Microstructure–hardness–corrosion performance of 17–4 precipitation hardening stainless steels processed by selective laser melting in comparison with commercial alloy
Abstract
Producción Científica
Full text
Vol.:(0123456789) 1 3 Metals and Materials International https://doi.org/10.1007/s12540-021-01155-8 Microstructure–Hardness–Corrosion Performance of17–4 Precipitation Hardening Stainless Steels Processed bySelective Laser Melting inComparison withCommercial Alloy C.Garcia‑Cabezon1 · M.A.Castro‑Sastre2· A.I.Fernandez‑Abia2· M.L.Rodriguez‑Mendez3· F.Martin‑Pedrosa1 Received: 22 September 2021 / Accepted: 14 December 2021 © The Author(s) 2022 Abstract The 17–4 Precipitation Hardening Stainless Steel (PH SS) manufactured by Selective Laser Melting (SLM) has wide application perspectives, but they are limited due to defects and anisotropy. The selection of the appropriate process variables plays a fundamental part in the microstructure and in the determination of the final mechanical and corrosion properties. The main purpose of this study is to analyze the corrosion behavior, hardness and microstructure of 17–4 PH SS manufactured by SLM in comparison to the commercial counterparts. The anisotropic behavior was investigated by analyzing the microstructure–hardness and corrosion interrelationship, both in the surface of the construction platform and in the growth direction of the element. The corrosion behavior of the SLM 17–4PH SS in its natural state was investigated in relation to that of the 17–4 PH SS heat treated in a 0.1M NaCl + 0.5M H2SO4 solution, using three electrochemical techniques. The results confirmed that the corrosion resistance of SLM 17–4 PH SS was considerably better than that of the forging, even after 60days of immersion in the test solution. This was attributed to the absence of important manufacturing defects, to the fine microstructure with an important amount of austenite produced by SLM, and to a small amount of non-metallic inclusions precipitated as a result of the fast cooling and the high speed of solidification associated with the SLM process. Keywords Additive manufacturing· 17–4 PH SS· SLM· Microstructure· Corrosion 1 Introduction Selective Laser Melting (SLM) is a Laser-Powder Bed Fusion (L-PBF) process that can create functional metal parts, and which provides significant advantages over conventional manufacturing processes. Yap etal. [1] reported that the SLM process is particularly advantageous for manufacturing parts with complex geometries, optimizing the strength-to-weight ratio. This property of manufacturing lightweight parts makes the SLM process especially interesting in the aeronautics and automotive industries, where it is essential to reduce the weight of the components [2]. The work carried out by Maconachie etal. revealed the ability of the SLM process to manufacture [3] with improved mechanical and geometric properties. SLM can process a wide variety of metals, but the most investigated have been titanium, nickel-based alloy and stainless steels. The 17–4 PH SS is a martensitic precipitation hardened stainless steel widely processed using SLM. This material has good weldability and is therefore suitable for processing by SLM [4]. The main applications of 17–4 PH SS are in the aerospace, automotive, naval, and chemical industries, where it is essential for the metal components to have a good combination of strength and corrosion resistance, such as turbine blades, piston rings, or injection molds with conformal cooling channels. These properties, which are intrinsic to the commercial 17–4 PH SS, can be modified by the SLM process. The parts created by SLM have different properties compared to the parts manufactured by other conventional processes due to the manufacturing method. SLM uses a * C. Garcia-Cabezon [email protected] 1 Materials Engineering, E.I.I., Universidad de Valladolid, Valladolid47011, Spain 2 Department ofMechanical, Informatics andAerospace Engineering, University ofLeón, Campus de Vegazana, León24071, Spain 3 UVASENS, E.I.I., Universidad de Valladolid, Valladolid47011, Spain
Metals and Materials International 1 3 focused laser beam to melt and fuse the metal powder spread on the work platform. The molten material quickly solidifies forming the final part. During the melting and solidification, the material experiences thermal fluctuations with local rapid heating and cooling rates, inducing microstructure variations. This mechanism is responsible for producing parts with high residual stress, as demonstrated by Fang etal. [5]. Another characteristic of SLM manufactured parts is the porosity, which can be produced for various reasons, such as an improper setting of the processing variables or during the gas atomization process [6]. Despite the large amount of recent research, most studies on 17–4 PH SLM have focused on analyzing the influence of the process parameters on the microstructure and mechanical properties [7, 8]. They have also searched for different strategies to improve mechanical [9, 10] and fatigue behavior [11–14]. The effect of part size and geometry on melt pool dimensions and porosity, and the relationship between porosity percentage and fatigue strength, have also been investigated [8]. Corrosion resistance is an important characteristic for 17–4 PH SS SLM applications. Most studies on the corrosion properties for SLM-produced stainless steel are mainly focused on austenitic SS (AISI 316L and AISI 304) [15]; while there is a lack of knowledge concerning the behavior of SLM PH SS. Most research work on 17–4 PH stainless steel has focused on analyzing the relationship between porosity and corrosion properties. Irrinki etal. [16] have studied the effect of the powder characteristics and the energy density on the corrosion resistance of 17–4 PH SS fabricated by laser-powder bed fusion. They concluded that density is the main factor affecting the corrosion resistance in the NaCl solution. The same conclusion was reached in the study by Schaller etal. [17], where they concluded that porosity, and especially larger pores, are responsible for the worse performance and corrosion resistance [18] of the parts in comparison to forgings. Most of the work carried out has focused on the effect of porosity on all the characteristics of steel, mechanical resistence and also corrosion resistance. There are, however, fewer studies on other factors that may also influence the work in this regard. The work by Alnajjar etal. [19], for instance, on the influence of the microstructure on the corrosion resistance of SLM 17l–4 PH in acidic chloride medium concludes that the microstructure has no effect on the general corrosion behavior if the chemical composition matches. They give a much more important role to the content of manganese sulfide inclusions in the susceptibility to localized corrosion. In addition, a recent study by Wang and al. [20], on SLM 15–5 PH steel, has shown that the processing parameters (low laser power, high scanning speed, and laser energy) are the key to reducing manufacturing defects. It should not be ignored that the defects (micro-cracks, binding defects, and voids) decrease the strength and plasticity of the material. Furthermore, it also results in a sharp decrease in resistance to pitting/crevice corrosion, especially when they exist at the bottom or interface of molten pool line [20]. These authors have also studied the heat treatments that can enhance the corrosion resistance and its relationship with the microstructural changes experienced by SLM 15–5 PH SS [21]. Stoudt etal. [22] also agree with the need for post-construction heat treatments to eliminate chemical segregation. Mujib etal. [23] indicate that the best corrosion resistence is provided by the MoS2 coatings, as indicated by the OCP results. 17–4 PH steel, fabricated by additive manufacturing, will therefore have a behavior similar to that of wrought stainless steel. In our case, we carried out a preliminary study [24] to optimize the processing parameters, which allowed us to obtain an almost complete densification and a low chemical segregation so as to perhaps be able to suppress the postconstruction heat treatments. The analysis of the relationship between the structural modifications inherent to the SLM process (without post-construction treatments) and the corrosion behavior in a highly aggressive solution is the main objective of this work. This paper provides a detailed analysis of the corrosion behavior of SLM 17–4 PH SS in build condition and the comparative study with commercial wrought heat treatment 17–4 PH SS. For this purpose, the microstructure and hardness of the SLM samples were analyzed. The corrosion tests were carried out using electrochemical techniques in a highly aggressive medium (acid with chlorides). In addition to the anodic polarization curves, usually used to study the corrosion behavior of SLM 17–4 PH SS, the electrochemical impedance technique was used. It was thus possible to evaluate the passive behavior of the samples in their original state and after 60days of exposure to the test solution. A relationship between the microstructure and corrosion properties was established. 2 Experimental 2.1 Materials andSample Preparation Longitudinal and transversal specimens were taken from a 25.4mm diameter round bar; the samples were identified as Wrought Longitudinal Direction (W-LD) and Wrought Transversal Direction (W-TD), respectively. The chemical composition of the commercial 17–4 PH SS samples is shown in Table1. The W 17–4 PH SS was in solution annealed and double precipitation hardening condition. The solution heat treatment was performed at 1040°C for 130min, followed by air cooling to room temperature. The first step of the precipitation hardening is to hold the specimens at 625°C for 7h, followed by air cooling to room
Metals and Materials International 1 3 temperature; while the second is to hold the specimens at 630°C for 9.5h, then air cooling to room temperature. Commercially available gas-atomized spherical 17–4 PH SS powder, with a chemical composition (in wt%) listed in Table1, was used in this study for the SLM samples. The chemical composition (wt%) of wrought 17–4 PH SS is also reported in Table1. The amount of chromium and copper were slightly higher for 17–4 PH SS powder. The Scanning Electron Microscope (SEM) micrograph (Fig.1a) shows a powder morphology that is almost Table 1 Chemical composition of the 17–4 PH SS powder for the SLM and for the W17–4 PH SS samples Units in weight percent Elements C Cr Ni Mo Mn Si Cu Nb N S Al Fe Powder – 16.93 4.17 – 0.58 0.62 3.56 0.21 – – – Bal Wrought 0.032 15.70 4.30 0.15 0.61 0.27 3.13 0.255 0.004 0.0005 0.005 Bal Fig. 1 SEM micrograph of the 17–4 SS powder morphology a and EDS analysis of powder b
Metals and Materials International 1 3 spherical in shape. The Energy-dispersive X-ray spectroscopy (EDX-ray) spectra of the entire area showed the existence of the elements in a greater percentage by weight in the powder (Fig.1b). The LS 13 320 Beckmann Coulter laser diffraction particle size analyzer had been used to determine the size distribution of the powder particles. Table2 shows the fraction of the population below 10%, 50% and 90% of the accumulative frequency distribution using the parameters d10, d50 and d90. The SLM samples were cubic specimens with dimensions 12 × 12 × 8mm, fabricated at the UFI 3D Laboratory (University of León, Spain) using a ProX 100 SLM machine (3DSystems). DMP ProX Manufacturing software was used to design the cubic specimens and to go from an STL file to a FAB3 file for direct transfer to the SLM machine. The processing parameters were set according to the manufacturer's recommendations. The hexagonal scanning strategy is recommended for 3D Systems metal printers in order to achieve high density parts and good mechanical properties. The layer height of 30 microns is the recommended value for printing 17–4 PH steel parts on the ProX 100 SLM machine. This value is set by default in the parameters of the said machine. This layer height allows high precision parts to be obtained. The main processing parameters are indicated in Table3. The printing procedure was carried out in a protecting chamber, using nitrogen to maintain an oxygen level below 1000ppm and thus avoid the oxidation of the powder. The SLM samples were analyzed in two sections: first, in the x–y build plane; and second, in the x–z plane (perpendicular to the build direction) according to ASTM 52,900 [25]. The superficial and transverse directions of these samples are denoted as SLM-Superficial Direction (SLM-SD) and SLM-Transversal Direction (SLM-TD), respectively. 2.2 Microstructural Characterization Microstructural characterization was done with optical metallography and scanning electronic microscopy with energy dispersive analysis of X-rays (SEM/EDS) using SEM-FEI (QUANTA 200F). To obtain microstructural features, a diamond suspension (1μm) was used for polishing and different attack reagents (Vilella, Fry and oxalic acid solutions) were used for chemical and electrochemical etching. The degree of residual porosity for SLM samples was determined by image analysis (Image J). X-ray diffraction (XRD) using Agilent SuperNova was used in the identification of some of the phases. A Ferrite meter was used to measure the Ferrite number (FN) or Ferrite Percentage (% F) of stainless steel. 2.3 Vickers Hardness Macrohardness was measured by the Vickers test with 30kg for 30s using a Centaur 920 Durometer. Five impressions were made on the center section of the specimen, while the mean hardness and standard deviation were also determined. The results of the macro-hardness test can be influenced by the possible effect of the porosity of the SLM samples. Therefore, a micro-hardness test was also performed with a Matsuzawa MXT70 micro-hardness meter with a 100g load during 30s. The microhardness was evaluated as the arithmetic mean value of at least ten hardness tests with acceptable impressions after discarding the two lowest values. 2.4 Corrosion Resistance Three electrochemical methods were used to characterize the corrosion resistance of Wrought and SLM samples: Open Circuit Potential (OCP), Anodic Polarization measurement (PA) and Electrochemical Impedance Spectroscopy (EIS), using a potentiostat 273A EG&G PAR and an impedance analyzer Solartron SI 1260. The corrosion tests were carried out in acid solution with chlorides (0.5M NaCl + 0.5M H2SO4 at 30°C) in a three-electrode conventional cell using a Saturated Calomel Electrode (SCE) as the reference electrode and graphite as the counter-electrode. The test was performed in deoxygenated conditions (purged with nitrogen). The samples were wet ground with SiC abrasive papers, followed by polishing with 1mm diamond aqueous suspension. The open circuit potential was measured for 3600s of immersion of the samples in the electrolyte solution. Potentiodynamic anodic potential curves were made following the ASTM G-5 [26]. Once a nearly quasi-stable potential had been reached, the anodic potentiodynamic scan started at 50mV below VOCP, reaching 1000 mVSCE, using 50mV/min as the potential scan rate. The corrosion potential and current densities were obtained through Tafel's analysis and was carried out to evaluate the corrosion polarization resistance Table 2 Particle size distribution of the 17–4PH SS by laser diffraction d10 d50 d90 Particle Size (μm) 4.56 15.11 43.76 Table 3 Main processing parameters used for SLM samples Parameter Value Laser power (W) 38 Scanning speed (mm/s) 140 Layer thickness (μm) 30 Hatch spacing (μm) 70 Scanning strategy Hexagons
Metals and Materials International 1 3 (RP). Impedance spectra were performed at open circuit potential after a stabilization step at open circuit during 1800s with a signal amplitude of 10mV at OCP and with a frequency range from 10MHz to 0.1Hz. Impedance results were fitted to equivalent circuits using CorrView software. To ensure statistical accuracy, the electrochemical essays were repeated three times. Observations by optical microscopy were done on the corroded samples to understand how the processing procedures influence the corrosion performance of 17–4 PH SS. 3 Results 3.1 Microstructure Characterization The microstructure study of the 17–4 PH SLM samples in the as-built condition was carried out in two sections, i.e., SD and TD. The microstructure of the wrought samples after heat-treatment was analyzed in transversal and longitudinal sections to cold rolled direction, denoted as TD and LD, respectively. Representative micrographs of polished SLM-SD and SLM-TD are displayed in Fig.2a and b; both sections show a low level of porosity, the porosity percentage obtained by image analysis was 0.5% for LM-SD and 0.8% for SLMTD, which suggests that the processing parameters were optimized. Suryawanshi etal. [27] confirmed that porosity and inclusion content are two important microstructural features related to corrosion behavior. Porosity is a typical fault in SLM parts; they can be spherical associated with gas entrapment during the solidification process or irregular due to unmelted powder particles or insufficient overlap between the scan tracks, as observed by Aboulkhair etal. [28]. Moreover, Suryawanshi etal. [29] found that the porosity level depended on such factors as the orientation of the surface in relation to the direction of construction and the scanning strategy. The microstructure of wrought samples was pore free; the dark points observed in Fig.2c correspond to non-metallic inclusions (oxides and manganese sulfides). Figure3a and b show the microstructure of W-TD and W-LD, respectively; while Fig.3c and d show the microstructures of the SLM-SD and SLM-TD. It is clear that SLM processing produced microstructures that are different from those of conventional processes. For SLM samples, there are important differences, depending on the orientation of the surface; while similar microstructures were observed for W-TD and W-LD, which had a fully martensitic microstructure (the prior austenite ASTM grain size number G was 8.0) with small carbide precipitates but without ferrite delta stringers (0%). This is consistent with the literature for heat-treated 17–4 PH SS [30]. The melt pool shapes and laser tracks are the most important microstructural features of the SLM as-built condition. Figure3d clearly shows the overlapping hemispherical melt pools created by the laser in the normal orientation to the build direction, SLM-TD. The average diameter of the molten pool structure was Fig. 2 Optical microstructure polishing of a SLM-SD, b and c SLMTD
Metals and Materials International 1 3 Fig. 3 Microstructure of a W-TD, b W-LD, c SLM-SD d SLM-TD, after electrochemically etched with 10% of oxalic acid e SLM-SD and f SLM-TD Fry´s etching
Metals and Materials International 1 3 approximately 80μm with a layer thickness of 18μm. Along the selective direction of the laser melted, strip-like tissues were observed. The presence of bulk austenite can be seen in the region near the molten pool line (Fig.3d). The attack with Fry's reagent (5g of CuCl2, 40ml of HCl, 25ml of ethanol and 30ml of H2O) in SLM-SD revealed evident signs of dendritic segregation, Fig.3e. These heterogeneities were developed as a consequence of the complex and successive passes of the laser beam. Also, Fig.3f shows large elongated grains growing parallel to the built direction, which can be seen around the limits of the track in SLM-TD. The differences in cooling rates at the melt pool zone are produced because of a high degree of convection heat transfer. Therefore, a finer and equiaxed microstructure was formed. Nevertheless, close to the melt pool edge, the cooling rate is lower. Therefore, elongated and larger grains were formed. Zhong etal. [31] and Trelewicz etal. [32] report similar results. X-ray diffraction spectra (Fig.4) shows the existence of different solid solutions and precipitates. These phases were similar for both the Wrought and SLM samples. Wrought 17–4 PH steels usually have a fully α´-martensitic (BCC) microstructure similar to that observed by Hsiao etal. [33]; however, the presence of austenite-stabilizing elements, such as Cu or Ni, can decrease the martensite start temperature (Ms). This gives rise to an incomplete martensite transformation, and consequently, it is relatively common to also find retained γ-austenite (FCC) in the microstructure similar to that described by Rafi etal. [34]. X-Ray diffraction for SLM also showed the BCC peaks, which can correspond to either ferrite or martensite. Alnajjar etal. [19] deduced that the as-built SLM 17–4 PH steel had a delta ferrite microstructure. This ferritic structure was justified by the high heating and cooling rates that do not allow austenite formation, so initial delta ferrite cannot be transformed. In this case, the presence of nitrogen as an austenite-stabilizing element allowed the formation of austenite which is partially transformed into martensite during rapid solidification cooling; so the martensite (α’) was also the primary phase, and this fact was confirmed by the subsequent hardness measurements confirmed. A slightly higher amount of γ-austenite (a high intensity γ (1 1 1) peak at 43.5°) than for W can also be identified. This is consistent with the lower ferrite percentage found in SLM (44.6% F) than in W (60.2% F). The reasons why SLM may have a higher amount of retained austenite are as follows: the use of nitrogen atmosphere during the SLM process, as the grain refinement observed in the SLM samples can lower the temperature Ms, also observed by Rafi etal. [34]; the grain boundaries where the atomic arrangement are irregular hinder the growth of martensite, in accordance with the literature [35]; and the dendritic segregation observed in SLM can lead to the enrichment of Ni, which can lead to the formation and stabilization of the austenite, as suggested by Caballero etal. [36]. The X-ray diffraction patterns also revealed the presence of precipitates. Furthermore, Nb-Cr intermetallic phases and complex Nb-Cr carbides were identified. The presence of copper precipitates cannot be discarded either, since the diffraction peaks coincide with those of the austenitic phase. The SEM analysis of the microstructure of W and SLM revealed fine Nb-rich phases in both materials. In Fig.5a, corresponding to W, light precipitates could be observed on the edges of the martensite plates. These very small precipitates are more visible in the sample in the polished state, Fig.5b. Large inclusions dispersed in the matrix were observed for wrought samples, Fig.5c. For SLM, the analysis of the microstructure within individual melt pools (Fig.5d) also revealed fine precipitates, which were small, spherical-shaped particles and were especially visible along the dendrite boundaries. The small size of the precipitates makes it difficult to analyze them by EDS, but in both samples an increase in Nb and Cr contents were observed in these areas. These microstructural features are consistent with Cheruvathur etal. [37]. The EDX analysis indicated that the inclusion was MnS type and contained Fe, Cr, and O. The MnS inclusions content of SLM samples was much lower than for the W samples. This could be related to the insufficient time for nucleation due the high cooling rates that can be achieved during their fabrication [19]. An enhancement of corrosion resistance has been proven for inclusions of free stainless steels [19]. The typical Cu-rich precipitates were not observed in any of the analyzed samples, as their small size (between 15 and 30nm) requires TEM microscopy for detection, which was used by Sarkar etal. [38] and Sanjeev etal. [39]. Fig.4 XRD spectra of testing samples
Metals and Materials International 1 3 3.2 Macro andMicrohardness Figure6 displays the macro- and microhardness of SLM and W samples for the two analyzed sections. The macrohardness values are slightly higher than those of the microhardness. This indicates that the degree of porosity of the samples is low in both materials. Moreover, both tests showed the same tendency. The hardness results were similar for both the W and SLM samples, confirming the martensitic structure obtained from both fabrication methods. The results of the macro- and microhardness tests showed that SLM-TD have a slightly lower hardness value than W-TD. However, Sarkar etal. [38], Shrestha etal. [8], and Sanjeev etal. [39] have all observed the opposite tendency, that the samples obtained by additive manufacturing are the hardest. So, the high cooling rate associated to the SLM process produced the finer grain microstructure that explains this hardening, according to the Hall–Petch effect: the hardness would increase as the grain size decreases in accordance with the literature [40]. In addition, the higher density of dislocations adjacent to the grain boundaries of a finer grain structure also results in higher hardness values compared to the coarser grain structures of samples processed by plastic deformation, as has been said by Dieter [40]. In explaining the results obtained in this work, it must be considered that the samples were in different treatment conditions, i.e., the SLM samples were in as-built condition, while the W samples were in heat-treatment condition. It is well known that coherent Cu-rich precipitates are responsible for the increase of hardness in 17–4 PH. The Cu-rich precipitates Fig. 5 SEM images showing the microstructure of a, b, c W and d SLM
Metals and Materials International 1 3 formed during aging are effective in preventing the movement of dislocations and provide a semi-coherent interface, which hardens the alloy, as seen in Sarkar etal. [38] and Zitelli etal. [41]. Therefore, in the as-produced state, the SLM material is typically softer than wrought and age hardened material; this was also observed by Guo and Kindt [42]. Additionally, another microstructural feature could explain the lower hardness of SLM samples, such as the amount of austenite phase. Yadollahi etal. [11] observed that the hardness of 17–4 PH SS samples is typically reduced with higher amounts of retained austenite phase; while this phase can be beneficial in increasing ductility and elongation. The lower magnetic response of SLM samples as compared to the W samples could indicate higher austenite content, which would result in lower hardening. In both manufacturing methods, the samples in the normal direction were slightly harder than in the built direction for the SLM samples or in the longitudinal section for the W samples. The differences are more remarkable for the samples obtained by additive manufacturing. As Hu etal. [13] concluded, the microstructural heterogeneities derived from the additive manufacturing could explain these differences. The higher values of standard deviation observed in SLM-SD and SLM-TD, also noticed by Yusuf etal. [43], could also be a consequence of such heterogeneities (dendritic segregation, grain morphology, differences in cell grain size, etc.). 3.3 Corrosion Behavior 3.3.1 Open Circuit Potential The evolution of OCP over time was used as an indicator to evaluate the thermodynamic tendency to corrosion of the SLM and W samples in a corrosive environment; the effect of the orientation of the samples was also analyzed to determine the isotropic or anisotropic corrosion behavior of the materials. Fig. 6 Vickers hardness and microhardness of every as-fabricated samples Fig. 7 OCP evolution of a as-fabricated samples and b SLM-SD and W-LD samples in acid solution with chlorides after 0 and 60days of immersion
Metals and Materials International 1 3 the article's Creative Commons licence and your intended use is not permitted by statutory regulation or exceeds the permitted use, you will need to obtain permission directly from the copyright holder. To view a copy of this licence, visit http:// creat iveco mmons. org/ licen ses/ by/4. 0/. References 1. C.Y. Yap, C.K. Chua, Z.L. Dong, Z.H. Liu, D.Q. Zhang, L.E. Loh, S.L. Sing, Appl. Phys. Rev. 2, 041101 (2015) 2. L.E. Murr, S.M. Gaytan, D.A. Ramirez, E. Martinez, J. Hernandez, K.N. Amato, P.W. Shindo, F.R. Medina, R.B. Wicker, J. Mater. Sci. Technol. 28, 1 (2012) 3. T. Maconachie, M. Leary, B. Lozanovski, X. Zhang, M. Qian, O. Faruque, M. Brandt, Mater. Design 183, 108137 (2019) 4. J. Hunt, F. Derguti, I. Todd, Ironmak. Steelmak. 41, 254 (2014) 5. Z.C. Fang, Z.L. Wu, C.G. Huang, C.W. Wu, Opt. Laser Technol. 129, 106283 (2020) 6. A. Sola, A. Nouri, J. Adv. Manuf. Process. 1, 21 (2019) 7. D. Wang, C.T. Chi, W.Q. Wang, Y.L. Li, M.S. Wang, X.G. Chen, Z.H. Chen, X.P. Cheng, Y.J. Xie, J. Mater. Sci. Technol. 35, 1315 (2019) 8. R. Shrestha, N. Shamsaei, M. Seifi, N. Phan, Addit. Manuf. 29, 100807 (2019) 9. R. Rashid, S.H. Masood, D. Ruan, S. Palanisamy, R.A.R. Rashid, M. Brandt, J. Mater. Process. Tech. 249, 502 (2017) 10. A. Kudzal, B. McWilliams, C. Hofmeister, F. Kellogg, J. Yu, J. Taggart-Scarff, J. Liang, Mater. Design 133, 205 (2017) 11. A. Yadollahi, N. Shamsaei, S.M. Thompson, A. Elwany, L. Bian, Int. J. Fatigue 94, 218 (2017) 12. X.D. Nong, X.L. Zhou, Mater. Charact. 174,111012 (2021) 13. Z. Hu, H. Zhu, H. Zhang, X. Zeng, Opt. Laser Technol. 87, 17 (2017) 14. M. Mahmoudi, A. Elwany, A. Yadollahi, S.M. Thompson, L. Bian, N. Shamsaei, Rapid Prototyp. J. 23, 280 (2017) 15. Y. Wang, N. Wang, C. Yan, T. Zhang, L. Chen, J. Gu, Mater. Test. 62, 5 (2020) 16. H. Irrinki, T. Harper, S. Badwe, J. Stitzel, O. Gulsoy, G. Gupta, S.V. Atre, Prog. Addit. Manuf. 3, 39 (2018) 17. R.F. Schaller, J.M. Taylor, J. Rodelas, E.J. Schindelholz, Corrosion 73, 796 (2017) 18. G. Ko, W. Kim, K. Kwon, T.-K. Lee, Metals 11, 516 (2021) 19. M. Alnajjar, F. Christien, V. Barnier, C. Bosch, K. Wolski, A.D. Fortes, M. Telling, Corros. Sci. 168, 108585 (2020) 20. L. Wang, C. Dong, D. Kong, C. Man, J. Liang, C. Wang, K. Xiao, X. Li, Steel Res. Int. 91, 1900447 (2020) 21. L. Wang, C. Donga, C. Manb, D. Konga, K. Xiaoa, X. Lia, Corros. Sci. 166, 108427 (2020) 22. M.R. Stoudt, R.E. Ricker, E.A. Lass, L.E. Levine, JOM 69, 506 (2017) 23. S.B. Mujib, S. Mukherjee, Z. Ren, G. Singh, R. Soc. Open Sci. 7, 200214 (2021) 24. P. Leo, S. D’Ostuni, P. Perulli, M.A.C. Sastre, A.I. Fernández- Abia, J. Barreiro, Procedia Manuf. 41, 66 (2019) 25. ISO/ASTM 52900:2015, Additive manufacturing-General principles-Terminology (International Organization for Standardization, Geneva, 2015) 26. ASTM G-5–87, Standard reference test method for making potentiostatic and potentiodynamic anodic polarization measurements (ASTM International, West Conshohocken, 1993) 27. J. Suryawanshi, T. Baskaran, O. Prakash, S.B. Arya, U. Ramamurty, Materialia 3, 153 (2018) 28. N.T. Aboulkhair, N.M. Everitt, I. Ashcroft, C. Tuck, Addit. Manuf. 1-4, 77 (2014) 29. J. Suryawanshi, K.G. Prashanth, U. Ramamurty, Mater. Sci. Eng. A 696, 113 (2017) 30. Y. Zhang, D. Zhan, X. Qi, Z. Jiang, J. Mater. Sci. Technol. 35, 1240 (2019) 31. Y. Zhong, L. Liu, S. Wikman, D. Cui, Z. Shen, J. Nucl. Mater. 470, 170 (2016) 32. J.R. Trelewicz, G.P. Halada, O.K. Donaldson, G. Manogharan, JOM 68, 850 (2016) 33. C.N. Hsiao, C.S. Chiou, J.R. Yang, Mater. Chem. Phys. 74, 134 (2002) 34. H.K. Rafi, D. Pal, N. Patil, T.L. Starr, B.E. Stucker, J. Mater. Eng. Perform. 23, 4421 (2014) 35. W.D. Callister, Material Science and Engineering: An Introduction, 5th edn. (Wiley and Sons, Hoboken, 1994), pp. 45–58 36. A. Caballero, J. Ding, S. Ganguly, S. Williams, J. Mater. Process. Tech. 268, 54 (2019) 37. S. Cheruvathur, E.A. Lass, C.E. Campbell, JOM 68, 930 (2016) 38. S. Sarkar, S. Mukherjee, C.S. Kumar, A.K. Nath, J. Manuf. Process. 50, 279 (2020) 39. K.C. Sanjeev, P.D. Nezhadfar, C. Phillips, M.S. Kennedy, N. Shamsaei, R.L. Jackson, Wear 440-441, 203100 (2019) 40. G.D. Dieter, Mechanical Metallurgy, 3rdedn. (McGraw-hill, New York, 1986), pp. 34–45 41. C. Zitelli, P. Folgarait, A. Di Schino, Metals 9, 731 (2019) 42. Z. Guo, J.T. Kindt, Langmuir 34, 12947 (2018) 43. S.M. Yusuf, N. Gao, Mater. Sci. Technol. 33, 1269 (2017) 44. X. Wang, M. Nie, C.T. Wang, S.C. Wang, N. Gao, Mater. Design 83, 193 (2015) 45. M.J.K. Lodhi, K.M. Deen, M.C. Greenlee-Wacker, W. Haider, Addit. Manuf. 27, 8 (2019) 46. N.S. Al-Mamun, K.M. Deen, W. Haider, E. Asselin, I. Shabib, Addit. Manuf. 34, 101237 (2020) 47. S.A. Saadi, Y. Yi, P. Cho, C. Jang, P. Beeley, Corros. Sci. 111, 720 (2016) 48. R.L. Jones, J. Stewart, J. Non.-Cryst. Solids 356, 2433 (2010) 49. S. Hao, P. Wu, J. Zou, T. Grosdidier, C. Dong, Appl. Surf. Sci. 253, 5349 (2007) 50. M. Laleh, A.E. Hughes, S. Yang, J. Li, W. Xu, I. Gibson, M.Y. Tan, Corros. Sci. 165, 108394 (2020) 51. J.A. Stull, M.A. Hill, T.J. Lienert, J. Tokash, K.R. Bohn, D.E. Hooks, JOM 70, 2677 (2018) 52. A. Raja Annamalai, A. Upadhyaya, D.K. Agrawal, Can. Metall. Quart. 54, 142 (2015) 53. S.S. Panda, V. Singh, A. Upadhyaya, D. Agrawal, ScriptaMater. 54, 2179 (2006) 54. I. Reynier, I. Revilla, B. Woutersa, F. Andreattab, A. Lanzuttib, L. Fedrizzib, I. De Graevea, Corros. Sci. 167, 108480 (2020) 55. M.P. Ryan, D.E. Williams, R.J. Chater, B.M. Hutton, D.S. McPhail, Nature 415, 770 (2002) 56. I. Muto, Y. Izumiyama, N. Hara, J. Electrochem. Soc. 154, C439 (2007) 57. Q. Chao, V. Cruz, S. Thomas, N. Birbilis, P. Collins, A. Taylor, P.D. Hodgson, Scripta Mater. 141, 94 (2017) 58. J.-R. Lee, M.-S. Lee, H. Chae, S.Y. Lee, T. Na, W.-S. Kim, T.-S. Jun,, Mater. Charact. 167, 110468 (2020) Publisher's Note Springer Nature remains neutral with regard to jurisdictional claims in published maps and institutional affiliations.