Variability and power enhancement of current controlled resistive switching devices
Abstract
Producción Científica
Full text
Microelectronic Engineering 276 (2023) 112008 Available online 15 April 2023 0167-9317/© 2023 The Authors. Published by Elsevier B.V. This is an open access article under the CC BY license (http://creativecommons.org/licenses/by/4.0/). Variability and power enhancement of current controlled resistive switching devices G. Vinuesa a , * , H. García a , J.M. Lendínez a , E. García-Ochoa a , M.B. Gonz´ alez b , D. Maldonado c , C. Aguilera-Pedregosa c , E. Moreno c , F. Jim´ enez-Molinos c , J.B. Rold´ an c , F. Campabadal b , H. Cast´ an a , S. Due˜ nas a a Departamento de Electr´ onica, Universidad de Valladolid, Paseo Bel´ en 15, 47011 Valladolid, Spain b Institut de Microelectr` onica de Barcelona IMB-CNM (CSIC), Campus UAB, Carrer dels Til⋅lers s/n, Campus UAB, 08193 Bellaterra, Spain c Departamento de Electr´ onica y Tecnología de Computadores, Universidad de Granada, Facultad de Ciencias, Avd. Fuentenueva s/n, 18071 Granada, Spain ARTICLE INFO Keywords: Resistive switching Hafnium oxide Current control Electrical characterization TCM RRAM ABSTRACT In this work, the unipolar resistive switching behaviour of Ni/HfO 2 /Si(n + ) devices is studied. The structures are characterized using both current and voltage sweeps, with the device resistance and its cycle-to-cycle variability being analysed in each case. Experimental measurements indicate a clear improvement on resistance states stability when using current sweeps to induce both set and reset processes. Moreover, it has been found that using current to induce these transitions is more efficient than using voltage sweeps, as seen when analysing the device power consumption. The same results are obtained for devices with a Ni top electrode and a bilayer or pentalayer of HfO 2 /Al 2 O 3 as dielectric. Finally, kinetic Monte Carlo and compact modelling simulation studies are performed to shed light on the experimental results. 1. Introduction In the last few years, several emerging technologies for non-volatile memories are being studied to work as storage-class memories [1]. Among these technologies, resistive random-access memories (RRAMs) based on the resistive switching (RS) effect are of great interest [2–4]. Their outstanding features allow to bridge the gap between flash memories and the low latency dynamical memories. RRAMs have shown great potential for scalability, high-speed operation (<10 ns), low power consumption and CMOS compatibility [5–7]. In addition, they also show remarkable endurance (above >10 10 cycles [8]), retention [9–11] and large HRS/LRS resistance ratios (>100) [1]. This technology is being used by different companies commercially, such as TSMC for its 40 nm [12], 28 nm [13] and 22 nm [14] nodes, and INTEL for its 22 nm [15] node. Moreover, RS devices are not only key elements for non-volatile memories [1], but have also proven outstanding properties for applications such as hardware cryptography [16–18] and neuromorphic computation [9,16,19]. As stated before, RRAMs are based on the resistive switching (RS) effect, which allows the devices to reversibly change their electrical resistance by applying a certain electric field [9]. The programmed resistance value remains without the application of any external voltage, which is what makes these devices good candidates for non-volatile memories. As RRAM devices are usually metal-insulator-metal or metal-insulator-(highly doped) semiconductor structures, this change in the device's resistance is explained by the modification of an energy barrier at one of the dielectric/electrode interfaces or by the formation of a conductive filament (CF) that short-circuits the electrodes [20–22]. Filamentary charge conduction linked to CF formation is the most common RS operation; the CF is created for the first time in the forming process (for forming-free devices this stage is not necessary), which demands higher voltages than the subsequent switching processes. After the forming, the filament can be disrupted (reset process) and rebuilt (set process) repeatedly, switching the device resistance state from high (HRS) to low (LRS) or vice versa, respectively. In addition, intermediate states are also allowed and controllable in some switching devices, which makes them specially interesting for the implementation of artificial synapses in neuromorphic computation, as this multilevel operation allows to electrically adjust the synaptic weight between neurons [23,24]. This filamentary model is widely accepted by the scientific community [7,25–27] and has been experimentally demonstrated in several previous works [20,28–30]. * Corresponding author. E-mail address: [email protected] (G. Vinuesa). Contents lists available at ScienceDirect Microelectronic Engineering journal homepage: www.elsevier.com/locate/mee https://doi.org/10.1016/j.mee.2023.112008 Received 21 February 2023; Received in revised form 5 April 2023; Accepted 14 April 2023
Microelectronic Engineering 276 (2023) 112008 2 Resistive switching can either be bipolar (BRS) if the set and reset occur at different polarities or unipolar (URS) when both transitions happen at the same voltage polarity. When the electrodes are inert metals, the BRS is usually due to electron hopping through dielectric regions with a high concentration of oxygen vacancies, which shape the conductive filaments (known as valence change mechanism or VCM [10,31,32]). However, if one of the electrodes is an electrochemically active metal (Ag, Cu or Ni), it may act as a source of highly mobile metal cations that may diffuse through the insulator, forming a metallic filament (electrochemical metallization mechanism or ECM) [2,27,33]. Thermal effects are known to play a key role to analyse RS in RRAMs [2,9,10,34]. They are particularly important in some types of URS devices, as they are based on the thermochemical mechanism (TCM), in which thermochemical processes dominate over the electrochemical ones [35–39]. It has been shown for URS devices with Ag electrodes [40–42], as well as for Ni/HfO 2 /Si-n + samples [33,43–46] that Joule heating is key to explain the physics that lies behind RS operation. As stated earlier, RRAMs are serious candidates to replace other technologies in the non-volatile memory realm. However, the cycle-to- cycle (C2C) variability hinders their progress to become the mainstream technology in the industry. This is especially apparent in unipolar resistive switching devices, which has led to a decrease in the number of scientific studies of samples presenting URS [47], despite the fact that they usually show much greater low to high resistance state ratio and easier circuit integration (because of their unipolar nature) when compared to their bipolar counterparts [48]. In this context, different alternatives have been explored to assess the potential of these devices; for instance, the use of the device current instead of the voltage to control RS operation. The use of the current to induce RS allows a better control of the device resistance in HfO 2 -based RRAM devices, especially in the set process [49,50]. We deal with this current-driven RS approach here to characterize Ni/HfO 2 /Si-n + cells from the experimental and simulation viewpoint. In addition, we consider Ni/HfO 2 / Al 2 O 3 /Si-n + and Ni/HfO 2 /Al 2 O 3 /HfO 2 /Al 2 O 3 /HfO 2 /Si-n + structures to extend our study since the presence of the alumina layer in the dielectric stack modifies the thermal effects [51] and allows to thermal engineer the dielectric stacks to improve RS operation. To shed light on these issues, the set and reset voltages, the power consumption at RS transitions, and the variability and thermal effects are studied in depth comparing current and voltage-controlled resistive switching and the physics behind RS by means of COMSOL-based simulations. 2. Material and methods Ni/insulator/Si stacks were fabricated on (100) n-type Czochralski silicon wafers with resistivity in the (0.007–0.013) Ω cm range. Both HfO 2 and Al 2 O 3 layers were grown at 225 ◦C using Atomic Layer Deposition in a Cambridge NanoTech Savannah 200 system equipped with tetrakis(dimethylamido)‑hafnium (TDMAH) and trimethylaluminum (TMA) as Hf and Al precursors, respectively, H 2 O as oxidant precursor and N 2 as carrier and purge gas. Three different types of devices are studied in the present work, namely a monolayer Ni/HfO 2 (20 nm)/ Si-n + , a bilayer Ni/HfO 2 (10 nm)/Al 2 O 3 (10 nm)/Si-n + and a pentalayer Ni/HfO 2 (4 nm)/Al 2 O 3 (4 nm)/HfO 2 (4 nm)/Al 2 O 3 (4 nm)/HfO 2 (4 nm)/ Si-n + . The 200 nm thick Ni electrode was deposited by magnetron sputtering. The resulting devices are squared cells of 60 ×60 μ m 2 . All fabrication details have been published and can be found at [51]. A schematic cross-section of the devices can be found in Fig. 1. Electrical measurements were made by means of a HP4155B semiconductor parameter analyzer. Voltage and current sweeps were applied to the top electrode (TE) of the devices, while the bottom electrode (BE) remained grounded in all cases. Current and voltage compliances were used when inducing a set process by applying voltage, or a reset process applying current, respectively. After each transition, a pulse at 0.5 V was applied to the device to measure the current at a low voltage and ensure that the transition had been completed by checking whether this value was over or under a current limit (I lim ) obtained experimentally. The automated measuring process is further detailed on a flowchart in Fig. 2. The equipment was connected to a computer via GPIB and controlled using Agilent VEE software. 3. Results and discussion 3.1. Experimental approach After an electroforming process carried out by applying a positive voltage ramp and using a current compliance of 100 μ A, Ni/HfO 2 /Si-n + devices showed unipolar resistive switching. Thus, both set and reset processes take place at a positive voltage polarity, with the set process occurring at higher voltages but consuming less power (because of the higher currents involved in the reset). The typical current-voltage (I-V) curves are shown in Fig. 3a, obtained under ramped voltage stress (RVS), the set was observed in a [1.8 V, 2.5 V] voltage interval, while the reset occurred in the [1.2 V, 2 V] range. A current compliance of 1 mA was used for the set transition to avoid irreversibly breaking the sample. As stated in the introduction section, the URS in these samples is driven by Joule heating inducing both the formation and rupture of CFs; high mobility Ni atoms diffuse from the top electrode into the dielectric creating a metallic conductive path [43,52]. The I-V curve is obtained by measuring the current through the device while applying a voltage bias. This is the usual characterization technique for both bi- and unipolar RS devices. As the aim of this work is to uncover the consequences and possible benefits of current controlled RS, we obtained a very similar hysteretic curve by applying ramped current stress (RCS) and measuring the voltage across the device (with a voltage compliance of 2 V). We shall call this a voltage-current V-I curve, which is depicted in Fig. 3b. Hereby we present an analysis of the charge, flux and energy, as these magnitudes control de Joule heating, which, as mentioned in the introduction, is essential for URS. Charge versus flux (Q-ϕ) and energy versus flux (E-ϕ) curves are plotted in Fig. 4 a-b for the reset cycles obtained under RVS (see Eqs. 1–3). The charge can be calculated from the conventional I-V curves as follows: Fig. 1. Schematic cross-sections of the fabricated a Ni/HfO 2 /Si-n + and b Ni/HfO 2 /Al 2 O 3 /Si-n + devices. G. Vinuesa et al.
Microelectronic Engineering 276 (2023) 112008 3 Fig. 2. a Schematic of the automated measuring process of the Ni/HfO 2 /Si-n + devices. The algorithm shows the necessary conditions to ensure that the transition has been completed for both voltage and current sweeps. b Schematic of the circuit used for the electrical measurements, the HP4155B semiconductor parameter analyzer allows for the application of voltage and current via its Source Measure Units (SMUs). TE and BE stand for top electrode and bottom electrode, respectively. Fig. 3. Experimental a I-V and b V-I curves of a Ni/HfO 2 /Si-n + device, LRS and reset processes are depicted in red, while HRS and set processes appear in blue. (For interpretation of the references to colour in this figure legend, the reader is referred to the web version of this article.) G. Vinuesa et al.
Microelectronic Engineering 276 (2023) 112008 4 Q(t) = ∫t 0 i(t′)dt′(1) where i(t) and v(t) are the measured current and voltage. And the flux can be computed as: Φ(t) = ∫t 0 v(t′)dt′(2) Thus, the corresponding energy value can be derived by the equation: E(t) = ∫t 0 i(t′)v(t′)dt′(3) At the reset point, the charge, flux and energy obtained are named as Q reset , ϕ reset and E reset . The Q reset versus ϕ reset experimental distributions are plotted in Fig. 4 c-d along with the E reset versus ϕ reset distributions for the RVS cycles. The cumulative distribution functions (CDF) for ϕ reset , Q reset and E reset , corresponding to these experimental distributions, are shown in Fig. 4 e-g. See that the distribution functions are much more abrupt in Fig. 4f and g. These results make sense since, as stated before, these magnitudes control the Joule heating and, therefore, the CF temperature that ultimately triggers the reset process (which is known to be a thermal-run-away process with positive feedback) [34,46]. In Fig. 5a the set voltage CDFs are shown both for I-V and V-I measurements, while their corresponding set currents are presented in Fig. 5b. Lower set voltages are obtained in the V-I case, while there is no difference between the two measurement approaches in the case of the set currents. The algorithms employed to extract the set voltages in the I- V curves are given in [53]. For the V-I curves, the set voltages are found at the point where the highest voltage change is obtained. Furthermore, the same observation can be made when analysing the reset transition. Reset voltages are lower using RCS in comparison with the voltagecontrolled approach (Fig. 5c); while reset currents were similar for both current and voltage measurements, as it can be seen in Fig. 5d. The algorithm used for the reset voltage extraction can also be found at [53]. To obtain significant information about the changes in the device resistance after each transition, the current was read at 0.5 V after the set or reset process (Fig. 2). This was made for both RVS and RCS using the Fig. 4. a Charge versus flux data, b energy versus flux data for the Ni/HfO 2 /Si-n + device measured under RVS (Fig. 3a). c Extracted charge and flux experimental data at the reset point, d energy versus flux at the reset point for the devices under study measured under RVS (Fig. 3a). Cumulative distribution functions for e ϕ reset , f Q reset and g E reset for the devices under study measured employing RVS (Fig. 3a). G. Vinuesa et al.
Microelectronic Engineering 276 (2023) 112008 5 following measurement sequence: (i) voltage or current sweep to trigger the set process, (ii) voltage pulse of 0.5 V to measure the current, (iii) voltage or current sweep to trigger the reset process, (iv) voltage pulse of 0.5 V to measure the current. Fig. 6a and b (HfO 2 monolayer) show the current measured at 0.5 V (steps (ii) and (iv)) after each set or reset transition versus the number of cycles. The resistance uniformity along cycling under RCS is notorious in comparison to RVS. Although the resistance variability in the LRS is similar for both cases, HRS variability is clearly lower in the RCS case. In order to shed light on the variability issue, we also considered devices with more complex dielectrics such as Ni/HfO 2 /Al 2 O 3 /Si-n + bilayers and Ni/HfO 2 /Al 2 O 3 /HfO 2 / Al 2 O 3 /HfO 2 /Si-n + pentalayers. We have observed a similar behaviour for the bi- (Fig. 6 c-d) and pentalayer (Fig. 6 e-f) devices in terms of the RCS advantages. Variability is lower due to uniformity in Joule heating under RCS, as thermal effects are controlled by the device current. These observations are supported by the calculation of the standard deviation of the HRS and LRS under both RCS and RVS for the three samples, which are shown in Table 1. The standard deviations show that applying current sweeps positively impacts both resistance states' variability when compared to the results obtained by applying voltage sweeps. HRS standard deviation decreases in one order of magnitude in all cases when using RCS, also decreasing one order of magnitude for the LRS of the bilayer device. In the monolayer and pentalayer structures, the standard deviation of the LRS also decreases, although within the same order of magnitude, when using RCS. When analysing the mean values, it can be seen that the mean current value obtained decreases greatly for the HRS in all cases, while the LRS mean values remain similar under RCS and RVS. Fig. 7 shows that the power involved in RS processes is lower for RCS than for RVS operation. These tendency holds for both set and reset transitions in all the dielectric stacks considered. Again, the efficiency in controlling Joule effects under RCS is behind the physics underlying this behaviour. This draws even more attention to the reset process, as it consumes less power while also delivering lower current values (see mean values on Table 1) under current control. Set and reset power values are obtained by multiplying current and voltage values at the point where the voltage presents a higher change in its value. 3.2. Simulation approach A 3D finite elements approach was employed to simulate the devices under study; in particular, the Ni/HfO 2 /Si-n + cell. The different materials and their properties were described making use of the commercial simulation software COMSOL Multiphysics. A cylindrical CF was assumed, whose radius was modified to reproduce the experimental RS processes. In addition to the ohmic CF, we have also included a constriction within the CF that corresponds to an atomic-size narrowing, where electron transport is ballistic and quantum effects show up. The transport regime can be described with the Landauer's formalism [54–56]. Under the assumption of a transmission probability function resembling an inverted parabolic function, Landauer's integral for the zerotemperature limit can be analytically solved. The current across the constriction can be obtained as follows, I=2eN h{eV +1 α ln[1+e[ α (Φ−βeV) ] 1+e{ α [Φ+(1−β)eV ] } ]} (4) where e is the electron charge, h is the Planck's constant, N is the number of active channels in the constriction, α affects the shape of the potential barrier, Φ stands for the potential barrier height, β is the fraction of the potential that drops in one of the constriction contacts and (1- β) the Fig. 5. Cumulative distribution functions for a V set under RVS (black) and RCS (pink), b I set under RVS (red) and RCS (dark green), c V reset under RVS (light green) and RCS (maroon), and d I reset under RVS (blue) and RCS (orange), for the Ni/HfO 2 /Si-n + device. (For interpretation of the references to colour in this figure legend, the reader is referred to the web version of this article.) G. Vinuesa et al.
Microelectronic Engineering 276 (2023) 112008 6 Fig. 6. Current values measured at 0.5 V after each set (LRS- red) and reset (HRS-blue) transition, carried out under RVS (left column) and RCS (right column) for the Ni/HfO 2 /Si-n + (a and b), Ni/HfO 2 /Al 2 O 3 /Si-n + (c and d) and Ni/HfO 2 /Al 2 O 3 /HfO 2 /Al 2 O 3 /HfO 2 /Si-n + (e and f) samples. (For interpretation of the references to colour in this figure legend, the reader is referred to the web version of this article.) Table 1 Standard deviation ( σ ) and mean ( μ ) values of the HRS and LRS under RVS and RCS for the three measured samples, a monolayer Ni/HfO 2 (20 nm)/Si-n + , a bilayer Ni/ HfO 2 (10 nm)/Al 2 O 3 (10 nm)/Si-n + and a pentalayer Ni/HfO 2 (4 nm)/Al 2 O 3 (4 nm)/HfO 2 (4 nm)/Al 2 O 3 (4 nm)/HfO 2 (4 nm)/Si-n + . HRS LRS σ (A) μ (A) σ (A) μ (A) Monolayer RVS 1.60 •10 −6 2.11 •10 −6 2.49 •10 −5 1.58 •10 −4 RCS 3.60 •10 −7 6.79 •10 −7 1.53 •10 −5 1.70 •10 −4 Bilayer RVS 1.79 •10 −6 1.47 •10 −6 1.03 •10 −4 2.36 •10 −4 RCS 2.42 •10 −7 5.72 •10 −7 1.23 •10 −5 1.51 •10 −4 Pentalayer RVS 1.11 •10 −6 1.24 •10 −6 3.19 •10 −5 1.40 •10 −4 RCS 2.43 •10 −7 2.05 •10 −7 1.58 •10 −5 1.28 •10 −4 G. Vinuesa et al.
Microelectronic Engineering 276 (2023) 112008 7 Fig. 7. Cumulative distribution functions for the power consumption for both reset (left column) and set (right column) transitions for Ni/HfO 2 /Si-n + (a - b), Ni/HfO 2 /Al 2 O 3 /Si-n + (c - d) and Ni/HfO 2 /Al 2 O 3 / HfO 2 /Al 2 O 3 /HfO 2 /Si-n + (e - f) samples. Panels (a, c, e) show the power absorbed by the reset transition when applying voltage (red) and current (yellow). Panels (b, d, f) show the power absorbed by the set transition when applying voltage (green) and current (blue). (For interpretation of the references to colour in this figure legend, the reader is referred to the web version of this article.) G. Vinuesa et al.
Microelectronic Engineering 276 (2023) 112008 8 other fraction. The simulation scheme is equivalent to the one proposed in [26,51] for the same kind of devices. In addition, the CF radius evolution is described assuming an average Arrhenius-like mechanism to account for the variation of the high concentration regions of metallic atoms that shape the CF and lead to the set and reset processes [57]. dr dt = ± A e−Ea kT (5) where r stands for the CF radius (cylindrical coordinates), A stands for a fitting preexponential constant and E a is the activation energy of the main physical mechanism behind the CF variation (we simplify the model under the assumption that the mechanism described in Eq. 2 has the strongest influence in the CF kinetics; a different simulation approach, accounting for the different physical mechanisms is based on kinetic Monte Carlo [33]). The CF thermal conductivity was 11 WK −1 m −1 , while it was 90 (148) WK −1 m −1 for the Ni (Silicon) electrode, and 1 WK −1 m −1 for HfO 2 ; the CF electrical conductivity was 2 ×10 5 Ω −1 m −1 and the activation energy, E a =0.84 eV. We show in Fig. 8 that the simulation tool reproduces reasonably well the experimental measurements once the CF radius and the QPC model parameters are fitted. See that both I-V and V-I operation regimes are correctly described, including the set and reset voltages, the current magnitude and the curves shape. This is also seen in Fig. 9, where a comparison with a group of experimental curves (note the cycle-to-cycle variability) is shown along with simulated ones. Our scheme is in line with previous simulation approaches; however, it makes no difference when V-I and I-V operation regimes are compared since it is a deterministic simulator. To shed light on this issue, we have plotted in Fig. 10 the product of temperature and electric field versus voltage drop in the device; these two magnitudes drive ion diffusion in the dielectric and, therefore, control RS. In this respect, the plot is representative to compare the V-I and I-V operation regimes. See that identical results are found. It is important to note that the simulation Fig. 8. Simulated (red lines) and experimental (black lines) curves for Ni/HfO 2 /Si-n + devices. a, c I-V operation regime, b, d V-I operation regime. (For interpretation of the references to colour in this figure legend, the reader is referred to the web version of this article.) G. Vinuesa et al.
Microelectronic Engineering 276 (2023) 112008 9 approaches are different: when the voltage is fixed externally, this is easily transformed to boundary conditions in our simulation domain; however, if the current is fixed, we employ average probes to estimate the device voltage. We have also studied the output of current and voltage ramps, obtaining non-significative differences when making a fair comparison in terms of initial conditions (voltage and current magnitudes). Considering the experimental results, it is clear that the V-I operation regime influences in a different way the physical processes behind RS. Consequently, a different modelling scheme is needed in this case (it might be related to modifications in Eq. 2, a reduction of the activation energy, or/and even linked to an increase of the heat generation term within the heat equation). Thus, the development of a new model would need of new experiments and indirect analysis of the experimental RS behaviour in our devices; in this respect, it is out the scope of this paper. As a general consideration, it is clear that the V-I regime influences RS operation, accelerating the physical mechanisms that create and destroy the CFs. These effects result in lower operation voltages (and power consumption) as well as lower variability. Therefore, it offers clear advantages for IC development in the non-volatile memories and neuromorphic computing realms. In order to complete the simulation study and shed light on the resulting current/voltage signal in the RVS and RCS, respectively, we have used a different simulation approach based on a compact circuital model described in ref. [58]. This model was previously fitted and successfully used for studying reset transitions in Ni/HfO 2 (20 nm)/Si-n + devices under different operation regimes (RVS and constant voltage stress) [58]. Fig. 11a shows the simulated I-V curve obtained under RVS (black line) and V-I under RCS (red lines) with the same slopes than the experimental input signals (0.4 V/s and 65 μ A/s). The reset voltage and current are slightly lower under the RCS. When current and voltage are plotted versus time (insets in Fig. 11a), we can appreciate that the resulting signals are different under the RVS and RCS. However, if we simulate RCS with a higher slope (resulting in current and voltage signals closer to those obtained under RVS, green lines in Fig. 11a), the current and reset voltages are quite similar. As a conclusion, as happened with the previously exposed simulation approach based on a 3D finite elements solver, there is no difference between RVS and RCS, as long as the resulting current/voltage signals are similar. Finally, Fig. 11b shows the simulated energy obtained by the time integration of the power. RCS with a lower slope leads to the highest total dissipated energy because the reset transition is delayed, even though the reset current/voltage are the lowest, this is consistent with the P reset shown in Fig. 7a. RVS and RCS with higher slope produce quite similar dissipated energy, although current and voltage (and, therefore, energy) is slightly higher under RCS with 158 μ A/s. 4. Conclusions Carrying out the set and reset transitions applying current to RRAM HfO 2 -based devices reduces set and reset voltages, as well as cycle-to- cycle variability in comparison with conventional voltage driven resistive switching operation. In addition, current controlled RS proves to be the most efficient method of carrying out the transitions between resistance states, as the power consumed is lower than voltage controlled resistive switching. This may be due to a better control of the Joule heating when applying current, as thermal effects are controlled by the device current. In addition, we have proven that, when employing conventional finite-element RRAM simulators, no apparent differences between I-V and V-I operation are obtained. Consequently, there is a need of further modelling in the case of V-I resistive switching since this regime influences in a different way the physical mechanisms behind the operation of the studied devices. Fig. 10. Simulation of Ni/HfO 2 /Si-n + devices; product of the temperature and the absolute value of the electric field versus the voltage value both for the I-V and V-I operation regimes. Fig. 9. Simulated (red lines) and experimental (black lines) curves for Ni/HfO 2 /Si-n + devices. a I-V operation regime, b V-I operation regime. (For interpretation of the references to colour in this figure legend, the reader is referred to the web version of this article.) G. Vinuesa et al.