scieee AI-readable full text Open interactive document viewer

Injection molding optimization in order to improve the dispersion of the nanoclays

Pascual Cuenca, Enric

Abstract

Injection molding is the most commonly manufacturing process used for the fabrication of plastic parts. Different products can be manufactured using injection molding which vary greatly in their size, complexity and application. Automotive industry is the most important sector that uses this technology. A wide variety of additives are used to modify the raw polymers and achieve new properties. Nanoadditives and nanoclays specifically, are used to improve various physical properties, such as reinforcement, synergistic flame retardant and barrier. This work is focused on the study the different parameters in the injection molding process in order to optimize the process using a specific grade of polypropylene and a specific grade of nanoclay. The main goal of the project is to improve the flexural modulus of the studied part using a lineal model taking into account the behavior the selected parameters.

Full text

TREBALL FI DE MÀSTER Màster en Enginyeria Química esp. Polimers INJECTION MOLDING OPTIMIZATION IN ORDER TO IMPROVE THE DISPERSION OF THE NANOCLAYS Memòria i Annexos Autor: Enric Pascual Cuenca Director: Alfonso Rodríguez Galán Co-Director: Encarnación Escudero Martínez Convocatòria: Maig 2018 Memoria 1 Memoria 2 Abstract Injection molding is the most commonly manufacturing process used for the fabrication of plastic parts. Different products can be manufactured using injection molding which vary greatly in their size, complexity and application. Automotive industry is the most important sector that uses this technology. A wide variety of additives are used to modify the raw polymers and achieve new properties. Nanoadditives and nanoclays specifically, are used to improve various physical properties, such as reinforcement, synergistic flame retardant and barrier. This work is focused on the study the different parameters in the injection molding process in order to optimize the process using a specific grade of polypropylene and a specific grade of nanoclay. The main goal of the project is to improve the flexural modulus of the studied part using a lineal model taking into account the behavior the selected parameters. Memoria 3 Memoria 4 Index 1. Introduction .......................................................................................................................................... 6 1.1. Polymer processing ....................................................................................................................... 7 1.2. Injection molding process ............................................................................................................. 9 1.3. Thermoplastic nanocomposites .................................................................................................. 11 1.4. Nano-clays ................................................................................................................................... 14 2. State of the art: Automotive Sector .................................................................................................... 16 3. Objective ............................................................................................................................................. 19 4. Experimental ....................................................................................................................................... 20 4.1. Materials ..................................................................................................................................... 20 4.2. Injection molding machine ......................................................................................................... 22 4.3. Injection molding tool ................................................................................................................. 24 4.4. Characterization methods ........................................................................................................... 25 4.5. Injection molding process optimization ...................................................................................... 28 4.6. Design of experiments (DOE) ...................................................................................................... 38 4.7. Lineal modelling .......................................................................................................................... 40 4.8. Residuals ..................................................................................................................................... 41 4.9. Model signification study ............................................................................................................ 44 4.10. Model validation ..................................................................................................................... 46 4.11. Results ..................................................................................................................................... 48 5. Conclusions ......................................................................................................................................... 50 6. References .......................................................................................................................................... 52 7. Annex .................................................................................................................................................. 56 7.1. Annex 1. Surface responses ........................................................................................................ 56 Memoria 5 Memoria 6 1. Introduction Injection molding process is one of the most important technology used in the automotive industry. Three main components are required: injection molding machine (IMM), tool or mold and plastic pellets. Depends on the final part, different plastic will be selected based on the final part properties. Additives are usually used with the aim of enhance some properties of the standard material. Nanoadditives are commonly used to enhance properties like barrier properties, mechanical properties, thermal properties, optical properties among others. Good dispersions is related directly to a high performance of these nanofiller within the polymer matrix. All experiment carried out during this work were performed in EURECAT, a technology center in Catalonia. EURECAT-Cerdanyola has experience in plastic injection for more than 30 years. The center participates in public and private projects researching in different applications using the injection molding process as a basis. This work is focused on study how some injection parameters may affect to the dispersion of the nanoadditives and the mechanical properties of the final part. Memoria 7 1.1. Polymer processing There are many different types of plastics processed by different methods to produce products meeting many different performance requirements, including costs. The basics in processing relate to temperature, time and pressure. In turn they interrelate with product requirements, including plastics type and the process to be used. Europe plastics consumtion in 2016 was 60 million tonnes and the worldwide plastic consumtion was 355 million tones. Packaging is the market sector which converts 39.9% of the consumtion and the autmotive sector consumes 10% of the total in Europe. All of this processes are used to fabricate all types and shapes of plastic products; household convenience packages, electronic devices and many others, including the strongest products in the world, used in space vehicles, aircraft, building structures, and so on. Proper process selection depends upon the nature and requirements of the plastic, the properties desired in the final product, the cost of the process, its speed, and product volume. Some materials can be used with many kinds of processes; others require a specific or specialized machine. Numerous fabrication process variables play an important role and can markedly influence a product's esthetics, performance, and cost. The relative use of these methods in Europe in 2016 is shown in Fig. 1 [1]. Figure 1. Plastic consumption by process. Europe 2016 Many of these variables and their behaviors are the same in the different processes, as they all relate to temperature, time, and pressure. The process depends on several interrelated factors: (1) designing a part to meet performance and manufacturing requirements at the lowest cost; (2) specifying the plastic; (3) specifying the manufacturing process, which requires (a) designing a tool 'around' the part, (b) putting the 'proper performance' fabricating process around the tool, (c) setting up necessary auxiliary equipment to interface with the main processing machine, and (d) setting up 'completely integrated' controls to meet the goal of zero defects; and (4) 'properly' purchasing equipment and materials, and warehousing the materials. Major advantages of using plastics include formability, consolidation of parts, and providing a low cost- to-performance ratio. For the majority of applications that require only minimum mechanical Extrusion 36% Injection 32% Blow 10% Calendring 6% Coating 5% Compression 3% Powder 2% Others 6% Memoria 8 performance, the product shape can help to overcome the limitations of commodity resins such as low stiffness; here improved performance is easily incorporated in a process. However, where extremely high performance is required, reinforced plastics or composites are used. Polymers are usually obtained in the form of granules, powder, pellets, and liquids. Processing mostly involves their physical change (thermoplastics), though chemical reactions sometimes occur (thermosets). Two of the main characteristics of the processing methods are compared in Fig. 2 [1]. One group consists of the extrusion processes (pipe, sheet, profiles, etc.). A second group takes extrusion and sometimes injection molding through an additional processing stage (blow molding, blown film, quenched film, etc.). A third group consists of injection and compression molding (different shapes and sizes), and a fourth group includes various other processes (thermoforming, calendaring, rotational molding, etc.). Figure 2. Process characteristics graph The common features of these groups are (1) mixing, melting, and plasticizing; (2) melt transporting and shaping; (3) drawing and blowing; and (4) finishing. Mixing, melting and plasticizing produce a plasticized melt, usually made in a screw (extruder or injection). Melt transport and shaping apply pressure to the hot melt to move it through a die or into a mold. The drawing and blowing technique stretches the melt to produce orientation of the different shapes (blow molding, forming, etc.). Finishing usually means solidification of the melt. The most common feature of all processes is deformation of the melt with its flow, which depends on its rheology. Another feature is heat exchange, which involves the study of thermodynamics. Changes in a plastic's molecular structure are chemical. 0 1 2 3 4 5 Blow molding Injection Molding CompressionThermoforming Extrusion Part complexity Part size Memoria 15 Different methods have been developed in order to improve the clays dispersion, based on two main methods of modification: (1) physical absorption and (2) chemical modifications, such as grafting functional polymers or functional groups on to the surface of clay or ion exchange with organic cations or anions [17]. First method is based on thermodynamics which improves their physical and chemical properties for composite and the structure of the clays remain unaltered. In this case, exists a weak force between the adsorbed molecules and the clay is an important disadvantage. Otherwise, the second method improves the interaction force between clays and modifiers, controlling and tuning their properties. Generally, clay can be classified into two categories: natural and synthetic clays. Figure 6 shows the classification of natural clays. They are basically composed of alternating sheets of SiO2 and AlO6 units in ratios of 1:1 (kaolinite), 2:1 (montmorillonite and vermiculite) and 2:2 (chlorite) [21]. Modification of clay minerals such as organoclay and organo-modified clay is a new path of clay mineral research. Memoria 16 2. State of the art: Automotive Sector The basic trends that nanotechnology enables for the automobile are  lighter but stronger materials (for better fuel consumption and increased safety)  improved engine efficiency and fuel consumption for gasoline-powered cars (catalysts; fuel additives; lubricants)  reduced environmental impact from hydrogen and fuel cell-powered cars  improved and miniaturized electronic systems  better economies (longer service life; lower component failure rate; smart materials for selfrepair) The use of polymer nanocomposites in the manufacturing chain started in 1991 when Toyota Motor Co., in collaboration with Ube Industries, introduced nylon-6/clay nano composites in the market to produce timing belt covers as a part of the engine for their Toyota Camry cars [22]. Then, Japan introduced nylon- 6 nanocomposites for engine covers on Mitsubishi GDI engines [23] manufactured by injection moulding. The product is said to offer a 20% weight reduction and excellent surface finish. In 2002, General Motors launched a step-assist automotive component made of polyolefin reinforced with 3% nanoclays, in collaboration with Basell (now LyondellBasell Industries) for GM's Safari and Chevrolet Astro vans, followed by the application of these nanocomposites in the doors of Chevrolet Impalas [24], [25]. The important increase in the commercialization of nanocomposites production occurred over the last years. In 2009, a one-piece compression moulded rear floor assembly was manufactured by General Motor for their Pontiac Solace using nano-enhanced Sheet Moulding Compounds (SMCs) developed by Molded Fiber Glass Companies (MFG), Ohio. This technology is also in use on GM's Chevrolet Corvette Coupe and Corvette ZO6. The nano-filled SMCs exhibit significantly lower density than conventional SMCs resulting in improved fuel efficiency [26]. At this point, the automotive industry can benefit from this material in several applications such engines, suspension, break systems, frames and body parts, paints and coatings, tires and electric and electronic equipment. In the latter part of the 1980s and the beginning of the 1990s, a research team from Toyota Central Research Development Laboratories (TCRDL) in Japan reported a work on a Nylon-6/clay nanocomposite and disclosed improved methods for producing nylon-6/ clay nanocomposites using in situ polymerization similar to the Unichika process [27] [28] [29] [30]. he research findings demonstrated a significant improvement in a wide range of physico-mechanical properties by reinforcing polymers with clay on the nanometer scale [31] [32]. The Toyota research team also reported various other types of clay nanocomposites based on polymers such as polystyrene, acrylic, polyimides, epoxy resin, and elastomers using a similar approach [33] [34] [35] [36] [37]. Since then, extensive research in nanocomposites field has been carried out worldwide. Figure 7 shows timeline for the commercialization of products by automotive players. Memoria 17 Figure 7. Timeline for the commercialization of products by automotive players. Among nanomaterials, nanoclays are the most commonly used commercial additive for the preparation of nanocomposites, accounting for nearly 80% of the volume used. Carbon nanofibers, carbon nanotubes (mainly MWCNTs), and Polyhedral Oligomeric Silsesquioxanes (POSS) are also being used commercially in nanocomposites, gaining ground fast with improvements in cost/performance and processability characteristics. The OEMs/Tier I, Tier II, Tier III, raw materials/nanointermediates manufacturers, researchers and technologists are realizing that other than clays, nanomaterials like graphene, carbon nanofibers, nanofoams, multiscale hybrid reinforcement and graphene-enabled rubber nanocomposites could drive the market dynamics. The price and performance advantages of graphene are challenging carbon nanotubes in polymer nanocomposites applications due to its intrinsic properties and it is predicted that a single, defect-free graphene platelet could have an intrinsic tensile strength higher than that of any other material [38]. In June 2010, a U.S. Patent was granted to The Trustees of Princeton University for functional graphenerubber nanocomposites [39], which can be produced at a much lower cost than carbon nanotubes and exhibits excellent mechanical strength, superior toughness, higher thermal stability and electrical conductivity. This graphene-rubber nanocomposite can be employed in all the areas for gas barrier applications including tires and packaging. Memoria 18 Another patent was granted in 2011, for a composite material of nanoscale graphene and an elastomer for vehicle tire application [40]. The multiscale hybrid reinforcement is another potential polymer nanocomposite material for the automotive industry due to its enhanced load transfer at the reinforcement/matrix interface, i.e. by tailoring the interfacial shear strength, which is made of micro sized carbon-fibre yarns and fabrics coated with carbon nanostructures. The high performance racing cars and high-end sports cars require excellent properties such as structural stiffness, heat shielding, impact and compressive strength, and many others. Otherwise, different works has been carried out regarding to the surface properties of the produced parts in order to enhance their properties. In 2009, viscoelastic properties and scratch morphologies were studied using various amounts of nano silica [41]. Different nano-silica particles were incorporated in an automotive OEM clear-coat based on acrylic/melamine chemistry in order to study their effect in the scratch/mar resistances using nano-indentation hardness measurements [42]. In 2014, H. Yari, et. al. studied the influence of OH-functionalized polyhedral oligomeric silsesquioxane(POSS) nano-structure in the same clear coat [43]. In 2015, the impact behaviour of hybrid nano-/micro-modified composite was investigated in Glass Fiber Reinforced Plastics (GFRP). The hybrid nano-/micro fillers chosen were Cloisite® 30B nanoclay and 3M™ Glass Bubbles iM16K [44]. Memoria 19 3. Objective The aim of this project is to optimize the injection molding process to achieve the best nano-additive dispersion in order to improve mechanical properties of the injected part. A good dispersion of the nano particles and their compatibility with the matrix polymer are the two critical points to assure the improvement of the properties comparing with the raw polymer. This work will be focused on the dispersion of the nano additives during the injection molding. A study of the interaction between some injection parameters and the dispersion will be carry out. First of all, the injection molding process needs to be optimized taking into account the most relevant injection parameters during the process, using Scientific Injection Molding (SIM). Once the process is optimized for the selected thermoplastic composite, injection tool and injection molding machine, four injection parameters will be selected to study their behavior related to the dispersion of the nanofiller. A mathematical model will be used to study how each parameter affect to the dispersion of the composite and determine which parameter combination enhance the selected mechanical property. In this work, Flexural Modulus is selected as an output of the linear model. Considering the Flexural Modulus of the raw polypropylene, the goal of the project will be to increase this value as much as possible. Memoria 20 4. Experimental In order to characterize the material within the project, a dog-bone specimens were produced using a special mold. Standardized specimens were tested and this data was used as an input to carry out a mathematical model. First step was to select the most important injection parameters related to the nano-additive dispersion and then to set up a design of experiments to study their behavior related to the dispersion. 4.1. Materials Plastic used to carry out this work is made up of two commercial grades: polypropylene and nanoclay additive. The formulation is composed by 8 wt. % of nanoclay. 4.1.1. Polymer matrix Polymer used during the whole work was polypropylene, in particular ISPLEN PP080G2M from Repsol. This is a homopolymer grade characterised by good flow properties that enables to fill the mould easier and by short cycle times with big articles. Parts manufactured with this grade have excellent chemical resistance, are easily decorated and can accept different colouring systems. Recommended melt temperatures range from 190 to 250°C. Main properties are shown in Table 1: PROPERTIES VALUE UNIT METHOD General Melt flow rate (230°C/ 2,16 kg) 20 g/10 min ISO 1133 Density at 23ºC 905 kg/m3 ISO 1183 Mechanical Flexural modulus of elasticity 1600 MPa ISO 178 Charpy impact strength (23°C,notched) 3 kJ/m2 ISO 179 Thermal HDT 0,45 MPa 85 °C ISO 75 Others Shore Hardness 70 - ISO 868 Table 1. Matrix polymer properties This material should be stored in a dry atmosphere, on a paved, drained and not flooded area, at temperatures under 60ºC and protected from UV radiation. Regarding to the pre-treatment of the material, it is not necessary to pre-dry the material due it not contains mineral additives. Memoria 21 4.1.2. Nanoclay additive The nanoclay used during this work was Cloisite 20 from BYK. This grade is bis(hydrogenated tallow alkyl)dimethyl, salt with bentonite. In Table 2 are shown the typical properties of this grade: PROPERTIES VALUE UNIT Moisture <3 % Typical Dry Particle Size <10 μm (d50) Color Off White Packed Bulk Density 175 g/l Density 1.77 g/cm3 X Ray Results 3.16 nm (d001) Table 2. Nanoclay main properties Using this material as an additive with the matrix, a pre-drying was needed in order to avoid processability problems during the injection process. Memoria 22 4.2. Injection molding machine An ENGEL E-motion 200/55 full electric was used in Eurecat to inject the dog-bone specimens and therefore to test the mechanical properties of the samples. Technical specifications of the machine used are shown in Table 3 and a picture of the machine in the Figure 8. VALUE UNIT Clamping unit Clamping force 550 kN Opening stroke 270 mm Ejector stroke 100 mm Ejector force 23 kN Injection unit Screw diameter 25 mm Max swept volume 59 cm3 Screw speed max 400 r/min Screw speed max current 400 r/min Injection rate 109 cm3/s Injection rate increased 109 cm3/s Spec. Injection pressure 2400 bar Spec. Injection pressure increased 2400 bar Nozzle stroke 225 mm Nozzle cont. pressure 28 kN Table 3. Injection machine specifications The election of this machine was determined by the mould used to inject the samples. There are some advantages of using fully electric injection moulding machines:  Electric machines are digitally controlled and mechanically driven. Their processes do not vary over time since they have no hoses to expand, no valves to potentially stick and no hydraulic fluid to heat up or compress.  Electric machines turn injection moulding into a more predictable operation. With a more consistent machine, the same process setup can be used repeatedly, without affecting part consistency or quality. For example, screw position for fill and pack is controlled with digital precision, eliminating over-packing and greatly reducing moulded-in stress. Consistent machine performance also allows labour cost reductions with unmanned shifts at night or on weekends. Utilization of skilled labour is greatly enhanced.  From the day the machine starts up, it reduces cost per part. All-electric machines produce faster cycle times because of independent clamp/injection functions. Their precision shot control saves material and prevents using more resin, colorant or additive than the part needs. Memoria 23 Figure 8. IMM used for this work Memoria 24 4.3. Injection molding tool A mould was manufactured in order to obtain samples to carry out mechanical characterization. Four different standardized specimens can be injected as shown in Figure 9: A. Tensile strength B. Hardness C. Tensile strength for thermoplastic elastomers D. Impact Figure 9. Standardized specimens which can be manufactured with injection The mould was designed with selectors to choose what part/s could be injected. Figure 10 shows the ejection side with the four parts and the sprue selector and the injection side. Injection side was equipped with a hot runner in order to ease the injection and to reduce the waste of material. Figure 10. Ejection side (left) and injection side (right). Only the A specimen were injected within the frame of the project. A variety of specimen shape can be used for this test, but the most commonly used specimen size for ASTM is 3.2mm x 12.7mm x 125mm and for ISO is 10mm x 4mm x 80mm. Figure 11 shows the dimensions of the standard sample used: Figure 11. Left: Standard sample dimensions. Right: 3D model of the sample Memoria 31 55 0,48 305 2,08 146 60 0,44 312 2,27 137 65 0,41 321 2,44 132 70 0,39 328 2,56 128 75 0,37 335 2,70 124 80 0,34 342 2,94 116 85 0,33 346 3,03 114 90 0,32 354 3,13 113 95 0,30 362 3,33 109 100 0,29 367 3,45 106 105 0,28 371 3,57 104 110 0,26 374 3,85 97 115 0,26 380 3,85 99 120 0,25 386 4,00 97 125 0,24 389 4,17 93 Table 5. Viscosity curve worksheet The optimal injection rate will be closer to the ‘knee’ part of the curve which in this case is 2.5 1/s of shear rate. Using the worksheet this shear rate corresponds to a 65 – 70 mm/s of injection rate. This is where a shift in the viscosity and greater consistency can be observed. Figure 14. Viscosity curve of composite used 0 100 200 300 400 500 600 700 800 0.00 0.50 1.00 1.50 2.00 2.50 3.00 3.50 4.00 4.50 Apparant Shear Viscosiy (P) Aparant shear rate (1/s) Rheology Study Memoria 32 Step 2. Determining the Pressure Drop – Pressure Drop Studies As plastic flows through the different sections of the nozzle and the mold, the flow front of the plastic experiences a loss of applied pressure because of drag and frictional effects. Additionally, as the plastic hits the walls of the mold, it begins to cool, increasing the viscosity o the plastic, which in turn requires additional pressure to push the plastic. The skin plastic that is formed on the internal walls of the runner system decreases the cross sectional area of the plastic flow, which also results in a pressure drop. Measurement zone Weight (g) Peak pressure (bar) % of total pressure Drop pressure (bar) Drop pressure (%) Nozzle n/a 50 2.3 50 2.3 Sprue/Hot sprue 3.64 170 7.7 120 5.5 Gate 4.73 195 8.9 25 1.1 95% of filling part 10.32 318 14.5 123 5.6 Max. pressure of the machine - 2200 100.0 Reserve pressure on the machine 1882 85.5 Table 6. Pressure Drop Worksheet Depending on the pump capacity of the molding machine, there is a limited maximum amount of pressure available to push the screw at the set injection speed. The required pressure to push the screw at the set injection speed should never be more than the maxim available pressure. If the pressure required is higher, the screw will never be able to maintain the set injection speed throughout the injection phase and the process is considered pressure limited. Initially the set speed may be reached, but as soon as process becomes pressure limited, the screw slows down. In order to determine the pressure drop during the whole injection process, several pressure data were recorded. Table 6 shows the data recorded during the experiments. Additionally, the different peak pressures are shown in Figure 16. Figure 15. Pressure Drop Graph 0 500 1000 1500 2000 2500 Nozzle Sprue/Hot sprue Gate 95% of filling part Max. pressure of the machine IMM presure (bar) Pressure Drop Study Memoria 33 Step 3. Determining the Process Window – Process Window Study Injection molding process is divided in two phases: the first phase in injection and the second phase is packing and holding phase. The holding pressure is the responsible of pack additional melt plastic into the cavity in order to avoid the shrinkage caused by the cooling phase when plastic is in contact with the cold mold walls. Packing pressure, holding pressure, packing time and holding time are the parameters which controls this second phase. In this work, packing and holding has not been differentiated mentioned as holding phase. The ideal holding pressure is determined by evaluation the process window of the mold. Two process variables were varied to establish the process window: holding pressure and melt temperature. This windows process is referred to the molding area diagram which is the area where the molded parts are aesthetically accepted. The bigger the window, the more robust process will be the process. It means that the parts which are located outside the illustrated process window will not be acceptable due to defects such as sinks, flash, or internal stresses. In order to determine the values which will form the process window, an experiment was carried out as follows in Figure 17: Figure 16. Process window study graph Following table (Table 7) was constructed using the data of the graph. The size of the process window is an indicator of how much variation the process will tolerate while still producing aesthetically acceptable parts. Regarding to the temperature, both values were applied taking into account the manufacturer recommendation. On the other hand, steps of 50 bar were used during the experiment. Due to the low complexity of the injected part, this values was considered enough. More complex parts could require smaller steps in order to ensure proper performance of the mold used. Memoria 34 Melt temperature (°C) Low Holding Pressure (bar) High Holding Pressure (bar) 195 150 100 265 400 350 Table 7. Process Window Worksheet Step 4: Determining the Gate Seal Time – Gate Seal Study The molten plastic enters the cavity through the gate. The mold filing phase is dynamic, during which melt temperature, pressure, and flow velocity are all changing with time. For the mold fill phase, time begins with injection, which is the start of the forward movement of the screw. As the cavity begins to fill and is nearly full, the pack and hold pressure phase starts. The melt flow velocity is reduced and the melt temperature simultaneously drops. This cause an increase of viscosity of the melt. The gate has a fixed cross sectional area. When the viscosity of the plastic in this and the surrounding area it drops to a value at which the plastic cannot flow anymore, the gate is considered frozen. The plastic molecules in the gate are now immobile and cannot flow into the cavity anymore. The time it takes to reach this stage is called the gate freeze time. Within the injection molding process, the pressure must be applied to the melted plastic until such time that the gate is frozen. If the pressure is no applied enough time, either the part will appear with internal voids sinks or plastic pressure inside the cavity is high enough to flow back out of the cavity and then will also result in a under-packing part. Figure 17. Gate seal graph Gate freeze time is a function of the type of plastic, gate geometry and the processing parameters of the machine. A gate freeze study is a graph of part weight versus holding time. Once the gate is froze, the part 11.00 11.10 11.20 11.30 11.40 11.50 11.60 0100 200 300 400 500 600 Part weight (g) Holdin pressure (bar) Gate Seal Study Memoria 35 weight will remain constant due the plastic can no longer get into or out of the cavity. A constant part weight is an indication of gate freeze. Figure 18 shows the study for part studied in this work. In this procedure, the injection speed was set to the value obtained from viscosity curve experiment. HP time was set high enough to no influence in the experiment. The value 300 bar of HP was considered the value in which part weight start to remain constant. Table 8 shows the values plotted in the gate seal graph. HP time (s) HP (bar) Average part weight (g) SD 30 50 11.11 ± 0.035 30 100 11.30 ± 0.007 30 150 11.36 ± 0.000 30 200 11.40 ± 0.000 30 250 11.43 ± 0.007 30 300 11.46 ± 0.000 30 350 11.47 ± 0.006 30 400 11.47 ± 0.002 30 450 11.47 ± 0.001 30 500 11.47 ± 0.001 30 550 11.47 ± 0.006 Table 8. Gate Seal Study Worksheet Once the optimal HP value was obtained, a study of optimal HP time was carried out. It consists on, using the optimal HP value, decrease the HP time until the weight part starts to also decrease. Table 9 shows the experiment. HP time (s) HP (bar) Average part weight (g) SD 30 300 11.46 ± 0.000 27 300 11.45 ± 0.000 24 300 11.43 ± 0.000 21 300 11.40 ± 0.000 18 300 11.30 ± 0.006 15 300 11.17 ± 0.061 12 300 10.54 ± 0.055 Table 9. Gate Seal Time Worksheet From this study, the optimal HP time was set to 18s. Figure 19 shows how the part weight varies when HP time decreases. Memoria 36 Figure 18. Gate Seal Time Graph Step 5. Determining the Cooling Time – Cooling Time Study Once the Holding Pressure Time is finished, the set cooling time starts. The plastic starts to cool down as soon as it hits the walls of the mold. The mold will remain closed until the end of the cooling time. After that, the part is ejected. Before the part is ejected, it needs to be reach the ejection temperature. If the part is ejected with not enough cooling time, it will be too soft and will get deformed during the injection. Otherwise, excessive cooling time is related to a waste of machine time and therefor profits. Cooling time should also be set so that the part dimensions remain consistent and the process is capable of molding acceptable parts over the time. The process used to determine to optimal cooling time is based on the final dimension part which depends directly on the time that the part remains inside the mold after to be injected. The standard process was not followed due to the dimensions of the part were not considered a critical point for the work. Different cooling times were tested and 18s was considered as good in order to obtain good parts ensuring that the part was solid enough to be ejected. Step 6. Determining the Screw Speed and Back Pressure – Dosing Phase Study There are no scientific experiments that can be easily performed to optimize screw speed or back pressure. The screw speed should be set such that the screw always recovers before the end of the cooling time and not degrades the material due shear stresses. Unlike amorphous plastics, in crystalline plastics, higher screw speeds are recommended because the melting of the crystallites require high energy that can be supplied by shear of the rotating screw. The heat from the heater bands may not be sufficient to produce a homogeneous and uniform melt. 10.00 10.20 10.40 10.60 10.80 11.00 11.20 11.40 11.60 10 15 20 25 30 35 Part weight (g) Holdin pressure time (s) Gate Seal Time Study Memoria 37 Maximal lineal screw speed recommended by the material manufacturer is 0.7 m/s for this grade. Taking into account the diameter of the screw used in this work, the maximal RPM used in this work was calculated as follows: 𝜔=𝑣∗60 ∅∗𝜋 =534.76 𝑟𝑝𝑚 (eq. 1) Where:  v is the lineal speed (m/s)  ø is the diameter of the screw used (m)  1 revolution is 2 π rad The obtained value is the maximum recommended by the manufacturer in rpm taking into account the screw used in this work. The value obtained above is high due to the small value of the screw diameter. The shear from the rotating screw contributes a significant amount of energy to help melt the plastic. The mold does not open until the screw recovery is completed and the cooling times are reached. If screw recovery takes longer than cooling time, the effective cooling time increases because the mold is still closed. Then taking into account the cooling time determined previously, the lowest value for the screw speed was set to 50 rpm. Otherwise, highest screw speed was limited by the IMM used to 300 rpm and not by the material manufacturer. The optimum back pressure is the lowest possible pressure to keep the screw recovery time consistent and avoid any surface and/or internal defects visible on the part. Surface defect would include splay and internal defects would include bubbles and voids. Back pressure was set to 55 bar as optimal value taking into account the recommendation of the manufacturer and finally, fine tuning by the necessity of the process. At the end of the optimization of the process, most important injection molding parameters were fixed. Table 10 shows all of this parameters: Parameter Value Unit Injection speed 70 mm/s Melt temp. Range 195-265 °C HP 300 bar HP time 18 s Screw speed <300 rpm Back pressure 55 bar Table 10. Summary of optimal injection molding parameters Memoria 38 4.6. Design of experiments (DOE) The goal in this stage was to get the best combination of parameters in which the high dispersion of nanoadditive was reached. The experiments were carried out using a formulation made up of the selected PP as matrix and Cloesite20 as nano-additive. Some investigation’s groups have investigated how to optimize the injection moulding process to get best results of nano-additive dispersions. For example: [45], with PP and multiwall carbon nanotubes, [46] with PP and nano-clay nano-composites and [15] with thermoplastics and carbon nanotubes nano-composites studied the nano-additive dispersion with four injection parameters: Injection rate, screw rotational rate, back pressure and melt temperature. Another example is [47] with PC and multi-walled carbon nanotubes [4] using different injection parameters: holding pressure, injection rate, mould temperature and melt temperature. The suggested DOE consists of four parameters with two levels as shown in Table 11: Factors Assigned test Level Barrel temperature[ºC] Injection Rate [mm/s] Back Pressure (BP) [bar] Screw rotational Speed [rpm] Low Level (L) 200 50 30 50 High Level (H) 260 90 80 300 Experiment Nº X1 X2 X3 X4 1 240 90 80 300 2 240 90 80 50 3 240 90 30 300 4 240 90 30 50 5 240 50 80 300 6 240 50 80 50 7 240 50 30 300 8 240 50 30 50 9 200 90 80 300 10 200 90 80 50 11 200 90 30 300 12 200 90 30 50 13 200 50 80 300 14 200 50 80 50 15 200 50 30 300 16 200 50 30 50 Table 11. Details of DOE Injection parameters codification is recommended for two reasons. On the one hand, it is easier to understand the results achieved maintaining the order of magnitude. On the other hand, the loss of decimals during the matrix calculations can be magnified depending on the injection parameter’s order of magnitude. The codified table is shown below (Table 12). Memoria 39 Factors Assigned test Level Barrel temperature[ºC] Injection Rate [mm/s] Back Pressure (BP) [bar] Screw rotational Speed [rpm] High Level (H) 200 50 30 50 Low Level (L) 260 90 80 300 Experiment Nº X1 X2 X3 X4 1 +1 +1 +1 +1 2 +1 +1 +1 -1 3 +1 +1 -1 +1 4 +1 +1 -1 -1 5 +1 -1 +1 +1 6 +1 -1 +1 -1 7 +1 -1 -1 +1 8 +1 -1 -1 -1 9 -1 +1 +1 +1 10 -1 +1 +1 -1 11 -1 +1 -1 +1 12 -1 +1 -1 -1 13 -1 -1 +1 +1 14 -1 -1 +1 -1 15 -1 -1 -1 +1 16 -1 -1 -1 -1 Table 12. DOE table with codified parameters From these parameters, the 16 corresponding experiments were carried out and the samples were mechanically tested to obtain an output that was be used to apply linear modelling in order to optimize the process. Table 13 shows two examples of commercial grades of compounded PP with enhanced mechanical properties. A lineal modelling was used in order to maximize the Flexural Modulus The aim of the work is to maximize the Flexural Modulus thus a linear modelling was run to obtain the highest value of Flexural Modulus as possible Property Innopol CS2-9120 (20wt.% talc) SABIC PP compound 7715 Density (g/cm3) 1,04 1 MFR (g/10 min) 30 20 Tensile modulus (MPa) 2100 Tensile stress (MPa), yield 25 26 Tensile strain (%), yield 3 Tensile strain (%), break 60 Flexural modulus (MPa) 2200 1800 Table 13. Target properties Memoria 40 4.7. Lineal modelling For the four selected parameters and two levels for each one, a lineal model has been used to determine the effect of each parameter in the dispersion. The output for modelling was the Flexural Modulus and the input was all 16 experiments. Five samples have been tested for each experiment getting a total of 80 flexural tests. General equation to solve for a lineal model was: 𝑌=𝛽 󰆹𝑋→𝛽 󰆹=(𝑋′𝑋)−1𝑋′𝑌→ 𝑌 =𝛽 󰆹𝑋 (eq. 2) Where: 𝑌= [ 𝑌1 𝑌2 𝑌3 ⋮ 𝑌𝑛 ] ; 𝑋= [ 1 𝑋11 𝑋21 𝑋11𝑋21 𝑋𝑛𝑘 𝑚 1 𝑋11 𝑋22 … … 1 1 ⋮ 1 𝑋12 𝑋12 ⋮ 𝑋1𝑘 𝑋21 … … 𝑋22 … … ⋮ 𝑋2𝑘 … … ] → 𝛽 󰆹= [ 𝛽 󰆹0 𝛽 󰆹1 𝛽 󰆹2 𝛽 󰆹12 ⋮ 𝛽 󰆹𝑛 ] (eq. 3)  𝑌  is the output or response of the model  𝑋 is the input from all experiments (independent variables)  𝛽 󰆹 are the estimated coefficients In this case, a first model was proposed taking into account all possible interactions between the selected parameters: 𝑌 = 𝛽0+𝛽1𝑋1+𝛽2𝑋2+𝛽3𝑋3+𝛽4𝑋4+𝛽12𝑋1𝑋2+𝛽13𝑋1𝑋3+𝛽14𝑋1𝑋4+𝛽23𝑋2𝑋3+𝛽24𝑋2𝑋4 (eq. 4) Where:  𝛽0 is the origin de coordinates  𝛽1 coefficient related to barrel temperature  𝛽2 coefficient related to injection rate  𝛽3 coefficient related to back pressure  𝛽4 coefficient related to screw rotational rate  𝛽12 is related to interactions between 𝛽1and 𝛽2  𝛽13 is related to interactions between 𝛽1and 𝛽3  𝛽14 is related to interactions between 𝛽1and 𝛽4  𝛽23 is related to interactions between 𝛽2and 𝛽3  𝛽24 is related to interactions between 𝛽2and 𝛽4 Memoria 47 First step consisted of deleting the highest value, which was related to β3. Next steps consisted of recalculate the model without the rejected coefficient. This two steps will be carried out until all p-values are below 0.025. Iterations are shown in Table 15 to Table 17. Coefficient β Diagonal (𝑿′𝑿) −𝟏 Error (Sβj ) T p β0 1760,92 0,013 4,181 β1 -108,58 0,013 4,181 -25,972 0,000 β2 2,17 0,013 4,181 0,519 0,605 β4 16,67 0,013 4,170 3,997 0,000 β12 -49,33 0,013 4,181 -11,799 0,000 β13 -1108,07 0,013 4,181 -265,041 0,000 β14 -17,33 0,013 4,170 -4,156 0,000 β23 2,67 0,013 4,181 0,638 0,525 β24 -12,58 0,013 4,170 -3,017 0,004 Table 15. Model validation's first iteration Coefficient β Diagonal (𝑿′𝑿) −𝟏 Error (Sβj ) T p β0 1760,82 0,013 4,189 β1 -108,68 0,013 4,189 -25,947 0,000 β4 16,71 0,013 4,178 3,999 0,000 β12 -49,43 0,013 4,189 -11,801 0,000 β13 -11,18 0,013 4,189 -2,670 0,009 β14 -17,29 0,013 4,178 -4,139 0,000 β23 2,57 0,013 4,189 0,613 0,542 β24 -12,54 0,013 4,178 -3,002 0,004 Table 16. Model validation's second iteration Coefficient β Diagonal (𝑿′𝑿) −𝟏 Error (Sβj ) T p β0 1760,70 0,013 4,200 β1 -108,80 0,013 4,200 -25,906 0,000 β4 16,75 0,013 4,189 3,999 0,000 β12 -49,55 0,013 4,200 -11,798 0,000 β13 -11,30 0,013 4,200 -2,690 0,009 β14 -17,25 0,013 4,189 -4,118 0,000 β24 -12,50 0,013 4,189 -2,984 0,004 Table 17. Model validation's third iteration After all iterations, a consistent model was obtained. Note that some coefficient parameters or coefficient interaction between parameter have been disappeared. The coefficients related to injection rate and back pressure were deleted but remained in the interactions. The final model is shown below: 𝐘 =𝟏𝟕𝟔𝟎,𝟕−𝟏𝟎𝟖,𝟖𝐗𝟏+𝟏𝟔,𝟕𝟔𝐗𝟒−𝟒𝟗,𝟓𝟓𝐗𝟏𝐗𝟐−𝟏𝟏,𝟑𝐗𝟏𝐗𝟑−𝟏𝟕,𝟐𝟓𝐗𝟏𝐗𝟒−𝟏𝟐,𝟓𝐗𝟐𝐗𝟒 (eq.10) Memoria 48 4.11. Results Once the model was solved, four response surfaces had been plotted. Each surface can represent 2 inputs (i.e. injection rate and back pressure) and the behaviour of the two remaining related to the output can be observed. An example is shown in Figure 26: Figure 26. Example of a surface response Note that the plot above has two variable parameters (melt temperature and injection rate) which varies from -1 to +1 due to the codification. The other two parameters (back pressure and screw rotational rate) have been fixed which in this case, are represented +1 for back pressure and +1 for screw rotational rate (maximum level). All 16 response surfaces are shown in ¡Error! No se encuentra el origen de la eferencia.. In one hand, if two parameters are fixed and two are variable, four combinations of them are possible. On the other hand, 4 combinations between fixed and variable parameters are possible which results in 16 surfaces. A summary of all combinations is shown in Table 18: Memoria 49 SURFACE 1 SURFACE 2 SURFACE 3 SURFACE 4 FIXEDED VARIABLE FIXED VARIABLE FIXED VARIABLE FIXED VARIABLE X3+ X4+ X1- X2+ X2+ X3+ X1- X4+ X1+ X2+ X3- X4- X1+ X4+ X2+ X3- X3+ X4- X1- X2+ X2+ X3- X1- X4+ X1+ X2- X3- X4+ X1+ X4- X2- X3- X3- X4- X1- X2+ X2- X3- X1- X4+ X1- X2- X3+ X4+ X1- X4- X2+ X3+ X3- X4+ X1- X2+ X2- X3+ X1- X4+ X1- X2+ X3+ X4+ X1- X4+ X2+ X3+ Table 18. Summary of the 16 surfaces response All possible combinations between parameters were plotted. Columns called FIXED are the immovable parameters (only was used one value: maximum level or minimum level). Otherwise, columns called VARIABLE are represented the variable parameter behaviour in order to obtain the high output value (Flexural Modulus). In Figure 27, X3 and X4 are fixed for the high level. In order to obtain the best output value, low level of melt temperature (X1 = -1) and high level of injection rate (X2 = +1) were required. Table 19 was created following the steps mentioned above. SURFACE 1 SURFACE 2 SURFACE 3 SURFACE 4 FIXEDED VARIABLE FIXED VARIABLE FIXED VARIABLE FIXED VARIABLE X3+ X4+ X1- X2+ X2+ X3+ X1- X4+ X1+ X2+ X3- X4- X1+ X4+ X2+ X3- X3+ X4- X1- X2+ X2+ X3- X1- X4+ X1+ X2- X3- X4+ X1+ X4- X2- X3- X3- X4- X1- X2+ X2- X3- X1- X4+ X1- X2- X3+ X4+ X1- X4- X2+ X3+ X3- X4+ X1- X2+ X2- X3+ X1- X4+ X1- X2+ X3+ X4+ X1- X4+ X2+ X3+ Table 19. Relations between surfaces response From Surface 1 and 2, two important facts were concluded: whatever combination of fixed parameters gave the same behaviour of variable parameter meaning that low level of melt temperature(X1- ), high level of injection rate (X2+), and high level of screw rotational rate(X4+), boosts the output value that is the flexural modulus obtained is higher. FIXING X1- X2+ X3+ X4+ X1- X4+ X2+ X3+ Table 20. Summing-up from all the surfaces response Memoria 50 5. Conclusions Scientific Injection Molding is a tool that should be used for every mold set-up in order to ensure the best performance during the injection molding process. It allows to study the most significant parameters taking into account the IMM, the tool features and the rheology of the material used for each specific case. Minimal variation on the system i.e. material batch variation, gate tool, etc. will require a new iteration of the SIM steps. Therefore, this project is focused on a specific system but may be useful as a guideline for another system. 1. Four parameters have been studied to see the significance of them into the mechanical properties of the final part. In this case, the target properties was Flexural Modulus of a standard specimen and depends on the application of the injected part, different property could be studied. 2. After the model was calculated and validated some trends were obtained. High values of back pressure, screw rotational speed and injection speed boosted the output of the model (Flexural Modulus) while low values of melt temperature also boosted the Flexural Modulus. 3. On one hand, high values of back pressure and screw rotational speed may maintain or improve the dispersion achieved during the extrusion compounding. High injection rate may aid the additives orientation and then keep them homogenous. 4. On the other hand, at first sight, high melt temperature should improve the nano-additives mobility but in this case, high temperature and then high viscosity may ease the nano-additive reaggregation and then reduce the mechanical. 5. To sum up, low values of melt temperature and high values of injection rate, back pressure and screw rotational speed will be required to achieve high values of Flexural Modulus. Memoria 51 Memoria 52 6. References [1] “https://www.plasticseurope.org,” [Online]. [2] P. E. P. E. a. T. H. H. Domininghaus, Kunststoffe: Eigenschaften und Anwendungen ; mit 240 Tabellen, Springer-Verlag GmbH, 2008. [3] D. Braun, Kunststofftechnik für Einsteiger, Hanser, 2003. [4] W. Kaiser, Kunststoffchemie für Ingenieure, Hanser Fachbuchverlag, 2007. [5] D. L. H. D. C. S. K. J. L. W. J. W. C. e. a. H. R. Dennis, “Effect of melt processing conditions on the extent of exfoliation in organoclay-based nanocomposites,” Polymer, vol. 42, pp. 9513-9522, 2001. [6] N. E. H. J. J. L. a. R. A. P. C. P. McAdam, “Synthesis and characterization of nylon 6/clay nanocomposites prepared by ultrasonication and in situ polymerization,” Journal of Applied Polymer Science, vol. 108, pp. 2242-2251, 2008. [7] R. K. S. D. L. H. a. D. R. P. F. Chavarria, “Effect of melt processing conditions on the morphology and properties of nylon 6 nanocomposites,” Polymer Engineering and Science, vol. 47, pp. 1847-1864, 2007 xxxxx. [8] D. R. P. a. L. M. Robeson, “Polymer nanotechnology: Nanocomposites,” Polymer, vol. 49, pp. 3187- 3204, 2008. [9] S. K. S. a. A. I. I. S. Lapshin, “Ultrasound aided extrusion process for preparation of polyolefin-clay nanocomposites,” Polymer Engineering and Science, vol. 48, pp. 1584-1591, 2008. [10] E. Bugnicourt, “Development of sub-micro structured composites based on an epoxy matrix and pyrogenic silica: mechanical behavior related to the interactions and morphology at multi-scale,” Villeurbanne, INSA, 2005. [11] S. P. P. P. a. U. W. T. Villmow, “Influence of injection molding parameters on the electrical resistivity of polycarbonate filled with multi-walled carbon nanotubes,” Composites Science and Technology, vol. 68, pp. 777-789, 2008. [12] A. J. K. X. H. a. L. S. T. A. Chandra, "Effect of injection molding parameters on the electrical conductivity of polycarbonate/carbon nanotube nanocomposites," in Annual Technical Conference - ANTEC, 2007. [13] L. I. S. a. C. F. F. Stan, “Effect of processing parameters and strain rate on mechanical properties of carbon nanotube-filled polypropylene nanocomposites,” Composites Part B-Engineering, vol. 59, pp. 109-122, 2014. Memoria 53 [14] V. P. J. V. A. P. A. P. a. P. F. A. Costantino, “Microstructure of PP/clay nanocomposites produced by shear induced injection moulding,” in 11th International Congress on Metallurgy & Materials, 2011. [15] P. F. Rios, A. Ophir, S. Kenig, R. Efrati, L. Zonder and R. Popovitz-Biro., "Impact of injection-moulding processing parameters on the electrical, mechanical, and thermal properties of thermoplastic/carbon nanotube nanocomposites.," 11th October 2010. [Online]. [Accessed 7th January 2018]. [16] M. Okamoto, “Recent advances in polymer/layered silicate nanocomposites: an overview from science to technology,” Materials Science and Technology , vol. 22, no. 7, pp. 756-779 , 2006. [17] J. Zhang, E. Manias and C. A. Wilkie, "Polymerically Modified Layered Silicates: An Effective Route to Nanocomposites," Journal of Nanoscience and Nanotechnology, vol. 8, no. 4, pp. 1597-1615, 2008. [18] C. D. P. S. Pavlidou, “A review on polymer–layered silicate nanocomposites,” Progress in Polymer Science, vol. 33, no. 12, pp. 1119-1198, 2008. [19] p. a. u. o. a. n. c. o. m. Polymer-layered silicate nanocomposites: preparation, “Michael Alexandre, Philippe Dubois,” Polymer-layered silicate nanocomposites: preparation, properties and uses of a new class of materials, vol. 28, no. 1-2, pp. 1-63, 2000. [20] A. K. B. C. O. Anusuya Choudhury, “Novel role of polymer–solvent and clay–solvent interaction parameters on the thermal, mechanical and optical properties of polymer nanocomposites,” Polymer, vol. 50, no. 1, pp. 201-210, 2009. [21] H. H.Murray, “Overview — clay mineral applications,” Applied Clay Science, vol. 5, no. 5-6, pp. 379- 395, 1991. [22] [Online]. Available: www.moldedfiberglass.com/library/news/newsCW8-09.pdf. [23] J. G. H. D. S. B. L.W Carter, "Elastomer Reinforced with a Modified Clay". US Patent 2,531,396, 1950. [24] P. G. N. a. P. S. Backlund, "Organoclay-Polyolefin Compositions". US Patent 3,084,117, 1963. [25] T. S. S. Fujiwara, “Method for Manufacturing a Clay/Polyamide Composite”. Japanese Kokai Patent Application Patent 109,998, 1976. [26] Y. F. a. S. Inagaki, “Synthesis of an Intercalated Compound of Montmorillonite and 6-Polyamide,” Journal of Inclusion Phenomena, vol. 5, pp. 473-482, 1987. [27] Y. K. M. K. A. O. Y. F. T. K. a. O. K. A. Usuki, “Synthesis of Nylon 6–Clay Hybrid,” Journal of Materials Research, no. 8, pp. 1179-1184, 1993. [28] T. M. Y. F. M. F. K. F. Y. K. ,. N. T. K. a. O. K. A. Usuki, “Composite Material containing a Layered Silicate”. US Patent 4,889,885, 1989. Memoria 54 [29] Y. K. e. al., “Sorption of Water in Nylon 6-clay Hybrid,” Journal of Applied Polymer Science, no. 4, pp. 1259-1264, 1993. [30] K. F. A. U. Y. K. N. S. T. K. a. O. K. A. Okada, “Rubber-Clay Hybrid-Synthesis and Properties,” ACS Polym Preprints, no. 32, pp. 540-541, 1991. [31] A. U. A. Okada, “The Chemistry of Ppolymer-Clay Hybrids,” Materials Science and Engineering, no. C 3, pp. 109-115, 1995. [32] K. Y. K. U. A. O. a. A. T. Kurauch, “Polyimide Composite Material and Process for Producing the Same”. US Patent 5,164,46, 17 Nov 1992. [33] A. U. a. A. O. K. Yano, “Synthesis and Properties of Polyimide-Clay Hybrid Films,” Journal of Applied Polymer Science: Part A, Polym Chem., no. 35, pp. 2289-2294, 1997. [34] F. Gao, “Clay/Polymer Composites:The Story,” Materials Today, no. 7, pp. 50-55, 2004. [35] C. Edser, “Auto Applications of Drive Commercialization of Nanocomposites,” Plastic Additives Compounding, no. 4, pp. 30-33, 2002. [36] A. O. T. N. T. N. S. S. a. R. D. T. Kurauchi, “Nylon 6-Clay Hybrid - Synthesis, Properties and Application to Automotive Timing Belt Cover,” SAE Technical Paper Ser, 910584, 1991. [37] e. a. H.Cox, “Nanocomposite Systems for Automotive Applications,” in 4th World Congress in Nanocomposites, EMC, San Francisco, 2004. [38] M. N. J. B. Q.Z. Zhao, “Ultimate Strength of Carbon nanotubes: A Theoretical Study,” Phys. Rev. B, no. 65, 2002. [39] B. O. I. A. R. R. a. D. A. R. Prud'homme, “"Functional Graphene–Rubber Nanocomposites"”. US Patent 7,745,528, 29 Jun 2010. [40] B. Z. J. Aruna Zhamu, “Pristine Nano Graphene-Modified Tires”. US Patent 7,999,027, 16 Aug 2011. [41] S. B. A. S. N. Tahmassebi, "Effect of addition of hydrophobic nano silica on viscoelastic properties and scratch resistance of an acrylic/melamine automotive clearcoat," TribologyInternational, no. 43, p. 685–693, 2010. [42] S. R. Zahra Ranjbara, “Nano mechanical properties of an automotive clear-coats containing nano silica,” Progress in Organic Coatings, no. 72, pp. 40-43, 2011. [43] M. M. M. M. Z. R. H. Yari, “Tribological properties and scratch healing of a typical automotive nano clearcoat modified by a polyhedral oligomeric silsesquioxane compound,” European Polymer Journal, no. 60, pp. 79-91, 2014. [44] A. K. M. H. L. T. D. G. B. Ermias G Koricho1, “Effect of hybrid (micro- and nano-) filler on impact response of GFRP composite,” Composite Structures, 2015. Memoria 55 [45] K. Prashantha, J. Soulestin, M. F. Lacrampe, E. Lafranche, P. Krawczak, G. Dupin and M. Claes., "Taguchi analysis of shrinkage and warpage ofinjection-moulded polypropylene/multiwall carbon nanotubes nanocomposites.," eXPRESS Polymer Letters, pp. 630-638, 2009. [46] J. J. Rajesh, J. Soulestin, M. F. Lacrampe and P. Krawczak., "Effect of injection moulding parameters on nanofillers dispersion in masterbatch based PP-clay nanocomposites.," eXPRESS Polymer Letters Vol.6, p. 237–248, 2012. [47] T. Villmow, S. Pegel, P. Pötschke and U. Wagenknecht., "Influence of injection moulding parameters on the electrical resistivity of polycarbonate filled with multi-walled carbon nanotubes.," Composites Science and Technology 68, p. 777–789, 2008. [48] S. Kulkarni, Robust Process Development. Theory and Practice, Munich: Hanser, 2010. [49] P. Dominick V. Rosato, Plastic Processing Data Handbook,, Second ed., Chatham, MA, 02633: Chapman & Hall, 1997. [50] D. M. Bryce, Plastic Injection Molding, vol. Manufacturing process fundamentals, Dearborn, Michigan: Society of Manufacturing Engineers, 1996. Memoria 56 7. Annex 7.1. Annex 1. Surface responses All surfaces response are shown as a result of the mathematical model in this annex. Figure 27. Surface response 1. Fixed parameters: Back pressure and Screw rotational rate. Variable parameters: Melt temperature and Injection rate. Memoria 63 Figure 40. Surface response 14. Fixed parameters: Screw rotational rate and melt temperature. Variable parameters: injection rate and back pressure. Figure 41. Surface response 15. Fixed parameters: Screw rotational rate and melt temperature. Variable parameters: injection rate and back pressure Memoria 64 Figure 42. Surface response 16. Fixed parameters: Screw rotational rate and melt temperature. Variable parameters: injection rate and back pressure.