominal capacity after 1000 cycles even if we were discharging faster than recommended by the manufacturer (2C instead of C/5). Concerning the delivered capacity at lower rates (C/25), the cells were still capable of delived the 90 % of the nominal capacity at the end of the test (Fig. 2.9). Moreover, capacity faded following two different tendencies at cycles after and before approximately 270 cycles. From this cycle on, the capacity fading followed a linear trend until the EoD. 0200 400 600 800 1000 320 340 360 380 400 420 440 Capacity (mAh) # cycle VIC01 VIC02 Slope1: 0.18 mAh·cycle-1 Slope2: - 0.086 mAh·cycle-1 Slope3: - 0.055 mAh·cycle-1 0.045 %·cycle-1 - 0.022 %·cycle-1 - 0.014 %·cycle-1 80 85 90 95 100 105 110 Normalized capacity (%) Fig. 2.8. Capacity evolution of the VIC cells (LFP) evaluated at a 2C discharge rate (in Ah on the left and as a percentage of the nominal capacity on the right). Some points have been skipped for clear representation.
Chapter 2 68 0200 400 600 800 1000 0,34 0,36 0,38 0,40 0,42 0,44 0,46 0,48 capacity VIC01 at C/25 capacity VIC02 at C/25 Capacity (Ah) # cycle - 0.015 %·cycle-1 85 90 95 100 105 110 115 120 Normalized capacity (%) slope: - 0.06 mAh·cycle-1 Fig. 2.9. Capacity evolution of the VIC cells (LFP) evaluated at a C/25 discharge rate (in Ah on the left and as a percentage of the nominal capacity on the right). 2.3.3.2. EVbat cells The capacity at a C/25 discharge rate decreased as more cycles were carried out to the EVbat cells (Fig. 2.10). Moreover, a high voltage drop could be appreciated at the beginning of discharge, which indeed, seemed to not be affected by the aging level. In addition, the highest voltage plateau (around 3.32 V), was reduced at the EoL. Thus, being one of the major contributors to capacity fade at low rates. 010 20 30 40 50 2,4 2,5 3,1 3,2 3,3 3,4 3,5 3,6 EVbat_1 (50 cycles) EVbat_2 (100 cycles) EVbat_3 (200 cycles) EVbat_4 (400 cycles) Cell Voltage (V) Extracted charge at C/25 (Ah) Fig. 2.10. Voltage profiles of EVbat cells (LFP) versus delivered capacity at a C/25 discharge rate at different aging levels. Discontinuity is due to the break for the sake of clarity in the representation. The capacity evolution of EVbat cells at a 2.5C discharge rate showed an initial increase during the first 10 – 15 cycles (Fig. 2.11), as it happened in VIC cells (Fig. 2.8). Then, the capacity decreased at different rates during the aging process. In particular, three “regions” showed an approximated linear behavior with different slopes. In the first 75 cycles, the capacity decreased faster compared to
69 Capacity Fade the rest of the test. From cycles 75 to 250, the decrease in capacity was slower than previously but faster than from cycles 250 to 400. Moreover, the capacity of those cells dropped below 80 % after 250 cycles although the cycle life of these cells was defined as 2000 cycles at 0.3C charge/discharge rates. Differences were expected from the specifications because discharge was done at 2.5C instead of 0.3C. From the results, it was clear that the increase in C-rate shorten battery life, in particular, ten times in our study. Although these cells are designed for operating at high discharge current pulses with a maximum amplitude of 10C (but only for ten seconds), the results suggested that continuous discharge at high rates could be severely degrading the cells. In addition, maximum allowed current by the manufacturer during charging process is 1C while we were charging the cells at 2.5C. Fast charging applied to batteries especially at high SoC levels highly reduces their cycle life [59]. Therefore, we associated the faster decrease of capacity to the fast charging process rather than to the discharge cycles. Initial capacities of the cells and their evolution with aging were consistent for EVbat_1, EVbat_2 and EVbat_3. Conversely, EVbat_4 started the test showing up a much lower capacity. Even though EVbat_4 started the analysis with lower capacity, the normalized decrease in capacity was consistent for all the cells (Table 2.8). 050 100 150 200 250 300 350 400 28 30 32 34 36 38 40 42 44 46 slope4 slope3 slope2 Capacity (Ah) # cycle Evbat_1 Evbat_2 Evbat_3 Evbat_4 slope1 70 75 80 85 90 95 100 105 110 115 Normalized capacity (%) Fig. 2.11. Capacity evolution of the EVbat cells (LFP) evaluated at a 2.5C discharge rate rate (in Ah on the left and as a percentage of the nominal capacity on the right). Estimated slopes of the capacity fade at different aging levels were represented. Some points have been skipped for clear representation. Slope1: 0.39 Ah·cycle-1 (0.97 %·cycle-1), slope2: - 0.066 Ah·cycle-1 (- 0.16 %·cycle-1), slope3: - 0.03 Ah·cycle-1 (- 0.08 %·cycle-1) and slope4: - 0.009 Ah·cycle-1 (- 0.02 %·cycle-1).
Chapter 2 70 Table 2.8. Capacity evolution of EVbat cells (LFP) during discharge at 2.5C. The decrease in capacity was calculated as the difference between the maximum capacity after initial cycles and the final capacity after the aging test. Cell Number of cycles Initial capacity at cycle (Ah) Maximum capacity (Ah) Final capacity (Ah) Decrease in capacity from maximum capacity (%) EVbat_1 50 38.82 43.49 41.73 4.05 EVbat_2 100 40.86 44.18 39.94 9.60 EVbat_3 200 41.52 44.31 37.07 16.34 EVbat_4 400 35.84 40.58 30.18 25.63 2.3.4. LCO cells LCO cells were cycled 150 times at 1C with a remaining capacity of the 80 % of the nominal capacity. Detailed data of the capacity evolution was not recorded during the test. Capacity was measured before the cycling process and after it. 2.4. Conclusions LGC2 cells showed better rate capabilities than VIC cells. Capacity depends on many parameters as temperature, SoH, charge/discharge rate or initial SoC. We evaluated the dependence of capacity on SoH and charge/discharge rates. The capacity of NMC cells at a 3C/2 discharge rate decreased at different rates during the aging test. VIC cells and EVbat cells (LFP) cells showed an initial increase of capacity from where capacity decreased linearly but at different rates. LCO were the first cells that were evaluated in this study. The importance of recording capacity evolution was not realized at that time, thus detailed data about the progress of capacity fade was not available. The validity of the results coming from EVbat_4 could not be assured. Cycle life of all the studied cells except EVbat cells, were in good agreement with the cycle life defined by the manufacturer. The faster decrease in capacity of EVbat cells was associated to the fast charging processes at which they were subjected.
Chapter 3 Impedance measurements In this chapter we study the evolution of impedance with aging and SoC. A rough estimation of the resistive effects was carried out. The different contributors to resistance rise were analyzed and discussed. Moreover, we estimated the impedance of supercapacitors and cells by digital signal processing methods. The results were compared to impedance obtained by EIS with commercial devices. 3.1. Introduction Resistance (R) is the opposition of a system to the flow of current (I) when a voltage drop (V) is applied to it. Electrical resistance follows the Ohm’s law and is defined for linear systems. 𝑅=∆𝑉 𝐼 (3.1) Resistance depends on the characteristics of the material and its shape. It is directly related to the material’s resistivity ( ), its length (l) and inversely proportional to the contact area (A). 𝑅=𝜌·𝑙𝐴 (3.2) Impedance is a more general formulation of resistance in which not only resistive (dissipative) effects are considered, but also time-dependent effects such as electric field (capacitances) or
Chapter 3 78 In addition, EVbat cells were also measured with the VSP potentiostat in our laboratory. In that case, an ac voltage signal was injected to the cells and the response in current was monitored. Impedance was measured at the beginning of life and at the end of life of each of the four evaluated cells. Therefore, impedance measurements were carried out after 50, 100, 200 and 400 cycles. Due to the fact that LCO cells were measured at the first stages of this study, before our laboratory was fully equipped, impedance measurements were carried out at IREC that is a research institute placed in Barcelona. The potentiostat employed in this period was Parstat 2273 provided by Princeton Applied Research. Impedance of LCO cells was measured at BoL and EoL (with a remaining capacity of 80 % after 150 cycles). The main parameters that were set for EIS measurements and their periodicity were summarized in Table 3.1. Table 3.1. Definition of the parameters for measuring impedance by EIS technique. Cell Excitation signal Amplitude Frequency range Periodicity LGC2 (NMC) Current 50 mA 3 mHz to 5 kHz Every 50 cycles VIC (LFP) Current 20 mA 10 mHz to 3 kHz Every 100 cycles EVbat (LFP) Voltage 2 mV 3 mHz to 5 kHz After 50, 100, 200 and 400 cycles Microbattery (LCO) - - 4 mHz to 1 kHz After 0 cycles and 150 cycles 3.2.1.1. Definition of resistance contributions A typical impedance spectrum of Li-ion batteries is represented in Fig. 3.6. In addition, typical characteristic frequencies of the different transport effects and electrochemical processes taking place in the cells, which are represented in the impedance spectra, are summarized in Fig. 3.7. At high frequencies, there is an inductive tail mainly caused by the measurement cables and connections. Furthermore, apart from the cables and connections, it is also associated to the number of windings of the electrodes in the jellyroll in the particular case of cylindrical cells [82]. The point at which this inductive tail crosses the zero at the imaginary part, has been considered as an approximation of the ohmic resistance (R). Actually, for being precise, ohmic resistance should also include SEI-layer resistance, and the resistance associated to contacts between electrodes and current collectors (refer to subsection 3.1.4). However, in this study, they were not included in the ohmic contribution because, as they have a capacitive effect associated to them, they appear at the impedance spectra as
79 Impedance Measurements semicircles instead of simple resistive contributions. Therefore, as they were overlapped with chargetransfer effects and no model was fitted, it was not possible to distinguish them. At medium frequencies, one semicircle (or more than one depending on the cell, temperature, SoC or aging level) was found. It can represent many different effects depending on its nature and origin but it is always represented by a resistive effect and a capacitive effect associated to it. The resistive effect, which is represented by the real part covered by the semicircles, represents the kinetics of the measured electrochemical process. The imaginary part represents the double-layer capacitance explained in subsection 3.1.4. In this study, only the variation with aging of the resistive part was considered. In particular, all the real part covered by the semicircles is termed as charge-transfer (CT) resistance in this study (RCT). Unfortunately, there are ohmic contributions (different than CT), which not only contribute as pure resistive affects but also have a capacitive effect associated to them (they show up at the impedance spectra as a semicircle). Those ohmic contributions may arise from contact resistance, SEI-film or carbon coating [83]. Thus, their associated capacitive effect comes from the accumulation of charge at these interfaces. In this study, these contributions were not separated, thus being considered as part of the charge-transfer resistance. At the low frequencies (until reaching the lowest measured frequency), there is a diffusional branch related to mass-transfer effects (MT), labeled as RMT. The shape and the phase associated to this effect can vary depending on many factors as the SoC, the aging level, or the temperature. The capacitive effect associated to the diffusional branch tends to dominate as the frequency decreases and is related to the restricted diffusion especially at the EoD [79]. Finally, in some cases, RCT and RMT were grouped and labeled as RCT + RMT. 0,00 0,05 0,10 0,15 0,20 0,25 0,00 -0,05 -0,10 -0,15 -0,20 -0,25 RCT+RMT RMT RCT Im Z () Re Z () R Fig. 3.6. Definition of different resistance contributions.
Chapter 3 80 Fig. 3.7. Typical time constants (or characteristic frequencies) of the transport effects and electrochemical processes occurring in a LFP cell [84]. Charge-transfer resistance was obtained by two different methods. In the first one, it was directly obtained from the radius of the resulting semicircles at the Nyquist representation of impedance. The second method was based on the reference tests carried out periodically during cycling. Chargetransfer resistance was obtained from the overvoltage obtained at least at three different low charge/discharge rates that assured to be working at the linear regime of Tafel behavior. Specifically, charge-transfer resistance corresponds to the slope of the overvoltage variation with respect to the charge/discharge current, according to equation (1.5) (for more information, refer to subsection 2.2.2). It must be taken into account that results obtained from this last method also included the ohmic drop, resulting in the joint contribution of ohmic and charge-transfer resistances. 3.2.2. Impedance from current pulses One of the aims of the dissertation was to develop a methodology to measure SoH online during the battery operation. Because sinusoidal signals are not currently available during battery operation, we attempteded to measure impedance using squared signals, which are commonly used to charge/discharge the cells. For analysis simplicity, first essays were performed on 1 F Panasonic supercapacitors, which were composed of activated charcoal having a nominal voltage of 5.5 V. Supercapacitors were charged and discharged at constant current or by pulses (for further information refer to [72]). Data was monitored with an Agilent 34970A data acquisition system at a sampling rate of 2 s. Charge/discharge current and voltage profiles were transformed into the frequency domain in order to get information about the impedance of the supercapacitors, according to equation (3.4). The transformations were done with FFT routines provided in either Matlab or Pspice. We carefully selected the total measurement time of voltage and current signals and the sampling period to operate in the defined impedance frequency range (refer to subchapter 3.1.3). Moreover, in order to evaluate the quality of the results, SNR was calculated for the resulting impedance according to equations (3.12) and (3.13). The method was extended to battery impedance of a LCO cell (Microbattery). Its impedance was obtained from its response to an impulse signal. The advantage of injecting a very short pulse is that the main lobe of its Fourier transformation spreads to a wide frequency range (around 1 Hz) and it is almost flat in that range. No windowing was used in this analysis.
81 Impedance Measurements In order to validate the results, impedance was measured in both cases with Parstat 2273 potentiostat (Princeton Applied Research) with a frequency response analyzer unit. 3.3. Results 3.3.1. Impedance from EIS measurements 3.3.1.1. NMC cells The evolution of impedance with the SoC, represented in Nyquist diagram in Fig. 3.8, was composed of two semicircles, a pure ohmic effect at high frequencies and a diffusional branch at low frequencies. However, the two semicircles were not clearly distinguishable in all the evaluated SoCs at BoL because their characteristic frequencies were as similar one to the other that they were overlapped in frequency. The tendency of both the fresh and the aged cells was an increase of impedance towards the EoD, especially the impedance related to the lowest frequency semicircle. 40 60 80 100 120 140 160 0 -20 -40 -60 -80 -100 -120 -140 LGC2078 BoL - Im Z (m) LGC2078 BoL - Re Z (m) 99.2 % 78.6 % 58.5 % 31.5 % 16.5 % 0.6 % 0 % 40 60 80 100 120 140 160 0 -20 -40 -60 -80 -100 -120 -140 LGC2075 EoL - Im Z (m) LGC2075 EoL - Re Z (m) 100 % 77 % 51.8 % 26 % 7.25 % 0.65 % 0 % Fig. 3.8. Nyquist representation of impedance evolution with SoC of a LGC2078 fresh NMC cell (left) and LGC2075 degraded NMC cell (right). A zoom of this impedance at BoL and EoL is depicted in Fig. 3.9 and Fig. 3.10, respectively. Impedance of the fresh cell showed one semicircle in the Nyquist representation except at very low SoCs, where two semicircles could be appreciated (Fig. 3.9). Nevertheless, in the case of the degraded cell, the two effects were clearly distinguishable even when the cell was fully charged (Fig. 3.10). Ohmic resistance (R) at BoL and EoL, which was defined as the intersection of the impedance curve with the real-axis (refer to section 3.2.1.1), was roughly constant in all the SoC range (it increased around 5 % between SoC = 100 % and SoC = 0 %), as illustrated in Fig. 3.9. Chargetransfer resistance (RCT) slightly decreased at beginning of discharge, and then remained almost constant at the intermediate SoCs and finally increased towards the end of discharge. The same behavior was found at BoL and EoL. In literature, charge-transfer resistance was found to follow the same trend [85]. Moreover, although the contribution of the different charge-transfer effects were
Chapter 3 82 not quantified separately, it was clear to the eye that the semicircle at higher frequencies was almost independent of SoC but, conversely, the effect at lower frequencies was strongly dependent on it. Fig. 3.9. Zoom of Nyquist representation of impedance evolution with the SoC of a fresh NMC (LGC2078) cell (on the left) and dependency on SoC of the total resistance ( R + R CT), chargetransfer resistance ( R CT) and ohmic resistance ( R ) (on the right). Fig. 3.10. Zoom of Nyquist representation of impedance evolution with SoC of a degraded NMC (LGC2075) cell (on the left) and dependency on SoC of the total resistance ( R + R CT), chargetransfer resistance ( R CT) and ohmic resistance ( R ) (on the right). The absolute increase of ohmic and charge-transfer resistances from BoL to EoL (calculated as the difference between the resistance at the EoL and the resistance at BoL) was not constant in all SoCs (left part of Fig. 3.11). Ohmic resistance increased more at intermediate SoCs where the increase in charge-transfer resistance was lower. Moreover, the absolute increase of ohmic resistance was higher except at SoCs below 20 %, where it was higher for the charge-transfer resistance. Concerning the relative increase, it was found to be higher for the charge-transfer resistance in all SoC range (right part of Fig. 3.11). 40 50 60 70 80 90 100 110 120 0 -5 -10 -15 -20 -25 LGC2075 EoL - Im Z (m) LGC2075 EoL - Re Z (m) 100 % 77 % 51.8 % 26 % 7.25 % 0.65 % 0 % 100 80 60 40 20 0 0 20 40 60 80 100 120 140 Resistances (m) SoC (%) R + RCT R RCT 100 80 60 40 20 0 0 20 40 60 80 100 120 140 Resistances (m) SoC (%) R + RCT R RCT 40 50 60 70 80 90 100 110 120 0 -5 -10 -15 -20 -25 LGC2078 BoL - Im Z (m) LGC2078 BoL - Re Z (m) 99.2 % 78.6 % 58.5 % 31.5 % 16.5 % 0.6 % 0 %
83 Impedance Measurements 100 80 60 40 20 0 20 40 60 80 R RCT Relative increase of R (%) SoC (%) Fig. 3.11. (left) Absolute and relative (right) increases of ohmic and charge-transfer resistances of LGC2075 cell (NMC) from BoL to EoL. Impedances of fully charged NMC cells at different degradation levels were plotted in Fig. 3.12. At the beginning of life, only one semicircle was appreciated at SoC = 100 % but it separated into two identifiable effects as long as the cell aged. Although the resistances of those effects were not estimated separately, it was clearly seen that the more affected semicircle due to cycle aging was the one at lower frequencies. The characteristic frequency of this effect after 335 cycles was around 7.75 Hz (Fig. 3.12). 40 50 60 70 80 90 100 0 -4 -8 -12 -16 -20 -24 -28 7.75 Hz 0 60 120 220 285 335 Im Z (m) Re Z (m) Fig. 3.12. Nyquist representation of LGC2074 cell’s impedance at SoC = 100 % after 60, 120, 220, 285 and 335 cycles at a 1.5C discharge rate. Ohmic resistance increased linearly for the three evaluated NMC cells with comparable slopes (0.028 m·cycle-1) (Fig. 3.13). With respect to charge-transfer resistance, it was obtained by the two considered methods: from the radius of the semicircle of the Nyquist representation of impedance (right part of Fig. 3.13) and from the slope of the overpotential produced at three different charge/discharge rates (Fig. 3.14). An example of the polarization curve from which charge-transfer resistance was calculated from the measured overvoltages was plotted in Fig. 3.15. As mentioned 100 80 60 40 20 0 8 12 16 20 24 R RCT Absolute increase of R (m) SoC (%)
Chapter 3 84 previously, the resistance obtained from overvoltage measurements (represented in the left side of Fig. 3.14) also included the ohmic resistance effect. Thus, in order to be able to compare chargetransfer resistance obtained by the two methods, the ohmic contribution (estimated from impedance measurements) was subtracted from the resistance estimated from the V-I polarization curve (right side of Fig. 3.14). As it can be seen, comparable results were obtained by the two methods (right sides of Fig. 3.13 and Fig. 3.14). In particular, it could be appreciated that charge-transfer resistance increased more slowly during the first 100 – 150 cycles and then started increasing faster until the end of the cycling test. Similar values and the same trend in charge-transfer resistance with aging were found with both measurements methods. 050 100 150 200 250 300 350 400 15 20 25 30 35 40 45 50 55 60 Ohmic resistance (m) # cycle LGC2074 LGC2075 LGC2076 Slope = 0.028 m·cycle-1 050 100 150 200 250 300 350 400 15 20 25 30 35 40 45 50 55 60 LGC2074 LGC2075 LGC2076 RCT from impedance (m) # cycle Fig. 3.13. (left) Ohmic and (right) charge-transfer resistances evolution with aging of three LGC2 (NMC) cells at SoC = 100 % obtained by impedance spectroscopy. 050 100 150 200 250 300 350 400 55 60 65 70 75 80 85 90 95 100 LGC2074 LGC2075 LGC2076 RV-I (m) SoC (%) 050 100 150 200 250 300 350 400 15 20 25 30 35 40 45 50 55 60 LGC2074 LGC2075 LGC2076 RV-I - R (m) # cycle Fig. 3.14. (left) Charge-transfer resistance ( R V-I in that case) of three LGC2 (NMC) cells at SoC = 100 % obtained from the overpotential generated at different discharge rates (C/25, C/5 and 1C) (V-I polarization curve). It has to be noted that the measurement was also affected by ohmic conduction, thus resulting as the joint contribution of both ohmic and charge-transfer resistances. In the right part, the ohmic contribution represented in Fig. 3.13 was subtracted in order to compare the chargetransfer resistance obtained by the two methods. In the polarization curves, we noticed, on the one hand, that the overpotential at zero current did not tend to zero in any case (Fig. 3.15). On the other hand, the curves at zero current got different
85 Impedance Measurements values during charge and discharge. Thus, these effects might indicate hysteresis between the OCV curves obtained during charge and discharge [86]. A further analysis and explanation will be given in Chapter 4. Fig. 3.15. Polarization curve of a fresh LGC2074 cell (NMC) (left) and of the same cell after 325 cycles (right) obtained at C/25, C/5 and 1C charge/discharge rates. In the first 50 – 75 cycles, charge-transfer resistance decreased whereas the ohmic contribution increased (Fig. 3.16). From this cycle on and until cycles 150 – 200 were reached, the relative increases of ohmic and charge-transfer resistances at SoC = 100 % were comparable and followed a linear tendency. At this point, charge-transfer resistance started to increase faster than the ohmic effect did (which continued following the same linear tendency unlike charge-transfer resistance). From these results, it might be inferred that different degradation mechanisms were taking place at these various stages. Further analysis and possible causes will be discussed in subsection 3.4. 050 100 150 200 250 300 350 400 450 0 10 20 30 40 50 60 LGC2076 LGC2075 LGC2074 LGC2076 LGC2074 R RCT Relative increase of resistance (%) # cycle LGC2075 Fig. 3.16. Relative increases of ohmic and polarization resistances at SoC = 100 % during the cycle aging process of the three NMC cells. 0,0 0,5 1,0 1,5 2,0 2,5 3,0 -300 -200 -100 0 100 200 300 Overpotential at BoL (mV) Current (A) BoC BoD 0,0 0,5 1,0 1,5 2,0 2,5 3,0 -300 -200 -100 0 100 200 300 Overpotential at EoL (mV) Current (A) BoC BoD
Chapter 3 86 3.3.1.2. LFP cells 3.3.1.2.1. VIC cells Nyquist representation of impedance of VIC cells was illustrated in Fig. 3.17. In this figure, ohmic resistance was subtracted because cells were measured with different holders and setups, and thus, the comparison of ohmic resistances of VIC cells was not possible. However, during the first part of cycling the same holder was used for the impedance measurements making the results comparable at this first stage. Ohmic resistance evolution during these initial cycles was plotted in left part of Fig. 3.18. It underwent a fast increase during the initial 50 cycles and then the increase was moderated. Concerning charge-transfer resistance, it appeared as a single semicircle in the Nyquist representation at BoL, which decreased after the first initial cycles. Then, it remained almost constant until some point between cycles 300 and 400 from which a second effect was distinguishable at low frequencies. Fig. 3.17. Nyquist representation of two VIC cells (LFP) impedance at SoC = 100 % after being subjected to different number of cycles. Serial resistance contribution was subtracted and only the more representative cycles were represented. At the inset, full spectra of the VIC cells at SoC = 100 %. A quantitative estimation of the charge-transfer resistance during the cycle aging process was not carried out because no model was fit to the impedance spectra and it was not clear to the eye where the semicircles would cross the real axis. However, in order to track the evolution of impedance, the maximum resistance in the studied frequency range was defined as the addition of RCT and RMT (refer to subchapter 3.2.1.1) and it was represented in the right part of Fig. 3.18. It suffered a high decrease during the first 30 cycles and then it remained almost constant until the transition between cycle 300 and 400 where a sudden increase occurred. From that point until the end of the test, the resistance increased gradually. 025 50 75 100 125 150 175 0 -10 -20 -30 -40 -50 -60 -70 -80 -90 -100 Im Z (m) Re(Z)-min{Re(Z)} (m) 0 33 117 408 622 1049 VIC01 SoC = 100 % 0200 400 0 -300 -600 -900 025 50 75 100 125 150 175 0 -10 -20 -30 -40 -50 -60 -70 -80 -90 -100 Im Z (m) Re(Z)-min{Re(Z)} (m) 6 30 170 407 661 985 VIC02 SoC = 100 % 0200 400 0 -300 -600 -900
87 Impedance Measurements 050 100 150 200 250 300 49 50 51 52 53 54 55 56 VIC01 VIC02 Ohmic resistance (m) # cycle 0200 400 600 800 1000 160 200 240 280 320 360 400 440 480 VIC01 VIC02 RCT + RMT resistance (m) # cycle Fig. 3.18. (left) Ohmic resistance ( R ) evolution during the first cycles where the employed holder allowed the comparison of the data. (right) Total resistance evolution represented as the addition of charge-transfer and mass-transfer resistances. Lines were only drown as a guide to the eye. In addition, charge-transfer resistance obtained from the overvoltage produced at three different rates obtained from the characterization cycles was not comparable for these cells because the ohmic resistive effect, which was also included in the measurement, was not consistent during the test due to the lack of an appropriate holder. Although data were not comparable, it was depicted in Fig. 3.19 an example of how the charge-transfer resistance was calculated from its polarization curve. Charge and discharge overvoltage curves were expected to cross the y-axis at the same point but measurements followed different tendencies for charge and discharge processes what could be related to hysteresis. Further analysis will be carried out in Chapter 4. 0,0 0,1 0,2 0,3 0,4 0,5 -160 -120 -80 -40 0 40 80 120 160 Overpotential (mV) Current (A) BoC BoD Fig. 3.19. Charge-transfer resistance of VIC01 cell (LFP) at BoL obtained from the slope of the overvoltage produced at C/25, C/5 and 1C charge/discharge rates. 3.3.1.2.2. EVbat cells EVbat cells were the first cells evaluated in this study. In addition, we were not able to cycle them in our facilities because they were high capacity cells. Thus, they were sent to an external center in
Chapter 3 94 We also obtained the impedance profile by injecting a very short pulse. The interesting point of this methodology is that this short pulse would not change the state of charge of the cell or supercapacitor during the measurement. For supercapacitors, we injected a voltage pulse of 5 V and a duration of 1 ms; its current response was depicted in Fig. 3.29. In this case, since the signal was rather noisy, several measurements were carried out in order to average the results. Impedance was subsequently calculated with FFT transformations (see top part of Fig. 3.30). The real part showed a good agreement approximately between 8 mHz and 1 Hz and the imaginary part between 27 mHz and 1 Hz. Furthermore, the SNR was calculated in order to establish a quality threshold for the global result (bottom part in Fig. 3.30). The comparison between the EIS impedance measurement and the Fourier transform approximation showed a good agreement as long as the signal to noise ratio remained above 15 dB. 0100 200 300 400 500 600 -0,265 -0,260 -0,255 0,00 0,05 0,10 time (s) 1F 5.5V Current (A) 0 2 4 6 0,0 2,5 5,0 Voltage (V) Fig. 3.29. Current response to a pulsed signal of 5 V and 1 ms (inset) averaged for 10 samples. 10-3 10-2 10-1 100 -100 -50 0 50 10-3 10-2 10-1 100 0 10 20 Impedance () Re_EIS Im_EIS Re_impulse Im_impulse Frequency (Hz) SNR(dB) Fig. 3.30. Comparison between impedance of a supercapacitor of 1 F and 5.5 V measured using a potentiostat and injecting a pulsed signal. The SNR (bottom part) indicated that below 15 dB, no fitting was possible.
95 Impedance Measurements 3.3.2.2. LCO cells We evaluated impedance determination from pulsed signals in LCO cells. The injected current pulse was of 1 A (representing a rate of 1.35 C) and the time duration of the pulse was 1 s. Measured real and imaginary parts of LCO impedance were plotted together with the results of impedance obtained from our FFT transformations (Fig. 3.31). The results showed a good agreement with measured impedance in the considered frequency range. 10-3 10-2 10-1 100 -0,1 0,0 0,1 0,2 0,3 0,4 Impedance (m) Frequency (Hz) EIS - Re Z EIS - Im Z FFT - Re Z FFT - Im Z Fig. 3.31. Comparison between impedance of Microbattery LCO cell measured using a potentiostat and injecting a current pulse of 1 A during 1 s and doing FFT transformations of current and voltage profiles. 3.4. Discussions Once we have presented the results on EIS measurements and pulses approximations, we aim to first, evaluate the different impedance effects we had measured in the cells and then, explore the obtained benefits of each measurement procedure. In general, the identification of the physical processes occurring in a cell from impedance measurements is not an easy task. Commonly, impedance spectra show the effects occurring at both the positive and the negative electrodes. These effects overlap in frequency and thus they are indistinguishable in a regular EIS measurement. In this context, different approaches are possible: to measure half-cells, symmetric-cells or full-cells with a reference electrode, in order to identify the correspondence between the effects and the electrode producing them [87–89], or to carry out the impedance measurements at very low temperatures, so the effects occur in a slower rate and are easier to identify [87]. According to the development of the dissertation, we decided not to develop electrical models because this was not the main stream of this study, and we decided to qualitatively analyze the results. The half-cells analyses were carried out in the post-mortem, in Chapter 5.
Chapter 3 96 3.4.1. Impedance from EIS measurements 3.4.1.1. LGC2 cells (NMC) 3.4.1.1.1. SoC dependency The results showed a general increase of impedance when SoC was decreased. Similar trends were found in other studies [33,85,87,90]. Particularly, the ohmic resistance of the cell was almost SoC independent (right side of Fig. 3.9 and Fig. 3.10), as stated in [14,85,91]. Ohmic resistance R arises mainly from the contributions of the ionic and electronic conductivities coming from the electrolyte, the separator, and current collectors [36]. Specifically, electronic conductivity is SoC independent but ionic conductivity in the electrolyte depends on the concentration of ions [92]. Therefore, it would explain the variation in ohmic resistance with SoC. In our study, we did not separate the resistance contribution of each of the processes contributing to charge-transfer polarization. However, the effect at higher frequencies (around 75 Hz) was apparently not dependent on SoC (left side of Fig. 3.9 and Fig. 3.10). Nonetheless, the one at lower frequencies was strongly dependent on it. The same trend had already been found [87]. There, the process at lower frequencies was strongly SoC-dependent but the one at higher frequencies was also dependent but not as strong as the other effect. This effect at lower frequencies was associated to the charge transfer process at the positive electrode (found between 0.1 Hz and 1 Hz) and the one at higher frequencies was associated to the charge transfer at the negative electrode (around 10 Hz). Thus, charge transfer at PE was determined to be more dependent on SoC than what charge transfer was at the NE. In contrast, the effect at higher frequencies have also been associated to SEI layer resistance [90]. The same trend of charge-transfer resistance with SoC that we found was reported in [90]. It was concluded that charge-transfer resistance and SEI-layer resistance exhibited the greatest variation with SoC, showing a monotonic relationship with it [90]. However, it was not explained why the effect associated to SEI layer was found to be SoC-dependent. Nevertheless, a possible explanation was given in [87] and [93]. Stiaszny et al. proposed that SEI-diffusion was SoC-dependent because of a possible change in SEI surface topology due to a dendritic deposition of lithium during charge/discharge cycles [87]. The lower polarization contribution at high SoCs was associated to lithium-ion deposition onto these dendrites, thus not needing to pass through the entire SEI layer. Contrarily, in [93], the SoC-dependency of the resistive effect associated to the SEI layer was related to the expansion and contraction of the NE during the lithiation and delithiation processes. It is widely accepted that charge transfer effect is a strongly SoC-dependent process [90,93–97]. Therefore, we associated the effect at lower frequencies to a charge transfer process. However, it was not clear if the charge transfer process was occurring at either the positive or the negative electrode. In literature, it is mainly found that the negative electrode has a relatively small influence to full-cell impedance even though the SEI layer is thick [87,98]. Moreover, if we consider the results in [87], the effect at lower frequencies should have been associated to charge transfer at the PE because it
97 Impedance Measurements was the effect more dependent on SoC. However, post-mortem analysis is convenient for unequivocally determining the electrode causing each of the effects obtained at the impedance spectra. Half-cells or symmetrical-cells impedance measurements would clarify the results obtained from the full-cells. Post-mortem analysis of those particular cells will be developed in Chapter 5. 3.4.1.1.2. SoH tendency In our study, we found that NMC cells showed only one semicircle at first aging states that separated into two distinct effects during the aging process (Fig. 3.12). The same trend was found in references [33,36,85]. Cells being charged at a moderate rate of 1C and discharged at 2C and 3C at a temperature of 25 ºC were investigated in [33]. This was comparable to our methodology. Fresh cells showed a unique semicircle but a change in the shape of the impedance spectra was found after 200 cycles where the two semicircles were already distinguishable. These two contributions were related to the charge transfer effect and to the resistance and capacitance associated to the SEI layer. In that case, the separation in frequency of those electrochemical effects was associated to the growth of the SEI layer. Moreover, an increase of the ohmic resistance due to aging was also found. Jalkanen et al. also reported an increase in both ohmic and charge-transfer resistances [36]. One of the cells they considered was charged/discharged at 1C/1C rate at room temperature. This cell showed only one semicircle in the beginning of cycling, which separated into two differentiable effects after 500 cycles. These two processes became even more distinguishable with cell aging. They suggested the effect at higher frequencies was mainly due to the graphite negative electrode and its SEI-layer whereas the one at lower frequencies was attributed to the charge transfer resistance at the NMC positive electrode, which was the dominant one. Regarding to the ohmic resistance, its increase was associated to the lack of electrolyte, possible blockage of the separator pores and separator resistance increase due to lithium plating on graphite electrodes and the SEI-layer formed on the top of plating. In addition, in the study of Waag et al. two semicircles could be distinguished at the impedance spectra of the aged cells [85]. They related the one at lower frequencies to interfacial charge transfer and the effect at higher frequencies to the SEI layer. Furthermore, charge-transfer semicircle increased and shifted toward lower frequencies during the aging process and the SEI growth caused the increase of the high frequency semicircle. The same trend of charge transfer resistance increase and shifting to lower frequencies was also found in [87]. Moreover, all of previously mentioned references agreed that the semicircle at higher frequencies corresponded to the SEI layer and the one at lower frequencies was associated to a charge transfer process. However, contrarily to [33], we found that the effect associated to SEI layer was not the predominant contributor to impedance rise but the one associated to charge transfer. Similar results to ours were found in [36,85,87], in which NMC/graphite cells were measured except in [87], in which the cell was composed of LMO-NMC/graphite. In particular, it was found that charge-transfer semicircle associated to PE increased and shifted towards lower frequencies being the major contributor to impedance rise of both of them.
Chapter 3 98 The impedance rise is commonly associated to the SEI formation and to the degradation of the positive electrode [36,87]. In our study, we had not enough information to unequivocally determine the process or the electrode behind each measured effect. However, the ohmic and charge-transfer resistances increase at the same rate during the first 200 cycles represented in Fig. 3.16 (at SoC = 100 %) might indicate loss of lithium was the predominant aging affect. Nevertheless, charge-transfer resistance started increasing faster than ohmic resistance after 200 cycles. We associated this result to an additional aging mechanisms taking place as loss of active material. Moreover, we found that resistance rise was SoC dependent (Fig. 3.11). In all SoCs above 20 %, the increase in ohmic resistance during the aging test was higher than that of charge-transfer resistance. It suggested that the electrochemical reaction was slowed down at the last stages of discharge during the aging test. However, the relative increase was found to be larger in all SoC range in the case of charge-transfer resistance. In addition, for a better understanding and determination of the electrode responsible of each effect measured at the full-cell impedance, post-mortem analysis will be developed in Chapter 5. 3.4.1.2. VIC cells (LFP) The impedance of VIC cells was composed of an inductive tail at high frequencies, chargetransfer resistance represented by one or two semicircles at medium frequencies and a diffusional branch at low frequencies. The shape of the impedance spectra changed during the aging process (Fig. 3.17). The fresh cells showed only one semicircle which decreased during the first cycles until some point between 300 and 400 cycles where it separated into two distinguishable effects. A qualitative analysis was carried out in order to compare the data at different degradation levels. Ohmic resistance was only estimated in the first stages of cycling where the holder was optimized for measuring low impedance values in a repetitive way. It suffered a sharp increase in the first 50 cycles and then continued increasing but gradually, reducing its increasing rate (Fig. 3.18). Ohmic resistance rise during cell aging is commonly found in literature [34,50,99–101], and it is usually associated to reduced ionic conductivity of the electrolyte due to electrolyte decomposition and to the increased resistance of the separator. Regarding the charge-transfer resistance (calculated as the real part of impedance covered by the semicircles), all the effects contributing to it (charge-transfer effects at PE and NE and ohmic contributions with an associated capacitive effect) were overlapped in frequency. Thus, they showed up at the impedance spectra as one single semicircle at intermediate frequencies (Fig. 3.17). In the first part of cycling (from cycle 0 to cycle 300-400), charge-transfer resistance decreased. It was also manifested in Fig. 3.18 that RCT + RMT decreased sharply in the first 30-50 cycles and then stayed in those low values until the 400th cycle. Although expected to increase with aging, the same behavior was found in other publications [31,101,102]. Petzl et al. carried out accelerated aging tests at 4C rate at 50 ºC and they found that charge-transfer resistance decreased during the first cycles [101]. However, no explanation was given to it. In addition, Groot et al. found that the impedance decreased
99 Impedance Measurements slightly in the first few months of cycle aging [102]. It was associated to the decrease of the stoichiometric window where the maximum lithium available for insertion to the LiFePO4 was diminished. It was found that transport limitations in LFP were significant, especially towards the end of discharge (i.e. large values of y in LiyFePO4). Thus, if ymax decreases due to loss of cyclable lithium, smaller impedance might be expected due to the better rate capability of LFP in that operating window. Zavalis et al. found that all cells that were cycled in a wide SoC range showed a first decrease in charge-transfer resistance followed by an increase towards the EoL [31]. It was suggested that it might be linked to rapid change in the thickness of the SEI layer. Moreover, it was observed that the cells with an initial decrease of RCT resulted in an overall rapid aging pattern. Therefore, they proposed to consider the decrease in RCT as an early sign of a rapid aging. As previously mentioned, two electrochemical process were distinguishable after 300-400 cycles. Moreover, the minimum at the imaginary part situated at the beginning of the diffusion branch was no longer visible after the 400th cycle. That is the main reasons for which in Fig. 3.18 both the contributions of charge-transfer and diffusion resistances were plotted instead of charge-transfer resistance by itself. It was not clear where to separate the contribution of the semicircle and the diffusional branch. The minimum in imaginary impedance found at the beginning of the lowfrequency tail was either no longer visible in [103]. They found a substantial increase of impedance during cycle aging manifested in the expansion in the imaginary and real directions of the semicircle. Zhang et al. concluded through their model that the cell cycling appeared to mostly have caused structural changes in the porous structure. Those structural changes eliminated the minimum in imaginary impedance while keeping the length of the low-frequency tail almost constant. The same behavior was found in our results. In addition, the cells suffered a sudden and sharp increase of the joint contribution of RCT and RMT, which accounts for charge transfer effect and solid-state diffusion, between 300 and 400 cycles. This increase corresponds to the cycle in which the intermediate frequency effect was split into two distinguishable semicircles and the effect at lower frequencies was spread over the real and imaginary directions (Fig. 3.17). Thus, this effect pointed out that the highest contributor to impedance rise in that part of the test (not considering the ohmic resistance contribution) was the charge-transfer resistance rather than the diffusion phenomena. From cycle 400 until the end of the test (around 1000 cycles) total resistance (without R contribution) kept growing at a smaller but constant rate. It was also found in [104] a sudden increase of charge-transfer resistance between cycles 300 and 600. Yancheng et al. associated it to the increase of interfacial resistance that was induced by the catalytic growth of SEI layer due to iron impurities dissolved and deposited on the anode [104]. Nevertheless, the semicircle associated to interfacial resistance was the one at higher frequencies together with the current collector interfaces while the semicircle at lower frequencies was the one related to slower processes like charge transfer at the electrode/electrolyte interfaces [74,105–107]. This behavior was not found in our results as we found that the effect at lower frequencies was the one increasing. Thus,
Chapter 3 100 the increase in resistance found in our study was associated to the charge transfer process instead of SEI or current collector interfaces. However, it was not possible to determine which electrode was causing it only from impedance measurements. If data obtained from impedance measurements are compared to capacity evolution during the cycle aging process (refer to Chapter 2), many similarities can be found (Fig. 3.32). In fact, both impedance rise and capacity fade at low and moderate rates changed in trend when they were at the same cycling level (Fig. 3.32). Conversely, no direct relation between impedance rise and capacity fade was found in [99]. However, in [108] it was demonstrated that power fade and capacity fade were correlated. In our study, during the first 30 – 50 cycles where RCT + RMT impedance decreased, the total capacity of the cell at a rate of 2C increased (Fig. 3.32). This capacity rise at the first aging stages in LFP cells was found in other published studies [74,106,109,110]. However, only in [109] the effect was mentioned and a possible explanation was given. Lewerenz et al. associated it to the flow of active lithium between the inactive and the active parts of the negative electrode [109]. The inactive or passive part of the negative electrode corresponds to the geometric excess of negative electrode with respect to the positive one, which is commonly found in Li-ion batteries where the risk of lithium plating is aimed to be reduced. If lithium is shared between the passive and the active parts of the negative electrode, as suggested in [109], the effective active area for charge-transfer reaction to take place would increase. Thus, the resistance associated to it, RCT, would decrease, which would confirm the obtained results.
101 Impedance Measurements 0200 400 600 800 1000 0,34 0,36 0,38 0,40 0,42 0,44 0,46 0,48 VIC01 VIC02 Capacity (Ah) # cycle C/25 85 90 95 100 105 110 115 120 Normalized capacity (%) 0200 400 600 800 1000 320 340 360 380 400 420 440 Capacity (mAh) # cycle VIC01 Slope 1 Slope 2 Slope 3 2C 80 85 90 95 100 105 110 Normalized capacity (%) 0200 400 600 800 1000 160 200 240 280 320 360 400 440 480 VIC01 VIC02 RCT + RMT resistance (m) # cycle Fig. 3.32. Capacity evolution of a VIC cell measured at C/25 (top) and 2C (middle) showing the different tendencies found during the aging test. Charge-transfer and mass-transfer resistances evolution with aging measured at SoC = 100 % (bottom). Dashed lines represent the ranges in which different behaviors were appreciated. Summarizing, we found that ohmic resistance sharply increased during the first 50 cycles, then the increasing rate was lowered but no data after cycle 300 was available. The fast increase in serial resistance during the first aging stages might be associated to the initial SEI layer formation. In the first cycling stages, SEI layer is formed at a higher rate until it stabilizes and completely covers the negative electrode. Thus, electrolyte solvents and lithium ions are consumed during this process what significantly reduces the electrolyte conductivity and consequently increases the ohmic resistance
Chapter 3 102 [34,50,104]. Even though SEI formation was carried out prior to the aging test, it is possible that it was not completely formed during these formation cycles. Thus, resulting in this fast increase of ohmic resistance during the first cycles of the aging test. Regarding to charge-transfer resistance, it was found to be the main contributor to impedance rise after the 400th cycle. However, at the first stages of cycle aging, ohmic resistance was larger than charge-transfer resistance. Furthermore, the relative increase during this period was also higher for the ohmic resistance. Concerning the initial decrease in RCT, we associated it to the passive electrode effect where lithium was shared between the passive and active parts of the negative electrode, what would increase the effective area for the reaction to take place. 3.4.1.3. EVbat cells (LFP) 3.4.1.3.1. SoC dependency Only one semicircle was visible at intermediate frequencies in all SoC range (Fig. 3.20). Ohmic resistance was almost constant in the full SoC range. Nevertheless, total resistance was found to decrease between 100 % SoC and 80 % and increase towards the fully discharge state due to the SoC- dependency of the charge-transfer resistance. Same trends were found in [101] and [111] where ohmic resistance was almost SoC independent and RCT increased towards the EoD. Unfortunately, the different effects overlapped in frequency could not be separated only by means of impedance measurements at room temperature. 3.4.1.3.2. SoH tendency When impedance results were compared at different aging states, three of the four evaluated cells followed the expected tendency. EVbat_4 (400 cycles) started with a lower capacity than the rest of the cells and it was also cycled in a temperature-controlled environment what differed from the other cells. Thus, only EVbat_1 (50 cycles), EVbat_2 (100 cycles) and EVbat_3 (200 cycles) are going to be considered for the evolution of the resistances with aging represented in Fig. 3.21. The shape and evolution of ohmic and charge-transfer resistances followed the same tendencies with SoC independently of the degradation level. No comparable data from the fresh cells was available as their impedance was measured with different connections in a different holder what affected considerably the results. Therefore, the evolution of impedance during the aging process was compared between cycles 50 and 200. EVbat cells showed only one semicircle at intermediate frequencies at the impedance spectra. This shape was maintained during all the aging process as it was found in other studies [99,112]. Ohmic resistance increased almost linearly from the 50th cycle to the 200th (Fig. 3.24). Conversely, charge-transfer resistance highly decreased between cycles 50 and 100. Although it also decreased between cycles 100 and 200, the decreasing factor was much below (Fig. 3.24). In addition, total resistance slightly decreased between cycles 50 and 100 but increased between cycles 100 and
103 Impedance Measurements 200 due to the lower decrease in polarization resistance in that part of the aging process. Same trend was found in [99], where total resistance first decrease and then increased towards the EoL. 3.4.1.4. LCO cells The impedance variation with SoC of the LCO cells was dependent on aging (Fig. 3.25 and Fig. 3.26). A unique semicircle was appreciated at BoL except at very low SoCs (below 7 %) whereas two semicircles were distinguishable in all SoCs at the EoL. In particular, the semicircle at lower frequencies was strongly dependent on SoC while the one at higher frequencies seemed to be independent of it. The same trend was found in [113] and [114]. In these studies, the semi-arc at higher frequencies was associated to the SEI layer and the one at lower frequencies to the charge transfer process. Regarding to aging, the effect at lower frequencies drastically increased. The same behavior was found in literature [115,116]. Furthermore, ohmic resistance also suffered a high increase (Fig. 3.27). Schoenleber et al. found it to increase linearly during the aging test [116]. Unfortunately, we did not record the evolution of impedance at intermediate cycles so no comparison could be made. Moreover, we found that the increases in ohmic and charge-transfer resistances were SoC dependent (Fig. 3.27). The relative increase was higher in all SoC range for the charge-transfer resistance. However, in absolute values, ohmic resistance increased in a higher extent than charge-transfer resistance at SoCs above 45 %. 3.4.2. Impedance from charging profiles and pulsed signals Impedance obtained from charging profiles or other temporal signals are of high interest to avoid time-consuming measurements of EIS impedance at very low frequencies. The time required for EIS measurements is not the only drawback but also the need of generating ac signals at different frequencies and measure them in portable systems. Thus, it would require a non-simple specific hardware that would be an inconvenient for these applications. Good agreement, valid methodology. It was possible to establish a good understanding between the behaviour in the time and frequency domains. The supercapacitor EIS spectra showed that a pure capacitive effect is only found at frequencies below 1 mHz. When charging the supercapacitor in the time domain at a constant current of 10 mA, the time to complete the charge is around 500 s, whose reciprocal frequency is 2 mHz. Under these conditions, the charging process looks like an ideal capacitor. However, in the pulsed charge, where the charging time is 60 s, and the corresponding frequency lies around 16 mHz, the resistive effects related to charge distribution and the non-ideal capacitance behaviour lead to the current flow during the resting time of the pulse signal. In this frame, it is convenient to charge the supercapacitor at low frequency (around 1 mHz) in order to have a capacitive behaviour. As long as the frequency of the pulse signal increases, the resistive effect increases.
Chapter 4 110 We are interested in measuring the variation of heat when it is converted to or from a different form of energy. In that case, thermodynamics introduce the quasi-equilibrium processes. A quasiequilibrium process is defined as the transition of the system through a series of equilibrium states as it moves slowly and gradually from the initial state to the final state. Quasi-equilibrium processes are considered as reversible processes where dissipative effects are neglected [118]. Therefore, classical thermodynamics only deals with reversible processes, which are not frequent in nature, even working close to equilibrium. However, beyond classical thermodynamics, it is also possible to consider the thermodynamics of irreversible processes where time is considered as a variable of the system. A key concept in thermodynamics is the definition of state. For describing the microscopic state of a system, a very detailed knowledge about the behavior of the conforming particles would be required [119]. This is investigated in statistical mechanics but it is not of interest for our battery characterization. Nevertheless, we are interested in macroscopic systems, which can be defined with few variables. A thermodynamic system is a set of matter of fixed identity, around which a boundary can be drawn [120]. Those boundaries have to be imposed in order to differentiate the system itself from the exterior or the universe. Depending on how the systems interact with the exterior, they can be classified into isolated, closed or open systems (Fig. 4.1). Fig. 4.1. Thermodynamic systems classified depending on how they interact with the environment. Thermodynamic variables can be path functions or point (or state) functions. Path functions are those dependent on the path taken when going from one state to another state. As an example, work and heat are path-dependent thermodynamic variables. Conversely, a variable that is a point or state function only depends on the values of state 1 and state 2, what means that the change on it is independent from the path taken during the process. Typical macroscopic state variables are internal energy, volume, pressure, temperature, and mole numbers of the chemical constituents. It is useful to classify thermodynamic variables into extensive or intensive. Extensive variables are the ones that are proportional to the size of the system like volume and mole number. On the contrary, temperature or pressure are intensive variables, which are independent of the size. Isolated systems They do not exchange energy or matter with the exterior Closed systems They exchange energy with the exterior but not matter Open systems They exchange both energy and matter with the exterior
111 Energy and Entropy The fundamentals of thermodynamics are stated in four laws. Each law leads to the definition of some particular properties of a physical system that help us to understand and predict its operation. 4.1.1.1. Zeroth Law of Thermodynamics The Zeroth Law of Thermodynamics states that when two bodies are in contact at different temperatures, heat will be transferred from the hottest body to the colder one until both of them reach the same constant temperature [121]. The final temperature of both of them will be the weighted average between their two respective initial temperatures. At this point, they are considered to be in thermal equilibrium. Moreover, the processes driving the state of a system towards the equilibrium are irreversible in nature [122]. Therefore, those irreversible processes vanish when the equilibrium is reached. 4.1.1.2. First Law of Thermodynamics First Law of Thermodynamics describes energy conservation of a system. Energy is not created or destroyed but transformed and it can be present in form of heat or work. Internal energy variation is path independent so it only depends on the initial and final states. However, heat and work depend on the way they are obtained and therefore they are not state functions as internal energy is [122]. In a closed system, the internal energy variation Uf – Ui equals the contributions of the heat transferred, Q and the work done or obtained from the system, W (4.1). Heat is considered positive when enters the system and negative when leaves it. 𝑈𝑓−𝑈𝑖=𝑄+ 𝑊 (4.1) In the case in which ther are only infinitesimal variations of the thermodynamic coordinates in a closed system, the differential form of the first principle becomes more convenient (4.2). In cyclic processes, the variation of the internal energy of a system can be zero as it ends up at the same initial state [123]. 𝑑𝑈=𝑑𝑄+𝑑𝑊 (4.2) 4.1.1.3. Second Law of Thermodynamics Due to the implications of the Second Law, we develop here a brief general introduction.
Chapter 4 112 4.1.1.3.1. Origin of the Second Law Sadi Carnot analyzed the steam engines, which performed mechanical work from the flow of heat. From these studies, he identified the heat flow as the fundamental mechanism required for the generation of work. Second law of thermodynamics says that there is a limit in the maximum work that can be generated from heat engines and it is independent of the machine itself and the way it is generated; it only depends on the difference in temperature of the heat sources. Carnot published his results in 1824 but they did not attract much attention from the scientific community until ten years later, once he had already passed away, thanks to Émile Clapyron. The heat engines defined by Carnot (Fig. 4.2) consisted of an ideal gas that generate mechanical work (W) due to its change in volume that produced the flow of heat between two heat reservoirs (QH and QC) at different temperatures (TH and TC). Fig. 4.2. Schematic of Carnot heat engine [124]. Carnot stated that for achieving the maximum work, all changes in volume should occur with minimum temperature gradients formation so the changes in temperature are almost all due to volume expansion and not due to flow caused by temperature gradients. It could be achieved if the transfer of heat was done very slowly so the temperature of the reservoirs remained as uniform as possible. He stated that in the limit of infinitely slow heat transfer, the operation of a heat engine is a reversible process. It means that if the heat transfer from the hotter reservoir to the colder one produces an amount of work, the same amount of work can be used to transfer the same amount of heat from the colder to the hotter reservoir. He also defined the concept of cycle, in which after a sequence of states, the engine went back to its initial state ready for starting a new cycle again. Carnot defined that the maximum obtainable work would be the one produced by a reversible cyclic engine because producing more than that would mean that work is produced endlessly and this would not be possible. To calculate the efficiency of the process first law of thermodynamics has to be applied. In that case, we have that a part of the heat 𝑄𝐻 (Fig. 4.2) is going to be converted into work, 𝑊=𝜂·𝑄𝐻 and by the law of conservation of energy, we have that 𝑊=𝑄𝐻−𝑄𝐶. Thus, the efficiency can be expressed as stated by Carnot’s Theorem (4.3) in which 𝑓(𝑇1,𝑇2) is a function only
113 Energy and Entropy of temperatures 𝑇𝐻 and 𝑇𝐶. His observations allowed to define an absolute scale of temperature that is independent of the material property used to measure it. 𝜂=1−𝑄𝐶 𝑄𝐻=1−𝑓(𝑇𝐻,𝑇𝐶) (4.3) 4.1.1.3.2. Second Law of Thermodynamics The full importance of Carnot’s Theorem was realized by Rudolf Clausius, who introduced in 1865 the concept of entropy, S. This was a new physical quantity as fundamental and universal as energy. Clausius defined the term entropy from the closed integral (4.4) evaluated across a reversible path of arbitrary cycle by considering a cycle as an addition of an infinite number of Carnot cycles that differed by an infinitesimal amount T. Δ𝑆=∮𝑑𝑄 𝑇=0 (4.4) It can be inferred that in a reversible process between states A and B, the integral only depends on those states being independent of the path taken. Therefore, he defined entropy S, which means transformation in Greek, as a state function in a reversible process. 𝑆𝐵−𝑆𝐴=∫ 𝑑𝑄 𝑇 𝑜𝑟 𝐵 𝐴𝑑𝑆=𝑑𝑄 𝑇 (4.5) Recalling Carnot cycle example (Fig. 4.2) and if an irreversible cycle is considered, only a fraction of 𝑄𝐻 can be converted into useful work. Therefore, the amount of heat transferred to the cold reservoir 𝑄′𝐶 is going to be higher than 𝑄𝐶, yielding to equations (4.6) and (4.7). Total change of entropy of the irreversible engine (system) 𝑄𝐻 𝑇𝐻−𝑄𝐶′ 𝑇𝐶<0 (4.6) Total change of entropy of the reservoirs (exterior) (−𝑄𝐻) 𝑇𝐻−(−𝑄𝐶′) 𝑇𝐶>0 (4.7) General expressions for an arbitrary cycle are summarized in equations (4.8) and (4.9). Total entropy of the system does not change in a complete cycle even if it is reversible or irreversible. It is because after a complete cycle, the system returns to its initial state. What usually happens is that more heat is expelled to the exterior generally converting mechanical energy to heat through irreversible processes.
Chapter 4 114 For a reversible cycle: 𝑑𝑆=𝑑𝑄 𝑇 ∮𝑑𝑆=∮𝑑𝑄 𝑇=0 (4.8) For an irreversible cycle: 𝑑𝑆>𝑑𝑄 𝑇 ∮𝑑𝑆=0, ∮𝑑𝑄 𝑇<0 (4.9) A more general expression of entropy is derived in the framework of thermodynamics of irreversible processes. Entropy is obtained by separating two effects: deS that is the change of the system’s entropy due to exchange of energy and matter, and diS that is the change in entropy due to irreversible processes within the system (4.10). deS can be positive or negative while diS has to be greater or equal than zero. 𝑑𝑆=𝑑𝑒𝑆+𝑑𝑖𝑆 (4.10) There is no real system in nature that can go through a cycle and return to its initial state without increasing the entropy of the exterior. The entropy diS generated by the irreversible processes has to be discarded to the exterior as heat. This expression is a generalization of thermodynamics, in which both reversible and irreversible processes are represented by the Clausius inequality. 𝑑𝑆≥𝑑𝑄 𝑇 (4.11) The Second law clearly manifests the limitation that is present in all natural processes when converting heat to work. In particular, the aim of this thesis is to relate battery aging or SoH to the generation of entropy inside the cells due to irreversible processes or diS. 4.1.1.4. Third Law of Thermodynamics The Second law of thermodynamics, only allows us to calculate entropy variations. However, in 1906, Walther Nernst conclude that at the absolute zero of temperature the entropy of every chemically homogeneous solid or liquid body has a zero value [122]. Therefore, the Third Law states that an absolute value of entropy can be obtained. The physical basis of Nernst heat theorem is explained by quantum theory, which defines the behavior of matter at low temperature. 4.1.2. Heat transfer Heat can be transferred by conduction, convection, or radiation [118]. Conduction is the transmission of heat between two solids (or within one single solid) that is isolated and its parts are at different temperatures. The particles of the substance gain kinetic energy and collide between them
115 Energy and Entropy transmitting the heat from hotter to colder parts. Thus, a coefficient of thermal conductivity k can be defined for a particular material involved in a heat flow 𝑑𝑄𝑐𝑜𝑛𝑑 𝑑𝑡 ⁄ across an area A in a temperature gradient 𝑑𝑇𝑑𝑥 ⁄ in the x direction. 𝑑𝑄𝑐𝑜𝑛𝑑 𝑑𝑡 =𝐴·𝑘·𝑑𝑇 𝑑𝑥 (4.12) Convection occurs when the heat source is in contact with a liquid or gas. The convective heat generation rate is given as 𝑑𝑄𝑐𝑜𝑛𝑣 𝑑𝑡 =𝐴·ℎ·(𝑇𝑎−𝑇𝑏) (4.13) Where A is the surface area of the solid, h is the heat transfer coefficient, Ta is the solid’s surface temperature, and Tb is the fluid temperature. Radiation is the heat transmission between two bodies that do not need to be in physical contact. The heat flow due to radiation 𝑑𝑄𝑟𝑎𝑑 𝑑𝑡 ⁄ is proportional to the fourth power of temperature yielding the equation 𝑑𝑄𝑟𝑎𝑑 𝑑𝑡 =𝐴·𝜖·𝜎·(𝑇𝑎4−𝑇𝑏4) (4.14) Where 𝜖 is the emissivity of the body (it is equal to one for an ideal black body) and 𝜎 is the Stefan-Boltzmann constant (5.6703·10-8 W·m-2·K-4). In our work, radiation is irrelevant, conduction is a key process and, even though convection is present, it is not addressed in this work. 4.1.3. Heat capacity Heat capacity of a system is defined as the heat required to increase its temperature in T increment. If it happens that the temperature goes from Ti to Tf when transferring Q amounts of heat, then the average calorific capacity of the system can be defined (4.15). 𝐶𝑎𝑣𝑔=∆𝑄 ∆𝑇=∆𝑄 𝑇𝑓−𝑇𝑖 (4.15) When the final temperature tends to the initial one meaning that Q and temperature variation are small, the average calorific capacity tends to its instantaneous value (4.16). Moreover, the calorific
Chapter 4 116 capacity can be positive, negative or zero depending on the nature of the process and if it absorbs or releases heat. 𝐶=𝑑𝑄 𝑑𝑇 (4.16) The heat capacity is an extensive magnitude so it depends on the amount of material involved in the process (i. e. the mass of the system, m). Therefore, it is commonly represented as the specific heat (4.17). 𝑐=1 𝑚·𝑑𝑄 𝑑𝑇 (4.17) For example, in the simple case of a resistor in which a current I is flowing through it producing a voltage difference V on its terminals and a temperature variation of T during a t period, the specific heat would be 𝑐=1 𝑚·𝐼·𝑉·Δ𝑡 Δ𝑇 (4.18) Where the product I·V represents the dissipated power by the resistor in the form of heat [122]. 4.1.4. Entropy In the field of non-equilibrium thermodynamics, entropy production is described by the contribution of thermodynamic forces F and thermodynamic flows dX [122]. Flows of heat or matter occur due to thermodynamic forces. Therefore, the irreversible entropy change within the system (diS) is expressed as the product of the force that is producing it and the corresponding flow. 𝑑𝑖𝑆=𝐹·𝑑𝑋 (4.19) diS is always equal or greater than zero as extracted from equations (4.10) and (4.11), being zero at the ideal case of reversible processes. When a system can be divided into smaller subsystems, the total entropy is the contribution of all the entropies of the subsystems. All of them will also have the irreversible part of the generation of entropy that will be equal or greater than zero. These statements go beyond the classical thermodynamics where diS was only defined for isolated systems. The entropy exchange with the exterior is expressed in terms of heat and matter. Equation (4.20) represents the entropy exchanged in an open system where a flow of matter exists. For the case in which the system is closed, there is no matter exchange so the term (deS)matter does not contribute to
117 Energy and Entropy the exchanged entropy. In the more restrictive case of an isolated system, deS is equal to zero because there is exchange of neither heat nor matter. 𝑑𝑒𝑆=𝑑𝑈+𝑝·𝑑𝑉 𝑇+(𝑑𝑒𝑆)𝑚𝑎𝑡𝑡𝑒𝑟 (4.20) Some thermodynamic forces and the associated flows are summarized in Table 4.1. The thermodynamic flows are consequences of the thermodynamic forces [122]. Table 4.1. Thermodynamic forces and flows and the corresponding laws. Law Force Flow Flick Concentration gradient Matter Fourier Temperature gradient Heat Ohm Voltage gradient Electrical current 4.1.4.1. Particular cases of entropy production 4.1.4.1.1. Electrical circuit elements The generation rate of irreversible entropy is calculated from the generic equation (4.19). In the particular case of electrical circuit elements where a current is flowing, the thermodynamic force would be the voltage gradient (V/T) and the flow would be the electrical current (I), following the Ohm’s Law, what yields to equation (4.21) for the particular case of electrical circuits [122]. For a resistor, ( can be identified in (4.21) as the voltage across the element and dQ/dt as the electric current I. In this particular case, irreversible entropy is produced due to heat generated by the Joule effect. 𝑑𝑖𝑆 𝑑𝑡=(𝜙2−𝜙1) 𝑇·𝑑𝑄 𝑑𝑡=𝑉·𝐼 𝑇=𝑅·𝐼2 𝑇>0 (4.21) 4.1.4.1.2. Electrochemical cells The irreversible entropy production due to the ongoing overall reaction and the current flowing through an electrochemical cell (I) is described in equation (4.22) [122]. 𝑑𝑖𝑆 𝑑𝑡=𝐴𝑇·𝑑𝜉 𝑑𝑡 (4.22)
Chapter 4 118 Where, 𝐴 is the electrochemical affinity of the reaction and 𝜉 is the extent of the reaction [122]. Where, 𝐼=𝑛𝐹·𝑑𝜉 𝑑𝑡 (4.23) 𝑉=𝐴 𝑛𝐹=𝑂𝐶𝑉−𝑉𝑐𝑒𝑙𝑙 (4.24) Therefore, the resulting expression for the entropy production in an electrochemical cell would be as follows 𝑑𝑖𝑆 𝑑𝑡=(𝑂𝐶𝑉−𝑉𝑐𝑒𝑙𝑙)·𝐼 𝑇 (4.25) 4.1.4.1.3. Degradation and entropy From a theoretical perspective, entropy generation rate is a parameter that “is important in engineering because its product with the temperature is a measure of the degradation or dissipation of energy in engines, and its minimization may be useful to enhance their efficiency”[125]. This approach has been applied to the study of mechanical damage and wear in solid materials [126–129]. Khonsari and Amiri have carried out a comprehensive investigation of thermodynamics of mechanical failure [130]. Also, Naderi et al. have investigated heat generation during mechanical stress in beams and proposed an entropy threshold for damage assessment [129,131]. The electrical behavior following mechanical fatigue has also been evaluated, where mechanical damage has been related to electrical damage [126]. Basaran and Yan [127] have pioneered the introduction of entropy as a damage metric in electromigration characterization, i.e., lattice degradation due to electron scattering. Thus, the combination of current and voltage as electrical variables, along with entropy from thermodynamics, could lead to an accurate description of electrical damage [127,132,133]. Entropy has also been introduced for understanding the physics leading to the failure of oxides in order to obtain accurate models of their reliability [134,135]. Reversible entropy is widely used in adiabatic computing [136], where heat dissipation must be minimized, and in electrochemical battery research, for characterizing their SoC and SoH [137,138]. Recently, Amiri and Modarres [139] have reviewed the possibilities for successfully implementing entropy as a parameter for measurement and instrumentation. While mainly theoretical, they highlighted its viability in electrical and mechanical systems. Nonetheless, entropy has not yet reached maturity for system monitoring. .
119 Energy and Entropy 4.1.5. Energy conversion in batteries Energy is stored in batteries as a chemical energy, i.e., potential energy stored in the chemical bonds of the chemical reaction products. This change in energy related to the chemical bonds is termed as the enthalpy of the reaction, H, which represents the total chemical available energy. Notwithstanding, when a reaction takes place, heat is absorbed, breaking bonds (endothermic) or released, forming new bonds (exothermic) [122]. The amount of heat released or absorbed (exchanged with the environment) is equal to the reversible entropy variation S at a constant temperature, T. Therefore, the Gibbs free energy G accounts for the available energy to perform work (4.26). In particular, for electrochemical reactions, it defines the maximum available electrical energy after the chemical-electrical conversion [122]. Δ𝐺=Δ𝐻−𝑇·Δ𝑆 (4.26) The change in Gibbs free energy was already defined in equation (1.1) where it was directly related to the open-circuit voltage of a battery, OCV. Despite the maximum electrical energy stored in batteries is related to the OCV, the actual energy that can be extracted from the cell is below G, due to the fact that the cell is not ideal. In fact, the maximum obtainable work from a battery is related to the cell voltage at its output terminals, Vcell. The difference between them is energy dissipated as heat (i.e. irreversible loses). The generation of reversible entropy dSrev/dt associated to the reversible entropy change S is related to the variation of the OCV with temperature and the current I flowing through the cell [123] and it is expressed as (for a complete derivation of the expression of reversible heat refer to [140]): 𝑑𝑆𝑟𝑒𝑣 𝑑𝑡 =𝑑𝑄𝑟𝑒𝑣 𝑑𝑡 ⁄ 𝑇=𝑑(𝑂𝐶𝑉) 𝑑𝑇 ·𝑇·𝐼 𝑇=𝑑(𝑂𝐶𝑉) 𝑑𝑇 ·𝐼 (4.27) Where, the derivative of the OCV with respect to temperature is termed as the entropic coefficient. 4.2. Materials and Methods 4.2.1. Open Circuit Voltage (OCV) measurement In batteries, the OCV is defined as the difference in voltage between the electrodes when no current is flowing through them and when they are at chemical equilibrium. Chemical equilibrium is important because OCV is a thermodynamic parameter and consequently it has to be evaluated after the relaxation of the kinetic processes [48,141]. In this study, OCV was measured by three different methods. At the first stage of the research, OCV was measured after a resting period of 24 hours, independently of the charge/discharge rate
Chapter 4 126 100 80 60 40 20 0 -50 -40 -30 -20 -10 0 10 20 30 BoL EoL Hysteresis voltage (mV) SoC (%) Fig. 4.6. Hysteresis voltage at BoL and EoL calculated as the difference in OCV during charge and discharge measured by using the GITT technique. 4.3.1.2. Incremental capacity analysis Incremental capacity analysis was carried out to LGC2 cells (NMC). The results showed the evolution of the shape of peaks, their position and intensity during their cycle life at a charge rate of C/25 (Fig. 4.7). The major differences with cycles were found at peaks 2, 4 and 5. Peak 2 got higher amplitude as more cycles were carried out, peak 4 decreased in capacity and peak 5 shifted to higher voltages and decreased in intensity. From the analysis of the IC data with Alawa battery emulation toolbox [155], LLI and LAM were quantified during the cycle life of the cells (Table 4.2). The results suggested that during the first 100 cycles, the decrease in capacity was mainly due to LLI and loss of active material at the negative electrode. From cycle 107 to 322, they continued growing until the EoL and the positive electrode started losing active material. The associated capacity fades to these aging mechanisms were 4 % during the initial 100 cycles and 13 % during the full completion of the aging test.
127 Energy and Entropy 3,5 3,6 3,7 3,8 3,9 4,0 4,1 0 5 10 15 20 25 30 dQ·dV-1 (Ah·V-1) Cell voltage (V) cycle 6 cycle 107 cycle 322 Fig. 4.7. Incremental capacity curves during charge process at a C/25 rate upon cycling of LGC2074 cell (NMC). It has to be noticed that resistive contributions has been subtracted prior to the analysis. Table 4.2. Loss of active material (LAM) and loss of lithium inventory (LLI) during the aging test of LGC2074 cell (NMC). LAMLiNE LAMdeNE LAMLiPE LAMdePE LLI Capacity fade From cycle 6 to 107 - 2.5 % - - 5 % 4 % From cycle 6 to 322 0.5 % 10 % - 1.8 % 11.8 % 13 % 4.3.1.3. Overpotential 4.3.1.3.1. Close-to-equilibrium measurements Overpotential was calculated subtracting discharge voltage curves at C/25 from ps-OCV curves. In Fig. 4.8, overpotentials generated by two NMC cells that were aged in the same conditions were represented. In both cases, the overvoltage increased as the cell aged, showing a good repeatability of the results. However, at some SoCs the overpotential increased faster with aging than at others. 1 2 3 4 5 6 7
Chapter 4 128 Fig. 4.8. Evolution of the overpotential at C/25 obtained from the ps-OCV curve of two NMC cells (LGC2074 cell to the left and LGC2075 to the right) during their cycle life. Overpotential generated at NMC/Li and graphite/Li half-cells during discharge The overpotential generated at a C/25 discharge rate at positive and negative electrodes was calculated with the data obtained from the half-cells we build during the post-mortem analysis (detailed in Chapter 5) by the use of equation (4.32) [48]. The counter electrode was lithium metal in both cases. The represented SoCs in Fig. 4.9 and Fig. 4.10 do not correspond to the full cell SoC but to the half-cells SoC. In particular, PE SoC and NE SoC were calculated between the corresponding minimum and maximum cut-off voltages selected for the tests carried out at each of the electrodes, without accounting for the electrode’s matching at the full cell. 𝑂𝐶𝑉=𝑂𝐶𝑉𝑃𝐸−𝑂𝐶𝑉𝑁𝐸 (4.32) The OCV shifted mostly to lower voltage values in both the PE and NE electrodes, except for intermediate SoCs at the PE where it shifted to higher values (left part in Fig. 4.9 and Fig. 4.10). In addition, the overpotential increased in both electrodes (right parts in Fig. 4.9 and Fig. 4.10). The initial overvoltage of the fresh cell was higher at the negative electrode (around 20 mV in contrast to 10 mV found at the PE). However, the highest increase during the aging process was found at the positive electrode, going from those 10 mV at SoCs higher than 30 % to around 28 mV at the EoL. In contrast, the increase in overpotential between BoL and EoL at the NE was around 2 mV. Furthermore, overpotential curves showed a characteristic shape with peak pattern, which was maintained during the aging process of the cells. 100 80 60 40 20 0 10 20 30 40 50 60 70 LGC2074 overpotential (mV) SoC (%) cycle 6 cycle 107 cycle 206 cycle 322 100 80 60 40 20 0 10 20 30 40 50 60 70 LGC2075 overpotential (mV) SoC (%) cycle 6 cycle 106 cycle 154 cycle 358
129 Energy and Entropy 100 80 60 40 20 0 3,4 3,6 3,8 4,0 4,2 4,4 BoL EoL PE OCV (V) PE SoC (%) 100 80 60 40 20 0 0 20 40 60 80 100 240 300 360 BoL EoL PE overpotential (mV) PE SoC (%) Fig. 4.9. (left) OCV evolution with cycle aging and (right) overpotential evolution at C/25 with cycle aging of the Li/NMC half-cell. 100 80 60 40 20 0 0,0 0,1 0,2 0,5 1,0 1,5 2,0 BoL EoL NE OCV (V) 1 - NE SoC (%) 100 80 60 40 20 0 0 20 40 60 80 100 240 300 360 BoL EoL NE overpotential (mV) 1 - NE SoC (%) Fig. 4.10. (left) OCV evolution with cycle aging and (right) overpotential evolution at C/25 with cycle aging of the Li/Graphite half-cell. Although it was previously mentioned that PE SoC and NE SoC did not correspond to the actual SoC of the full-cell neither they corresponded to each other, they were assumed both equal to the PE SoC in order to make a rough approximation of the total generated overpotential at the full-cell. (Fig. 4.11). The highest contributor to overpotential at BoL was the NE. However, the overpotential generated at the PE suffered a higher increase from BoL to EoL making both contributions comparable. The addition of the overpotentials generated at both electrodes, maintained a characteristic peak of the NE at intermediate PE SoCs and a characteristic peak of the PE at low PE SoCs.
Chapter 4 130 100 80 60 40 20 0 0 50 100 150 400 600 800 NE PE NE + PE Oveportential at BoL (mV) SoC (%) 100 80 60 40 20 0 0 50 100 150 400 600 800 NE PE NE + PE Oveportential at EoL (mV) SoC (%) Fig. 4.11. Overpotential generated at the PE and NE electrodes measured in half-cell configurations discharged at a C/25 rate (NMC/Li and graphite/Li) at BoL (left) and EoL (right). PE and NE overpotentials were added without taking into account the matching of the electrodes in order to obtain a rough approximation of the overpotential generated at the full-cell. 4.3.1.3.2. Far-from-equilibrium measurements Overpotential was calculated at a discharge rate of 3C/2 as the difference in voltage between the ps-OCV and the cell voltage under this current (Fig. 4.12). The evolution with cycle aging showed an increase of the overpotential in all SoCs during the aging process. In all the evaluated cycles, the shape of the curve was maintained: the overvoltage was rather constant between 100 % and 60 %, then slightly decreased from 60 % to 50 %, and finally suffered a sharp increase between 50 % and the EoD. 100 80 60 40 20 0 0,25 0,30 0,35 0,40 0,45 0,50 0,55 0,60 0,65 0,70 Cycle 9 Cycle 80 Cycle 155 Cycle 236 Cycle 305 Overpotential at 3C/2 (V) SoC (%) Fig. 4.12. Overpotential generated in a NMC cell at a 3C/2 discharge rate at different aging stages. 4.3.1.3.3. GITT and ps-OCV approximations GITT-OCV and ps-OCV were compared in order to estimate the error introduced when using ps-OCV curves instead of the actual OCV of the cell. One particularity of the OCV curves obtained
131 Energy and Entropy from GITT measurements is that they account for hysteresis during charge and discharge, making them more accurate than ps-OCV. However, ps-OCV is a less time consuming technique and gives more resolution in the SoC range because the resolution is fixed by the Vcell measurement (relaxation periods before the measurements are not required). In Fig. 4.13, the overpotentials obtained by using the OCV obtained by the two methods were plotted at BoL (left) and at EoL (right). At SoC = 100 %, the difference in overvoltage obtained by the two methods (calculated as the difference between the overpotential calculated by GITT technique and the one obtained by the ps-OCV approximation) differed in less than 5 mV but then this difference went to 10 – 15 mV until 60 – 65 % SoC (Fig. 4.14). From here on, the difference decreased and stayed below 5 mV until SoC was 30 % from which both curves showed a negative error until SoC was 15 %. At that point, the difference increased sharply and positively until the EoD, where it was in between 50 mV and 60 mV. 100 80 60 40 20 0 0 20 40 60 80 100 from GITT at C/25 - BoL from ps-OCV at C/25 - BoL Overpotential at BoL (mV) SoC (%) 100 80 60 40 20 0 0 20 40 60 80 100 from GITT at C/25 - EoL from ps-OCV at C/25 - EoL Overpotential at EoL (mV) SoC (%) Fig. 4.13. Comparison of the overpotential generated at C/25 calculated from the discharge GITT OCV (line + markers) and the ps-OCV (solid line) at BoL (left) and at the EoL (right). 100 80 60 40 20 0 -20 -10 0 10 20 30 40 50 60 BoL EoL Error in overpotential at C/25 (mV) SoC (%) Fig. 4.14. Error in overpotential at C/25 introduced when using ps-OCV instead of GITT OCV during discharge at BoL and EoL
Chapter 4 132 4.3.1.3.4. Apparent resistance The apparent resistance was calculated as the overpotential divided by the discharge current. It was obtained at low and moderate rates at BoL and EoL (Fig. 4.15). The apparent resistance at a C/25 discharge rate was higher than that at 3C/2. Nevertheless, at both discharge rates, the associated resistance was higher at the EoL than at BoL. 100 80 60 40 20 0 0,0 0,1 0,2 0,3 0,4 0,5 0,6 0,7 BoL EoL Apparent resistance at C/25 () SoC (%) 100 80 60 40 20 0 0,0 0,1 0,2 0,3 0,4 0,5 0,6 0,7 BoL EoL Apparent resistance at 3C/2 () SoC (%) Fig. 4.15. Apparent resistance calculated from the overvoltage curves while discharging a NMC cell at C/25 (left) and at 3C/2 (right) rates. 4.3.1.3.5. Contributions to overpotential Contributions to overpotential at a C/25 discharge rate obtained from the discharge GITT-OCV were represented in Fig. 4.16 at BoL (left) and EoL (right). As it was explained at section Chapter 4, ohmic and activation polarizations were obtained from impedance measurements carried out in Chapter 3. Thus, estimated ohmic and charge-transfer resistances from impedance measurements were employed for calculating the corresponding overpotentials. The smallest contribution was due to the activation overpotential followed by the ohmic contribution. In our impedance study, the contribution of mass transfer effects was not estimated. However, it cannot be avoided during a complete discharge cycle in which most of the cases it becomes dominant. Therefore, concentration overpotential represented in Fig. 4.16 was obtained as the difference between total overpotential and ohmic and activation overpotentials. As it can be seen, concentration overpotential became dominant at these low discharge rates (C/25) in all SoC ranges at both BoL and EoL except at SoC around 25 % at BoL.
133 Energy and Entropy Fig. 4.16. Overpotential contributions at BoL (left) and EoL (right) while discharging the NMC cell at a C/25 rate at ambient temperature. Calculations were made with discharge GITT OCV. The overpotential generated at a discharge rate of 3C/2 was represented in Fig. 4.17. The increasing factor of the overpotential at this rate with respect to C/25 was around 10. Moreover, the different contributions were present in a different extent when compared to lower discharge rates (Fig. 4.16). In that case, the dominant effect was the one associated to ohmic conduction. Ohmic and activation polarizations were also obtained from the impedance data analyzed in Chapter 3. However, charge transfer resistance had to be recalculated in order to account for the dependence of this resistance to high currents. In addition, concentration polarization was calculated as the difference between total overpotential and the addition of ohmic and activation polarizations. In particular, concentration polarization started the discharge process being the less dominant effect but increased during the process exceeding ohmic and activation polarizations at the EoD. The same behavior at BoD was found at a discharge rate of C/25 (Fig. 4.16). 100 80 60 40 20 0 0,0 0,1 0,2 0,3 0,4 0,5 0,6 0,7 0,8 Total Ohmic Activation Concentration Overpotential contributions (V) SoC (%) 100 80 60 40 20 0 0,0 0,1 0,2 0,3 0,4 0,5 0,6 0,7 0,8 Total Ohmic Activation Concentration Overpotential contributions (V) SoC (%) Fig. 4.17. Overpotential contributions at BoL (left) and EoL (right) while discharging the NMC cell at a 3C/2 rate at ambient temperature. 100 80 60 40 20 0 0 10 20 30 40 50 60 70 80 90 100 Total Ohmic Activation Concentration Overpotential contributions (mV) SoC (%) 100 80 60 40 20 0 0 10 20 30 40 50 60 70 80 90 100 Total Ohmic Activation Concentration Overpotential contributions (mV) SoC (%)
Chapter 4 134 4.3.1.4. Entropy 4.3.1.4.1. Reversible entropy The entropic coefficient measured at different SoCs was obtained from the variation of the OCV with temperature (Fig. 4.18). In all the evaluated SoCs, the entropic coefficient got negative values. Thus, contributing additional heat during discharge and subtracting heat during charge. Moreover, no significant differences between BoL and EoL were found. 100 80 60 40 20 0 -0,7 -0,6 -0,5 -0,4 -0,3 -0,2 -0,1 0,0 Entropic coefficient (mV·K-1) SoC (%) BoL EoL Fig. 4.18. Derivative of the OCV with respect to temperature of a LGC2 cell (NMC) at BoL (black filled squares) and at the EoL (red unfilled circles). 4.3.1.4.2. Irreversible entropy Close-to-equilibrium measurements The generation rate of irreversible entropy at a C/25 discharge rate was obtained during the cycle life of two LGC2 cells (NMC) at room temperature (Fig. 4.19). Right and left figures in Fig. 4.19 represent the evolution of two NMC cells cycled in the same conditions, what showed a good repeatability of the results. diS showed a general increasing tendency as the cells were aged. However, in the first 100 cycles it decreased in the initial 15 - 20 % SoCs of the discharge process. Moreover, it was true for all cycles that at some particular SoCs, the increasing factor with aging of diS was lower. These particular SoCs were 60 % and the range between 25 % and 10 %. Similar results were obtained from the GITT OCV curves, as illustrated in Fig. 4.20 at BoL and EoL. When comparing the entropy production obtained from ps-OCV with the one obtained with GITT, it has to be taken into account the error in overpotential calculations we introduced in the ps-OCV approximation (Fig. 4.14).
135 Energy and Entropy Fig. 4.19. Evolution of the irreversible entropy generation rate obtained from the ps-OCV curve at C/25 of two NMC cells (LGC2074 cell to the left and LGC2075 to the right) during their cycle life. 100 80 60 40 20 0 0 10 20 30 40 BoL EoL diS/dt (W·K-1) SoC (%) Fig. 4.20. Irreversible entropy production in a NMC cell at BoL and EoL when discharged at a C/25 rate at ambient temperature. It was obtained from the OCV curves obtained from the GITT measurements. The different effects contributing to the generation rate of irreversible entropy at BoL and EoL were plotted in the left and right parts of Fig. 4.21. At a C/25 discharge rate, ohmic and activation effects were those that contributed least to the total generation rate. Thus, the generation rate of irreversible entropy associated to concentration polarization was the predominant effect, which increased faster towards the EoD. 100 80 60 40 20 0 0 5 10 15 20 25 30 diS/dt (W·K-1) SoC (%) cycle 6 cycle 107 cycle 206 cycle 322 100 80 60 40 20 0 0 5 10 15 20 25 30 diS/dt (W·K-1) SoC (%) cycle 6 cycle 106 cycle 154 cycle 358
Chapter 4 142 100 80 60 40 20 0 0 10 20 30 40 50 60 70 5 C - EoL 15 C - EoL 32 C - EoL diS at C/25 (W·K-1) SoC (%) 5 C - BoL 15 C - BoL 32 C - BoL Fig. 4.30. Evolution of the irreversible entropy generation rate with temperature at C/25 of a NMC cell at BoL (solid lines) and at the EoL (dashed lines). At the heat balance evaluated at a C/25 discharge rate at different temperatures (5 ºC, 15 ºC and 32 ºC), reversible heat was higher than the irreversible term especially at SoCs below 50 % (Fig. 4.31). Nevertheless, dQP suffered a high increase during the aging test (higher than dQS) especially at low temperatures (5 ºC) what made it comparable to dQS. Thus, total generation of heat (bottom in Fig. 4.31) also suffered the higher increase from BoL to EoL at 5 ºC. Moreover, relevant differences were not found between cycling the cells at 15 ºC and 32 ºC at a discharge rate of C/25.
143 Energy and Entropy 100 80 60 40 20 0 0 4 8 12 16 20 24 28 32 36 40 dQP at C/25 (mW) SoC (%) 5 C 15 C 32 C 100 80 60 40 20 0 0 4 8 12 16 20 24 28 32 36 40 dQS at C/25 (mW) SoC (%) 5 oC 15 oC 32 oC 100 80 60 40 20 0 0 4 8 12 16 20 24 28 32 36 40 dQTOTAL at C/25 (mW) SoC (%) 5 oC 15 oC 32 oC Fig. 4.31. Irreversible heat generation rate (topleft), reversible heat generation rate (topright), and total heat generation rate (bottom) at BoL (solid lines) and EoL (dashed lines) of a LGC2 cell (NMC) discharged at a rate of C/25 at different temperatures (5 ºC, 15 ºC and 32ºC). 4.3.2. LFP cells 4.3.2.1. VIC cells 4.3.2.1.1. Open circuit voltage Ps-OCV curves were obtained for VIC01 and VIC02 cells (LFP) at a charge/discharge rate of C/25 (Fig. 4.32). At high SoCs (between 70 % and 80 % depending on the cycle), the OCV started decreasing sooner as the cell was more aged. The first labeled plateau (1) in Fig. 4.32, maintained the same voltage value but lower percentage of SoC was employed on this plateau, as more cycled was the cell. Consequently, plateau (2) was reached sooner but it also maintained the same voltage value during cycling. Even though the SoC range covered by the plateau (2) was not decreased, the plateau was shifted to higher SoC values. In the case of plateau (3), it was also shifted to higher SoC values due to the decrease in plateau (1).
Chapter 4 144 Fig. 4.32. Pseudo-OCV evolution during cycle life of VIC01 cell (left) and VIC02 cell (right) calculated from charge/discharge voltage curves at C/25. Differences in the resulting ps-OCV curves calculated at different rates would mean that the measurements were not carried out slow enough so they were still affected by kinetics. Ps-OCV curves were obtained at C/25, C/50 and C/100 rates in order to compare the resulting OCV curves (Fig. 4.33). In the right part of Fig. 4.33, we can see the transitions between plateaus were slower at lower rates. Therefore, kinetic effects were affecting the measurements. Thus, if higher accuracies were required, ps-OCV at rates lower than C/25 (for instance, C/100) should be considered for these cells. However, discharging at lower rates means longer measurement times. Thus, working at C/25 instead of C/100 gives lower accuracies but reduces the measurement time at least in a factor 4. Fig. 4.33. (left) Cell voltage of a VIC cell (LFP) under different charge/discharge rates. (right) ps- OCV curves of a VIC cell (LFP) obtained at different charge/discharge rates. The OCV obtained from averaging (ps-OCV) and that obtained during charge and discharge by the GITT technique, were plotted in Fig. 4.34. In general, the ps-OCV curves stayed between charge and discharge GITT OCV curves. However, a higher mismatch was found between them at the EoL. Furthermore, the evolution of the GITT OCV obtained during discharge from BoL to EoL was 100 90 80 70 60 50 40 30 20 10 3,15 3,20 3,25 3,30 3,35 3,40 3,45 3,50 Cell Voltage (V) SoC (%) C/25 charge C/25 discharge C/50 charge C/50 discharge C/100 charge C/100 discharge 100 90 80 70 60 50 40 30 20 10 3,20 3,24 3,28 3,32 3,36 3,40 ps-OCV (V) SoC (%) C/25 C/50 C/100 100 80 60 40 20 3,15 3,20 3,25 3,30 3,35 3,40 3,45 ps-OCV (V) SoC (%) 6 33 201 396 610 823 1037 VIC01 100 80 60 40 20 3,15 3,20 3,25 3,30 3,35 3,40 3,45 ps-OCV (V) SoC (%) 6 94 362 585 801 1017 VIC02 1 2 3 1 2 3 1 2 3
145 Energy and Entropy depicted in Fig. 4.35. The curves followed the same tendency that we found with ps-OCV (Fig. 4.32) but the curves presented lower voltage values with the GITT technique. 100 80 60 40 20 0 2,5 2,6 3,15 3,20 3,25 3,30 3,35 3,40 GITT OCV - charge GITT OCV - discharge ps-OCV OCV at BoL (V) SoC (%) 100 80 60 40 20 0 2,5 2,6 3,15 3,20 3,25 3,30 3,35 3,40 OCV at EoL (V) SoC (%) GITT OCV - charge GITT OCV - discharge ps-OCV Fig. 4.34. Comparison of charge and discharge OCV curves of VIC cells (LFP) at BoL (left) and EoL (right) measured by GITT and ps-OCV. 100 80 60 40 20 0 2,5 2,6 3,15 3,20 3,25 3,30 3,35 3,40 discharge GITT_OCV (V) SoC (%) BoL EoL Fig. 4.35. Discharge OCV curves at BoL and EoL of a VIC cell (LFP) obtained from GITT measurements at ambient temperature. Hysteresis The voltage difference between OCV-GITT curves obtained during charge and discharge (hysteresis voltage) at both BoL and EoL was represented in Fig. 4.36. In general, hysteresis voltage increased as the SoC decreased. Considering the hysteresis in the SoC range between 95.5 % and 11.5%, hysteresis voltage stayed below 34 mV at BoL and 36 mV at EoL. Three different regions belonging to the three visible plateaus at the OCV curves (Fig. 4.32) were also distinguishable at the hysteresis curves. The region at highest SoCs showed the lowest hysteresis voltage, followed by the region at intermediate SoCs and then the one at lowest SoCs. Concerning to the effect of aging on
Chapter 4 146 the hysteresis voltage, it increased from BoL to EoL at some particular SoC ranges (between 80 % and 65 %, between 44 % and 28 % and below 10 %). In the other SoCs, it remained unchanged. 100 80 60 40 20 0 -100 -75 -50 -25 0 25 50 75 100 BoL EoL Hysteresis voltage (mV) SoC (%) Fig. 4.36. Hysteresis voltage of a VIC cell (LFP) calculated as the difference between charging and discharging GITT OCV curves at BoL and EoL. 4.3.2.1.1. Incremental capacity analysis Incremental capacity analysis was carried out to VIC cells. The results obtained at different aging levels were plotted in Fig. 4.37. The observed peaks correspond to the different stages of the graphite negative electrode (labeled from 1 to 5). This is because LFP electrodes exhibit a unique plateau that extends to almost all the SoC range. Thus, the peaks plotted in Fig. 4.37 correspond to lithium extraction from the graphite electrode. In particular, peaks 4 and 5 are related to the phenomena of Li+ deintercalation at stages LiC12 and LiC6, where most of the capacity is extracted [157]. As it can be appreciated, peaks 2, 3 and 4 remain almost unaffected by aging. However, peaks 1 and 5 decreased with aging. In other studies, the decrease in peaks 1 and 5 was assoaciated to LAMLiNE [158]. In addition, the additional decrease measured in peak 5 was attributed to LLI [37,158]. 3,20 3,25 3,30 -18 -16 -14 -12 -10 -8 -6 -4 -2 0 dQ·dV-1 (Ah·V-1) Cell Voltage (V) 33 201 396 610 823 1037 0200 400 600 800 1000 0,00 0,04 0,08 0,12 0,16 peak 1 peak 4 peak 5 Peak area (Ah) # cycle Fig. 4.37. Incremental capacity analysis of a VIC cell (LFP) at different SoH at a C/25 discharge rate. On the left, IC curves. On the right: evolution of the area of peaks. 1 5 4 2 3
147 Energy and Entropy 4.3.2.1.2. Overpotential Close-to-equilibrium measurements The overpotential produced in a VIC cell (LFP) at a C/25 discharge rate was obtained from the difference between ps-OCV and cell voltage (Fig. 4.38). The highest overvoltages were found at very low and very high SoC values. Overpotential at central SoCs showed two main peaks that were shifted to higher SoC values as long as cycling was carried out. Furthermore, during the first 400 - 450 cycles, the overpotential decreased to its lowest value from which started increasing until the EoL of the cells (Fig. 4.38). 100 80 60 40 20 0 20 25 30 35 200 300 400 6 33 209 408 622 835 1049 Overpotential at C/25 (mV) SoC (%) Fig. 4.38. Overpotential of a VIC cell (LFP) generated during a discharge at a C/25 rate and calculated from the ps-OCV at room temperature. Far-from-equilibrium measurements The overpotential generated in a VIC cell (LFP) subjected to a discharge rate of 2C was plotted in Fig. 4.39. In the SoC range between 90 % and 20 %, the overpotential generated increased between BoL and EoL. At SoCs below the 20 %, overpotentials at BoL and EoL were very similar but slightly higher at BoL.
Chapter 4 148 100 80 60 40 20 0 0 200 400 600 800 1000 1200 Overpotential at 2C (mV) SoC (%) BoL EoL Fig. 4.39. Overpotential generated in a VIC cell (LFP) at a 2C discharge rate evaluated at BoL (solid line) and EoL (dashed line). GITT and ps-OCV approximations The overpotential generated at a C/25 discharge rate was calculated from the ps-OCV and compared to the one obtained from the discharge GITT OCV (right side of Fig. 4.40). The generated overpotential was larger at BoL than at the EoL. In fact, it happened because the decrease in OCV due to the aging process was higher than the decrease in cell voltage at this rate (left side of Fig. 4.40). Moreover, regarding the differences between ps-OCV and GITT-OCV methods, their absolute values differed between 5 mV and 20 mV in the SoC range between 95 % and 10 % (Fig. 4.41). 100 80 60 40 20 0 2,0 2,4 3,15 3,20 3,25 3,30 3,35 3,40 Vcell BoL Vcell EoL OCV BoL OCV EoL Voltage (V) SoC (%) 100 80 60 40 20 0 10 15 20 25 30 35 200 400 600 BoL (GITT) EoL (GITT) BoL (ps-OCV) EoL (ps-OCV) Overpotential at C/25 (mV) SoC (%) Fig. 4.40. (left) Cell voltage of a VIC cell (LFP) at a discharge rate of C/25 and discharge OCV obtained from GITT measurements at BoL and EoL. (right) Comparison of the overpotential generated at a discharge rate of C/25 calculated from the discharge GITT OCV (line + markers) and the ps-OCV (lines) at BoL and EoL.
149 Energy and Entropy 100 80 60 40 20 0 -10 0 10 20 30 75 100 125 BoL EoL Error in OCV (mV) SoC (%) Fig. 4.41. Error in overpotential introduced when using ps-OCV instead of discharge GITT OCV at BoL and EoL. Overpotential obtained from GITT and ps-OCV approximations was also calculated at higher discharge rates (2C). No relevant differences were found between the two methods (Fig. 4.42) because the introduced error was below 20 mV (Fig. 4.41) and the produced overpotentials at 2C were above 200 mV and raised to more than 1 V at the EoD, what made the error not relevant when compared to low rates. 100 80 60 40 20 0 0 200 400 600 800 1000 1200 Overpotential at 2C (mV) Math X1 BoL (GITT) EoL (GITT) BoL (ps-OCV) EoL (ps-OCV) Fig. 4.42. Comparison of the overpotential generated in a VIC cell (LFP) at 2C discharge rate calculated from the discharge GITT OCV and ps-OCV. Apparent resistance Apparent resistance obtained from the overpotential produced at a C/25 discharge rate was represented in Fig. 4.43 at BoL and EoL. Except at SoCs between 20 % and 10 %, the apparent resistance was found to be larger at BoL.
Chapter 4 150 100 80 60 40 20 0 0,0 0,5 1,0 1,5 2,0 2,5 3,0 3,5 20 30 40 50 BoL EoL Apparent resistance at C/25 () SoC (%) Fig. 4.43. Apparent resistance of a VIC cell (LFP) at a discharge rate of C/25 represented at BoL and EoL. It was calculated from OCV values coming from GITT tests. The apparent resistance at high rates (2C) represented in Fig. 4.44 was much lower than that a C/25 rate, (Fig. 4.43). Concretely, the apparent resistance is calculated from the overpotential divided by the current that produced it. Thus, as the overpotential was around 8 times higher at 2C and the ratio between currents was 50, it yield to an apparent resistance around 6 times smaller at high rates. Furthermore, the apparent resistance at high rates was larger at the EoL except at SoCs below 20 %. 100 80 60 40 20 0 0,0 0,2 0,4 0,6 0,8 1,0 1,2 1,4 Apparent resistance at 2C () SoC (%) BoL EoL Fig. 4.44. Apparent resistance of a VIC cell (LFP) at a discharge rate of 2C represented at BoL and EoL. It was calculated from OCV values coming from GITT tests. Contributions to overpotential Different contributions to overpotential at BoL during a discharge at a C/25 and 2C rates were plotted in Fig. 4.45. Due to the fact that impedance of those cells was only measured at SoC equal to 100 %, the ohmic contribution was estimated from the impedance measured at this SoC and it was considered to be constant in all the SoC range. Furthermore, charge transfer resistance was also
151 Energy and Entropy measured at SoC = 100 %. Even though it is known that charge transfer resistance is strongly dependent on SoC, as its contribution to total polarization was small compared to concentration polarization, it was also assumed to be constant in all the SoC range. In addition, different contributions were only represented at BoL because a different holder was employed at the EoL what gave non-comparable results (for further information refer to Chapter 3). Moreover, at both discharge rates, the major contributor was the concentration polarization, which in both cases increased sharply towards the EoD. 100 80 60 40 20 0 0 10 20 30 500 600 700 Total Ohmic Activation Concentration Overpotential contributions (mV) SoC (%) 100 80 60 40 20 0 0 200 400 600 800 1000 1200 Total Ohmic Activation Concentration Overpotential contributions (mV) SoC (%) Fig. 4.45. Different contributions to overpotential of a VIC cell (LFP) at BoL subjected to a discharge at a rate of C/25 (left) and 2C (right). 4.3.2.1.3. Entropy Reversible entropy The entropic coefficient was calculated as the derivative of the OCV with temperature. The results at BoL and EoL were plotted in Fig. 4.46. As it can be seen, similar trends were found at BoL and EoL. The entropic coefficient showed positive values for high SoCs above 20 % - 30 % and became negative for lower SoCs. Therefore, during discharge, heat would be subtracted from the dissipative effect (refer to equation (4.31)) at SoCs above 30 % and heat will be added at the last stages of discharge.
Chapter 7 254 6. A good approximation of EIS impedance was obtained from the FFT transforms of constant/pulsed charge/discharge profiles of a supercapacitor and the impulse response of a LCO cell. Chapter 4 – On energetic and entropic characterization 7. OCV depended on the aging level in all the evaluated chemistries. 8. Hysteresis was dependent on the aging level. 9. Ohmic, activation and polarization contributions were separated from the total overpotential at low and high discharge rates. 10. Concentration polarization was the dominant effect at low discharge rates. 11. Ohmic contribution was the dominant effect at high rates, except for LFP cells in which concentration polarization was the major contributor. 12. In reversible entropy, great differences in the entropic coefficient between BoL and EoL were not appreciated. 13. The irreversible entropy production was calculated from the measured overpotential at different rates and aging levels. 14. At low rates, NMC cells produced irreversible entropy faster at the EoL than at BoL. 15. At low rates, VIC cells (LFP) showed first a decrease in the generation rate of irreversible entropy and then an increase during the aging process. 16. At low rates, in EVbat cells (LFP) discharged at a C/8 rate, the entropy production remained almost constant during the aging process. 17. At low rates, LCO cells increased their generation rate of irreversible entropy from BoL to EoL in all the SoC range. 18. At high rates, the irreversible entropy production was larger at the EoL than at BoL in the two evaluated cells (NMC and VIC) except at SoCs below 20 % in the case of VIC cells. 19. At high rates, the major contributors were ohmic (NMC) and concentration polarization (VIC) terms. 20. We found that the heat generation during discharge at high and low rates was exothermic in all cases except in LFP. Chapter 5 – On post-mortem characterization of NMC cells 21. Heterogeneous pressure was detected along the electrodes during cycling. 22. The highest capacity fade was found at the inner parts of NE and PE. 23. The most relevant possible causes of capacity fade at the NE were isolation of the active material and changes in the crystal structure.
255 General Conclusions 24. The most probably causes of capacity fade at PE were particle isolation, metals dissolution and changes in the crystal structure. 25. Contributions to capacity fade at the full-cell such as LLI, LAM and increase in overpotentials were quantified. Chapter 6 – Overall discussions 26. We introduced a new parameter for system degradation characterization, the Relative- Entropy-Production or REP, defined as the irreversible entropy generation ratio at actual state and the initial state. 27. A relation was found between capacity fade and impedance rise. 28. The ongoing aging mechanisms in the NMC cells during the aging process were determined. 29. A relation between irreversible entropy production and transitions between two-phase and single-phase domains was found. 30. Local maxims in irreversible entropy production were found at the last stages of phase transformations. 31. In NMC cells, REP was below 1 at low and high rates. 32. In NMC cells and at both discharge rates, the concentration term, which includes the irreversible entropy production due to aging (diSaging/dt), was the one increasing more during the aging test. Therefore, or the diffusion process was the more affected by degradation (if the term diSheat/dt related to diffusion was the one increasing more) or more energy was being used in general to degrade the cell (increase related to the term diSaging/dt). 33. Tracking REP at high rates in NMC cells during the cycle life allowed the detection of enhanced degradation. 34. In VIC cells (LFP), REP was mostly below 1 at low rates and above 1 at high rates. We associated the decrease in REP at low rates to a decrease in the irreversible entropy production due to aging. 35. It was deduced from REP that the most affected part due to aging in EVbat cells evaluated at low rates was the one associated to ohmic resistance. 36. In the SoC ranges belonging to solid-solution phases, minimum differences between entropy generation at BoL and EoL were appreciated in all the evaluated chemistries. 37. Comparable values of REP were obtained independently of the rate in the case of NMC, LFP (high rates) and LCO.
Chapter 7 256 7.1. Future work Future analysis of already available data Fit a model to the impedance data Processing data of EVbat cells at high rates Process data of post-mortem analysis of VIC cells Local entropy production from half-cells Entropy production during charge Analysis of the formation cycles Estimate the matching of the electrodes in NMC cells from half-cell measurements Other approaches to be carried out Measure impedance at different temperatures Thermal impedance GITT OCV measurements at intermediate SoHs Impedance during charge Measurement of the dissipated heat with a calorimeter Measurement or estimation of the internal temperature of the cells 7.2. Research lines derived from this study Due to the fact that batteries are complex systems that undergo many degradation mechanisms during their life cycle, we decided to evaluate the entropy production in simplier systems such resistors and capacitors. Concretely, resistors and capacitors were chosen because batteries show resistive and capacitive behavior [172,194]. In these studies, we investigated entropy evolution to characterize commercial resistor or capacitor damage, with the aim of generalizing the effects for any dissipative/capacitive system. Our objective was to demonstrate that entropy is a valuable parameter for studying resistor and capacitor deterioration, even more so than resistance and capacitance. In fact, both resistance and capacitance can increase or decrease due to degradation.
257 References [1] D. Linden, T.B. Reddy, “Handbook of batteries,” McGraw-Hill, 2001. doi:10.1016/0378- 7753(86)80059-3. [2] D.F. Warne, “Electrical Power Engineer’s Handbook,” Newnes, 2005. [3] C. Daniel, “Materials and processing for lithium-ion batteries,” J. Miner. Met. Mater. Soc. 60 (2008) 43–48. doi:10.1007/s11837-008-0116-x. [4] R. Huggins, “Energy Storage,” Springer, 2010. doi:10.1002/9781118671603.ch8. [5] PMBL Limited, “History of the Lithium Ion Battery,” (n.d.). http://www.pmbl.co.uk/blog/lithium-ion-battery-history (accessed July 2, 2017). [6] I. Buchmann, “Basics about Batteries,” (2014). http://www.cadex.com/en/batteries/basicsabout-batteries (accessed July 1, 2017). [7] Sanyo, “Types of Battery Cells; Cylindrical Cell, Button Cell, Pouch Cell,” Batter. Univ. (2016) 1. http://batteryuniversity.com/learn/article/types_of_battery_cells (accessed July 1, 2017). [8] I. Buchmann, “Battery packaging - a look at old and new systems,” (n.d.). http://batteryuniversity.com/learn/article/battery_packaging_a_look_at_old_and_new_sys tems (accessed July 1, 2017). [9] MTI Corp, “Find Crystal by Application,” (2013) 2013. http://www.mtixtl.com/ (accessed July 1, 2017). [10] CNET, “International Battery expands for utility storage,” (n.d.). https://www.cnet.com/news/international-battery-expands-for-utility-storage/ (accessed July 1, 2017). [11] P. Taheri, A. Mansouri, B. Schweitzer, M. Yazdanpour, M. Bahrami, “Electrical Constriction Resistance in Current Collectors of Large-Scale Lithium-Ion Batteries,” J. Electrochem. Soc. 160 (2013) A1731–A1740. doi:10.1149/2.041310jes. [12] M.M. Doeff, Battery Cathodes, in: Encycl. Sustain. Sci. Technol., 2013: pp. 5–49. doi:10.1007/978-1-4419-0851-3. [13] B. Isidor, “Types of Lithium-ion Batteries – Battery University,” Cadex Electron. Inc. (2016) 1– 16. http://batteryuniversity.com/learn/article/types_of_lithium_ion (accessed July 1, 2017). [14] J.N. Illig, Physically based Impedance Modelling of Lithium-ion Cells, KIT Scientific Publishing, 2014. doi:10.5445/KSP/1000042281. [15] C.D. Rahn, C.-Y. Wang, “Battery Systems Engineering,” 2013. doi:10.1002/9781118517048. [16] J.S. Newman, K. Thomas-Alyea, “Electrochemical systems,” J. Wiley, 2004. [17] J.B. Gerschler, D.U. Sauer, “Investigation of open-circuit-voltage behaviour of lithium-ion batteries with various cathode materials under special consideration of voltage equalisation phenomena,” 24th Int. Batter. Hybrid Fuel Cell Electr. Veh. Symp. Exhib. 2009, EVS 24. 3 (2009) 1550–1563. [18] M. Heβ, “Kinetics and stage transitions of graphite for lithium-ion batteries,” 2013.
258 doi:10.3929/ethz-a-010000442. [19] “Does-the-voltage-of-a-Li-Ion-get-lower-as-it-discharges,” (n.d.). https://www.quora.com/Does-the-voltage-of-a-Li-Ion-get-lower-as-it-discharges. [20] “AN023 | Richtek Technology,” (n.d.). http://www.richtek.com/en/Design Support/Technical Document/AN023 (accessed July 11, 2017). [21] I.H. Buchberger, Electrochemical and structural investigations on lithium-ion battery materials and related degradation processes, 2016. https://mediatum.ub.tum.de/doc/1311652/1311652.pdf (accessed May 31, 2017). [22] B. Saha, P. Quach, K. Goebel, “Exploring the model design space for battery health management,” Annu. Conf. Progn. Heal. Manag. Soc. (2011) 1–8. [23] J.-K. Park, “Principles and Applications of Lithium Secondary Batteries,” Wiley-VCH, 2013. [24] V.R. Stamenkovic, B. Fowler, B.S. Mun, G. Wang, P.N. Ross, C. a Lucas, N.M. Marković, C. Song, Y. Tang, J. Lu, J. Zhang, H. Wang, J. Shen, S. Mcdermid, J. Li, P. Kozak, P. Pietrasz, B. Orr, T. Simes, A. Staff, S. Daniel, C. Lim, “III . Reaction Kinetics Lecture 1 3 : Butler- Volmer equation,” Science. 315 (2007) 493–7. doi:10.1016/j.electacta.2006.09.008. [25] M.V. Tibor Erdey-Grúz, “Zeitschrift für physikalische Chemie, Abteilung A, Chemische Thermodynamik, Kinetik, Elektrochemie, Eigenschaftslehre,” 1930. http://wikivisually.com/lang-de/wiki/Butler-Volmer-Gleichung (accessed May 15, 2017). [26] E.J. Calvo, The Current-Potential Relationship, in: Encycl. Electrochem., Wiley-VCH Verlag GmbH & Co. KGaA, Weinheim, Germany, 2007: pp. 3–30. doi:10.1002/9783527610426.bard020101. [27] P. Liu, J. Wang, J. Hicks-Garner, E. Sherman, S. Soukiazian, M. Verbrugge, H. Tataria, J. Musser, P. Finamore, “Aging Mechanisms of LiFePO4 Batteries Deduced by Electrochemical and Structural Analyses,” J. Electrochem. Soc. 157 (2010) A499. doi:10.1149/1.3294790. [28] Y. Gao, J. Jiang, C. Zhang, W. Zhang, Z. Ma, Y. Jiang, “Lithium-ion battery aging mechanisms and life model under different charging stresses,” J. Power Sources. 356 (2017) 103–114. doi:10.1016/j.jpowsour.2017.04.084. [29] C. Lin, A. Tang, H. Mu, W. Wang, C. Wang, “Aging mechanisms of electrode materials in lithium-ion batteries for electric vehicles,” J. Chem. (2015) 1–11. doi:10.1155/2015/104673. [30] M. Broussely, “Aging Mechanisms and Calendar-Life Predictions in Lithium-Ion Batteries,” Adv. Lithium-Ion Batter. (2002) 293–432. doi:10.1007/0-306-47508-1_14. [31] J. Groot, State-of-health estimation of Li-ion batteries: cycle life test methods, Chalmers University of Technology, 2012. [32] T. Waldmann, M. Wilka, M. Kasper, M. Fleischhammer, M. Wohlfahrt-Mehrens, “Temperature dependent ageing mechanisms in Lithium-ion batteries – A Post-Mortem study,” J. Power Sources. 262 (2014) 129–135. doi:10.1016/j.jpowsour.2014.03.112. [33] R. Arunachala, K. Makinejad, S. Athlekar, A. Jossen, J. Garche, Cycle life characterisation of
259 large format lithium-ion cells, in: 2013 World Electr. Veh. Symp. Exhib. EVS 2014, 2014. doi:10.1109/EVS.2013.6914865. [34] E. Prada, D. Di Domenico, Y. Creff, J. Bernard, V. Sauvant-moynot, F. Huet, “A Simplified Electrochemical and Thermal Aging Model of LiFePO4-Graphite Li-ion Batteries : Power and Capacity Fade Simulations,” J. Electrochem. Soc. 160 (2013) A616–A628. doi:10.1149/2.053304jes. [35] J. Vetter, P. Novák, M.R. Wagner, C. Veit, K.C. Möller, J.O. Besenhard, M. Winter, M. Wohlfahrt-Mehrens, C. Vogler, A. Hammouche, “Ageing mechanisms in lithium-ion batteries,” J. Power Sources. 147 (2005) 269–281. doi:10.1016/j.jpowsour.2005.01.006. [36] K. Jalkanen, J. Karppinen, L. Skogström, T. Laurila, M. Nisula, K. Vuorilehto, “Cycle aging of commercial NMC/graphite pouch cells at different temperatures,” Appl. Energy. 154 (2015) 160–172. doi:10.1016/j.apenergy.2015.04.110. [37] E. Sarasketa-Zabala, F. Aguesse, I. Villarreal, L.M. Rodriguez-Martinez, C.M. López, P. Kubiak, “Understanding lithium inventory loss and sudden performance fade in cylindrical cells during cycling with deep-discharge steps,” J. Phys. Chem. C. 119 (2015) 896–906. doi:10.1021/jp510071d. [38] E. Ignatev, Performance Degradation Modelling and Techno-Economic Analysis of Lithium- Ion Battery Energy, Lappeenranta University of Technology, 2016. [39] S.J. An, J. Li, C. Daniel, D. Mohanty, S. Nagpure, D.L. Wood, “The state of understanding of the lithium-ion-battery graphite solid electrolyte interphase (SEI) and its relationship to formation cycling,” Carbon N. Y. 105 (2016) 52–76. doi:10.1016/j.carbon.2016.04.008. [40] R. Fu, S.Y. Choe, V. Agubra, J. Fergus, “Development of a physics-based degradation model for lithium ion polymer batteries considering side reactions,” J. Power Sources. 278 (2015) 506– 521. doi:10.1016/j.jpowsour.2014.12.059. [41] Z. Li, J. Huang, B.Y. Liaw, J. Zhang, “On state-of-charge determination for lithium-ion batteries,” J. Power Sources. 348 (2017) 281–301. doi:10.1016/j.jpowsour.2017.03.001. [42] W.-Y. Chang, “The State of Charge Estimating Methods for Battery: A Review,” ISRN Appl. Math. 2013 (2013) 1–7. doi:10.1155/2013/953792. [43] M. Murnane, A. Ghazel, “A Closer Look at State of Charge (SOC) and State of Health (SOH) Estimation Techniques for Batteries,” n.d. http://www.analog.com/media/en/technicaldocumentation/technical-articles/A-Closer-Look-at-State-Of-Charge-and-State-Health- Estimation-Techniques-....pdf (accessed July 3, 2017). [44] S. Piller, M. Perrin, A. Jossen, “Methods for state-of-charge determination and their applications,” J. Power Sources. 96 (2001) 113–120. doi:10.1016/S0378-7753(01)00560-2. [45] W. Waag, C. Fleischer, D.U. Sauer, “Critical review of the methods for monitoring of lithiumion batteries in electric and hybrid vehicles,” J. Power Sources. 258 (2014) 321–339. doi:10.1016/j.jpowsour.2014.02.064.
260 [46] L. Lu, X. Han, J. Li, J. Hua, M. Ouyang, “A review on the key issues for lithium-ion battery management in electric vehicles,” J. Power Sources. 226 (2013) 272–288. doi:10.1016/j.jpowsour.2012.10.060. [47] V. Pop, “Battery management systems : accurate state-of-charge indication for battery powered applications,” Springer, 2008. [48] C.R. Birkl, E. McTurk, M.R. Roberts, P.G. Bruce, D.A. Howey, “A Parametric Open Circuit Voltage Model for Lithium Ion Batteries,” J. Electrochem. Soc. 162 (2015) A2271–A2280. doi:10.1149/2.0331512jes. [49] T. Waldmann, A. Iturrondobeitia, M. Kasper, N. Ghanbari, F. Aguesse, E. Bekaert, L. Daniel, S. Genies, I.J. Gordon, M.W. Löble, E. De Vito, M. Wohlfahrt-Mehrens, “Review—Post- Mortem Analysis of Aged Lithium-Ion Batteries: Disassembly Methodology and Physico- Chemical Analysis Techniques,” J. Electrochem. Soc. 163 (2016) A2149–A2164. doi:10.1149/2.1211609jes. [50] M. Petzl, M. Kasper, M.A. Danzer, “Lithium plating in a commercial lithium-ion battery - A low-temperature aging study,” J. Power Sources. 275 (2015) 799–807. doi:10.1016/j.jpowsour.2014.11.065. [51] M. Berecibar, I. Gandiaga, I. Villarreal, N. Omar, J. Van Mierlo, P. Van Den Bossche, “Critical review of state of health estimation methods of Li-ion batteries for real applications,” Renew. Sustain. Energy Rev. 56 (2016) 572–587. doi:10.1016/j.rser.2015.11.042. [52] M. Landi, G. Gross, “Measurement techniques for online battery state of health estimation in vehicle-to-grid applications,” IEEE Trans. Instrum. Meas. 63 (2014) 1224–1234. doi:10.1109/TIM.2013.2292318. [53] J. Jiang, C. (Chemist) Zhang, “Fundamentals and applications of lithium-ion batteries in electric drive vehicles,” n.d. [54] J. Garche, C.K. Dyer, “Encyclopedia of electrochemical power sources,” Academic Press, 2009. [55] G. Lacey, G. Putrus, A. Salim, The use of second life electric vehicle batteries for grid support, in: EUROCON, 2013 IEEE, 2013: pp. 1255–1261. doi:10.1109/EUROCON.2013.6625141. [56] V. Pop, H.J. Bergveld, P.H.L. Notten, P.P.L. Regtien, “State-of-the-art of battery state-of- charge determination,” Meas. Sci. Technol. 16 (2005) R93–R110. doi:10.1088/0957- 0233/16/12/R01. [57] M. Dubarry, V. Svoboda, R. Hwu, B.Y. Liaw, “Capacity and power fading mechanism identification from a commercial cell evaluation,” J. Power Sources. 165 (2007) 566–572. doi:10.1016/j.jpowsour.2006.10.046. [58] M. Dubarry, V. Svoboda, R. Hwu, B.Y. Liaw, “Capacity loss in rechargeable lithium cells during cycle life testing: The importance of determining state-of-charge,” J. Power Sources. 174 (2007) 1121–1125. doi:10.1016/j.jpowsour.2007.06.185. [59] V. García Fernández, C. Blanco Viejo, D. Anseán González, M. González Vega, Y. Fernández
261 Pulido, J. Alvarez Antón, “Thermal Analysis of a Fast Charging Technique for a High Power Lithium-Ion Cell,” Batteries. 2 (2016) 32. doi:10.3390/batteries2040032. [60] A.J. Bard, L.R. Faulkner, “Elecrochemical Methods : Fundamentals and Applications,” Wiley, 1980. [61] A. Rahmoun, M. Loske, A. Rosin, Determination of the impedance of Lithium-Ion batteries using methods of digital signal processing, in: Energy Procedia, 2014: pp. 204–213. doi:10.1016/j.egypro.2014.01.174. [62] E. Barsoukov, S.H. Ryu, H. Lee, “A novel impedance spectrometer based on carrier function Laplace-transform of the response to arbitrary excitation,” J. Electroanal. Chem. 536 (2002) 109–122. doi:10.1016/S0022-0728(02)01209-3. [63] M. Nakayama, K. Fukuda, Y. Ohmori, K. Wakahara, T. Araki, K. Onda, “Battery Impedance Measurement by Laplace Transformation of Charge or Discharge Current/Voltage,” IEEJ Trans. Power Energy. 125 (2005) 1279–1286. doi:10.1541/ieejpes.125.1279. [64] J.R. Macdonald, W.B. Johnson, Fundamentals of Impedance Spectroscopy, in: Impedance Spectrosc. Theory, Exp. Appl. Second Ed., John Wiley & Sons, Inc., Hoboken, NJ, USA, 2005: pp. 1–26. doi:10.1002/0471716243.ch1. [65] Gamry Instruments, “Basics of EIS: Electrochemical Research-Impedance,” (2016). https://www.gamry.com/application-notes/EIS/basics-of-electrochemical-impedance- spectroscopy/ (accessed May 7, 2017). [66] D. Hilmiye, “Impedimetric Biosensors for Label-Free and Enzymless Detection,” State Art Biosens. - Gen. Asp. (2013) 360. doi:10.5772/45832. [67] K. Sangüesa, “Determinació de la càrrega de bateries i condensadors mitjançant mesures d’impedància,” Master Thesis. (2015). [68] M. Schoenleber, A. Weber, E. Ivers-Tiffée, “Obtaining the Low Frequency Impedance of Li- Ion Batteries from Arbitrary Excitation Signals,” Meet. Abstr. MA2014-04 (2014) 719. [69] D.A. Howey, P.D. Mitcheson, V. Yufit, G.J. Offer, N.P. Brandon, “Online measurement of battery impedance using motor controller excitation,” IEEE Trans. Veh. Technol. 63 (2014) 2557–2566. doi:10.1109/TVT.2013.2293597. [70] M. Neumann-Spallart, M. Etman, “Calculation of impedance spectra by Laplace transformation of voltage transients generated by current-step excitation,” J. Electroanal. Chem. 372 (1994) 33–37. doi:10.1016/0022-0728(93)03265-Q. [71] M. Wickert, “10 Signals and Systems Properties You Never Want to Forget,” (n.d.). http://www.dummies.com/education/science/science-engineering/10-signals-and-systems- properties-you-never-want-to-forget/ (accessed June 16, 2017). [72] A. Cuadras, V.J. Ovejas, Supercapacitor impedance in time and frequency domains, in: Int. Multi-Conference Syst. Signals Devices, SSD 2012, IEEE, 2012: pp. 1–6. doi:10.1109/SSD.2012.6198096.
262 [73] B. Sanchez, G. Vandersteen, R. Bragos, J. Schoukens, “Optimal multisine excitation design for broadband electrical impedance spectroscopy,” Meas. Sci. Technol. 22 (2011) 115601. doi:10.1088/0957-0233/22/11/115601. [74] Y. Zheng, K. Qian, D. Luo, Y. Li, Q. Lu, B. Li, Y.-B. He, X. Wang, J. Li, F. Kang, “Influence of over-discharge on the lifetime and performance of LiFePO4/graphite batteries,” RSC Adv. 6 (2016) 30474–30483. doi:10.1039/C6RA01677D. [75] Gamry Instruments, “Physical Electrochemistry and Equivalent Circuit Elements,” (n.d.). http://mmrc.caltech.edu/Gamry/manuals/Gamry-EIS-Part-2.pdf (accessed June 16, 2017). [76] X. Feng, “Nanocarbons for Advanced Energy Storage,” Volume 1, 2015. [77] H. Helmholtz, “Ueber einige Gesetze der Vertheilung elektrischer Ströme in körperlichen Leitern mit Anwendung auf die thierisch‐elektrischen Versuche,” Ann. Phys. 165 (1853) 211– 233. doi:10.1002/andp.18531650603. [78] K. Smith, C.Y. Wang, “Solid-state diffusion limitations on pulse operation of a lithium ion cell for hybrid electric vehicles,” J. Power Sources. 161 (2006) 628–639. doi:10.1016/j.jpowsour.2006.03.050. [79] C. Lim, “Warburg Impedance,” (2011). https://ocw.mit.edu/courses/chemicalengineering/10-626-electrochemical-energy-systems-spring-2014/lecturenotes/MIT10_626S14_S11lec20.pdf (accessed June 16, 2017). [80] Bio-Logic, “EIS measurements : Potentio ( PEIS ) or Galvano ( GEIS ) mode , that is the question,” (2013). [81] Gamry Instruments, “EIS - Potentiostatic or Galvanostatic Mode,” (n.d.). https://www.gamry.com/application-notes/EIS/eis-potentiostatic-galvanostatic-mode/ (accessed July 12, 2017). [82] P.J. Osswald, S. V. Erhard, A. Noel, P. Keil, F.M. Kindermann, H. Hoster, A. Jossen, “Current density distribution in cylindrical Li-Ion cells during impedance measurements,” J. Power Sources. 314 (2016) 93–101. doi:10.1016/j.jpowsour.2016.02.070. [83] C. Heubner, M. Schneider, A. Michaelis, “Investigation of charge transfer kinetics of Li- Intercalation in LiFePO4,” J. Power Sources. 288 (2015) 115–120. doi:10.1016/j.jpowsour.2015.04.103. [84] J.P. Schmidt, T. Chrobak, M. Ender, J. Illig, D. Klotz, E. Ivers-Tiffée, “Studies on LiFePO4 as cathode material using impedance spectroscopy,” J. Power Sources. 196 (2011) 5342–5348. doi:10.1016/j.jpowsour.2010.09.121. [85] W. Waag, S. Käbitz, D.U. Sauer, “Experimental investigation of the lithium-ion battery impedance characteristic at various conditions and aging states and its influence on the application,” Appl. Energy. 102 (2013) 885–897. doi:10.1016/j.apenergy.2012.09.030. [86] A. Barai, W.D. Widanage, J. Marco, A. McGordon, P. Jennings, “A study of the open circuit voltage characterization technique and hysteresis assessment of lithium-ion cells,” J. Power
263 Sources. 295 (2015) 99–107. doi:10.1016/j.jpowsour.2015.06.140. [87] B. Stiaszny, J.C. Ziegler, E.E. Krauß, J.P. Schmidt, E. Ivers-Tiffée, “Electrochemical characterization and post-mortem analysis of aged LiMn2O4-Li(Ni0.5Mn0.3Co0.2)O2/graphite lithium ion batteries. Part I: Cycle aging,” J. Power Sources. 251 (2014) 439–450. doi:10.1016/j.jpowsour.2013.11.080. [88] J. Costard, M. Ender, M. Weiss, E. Ivers-Tiffée, “Three-Electrode Setups for Lithium-Ion Batteries,” J. Electrochem. Soc. 164 (2017) A80–A87. doi:10.1149/2.0241702jes. [89] H. Zheng, Q. Qu, G. Zhu, G. Liu, V.S. Battaglia, H. Zheng, “Quantitative Characterization of the Surface Evolution for LiNi0.5Co0.2Mn0.3O2/Graphite Cell during Long-Term Cycling,” ACS Appl. Mater. Interfaces. 9 (2017) acsami.7b00427. doi:10.1021/acsami.7b00427. [90] D.A. Howey, V. Yufit, P.D. Mitcheson, G.J. Offer, N.P. Brandon, “Impedance measurement for advanced battery management systems,” 2013 World Electr. Veh. Symp. Exhib. (2013) 1–7. doi:10.1109/EVS.2013.6914960. [91] L. Lam, A Practical Circuit-based Model for State of Health Estimation of Li-ion Battery Cells in Electric Vehicles, 2011. doi:10.1109/INTLEC.2011.6099803. [92] E.U. Franck, R.A. Robinson, R.H. Stokes, “Electrolyte Solutions: The Measurement and Interpretation of Conductance, Chemical Potential and Diffusion in Solutions of Simple Electrolytes. 2e Ed.(rev.).,” Butterworths, 1968. doi:10.1002/ange.19600721222. [93] S.S. Zhang, K. Xu, T.R. Jow, EIS study on the formation of solid electrolyte interface in Liion battery, in: Electrochim. Acta, 2006: pp. 1636–1640. doi:10.1016/j.electacta.2005.02.137. [94] J. Illig, T. Chrobak, D. Klotz, E. Ivers-Tiffée, “Evaluation of the Rate Determining Processes for LiFePO 4 as Cathode Material in Lithium-Ion-Batteries,” ECS Trans. 33 (2011) 3–15. doi:10.1149/1.3564865. [95] C. Uhlmann, J. Illig, M. Ender, R. Schuster, E. Ivers-Tiffée, “In situ detection of lithium metal plating on graphite in experimental cells,” J. Power Sources. 279 (2015) 428–438. doi:10.1016/j.jpowsour.2015.01.046. [96] J. Illig, J.P. Schmidt, M. Weiss, A. Weber, E. Ivers-Tiffée, “Understanding the impedance spectrum of 18650 LiFePO4-cells,” J. Power Sources. 239 (2013) 670–679. doi:10.1016/j.jpowsour.2012.12.020. [97] J. Illig, M. Ender, T. Chrobak, J.P. Schmidt, D. Klotz, E. Ivers-Tiffee, “Separation of Charge Transfer and Contact Resistance in LiFePO4-Cathodes by Impedance Modeling,” J. Electrochem. Soc. 159 (2012) A952–A960. doi:10.1149/2.030207jes. [98] Y. Li, M. Bettge, B. Polzin, Y. Zhu, M. Balasubramanian, D.P. Abraham, “Understanding Long-Term Cycling Performance of Li1.2Ni0.15Mn0.55Co0.1O2–Graphite Lithium-Ion Cells,” J. Electrochem. Soc. 160 (2013) A3006–A3019. doi:10.1149/2.002305jes. [99] J. Groot, M. Swierczynski, A.I. Stan, S.K. Kaer, “On the complex ageing characteristics of high-power LiFePO4/graphite battery cells cycled with high charge and discharge currents,”
270 lithium-ion cells linked to heterogeneous compression,” J. Energy Storage. 5 (2016) 212–223. doi:10.1016/j.est.2016.01.003. [186] Qnovo, “Lithium plating is immensely hazardous,” (n.d.). https://qnovo.com/lithiumplating-is-immensely-hazardous/ (accessed June 14, 2017). [187] J. Illig, T. Chrobak, D. Klotz, E. Ivers-Tiffee, “Evaluation of the Rate Determining Processes for LiFePO4 as Cathode Material in Lithium-Ion-Batteries,” ECS Trans. 33 (2011) 3–15. doi:10.1149/1.3564865. [188] E.M. Krieger, Effects of variability and rate on battery charge storage and lifespan, 2013. http://citeseerx.ist.psu.edu/viewdoc/download?doi=10.1.1.876.2485&rep=rep1&type=pdf (accessed April 28, 2017). [189] T. Liu, A. Garsuch, F. Chesneau, B.L. Lucht, “Surface phenomena of high energy Li(Ni1/3Co1/3Mn1/3)O2 /graphite cells at high temperature and high cutoff voltages,” J. Power Sources. 269 (2014) 920–926. doi:10.1016/j.jpowsour.2014.07.051. [190] M. Kerlau, J.A. Reimer, E.J. Cairns, “Investigation of particle isolation in Li-ion battery electrodes using 7Li NMR spectroscopy,” Electrochem. Commun. 7 (2005) 1249–1251. doi:10.1016/j.elecom.2005.09.003. [191] R. Dell, D.A.J. (David A.J. Rand, “Understanding Batteries,” Royal Society of Chemistry, 2001. doi:10.1039/9781847552228. [192] J. Prakash, D. Chu, D. Scherson, M. Enayetullah, I. Tae Bae, “Fundamental understanding of electrode processes in memory of Professor Ernest B. Yeager,” Electrochemical Society, 2005. [193] S. Santhanagopalan, K. Smith, J. Neubauer, G.H. Kim, A. Pesaran, M. Keyser, “Design and Analysis of Large Lithium-Ion Battery Systems,” Artech House, 2014. [194] A. Cuadras, R. Romero, V.J. Ovejas, “Entropy characterisation of overstressed capacitors for lifetime prediction,” J. Power Sources. 336 (2016) 272–278. doi:10.1016/j.jpowsour.2016.10.077.