scieee AI-readable full text Open interactive document viewer

Unveiling the inner structure of micrometric hollow polymeric fibers using synchrotron X-Ray nanotomography

Torre Ordás, Jorge,Cimavilla Román, Paula,Cuadra Rodríguez, Daniel,Rodríguez Pérez, Miguel Ángel,Guttmann, Peter,Werner, Stephan,Pinto Sanz, Javier,Barroso Solares, Suset

Abstract

Producción Científica

Full text

1 Unveiling the Inner Structure of Micrometric Hollow Polymeric Fibers Using Synchrotron X-ray Nanotomography Jorge Torre1,2,3*, P. Cimavilla-Roman1, D. Cuadra-Rodriguez1,3, M. A. Rodriguez- Perez1,2, Peter Guttmann4, Stephan Werner4, Javier Pinto1,2,3, Suset Barroso-Solares1,2,3*, 1Cellular Materials Laboratory (CellMat), Condensed Matter Physics, Crystallography, and Mineralogy Department, Faculty of Science, University of Valladolid (Spain) 2BioEcoUVA Research Institute on Bioeconomy, University of Valladolid (Spain) 3Study, Preservation, and Recovery of Archaeological, Historical and Environmental Heritage (AHMAT) Research Group, Condensed Matter Physics, Crystallography, and Mineralogy Department, Faculty of Science, University of Valladolid (Spain) 4 Helmholtz-Zentrum Berlin für Materialien und Energie, Dep. X-Ray Microscopy, Electron Storage Ring at BESSY II, Berlin, (Germany) *Corresponding author: Jorge Torre ([email protected]) +34 662 072 871, Suset Barroso-Solares ([email protected]) ABSTRACT In this study, a novel application of synchrotron X-ray nanotomography based on high-resolution full-field transmission X-ray microscopy (TXM) for characterizing the structure and morphology of micrometric hollow polymeric fibers is presented. By employing post-image analysis using an open-source software such as Tomviz and ImageJ, various key parameters in fibers morphology, including diameter, wall thickness, 2 wall thickness distribution, pore size, porosity, and surface roughness were assessed. Electrospun polycaprolactone (PCL) fibers with micrometric diameters and submicrometric features with induced porosity via gas dissolution foaming were used to this aim. The acquired synchrotron X-ray nanotomography data was analyzed using two approaches: 3D tomographic reconstruction and 2D radiographic projections-based analysis. The results of the combination of both approaches demonstrate unique capabilities of this technique, not achievable by other available techniques, allowing for a full characterization of the internal and external morphology and structure of the fibers as well as to obtain valuable qualitative insights into the overall fiber structure. Keywords: Characterization, polycaprolactone, morphology, image analysis, 3D reconstruction, wall thickness, pore size, surface roughness. 1. INTRODUCTION Electrospun polymeric fibers have recently become particularly appealing in a wide variety of fields, such as bioengineering, biotechnology, energy, electronics, defense, and security, etc. (Salem, 2001; Barhoum, 2019). The versatility of electrospinning allows not only to produce fibers with exceptional properties, such as high area-to-volume ratio, high porosity or high mechanical flexibility, among others, but also to produce tailored fibers adapted to every specific applications (Ariff et al., 2016; Stanger et al., 2005). In particular, electrospun fibers have shown great potential in biomedical applications, such as drug delivery (Duan et al., 2022; Williams et al., 2018), tissue engineering (Lucy A Bosworth, 2011), or wound healing (Xinkuan Liu et al., 2021), due to their ability to mimic the native extracellular matrix of tissues and organs. Other applications outside the 3 biomedicine field include water treatment (Barroso-Solares et al., 2016), sensors (Halicka & Cabaj, 2021), filters (Valencia-Osorio & Álvarez-Láinez, 2021), etc. The morphology and structure of the fibers are crucial in determining their performance and suitability for each specific application (Li & Wan, 2017; Bhat, 2017). Some of the most commonly used parameters to describe the morphology of electrospun fibers include the average fiber diameter and distribution, pore size and porosity, surface area, and surface roughness (Barhoum, 2019; Ramakrishna et al., 2005). For example, reducing the fiber diameter can enhance mechanical strength and stiffness (Wong et al., 2008), and inducing porosity can lead to higher specific areas, making the fiber mat a promising candidate for tissue engineering or filtration membranes (Soliman et al., 2011). Additionally, increasing fibers surface roughness also contributes to maximizing the available surface area without merely relying on decreasing the fiber diameter, which renders them highly appropriate for some biomedical applications (Laijun Liu et al., 2021; Ferreira et al., 2015). Besides that, hollow fibers have gained significant attention in recent years, as their structure provides an additional way of achieving larger surface-to-volume ratio compared to solid fibers (Vohra et al., 2023). Albeit the fabrication of hollow fibers can be challenging, recent advancements have paved the way for more precise and efficient manufacturing methods (Vohra et al., 2023; Tian et al., 2021). Among the various available techniques, a few have proved to be reliable in hollow fiber fabrication (Tian et al., 2021). For example, co-axial electrospinning involves the simultaneous electrospinning of two polymer solutions in a co-axial spinneret, where one solution forms the shell and the other the core of the hollow fiber. After the solidification, the core 4 can be removed mixing it with a solvent immiscible in the shell, obtaining the hollow fiber (Han & Steckl, 2019; Elahi & Lu, 2013). In co-extrusion, similarly, a spinneret with two concentric orifices is used as well. The outer orifice delivers the shell, while the inner orifice carries a core polymer solution that serves as a removable template (Tian et al., 2021). However, in this case, the solutions are extruded from the tubes and are rapidly passed through a coagulation bath, in which the outer layer is solidified using a crosslinking reaction. After the removal of the core layer, the hollow fiber is obtained. Both of these techniques need to have precise control of a wide variety of parameters, not only in the process itself, but also in the polymeric solution (DeFrates et al., 2018). In order to produce hollow fibers with diameter down to a few microns in a simpler way which does not require such strict control of the experiment conditions, an additional very recent technique proposed by Barroso-Solares et al. (Barroso-Solares et al., 2020) has proved reliable. It works by producing solid fibers following a conventional electrospinning approach and subsequently saturating the fiber mat with 𝐶𝑂2 at high pressure causing the formation of axial holes inside and pores on the fibers surface by releasing the pressure (gas dissolution foaming (GDF)). GDF is a well-known environmentally friendly technique to produce porous polymers (Kumar & Suh, 1988; Cuadra-Rodríguez et al., 2022; Ventura et al., 2018). However, the use of GDF on polymer samples with dimensions in the micrometric range or below have been elusive until the recent development of a novel approach using gas diffusion barriers (Barroso-Solares et al., 2020; Cuadra-Rodríguez et al., 2022; Orsi et al., 2014). In the case of polymeric fibers, this approach has proved to be able to tune the surface porosity, as well as to provide a hollow structure by merging of the inner pores (Barroso-Solares et al., 2020). Hollow fibers produced with this method can reach diameters of only a few units of micrometers, showing features such as wall thickness or pores within hundreds of nanometers, which 5 hinders the accurate characterization of their morphology by using conventional techniques. Accurate and comprehensive methods for characterizing fibers morphology and structure are essential for optimizing fabrication processes and further developing their applications. In recent years, there has been a growing interest in developing new methods for this purpose (Barhoum, 2019; Mitchell, 2011; Singh & Singh, 2021). While conventional techniques, such as scanning electron microscopy (SEM) (Doan et al., 2016; Angel et al., 2020) transmission electron microscopy (TEM) (Yoshioka et al., 2010; He et al., 2006), and atomic force microscopy (AFM) (Casper et al., 2004; Ji et al., 2006) have been widely used to analyze the morphology of electrospun fibers, these techniques are often limited in their ability to provide detailed information on the internal structure of fibers (Sensini et al., 2018). For instance, assessing parameters like wall thickness distribution in hollow fibers or the continuity of hole within them is challenging using the aforementioned techniques. Moreover, the resolution of X-ray-tomography-based techniques at laboratory scales often falls short when attempting to investigate features of fibers with sizes close to the nanoscale. In such cases, synchrotron X-ray tomography emerges as a highly valuable technique. Its use enables exceptional spatial resolution, facilitating the visualization and analysis of a wide range of materials with unprecedented detail (Shen et al., 2004; Wang et al., 2017; Das et al., 2022; Lang et al., 2023). In particular, high-resolution full-field TXM synchrotron X-ray nanotomography proves very useful in situations where 𝜇CT techniques struggle to provide the necessary resolution and comprehensive analysis of internal structures. 6 The high-resolution TXM X-ray nanotomography field is currently an area of active research and innovation. In the context of porous materials characterization, the technique has emerged as a versatile tool, allowing for the detailed analysis of internal structures and dimensions in various materials (Wang et al., 2016; Xiaoyang Liu et al., 2021; Zou et al., 2020; Chen et al., 2023). In the case of polymeric fibers, a limited number of researchers have already approached structural characterization using any kind of synchrotron X-ray tomography. Recently, authors such as Sensini et al. (Sensini et al., 2018), Svetlana Shkarina et al. (Shkarina et al., 2018), and Jekaterina Maksimcuka et al. (Maksimcuka et al., 2017), assessed macroscopic electrospun fiber orientation in bundles and scaffolds with this technique, which proved synchrotron X-Ray Computed Nanotomography reliable for this purpose, when complemented with SEM analysis. Another notable example is the work carried out by Jens Vinge Nygaard et al. (Nygaard et al., 2011), which demonstrated the capabilities of the technique to study details of the internal morphology of single fibers or beads with diameters in the nanometers range. Despite the aforementioned advantages of synchrotron X-ray nanotomography, it is important to acknowledge certain limitations associated with the technique. One notable limitation is that an increase in spatial resolution typically comes at the expense of a reduced field of view. In the TXM setup utilized for this work the FOV was restricted to 26.0 𝜇𝑚 at a pixel size of 20 𝑛𝑚. This means that in a single synchrotron X-ray nanotomography analysis, it became impractical to analyze more than a segment of typically less than fifty micrometers (Blykers et al., 2021; Cimavilla-Román et al., 2022). Also, it is important to consider the potential for sample damage during the preparation 7 process. Manipulating and handling the delicate fibers during sample preparation can lead to deformations or alterations in the fiber morphology, which can impact the accuracy and reliability of the obtained results. Furthermore, it is worth noting some highresolution full-field TXM synchrotron setups for X-ray nanotomography, as in this case, might be constrained in their ability to achieve nanometric resolution data. To overcome this limitation, specific experimental setups are required to enhance the resolution capabilities. However, due to technical considerations, high-resolution TXM X-ray nanotomography at synchrotron facilities are sometimes restricted to the use of tilt tomography over rotational tomography. Tilt tomography involves acquiring images at a limited range of angles instead of full rotational scans, which pose challenges in the reconstruction process (Barutcu et al., 2021). In this case, the missing range of angles is comparable to EM tomography, however, the tilt range was large enough to minimize its effects, as proved by the results below. Herein, the accuracy of the synchrotron X-ray nanotomography technique for the structural and morphological characterization of individual pure and hollow polymeric microfibers will be examined, considering the inherent limitations associated with this method. For this, a comprehensive analysis will be conducted using two approaches: one involving the utilization of 3D reconstruction from tomographic data, and other relying solely on the analysis of radiographic 2D images. By comparing the results obtained from both approaches, the reliability and consistency of the data obtained from the 3D reconstruction will also be assessed. It is important to clarify that the study will be focused on the characterization of individual fibers rather than the properties of the entire fiber mat. 8 2. MATERIALS AND METHODS 2.1 Materials The materials employed included Polycaprolactone (PCL) (𝑀𝑛=80.000,𝜌= 1.15𝑔 𝑐𝑚3, melting temperature 𝑇𝑚 = 61 °𝐶), purchased from Sigma-Aldrich (USA) and Poly (vinyl alcohol) (PVOH) (Mowiflex C17, 𝜌 = 1.25 𝑔/𝑐𝑚3, glass transition temperature (𝑇𝑔) = 60 °𝐶 and 𝑇𝑚 = 170 °𝐶) that was gently provided by Kuraray. Chloroform was sourced from Scharlab (Barcelona, Spain). Deionized water and medical-grade carbon dioxide (𝐶𝑂2) with a purity of 99.9% were utilized in the incorporation and removal of the gas diffusion barriers and foaming processes, respectively. 2.2 Fibers preparation The fibers studied in this work were produced using the procedure detailed in a previous work (Barroso-Solares et al., 2020). In brief, the fabrication of solid fibers involved electrospinning a 10 𝑤𝑡.% PCL solution in chloroform at a voltage of 15 𝑘𝑉, flow rate of 1 𝑚𝐿·ℎ−1, and collector distance of 20 𝑐𝑚, resulting in fiber mats with controlled thicknesses of around 200 μm. Then, the solid fibers were subjected to a gas dissolution foaming (GDF) procedure after being imbibed within a 300 𝜇𝑚 thickness film of PVOH obtained from a 5 𝑤𝑡.% solution in water. The GDF was performed with 𝐶𝑂2 during 24 hours at 30 MPa and 45 ºC. Then, the PVOH coating was completely removed from the foamed fibers by immersing them into a 60ºC water bath before their characterization. 9 2.3 Scanning Electron Microscopy (SEM) Scanning electron microscopy (SEM) was first employed to characterize the fibers coating the surface with gold. It served as a reference for the subsequent analysis. SEM allowed for the detailed visualization of fiber surface morphology and homogeneity which helped demonstrate structural integrity and overall quality of the fibers. The device model was FlexSEM 1000, Hitachi. 2.4 Synchrotron X-ray Nanotomography High resolution X-ray synchrotron nanotomography experiments were performed at the XM – X-ray Microscopy beamline (Guttmann et al., 2018; Werner et al., 2023), a beamline at BESSY II facility of the Helmholtz-Zentrum Berlin in Berlin (Germany). The X-ray microscope was equipped with Fresnel zone plate objective with an outermost zone width of 25 𝑛𝑚 resulting in a 3D resolution of about 36 𝑛𝑚 (Schneider et al., 2012). The X-ray detector was a thinned, backside illuminated CCD, 1340𝑥1300 pixels (Roper Scientific PI SX1300). The photon energy of the X-rays used for the experiment was fixed to 1.0 keV. The selected exposure time of the detector was around 3 to 4 𝑠, the tilt step was 1º and the number of projections varied between samples but always being greater than 70. The acquisition time for a full tomographic data set was about 20−30 min, the field of view was set to 26.0 µm and the reconstructed images achieved a pixel size of 20.0 nm. Individual fibers were manually separated with tweezers from the produced fiber mats and located into the sample holder for the X-ray nanotomography experiments. Each fiber was studied at different positions along their length, aiming to overcome the limitations of the narrow field of view. Two individual reference solid fibers were studied 16 and N their total amount. Note that this method would need adjustments in images of samples with curvature. 𝑅𝑎=√1𝑁∑(ℎ𝑖(𝑥)−ℎ) 𝑁 𝑖=1 (5) Figure 2. Schematic visualization of the calculation of the surface roughness (Ra). 3. RESULTS AND DISCUSSION 3.1 Scanning Electron Microscopy (SEM) results The SEM images provided a first look into the morphology of the fibers. Upon examination (see Figure 3), the fibers displayed a consistent and homogeneous structure, reinforcing the validity of the subsequent analysis in which single fibers were taken randomly from the mat. It was also possible to observe the presence of holes and welldefined external walls in the hollow fibers, which, in some cases, show clearly inhomogeneous thickness (see Supplementary Information, Figure S6), as well as clearly visible surface pores exhibited in both solid and hollow fibers (see Supplementary Information, Figure S7.a)). 17 Figure 3. SEM micrographs of Fibers (a) F1, (b) F2, (c) F3, and (d) F4. 3.2 Synchrotron X-ray nanotomography results In this section, the visual examination of the synchrotron nanotomography data is shown. Figure 4 shows some examples of the 2D projections obtained with this experiment. These images provided a preliminary overview of the fiber shape and structure, imperfections, and internal characteristics. A cursory observation of these 2D projections also allowed for the categorization of the fiber as hollow or solid. For example, solid fibers like samples 1, 2, and 3, appear darker in the projections due to their denser and more compact structure, resulting in higher X-ray attenuation. This is visualized as a darker region in the projection images. In contrast, hollow fibers of samples 4 – 9 in Figure 4, which contain an internal void or cavity, exhibit lower X-ray attenuation in the inner parts as the X-rays pass through the empty space. Consequently, these hollow regions appear brighter in the 2D projections. In the cases of samples 4, 5, 18 7 and 8, the 2D projections provide a clear visualization of its openness, suggesting hole continuity along the fiber. Figure 4. Representative synchrotron X-ray tomography 2D projections of the nine samples included in this study (see Table 1). Figure 5 shows examples of some 3D reconstructions that could be obtained from their corresponding 2D projections. A quick overview of these reconstructions revealed insightful information about the overall morphology, allowing for a comprehensive understanding of the fibers three-dimensional shape and internal structure. Furthermore, the results showcased remarkable agreement with the 2D images in terms of morphology and the ability to detect fiber imperfections such as dust depositions or shape irregularities. This is even in spite of the original images not covering the whole range of 360º (see Supplementary Information, Table S1). However, it is important to note the limitations encountered during the analysis. In some cases, the fiber closure was not welldefined, which could be attributed to this limited number of projections used in the reconstruction process. Additionally, the fibers appeared slightly flattened in the 19 reconstructions, possibly indicating deformation or damage incurred during handling, despite their circular appearance in the SEM images. This flattening effect was also observed in the 2D projections, further supporting the presence of fiber deformation. In this case, the 3D reconstructions provided clear confirmation of the continuity and openness of the hollow structure along the entire length of the fiber segments, further validating the results obtained from the 2D projections. While the 2D projections alone can provide some assessment of hole continuity, the 3D reconstructions offered a more comprehensive and unambiguous visualization, leaving no doubt about the reliability of the results. Figure 5. Representative examples of 3D reconstructions. Samples 6 - 9. For each sample, the longitudinal view, together with two cross-sectional views (one from Tomviz (right) and one from ImageJ (left)) are shown. 20 These visual results provide a clear visualization of the fiber overall properties, guiding further analysis and quantification of the parameters that characterize the fiber structure and morphology. A complete and thorough analysis must be carried out by combining the insights obtained from both 2D radiographies and 3D reconstructions. 3.3 Determination of fiber parameters Wall thickness The characterization of fiber wall thickness was successfully achieved with both aforementioned approaches. A schematic overview of the results of every possible case can be found in Figure 6. Two results of the thickness are given for the 3D case as it can be computed in two opposite walls. However, in the 2D projections case, as every projection corresponds to a different tilt angle, the average of both values is given. The obtained values of wall thickness are exposed in Table 2. The results obtained exhibited remarkable similarity in both characterization methods, reaffirming their reliability and consistency. The value of 6.46 μm observed in sample 6 stands in glaring contrast to the other measured values of wall thickness due to the fact that the hole within the fiber is positioned far from the center and thinner than those of other samples, resulting in an uneven distribution of wall thickness. As a consequence, one side of the fiber exhibits a considerably higher wall thickness compared to the rest (refer to Figure 4). 21 Figure 6. Examples of intensity profiles for the three cases: solid fiber and hollow fiber from 2D projections, and hollow fiber cross-section from 3D reconstruction. Table 2. Results of wall thickness from both 2D projections and 3D reconstructions for the larger and shorter walls of every sample. Sample 𝒕𝟑𝑫 (𝝁𝒎) 𝒕𝟐𝑫 (𝝁𝒎) 𝑡1 𝑡2 4 2.12±0.23 1.76±0.35 2.49 ± 0.61 5 1.60±0.20 0.95±0.24 1.32 ± 0.15 6 6.46±0.96 1.05±0.16 3.71 ± 0.30 7 1.70±0.28 1.17±0.16 1.54 ± 0.47 8 1.25±0.27 1.08±0.15 1.45 ± 0.20 9 2.71±0.36 1.51±0.41 2.68 ± 0.61 Upon closer examination, it was observed that the ratio of thicknesses 𝑡3𝐷/𝑡2𝐷 was slightly lower than one in general (see Figure 7), with the only exception being sample 6, for the reasons explained before. This means that the 3D reconstructions-based approach yielded slightly lower wall thickness values compared to the 2D projections, which indicates that the 3D reconstructions provide a more conservative estimation of the wall thickness. Several factors could contribute to this observed difference. One possibility is the reconstruction process, which may introduce some level of distortion or 22 loss of information. Additionally, the binarization process in ImageJ, which plays a crucial role in segmenting the fiber from the background, may have involved the deletion of a small, but appreciable number of external pixels with values close to the ones in the background. However, the deviations from the ideal value are not significantly large, which proves a certain agreement between the two characterization methods. Figure 7. Wall thickness ratios of both techniques. In the case of 𝑡3𝐷, the thickness of both sides was averaged. Wall thickness distribution The wall thickness distribution was successfully quantified, this time, using the 2D radiography projections. 3D reconstructions were not used in this case given that, although it is achievable, the values of wall thickness can be subjected to image processing bias, as exposed in the previous subsection. Two examples of wall thickness distributions can be seen in Figure 8. In the case of sample 8, the uniformity in the measured wall thickness across different sections of the fiber suggests that the hollow structure maintains its integrity and extends throughout the entire length of the segment. In sample 9, even though the hollow structure does not have a central symmetry, the wall thickness never tends towards the diameter of the fiber, also indicating hole continuity. 23 Figure 8. Example of ROIs and wall thickness distribution corresponding to samples (a) 8 and (b) 9. The histograms in Figure 9illustrate the frequency distribution of the wall thickness values of fibers F2, F3 and F4. Fiber F2 exhibits a normal-like distribution in its histogram. The majority of the wall thickness values fall within the range of 2.0 - 2.5 𝜇𝑚, indicating a relatively consistent thickness for this fiber, with some minor variations observed. In the case of fiber F3, the histogram shows a bimodal shape. This shows that fiber F3 possesses a non-uniform wall thickness around its shape, with the hole being displaced from the center, resulting in different wall thicknesses on opposite sides of the fiber. This could also be qualitatively seen in the Supplementary Information, Figure S6, or in Figure 4, sample 6. Lastly, for fiber F4, it can be observed that the majority of segments exhibited a relatively consistent wall thickness, with a narrow range of values between 1.0 and 2.0. However, some segments displayed variations in the wall thickness, indicating potential structural heterogeneity. The histograms corresponding to F2 and F4 24 contain the data from at least two samples of each fiber, which contributes to assess the continuity of the inner hole in a more representative manner, overcoming the limitations caused by the low field of vision. Figure 9. Wall thickness relative frequency histograms corresponding to fibers (a) F2, (b) F3, and (c) F4. Overall, the successful determination of the wall thickness distribution using the 2D projections highlights the capability of this technique to provide valuable information about the morphological characteristics of the fibers. Pore size The pore size calculation of fiber F1 obtained from images such as the example projection displayed in Figure 10.a) yielded the frequency histogram shown in Figure 10.b). The histogram exhibits a bell-shaped distribution, resembling a normal distribution curve. The peak was observed in the range of 0.3 to 0.4 𝜇𝑚, indicating a prevalent pore size within this interval, which is influenced by the electrospinning process and can have implications for various applications requiring controlled pore characteristics. The value is also in correspondence with the average pore size value. The normal distribution shape implies a balanced distribution of smaller and larger pores. These results are found to be in agreement with the pore size values obtainable using SEM micrographs (Supplementary Information, Figure S7.a)) whose mean value falls within 0.3− 25 0.4 𝜇𝑚. In this case, both methods would provide consistent measurements, although SEM exhibits a clearer visibility for this purpose. Figure 10. (a) Identification of individual pores. (b) Pore size frequency histogram and two-dimensional mean pore size of fiber F1. The pore size calculation was not possible to perform in any sample that underwent the gas dissolution process. This is due to the complete lack of visible pores in the 2D projections, regardless of the known presence of pores as evidenced by SEM (see Figure 3). A possible explanation for the increased visibility of pores in solid fibers compared to hollow fibers in X-ray nanotomography is related to the contrast mechanism employed in the imaging technique. X-ray tomography relies on the attenuation of X-rays as they pass through the sample. In solid fibers, the presence of pores creates localized regions with lower X-ray attenuation due to the large difference in density between the solid fiber and the void spaces of the surface pores. This density contrast leads to a higher contrast between the pore regions and the surrounding solid material, making the pores more distinguishable in the resulting images. On the other hand, in hollow fibers, the absence of a solid material within the central region reduces the density contrast provided by the polymer, making the pores less visible in the tomographic reconstructions (i.e., the contrast between the void surface pores and the mostly empty fibers is not enough to 32 DEFRATES, K. G., MOORE, R., BORGESI, J., LIN, G., MULDERIG, T., BEACHLEY, V. & HU, X. (2018). Protein-based fiber materials in medicine: A review. Nanomaterials 8. DOAN, T. Q., LESLIE, L. S., KIM, S. Y., BHARGAVA, R., WHITE, S. R. & SOTTOS, N. R. (2016). Characterization of core-shell microstructure and self-healing performance of electrospun fiber coatings. Polymer 107, 263–272. http://dx.doi.org/10.1016/j.polymer.2016.10.062. DUAN, X., CHEN, H. LAN & GUO, C. (2022). Polymeric Nanofibers for Drug Delivery Applications: A Recent Review. Journal of Materials Science: Materials in Medicine 33. ELAHI, M. F. & LU, W. (2013). Core-shell Fibers for Biomedical Applications-A Review. Journal of Bioengineering & Biomedical Science 03, 1–14. FERREIRA, P., ALVES, P., COIMBRA, P. & GIL, M. H. (2015). Improving polymeric surfaces for biomedical applications: a review. Journal of Coatings Technology and Research 12, 463–475. http://dx.doi.org/10.1007/s11998-015-9658-3. GUTTMANN, P., WERNER, S., SIEWERT, F., SOKOLOV, A., SCHMIDT, J.-S., MAST, M., BRZHEZINSKAYA, M., JUNG, C., FOLLATH, R. & SCHNEIDER, G. (2018). The New HZB X-Ray Microscopy Beamline U41-PGM1-XM at BESSY II. Microscopy and Microanalysis 24, 206–207. HALICKA, K. & CABAJ, J. (2021). Electrospun nanofibers for sensing and biosensing applications—a review. International Journal of Molecular Sciences 22, 1–24. HAN, D. & STECKL, A. J. (2019). Coaxial Electrospinning Formation of Complex Polymer Fibers and their Applications. ChemPlusChem 84, 1453–1497. HE, C. L., HUANG, Z. M., HAN, X. J., LIU, L., ZHANG, H. S. & CHEN, L. S. (2006). Coaxial electrospun poly(L-lactic acid) ultrafine fibers for sustained drug delivery. Journal 33 of Macromolecular Science, Part B: Physics 45 B, 515–524. JI, Y., LI, B., GE, S., SOKOLOV, J. C. & RAFAILOVICH, M. H. (2006). Structure and nanomechanical characterization of electrospun PS/clay nanocomposite fibers. Langmuir 22, 1321–1328. KUMAR, V. & SUH, N. P. (1988). ‘Process Synthesis for Manufacturing Microcellular Thermoplastic Parts: a Case Study in Axiomatic Design.’ Massachusetts Institute of Technology http://hdl.handle.net/1721.1/14616. LANG, J. T., KULKARNI, D., FOSTER, C. W., HUANG, Y., SEPE, M. A., SHIMPALEE, S., PARKINSON, D. Y. & ZENYUK, I. V. (2023). X-ray Tomography Applied to Electrochemical Devices and Electrocatalysis. Chemical reviews 123, 9880–9914. LI, Y. & WAN, W. (2017). Exploring Polymer Nanofiber Mechanics: A review of the methods for determining their properties. IEEE Nanotechnology Magazine 11, 16– 28. LIU, LAIJUN, ZHANG, T., LI, C., JIANG, G., WANG, F. & WANG, L. (2021). Regulating surface roughness of electrospun poly(ε-caprolactone)/β-tricalcium phosphate fibers for enhancing bone tissue regeneration. European Polymer Journal 143, 110201. https://doi.org/10.1016/j.eurpolymj.2020.110201. LIU, XIAOYANG, RONNE, A., YU, L. C., LIU, Y., GE, M., LIN, C. H., LAYNE, B., HALSTENBERG, P., MALTSEV, D. S., IVANOV, A. S., ANTONELLI, S., DAI, S., LEE, W. K., MAHURIN, S. M., FRENKEL, A. I., WISHART, J. F., XIAO, X. & CHEN-WIEGART, Y. CHEN K. (2021). Formation of three-dimensional bicontinuous structures via molten salt dealloying studied in real-time by in situ synchrotron X-ray nanotomography. Nature Communications 12. http://dx.doi.org/10.1038/s41467-021- 23598-8. 34 LIU, XINKUAN, XU, H., ZHANG, M. & YU, D. G. (2021). Electrospun medicated nanofibers for wound healing: Review. Membranes 11. LUCY A BOSWORTH, S. D. (2011). Electrospinning for Tissue Regeneration. Woodhead Publishing. MAKSIMCUKA, J., OBATA, A., SAMPSON, W. W., BLANC, R., GAO, C., WITHERS, P. J., TSIGKOU, O., KASUGA, T., LEE, P. D. & POOLOGASUNDARAMPILLAI, G. (2017). X- ray tomographic imaging of tensile deformation modes of electrospun biodegradable polyester fibers. Frontiers in Materials 4, 1–11. MITCHELL, G. R. (2011). Electrospinning principles, practice and possibilities. The Royal Society of Chemistry , www.rsc.org. NYGAARD, J. V., UYAR, T., CHEN, M., CLOETENS, P., KINGSHOTT, P. & BESENBACHER, F. (2011). Characterisation of internal morphologies in electrospun fibers by X-ray tomographic microscopy. Nanoscale 3, 3594–3597. ORSI, S., DI MAIO, E., IANNACE, S. & NETTI, P. A. (2014). Hollow micro- and nanoparticles by gas foaming. Nano Research 7, 1018–1026. RAMAKRISHNA, S., FUJIHARA, K., TEO, W. E., LIM, T. C. & MA, Z. (2005). An introduction to electrospinning and nanofibers. World Scientific. SALEM, D. R. (2001). Structure Formation in Polymeric Fibers. Hanser. SCHNEIDER, G., GUTTMANN, P., REHBEIN, S., WERNER, S. & FOLLATH, R. (2012). Cryo X-ray microscope with flat sample geometry for correlative fluorescence and nanoscale tomographic imaging. Journal of Structural Biology 177, 212–223. http://dx.doi.org/10.1016/j.jsb.2011.12.023. SENSINI, A., CRISTOFOLINI, L., FOCARETE, M. L., BELCARI, J., ZUCCHELLI, A., KAO, A. & 35 TOZZI, G. (2018). High-resolution x-ray tomographic morphological characterisation of electrospun nanofibrous bundles for tendon and ligament regeneration and replacement. Journal of Microscopy 272, 196–206. SHEN, H., NUTT, S. & HULL, D. (2004). Direct observation and measurement of fiber architecture in short fiber-polymer composite foam through micro-CT imaging. Composites Science and Technology 64, 2113–2120. SHKARINA, S., SHKARIN, R., WEINHARDT, V., MELNIK, E., VACUN, G., KLUGER, P., LOZA, K., EPPLE, M., IVLEV, S. I., BAUMBACH, T., SURMENEVA, M. A. & SURMENEV, R. A. (2018). 3D biodegradable scaffolds of polycaprolactone with silicate-containing hydroxyapatite microparticles for bone tissue engineering: High-resolution tomography and in vitro study. Scientific Reports 8, 1–13. SINGH, M. & SINGH, A. (2021). Characterization of Polymers and Fibers. Woodhead Publishing. SOLIMAN, S., SANT, S., NICHOL, J. W., KHABIRY, M., TRAVERSA, E. & KHADEMHOSSEINI, A. (2011). Controlling the porosity of fibrous scaffolds by modulating the fiber diameter and packing density. Journal of Biomedical Materials Research - Part A 96 A, 566–574. STANGER, J., TUCKER, N. & STAIGER, M. (2005). Electrospinning: Expert overviews covering the science and technology of rubber and plastics. Rapra Review Reports. THOMAS, T. R. (1981). Characterization of surface roughness. Precision Engineering 3, 97–104. TIAN, Y., WANG, Z. & WANG, L. (2021). Hollow fibers: From fabrication to applications. Chemical Communications 57, 9166–9177. Tomviz Software (n.d.). https://tomviz.org/ (Accessed May 24, 2023). 36 TORRE, J. (2023). ImageJ-Scripts Repository. https://github.com/Axeh99/ImageJ-Scripts. VALENCIA-OSORIO, L. M. & ÁLVAREZ-LÁINEZ, M. L. (2021). Global View and Trends in Electrospun Nanofiber Membranes for Particulate Matter Filtration: A Review. Macromolecular Materials and Engineering 306, 1–20. VENTURA, H., SORRENTINO, L., LAGUNA-GUTIERREZ, E., RODRIGUEZ-PEREZ, M. A. & ARDANUY, M. (2018). Gas dissolution foaming as a novel approach for the production of lightweight biocomposites of PHB/natural fibre fabrics. Polymers 10. VOHRA, A., RATURI, P. & HUSSAIN, E. (2023). Scope of using hollow fibers as a medium for drug delivery. Fiber and Textile Engineering in Drug Delivery Systems 169–213. http://dx.doi.org/10.1016/B978-0-323-96117-2.00013-3. WANG, J., GUO, Z. & XIONG, S. M. (2017). Characterization of the morphology of primary silicon particles using synchrotron X-ray tomography. Materials Characterization 123, 354–359. http://dx.doi.org/10.1016/j.matchar.2016.12.004. WANG, YU, PU, J., WANG, L., WANG, J., JIANG, Z., SONG, Y. F., WANG, C. C., WANG, YANFEI & JIN, C. (2016). Characterization of typical 3D pore networks of Jiulaodong formation shale using nano-transmission X-ray microscopy. Fuel 170, 84–91. http://dx.doi.org/10.1016/j.fuel.2015.11.086. WERNER, S., GUTTMANN, P., SIEWERT, F., SOKOLOV, A., MAST, M., HUANG, Q., FENG, Y., LI, T., SENF, F., FOLLATH, R., LIAO, Z., KUTUKOVA, K., ZHANG, J., FENG, X., WANG, Z. S., ZSCHECH, E. & SCHNEIDER, G. (2023). Spectromicroscopy of Nanoscale Materials in the Tender X-Ray Regime Enabled by a High Efficient Multilayer-Based Grating Monochromator. Small Methods 7. WILLIAMS, G. R., RAIMI-ABRAHAM, B. T. & LUO, C. J. (2018). Nanofibres in Drug Delivery. UCL Press. 37 WONG, S. C., BAJI, A. & LENG, S. (2008). Effect of fiber diameter on tensile properties of electrospun poly(ε-caprolactone). Polymer 49, 4713–4722. YOSHIOKA, T., DERSCH, R., TSUJI, M. & SCHAPER, A. K. (2010). Orientation analysis of individual electrospun PE nanofibers by transmission electron microscopy. Polymer 51, 2383–2389. http://dx.doi.org/10.1016/j.polymer.2010.03.031. ZOU, L., GE, M., ZHAO, C., MENG, Q., WANG, H., LIU, X., LIN, C. H., XIAO, X., LEE, W. K., SHEN, Q., CHEN, F. & CHEN-WIEGART, Y. C. K. (2020). Designing Multiscale Porous Metal by Simple Dealloying with 3D Morphological Evolution Mechanism Revealed via X-ray Nano-tomography. ACS Applied Materials and Interfaces 12, 2793–2804.