scieee AI-readable full text Open interactive document viewer

Hemp crop waste for green solutions in construction: physical and mechanical characterization

Martínez Martínez, Borja

Abstract

(English) The primary goal of this thesis is to unlock the potential of hemp stalk, an agricultural byproduct that currently lacks practical applications. The overarching aim is to promote the use of eco-friendly materials, reduce waste, emphasize recyclability, and embrace the principles of a circular economy, all while combating climate change by adopting more sustainable materials in lieu of synthetic ones. To achieve these objectives, an extensive review of existing literature served as an initial step to explore the untapped potential of hemp stalk. This thorough exploration identified five possible applications: acoustic insulation materials, thermal insulation materials, particleboard, coffered ceiling, and parquet flooring. Subsequent research delved into identifying suitable plant-based binders and environmentally responsible manufacturing techniques. Following this material-focused phase, an initial investigation was carried out by experimenting with various materials and manufacturing methods to ascertain which of the five applications held the most promise. The results were particularly encouraging for insulation materials, although coffered ceiling also displayed significant potential. The insulation materials utilize recycled cardboard as a binder and employ manufacturing methods with minimal energy consumption during mixing and drying, resulting in low carbon emissions and sustainable materials. Once the material was selected, efforts were made to enhance its properties. This involved incorporating a plant-based coating (comprising arabic gum and colophony) to provide protection and introducing a crosslinking agent (citric acid) to bolster durability and material properties. These additions were meticulously assessed through a battery of tests related to thermal and acoustic insulation, mechanical characteristics, water resistance, fire resistance, and chemical analysis, such as FTIR spectroscopy. To validate the material’s performance, durability tests were conducted, exposing samples to humidity cycles over 0, 3, 6, and 9 months, alongside a scaled-down life cycle analysis. The end result was a material boasting superior thermal insulation properties compared to commercial alternatives, albeit with slightly lower acoustic insulation performance. Notably, citric acid was found to marginally enhance the material’s durability. Furthermore, it was determined that different coatings could be selected depending on the application environment, thereby optimizing specific properties.

Full text

Hemp crop waste for green solutions in construction: physical and mechanical characterization Author: Borja Mart´ınez Mart´ınez Director/Co-director: Llu´ıs Gil Espert Ernest Bernat Mas´o Ph.D. program Enginyeria Mec`anica, Fluids i Aeron`autica Examination session: Autum 2023 Hemp crop waste for green solutions in construction: physical and mechanical characterization Author: Borja Mart´ınez Mart´ınez Director/Co-director: Llu´ ıs Gil Espert Ernest Bernat Mas´o Ph.D. thesis presented to obtain the Doctoral degree by the Universitat Polit`ecnica de Catalunya Ph.D. program: Enginyeria Mec`anica, Fluids i Aeron`autica Departament de Resist`encia de Materials i Estructures a l’Enginyeria CATMech - Centre Avan¸cat de Tecnologies Mec`aniques 19 October 2023 Terrassa Hemp crop waste for green solutions in construction: physical and mechanical characterization Acknowledgedment I would like to begin by expressing my gratitude to my thesis directors, Llu´ıs Gil and Ernest Bernat, who have shown confidence in me for the past six years. It all started with my internships and TFG at LITEM, which is now CATMECH. They have continuously supported me and kept me engaged in research activities, leading to my doctoral studies. Their positive work environment, camaraderie, support in learning, and enthusiasm for research greatly influenced my decision to pursue an academic career. I extend my thanks to all my colleagues at CATMECH, particularly Virginia Mendizabal and Luis Mercedes, for their invaluable assistance, guidance, and the shared moments we’ve experienced over these years. I’d also like to acknowledge Jordi Cabrerizo, the laboratory technician at CATMECH, who provided crucial support during the experimental campaign in the past year. My appreciation goes out to the members of CELBIOTECH for warmly welcoming me into their group and helping me become acquainted with equipment I initially wasn’t familiar with. I am grateful to the researchers from other departments who lent their support throughout my research journey; Blanca Roncero, Xavier Ca˜navate, Monica Ardanuy and Manel Lis. I also want to thank the students who participated in the project through their final degree projects (TFEs). Andrea, Pol, Mireia, Pau, Josep, and Pau, your contributions created a positive research environment where we learned and grew together. To my family, I extend heartfelt thanks for their unwavering support, no matter the circumstances, all the way from Alicante. And to my friends, with whom I’ve shared countless memorable moments, some dating back to when we were just three years old in Alicante, and others during our university years in Terrassa. I would like to express our gratitude to ACCIO for their invaluable funding of the Valsucanem project (grant number VALSUCANEM ACE014/20/000024 ), which has made this thesis possible. This support has enabled us to carry out scientific research, resulting in the publication ”Applications and Properties of Hemp Stalk-Based Insulating Biomaterials for Buildings: Review” in the Materials Q2 journal [1]. Additionally, we appreciate the opportunity to participate in the MATCOMP21 conference in Sevilla, where we presented ”Study of an insulating hemp-based bio-material: mechanical, thermal, and acoustic properties” [2]. We eagerly anticipate the future publication in the Q1 journal Materials titled ”Towards Sustainable Building I Solutions: Development of Hemp Stalk-Based Green Insulation Material,” which is currently undergoing the review process. I appreciate UPC and Banco Santander for their support of my research through the FPU-UPC scholarship. Finally, to you, the reader, I express my gratitude for taking the time to delve into this research, which has been a significant part of my life’s journey. I hope you find it engaging and informative, serving as a valuable source of knowledge. II Hemp crop waste for green solutions in construction: physical and mechanical characterization Abstract The primary goal of this thesis is to unlock the potential of hemp stalk, an agricultural byproduct that currently lacks practical applications. The overarching aim is to promote the use of eco-friendly materials, reduce waste, emphasize recyclability, and embrace the principles of a circular economy, all while combating climate change by adopting more sustainable materials in lieu of synthetic ones. To achieve these objectives, an extensive review of existing literature served as an initial step to explore the untapped potential of hemp stalk. This thorough exploration identified five possible applications: acoustic insulation materials, thermal insulation materials, particleboard, coffered ceiling, and parquet flooring. Subsequent research delved into identifying suitable plant-based binders and environmentally responsible manufacturing techniques. Following this material-focused phase, an initial investigation was carried out by experimenting with various materials and manufacturing methods to ascertain which of the five applications held the most promise. The results were particularly encouraging for insulation materials, although coffered ceiling also displayed significant potential. The insulation materials utilize recycled cardboard as a binder and employ manufacturing methods with minimal energy consumption during mixing and drying, resulting in low carbon emissions and sustainable materials. Once the material was selected, efforts were made to enhance its properties. This involved incorporating a plant-based coating (comprising arabic gum and colophony) to provide protection and introducing a crosslinking agent (citric acid) to bolster durability and material properties. These additions were meticulously assessed through a battery of tests related to thermal and acoustic insulation, mechanical characteristics, water resistance, fire resistance, and chemical analysis, such as FTIR spectroscopy. To validate the material’s performance, durability tests were conducted, exposing samples to humidity cycles over 0, 3, 6, and 9 months, alongside a scaled-down life cycle analysis. The end result was a material boasting superior thermal insulation properties compared to commercial alternatives, albeit with slightly lower acoustic insulation performance. Notably, citric acid was found to marginally enhance the material’s durability. Furthermore, it was determined that different coatings could be selected depending on the application environment, thereby optimizing specific properties. III Hemp crop waste for green solutions in construction: physical and mechanical characterization Resum L’objectiu principal d’aquesta tesi ´es revelar el potencial dela canemuixa, un subproducte agr´ıcola que actualment manca d’aplicacions pr`actiques. L’objectiu general ´es promoure l’´us de materials respectuosos amb el medi ambient, reduir els residus, fer `emfasi en la capacitat de reciclatge i abra¸car els principis d’una economia circular, tot mentre es combat el canvi clim`atic mitjan¸cant l’adopci´o de materials m´es sostenibles en lloc dels sint`etics. Per assolir aquests objectius, es va dur a terme una exhaustiva revisi´o de la literatura existent per explorar el potencial encara no aprofitat de la canemuixa. Es van identificar cinc possibles aplicacions: materials a¨ıllants ac´ustics i t`ermics, taulells aglomerats, cassetons i parquet. La investigaci´o posterior es va centrar en identificar aglutinants d’origen vegetal adequats i t`ecniques de fabricaci´o respectuoses amb el medi ambient. Despr´es, es va dur a terme una investigaci´o inicial experimentant amb diversos materials i m`etodes de fabricaci´o per determinar quina de les cinc aplicacions tenia m´es potencial. Els resultats van ser especialment esperan¸cadors pels materials a¨ıllants, tot i que els cassetons tamb´e van mostrar un gran potencial. Els materials a¨ıllants utilitzen cartr´o reciclat com a aglutinant i empren m`etodes de fabricaci´o amb un consum m´ınim d’energia durant la mescla i l’assecat, la qual cosa d´ona lloc a baixes emissions de carboni i materials sostenibles. Un cop seleccionat el material, es van fer esfor¸cos per millorar-ne les propietats. Aix`o va implicar la incorporaci´o d’un revestiment d’origen vegetal (goma ar`abiga i colof`onia) per proporcionar protecci´o i la introducci´o d’un agent de reticulaci´o (`acid c´ıtric) per refor¸car la durabilitat i les propietats del material. Aquestes addicions van ser avaluades a trav´es d’una s`erie de proves relacionades amb l’a¨ıllament t`ermic i ac´ustic, les caracter´ıstiques mec`aniques, la resist`encia a l’aigua, la resist`encia al foc, i l’espectrosc`opia FTIR. Per validar el rendiment del material, es van dur a terme proves de durabilitat que van exposar mostres a cicles d’humitat durant 0, 3, 6 i 9 mesos, juntament amb un an`alisi del cicle de vida a petita escala. El resultat final va ser un material amb propietats d’a¨ıllament t`ermic superiors a les alternatives comercials, tot i que amb un rendiment lleugerament inferior en l’a¨ıllament ac´ustic. Cabe destacar que l’`acid c´ıtric millorava marginalment la durabilitat del material. A m´es, es va determinar que es podrien seleccionar diferents revestiments segons l’entorn d’aplicaci´o, optimitzant aix´ı propietats espec´ıfiques. IV Hemp crop waste for green solutions in construction: physical and mechanical characterization Resumen El objetivo principal de esta tesis es revelar el potencial de la ca˜namiza, un subproducto agr´ıcola que actualmente carece de aplicaciones pr´acticas. El objetivo general es promover el uso de materiales respetuosos con el medio ambiente, reducir los residuos, hacer hincapi´e en la capacidad de reciclaje y abrazar los principios de una econom´ıa circular, todo ello mientras se combate el cambio clim´atico mediante la adopci´on de materiales m´as sostenibles en lugar de los sint´eticos. Para alcanzar estos objetivos, se llev´o a cabo una exhaustiva revisi´on de la literatura para explorar el potencial a´un no aprovechado de la ca˜namiza. Se identificaron cinco posibles aplicaciones: materiales aislantes ac´usticos y t´ermicos, tableros aglomerados, casetones y parquet. La investigaci´on posterior se centr´o en identificar aglutinantes de origen vegetal adecuados y t´ecnicas de fabricaci´on respetuosas con el medio ambiente. Tras esta fase centrada en el material, se llev´o a cabo una investigaci´on inicial experimentando con diversos materiales y m´etodos de fabricaci´on para determinar cu´al de las cinco aplicaciones ten´ıa m´as potencial. Los resultados fueron especialmente alentadores para los materiales aislantes, aunque los encofrados tambi´en mostraron un gran potencial. Los materiales aislantes utilizan cart´on reciclado como aglutinante y emplean m´etodos de fabricaci´on con un consumo m´ınimo de energ´ıa durante la mezcla y el secado, lo que resulta en bajas emisiones de carbono y materiales sostenibles. Una vez seleccionado el material, se realizaron esfuerzos para mejorar sus propiedades. Esto implic´o la incorporaci´on de un revestimiento de origen vegetal (goma ar´abiga y colofonia) para proporcionar protecci´on e introducir un agente de reticulaci´on (´acido c´ıtrico) para reforzar la durabilidad y las propiedades del material. Estas adiciones fueron evaluadas a trav´es de una bater´ıa de ensayos relacionados con el aislamiento t´ermico y ac´ustico, las caracter´ısticas mec´anicas, la resistencia al agua, la resistencia al fuego y la espectroscopia FTIR. Para validar el rendimiento del material, se llevaron a cabo pruebas de durabilidad que expusieron muestras a ciclos de humedad durante 0, 3, 6 y 9 meses, junto con un an´alisis del ciclo de vida a peque˜na escala. El resultado final fue un material con propiedades de aislamiento t´ermico superiores a las alternativas comerciales, aunque con un rendimiento ligeramente inferior en el aislamiento ac´ustico. Destacablemente, se descubri´o que el ´acido c´ıtrico mejoraba marginalmente la durabilidad del material. Adem´as, se determin´o que se podr´ıan seleccionar diferentes revestimientos seg´un el entorno de aplicaci´on, optimizando as´ı propiedades espec´ıficas. V Hemp crop waste for green solutions in construction: physical and mechanical characterization Contents 1 Introduction 1 1.1 The importance of hemp nowadays . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 1 1.2 Objectives............................................... 4 1.3 Methodology ............................................. 5 1.3.1 Stateoftheart........................................ 5 1.3.2 Initial exploration of various material options and the selection of the most promising one 5 1.3.3 Characterization and durability test of the selected material . . . . . . . . . . . . . . . 6 1.3.4 Lifecycle ........................................... 6 2 State of the art 8 2.1 History of hemp and its applications . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 8 2.2 Applications for low density solutions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 12 2.2.1 Commercialmaterial..................................... 12 2.2.2 Insulating properties of hemp stalk . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 13 2.3 Applications for medium density solutions . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 14 2.3.1 Commercialmaterial..................................... 14 2.3.2 Mechanical properties of hemp stalk . . . . . . . . . . . . . . . . . . . . . . . . . . . . 17 2.4 Greenbindermaterials ....................................... 18 2.4.1 Green binder for low density material . . . . . . . . . . . . . . . . . . . . . . . . . . . 21 2.4.2 Green binder for medium density material . . . . . . . . . . . . . . . . . . . . . . . . . 27 2.5 Lifecycle ............................................... 29 2.5.1 Carbon storage properties of hemp stalk . . . . . . . . . . . . . . . . . . . . . . . . . . 29 2.5.2 Durability of the selected green materials . . . . . . . . . . . . . . . . . . . . . . . . . 30 2.6 Conclusions.............................................. 32 3 Exploring applications 35 3.1 Lowdensitysolution......................................... 36 3.1.1 Materials ........................................... 36 3.1.2 Characterizationtest..................................... 36 3.1.3 Compatibility of the materials . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 37 VI LIST OF FIGURES LIST OF FIGURES A.4 Sample60E..............................................152 A.5 Sample50E..............................................152 A.6 Sample40E..............................................153 A.7 Sample30E..............................................153 A.8 Sample20E..............................................154 A.9 Sample0E ..............................................154 A.10 Sample 30E with different weight . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 155 A.11 Acoustic absorption of commercial materials . . . . . . . . . . . . . . . . . . . . . . . . . . . 156 A.12 Acoustic absorption of eucalyptus-hemp stalk samples along the thickness . . . . . . . . . . . 157 A.13 Comparison of acoustic absorption . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 157 A.14 Comparison of acoustic absorption of cardboard-hemp stalk samples . . . . . . . . . . . . . . 158 A.15 Comparison of acoustic absorption of durability samples . . . . . . . . . . . . . . . . . . . . 158 A.16 Temperature gradient-time of eucalyptus-hemp stalk samples . . . . . . . . . . . . . . . . . . 159 A.17 Temperature gradient-time of eucalyptus-hemp stalk samples with coating . . . . . . . . . . . 159 A.18 Temperature gradient-time of hemp stalk-cardboard samples . . . . . . . . . . . . . . . . . . 160 A.19 Temperature gradient-time of hemp stalk-cardboard durability M0 samples . . . . . . . . . . 160 A.20 Temperature gradient-time of hemp stalk-cardboard durability M3 samples . . . . . . . . . . 161 A.21 Temperature gradient-time of hemp stalk-cardboard durability M6 samples . . . . . . . . . . 161 A.22 Temperature gradient-time of hemp stalk-cardboard durability M9 samples . . . . . . . . . . 162 A.23 Compression test of eucalyptus-hemp stalk samples . . . . . . . . . . . . . . . . . . . . . . . 163 A.24 Compression test of hemp stalk-cardboard samples . . . . . . . . . . . . . . . . . . . . . . . . 163 A.25 Compression test of hemp stalk-cardboard durability M0 samples . . . . . . . . . . . . . . . . 164 A.26 Compression test of hemp stalk-cardboard durability M3 samples . . . . . . . . . . . . . . . . 164 A.27 Compression test of hemp stalk-cardboard durability M6 samples . . . . . . . . . . . . . . . . 165 A.28 Compression test of hemp stalk-cardboard durability M9 samples . . . . . . . . . . . . . . . . 165 A.29 Shear test of eucalyptus-hemp stalk samples . . . . . . . . . . . . . . . . . . . . . . . . . . . 166 A.30 Shear test of hemp stalk-cardboard samples . . . . . . . . . . . . . . . . . . . . . . . . . . . . 166 A.31 Shear test of hemp stalk-cardboard durability M0 samples . . . . . . . . . . . . . . . . . . . . 167 A.32 Shear test of hemp stalk-cardboard durability M3 samples . . . . . . . . . . . . . . . . . . . . 167 A.33 Shear test of hemp stalk-cardboard durability M6 samples . . . . . . . . . . . . . . . . . . . . 168 A.34 Shear test of hemp stalk-cardboard durability M9 samples . . . . . . . . . . . . . . . . . . . . 168 A.35 Bending test of hemp stalk-cardboard samples . . . . . . . . . . . . . . . . . . . . . . . . . . 169 A.36 Bending test of hemp stalk-cardboard durability M0 samples . . . . . . . . . . . . . . . . . . 169 A.37 Bending test of hemp stalk-cardboard durability M3 samples . . . . . . . . . . . . . . . . . . 170 A.38 Bending test of hemp stalk-cardboard durability M6 samples . . . . . . . . . . . . . . . . . . 170 A.39 Bending test of hemp stalk-cardboard durability M9 samples . . . . . . . . . . . . . . . . . . 171 XIII LIST OF FIGURES LIST OF FIGURES A.40 Tensile test of eucalyptus-hemp stalk samples . . . . . . . . . . . . . . . . . . . . . . . . . . . 172 A.41Sample30R-H-C-AC.........................................173 A.42Sample30R-H-C-0 ..........................................174 A.43Sample30R-H-GA-AC........................................175 A.44Sample30R-H-GA-0 .........................................176 A.45 Weight of the different samples during the MBV test . . . . . . . . . . . . . . . . . . . . . . . 177 A.46Tensiletest ..............................................178 A.47 Tensile test - first samples . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 179 A.48 Tensile test - manufacture modifications . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 180 A.49Bendingtest-Bestsamples .................................... 181 A.50 Bending test - first samples . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 182 A.51 Bending test - manufacture modifications . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 183 B.1 DatasheetBioepoxyONE ......................................184 B.2 Datasheet white glue HM-425 1/2 . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 185 B.3 Datasheet white glue HM-425 2/2 . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 186 B.4 Datashhetcitricacid1/2 ......................................187 B.5 Datasheetcitricacid2/2 ......................................188 XIV Hemp crop waste for green solutions in construction: physical and mechanical characterization List of Tables 2.1 Percentage of cellulose contained in hemp stalk . . . . . . . . . . . . . . . . . . . . . . . . . . 11 2.2 Propertiesofhempstalk ...................................... 14 2.3 Advantages and disadvantages of bio-binder for stalk [9, 84, 103, 104, 105, 106, 108, 109, 110, 111, 112, 113, 114, 115, 116, 117] . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 20 2.4 Results of acoustic absorption of vegetal particles with different binders . . . . . . . . . . . . 23 2.5 Results of thermal absorption of vegetal particles with different binders . . . . . . . . . . . . 25 2.6 Chemical composition of different plant fibers [16] . . . . . . . . . . . . . . . . . . . . . . . . 27 2.7 Compression young modulus compared with other stalk based materials . . . . . . . . . . . . 27 3.1 Characterization test for low density solution . . . . . . . . . . . . . . . . . . . . . . . . . . . 37 3.2 Sample thickness with different weight . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 43 3.3 Compression, shear and bending test results . . . . . . . . . . . . . . . . . . . . . . . . . . . 58 3.4 Characterization test for medium density solution . . . . . . . . . . . . . . . . . . . . . . . . 61 3.5 Nomenclature structure of the samples . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 63 3.6 Tensile and bending test results . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 68 3.7 Tensile and bending test results with concentrated arabic gum . . . . . . . . . . . . . . . . . 69 3.8 Results of tensile and bending tests varying the manufacturing methods . . . . . . . . . . . . 71 3.9 Results of tensile and bending tests varying the curing times in the mold with absorbent paper 73 3.10 Results of tensile and bending tests for the best cases . . . . . . . . . . . . . . . . . . . . . . 73 3.11Applicationscoretable ....................................... 79 4.1 Characterization test of insulating materials . . . . . . . . . . . . . . . . . . . . . . . . . . . 90 4.2 Durability test of insulating materials . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 91 4.3 Nomenclature structure of the samples . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 92 4.4 Moisturebufferresults ....................................... 97 4.5 Watercontactangleresults ..................................... 101 4.6 Results of acoustic absorption of vegetal particles with different binders. . . . . . . . . . . . . 105 4.7 Results of thermal absorption of vegetal particles with different binders. . . . . . . . . . . . . 108 4.8 Fireresistance ............................................ 111 4.9 Bending Strength of Insulating Panels . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 113 4.10 Compression, shear and bending test results . . . . . . . . . . . . . . . . . . . . . . . . . . . 113 XV LIST OF TABLES LIST OF TABLES 4.11 Mechanical properties of EPS . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . . 114 4.12 Compression young modulus compared with other stalk based materials . . . . . . . . . . . . 116 XVI Hemp crop waste for green solutions in construction: physical and mechanical characterization Chapter 1 Introduction 1.1 The importance of hemp nowadays Hemp (c`annabis sativa L.), a versatile and environmentally friendly plant, has been cultivated for thousands of years, primary for its fibers and seeds. Currently hemp is mainly produced for industrial or food purposes. Hemp is a multi-functional crop with diverse applications across several fields. The cultivation of hemp has played a crucial role throughout human history, providing numerous applications for each part of the plant. Amidst this extensive range of applications, the immense potential lying within hemp stalks has been largely overlooked. At present, hemp stalks are merely considered waste by-products of hemp cultivation. In light of the urgent need to adopt eco-friendly practices and minimize waste, this research will focus on unlocking the hidden value of hemp stalks through reuse and recycling. As the world faces an ever-increasing challenge of waste accumulation, hemp cultivation compounds this issue with its rapid growth and potential for up to four harvests annually, leading to a surplus of hemp stalks. Conventional disposal methods, such as landfills and incineration, only exacerbate pollution, climate change, and the depletion of precious natural resources. As responsible stewards of our planet, this research endeavors to seek alternative solutions, reducing our ecological footprint and embracing sustainable practices to make the most of this valuable resource. Hemp stalks, a material rich in cellulose and lignin, present a unique opportunity for resource utilization. By harnessing this eco-friendly material, we open the door to a diverse array of sustainable products that can effectively replace less environmentally friendly alternatives. This, in turn, fosters a circular economy and significantly reduces our overall environmental impact. The extraordinary properties of hemp stalks make them ideal candidates for recycling initiatives, propelling us towards a greener and more responsible future. 1 1.1. THE IMPORTANCE OF HEMP NOWADAYS CHAPTER 1. INTRODUCTION The key properties of hemp stalks include: •High insulating properties •Low density •Affordability •Recyclable material •Environmentally friendly material During the 21st century, hemp stalks have garnered significant attention within the scientific community, leading to a notable rise in related publications, as depicted in Figure 1.1. This figure demonstrates the growing trend of scientific interest, showcasing the increased number of published articles. Nevertheless, this review extends its scope encompassing articles from various editors and taking into account factors such as the year of publication, methodology, and citation count for each article. Figure 1.1: Number of articles published about hemp and green insulation materials Energy consumption has shown a continuous upward trend, leading to a proportional surge in greenhouse gas emissions. Specifically, in the building sector, a substantial 45% of the total energy usage can be attributed to climate conditioning efforts [3]. Furthermore, in Europe, approximately 36-38% of all CO 2 emissions are associated with the building sector [4]. This trend is exacerbated each year as the changing climate provoke a higher energy consumption to maintain optimal indoor temperatures. Moreover, effective noise management is essential to create comfortable living conditions within buildings. High noise levels in residential environments can have negative effects, such as sleep disturbance and long-term health issues including psychiatric problem, cardiovascular disease and hypertension [5]. Consequently, there is a pressing need for studies aimed at enhancing the energy performance and improve the acoustic comfort of buildings. Additionally, in the coming years, there will be a substantial surge in demand for green buildings, defined as structures designed, constructed, or operated in a manner that minimizes negative environmental impacts while also creating 2 1.1. THE IMPORTANCE OF HEMP NOWADAYS CHAPTER 1. INTRODUCTION positive ones [6]. Through this type of technologies it is possible to reduce the carbon footprint of human activities and to achieve the objectives set in the Paris agreements; to aim a “net-zero” emissions by 2050 [7]. A technique that can be explored in this field of research is the improvement of the performance of insulating materials based in green materials [8, 9] with a positive carbon footprint [10]. A biomaterial or eco-friendly material are materials has been designed, produced, and utilized in a manner that minimizes its negative impact on the environment throughout its entire lifecycle. Eco-friendly materials are characterized by their sustainable sourcing, minimal energy consumption during production, reduced emissions, and biodegradability or recyclability at the end of their useful life. These materials aim to conserve natural resources, mitigate pollution, and promote ecological balance while meeting specific functional or performance requirements. These materials have a reduced carbon footprint compared to traditional materials and reduce the amount of waste generated and decreasing the need for raw materials. The use of eco-friendly materials is an important step towards achieving a more sustainable future. The European Industrial Hemp Association (EIHA) states that the hemp industry is an economically viable and socially responsible enterprise, as it contributes to restoring ecological balance and achieving decarbonization goals for a promising sustainable economy [11]. Considering that it is a plant-based material, this research aims to add value to hemp stalk by incorporating it into construction applications where it can replace synthetic materials. This will help to revalorize hemp cultivation by increasing the value of a part that is currently considered a low value by-product. Consequently, it will reduce the use of synthetic materials that generate CO 2 during their production, and replacing them with a plant-based material. To further enhance the value of green materials, the developed materials are intended to be recyclable. This way, once they reach the end of their useful life, they can be reused as raw materials, contributing to a circular economy that prolongs the lifespan of different materials. The properties of the hemp stalk make it a suitable material to manufacture more sustainable materials for the construction and urban furniture industry. Furthermore, by integrating local communities and industries into this process, we can create new economic opportunities and foster a greener, more resilient future. Furthermore, in the literature, the utilization of hemp or other agricultural waste in combination with plant-based resins for various construction applications has been documented. Remarkably, no studies have been found that confirm the efficacy when paired with recycled cardboard or when employing manufacturing methods that do not necessitate the use of pressure. In conclusion, the proposed study aligns seamlessly with the objectives of waste reduction, recycling, and sustainability. By unlocking the untapped potential of hemp stalks and utilizing their properties to create environmentally friendly green composite materials for construction, a promotion of the circular economy can also be achieved. This approach facilitates significant progress in conserving our planet’s valuable resources and alleviating the strain on the environment. Embracing this innovative endeavor collectively paves the way towards a greener and more responsible future. 3 1.2. OBJECTIVES CHAPTER 1. INTRODUCTION 1.2 Objectives The main goal of this thesis is to produce a new a composite material made form hemp stalk and to the understanding of its various properties according aplicattions in construction and urban furniture. This aims to provide a solution for hemp stalk, a waste material, so that it can replace synthetic materials in specific applications where the full potential of hemp stalk can be utilized, thereby increasing sustainable materials. To achieve this, it is necessary to study the different factors that influence the characteristics of the material. The study focuses on the following specifics objectives: •OBJECTIVE 1. Develop a new green composite material using hemp stalk The primary objective of this research is to explore the potential of hemp stalk as a base material for developing a new green composite material. This involves conducting a thorough study of hemp stalk to understand its properties and characteristics. Additionally, various potential materials will be investigated to identify suitable binding matrices that can effectively combine with hemp stalk to create a stable and durable composite material. •OBJECTIVE 2. Manufacture of the composite material and study of its properties Once the material study is complete, the focus shifts to the manufacturing process of the composite material. Different combinations of hemp stalk and binding matrices will be fabricated, and their properties will be thoroughly analyzed. Mechanical tests, insulation properties analysis, fire behavior studies, and durability assessments will be conducted to characterize the performance of each composite material. In order to select the most suitable combination that exhibits the desired properties for specific applications. •OBJECTIVE 3. Applications of the composite material and solutions for construction This objective centers on studying the potential applications of the newly developed composite material in the field of construction. Different areas within construction will be explored to identify the most promising applications for the green composite material. Furthermore, studies on industrial-scale manufacturing processes will be carried out to assess the feasibility of large-scale production and its integration into construction practices. The overarching goal is to present viable, environmentally conscious remedies for construction through the utilization of green composite materials. To verify the ecological friendliness throughout all stages of the novel material, a comprehensive life cycle analysis will be undertaken. The three objectives are interconnected and not sequential; instead, they complement each other in the research development process. 4 1.3. METHODOLOGY CHAPTER 1. INTRODUCTION 1.3 Methodology This section will explain the methodology followed throughout the thesis, including the path taken and decisions made to achieve the established objectives. Figure 1.2 illustrates the flowchart of the study. 1.3.1 State of the art Initially, the study will focus on conducting an extensive literature review aimed at identifying the key properties of hemp stalk. Furthermore, it will explore various construction industry applications where these characteristics can be effectively utilized, while also assessing the viability of green materials for these purposes. Consequently, different vegetal binders and their potential limitations in each application will also be studied. During this phase of the thesis, five applications have been identified for conducting preliminary studies. 1.3.2 Initial exploration of various material options and the selection of the most promising one This thesis endeavors to unlock the potential of hemp-based materials for sustainable applications within the construction and urban furniture industries. The thesis centers on harnessing the distinctive qualities of hemp to create eco-friendly materials and explores five distinct applications. The primary step is to initiate a preliminary investigation to validate material properties and evaluate its feasibility in each application. This includes compatibility tests with chosen binders and fabrication methods. Following the identification of suitable green binders and fabrication techniques in alignment with the specific prerequisites outlined in the literature, a comprehensive material characterization is conducted to determine the key properties for each application. In this characterization phase, the applications are categorized based on the chosen binder and fabrication method. The initial stage involves the selection of a mixing rule to evaluate the bonding potential between hemp stalk and the green binder, a combination that has received limited study thus far. The study includes the creation of initial material samples, followed by manual agitation to assess their adhesion and stability. By progressively increasing the hemp stalk content in each sample, we can ascertain the maximum bonding capacity. Once this maximum bonding capacity is determined, test specimens are prepared for characterization tests, with a focus on identifying the most promising scenarios for the key properties relevant to each application. To maintain a manageable scope, a decision-making process based on the characterization results is conducted based on the comparison with commercial materials, leading to the selection of one application for an in-depth study. If other promising materials are identified, future studies for those applications will be proposed. 5 1.3. METHODOLOGY CHAPTER 1. INTRODUCTION 1.3.3 Characterization and durability test of the selected material Once the application is selected, a property enhancement process is undertaken, incorporating both mechanical and chemical methods. This optimization process involves conducting several tests to validate the results and determine the material’s characteristics. Additionally, a long-term study of the material properties is conducted. After the initial investigations, commercial-sized demonstrators will be manufactured to explore the feasibility of large-scale industrial production. An experimental investigation will then be undertaken to further optimize the material’s properties, including applying a vegetable coating and enhancing cellulose crosslinking. This comprehensive study will involve various tests, including microscopy, FTIR-ATR analysis, and assessments of mechanical strength (compression, shear, and bending), fire resistance, moisture resistance, and water resistance. The specific characterization tests will depend on the selected application. To ensure the long-term viability of the organic materials used, a durability test will be conducted to verify the material’s performance over time. This step is essential to assess the material’s stability and reliability throughout its lifespan. By addressing these aspects comprehensively, this thesis seeks to contribute valuable insights into the potential of hemp-based materials. The material will be subjected to environmental cycles in a laboratory environment with precise monitoring of temperature and humidity conditions. This approach entails conducting periodic characterization tests to evaluate any possible degradation in the material’s properties over time. Throughout this thesis, durability cycles spanning 0-3-6-9 months have been conducted. Morever, the durability process will be extended to 12 and 17 months outside the thesis to corroborate the data. 1.3.4 Life cycle In the preceding stages of the thesis, eco-friendly materials are employed to create a sustainable product. The purpose of conducting a life cycle analysis is to substantiate the eco-friendly attributes proposed in the thesis across all phases of the material’s lifespan, confirming a reduced carbon footprint and more efficient utilization of resources through recycling. The stages considered in this study encompass: •Material and component acquisition •Factory production •Distribution and sale •Usage •Final disposal/Recycling 6 2.2. APPLICATIONS FOR LOW DENSITY SOLUTIONS CHAPTER 2. STATE OF THE ART Figure 2.4: Rockwool (left) [46] & EPS (right) [47] Both of these materials exhibit lightweight characteristics along with a notable level of porosity. As part of the characterization process for the new green material, a comparative analysis will be conducted to assess its properties in relation to the aforementioned materials. The objective is to ensure that the new material is competitive and meets the requirements outlined by current regulations. The different regulatory aspects to be considered for the characterization of the material are as follows: •Thermal resistance: UNE EN-12664 [48] •Acoustic resistance: ISO 10534 [49] •Compression resistance: UNE EN-826 [50] •Shear resistance: ISO 12236:2006 [51] •Bending strength: UNE EN 12089 [52] •Determination of short and long-term water absorption: ISO 29767:2019 [53] •Fire resistance: UNE EN 13501 [54] In addition to comparing the results with reference commercial materials, other regulatory aspects must be taken into account. In Europe in order to consider a material as thermal insulation, the thermal conductivity coefficient must be lower than 0.1 W/m K [55]. 2.2.2 Insulating properties of hemp stalk One of the most attractive properties of hemp are its insulating properties [56]. Moreover, in a comparison with conventional materials, natural fibers have similar hygrothermal properties and the process of retrofitting historical building envelopes is made more harmonious by their involvement [57]. 13 2.3. APPLICATIONS FOR MEDIUM DENSITY SOLUTIONS CHAPTER 2. STATE OF THE ART Table 2.2: Properties of hemp stalk Thermal conductivity (W/m K) Acoustic absorption (α) Density ρshives ( kg/m3 ) Porosity ϕinter(%) Reference 0.049-0.082 0.88-0.95 110-125 40 [33] - 0.7-0.95 80-160 65-85 [58, 59] 0.064-0.115 0.88-0.99 97-120 - [60] 0.051 - 72 70-80 [61] According to the hemp stalk insulating properties, Table 2.2. Hemp stalk is a green material that can be use in insulating applications, even though its properties are less competitive than commercial materials. The thermal conductivity of rockwool is 0.036-0.037 (W/m k) (28%, better performance than hemp stalk) [62, 63] and EPS have 0.038 [63] (28%, better performance than hemp stalk). The acoustic absorption ( α ) of rockwool is 0.98-0.99 dB/dB [64, 65] (0.1 dB/dB, better performance than hemp stalk) and EPS 0.8-0.9 dB/dB [66] (same performance of hemp stalk). The properties shown by the stalk are suitable for use as both thermal and acoustic insulating material, however it is a particle material, so it is necessary to use a green binder to manufacture a lightweight green composite material. In this insulating application, the mechanical resistance of the material is not a critical value, it is only necessary that it satisfy the minimum requirements and to be a stable material. Hemp possesses exceptional insulating qualities, which are retained in the stalk. However, it is crucial to ensure its long-term stability as well as its chemical compatibility with the binders [67]. Since hemp is a particulate material, the sample’s morphology and the internal porosity of the material is the critical factor that determines its performance [68]. 2.3 Applications for medium density solutions This section will proceed to conduct a comparable analysis for chipboard, coffer ceiling and parquet. The three applications will be categorized together based on the similarities in their manufacturing processes that result in medium-density green composite materials. 2.3.1 Commercial material Particleboard The particleboard, as shown in Figure 2.5, is a type of board manufactured using small wood chips. These chips are dried, mixed with resin glues, and then subjected to high-pressure pressing. 14 2.3. APPLICATIONS FOR MEDIUM DENSITY SOLUTIONS CHAPTER 2. STATE OF THE ART Figure 2.5: Particleboard [69] There are various types of commercial particleboards available, each with modifications in particle size, particle orientation, and the type of synthetic resins used as binders. The most frequently utilized resins in the industry are: •Melamine resins •Phenol-Formaldehyde (PF) •Urea Formaldehyde-Melamine (MUF) •Polymeric Diphenylmethane Diisocyanate (PMDI) •Binary mixture of the above Using binder proportions between 5% and 10% by weight, the manufacturing process involves applying a pressure of 8-13 MPa and curing the resin at the specified temperature for no more than 5 minutes [70]. For this case, a commercial particleboard will be used as a reference for comparing its properties with those obtained using green-based resins. Additionally, test specimens with non-green-based resins will also be fabricated to compare the manufacturing process conducted in the laboratory. The characteristic properties taken as reference correspond to a P2-type particleboard (for indoor applications, including urban furniture, in dry environments) with the same thickness as the test specimens. In the existing literature, no research has been discovered that achieves a P2 performance using 100% green materials. The different normative aspects that will be considered to characterize the P2-type particleboard are as follows: •Tensile strength, UNE EN 319 [71] (0.4 N/mm2for commercial particleboard [72]) •Bending strength, UNE EN 310 [73] (11 N/mm2for commercial particleboard [72]) •Bending young modulus, UNE EN 310 [73] (1800 N/mm2for commercial particleboard [72]) •Industrial requirements for particleboards, EN 622 [74] 15 2.3. APPLICATIONS FOR MEDIUM DENSITY SOLUTIONS CHAPTER 2. STATE OF THE ART Coffered ceiling The coffered ceiling, shown in Figure 2.6, serves as elements used in formwork to reduce the weight of constructions. Figure 2.6: Coffered ceiling [75] The purpose of this application is to replace non-reusable expanded polystyrene (EPS) coffers, which are commonly used to reduce the weight of constructions at a lower cost, but these coffers remain embedded in the structure and cannot be reused. In this context, a primary limitation of green materials, as indicated by the literature, is the challenge of maintaining the stability of the hemp stalk and plant-based resin mixture under alkaline and highly humid conditions that occur during the concrete curing process. Furthermore, the material must exhibit adequate mechanical strength to endure the weight of the concrete during this curing phase. To meet the construction standards for coffers and vaults, the material must exhibit a bending strength greater than 150 kPa and achieve a fire reaction rating of at least class E, which indicates the ability to withstand the attack of a small flame for a brief period without significant propagation of the flame [76]. Moreover, as a novel green material, it is crucial to ensure its stability under the specified environmental conditions. The following properties will be tested for this application: •Bending strength, UNE EN 12089 [52] •Fire reaction, UNE EN 13501 [54] •Static puncture test (CBR test), UNE EN 53974 [77] In this application, the focus will be on utilizing plant-based resins, and their performance in the alkaline environment will be thoroughly evaluated. To ensure the material’s durability and long-term functionality, a coating will be considered, if needed, to shield the composite from the impact of environmental conditions. 16 2.3. APPLICATIONS FOR MEDIUM DENSITY SOLUTIONS CHAPTER 2. STATE OF THE ART Parquet flooring The parquet flooring, shown in Figure 2.7, consists of thin wooden pieces mechanically joined together to create a decorative pattern. To enhance its durability and scratch resistance, a protective surface layer is applied. The primary material used can be either natural wood or synthetic materials such as vinyl (PVC). Figure 2.7: Parquet flooring [78] This type of material involves using hemp stalk and plant-based resin for the interior part, providing the required mechanical strength, and combining it with a PVC coating to offer surface qualities, a visual pattern for the flooring, and interlocking between different strips. In this approach, the compression and indentation resistance of the hemp-based material will be taken into account. The different normative aspects that will be considered to characterize the material are as follows: •Industrial requirements, EN 13489 [79] •Hardness requirements, EN 1534 [80] The patent by FLOORING TECHNOLOGIES LTD [81] showcases their manufacturing process, which includes applying pressure between 3 and 6 MPa and a temperature of 165°C for a brief duration, similar to the process used for particleboards. According to this material specification, the resin and binder mixture must meet the hardness requirements, assessing the material’s deformation when subjected to a constant load for a specific time frame. Furthermore, the final material must comply with all regulatory standards, ensuring there will be no slippage between the two layers of the material. 2.3.2 Mechanical properties of hemp stalk The elastic modulus of the hemp stalk (10-16 GPa) depends on its position in the stem of the plant according to the height at which it is located [82, 83]. However, the area where the elastic modulus is greater is different 17 2.4. GREEN BINDER MATERIALS CHAPTER 2. STATE OF THE ART among the species of hemp. The differences between the elastic modulus correspond to an increase or decrease in the size of the cell wall along the stem [82]. In these particular applications, the mechanical strength offered by plant-based resins might not meet the current regulations. Previous studies on materials incorporating hemp stalk with plant-based binders have demonstrated a maximum bending strength of 7 MPa using starch as a binder [84]. Consequently, the option of utilizing non-plant-based materials (up to 10%) is put forth, should the need arise. Furthermore, investigating structural strategies to augment the material’s characteristics, like the creation of a sandwich-type composite, could be contemplated as an alternate avenue. Additionally, in the context of these three applications, the material must endure direct exposure to water, fire, or alkaline environments. Therefore, the application of an inorganic protective coating might be essential when employing hemp stalk for the proposed uses. 2.4 Green binder materials The literature study in this section aims to explore various green materials that can serve as binders for the development of a green composite material based on hemp stalk. Recent publications have suggested that lignin-based resin, bio-epoxy resin [9], and recyclable cardboard fiber [2] hold promise as potential binding materials for creating a novel bio-composite material using hemp stalk. This study focuses on green materials, however there are not many studies with a 100% green material, so some results of non-green binder will be presented to study the behavior of the material and find out which green materials could obtain the best performance. Different applications are being studied to use hemp stalk, taking advantage of its low price, such as using it as insulation in buildings, adding lime to form non-structural blocks [85, 86]. A sustainable substitute for traditional walls, carried out a study of the acoustic absorption properties of lime and hemp stalk walls, obtaining an average of between 40-50% of acoustic absorption, obtaining better results with the less hydric binders, it can be manufactured on-site or placed prefabricated [87]. The main advantages of hempcrete is the insulating properties provide by the hemp stalk, and the lime binder provides a protection against moisture, fungi and fire [88]. In the same approach, adding hemp particles to the mortar as aggregates to reduce its density, increase the insulating properties and also the material will increase the capability of CO 2 storage, nevertheless, the mechanical properties decrease (maximum stress is reduced up to 30% when adding 8% hemp) [89, 90, 91]. Although cementitious matrices offer the benefits of affordability and adaptability, their use can result in chemical damage to hemp stalk [92]. In hot-dry regions where naturally ventilated buildings are preferred, the thermal design of walls based on compressed earth blocks (CEB) could be a viable and more ecological option [93]. Moreover, the thermal behavior of CEB was improved by 10% by incorporating a 0.5% of date palm waste [94]. While compacted earth is a compelling environmentally-friendly material, it 18 2.4. GREEN BINDER MATERIALS CHAPTER 2. STATE OF THE ART is crucial to thoroughly examine its dependability and longevity in the absence of long fibers [95]. Hemp stalk particles, its also use as a raw material for materials that are made up of wood particles. In this way, a manufacture process is to mix it with a binder to fabricate a material similar to a chipboard. The manufacture of this type of material consists of mixing the stalk with the binder material and applying pressure and temperature in a mold, the adhesive cures and the material obtains the shape of the mold. The most commonly used binders are currently based on formaldehyde because of its mechanical properties, dynamic properties, abrasion resistance and affordability [96]. Nevertheless, due to the fact that it is a toxic material in large quantities, its use has been decreasing in order to reduce the formaldehyde. An intermediate solution is the use of 2 formaldehyde-based adhesives by partially substituting them for lignocellulose-based materials (wheat straw and pine and poplar particles) obtaining better results with PDMI (Polymeric Diphenylmethane Diisocyanate), by increasing the percentage of binding material [97, 98]. PDMI shows better binding properties than UF (Urea formaldehyde), curing at a temperature of 180°C and applying pressure for 3 minutes [99], these are the usual values in the industry. The process is also the same with vegetable agglomerate taking into account the curing temperature for each vegetable binder [100, 101]. In this type of manufacturing, the structure and size of the particles is also an important factor in the final properties of the material. If the particle size is very large, air gaps will be produced in the material as all the chips cannot be compacted together because the manufacture process do not use vacuum to prevent the air gaps. However, it can be solved by including saws and wood dust that occupy these holes together with the resin, thus increasing the mechanical properties of the material [102]. Another alternative is to completely eliminate formaldehyde-based resins by using natural ones. Although studies are being carried out to obtain vegetable resins that can achieve the regulatory requirements of the different applications, such as lignin-based wood adhesives [103, 104], obtaining a materials with great thermal properties, or vegetable proteins such as camellia protein, which is also a residue in the biodiesel production [105]. However, the main problem is the resistance to fire, that problem can be solved adding a fire resistance coating. There is also studies to develop a sustainable, high-performance, and flame-retardant wood coating based in a curing agent of ammonium hydrogen phytate (AHP) [106, 107]. Starch is also a good biobased binder for wood particles, for example, cassava starch binder can be use to elaborate a low density particleboard wit and excellent performance [108]. The fungi resistance is low, however it can be added citric acid to improve the fungal degradation in a 10% [109]. Different innovative renewable binders materials for thermal insulating application are studied. However, the technology still needs more research to have a competitive price and solve different technical difficulties to use materials like vacuum insulating panels, aerogels or nanocellulose. The researcher also proposes the use of recycled paper fiber as insulating material based on cellulose [110]. To bind the different hemp particles in a material that can be lightweight, a manufacture method is needed that does not require applying high pressure to provide the maximum porosity in the material, paper pulp fiber is proposed, witch also have a 19 2.4. GREEN BINDER MATERIALS CHAPTER 2. STATE OF THE ART great thermal properties, cellulose paper waste have a thermal conductivity value of 0.046–0.054 W/m K [111]. Among the different paper fiber, cardboard is a great option due to the facility for recycling and the mechanical/binding properties. Cardboard fibers have a mechanical resistance 4 times greater than eucalyptus fibers (one of the most commonly used paper pulp fibers), measured from the binding [112, 113]. Moreover, the length of the fiber is longer (cardboard 2.7 mm in average length and eucalyptus 0.76 mm [114]). Several layers of corrugated cardboard were texted obtaining thermal conductivity values of 0.053 W/m K and a reduction of up to 80 dB in acoustic waves using several layers of corrugated cardboard [9]. In that case, the main problems are the durability and moisture/fungi/fire resistance. Table 2.3: Advantages and disadvantages of bio-binder for stalk [9, 84, 103, 104, 105, 106, 108, 109, 110, 111, 112, 113, 114, 115, 116, 117] Type of Biobinder Advantages Disadvantages Recycle the secondary products produced in paper pulping industries Need to add a catalyst material Improve the modulus of elasticity Increase the viscosity of adhesive Lignin based Improve the thermal properties Low fire resistance Improve the water resistance Reduce the curing rate Good bonding strength Low porous structure Low level of substitution Low stability upon time Low fungal resistance Good film formation property Low fire resistance Starch based High level of substitution Slow drying process Good bonding strength Poor water resistance Need a surface treatment to increase the water resistance Improve thermal stability Poor water resistance Plant protein based Good adhesion strength Need a surface treatment to increase the water resistance High level of substitution Low porous structure Low fire resistance Recyclable Poor fire resistance Good bonding strength Slow drying process Paper pulp based Improve thermal/acoustic properties Need a surface treatment to increase the water resistance High porous structure Low stability upon time High level of substitution Low fungal resistance 20 2.4. GREEN BINDER MATERIALS CHAPTER 2. STATE OF THE ART Table 2.3 summarizes the comparison of performance, advantages, and disadvantages of bio-based wood adhesives for stalk. Regardless of the type of bio-based adhesive used, it is crucial to assess their potential for wood composite application and comprehend their interaction with wood. This evaluation can provide valuable scientific insights to guide the development of adhesives in terms of mechanical strength, water and moisture resistance, and thermal and acoustic properties. 2.4.1 Green binder for low density material In this section, an analysis of the insulation parameters of composite materials will be conducted to enhance understanding of crucial characteristics for the mixture of hemp stalk and the green binder. Furthermore, the insulation properties of green materials with different binders will be presented and compared to assess their compatibility with binder characteristics. This evaluation aims to identify the most suitable binder for the applications studied in the thesis, with a specific focus on hemp stalk. Acoustic insulation properties When a surface is contacted by sound waves, the energy is distributed into three categories: incident, reflected and absorbed energy. In architectural acoustics design, it’s helpful to utilize an average absorption coefficient that is assumed to rely solely on the physical attributes of the material. The sound absorption coefficient of any material is determined by the angle at which the sound wave hits the material and the frequency of the sound [118]. In the case of acoustic properties, the parameters of the hemp particles that influence the acoustic properties are the density of the particles, the bulk density, the thickness of the particles and the shape factor [58]; this relationship is also shown in others biomaterials. On the other hand, the results also show that for low-frequency waves, acoustic insulation is not very effective due to the porosity of the material. Reducing the particle size and density of the stalk leads to enhanced acoustic properties, with optimal conditions achieved at a particle length of 6 mm and a density of 0.3 g/cm3 . This configuration significantly improves the acoustic absorption capabilities of the stalk material, Figure 2.8. Furthermore, the internal porosity can be predicted from the density of the particles [58, 59]. At a microscopic level, hemp has a structure that bring on the absorption of acoustic waves due to the voids provided by the porosity of the material [41]. Hemp has a porosity of 78% with pores between 0.9-3 µm [33, 119]. No studies have been found that prove whether the differences in cell size along the stem affect the insulating properties, detecting a research gap that could be interesting future research to increase hemp performance as raw material for insulating applications. 21 2.4. GREEN BINDER MATERIALS CHAPTER 2. STATE OF THE ART Figure 2.8: Acoustic absorption as a function of particle size, size 1 > size 2 > size 3 (left) [58] and the relationship between density and porosity of hemp stalk (right) [59] In the case of a composite material based in hemp stalk. The mechanism by which the materials absorb sound energy mainly involves 3 physical processes. Sound-absorbing composite materials have small holes that allow sound waves to access to their interior, causing gas flow and friction. It triggers the conversion of a portion of the sound energy into heat energy, which leads to sound absorption. In the case of hemp stalks, when sound waves hit them, the viscous effects between air cavities attenuate some of the sound energy, converting it into heat. Moreover, the sound-absorbing composite materials have the ability to absorb certain sound waves through their own vibrations. Due to the force between chain segments, unique hollow structure, and large specific surface of hemp stalks, sound energy is attenuated and converted into heat and mechanical energy during propagation, resulting in an effective sound-absorbing effect [41, 120, 121]. The internal porosity of the composite is a crucial factor to consider in the sound absorption mechanism of a low-density insulation panel. The presence of voids, inner and outer spaces, as well as the density and thickness of the composites directly influence sound absorption [122, 123]. Low-density materials with more open structures exhibit lower absorption at low frequencies, while denser structures show better performance at higher frequencies (above 2000 Hz) [118]. Several studies investigating sound absorption in porous materials have found a direct relationship between thickness and low frequency sound absorption. Increasing the thickness of the material leads to an increase in sound absorption at low frequencies. However, at higher frequencies, thickness has an insignificant effect on sound absorption [124]. Nevertheless, a sandwich-type material can increase acoustic absorption in low frequencies. The low porosity and high density of the material’s surface cause sound waves to be reflected [68]. 22 2.5. LIFE CYCLE CHAPTER 2. STATE OF THE ART boundary conditions, initial imperfection of the material and the crosssection material relation. 2.5 Life cycle The purpose of conducting a life cycle analysis is to substantiate the eco-friendly attributes proposed in the thesis across all phases of the material’s lifespan, confirming a reduced carbon footprint and more efficient utilization of resources through recycling. The stages considered in this study encompass: •Material and component acquisition •Factory production •Distribution and sale •Usage •Final disposal/Recycling The subsequent guidelines prescribe how to conduct a life cycle analysis of materials: • Environmental management - Life cycle assessment - Principles and framework: ISO 14040:2006 [149] • Environmental management - Life cycle assessment - Requirements and guidelines Amendment 2: ISO 14044:2006 [150] For the proposed material, the emphasis will lie on utilizing secondary materials with a minimal carbon footprint. The aim is to guarantee that the material’s carbon footprint contributes to a reduction in emissions generated during all the life phase. Furthermore, it is essential that the material is recyclable and does not generate harmful chemical byproducts that could adversely affect the environment. To conduct a life cycle analysis, properties such as carbon storage and the durability of green materials will be reviewed. 2.5.1 Carbon storage properties of hemp stalk Developing a biomaterial based on hemp stalk can increase the value of the hemp crop, produce more environmentally friendly materials, and also result in materials that act as CO2accumulators [6]. The hemp absorbs CO 2 meanwhile it is growing by the photosynthesis process. Moreover, due to very rapid growing, the biomass accumulated by hemp crop has significant effect in absorbing atmospheric CO 2 , however some of the carbon stored in this biomass is turned back to atmosphere as CO 2 due to biodegradation of leaves and roots. Assuming a concentration of 0.5 kg of carbon per kg of dry matter, it can be calculated that 1.84 kg of CO 2 are sequestered per kg of dry hemp through photosynthesis during the plant’s growth. 29 2.5. LIFE CYCLE CHAPTER 2. STATE OF THE ART This means that a ton of dry hemp can store 325 kg of CO 2 , taking into account the amount of emissions during the farming as the diesel consumption, transportation of the seeds, etc [151]. An example of a CO 2 accumulator is hempcrete, a sustainable building material made from hemp stalks, lime, and water. Lime in the material also contributes to CO 2 sequestration due to the carbonation process, but the overall process has a positive carbon footprint due to the CO 2 released during the lime manufacturing process. During the carbonation process, the lime reacts with the CO 2 present in the air, resulting in the conversion of calcium hydroxide (Ca(OH) 2 ) into calcium carbonate (CaCO 3 ) [152]. The carbonation increases the mechanical resistance of the hempcrete and, additionally, the absorption of CO 2 during this process can have significant implications for the environmental impact of this product [153]. Hempcrete can store 300 kg of CO 2 per m 3 [154, 155, 156]. With these two properties hempcrete reduce the energy consumption on the building due to the thermal insulation capacities and also store CO 2 , obtaining a material that would passively help to obtain buildings with zero emissions [157]. However, the carbonation process is notably slow, and the amount of CO 2 absorbed is lower than what is generated during the material acquisition phase. As a result, the overall carbon footprint is not deemed sufficient. Inferences can be drawn from the provided examples that underscore the considerable influence of the binder choice on the composite material’s carbon footprint. The suggestion involves the utilization of recyclable materials with minimal carbon footprint impact for the binder material. 2.5.2 Durability of the selected green materials In order to develop a new biocomposite insulating materials it is necessary to ensure the durability conditions to ensure the commercial product can be reached. However, there are only a few papers that study the durability for long term test in those materials. The longevity of bio-composites can be impacted by various forms of biological degradation, such as mold growth, as well as environmental factors like fluctuations in temperature and humidity [131]. Investigating the water absorption characteristics of biocomposites is crucial, given the weak water resistance of biomaterial. For biocomposites used outdoors in construction applications, their water absorbency is a critical factor affecting their insulating, mechanical properties and dimensional stability [143, 158]. Hemp fibers also present a low stability against the contact with water, which see their Young’s modulus reduced by 50% after immersion in water [159]. Moreover, using a 100% vegetable material increase the risk to the mold growing in high humidity conditions [142]. Mold growth can be relieve by increasing the pH of the material, as is the case with hempcrete, which has an antifungal properties [88]. In the case of VFRCM (vegetal fabric reinforced cementitious matrix), the issue arises from the alkaline hydrolysis resulting from the production of Ca(OH) 2 during cement hydration. The calcium adsorption is pH dependant, the pectin contained in fibres can react with calcium ions in an alkaline environment [160]. Moreover, a reduction in compressive strength has been observed in hempcrete when using Ca(OH) 2 treated 30 2.5. LIFE CYCLE CHAPTER 2. STATE OF THE ART hemp stalks compared to untreated ones [161, 162]. To incorporate a material that is rich in Al 2 O 3 and SiO 2 can mitigate the degradation of the hemp fibers. This material should have the ability to consume Ca(OH) 2 during mortar hydration [163]. Alternatively, the fiber can undergo physical or chemical treatment. To extend these findings to vegetable binders, it is crucial to ensure compatibility between the hemp stalk and the vegetal binder to achieve optimal results. To prevent the degradation of the biomaterials, a solution is to introduce a coating in order to protect the material against the environmental effects. To increase the water resistance of these materials, surface coatings such as NaOH, silane and epoxy have been studied, which reduce the moisture absorption of the fibers [164, 165, 166, 167]. A treatment of colophony is apply to bamboo particle in order to obtain a hydrophobic material. After the coating, bamboo particles become a stable material against the environment [144]. The diterpenoid structure equips rosin with excellent hydrophobicity. Over the recent years, rosin and its derivatives have been used to modify wood materials, wood-based panels, packaging, and nanocomposites increasin the water resistance and the mechanical strenght [168, 169]. Nevertheless, the colophony worsen the fire resistance properties. Arabic gum also presents good results as a coating in cases of humidity and fire, although it could not be used in direct contact with water, since arabic gum is soluble in water, so when the layer is in direct contact protective coating is removed until the material is uncoated [145]. Although these coatings increase the durability of the material, no studies have been found that investigate how the insulating properties behave when these coatings are added. The coating would not only have the function of protecting the material, but also of stabilizing the interior moisture. Since the moisture has a great impact on the insulating properties, as seen in the previous sections. 31 2.6. CONCLUSIONS CHAPTER 2. STATE OF THE ART 2.6 Conclusions According on the results presented in the different studies of the last decades, hemp is positioned as a green material with great insulating properties that could replace some inorganic commercial materials, to improve the insulating performance of building and produce non-structural materials to build green building. These data can be corroborate by the increase in interest in the scientific community, with an increase in research each year, and also with the increase in the hemp industry in the business sector. • Varieties and positions on the stem can cause differences in the elastic modulus of the hemp stalk of up to 60%. However, no studies have been found to confirm whether these differences in cell size impact the insulating properties of hemp. This research gap presents an interesting opportunity for future studies to explore ways to enhance the performance of hemp as a raw material for insulating applications. With the farming of the different varieties of hemp, it is necessary to study which variety produces the hemp stalk with the best insulating properties and in which part of the stem is localized. • It is suggested to use a binder that aids in creating a low-density and porous material as the microstructure of the composite material plays a significant role in determining its insulating properties. It is still necessary to delve into some issues in order to develop new green insulating materials, such as the study of more green binders that do not need to apply pressure or temperature during manufacturing process. In this way, the manufacturing cost is reduced, and lightweight materials with high porosity would be produced that would stimulate the insulating properties of the composite material. In this way, paper pulp based binder shows great opportunities for the development of future research. Interestingly, although cardboard fiber exhibits favorable insulation characteristics, no studies investigating its combination with hemp shiv have been found. • Despite all the studies, further research is still needed on the use of a 100% plant-based composite material, including the binder. However, among those presented, starch stands out. By using starch as a binder, an acoustic absorption ( α ) of 0.7 and a thermal conductivity of 0.03 W/m K have been achieved, which are respectively 0.2db/db lower and 15% higher than conventional materials. • The studies reviewed have indicated that the mechanical properties of a fully plant-based material might fall short of meeting the criteria for utilization in the suggested non-structural applications. To enhance the material’s mechanical performance, a proposal is put forth to incorporate an inorganic skin that would additionally serve to safeguard against degradation due to environmental conditions. Another approach involves utilizing a resin containing a proportion of green materials to enhance mechanical performance, offering a cleaner alternative than commercial materials, even though it may not constitute a completely 100% environmentally friendly solution. 32 2.6. CONCLUSIONS CHAPTER 2. STATE OF THE ART • It has been observed that only a few studies have investigated the acoustic properties, fire resistance, fungi growing and long-term durability of 100% green composite materials. •A ton of dry hemp can store 325 kg of CO2. Hemp is exhibit as a material capable of storing CO 2 , and to produce a renewable material with circular economy. The binder also affect to the carbon footprint of the composite material. To prioritize the carbon footprint, a recycled biomaterial such as cardboard fiber can be chosen as a binder. •It is necessary to protect the biomaterial against the ambient condition. The main problem for a biocomposite material is the degradation over time. So in order to produce a commercial product it will be necessary to ensure the stability of the material in ambient conditions. Nevertheless, no research has been found that investigates the influence of using an eco-friendly coating on the insulation properties of a composite material To protect the biocomposite material against ambient degradation some vegetable coating such as colophony shows a great performance. Arabic gum is proposed as an effective solution for fire protection, but it only provides protection against moisture and not direct contact with water. In this thesis study, a large amount of research related to the development of new hemp stalk-based composite materials has been compiled, a lot of research has been done and it is arousing increasing interest in the scientific community for its performance and sustainability reasons. Therefore, it is recommended that these issues continue to be investigated in order to develop a new competitive material capable of replacing current inorganic materials. It is proposed the use of hemp stalk as a primary material for a sustainable insulation product using a 100% green material to develop it. While previous studies have explored insulating materials based on hemp stalk and vegetal binders, there is still a need for further research to enhance their insulating properties and evaluate their resistance to moisture and fire. Interestingly, although cardboard fiber exhibits favorable insulation characteristics, no studies investigating its combination with hempstalk have been found. It is possible that the compatibility between these two materials may not be optimal, despite their similar compositions. Hence, this study proposes the investigation of a potential cross-linking agent, such as citric acid, which has not been previously explored in relation to its effect on hemp stalk. While this new bio-composite material based on hemp stalk and eco-friendly binding materials shows promise as a replacement for traditional inorganic insulating materials in building construction, further research is needed to improve its long-term stability. It is important to ensure that the material maintains its structural integrity and insulating properties over time to ensure its effectiveness and durability in real-world applications. Continued investigation and development of this material will be crucial to its success as a sustainable building material. 33 2.6. CONCLUSIONS CHAPTER 2. STATE OF THE ART The main characteristics of hemp stalk that make it suitable for various applications are its insulating properties and low density, which can be advantageous in non-structural construction applications and urban furniture. To obtain stable materials from hemp stalk particles, it is necessary to add a second material that acts as a binder for the particles. There are numerous plant-based materials that can fulfill this function. However, they generally have certain disadvantages compared to synthetic materials, such as higher raw material costs and lower mechanical properties. Despite these drawbacks, different materials can be selected depending on the application, where high mechanical properties are not required, thus compensating for the extra cost by using more environmentally friendly materials. Examples include plant-based resins and binders, as well as recycled waste materials such as recycled paper fibers. 34 Hemp crop waste for green solutions in construction: physical and mechanical characterization Chapter 3 Exploring applications: material composition and manufacturing process In this chapter, the preliminary studies conducted are presented. These studies encompass the exploration of compatibility between different plant-based binders and hemp stalk, the formulation of material mixing rules, and the thorough characterization of their properties. This constitutes a research study on the material and evaluates the viability of various applications. Based on these studies, the most promising application is chosen as the primary focus of the thesis. Considering that this is a characterization phase, it will not be necessary to obtain all properties of the material, but rather the most characteristic ones, in order to observe the most promising manufacturing methods and applications. Compatibility tests between hemp stalk and different selected binders will be carried out, along with initial characterization tests to choose the best binders and their proportions. The manufacturing process will also be adapted for each selected application. Based on the literature, five applications have been selected: thermal insulation material, acoustic insulation material, coffered ceiling, particleboard, and parquet flooring. The study will be divided into 2 blocks due to the similarities in specimen fabrication, potential binder materials, and necessary tests. The two blocks are as follows: •Low density solution: Thermal Insulation Material & Acoustic Insulation Material •Medium density solution: Coffered ceiling, Particleboard & Parquet Flooring 35 3.1. LOW DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS 3.1 Characterization of low density solution In the application of the insulating material, following the recommendations from the literature, a binder with high insulating properties and a manufacturing method that promotes a highly porous microstructure will be used. This approach will enhance both acoustic and thermal insulation properties. However, these a low density with high porosity material also result in lower mechanical properties of the material. Given these considerations, the selected binder material is paper fiber, and the manufacturing method involves mixing the components in water, using the interlacing of fibers to achieve cohesion during the material’s drying process. 3.1.1 Materials Hemp stalk The hemp stalk used in this research was provided by Planteles Lloveras, a harvesting company. The moisture content of the hemp stalk used in ambient conditions is 9-13% with a particle leng among 5-20 mm, Figure 3.1. For additional details regarding the properties of hemp stalk, refer to section 2.2.2 & 2.3.2. Eucalyptus pulp The paper pulp used is a ECF (elementary chlorine free) bleached eucalyptus kraft pulp, which was supplied by the company ENCE, Figure 3.4. Since hemp stalk and eucaliptus pulp are of plant origin and possess similar compositions, the cellulose bonds are more likely to form, thereby facilitating the connection between the two components and resulting in the creation of the new biomaterial. Initially, the use of commercial paper fiber was chosen to confirm the effectiveness of the bond formed by the paper fibers and assess their properties. This approach involved using a controlled commercial material before proceeding with the experimentation using recycled fiber (newspaper, cardboard, etc ), which can introduce greater variability and dispersion in the results obtained. 3.1.2 Characterization test In this section, the tests that will be used to characterize the material and verify its feasibility for use in the application as an insulating material will be defined. The tests conducted encompassed an examination of the material’s compatibility, acoustic and thermal insulation properties, as well as its mechanical response under compression, shear and tension, Table 3.1, where %wt means the composition of every material in weight . The raw result of the different test carried out in the thesis are provided in the Appendix A section. 36 3.1. LOW DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS Table 3.1: Characterization test for low density solution Test Variable Number of samples Compatibility with paper fiber %wt. of materials: 9 18 Moisture of hemp stalk: 2 Thermal resistance - ISO 12664 %wt. of materials: 2 8 Acoustic resistance - ISO 10534 %wt. of materials: 2 8 Compression resistance - EN 826 %wt. of materials: 2 6 Shear resistance - EN 12236 %wt. of materials: 2 6 Tensile resistance - ISO 1607 %wt. of materials: 1 6 Fabrication pressure: 1 3.1.3 Compatibility of the materials Methodology The initial step involves assessing the compatibility and feasibility of manufacturing using the proposed materials. To achieve this, small samples with varying composition percentages will be fabricated, and their stability will be carefully observed. The outcomes will be visually assessed using the fabricated specimens by manipulating them to confirm the material’s stability and absence of drooping. The objective is to identify any differences among the materials’ compositions. In Appendix A.1, the conducted tests are described in detail. Results To study the compatibility of hemp stalk (Figure 3.1 ) with fibers, different specimens were prepared to assess the material’s stability. Subsequently, mechanical strength, thermal insulation, and acoustic isolation tests will be conducted. The bonding method employs water to facilitate polymer bonding, specifically through the crosslinking of cellulose, between the two materials. In this process, both materials are mixed in water and then dried to achieve the union. Before initiating the manufacture of the test samples, an initial evaluation of the raw hemp stalk material to be employed was carried out. Initially, an inspection unveiled that the dried straw comprised a blend of diverse particle and fiber dimensions, Figure 3.2. Consequently, it was determined to submerge the material in water for several days to observe its interaction with water, considering its intended mixing in water during the manufacture process. 37 3.1. LOW DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS Figure 3.1: Hemp stalk size Figure 3.2 illustrates the makeup of the material, with two distinct samples being gathered. Sample 1 consisted of larger straw pieces akin to wood shavings, while sample 2 consisted of shorter, more delicate fibers. Finally, sample 3 encompassed the complete mixture of straw. Furthermore, the two samples exhibit distinct behaviors in water due to their differing densities. As depicted in Figure 3.2, it can be observed that sample 1 floats, whereas sample 2 sinks. Hence, a proposition was made to investigate the impact of using dry or wet hemp stalk in the mixing process. This suggestion stems from the possibility of generating a less uniform material if the hemp stalk were to float in the mix, Figure 3.3. Certain considerations must be taken into account before proceeding. Initially, commercial paper paste is used, utilizing bleached eucalyptus Kraft paste (ECF) to ensure consistent composition in each sample and eliminate possible variations between paper specimens. Once the potential use of hemp stalk as an insulator is confirmed, the commercial paste will be replaced with recycled fibers. 38 3.1. LOW DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS Figure 3.13: Sandwich type sample, core formed with 30E and skin with 50E compressed In the characterization tests, three distinct sample types were analyzed, both employing the identical binder, eucalyptus fiber, albeit in varying weight proportions. One sample contained 30% eucalyptus fiber by weight, designated as 30E, while the other contained 40%, labeled as 40E. Additionally, a compressed sample with 50% eucalyptus fiber by weight was labeled as 50E. 3.1.5 Acoustic insulation properties Methodology The acoustic properties were assessed using a two-microphone impedance tube, specifically the Br¨uel & Kjaer type 4206, Figure 3.14, in accordance with EN 10534 [49]. This standard test method involves the use of a tube, two microphones, and a digital frequency analysis system to measure the impedance and absorption of acoustical materials, Figure 3.15. The measurements were conducted within the frequency range of 100-6500 Hz. Cylindrical samples, with a radius of 1.5 cm and a thickness of 2 cm, were subjected to a plane sound wave, and the sound pressures were simultaneously measured at two microphone positions. By comparing the absorbed acoustic energy to the total incident energy, the normal incidence sound absorption coefficient ( α ) was determined. In Appendix A.2, the conducted tests and the raw data obtained are described in detail. The test sample is mounted at one end of a straight, rigid, smooth and airtight impedance tube. Plane waves are generated in the tube by a sound source (random, pseudo-random sequence, or chirp), and the sound pressures are measured at two locations near to the sample. The complex acoustic transfer function of the two microphone signals is determined and used to compute the normal-incidence complex reflection factor, the normal-incidence absorption coefficient, and the impedance ratio of the test material. From these data, a result is obtained for normal incidence on the sample, from which diffuse incidence coefficients can be estimated. This represents a rapid and valid prototype-level study, eliminating the need 45 3.1. LOW DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS for tests in large acoustic chambers. In this case, 2 microphones are used, so it is necessary to calibrate the equipment before conducting the test to ensure that the two microphones are in phase and amplitude. Figure 3.14: Kundt’s Tube Figure 3.15: Layout for acoustic test equipment [49] 46 3.1. LOW DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS Equipment: • Impedance tube: tube with a test sample holder at one end, a sound source at the other and two microphone ports. • Microphones: two identical microphones to produce the sound waves with the same amplitude and phase. • Signal generator: a signal generator capable to o generate a stationary signal with a flat spectral density within the frequency range of interest. It may generate one or more of the following: random, pseudo-random, periodic pseudo-random or chirp excitation. Br¨uel & Kjaer type 4206 produces random signal. •Amplifier: sound signal amplifier • Frequency analysis system: a two-channel Fast Fourier Transform (FFT) analysing system. The system is required to measure the sound pressure at two microphone locations and to calculate the transfer function H12 between them. •Computer with the Br¨uel & Kjaer signal analysis software Results During the acoustic test, it’s crucial to consider that the test requires completely flat sample surfaces for accurate results. In the case of the material developed in this thesis, the surface displays some roughness due to the presence of hemp stalk. This roughness appeared to affect the acoustic absorption within a specific frequency range during the test. However, it’s important to note that this reduction is merely an artifact caused by the sample’s geometry and does not reflect accurate values. To address this, the same sample was tested with a rotation around its central axis, altering the wave’s path and eliminating the artifact. It’s essential to highlight that this rotation only impacts the frequency range where accurate results weren’t initially obtained, while in the remaining range, the margin of error is less than 1%, thus validating the final sample results. Additionally, it is important to note that the thickness of the test specimen is 2 cm, while the manufactured sample has a thickness of 5 cm, and there is a difference in porosity along the thickness. For this reason, three specimens were created based on the selected position: •1: Bottom part •2: Middle part •3: Top part 47 3.1. LOW DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS Figure 3.16: Distribution of paper fiber along the sample: top part in the image was in contact with the vacuum Due to the vacuum process during manufacturing, it is observed in the samples that the lower part contains a higher amount of paper fibers, Figure 3.16. This is because they are capable of penetrating the gaps formed by the hemp stalk, resulting in a non-completely homogeneous distribution. This effect is less noticeable with a lower percentage of hemp stalk. In Figure 3.17 the impact of this process on performance can be observed, where the sample of the top part show a better acoustic properties due to have a higher porosity. Furthermore, to achieve a more homogeneous material for future studies, it is advisable to reduce the thickness and avoid using the vacuum process, even though it may require more time for the samples to dry. Figure 3.17: Acoustic absorption of the hemp stalk-eucalyptus specimens In Figure 3.18 the results of the acoustic absorption ( α ) of hemp stalk-Kraft paste specimens with 40% and 30% weight of the top part in the sample are compared with commercial synthetic materials such as rock wool and EPS. 48 3.1. LOW DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS It can be observe that the absorption is reduced in the lower frequency range (below 1000 Hz) but increases until reaching a maximum and then decreases, following the trend reported in the literature [59]. The lower absorption at low-frequency ranges is attributed to the material’s high porosity, while the increased porosity favors higher absorption at higher frequencies. From 1000 Hz onwards, the absorption values remain above 0.7, making it an effective insulating material, although the results are slightly inferior to those of rock wool. Figure 3.18: Acoustic absorption of the hemp stalk-eucalyptus specimens compared to commercial materials (EPS and rockwoll) 3.1.6 Thermal insulation properties Methodology For assessing thermal insulation properties, a square test specimen measuring 10 cm in width and 5 cm in thickness is positioned within a thermal chamber, Figure 3.19 & Figure 3.20 . The objective is to measure the temperature difference between the two surfaces of the specimen using two K-type thermocouples as sensors, following the guidelines specified in the EN 12664 [48] standard in order to calculate the thermal conductivity ( λ ) which represents the ability of a material to conduct heat when a temperature gradient exists perpendicular to a unit cross-sectional area. To ensure the thermal stability of the material the gradient of temperature is calculated after 1 hour of test, when the quasi-stationary phase is archived. In Appendix A.3, the conducted tests and the raw data obtained are described in detail. 49 3.1. LOW DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS Figure 3.19: Thermal resistance test Figure 3.20: Layout for thermal test equipment Under the assumption of a steady-state condition, a unidirectional heat flow within the thermal chamber, and exclusive heat transfer through conduction along the specimen, the thermal conductivity coefficient of the material ( λ ) is determined by utilizing the two acquired temperature values and the geometric properties of the test specimen. Qx=−λ A ∂T ∂x (3.1) ∂T ∂x ≈∆T ∆x=T2−T1 e(3.2) λ=Qxe A(T1−T2)(3.3) •Qx: Applied heat (W) •λ: Thermal conductivity coefficient ( W m K ) •A: Crosssection of the sample (m2) 50 3.1. LOW DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS •e: Thickness of the sample (m) •∂T ∂x : Temperature gradient in the x-direction •T1: Temperature measured with the thermocouple in the position near to the heat font (K) •T2: Temperature measured with the thermocouple in the outer part of the sample (K) For calibrating the Qx value, a commercially available material with tabulated thermal conductivity ( λ ) is introduced into the thermal chamber. As a result, Qx is determined using the temperature values recorded by the thermocouples. Equipment: • Thermal chamber: Insulating chamber capable to reduce the heat transfer to the exterior in order to obtain a high data accuracy. •60 W heat font. •Thermocouples: 2 identical thermocouples to measured the temperature of the sample. •MGCPlus: HBM signal acquisition. •Computer with the CATMANEasy software. Results The outcomes of the various conducted specimens are presented in Figure 3.21. Notably, in this instance, the thermal conductivity ( λ ) is observed to be 10-15% higher than that of commercial materials, indicating that the developed material holds promise as an exceptional thermal insulator. Figure 3.21: Thermal resistance of the hemp stalk-Kraft specimens compared to commercial materials 51 3.1. LOW DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS 3.1.7 Mechanical resistance: compression, shear & tension In addition to the previous tests, mechanical property tests were conducted to assess the strength of the material. These tests aimed to compare the mechanical properties of the material with those of commercially available materials used in similar applications. The objective was to ensure that the material would withstand its intended lifespan without experiencing any significant breakage or failure by comparing its mechanical performance with other commercial insulating panels (EPS). Methodology - compression For the compression test, prismatic specimens with dimensions of 100x100x50 mm were prepared. These specimens were subjected to compression testing at a constant test speed of 5 mm/min with a MTS insight 10 kN. The purpose of the test was to evaluate the material’s resistance to compression and determine its ability to withstand applied loads. The deformation of the specimens was monitored during the test, and the resistance of the material was assessed based on its ability to withstand strain up to 10% of its original dimensions, as specified by the EN 826 standard [50]. A preload of 10 N is applied to the samples. In Appendix A.4, the conducted tests and the raw data obtained are described in detail. When the value of the maximum stress corresponds to a strain of less than 10%, it is designated as compressive strength and the corresponding strain is reported. If no failure is observed before the 10% strain has been reached, the compressive stress at 10% strain is calculated and its value reported as compressive stress at 10% strain, Figure 3.22. Figure 3.22: Example of compression strain-stress curves [50] 52 3.1. LOW DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS σ=F A0 (3.4) ε=x e100 (3.5) E=σ10 e x10 (3.6) •σ: Compressive stress (MPa) •ε: Relative deformation (mm/mm) •F: Applied force (N) •x: Displacement (mm) •A0: Initial surface of the sample (mm2) •e: Initial thickness of the sample (mm) •E: Compression modulus of elasticity (MPa) Equipment: • MTS insight 10 kN: Universal testing machine, designed to suit the range of force and displacement involved and having two very rigid, polished, square or circular plane parallel platens with a minimum side length (or diameter) equal to the side length (or diagonal) of the test specimen. One of the plates shall be fixed and the other movable. •Computer with the MTS software. Methodology - shear The shear test was performed using a static puncture test (CBR test). Cylindrical specimens with a radius of 10 cm and thickness of 5 cm were prepared for this test. The specimens were placed on a cylindrical support with a radius of 6 cm, and a puncture with a radius of 3 cm was used. The test procedure followed the regulations outlined in ISO 12236 [51]. The shear test was conducted using an MTS Insight 300 kN machine, with a constant test speed of 5 mm/min. A preload of 20 N is applied. In Appendix A.5, the conducted tests and the raw data obtained are described in detail, Figure 3.23. 53 3.1. LOW DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS Figure 3.23: Example of static puncture test curves [51] τ=F A0 (3.7) γ=h e(3.8) •τ: Shear stress (MPa) •γ: Relative deformation (mm/mm) •F: Applied force (N) •h: Displacement (mm) • A 0 : Initial shear surface of the sample ( mm2 ), which correspond to the lateral surface that the plunger will pass through (2 π rplunger e). •e: Initial thickness of the sample (mm) Equipment: • MTS insight 300 kN: Universal testing machine, designed to suit the range of force and displacement involved and having two very rigid, polished, square or circular plane parallel platens with a minimum side length (or diameter) equal to the side length (or diagonal) of the test specimen. One of the plates shall be fixed and the other movable. •Plunger: Steel plunger with a diameter of 60 mm. • Clamping system: PVC clamping system that prevent slippage or cutting of the specimens with a 54 3.2. MEDIUM DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS (a) Colophony (b) Arabic gum (c) Corn starch (d) White glue (e) Bioepoxy Figure 3.30: Binder for medium density application 3.2.2 Characterization test In this section, the characterization tests that are utilized to assess the material’s suitability for different applications and validate its feasibility will be defined. Table 3.4: Characterization test for medium density solution Test Variable Number of samples Binder: 7 Tensile test - EN 319 %wt. of materials: 3 78 Curing time: 3 Fabrication method: 3 Binder: 7 Bending test - EN 310 %wt. of materials: 3 78 Curing time: 3 Fabrication method: 3 61 3.2. MEDIUM DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS The tests carried out encompass the examination of material compatibility, involving the characterization of its mechanical response in both tensile and bending scenarios, Table 3.4. Should a particular application be identified as the most promising, the corresponding test will be conducted accordingly. 3.2.3 Fabrication method This section presents the study of the compatibility between hemp stalk and the resins to be used in the applications of particle boards, parquet, and coffer ceiling. To conduct the study, composite specimens were fabricated using different resin selections and three different compositions (10 g of hemp stalk with 2/4/6 g of binder) to verify the stability of the resulting material, Figure 3.33. Subsequently, mechanical characterization tests were performed to determine the best proportions and binders. In the case of arabic gum and colophony, they are in a solid state initially. To create the binder, they need to be dissolved. Colophony is dissolved in acetone with a 2:1 ratio at 50°C, while arabic gum is dissolved in water at a 2:1 ratio at 90°C, as shown in Figure 3.31. Figure 3.31: Colophony (left), arabic gum (center) and adhesive made with corn starch (right) Corn starch was employed as a binding agent. For this purpose, food-grade starch was utilized following proportions outlined in the literature, with a ratio of 100 g of water for every 18 g of starch at 65°C, and the mixture was subjected to temperature and agitation [84], as illustrated in Figure 3.31. For making the specimens, two steel molds were purchased, Figure 3.32, to contain the hemp stalk mixed with the previously prepared binder, and pressure was applied from below to obtain the correct dimensions. In industrial manufacturing, 5 MPa pressure is applied for 5 minutes at temperatures above 100°C, depending on the binder used. Synthetic binders employed in the industry can cure in 5 minutes under these conditions. They use synthetic binders that accelerate the curing process at high temperatures, such as PMDI or UF. In the case of vegetable resins, temperature does not reduce the curing time. To make an initial approximation of the best selection, it was decided to apply 5 MPa pressure within the molds for 5 minutes instead of applying pressure during the entire curing time and completing the curing process outside the molds at ambient conditions. This process results in slightly lower properties, but it will facilitate the selection of resins with comparable results. 62 3.2. MEDIUM DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS Once the resins are selected, the improvement of the manufacturing process will be considered to meet the necessary specifications for each proposed application. Figure 3.32: Molds for the fabrication of tensile and bending specimens Table 3.5: Nomenclature structure of the samples Composition - % wt. relation binder-hemp stalk Binder Colophony 2-10 Arabic Gum 4-10 Corn starch 6-10 Bioepoxy White glue Figure 3.33: Specimens made with arabic gum Favorable results were obtained with the five resin tested, allowing subsequent mechanical tests to be carried out. However, it was observed that curing outside the mold at ambient temperature caused the specimens to increase in size during curing. Consequently, the properties obtained will be inferior to those achieved when pressure is applied throughout the entire curing process. In adition, a highly viscous binder, such as white glue, presented challenges during the mixing process of the two materials, especially when used in small quantities, leading to a non-homogeneous mixture. Notably, the specimens made with arabic gum, which utilizes water, exhibited the most significant changes in dimensions. Specimens with higher proportions of binder tended to break due to the significant increase in 63 3.2. MEDIUM DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS dimensions. This phenomenon occurs because the hemp absorbs water from the resin, leading to volume expansion. Due to the similar behavior observed in the samples, an optimization study of the fabrication method was conducted using the most promising resin. Subsequently, this optimization process will be extended to the other resins that were utilized. The primary emphasis of the optimization for vegetable-based resins was placed on refining the manufacturing process and managing humidity levels during the curing stage, as these were the primary challenges encountered during the initial fabrication. 3.2.4 Mechanical test: Tensile & bending Methodology - tensile The test procedure followed the regulations outlined in EN 319 [71]. Prismatic specimens with dimensions of 50x50x5 mm were used. Tensile test was conducted using an MTS Insight machine 10 kN, with a constant test speed of 5 mm/min. In Appendix A.10, the conducted tests and the raw data obtained are described in detail. The test setup resembles the tensile test described in the preceding section, but with a variation in the mechanism. In this case, a self-aligning ball and socket joint component is positioned within the testing machine and connected to a wooden block to exert force on the sample, as shown in Figure 3.34. The sample is affixed to the wooden block using white glue to ensure that the failure occurs within the sample itself and not at the bonding interface. Figure 3.34: Self-aligning ball and socket joint configuration [71] 64 3.2. MEDIUM DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS σ=F A0 (3.11) ε=d l(3.12) •σ: Tensile stress (MPa) •ε: Relative deformation (mm/mm) •F: Applied force (N) •d: Displacement (mm) •A0: Initial crossection area of the sample (mm2). •l: Initial length of the sample (mm) Equipment: •MTS insight 10 kN: Universal testing machine, for more details see 3.1.7. • Self-aligning ball and socket joint: This component is responsible for securing the sample and aligning the test configuration to generate tensile stress. The wooden piece and adhesive utilized to secure the sample must offer sufficient strength without interfering with the test, thus preserving the properties of the sample. •Computer with the MTS software. In this situation, it was not possible to install the extensometer during the tensile test due to limitations in the sample’s geometry. Nevertheless, the applied load was small enough to disregard any displacement of the connecting tools. Consequently, it is assumed that the displacement of the machine is the same that the displacement of the test sample. Methodology - bending A 3-point bending test configuration was employed, Figure 3.35, with a distance of 200 mm between the supports. The test procedure followed the regulations outlined in EN 310 [73]. Prismatic specimens with dimensions of 250x50x5 mm wer tested. Tensile test was conducted using an MTS Insight machine 10 kN, with a constant test speed of 5 mm/min. In Appendix A.11, the conducted tests and the raw data obtained are described in detail. The formulas described below correspond to the standard used, where a linear stress distribution is assumed. It’s important to note that this assumption doesn’t hold for the proposed material. However, the formulation will be retained to facilitate comparisons between the test specimens and commercially available results. 65 3.2. MEDIUM DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS Developing a formulation capable of addressing the nonlinearity of this material would increase the complexity of the results analysis, which is not the primary scope of this thesis. Figure 3.35: Bending test configuration [73] σ=3F l1 2b t2(3.13) E=l3 1(F2−F1) 4b t3(a2−a1)(3.14) •σ: Bending stress (MPa) •E: Bending young modulus. •F: Applied force (N) •d: Displacement (mm) •l1: Distance between the centres of the supports (mm) •b: Width of the sample (mm) •t: Thickness of the sample (mm) •F2−F1 : Increment of load on the straight line portion of the load-deflection curve. F1 and F2 shall be approximately 10% and 40% of the maximum load (N). •a2−a1: Increment of deflection at the mid-lenght of the sample corresponding to F1and F2(mm). Equipment: •MTS insight 10 kN: Universal testing machine, for more details see 3.1.7. •Cylindrical load head. 66 3.2. MEDIUM DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS •Two parallel supports. •Computer with the MTS software. Figure 3.36 show the configuration of the 2 mechanical test presented. Figure 3.36: Tensile test (left) and bending test (right) Results The outcomes of the preliminary specimens are presented in Table 3.6. The table presents the results obtained for each case. However, it should be noted that certain samples became unstable and broke on their own before testing, leading to values in the table without a coefficient of variation. Of particular significance is the case of starch resin, where all the samples prepared proved to be unstable due to the high moisture content of the resin, causing the samples to swell during the curing process, so it was removed from the table. The primary objective of this initial investigation is to establish the appropriate blending protocol and validate specimen fabrication. For non-vegetable resins, an increase in resin quantity corresponds to improved tensile and bending properties. For the white glue, the 2-10 composition exhibited low binder content to produce a good mix. However, this pattern does not hold true for vegetable resins. In the case of 6-10 composition with arabic gum and colophony, the tensile sample were unstable. This discrepancy is attributed to residual moisture in these resins, which leads to an enlargement of hemp stalk and an expansion of specimen dimensions during air curing. Both vegetable and synthetic resin results obtained fall significantly below the benchmarks set by commercial materials (tensile strenght: 0.4 MPa & bending strenght: 11 MPa [72]), underscoring the need for production enhancements. Subsequently, the focus shifts toward refining the conducted processes to minimize specimen numbers. These interim steps will exclusively involve vegetable resins. Once the final process is selected, specimens of all types would be produced to facilitate comparative analysis. 67 3.2. MEDIUM DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS Table 3.6: Tensile and bending test results Binder Composition Tensile strength (kPa), C.V. (%) Bending young modulus (MPa), C.V. (%) Bending strength (kPa), C.V. (%) 2-10 45.7 (15) - - White glue 4-10 109.5 (40) 21.27 (-) 150.6 (-) 6-10 279.5 (-) 39.70 (-) 491.9 (1) 2-10 19.5 (35) 2.12 (29) 317 (45) Bioepoxy 4-10 139.7 (15) 59.16 (26) 208.9 (23) 6-10 298.6 (26) 44.85 (1) 317 (36) 2-10 174.1 (40) 32.74 (9) 150.7 (5) Arabic gum 4-10 46.3 (5) 31.91 (3) 106.3 (6) 6-10 - 45.97 (47) 202.6 (26) 2-10 22.8 (23) 75.55 (28) 195.8 (34) Colophony 4-10 33.1 (28) 136.48 (16) 486.2 (33) 6-10 - 148 (12) 586.3 (4) Based on the outcomes presented modifications in the manufacture process are proposed to improve the quality of the samples. In terms of composition, mechanical strength exhibits linear dependence on applied resin. As a result in the following characterization process, the compositions will be reduced to two, representing the highest and lowest resin content. The first suggestion is to concentrate the resins for the purpose of minimizing moisture within the mold. The designation ”C” denotes a reduced water-to-gum arabic ratio during formation. Initially, the ratio is 2g of water per 1g of arabic gum; however, in these instances, a 3:2 ratio is adopted. This proportion was applied to two different cases, 2-10 and 6-10. In both cases, the dimensions expansion of the specimens decreased during curing. This effect was more pronounced in the 6-10 case, where a greater reduction in water was achieved, resulting in improved stability. In the case of colophony, the concentration ratio was adjusted to 1:1 instead of the initial 2g of acetone for every 1g of colophony. For specimens featuring higher resin content, superior results are attained by enhancing the maximum resistance strength, Table 3.7. These results follow the trend that higher proportions of binder yield better mechanical properties. Conversely, in cases of lower resin content, the outcome remains comparable due to the diminished water usage (and subsequently less reduction in overall water quantity) as well as the heightened challenge in blending the two components with a smaller amount. Based on the garnered findings, it is recommended to utilize concentrated resin exclusively in the scenario of the 6-10 composition. This adaptation results in a reduction of 30 g of water within the bending specimens. 68 3.2. MEDIUM DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS Table 3.7: Tensile and bending test results with concentrated arabic gum Binder Composition Tensile strength (kPa) (C.V.) Bending young modulus (MPa) (C.V.) Bending strength (kPa) (C.V.) 2-10 174.1 (40) 32.74 (9) 150.7 (5) Arabic gum 2-10 C 109.2 (9) 34.01 (3) 219.5 (12) 6-10 - 45.97 (47) 202.6 (26) 6-10 C 397.3 23.01 (8) 339.9 (5) A further recommendation is to prolong the duration of pressure application within the mold. The label ”5h MTS” indicates that the sample remained in the steel mold under pressure for 5 hours at 5 MPa and was then left to air dry for 1 week. This approach aims to mitigate sample expansion by allowing more time for resin curing, resulting in higher strength upon specimen demolding. ”1h oven” signifies that following a 5-minute pressure application, the mold was introduced into a 120°C oven for 1 hour. Similar to the previous modification, this method aims to expedite sample drying, thereby reducing the curing time while the specimen remains in the mold. Samples were also fabricated using smaller-sized hemp shivs, Figure 3.37. Using smaller hemp particles can enhance properties [171]; however, the hemp stalk used were already within the described range. To obtain the finer hemp stalk, the sample was filtered through a sieve, resulting in a median particle size of 5 mm compared to the initial 10 mm medium lenght. That modification is labeled as ”Thin”. Figure 3.37: Hemp stalk thin size Table 3.8 show the results of the different fabrication methods proposed. Unfortunately, the achieved outcomes are not favorable, mainly because the 5-hour duration within the mold proves inadequate for the complete resin curing process. After removing the specimen from the mold, it was observed that the humidity inside the mold was substantial. Moreover, during the week of curing outside the mold at ambient conditions, the dimensions increased significantly. This phenomenon occurred because the 69 3.2. MEDIUM DENSITY SOLUTION CHAPTER 3. EXPLORING APPLICATIONS binder began to cure inside the mold, causing the hemp to absorb the remaining water, as the mold did not allow moisture to escape. Figure 3.38: Sample with pressure applied in the mold Endeavors to expedite the curing process through elevated temperatures fail to enhance specimen outcomes, as this approach leads to the development of internal cracks caused by the swift removal of water, as illustrated in Figure 3.39. Figure 3.39: Crack formed during drying in the oven at 120°C The filtration of hemp stalk in order to use smaller particles does not contribute to improved results, Figure 3.40. Consequently, these attempted modifications are disregarded. 70 3.3. SELECTION CHAPTER 3. EXPLORING APPLICATIONS A score of 9 is assigned as the material is composed of 60% hemp and 40% arabic gum. However, adding a non-environmentally friendly reinforcement might be necessary to enhance the properties if this application is selected. A hemp mesh with epoxy resin could be used in that case. –Recyclability: 5 Similarly to the previous cases, a score of 5 is assigned due to the non-recycled nature of arabic gum, which comprises 40% of the material. An additional point is deducted for potential modifications that might be required. –Circular economy: 8 In this case, the lifespan is shorter, and the proposed material would be 100% recyclable except for the reinforcement part, thus receiving a score of 8. –Environmental impact: 9 The environmental impact for this type of material is minimal, thus receiving a score of 9, similar to the insulation panels, considering the potential impact of the reinforcement. –Potential limitations: 5 In this case, several limitations could affect the application, such as a high percentage of nonsustainable materials in the reinforcement or concerns about the water resistance of the assembly. •Coffer ceiling –Key characteristic: 10 The bending strength exhibited by the samples with colophony, even in the case of lower resin content (350 kPa), surpasses that of EPS (150 kPa). –Eco-friendly material: 9 A score of 9 is assigned because 82% of the material is composed of hemp, which receives a score of 10, while 18% is the binder. In this case, the binder must be colophony due to its resistance to moisture ambient. The colophony is mixed with acetone in a 1:1 ratio, resulting in a score of 5. –Recyclability:8 A score of 8 is assigned because 82% of the material is composed of hemp, which receives a score of 10, while 18% is the binder. In this case, the binder must be colophony due to its resistance to moisture ambient. Colophony could not be obtained from recyclable sources. –Circular economy: 0 The material will have amalgamated with the concrete and undergone significant degradation over time. Consequently, it cannot be repurposed as raw material for other applications, it receives a 77 3.3. SELECTION CHAPTER 3. EXPLORING APPLICATIONS score of 0. –Environmental impact: 9 Similarly to the previous application, the environmental impact of this material will be positive. However, it receives one point less due to the use of acetone. –Potential limitations: 8 There are potential limitations that might impede its application, primarily related to compatibility during concrete curing and fire safety regulations. Nonetheless, if these challenges arise, they can be addressed by adding a surface coating to safeguard the material. While this may reduce sustainability to some extent, it wouldn’t be a definitive barrier. Hence, a score of 8 is chosen. •Parquet –Key characteristic: 0 The primary characteristics considered are hardness and incompressibility. However, these properties have not been tested. A rating of 0 is assigned because the test specimens used demonstrate deformation under low loads, suggesting that their use as ground material may not be viable. –Eco-friendly material: 9 The green factor section is scored similarly to the chipboard case because the material and its usage over its lifecycle are comparable. –Recyclability: 5 –Circular economy: 8 –Environmental impact: 9 –Potential limitations: 0 It received a score of 0 due to its potential infeasibility for use in this application because of its lower mechanical properties. In Table 3.11, the scores for each of the applications are presented. Based on the obtained data, thermal insulation is the selected application. However, both types of insulation will be retained in the research due to the similarity in the test specimens and procedures. 78 3.3. SELECTION CHAPTER 3. EXPLORING APPLICATIONS Table 3.11: Application score table Thermal Acoustic Chipboard Coffer ceiling Parquet Key characteristic (45%) 10 8 4 10 0 Eco-friendly material (10%) 10 10 9 9 9 Recyclability (10%) 10 10 585 Circular economy (10%) 5 5 808 Envirommental impact (10%) 10 10 9 9 9 Potential limitations (15%) 66580 Score 8.9 8 5.65 8.3 3.1 This newly developed bio-composite material, incorporating hemp stalk and eco-friendly binders, demonstrates potential as a sustainable alternative to conventional inorganic insulating materials in the construction industry. However, to ensure its practical viability and long-term stability, further research is required. It is crucial to verify that the material retains its structural integrity and insulating properties over extended periods, thus ensuring its efficacy and durability in real-world applications. Continued investigation and development of this material will play a pivotal role in its success as a sustainable building material. The subsequent sections of this chapter will delve into the specific properties of hemp stalk, the evaluation of potential green binders, and the characterization of the resulting bio-composite material to shed light on its suitability for the selected applications. By comprehensively understanding and optimizing this material, we aim to contribute to the advancement of eco-friendly solutions in the construction industry. This material could be more versatile, not only serving as an insulating panel but also as a suitable substitute for EPS in various applications. For instance, in concrete sandwich materials or even coffer ceiling. The addition of EPS in concrete sandwitch composite materials results in a lighter, impact-resistant, thermally efficient, and cost-effective material, with an extended lifespan [172, 173]. This opens up more potential applications for the proposed material. However, this research will primarily focus on its individual application as an insulating panel. 79 3.4. CONCLUSIONS CHAPTER 3. EXPLORING APPLICATIONS 3.4 Conclusions Insulation panel and the coffer ceiling application exhibit significant potential. The thesis will primarily investigate the insulation panel, while the coffer ceiling is suggested for future research. •At least 30% by weight of short fiber material based on cellulose is needed to bind the stalk particles • The proposed insulating material is a hemp-based material composed of the following materials: 70% by weight of stalk and 30% by weight of recycled paper fiber (cardboard or newspaper) Based on the results obtained with eucalyptus fiber, a proposal is to replace it with recycled cardboard fiber, which is more durable. Since reducing eucalyptus fiber improves insulation properties, and the aim is to maximize hemp stalk usage, the initial ratios remain unchanged. However, further investigation is required to validate this relationship. If the hemp stalk does not interact well with cardboard fiber, one potential solution could involve using recycled newspaper fiber or alternative eucalyptus fibers for the application. •It necessary to use a coating to protect the material against moisture Additionally, there is a suggestion to explore the use of plant-based coatings on the material’s surface for protection against environmental and external factors. Gum arabic provides protection against moisture. Colophony protects against direct contact with water for a long period of time. • Once the insulating material is damaged, it can be disintegrated with water and reused as a raw material, obtaining great recycling and increasing the useful life of the materials and a circular economy •The insulating properties obtained are comparable to the commercial material The final material obtained has a high coefficient of acoustic insulation 0.8, although it is 0.1-0.2 dB/dB lower than commercial materials. In the case of thermal insulation, the proposed material is between 5-10% higher than conventional commercial synthetic materials. Obtaining a material with thermal conductivity coefficient of 0.035 W/m K. • The proposed insulating material meets the mechanical resistance requirements necessary to be used as an insulating panel in construction. Reaching compressive and shear strength values higher than EPS •The application of coffer ceiling is feasible using colophony as binder. While the mechanical properties of green resins may not match those of commercial materials, they are adequate for cofer ceiling application. Hence, colophony is recommended due to its water and moisture resistance. For particleboard application, structural reinforcement is necessary to improve bending strength. However, using hemp stalk with the proposed solutions for parquet is not feasible. • For the manufacture of these composite materials, it is advisable to use manufacturing processes and materials with low water content 80 3.4. CONCLUSIONS CHAPTER 3. EXPLORING APPLICATIONS The mechanical properties are greatly influenced by moisture during the curing process, as the hemp stalk absorb water, leading to swelling and a reduction in mechanical properties. Therefore, employing techniques to minimize moisture content in the material during curing is recommended. Comparing the requirements for insulating panels and the properties offered by synthetic materials with the properties of hemp stalk, this study proposes a solution for creating a fully plant-based material using hemp stalk as the primary component. In the context of this specific application, mechanical strength is not of utmost importance; rather, the material needs to meet minimum criteria to ensure stability during transportation and installation, preventing breakage, material detachment, or fissures. Consequently, a 100% plant-based material is defined for this purpose. Following the selection of the most promising application from the ones studied, the subsequent section will conduct a more in-depth analysis to confirm the properties using recycled cardboard, a more eco-friendly material. Furthermore, a thorough examination of the properties will be carried out, considering aspects such as material durability and compliance with regulatory requirements, including fire and moisture resistance. 81 Hemp crop waste for green solutions in construction: physical and mechanical characterization Chapter 4 Insulating panels In this chapter, the development process for the selected application, which involves creating insulating panels using hemp and recycled cardboard, will be outlined. The procedures encompass both mechanical and chemical processes aimed at improving the material composition. Subsequently, the material will undergo comprehensive testing for evaluation, including a durability test to assess its real-world feasibility. This study presents a unique approach, focusing on the development of a sustainable and environmentally friendly material primarily using hemp stalk while incorporating recycled cardboard fiber as a binding agent. The following sections will explain the material improvement process, emphasizing enhancements in insulating properties, durability, and compliance with regulatory standards such as fire resistance. To facilitate comparisons, samples with cardboard without any modifications will be manufactured and compared with the eucalyptus samples from the previous chapter. Then, various modifications will be introduced to assess their impact on material properties. The chapter will commence with an explanation of the theoretical basis for these modifications, followed by details on the materials used and the new fabrication method. Finally, characterization tests will be conducted, and once the optimal mix is selected, durability tests will be performed. 4.1 Improving the insulating panel In this section, an explanation of the three proposed modifications to the material mix will be provided. 4.1.1 Material & fabrication method The utilization of recycled paper and cardboard for cellulose-based insulation materials has been previously proposed in prior research [110]. Nevertheless, this thesis introduces an innovative approach by incorporating hemp stalk along with recycled cardboard fibers for the production of insulating panels [1]. Recycled cardboard possesses several key attributes that render it an excellent choice for these applications: 82 4.1. IMPROVING THE INSULATING PANEL CHAPTER 4. INSULATING PANELS • Recycled cardboard can be easily disintegrated to achieve desired bonding and shape through cellulose crosslinking •No chemical products are required to process the recycled fiber. •Recycled cardboard exhibits remarkable insulating properties. • It is a lightweight material with a hollow microstructure, depending on the manufacturing method employed. Furthermore, in the previous chapter, non-homogeneity was observed due to the application of vacuum. Therefore, in this case, the manufacturing process will not necessitate the use of a vacuum. However, for the initial samples, vacuum will still be employed for comparative purposes. Nevertheless, considering that the cardboard fibers are longer than the eucalyptus fibers, the use of vacuum should have a lower impact on the cardboard samples. 4.1.2 Green coating The primary challenges associated with this material involve its susceptibility to water, moisture, and fire. To address these issues, green surface coatings using colophony and arabic gum are proposed as protective measures. By applying a pine resin coating to the fibers, a hydrophobic material is created, providing increased stability against environmental factors. The addition of colophony in bamboo raises the contact angle from 60ºto 93º and reduce the porosity [144], and when the contact angle exceeds 90º, the material is considered hydrophobic. It is important to note that the addition of colophony may adversely affect the fire resistance properties of the material. On the other hand, arabic gum shows promising results as a coating in terms of humidity and fire resistance. Arabic gum can protect against moisture by creating a barrier that prevents water from penetrating the surface of the coated material. This is due to the film-forming properties of arabic gum, which enable it to create a continuous and uniform coating over the surface of the material. This coating can reduce the permeability of the material to water vapor and prevent the absorption of moisture, which can cause degradation, spoilage, or loss of functionality in the product. However, it cannot be used in direct contact with water, as it is soluble and may cause the protective coating to be removed when in contact with water [145]. The gum arabic membrane, as evidenced by a water contact angle of 43º, does not produce a hydrophobic coating [174]. However, it is worth noting that gum arabic contains active enzymes such as peroxidases, oxidases, and pectinases, which possess antimicrobial and antifungal properties [175]. Overall, the coating not only protect the material but also contributes to stabilizing its properties. 83 4.1. IMPROVING THE INSULATING PANEL CHAPTER 4. INSULATING PANELS 4.1.3 Crosslinking agent Recycled cardboard has remarkable insulating properties and easy disintegration, which facilitates the desired bonding and shaping process. Cellulose bonds are employed as the bonding method. Hence, a comprehensive investigation has been conducted to enhance the bonding process between the two materials and explore various methods for improving their properties and overall durability. Several types of acids have been found to enhance the bonding between cellulose molecules, including: •Citric acid (CA) •Tannic acid (TA) •Butyltetracarboxylic acid (BTCA) •Ethylenediaminetetraacetic acid (EDTA) •Polycarboxylic acid (PCA) •Hyaluronate acid (HA) Numerous studies in the literature have utilized these acids to enhance cellulose bonding in various materials. A biodegradable hydrogel can be developed from cellulose using EDTA to enhance water retention in soil and reduce the required fertilizer amount [176]. A biodegradable hydrogel can be manufacture using HA as a crosslinker and a carboamide solution as a reticulant, resulting in improved bonding between cellulose and enhanced mechanical properties of the hydrogel [177]. Adding BTCA in cotton fibers improve the efficiency of cellulose reticulation, which can be determined by chemical or mechanical processes [178]. In addition to using acids to enhance cellulose reticulation, catalysts can also be incorporated. For instance, in the case of tannic acid, the inclusion of cellulose nanocrystals improves the mechanical and physicochemical properties of chitosan films [179]. Among these, PCA and CA are noteworthy reticulants for paper fibers. Moreover, CA can be obtained from certain fruit wich could be suitable for a gree solution. CA have demonstrated their ability to enhance the mechanical properties of corrugated cardboard boxes and improve their resistance to moisture, thereby extending their lifespan [180]. Furthermore, citric acid augments the moisture barrier properties in other materials, such as starch. Acting as a crosslinker between starch and cellulose, it forms a viscoelastic foam, thereby enhancing thermal, mechanical, and water absorption properties [181]. Acid citric has been identified as potential additives to enhance specific properties of paper products. This improvement is attributed to the reduction of OH groups, which enhances the resistance to moisture of the cellulose bonding [182, 183]. In order for the acid to be effective, the curing temperature must exceed the acid’s melting point, leading to thermolysis decomposition and the production of di- and tricarboxylic acids (UAs), among others. The percentage of bonding improves as the curing temperature increases. As shown in Figure 4.1, when the temperature reaches 170°C or higher, the percentage of unbound citric acid is less than 84 4.1. IMPROVING THE INSULATING PANEL CHAPTER 4. INSULATING PANELS 10%. Moreover, the curing temperature impacts the curing time of the sample, reducing it, and influences the final color. Higher temperatures result in a darker color due to increased CA decomposition. However, there are no significant differences in compression strength after moisture loss [180]. Figure 4.1: Effect of curing temperature on the percentage of citric acid (CA) crosslinks and their thermal decomposition [180] Apart from using acid, it is advisable to consider the use of a catalyst or ensure that the mixture falls within an optimal pH range. In the case of PCA, NaH 2 PO 2 can serve as a catalyst, or if not using a catalyst, the pH should be maintained between 2.0 and 3.5 [180]. Other studies have employed NaH 2 PO 2 as a catalyst between citric acid and polyethylene glycol. However, better results are observed without the use of a catalyst as it leads to the formation of macromolecules that cannot be leached out during the filtration process through the filter paper [184]. Regarding citric acid (CA), there is no evidence indicating the necessity for a catalyst. As for pH, there seems to be no specific optimal range for cellulose bonding, suggesting that CA acts as a self-catalyst (see Figure 4.2). An additional advantage of CA over the other presented acids is its lower melting point, enabling curing at lower temperatures. Figure 4.3 illustrates how the addition of CA increases the lifespan of cardboard boxes up to 4 times. However, when the catalyst is added, the lifespan decreases as the catalyst makes the box more susceptible to ambient humidity [180]. The lifespan of CA-treated cardboard diminishes over time during storage, as the percentage of cellulose-CA bonds reduces with time, as confirmed by the FTIR-ATR spectrum analysis [180]. 85 4.1. IMPROVING THE INSULATING PANEL CHAPTER 4. INSULATING PANELS Figure 4.2: Crosslinking of cellulose molecule with citric acid [180] Figure 4.3: Crosslinking of cellulose molecule with citric acid [180] 86 4.4. FABRICATION METHOD CHAPTER 4. INSULATING PANELS The manufacturing process for the samples involved some variations depending on the specific materials used and the inclusion of citric acid, CA in the nomenclature Table 4.3. The samples made with eucalyptus fiber and the first cardboard fiber (XXE/R-L-E/C-0), where citric acid was not used, the vacuum water extraction method was employed to remove excess water. Subsequently, the samples were manually mixed and then dried in an oven at a temperature of 60°C for 48 hours. The samples made with the cardboard fiber that incorporated citric acid (XXR-L-C-0/AC-0/C/GA), a different approach was taken. The drip water extraction method was used to remove excess water from the samples. The drying process involved placing the samples in an oven at a higher temperature of 170°C to activate the citric acid in the mixture. This activation was carried out over a duration of 24h. Additionally, the mixing of the materials was conducted using an electric mixer at a speed of 900 rpm for 3 minutes, ensuring thorough blending and distribution of the components. This adjustment was implemented to standardize the samples, irrespective of their manufacturing date. The cardboard was fully disintegrated on the same day and subsequently stored to maintain consistent properties across all samples. Over time, during storage, the cardboard fibers tend to bind together, making it challenging to blend with the hemp stalk. To address this issue, the introduction of an electric agitator proved effective, as it helped to separate the cardboard fibers and enhance the mixture of the two materials. 4.4.2 Fabrication method of insulating panels Following the completion of the respective tests, the subsequent phase entailed the fabrication of demonstrator panels to assess the potential for producing larger sizes and to conduct bending tests. The manufacturing process involved introducing a blend of hemp and paper fiber into a mold equipped with a drainage mesh, relying on gravity for water removal, Figure 4.6. Figure 4.6: Manufacture process of insulating panel The mold is placed within a drying oven at 60°C for a period of 48 hours. Subsequently, the surface coating is applied, and the resin is cured within the oven. The initial test specimens that were produced include: •70% hemp stalk - 30% cardboard fiber with colophony 93 4.5. MICROSTRUCTURE CHAPTER 4. INSULATING PANELS •70% hemp stalk - 30% cardboard fiber with arabic gum •60% hemp stalk - 40% cardboard fiber with colophony •60% hemp stalk - 40% cardboard fiber with arabic gum These panels are employed to confirm that the results obtained from the small samples are equivalent to the performance of a full-sized panel. 4.5 Microstructure 4.5.1 Methodology The microstructure analysis of the samples was conducted using an Olympus BH-2 optical microscope, which was equipped with a x4 objective lens, Figure 4.7. This setup enabled to examine and observe the surface coating as well as the internal structure of the samples. To ensure that the captured images accurately represent each of the samples, the surfaces of various test specimens were examined at both central and lateral positions. Figure 4.7: Olympus BH-2 optical microscope 4.5.2 Results Microstructure plays a crucial role in determining the insulating properties of green materials. As such, it is important to understand how the application of coatings on the surface of these materials can impact their microstructure and ultimately affect their insulating properties. This information is of great significance 94 4.5. MICROSTRUCTURE CHAPTER 4. INSULATING PANELS in the development of effective and sustainable insulation materials. Additional figures of the samples are presented in Appendix A.8. Figure 4.8: Surface of different samples: a) Colophony with acid citric, b) colofony, c) arabic gum with acid citric, d) arabic gum Both coatings exhibit full surface adherence to the hemp-based material, Figure 4.8. However, there is a noticeable distinction between them. The colophony coating effectively seals the smaller radius pores while leaving the larger ones intact, whereas the gum arabic coating forms a superficial membrane that effectively covers the pores of the material. The size of the membrane pores falls within the range of 38-60 nm [174]. This difference in behavior is crucial to consider when choosing a coating material, as it can significantly impact the material’s microstructure and overall insulation properties. In the case of bamboo, the introduction of colophony into the internal pores resulted in a reduction of porosity and total pore volume by 14.42% and 23.81%, respectively [144], the colophony fill the pores creating a barrier that inhibited water diffusion and transmission [185]. The internal microstructure of the material was examined in Figure 4.9, and no discernible differences were detected at the microscopic level between the samples treated with citric acid and those that were not treated. The internal microstructure of the samples exhibits horizontal layers with fibers arranged in a random fashion. 95 4.6. MOISTURE BUFFER VALUE CHAPTER 4. INSULATING PANELS Figure 4.9: Internal microestructure of sample with acid citric (a), and without it (b) 4.6 Moisture Buffer Value 4.6.1 Methodology The moisture buffer value (MBV) is a measure of a material’s ability to regulate moisture levels. It is determined using the method specified in the NORDTEST project [186], which provides a standardized approach for assessing the practical moisture buffer value of materials under dynamic conditions. The MBV quantifies the amount of moisture that a material can absorb and release per unit of open surface area, taking into account daily cyclic variations in relative humidity. By measuring and understanding the moisture buffer value, we can evaluate a material’s ability to regulate moisture and its potential impact on indoor environments and occupant comfort. The method involves subjecting the samples to humidity cycles of 75-33% for 8-16 hours each at a constant temperature of 23°C. The Ineltec climatic chamber was used to conduct the test. During the test, the weight of the samples was monitored until mass stability was achieved. Mass stability was defined as a mass change of less than 5% over three consecutive cycles. For the test, 100x100x30 mm samples were employed, and to ensure their sealing, aluminum coating was applied to five out of the six faces of the sample, Figure 4.10. Figure 4.10: Ineltec climatic chamber 96 4.6. MOISTURE BUFFER VALUE CHAPTER 4. INSULATING PANELS 4.6.2 Results Based on the categorization from the NORDTEST Project, these materials demonstrate exceptional hygroscopic regulation properties (MBV > 2 g/(m 2 %RH)) [186]. When the moisture buffering capacity of a material results in a comparable average moisture flow rate to that caused by the minimum necessary air exchange, the buffering effect can be regarded as highly impactful for the moisture dynamics within a room. The ideal moisture buffering response should aim for maximum effectiveness and rapidity. In Appendix A.9 the data of the tested samples are presented. Table 4.4: Moisture buffer results Sample MBV (g/m2%RH)C.V. (%) 30R-H-0-0 4.49 7.4 30R-H-0-CA 4.20 3.2 30R-H-C-0 3.78 7.9 30R-H-C-CA 3.95 5.4 30R-H-GA-0 6.01 26.5 30R-H-GA-CA 5.37 6.5 All the samples presented exhibit similar values within a consistent range, indicating a rapid response to fluctuations in ambient humidity, Table 4.4. The addition of citric acid to the samples leads to a reduction in the measured values. However, this effect is minimal and falls within the expected range of variability among the samples. The presence of a colophony coating on the sample (30R-H-C-0/AC) acts as a protective surface barrier, resulting in a modest 11% decrease in MBV compared to the uncoated samples (30R-H-0-0/AC). In the case of bamboo, previous studies have shown a more significant reduction in water uptake of 24.7% due to the treatment’s ability to decrease porosity [144]. The applied coating on the proposed material primarily impacted the surface layer, resulting in a limited reduction in internal porosity. Consequently, the decrease in water uptake was smaller in comparison to previous studies and does not significantly differ from that of the uncoated samples. In contrast, the incorporation of arabic gum (30R-H-GA-0/AC) amplifies the moisture transfer process by 30%. Although the arabic gum membrane is able to fill all the superficial pores of the material [174], its water-soluble nature results in a higher tendency for moisture absorption on the surface of the coated sample. Consequently, the moisture buffer value is increased, indicating an enhanced capability for regulating moisture within the material. Regarding the presented material, the findings demonstrate its notable capacity to absorb substantial quantities of ambient humidity, which improves the comfort and quality of life for the residents. However, it is important to note that excessive levels of humidity can have adverse effects on the material. High humidity 97 4.7. WATER ABSORPTION BY PARTIAL IMMERSION CHAPTER 4. INSULATING PANELS content weakens the cellulose bonds, leading to a reduction in insulation properties and material strength [187]. 4.7 Water absorption by partial immersion 4.7.1 Methodology In accordance with ISO 29767:2019 [53], a partial immersion experiment was conducted to assess the material’s behavior during short periods of direct contact with water. The samples were partially immersed in water for a duration of 10 minutes. This test was conducted to evaluate the material’s response to water exposure and assess its performance in terms of water resistance and durability. 4.7.2 Results To complement the findings, a water immersion test was conducted using three test samples: one without any coating, one coated with colophony, and one coated with gum arabic, Figure 4.11. The results revealed that the uncoated material could withstand immersion for approximately 3 minutes before disintegration, while the gum arabic-coated sample exhibited extended resilience, lasting for approximately 15 minutes. The water contact angle of hemp fiber has been reported to be 77-87º[188], whereas the arabic gum membrane exhibits a contact angle of 43º. Despite the reduction in contact angle observed with the arabic gum coating, it serves as a protective layer that shields the interior of the material until it dissolves in water. This characteristic leads to an increased duration of contact between the material and water, thereby extending the material’s resistance to water exposure. Importantly, if the material was removed from water before complete disintegration, it showed the ability to regain its structural integrity upon complete drying. Regarding the colophony coating, after 15 minutes, the sample experienced a 5% increase in weight, and the inner part remained dry, indicating effective moisture absorption by the surface layer and a successful coating. The colophony-coated sample demonstrated exceptional durability due to the hidrophobic properties (raising the water contact angle [189]). The material remained intact when immersed in water for a duration of 90 days without any visible damage; however, some discoloration of the coating was observed, Figure 4.12. This observation may indicate a degradation process happened, highlighting the need for further investigation. Additionally, literature reports indicate that the water uptake of samples treated with colophony increased after 30 days of water immersion [142]. Based on these findings, it can be confirmed that the application of colophony creates a hydrophobic characteristic in the material, as evidenced by its performance in the water immersion test. However, it is important to note that the moisture buffer value (MBV) test showed that the material still allows for moisture transfer with the surrounding environment. 98 4.7. WATER ABSORPTION BY PARTIAL IMMERSION CHAPTER 4. INSULATING PANELS (a) Colophony (b) Arabic gum (c) Whitout coating Figure 4.11: Water absorption test Figure 4.12: Decoloration of colophony after 90 days 99 4.7. WATER ABSORPTION BY PARTIAL IMMERSION CHAPTER 4. INSULATING PANELS Nevertheless, the disintegration of the material upon contact with water has an advantage. Once the material has deteriorated, broken, or reached the end of its lifespan, it can be easily disintegrated using water to obtain the raw material and be manufactured again. In the case of colophony, a mechanical process can be applied to remove the superficial part, allowing the interior zone to be reused as raw material for manufacturing. On the other hand, gum arabic can be completely reused by separating the coating using water. Although gum arabic is not suitable as a coating in direct contact with water, it still offers protection against moisture, making it suitable for specific applications. Figure 4.13: Water contact angle: arabic gum (up) and colophony (down) To confirm the similarity of the water contact angles reported in colophony and arabic gum to the samples used, a water contact angle test was conducted on the raw solid resin. To ensure an appropriate surface for the test, the resin blocks were filed. The test was carried out using an optical contact angle apparatus with SCA 20-U software, employing the sessile method with a 4 µ L drop of distilled water dispensed via 100 4.8. FTIR-ATR CHAPTER 4. INSULATING PANELS a Hamilton 500 µ L needle, Figure 4.13. A total of 5 repetitions were performed on different surfaces. The results obtained are presented in Table 4.5: Table 4.5: Water contact angle results Sample Water contact angle (º) C.V. (%) C 95 3 GA 72 7 4.8 FTIR-ATR 4.8.1 Methodology Fourier Transform Infrared–Attenuated Total Reflectance (FTIR-ATR) spectra of a sample treated with acid citric and untreated were collected with a Thermo Scientific Nicolet 6700 FT-IR spectrometer, Figure 4.14. For each sample, absorbance spectra of the scan range 4000-400 cm −1 were recorded. To identify the chemical groups present in the samples, spectra of the most significant groups in similar materials were examined based on existing literature. Additionally, to assess the impact of citric acid, the spectra of all three samples were compared, with consideration given to the area of each group. Any alterations in the areas of these groups indicated changes in chemical composition. Figure 4.14: Sample 80E 4.8.2 Results According to the literature, specific bands should be considered for analyzing the effect of the acid on the sample. The decrease in intensity of the hydroxyl group (OH) stretching vibrations, indicated by a broad peak at 3336 cm −1 , along with the appearance of a shifted peak at 1726 cm −1 corresponding to the formation of ester’s carbonyl group (C=O), can be regarded as characteristic peaks for crosslinking reaction according to several studies [180, 190, 191], however in Figure 4.15 a reduction in the intensity of these peaks is not observed in the sample treated with CA. The 2900 cm −1 band represent the CH stretching [192]. Futhermore, the weakening of the hydrogen bond likely alters the vibrational energy of the entire cellulose chain, thereby 101 4.8. FTIR-ATR CHAPTER 4. INSULATING PANELS influencing the characteristic band at 1159 cm−1[182], as can be observed in Figure 4.16. Additionally, with the addition of CA, characteristic bands of C–O stretching, which are characteristic of CA, can be observed at 1704 cm −1 in the spectra, Figure 4.16. This observation confirms the continued presence of the acid in the material’s composition [193]. The appearance of the strip at 1725 cm −1 in the 30R-H-0-AC sample provides evidence of the chemical process involving the crosslinking of cardboard with citric acid [192]. However, this peak is relatively inconspicuous due to the limited quantity of cardboard fiber in comparison to the hemp stalk. The presence of a peak at 1373 cm −1 indicates CH bending in cellulose [180]. Peaks at 1730 cm −1 and 1720 cm −1 correspond to esterified carboxyl groups of both CA and UAs, while the absorbance at 1030 cm−1can be attributed to the vibration associated with C–O–H deformation [192]. In summary, the spectra indicate a minimal presence of acid in the sample and a reduction in hydrogen bonds, possibly resulting from a brief reaction between cellulose present in the cardboard and citric acid, followed by acid decomposition producing the increase of esterified carboxyl groups. However, the spectra also reveal that the crosslinking of cellulose has not significantly improved. This may be due to the absence of cellulose reaction in the hemp stalk, suggesting the potential need for a catalytic material to initiate the reaction. Therefore, The spectra suggest that the addition of CA to the samples does not enhance their mechanical properties, indicating that CA does not improve the crosslinking between the cardboard and the hemp stalk. However, it could potentially improve the durability of the samples by reducing the hydrogen bonding within the cellulose chain. In this manner, the durability test will aid in confirming the hypothesis. Figure 4.15: Comparison of the spectre of the samples with acid citric 102 4.11. FIRE RESISTANCE CHAPTER 4. INSULATING PANELS insights into its performance in fire scenarios and ensuring compliance with the necessary standards. Figure 4.19: Typical flame impingement points for products with thickness greater than 3 mm [76] Equipment: • Ignition source: consisting of burner constructed and designed so that it can be used vertically or be tilted at 45°with respect to the vertical axis. The burner shall be mounted onto a horizontal plate so that it moves smoothly forwards and backwards in a horizontal plane along the centreline of the combustion chamber • Fuel: consisting of commercial propane of 95% minimum purity. In order to obtain flame stability with the burner tilted at 45°, the gas pressure shall be between 10 kPa and 50 kPa • Support, consisting of a vertical stand to which the specimen holder is attached such that it hangs vertically and exposes its open edge containing the specimen to the burner flame • Flame-height measuring device: capable of indicating a flame height of 20 mm when located against a fixed point of the burner. •Timing device 109 4.11. FIRE RESISTANCE CHAPTER 4. INSULATING PANELS Figure 4.20: Fire test - sample 30R-C-O Figure 4.21: Fire test - sample 30R-GA-O 110 4.12. MECHANICAL TESTS CHAPTER 4. INSULATING PANELS 4.11.2 Results Materials are classified based on their fire resistance according to fire regulations. The minimum required classification for construction materials is Type E. In the test, the material should not ignite, meaning that there should be no presence of a flame for a duration exceeding 3 seconds. Additionally, the flame height (F s ) should not exceed 15 cm from the point of application within a 20 second period. Table 4.8: Fire resistance Sample Fs(cm) Ignition Type E 30R-L-0 25 YES NO 30R-H-C-C-0 >30 YES NO 30R-H-C-AC >30 YES NO 30R-H-GA-0 15 NO YES 30R-H-GA-AC 11 NO YES In order to meet the fire resistance regulations, the three coating materials were studied, Table 4.8. Based on the findings from the uncoated specimen (30R-L-O), the material exhibits a low level of fire resistance, it does not meet the necessary criteria for classification in the E category. Consequently, for building applications, the incorporation of a fire-resistant coating is imperative.This coating must provide enhanced fire resistance and also serve to safeguard the interior of the material, effectively preventing the fire from coming into contact with the interior. Both coatings have achieved the expected results. The colophony coating (30R-H-C-O/AC), Figure 4.20, which is not a good fire-resistant material, and considering that acetone was used for its application, obtained a negative rating in the test. However, when using gum arabic (30R-H-GA-O/AC), Figure 4.21, the results were successful. Only a small and superficial charred area was observed where the flame was applied, while the rest of the material remained intact as the fire did not spread. 4.12 Mechanical tests: compression, shear and bending In addition to the previous tests, mechanical property tests were conducted to assess the strength and durability of the material. These tests aimed to compare the mechanical properties of the material with those of commercially available materials used in similar applications. The objective was to ensure that the material would withstand its intended lifespan without experiencing any significant breakage or failure. By evaluating its mechanical performance, it can be confirmed that the material is capable of meeting the required standards and specifications for its intended use, providing assurance of its reliability and suitability for the intended application. 111 4.12. MECHANICAL TESTS CHAPTER 4. INSULATING PANELS 4.12.1 Methodology For the compression test, prismatic specimens with dimensions of 100x100x30 mm were prepared following the EN 826 standard [50]. The shear test was performed using a static puncture test (CBR test). Cylindrical specimens with a radius of 10 cm and thickness of 3 cm were prepared for this test, following ISO 12236 [51]. The bending test was conducted using 250x50x30 mm samples. A 3-point test configuration was employed, with a distance of 200 mm between the supports. The test was performed at a constant speed of 5 mm/min using a MTS insight following the EN 12089 standard [52]. For more details about the methodology see section 3.1.7. In Appendix A.4, A.5 and A.6 the raw data of the conducted tests are detailed. 4.12.2 Results Bending test in commercial size insulating panels The bending strength test was conducted using the manufactured panels. This test adhered to EN 12089 standards [52], employing panels with dimensions of 90x42 cm and a thickness of 5 cm, as illustrated in Figure 4.22. Figure 4.22: Bending test in insulating panels In Table 4.9, the results are presented, and in all cases, the values surpass the strength of EPS, which is 100 kPa. Consequently, the mechanical stability of the material is confirmed with this data and also corroborate that the result obtained in the small size panels are in the same range of values. 112 4.12. MECHANICAL TESTS CHAPTER 4. INSULATING PANELS Table 4.9: Bending Strength of Insulating Panels Sample Bending test Bending strength (kPa) C.V. (%) 40R-L-GA-0 235.7 (13) 30R-L-GA-0 317.7 (16) 30R-L-C-0 179.8 (16) Mechanical properties of the samples After confirming the insulation capabilities of the material, mechanical resistance tests were conducted to compare the obtained results with other ongoing developments in insulation materials. Additionally, the results can also be compared with the EPS (in Table 4.10 is highlighting in bold the values that are higher than EPS ) so that the material is resistant enough not to be damaged during transport or placement of the panels. Table 4.10: Compression, shear and bending test results Sample Compression test Shear test Bending test Young Modulus (MPa) C.V. (%) Shear stress (kPa) C.V. (%) Bending strength (kPa) C.V. (%) 30E-L-0-0 0.810 (15) 15.1 (27) - 40E-L-0-0 0.664 (39) 17.0 (33) - 40R-L-GA-0 0.526 (42) 15.4 (13) 235.7 (13) 40R-L-C-0 0.221 (7) 30.4 (4) - 30R-L-GA-0 0.239 (54) 39.0 (8) 317.7 (16) 30R-L-C-0 0.541 (43) 30.2 (17) 179.8 (16) 30R-H-GA- 00.667 (27) 41.5 (16) 306.4 (16) 30R-H-GA- CA 0.676 (14) 31.5 (25) 230.1 (12) 30R-H-C-0 0.960 (28) 41.9 (39) 431.5 (35) 30R-H-C- CA 0.523 (31) 37.8 (25) 260.8 (10) Table 4.11 presents the results from both commercial sources and experimental testing. Nevertheless, for comparing the mechanical properties of the insulating panels, the commercial data will be utilized. It’s worth noting that the EPS used in the test had been stored in the laboratory and may have undergone degradation. 113 4.12. MECHANICAL TESTS CHAPTER 4. INSULATING PANELS Table 4.11: Mechanical properties of EPS Sample Compression test Shear test Bending test Young Modulus (MPa) C.V. (%) Shear stress (kPa) C.V. (%) Bending strength (kPa) C.V. (%) Commercial data 0.50 30 150 Experimental results 0.36 (4) 14.9 (13) 110.6 (2) The first case was a compression test, where the material is compressed between two steel plates, calculating the elastic modulus up to 10% compression strain as indicated by the regulations. EPS has a compressive strength of 0.5 MPa, so in the first case with uncoated Kraft pulp these values are exceeded, Table 4.10. By adding the cardboard fiber, despite being a more resistant fiber, the compressive strength is reduced. When the coating is applied, the surface area of the specimen becomes moistened, causing the bonds of the material to soften. This is more noticeable in compression tests, as if the surface has low resistance, the 10% of strain compression occurs mainly on the surface rather than being evenly distributed throughout the entire thickness. This also leads to an increase in variation between different samples. Comparing the results of the cardboard specimens treated without citric acid (30R-H-C/GA-0), which were cured at a higher temperature (170°C) and the sample with the same composition cured at lower temperature (60°C) (30R-L-C/GA-0), can be observe that they show lower result dispersion and improved mechanical properties. This suggests that the effect of the curing temperature diminishes that effect, as reducing the curing time allows the bonds to have less contact with water, resulting in less weakening. For future samples it will be necessary to study the effect of curing temperature and speed. Furthermore, to minimize the dispersion of the sample, it is recommended to explore the effect of applying pressure during the fabrication process to achieve uniformity. However, it is crucial to avoid applying excessive pressure, as this could compromise the porosity of the material. In Table 4.10 it is compared the compression young modulus to other proposed insulating material. It can be noted that the mechanical properties of the binder have a important effect on the performance of the composite material. The shear test involves conducting a static puncture test to compare it with EPS, resulting in a value of 30 kPa. Notably, when considering the fiber length as a significant factor, the utilization of cardboard fiber leads to a substantial increase in shear strength. Eucalyptus fiber exhibits shear strength 50% lower than EPS. However, recycled cardboard demonstrates superior mechanical resistance and possesses longer fibers compared to eucalyptus. Remarkably, the cardboard samples demonstrate a substantial increase in resistance, with fibers that are 2.5 times longer than eucalyptus fiber, resulting in a 40% higher resistance than EPS, Table 4.10. Additionally, the cardboard fibers exhibit a higher lignin content, which enhances the stiffness of the material. In the case of samples with CA, its inclusion does not lead to an improvement in the mechanical 114 4.12. MECHANICAL TESTS CHAPTER 4. INSULATING PANELS properties. These findings align with the results mentioned earlier, indicating that citric acid did not undergo a significant reaction with the hemp stalk. The results obtained in the bending test follow a similar pattern as the other two tests, Table 4.10, with the notable observation that the range of values obtained is higher than that of EPS (150 kPa) even double it in the best cases (30R-GA/C-O). In the three mechanical tests conducted, no significant difference was observed between the samples treated with citric acid, with corroboorate that the acid citric do not improve the crosslinking of the cellulose. However, it should be noted that there was a high variance in all the samples, which can be attributed to the significant impact of moisture on the mechanical properties of paper fibers. The mechanical test results demonstrate the enhanced properties of cardboard specimens produced with an electric mixer (30R-GA/C-O) compared to those mixed manually (30R-GA/C). The use of a high-speed mixing tool facilitates better fiber disintegration of the cardboard, leading to a more percentage of bonding among all the materials. Therefore, a material that meets the mechanical resistance requirements has been obtained using the 70% stalk composition and recycled cardboard, and is also a good thermal and acoustic insulation, using the 2 different coating. The density of the specimens is 130-160 kg/m3. The coating plays a crucial role, with improved results seen in cases involving arabic gum. The quantity of hemp is also a significant factor, as increasing its proportion leads to higher bending strength. Based on the three conducted tests, the addition of arabic gum as a coating enhances the biomaterial’s mechanical properties. However, an exception is noted in compressive strength. Nonetheless, for this material, the critical focus is on enhancing its insulating properties, and in this regard, colophony demonstrates superior results. Considering that using colophony aligns with regulatory prerequisites for mechanical strength and offers enhanced resistance to moisture, the configuration comprising 70% hemp, 30% recycled cardboard fiber, and a colophony coating stands out as the most promising choice among the options explored in term of mechanical properties. Table 4.12 presents a comparison of the compression Young’s modulus of the hemp-based materials with other materials. The compression modulus is chosen as a representative and widely studied parameter. The mechanical properties of the composite are significantly influenced by the binder used. In the context of structural applications, it is recommended to incorporate a small amount of hemp stalk into traditional materials like concrete. This addition of hemp particles as aggregates serves multiple purposes, such as reducing the density of the material, enhancing its insulation properties, and increasing its potential for CO 2 storage. However, it should be noted that the mechanical properties of the composite may decrease as a result (up to a 30% reduction when incorporating 8% hemp) [89, 90, 91]. Additionally, the use of cementitious matrices can lead to chemical damage to the hemp stalk, despite the advantages of affordability and adaptability they offer [92]. 115 4.13. DURABILITY CHAPTER 4. INSULATING PANELS Table 4.12: Compression young modulus compared with other stalk based materials Fiber Matrix Ecofriendly material Compression Young Modulus (MPa) Reference Hemp stalk Cardboard & arabic gum/colophony YES 0.67-0.96 This study Hemp stalk Wheat starch YES 0.1-0.15 [84, 128] Hemp stalk Reactive vegetable protein YES 1.1-3.0 [141] Corn stalk Epoxy NO 0.11-0.29 [68, 100] Hemp stalk Porltand & MgO- cement NO 0.4-2.1 [89] Hemp stalk Lime NO 0.3-0.5 [85] 4.13 Durability In this section, a detailed overview of the durability tests conducted on the developed composite material will be provided. These tests are crucial to ensure the material’s stability throughout its expected service life, enabling its use in various applications. For the durability test the sample used were 30R-H-C/GA-CA/0 in order to compare que coating and the acid citric with the best composition obtained. Therefore, in this section, the label will be simplified to the coating, crosslinking agent, and durability time. 4.13.1 Methodology The durability testing method involves subjecting the material to natural cycles under ambient conditions, replicating the environmental conditions it would encounter during real application use, Figure 4.25. A range of test specimens were prepared and exposed to different durations of ambient conditions. These specimens were then tested to evaluate the potential property degradation. To conduct this investigation, thermal insulation, acoustic insulation and mechanical properties (compression, shear and bending) were chosen as the key parameters. These properties were evaluated at specific intervals of 0, 3, 6, and 9 months, following the testing procedures outlined in the previous sections (3.1.5, 3.1.6 & 3.1.7. 116 4.13. DURABILITY CHAPTER 4. INSULATING PANELS Figure 4.23: Temperature and moisture in the laboratori Figure 4.24: Sample weights across durability process 117 4.13. DURABILITY CHAPTER 4. INSULATING PANELS Figure 4.25: Samples storage in laborataory conditions 4.13.2 Results Prior to presenting the test outcomes, it is essential to outline the temperature and moisture conditions to which the samples were subjected and their impact on weight over time, Figure 4.23 and Figure 4.24. The tests began during the winter, the laboratory temperature remained stable due to the heating. This heating was temporarily halted during the weeks coinciding with the New Year holiday. The heating was turned off at the end of winter. As depicted in the two graphs, the ambient humidity percentage is the primary factor influencing weight due to moisture absorption by the test specimens. It can be observed that both types of coatings follow the same trend, although there is a difference in their initial weight. This is because arabic gum takes longer to eliminate the water used to form the resin than acetone in colophony. Consequently, its initial weight is higher due to the extra water content that evaporates during the first two weeks. Since the graph is expressed relative to the initial weight of each sample, this difference reflects the initial conditions. However, as the results of the MBV test show, the water diffusion properties are similar, so they follow the same trend, although variability is slightly higher in the case of arabic gum. These tests also serve to validate the findings from the FTIR analysis, which indicated that the acid does not enhance cellulose crosslinking but may offer a slight improvement in moisture resistance. In other words, degradation over time may be less than in cases where citric acid was used. 118 Hemp crop waste for green solutions in construction: physical and mechanical characterization Chapter 5 Life cycle In this section, the objective is to examine whether the use of the developed material aligns with a sustainable development model: one that satisfies the needs of the current generation without compromising those of future generations. Understood as a necessity, it involves consuming services formed from limited resources. Thus, it should not exceed what can be generated sustainably. To achieve this, three sustainability indicators are used: carrying capacity, carbon footprint, and life cycle analysis. • Carrying Capacity: This indicator represents the maximum number of individuals a service can support without jeopardizing future needs. • Carbon Footprint: This measures the amount of land or sea required to support the human population and absorb the carbon and waste they generate. • Life Cycle Analysis: This is an objective procedure aimed at assessing the environmental impacts of a product’s entire life cycle, from extraction and processing to use, disposal, and even recycling. It quantifies resource consumption, water and energy usage, emissions, and waste generation at each stage, ultimately expressing these processes as the product’s environmental impact. In this section, an exhaustive life cycle analysis of the material will not be conducted as it falls beyond the scope of this thesis. Instead, a short analysis will be performed using the life cycle methodology. These analyses will aid in presenting the material as environmentally friendly and a greener alternative compared to the synthetic materials commonly employed today. Therefore, the analysis is conducted manually without utilizing commercial software databases such as SigmaPro. 125 5.1. METHODOLOGY CHAPTER 5. LIFE CYCLE 5.1 Methodology The subsequent guidelines prescribe how to conduct a life cycle analysis of materials: • Environmental management - Life cycle assessment - Principles and framework: ISO 14040:2006 [149] • Environmental management - Life cycle assessment - Requirements and guidelines Amendment 2: ISO 14044:2006 [150] In order to be more rigurous methology, the life cicle analyse will follow the guidance outlined in the PCR (Product Category Rules) for insulating materials made of foam plastics [195]. The document contains the requirements on an Environmental Product Declaration (EPD) for the range of environmental product declarations published by Institut Bauen und Umwelt e.V. (IBU). In the document the results of the life cycle are presented in the following stages: •Product stage –Raw material supply –Transport –Manufacturing •Construction process stage –Transport from the gate to the site –Assembly •Use stage –Use –Maintenance –Repair –Replacement –Refurbishment –Operational energy use –Operational water use •Ends of life stage –De-construction demolition –Transport –Waste processing 126 5.2. LIFE CYCLE ANALYSIS CHAPTER 5. LIFE CYCLE –Disposal •Benefits and loads beyond the system boundaries –Reuse/Recovery/Recycling potential These phases align with a cradle to cradle system; however, for the purposes of this analysis, it will be simplifyied. Consequently, the emphasis will be on examining until the material’s use, excluding considerations of end-of-life phases and recycling, which have not been extensively investigated in the thesis. Corresponding to a cradle to use system. The material being studied is the insulating panel made up of 70% hemp stalk, 30% recycled cardboard fibers, and an arabic gum coating. This material is fabricated under laboratory conditions. To simplify the analysis, it’s important to note that resources related to the construction of the factory, waste generated from personal protective equipment (PPE) like gloves, the production of the panels, packaging, or the initial stages of secondary materials like arabic gum, etc., will not be included in the assessment. In order to perform the analysis the PCR define that the declared unit for coated insulating materials is 1 m2. This measured will be use to calculate the inputs and outputs of every stage that are needed. 5.2 Life cycle analysis In that section the life cycle analysis will be perform taking into account the coonsiderations explaned in the methodology. 5.2.1 Product stage Raw material supply In this stage, arabic gum will not be considered for simplification. On the other hand, cardboard and hemp stalk are regarded as recycled and waste materials, so in this case, the inputs and outputs are treated as zero. Regarding hemp stalk, some inputs include water, fertilizer, and other products used in cultivation, while outputs include CO 2 emissions from chemical products, etc. However, since it is considered a waste material, all these contributions are associated with the main products of the crops, which are the textile industry. Transport For this part, the fuel consumption of the transport truck to carry the raw material to the factory where the panel is processed is considered. In this way, the amount of equivalent CO 2 for the functional unit of the panel is estimated, taking into account that, for simplification, other inputs such as worn tire rubber, vehicle maintenance oil, etc., are not considered. In the PCR document, the specific quantity of kilometers used to estimate CO 2 emissions is not specified. 127 5.2. LIFE CYCLE ANALYSIS CHAPTER 5. LIFE CYCLE Therefore, for the purpose of this analysis, and given that the material promotes a local economy approach (km 0), a transportation distance of a maximum of 100 kilometers will be assumed. Consequently, it is assumed that a truck carrying 10,000 kg of raw materials consumes an average of 40 liters of fuel for every 100 kilometers traveled. Based on this, the functional unit is calculated to be 6.5 kg of raw material. Therefore, for the functional unit, a fuel consumption of 0.056 liters is considered, resulting in the production of 0.148 kg of CO 2 equivalent emissions. Manufacturing In the manufacturing stage, the electricity consumption in the laboratory factory will be taken into account. This includes the disintegration of the recycled cardboard fiber, the mixing of raw materials, the preparation of resin with Arabic gum, and the electricity consumed by the oven during the curing process. The disintegrator machine consumes 0.3 kW h, and it is required for 1 hour to produce the material for one functional unit. The preparation of the coating consumes 0.1 kW h for 15 minutes. However, the oven is the most energy-consuming component, using 0.5 kW h for 48 hours for one functional unit. In total, the energy consumption amounts to 24.3 kW h for manufacturing one functional unit. In the case of Catalonia, the emission are 273 g CO 2eq /kW h considering the data provided by the government for the year 2023. This energy consumption is associated with 6.6 kg of equivalent CO2, On the other hand, the production of the material requires the use of 100 liters of water. However, this water can be reused for each functional unit. Nevertheless, a 1% loss will be taken into account, considering the losses of water during the reusing process, the need to change the water between several cycles, and the cleaning process of the machines. Moreover, to produce the arabic gum used for coating the functional unit, 0.8 L of water is needed. In that case, a consumption of 1.8 L of water is considered. 5.2.2 Construction process stage Transport from the gate to the site In this stage, the same assumptions made in the previous stage will be applied, as the same inputs and outputs are provided. Assembly In this stage, the inputs and outputs are null because no machinery is required for the installation of the insulating panel, and it can be installed manually by the operator. 128 5.2. LIFE CYCLE ANALYSIS CHAPTER 5. LIFE CYCLE 5.2.3 Use stage In this stage, it will be assumed that the material does not require any repairs. Given that it doesn’t need energy or consume other materials to operate, the inputs and outputs for this stage are considered as zero. 5.2.4 Results Considering all the simplifications made in this analysis, to prduce a funtional unit oof 1 m 2 of the green insulating panels, is necesary a compsutioon of 6.5 kg of raw material and 1.8 L of water resulting in a emissions of equivalent CO2. Considering all the simplifications made in this analysis, to produce a functional unit of 1 m 2 of the green insulating panels, it is necessary to consume 6.5 kg of raw material and 1.8 L of water, resulting in emissions of 6.9 kg of equivalent CO2. Furthermore, it’s crucial to consider that hemp absorbs CO 2 during its growth, a factor not accounted for in this analysis. In the first stage, a ton of hemp can absorb 325 kg of CO 2 during crop growth. In the functional unit, 4 kg of raw hemp stalk is used, which results in an absorption of 1.3 kg of CO 2 . With this data, the insulating panels’ final carbon emissions are still positive (5.6 kg of CO2emitted into the atmosphere). Additionally, this analysis highlights that the curing stage in the oven is the phase with the highest emissions, accounting for 95% of the total emissions. This could potentially be improved in a large-scale industrial factory by implementing more efficient machinery, ultimately achieving the desired negative CO2emissions. Moreover, the CO2absorbtion during the cultivation of arabic gum should be taken into account. Lastly, under optimal conditions, the material could potentially be reused as a raw material to produce other green insulating materials, extending the material’s life cycle. However, further studies would be necessary to confirm this and incorporate it into the life cycle analysis. 129 5.3. CONCLUSIONS CHAPTER 5. LIFE CYCLE 5.3 Conclusions The life cycle analysis conducted in this thesis has been simplified to provide a basic technical characterization of the material. A more comprehensive study and the utilization of commercial software will be necessary for validation at each stage. However, this approach serves as a valuable method to validate the environmental advantages of replacing synthetic commercial materials with a green insulating panel made from hemp stalk. • A functional unit of the green insulating panel is associated with 6.9 kg of equivalent CO 2 . The total carbon footprint of the panel is currently positive. However, with a more efficient curing process, emissions could potentially be reduced, eventually achieving a negative carbon footprint. 130 Hemp crop waste for green solutions in construction: physical and mechanical characterization Chapter 6 Conclusions and future research 6.1 Conclusions Based on the results presented in various studies conducted over the past few decades, hemp stalk emerges as a green material with exceptional insulating properties, positioning it as a replacement for certain inorganic commercial materials. This growing interest in hemp stalk can be observed through the increasing number of research initiatives and the expansion of the hemp industry in the business sector. The insulating panels developed in this thesis improve thermal insulation and acoustic comfort in buildings, thereby aiding in the creation of non-structural materials for eco-friendly construction. Here are some key conclusions and recommendations based on the findings of this thesis: • Hemp stalk applications: Based on the initial studies conducted, hemp stalk exhibits significant thermal and acoustical insulating properties for the production of eco-friendly insulation materials, which is the primary focus of this thesis. Moreover, coffered ceilings are also an application where hemp stalk can be a substitute for synthetic materials. • Variability in hemp stalk properties: Different hemp varieties and positions on the stem can result in significant variations in the elastic modulus of hemp stalk, up to 60%. These variations can be attributed to the distinct sizes of cell walls in different hemp varieties, as segments with larger cell walls exhibit a higher elastic modulus. Nonetheless, it is still uncertain whether these fluctuations in cell size directly affect the insulating properties of hemp. To enhance the material’s performance, it is crucial to confirm the stability of the raw material’s properties. It’s possible that to achieve higher quality, the hemp stalk should be provided from a specific section of the stem. • Importance of binders: The choice of binder plays a critical role in creating a low-density and porous material, which is essential for achieving optimal insulating properties. A notable gap in the existing literature is the scarcity of studies employing recycled cardboard fibers as a binder in combination 131 6.1. CONCLUSIONS CHAPTER 6. CONCLUSIONS AND FUTURE RESEARCH with other eco-friendly particles to fabricate insulating panels. Recycled cardboard exhibits great compatibility with hemp stalk, resulting in a stable material comprising a minimum of 30% cardboard fiber. This manufacturing process does not require high temperatures or pressure, reducing the energy consumption during production while also yielding a low-density material with high porosity, thus enhancing its insulation properties. • Green insulating panels: The proposed insulating material is primarily composed of hemp, with 70% of the composition consisting of hemp stalk and the remaining 30% comprising recycled cardboard fiber. Increasing the quantity of hemp enhances the acoustical and thermal insulating properties, surpassing the performance of both materials individually due to the synergistic qualities of the hollow microstructure it creates. Additionally, a surface coating is applied, with the choice between colophony or gum arabic depending on the specific application. The material offers excellent insulation properties, positioning it as a viable alternative. • Insulating properties: Hemp-based insulating materials demonstrate competitive insulating properties (0.02-0.03 W/m K and 0.85-0.95 dB/dB). Surpassing some commercial alternatives in thermal insulation by 15-40% and closely matching them in acoustic insulation (0.2 dB/dB lower) when compared to rockwool. The exceptional insulating properties are achieved through the intrinsic characteristics of the materials themselves and their synergistic interactions, creating a hollow microstructure that forms air gaps. These air gaps effectively reduce heat transfer and dampen sound waves. • Protection against ambient conditions: Hemp-based composite materials are susceptible to environmental degradation. The green insulating panel disintegrates in just 3 minutes upon direct contact with water. To address this, a protective coating is essential. Arabic gum is effective in shielding the material from moisture, while a colophony coating renders the material hydrophobic. • Ambient confort: The material possesses a notable capability for absorbing ambient humidity, thereby enhancing hydrothermal comfort by reducing humidity fluctuations within the building environment. By adding a coating of arabic gum, the MBV increased in a 30% due to its capacity to dissolve in water, resulting in a significant uptake of ambient moisture. • Mechanical strength: The proposed materials meet the necessary mechanical strength requirements for insulating panels in construction. They have a compression elastic modulus of 0.65-0.95 MPa, shear strength of 40.0-42.0 kPa, and bending strength of 310-430 kPa in the best cases studied, surpassing the performance of Expanded Polystyrene (EPS). In the case of mechanical properties, the binder has a significant influence. The sample with cardboard increased the shear strength of the eucalyptus by 100% due to the longer fiber length and improved mechanical properties. Additionally, applying pressure in the fabrication method can enhance the mechanical properties; however, it also reduces the material’s porosity, resulting in lower insulation performance. As a result, this approach was ultimately discarded. 132 6.2. FUTURE RESEARCH CHAPTER 6. CONCLUSIONS AND FUTURE RESEARCH • Influence of citric acid: The inclusion of citric acid enhances the material’s durability by reducing hydrogen bonds within cellulose molecules in the cardboard fibers. • Fire resistance: The insulating panel developed cannot withstand direct contact with an open flame. However, this limitation can be addressed by applying a coating. When coated with arabic gum, the material can come into contact with a flame for a short duration without igniting or propagating the flame. • Life cicle analysis: A functional unit of the green insulating panels (1 m2 ), produced in laboratory conditions, is associated with 6.9 kg of equivalent CO 2 . However, it’s important to note that hemp has the capability to sequester carbon dioxide (CO 2 ) during its cultivation, which results in a net carbon footprint of 5.6 kg emitted into the atmosphere. The negative result could potentially be reversed with the use of an efficient industrial manufacturing process that could achieve a total negative carbon footprint. Additionally, opting for biomaterials like cardboard fiber and arabic gum can significantly reduce the carbon footprint. However, these factors were omitted in the analysis. • Recycling and circular economy: Once hemp-based insulating materials reach the end of their life cycle or are damaged, they can be disintegrated with water and reused as raw materials. This offers significant potential for recycling and supports a circular economy. In conclusion, the research conducted thus far highlights the promising potential of hemp-based composite materials for sustainable insulation and construction applications. However, continued research and development are essential to optimize these materials for real-world use, enhance their properties, and ensure their long-term durability. This ongoing exploration will play a crucial role in advancing sustainable building materials and reducing the environmental impact of construction practices. 6.2 Future research As a result of the research conducted in this thesis, several questions have arisen, identified as gaps in the current state of knowledge, and potential avenues for future research. These may prove to be compelling areas for future studies that will contribute to a deeper understanding within the scientific community on this topic. Future research should investigate the relationship between hemp stalk properties, including variety and stem position, and their effect on insulation properties. Plant-based composite materials, although significant for reducing the planet’s negative impact, may not always meet the mechanical property criteria for non-structural applications. To tackle this challenge, researchers can investigate the incorporation of inorganic components or a proportion of green materials into the resin to improve mechanical performance, all while adhering to their commitment to environmentally friendly solutions. Moreover, further research is required to investigate the acoustic properties, fire resistance, 133 6.2. FUTURE RESEARCH CHAPTER 6. CONCLUSIONS AND FUTURE RESEARCH resistance to fungal growth, and long-term durability of 100% green composite materials. The existing literature contains limited information on these topics. Future research should explore the compatibility of inorganic coatings with the composite material to meet specific requirements such as moisture resistance, fire protection, and long-term stability. Additionally, investigations into fabrication methods and the influence of different levels of applied pressure on insulating and mechanical properties should be conducted. An extended durability and end-of-life test could also be of interest to comprehend how the material performs over an exceptionally long period, such as 20 or 50 years. Coffered ceilings presents itself as an intriguing avenue for further investigation. This could involve the utilization of colophony as a binder or potentially employing the same approach as with the insulating panels, using recycled cardboard as a binder and incorporating colophony as a protective coating. Further research is necessary to accurately measure the enhancement in the durability of insulating panels through the addition of citric acid. Furthermore, exploring various chemical catalysts to activate cellulose crosslinking in hemp stalk and assessing their impact on insulating properties is an intriguing area of study. 134