Full text
NUMERICAL SIMULATION OF FATIGUE PROCESSES. APPLICATION TO STEEL AND COMPOSITE STRUCTURES. Lucia Gratiela Barbu Escola T`ecnica Superior d’Enginyers de Camins, Canals i Ports de Barcelona Universitat Polit`ecnica de Catalunya PhD Thesis Structural Analysis Programme Advisors: Prof. Sergio Oller Prof. Xavier Mart´ınez Prof. Alex H. Barbat December 2015
Numerical simulation of fatigue processes. Application to steel and composite structures. December 2015 Universitat Polit`ecnica de Catalunya c/ Jordi Girona 1-3, 08034 Barcelona www.upc.edu
Acta de calificación de tesis doctoral Curso académico: Nombre y apellidos Programa de doctorado Unidad estructural responsable del programa Resolución del Tribunal Reunido el Tribunal designado a tal efecto, el doctorando / la doctoranda expone el tema de la su tesis doctoral titulada ____________________________________________________________________________________ __________________________________________________________________________________________. Acabada la lectura y después de dar respuesta a las cuestiones formuladas por los miembros titulares del tribunal, éste otorga la calificación: NO APTO APROBADO NOTABLE SOBRESALIENTE (Nombre, apellidos y firma) Presidente/a (Nombre, apellidos y firma) Secretario/a (Nombre, apellidos y firma) Vocal (Nombre, apellidos y firma) Vocal (Nombre, apellidos y firma) Vocal ______________________, _______ de __________________ de _______________ El resultado del escrutinio de los votos emitidos por los miembros titulares del tribunal, efectuado por la Escuela de Doctorado, a instancia de la Comisión de Doctorado de la UPC, otorga la MENCIÓN CUM LAUDE: SÍ NO (Nombre, apellidos y firma) Presidente de la Comisión Permanente de la Escuela de Doctorado (Nombre, apellidos y firma) Secretario de la Comisión Permanente de la Escuela de Doctorado Barcelona a _______ de ____________________ de __________
Abstract The present thesis aims at advancing an innovative computational methodology that simulates steel and composite material fracture under cyclic loading following a phenomenological approach, with calibration from both small scale and large scale testing. This work addresses fatigue processes ranging from high cycle to ultra-low-cycle fatigue. An assessment of the current state of the art is done for all the different fatigue types. Following, for ultra-low cycle fatigue a new constitutive law is proposed and validated with experimental results obtained on small scale samples. Industrial applications are shown for a large diameter straight pipe under monotonic loading conditions and for a bent pipe under cyclic loading. Emphasis is made on the capacity of the model to represent different failure modes depending on the loading conditions. The research regarding this part has been used in the frame of the European Project: Ultra low cycle fatigue of steel under cyclic high-strain loading conditions (ULCF). Regarding high cycle fatigue, a classic damage model is presented in combination with an automatic load advancing strategy that saves computational time when dealing with load histories of millions of cycles. Numerical examples are shown in order to demonstrate the capabilities of the advancing strategy and a validation of the model is done on small scale samples. A new constitutive model is presented for Low Cycle Fatigue that uses the classic plasticity and damage theories and simultaneously integrates both processes in the softening regime. The capabilities of the model are shown in numerical examples. Finally, the high cycle fatigue damage model is applied to the constituents of a composite material and the structural behaviour is obtained by means of the v
serial/parallel rule of mixtures. Validation of the constitutive formulation is done on pultruded glass fiber reinforced polymer profiles.
Resumen La presente tesis propone una metodolog´ıa innovadora para la simulaci´on num´erica de la rotura de materiales met´alicos y compuestos sometidos a cargas c´ıclicas. El enfoque es fenomenol´ogico y la formulaci´on se calibra con resultados experimentales obtenidos en espec´ımenes a peque˜na escala y con experimentos a gran escala. Este trabajo abarca procesos de fatiga desde alto n´umero de ciclos hasta muy bajo n´umero de ciclos. Una evaluaci´on del estado del arte hasta el momento se ha llevado a cabo para los diferentes tipos de fatiga. A continuaci´on, se propone una nueva ley constitutiva para la fatiga de muy bajo n´umero de ciclos y se presenta la validaci´on con resultados experimentales obtenidos en espec´ımenes a escala peque˜na. El modelo constitutivo se ha probado en dos aplicaciones industriales: una tuber´ıa de gran di´ametro bajo condiciones de carga mon´otonas y una tuber´ıa doblada a un ´angulo de 90 grados sometida a cargas c´ıclicas. Se ha enfatizado la capacidad del modelo de reproducir diferentes modos de rotura dependiendo de las condiciones de carga. El trabajo referente a este modelo se ha usado en el marco del proyecto europeo: Fatiga de muy bajo n´umero de ciclos del acero bajo grandes deformaciones c´ıclicas. Respecto a la fatiga de alto n´umero de ciclos, se presenta un modelo cl´asico de da˜no combinado con una estrategia automatizada de avance en la carga por n´umero de ciclos. La estrategia conduce a un ahorro en tiempo de computaci´on cuando se aplican millones de ciclos de carga. Las capacidades y particularidades de la estrategia de avance en la carga se ense˜nan en una serie de ejemplos num´ericos. El modelo se valida con resultados experimentales obtenidos en espec´ımenes a peque˜na escala. vii
Un nuevo modelo constitutivo se presenta para la fatiga de bajo n´umero de ciclos que se basa en las teor´ıas b´asicas de plasticidad y da˜no y que integra simult´aneamente las ecuaciones de ambos procesos en el r´egimen de ablandamiento. Las capacidades del modelo se ense˜nan a trav´es de ejemplos num´ericos. Finalmente, se estudia la aplicaci´on del modelo de da˜no para fatiga de alto n´umero de ciclos en los componentes de materiales compuestos. El comportamiento estructural del material compuesto se obtiene a trav´es de la teor´ıa de mezclas serie/paralelo. La formulaci´on se valida con resultados experimentales obtenidos en perfiles de GFRP.
Acknowledgements I would like to thank all the people that in some way have helped me to complete my PhD. I would like to express my gratitude to my PhD advisors, Sergio Oller, Xavier Martinez and ´ Alex Barbat, for their faith in me and for their dedication during these years. You have contributed greatly in shaping my understanding and my knowledge both at a scientific and at a personal level. I consider myself immensely fortunate to have had the opportunity to learn from you. I would like to thank the Spanish Minisitry of Education for the FPU Grant I have received during my PhD years and the European Union for the funding given to the ”Ultra low cycle fatigue under high-strain loading conditions” project. Also, my PhD advisors for giving me the opportunity to participate in this project. The knowledge generated from the project constitutes an important part of this work. I would like to express my gratitude to CIMNE at an institutional level for all the opportunities it has offered me in attending international conferences and for participating and assisting at many high-quality lectures held in its premises. I have found here a family away from home. Thank you Kike and Miguel for always being there when I had troubles with GiD and, together with Salva and Guillermo, for all the conversations we enjoyed daily at lunch. It has been very refreshing and thought provoking to share ideas and opinions with you and together we have made many great memories. I would like to give a special thank you to ´ Alex, Manuel and Stefano, my office colleagues, who have made my day to day entertaining during these years. Also, ix
6.3.2 Finite element model . . . . . . . . . . . . . . . . . . . . . . 170 6.3.3 Experimental program . . . . . . . . . . . . . . . . . . . . . 171 6.3.4 Results and discussion . . . . . . . . . . . . . . . . . . . . . 173 7 Conclusions 191 7.1 Futurework...............................196 7.2 Innovative contributions . . . . . . . . . . . . . . . . . . . . . . . . 197 7.3 Publications derived from this work and participation in projects . 197 References 201
List of Figures 3.1 Translation of the yield surface result of kinematic hardening . . . 30 3.2 Expansion of the yield surface result of isotropic hardening . . . . 31 3.3 Evolution of the equivalent stress . . . . . . . . . . . . . . . . . . . 35 3.4 Representation of the volumetric fracture energy of a metallic material................................... 36 3.5 Dimensions, in millimeters, of the SP specimen . . . . . . . . . . . 40 3.6 Dimensions, in millimeters, of the OH specimen . . . . . . . . . . . 40 3.7 Mesh defined for the SP and OH numerical models. The SP model has marked, with red dots, the points used to calculate the equivalent strain applied. . . . . . . . . . . . . . . . . . . . . . . . . . . 41 3.8 Stress-strain graphs for the SP sample with an applied deformation rangeof2.75% ............................. 44 3.9 Values of κpfor the SP sample with an applied deformation range of 2.75%, when applying the maximum tensile and compression strain before ULCF failure. Deformation is magnified by 20. . . . . 44 3.10 Evolution of the stress strain graph for different cycles of the SP numericalanalysis ........................... 45 3.11 Stress-strain graphs for the SP sample with an applied deformation rangeof4.00% ............................. 46 3.12 Stress-strain graphs for the OH sample with an applied deformationrangeof1.20%........................... 47 3.13 ULCF failure prediction for SP samples . . . . . . . . . . . . . . . 48 3.14 ULCF failure prediction for OH samples . . . . . . . . . . . . . . . 49 3.15 Evolution of the equivalent plastic stress . . . . . . . . . . . . . . . 50 3.16 Representation of the volumetric fracture energy of a metallic material................................... 51 3.17 Geometry of the specimen used for calibration . . . . . . . . . . . . 54 3.18 Comparison between the stress strain curve for the uniaxial monotonic tensile test and the points chosen for the numerical model . . 55 3.19 Monotonic stressstrain curve. Numerical vs. experimental. . . . . 56 xvii
3.20 Stress-strain hysteresis loop for ∆ε=8%. Numerical vs. experimental. 57 3.21 Stress-strain hysteresis loop for ∆ε=5%. Numerical vs. experimental. 58 3.22 Stress-strain hysteresis loop for ∆ε=2%. Numerical vs. experimental. 58 3.23 Distribution of the normalized plastic dissipation at total fracture . 59 3.24 Comparison between numerical and experimental fatigue life for different strain amplitudes when calibrating with ∆ε=5% . . . . . 59 3.25 Overview of the general dimensions of the specimen . . . . . . . . 62 3.26 Specimen SP1-SP2 (X60, 90◦)..................... 63 3.27Modelgeometry............................. 64 3.28 Mesh of hexahedral quadratic elements . . . . . . . . . . . . . . . . 65 3.29 Evolution of the applied displacement in the experiment . . . . . . 67 3.30 Boundary condition for the large scale model . . . . . . . . . . . . 68 3.31 Force-displacement curve. Experimental vs. numerical . . . . . . . 69 3.32 Distribution of the plastic internal variable of the model on the deformedshape(x2) .......................... 69 3.33 Distribution of the total strain in the three model axes on the deformed shape of the model (x2) . . . . . . . . . . . . . . . . . . . 70 3.34 Experimental failure (Schaffrath et al. [104]) . . . . . . . . . . . . . 70 3.35 Geometry of the model with the initially imposed buckle . . . . . . 71 3.36 Distribution of the plastic internal variable of the model on the deformedshape............................. 71 3.37 Evolution of the maximum dissipation in the two areas of interest 72 3.38 Specimen drawing for X52 full scale testing . . . . . . . . . . . . . 74 3.39 Sections of interest in the mechanization of the straight pipe . . . . 75 3.40 Model geometry in GiD . . . . . . . . . . . . . . . . . . . . . . . . 75 3.41 Mesh of hexahedral quadratic elements . . . . . . . . . . . . . . . . 76 3.42 Boundary conditions for the straight pipe . . . . . . . . . . . . . . 76 3.43 Loading scenarios for the straight pipe . . . . . . . . . . . . . . . . 77 3.44 Stress-strain curves for the monotonic case . . . . . . . . . . . . . . 78 3.45 Stress-strain hysteresis loop for ∆ε=4%. Numerical vs. experimental. 79 3.46 Comparison between the numerical and experimental results for theSPEC1case ............................ 80 3.47 View of the deformed shape at the end of the analysis with an indication of the most damaged material point in the geometry . . 81 3.48 View of the pipe burst as recorded by the experiment for the SPEC1test ............................... 82 3.49 View of the pipe burst as recorded by the experiment for the SPEC2test ............................... 82 3.50 Evolution of the κpvariable when applying internal pressure in constant steps of 2.7 bars . . . . . . . . . . . . . . . . . . . . . . . 85
3.51 Comparison between the numerical and experimental results for theSPEC2case ............................ 85 3.52 View of the deformed shape for the SPEC 2 case . . . . . . . . . . 86 3.53 Seismic-type load applied . . . . . . . . . . . . . . . . . . . . . . . 87 3.54 Material stress-strain response . . . . . . . . . . . . . . . . . . . . 88 3.55 Seismic-type load applied: ten seismic-type cycles . . . . . . . . . . 89 3.56 Material stress-strain response after ten seismic-type cycles . . . . 89 4.1 a: Stress evolution at a single point; b: S−N(W¨ohler’s) Curves . 97 4.2 Schematic representation of the evolution of the residual strength with the applied load and number of cycles . . . . . . . . . . . . . 97 4.3 Proposed S−Ncurves for different values of R= (Smin/Smax). [100]................................... 99 4.4 Flow chart for the stepwise advancing algorithm . . . . . . . . . . 105 4.5 Applied displacement for load case S1................109 4.6 Parameters of interest for the fatigue analysis under load S1. . . . 110 4.7 Parameters of interest for the fatigue analysis under load S1in the nonlinearzone .............................111 4.8 Stress-Strain at integration point for load S1............112 4.9 Evolution of the damage internal variable with the number of cycles113 4.10 Parameters of interest for the fatigue analysis under load S2. . . . 115 4.11 Stress-Strain at integration point for load S2............116 4.12 Parameters of interest for the fatigue analysis under loads S1+S2. 118 4.13 Stress-Strain at integration point for loads S1+S2..........119 4.14 Parameters of interest for the fatigue analysis under loads S2+S1. 120 4.15 Stress-Strain at integration point for loads S2+S1..........121 4.16 Parameters of interest for the fatigue analysis under load combination 1 in 3d representation . . . . . . . . . . . . . . . . . . . . . . 122 4.17 Parameters of interest for the fatigue analysis under load combination 2 in 3d representation . . . . . . . . . . . . . . . . . . . . . . 123 4.18 Parameters of interest for the fatigue analysis under load S2in 3d representation..............................124 4.19 Comparison between the stress-strain curves at the integration point for different load combinations . . . . . . . . . . . . . . . . . 125 4.20 Comparison between the stress evolution at the integration point for different load combinations in 3d representation . . . . . . . . . 126 4.21 Shape and dimension of ultrasonic fatigue specimen as given by Marinesetal.[68]............................128 4.22 Finite element mesh of linear hexahedral elements . . . . . . . . . 129 4.23 Boundary and loading conditions for the analysed geometry . . . . 130
4.24 Fatigue S-N curve of HSLA steel D38MSV5S with R = -1, 20 kHz and30kHz[68] .............................131 4.25 S−Ncurve for HSLA steel D38MSV5S. Experimental vs. numerical.133 4.26 Parameters of interest for the fatigue analysis of D38MSV5S specimen at the first integration point that fractures completely . . . 134 4.27 Zoom on fatigue parameters of interest in the nonlinear zone (post S−Ncurve).Dots indicate the analysis steps at which damage evolution is presented in figure 4.28 . . . . . . . . . . . . . . . . . . 135 4.28 Damage evolution for a maximum induced stress of 350MPa and R=-1..................................136 4.29 Deformed shape (x 200) at the last maximum stress before rupture and at the last minimum stress, when rupture occurs . . . . . . . . 137 5.1 Evolution of the equivalent stress . . . . . . . . . . . . . . . . . . . 148 5.2 Experimental stress-strain curve for X52 steel [95] . . . . . . . . . 149 5.3 Schematic representation of the energy distribution law in softening over the entire fatigue domain (X axis not scaled) . . . . . . . 151 5.4 Stress evolution for the plastic damage model as compared to the classical plasticity and damage models . . . . . . . . . . . . . . . . 153 5.5 Stress – strain curve obtained with the plastic damage model . . . 156 5.6 Evolution of the internal variables of the plastic damage model . . 157 5.7 Evolution of the stressstrain curve. Comparison between the experimental behavior and the numerical one when using plasticity equations and plastic damage equations at cycles 1-59 . . . . . . . 158 5.8 Evolution of the stressstrain curve. Comparison between the experimental behavior and the numerical one when using plasticity equations and plastic damage equations at cycle 69 . . . . . . . . . 159 5.9 Evolution of the stressstrain curve. Comparison between the experimental behavior and the numerical one when using plasticity equations and plastic damage equations at cycle 79 . . . . . . . . . 160 5.10 Evolution of the stressstrain curve. Comparison between the experimental behavior and the numerical one when using plasticity equations and plastic damage equations at cycle 89 . . . . . . . . . 161 5.11 Evolution of the stressstrain curve. Comparison between the experimental behavior and the numerical one when using plasticity equations and plastic damage equations at the last cycle of the numerical simulation . . . . . . . . . . . . . . . . . . . . . . . . . . 162 6.1 Experiment specimen with strain and temperature gages [51] . . . 171 6.2 Finite element mesh of quadratic hexahedral elements . . . . . . . 172
6.3 Boundary and loading conditions for the analysed geometry . . . . 172 6.4 Initial stiffness for the static case. Comparison between experimental and numerical values. . . . . . . . . . . . . . . . . . . . . . 175 6.5 Static (above) and fatigue (below) experimental failure modes . . . 176 6.6 Distribution of the damage internal variable for the composite at differenttimesteps...........................180 6.7 Distribution of the damage parameter in the glass fibers at differenttimesteps..............................181 6.8 Distribution of the damage parameter in the isophtalic matrix at differenttimesteps...........................182 6.9 Composite damage distribution in the last step of the analysis on the deformed specimen shape (20x) . . . . . . . . . . . . . . . . . . 183 6.10 Distribution of the longitudinal strain of the composite in the last step of the analysis on the deformed specimen shape (20x) . . . . . 183 6.11 Evolution of the curves of interest for the fatigue model at the first integration point where damage initiates in the model . . . . . . . 184 6.12 Evolution of the damage internal variables at the first integration point where damage initiates in the model . . . . . . . . . . . . . . 185 6.13 Evolution of the matrix stress-strain at the first integration point where damage initiates in the model . . . . . . . . . . . . . . . . . 186 6.14 Evolution of the curves of interest for the fatigue model in the fiber of one of the integration points situated at the location of the strain gauge in the experiment . . . . . . . . . . . . . . . . . . 187 6.15 Evolution of the curves of interest for the fatigue model in the matrix of one of the integration points situated at the location of the strain gauge in the experiment . . . . . . . . . . . . . . . . . . 188 6.16 Comparison between the numerical and experimental S-N curves . 189
List of Tables 3.1 Mechanical properties of steel X52 . . . . . . . . . . . . . . . . . . 42 3.2 Polynomial constants used to describe the hardening region of X52 material................................. 42 3.3 Polynomial coefficients for the X60 material as obtained from curve fitting .................................. 57 3.4 Material parameters for the numerical model for an X60 steel . . . 60 3.5 Loading sequence for SP2 specimen . . . . . . . . . . . . . . . . . . 66 3.6 Distribution of the maximum dissipation normalized to the fracture energy on the deformed shape of the model (x5) . . . . . . . . 73 3.7 Wall thickness and outer diameter at different points of each sectionofthepipe............................. 83 3.8 Polynomial coefficients for the X52 material as obtained from curve fitting .................................. 84 3.9 Material parameters for the numerical model for an X52 steel . . . 84 4.1 Characterization of the tensional state induced by the single load S1108 4.2 Computational time for case S1depending on the number of cycles chosenasstep..............................114 4.3 Characterization of the tensional state induced by the single load S2114 4.4 Fatigue life for loads S1and S2and their combination . . . . . . . 117 4.5 Characterization of the combination cases analysed (monotonic andcyclic)................................117 4.6 Material properties of HSLA steel, D38MSV5S . . . . . . . . . . . 127 4.7 Fatigue life as resulting from the numerical simulation. Same stress levels and reversion factor as [68]. (20 kHz) . . . . . . . . . . . . . 132 5.1 Material characteristics . . . . . . . . . . . . . . . . . . . . . . . . 152 5.2 Mechanical properties of steel . . . . . . . . . . . . . . . . . . . . . 155 6.1 Fiber architecture and fractions by volume and weight of the pultruded profiles used [51] . . . . . . . . . . . . . . . . . . . . . . . . 170 xxiii
6.2 Material properties used in the numerical simulations . . . . . . . 173 6.3 Composite properties as recorded from the static experimental tests[51] .................................173 6.4 Overview of experimental results [51] . . . . . . . . . . . . . . . . . 174 6.5 Overview of numerical and experimental results . . . . . . . . . . . 179
Chapter 1 Introduction, objectives and motivation 1.1 Antecedents The present thesis aims at advancing an innovative computational methodology that simulates metal and composite material fracture under cyclic loading following a phenomenological approach, with calibration from both small scale and large scale testing. Time varying cyclic loads produce failure of structural parts for values of stress lower than those obtained in static tests. This phenomenon is called fatigue and it is defined more generally in the ASTM E1823 standard [29] as: the process of permanent, progressive and localized structural change which occurs to a material point subjected to strains and stresses of variable amplitudes which produces cracks which lead to total failure after a certain number of cycles. 1
8Chapter 2. State of the art While there is a general agreement that for failures in the range of 106to 108 cycles the structure has failed in the high cycle fatigue range, there is not such agreement in defining the limits for LCF and ULCF. Authors such as Kanvinde and Deierlein [45] consider that LCF is found between 100 s and 1000 s cycles and that ULCF is in the range of 10 to 20 cycles; and other authors, such as Xue [125], put these limits in 104for LCF and 100 for ULCF. However, despite these discrepancies, there is a general agreement that plastic behavior of the material plays an important role in the failure due to LCF or ULCF [18]. 2.1 Coffin −Manson law According to the literature review made by Yao and Munse in [127], first attempts to characterize LCF and ULCF can be attributed to Kommers who, in 1912, conducted several tests on a cantilever specimen subjected to cyclic bending. After these tests he reached the conclusion that the magnitude of deflection plays an important role in low cycle fatigue. However, main efforts to characterize the parameters driving LCF and ULCF are not found until 1950s, when numerous experimental programs where carried out to calibrate the material constants for various metals. A large amount of work is documented from this period. The experimental data is usually plotted on a loglog scale with the abscissa representing the number of life cycles and the ordinate the plastic strain amplitude. This graph is known as the ∆εp−Ncurve. Following this approach, probably the most know, and most widely used, procedure to predict material failure under LCF and ULCF is the Coffin −Manson law [18], [112] and [53]: ∆εp·Nα=C(2.1) ∆εpbeing the plastic strain range in the material, Nthe number of cycles that can be applied before ULCF and LCF failure, and αand Cmaterial constants. From this first equation proposed by Coffin and Manson, several authors have provided their own law in order to improve the accuracy on the predicted cycles before failure, especially in the ULCF regime. For instance, Xue [125] observed, from experimental results, that the law did not fit well in the range of very low life cycles, less than 100, so he proposed a new exponential damage rule that improved this accuracy. Kuroda [53] also provided a modification on the original CoffinManson law in order to predict the failure below 100 cycles. In this case the model is based on the accumulation of damage due to three different effects: tensile straining, cyclic straining and crack propagation.
2.2. HCF models 9 The approach used by Tateishi et al. [116] to simulate LCF failure is also interesting. These authors use Miners rule to couple the effect of high cycle fatigue with the effect of low cycle fatigue, by adding a ductile damage term. This last term depends on the yield strain of the material, the rupture strain and the strain that is applied in a given cycle. 2.2 HCF models Regarding the high cycle fatigue (HCF) phenomenon, it is known that the type of fracture involved at macroscale level occurs with little or no plastic deformation. Therefore, HCF does not introduce macroscopic plastic strain, but it introduces porosity [105]. These are the reasons that have led to describe this failure mode by means of damage models. These can be categorized into five groups: damage curve approach, crack growthbased approach, life curve modification approach, energy based damage theories and continuum damage mechanics (CDM) approaches [31]. However, in spite of the great number of models proposed in the HCF field, there is not yet a universally accepted one. In particular, the CDM approach is based on the original concepts of Kachanov [44], [43] for treating creep damage problems. The posterior work of Chaboche [20], [19], Chaboche and Lemaitre [59], [58], Wang [121], Wang and Lou [122], Li et al. [60] and Oller et al. [100] established the CDM framework as a valid alternative to the fracture mechanics formulations in order to assess in a unified way both crack initiation and propagation. Furthermore, they enhanced the study of fatigue problems by recognizing that the theoretical structure of continuum mechanics, such as damage, is suitable for the study of nonlinear fatigue problems and that the mechanical effect known as fatigue produces a loss of material strength as a function of the number of cycles, load amplitude, reversion index, etc. Regarding fatigue life prediction, many different approaches have been proposed such as the early methods of stress-life approach and strain-life approach [40]. One of the most used models is based on the Palmgren-Miner linear damage law [92], [78]. However, such models do not recognize the effects of prior history of loading, or the load sequence on the subsequent life. Strain-life models, on the other hand, account for the local plasticity effects at stress concentrations regions [120]. Information is abundant in literature as there are many different crack initiation models [36], with a large number of empirical models proposed for the long crack growth prediction [39]. Despite the abundant information existent
10 Chapter 2. State of the art on fatigue constitutive models, no attention is given to load advancing strategies utilized in numerical simulations, where one of the objectives of this work resides. 2.3 Strain-based design method Given that ULCF is defined by cyclic loads which generate plastic effects, stress based design criteria for structures which are subjected to extreme loads do not yield good results. Therefore, advanced analysis and modelling of structures or components subjected to extreme loads is presently done using strain-based design criteria which are based on limit state design and displacement control load. The primary areas where strain based design is expected to be applicable, taking into account the current industrial application focus of the thesis, pipelines, are in design of reeled laying of offshore pipelines, in thermal design of arctic pipelines, in design of types of offshore pipe lay systems, in design and assessment of pipelines in areas with significant expected ground movement, and in HT/HP pipeline designs. Some pipelines may also have some applications of strain-based design where cyclic loadings cause occasional peak stresses above the pipe yield strength. Here, the cyclic lifetime assessment is improved by using strain ranges for the cycles, instead of stress ranges. However, the cyclic lifetime assessment needs further development and validation, mainly for LCF or ULCF load conditions. Some important drawbacks can be pointed out to the current state-of-the-art strain-based design [30]: •The current use of strain-based design has many project-specific components. This limits the ability of a cookbook approach where each step can be laid out as part of common design sequence to apply to all areas of pipe strain-based design. This situation would indicate that taking the current state-of-the-art methods and creating a code or standard would be ineffective at covering the range of needs for future pipeline designs. •Past design practices have asked designers to determine whether a particular loading was load-controlled or displacement-controlled without any other possible choices. Designers today need to recognize that there are a range of intermediate cases between full-load control and full displacement control. The behaviour of the pipe, particularly its buckling resistance, can
2.3. Strain-based design method 11 change significantly depending upon the designers choice of the appropriate intermediate case for design. Guidance on local buckling compression resistance of pipelines appears to be well founded when using the critical strain. The additional strains that can be achieved under partly or fully displacement controlled loading should be more thoroughly studied to allow more specific guidance. •The methods for assessing tensile failure resistance of pipelines by Engineering Critical Analysis (ECA) become fewer when the plastic strain exceeds 0.5% and fewer still as the strain increases to 2% or more. More validations trials are needed in the open literature to support the use of the few existing methods up to high axial strains. •Further study is needed on the effects of prior strain history on the resistance of pipeline materials to different failure modes. •Methods of assessing cycles of loading that include plastic strain are available. But the limited number of tests on which they are based may mean that these methods are conservative for many pipeline design situations to which they might be applied. Additional testing and analysis of cyclic behaviour of pipelines is needed to improve the method currently available. •Design of pipelines to resist ratcheting has become more important recently because of thermal cycle effects on high-temperature pipelines and flow lines. As for other types of cyclic loading, the current design methods are relatively conservative, but have been shifting to allow more cycles of plastic strain. Additional testing and assessment is needed in this area to improve the current methods. •Although some workable strain-based design methodology and the supporting engineering processes and models have been achieved and validated, some improvements and enhancements are needed, especially as we move to high pressure, high strength pipe and large-diameter pipelines [61]. Under cyclic action, the initial loss of strength can be produced by plastic behaviour (or other non-linear phenomena) coupled with the loss of strength by fatigue, which also conduces to the high reduction of the residual strength, causing a decrease of the residual life under very low number of cycles. The capturing of this life reduction is possible by means of a new constitutive model based on the residual strength of the solids under fatigue loads coupled with other nonlinear models (ex: plasticity, ductile damage).
12 Chapter 2. State of the art Plastic design is applied in two areas: for structures subjected to static loads and for structures subjected to loads varying with time. Extreme transient loading conditions involving widespread yielding may lead to monotonic ductile fractures or to fatigue failures after a very short number of load fluctuations (Nf in the order of 102cycles). The latter failure mechanism is often called ULCF to distinguish it from the well-known low-cycle fatigue process (Nf in the order of 103cycles or greater) since it involves distinct micromechanisms, not fully understood and characterized until now. 2.4 Elastoplastic fracture mechanics and Engineering Critical Analysis methods Conventional elastoplastic fracture mechanics (EPFM), using parameters such as the J-Integral or the Crack Opening Displacement, has been very often applied to assess the ultimate failure loads under plastic conditions. However, this approach shows very important limitations, namely: •it requires the assumption of an initial flaw (cannot handle flaw-free details); •EPFM assumes small-scale (limited) yielding; •EPFM based approaches do not explicitly include effects of reversed cyclic loading, thus cannot be conveniently applied to situations of ULCF. Engineering Critical Analysis (ECA) is primarily used in strain-based design to set the allowable flaw size for inspection or to check that the material toughness is sufficient for a given flaw size. The methods are applied to both girth- and seam-welded areas based on the engineering understanding of brittle and ductile fracture and plastic collapse. ECA for strain-based design must use a rather high level of complexity. The assessment of flaws in areas of general plasticity was not the original domain of any of the standard assessment techniques and these have been extended to cover it by various modifications. Damage mechanics is frequently proposed as an alternative approach to EPFM to assess the macroscopic crack initiation. This thesis proposes developments of the Continuum Damage Mechanics (CDM) based approach to predict the ULCF under conditions of generalized plasticity.
2.5. Continuum Damage Mechanics method 13 2.5 Continuum Damage Mechanics method The CDM is an alternative to the Fracture Mechanics Approach, with important advantages, namely that it handles, in a unified way, both crack initiation and crack propagation. Failure in metals and alloys is a multiscale phenomenon, in general. Macroscopic rupture is the result of the irreversible processes that occur at smaller material length-scales. Both pre-existing and load generated micro/mesoscale flaws may grow reducing the nominal material resistance. Consequently, the conditions under which failure can occur should be evaluated based on meso/micromechanics considerations. In metals, all failure modes can be ascribed only to five micromechanisms and their combinations: cleavage, ductile fracture, creep, fatigue, and corrosion. For all of them, the reduction of the material load carrying capability is always associated to the appearance of irreversible strain, which may be either highly localized in the microstructure, as for cleavage, or spread across the entire geometry volume, as for ductile rupture or creep. In addition to global theories, such as fracture mechanics concepts, in the last two decades, micromechanical modelling has been proved to be a powerful approach to understand and predict failure in materials. The real advantage of micromechanics relies on the assumption that the model parameters are only material characteristics and do not depend on the geometry. Damage resulting from plastic deformation is mainly due to the formation of micro voids which initiate either as a result of fracturing or debonding from the ductile matrix, of inclusions such as carbides and sulphides. In pure metals, micro voids are nucleated at the grain triple points and along the grain boundary as a result of the incapacity of the microstructure to accommodate, in a congruent manner, the imposed displacement field. The growth of micro voids, under increasing strain level, progressively reduces the material capability to carry loads up to complete failure. A proper modelling of this micro mechanism at the mesoscale is the basis for the prediction of ductile failure in real life components and structures (i.e., the macroscale). Damage models can be grouped in three main categories: •Abrupt failure criteria •Porous solid plasticity •Continuum damage mechanics (CDM).
14 Chapter 2. State of the art In abrupt failure criteria, failure is predicted to occur when one external variable, that is uncoupled from other internal variables, reaches its critical value (e.g. Rice and Tracy critical cavity growth criterion). In porous solid plasticity, the effect of ductile damage (Gurson [35], Needleman and Tvergaard [80], hereafter GTN) is accounted for in the yield condition by a porosity term that progressively shrinks the yield surface. The GTN model, although extensively used is known to suffer from a number of limitations: •A large number of material parameters which makes difficult to evaluate possible mutual influence; •The material parameters are not physically based and cannot be directly measured for a material; •A poor geometry transferability of damage parameters which often requires a posteriori adjustments; •Damage softening introduces a length scale dependency, (mesh effect) [3]. In the last category, damage is assumed to be one of the internal constitutive variables that accounts for the effects on the material constitutive response induced by the irreversible processes that occurs in the material microstructure. Starting from the early work of Kachanov [43], the CDM framework for ductile damage was later developed by Lemaitre [57] and Chaboche [21]. In the last two decades, a number of CDM based formulations have been proposed. Also, these models show a number of limitations: •The proposed choice for the damage dissipation potential is, in many cases, specific of the particular material; •Damage evolution laws are often validated only with experimental data obtained under uniaxial stress. Therefore, the transferability of parameters to multiaxial stresses is not always demonstrated; •Similarly to the porosity models, also the CDM formulations are affected by mesh size effect due to damage softening. More recently CDM formulations have been proposed [17] which try to overcome the above limitations: the damage variable is uncoupled from plasticity, so
2.5. Continuum Damage Mechanics method 15 avoiding mesh size influence, and the damage evolution law take into account for nonlinear accumulation effects. All the cited approaches are based on the void growth and coalescence descriptions which, as already stated, strongly depend on stress triaxiality. Anyway, in the final phase of the fracture process two different mechanisms may compete, the internal necking of ligaments between voids, which is mainly influenced by medium-high values of the stress triaxiality, and the shear failure which is evident at low stress triaxiality, as described by Bao and Wierzbicki [7]. Experimental evidences of a different fracture behaviour at similar triaxiality level, but obtained from different geometrical conditions were early found by Clausing [23]. McClintock [76] also found that for many materials the equivalent plastic strain at failure is lower in torsion than in tension, even if the stress triaxiality in torsion is zero, which is not consistent with any of the hydrostatic pressure dependence (i.e. triaxiality) models described. A step forward with respect to the classical damage theories was proposed by Wierzbicki et al. [124] by introducing another normalized parameter - the deviatoric parameter, based on the third invariant of the stress tensor, beside the stress triaxiality, to capture the strain to fracture dependence from the stress state, thus covering both the hydrostatic and the shear type failure modes. The sensitivity of a material to the third invariant has as consequence the non-uniqueness of the relation between triaxiality and fracture strain, which is bound between two distinct limits (upper and lower). These evidences have also been confirmed in recent works by Barsoum [13] and Coppola [26]. In contrast to monotonic ductile failures and low/high-cycle fatigue, models are less well developed for ULCF. The fundamental physical processes responsible for this type of fracture cannot be modelled using traditional fracture mechanics and fatigue models. ULCF is often accompanied by large-scale yielding, which may invalidate stress intensity-based K- or J-type approaches. It is well known that Coffin-Manson approach used in Low-cycle fatigue tends to over-predict the cyclic life under extremely low cycle fatigue conditions [125]. Like monotonic ductile fracture, ULCF is ultimately controlled by the growth and coalescence of microscopic voids. However, the reversed plasticity induced by the severe cyclic loading degrades the fracture resistance, or toughness, due to the accumulation of material damage. This degradation mechanism is similar, in concept, to that of low cycle fatigue. Thus, ULCF is more accurately conceptualized as an interaction between ductile fracture and fatigue.
16 Chapter 2. State of the art 2.6 ULCF and LCF models Current ULCF and LCF models may be broadly organized into two categories: those that couple the fracture behaviour with constitutive behaviour and those that do not. In the former, the effects of material damage are considered through the constitutive model while in the latter, material damage is an independent variable whose value has no direct effect on the constitutive model. Rather, the material damage combined with a fracture condition can predict geometric changes (i.e., material separation) which, in turn, will affect the constitutive response. Since the constitutive response of coupled models is explicitly tied to the damage/fracture model, coupled models can readily predict crack propagation rate and direction, whereas uncoupled models must implement a separate material separation criterion which often pre-determines the crack path. Despite this advantage, coupled models are generally more difficult to calibrate because of additional parameters which may have loose physical meaning. Micromechanicalbased models have been given a major emphasis to predict ULCF fracture. Among these models, the more relevant ones are: •the Cyclic Void Growth Model (CVGM) proposed by Kanvinde and Deierlein [47]; •the Effective Damage Concept (EDC) developed by Ohata and Toyoda [82]; •the Leblond Model (usually called LPD model) [55] and •the Continuum Damage Mechanics model proposed by Bonora [96]. While the first two models are uncoupled models, the latter two consider coupling between damage and constitutive equations. 2.6.1 Cyclic Void Growth Model (CVGM) Because the mechanism of ULCF is controlled by void growth and coalescence, the CVGM proposed by Kanvinde and Deierlein [45], [47] and [46] extends upon the widely used void growth model (VGM), developed by Rice and Tracey [99], Hancock and Mackenzie [37] and others for monotonic loading. The CVGM is
2.6. ULCF and LCF models 17 defined by two equations defining the fracture demands, imposed on a material by ULCF loads, and the fracture toughness of a material, under ULCF loads. The fracture condition (crack initiation) occurs when the fracture demand exceeds the fracture toughness. In order to account for the effects of void growth and coalescence that drive the fracture of metallic materials, the authors propose a model that calculates the void growth and compares it with a critical value to detect material failure. This parameter is obtained experimentally. The initial formulation developed for monotonic cases (Void Growth Model VGM [46]) is extended to cyclic loads by differentiating the void growth obtained in the tensile and compressive regions of the load cycle. Therefore, the void growth in the Cyclic Void Growth Model (CVGM) can be obtained as [47]: V GIcyclic =∑ tensile cycles C1·∫ε2 ε1 exp (−1.5σm σe)dεp− −∑ compressive cycles C2·∫ε2 ε1 exp (−1.5σm σe)dεp< V GIcritical cyclic (2.2) Two assumptions are inherent to the fracture demands: •Voids grow during tensile cycles, where tensile cycles are defined to occur whenever triaxiality is positive; •Voids shrink during compressive cycles, similarly defined as whenever the triaxiality is negative. In the VGM, the critical void size varies only with material; however with the CVGM the critical void size varies both with material and with the extent of material damage, induced by the reversed plasticity of the cyclic loading. 2.6.2 Effective Damage Concept (EDC) The Effective Damage Concept (EDC), like the CVGM, is valid for arbitrary ULCF loading and controlled by the growth and coalescence of voids. The CVGM and EDC are conceptually similar. Both are based on the mechanism of void growth and coalescence with accompanying material damage induced by reversed
24 Chapter 2. State of the art
Chapter 3 Constitutive modelling of Ultra Low Cycle Fatigue 3.1 Introduction ULCF can occur in the metallic materials of modern steel devices that are designed to absorb seismic energy by sustaining large inelastic deformations under cyclic loads. Pipelines installed in seismic or permafrost regions must have sufficient strength against buckling or fracture caused by large ground deformation of buried pipeline. ULCF can be defined as a failure that occurs at a relatively small number on the repeated stress or strain cycles. The upper limit in low-cycle life has generally been selected arbitrarily by different researchers to lie in the range of 104to 105cycles. On the other hand, the lower limit of life is the static test which has been represented by various investigators as 1/4, 1/2, 3/4 or even one cycle ([127], [24]). For ductile metals under periodic plastic loading, materials often fail within a reduced number of life cycles. Within this regime, the failure mechanism is 25
26 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue governed by the plastic and damage (or sometimes called ductile damage), which is characterized by micro structure deterioration such as micro void nucleation, growth and coalescence and micro crack initiation and propagation [125]. So, this process is governed by void growth and coalescence-type mechanisms, which are associated, typically, with ductile fracture phenomenon driven by Bauschinger plasticity non-linear mechanical processes, depending of the plastic strain [4]. While previous studies (e.g., Kuwamura and K. Yamamoto [54]) have identified this issue, models and mechanisms to characterize ULCF are not well established. Prediction models for the cyclic life of materials are thus often based on the alternating plastic and damage strain amplitude. The most commonly used relationship between the alternating damage and plastic strain and the life cycles is the so-called uniaxial Manson–Coffin law ([24], [67]), based on small uniaxial strains formulation. This law is essentially a two parameter power law curve and can be plotted in a log–log scale as a straight line where the slope of the curve depicts the exponent of the power law relationship. The ULCF mechanical processes cannot be modelled using traditional fracture mechanics and fatigue models. Primarily, ULCF is often accompanied by large inelastic strain (damage and/or plasticity), which may invalidate stress intensitybased ∆Kor ∆Japproaches [94]. Second, the induced loading histories are extremely random with very few cycles, making them difficult to adapt to conventional cycle counting techniques such as rain flow analysis ([78], [117]) or strain life approaches. Finally, ∆Kor ∆Jmethods, require an initial sharp crack or flaw, which is absent in many structural details. These limitations, coupled with the large strain advanced finite-element formulation methods, create the need for an improved understanding of the underlying ULCF process and the development of models to predict it. Since 1950s, numerous experimental programs have been carried out to calibrate the material constants for different steels and a large amount of information is available . The experimental data is usually plotted on a log–log scale with the abscissa the number of life cycles and the coordinate the plastic strain amplitude, which is known as the ∆εp−Ncurve. From the experimental results, it is observed that the Manson–Coffin law does not fit well in the range of very low life cycles, i.e. about less than 100 cycles [125]. ULCF damage is bounded by monotonic ductile failure and low-cycle fatigue (LCF). Typically, models for ULCF are extensions of LCF models. However, it is recognized in the literature that LCF models are not fully adequate without any kind of correction. In this context, the use of a plastic damage model to simulate ULCF is proposed,
3.1. Introduction 27 and a new isotropic hardening law is presented. The model is the well-known Barcelona plastic damage model, proposed by Lubliner et al. [64],[88], [89] and [56]. An innovative application is given to this formulation by considering it for the cyclic loading case and incorporating a Friederick-Armstrong kinematic hardening law that allows the description of phenomena like cyclic ratcheting (under stress control conditions) or cyclic stress relaxation (under strain control or elastically constrained conditions). A new isotropic hardening law is developed especially for steel materials, designed to reproduce their hardening and softening performance under monotonic and cyclic loading conditions. The complete nonlinear constitutive model is an extension of a given plasticity model to incorporate the damage effects due to cyclic action. It is an energetic based approach that accounts for the energy dissipated during the plastic action and compares it with a fracture energy that has to be calibrated by experiments. The model considers that complete failure is obtained when all the fracture energy of the material is dissipated. A first preliminary description of the procedure used by the proposed model has been presented in [72] and the results shown in this chapter have been published in [73] and [8]. This work proves that the proposed model it capable of simulating material failure due to ULCF by its own, without the need of any other damage variable computed independently of the plastic formulation. Besides, the proposed approach is not only capable of predicting material failure for regular and non-regular cyclic loads, but it is also capable of coupling cyclic loads with monotonic loads, which allows predicting that the structure will fail sooner if the monotonic load is applied after several hysteresis cycles, than if these cycles are not applied. This capability is obtained as a consequence of the fact that the material failure is predicted by the plastic non-linear constitutive equation itself. Another advantage of the formulation proposed is that it is capable of using any yield and potential surfaces to characterize the material, which increases its applicability to different steel alloys. In Section 3.2 an outline of the constitutive model is made and in sections 3.3 and 3.4 of this chapter the new isotropic hardening law is presented in two different versions. In Section 3.4.3 the complete calibration procedure on small scale samples is presented step by step. Section 3.5 illustrates the results made on a 16-inch 90◦elbow subjected to a variable in-plane displacement and internal pressure.In Section 3.6 results are shown for a large diameter straight pipe under monotonic combined loading: uniaxial displacement and internal pressure. Two different loading histories are taken into account that exhibit different failure modes. Finally, the advantages of the constitutive model proposed are emphas-
28 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue ized in 3.7. 3.2 Plastic damage model The inelastic theory of plasticity can simulate the material behavior beyond the elastic range, taking into account the change in the strength of the material through the movement of the yield surface, isotropic and kinematic. It is assumed that each point of the solid follows a thermo-elasto-plastic constitutive law (hardening/softening) ([64], [65] and [85]) with the stress evolution depending on the free strain variable and plastic internal variables. 3.2.1 Plastic Model Since this work is guided to mechanical problems with small elastic strains and large inelastic strains, the free energy additively hypothesis is accepted ψ= ψe+ψp([62], [63]). The elastic ψeand plastic ψpparts of the free energy are written, in the reference configuration for a given entropy ηand temperature θ field, as the elastic Green strains Ee ij =Eij −Ep ij −Eθ ij; the two last variables operate as free field variables ([65], [63] and [33]). The free energy is thus written as, ψ=ψe(Ee ij, θ) + ψp(γp, θ) = {1 2m[Ee ij ·Cijkl ·Ee kl]+ψp(γp, θ)}−θ·η(3.1) Considering the second thermodynamic law (Clausius-Duhem inequality, [62], [66] and [75]), the thermo mechanical dissipation can be obtained as [63]: Ξ = Sij ˙ Ep ij m−∂ψ ∂γp˙γp−1 θmqi∇θ≥0 (3.2) The accomplishment of this dissipation condition, equation 3.2, demands that the expression of the stress and the entropy should be defined as (Coleman method; see [75]);
3.2. Plastic damage model 29 Sij =m∂ψe ∂Ee ij =Cijkl ·Ee kl;η=−∂ψ ∂θ (3.3) From the last expression is possible to obtain the general expression of the tangent constitutive tensor, Ct ijkl =∂Sij ∂Ee ij =m∂2ψe ∂Ee ij ∂Ee kl (3.4) where mis the material density, Eij ,Ee ij,Ep ij are the total, elastic and plastic strain tensors, respectively, Sij is the stress tensor for a single material point, Cijkl and Ct ijkl are the initial and tangent constitutive tensors, and γpare the plastic internal variables. 3.2.2 Yield plastic functions The yield function Faccounts for the residual strength of the material, which depends on the current stress state, the temperature and the plastic internal variables. This Ffunction and the plastic potential Ghave the following form, taking into account isotropic and kinematic plastic hardening (Bauschinger effect; [58], [16] and [77]), F(Sij, αp, θ) = f(Sij −αij )−K(Sij , κp, θ)≤0 G(Sij, αp, θ) = g(Sij −αij ) = cte (3.5) where f(Sij −αij) and g(Sij −αij) are the uniaxial equivalent stress functions depending of the current value of the stresses Sij ,αij the kinematic plastic hardening internal variable, K(Sij , κp, θ) is the plastic strength threshold, κpis the plastic isotropic hardening internal variable, and θis the temperature at current time t([64],[65] and [85]). The evolution law for the plastic strain obtained from the evolution of the plastic potential as,
30 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue ˙ Ep ij =˙ λ∂Gp ∂Sij (3.6) Being ˙ λthe plastic consistency parameter. We will talk of associated plasticity when the plastic potential is the same as the plastic yield function. 3.2.3 Kinematic Hardening Kinematic hardening accounts for a translation of the yield function and allows the representation of the Bauschinger effect in the case of cyclic loading. A two dimensional representation of this movement in the plane S1−S2is shown in figure 3.1: Figure 3.1: Translation of the yield surface result of kinematic hardening This translation is driven by the kinematic hardening internal variable αij which, in a general case, varies proportionally to the plastic strain of the material point ([58], [86]). There are several laws that define the evolution of this parameter. Current work uses a non-linear kinematic hardening law, which can be written as: ˙αij =ck˙ EP ij −dkαij ˙p(3.7) Where ckand dkare material constants, Ep ij is the plastic strain, and ˙pis the increment of accumulative plastic strain, which can be computed as: ˙p=
3.2. Plastic damage model 31 √2/3·˙ Ep ij :˙ Ep kl. Note that the 2/3 is valid in case of using Von-Mises as the actual yield surface. In other cases, this value should be modified. 3.2.4 Isotropic Hardening Isotropic hardening provides an expansion or a contraction of the yield surface. The expansion corresponds to hardening and the contraction to a softening behavior. In figure 3.2 a two dimensional representation of this effect in the plane S1−S2is depicted: Figure 3.2: Expansion of the yield surface result of isotropic hardening The evolution of isotropic hardening is controlled by the evolution of the plastic hardening function K, which is often defined by an internal variable κp. The rate equation for these two functions may be defined, respectively: ˙ K=˙ λ·Hk=hk·˙κp ˙κp=˙ λ·Hk=˙ λ·[hk:∂G ∂S ]=hk·˙ Ep(3.8) where kdenotes scalar and kstates for a tensor function. Depending on the functions defined to characterize these two parameters different solid performances can be obtained. Two new functions valid for characterizing metallic materials are proposed in this work and described in sections 3.3 and 3.4 of this document.
32 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue 3.2.5 Stress-strain relation and consistency factor Once the material has exceeded its yield threshold, the stress-strain relation is defined by the tangent stiffness matrix. The expression of this matrix, as well as the expression of the plastic consistency parameter can be obtained from the plastic yield criterion and the Prager consistency condition [86]: F(Sij, αp, θ) = f(Sij −αij )−K(Sij , κp, θ) = 0 ˙ F=∂F ∂S ˙ S+∂F ∂α ˙α+∂F ∂K ˙ K= 0 ∂F ∂S ˙ S+∂F ∂α ˙α−˙ K= 0 (3.9) Using previous expressions, it is possible to rewrite equation 3.9 as: ∂F ∂S :C:(˙ E−˙ Ep)+∂F ∂α :(ck˙ EP ij −dkαij ˙p)−hk(hk:˙ Ep)= 0 (3.10) From this expression it is possible to obtain the consistency factor using equation 3.6. ∂F ∂S :C:˙ E−∂F ∂α : (dkαij ˙p)−˙ λ·[∂F ∂S :C:∂G ∂S −ck ∂F ∂α :∂G ∂S +hk·hk:∂G ∂S ]= 0 (3.11) Therefore: ˙ λ= ∂F ∂S :C:˙ E−∂F ∂α : (dkαij ˙p) ∂F ∂S :C:∂G ∂S −ck∂F ∂α :∂G ∂S +hk·hk:∂G ∂S (3.12) The tangent stiffness tensor relates the total strain rate to the stress rate: ˙ S=CT:˙ E(3.13) Finally, the expression of the tangent stiffness matrix can be obtained from the consistency factor:
3.3. New isotropic hardening law 33 Ct=C−[C:∂G ∂S ]⊗[∂F ∂S :C] ∂F ∂S :C:∂G ∂S −ck∂F ∂α :∂G ∂S +hk·hk:∂G ∂S (3.14) It has to be noted that expression 3.14 has been obtained disregarding the nonlinear term of kinematic hardening. Despite having a first approximation of the analytical expression that provides the tangent stiffness tensor, in many occasions the calculation of the partial derivatives of the yield and potential functions is not straightforward. In those cases, a numerical derivation can be performed. This procedure, although expensive, provide an accurate approximation that improves the global convergence of the problem. An efficient procedure to conduct this numerical derivation, as well as the advantages obtained with it, are shown in [74]. A detailed description of the integration procedure of the constitutive equations can be found in references [63] and [86]. 3.3 New isotropic hardening law Equation 3.8 allow the incorporation of different hardening laws to describe the material performance. In the Barcelona model defined in [64], the laws defined are driven by the fracture energy of the material. This work presents a new law, specially developed for steel materials, that has been designed to reproduce their hardening and softening performance under monotonic and cyclic loading conditions. This law also depends on the fracture energy of the material. 3.3.1 Fracture Energy Classical fracture mechanics defines the fracture energy of a material as the energy that has to be dissipated to open a fracture in a unitary area of the material. This energy is defined as: Gf=Wf Af (3.15) where Wfis the energy dissipated by the fracture at the end of the process, and
40 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue temperature in air. The fatigue tests were conducted under constant strain amplitudes and with a frequency adjusted to result an average strain rate of 0.008s−1. The longitudinal strain was measured using a clip gauge with limit displacements of ±2.5 mm with a gauge length of 12.5 mm (INSTRON 2620-602). This extensometer was also used in two monotonic tensile tests allowing the registration of the longitudinal strains until approximately 17%. All tested specimens were machined according the longitudinal direction of 6 inch pipes made of X52 steel. The dimensions of the specimens are in accordance with the ASTM E606 standard, as illustrated in figure 3.5. The shown specimen corresponds to the SP series. The side faces of the specimens were milled and finished in order to remove the circumferential pipe curvature as well as surface imperfections. In order to achieve larger strain values in the specimen some of them where machined in order to reduce their section in their middle. This is the case of the OH specimen, shown in figure 3.6, in which the geometry is modified with an oval hole in its center. The experimental results obtained for this specimen have been also used to validate the model performance. Figure 3.5: Dimensions, in millimeters, of the SP specimen Figure 3.6: Dimensions, in millimeters, of the OH specimen
3.3. New isotropic hardening law 41 3.3.4.2 Description of the numerical models Two different numerical models have been defined, one for each experimental specimen. Figure 3.7 shows the meshes of both models. The SP model is made with 1608 quadratic hexahedral elements and 8839 nodes. It has three elements along its thickness and 563 elements in the face shown in figure 3.7 (YZ). The OH model has 3080 quadratic hexahedral elements and 15460 nodes. It has five elements along the thickness and 616 elements in the YZ face. This second model requires nearly double the number of elements because the element size has to be significantly smaller around the hole for its correct simulation. Figure 3.7: Mesh defined for the SP and OH numerical models. The SP model has marked, with red dots, the points used to calculate the equivalent strain applied. Regarding boundary conditions, the left border of the model has the displacement fixed to zero in all its directions, while the right border is moved with an imposed displacement in the longitudinal direction of the sample. The reaction force is obtained as a result of the numerical analysis. All samples analyzed are defined with the same plastic material, defined with an associated plasticity and Von-Mises as yield law. The material properties are obtained with the calibration process that is described in the following section. All the material properties required by the model are displayed in table 3.1. A parameter of this table that may seem surprising is the value of the yield stress, which is lower than the one expected for an X52 steel. This value is required because, if the yield stress is defined with a higher value, the kinematic hardening parameters lead to stress values too high in the hysteresis cycles. As the purpose of the model is the simulation of ULCF, which requires large plastic strain values, the requirement of defining a lower yield stress is not considered a major drawback. The hardening region is defined with a polynomial of order five which is computed
42 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue Young Modulus 180 GPa Poisson Ratio 0.30 Yield Stress (σeq Y) 240 MPa Plastic Strain threshold (Ep 2) 13 % c1kinematic hardening param. 60 GPa d1kinematic hardening param. 280 Fracture Energy (Gf) 1.9 MN * m/m2 Table 3.1: Mechanical properties of steel X52 with the least squares method using available the experimental data. The constants of this polynomial, following notation shown in equation 3.21, are shown in table 3.2. In order to define the polynomial constants, it has been necessary to take into account that the effects of the kinematic and the isotropic hardening laws are coupled. This implies that the definition of the first region of isotropic hardening cannot be obtained from the experimental curve straightforward, as this curve does not take into account the displacement of the yield surface due to the kinematic hardening law. a02.4000E+08 a18.0084E+07 a2-1.1143E+08 a38.7400E+07 a4-3.0507E+07 a53.9073E+06 Table 3.2: Polynomial constants used to describe the hardening region of X52 material
3.3. New isotropic hardening law 43 3.3.4.3 Calibration of the numerical model The material data previously exposed has been obtained by model calibration. This is, adjusting the different parameters required by the model to obtain a good fitting with one of the experimental results available. For the current case, the experimental results considered are those of the specimen loaded with an imposed strain range of 2.75%. The results used to conduct the material calibration are the equivalent stressequivalent strain graph obtained from the experimental test. The stress is computed as the total force applied to the specimen divided by the area of the cross section. The strains are computed dividing the measured displacement of the clipped gauge by the length of the gauge. In the numerical model these two parameters were calculated following the same procedure, using the red nodes depicted in figure 3.7. The initial material parameters used in the calibration process are ones commonly found in literature and the polynomial constants correspond to the ones obtained by curve fitting of the experimental results, ignoring the effect of kinematic hardening. Based on the strain-stress graph obtained with these first values, the different parameters shown in table 3.1 and table 3.2 have been modified until obtaining a numerical result that fits the experimental results. Figure 3.8 shows the stress-strain graph provided by the two experimental samples tested and by the numerical model, which uses the material parameters obtained from the calibration process and described in table 3.1 and in table 3.2. As it can be seen, the agreement in the cyclic behavior of the numerical and experimental samples is rather good. This agreement is not achieved in the first loading cycle, as the model developed is not prepared to reproduce the initial plateau defined by the material. However, this disagreement is not considered relevant, as the model has been developed thinking on the cyclic behavior and the evolution of plastic response for larger plastic strain values, found beyond this initial plateau. The fitting of the stress-strain graph allows defining all material parameters except the fracture energy of the material and the equivalent plastic strain value at which softening is expected to start (Ep 2). These two parameters have been defined to match the number of cycles that can be applied to the specimen before it fails. In the experimental campaign, the first specimen failed after 150 cycles, and the second specimen failed after 103 cycles. With these results, an initial value of Ep 2= 13%, as the maximum hardening strain has been defined. Afterwards, the parameter of the material fracture energy, Gf, is modified until
44 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue -5e+008 -4e+008 -3e+008 -2e+008 -1e+008 0 1e+008 2e+008 3e+008 4e+008 5e+008 -0.015 -0.01 -0.005 0 0.005 0.01 0.015 Equivalent Stress [Pa] Equivalent Strain ’Experimental 1’ ’Experimental 2’ ’Numerical’ Figure 3.8: Stress-strain graphs for the SP sample with an applied deformation range of 2.75% finding a value that predicts the failure of the numerical test after 128 cycles. These values are shown in table 3.1 and used in the numerical simulations. Material failure is found when some gauss points reach a plastic damage value close to one. At this stage the numerical analysis cannot reach convergence and the specimen can be considered to be completely broken. In current simulation, the convergence is lost for a κpvalue close to 0.9, as it is shown in figure 3.9, where the value of plastic damage is represented in the last tensile and compressive stages. The mechanical performance of the numerical specimen along the simulation is Figure 3.9: Values of κpfor the SP sample with an applied deformation range of 2.75%, when applying the maximum tensile and compression strain before ULCF failure. Deformation is magnified by 20.
3.3. New isotropic hardening law 45 shown in figure 3.10, where the stress-strain loops for different cycles are represented. This picture shows that the effect of material softening in the specimen consists of a reduction of the equivalent stress obtained as the number of cycles applied to the specimen increase. The figure shows that softening has already started in cycle 60, although the difference between the first loop and loop 60 is very small. In further cycles the effect of softening becomes more visible, until material failure in cycle 128, where the reduction of equivalent stress is close to a 20%. Figure 3.10 also shows that the strain amplitude increases with the number of cycles applied to the specimen. This increase is obtained because equivalent strain is calculated as the relative displacement of two given nodes (red dots in figure 3.7), divided by the original length between both nodes, and does not take into account that it is modified due to the plastic deformations existing in the whole specimen. -5e+008 -4e+008 -3e+008 -2e+008 -1e+008 0 1e+008 2e+008 3e+008 4e+008 5e+008 -0.02 -0.015 -0.01 -0.005 0 0.005 0.01 0.015 0.02 Equivalent Stress [Pa] Equivalent Strain ’cycle 01’ ’cycle 60’ ’cycle 100’ ’cycle 128’ Figure 3.10: Evolution of the stress strain graph for different cycles of the SP numerical analysis The results shown for the calibration test prove that the constitutive law proposed can be adjusted to any given stress-strain law by adjusting properly the material parameters. The calibration model has also been used to show the numerical and mechanical performance of the formulation developed. The prediction capacity of the model will be shown in further simulations, in which the material parameters are fixed and are used to analyze different specimens and load cases.
46 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue 3.3.4.4 Validation of the developed theory After having calibrated the material parameters, the rest of experimental tests available have been simulated in order to compare the ULCF failure prediction made by the numerical model with the results obtained from the experimental campaign. The constitutive model proposed in this work will succeed if it is capable of representing accurately the equivalent stress-strain graphs for the different deformation ranges tested experimentally and, even more important, if it is capable of predicting the number of cycles that can be applied to the specimen before its failure. Figure 3.11 shows the stress-strain graph corresponding to the experimental and numerical sample with an applied equivalent strain of 4%. In order to achieve this strain value, and to avoid the buckling of the specimen, the experimental test is conducted only on the positive strain region and with an antibuckling device. As can be seen, the experimental and the numerical results are in good agreement of the cyclic region of the curve. So, with this example it is proved that the model is capable of reproducing large strain values and non-symmetric cyclic patterns. -6e+008 -4e+008 -2e+008 0 2e+008 4e+008 6e+008 -0.005 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 0.045 Equivalent Stress [Pa] Equivalent Strain ’Experimental’ ’Numerical’ Figure 3.11: Stress-strain graphs for the SP sample with an applied deformation range of 4.00% Finally, figure 3.12 compares the stress-strain experimental-numerical results obtained for one of the OH samples. The stress value for the OH samples is computed with the same procedure used for the SP samples, dividing the total force
3.3. New isotropic hardening law 47 applied by the area of the cross section where the notch is found; and the strain value is obtained dividing with the gauge length described in section 3.3.4.1. In this case, the numerical result prediction falls a bit shorter in terms of equivalent stress when compared to the experimental test. However, a closer look to the experimental curve shows that in the first loading branch the experimental and numerical tests match perfectly, and it is in further cycles that the experimental test provides larger equivalent stress values. This difference between cycles in the experimental test may be due to some sort of hardening around the notch, which cannot be captured by the proposed model. Despite this difference, results are considered similar enough to validate the material parameters defined in the numerical model calibration. -6e+008 -4e+008 -2e+008 0 2e+008 4e+008 6e+008 -0.008 -0.006 -0.004 -0.002 0 0.002 0.004 0.006 0.008 Equivalent Stress [Pa] Equivalent Strain ’Experimental’ ’Numerical’ Figure 3.12: Stress-strain graphs for the OH sample with an applied deformation range of 1.20% Once having proved that the developed formulation is capable of reproducing quite accurately the mechanical response obtained with the experimental samples, the following step is to verify if the formulation is capable of predicting the failure of the specimens due to ULCF. This validation is performed counting the number of cycles that can be applied to the numerical model before its failure. The numerical model is considered to have failed when the convergence of the analysis is lost. This occurs when some gauss points reach a κpvalue close to 1,0. The number of cycles applied to the numerical model are compared with the cycles obtained in the experimental campaign.
48 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue Figure 3.13 shows the results obtained for the SP samples. Results with reversion strain factor of –1 and of 0 are plotted together because the reversion factor does not play a significant role in the material response to ULCF. This figure shows that the number of cycles to failure predicted by the numerical simulation are in very good agreement with the number of cycles obtained in the experimental campaign. The only value that is not contained between the experimental results is the one corresponding to an applied strain range of 3.5%. However, the value provided by the numerical simulation looks more coherent than the one obtained with the experimental test, as the number of cycles obtained in the experimental test is larger than the one obtained for an applied strain range of 2.75%. 0.02 0.025 0.03 0.035 0.04 50 100 150 200 250 300 350 Equivalent Strain Number of Cycles ’Experimental SP R0’ ’Experimental SP R1’ ’Numerical’ ’Calibration value’ Figure 3.13: ULCF failure prediction for SP samples The results obtained for the OH samples are shown in figure 3.14. For these samples the experimental test was conducted in just one specimen for each strain value, therefore there is no possibility to know the scatter expected in the experimental tests. However, the number of cycles predicted by the formulation is, for all strains, in the same order of magnitude than the experimental results obtained. Therefore, it can be concluded that the formulation is, again, capable of predicting accurately the ULCF failure of the OH specimens. It is important to remark that the material properties used for all numerical simulations are exactly the same. Therefore, the variation in the prediction of the number of cycles that can be applied to any of the specimens considered is the result of the energy dissipated in each case. The agreement obtained in all
3.4. Extension of the new isotropic hardening law for large problems 49 0.012 0.013 0.014 0.015 0.016 0.017 0.018 0.019 0.02 0.021 0.022 0.023 10 20 30 40 50 60 70 80 90 Equivalent Strain Number of Cycles ’Experimental’ ’Numerical’ Figure 3.14: ULCF failure prediction for OH samples cases, independently of the reversion factor or the stress concentrations due to the existing hole (OH sample) allows considering the approach used to characterize ULCF failure an excellent option. Moreover the formulation allows conducting simulations in which the cycles can be non-regular, with varying amplitude and frequency, in which there can be sustained monotonic loads between cycles or, in general, in which the load applied is not a regular one. This capability is not offered by any other formulation available. 3.4 Extension of the new isotropic hardening law for large problems 3.4.1 Hardening Function and Hardening Internal Variable The constitutive law presented in section 3.3 has been modified in order to ensure faster convergence in the numerical model and therefore make feasible the application of the model on large problems.
56 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue 0 1e+008 2e+008 3e+008 4e+008 5e+008 6e+008 0 0.02 0.04 0.06 0.08 0.1 0.12 Stress (N/m2) Strain (-) numerical experimental 1 experimental 2 Figure 3.19: Monotonic stressstrain curve. Numerical vs. experimental. deformed shape of the specimen in the last step of the analysis for the calibration case. The null value for the plastic internal variable represents an elastic state in the material, while κp= 1 means the entire fracture energy of the material has been dissipated at that material point. It can be seen that the lateral necking is in accordance to standard metal fracture under uniaxial cyclic loading. After the adjustment of the ∆ε=5% case, simulations were ran with the exact same material parameters and with strain amplitudes of 8%(figure 3.20) and 2% (figure 3.22). It can be seen that the considered material parameters offer a good aproximation of the hysteresis loop for these strain amplitudes also. The results in terms of life prediction can be seen in figure 3.24. In table 3.3 and table 3.4 a summary of the material properties as resulting from the calibration can be seen. A polynomial of the 5th degree was chosen for the curve fitting zone of the hardening function.
3.4. Extension of the new isotropic hardening law for large problems 57 -6e+008 -4e+008 -2e+008 0 2e+008 4e+008 6e+008 0 0.01 0.02 0.03 0.04 0.05 0.06 0.07 0.08 Stress (N/m2) Strain (-) numerical experimental Figure 3.20: Stress-strain hysteresis loop for ∆ε=8%. Numerical vs. experimental. Coefficient no. 1 a0380000000,00 Coefficient no. 2 a1326947332,25 Coefficient no. 3 a2-861244568,93 Coefficient no. 4 a31103673406,83 Coefficient no. 5 a4-657861660,66 Coefficient no. 6 a5147925577,48 Table 3.3: Polynomial coefficients for the X60 material as obtained from curve fitting
58 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue -6e+008 -4e+008 -2e+008 0 2e+008 4e+008 6e+008 -0.01 0 0.01 0.02 0.03 0.04 0.05 0.06 Stress (N/m2) Strain (-) numerical experimental Figure 3.21: Stress-strain hysteresis loop for ∆ε=5%. Numerical vs. experimental. -6e+008 -4e+008 -2e+008 0 2e+008 4e+008 6e+008 -0.015 -0.01 -0.005 0 0.005 0.01 0.015 Stress (N/m2) Strain (-) numerical experimental Figure 3.22: Stress-strain hysteresis loop for ∆ε=2%. Numerical vs. experimental.
3.4. Extension of the new isotropic hardening law for large problems 59 Figure 3.23: Distribution of the normalized plastic dissipation at total fracture 0 0.02 0.04 0.06 0.08 0.1 0 50 100 150 200 250 300 350 400 Strain amplitude (-) No. of cycles (-) numerical experimental calibration Figure 3.24: Comparison between numerical and experimental fatigue life for different strain amplitudes when calibrating with ∆ε=5%
60 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue Young Modulus 1.95 105MPa Poisson Modulus 0.30 Elastic Stress (σeq Y) 380 MPa Plastic Strain Limit for region 1(Ep 1) 10 % Plastic Strain Softening (Ep 2) 1300 % c1kinematic hardening 6.0 104MPa d1kinematic hardening 400 Fracture Energy 2.7 MN * m/m2 Table 3.4: Material parameters for the numerical model for an X60 steel
3.5. Large scale validation on a bent pipe under variable cyclic loading 61 3.5 Large scale validation on a bent pipe under variable cyclic loading This section presents the results of finite element simulations made on a bent pipe subjected to an in-plane variable cyclic displacement combined with internal pressure. Special emphasis is put on the capacity of the model to illustrate different failure modes depending on the internal pressure applied on the pipe. The results of the numerical analyses will be compared to experimental ones. 3.5.1 Geometry of the model Following the validation of the constitutive model made on small scale specimens, the model is to be applied to large scale numerical simulations of a bent pipe. The geometry of the model, boundary conditions and the sequence of loading are in accordance to the experiment made by Schaffrath et al. [104]. The specimens consist of a bended middle section (elbow pipe) and a straight pipe section at each end of the elbow. The fillet radius of the elbow pipe is three times the pipe diameter (R=3 x D). For the length of both straight pipe sections a value of five times the diameter (L=5 x D) was used, whereby the influence of the load introduction can be neglected. Figure 3.25 shows the general dimensions of the specimen as a function of the diameter of the pipe, while in figure 3.26 the geometry of the specimen after manufacturing can be observed. For the numerical simulation, a specimen made of X60 steel has been chosen from the experimental program, with a diameter of 406.4 mm and a wall thickness of 9.5 mm. The pipe has an elbow angle of 90◦. Figure 3.27 shows the model used for the numerical simulation as generated with the pre-postprocessor GiD. Following, in figure 3.28 a view of the mesh is shown. For this simulation quadratic hexahedral elements were used, each with 20 nodes and 27 integration points. The mesh consisted of 42853 elements and 213415 nodes. Three elements were considered in the pipe thickness.
62 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue Figure 3.25: Overview of the general dimensions of the specimen 3.5.2 Loading history The loading history is based on the actual load history of the experimental test done by Schaffrath et al. [104]. The loading scheme was decided by the authors in accordance with the ECCS procedure ECCS-Nr. 45-1986 Recommended Testing Procedure for Assessing the Behavior of Structural Steel Elements under Cyclic Loads [1]. For practical reasons it was decided to neglect the mostly small difference between the compressive and tensile yield strain by choosing an average value ey= (e+ y+e− y)/2 as the reference amplitude. In table 3.5 the experimental loading sequence is described as a function of ey.The value adopted for this parameter was set by [104] at ±82mm. The entire loading sequence is comprised of 49 cycles with increasing amplitude, 44 of which have amplitudes in the plastic range. The reversion factor of the applied displacement is -1 (figure 3.29). The pipe is also submitted to internal pressure. First, the pipe is loaded until a level of internal pressure equal to 20 bars. Afterwards, it is submitted to the varying cyclic displacement presented in table 3.5. The experimental test has shown that the internal pressure also oscillates when the cyclic displacement is applied. The boundary conditions of the model were chosen in accordance with the setting of the experiment. One end of the model has its displacement blocked in the x, y and z direction while in the other end the cyclic displacement is applied in the z in-plane direction, as shown in figure 3.30. In the numerical simulation the loads have been applied in two stages. First,
3.5. Large scale validation on a bent pipe under variable cyclic loading 63 Figure 3.26: Specimen SP1-SP2 (X60, 90◦) the internal pressure was applied and, in this stage, one end of the pipe was clamped and on the other end the pipe was only allowed in-plane gliding. The variable displacement was applied in the second stage on the deformed geometry obtained from applying the internal pressure. The movement was restrained in the two directions perpendicular to the in-plane one. 3.5.3 Material characteristics The exact calibration procedure for the X60 material can be seen in Section 4, as well as the properties defined, that are presented in table 3.3 and table 3.4. 3.5.4 Results and discussion In figure 3.31 the comparison between the experimental forcedisplacement curve and the numerical one can be seen. The numerical curve is in very good agreement with the experimental one taking into consideration that the material calibration
64 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue Figure 3.27: Model geometry was done on small scale specimens with different experimental results. It can be seen how in compression the constitutive equation tends to underestimate the maximum force level, while in traction the opposite tendency is present. Furthermore, this tendency is more obvious as the displacement increases. This is due to the existence of oscillations of the internal pressure applied in the experiment, caused by applying the cyclic displacement. This oscillation of the internal pressure has not been taken into account in the numerical simulation. Regarding the fatigue life, the simulation lasted a total of 41.75 plastic cycles as compared to the experimental life of 44 complete cycles. This result also shows a good agreement between the experiment and the numerical simulation. Figure 3.32 illustrates the deformed shape of the geometry in the last step of the analysis and presents the distribution of the plastic internal variable of the model. The deformed shape is represented with a scale factor of 2 in order to better reflect the general tendency. Only the central zone of the elbow is shown, as this is the zone where nonlinear effects appear. It can be seen that the failure mode resulting from the numerical simulation is by cross-sectional ovalization with a crack opening in the longitudinal direction of the elbow, at its flank. In figure 3.33 the total strain distribution can be seen in the last step of the analysis in the three model axes. The distribution is also plotted on the deformed shape of the model, where the cross-sectional ovalization is clearly visible. It can be seen that strain accumulation occurs in all three directions in the critical area where the normalized dissipation parameter, κp, accumulates. The comparison of the failure mode obtained with the numerical simulation with
3.5. Large scale validation on a bent pipe under variable cyclic loading 65 Figure 3.28: Mesh of hexahedral quadratic elements the failure mode obtained in the experimental test (figure 3.34) shows that the model has been able to capture the number of cycles to failure but has not been able to capture the failure mode shown in the experiment. Under extreme loading conditions, such as the high repeated incursions in the nonlinear zone that the imposed displacement in this case causes, elbows exhibit two different failure modes. These are either significant cross-sectional ovalization or local buckling, as reported by the experimental work described in Sobel and Newman [110], [111], Dhalla [28] and Greenstreet [34], Tan et al. [115], Shalaby and Younan [107] and Suzuki and Nasu [114] for monotonic bending moments and Yahiaoui et al. [126], Slagis [109]and Fujiwaka et al. [32] for cyclic loading, and from the work of Karamanos et al. [48], [49], Pappa et al. [93], Varelis et al. [119], [118]. An important conclusion can be drawn from the work above mentioned. The first failure mode can be generally found when the elbow internal pressure is relatively low compared to the yield pressure, as is the case in the numerical simulation presented above. The second failure mode, occurring due to local buckling is habitual in the cases where internal pressure is significantly higher. This is the failure mode yielded by the experiment made by Schaffrath et al. [104] as it can be seen in figure 3.34.
72 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue 0 0.1 0.2 0.3 0.4 0.5 0.6 0.7 0.8 0.9 1 0 0.15 0.3 0.45 0.6 0.75 0.9 1 Dissipation normalized to max. value (-) Internal pressure/Yield pressure (-) Max. value in zone A Max. value in zone B Figure 3.37: Evolution of the maximum dissipation in the two areas of interest
3.5. Large scale validation on a bent pipe under variable cyclic loading 73 Py (%) Zone A Zone B 0 25 30 35 50 100 Table 3.6: Distribution of the maximum dissipation normalized to the fracture energy on the deformed shape of the model (x5)
74 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue 3.6 Large diameter straight pipe loaded monotonically In order to analyze the capabilities of the constitutive model presented in previous sections, large scale numerical simulations of a straight pipe OD 168.3 x 4.78mm, X52 grade, will be conducted. The geometry of the model, boundary conditions and sequence of loading are established by the experiment made by Coppola et al. [27]. The specimen drawing can be seen in figure 3.38. Figure 3.38: Specimen drawing for X52 full scale testing 3.6.1 Geometry of the model The specimen consists of a straight pipe, with three differentiated sections. The central one is mechanized with a reduced thickness, as seen in figure 3.39 and
3.6. Large diameter straight pipe loaded monotonically 75 table 3.7. Figure 3.39: Sections of interest in the mechanization of the straight pipe Figure 3.40: Model geometry in GiD In the numerical model the variation in thickness throughout the central zone has been accounted for, as well as the thickness variation throughout the same cross-section. A view of the model geometry in the pre-postprocessor GiD can be seen in figure 3.40. Following, in figure 3.41 a view of the mesh is shown. For this simulation quadratic hexahedral elements were used, each with 20 nodes and 27 integration points. The mesh consisted of 8162 elements and 45865 nodes. Regarding boundary conditions, shown in figure 3.42, one capped end of the pipe has its displacement restricted in all directions, while on the other capped end either force or displacement is applied as required by the loading history. When applying internal pressure, one end remains fixed while on the other one the
76 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue Figure 3.41: Mesh of hexahedral quadratic elements displacement in the longitudinal axis of the pipe is allowed (z-z axis in figure 3.41) and restrained in the other two directions. The material of the mechanized part is an X52 steel. The outer parts have an elastic material, with the same Young modulus as X52. The pipe caps have been defined as a rigid material in agreement with the setup of the experiment (see figure 3.38). Figure 3.42: Boundary conditions for the straight pipe
3.6. Large diameter straight pipe loaded monotonically 77 3.6.2 Loading history For this simulation two load combinations were made. In the first case (SPEC1) a traction force was applied on one of the caps in the longitudinal pipe axis until a level of 400KN. Afterwards, an internal pressure was applied and gradually increased up to burst. Pipe failure occurred at 270bar with an associated total axial load of 940KN. In the second case, the test has been done with internal pressure followed by tension. The internal pressure in the first step is 200 bars. Afterwards, the load was increased up to failure which occurred at 884KN mechanical load (1284KN total axial load). Pressure in the second step was maintained constant at 200 bars. In figure 3.43 the two loading scenarios are presented. Figure 3.43: Loading scenarios for the straight pipe 3.6.3 Material characteristics The material parameters for the X52 steel have been obtained by undergoing the calibration process described in section 3.4.3 of this document. A polynomial of the 5th degree was chosen for the curve fitting zone of the hardening function. The polynomial coefficients as given by the least squares method are shown in table 3.8.
78 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue The remaining material parameters are shown in table 3.9.These material parameters were obtained by conducting a calibration process on small scale smooth sample specimens. The geometry of the samples and some calibration results for the cyclic case are presented in section 3.3. In figure 3.44, the monotonic stress strain curve can be seen as obtained with the material parameters presented before. The comparison with the experimental monotonic curves for the X52 steel as obtained from Pereira et al. [95] can also be seen. Figure 3.45 exhibits the comparison between the numerical hysteresis loop shape and the experimental one. Although the straight pipe is loaded monotonically, when conducting the calibration analysis for the material, the shape of the hysteresis was one of the factors taken into account as the model is prepared to conduct monotonic and cyclic tests. The calibration process for a monotonic analysis follows the same guidelines as that of a cyclic analysis. The main difference resides in the plastic strain chosen as threshold for the softening behavior and in the fracture energy assigned to the material. 0 1e+008 2e+008 3e+008 4e+008 5e+008 6e+008 0 0.05 0.1 0.15 0.2 0.25 0.3 0.35 0.4 0.45 0.5 Stress (N/m2) Strain (-) numerical experimental 1 experimental 2 Figure 3.44: Stress-strain curves for the monotonic case 3.6.4 Results and discussion Case no. 1 - Tension followed by pressure In figure 3.46, the comparison between the experimental and the numerical force-
3.6. Large diameter straight pipe loaded monotonically 79 -6e+008 -4e+008 -2e+008 0 2e+008 4e+008 6e+008 0 0.005 0.01 0.015 0.02 0.025 0.03 0.035 0.04 Stress (N/m2) Strain (-) numerical experimental Figure 3.45: Stress-strain hysteresis loop for ∆ε=4%. Numerical vs. experimental. pressure measurements can be seen. The total reaction recorded by the numerical simulation reached a level of 948KN in the last converged increment, corresponding to an applied internal pressure of 278.1bars. For this increment, the deformed shape of the specimen is shown in figure 3.47, where the distribution of the hardening internal variable κpcan also be seen. This variable is of relevance in showing the level of dissipated energy at material point level and, in this sense, gives a measure of the level of degradation suffered. Consequently, for κp= 0 the material is in an elastic state, while for κp= 1 the material has reached total failure at that material point. From the deformed shape it can be seen that the pipe failure is oriented following the direction of least resistance represented by the minimum thickness area. This is in agreement with the experimental localization of the failure as can be seen in figure 3.48. Also, there is good agreement of the failure mode between the experiment and the numerical simulation with a final burst opening oriented in the longitudinal direction. In the numerical model the burst area is represented by the localized plastic strain accumulation reflected in the distribution of the normalized dissipation parameter. Figure 3.50 shows the evolution of the hardening internal variable κpat the most damaged integration point in the material. Its exact location is indicated in figure 3.47. As it can be seen from figure 3.50, the simulation converged up until a
80 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue 0 50 100 150 200 250 300 0 100 200 300 400 500 600 700 800 900 1000 Internal pressure (bar) Axial load (kN) experimental T+P numerical T+P Figure 3.46: Comparison between the numerical and experimental results for the SPEC 1 case maximum value of the κpinternal variable of 0.7. Given that the internal pressure has been applied in constant increments of 2.7 bars per analysis step, it can be seen that the evolution of the κpparameter exhibits an exponential curve. Taking into account this tendency and extrapolating on the last converged increment that had a value of 0.7, loss of convergence seems to have occurred when the plastic internal variable reached a value very close to 1, corresponding to an open crack generated at the material points where the entire fracture energy of the material has been spent. However, this value is not visible in figure 3.50 since convergence was not reached for this increment. Case no. 2 – Internal pressure followed by tension In figure 3.51 the comparison between the experimental and the numerical forcepressure measurements can be seen for this case. The total reaction recorded by the numerical simulation reached a level of 1167KN in the last converged step, corresponding to a total applied displacement of 1.375m. The experimental failure occurred at a total axial load level of 1284kN. As specified before, during the applied displacement stage the internal pressure was maintained constant at a level of 200 bars. For the last step of the simulation the deformed shape is shown in figure 3.52, where the distribution of the hardening internal variable κpcan also be seen.
3.6. Large diameter straight pipe loaded monotonically 81 Figure 3.47: View of the deformed shape at the end of the analysis with an indication of the most damaged material point in the geometry The localization of the failure zone corresponds to the behavior shown in the experiment, presented in figure 3.49. When considering the pipe cross section where the maximum dissipation is present, the most stressed area is directed towards the smallest thickness in that particular circumference, corresponding with the data recorded by the experimental campaign and taking into account the orientation of the numerical model with respect to that of the experimental setting. The failure mode is a tensile one, in agreement to the applied sequence of loading.
88 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue -0.0006 -0.0004 -0.0002 0 0.0002 0.0004 0.0006 0.0008 0.001 0 10 20 30 40 50 60 70 80 90 100 Displacement [m] Step increment ’Seismic Load’ Figure 3.54: Material stress-strain response figure 3.54. As can be seen, the applied load produces several hysteresis loops, each one with a different plastic strain. The model is capable of capturing the energy dissipated in each one of these loops and, therefore, to evaluate the energy available in the material after having applied the load, which is equivalent to the residual strength of the material. It is also possible to repeat several times the irregular load, as shown in figure 3.53, to study the number of repetitions that are required to reach material failure. Figure 3.56 shows the stress-strain response of the material after 10 cycles (figure 3.55). At this point there are some points in the model that have lost most of their fracture strength and specimen failure occurs. As occurred with the SP model, this simulation also shows some lateral displacement on the equivalent strains due to the plastic strains suffered by the whole specimen. Concluding, in this chapter a new plasticity constitutive law has been developed for the ULCF case that takes into account isotropic and kinematic hardening. The constitutive law has been validated on small scale samples and on large scale simulations made on pipelines. From an industrial point of view the constitutive model has proved to be a valid tool for the simulation of pipelines subjected to complex load conditions, both for the monotonic case and for the cyclic one.
3.7. Advantages of the approach proposed 89 -0.0006 -0.0004 -0.0002 0 0.0002 0.0004 0.0006 0.0008 0.001 0 100 200 300 400 500 600 700 800 900 1000 Displacement [m] Step Increment ’Seismic Load’ Figure 3.55: Seismic-type load applied: ten seismic-type cycles -5e+008 -4e+008 -3e+008 -2e+008 -1e+008 0 1e+008 2e+008 3e+008 4e+008 5e+008 -0.08 -0.06 -0.04 -0.02 0 0.02 0.04 0.06 Equivalent Stress [MPa] Equivalent Strain ’Cycle 01’ ’Cycle 10’ Figure 3.56: Material stress-strain response after ten seismic-type cycles
90 Chapter 3. Constitutive modelling of Ultra Low Cycle Fatigue
Chapter 4 Constitutive modelling of High Cycle Fatigue 4.1 Introduction A stepwise load-advancing strategy for cyclic loading will be presented in this chapter that yields convergence in reasonable computational time for highly nonlinear behaviour occurring past the S-N curve. The algorithm is also effective when dealing with combinations of cyclical loads. The strategy is coupled to a continuum damage model for mechanical fatigue analysis. An overview of the constitutive model is also presented. The capabilities of the proposed procedure are shown in several numerical examples. The model is validated by comparison to experimental results. The basis of the HCF constitutive model used was initially developed by Oller et al. [100]. The model establishes a relationship between the residual material strength and the damage threshold evolution, controlled by the material internal variables and by a new state variable of fatigue that incorporates the influence of 91
92 Chapter 4. Constitutive modelling of High Cycle Fatigue the cyclic load. A brief overview of the constitutive formulation for the HCF case is provided in order to clarify the material behaviour exhibited in the numerical examples. Several model assumptions are to be made. Defect concentration on the microscale occurs during the whole period of cyclic loading. This is reflected in the model in a continuous reduction of the material strength, occurring even in the elastic stage. Stiffness degradation occurs only in the post critical stage, once the S−Ncurve has been passed and, therefore, only in the final stage before failure. The damage parameter has a phenomenological significance indicating the irreversibility of the fatigue process. Depending on the size of the domain chosen for a fatigue numerical simulation, computational time for a numerical analysis can vary considerably. Nowadays, running simulations at macroscale level (mechanical part, structural element) continues to be a challenge, especially if the high level of structural complexity attained at the microscale needs to be taken into account to some extent at other scales. This work offers a stepwise load-advancing strategy that allows a saving of computational time and can help push the barrier of what if possible in terms of numerical simulation one step further. The strategy can be especially effective when dealing with HCF where material lives are in the range of 106– 107cycles. If a single loading cycle is described by nloading steps, then the number of loading steps required to complete a HCF analysis would be in the order of 107xn. Furthermore, if the mechanical piece has a complex geometry and a high level of discretization is required at finite element level, then at each of the 107xnload steps a large number of constitutive operations need to be computed for each integration point. The above serve as a clear example of why load-advancing strategies are of the utmost importance in HCF simulations. Furthermore, increasingly more attention has been given to material behaviour in the very high cycle regime from an experimental point of view. The general belief that steel experiences no alteration in its properties after reaching its fatigue limit at 107cycles has been invalidated [14], [15], [69]. In this context, this work provides a tool for rapid automatized time-advance that allows taking numerical simulations beyond the limit of 107cycles in reasonable computational time.
4.2. HCF damage model 93 4.2 HCF damage model A description of the constitutive model is offered in this section. The fundamentals of a fatigue continuum damage model are presented with a clear emphasis on the dependence of the model on the S-N curves. An exhaustive description of the formulation used can be found in Oller et al. [100], where the complete thermomechanical constitutive model for the prediction of fatigue effects in structures is formulated. The model is capable of taking into account the effect of the mean stress. The treatment of the highly complex processes generated by fatigue is made from a phenomenological point of view. 4.2.1 Mechanical damage formulation The free Helmholtz energy is formulated in the reference configuration for elastic Green strains, Eij =Ee ij, as [63]: Ψ = Ψ(Eij, d) = (1 −d)1 2m0(EijC0 ijklEkl) (4.1) where m0is the material density, Eij =Ee ij is the total strain tensor, 0 ≤d≤1 is the internal damage variable taking values between its initial value 0 and its maximum value 1 and C0 ijkl is the initial constitutive tensor. Considering the second thermodynamic law (Clausius-Duhem inequality – [66] [62] [75]), the mechanical dissipation can be obtained as [63] Ξ = −∂Ψ ∂d ˙ d≥0 (4.2) The accomplishment of this dissipation condition (Equation 4.2) demands that the expression of the stress should be defined as (Coleman method; see [75])
94 Chapter 4. Constitutive modelling of High Cycle Fatigue Sij =m0∂Ψ ∂Eij = (1 −d)C0 ijklEkl (4.3) Also, from the last expressions, the secant constitutive tensor Cs ijkl can be obtained as: Cs ijkl(d) = ∂Sij ∂Eij =m0∂2Ψ ∂Eij∂Ekl = (1 −d)C0 ijkl (4.4) where Sij is the stress tensor for a single material point. 4.2.2 Threshold damage function oriented to fatigue analysis. Phenomenological approach The effects caused by applying an increasing number of loading cycles are taken into account by means of a proposed fred(N, Smax, R) function. This function is introduced in the above formulation in the expression of the damage threshold surface, FD(Sij, d), proposed by [75], [108] and [83]. The number of cycles Ncan then be incorporated as a new variable. This enables the classical constitutive damage formulation to account for fatigue phenomena by translating the accumulation of number of cycles into a readjustment of the damage threshold function. The non-linear behaviour caused by fatigue is introduced in this procedure implicitly, by incorporating a fatigue state variable, fred(N, Smax, R), that is irreversible and depends on the number of cycles, the maximum value of the equivalent stress in the material, Smax, and on the factor of reversion of the equivalent stress, R=Smin/Smax. This new variable affects the residual strength of the material by modifying the damage threshold, FD(Sij , d, N), either on the equivalent stress function fD(Sij ) (equation 4.5), or on the damage strength threshold ¯ KD(Sij, d)(equation 4.6) [100]. FD′(Sij, d, N) = fD(Sij) fred(N, Smax, R) | {z } fD′(Sij ,N,R) −¯ KD(Sij, d)≤0 (4.5)
4.2. HCF damage model 95 FD′′ (Sij, d, N) = fD(Sij)−¯ KD(Sij, d)·fred(N, Smax, R) | {z } KD′(Sij ,d,N) ≤0 (4.6) In the above, fD′=fD/fred(N, Smax, R),is the reduced equivalent stress function in the undamaged space, KD′(Sij, d, N) is the fatigue damage strength threshold, and d=∫t 0˙ ddt the damage internal variable. In the following, the form in equation 4.5 has been used for the damage threshold criterion. The evolution of the damage variable is defined as: ˙ d= ˙µ∂FD ∂fD(4.7) being µthe consistency damage factor, which is equivalent to the consistency plastic factor defined in [63]. Consequently, for the isotropic damage case, ˙ d=˙µ fred (4.8) 4.2.3 Particularization of the damage threshold function for exponential softening The type of softening to be defined in the general damage criterion depends on the problem to be solved. The scalar function defining the evolution of the damage threshold must be monotonous and with a value ranging from 0 to 1. In various publications about the scalar damage problem, the stress behaviour with softening is represented in a variety of forms. Particularly, in Oliver et al. [83] the following function is proposed, G[¯ KD(d)]= 1 −¯ KDmax ¯ KD(d)eA(1− ¯ KD(d) ¯ KDmax )with 0 ≤¯ KDmax ≤¯ KD(d) (4.9) This function can also be expressed as,
96 Chapter 4. Constitutive modelling of High Cycle Fatigue G[fD′(S0, N)]= 1 −fD′ 0(S0, N) fD′(S0, N)e A(1− fD′ (S0,N) fD′ 0(S0,N))with fD′ 0(S0, N) = ¯ KDmax (4.10) where Ais a parameter that depends on the fracture energy of the material and fD′(S0, N) = fD(S0)/fred(Smax, N, R). The value of fD′ 0(S0, N) = ¯ KDmax is obtained from the fulfilment of the damage criterion for the first threshold of degradation. This complies with G[fD′ 0(S0, N)]−G[¯ KDmax]= 0 , and G[fD′ 0(S0, N)]=G[¯ KDmax]≡0. The A parameter is calculated from the dissipation expression shown in equation Ξ = Ψ0˙ d≥0, particularized for a uniaxial process subjected to a growing monotonic load. The parameter deduction can be obtained from [86] and has the following expression for exponential softening: A=1 C0gf (τ0)2−1 2 (4.11) 4.2.4 Function of residual strength reduction for fatigue – W¨ohler curve definition W¨ohler or ”Stress-Number of cycles” (S-N ) curves (figure 4.1) are experimentally obtained by subjecting identical smooth specimens to cyclic harmonic stresses and establishing their life span measured in number of cycles. The curves depend on the level of the maximum applied stress and the ratio between the lowest and the highest stresses (R=Smin/Smax). In figure 4.1b Slim is the endurance limit for a reversion factor of -1 and S0 fis the material elastic limit. In figure 4.1a the instantaneous stress level is depicted, while in figure 4.1b the cyclic stress is represented only by the maximum value it reaches in every cycle. Usually, S- Ncurves are obtained for fully reversed stress (R=Smin/Smax=-1) by rotating bending fatigue tests. S−Ncurves are, therefore, fatigue life estimators for a material point with a fixed maximum stress and a given ratio R. If, after a number of cycles lower than the cycles to failure, the cyclic load stops, a change in the elastic threshold
4.2. HCF damage model 97 Figure 4.1: a: Stress evolution at a single point; b: S−N(W¨ohler’s) Curves of the material is expected due to accumulation of fatigue cycles. Furthermore, if the number of cycles exceeds Nf, being Nf the fatigue life as resulting from figure 4.2, the material will fail with the consequent reduction of strength and stiffness. The change in strength is quantified by the strength reduction function, fred(N, Smax, R), while the change in stiffness is taken into account by means of the damage parameter. In figure 4.2, Seis the endurance limit for any given reversion factor and Sth!!!!!!!!!! is the elastic threshold limit. Figure 4.2: Schematic representation of the evolution of the residual strength with the applied load and number of cycles In the case of a cyclic load with constant Smax and Rthroughout the entire life of a material, the S−Ncurve is sufficient for determining fatigue life. However, when dealing with different load interactions the main focus resides on the residual strength curve. The curve quantifies the loss of strength in the material as the
104 Chapter 4. Constitutive modelling of High Cycle Fatigue and having reached the S-N curve, stress in the material progressively relaxes as it suffers damage until total rupture. In the case of applying different cyclic loads, damage can appear either due to fatigue or due to a new load being applied that leads to stress values that surpass the elastic threshold. In both cases the model will jump automatically from the large increments phase to the load-tracking phase. Even if the different cyclic loads applied induce stress levels below the elastic threshold, when passing from one cyclic load to another one of different characteristics an activation of the load-tracking is required. This is necessary regardless of the elastic regime due to the fact that, by applying a new load, the maximum equivalent stress induced and/or the reversion factor has changed and, consequently, the fatigue parameters calculated for the first load are no longer valid. The flow chart presented in figure 4.4 shows the operations conducted in both phases, as well as the conditions required to jump from load-tracking to large increments. These jumps are indicated with hyphenated arrows. The algorithm is user controlled by means of two parameters. The first one is the tolerance at which the reversion factor norm (defined in equation 4.18) is considered to have converged. If, for instance, a numerical tolerance of 10−10 is used, time advance runs the risk of being continually conducted in the loadtracking phase. This would lead to a dramatic increase in computational time. On the other hand, if the tolerance is set too high the model may no longer capture changes in the cyclical load applied, leading to an incorrect life prediction. The tolerance used for the calculation of the numerical examples presented in section 4 was 10−4and the author recommends this value for future use of the strategy. The second parameter that allows the user to control the developed stepwise load advancing algorithm is the number of cycles chosen as time step for the large increments phase. The influence it has is in accordance with the level of nonlinearity of the problem. While a too low number of cycles used as step implies an increase in computational time, a too big one can lead to loss of solution convergence. A calibration analysis consisting of a study of the solution convergence depending on the number of cycles used as a step is highly recommended. The analysis should begin by using large steps. Then the Ncused as a step should be progressively lowered until convergence is reached, as this would ensure the lowest computational time.
4.3. Stepwise load advancing strategy 105 Figure 4.4: Flow chart for the stepwise advancing algorithm
106 Chapter 4. Constitutive modelling of High Cycle Fatigue 4.4 Numerical examples The capabilities of the stepwise load-advancing strategy, together with the fatigue constitutive model presented, will be shown with several simulations made over a hexahedral finite element subjected to cyclic loads. These examples will illustrate the fatigue behaviour under a single cyclical load and under load interaction of two different cyclic loads. Also, the material behaviour is shown when combining a cyclical load with a monotonic one. After that, the model is validated comparing the results obtained from the numerical simulation with the results provided by the experiment presented in Marines et al. [68]. All the examples presented in this section have been calculated with the PLCd finite element code [98], where the formulation presented here has been implemented. In order to understand the capabilities of the stepwise load advancing strategy, a test case of one linear hexahedral element with 8 integration points will be presented. A single element was chosen for the simulation due to its reduced computational cost and due to the fact that it suffices for accurately showing material behaviour as described by the formulation presented. 4.4.1 Problem definition. Geometry and material. The element has one of its faces subjected to a cyclical displacement while the opposite face has boundary conditions that fix its longitudinal displacement, allowing transversal expansion and contraction. Geometry dimensions are 10x10x10mm. The material used has the following characteristics: Young modulus = 2.01 x 105MPa ; Poisson ratio = 0.3 ; Static elastic threshold is Su= 838.9MPa and the material fracture energy has a value of Gt= Gc= 20 kN*m/m2. The damage model used has exponential softening and a Von Mises failure surface. The S−Ncurve for this material was obtained using the analytical formulation described in [113]. The parameters required in order to correctly describe the curve are Su,Smax and R. One of the model’s particularities is the progressive loss of resistance leading to the initiation of damage, represented in the strength reduction curve. In order for it to be clearly differentiated from the W¨ohler curve, a direct jump to the point
4.4. Numerical examples 107 where damage initiates was not done. Rather, an approximation of the damage initiation point was made by choosing a suitable number of cycles as the time step. The first two numerical simulations presented exhibit a load history composed of a single cyclical load, while the last two simulations consist of applying both cyclical loads in different order. The characteristics of the cyclical loads taken into account are: for the first one, S1, a reversion factor of 0.3, a minimum displacement of 0.0114mm and a maximum displacement of 0.038mm; in the second case, S2, the first load applied has a null reversion factor, a maximum displacement of 0.035mm and a null minimum displacement. The number of cycles adopted as a step for the large increments phase in the both cases is 106cycles. For the combination cases the load applied is the first one, S1, and, after 106 cycles, this load is replaced by S2. The number of cycles used as a step for the large increments phase in this case is 105cycles. In the second combination case the order of loads applied has been changed. First, load 2 is applied 106cycles and afterwards the material continues to be loaded with load 1 until total failure. The number of cycles adopted as a step for the large increments phase in this case is also 105cycles. 4.4.2 Single cyclical load Table 4.1 shows the stresses obtained at each integration point by the imposed displacement presented in figure 4.5, as well as the fatigue life provided by the FEM model. The stresses induced by the cyclic displacement applied lead to a fatigue life, according to the material W¨ohler curve, of 4,9 x 106cycles. This number of cycles marks the beginning of the nonlinear process and, therefore, of the energy dissipation. In figure 4.6, the stress in the specimen, the material W¨ohler curve, the residual strength variable and the material damage value are presented. It can be seen that, while the residual strength curve is above the Wohler fatigue life curve, there is no stress alteration or damage accumulation.
108 Chapter 4. Constitutive modelling of High Cycle Fatigue (normalized with threshold limit) Case code Reversion factor Max. Stress PG Min. Stress PG Med. Stress PG Nc when damage initiates S10,3 0,91 0,273 0,59 4,90E+06 Table 4.1: Characterization of the tensional state induced by the single load S1 The stress level shown refers to the instantaneous stress divided by the initial elastic threshold. It can be seen that at the beginning an initial load-tracking stage is necessary for recording the characteristics of the stress evolution: reversion factor, maximum stress value and stress amplitude in every cycle. When the cyclic stress characteristics do not change from one loading cycle to the other (at every Gauss point) large increments start to be applied, where the load is maintained at the maximum value reached in previous cycles and only the number of cycles variable increases. At this point the material is considered to be in an elastic state but the evolution of the S-N and of the residual strength curves continues to be monitored. Once the number of cycles applied reaches the fatigue life defined by the W¨ohler curve for that level of maximum stress, event marked by the stress curve intersecting the W¨ohler curve, it also intersects the residual strength curve. After this point, the stress in the material is higher than the residual strength and a softening process begins with the consequent increase of the damage variable. As soon as this event occurs at the first Gauss point a load-tracking stage is automatically activated for the entire finite element model. This is necessary as the onset of the degradation process leads to a change in the internal forces and a new equilibrium configuration is reached. When this equilibrium configuration has stabilized under small increments, the stress characteristics from one cycle to the other remain constant. This enables the application of a large increment, maintaining the load at the maximum level reached in previous stable cycles. However, when applying this large increment the equilibrium is lost again as the structure is pushed further in the nonlinear zone with a consequent damage accumulation and stiffness loss. This effect can be seen in the stress relaxation occurring at the end of each large scale increment (figure 4.6 and figure 4.7).
4.4. Numerical examples 109 1e-005 1.5e-005 2e-005 2.5e-005 3e-005 3.5e-005 4e-005 1 10 100 1000 10000 100000 1e+006 1e+007 1e+008 Applied displacement (m) No. cycles (-) (log. scale) small increments in load-tracking phase large increments phase Figure 4.5: Applied displacement for load case S1 From that point forward, after each large increment where ˙ d > 0, the loadtracking phase is automatically activated so that damage evolution can be monitored from cycle to cycle. If, after describing several cycles with small increments, the stress state throughout the solid has stabilized, a new large increment can be applied. This process is repeated automatically until the material reaches a state of complete degradation. Figure 4.7 zooms the end part of figure 4.6 to show more clearly the material performance described. The load-tracking phase is represented by the vertical lines. The large increments phase is represented by the in between segments. Both figure 4.6 and figure 4.7 have a logarithmical scale along the horizontal axis. In figure 4.8, the effects of material degradation are shown in the stress-strain curve. The vertical axis refers to the instantaneous stress level divided by the material elastic limit. The large increments phase occurs only when the displacement is maintained at its maximum value and ε=εmax. Therefore, it is represented in this figure by the vertical lines descending from the point of maximum stress. The stress interval represented by each jump in the stress level quantifies the
110 Chapter 4. Constitutive modelling of High Cycle Fatigue 0 0.2 0.4 0.6 0.8 1 1 10 100 1000 10000 100000 1e+006 1e+007 1e+008 Stress normalized with elastic threshold / Damage (-) No. cycles (-) (log. scale) Instantaneous stress level Fatigue life Residual strength Damage internal variable Figure 4.6: Parameters of interest for the fatigue analysis under load S1 stress softening caused by a single, large number of cycles, interval. Each of these stress-softening intervals is followed by a few unloading (until minimum displacement) - loading cycles. These mark the load-tracking phase where a clear change in material stiffness is visible. It can be seen that, as the material progressively suffers loss of stiffness, for the same large step there is less stress softening. Furthermore, in order to demonstrate the good accuracy of the method, this simulation has been done with four different sizes for the large increments phase. Figure 4.9 presents the evolution of the damage internal variable (as resulting from equation 4.8) with the number of cycles in all four cases. It can be seen that, even though the simulation is done by using different steps in the large increments phase: 50.000, 100.000, 1 x 106and 5 x 106cycles, the damage variable has the same evolution. As indicated in Section 4.3.4 the number of cycles used as a step in the large increments phase is a key parameter for the load-advancing algorithm. In table 4.2 the computational time obtained for the different Ncsteps is presented. It
4.4. Numerical examples 111 0 0.1 0.2 0.3 0.4 0.5 0.6 0.7 0.8 0.9 1 4.2e+006 8.4e+006 1.7e+007 3.4e+007 Stress normalized with elastic threshold / Damage (-) No. cycles (-) (log.scale) Instantaneous stress level Fatigue life Residual strength Damage internal variable Figure 4.7: Parameters of interest for the fatigue analysis under load S1in the nonlinear zone can be seen that, even though the simulation is made on a single linear element, computational time can vary considerably depending on the number of cycles chosen as time step. A comparison was made between the computational time required when using the proposed load-advancing strategy and the computational time needed if in the nonlinear stage only load-tracking were to be used. As it can be seen from table 4.2, the CPU time needed in the case of a step of 1 x 106cycles was 30 seconds for a total analysis of 53.5 x 106cycles, out of which 4.9 x 106cycles consisted of elastic behaviour. When advancing only by load-tracking after the 4.9 x 106elastic cycles, in 10 hours of computational time only 84.000 cycles were computed, with a correspondant damage level at the end of the 84.000 cycles of 0.018. Taking into account this rate of advance, if the entire analysis of 53.5 x 106cycles were to be conducted under load-tracking, a computational time of 265 days would be needed. This study was carried out on only one linear element. In real-life simulations, the dimensions of the problem are much larger and load history is more complex and this demonstrates that it is of the upmost importance having a load-saving advancing strategy.
112 Chapter 4. Constitutive modelling of High Cycle Fatigue 0 0.1 0.2 0.3 0.4 0.5 0.6 0.7 0.8 0.9 1 0 0.0005 0.001 0.0015 0.002 0.0025 0.003 0.0035 0.004 Stress normalized with elastic limit (-) Strain (-) Load-tracking phase Large increments phase Figure 4.8: Stress-Strain at integration point for load S1 An important feature of the constititutive model coupled with the load-advancing strategy is the ability to account for the order in which different loads are applied within a determined load history. In order to demonstrate this, a different regular cyclic load will be shown and, in the next section, the combination of the two loads, S1and S2will be analysed. The characteristics of the tensional state induced by the load S2are shown in table 4.3. In figure 4.10, the stress evolution at the integration point, the material W¨ohler curve, the residual strength variable and the material damage value are presented, and in figure 4.11 the effects of material degradation are shown in the stress-strain curve. 4.4.3 Load history with two different cyclical loads In table 4.4 the stresses generated at integration point level by the imposed maximum and minimum displacements are included. These are displayed for the two cyclical loads applied, S1and S2, as well as the fatigue life resulting from
4.4. Numerical examples 113 0 0.1 0.2 0.3 0.4 0.5 0.6 0.7 0.8 0.9 1 0 1e+007 2e+007 3e+007 4e+007 5e+007 6e+007 Damage (-) No. cycles (-) (log. scale) 50.000c/step 100.000c/step 1.000.000c/step 5.000.000c/step Figure 4.9: Evolution of the damage internal variable with the number of cycles the FEM model if only one of the loads, be it S1or S2, were to be applied until fracture. Table 4.4 also includes the number of cycles at which damage starts when applying both S1and S2. The simulation of the load combination was made by first imposing the S1load during 106cycles, followed by load S2being applied from 106cycles to 108cycles. By applying first load S1, followed by load S2, the resulting life for the material is 3,62 x 106cycles, less than if only load S1were applied, but more than if only S2 were applied. This shows that the formulation is capable of taking into account the effect of a cyclical load even if it is applied for a number of cycles that does not lead to failure. This is achieved by quantifying the strength reduction caused by each event in the load history and by dynamically describing the S−Ncurve according to changes in load characteristics. In figure 4.12 it can be seen how the slope of both curves, residual strength and S−Ncurve, changes as a different load starts being applied. This is possible due to the load-tracking phase being automatically activated once a change in the load is detected, as can be seen from the vertical line dividing the two maximum stress levels exhibited. The intermediate load-tracking phase appears as a straight line
120 Chapter 4. Constitutive modelling of High Cycle Fatigue 0 0.2 0.4 0.6 0.8 1 1 10 100 1000 10000 100000 1e+006 1e+007 1e+008 Stress normalized with elastic threshold / Damage (-) No. cycles (-) (log. scale) Instantaneous stress level Fatigue life Residual strength Damage internal variable Figure 4.14: Parameters of interest for the fatigue analysis under loads S2+S1 In figure 4.19 the dissipative cost of the strength reduction occurring in the elastic zone can be seen by comparing the stress-strain curve for the monotonic case and for the other cases. The maximum energy dissipation cost (maximum area difference with respect to the monotonic curve) is visible for the case with only cyclic loading applied (case 3 in table 4.5). For a final overview on the different stress histories used in this analysis figure 4.20 can be consulted. The stress due to monotonic loads has been marked for each case analysed.
4.4. Numerical examples 121 0 0.2 0.4 0.6 0.8 1 0.0e+000 5.0e-004 1.0e-003 1.5e-003 2.0e-003 2.5e-003 3.0e-003 3.5e-003 4.0e-003 Stress normalized with elastic limit (-) Strain (-) Load-tracking phase Large increments phase Figure 4.15: Stress-Strain at integration point for loads S2+S1
122 Chapter 4. Constitutive modelling of High Cycle Fatigue Instantaneous stress level Residual strength Fatigue life Instantaneous stress level for the monotonic case 1 10 100 1000 10000 100000 1e+006 1e+007 1e+008 No. of cycles (-) (log. scale) 0 0.2 0.4 0.6 0.8 1 Damage internal variable (-) 0 0.2 0.4 0.6 0.8 1 Stress normalized with the elastic limit (-) Figure 4.16: Parameters of interest for the fatigue analysis under load combination 1 in 3d representation
4.4. Numerical examples 123 Instantaneous stress level Residual strength Fatigue life Instantaneous stress level for the monotonic case 1 10 100 1000 10000 100000 1e+006 1e+007 1e+008 No. of cycles (-) (log. scale) 0 0.2 0.4 0.6 0.8 1 Damage internal variable (-) 0 0.2 0.4 0.6 0.8 1 Stress normalized with the elastic limit (-) Figure 4.17: Parameters of interest for the fatigue analysis under load combination 2 in 3d representation
124 Chapter 4. Constitutive modelling of High Cycle Fatigue Instantaneous stress level Residual strength Fatigue life Instantaneous stress level for the monotonic case 1 10 100 1000 10000 100000 1e+006 1e+007 1e+008 No. of cycles (-) (log. scale) 0 0.2 0.4 0.6 0.8 1 Damage internal variable (-) -0.2 0 0.2 0.4 0.6 0.8 1 Stress normalized with the elastic limit (-) Figure 4.18: Parameters of interest for the fatigue analysis under load S2in 3d representation
4.4. Numerical examples 125 0 1e+008 2e+008 3e+008 4e+008 5e+008 6e+008 7e+008 8e+008 0 0.001 0.002 0.003 0.004 0.005 0.006 Instantaneous stress (Pa) Strain (-) case 1 case 2 case 3 monotonic Figure 4.19: Comparison between the stress-strain curves at the integration point for different load combinations
126 Chapter 4. Constitutive modelling of High Cycle Fatigue Residual strength Fatigue life Stress during monotonic load Instantaneous stress level for case 1 Instantaneous stress level for case 2 Instantaneous stress level case 3 1 10 100 1000 10000 100000 1e+006 1e+007 1e+008 No. of cycles (-) (log. scale) 0 0.2 0.4 0.6 0.8 1 Damage internal variable (-) -0.2 0 0.2 0.4 0.6 0.8 1 Stress normalized with the elastic limit (-) Figure 4.20: Comparison between the stress evolution at the integration point for different load combinations in 3d representation
4.5. Validation of the formulation proposed 127 4.5 Validation of the formulation proposed 4.5.1 Problem definition. Geometry and material. The experiment undertaken by Marines et al. [68] has been chosen to validate the stepwise load advancing strategy presented in this work, together with the continuum damage model for fatigue described in section 4.2. In table 4.6, the material characteristics given by the aforementioned authors are presented along with the shape and dimensions of the fatigue specimen adopted in the experiment. The experimental results obtained with a loading frequency of 20 kHz and a reversion factor R=−1 have been taken into account for the comparison with numerical results. Ed(10kHz) (GPa) Ed(20kHz) (GPa) σy(0.2%) (MPa) UTS (MPa) A (%) ρ (kg/m3) 208.3 211.5 608 878 20 7850 Table 4.6: Material properties of HSLA steel, D38MSV5S 4.5.2 Finite element model The fatigue specimen presented in figure 4.21 has been reproduced by means of a finite element model. Due to the symmetrical nature of the geometry, loading and boundary conditions, only half of the specimen has been modelled in order to minimize computational time. The semi-cylindrical volume has been meshed with linear hexahedral elements as shown in figure 4.22. The mesh has 2666 nodes and 1920 elements. Each finite element is described with eight integration points. The boundary conditions applied are shown in figure 4.23. The specimen is restrained at one end and subjected to a cyclical displacement at the other end. The entire base is defined with a symmetry condition.
128 Chapter 4. Constitutive modelling of High Cycle Fatigue Figure 4.21: Shape and dimension of ultrasonic fatigue specimen as given by Marines et al.[68] The analytical formulation for the S−Ncurve used by the numerical model was the one presented in [113]. The parameters used for the adjustment of the curve to the experimental one proposed by Marines et al. [68] are Su= 608Mpa, Slim=325Mpa, α=β=1.3; a correction factor of 1.23 was applied when calculating the auxiliary term AUX = 1/1.26 + R/3.3. 4.5.3 Results and discussion In figure 4.24, the results obtained by Marines et al. [68] are presented. As expected, a scatter of test results can be seen both for 20 kHz resonating material and for the 30 kHz one. Since the material characteristics taken into account for the numerical analysis are that of the 20 kHz one, simulations have been run only
4.5. Validation of the formulation proposed 129 Figure 4.22: Finite element mesh of linear hexahedral elements with the maximum stress levels exhibited for this particular testing frequency. The experimental results showed that, even though the geometry and loading conditions are axisymmetric, the failure mode is not symmetric [68]. 4.5.3.1 Validation of the results obtained with the numerical simulation The expression for the S−Ncurve proposed in figure 4.24 by Marines et al. [68] has been compared to the numerical results obtained from the described finite element model. The comparison can be seen in figure 4.25. Since the model has a deterministic nature, no scatter can be seen in numerical results. The numerical data depicted in figure 4.25 is in accordance with table 4.7 where the information on the exact characteristics of each simulation case is given. Some observations are to be made, however, in order to better understand the results presented in figure 4.25. The points signalled as results obtained with the proposed formulation, mark the start of the stiffness reduction. In a force controlled test, when the force level is taken to the following maximum after the fatigue life depicted in figure 4.25, abrupt failure occurs. However, as the numer-