scieee AI-readable full text Open interactive document viewer

Mechanical, stress corrosion cracking and crystallographic study on flat components processed by two combined severe plastic deformation techniques

Romero Resendiz, L.,Cabrera Marrero, José M.,Elizalde Huitrón, Sergio Alberto,Amigó Borrás, Vicente,Figueroa, I. A.,González, Gonzalo

Abstract

Although the current field of application of Al–alloy 7075 (AA7075) is vast, it is still limited due to some drawbacks, especially due to its susceptibility to stress corrosion cracking (SCC). This work aims to evaluate the microstructural, mechanical, and stress corrosion cracking (SCC) behaviors on an AA7075 in flat format deformed by a combination of repetitive corrugation and straightening (RCS) and accumulative roll bonding (ARB) techniques. Four different deformation routes were applied, namely: ARB (A), RCS (R), RCS + ARB (RA) and ARB + RCS (AR). As expected, the efficiency for grain refinement depends on the applied route, in terms of average grain size regarding the initial condition IC): AR > A > RA > R. All conditions resulted in unimodal and widened grain size distributions of micro-, submicro- and nano-metric dimensions. The study of crystallographic orientations showed that route R did not generate any new texture, whereas different preferred orientations were obtained for routes A, RA, and AR. The hardness and three-point bending tests showed an improvement of mechanical strength in the following order: AR > RA > A > R. The cracks per cm2 obtained in the corrosion study indicated that the best SCC resistance was R > A > AR > RA. Based on the above, the best combination of microstructural, mechanical, and SCC properties until one deformation pass was obtained by the single route of the ARB process.

Full text

Original Article Mechanical, stress corrosion cracking and crystallographic study on flat components processed by two combined severe plastic deformation techniques L. Romero-Resendiz a , J.M. Cabrera b , S. Elizalde b , V. Amig o-Borr as c , I.A. Figueroa a , G. Gonzalez a,* a Instituto de Investigaciones en Materiales, Universidad Nacional Aut onoma de M exico, Circuito Exterior S/N, Cd. Universitaria, A. P. 70-360, Coyoac an, C.P. 04510, Mexico b Departamento de Ciencia e Ingenierı´a de Materiales, EEBE eUniversitat Polit ecnica de Catalunya, Eduard Maristany 10-14, 08019, Barcelona, Spain c Universitat Polit ecnica de Val encia, Instituto de Tecnologı´a de Materiales, Camino de Vera S/n, 46022, Valencia, Spain article info Article history: Received 3 December 2021 Accepted 2 March 2022 Available online 12 March 2022 Keywords: Alealloy Repetitive corrugation and straightening Accumulative roll bonding Stress corrosion cracking Texture Mechanical behavior abstract Although the current field of application of Alealloy 7075 (AA7075) is vast, it is still limited due to some drawbacks, especially due to its susceptibility to stress corrosion cracking (SCC). This work aims to evaluate the microstructural, mechanical, and stress corrosion cracking (SCC) behaviors on an AA7075 in flat format deformed by a combination of repetitive corrugation and straightening (RCS) and accumulative roll bonding (ARB) techniques. Four different deformation routes were applied, namely: ARB (A), RCS (R), RCS þARB (RA) and ARB þRCS (AR). As expected, the efficiency for grain refinement depends on the applied route, in terms of average grain size regarding the initial condition IC): AR >A>RA >R. All conditions resulted in unimodal and widened grain size distributions of micro-, submicro- and nano-metric dimensions. The study of crystallographic orientations showed that route R did not generate any new texture, whereas different preferred orientations were obtained for routes A, RA, and AR. The hardness and threepoint bending tests showed an improvement of mechanical strength in the following order: AR >RA >A>R. The cracks per cm 2 obtained in the corrosion study indicated that the best SCC resistance was R >A>AR >RA. Based on the above, the best combination of microstructural, mechanical, and SCC properties until one deformation pass was obtained by the single route of the ARB process. ©2022 The Author(s). Published by Elsevier B.V. This is an open access article under the CC BY-NC-ND license (http://creativecommons.org/licenses/by-nc-nd/4.0/). *Corresponding author. E-mail address: [email protected] (G. Gonzalez). Available online at www.sciencedirect.com journal homepage: www.elsevier.com/locate/jmrt journal of materials research and technology 2022;18:1281e1294 https://doi.org/10.1016/j.jmrt.2022.03.010 2238-7854/©2022 The Author(s). Published by Elsevier B.V. This is an open access article under the CC BY-NC-ND license (http:// creativecommons.org/licenses/by-nc-nd/4.0/). 1. Introduction Flat components of Al alloys with distinct geometries are highly used in several industries, such as aeronautic, naval, automobile bodies, machinery, and equipment, storage tanks, cans, among others [1,2]. In 2018, the global Al-based alloys flat products market size exceeded USD 52 billion and the growing estimations are over 5.0% of the compound annual growth rate for the period between 2019 and 2026 [3]. From the abovementioned flat products, the 7075 Alealloy (AA7075) is commonly applied in aircraft parts, particularly in wing coating, spars, and stabilizers, as well as in machinery and equipments, due to its high mechanical strength, high strength-to-weight ratio and fatigue resistance [4]. However, the field of application of the AA7075 is still limited for some drawbacks, such as its susceptibility to stress corrosion cracking (SCC). To overcome the previous problem, a few authors have reported the improvement of SCC susceptibility on AA7075 through superficial severe plastic deformation techniques (SPD) as laser peening [5,6]. This result is related to the generation of a compressive stress state that delays cracking formation and propagation [7e9]. However, these efforts have been addressed to superficial studies and not to the entire volume of the material. Repetitive corrugation and straightening (RCS) and accumulative roll bonding (ARB) are two promising techniques of the SPD family, which were designed for flat geometries. Both processes induced compressive stress state [10,11] and are highly efficient to refine bulk Albased microstructures to submicro-metric or nano-metric sizes [12e17]. As result, ARB and RCS materials have enhanced mechanical properties [16,18e22] in comparison with their coarse-grained counterparts. Moreover, the ARB process has improved the electrochemical corrosion susceptibility of AleMn and Al-1050 alloys [23,24]. This was explained in terms of residual stress and defects that create better conditions for continuous and adhered passive films. Besides, the RCS process has been shown not to aggravate resistance to SCC in an Al-7075 alloy with broad grain sizes distributions [18]. From the above, RCS and ARB processes could increase the shelf life of the abovementioned applications of AA7075 flat-made components as automobile carcass, pressure vessels, chemical containers, aircraft parts, ship body components, machinery, architecture, among others [18,25]. However, none of the previous works has studied the relationship between mechanical emicrostructural ecrystallographic features and their effect on the corrosion behavior of these alloys. It is well known that microstructure and preferred orientation significantly impact the mechanical assessment of metallic materials. Studying the relationship between them is fundamental for a good understanding of the final performance. It is widely reported that RCS and ARB processes reduced the grain size and improved mechanical properties since the first deformation pass [14,17,25,26]. Accordingly, this work focuses on studying the first pass of deformation by each of the abovementioned routes. The need for a single deformation pass could be advantageous for many applications due to the cost-effective process, the requirement of low labor demands, and high-volume production. This work aims to study the microstructure, texture, and mechanical response generated by the application of RCS and ARB and their combination on an AA7075. The results were correlated to the SCC susceptibility of the processed alloy. The comparison between four deformation routes (RCS, ARB, RCS þARB, and ARB þRCS) allowed determining the most effective path for improving the mechanical assessment without affecting the SCC of the AA7075. To date, no previous literature specifically studying the SCC susceptibility or texture performance of the AA7075 processed by a combination of RCS and ARB processes has been reported. The results of this work might reduce the current limitations of the AA7075 and broaden the knowledge of flat Al-based alloys processed by SPD techniques. 2. Experimental procedure A commercially available AA7075 in T4 condition from “La Paloma Compa~ nia de Metales”was used as starting material. The chemical composition of the alloy was Al-5.3Zn-2.2Mg-1.8Cu- 0.3Fe-0.28Cr-0.06Ti-0.01Ni (wt.%). The supplied plates had a thickness of 12.5 mm, but they were subjected to cold-rolled down to a thickness of 1 mm. A heat treatment at 450 C for 2 h and slow cooling in the furnace down to room temperature (RT) was applied to obtain an initial homogeneous texture on the sheets of 1 mm in thickness, 120 mm in width, and 120 mm in length. These samples are identified in this work as the initial condition (IC). 2.1. Plastic deformation processing 2.1.1. RCS processing The IC samples were further processed by RCS at room temperature. An Instron 8802 hydraulic press with a maximum capacity of 200 kN was used for this purpose. Polytetrafluoroethylene sheets of 0.39 mm thickness were used to minimize the friction coefficient between the sample and the RCS dies. The geometry of the two D2 steel dies based on sinusoidal profiles for the corrugation stages can be observed in Fig. 1a. The straightening steps of the RCS process were carried out between two flat dies. The processed sheets were rotated 90around the normal direction to alternate the most deformed zone between each corrugation stage. For this work, each RCS pass consists of 5 stages: 1) corrugation e2) straightening e3) 90rotation e4) corrugation e5) straightening. As a result, all sheets are flat at the end of each RCS pass. The effective strain for each RCS pass using the design shown in Fig. 1 was equal to ~0.8, in the most deformed zones [17]. It is worth mentioning that two of those flat sheets were cleaned, brushed up, and piled up before being subjected to the ARB process (as explained below). 2.1.2. ARB processing The IC sheets were brushed and cleaned with acetone before the deformation process. ARB was performed at 300 Cata compression rate of 0.5 m s 1 . This temperature corresponds to 0.6 of the homologous temperature, which is above the range of cold working for Al-based alloys [27]. The selection of this temperature facilitated the passage of the strips journal of materials research and technology 2022;18:1281e12941282 through the laminating rollers, activating the diffusion mechanisms that allow the mechanical union between the plates. Before the rolling processing, the sheets (consisting of two stacked IC strips) were pre-heated for 15 min. This methodology was based on previous literature reports [14,28]. For the present work, a deformation pass by ARB refers to the following 2-stage process: 1) stacking of two IC strips, 2) single lamination with a 50% reduction in thickness. Considering the reduction in thickness per pass, the equivalent deformation (ε) estimated for each ARB processing step is ~0.8 [29]. 2.1.3. RCS mixed ARB processing For the combination of deformation techniques, both processes were carried out following the methodology described in 2.1.1. and 2.1.2. Subsections. The processed samples were identified as R, A, AR, and RA, where the letters R and A correspond to one pass RCS and ARB processes, respectively. The sequence of the letters indicates the order of application of the processes. 2.2. Microstructural evaluation X-ray diffraction (XRD) measurements were performed using a Rigaku Ultima IV diffractometer, with Cu-Karadiation, crossbeam optics (CBO), operating at 40 kV and 44 mA. A step size of 0.02and a scanning speed of 0.07min 1 were used for peak broadening measurements. Moreover, a sampling step of 1.5and a scanning speed of 100min 1 were used for texture measurements (a:0e90;b:0e360). The macro residual strain (ε) was estimated using the slope of εversus sin 2 j, where jis the angle formed between the normal of the sample and the normal of the diffraction plane. The (422) plane and 10 experimental jvalues (from 60to 54) were taken for each curve. The measurements were done on the raw surface of the IC, R, and A samples. For the electron backscattering diffraction (EBSD) analysis, the AA7075 samples were prepared by standard metallographic preparation and finished by vibratory polishing (VibroMet 2), using a colloidal silica solution with a particle size of 0.3 mm. The EBSD analysis was carried out in a Jeol JSM- 7001F scanning electron microscope (SEM) with a Bruker Quantax EBSD detector (15 KV). Based on the experimental EBSD results, orientation distribution functions (ODF) were calculated with MTEX 5.6 software (MATLAB toolbox R2020b) [30]. 2.3. Mechanical behavior The processed samples were cut along the rolling direction into bone-shaped specimens. The tested samples sized 12.5 mm in gauge length, 3.3 mm width, and ~1 mm thickness after SiC grinding until 2000 grade. Uniaxial tensile tests were performed on a universal testing machine (Instron 3382,100 kN) with a strain rate of 10 4 s 1 at RT. Three samples of each studied condition were tested. The yield strength was determined at the 0.2% strain. The end of the uniform elongation was determined by the Consid ere criterion [31]. For determining the bending stress applied during the SCC tests, three-point bending tests were performed utilizing a Shimadzu AGX universal testing machine. Results were recorded and plotted with the TrapeziumX software. The bending load was applied by exerting a concentric load on the center of the rectangular geometries described in Table 1. The span between both supports, as well as the diameter of punch and supports, are also shown in Table 1. The bending rate was 2 mm min 1 . A Shimadzu microdurometer model HMV-FA2 with an applied load of 100 gf for 10 s was used to evaluate the hardness of the samples. An average of 10 microhardness measurements were taken per sample. 2.4. Stress corrosion cracking evaluation The surface of three samples from each condition (IC, R, A, RA, and AR) was cleaned with acetone before the SCC testing. The samples with the geometry dimensions specified in Table 1 Fig. 1 ea) Corrugation RCS die used in this work and b) site where the samples were taken for the characterization. In white and yellow, the location of samples for bending and all the rest studies, respectively. ND, TD, and RD are the normal, transversal, and rolling directions, respectively. h(x) is the height, and x is the horizontal coordinate. journal of materials research and technology 2022;18:1281e1294 1283 were immersed in a 3.5 wt. % NaCl solution for 168 h at RT. Constant flexural stress equal to 1 and 1.2 times the yield strength (YS) was applied on all samples. The length of the tested samples was parallel to the rolling direction. The SCC study was carried out following the standard ISO 9591 [32]. After testing, samples were prepared by conventional metallographic procedures until mirror finishing appearance with a diamond solution of 0.1 mm in particle size. Optical microscopy observations were carried out to evaluate the cracking morphology and quantification. The standard deviation from the mean values was estimated considering the three measurements per condition. 3. Results and discussion 3.1. Microstructural evaluation Figure 2 shows the EBSD inverse pole figures (IPF) micrographs of the IC, R, A, RA, AR samples, as well as the orientation map key. A substantial microstructural evolution after the ARB process can be observed. According to the color orientation map key, IC and R samples showed preferred orientations to the [001] and [101] directions, the A sample to the [111], and the RA and AR samples to more complex orientations. The IC and R (Fig. 2a,b) samples showed some of their crystals with Fig. 2 eEBSD IPF micrographs in the normal direction (ND) for a) IC, b) R, c) A, d) RA, and e) AR samples and f) orientation map key. Deformation bands were indicated by white solid lines. Table 1 eSamples dimensions and employed parameters for bending test. Sample Thickness/mm Width/mm Length/mm Span between supports/mm Diameter of punch and supports/mm IC 1.0 16.0 115.0 100.0 5.0 R 1.0 16.0 115.0 100.0 5.0 A 1.0 10.0 60.0 50.0 5.0 RA 1.0 10.0 35.0 25.0 2.5 AR 1.0 10.0 35.0 25.0 2.5 journal of materials research and technology 2022;18:1281e12941284 <100>parallel to the ND, i.e., in the cube texture typically obtained from recrystallization processes as the homogenization applied to the IC sample [33]. This suggests that the deformation induced by 1 RCS pass was not enough to cause a significant microstructural evolution. The visible lower grain refinement supports the previous statement in the R sample compared to the A, RA, and AR. This was totally expected due to the largest "ε" applied in the overall sample by ARB (ε~0.8) compared to that of the RCS process (0.003 <ε<0.808) [17,29]. From Fig. 2c, the high crystals density, parallel to the ND and oriented to <111>in the sample A is similar to the reported for the AA7075 processed by one hot-ARB pass [14]. This coppertype texture can be expected for rolled high stacking fault energy (SFE) materials [34], as Al with an SFE of 200 mJ m-2 [35]. This copper-type texture has been related to the dominant cross slip deformation mechanism in high-SFE FCC metals [34,36]. From the combination of deformation techniques, more complex textures were obtained. Furthermore, the micrographs of Fig. 2 display a severe grain refinement, especially when the ARB process is applied (samples A, RA, and AR). As a result of the higher equivalent strain applied with the ARB to the AA7075, deformation bands were observed in samples A, RA, and AR. Similar coarse deformation bands have been reported in the AA7075 under equivalent strain by equal channel angular pressing (ECAP) with a 120 die angular channel [34]. As in the RA and AR samples (Fig. 2d,e), the deformation bands in the AA7075 subjected to ECAP showed no well-defined angles when the deformation increased [37]. The creation of deformation bands with the ARB process might encourage the grain sub-division and provide nucleation sites for new forming grains in Al alloys when further deformation is applied [37,38]. Figure 3 shows the grain size histograms weighted by area for the IC, R, A, RA, AR samples to analyze the grain refinement that occurred after every deformation route Compared to the average grain size of the IC sample (126 mm, Fig. 3a), the order from larger to lower grain refinement produced by the four routes was AR (1.2 mm, Fig. 3e) >A (3.2 mm, Fig. 3c) >RA (3.7 mm, Fig. 3d) >R (83.1 mm, Fig. 3b). The obtained grain refinement by 1 RCS pass in the AA7075 was similar to the obtained in AA6061 processed under same conditions [17]. However, the grain refinement in the A sample Fig. 3 eGrain size histograms weighted by area for a) IC, b) R, c) A, d) RA, and e) AR samples. journal of materials research and technology 2022;18:1281e1294 1285 was lower than the reported in the literature for AA7075 processed by 1 ARB pass [14], which reached a grain size average of 440 nm. This difference could be related to the higher εper pass (~1.1) reported in the literature [14] compared to that applied in this work (~0.8). Furthermore, the εfor the combination of RCS and ARB in the samples RA and AR is of ~1.0 for the less deformed zones to ~1.6 for the most deformed zones. Compared with the grain size reduction of about 98.9% (considering the final grain length) after two ECAP passes (ε~2.0) in the AA7075 [39], the grain size reduction of 97.0 and 99.0% for the RA and AR samples is similar. This suggests that the heterogeneous nature of the deformation applied by the RCS process might not be so significant in terms of grain refinement. It is noteworthy that the grain size distribution of the IC and R samples are unimodal and nearly symmetrical. However, the distribution profiles are unimodal and asymmetrical with right-skewed distributions in samples A, RA, and AR. Besides, a large percentage of grains in the samples where the ARB process was applied were below the sub-micrometric range (1 mm). It is also remarkable that the coexistence between sub-micrometric and micrometric grain sizes in all samples, especially in A, RA, and AR, were almost homogeneous throughout the samples. The finest grains are distributed randomly through every microstructure without forming colonies or clusters. A bigger grain size average in the RA sample compared to the AR was also observed. This could be related to the probable dynamic recovery occurrence due to the process temperature employed for ARB. The RA sample received a stimulus (temperature) on an already high-dense defects structure, increasing the probability of partialdynamic recovery. The occurrence of dynamic recovery in AA7075 processed under similar conditions (warm ARB process at ~350 C) has been reported before [14]. On the other hand, the final microstructure of the AR sample retained the effect of the last deformation step. Figure 4 shows the correlated misorientation histograms, uncorrelated misorientation profiles (red line), and the distribution of grain fractions for certain ranges of misorientation of the IC, R, A, RA, and AR samples. The uncorrelated profiles (or texture derivatives profiles) do not assume a spatial correlation between pixels, i.e., they account for all possible misorientations, including those between points that are not adjacent to each other (even between different grains). These profiles show the effects of transgranular strain, such as grain rotations or the formation of new grains. The correlated histograms result from the angle measurements between contiguous pixels, resulting in a high density of misorientation values lower than 5. Considering that the largest fraction of the area of the samples belongs to the interior of grains and not to the borders, the histograms were plotted since 5of misorientation. The correlated and uncorrelated profiles of the IC sample have similar tendencies, indicating that within the grains and in their neighborhood, there is a similar misorientation. This means that the IC sample is practically free of substructures or lineal defects that could noticeably vary the misorientation. The correlated and uncorrelated profiles also showed a large similarity on the R sample, which indicates again that the microstructural evolution until one RCS pass is not enough to alter the crystalline domains of the sample significantly. This is congruent with the low grain refinement obtained on the R sample. Nonetheless, after the AA7075 was subjected to the ARB process, the differences between both misorientation profiles became clearer. This could be an indication of the presence of subgrains, resulting from the polygonization process that controls the substructures or from twins formation. However, considering that twinning is rarely observed in aluminum due to its high stacking fault energy [40], it can be considered that these misorientation profiles differences are related to polygonization. The above can be understood as a substantial difference in the misorientation of the individual grains and the whole sample, i.e., intra- and inter-granular strain, which in turn could be linked to the grain size distributions. The grain size histograms showed ranges from submicrometric to micrometric on the A, RA, and AR samples, indicating that, while some dislocations have already formed subgrains, several others are being continuously accumulated. From the distribution of misorientation fraction in all samples illustrated in Fig. 4f, the IC sample showed 90.2% of misorientation boundaries greater than 15, i.e., high angle grain borders (HAGB). The high density of HAGBs is consistent with the micrometric and stress-relieved microstructure resulting from the homogenization heat treatment. Despite the grain refinement shown from the grain size histograms, the R sample presents more than 90% of HAGBs. This indicates that up to one RCS pass, the formation of substructures does not occur in high density. On the other hand, when the ARB process was applied (A, RA, and AR samples), less than 50% of borders were considered HAGBs, agreeing with the largest grain refinement promoted by ARB. The increment of low angle grain boundaries (LAGBs) i.e., boundaries with misorientations below 15, after applying the ARB process is a clear indication of the subgrain formation [13], which is also in agreement with the differences between correlated and uncorrelated profiles. The presence of HAGBs in the A, RA, and AR samples, is a positive indicator of ductility without a high sacrifice of mechanical resistance in various alloys [41,42]. This phenomenon has been explained in terms of the accumulation of linear defects, leading to polygonization and new LAGBs. Such new LAGBs will absorb dislocations and later become HAGBs [43,44], decreasing the dislocations density and allowing ductility in the material. Figure 5 shows the IPF in the normal direction (ND) and representations of the high-density oriented crystals for the IC, R, A, RA, and AR samples. Compared to the IC sample (Fig. 5a), the higher dense crystals positions mainly oriented to the <001>and <011>directions in the R sample are almost similar (Fig. 5b). This is congruent with the low grain refinement, and the similarity between correlated and uncorrelated profiles of IC and R observed in Fig. 4. After applying the ARB process, a high density of crystals rotated to different positions. The A sample is characterized by the highest density of preferred oriented crystals on the <111>direction that is parallel to the ND of the sample (Fig. 5c). Otherwise, the largest density of crystals on the RA sample is oriented to the <-3 7 11>direction (Fig. 5d), while a high density of crystals is oriented towards the <-1 1 2>and <-1 1 7>directions (Fig. 5e) in the AR sample. The evolution of crystallographic texture journal of materials research and technology 2022;18:1281e12941286 when the ARB process is apply (A, RA and AR samples) agrees with the observation of deformation bands (Fig. 2), which origins from crystallographic rotation occurrence [38,45]. It is worth mentioning that the texture intensity decreased with the applied strain. The previously explained differences between grain refinement and texture evolution on the four different samples imply that each process has a different effect on the current AA7075. This means that the order and nature of the applied strain alter the microstructural result. This could be due to the different slip systems that were activated by each deformation route. Such slip systems depend on the material's prior stress state, the Schmid factor associated with each crystallographic plane [46,47], and the strain restrictions (for instance, ARB is a plane strain process). The larger the Schmid factor the higher the shear stresses acting on a given slip system, and therefore a greater facility to deform the grain [48]. As the behavior of the grains located several atomic layers below is expected to be different from that on the surface, the previous phenomenon is representative of the surface grains on the material [46]. Therefore, the activation of different slip systems and its dependence on the associated Schmid factor is feasible for the present work in which the zone analyzed by EBSD was superficial. Figure 6 shows the peak broadening by the differences of the full width at half maximum for the IC, A, R, RA, and AR samples. The profile of the Al-(420) peak on the IC sample observed in Fig. 6a shows the doublet of K-a 1 and K-a 2 contributions, while the convolution of both peaks is not visible for all the deformed samples. This suggested that the grain refinement could be reached down to the sub-micrometric sizes. Considering the typical range of sensibility of the XRD technique, the peak broadening in all the deformed samples (Fig. 6b) is indicative of the formation of nano-metric grains. It Fig. 4 eCorrelated misorientation histograms and uncorrelated misorientation profiles for a) IC, b) R, c) A, d) RA, and e) AR samples, and f) distribution of correlated misorientation angles for the same samples. journal of materials research and technology 2022;18:1281e1294 1287 was also observed the peak shifting from the IC Al-(420) peak for the samples after the ARB process (Fig. 6a). This could be related to the increment of macro-strains in such samples, being congruent with the larger grain refinement (Fig. 3) observed in A, RA, and AR samples in comparison with the R sample. Along with the high grain refinement, the formation of its crystallographic texture, and the suggestion of larger macro-strains, the ARB process causes more significant microstructural changes than the RCS process in the present AA7075. 3.2. Mechanical behavior Tensile test, microhardness, and three-point bending test measurements after applying each deformation route are shown in Fig. 7. The UTS values for the IC, R, A, RA, and AR Fig. 5 eIPFs in the normal direction and position of high-density oriented crystals for a) IC, b) R, c) A, d) RA, and e) AR samples. journal of materials research and technology 2022;18:1281e12941288 samples were 250.6, 217.3, 301.8, 253.7, and 293.2 MPa, respectively (Fig. 7a). The UTS between the A and the AR condition are similar, which was congruent with the higher grain refinement shown in Fig. 3. However, the A condition showed a slightly higher strain hardening rate (Fig. 7b). This suggests a ductility improvement (necking delaying) due to dislocation accumulation in sample A [49]. The higher ductility in sample A was confirmed by a higher uniform elongation (UE) in Fig. 7c. The higher mechanical properties (UTS, YS, and UE) in the samples processed by ARB compared Fig. 7 eMechanical properties of all samples studied in this work: a,b,c) tensile test and d) microhardness, tensile test, and three-point bending tests. FE, UE, YS, HV, UTS, and UBS refer to final elongation, uniform elongation, yield strength, Vickers microhardness, ultimate tensile strength, and ultimate bending strength, respectively. Fig. 6 ePeak broadening for the processed samples by the four different deformation routes employed in this work in comparison with the initial condition sample: a) diffractogram of Al-(420) peak and b) full width at half maximum (FWHM) values for each sample. journal of materials research and technology 2022;18:1281e1294 1289