scieee AI-readable full text Open interactive document viewer

Strengthening of existing concrete structures with fibre reinforced polymers (FRP) in the new version of Eurocode 2

Oller Ibars, Eva,de Diego, Ana,Torres Llinàs, Lluís,Madera, Pedro

Abstract

This paper aims to introduce the content of Annex J “Strengthening of Existing Concrete Structures with CFRP” of Eurocode 2 [1]. This is first time that the design of adhesively bonded reinforcement with CFRP has been introduced in the European regulations through an informative annex. Annex J considers two different bonded strengthening techniques: externally bonded reinforcement (EBR) that consists of bonding CFRP strips or sheets to the surface of concrete elements, and near surface mounted reinforcement (NSM) that consists of embedded CFRP strips or rods to the slot cut in the concrete cover. Since, the content of Annex J is new, a summary and background related to all aspects required for designing CFRP strengthened systems for concrete structures, are given in this paper.

Full text

Oller, E., De Diego, A., Torres, L., & Madera, P. (2023) Hormigón y Acero 74(299-300); 151-167 – 151 Strengthening of Existing Concrete Structures with Fibre Reinforced Polymers (FRP) in the New Version of Eurocode 2 Refuerzo de estructuras existentes de hormigón con polímeros reforzados con fibras (PRF) en la nueva versión del Eurocódigo 2 Eva Oller *,a , Ana de Diego b , Lluís Torres c , y Pedro Madera d a Department of Civil and Environmental Engineering. Universitat Politècnica de Catalunya b Instituto de Ciencias de la Construcción Eduardo Torroja (IETCC), CSIC c Department of Mechanical Engineering and Industrial Construction. Universitat de Girona d Mapei Recibido el 11 de agosto de 2022; aceptado el 5 de diciembre de 2022 * Persona de contacto / Corresponding author: Correo-e / e-mail: [email protected] (Eva Oller Ibars). Hormigón y Acero 2023; 74(299-300):151-167 https://doi.org/10.33586/hya.2022.3099 Disponible en www.hormigonyacero.com How to cite this article: Oller, E., De Diego, A., Torres, L., & Madera, P. (2023) Strengthening of Existing Concrete Structures with Fibre Reinforced Polymers (FRP) in the New Version of Eurocode 2, Hormigón y Acero 74(299-300):151-167, https://doi.org/10.33586/hya.2022.3099 abstract This paper aims to introduce the content of Annex J “Strengthening of Existing Concrete Structures with CFRP” of Eurocode 2 [1]. This is first time that the design of adhesively bonded reinforcement with CFRP has been introduced in the European regulations through an informative annex. Annex J considers two different bonded strengthening techniques: externally bonded reinforcement (EBR) that consists of bonding CFRP strips or sheets to the surface of concrete elements, and near surface mounted reinforcement (NSM) that consists of embedded CFRP strips or rods to the slot cut in the concrete cover. Since, the content of Annex J is new, a summary and background related to all aspects required for designing CFRP strengthened systems for concrete structures, are given in this paper.. keywordS: Strengthening, fibre reinforced polymer, externally bonded reinforcement, near surface bonded reinforcement, bond, reinforced concrete, prestressed concrete. ©2023 Hormigón y Acero, the journal of the Spanish Association of Structural Engineering (ACHE). Published by Cinter Divulgación Técnica S.L. This is an open-access article distributed under the terms of the Creative Commons (CC BY-NC-ND 4.0) License resumen Este artículo tiene por objeto introducir el contenido del Anejo J del Eurocódigo 2 [1]: “Refuerzo de estructuras de hormigón existentes con CFRP”. Esta es la primera vez que el dimensionamiento de refuerzos adheridos con CFRP se introduce en la normativa europea a través de un anejo informativo. El Anejo J contempla dos técnicas de refuerzo adherido diferentes: el refuerzo adherido externamente (EBR) que consiste en pegar laminados o tejidos de CFRP a la superficie de los elementos de hormigón a reforzar, y el refuerzo insertado en el recubrimiento (NSM) que consiste en instalar el laminado o barra de CFRP en una ranura realizada en el recubrimiento del hormigón. Como el Anejo J en sí es una novedad, este artículo presenta un resumen de su contenido y algunos antecedentes relacionados con todos los aspectos necesarios para diseñar un sistema de refuerzo con CFRP para estructuras de hormigón. palabraS clave: Refuerzo, polímeros reforzados con fibras, refuerzo adherido externamente, refuerzo embebido en ranuras, adherencia, hormigón armado, hormigón pretensado. ©2023 Hormigón y Acero, la revista de la Asociación Española de Ingeniería Estructural (ACHE). Publicado por Cinter Divulgación Técnica S.L. Este es un artículo de acceso abierto distribuido bajo los términos de la licencia de uso Creative Commons (CC BY-NC-ND 4.0) 1. introduction Strengthening of existing reinforced and prestressed concrete structures might be necessary to restore or increase their load-bearing capacity due to different reasons: an increase of load demand caused by a change of use, a loss of carrying capacity due to deterioration or structural damage, or to eliminate structural design or construction deficiencies. During the 1990’s, fibre reinforced polymer (FRP) laminates, which were related to other industries such aeronautics or sports, were introduced in the construction field to overcome the drawbacks of steel plates bonded to the tensile concrete surface, which were corrosion and weight among others. FRP is the denomination of a composite material formed by a polymeric matrix reinforced with continuous glass (GFRP), basalt (BFRP), carbon (CFRP) or aramid (AFRP) fibres. Recently, other composites formed by natural fibres or PBO (polyphenylene bezobisoxazole) with a cementitious matrix [2,3] have been introduced in the strengthening field but with limited research applications. The first application of FRP strengthening in Europe was in 1991, in the Ibach bridge (Switzerland), a historic wooden bridge that was strengthened by externally bonded CFRP laminates [4]. Since then, the strengthening technique consisting on adhesively bonding a reinforcement (ABR) of FRP to an existing structure constitutes a well established technology. FRPs have been effectively applied as flexural strengthening, shear strengthening and confinement of columns (see Figure 1). There are many reasons of their increasing use, especially in aggressive environments, since they show a high strength-to-weight and stiffness-to-weight ratio, a potential high durability given by their resistance to corrosion, no need of scaffolding, reduction in labour costs, and versatility with practically unlimited availability of dimensions. However, FRP strengthened systems present also some drawbacks such as their reduced ductility due to their linear elastic behaviour up to failure, possible degradation under high temperatures depending on the glass transition temperature of the resin, and the cost of the material itself. The future version of Eurocode 2 [1] will include an informative annex (Annex J) with the rules for strengthening existing plain, reinforced and prestressed normal weight concrete structures only with CFRP materials. This annex covers only CFRP materials because it is the most common fibre type in research and real applications. In addition, there is not enough experience in strengthening of special concrete structures, such as lightweight concrete or concrete with recycled aggregates. Adhesively bonded reinforcement (ABR) gives wider applications for different methods and products. Annex J of Eurocode 2 [1] considers two possible applications: externally bonded reinforcement (EBR) [5–8] and near surface mounted reinforcement (NSM) [9–13]. EBR consists of strips or sheets bonded on the surface of a concrete support (see Figure 2a) and NSM consists of strips or bars applied in slot cuts in the concrete cover (see Figure 2b). Compared to EBR, the NSM technique provides better bond characteristics, the reinforcement can be anchored more easily to prevent debonding and it is more protected against mechanical damage or vandalism. Other strengthening techniques such as Textile Reinforced Mortar (TRM) [14], embedded through the section reinforcement [15] or other bonded configurations are not included in Annex J because there is not a consolidate experience with all of them. In addition, prestressed ABR is not considered for the same reason. This paper aims to introduce the content of Annex J “Strengthening of Existing Concrete Structures with CFRP” of Eurocode 2 [1]. This is the first time that the design of CFRP strengthening systems has been introduced in European regulations. Model Code 2010 [17] included FRP reinforcement in two sections 5.5 “Non-metallic reinforcement” and 6.2 “Bond 152 – Oller, E., De Diego, A., Torres, L., & Madera, P. (2023) Hormigón y Acero 74(299-300); 151-167 a) b) c) Figure 1. a) Flexural strengthening, b) shear strengthening, c) column confinement (courtesy of Mapei). a) b) Figure 2. a) Externally bonded reinforcement (courtesy of Mapei), b) Near surface mounted reinforcement [16]. Oller, E., De Diego, A., Torres, L., & Madera, P. (2023) Hormigón y Acero 74(299-300); 151-167 – 153 of non-metallic reinforcement”, explaining the main principles of this technique. There are also some European guidelines such as DAfStb Heft 595 [18], TR-55 [19], CNR-DT-200 R1 2013 [20], AFGC [21], SIA [22] and GRECO [23]. The fib Bulletin 14 [24] was published in 2001 and gave detailed guidelines on the use of FRP externally bonded reinforcement, practical execution and quality control, based on the expertise of the members of fib TG9.3 “FRP Reinforcement for concrete structures”. The advance of the state-of-the-art of the last two decades was updated in fib Bulletin 90 [16] by fib TG5.1 (former TG9.3) in 2019. This document aimed to cover both externally bonded and near-surface mounted reinforcement for concrete structures. It was presented in a Eurocode-com- patible format, with the objective of being also a background document for Annex J and to form the basis for the updating of the text on seismic retrofitting with composites in the next version of Eurocode 8. In addition, there is a background document of Annex J [25] with more details about the derivation of the formulations included in this paper. 2. basis of design, materials and durability In general, the basis of design of concrete structures with conventional materials can be applied to reinforced (RC) and prestressed concrete (PC) strengthened with adhesively bonded CFRP reinforcement. However, there are some aspects such as the material safety factors that should be particularized for this case. Unless a National Annex gives different values, Table 1 complies the partial safety factors for ABR. As observed, safety factors are higher for in-situ wet lay-up sheets than for prefabricated strips and bars. These safety factors were obtained based on the regulations of prEN 1990:2020 [26] and the products considered in the determination of these factors were those used in the structural tests used in the calibration of approaches included in the subsections of Annex J related to Ultimate Limit States, Serviceability Limit States, Fatigue and Bond. The safety concept for bond is based on design assisted by testing. The safety factor for bond, γBA, was taken from [16], assuming failure in the concrete substrate or failure of the adhesive. This factor is the one specified in the main text of Eurocode 2 [1] for the design value of the ultimate bond stress. TABLE 1. Partial safety factors for ABR strengthening [1]. Design situation Tensile strength Bond strength CFRP strips and bars In-situ lay-up Failure CF sheets in concrete or adhesive Designation γf γBA Persistent and transient 1.30 1.40 1.50 Accidental 1.10 1.15 1.15 Serviceability 1.00 1.00 1.00 Fatigue 1.30 1.40 1.50 In relation to the materials employed for strengthening, there is a different particularity in comparison with other construction materials. The system is made by the combination of fibres and a matrix, designed to work together, and with a specific binder applied to the surface of the support [16]. Therefore, only systems that have been tested and applied to real scale structures can be applied as ABR. In addition, the selection of the system type depends on the configuration and on the structure to be strengthened. A general description on FRP materials, systems and techniques can be found in fib Bulletin 90 [16]. The material properties should be given by the suppliers. The FRP strengthening systems shall comply with national or international product standards, such as ISO 10406 [27] that specify their geometrical, mechanical and technological properties. Annex J gives recommended values of some parameters where test procedures are not standardized yet. Test procedures for the essential characteristics of construction products at European level, may be included in two types of technical specifications: European harmonised product standards or European Assessment Documents (EAD). EADs are currently under preparation for CFRP strengthening systems. The design rules included in Annex J are for CFRP systems that accomplish the following conditions: . interlaminar shear strength of CFRP strips according to EN ISO 14130 [28] shall be equal or larger than the adhesive bond strength for any system, . mean modulus of elasticity of CFRP strips: 150 000 MPa ≤ Ef ≤ 250 000 MPa, . elastic stiffness per unit width of carbon fibre (CF) sheets: 20 kN/mm ≤ Ef Af ⁄bf ≤ 400 kN/mm, . total CF cross section per unit width of CF sheets in the total of all layers determined in the direction of the tension action effect applied to the system: 100 mm²/m ≤ Af ⁄bf ≤ 1800 mm²/m. . characteristic tensile strength of the adhesive fAtk, determined in accordance with EN 1504-4 [29] shall be fAtk ≥ 14 N/mm². Annex J requires the definition of the following properties for CFRP strips and sheets that are going to be used as ABR strengthening systems: ffuk, characteristic short-term tensile strength of the ABR according to ISO 10406 [27]; ηf, reduction factor applied to the tensile strength; Ef, average mean modulus of elasticity of the ABR in the longitudinal direction; εfuk, characteristic ultimate strain; and Af, cross sectional area. For strips Af is taken as bf ∙ tf (where bf is the width and tf is the thickness of the cross section). For sheets, Af is obtained from relevant production data, considering tf = nf kf Af ⁄bf being nf the number of layers, Af ⁄bf the cross sectional area of the fibres per meter of a single layer of CF sheet, and kf = 0.85 if the number of layers is higher than 3, or 1.00 otherwise. For the adhesive, Annex J requires the characteristic compressive strength, fAck, and the characteristic tensile strength, fAtk, determined in accordance with EN 1504-4 [29]. FRP materials are linear elastic up to failure, as shown in the design stress-strain relationship in Figure 3. The design tensile strength of the ABR system shall be obtained as: where: ffuk is the characteristic tensile strength, γf is the partial safety factor, and ηf is a reduction factor applied to the tensile strength of the ABR for the relevant exposure conditions in accordance with ISO 10406 [27], and may be taken as 0.7 unless more accurate information is available. In a similar manner to conventional RC and PC structures, durability of the strengthened structure, and in particular of the CFRP system and adhesive should be ensured during lifetime according to the exposure classes. The FRP-concrete interface is the critical component of the system since the transfer of stresses occurs through it, and bond quality is affected by the environmental conditions. Therefore, additional protective measures should be included to ensure durability if necessary. Special attention should be paid to the exposure of the strengthened element to direct UV radiation, penetration of moisture and temperature. 3. structural analysis According to Annex J, members strengthened with ABR should not be analysed using linear elastic analysis with limited redistribution or plastic analysis, since the CFRP systems are linear elastic up to failure. The glass transition temperature usually ranges from 50 to 80oC for epoxy and for processed FRP elements ranges from 130 to 140oC. This means that in the event of fire, protection systems may be required in such a way that service temperature is limited with respect to the glass transition temperature. During fire, the CFRP strengthening system will be lost due to the weakening of the adhesive. If this is the case, the existing structure should bear this accidental design situation without collapse, complying with the robustness requirement. This is similar to other accidental situations such as vandalism, blast or impact, where the design engineer should verify the structure against accidental loss of FRP. 4. ultimate limit states 4.1. Bending with and without axial forces When strengthening in flexure RC or PC sections, the design of the required ABR area can be obtained by applying sectional equilibrium and compatibility conditions, in a similar manner than conventional concrete elements but with an additional reinforcement, assuming that the slip between the CFRP reinforcement and the concrete substrate is neglected, that is, full composite action between the CFRP and the substrate. The strain state of the unstrengthened element before strengthening should be considered since the strains from additional bending effects after strengthened should be superimposed to the existing ones when verifying the capacity of the strengthened element. Fib bulletin 90 [16] recommends the process given by the flow chart of Figure 4. Figure 4. Design process when strengthening a section in flexure recommended by fib Bulletin 90 [16]. When designing the CFRP strengthening system, it is desirable that the strengthened element fails in a ductile manner after steel yielding. So, the governing modes of failure of a flexural element will be steel yielding followed by concrete crushing or steel yielding followed by FRP rupture. As observed in many experimental programs, debonding of the CFRP strengthening system might occur before reaching a classical failure mode (see Figure 5). Debonding is more common in externally bonded reinforcement and might initiate at any location different from the critical section considered to design the flexural strengthening system. To avoid this type of premature failure, debonding should be checked following the procedure described in Section 7 of this paper. Usually, the reason for strengthening is motivated by strength increase to comply with ULS requirements. However, sometimes the serviceability limit state governs the design, Figure 3. Design stress-strain relationship for the CFRP strengthening system [16]. 154 – Oller, E., De Diego, A., Torres, L., & Madera, P. (2023) Hormigón y Acero 74(299-300); 151-167 and larger amounts of CFRP than those required for ULS should be applied. Provisions of Annex J for flexural strengthening with and without axial forces for both EBR and NSM are in accordance with fib Bulletin 90 [16]. Figure 5. Debonding of the CFRP strengthening system [30]. 4.2. Confinement It is well known that confinement can enhance the load bearing capacity of axial loaded members. Concrete confined by FRP behaves differently from concrete confined by steel. Due to the linear elastic behaviour up to failure, FRP apply an ever-increasing confinement pressure to the concrete core. The stress–strain behaviour of FRP-con- fined concrete typically displays an approximately bilinear ascending response, and ultimate capacity is governed by tensile failure of the FRP (Figure 6). The ultimate strength of the confined concrete is closely related with the rupture strain of the FRP reinforcement. Many experimental studies have shown that the rupture strain values of FRP jackets are consistently lower than the ultimate tensile strain obtained by standard tensile testing of FRP coupons [31,32]. The ratio between the two values is called strain efficiency factor. There are a number of possible reasons for this premature failure of the FRP jacket, such as the multiaxial stress state, stress concentrations due to concrete failure, or the jacket curvature, especially at corners with low radius. Figure 6. Failure mode of FRP confined concrete. Current international design guidelines provide predictive design equations to calculate the ultimate strength and strain of FRP confined concrete columns subjected to pure axial load, as a function of the confining pressure applied by the FRP jacket. It is known that the confinement of non-cir- cular columns is less efficient than the confinement of circular columns [33–35] (see Figure 7a). In a circular cross section, the jacket exerts a uniform confining pressure over the entire perimeter. In the case of a rectangular cross section, the confining action is mostly concentrated at the corners. The predictive equations found in the design guides are mostly based on approaches deduced for circular columns and then modified by a shape factor, usually defined as the ratio of the effectively confined area to the gross area. Annex J gives provisions to consider the effect of concrete confinement achieved by bonding hoop CFRP around existing columns (see Figure 7b and 7c). Since the formulations have an empirical basis, Annex J limits them to columns with a diameter greater than 150 mm and with characteristic concrete strength less than 50 MPa. Experimental studies outside this range are scarce and show that the effect of confinement is very limited in high strength concrete. In addition, the first-order eccentricity of the axial load must meet the condition e0 ⁄ Deq ≤ 0.20 and the slenderness satisfy the condition l0 ⁄ Deq ≤40. For the application of the equations given in Annex J to rectangular sections the rounding radius of the corners must be rc ≥ 20 mm and the aspect ratio h ∕ b ≤ 2. According to Annex J, the increase in compressive strength of concrete due to CFRP confinement can be calculated as follows: For circular columns: ∆fcd = 0 for < 0.07 (2) tf ffud D fcd ∆fcd = kcc ffud for ≥ 0.07 (3) tf ffud D fcd tf D with kcc = 2.5 unless more accurate information is available. In the case of discontinuous and/or helical wrapping the value of ffud in equations (2) and (3) should be multiplied by the efficiency factor kh (see Figure 7b and 7c): kh = 1– (4) (sf – bf) 2 D 1 1+(tanβf)2 2 For rectangular columns: ∆fcd = kcc ke kr ffud for ke ≥ 0.07 (6) tf kr ffud D fcd tf Deq b h b h 2 2 ∆fcd = 0 for ke < 0.07 (5) tf kr ffud Deq fcd b h 2 where: kcc = 1.5 unless more accurate information is available. Deq = (7) 2 b h b + h ke = 1– (8) (b – 2 rc)2+(h – 2 rc)2 3 b h Oller, E., De Diego, A., Torres, L., & Madera, P. (2023) Hormigón y Acero 74(299-300); 151-167 – 155 kr = (9) ke is the ratio between effectively confined area and gross area (see Figure 7a). kr is a reduction factor that takes into account that, for rectangular sections, the smaller the corner radius the lower the rupture strain of the FRP jacket. For discontinuous and/or helical wrapping on rectangular columns the value of ffud in equations (5) and (6) should be multiplied by kh according to (10): kh = 1– 1– (10) (sf – bf) 2 b 1 1+(tanβf)2 (sf – bf) 2 h The above equations largely align with the provisions of fib bulletin 90 [16]. Equations (3) and (6) implicitly include a strain efficiency factor equal to 0.5, in accordance with [16], for circular and square or rectangular sections with a corner radius rc ≥ 50 mm. However, while in [16] the factor kcc is 3.3, according to the original model of Lam and Teng [32], Annex J indicates that the value of kcc can be taken as 2.5 for circular columns and 1.5 for square and rectangular columns unless more accurate information is available. 4.3. Shear In a RC or PC element, the shear strength should be checked by following the general provisions of §8.2 of new Eurocode 2 [1], without considering the flexural CFRP ABR (if this is the case) in the contribution of the longitudinal reinforcement. If the design shear stress is higher than the shear strength, then shear strengthening is required, and the section can be strengthened by EBR or NSM techniques. Externally bonded CFRP shear strengthening can be performed in two different configurations (see Figure 8): a) sheets fully wrapping the section (closed wrapped); b) sheets or L‐shaped strips bonded on the lateral sides and the bottom surface of the beam (open or U‐shaped systems). The side-bonded configuration, which consists of bonding sheets or strips in the lateral faces of the section is not allowed since they are prompt to debond at both sides of the critical shear crack once it opens and widens. The sheets and strips can be bonded in a continuous or discontinuous configuration. Closed wrapped CFRP configurations fail due to fibre rupture, sometimes initiated near the corner of the sections that have been rounded to avoid sharp zones that may lead to fibre rupture. Open or U-shaped configurations are susceptible of debonding once a critical shear crack opens and propagates. Then, if the bonded length of each strip at the upper side of the crack (for the U‐shaped) is not long enough to anchor the tensile force of the FRP, the laminate debonds suddenly 156 – Oller, E., De Diego, A., Torres, L., & Madera, P. (2023) Hormigón y Acero 74(299-300); 151-167 a) b) c) Figure 7. a) Effectively confined section in a rectangular section; b) confinement with discrete strips and c) with helically bonded strips, adapted from [16]. Figure 8. Shear strengthening configurations. before reaching its ultimate tensile strength. This debonding failure mode should be considered in the calculation of the shear capacity of the strengthened element and can be delayed or can be avoided by using appropriate anchorage devices. Annex J recommends the application of anchorage devices when strengthening T-shaped cross sections. The total shear strength of a section strengthened with CFRP may be taken as: where: τRd is the design shear strength according to Section 8.2 of Eurocode 2 [1]. = (13) for discrete CFRP strips or CF sheets 2tf sinαf for continuous CF sheets Af sf 2tf bf sf αf is the angle formed between the CFRP system and the longitudinal member axis; ffwd is the design shear strength of the CFRP system. θ should be taken as 45 degrees for the calculation of τRd and τRd,f, unless more rigorous analysis is undertaken. Formulations to assess the contribution of the CFRP strip or sheet to the total shear strength consider the different type of configurations. For closed CFRP systems, the design shear strength is defined as Equation (14). ffwd = 0.8 kr ffud (14) Where: ffud should be determined using Equation (1) and kr should be determined using Equation (9). For open discrete CFRP systems, debonding should be tak- en in consideration and the shear strength can be obtained through Equation (15) and (16), depending on the length of the strip above the critical shear crack and the maximum bond length, lbf,max,k. In any case, the shear strength ffwd is limited by Equation (14). ffwd is determined by Equation (15) if the anchorage length into the compression zone of the member of all CFRP strips, lbf is less than lbf,max,k. ffwd is determined by Equation (16) if the anchorage length into the compression zone of the member of some CFRP strips, lbf is less than lbf,max,k. where the parameters m and n are defined in Equation (17) and (18), and in Figure 9. The maximum bond length lbf,max,k and the anchorage resistance fbfRd shall be determined according to §8 of this paper. The open continuous sheet system can be treated as a particular case of the discontinuous case with sf = bf ⁄ sinα. Then, n sf = hf (cotθ+cotαf), m sαf = lbf,max,k (cotθ + cotαf) sinαf and m ⁄ n = lbf,max,k sinαf ⁄ hf [16]. D’Antino and Triantafillou [36] performed an assessment of five design guidelines (EN 1998‐3 [37], ACI 440.2 R‐08 [38], DAfStb Heft 595 [18], TR‐55 [19], CNR‐DT/200‐R1. 2013 [20]) and a new proposed model, based on the German guideline [18], which is very similar to the proposal included in Annex J. The assessment was performed with a database of 229 RC shear - strengthened beams that failed in shear. They concluded that all models tend to underestimate the FRP shear strength for the completely wrapped configuration. However, models were more accurate for the U‐shaped configuration. The proposal gave conservative results (mean value of the experimental to theoretical ratio MV=1.77 and coefficient of variation COV=2.21 for U‐shaped and MV=3.51 and COV=4.32 for wrapped). In the framework of TG1, Oller and Kotynia presented in [39] an analysis of the performance of different existing Oller, E., De Diego, A., Torres, L., & Madera, P. (2023) Hormigón y Acero 74(299-300); 151-167 – 157 Figure 9. n and m parameters in a CFRP shear-strengthened beam [1]. formulations to quantify the FRP contribution to the shear strength of RC elements strengthened in shear by externally bonded FRP sheets [16,18–20,24,40–48]. A large database of 555 tests (355 with rectangular section and 200 with T-sec- tion) has been assembled distinguishing between the shape of the section, the existence of internal transverse reinforcement and the FRP configurations. Selected beams with a/d higher than 2.5, that were well‐documented, and which had a rectangular (276) or a T (180) cross‐section, were externally strengthened in a closed (71 R + 68 T), open (114 R + 98 T) or side bonded (91 R + 14 T) configuration with FRP wet lay‐up or pultruded strips in a continuous or discontinuous manner, and with or without internal transverse steel reinforcement. In general, predictions for all models were more conservative for beams without transverse reinforcement. In some cases, predictions were unsafe for beams with transverse reinforcement, showing a possible interaction with the internal transverse reinforcement which is not considered in the experimental FRP contribution to the shear strength. For closed FRP configurations, models generally assumed failure at the bottom corner of the section and predictions were very conservative where failure was experimentally observed along the web. This is the case of the formulation included in Annex J, with a mean value of the experimental to the theoretical ultimate shear force ranging between 1.21 and 2.91 for beams without transverse reinforcement and coefficient of variation (COV) ranging from 38 to 49%. For beams with rectangular section with internal stirrups and continuous CFRP configuration, the mean value is less conservative than for the remaining cases, 0.83 with a similar COV. For open configurations, results depended mainly on the assumed bond model and are more accurate than in the previous case, showing for some models unsafe predictions for the continuous FRP system applied in beams with transverse reinforcement. This is the case of the formulation of Annex J, where MV = 0.85 and 0.53 for rectangular beams with internal stirrups and with a discontinuous and continuous CFRP configuration, respectively. According to fib Bulletin 90 [16], the contribution of anchored NSM reinforcement to the shear capacity of the element can be approximately computed with the same model of EBR. 4.4. Torsion, Punching and Design with strut-and-tie models Annex J doesn’t give provisions for CFRP strengthening in torsion or in punching-shear. There is not enough data in the literature to include provisions related to both torsion and punching-shear. 5. serviceability limit states The verification of serviceability limit states (SLS) considers the limitation of stresses to avoid steel yielding, damage or excessive creep of concrete, adhesives or FRP, or creep rupture of FRP, limitation of cracking and deflections. In some cases, SLS governs the design of the strengthening system, even the main purpose was the strength increase. The previous state of stresses and deflections should be considered in the verification of the SLS. Under service load conditions, stresses in the concrete and in the longitudinal reinforcement of the strengthened struc- 158 – Oller, E., De Diego, A., Torres, L., & Madera, P. (2023) Hormigón y Acero 74(299-300); 151-167 Figure 10. Example of cracking pattern after strengthening [30]. ture are limited according to the main text of Eurocode. As a result of the limitations of the longitudinal tensile steel reinforcement stresses, the stress in the FRP should be limited due to compatibility reasons. Therefore, under the characteristic combination of loading, the stress in the EBR or NSM CFRP reinforcement should be limited to: σf ≤ 0.8 fyk (19) Ef Es In relation to cracking, it has been observed experimentally that the presence of the CFRP strengthened systems induces the appearance of new cracks in between the existing ones due to the additional tensile stress transfer from the CFRP system to the concrete (see Figure 10). These new cracks usually show smaller crack widths and might be less conditioning than for the unstrengthened element. The strengthened element should fulfil the deflection limitations given by the main text of Eurocode 2 [1]. Deflections of beams or slabs strengthened with ABR may be estimated by ignoring the slip between the CFRP and concrete and transforming the area of CFRP to steel by taking account of the modular ratio, as considered in Annex J [1]. Deflections can be obtained for instance, by the double integration of the curvature, determined by a cross-section analysis along the RC element. In relation to long-term effects, they can be considered by considering the quasi-permanent load combinations and the modular ratios that consider the creep coefficient. However, there are limited existing studies about the long-term behaviour of concrete elements strengthened with FRP [49–51]. 6. fatigue Fatigue damage is not significant if the strengthened structure is exposed to typical service load ranges, but damage can occur if the load range exceeds 60% of load at first yield [52]. For this reason, special care should be taken in consideration, if the increase of service loading in the strengthened structures is significantly high. According to fib Bulletin 90 [16], in such cases under fatigue loading, failure occurs due to fracture of the longitudinal tensile reinforcement. Despite that FRP has an excellent fatigue strength, fatigue of bond should be considered since the loss of bond may lead to higher stresses in the longitudinal reinforcement with increased number of cycles. 6.1. Fatigue of externally bonded reinforcement (EBR) systems For EBR, Annex J presents a basic and a refined analysis for fatigue analysis for EBR CFRP systems, which is based on [18]. The basic analysis verifies that no damage due to cycling loading occurs, by limiting the increment of CFRP tensile forces in between cracks or at the laminate end to the elastic zone of the bond stress-slip relationship. Fatigue checking for EBR may be omitted if Equation (20) is accomplished. If this is the case, the upper load is limited by the load associated to the maximum bond stress. Then, strains are in the elastic range and no damage occurs. ΔFfE,equ ≤ ΔFfRd,fat1 = 0.35 fctm,surf1⁄4 fbfRd bf tf (20) where: ΔFfE,equ = max { bf tf ΔffEd,max ; FfEd,cr } (21) fbfRd is the limiting design strength of the bond in the area being considered, calculated according Equation (33). fctm,surf is the mean value of the tensile strength at the surface that can be determined by testing or estimated by Equation (31). ΔffEd,max is the maximum difference in CFRP stress under the relevant load combination between cracks given by Equation (39). FfEd,cr is the force in the CFRP at the first crack of the strengthened area. If Equation (20) is not accomplished, the refined analysis should be performed. In the refined analysis, the fatigue range S is used to obtain the tolerable number of cycles based on the S-N curve. As explained in [25], the refined analysis uses the S-N curve determined by some experimental data [53–58]. The number of load cycles needed for reaching a debonded length of 30 mm are calculated from the experimental programs of [53,54,57,58] by linear interpolation using the bond length and the number of cycles until completely debonding. For fitting the curve S-N, the unified related load ranges So,i, at a lower load level of 0, and the corresponding number of cycles N30 is needed. So,i is determined in a projection analysis using the Goodman relation. So is the difference between the maximum and minimum load related to the monotonic quasi-static load carrying capacity of the interface. The curve S-N has been obtained fitted to the experimental data. Under the frequent combination, the following condition, Equation (22), should be checked: where: ΔFfEd,fat is the design force range due to forces at the crack edge, Δff,max – Δff,min Δff,min is the minimum value of bf • tf • ΔffEd under the relevant fatigue load combination specified in Clause 10.2 of the main text of Eurocode 2 [1]. Δff,max is the maximum value of bf • tf • ΔffEd under the relevant fatigue load combination specified in Clause 10.2 of the main text of Eurocode 2 [1]. Δffk,B = bf tf ΔffEd where Δffk,B is calculated according Equation (44). αfat = 0.35 (24) N* 2 106 1 kf3 N* is the number of stress cycles. Oller, E., De Diego, A., Torres, L., & Madera, P. (2023) Hormigón y Acero 74(299-300); 151-167 – 159 [19] C.S.T.R. 55, Design guidance for strengthening concrete structures using fibre composite materials, London, Great Britain, 2012. [20] CNR (National Research Council) Advisory Committee on technical recommendations for construction, Instruzioni per la Progettazione, l’Esecuzione ed il Controllo di Interventi di Conslidamento Statico mediante l’utilizzo di Compositi Fibrorinforzati, CNR-DT200, Rome, Italy, 2013. [21] Association Française de Genie Civil, AFGC Réparacion et renforcement des structures en béton au moyen des matériaux compsites. Recommandations provisoires, 2011. [22] Schweirzerischer Ingenieur und Arhitektenverein, SIA166 Klebebewehrungen (Eternally bonded reinforcement), 2004. [23] Earthquake and protection planning organization, Greek Seismic Assessment Retrofit Code GRECO, 2013. [24] fib Task Group 9.3 FRP Reinforcement for Concrete Structures, Externally bonded FRP reinforcement for RC structures (2001). Technical report on the design and use of externally bonded fibre reinforced polymer reinforcement (FRP EBR) for reinforced concrete structures, Fib Bulletin 14., 2001. [25] European Committee for Standardization CEN, Background document for pr EN1992-1-1:2021, 2021. (*) [26] prEN 1990:2020: Eurocode – Basis of structural and geotechnical design, (2020). (*) [27] ISO/TC 71/SC 6 Non-traditional reinforcing materials for concrete structures, ISO 10406-1. Fibre-reinforced polymer (FRP) reinforcement of concrete Test methods Part 1: FRP bars and grids, 2015. [28] ISO/TC 61/SC 13 Composites and reinforcement fibres, ISO 14130:1997 Fibre-reinforced plastic composites — Determination of apparent interlaminar shear strength by short-beam method, 1997. [29] European Committee for Standardization CEN, EN 1504-4: 2004 Products and systems for the protection and repair of concrete structures - Definitions, requirements, quality control and evaluation of conformity - Part 4: Structural bonding, 2004. [30] E. Oller, Peeling failure in beams strengthened by plate bonding. A design proposal, Universitat Politécnica de Catalunya, 2005. [31] A. de Diego, Á. Arteaga, J. Fernández, Strengthening of square concrete columns with composite materials. Investigation on the FRP jacket ultimate strain, Compos. Part B Eng. 162 (2019) 454–460. https://doi. org/10.1016/j.compositesb.2019.01.017. [32] L. Lam, J.G. Teng, Design-oriented stress-strain model for FRP-con- fined concrete, Constr. Build. Mater. 17 (2003) 471–489. https://doi. org/10.1016/S0950-0618(03)00045-X. [33] T.M. Pham, M.N.S. Hadi, Stress Prediction Model for FRP Confined Rectangular Concrete Columns with Rounded Corners, J. Compos. Constr. 18 (2014). https://doi.org/10.1061/(asce)cc.1943-5614.0000407. [34] B. Shan, F.C. Gui, G. Monti, Y. Xiao, Effectiveness of CFRP Confinement and Compressive Strength of Square Concrete Columns, J. Compos. Constr. 23 (2019). https://doi.org/10.1061/(asce)cc.1943-5614.0000967. [35] A. de Diego, S. Martínez, V.J. Castro, L. Echevarría, F.J. Barroso, J.P. Gutiérrez, Experimental investigation on the compressive behaviour of FRP-con- fined rectangular concrete columns, Arch. Civ. Mech. Eng. 22 (2022). https://doi.org/10.1007/s43452-022-00450-4. [36] T. D’Antino, T.C. Triantafillou, Accuracy of design-oriented formulations for evaluating the flexural and shear capacities of FRP-strengthened RC beams, Struct. Concr. 17 (2016) 425–442. https://doi.org/10.1002/ suco.201500066. [37] Comité Européen de Normalisation (CEN), Eurocode 8. Design of structures for earthquake resistance. Part 3. Assessment and retrofitting of buildings, EN 1998-3, Brussels, 2005. [38] A.C.I. (ACI) ACI Committee 440, Guide for the design and construction of externally bonded FRP systems for strengthening concrete structures, ACI 440.2R, 2008. [39] E. Oller, R. Kotynia, A. Marí, Assessment of the existing models to evaluate the shear strength contribution of externally bonded frp shear reinforcements, Compos. Struct. 266 (2021). https://doi.org/10.1016/j.compstruct.2021.113641. [40] G. Monti, M. Liotta, Tests and design equations for FRP-strengthening in shear, Constr. Build. Mater. 21 (2007) 799–809. https://doi.org/10.1016/j. conbuildmat.2006.06.023. [41] A. Carolin, B. Täljsten, Theoretical study of strengthening for increased shear bearing capacity, J. Compos. Constr. 9 (2005) 488–496. https://doi. org/10.1061/(ASCE)1090-0268(2005)9:6(488). [42] J.F.F. Chen, J.G.G. Teng, Shear capacity of FRP-strengthened RC beams: FRP debonding, in: Constr. Build. Mater., 2003: pp. 27–41. https://doi. org/10.1016/S0950-0618(02)00091-0. [43] Japan Society of Civil Engineers, Recommendation for design and construction of concrete structures using continuous fibre reinforcing materials, Concrete E, Tokyo (Japan), 1997. [44] T.C. Rousakis, M.E. Saridaki, S.A. Mavrothalassitou, D. Hui, Utilization of hybrid approach towards advanced database of concrete beams strengthened in shear with FRPs, Compos. Part B Eng. 85 (2016) 315–335. https:// doi.org/10.1016/j.compositesb.2015.09.031. [45] R. Kotynia, Shear strengthening of RC beams with polymer composites, Lodz University of Technology, 2011. [46] A. Mofidi, O. Chaallal, Shear Strengthening of RC Beams with EB FRP: Influencing Factors and Conceptual Debonding Model, J. Compos. Constr. 15 (2011) 62–74. https://doi.org/10.1061/(ASCE)CC.1943-5614.0000153. [47] C. Pellegrino, C. Modena, Fiber-reinforced polymer shear strengthening of reinforced concrete beams: Experimental study and analytical modeling, ACI Struct. J. 103 (2006) 720–728. https://www.scopus.com/inward/record.url?eid=2-s2.0-33748587309&partnerID=40&md5=fdb67a21a2eb- 606f645b2bd1b5d1fd9e. [48] ACI Committee 440, ACI 440.2R-17, Guide for the Design and Construction of Externally Bonded FRP Systems for Strengthening Concrete Structures, Farmington Hills, Michigan, USA, 2017. [49] S. Jiang, W. Yao, J. Chen, S. Tao, Time dependent behavior of FRP-strength- ened RC beams subjected to preload: Experimental study and finite element modeling, Compos. Struct. 200 (2018) 599–613. https://doi. org/10.1016/j.compstruct.2018.05.110. [50] M. Moawad, M. Baena, C. Barris, L. Torres, H.E.M. Sallam, Time-depend- ent behavior of NSM strengthened RC beams under sustained loading, Eng. Struct. 247 (2021). https://doi.org/10.1016/j.engstruct.2021.113210. [51] A. Mari, E. Oller, J.M. Bairan, N. Duarte, A.R. Marí, E. Oller, J.M. Bairán, N. Duarte, Simplified method for the calculation of long-term deflections in FRP-strengthened reinforced concrete beams, in: Int. Symp. Fiber Reinf. Polym. Reinf. Concr. Struct., 2013: pp. 147–149. https://doi.org/10.1016/j. compositesb.2012.07.003. [52] Y.J. Kim, P.J. Heffernan, Fatigue Behavior of Externally Strengthened Concrete Beams with Fiber-Reinforced Polymers: State of the Art, J. Compos. Constr. 12 (2008) 246–256. https://doi.org/10.1061/(asce)1090- 0268(2008)12:3(246). [53] L. Bizindavyi, K.W. Neale, M.A. Erki, Experimental Investigation of Bonded Fiber Reinforced Polymer-Concrete Joints under Cyclic Loading, J. Compos. Constr. 7 (2003) 127–134. https://doi.org/10.1061/(asce)1090- 0268(2003)7:2(127). [54] C. Carloni, K. V. Subramaniam, M. Savoia, C. Mazzotti, Experimental determination of FRP-concrete cohesive interface properties under fatigue loading, Compos. Struct. 94 (2012) 1288–1296. https://doi.org/10.1016/j. compstruct.2011.10.026. [55] H. Budelmann, et al., Praxisgerechte Bemessungsansätze für das wirtschaftliche Verstärken von Betonbauteilen mit geklebter Bewehrung - Verbundtragfähigkeit unter dynamischer Belastung, DAfStb H. 593. (2013). [56] T. Leusmann, Das Verbundtragverhalten geklebter Kohlefaserkunststoffe auf Beton unter schwingender Beanspruchung Tho rste n Leusmann, Technische Universität Braunschweig., 2015. [57] J. Dai, Y. Saito, T. Ueda, Y. Sato, Static and fatigue bond characteristics of interfaces between CFRP sheets and frost damage experienced concrete, in: Am. Concr. Institute, ACI Spec. Publ., 2005: pp. 1515–1530. https:// doi.org/10.14359/14907. [58] E. Ferrier, D. Bigaud, P. Hamelin, L. Bizindavyi, K.W. Neale, Fatigue of CFRPs externally bonded to concrete, Mater. Struct. 38 (2005) 39–46. https://doi.org/10.1007/bf02480573. [59] B. M., Zum tragverhalten von betonbauteilen mit in schlitze eingeklebten CFK-lamellen, Munich TU, 2001. [60] E. Oller Ibars, D. Cobo Del Arco, A.R. Marí Bernat, Design proposal to avoid peeling failure in FRP-strengthened reinforced concrete beams, J. Compos. Constr. 13 (2009). https://doi.org/10.1061/(ASCE)CC.1943- 5614.0000038. [61] E. Oller, A.R. Marí, L. Bellido, Design method for flexural strengthening with fiber reinforced polymer (FRP) laminates avoiding its premature debonding, Inf. La Construcción. 65 (2013) 519–531. https://doi. org/10.3989/ic.12.087. 166 – Oller, E., De Diego, A., Torres, L., & Madera, P. (2023) Hormigón y Acero 74(299-300); 151-167 [62] M. Bilotta, A., Ceroni, F., Nigro, E. And Pecce, Design by testing procedure of debonding load for RC elements strengthened with EBR FRP materials, in: C. R. Sen, R. Seracino, C. Shield and W. Gold (eds), Tampa, Florida (Ed.), Proc. 10th FRPRCS Int. Symp. ACI SP-275 Fiber-Reinforced Polym. Reinf. Concr. Struct., 2011. [63] J.G. Teng, S.T. Smith, J. Yao, J.F. Chen, Intermediate crack-induced debonding in RC beams and slabs, Constr. Build. Mater. 17 (2003) 447–462. https://doi.org/10.1016/S0950-0618(03)00043-6. [64] X.Z. Lu, Studies of FRP-concrete interface, Tsinghua University, Beijing, China, 2004. [65] J.C. López González, Estudio de la redistribución tensional en la interfase FRP-Hormigón, Universidad Politécnica de Madrid, 2012. [66] R. Niedermeier, Envelope line of tensile forces while using externally bonded reinforcement., TU Münich, Munchen, 2000. [67] S. Matthys, Structural behaviour and design of concrete members strengthened with externally bonded FRP reinforcement, University of Ghent, Belgium, 2000. [68] W. Finckh, K. Zilch, Strengthening and Rehabilitation of Reinforced Concrete Slabs with Carbon-Fiber Reinforced Polymers Using a Refined Bond Model, Comput. Civ. Infrastruct. Eng. 27 (2012) 333–346. https://doi. org/10.1111/j.1467-8667.2011.00752.x. [69] Japan Society of Civil Engineers, Recommendations for upgrading of concrete structures with use of continuous fiber sheets, JSCE Concr. Eng. Ser. 41 (2001). [70] G. Zehetmaier, K. Zilch, Interaction between internal bars and externally FRP Reinforcement in RC Members, in: Proc. Sixth Int. Symp. FRP Reinf. Concr. Struct., Singapore, 2003: pp. 397–406. [71] M. Blaschko, Bond Behaviour of CFRP Strips Glued into Slits, in: Proc. Sixth Int. Symp. FRP Reinf. Concr. Struct., Singapore, 2003: pp. 205–214. *This document is available through the National members at CEN TC250/SC2 Oller, E., De Diego, A., Torres, L., & Madera, P. (2023) Hormigón y Acero 74(299-300); 151-167 – 167