Full text
Challenging Isodimorphism Concepts: Formation of Three Crystalline Phases in Poly(hexamethylene-ran-octamethylene carbonate) Copolymers Yilong Liao, Ricardo A. Pérez-Camargo, Haritz Sardon, Antxon Martínez de Ilarduya, Wenxian Hu, Guoming Liu,*Dujin Wang, and Alejandro J. Muller* Cite This: Macromolecules 2023, 56, 8199−8213 Read Online ACCESS Metrics & More Article Recommendations * sı Supporting Information ABSTRACT: In this work, poly(hexamethylene-ran-octamethylene carbonate) copolycarbonates were synthesized by melt polycondensation in a wide range of compositions. The copolymers displayed some of the characteristic isodimorphic thermal behavior, such as crystallization for all the compositions and a pseudoeutectic behavior of the melting temperature (Tm) versus composition. The pseudoeutectic point was located at 33 mol % poly(octamethylene carbonate) (POC) content (i.e., corresponding to the PH67O33C copolymer). Surprisingly, the crystallinities (Xc) for a wide range of copolymer compositions were higher than those of the parent components, a phenomenon that has not been observed before in isodimorphic random copolymers. The structural characterization, performed by wide-angle X-ray scattering (WAXS) and small-angle X-ray scattering experiments, revealed unexpected results depending on composition. On the one hand, the poly(hexamethylene carbonate) (PHC)- and POC-rich copolymers crystallize in PHC- and POC-type crystals, as expected. Moreover, upon cooling and heating, in situ WAXS experiments evidenced that these materials undergo reversible solid−solid transitions [δ-α(PHC) and δ-α-β (POC)] present in the parent components but at lower temperatures. On the other hand, a novel behavior was found for copolymers with 33−73 mol % POC (including the pseudoeutectic point), which are those with higher crystallinities than the parent components. For these copolymers, a new crystalline phase that is different from that of both homopolymers was observed. The in situ WAXS results for these copolymers confirmed that this novel phase is stable upon cooling and heating and does not show any crystallographic feature of the parent components or their solid−solid transitions. FTIR experiments confirmed this behavior, revealing that the new phase adopts a polyethylene-like chain conformation that differs from the trans-dominant ones exhibited by the parent components. This finding challenges the established concepts of isodimorphism and questions whether a combination of crystallization modes (isodimorphism and isomorphism) is possible in the same family of random copolymers just by changing the composition. 1. INTRODUCTION Aliphatic polycarbonates (PCs) have been developed as a promising class of biodegradable polymer due to their biocompatibility, biodegradability, nontoxicity, and excellent chemical and physical properties. 1−4 In particular, they do not generate any acidic compounds upon degradation through surface erosion, 5,6 which allows them to be suitable for medical applications (e.g., surgical sutures, bone fixation, and drugcontrolled release). 3,7 Moreover, PCs are also intriguing solid polymer electrolytes because of their remarkable ionic conductivity, excellent electrochemical stability, and high lithium transference. This property makes PCs a potential alternative material to poly(ethylene oxide). 8,9 The advances in synthesis methods allow obtaining PCs without potential toxicity issues from metal catalysts and with a practically unlimited range of chain lengths, nCH2. 4,10−12 The use of the polycondensation between diols and dimethyl carbonate opened the possibility of creating PCs with a wide range of nCH2 and permitted studying the even−odd effect on PCs with nCH2 = 6 to 12. 13 Such advances in the synthesis methods allow the preparation of copolycarbonates that combine comonomers (i.e., PCs) with different nCH2, aiming to widen the range of properties of these materials. Copolymerization offers a better modification over the Received: June 28, 2023 Revised: September 1, 2023 Published: October 11, 2023 Article pubs.acs.org/Macromolecules © 2023 The Authors. Published by American Chemical Society 8199 https://doi.org/10.1021/acs.macromol.3c01265 Macromolecules 2023, 56, 8199−8213 This article is licensed under CC-BY 4.0 Downloaded via 147.83.201.96 on October 24, 2023 at 08:17:02 (UTC). See https://pubs.acs.org/sharingguidelines for options on how to legitimately share published articles.
structures than blends to achieve tunable properties matching various applications. 14−17 Random covalent links ensure the miscibility of the material obtained from different comonomers that might otherwise be immiscible. This allows for the adjustment of the crystallinity degrees and tailoring of biodegradation rates by introducing a comonomer and varying the composition. The crystallization behavior of random copolymers is an exciting topic since they can crystallize in three different crystallization modes: isomorphism, isodimorphism, and comonomer exclusion or no-crystallization mode. 18 All of these modes depend on the comonomer exclusion/inclusion balance. Isomorphic copolymers are characterized by total comonomer inclusion within the crystal lattice (i.e., cocrystallization), which occurs under strict molecular features, 19−21 e.g., similar chemical structures of the repeating units. This total comonomer inclusion is evidenced by the crystallization in all of the compositions, exhibiting thermal and structural properties that show a linear dependence on the composition. On the contrary, when total comonomer exclusion dominates, the resulting random copolymers can only crystallize in a limited composition range, as even smaller comonomer contents can limit the crystallization of the second comonomer-rich phase. Isodimorphism is an intermediate case between the crystallization modes mentioned above and can be viewed as its combination. In isodimorphic copolymers, a competition between inclusion and exclusion occurs, where typically inclusion can only be tolerated up to a certain degree that depends on the chemical affinity of the comonomers. Comonomer exclusion hinders the crystallization of the major phase, provoking the depression of different physical properties, e.g., crystallinity degree, crystallization (Tc), and melting (Tm) temperatures. Partial comonomer inclusion, as evidenced by the changes in the major crystalline phase, e.g., different interplanar distances within the lattice unit cell of the copolymers compared with the parent components, avoids the complete depression of these properties, allowing crystallization for all of the compositions. This particular comonomer exclusion/inclusion balance provokes a pseudoeutectic behavior of the thermal transitions, e.g., Tm, as a function of the comonomer content. Considering AxBycopolymers, on one side of the pseudoeutectic point, where the material typically exhibits minimum values of Tcand Tm, the material crystallizes in the A-rich crystalline phase with the inclusion of some percentage of B counits. On the opposite side, the material crystallizes in the B-rich crystalline phase with the inclusion of some percentage of A counits. In our previous findings, we observed the coexistence of both A-rich and B-rich crystalline phases at the pseudoeutectic point, as detected by wide-angle X-ray scattering (WAXS) experiments or double melting (sequential melting of each phase) detected by differential scanning calorimetry (DSC). 15,22−25 The chemical demands of isodimorphism are not as strict as those of isomorphism; thus, isodimorphic behavior has been widely reported for several random copolymer systems. In particular, isodimorphism in copolyesters has been thoroughly studied. 15,19,22,23,26−28 In the case of copolycarbonates, a few systems have been prepared to combine aliphatic PCs comonomers with different nCH2 (PCnCH2). Zhu et al. 29 studied PC4-ran-PC6 copolycarbonates, determining that cocrystallization cannot occur, thus limiting the crystallization to the richest compositions in one or another comonomer, i.e., 10:90 and 90:10 PC4-ran-PC6. Similar results were reported by Arandia et al. 15 in PC4-ran-PC7 copolycarbonates in which only compositions with higher contents than 80 mol % PC4 or 80 mol % PC7 can crystallize. These authors explained that rather than comonomer exclusion, which occurs when there is a significant disparity in the chemical structures of the two repeating units, the observed behavior is provoked by the slow crystallization kinetics of both comonomers. It was argued that under the right conditions, e.g., extremely slow cooling, these copolycarbonates should display isodimorphic behavior. The isodimorphic behavior in copolycarbonates is more apparent when PC4 is combined with nCH2 > 7 comonomers. Zhang et al. 11 found that PC4-ran-PC10 copolycarbonates crystallize for all compositions showing a pseudoeutectic behavior with the pseudoeutectic point at 20 mol % of PC10. Therefore, only the richest composition in PC4, i.e., 90:10 PC4-ran-PC10, can crystallize with a PC4 crystalline structure. Arandia et al. 15 reported isodimorphic behavior in PC4-ran- PC12 copolycarbonates. These copolycarbonates crystallize for all compositions, displaying a pseudoeutectic point at 15 mol % of PC12 content. At the pseudoeutectic point, a double melting transition was found due to PC4-rich phase crystals melting at low temperatures, followed by PC12-rich phase crystals melting. Besides the PC4-based combinations, they also studied the PC7-ran-PC12 copolycarbonates, which are also isodimorphic, with a pseudoeutectic point at 20 mol % of PC12 content. The 80:20 PC7-ran-PC12 copolycarbonate displayed a novel behavior since the nonisothermal DSC scans revealed both coincident crystallization and melting despite being a double crystalline structure containing PC7- and PC12-rich crystalline phases detected by WAXS. Recently, Hung et al. 27 studied PC8-ran-PC10 copolycarbonates. These authors found that these materials are isodimorphic with a pseudoeutectic region between 21 and 36 mol % of PC10 content. In addition, they studied the solid−solid transition for those compositions with PC8 content ≥79 mol %. Poly(octamethylene carbonate) (PC8 or POC) exhibits a solid−solid crystalline transition. For POC, Zhao et al. 10 first reported a reversible α-βsolid phase transition, which is analogous to the Brill transition observed in polyamides. 30,31 It was primarily related to the reversible conformational change in methylene sequences, transitioning from a predominantly trans configuration at low temperatures to a coexistence of trans/gauche conformations at high temperatures. Perez- Camargo et al. 32,33 disclosed a new reversible α-δsolid phase transition that occurs at a lower temperature than the α-β phase transition. The δphase is characterized by more efficient packing of methylene groups and ordered chain conformations in comparison to the αphase. A reversible δ-αsolid−solid phase transition has been disclosed in poly(hexamethylene carbonate) (PHC). 32,33 This work represents the first contribution to the study of a new series of aliphatic random copolycarbonates based on POC: poly(hexamethylene-ran-octamethylene carbonate) (PHxOyC), poly(heptamethylene-ran-octamethylene carbonate), and poly(octamethylene-ran-dodecamethylene carbonate) copolycarbonates. Here, we focus on PHxOyC copolycarbonates synthesized using 4-dimethylaminopyridine (DMAP) as an organocatalyst in a two-step polycondensation process. The thermal properties, structure, conformation, and morphology of the PHxOyC copolymers were investigated in Macromolecules pubs.acs.org/Macromolecules Article https://doi.org/10.1021/acs.macromol.3c01265 Macromolecules 2023, 56, 8199−8213 8200
detail. The DSC results demonstrate the isodimorphic-like behavior in these copolymers. Structural characterization shows that PHC- and POC-rich copolymers follow an isodimorphic-like behavior, crystallizing in PHC- or POC- type crystals, including the solid−solid transitions of these materials. But a novel and unique behavior was found for a wide range of compositions. A new stable crystalline phase was observed, similar to those observed in some isomorphic copolymers, without any trace of the crystalline structure of the parent components, not even their solid−solid transitions, instead of the typical mixture of crystalline phases that are found in other isodimorphic copolycarbonates. FTIR confirmed the presence of this new stable phase, which adopts a PE-like chain conformation, differing from the trans-dominant conformations of the parent homopolymers. This finding challenges the isodimorphism concepts and leads us to ask whether a combined isomorphism−isodimorphism crystallization is possible. 2. EXPERIMENTAL PART 2.1. Materials. Dry dimethyl carbonate (DMC) (99+ %) and DMAP (99%) were purchased from Across Organics. Sigma-Aldrich supplied 1,6-hexanediol (99+ %) and 1,8-octanediol (99+ %). Before use, the two diols and DMAP were dried for 5 h. Chloroform (99+ %) and methanol (MeOH) (certified AR for Analysis) were purchased from Fisher Scientific. Tetrahydrofuran (THF) [size exclusion chromatography (SEC) grade] was obtained from Scharlab, toluene (HPLC grade) from Sigma-Aldrich, and deuterated chloroform (99.8%) (CDCl3) from Deutero GmbH. The chemical route for synthesizing copolycarbonates via the melt polycondensation method has been reported in our previous work. 9,15 2.2. Chemical Structure Characterization (NMR and SEC). The 1H and 13C nuclear magnetic resonance (NMR) tests were carried out on Bruker AVANCE NEO 500 spectrometers at room temperature, with CDCl3used as the solvent. We calibrated the spectra using the CDCl3peak (δH= 7.26 ppm and δC= 77.16 ppm). The number-average (Mn) and weight-average (Mw) molecular weights, as well as the dispersity (D), of the synthesized materials were measured by using SEC. The equipment utilized for this purpose consisted of three columns in series (Styragel HR2, HR4, and HR6, with pore sizes ranging from 1 ×102to 1 ×106Å), an LC20 pump (Shimadzu) coupled to a DAWN Heleos multiangle light scattering laser photometer, and a differential refractometer (all from Wyatt Technology Corp., USA). The sample was dissolved in THF (SEC grade) at a concentration of 5 mg/mL, and the analyses were performed at 35 °C using THF as a mobile phase at a flow rate of 1 mL/min. Narrow polystyrene standards were used for calibration. 2.3. Differential Scanning Calorimetry. This study used a PerkinElmer 8500 calorimeter with a controlled liquid nitrogen cooling system, model CLN2, to investigate homopolymers’ and copolymers’ nonisothermal crystallization and melting behavior. The instrument calibration was achieved by using high-purity indium and tin standards. Samples weighing around 5 mg were encapsulated in standard aluminum DSC pans and subjected to DSC experiments in an ultrapure nitrogen atmosphere with a flow rate of 20 mL/min. The DSC experiments were conducted at a scan rate of 10 °C/min over a temperature range of −40−100 °C. Thermal history was erased by heating the samples to 100 °C for 3 min and then cooling down to −40 °C for 1 min to crystallize. Finally, a heating scan was conducted to record the melting endotherms. 2.4. Small-Angle and Wide-Angle X-ray Scattering. Simultaneous small-angle X-ray scattering (SAXS)/WAXS data were obtained at the 1W2A beamline (λ= 1.54 Å) of the Beijing Synchrotron Radiation Facility (BSRF). The WAXS patterns were recorded using a MAR165 CCD detector, with a resolution of 2048 ×2048 pixels (pixel size: 79 μm×79 μm), and the sample-to-detector distance was 263.9 mm with a tilt angle of 15°. In the SAXS configuration, a Pilatus 1 M detector, with a resolution of 981 ×1043 pixels (pixel size: 172 μm×172 μm), was employed. The sample-to-detector distance was 3202 mm. One-dimensional intensity profiles were integrated using the standard procedure with the substrate for background and reported as the scattering intensity versus scattering vector, q= 4πsin θ/λ, in which 2θis the Bragg angle. For nonisothermal measurements, samples were encapsulated in a DSC aluminum pan and placed in a Linkam THMS600 hot stage coupled to a liquid nitrogen cooling system. Simultaneous WAXS/ SAXS diffractograms were recorded every 2 °C as the polymers underwent crystallization and melting. The cooling and heating conditions employed in the nonisothermal DSC experiments were replicated, ensuring that the results obtained from WAXS/SAXS were comparable. 2.5. Fourier Transform Infrared Spectroscopy. The variabletemperature infrared spectra were recorded by a Nicolet 6700 FTIR spectrometer from Thermo Fisher connected to a Linkam FTIR600 hot-stage. The resolution of spectra was 4.0 cm−1, and the acquisition time of each spectrum was 30 s. The samples for FTIR measurements were drop-cast onto potassium bromide (KBr) plates from a solution in chloroform with a concentration of 5 mg/mL. The same thermal protocol described in Section 2.3 was applied. 2.6. Polarized Light Optical Microscopy. The morphology of the sample was studied using an Olympus BX51 polarized light optical microscope equipped with a λplate inserted at 45°with respect to the polarization direction. Images were captured using an Olympus SC50 digital camera, and precise temperature control was achieved with a THMS600 Linkam hot stage connected to liquid nitrogen. The samples were melted on a glass slide covered with a thin glass coverslip and crystallized from the melt. First, the thermal history was erased for 3 min at 100 °C. Next, the samples were cooled to −40 °C at 1 °C/min. The micrographs were taken at −40 °C. 3. RESULTS AND DISCUSSION 3.1. Synthesis and Chemical Characterization. We employed a melt polycondensation synthetic protocol, as outlined in Scheme 1, to synthesize PHxOyC copolymers in a wide range of compositions. The monomers, 1,6-hexanediol, and 1,8-octanediol, were coreacted with DMC catalyzed by DMAP. The syntheses were conducted in a 50 mL roundbottom flask connected to a vacuum. During the initial step, the dried reagents, including DMC, diols, and the organocatalyst DMAP, were added to the flask and placed in an oil bath at 130 °C for 4 h. The temperature was then raised to 180 °C, and a high vacuum was applied overnight to remove the Scheme 1. Synthesis by Polycondensation of Diols with Dimethyl Carbonate of Aliphatic Polycarbonate Copolymers Macromolecules pubs.acs.org/Macromolecules Article https://doi.org/10.1021/acs.macromol.3c01265 Macromolecules 2023, 56, 8199−8213 8201
reaction byproduct. The high temperature and vacuum conditions were critical for increasing the molar masses. To purify the polymers, we dissolved the obtained samples in chloroform and then precipitated them in cold methanol. A 2:1:0.01 molar ratio of DMC/diol/DMAP was used for all reactions. By adjusting the feed contents of 1,6-hexanediol and 1,8-octanediol, PHxOyCs were synthesized. The chemical structures of the copolymers were first analyzed by NMR. Figure 1 provides the 1H NMR and 13C NMR spectra of a representative copolymer with the initial monomer feed of 60:40 (hexanediol/octanediol). The remaining copolymers were also analyzed by 1H and 13C NMR, and the corresponding spectra are provided in Figures S1 and S2. The composition of the resulting copolymer can be quantified by utilizing the integral intensities of the characteristic signals in the 1H NMR spectrum. The chemical shifts and peak assignments are as follows: δ= 4.12 ppm (t, OCOOCH2, 4H·(xPHC +xPOC)), 1.68 ppm (q, OCOOCH2CH2, 4H·(xPHC +xPOC)), 1.41 ppm (t, OCOOCH2CH2CH2CH2CH2CH2OCOO, 4H·xPHC (PHC)), and 1.33 ppm (m, OCOOCH2CH2CH2CH2CH2CH2CH2CH2OCOO, 8H·xPOC (POC)). A triplet between 4.0 and 4.15 ppm is ascribed to the resonance peaks of methylene protons adjacent to the oxygen atom of the carbonate group (4·xPHC for PHC and 4· xPOC for POC), which integrates 4 protons. The integrated area of the rest of the peaks was thus obtained with respect to this area. Specifically, the signal peaks at 1.41 and 1.33 ppm, assigned to the inner methylenes of PHC and POC repeating units, respectively, have an integration value of 5.68. This value comprises 4·xPHC protons from PHC and 8·xPOC protons from POC. Based on these findings, two equations were used to estimate the molar ratio of repeating units (xPOC and xPHC) =x I I 4 POC 1.2 1.5 4.0 4.15 (1) =x x1 PHC POC (2) where I4.0−4.15 denotes an integral area between 4.0 and 4.15 ppm, corresponding to those protons assigned to the methylenes close to the oxygen atoms, while I1.2−1.5 represents the area between 1.2 and 1.5 ppm, representing those inner methylenes of the PHC and POC repeating units. Therefore, the molar ratio of repetitive units in this copolymer was calculated to be around 58 mol % PHC and 42 mol % POC, and thereby, the sample was named PH58O42C based on the calculated molar ratio of PHC and POC in the copolymer. The final compositions of other copolymers were determined by using the same methodology, and the results are listed in Table 1. Although the calculated compositions are not identical to the feed ratio, the two values are very close. The distribution of the two comonomers plays a crucial role in determining the final properties of copolymers. The sensitivity of 13C NMR to the difference of carbon atoms within different chemical environments can be used to obtain valuable information on the distribution of the repeating units along the backbone and the degree of randomness. 34 To this end, Figure 1b presents the 13C NMR spectrum of copolymer PH58O42C, and a precise assignment of the characteristic peaks was made along with the NMR spectrum to determine its microstructure. The signals around 155.3 and 67.8 ppm split into three and four peaks, respectively, and were assigned to carbonyl and -OCH2carbon resonance. The three peaks located at 155.31, 155.34, and 155.37 ppm were further attributed to different dyad sequence distributions: HH (PHCPHC), HO (PHC-POC), OH (POC-PHC), and OO (POCPOC), respectively. Additionally, the four split peaks at 67.70, 67.74, 67.90, and 67.94 ppm were assigned to the HO, HH, OO, and OH dyads. In this way, the degree of randomness (R) could be calculated with the −OCH2carbon resonance signals at around 67.7 ppm using eqs 3−5 = + + N I I I 1 2 PHC HH HO OH (3) = + + N I I I 1 2 POC OO HO OH (4) = +R N N 1 1 PHC POC (5) where IHH,IHO,IOH, and IOH are the integration of the −OCH2 carbon resonance signals of HH, HO, OH, and OO, respectively. NPHC and NPOC represent the number-average sequence length of the PHC and POC repetitive units, respectively. Regarding copolymer microstructures, R= 1 indicates a random copolymer, while R= 2 means the copolymer is alternating, and in a block copolymer, R∼0. As seen in Figure S3, similar NMR analyses were conducted on all copolymers, and using eqs 3−5, the degrees of randomness Figure 1. (a) 1H and (b) 13C NMR spectra of copolymer PH58O42C in CDCl3. The peaks’ assignment is marked with red letters in the chemical structure. Macromolecules pubs.acs.org/Macromolecules Article https://doi.org/10.1021/acs.macromol.3c01265 Macromolecules 2023, 56, 8199−8213 8202
thus were obtained. As summarized in Table 1, the Rvalues are close to 1, indicating a random microstructure of the synthesized PHxOyC copolymers. Molecular weight is another important factor affecting the properties of the materials. The molecular weights and dispersity were determined by SEC. As shown in Figure S4 and Table 1, the Mwof the polymers obtained falls mostly in the range of 13,000−28,000 g/mol, with dispersity of 1.80− 2.40, which are common values for polycondensation polymers. These results demonstrate a comparable level, which facilitates further exploration. 3.2. Nonisothermal DSC Experiments. The thermal properties of PHC and POC homopolymers and PHxOyC copolymers were examined by nonisothermal DSC scans. Figure 2 displays the standard nonisothermal cooling (Figure 2a) and second heating (Figure 2b) DSC scans, and all relevant transition temperatures and enthalpies are listed in Table 2. As reported in previous papers, 9,13 POC crystallizes and melts at higher temperatures than PHC. Both parent components show (see an asterisk in Figure 2) exothermic and endothermic signals that correspond to the α-δand δ-α reversible solid−solid phase transition, respectively. 10,32,33 In POC, a shoulder in between the δ-αtransition and the melting peak (Tm) corresponds to the reported α-βtransition. 10,32 This transition is easier to detect by WAXS experiments (see Section 3.3). Figure 2b shows the δ-αtransition for PH5O95C at lower values than for the POC. Details on how this transition is influenced by copolymerization are presented below. Figure 2 shows that despite the random comonomer distribution (confirmed previously by 13C NMR), all PHxOyC copolymers can crystallize during cooling (Figure 2a), displaying a single crystallization peak (Tc). The DSC heating curves are plotted in Figure 2b. It can be seen that Tcand Tm of the copolymers are located below those exhibited by the parent components. Both exo- and endothermic signals are broader for PHC-rich compositions and sharper for POC-rich and intermediate compositions. The neat PHC and its PHC- rich copolymers (PH85O15C and PH78O22C) display an extra endothermic signal, corresponding to melting recrystallization behavior similar to the PHC. 32,35 The thermal transition temperatures extracted from Figure 2 are plotted as a function of the POC content in Figure 3. Figure 3a illustrates the correlation between the molar fraction of POC, i.e., the comonomer content, and the corresponding Tcand Tmof all materials. From a thermodynamic point of view, a pseudoeutectic-like behavior of the isodimorphic copolymers was observed, as characterized by a decreasing trend in Tcand Tmas the composition moves away from the two homopolymers of PHC and POC. This decreasing trend, which is also roughly observed in the composition-dependent behavior of the nucleation density on polarized light optical microscopy (PLOM) images (see Figure S5), is provoked by the changes in composition and the exclusion/inclusion competition. Minimum Tcand Tmvalues are observed for PH67O33C (with 33 mol % POC), considered the pseudoeutectic point. Such a low POC content in the eutectic copolymer suggests that the OC units, with their eight repetitive methylene units, play a dominant role compared to HC, with only six repeating methylene units, in the crystallization of the copolymers. Despite the POC dominance on copolymer crystallization, among copolycarbonates, the apparent pseudoeutectic position found in this work is higher Table 1. Composition and Microstructure of PHxOyC Copolymers and Parent Homopolymers copolycarbonates composition (mol %) a dyad content (mol %) b sequence length R Mw(kg/mol) c D c XPHC XPOC HH HO/OH OO NHC NOC PHC 100.0 0 100.0 0 0 28 1.92 PH85O15C 84.7 15.3 78.7 19.0 2.3 9.2 1.2 0.9 8 1.92 PH78O22C 77.9 22.1 60.5 32.4 7.1 4.7 1.4 0.9 19 2.28 PH67O33C 67.2 32.8 44.0 41.7 14.3 3.1 1.7 0.9 14 2.10 PH58O42C 58.0 42.0 35.9 48.5 15.7 2.5 1.7 1.0 15 2.39 PH49O51C 49.1 50.9 25.0 51.0 24.0 2.0 1.9 1.0 16 2.10 PH40O60C 39.5 60.5 14.5 47.0 38.5 1.6 2.6 1.0 10 1.86 PH27O73C 27.0 73.0 10.5 45.1 44.4 1.5 3.0 1.0 22 2.19 PH20O80C 20.0 80.0 3.6 35.5 60.9 1.2 4.4 1.0 16 2.11 PH5O95C 5.0 95.0 0.4 20.3 79.3 1.0 8.8 1.1 13 2.21 POC 0 100.0 0 0 100.0 14 2.05 a Compositions of copolymers were calculated by1H NMR, and the copolymers were named PHxOyC, where the subscripts of xand yrepresent the molar percent (as integers) of PHC and POC, respectively. b The sequence distributions of HH, HO/OH, and OO dyads were calculated based on the intensity ratio of the signals appearing around 67.8 ppm in the13C NMR spectra. The degree of randomness was determined from the average sequence lengths. c The weight-average molecular weight Mwand dispersity Dwere determined through SEC. Figure 2. DSC (a) cooling scan from the isotropic melt and (b) subsequent heating scans for all materials. Scanning rates: 10 °C/min. The enlarged signals marked with an asterisk (*) correspond to the reversible α-δsolid−solid phase transition during cooling and heating scans. The arrows indicate the melt-recrystallization behavior. Macromolecules pubs.acs.org/Macromolecules Article https://doi.org/10.1021/acs.macromol.3c01265 Macromolecules 2023, 56, 8199−8213 8203
than in other copolycarbonates, with a higher difference of methylene units between the parent components. But it is comparable to the 21−36 mol % of PC10 content found in PC8-ran-PC10 copolymers, also characterized by a difference of two methylene units between the parent components. One factor that can influence this behavior is the relative chain lengths of the two comonomers, as shown in previous studies on aliphatic copolyesters, 15,27,36 and also the parity of the chain lengths of the two comonomers as has been recently highlighted in the literature. 19 However, the factors that influence the position of the pseudoeutectic point still need to be completely understood, and their understanding is beyond the scope of this contribution. But further understanding of this issue will be presented in a future contribution, in which a diverse series of copolycarbonates synthesized using different diols with varying even and odd chain lengths will be studied. Interestingly, as shown in Figures 2b and 3a, double melting peaks are not detected at the pseudoeutectic position, as often reported for other isodimorphic random copolymers. In PC7- ran-PC12 copolycarbonates, a similar observation from nonisothermal DSC corresponded to a coincident crystallization and melting, while WAXS detected two crystalline structures. 15 More details regarding this behavior are discussed below. Figure 3b shows an irregular ΔHmvariation (i.e., the copolymers display ΔHmhigher than the parent components and even show a maximum of around 60 mol % POC) with the composition, which does not correspond to the pseudoeutectic trend of the temperature vs POC content observed in Figure 3a. The equilibrium melting enthalpies (ΔHm°) of the copolymers needed to calculate the crystallinity degree by DSC (Xc,DSC) have not yet been estimated yet. Still, they can be estimated through the Van Krevelen contribution group theory, 37 as shown in Section S2. Despite the fact that Xc,DSC values might not include the comonomer inclusion/exclusion balance, they show the same trend as crystallinities values determined by WAXS (Xc,WAXS) (see Figure S6). In this work, we considered the Xc,WAXS estimation to be more accurate. Therefore, the Xc,WAXS were calculated by fitting the peaks from the WAXS curves at −40 °C after cooling from the isotropic melt at 10 °C/min. Figure S7 gives an example of how the Xc,WAXS were obtained. As expected, in Figure 3b, the Xc,WAXS exhibits a similar variation trend as the ΔHmwith the increase of POC content. Compared to the PHC and POC homopolymers on both sides, Xc,WAXS initially decreases to two minimum values, corresponding to the PHC-rich copolymer PH78O22C and POC-rich copolymer PH5O95C. This can be attributed to the fact that some comonomer units act as defects excluded from the crystalline regions, limiting crystallinity and reducing the lamellar size. According to the literature, the crystallinity of isodimorphic copolymers also follows a pseudoeutectic behavior. 24 Surprisingly, as the content of comonomers increases, the Xc,WAXS unexpectedly shows an upward trend instead of the expected downward one, reaching a maximum value for copolymer PH40O60C. This behavior is highly counterintuitive as the maximum Xc,WAXS value greatly surpasses that of both PHC and POC homopolymers despite the continued decrease in Tcand Tm toward the pseudoeutectic point. As shown below, this unique behavior is related to the presence of the third novel phase detected by WAXS and that shows a distinct conformation detected by FTIR. 3.3. Small-Angle X-ray Scattering and Wide-Angle X- ray Scattering. In situ WAXS/SAXS measurements were conducted to explore the crystalline structure using the same thermal conditions as those of the DSC test to ensure consistency. Figure 4a compares the WAXS profiles of all materials obtained at 0 °C during heating. At this temperature, according to Figure 2b and the observations of Perez-Camargo et al., 32,33 the diffraction pattern for both PHC and POC corresponds to the (110) and (200) planes of the δ-phase. According to their Table 2. Thermal Properties Obtained by DSC for PHC, POC, and PHxOyC Copolymers sample Tc(°C) Tm(°C) Tm,end (°C) ΔHm(J/g) a Xc,WAXS (%) b PHC 26.9 45.5/53.6 47.2/55.1 40 47.3 PH85O15C 6.5 28.1/40.0 30.0/42.5 35 46.3 PH78O22C−11.5 20.7/29.6 23.2/32.3 27 43.9 PH67O33C−17.8 13.2 15.4 40 47.1 PH58O42C−2.3 21.0 22.7 41 50.3 PH49O51C 1.5 23.0 24.7 43 51.8 PH40O60C 5.6 26.3 28.0 47 55.3 PH27O73C 9.7 30.2 32.0 44 53.1 PH20O80C 17.3 27.0/39.2 29.6/41.8 43 53.4 PH5O95C 26.0 47.3 49.0 40 51.1 POC 33.6 25.0/34.1/56.9 27.8/41.6/59.0 43 48.5 a Melting enthalpy (ΔHm) obtained using DSC at 10 °C/min. b The degree of crystallinity (Xc,WAXS) for all samples was calculated based on the results of peak fitting to WAXS curves (see Figure S7). Figure 3. (a) Tcand Tmand (b) ΔHmand Xc,WAXS as a function of POC composition. Lines have been drawn joining the data points to guide the eye. Macromolecules pubs.acs.org/Macromolecules Article https://doi.org/10.1021/acs.macromol.3c01265 Macromolecules 2023, 56, 8199−8213 8204
results, 32,33 the δ-PHC/POC maintain similar crystalline forms as those of α-PHC and α-POC, but with more efficient chain packing, although the specific crystal structure of δphase has not been reported. As an additional avenue of investigation, we aspire to elucidate their structures by conducting fiber diffraction using high-molecular-weight samples or by cultivating single crystals for electron diffraction; however, such a determination is outside the scope of the present work. Still, provisionally, α-PHC has been previously indexed to a monoclinic unit cell (a= 0.746 nm, b= 0.631 nm) and α= 60°with (110) and (200) as its main planes (d(110) = 0.441 nm and d(200) = 0.373 nm) due to the similarity between PHC and the known structure of the poly (hexamethylene carbonate-glycol) analogue. 38 The crystalline structure of POC was determined by Zhao et al. 10 They found that both α- and β-forms are monoclinic [αform: a= 0.77 nm, b= 1.01 nm, c(fiber axis) = 2.52 nm and α = 31.5°with (110) and (200) as its main planes d(110) = 0.430 nm and d(200) = 0.380 nm; β-form: a= 0.81 nm, b= 0.89 nm, c(fiber axis) = 2.42 nm, and α= 31.9°with a single reflection from the (110/200) planes d(110/200) = 0.41 nm]. Figure 4a shows that a small amount of the αphase remains for POC, as indicated by the diffraction peak at q= 1.39 Å−1. A similar result was reported by Hung et al. 27 and attributed to an incomplete α-δsolid−solid phase transition during the previous cooling process rather than the occurrence of reversible δ-αtransition during heating. Figure 4a shows that in the PHC-rich compositions, only the PH85O15C sample displays an analogous WAXS pattern to the PHC homopolymer, with two primary crystalline reflections at q= 1.42 and 1.67 Å−1assigned to the (110) and (200) planes of the δ-phase. For the PH78O22C copolymer, even though the crystalline structure is dominated by PHC-type crystals, as evidenced by its two analogous main diffraction peaks, a newly observed peak at approximately q= 1.51 Å−1suggests the presence of a new crystal phase. This signal does not correspond to the distinct signals from the PHC-type crystals. A similar behavior as that observed for PH78O22C was reported in poly (decamethylene succinate-ran-decamethylene fumarate) copolymers. 28 In this case, for DF contents of 37 and 57 mol %, the WAXS pattern displays a mixture of the main PDS and PDF reflections and extra reflections (like in this work) that do not belong to any of the parent components. Still, the authors claim that the copolymers were at pseudoeutectic conditions in these compositions rather than adopting a completely new crystalline form. In addition, slight changes in Tcand Tmwere detected, corroborating that these copolymers seem to be at a wide pseudoeutectic region. Moreover, the melting enthalpy ΔHmvs DF content displays a typical pseudoeutectic behavior. Thus, similarly to the literature, we can consider that the PH78O22C crystallizes in PHC-type crystals despite the extra peak. The extra peak might indicate the coexistence between PHC-type crystals and the new phase ones, as it occurs in the pseudoeutectic region or point of isodimorphic copolymers. A unique and novel behavior is observed as the POC content increased between 33 and 73 mol %. For these compositions, only two prominent diffraction peaks at q= 1.51 and 1.68 Å−1were detected; we denote them “Plane I″and “Plane II” (see Figure 4a). These reflections do not correspond to any known crystalline diffraction planes of either PHC or POC or a mixture of them, as typically reported in isodimorphic copolymers. In addition, Planes I and II are also the main planes for the PH20O80C copolymer. Due to the lack of sufficient diffraction peaks, we cannot precisely determine this phase’s crystalline structure at present. However, by combining the results of FTIR, we propose a plausible hypothesis (see Section 3.4). Yet, until substantial experimental evidence is obtained, we continue to temporarily refer to this crystalline structure formed in these copolymers as the “new phase”. The WAXS results suggest the formation of a dominant new phase, distinct to PHC- and POC-type crystals, for an extensive range of compositions, i.e., POC contents of 33 to 80 mol %. The formation of this new phase coincides with the compositions in which the Xc,WAXS vs POC content (see Figure 3b) behavior deviates from the expected one (e.g., a pseudoeutectic behavior), exhibiting an “inverse” pseudoeutectic trend. Interestingly, despite forming a new phase for such an extensive composition range, these copolymers continue displaying a pseudoeutectic behavior in temperatures vs POC content plots (see Figure 3a). For the POC-richest compositions, both copolymers, PH5O95C and PH20O80C, generate a mixture of POC-type crystals and a new crystal phase during crystallization. But the dominant crystalline phase is different. The PH20O80C copolymer, which crystallizes in the new phase-dominant crystals, also displays a small diffraction peak at q= 1.41 Å−1, indicating the coexistence of the POC-type crystals. In contrast, the PH5O95C copolymer crystallization is dominated by POC-type crystals. It exhibits the characteristic peak of the new crystal phase at q= 1.51 Å−1, together with the diffraction peaks of the δand αphases of homopolymer POC. Specifically, the peaks at q= 1.39 Å−1belong to the (110) plane of the αphase, whereas the diffraction peaks at q= 1.42 and 1.65 Å−1were attributed to the (110) and (200) planes of POC δphase, respectively. Notably, in the homopolymer of POC, the induction of the new phase crystallization requires only 5 mol % of HC units, while in the case of PHC, a critical concentration of 22 mol % OC units is required to induce the formation of new phases. Figure 4. (a) WAXS profiles of all samples taken at 0 °C during the heating process after a previous cooling to −40 °C at 10 °C/min from the isotropic melt. (b) d-spacing of the indicated planes in (a) as a function of POC compositions. To differentiate between the crystal forms and planes of the two homopolymers, PHC and POC, which exhibit some similarities, two distinct colors were used: red for PHC and purple for POC. For several PHxOyC copolymers, a novel crystal form that is distinct from the two homopolymers was observed and denoted “Plane I″and “Plane II” due to its unknown crystal structure and unit cell parameters. Macromolecules pubs.acs.org/Macromolecules Article https://doi.org/10.1021/acs.macromol.3c01265 Macromolecules 2023, 56, 8199−8213 8205
Figure 4b shows the interplanar distances (of the planes indicated in Figure 4a), d-spacings, calculated with Bragg’s law plotted as a function of the POC content. For clarity, we separately analyzed the three regions found in Figure 4a: PHC- rich, POC-rich, and new-phase regions. For PHC-rich copolymers, d(200)δincreases as the POC content increases, whereas d(110)δslightly increases and then decreases. This enlargement in the d-spacing values indicates that PHC crystal unit cells must expand their volume (i.e., a and bsizes) to incorporate larger OC units. Analogous dspacings increase with composition to accommodate comonomer inclusion has also been reported for other random copolymers. 15,19,23,27 In the case of POC-rich compositions, dspacing values (d(110)δand d(200)δ) also increase with PHC content due to the inclusion of PHC counits. The changes in d(110)αvalues as PHC content increases also are provoked by PHC counits incorporation; otherwise (i.e., comonomer exclusion), the d-spacing should remain unchanged. Within the range of intermediate compositions (22−95 mol % POC), where PHxOyCs can crystallize into the new phase, an upward trend is observed in the spacing of Plane I as POC compositions increase, resembling the findings in isomorphic systems. 19,20 In contrast, the d-spacing values of Plane II initially decrease to a minimum at PH40O60C before subsequently increasing. In situ temperature-dependent WAXS was performed to understand further the formation of the new crystalline phase and the relationship with the PHC and POC solid−solid transitions. Figure 5 shows the WAXS patterns collected during cooling and heating, at 10 °C/min, for representative samples. The temperature-dependent WAXS profiles of the remaining samples are presented in the Supporting Information (Figure S8). Figure 5a illustrates that during cooling of the PH78O22C copolymer, two diffraction peaks assigned to PHC-type crystals appear starting from −6°C, while the appearance of a diffraction peak at q= 1.51 Å−1from −19 °C indicates the formation of the new phase. Next, this new phase and the PHC-type crystals subsequently melted at 11 and 32 °C, respectively, while no thermal signal was observed at 11 °C in the DSC heating scan. Moreover, the FTIR variable-temper- ature spectra shown in Figure S12a during the heating from 10 to 15 °C did not reveal any changes in the chain packing mode. Therefore, the imperceptible thermal signal might be attributed to the small amount of the new phase, causing its melting peak to be overlapped by the broad thermal transition of melting and recrystallization that initiates at around 5 °C. The small endothermic peak at 23.2 °C does not fit the vanishing temperature of the diffraction peak, as shown in Figure 2b and Table 2. These results support the assertion that the double melting peaks arise from melting recrystallization rather than polymorphism. Initial examination of the diffraction pattern collected at 0 °C for the PH67O33C copolymer, as depicted in Figure 4, demonstrates its crystallization as a pure new crystalline phase. Of particular note is the absence of characteristic peaks associated with known PHC- or POC-type crystals throughout the applied thermal treatment shown in Figure 5b. This observation effectively precludes the possibility of the new crystal phase being derived from the phase transition of the known crystal structures. The evidence presented in the in situ results suggests that the new phase in PH67O33C was directly generated via melt crystallization. In addition, the characteristic single strong peak corresponding to the β-POC phase (see Figure S8g) is absent, indicating that such a solid−solid transition does not occur in these materials. An analogous behavior is observed for PH58O42C, PH49O51C, PH40O60C, and PH27O73C (see Figure S8c,f). Figure 5c shows that PH20O80C copolymer crystallization starts with forming POC-type crystals as indicated by the signal of the (110) and (200) planes at 18 °C. But at 14 °C, the new crystalline phase starts forming (see Planes I and II). As the temperature decreases, the coexistence of the POC-type and the new phase-type crystals occurs, with dominance of the new phase-type crystals. Upon heating, the new phase-type crystals melt before (∼30 °C) the POC-type ones (∼41.8 °C). At around 28 °C, an additional indicator of the dominance of the remaining POC-type crystals is the strong peak [(110/200)β] corresponding to the β-POC phase crystals, i.e., Brill-like transition. The observed melting temperatures in the in situ WAXS experiments are consistent with the endothermic peaks detected during the second heating DSC scans (see PH20O80C in Figure 2b and Tm,end values in Table 2). This observation Figure 5. Temperature-dependent WAXS diffractograms acquired during cooling and heating at 10 °C/min for (a) PH78O22C, (b) PH67O33C, (c) PH20O80C, and (d) PH5O95C. The blue curves represent the cooling process, while the red curves represent the subsequent heating process. The two green curves in both the cooling and heating processes represent the critical temperatures for the appearance and disappearance of the new crystal phase, respectively. The black curves indicate the initial temperature of crystallization (Tc,initial) and the final melting temperature (Tm,final), defined as the first temperature at which a crystalline signal appeared and the first temperature at which the crystalline signal disappeared, respectively. This notation is employed to differentiate between WAXS and DSC experiments. The corresponding temperature values are also marked on the side. Macromolecules pubs.acs.org/Macromolecules Article https://doi.org/10.1021/acs.macromol.3c01265 Macromolecules 2023, 56, 8199−8213 8206
demonstrates that the smaller melting peak detected during the second heating DSC scan can be attributed to melting of the new phase. A different situation is observed for PH5O95C since the POC-type crystals dominate the crystallization. In this case, POC crystals are formed at ∼25 °C (see peaks generated by (110) and (200) planes in Figure 5d), and at a lower temperature, ∼ −2°C, a peak from the new phase (see the peak generated by Plane I in Figure 5d) is detected. Upon heating, the peak of the new phase melts at 28 °C, followed by the melt of POC-type crystals at 49 °C. This latter value is in line with DSC results (see Figure 2b). Figure 5d also shows the characteristic signal generated by the β-POC phase [see the Figure 6. d-Spacing evolution for (a) PHC, (b) PH78O22C, (c) PH20O80C, (d) PH5O95C, and (e) POC. The blue open points represent the cooling process, while the orange solid points correspond to the heating process. (f) Solid−solid phase transition temperatures as a function of POC molar fraction. In (f), the solid points indicate the phase transition occurring during the cooling process (β-αand α-δtransitions), while the open points represent the corresponding reversible transition process during heating (δ-αand α-βtransitions). Macromolecules pubs.acs.org/Macromolecules Article https://doi.org/10.1021/acs.macromol.3c01265 Macromolecules 2023, 56, 8199−8213 8207