Effects of protonation, hydroxylamination, and hydrazination of g-C3N4 on the performance of Matrimid®/g-C3N4 membranes
Abstract
Producción Científica
Full text
nanomaterials Article Effects of Protonation, Hydroxylamination, and Hydrazination of g-C3N4on the Performance of Matrimid®/g-C3N4Membranes María Soto-Herranz 1,*, Mercedes Sánchez-Báscones 1, Antonio Hérnandez-Giménez 2, JoséI. Calvo-Díez 2, Jesús Martín-Gil 3and Pablo Martín-Ramos 4,* 1Department of Agroforestry Sciences, ETSIIAA, University of Valladolid, Avenida de Madrid 44, 34004 Palencia, Spain; [email protected] 2SMAP, UA-UVa_CSIC, Associated Research Unit to CSIC, Universidad de Valladolid, Paseo Belén 7, 47011 Valladolid, Spain; [email protected] (A.H.-G.); [email protected] (J.I.C.-D.) 3Agriculture and Forestry Engineering Department, ETSIIAA, Universidad de Valladolid, Avenida de Madrid 44, 34004 Palencia, Spain; [email protected] 4Department of Agricultural and Environmental Sciences, Instituto Universitario de Investigación en Ciencias Ambientales (IUCA), EPS, Universidad de Zaragoza, Carretera de Cuarte s/n, 22071 Huesca, Spain *Correspondence: [email protected] (M.S.-H.); [email protected] (P.M.-R.); Tel.: +34-(974)-292668 (P.M.-R.) Received: 29 October 2018; Accepted: 4 December 2018; Published: 5 December 2018 Abstract: One of the challenges to continue improving polymeric membranes properties involves the development of novel chemically modified fillers, such as nitrogen-rich 2-D nanomaterials. Graphitic carbon nitride (g-C 3 N 4 ) has attracted significant interest as a new class of these fillers. Protonation is known to afford it desirable functionalities to form unique architectures for various applications. In the work presented herein, doping of Matrimid ® with protonated g-C 3 N 4 to yield Matrimid ® /g-C 3 N 4 mixed matrix membranes was found to improve gas separation by enhancing the selectivity for CO 2 /CH 4 by up to 36.9% at 0.5 wt % filler doping. With a view to further enhancing the contribution of g-C 3 N 4 to the performance of the composite membrane, oxygen plasma and hydrazine monohydrate treatments were also assayed as alternatives to protonation. Hydroxylamination by oxygen plasma treatment increased the selectivity for CO 2 /CH 4 by up to 52.2% (at 2 wt % doping) and that for O 2 /N 2 by up to 26.3% (at 0.5 wt % doping). Hydrazination led to lower enhancements in CO 2 /CH 4 separation, by up to 11.4%. This study suggests that chemically-modified g-C 3 N 4 may hold promise as an additive for modifying the surface of Matrimid®and other membranes. Keywords: carbon nitride; CO 2 /CH 4 ; gas separation; Matrimid ® 5218; mixed matrix membrane; O2/N2 1. Introduction CO 2 is significantly present in mixtures where CH 4 is the major and valuable component. Its removal from CH 4 mixtures is particularly important in processes such as biogas upgrading or natural gas sweetening. Conventional industrial methods used for such CO 2 removal include adsorption [ 1 ], and water scrubbing and absorption [ 2 ] processes. Nonetheless, separation processes mediated by membranes can generally offer advantages over aforementioned techniques in terms of low capital cost, ease of processing, small footprint area, high energy efficiency, and ease of preparation and control [3,4]. Another closely related burgeoning field is that of oxygen production from air separation, since it can be used in many environmental applications, such as in the combustion enhancement of natural Nanomaterials 2018,8, 1010; doi:10.3390/nano8121010 www.mdpi.com/journal/nanomaterials
Nanomaterials 2018,8, 1010 2 of 13 gas or in coal gasification [ 5 ]. Although cryogenic distillation and pressure swing adsorption are the mainstream technologies for oxygen-enriched air production, the use of membranes has been deemed as specially promising. Basu et al. [ 6 ] and Zhang et al. [ 7 ] published two reviews on membrane materials used for CO 2 /CH 4 separation. Among them, and apart from zeolite SAPO-34-based membranes [ 8 – 12 ], polyimides (PI) were claimed to exhibit the best combination of permeability and selectivity, thermal and chemical stability, and water resistance in biogas upgrading. In a similar fashion, glassy polyimides have also proven to exhibit excellent O2/N2selectivity [13]. The most popular commercially available PI, 3,3’-4,4’-benzophenone tetracarboxylic-dianhydride diaminophenylindane, better known as Matrimid ® 5218A, has been shown to combine a remarkable gas separation performance with other desirable features in terms of solubility, processability, thermal stability, chemical resistance, adhesion, film durability, and toughness. The state-of-the art based on this thermoplastic PI for gas separation applications has been recently covered in a thorough review by Castro-Muñoz et al. [ 14 ]. In terms of future trends to further enhance Matrimid’s properties, they insisted on the need to continue developing novel chemically modified fillers as a key challenge. Amongst two-dimensional nanomaterials that are being explored for the development of high-performance separation membranes, discussed in a recent review by Zhu et al. [ 15 ], graphitic carbon nitride (g-C 3 N 4 ) has attracted significant interest as a new class of filler. This mild bandgap metal-free organic semiconductor has remarkable applications as a catalyst for environmental pollution remediation [16,17]. Theoretical studies have preconized its suitability for H 2 or He purification from other gases [ 18 – 21 ], and several experimental works have shown that it can be successfully used in the fabrication of hybrid membranes with enhanced properties. For instance, Hou et al. [ 22 ] reported a zeolitic imidazolate framework-8 (ZIF-8) hybrid membrane doped with g-C 3 N 4 nanosheets for H 2 /CO 2 separation, with an excellent selectivity. g-C 3 N 4 nanosheets were also incorporated into the matrix of polymers of intrinsic microporosity (PIM-1) by Tian et al. [ 23 ], resulting in an increase in the selectivities for H 2 /CH 4 and H2/N2. As regards other membrane separation (non-gas) applications, Wang et al. [ 24 ] co-doped a polyamide (PA) forward osmosis membrane, based on a porous polyethersulfone substrate, with reduced graphene oxide and graphitic g-C 3 N 4 . By doing so, they obtained an osmotic water flux nearly 20% higher than that of the control membrane. Also in a PA nanofiltration membrane, modification with g-C 3 N 4 nanosheets was shown to improve the permeability, antifouling properties, hydrophilicity, negative charge density, roughness and thermal stability [ 25 ]. Similar conclusions were reached for reverse osmosis PA membranes doped with acidified g-C 3 N 4 by Gao et al. [ 26 ]. Doping g-C 3 N 4 into a sodium alginate matrix or into poly(vinyl alcohol) also improved the performance of hybrid membranes for water/ethanol separation [ 27 , 28 ]; and doping of g-C 3 N 4 co-impregnated with Cu + and Fe2+ ions into a Pebax®membrane improved gasoline desulfurization [29]. Nonetheless, to the best of the authors’ knowledge, there have been no reports on the utilization of g-C 3 N 4 as a filler for Matrimid ® mixed matrix membranes (MMMs). The work presented herein addresses this literature gap by assessing the effects of protonation of g-C 3 N 4 as well as its treatment with hydrazine monohydrate and with oxygen plasma on the performance of MMMs for CO 2 /CH 4 and O2/N2separation. 2. Materials and Methods 2.1. Materials Matrimid ® 5218 polymer (CAS no. 104983-64-4) was obtained from Huntsman Chemical, Advanced Materials Americas Inc. (Los Angeles, CA, USA). Melamine cyanurate (CAS no. 37640-57-6) was supplied by Ferro-plast S.r.l. (Vimodrone, Italy) with a purity superior to 99%. N-N-Dimethylacetamide (DMAc; CAS no. CAS: 127-19-5; ≥ 99%) and hydrazine monohydrate (CAS
Nanomaterials 2018,8, 1010 3 of 13 no. 7803-57-8; 98%) were purchased from Sigma-Aldrich (Munich, Germany). Reagents were used as received, without any further purification. 2.2. Methods 2.2.1. Synthesis of Graphitic Carbon Nitride (g-C3N4) Graphitic carbon nitride was prepared by a modification of the thermal oxidation method [ 30 ], using melamine cyanurate as a starting material for the polymerization/condensation reaction [ 31 ]. The reagent was placed in a Vycor ® glass vial and heated at 650 ◦ C for 4 h under aeration, with a cooling/heating ramp of 10 ◦ C · min −1 . The resulting yellow powder was transferred to an agate mortar and ground. Subsequently, the samples were exposed to ultrasonic treatment for approximately 2 h using a Branson (FisherScientific, Hampton, NH, USA) Sonifier 450. Samples were dried in an oven at 105 ◦C for 24 h to remove moisture. 2.2.2. Synthesis of Protonated g-C3N4 Due to the presence of abundant –C–N– bonds in the g-C 3 N 4 framework, it can be easily protonated by HCl, resulting in a modification of the surface charge, from a negatively to positively charged (Figure 1a) [ 32 ]. The process consisted in adding 2 g of pristine g-C 3 N 4 sample to a 12 mL diluted 3% solution of HCl and treating it with ultrasound for 2 h. Samples were not subsequently washed. They were placed in an oven at 105 ◦C for approximately 24 h and were then ground. Nanomaterials 2018, 8, x FOR PEER REVIEW 3 of 13 Dimethylacetamide (DMAc; CAS no. CAS: 127-19-5; ≥99%) and hydrazine monohydrate (CAS no. 7803-57-8; 98%) were purchased from Sigma-Aldrich (Munich, Germany). Reagents were used as received, without any further purification. 2.2. Methods 2.2.1. Synthesis of Graphitic Carbon Nitride (g-C3N4) Graphitic carbon nitride was prepared by a modification of the thermal oxidation method [30], using melamine cyanurate as a starting material for the polymerization/condensation reaction [31]. The reagent was placed in a Vycor® glass vial and heated at 650 °C for 4 h under aeration, with a cooling/heating ramp of 10 °C·min−1. The resulting yellow powder was transferred to an agate mortar and ground. Subsequently, the samples were exposed to ultrasonic treatment for approximately 2 h using a Branson (FisherScientific, Hampton, NH, USA) Sonifier 450. Samples were dried in an oven at 105 °C for 24 h to remove moisture. 2.2.2. Synthesis of Protonated g-C3N4 Due to the presence of abundant –C–N– bonds in the g-C3N4 framework, it can be easily protonated by HCl, resulting in a modification of the surface charge, from a negatively to positively charged (Figure 1a) [32]. The process consisted in adding 2 g of pristine g-C3N4 sample to a 12 mL diluted 3% solution of HCl and treating it with ultrasound for 2 h. Samples were not subsequently washed. They were placed in an oven at 105 °C for approximately 24 h and were then ground. Figure 1. Scheme of the synthesis of: (a) protonated g-C3N4; (b) oxygen plasm treatment used to introduce hydroxylamine structure (N-OH) on the surface of g-C3N4 (hydroxylaminated g-C3N4); and (c) hydrazinated g-C3N4. 2.2.3. Modifications of g-C3N4 with Oxygen Plasma and Hydrazine Monohydrate g-C3N4 is a laminar material with non-oxidized aromatic regions and aliphatic regions containing phenolic, carboxyl, and oxygen epoxide groups that make it hydrophilic in aqueous media. This behavior can be modified through treatment with oxygen plasma or with hydrazine monohydrate. In the former approach, interfacial forces are improved via plasma treatment, an ecologically benign process that does not produce liquid chemical residues. When the plasma is used with oxygen gas, it dissociates in order to generate oxygen-containing radicals [33], which incorporate –OH, as Figure 1. Scheme of the synthesis of: ( a ) protonated g-C 3 N 4 ; ( b ) oxygen plasm treatment used to introduce hydroxylamine structure (N-OH) on the surface of g-C 3 N 4 (hydroxylaminated g-C 3 N 4 ); and (c) hydrazinated g-C3N4. 2.2.3. Modifications of g-C3N4with Oxygen Plasma and Hydrazine Monohydrate g-C 3 N 4 is a laminar material with non-oxidized aromatic regions and aliphatic regions containing phenolic, carboxyl, and oxygen epoxide groups that make it hydrophilic in aqueous media. This behavior can be modified through treatment with oxygen plasma or with hydrazine monohydrate. In the former approach, interfacial forces are improved via plasma treatment, an ecologically benign process that does not produce liquid chemical residues. When the plasma is used with oxygen gas, it dissociates in order to generate oxygen-containing radicals [ 33 ], which incorporate –OH, as hydroxylamine groups, into the surface of g-C 3 N 4 , improving its dispersibility [ 34 ] (Figure 1b).
Nanomaterials 2018,8, 1010 4 of 13 The oxygen plasma treatment was conducted using a Harrick Plasma (Ithaca, NY, USA) PDC-002 apparatus. 150 mg of g-C 3 N 4 were placed on a Petri dish on a quartz sample holder within the plasma cavity. The operating power remained at 10.2 W, the chamber pressure was 300 Torr with an O 2 flow of 35 cm3·min−1, and the treatment time was 90 min. In the later approach, diazanyl group modified g-C 3 N 4 -NHNH 2 (Figure 1c) was obtained according to the procedure described by Chen et al. [ 35 ]: 1 g of as-synthesized g-C 3 N 4 was mixed with 20 mL water and 4 mL hydrazine hydrate, followed by stirring at 80 ◦C for 40 min. 2.2.4. Preparation of the Matrimid/g-C3N4Mixed Matrix Membranes The Matrimid/g-C 3 N 4 MMMs were prepared from a Matrimid commercial polymer solution doped with 0.5 wt % or 2 wt % g-C 3 N 4 loading in 5 mL of DMAc solvent at adequate concentration (6% w/v) to achieve a reasonable viscosity. Working at such g-C 3 N 4 loadings, previous work showed that measurable effects were obtained as compared with pristine Matrimid membranes, while much higher loadings led to an inhomogeneous distribution of g-C 3 N 4 across the membrane film, thus compromising the mechanical stability of the resulting membranes. After stirring until complete homogenization, all solutions were sonicated for 5 min at an amplitude of 60% in a sonicator with a work/rest period of 20 s and 10 s. Next, membranes were prepared by the casting method following the protocol described by Recio et al. [ 36 ], using a glass plate at 25 ◦ C. The resulting films were dried at 60 ◦ C for 24 h to complete the removal of the solvent and were then placed in a vacuum oven, where they remained at 120 ◦ C for 4 hours before raising the temperature to 180 ◦ C for another 4–6 h. Finally, the membranes were separated from the glass plates and their thickness was determined using a Fischer (Sindelfingen, Germany) Dualscope MP0R. All thicknesses were in the 40–60 µ m range. Three samples of each formulation were prepared, and at least two pieces of each membrane were tested. Their results were averaged, with a sample to sample variability in the usual range for laboratory prepared membranes (5–10%). 2.2.5. Characterization Methods Vibrational information of the dopant and the Matrimid/g-C 3 N 4 MMMs was retrieved by using a Thermo Scientific (Waltham, MA, USA) Nicolet iS50 Fourier-Transform Infrared (FTIR) spectrometer. 8–10 mm Ø samples were cut from the films and their transmittance was measured at room temperature in a scanning range between 410 and 4000 cm−1, with a 1 cm−1spectral resolution and 64 scans. The morphology of the as-prepared samples was examined using field emission scanning electron microscopy (FESEM), with a FEI (Hillsboro, OR, USA) QUANTA 200F device. Thermogravimetric analysis (TG) was used to determine the thermal and/or oxidative stability of the materials. TG experiments were performed with a Mettler Toledo (Columbus, OH, USA) DMA/SDTA 861 device, heating the samples from 50 ◦ C to 850 ◦ C at a heating rate of 10 ◦ C · min −1 , under a N2flow of 20 cm3·min−1. 2.2.6. Gas Separation Performance Measurement The pure gas permeation tests were performed on an isochoric (constant volume, variable pressure) permeation system to measure the permeability properties of the membranes. Five pure gas species (He, N 2 , O 2 , CH 4 , and CO 2 ) were applied as test gases, and the permeability and perm-selectivity of Matrimid/g-C 3 N 4 MMMs were evaluated. Experiments were carried out at 35 ◦ C using a constant feed pressure of 3 bar. To assure constant flow of each gas tested, desired pressure was maintained during 1 h and then flow measurements were taken by using a gas flow meter. The permeability of a given membrane was calculated from Equation (1) P= Q×L ∆P×A(1)
Nanomaterials 2018,8, 1010 5 of 13 where Pis the permeability in barrer (1 barrer = (10 −10 cm 3 (STP) × cm)/(cm 2× s × cmHg)), Qis the volumetric flow rate [cm 3 (STP)/s], Lis the membrane thickness [cm], ∆ Pis the pressure difference between two sides of the membrane [cmHg], and Ais the effective membrane area [cm 2 ]. The perm-selectivity αA/B is defined as the ratio of the permeability coefficients of two gases Aand B (PAand PB), according to Equation (2) αA/B= PA PB (2) 3. Results and Discussion 3.1. Vibrational Characterization 3.1.1. ATR-FTIR Spectra of the Modified g-C3N4Fillers The spectra of the protonated g-C 3 N 4 samples revealed similar characteristic features to those found in the as-prepared g-C 3 N 4 , thus confirming that the structural integrity of g-C 3 N 4 remained intact after protonation (Figure 2). Strong absorption bands could be observed in the 1200-1650 cm −1 range, arising from the skeletal stretching of C–N heterocycles and comprising both trigonal (N–(C)3) (full condensation) and bridging C–NH–C units (partial condensation) [ 37 ]. This would point at a successful development of an extended C–N–C network. The broad band ranging from 3000 to 3700 cm −1 was assigned to N–H and O–H stretching, due to the free amino groups and adsorbed hydroxyl species, respectively, whereas the sharp band at ca. 805 cm −1 was originated from the breathing vibration of tri-s-triazine units [38]. Nanomaterials 2018, 8, x FOR PEER REVIEW 5 of 13 where P is the permeability in barrer (1 barrer = (10−10 cm3 (STP) × cm)/(cm2 × s × cmHg)), Q is the volumetric flow rate [cm3 (STP)/s], L is the membrane thickness [cm], ΔP is the pressure difference between two sides of the membrane [cmHg], and A is the effective membrane area [cm2]. The permselectivity αA/B is defined as the ratio of the permeability coefficients of two gases A and B (PA and PB), according to Equation (2) 𝛼𝐴/𝐵 =𝑃𝐴 𝑃𝐵 (2) 3. Results and Discussion 3.1. Vibrational Characterization 3.1.1. ATR-FTIR Spectra of the Modified g-C3N4 Fillers The spectra of the protonated g-C3N4 samples revealed similar characteristic features to those found in the as-prepared g-C3N4, thus confirming that the structural integrity of g-C3N4 remained intact after protonation (Figure 2). Strong absorption bands could be observed in the 1200-1650 cm−1 range, arising from the skeletal stretching of C–N heterocycles and comprising both trigonal (N–(C)3) (full condensation) and bridging C–NH–C units (partial condensation) [37]. This would point at a successful development of an extended C–N–C network. The broad band ranging from 3000 to 3700 cm−1 was assigned to N–H and O–H stretching, due to the free amino groups and adsorbed hydroxyl species, respectively, whereas the sharp band at ca. 805 cm−1 was originated from the breathing vibration of tri-s-triazine units [38]. 3500 3000 1500 1000 500 1079 1010 1627 1533 1455 1395 1309 1200 800 d c b Transmittance (%) Wavenumber (cm-1) a O-H and N-H strecthing skeletal heterocycles C-N stretching 805 >3000 Figure 2. ATR-FTIR spectra of: (a) pristine g-C3N4, (b) protonated g-C3N4, (c) hydroxylaminated g- C3N4, and (d) hydrazinated g-C3N4. After oxygen plasma treatment, all the characteristic bands were retained (Figure 2), featuring bands at 800 cm−1 (assigned to the tri-s-triazine ring); and at 1200, 1309, 1395, 1455, 1533, and 1627 cm−1 (related to C–NH–C and N–(C) stretching modes). The peaks located at 1010 cm−1, 1079 cm−1, and above 3000 cm−1 corresponded to signals from N–OH groups. These results indicated that the oxygen plasma treatment led to the incorporation of N–OH on the surface of the C3N4. The treatment of g-C3N4 with hydrazine monohydrate (Figure 2) appeared to decrease the signal intensity of all peaks with respect to the original untreated g-C3N4 sample or to that treated with oxygen plasma. Figure 2. ATR-FTIR spectra of: ( a ) pristine g-C 3 N 4 , ( b ) protonated g-C 3 N 4 , ( c ) hydroxylaminated g-C3N4, and (d) hydrazinated g-C3N4. After oxygen plasma treatment, all the characteristic bands were retained (Figure 2), featuring bands at 800 cm −1 (assigned to the tri-s-triazine ring); and at 1200, 1309, 1395, 1455, 1533, and 1627 cm −1 (related to C–NH–C and N–(C) stretching modes). The peaks located at 1010 cm −1 , 1079 cm −1 , and above 3000 cm −1 corresponded to signals from N–OH groups. These results indicated that the oxygen plasma treatment led to the incorporation of N–OH on the surface of the C3N4. The treatment of g-C 3 N 4 with hydrazine monohydrate (Figure 2) appeared to decrease the signal intensity of all peaks with respect to the original untreated g-C 3 N 4 sample or to that treated with oxygen plasma.
Nanomaterials 2018,8, 1010 6 of 13 3.1.2. ATR-FTIR Spectra of Matrimid/g-C3N4MMMs A first comparison of the spectra of pure Matrimid and of the Matrimid MMMs doped with as-prepared or protonated g-C 3 N 4 (Figure 3) evidenced shifts in the bands at 819 cm −1 (shifted to 824 cm −1 ), 849 cm −1 (to 858 cm −1 ), 919 cm −1 (to 924 cm −1 ), 1475 cm −1 (to 1489 cm −1 ), and 1606 cm −1 (to 1618 cm −1 ). These shifts were sufficient to suggest an interaction between Matrimid and g-C 3 N 4 . As regards other strong bands in the doped samples, they were found at 708 cm −1 (v(CNC) out-of-plane bending); 1090 cm −1 (v(CNC) transversal stretching); 1364 cm −1 (v(CNC) axial stretching); 1510 cm −1 (v(C=C) aromatic stretching); 1663 cm −1 (v(C=O) benzophenone carbonyl stretching); 1715 cm −1 and 1784 cm −1 (v(C=O) symmetric and asymmetric stretching, respectively); 2861 and 2924 cm −1 (aliphatic C–H stretching); and 2958 cm−1(aromatic C–H stretching). Nanomaterials 2018, 8, x FOR PEER REVIEW 6 of 13 3.1.2. ATR-FTIR Spectra of Matrimid/g-C3N4 MMMs A first comparison of the spectra of pure Matrimid and of the Matrimid MMMs doped with asprepared or protonated g-C3N4 (Figure 3) evidenced shifts in the bands at 819 cm−1 (shifted to 824 cm−1), 849 cm−1 (to 858 cm−1), 919 cm−1 (to 924 cm−1), 1475 cm−1 (to 1489 cm−1), and 1606 cm−1 (to 1618 cm−1). These shifts were sufficient to suggest an interaction between Matrimid and g-C3N4. As regards other strong bands in the doped samples, they were found at 708 cm−1 (ѵ(CNC) out-of-plane bending); 1090 cm−1 (ѵ(CNC) transversal stretching); 1364 cm−1 (ѵ(CNC) axial stretching); 1510 cm−1 (ѵ(C=C) aromatic stretching); 1663 cm−1 (ѵ(C=O) benzophenone carbonyl stretching); 1715 cm−1 and 1784 cm−1 (ѵ(C=O) symmetric and asymmetric stretching, respectively); 2861 and 2924 cm−1 (aliphatic C–H stretching); and 2958 cm−1 (aromatic C–H stretching). 3000 2900 2000 1500 1000 500 1510 1475 849 e d c b Transmittance (%) Wavenumber (cm-1) a819 919 1606 708 1090 1364 1663 1715 1784 2861 2924 2958 Figure 3. ATR-FTIR spectra of (a) a pristine Matrimid matrix and of Matrimid MMMs doped at 2 wt % with different fillers: (b) as-prepared g-C3N4, (c) protonated g-C3N4, (d) oxygen plasma-treated g-C3N4, and (e) hydrazinated g-C3N4. Differences in the nature of the dopant, i.e., protonated vs. non-protonated g-C3N4, mainly affected the band at 1672 cm−1 (amide C=O stretching), which, after protonation, was shifted to 1663 cm−1. This finding is important because it suggests that the carbonyl groups in Matrimid can act as electron acceptors from –NH+ units from exfoliated protonated g-C3N4, resulting in a material assembled through electrostatic interactions (this matter will be discussed in detail in Subsection 3.4). In relation to the ATR-FTIR spectra of MMMs doped with oxygen plasma and hydrazine treated g-C3N4, also depicted in Figure 3, it is worth noting that no bands associated with the N–OH or –NHNH2 groups of g-C3N4 (which would result from those treatments) were observed. This may be due to low dopant doses, and would be in agreement with the findings of Chen et al. [35], who reported no remarkable differences between pristine g-C3N4 and g-C3N4-NHNH2. On the other hand, the band at 1606 cm−1, present in the pristine matrix, was found to disappear upon doping in both cases. 3.2. SEM Analysis SEM was used to study the MMMs cross-section morphology. The micrographs of the neat Matrimid membrane (not shown) featured a smooth surface without obvious imperfections, in good agreement with those reported, for instance, by Ebadi Amooghin et al. [39]. Representative micrographs of Matrimid/g-C3N4 MMMs with different g-C3N4 loadings and sonication times are shown in Figure 4a–c. At low loadings (0.5 wt %, Figure 4a,b) and sonication times (30 min), the g-C3N4 dopant was typically well dispersed. However, at higher loadings (e.g., 10 wt %, Figure 4c) and moderate sonication times (4 h), several large clusters of g-C3N4 could be found. Figure 3. ATR-FTIR spectra of ( a ) a pristine Matrimid matrix and of Matrimid MMMs doped at 2 wt % with different fillers: ( b ) as-prepared g-C 3 N 4 , ( c ) protonated g-C 3 N 4 , ( d ) oxygen plasma-treated g-C3N4, and (e) hydrazinated g-C3N4. Differences in the nature of the dopant, i.e., protonated vs. non-protonated g-C 3 N 4 , mainly affected the band at 1672 cm −1 (amide C=O stretching), which, after protonation, was shifted to 1663 cm −1 . This finding is important because it suggests that the carbonyl groups in Matrimid can act as electron acceptors from –NH + units from exfoliated protonated g-C 3 N 4 , resulting in a material assembled through electrostatic interactions (this matter will be discussed in detail in Section 3.4). In relation to the ATR-FTIR spectra of MMMs doped with oxygen plasma and hydrazine treated g-C 3 N 4 , also depicted in Figure 3, it is worth noting that no bands associated with the N–OH or –NHNH 2 groups of g-C 3 N 4 (which would result from those treatments) were observed. This may be due to low dopant doses, and would be in agreement with the findings of Chen et al. [ 35 ], who reported no remarkable differences between pristine g-C 3 N 4 and g-C 3 N 4 -NHNH 2 . On the other hand, the band at 1606 cm−1, present in the pristine matrix, was found to disappear upon doping in both cases. 3.2. SEM Analysis SEM was used to study the MMMs cross-section morphology. The micrographs of the neat Matrimid membrane (not shown) featured a smooth surface without obvious imperfections, in good agreement with those reported, for instance, by Ebadi Amooghin et al. [39]. Representative micrographs of Matrimid/g-C 3 N 4 MMMs with different g-C 3 N 4 loadings and sonication times are shown in Figure 4a–c. At low loadings (0.5 wt %, Figure 4a,b) and sonication times (30 min), the g-C 3 N 4 dopant was typically well dispersed. However, at higher loadings (e.g., 10 wt %,
Nanomaterials 2018,8, 1010 7 of 13 Figure 4c) and moderate sonication times (4 h), several large clusters of g-C 3 N 4 could be found. These clusters ranged in size from 20 to 50 nm. This would be in agreement with the findings of Tian et al. [ 23 ], who evaluated the improvement of gas separation performance of mixed matrix membranes composed of PIM-1 doped with different g-C 3 N 4 loads as compared to pure PIM-1 membranes. They found that, using CHCl 3 as a solvent and after sonication for 12 h, the g-C 3 N 4 dopant was well dispersed throughout the matrix at low loading levels (0.5–1 wt %), and also observed the presence of partial agglomeration for higher filler contents (>1 wt %). Nanomaterials 2018, 8, x FOR PEER REVIEW 7 of 13 These clusters ranged in size from 20 to 50 nm. This would be in agreement with the findings of Tian et al. [23], who evaluated the improvement of gas separation performance of mixed matrix membranes composed of PIM-1 doped with different g-C3N4 loads as compared to pure PIM-1 membranes. They found that, using CHCl3 as a solvent and after sonication for 12 h, the g-C3N4 dopant was well dispersed throughout the matrix at low loading levels (0.5–1 wt %), and also observed the presence of partial agglomeration for higher filler contents (>1 wt %). It is also worth noting that, in contrast with the neat Matrimid membrane, a scalloped morphology was observed for the MMMs doped with protonated g-C3N4 (Figure 4a,b). As noted by Venna et al. [40] (and references therein), it may be attributed to the formation of elongated polymer segments with increased plastic deformation of the polymer and can be regarded as an indication of a good interaction between the polymer and the filler, further supported by the absence of a sieve-in- a-cage morphology (i.e., when there are interfacial voids larger than the penetrating molecules, so a by-pass around the particles is produced, enhancing the permeability and reducing the apparent selectivity [41]) at each loading. SEM analysis was also conducted upon Matrimid doping with 0.5 wt % of g-C3N4 treated with oxygen plasma (Figure 4d,e) or with hydrazine monohydrate (Figure 4f). In the hydroxylaminated g- C3N4-doped samples, one could observe a crater-like pattern in which the eye of each crater was formed by nanosized fillers, similar to that obtained for protonated g-C3N4, albeit more evident. The filler also appeared to be uniformly distributed along the polymer matrix. According to Ebadi Amooghin et al. [39], such crater-like morphology of MMMs arises from an adequate compatibility existing between two phases, possibly due to the interfacial stress concentrations because of the polymer matrix/filler consecutive debonding. Thus, this deformation of the polymer matrix was again indicative of a strong interaction of polymer chains and filler. On the other hand, the MMMs doped with hydrazinolyzed g-C3N4 did not show a significant modification of the smooth aspect of pristine Matrimid, thus suggesting a weaker interaction. Figure 4. Cross-sectional SEM micrographs for MMMs doped with g-C3N4 subjected to different treatments and prepared with different sonication times: Matrimid membrane doped with 0.5 wt % protonated g-C3N4 at 3000× (a) and 6000× (b) magnification; Matrimid membrane doped with 10 wt % protonated g-C3N4 loading after 4 hours of sonication (c) at 3000×; Matrimid loaded with 0.5 wt % g- C3N4 treated with oxygen plasma at 3000× (d) and 10000× (e); Matrimid loaded with 0.5 wt % hydrazine monohydrate-treated g-C3N4 at 3000× (f). Micrographs of MMMs at 2 wt % loading were analogous to the ones at 0.5 wt %. Figure 4. Cross-sectional SEM micrographs for MMMs doped with g-C 3 N 4 subjected to different treatments and prepared with different sonication times: Matrimid membrane doped with 0.5 wt % protonated g-C 3 N 4 at 3000 × ( a ) and 6000 × ( b ) magnification; Matrimid membrane doped with 10 wt % protonated g-C 3 N 4 loading after 4 hours of sonication ( c ) at 3000 × ; Matrimid loaded with 0.5 wt % g-C 3 N 4 treated with oxygen plasma at 3000 × ( d ) and 10000 × ( e ); Matrimid loaded with 0.5 wt % hydrazine monohydrate-treated g-C 3 N 4 at 3000 × ( f ). Micrographs of MMMs at 2 wt % loading were analogous to the ones at 0.5 wt %. It is also worth noting that, in contrast with the neat Matrimid membrane, a scalloped morphology was observed for the MMMs doped with protonated g-C 3 N 4 (Figure 4a,b). As noted by Venna et al. [ 40 ] (and references therein), it may be attributed to the formation of elongated polymer segments with increased plastic deformation of the polymer and can be regarded as an indication of a good interaction between the polymer and the filler, further supported by the absence of a sieve-in-a-cage morphology (i.e., when there are interfacial voids larger than the penetrating molecules, so a by-pass around the particles is produced, enhancing the permeability and reducing the apparent selectivity [ 41 ]) at each loading. SEM analysis was also conducted upon Matrimid doping with 0.5 wt % of g-C 3 N 4 treated with oxygen plasma (Figure 4d,e) or with hydrazine monohydrate (Figure 4f). In the hydroxylaminated g-C 3 N 4 -doped samples, one could observe a crater-like pattern in which the eye of each crater was formed by nanosized fillers, similar to that obtained for protonated g-C 3 N 4 , albeit more evident. The filler also appeared to be uniformly distributed along the polymer matrix. According to Ebadi Amooghin et al. [ 39 ], such crater-like morphology of MMMs arises from an adequate compatibility existing between two phases, possibly due to the interfacial stress concentrations because of the polymer matrix/filler consecutive debonding. Thus, this deformation of the polymer matrix was again indicative of a strong interaction of polymer chains and filler. On the other hand, the MMMs doped
Nanomaterials 2018,8, 1010 8 of 13 with hydrazinolyzed g-C 3 N 4 did not show a significant modification of the smooth aspect of pristine Matrimid, thus suggesting a weaker interaction. 3.3. Studies on Thermal Stability of the Matrimid/g-C3N4Membranes The thermal stability of the Matrimid/g-C 3 N 4 membranes was evaluated in comparison to pristine Matrimid (Figure 5). The thermograms showed that all the studied membranes were stable up to 470 ◦ C and that only a small weight loss was observed between 200 ◦ C and 250 ◦ C (see Table 1), which could be attributed to residual solvent evaporation (the boiling point of DMAc is 202–204 ◦ C). The inflection point for this first stage occurred at 351 ◦ C for pristine Matrimid, and at lower temperatures for the MMMs membranes: 295 ◦ C for Matrimid loaded with protonated g-C 3 N 4 , 247 ◦ C for Matrimid doped with oxygen plasm-treated g-C 3 N 4 , and 287 ◦ C for Matrimid with hydrazine-treated g-C 3 N 4 . Above 450 ◦ C, a decomposition in two stages took place, with inflection points at around 517 ◦ C and 591 ◦ C (for pristine Matrimid they appeared at 518 ◦ C and 580 ◦ C, respectively). This second weight loss could be ascribed to the evolution of CO, CO 2 , and CH 4 from the cleavage of the benzene ring pattern of the Matrimid matrix. Degradation of the Matrimid/g-C 3 N 4 composites ended at 850 ◦ C after a brief carbonization process. Nanomaterials 2018, 8, x FOR PEER REVIEW 8 of 13 3.3. Studies on Thermal Stability of the Matrimid/g-C3N4 Membranes The thermal stability of the Matrimid/g-C3N4 membranes was evaluated in comparison to pristine Matrimid (Figure 5). The thermograms showed that all the studied membranes were stable up to 470 °C and that only a small weight loss was observed between 200 °C and 250 °C (see Table 1), which could be attributed to residual solvent evaporation (the boiling point of DMAc is 202–204 °C). The inflection point for this first stage occurred at 351 °C for pristine Matrimid, and at lower temperatures for the MMMs membranes: 295 °C for Matrimid loaded with protonated g-C3N4, 247 °C for Matrimid doped with oxygen plasm-treated g-C3N4, and 287 °C for Matrimid with hydrazinetreated g-C3N4. Above 450 °C, a decomposition in two stages took place, with inflection points at around 517 °C and 591 °C (for pristine Matrimid they appeared at 518 °C and 580 °C, respectively). This second weight loss could be ascribed to the evolution of CO, CO2, and CH4 from the cleavage of the benzene ring pattern of the Matrimid matrix. Degradation of the Matrimid/g-C3N4 composites ended at 850 °C after a brief carbonization process. 200 400 600 800 50 60 70 80 90 100 200 400 600 800 0 20 40 60 80 100 Weight (%) Temperature (ºC) Neat Matrimid Matrimid + protonated g-C3N4 Matrimid + O2 plasma g-C3N4 Matrimid + hydrazinated g-C3N4 -1.00E-03 -7.50E-04 -5.00E-04 -2.50E-04 0.00E+00 Derivative weight (%·ºC-1) Weight (%) Temperature (ºC) g-C3N4-0.003 -0.002 -0.001 0.000 Derivative weight (%·ºC-1) Figure 5. TG (solid line, y-axis on the left side of the graph) and DTG (dashed line, y-axis on the right side of the graph) curves for neat Matrimid and Matrimid-based membranes doped with 0.5 wt % of protonated g-C3N4, hydroxylaminated g-C3N4, and hydrazinated g-C3N4. The inset shows the TG/DTG curves for the untreated g-C3N4 filler. Table 1. TG curves features for neat Matrimid, the g-C3N4 filler and the three MMMs under study Pristine Matrimid g-C3N4 Protonated g-C3N4 Oxygen Plasma- Treated g-C3N4 Hydrazinated g-C3N4 Weight Loss (%) Midpoint (°C ) Weight Loss (%) Midpoint (°C ) Weight Loss (%) Midpoint (°C ) Weight Loss (%) Midpoint (°C ) Weight Loss (%) Midpoint (°C ) 2.8 287 97.6 700 4.2 29.4 2.70 284 2.2 280 23.4 516 23.3 518 24.8 518 25.9 517 14.9 609 15.9 611 17.0 611 17.1 611 Taking in account the delayed TG inflection points for MMMs vs. neat Matrimid at around 591 °C (588 °C for Matrimid/hydrazinated g-C3N4; 589 °C for Matrimid/hydroxylaminated g-C3N4 and 593 °C for Matrimid/protonated g-C3N4 vs. 580 °C for pristine Matrimid, as shown in Figure 5), it may be inferred that thermally stable structures were created in the membrane matrix after treatment with either g-C3N4(N–OH) or g-C3N4(N–H+). 3.4. CO2/CH4 and O2/N2 Gas Separation Performance of Matrimid/g-C3N4 MMMs Apropos of the pristine Matrimid membrane, the CO2/CH4 selectivity value was within the range reported in other recent works (34.2 [42], 34.9 [43], 35.7 [44], 36.3 [45]), and so was the O2/N2 selectivity (6.5–6.8 [42,46,47]). Doping of the Matrimid MMMs with protonated g-C3N particulates at 0.5 wt % increased the CO2/CH4 selectivity by 36.9% (from 36.3 to 49.6) as compared to the neat Matrimid membrane, Figure 5. TG (solid line, y-axis on the left side of the graph) and DTG (dashed line, y-axis on the right side of the graph) curves for neat Matrimid and Matrimid-based membranes doped with 0.5 wt % of protonated g-C 3 N 4 , hydroxylaminated g-C 3 N 4 , and hydrazinated g-C 3 N 4 . The inset shows the TG/DTG curves for the untreated g-C3N4filler. Table 1. TG curves features for neat Matrimid, the g-C3N4filler and the three MMMs under study Pristine Matrimid g-C3N4Protonated g-C3N4 Oxygen Plasma-Treated g-C3N4 Hydrazinated g-C3N4 Weight Loss (%) Midpoint (◦C) Weight Loss (%) Midpoint (◦C) Weight Loss (%) Midpoint (◦C) Weight Loss (%) Midpoint (◦C) Weight Loss (%) Midpoint (◦C) 2.8 287 97.6 700 4.2 29.4 2.70 284 2.2 280 23.4 516 23.3 518 24.8 518 25.9 517 14.9 609 15.9 611 17.0 611 17.1 611 Taking in account the delayed TG inflection points for MMMs vs. neat Matrimid at around 591 ◦ C (588 ◦ C for Matrimid/hydrazinated g-C 3 N 4 ; 589 ◦ C for Matrimid/hydroxylaminated g-C 3 N 4 and 593 ◦ C for Matrimid/protonated g-C 3 N 4 vs. 580 ◦ C for pristine Matrimid, as shown in Figure 5), it may be inferred that thermally stable structures were created in the membrane matrix after treatment with either g-C3N4(N–OH) or g-C3N4(N–H+).
Nanomaterials 2018,8, 1010 9 of 13 3.4. CO2/CH4and O2/N2Gas Separation Performance of Matrimid/g-C3N4MMMs Apropos of the pristine Matrimid membrane, the CO 2 /CH 4 selectivity value was within the range reported in other recent works (34.2 [ 42 ], 34.9 [ 43 ], 35.7 [ 44 ], 36.3 [ 45 ]), and so was the O 2 /N 2 selectivity (6.5–6.8 [42,46,47]). Doping of the Matrimid MMMs with protonated g-C 3 N particulates at 0.5 wt % increased the CO 2 /CH 4 selectivity by 36.9% (from 36.3 to 49.6) as compared to the neat Matrimid membrane, although the O 2 /N 2 selectivity decreased by 5.7% (from 7.0 to 6.6). Doping at 2 wt % led to a lower increase in the CO 2 /CH 4 selectivity (by 16.5%, from 36.3 to 42.2), but the O 2 /N 2 selectivity was preserved (Table 2). Table 2. Permeabilities/selectivities of the Matrimid/g-C 3 N 4 MMMs for He, N 2 , O 2 , CH 4 , CO 2 , O 2 /N 2 , and CO 2 /CH 4 as a function of different filler treatments at different doping levels (0.5 wt % and 2 wt %) MMM Permeability (Barrer) Selectivity Ref. He N2O2CH4CO2O2/N2CO2/CH4 Matrimid (control) 22.00 0.27 1.90 0.24 8.70 7.0 36.3 [48] Matrimid/protonated g-C3N40.5 wt % 23.53 0.26 1.70 0.15 7.69 6.6 49.6 This study Matrimid/protonated g-C3N42 wt % 20.17 0.20 1.44 0.15 6.45 7.1 42.2 This study Matrimid/hydroxylaminated g-C 3 N 4 0.5 wt % 24.12 0.19 1.71 0.21 7.86 8.9 37.9 This study Matrimid/hydroxylaminated g-C3N42 wt % 23.63 0.23 1.69 0.13 7.15 7.2 55.2 This study Matrimid/hydrazinated g-C3N40.5 wt % 20.60 0.20 1.44 0.17 6.56 7.1 39.0 This study Matrimid/hydrazinated g-C3N42 wt % 18.65 0.20 1.36 0.15 6.19 6.8 40.4 This study The behavior for the MMMs doped with oxygen plasma-treated g-C 3 N 4 treatment as a function of the filler doping values was the opposite: doping at 2 wt % led to a larger increase in the CO 2 /CH 4 selectivity (by 52.2%, from 36.3 to 55.2) than doping at 0.5 wt % (4.4% increase). On the other hand, doping at 0.5 wt % led to a significant enhancement of O 2 /N 2 selectivity (26.3% increase, from 7.0 to 8.9), while the increase for 2 wt % doping was only 2.7%. In relation to the hydrazine treatment, it enhanced CO 2 /CH 4 selectivities (by 7.5% and by 11.4% for 0.5 wt % and 2 wt % doping, respectively), while O 2 /N 2 separation values remained similar to those of the Matrimid matrix (0.7% and −3.7% variation). The results in the two latter treatments would be in agreement with observations by other authors, such as Tian et al. [ 23 ], who synthesized MMMs with a PIM matrix doped with g-C 3 N 4 , and an increase in the permeability values was observed as the filler concentration was increased to reach >1 wt %. The enhancement of gas separation in the Matrimid membranes after doping with modified g-C 3 N 4 may be referred either to an increase of hydrogen bonding in the Matrimid/g-C 3 N 4 composite structure or to cross-linking modifications in Matrimid mediated by g-C3N4. The first hypothesis suggests that the good results obtained for Matrimid MMMs doped with protonated g-C 3 N 4 would be referred to, on the one hand, their exfoliated nature and the associated surface gain for interaction, and, on the other hand, to the presence of –NH + groups capable of bonding, through hydrogen bonding, with the carbonyl groups of the Matrimid matrix. The benzene rings of both g-C3N4and Matrimid would lend themselves to the formation of “π-staking” (Figure 6a). In the case of g-C 3 N 4 treated with oxygen plasma, designed to provide hydroxylamine N–OH groups that would bond with the carbonyl groups of Matrimid, it is unclear whether interactions between filler and matrix would be mediated by subsequent hydrogen bonding between such groups. There is also the possibility of formation of charge transfer between the –OH (behaving as electron acceptor group) and the aromatic nucleus in Matrimid (behaving as an electron donor group), as depicted in Figure 6b.