Bioengineered dynamic systems based on elastin-like recombinamers
Abstract
Departamento de Bioquímica y Biología Molecular y Fisiología
Full text
PROGRAMA DE DOCTORADO EN INVESTIGACION BIOMEDICA TESIS DOCTORAL BIOENGINEERED DYNAMIC SYSTEMS BASED ON ELASTIN-LIKE RECOMBINAMERS Presentada por Tatjana Flora para optar al grado de Doctora por la Universidad de Valladolid Dirigida por: Prof. Jose Carlos Rodriguez-Cabello
INDEX
Abstract ....................................................................................... 15 Objectives .................................................................................... 22 Resumen ...................................................................................... 27 1. INTRODUCTION .................................................................. 34 1.1. Biomaterials for tissue engineering .................................... 34 1.2. Elastin as a biomaterial ...................................................... 36 1.3. Elastin-like Recombinamers (ELRs) .................................. 38 1.4. ELR-based hydrogels and their application in tissue engineering 41 1.5. Vascularization in tissue engineering constructs ................ 43 1.6. Biofounctionalization of surfaces with ELRs for biomedical application ............................................................................... 46 2. MATERIALS AND METHODS ........................................... 53 2.1. Materials ........................................................................... 53 2.1.1. Reagents ...................................................................... 53 2.1.2. Other materials............................................................. 55 2.1.3. Cell lines ...................................................................... 56 2.1.4. Animal models ............................................................. 56 2.1.5. Elastin-like recombinamers (ELRs) .............................. 56 2.2. Methods ............................................................................ 57 2.2.1. Synthesis of ELRs ........................................................ 57 2.2.2. Physicochemical characterization of the ELRs ............ 58 2.2.2.1. Polyacrilamide gel electrphoresis (SDS-PAGE) ..... 59 2.2.2.2. Mass spectroscopy (MALDI-TOF) ........................ 60 2.2.2.3. Aminoacid analysis (HPLC) .................................. 60
2.2.2.4. Differential scanning calorimetry (DSC) ................ 60 2.2.2.5. Nuclear magnetic resonance spectroscopy (1H-NMR)61 2.2.2.6.Fourier transform infrared spectroscopy (FTIR) ...... 62 2.2.3. Contact angle ............................................................ 63 2.2.4. X-ray photoelectron spectroscopy (XPS) .................. 63 2.2.5. Quartz crystal microbalance with dissipation (QCM-D)63 2.2.6. Atomic force microscopy (AFM) .............................. 64 2.2.7. Laser ablation ........................................................... 65 2.2.8. Scanning electrom microscopy (SEM) ...................... 65 2.2.9. Chemical modification of the ELRs .............................. 65 2.2.10. Porosity studies .......................................................... 66 2.2.11. Mechanical characterization of ELR-based hydrogels by rheological measurements ...................................................... 66 2.2.12. In vitro studies ............................................................ 67 2.2.13. In vivo studies ............................................................ 67 2.2.13.1. Intramuscularly injection of ELR-based hydrogels .. 68 2.2.13.2. Subcutaneous implantation of ELR-based hydrogels 68 2.2.14. Histological and immunohistochemistry analysis ........ 68 2.2.15. Statistical analysis ...................................................... 70 3. References ............................................................................ 71 CHAPTER 1: SPATIAL CONTROL AND CELL ADHESION SELECTIVITY ON MODEL GOLD SURFACES GRAFTED WITH ELASTIN-LIKE RECOMBINAMERS Abstract ........................................................................................ 78 1. INTRODUCTION .................................................................... 79 2. MATERIALS AND METHODS .............................................. 85
2.1. Materials ........................................................................... 85 2.1.1 Gold surfaces ................................................................ 85 2.1.2 Elastin-like recombinamers ........................................... 85 2.1.3. Cell culture .................................................................. 87 2.2. Methods ............................................................................ 87 2.2.1 Surface celaning / activation ......................................... 87 2.2.2 Surface functionalization .............................................. 87 2.2.3. Contact angle ............................................................... 88 2.2.4 X-ray photoelectron spectroscopy (XPS) ...................... 88 2.2.5 Scanning electron microscopy (SEM) ........................... 89 2.2.6 Atomic force microscopy (AFM) .................................. 89 2.2.7 Quartz crystal microbalance with dissipation (QCM-D) 90 2.2.8 Laser ablation ............................................................... 92 2.2.9 In vitro cellular studies ................................................. 92 2.2.10 Statistical analysis....................................................... 93 3. RESULTS ................................................................................ 94 3.1. Contact angle..................................................................... 94 3.2. X-ray photoelectron spectroscopy (XPS) ........................... 95 3.3. Scanning electron microscopy (SEM) ................................ 97 3.4. Atomic force microscopy (AFM) ....................................... 99 3.5. Quartz crystal microbalance with dissipation (QCM-D) ... 100 3.6. Selective cell adhesion on ELR-bio functionalized model gold surfaces ................................................................................. 106 3.7. Spatial control of endothelial cell behaviour .................... 109 4. DISCUSSION ........................................................................ 111
5. CONCLUSIONS .................................................................... 114 6. ACKNOWLEDGMENTS ...................................................... 115 7. REFERENCES ....................................................................... 116 8. SUPPORTING INFORMATION ........................................... 121 CHAPTER 2: TETHERING QK PEPTIDE TO ENHANCE ANGIOGENESIS IN ELASTIN-LIKE RECOMBINAMER (ELR) HYDROGELS Abstract ...................................................................................... 132 1. INTRODUCTION .................................................................. 134 2. MATERIALS AND METHODS ............................................ 140 2.1. ELR bio-production, modification and characterization ... 140 2.2. QK peptide and recombinant human VEGF165 ................. 140 2.3. Mechanical and morphological properties of ELR-based hydrogels ............................................................................................... 141 2.4. Cell cultures....................................................................... 14 2.5 In vitro 3D proliferation test and histological analysis ....... 143 2.6. Ethical approval ............................................................... 143 2.7. In vivo studies .................................................................. 144 2.8. Histological analysis of in vivo studies ............................. 144 2.9. Immunohistochemistry .................................................... 145 2.10. Statistical analysis .......................................................... 145 3. RESULTS .............................................................................. 146 3.1. Morphological and rheological properties ........................ 146 3.2. In vitro 3D cell proliferation assay ................................... 148 3.3. In vivo behaviour of QK peptide ...................................... 153 4. DISCUSSION ........................................................................ 157
5. CONCLUSIONS .................................................................... 162 5. ACKNOWLEDGEMENTS .................................................... 162 6. REFERENCES ...................................................................... 163 7. SUPPORTING INFORMATION ........................................... 167 CHAPTER 3: USE OF PROTEOLYTIC SEQUENCES WITH DIFFERENT CLEAVAGE KINETICS AS A WAY TO GENERATE HYDROGELS WITH PREPROGRAMED CELL INFILTRATION PATTERNS IMPARTED OVER THEIR GIVEN 3D SPATIAL STRUCTURE Abstract ..................................................................................... 173 1. INTRODUCTION ................................................................. 174 2. MATERIALS AND METHODS ............................................ 180 2.1. Synthesis of GTRA-ELR and DRIR-ELR ........................ 180 2.2. Expression and characterization of GTAR-ELR and DRIR-ELR 181 2.3. In vitro analysis of the degradation rate using a recombinant human uPA enzyme ........................................................................... 182 2.4. Hydrogel formation and its chemical-physical characterization182 2.5. Porosity of proteolytic ELR-based hydrogel .................... 183 2.6. Mechanical properties of proteolytic ELR-based hydrogels184 2.7. Morphological characterization via scanning electron microscopy (SEM) .................................................................................... 184 2.8. In vitro degradation analysis of proteolytic ELR-based hydrogels ............................................................................................... 184 2.9. Cytocompatibility evaluation in a 2D cell culture ............ 185 2.10. In vivo studies of each proteolytic ELR-based hydrogels 186 2.11. Histology and immunohistochemistry analysis .............. 186 2.12. Preparation of the 3D structured system ......................... 188 2.11. In vivo studies of the 3D structured system ................... 188
2.13. Statistical analysis .......................................................... 189 3. RESULTS .............................................................................. 190 3.1. Construction, production and purification of proteolytic ELRs 190 3.2. In vitro enzymatic degradation of proteolytic ELRs ......... 191 3.3. Morphology studies of proteolytic ELR-based hydrogels . 192 3.4. Mechanical properties of proteolytic hydrogels ................ 195 3.5. Degradation rate of the proteolytic ELR-based hydrogels evaluated by analysing the mechanical properties ................................... 197 3.6. Cytocompatibility ............................................................ 199 3.7. Individual in vivo behaviour of proteolytic ELR-based hydrogels ............................................................................................... 200 3.8. In vivo studies of sandwiched three-layer system ............. 206 4. DISCUSSION ........................................................................ 212 5. CONCLUSION ...................................................................... 217 6. ACKNOWLEDGEMENTS .................................................... 217 7. REFERENCES ....................................................................... 218 8. SUPPORTING INFORMATION ........................................... 223 3. CONCLUSIONS .................................................................. 23539 4. APPENDIX .............................................................................. 235 Abbreviations ............................................................................. 237 Table of standard amino acid abbreviations ................................ 238 Publications ................................................................................ 239 Congresses and conferences ....................................................... 240 Other contributions ..................................................................... 242
ABSTRACT 18 observed a well-defined distribution of HUVEC and HFF1 cells namely a selective spatial control over HUVEC adhesion. These findings suggest an innovative approach for biosensors generation e/o scaffolds that require spatial and temporal organization of cells. Following, the second study of this thesis consists on the enhancement of angiogenic activity of ELR-based hydrogels when tethered chemically a small VEGF mimetic peptide called QK. In addition to cell adhesion sequences (RGD and REDV), an ELR used in this work present a proteolytic site (VGVAPG) that belong to elastase enzyme. The angiogenic acticity of these hydrogels were studied in vitro demonstrating that it does not alter the mechanical and morphological properties of the ELRs but the biological activity such as cell adhesion and proliferation. When injected in vivo an improved microvasculature formation was observed that facilitate perfusion and connection with the surrounding tissue. These results showed that ELR-QK-based hydrogels are optimal engineered constructs with a potential angiogenic activity that could be employed in tissue engineering and regenerative medicine for treatment of cardiovascular diseases. The third study of this thesis aims to control in time and space cell infiltration and biodegradation in a three dimensional (3D)-structured system. The ELRs employed in this work, in addition to a universal cell
ABSTRACT 19 adhesion sequence (RGD), contain proteolytic target sites that degrade in response to urokinase plasminogen activator (uPA) with different degradation rate (fast and slow). Exploiting these features, in this study a 3D system was developed which consist in a three-layer disk hydrogel with an internal layer that contains the rapid degrading component and the external layers that contain the slow-degrading ELR. Those disks have been implanted subcutaneously in mice and its evolution was followed over time. As a result of the design and the programmed cell infiltration sequence, the internal layer was colonized firstly following an inside-to- outside pattern. These results demonstrated that the 3D-ELR based system could be applied as a tissue substitute for biomedical application that require a controlled regeneration and vascularization over time. In summary, the studies showed in this thesis provides new insights regarding ELR-based hydrogels to be used in tissue engineering and regenerative medicine. Specifically, it describes the importance of the inclusion of several epitopes into the backbone of the ELR such as for example universal and specific adhesion sequences that influence cell behaviour. Furthermore, the presence of a VEGF mimetic peptide called QK enhance the angiogenic properties of ELR-based hydrogels and on the other hand, ELRs with a controlled degradation rate could be implicated
ABSTRACT 20 in the construction of complex biological structures that require specific time to regenerate.
ABSTRACT 21 OBJECTIVES
22 Objectives o The main objective of this thesis is the development of multifunctional systems based on ELRs for their subsequent application in tissue engineering and regenerative medicine. For that we aim to take advantage of their features such as the possibility to tailor them at the genetic level allowing the inclusion of specific epitopes that lead to an efficient and faster cell responses promoting a better regeneration. o The aim of the first study is to develop a 2D system for biomedical application such as cell-based biosensors or diagnostic devices. This approach consists on using model gold surfaces functionalized with ELRs codifying into their backbone complementary bioactivities as RGD and REDV sequences. The purpose is to obtain a simple system for cell selectivity and spatially controlled cell adhesion onto the surfaces exploiting the synergy between two bioactivities. o The objective of the second study is to enhance vascularization in ELR-based hydrogels tethering chemically the so-called QK peptide. The presence of cell adhesiveness motifs into their peptide chain (RGD and REDV) increase cell recruitment into the construct and the inclusion of a VGVAPG sequence, sensitive to
23 proteases, favors its biodegradation which is an important prerequisite for the scaffolds implied in tissue engineering. o Lastly, the aim of the third study is to design and obtain advanced functional structures with a preprogrammed cell-infiltration and biodegradation pattern. These are 3D systems composed of two ELRs with differences in peptide cleavage kinetic and coupling cell adhesiveness bioactivity. Theoretically this 3D system should invert conventional cell infiltration patterns conducting cell invasion.
25 RESUMEN
RESUMEN 27 Resumen La ingeniería tisular y la medicina regenerativa son campos interdisciplinares que tienen como objetivo desarrollar sustitutos biológicos que restauren, mantengan o mejoren la función de un tejido o de un órgano perdida por lesión o enfermedad. Los biomateriales utilizados en aplicaciones biomédicas persiguen alcanzar características esenciales que promuevan la nueva morfogénesis tisular creando un entorno favorable para el crecimiento celular, así como las propiedades físicas y químicas adecuadas requeridas para un tejido determinado. En décadas pasadas, se han encontrado varios obstáculos para seleccionar biomateriales funcionales que imiten la matriz extracelular natural (MEC). Por ejemplo, algunos de los polímeros sintéticos a menudo son biocompatibles, pero carecen de interacción con las células y el crecimiento del tejido, lo que ha llevado a la necesidad de modificar muchos de estos materiales con secuencias y factores bioactivos. A la inversa, los polímeros naturales derivados de proteínas de la matriz extracelular ofrecen la ventaja de la señalización biológica, pero pueden ser antigénicas y sus propiedades físicas son más difíciles de modular que en los polímeros sintéticos. La biodegradación es una característica crucial en los implantes biomédicos y su modulación ha sido ampliamente estudiada. Presentar un tiempo de degradación sincronizado con la
INTRODUCTION 34 1. Introduction 1.1 Biomaterials for tissue engineering Nowadays, there is a significant demand for advanced biomaterials able to replace or regenerate the biological functions of the tissues or organs that have been damaged through diseases or trauma. [1] The definition of the ideal biomaterial has changed considerably during the past 50 years and, in fact, it changes depending on the area of application. [2] The basic role of a biomaterial in tissue regeneration is to provide support and scaffolding for cell growth namely there must be a combination of cells, biological matrices, signals and biophysical cues mimicking in this way the extracellular matrix (ECM). [3][4][5] Biomaterials used in tissue engineering are divided into three groups such as bioceramics materials, polymer-based materials and protein-based materials. In most cases, bioceramic materials (alumina, zirconia, bioactive glasses, calcium phosphates, and glass-ceramics) have been used for hard tissue regeneration due to their low elasticity but they are characterized by optimal mechanical stiffness and biocompatibility. However, their clinical applications for tissue engineering has been limited because of their brittleness, difficulty of shaping for implantation and difficulties to control their degradation rate. [6]
INTRODUCTION 35 Polymer-based materials have been developed both from natural and synthetic resources. Regarding synthetic polymers such as polystyrene, poly-l-lactic acid (PLLA), polyglycolic acid (PGA) and poly-dl-lactic-co- glycolic acid (PLGA) are attractive biomaterials for tissue engineering scaffold applications as they can be fabricated with a tailored architecture. However, these polymers are hydrophobic which can be disadvantageous in tissue engineering application due to poor wetting and lack of cellular attachment and interaction. [7][8][9] Natural materials such as silk and chitosan or polymers extracted from other biological systems or compounds of the native ECM (collagen, elastin and glycosaminoglycans) have been recognized as an attractive choice for tissue engineering application. Natural materials are biocompatible and mechanical and biological properties consistent with in vivo features but the limitations are short supply, expensive, batch-to-batch variation, and are susceptible to cross-contamination. [10] A number of groups have attempted to combine ceramics with polymerbased scaffolds while others have combined synthetic polymers with natural polymers in order to enhance their biological capacity. While composite scaffolds such as these have shown some promise, each consists of at least one phase which is not found naturally in the body and they all have associated problems with biocompatibility, biodegradability or both.
INTRODUCTION 36 [11][12] Protein-based materials have excellent advantages such as control over their structure, high biocompatibility and ease of functionalization making them optimal candidates for biomedical application. Extensive studies, over the last two decades, have elucidated precise structure–function relationships for many proteins; an excellent example of this is elastin, a protein that provide elasticity to a variety of tissues. 1.2 Elastin as a biomaterial In recent years, elastin based-materials are increasly investigated as promising advanced biomaterials for their use in the field of tissue engineering. This interest is fuelled by the remarkable properties of this structural protein, such as elasticity, self-assembly, long-term stability, and biological activity. [13][14] Elastin is an extracellular matrix (ECM) protein that provide elasticity to connective tissues or organs, especially where elasticity and resilience is of major importance as for example in blood vessels, elastic ligaments, in lung and skin. Tropoelastin is the main precursor of elastin and is amongst the most elastic of all known natural proteins, with an ability to stretch eight times its resting molecular length and recoil without damage to the protein. In humans, there is only one tropoelastin gene and its expression occurs before birth and in the first few years of life when the cells of elastic
INTRODUCTION 37 tissues produce the elastin required for the body to develop. The elastin formation process consists in the association of many tropoelastin molecules that are subsequently cross-linked or connected. [15][16] In the event of damage to the elastin such as injury, burns, sun damage or, simply as a result of aging due to the low level of elastin production in adult aging, the damage cannot be efficiently repaired and the skin gradually loses its elasticity. Researchers have for many years pursued elastin-based materials which may be useful in the repair or regeneration of elastic tissues. Such materials have evolved from fragments of elastin isolated from animal tissue through to synthetic proteins which mimic the elastic nature of tropoelastin. Elastin can be applied as a biomaterial in various forms such as insoluble elastin fibres, hydrolysed soluble elastin, recombinant tropoelastin (fragments), repeats of synthetic peptide sequences and as block copolymers of elastin, possibly in combination with other (bio) polymers. [17] There are different forms of elastin applied as biomaterials such as elastin in autografts, allografts and xenografts; decellularized tissue and hydrolysed elastin. Recent improvements in recombinant DNA technology allows to design and manufacture materials that lead to the production of repeated elastin-like sequences reaching complex
INTRODUCTION 38 composition. However, this method is the most efficacious as is characterized by several advantages compared to the techniques mentioned above. [18] There are other biomaterials combined with elastin such as silk elastin-like recombinamers (SELRs) that include repetition of silk domain. They have been deeply studied as scaffolds for tissue engineering as well as for the generation of nanoparticle system for application in drug delivery. [19] 1.3. Elastin-like recombinamers (ELRs) Elastin-like recombinamers (ELRs) are one of the most widely studied protein-derived materials. The more conventional terminology elastinlike polymers (ELPs), which include those first chemically synthesized materials, was replaced by elastin-like recombinamers (ELRs) due to their recombinant nature. [20] ELRs are based on the repetitive of the most common pentapeptide (VPGXG) n, where X stands for any amino acid except proline, and n is the number of repetitions. [21] One particular property of the ELRs is their thermally responsiveness namely are characterized by a transition temperature (Tt). They undergo a reversible phase transition from a soluble to an insoluble state upon increasing or lowering the temperature above a specific threshold. Below a given “critical” temperature, the polymer chains remain relatively
INTRODUCTION 39 extended and hydrated mainly by hydrophobic hydration and thus are soluble in aqueous solution. This hydration around its hydrophobic moiety is characterized by the existence of ordered caged-like, clathrate water structures surrounding the moieties of the polymer and stabilized by hydrogen bonding among them. When the temperature increase, the polymer chain hydrophobically folds and aggregates to other polymer chains by formation of intra- and inter-chain hydrophobic contacts. In this state, the polymer adopts a dynamic, regular, non-random structure, called β-spiral, formed by concatenation of adjacent type II β-turns and stabilized by intra-spiral, inter-turn and inter-spiral hydrophobic contacts. This is the product of the ITT in which the folded and associated state is maintained by loss of the ordered water structures of hydrophobic hydration. The Tt of the ELRs could be extensively manipulated by the amino acid at the Xaa position and resulted in a dependency on e.g. temperature, pH, and electrochemical potential. [22][23] Using protein engineering, many different parameters of elastin-like recombinamers can be controlled: including amino acid sequence, peptide length, namely the length and number of the blocks. The possibility to incorporate specific sequences that have cell biological effects lead to the obtainment of biomaterials with advanced functionalities (stimulating characteristics of ECM) in a simple way which
INTRODUCTION 40 can be used for specific applications such as enhancement interaction with the cells like adhesion, proliferation, migration and differentiation. [24] For example, the fusion of the tripeptide Arginine-Glycine-Aspartic (RGD), present in fibronectin and in other extracellular matrix proteins, would enhance cell adhesion to ELRs in multiple cell types, preferably via integrins of the type α5β1 and α5β3. [25] Another example is REDV sequence, (arginine–glutamic acid–aspartic acid–valine), which is a specific adhesive sequence for endothelial cells found in the alternativelyspliced IIICS-5 domain of human plasma fibronectin. This motif mediates cell adhesion and spreading via α4β1 integrin in endothelial cells, but not in smooth muscle cells or fibroblasts.[26] Similarly, the inclusion of enzymatic degradation sequences, such as those recognized by elastase, which contain the L-Valine-Glycine-L-Valine-L- Alanine-L-Proline-Glycine hexapeptide (VGVAPG) would improve the biodegradability of ELRs, which should happen in parallel to the therapeutic process, such as, for example, tissue regeneration.[21] New biomaterials that provide a combination of protease sensitiveness as well as bioactive epitopes, are of particular interests in tissue repair process. Material degradation rate needs to fit the envisioned application allowing the desired ingrowth of host cells and ECM deposition. [27] ELRs are slowly degraded in vivo, and their rate of degradation could be tuned, as it
INTRODUCTION 41 has already find out, by the explicit incorporation of specific protease recognition sites within their amino acidic sequence. In particular, ELRs with specific proteolytic sites that belong to metalloproteasis (MMP) or to plasminogen activator system have been produced with an important feature regarding their degradation rate. Lastly, ELRs for more specific applications have been produced namely growth factors have been fused, such as bone-2 morphogenetic protein ("bone morphogenetic protein-2", BMP-2), which has demonstrated its capacity to promote the regeneration of damaged bone tissue, thus conferring osteoinductive properties to ELRs. [28] 1.4. ELR-based hydrogels and their application in tissue engineering The first ELP-based hydrogels were described by Urry et al., a poly- VPGVG ELP, which was chemically crosslinked using γ-radiation to provide a stable matrix. Eleven tests, including mutagenicity, cytotoxicity, antigenicity, sensitization, pyrogenicity and haemolysis, amongst others, were performed to prove the biocompatibility of this family of hydrogels. [29] Since then, numerous other crosslinking methods have been reported for the formation of physical or chemical gels which differs for the forces that maintain the structure. Thus, physical hydrogels, are stabilized by weak forces such as molecular entanglements, H-bonding hydrophobic interactions or coulomb forces. Chemical crosslinking produces hydrogels
INTRODUCTION 42 with enhanced mechanical properties and, although different options are available to chemically crosslink ELRs, almost all of them involve the amino group of the lateral chain of lysine residues. Amongst the crosslinking options, the use of chemicals is the most extended option. [30] Recently, G. de Torre et al., have developed a rapid, tuneable, biocompatible and cell-friendly crosslinking system based on a 1, 3- dipolar cycloaddition reaction, a clear example of “click chemistry”. [31] [32]‘‘Click chemistry’’ was introduced by Kolb et al. in 2001, and specifically the Huisgen 1,3-dipolar cycloadition of azides and alkynes, has been shown to be stereospecific, easy to perform in aqueous solution under mild conditions and provides high reaction yields. They are stable within biological systems, and have limited side product formation. As a result of these advantages, this reaction has been widely employed in drug discovery, bioconjugation with proteins and DNA, cell surface labelling and surface modifications with ELRs, among other molecules. As an improvement to conventional ‘‘click chemistry’’, the use of activated alkyne groups, such as cyclooctyne derivatives, has allowed these reactions to be carried out without the need of a catalyst. This reaction requires the presence of azides and alkynes, which react orthogonally to form an irreversible covalent bond. [33][34][35] This rapid and biocompatible approach allows the homogeneous
INTRODUCTION 43 encapsulation of different cell types and has proved its cytocompatibility with several cell lines and in different applications. ELR-based hydrogels have proved to be an excellent platform for cell growth and proliferation for their application in wound healing, cartilage repair, liver tissue engineering, cardiovascular applications or ocular tissue engineering. [36] These “tunable” hydrogels have proven to be extremely useful in biomedical and pharmaceutical applications due to their high water content and rubbery nature, which is similar to that of natural tissue. The structural complexity of ELRs with specific mechanical, chemical, and biological properties allows us to design specific features that make them useful for a wide variety of applications, including skin substitutes, vascular grafts, heart valves, and elastic cartilage. [37][38] 1.5 Vascularization in tissue engineering constructs In past decades a variety of biomaterials have been deeply studied to generate engineered templates for consequent application in tissue engineering but they still present a big challenge as for example vascularization before their employement in clinical application. [39] The formation of a mature vascular network in a construct supply an adequate oxygen and nutrient diffusion ensuring a successful integration into host tissue with consequent regeneration of a mature functional tissue. Primarily, one of the most important feature of the biological constructs,
MATERIALS AND METHODS 50 MATERIALS AND METHODS
MATERIALS AND METHODS 51 2. Materials and Methods 2.1 Materials The reagents used in this thesis are reported in Table 1. Table 1. Reagents used in this thesis. Reactive and abbreviation Brand Chloridric acid Fisher Scientific Ethylenediaminetetraacetic acid (EDTA) Sigma-Aldrich Acrylamide/Bis-acrylamide Amresco AEBSF Apollo Scientific Agar BD Agarose Seakem Cambrex Ultrapure water (MilliQ) Millipore Antifoam 204 Sigma-Aldrich Ampicillin Apollo Scientific Bromophenol Blue Sigma-Aldrich Copper cloride Sigma-Aldrich Sodium chloride (NaCl) Fisher Scientific Dimethyl sulfoxide (DMSO) Sigma-Aldrich Sodium dodecyl sulfate (SDS) Sigma-Aldrich E-64 Apollo Scientific
MATERIALS AND METHODS 52 Restriction enzymes (SapI, EarI, EcoRI, DpnI) y other enzymes (T4 DNA ligasa, FastAP, SAP) Thermo Scientific Ethanol Panreac Phenyl methyl sulfonyl fluoride (PMSF) Apollo Scientific Gentamicin/Amphotericin Gibco Glicerol Fisher Scientific Glycine Sigma-Aldrich Glucose Panreac Hematoxylin-eosin Sigma-Aldrich Sodium hydroxide (NaOH) Fisher Scientific Plasmid purification Kit “NucleoSpin Plasmid” Macherey-Nagel DNA extraction kit in agarose gels “PureLink Quick Gel Extraction” Invitrogen Leupeptine Apollo Scientific DNA marker 1kb Plus Ladder Invitrogen Protein marker “Pierce Unstained” Thermo Scientific Auto-induction culture medium “Terrific” (TB) Formedium Bacterial Culture medium (Luria Bertani, LB) Conda Cell culture medium (DMEM 1g/L glucosa, Medium 200) Gibco
MATERIALS AND METHODS 53 Paraffin Sigma-Aldrich Paraformaaldehyde Sigma-Aldrich Penicillin/Streptomycin Gibco Pepstatin A Apollo Scientific Ammonium persulfate Sigma-Aldrich Bovine serum albumin (FBS) Gibco Ammonium sulphate Fisher Scientific Growth supplement with low serum (LSGS) Gibco Phosfate buffered saline (PBS) Gibco Tetramethylethylenediamine (TEMED) Sigma-Aldrich DNA staining “SimplySafe” Eurx Trypsin/EDTA 0.05% Gibco Tris (hydroxymethyl) aminomethane (Tris) Sigma-Aldrich Triton X-100 Sigma-Aldrich Trypan blue Invitrogen Xylol Sigma-Aldrich β-Mercaptoethanol Sigma-Aldrich 2.1.1 Other Materials All disposable plastic material (pipette tips, pipettes, centrifuge tubes, microcentrifuge tubes, etc.) were washed and rinsed several times with
MATERIALS AND METHODS 54 distilled water and sterilized on an autoclave (Selecta Autotester E-75, 20 min 120 °C 1 atmosphere). The glassware (beakers, flasks, pipettes, etc.) was suitably washed and sterilized in the same way. 2.1.2 Cell lines • Human foreskin fibroblasts (HFF1, ATCC® SCRC-1041™). Cells between 6 and 14 passages were used. • Human endothelial primary cells of the umbilical cord vein (HUVECs, ATCC CRL-1730). Passages between 2 and 6 were used. 2.1.3 Animal model • Swiss C57 mice (male) provided by the University of Valladolid animal facility. 2.1.4 Elastin like recombinamers (ELRs) The amino acid sequence of the ELRs employed in this thesis are reported in Table 2. Table 2. ELRs used in this work, obtained in the laboratories of G.I.R. BIOFORGE of the University of Valladolid. ELR Amino acid sequences MW (kDa) CC-RGD CC((VPGIG)2(VPGKG)(VPGIG)2EEQIGHIPRGDDYHLYP (VPGIG)2(VPGKG)(VPGIG)2(VGVAPG)3)10 39 CCC-REDV CCC((VPGIG)2(VPGKG)(VPGIG)2EEQIGHIPREDVDYHLYP(VP GIG)2(VPGKG)(VPGIG)2)10 59
MATERIALS AND METHODS 55 CCC-EI CCC[(VPGVG)2VPGEG(VPGVG)2]10(VGIPG)60V 47 HRGD MGSSHHHHHHSSGLVPRGSHMESLLP-{[(VPGIG)2-(VPGKG)- (VPGIG)2]2-AVTGRGDSPASS-[(VPGIG)2-(VPGKG)- (VPGIG)2]2}6V 61 REDV MESLLP{(VPGIG)2VPGKG(VPGIG)2EEIQIGHIPREDVDYHLYP (VPGIG)2VPGKG(VPGIG)2(VGVAPG)3}10 80 GTAR MESLLPV (((VPGIG)2 VPGKG (VPGIG)2)2YAVTG GTAR SASPASSA ((VPGIG)2 VPGKG (VPGIG)2)2V)4 41 DRIR MESLLPV (((VPGIG)2 VPGKG (VPGIG)2)2YAVTG DRIR SASPASSA ((VPGIG)2 VPGKG (VPGIG)2)2V)4 41 VKV MESLLPV VPGVG [VPGKG(VPGVG)5]23 VPGKG VPGVG VPGVG VPGVG VPGVG 60 2.2. Methods 2.2.1 Synthesis of the ELRs All the genes encoding the ELRs used in this work were obtained by genetic engineering techniques described in literature. [56] The GTARELR and DRIR-ELR have been synthetized esclusively for the development of this thesis. Briefly, the genes encoding the monomer peptides of the ELRs or the bioactive sequences were synthesized by NZYTech Company, Portugal. They were subsequently cloned in the plasmid pDriveAll, which had been mutated deleting the endogenous restriction site for SapI and adapting the poly-linker of pDm to the seamless iterative-recursive to obtain multimers. [24] The restriction
MATERIALS AND METHODS 56 enzymes used for cloning are EarI and SapI as they have endonuclease activity on a contiguous sequence to the recognition. Once the final gene construct is obtained, it is extracted from the cloning plasmid and a subcloning is carried out in the expression plasmid pET7RARE, resulting from different modifications on the commercial vector pET-25b (+). Afterwards, this plasmid is used to transform expression strains of E.Coli, in particular BL21 Star (DE3) strain (Novagen), which are cultured in a 15 L bioreactor (Applikon Biotechnology) under controlled conditions of pH, temperature, agitation and O2 concentration. Lastely, after the mechanical breakdown of the cell wall and the bacterial membrane by disruption (model TS 0.75KW, Constant Systems), the recombinamers are purified taking advantage of their thermosensitive characteristic through successive cooling and heating cycles which is called, "Inverse Transition Cycling", ITC, followed by centrifugation at each step. Thus, finally, a pure product is obtained that is dialysed against MQ water and subsequently lyophilized (FreeZone 1, LABCONCO) for a better preservation of the product. 2.2.2 Physicochemical characterization of the ELRS 2.2.2.1 Sodium Dodecyl Sulphate - PolyAcrylamide Gel Electrophoresis (SDS PAGE Electrophoresis)
MATERIALS AND METHODS 57 Polyacrylamide gel electrophoresis with SDS is a technique used to separate molecules basing on their molecular weight (Mw). The SDS molecules are negatively charged able to bind to proteins providing a uniform charge-to-mass ratio. By binding to proteins, the detergent destroys to secondary, tertiary and/or quaternary structure denaturating them and turning them into negatively charged linear polypeptide chains. In this work, the vertical electrophoresis system "MiniVE" of Hoefer (Amersham Pharmacia Biotec) was used. The resulting polyacrylamide gels were stained with copper chloride or commassie brilliant blue. Copper staining is a negative stain, which does not stain the proteins, but the copper interacts electrostatically with the SDS that contains the gel itself, leaving the areas that contain unstained proteins, being observed, therefore, as dark bands. On the other hand, the Coomassie dye binds to proteins through ionic interactions between sulfonic acid groups and positive protein amine groups through Van der Waals attractions. The images of the gels in both cases were taken with the Gel Logic 100 Imaging System (Eastman Kodak) and analyzed with the Kodak 1D Image Analysis program (Eastman Kodak). 2.2.2.2 Matrix-assisted laser desorption/ionization-Time-of-flight (MALDI TOF)
MATERIALS AND METHODS 58 Mass spectrometry of the type "Matrix-assisted laser desorption / ionization-Time-of-flight" (MALDI-TOF) allows to know exactly the Mw, so it can be considered complementary to the SDS-PAGE technique. This technique has been carried out in the Laboratory of Instrumental Techniques (LTI) of the University of Valladolid (UVa) in the MALDITOF Voyager STR (Applied Biosystems). 2.2.2.3 High-Performance Liquid Chromatography (HPLC) The analysis of ELR samples previously hydrolyzed by "High- Performance Liquid Chromatography" (HPLC) allows to know the amino acid composition of the ELRs. This method was carried out in the LTI of the UVa with the Waters 600 gradient HPLC equipment coupled to a Waters 2487 UV detector (Waters). 2.2.2.4 Differential scanning calorimetry (DSC) Differential scanning calorimetry (DSC) is a thermoanalytical technique, where sample and reference are subjected to the same temperature program and the amount of heat needed to fulfill such program is monitored and compared to that of the reference. In our case, this technique was accomplished to study the inverse transition temperature of ELRs when temperature changes were applied. For this work, Mettler Toledo 822e equipment was used with refrigeration using
MATERIALS AND METHODS 59 liquid nitrogen. Samples were dissolved in PBS at a concentration of 50 mg /mL. Afterwards, 20µL was loaded into a standard aluminium pan and sealed hermetically. As reference, 20µL of the solvent, in this case PBS, was placed in another pan. Both temperature and enthalpy were calibrated using a standard sample of indium. The experiments consisted of a first isothermal stage at 0 ° C for 5 minutes, followed by a heating step, from 0 to 60 ° C, at a rate of 5 ° C / min. 2.2.2.5 Nuclear magnetic resonance (1H-NMR) Nuclear magnetic resonance spectroscopy (1H-NMR) studies the behavior of certain atomic nuclei (those with non-zero nuclear spin) in the presence of an external magnetic field. The applied magnetic field produces a split of the degenerated energy levels of the nuclear spin, so that transitions between them can be induced because of absorption of the adequate electromagnetic radiation. The arrangement of energy levels is a property of both the nuclei of a molecule and their electronic environment and interactions between them. Thus, the intensity, shape and position of the signals in the spectrum of a given nucleus are closely related to their molecule structure, and the whole NMR spectrum of a molecule can be considered as a fingerprint of it. In this work, NMR analysis was performed routinely with each batch of recombinamer to verify the purity of the material. The equipment used was NMR 500 (Agilent
MATERIALS AND METHODS 66 ELRs were dissolved in PBS at a concentration of 50 mg/mL and subsequently were mixed in an eppendorf with a final volume of 30 μL. Animals were anesthetized by inalation of isofluorano at 3%. A 20G syringe was used to inject the hydrogels intramuscularly in a hind limb zone. After each time point the animals were euthanized by cervical dislocation. All the procedures were carried out under sterile conditions in rooms with positive pressure and equipped with laminar flow hoods. 2.2.13.2 Subcutaneous implantation of ELR-based hydrogels Subcutaneous implantation was made performing a small incision on the dorsal area forming a skin pocket using surgical scissors. Afterwards, the wound was closed using absorbable sutures. Animals were anesthetized using ketamine and diazepam at a concentration of 100mg/mL and 5mg/ml, respectively. Different time points were analysed and after each time point the samples were analysed by histology and immunohistochemistry. 2.2.14 Histological and immunohistochemistry analysis Once extracted the samples, they were fixed with paraformaldehyde at 4% for at least 24 hours at 4°C. Subsequently, a dehydratation by immersion in ethanol solutions of increasing concentration was performed ending with a final step in xylol. Finally, all the samples were included in paraffin
MATERIALS AND METHODS 67 for about six hours and were cut with a thickness of 6 µm using a rotatory microtome. Each slide was rehydrated by immersion in xylene and subsequently in decreasing concentrations of ethanol and finally in distilled water. Hematoxylin-eosin staining was carried out following methods described in the literature. [58] The images of the cuts were obtained with a light-field optical microscope (Nikon Eclipse 80i) equipped with a color camera (Nikon Digital Sight DS-Fi1). Immunofluorescence staining were performed on micro-sections, previously deparaffinised and subsequently incubated for 1 hour in 10% donkey blocking serum. After several washing steps in PBS 1X, all the samples were incubated O/N at 4°C with a donkey polyclonal primary PECAM antibody at a concentration of 1µg/mL in 1% with the blocking serum. Subsequently, samples were washed three times with PBS 1X for five minutes each and incubated for 2 hours with goat anti-mouse fluorescein-conjugated secondary antibodies at a concentration of 1 µg/mL with 1.5% normal blocking serum.A vectashield HardSet Antifade Mounting Medium with DAPI (Vector Laboratories, USA) was used to stain the nuclei of the cells. All images were acquired with a fluorescent microscope.
MATERIALS AND METHODS 68 2.2.15 Statistical analysis The data presented in this thesis is presented as the mean ± standard deviation. The statistical analysis was carried out using a one-way variance analysis with the post-hoc Holm-Sidak test. A p-value less than 0.05 has been considered significant. The significant differences are shown as follows: (*) p <0.05; (**) p <0.01; (***) p <0.001; p> 0.05 indicates absence of significant differences ("no significant differences", n.s.d).
MATERIALS AND METHODS 69 3. References [1] Khan, Ferdous, and Masaru Tanaka. "Designing smart biomaterials for tissue engineering." International journal of molecular sciences 19.1 (2018): 17. [2] Huebsch, Nathaniel, and David J. Mooney. "Inspiration and application in the evolution of biomaterials." Nature 462.7272 (2009): 426. [3] O'brien, Fergal J. "Biomaterials & scaffolds for tissue engineering." Materials today 14.3 (2011): 88-95. [4] Rahmati, Maryam, et al. "Biomaterials for Regenerative Medicine: Historical Perspectives and Current Trends." Cell Biology and Translational Medicine, Volume 4. Springer, Cham, 2018. 1-19. [5] Reis, Rui L., et al. Natural-based polymers for biomedical applications. Elsevier, 2008. [6] Hardy, John G., Jae Y. Lee, and Christine E. Schmidt. "Biomimetic conducting polymer-based tissue scaffolds." Current opinion in biotechnology 24.5 (2013): 847-854. [7] Cheung, Hoi-Yan, et al. "A critical review on polymer-based bio-engineered materials for scaffold development." Composites Part B: Engineering 38.3 (2007): 291-300. [8] Stevens, Molly M. "Biomaterials for bone tissue engineering." Materials today 11.5 (2008): 18-25. [9] Ma, Peter X. "Biomimetic materials for tissue engineering." Advanced drug delivery reviews 60.2 (2008): 184-198. [10] Stratton, Scott, et al. "Bioactive polymeric scaffolds for tissue engineering." Bioactive materials 1.2 (2016): 93-108. [11] Gloria, Antonio, Roberto De Santis, and Luigi Ambrosio. "Polymer-based composite scaffolds for tissue engineering." Journal of Applied Biomaterials and Biomechanics 8.2 (2010): 57-67. [12] Almine, Jessica F., et al. "Elastin-based materials." Chemical Society Reviews 39.9 (2010): 3371-3379. [13] Wise, Steven G., Suzanne M. Mithieux, and Anthony S. Weiss. "Engineered tropoelastin and elastin-based biomaterials." Advances in protein chemistry and structural biology. Vol. 78. Academic Press, 2009. 1-24. [14] Vrhovski, Bernadette, and Anthony S. Weiss. "Biochemistry of tropoelastin." European Journal of Biochemistry 258.1 (1998): 1-18. [15] Wise, Steven G., and Anthony S. Weiss. "Tropoelastin." The international journal of biochemistry & cell biology 41.3 (2009): 494-497. [16] Daamen, Wilhelmina Francisca, et al. "Elastin as a biomaterial for tissue engineering." Biomaterials 28.30 (2007): 4378-4398. [17] Gregory, Kenton W. "Elastin and elastin-based materials." U.S. Patent No. 6,110,212. 29 Aug. 2000.
MATERIALS AND METHODS 70 [18] Rodríguez-Cabello, José Carlos, et al. "Elastin-like polypeptides in drug delivery." Advanced drug delivery reviews 97 (2016): 85-100. [19] Rodríguez-Cabello, J. Carlos, et al. "“Recombinamers” as advanced materials for the post-oil age." Polymer 50.22 (2009): 5159-5169. [20] Nettles, Dana L., Ashutosh Chilkoti, and Lori A. Setton. "Applications of elastinlike polypeptides in tissue engineering." Advanced drug delivery reviews 62.15 (2010): 1479-1485. [21] Meyer, Dan E., and Ashutosh Chilkoti. "Quantification of the effects of chain length and concentration on the thermal behavior of elastin-like polypeptides." Biomacromolecules 5.3 (2004): 846-851. [22] Ribeiro, Artur, et al. "Influence of the amino-acid sequence on the inverse temperature transition of elastin-like polymers." Biophysical journal 97.1 (2009): 312-320. [23] Girotti, Alessandra, et al. "Elastin‐like recombinamers: Biosynthetic strategies and biotechnological applications." Biotechnology journal 6.10 (2011): 1174- 1186. [24] Ruoslahti, Erkki. "RGD and other recognition sequences for integrins." Annual review of cell and developmental biology 12.1 (1996): 697-715. [25] Humphries, Martin J. "Peptide recognition motifs involved in the binding of integrins to their ligands." Kidney international 41.3 (1992): 645-649. [26] Tan, Huaping, and Kacey G. Marra. "Injectable, biodegradable hydrogels for tissue engineering applications." Materials 3.3 (2010): 1746-1767. [27] Coletta, Dante J., et al. "Bone regeneration mediated by a bioactive and biodegradable extracellular matrix-like hydrogel based on elastin-like recombinamers." Tissue Engineering Part A 23.23-24 (2017): 1361-1371. [28] Urry, Dan W., et al. "Biocompatibility of the bioelastic materials, poly (GVGVP) and its γ-irradiation cross-linked matrix: summary of generic biological test results." Journal of Bioactive and Compatible Polymers 6.3 (1991): 263-282. [29] Sallach, Rory E., et al. "Elastin-mimetic protein polymers capable of physical and chemical crosslinking." Biomaterials 30.3 (2009): 409-422. [30] Testera, Ana M., et al. "Biocompatible elastin-like click gels: design, synthesis and characterization." Journal of Materials Science: Materials in Medicine 26.2 (2015): 105. [31] de Torre, Israel González, et al. "Random and oriented electrospun fibers based on a multicomponent, in situ clickable elastin-like recombinamer system for dermal tissue engineering." Acta biomaterialia 72 (2018): 137-149. [32] Huisgen, Rolf. "1, 3‐dipolar cycloadditions. Past and future." Angewandte Chemie International Edition in English 2.10 (1963): 565-598. [33] Baskin, Jeremy M., et al. "Copper-free click chemistry for dynamic in vivo imaging." Proceedings of the National Academy of Sciences 104.43 (2007): 16793-16797.
MATERIALS AND METHODS 71 [34] Wenge, Ulrike, Thomas Ehrenschwender, and Hans-Achim Wagenknecht. "Synthesis of 2′-O-propargyl nucleoside triphosphates for enzymatic oligonucleotide preparation and “click” modification of DNA with nile red as fluorescent probe." Bioconjugate chemistry 24.3 (2013): 301-304. [35] Rodríguez-Cabello, J. Carlos, et al. "Bioactive scaffolds based on elastin-like materials for wound healing." Advanced drug delivery reviews 129 (2018): 118- 133. [36] de Torre, Israel González, et al. "Elastin-like recombinamer-covered stents: Towards a fully biocompatible and non-thrombogenic device for cardiovascular diseases." Acta biomaterialia 12 (2015): 146-155. [37] Mahara, Atsushi, Kristi L. Kiick, and Tetsuji Yamaoka. "In vivo guided vascular regeneration with a non‐porous elastin‐like polypeptide hydrogel tubular scaffold." Journal of Biomedical Materials Research Part A 105.6 (2017): 1746- 1755. [38] Brey, Eric M., ed. Vascularization: regenerative medicine and tissue engineering. CRC Press, 2014. [39] Rouwkema, Jeroen, Nicolas C. Rivron, and Clemens A. van Blitterswijk. "Vascularization in tissue engineering." Trends in biotechnology 26.8 (2008): 434-441. [40] Serbo, Janna V., and Sharon Gerecht. "Vascular tissue engineering: biodegradable scaffold platforms to promote angiogenesis." Stem cell research & therapy 4.1 (2013): 8. [41] Mitchell, Geraldine M., and Wayne A. Morrison. "In vitro and in vivo approaches for pre-vascularization of 3-dimensional engineered tissues." Vascularization for Tissue Engineering and Regenerative Medicine (2017): 1-27. [42] Laschke, Matthias W., and Michael D. Menger. "Prevascularization in tissue engineering: current concepts and future directions." Biotechnology advances 34.2 (2016): 112-121. [43] Lovett, Michael, et al. "Vascularization strategies for tissue engineering." Tissue Engineering Part B: Reviews 15.3 (2009): 353-370. [44] West, Jennifer L., and James J. Moon. "Vascularization of engineered tissues: approaches to promote angiogenesis in biomaterials." Current topics in medicinal chemistry 8.4 (2008): 300-310. [45] Kim, Joseph J., Luqia Hou, and Ngan F. Huang. "Vascularization of threedimensional engineered tissues for regenerative medicine applications." Acta biomaterialia 41 (2016): 17-26. [46] Balani, Kantesh, Roger Narayan, and Arvind Agarwal. "Surface engineering and modification for biomedical applications." Biosurfaces: A Materials Science and Engineering Perspective (2015): 201. [47] Tampieri, Anna, and Simone Sprio, eds. Bio-Inspired Regenerative Medicine: Materials, Processes, and Clinical Applications. CRC Press, 2016. [48] Nyanhongo, Gibson Stephen, Walter Steiner, and Georg M. Gübitz, eds. Biofunctionalization of Polymers and their Applications. Vol. 125. Springer
MATERIALS AND METHODS 72 Science & Business Media, 2011. [49] Frey, Wolfgang, Dan E. Meyer, and Ashutosh Chilkoti. "Thermodynamically reversible addressing of a stimuli responsive fusion protein onto a patterned surface template." Langmuir 19.5 (2003): 1641-1653. [50] Costa, Rui R., et al. "Stimuli‐responsive thin coatings using elastin‐like polymers for biomedical applications." Advanced Functional Materials 19.20 (2009): 3210-3218. [51] Ekerdt, Barbara L., Rachel A. Segalman, and David V. Schaffer. "Spatial organization of cell‐adhesive ligands for advanced cell culture." Biotechnology journal 8.12 (2013): 1411-1423. [52] Li, Linying, et al. "Creating cellular patterns using genetically engineered, gold- and cell-binding polypeptides." Biointerphases11.2 (2016): 021009. [53] García-Arévalo, Carmen, et al. "A comparative study of cell behavior on different energetic and bioactive polymeric surfaces made from elastin-like recombinamers." Soft Matter 8.11 (2012): 3239-3249. [54] Rodríguez-Cabello, J. Carlos, et al. "Emerging applications of multifunctional elastin-like recombinamers." Nanomedicine 6.1 (2011): 111-122.
CHAPTER 1 73 CHAPTER 1 SPATIAL CONTROL AND CELL ADHESION SELECTIVITY ON MODEL GOLD SURFACES GRAFTED WITH ELASTIN-LIKE RECOMBINAMERS Tatjana Flora, 1 Israel González de Torre, 2 Luis Quintanilla, 1 Matilde Alonso, 1 José Carlos Rodríguez-Cabello1 1BIOFORGE, CIBER-BBN, University of Valladolid, Spain 2Technical Proteinn Nanotechnology (TPNBT S.L), Valladolid, Spain Flora, T., de Torre, I. G., Quintanilla, L., Alonso, M., & Rodríguez-Cabello, J. C. (2018). Spatial control and cell adhesion selectivity on model gold surfaces grafted with elastin-like recombinamers. European Polymer Journal, 106, 19-29.
CHAPTER 1 74 Abstract A simple system for cell selectivity and spatially controlled cell adhesion has been developed using model gold surfaces grafted with a combination of two ELRs containing into their backbone cell-adhesion domains such as RGD and REDV. Grafting onto gold was achieved via redox reaction through thiol groups present in amino terminal cysteine tails of the ELRs. The correlation among contact angle, SEM micrographs, AFM, XPS and QCMD have been carried out. After in-depth adhesion studies, a mixture of 75% ELR-REDV and 25% ELR-RGD was found to exhibit high selectivity for endothelial cells, promoting strong adhesion thereof. Consequently, certain areas of gold surfaces (strips) were cleaned by laser ablation and functionalized with the mixture 75% ELR-REDV – 25% ELR-RGD leading to a spatial segregation of the co-culture made of HUVEC and HFF1 cells. This platform therefore exhibits selective spatial control over cell adhesion associated with the bioactive epitopes (RGD and REDV) contained in the ELR sequence, since each functionalized surface (including strips) have similar topographic and hydrophobic characteristics and mechanical properties are in the same order of magnitude.
CHAPTER 1 75 1. Introduction Spatial cellular adhesion control plays a pivotal role in the production of novel cellular biosensors as well as in the development of tissue engineering constructs that require an organized structure with a specific placement of cells [1, 2]. This technique consists in creating specific areas in an artificial substrate where cells can be adhered or have resistant areas (non-adhesive zones) or even more have selective areas where only specific cells can adhere. Spatial arragement of cells is a new tool for cell biology that allows an improved control over cell behaviour and has a wide application in fundamental cell biology and biomedical engineering [3, 4]. In such a way, for the attachment of the cells on a solid substrate is necessary an interaction with specific surface-bound ligands that in vivo are allowed by the extracellular matrix (ECM): proteins such as collagen, fibronectin, elastin and laminin. The integrins are able to link the cell cytoskeleton to a material surface via these proteins present on the artificial substrate [5]. Surface bio-functionalization with cell-adhesion molecules has attracted significant interest as regards the design of surfaces with tailored properties, such as wettability, adhesion, and biocompatibility, which are essential for various biological evaluation such as controlling cellular response [6]. Currently, recombinant proteins such as elastin-like recombinamers (ELRs) are excellent candidates for the
CHAPTER 1 82 bioactive sequence, which showed antifouling behavior. The sequences of the three ELRs used in this work are: REDV:CCC((VPGIG)2(VPGKG)(VPGIG)2EEQIGHIPREDVDYHLYP (VPGIG)2(VPGKG)(VPGIG)2)10 RGD:CC((VPGIG)2(VPGKG)(VPGIG)2EEQIGHIPRGDDYHLYP(VP GIG)2(VPGKG)(VPGIG)2(VGVAPG)3)10 EI: CCC[(VPGVG)2VPGEG(VPGVG)2]10(VGIPG)60V The purity and molecular weight of the ELRs were verified by sodium dodecyl sulfate–polyacrylamide gel electrophoresis and matrixassisted laser desorption/ionization time-of-flight (MALDI-TOF) mass spectrometry. An amino acid composition analysis was also performed. Additional characterization of the ELRs was accomplished by infrared spectroscopy, differential scanning calorimetry (DSC) and nuclear magnetic resonance (NMR) techniques. The characterization results for the ELRs are provided in Supporting Information (see Figs. S1–S5 in Supporting Information). The corresponding ELR transition temperatures are: 31 °C (CC-RGD), 29 °C (CCC-REDV), and 30 °C (CCC-EI) (see Fig. S2 in Supporting Information). CC-RGD was designed with two cysteines in order to improve its production yield. Different number of cysteines does not affect the efficiency of grafting [36, 14].
CHAPTER 1 83 2.1.3 Cell culture Human umbilical vein endothelial cells (HUVEC) were purchased from Life Technologies S.A. (Madrid, Spain). These cells were cultured at 37 °C and 5% CO2 in MED200 culture medium (M200500, Life Technologies S.A, Madrid, Spain) supplemented with 100 U/100 mg/ Ml penicillin/streptomycin (15140-122, Invitrogen Corporation, Madrid, Spain). HUVEC between passages 2 and 6 were used in all experiments. Human foreskin fibroblasts (HFF1) were purchased from Life Technologies S.A. (Madrid, Spain) and were cultured in DMEM medium supplemented with 15% FBS and 100 U/100 mg/mL penicillin/streptomycin at 37 °C and 10% CO2. Fibroblasts between passages 6 and 10 were used in all experiments. 2.2. Methods 2.2.1. Surface cleaning/activation The surfaces were treated with Plasma Cleaner (Sterilizer PDC-002, Harrick Scientific Corporation, USA) using Argon plasma for 20 min at a high power setting (30W applied to the RF coil) in order to etch the surface before each experiment. 2.2.2. Surface functionalization After cleaning/activation by plasma treatment, the surfaces were immersed in ELR solutions with a concentration of 5 mg/mL for 6 h. Although
CHAPTER 1 84 several ELR concentrations were considered, a value 5 mg/mL was selected due to the homogeneous coverage obtained analyzed by SEM. Subsequently, several washing steps with milliQ water were performed in order to remove remnants of ELRs not grafted to the surfaces. Finally, the surfaces were dried under a nitrogen flow and submitted to several treatments reported below. 2.2.3. Contact angle Contact angle measurements were performed using the sessile drop method with a Data Physics OCA20 system instrument. The drop profile images during micro-syringe dispensation were recorded using an adapted CCD video camera. The stainless-steel needle tip was always kept at the top of the sessile drop and immersion of the needle into the drop was avoided during the measurements to prevent distortion of the drop shape by the needle. Ten measurements at 37 °C from different locations on each surface were measured to ensure a representative value of the contact angle. 2.2.4. X-ray photoelectron spectroscopy (XPS) XPS experiments were carried out using a Physical Electronics (PHI) 5500 spectrometer equipped with a monochromatic X-ray source (Al Ka line with an energy of 1486.6 eV and 350 W). The pressure inside the analysis chamber was 10−7 Pa. All measurements were performed at an angle of
CHAPTER 1 85 45° with respect to both the X-ray source and analyzer. Survey scans were taken in the range 0–1100 eV and high resolution scans were obtained for the C1s, N1s, O1s and Au peaks. The elemental surface composition was estimated from the area of the different photoemission peaks taken from the survey scans modified by their corresponding sensitivity factors. The signal coming from a circular spot area of 100 μm of radius has been collected. Different areas of each surface were analyzed and the average signal is calculated. 2.2.5. Scanning electron microscopy (SEM) Scanning electron microscopy (SEM) was used to investigate the surface morphology. Thus, the surfaces were immersed in recombinamer solutions with a concentration of 5 mg/mL for 6 h. After several washing steps with MilliQ water, the surfaces were dried with gaseous nitrogen. Micrographs were obtained using a scanning electron microscope (FEI Quanta 200 FEG) in low vacuum mode at 3 keV. Morphological details were evaluated quantitatively using the ZEN (Blue Edition, 2012) software package (Carl Zeiss Microscopy). 2.2.6. Atomic force microscopy (AFM) AFM measurements were performed using a Dimension 3100 microscope controlled by a Nanoscope IV controller system (Digital Instruments) in tapping mode using V-shaped Si3N4 tips (OMCL TR400PSA, Olympus,
CHAPTER 1 86 Japan). AFM images were taken from PBS immersed samples, with a nominal spring constant of 0.32 N/m. The scan area was 10 μm×10 μm and the root-mean-square (RMS) roughness of the surfaces was evaluated for regions of 1 μm×1μm. Surface roughness quantifies the vertical variations of a real surface from its ideal form. One of the most common parameters used to describe the degree of roughness of a surface is the root mean square (RMS) roughness, Rq, which is defined as: where “Zn” corresponds to the vertical height for a given point, 〈z〉 corresponds to the mean value of the surface height and N to the number of points in the sample area. Five randomized sections were created for each image to determine the surface roughness of the polymeric surfaces. 2.2.7. Quartz crystal microbalance with dissipation The QCM-D technique was applied in order to estimate the physical parameters representing the ELR thin film adsorbed on the surface [37, 38]. This technique allows simultaneous measurements of both frequency and energy dissipation changes. A Q-Sense Explorer System equipment (Biolin Scientific, Sweden) was used, with a peristaltic pump pumping every solution through the circular flow-through circuit at a flow rate of 50 μL/min. An AT-cut 5 MHz quartz crystal coated with gold (Biolin
CHAPTER 1 87 Scientific) was used as sensor, and the frequency and dissipation changes were recorded up to the 13th overtone number. The following sequence of flows (or events) was allowed to occur in each QCM-D measurement. First, since PBS was used as buffer for the polymer solutions, a flow of PBS at 23 °C was injected for 3 min to define a stable baseline, followed by the flow of the polymer solution under study at 23 °C for 20 min; next, a buffer rinse at 23 °C for 10 min. was accomplished; the last event corresponded to a buffer rinse at 37 °C for 15 min. Pure CC-RGD and pure CCC-REDV have been measured. Based on preliminary co-culture cellular assays that showed better performance with this ratio, a mixture of 75% REDV/ 25% RGD has been also measured. QCM-D measurements where the temperature of all the events (both polymer deposition and flows of PBS) is 37 °C have been also carried out. Three replicates were performed for each measurement. The QCM-D experimental data were numerically fitted to the Voigt (continuous) viscoelastic model using Dantzig’s Simplex algorithm as implemented in the software from Biolin Scientific (Q-Sense Dfind) [39, 40]. An explicit consideration of the frequency dependence of viscoelastic properties was assumed according to a power law. A descending incremental fitting was used, with the quality of the fitting being determined by the parameter χ2 (lower χ2 values
CHAPTER 1 88 indicate a better fitting). Only fits providing fitting without jumps between solutions in the resulting physical parameters have been considered. 2.2.8. Laser ablation After functionalization of the whole surface with 100% CC-RGD, some regions (width: 200 μm) were ablated using a smart beam MALDI laser in a MALDI TOF/TOF UltrafleXtrem instrument from Bruker (Center for Omic Sciences, Reus, Spain). Smartbeam technology combines the speed of a solid-state laser with the wide range of applications associated with nitrogen lasers. The new UltrafleXtreme, with a 1000 Hz smartbeam-II laser, enables laser focus diameters down to 10 μm for high spatial resolution imaging without pixel overlap. The Smartbeam MALDI laser was used at low intensity by preparing 500 shots/raster spots at 20% laser intensity and a large smartbeam. 2.2.9. In vitro cellular studies A reference standard cell adhesion curve for each cell type was created to convert sample fluorescence values into cell numbers per unit well area. HUVEC and HFF1 cells were labeled following the protocols for the PKH67 Fluorescent Cell Linker Kit and PKH26 Red Fluorescent Cell Linker Kit respectively, which were purchased from Sigma-Aldrich Quimica S.L. (Madrid, Spain). A range from 500 to 4000 cells were seeded on the functionalized surfaces and subsequently were incubated for 4 h at
CHAPTER 1 89 37 °C in a 5% CO2 atmosphere with the corresponding medium without adding FBS in either in order to avoid the interaction of serum proteins with the cell adhesive domains of the coatings. A fluorescence microplate reader with appropriate filters (490 nm excitation, and 502 nm emission for green fluorescence; 551 nm excitation, and 567 nm emission for red fluorescence) was used to measure the sample fluorescence. After the determination of the standard adhesion curves, cell adhesion studies were performed co-seeding onto the surfaces HUVEC and HFF1 cells previously labeled with PKH67 and PKH26 Red Fluorescent Cell Linker Kit, with a 1:1 ratio. Both of them were seeded at a density of 5 · 103 cells/surface using MED200 culture medium for the co-culture supplemented exclusively with 100 U/100 mg/mL penicillin/streptomycin. After 4 h of culture, the medium was removed and the functionalized surfaces were washed with DPBS (Dulbecco’s Phosphate- Buffered Saline, Life Technologies, Madrid, Spain). Adhesion was evaluated by measuring the fluorescence with a photometer plate reader. Fluorescence images were also used to count the HUVEC and HFF1 cells adhered to the strips using ImageJ software. 2.2.10. Statistical analysis Data are reported as mean±SD (n=3). Statistical analysis was evaluated by one-way analysis of variance using the Holm–Sidak method. A p value
CHAPTER 1 90 of<0.05 was considered to be statistically significant. (**) p < 0.001, (*) p < 0.05, and p > 0.05 indicates no significant differences (n.s.d.). 3. Results 3.1. Contact angle The functionalization of gold surfaces were characterized by contact angle measurements (Fig. 2). Thus, non-functionalized and non-activated (control) surfaces exhibited average contact angles of 57°, whereas after functionalization these values increased to around 92°. The contact angle for activated control surfaces was small enough to be measured under our experimental conditions (< 8°). As expected, the contact angle was significantly affected by functionalization, with the high value of the contact angle corresponding to a high surface hydrophobicity. No significant differences were found for the three samples functionalized with ELRs. Even after vigorous rinsing with MilliQ water, a layer of recombinamers remains grafted to the surface.
CHAPTER 1 91 Fig 2. Contact angle for a non-functionalized and non-activated surface (Au), surface functionalized with CC-RGD, surface functionalized with CCC-REDV and surface functionalized with CCC-EI. Data are reported as mean ± SD (n=3). Statistical analysis was evaluated by analysis of variance using the Holm–Sidak method. *p<0.05; n.s.d., no significant differences. 3.2. X-Ray photoelectron microscopy (XPS) XPS is the most widely used surface-analysis technique as it can be applied to a broad range of materials and provides valuable quantitative and chemical information about the surface of the material being studied. Detailed XPS spectra of some fundamental elements can be found in the Supporting Information (Fig. S6). Table 1 shows the atomic percentage for some significant surface atoms for the functionalized surfaces, control sample and the strip ablated and subsequently functionalized with 75%
CHAPTER 1 98 Voigt model is still useful) has been previously reported [44–46]. Yet, when the deposition event is accomplished at 23 °C no signal loss is found (Fig. 6). This different behavior with temperature is associated with the ELR transition temperature, Tt, where a conformational reorganization at the molecular level occurs, determining the deposition characteristics during the QCM measurement. The simultaneously measured shifts in frequency (normalized to the corresponding overtone, n), Δfn/n (Fig. 6a), and in energy dissipation, ΔDn (Fig. 6b), obtained at n=3 (15 MHz) are displayed as a function of time. Although measurements were carried out up to the 13th overtone (65 MHz) under our experimental conditions, only the third harmonic is shown for clarity. The frequency change at the fundamental frequency is not generally analyzed since this is affected by the flow of the bulk solution and is prone to more pronounced instabilities than the overtones [47–49]. Thus, only overtones are used for further quantitative analysis. Four events can be distinguished in the transient evolution: (i) flow of pure PBS at 23 °C to establish the baseline, (ii) flow of the polymer solution at 23 °C, (iii) pure buffer rinse at 23 °C, followed by (iv) a final pure buffer rinse at 37 °C to determine the impact of the conformational transition on the properties of the deposited thin film. At this point we will focus our attention on the results obtained for pure CCCREDV and pure CC-RGD (Fig. 6). Upon exposure to the polymer solution,
CHAPTER 1 99 the decrease in frequency indicates adsorption on the side of the sensor. A higher frequency change was observed for CCCREDV (around −53 Hz, n=3) than for CC-RGD (around −35 Hz, n=3). This mass uptake is accompanied by a strong increase in dissipation for both CCC-REDV and CC-RGD (up to 10×10−6, n=3; 7×10−6, n=3, respectively). Next event in the QCM-D experiment corresponds to rinsing with pure PBS solution at 23 °C to stabilize and eliminate any material accumulated on the surface. Thus, along with fairly small variations are found in the frequency changes, a similar dissipation for both ELRs is observed (at saturation, 3×10−6, n=3). The final stage corresponds to a PBS rinse at 37 °C. As can be seen, significant frequency and dissipation changes are found with respect to the PBS rinse at 23 °C. These experimental results suggest that a thin film stabilization occurs, more noticeable for the conformation at 37 °C. The frequency dependence observed for the three overtones in Supporting Information Fig. S8, and the high energy dissipation, indicate that the simple Sauerbrey model is not valid and therefore that a viscoelastic model is required. In this case, a Voigt viscoelastic model based on a single layer was used [39, 50, 40]. The adsorbed film is represented by a lateral homogeneous film with uniform thickness and density which, in our case, was estimated at 1.1 g/cm3 (corresponding to a hydrated protein) [51]. This film is situated between the sensor surface
CHAPTER 1 100 and on its other side is in contact with a semi-infinite bulk solution (in our case, PBS) that was assumed to be Newtonian, with a viscosity and density of 0.92 mPa.s and 1.005 g/cm3, respectively. No significant impact of surface roughness on the QCM experimental values is expected since, given the average RMS roughness obtained by AFM (< 1 nm for each polymer coating), the coated QCM sensor can be regarded as flat [37]. Moreover, within the resolution of the AFM images (Fig. 5) the thin film can be considered to be laterally homogeneous. Subsequent characterization of the adsorbed thin film was based on the QCM-raw data. Several sets of raw experimental data and the corresponding fitted curves can be found in the Supporting Information (Fig. S8). At the end of the third and four event, the Voigt model provides the parameters that characterize the stabilized thin film. The corresponding values for CCRGD, CCC-REDV and the mixture are summarized in Table 2. It should be pointed out that the rheological parameters are measured in the MHz frequency range, whereas rheological characterization is usually accomplished in the Hz-kHz range. It should also be noted that, during QCM measurements, liquid or solvent molecules may couple as an additional mass via direct hydration, viscous drag, or entrapment in cavities in the adsorbed film [38]. For both polymers after the PBS rinse at 37 °C, the conformational transformation gives rise to a decrease of the
CHAPTER 1 101 thickness. As can be seen, when the deposition event is carried out at 23 °C, film thickness are clearly lower than the viscous penetration depth around 140 nm and, therefore, the microbalance response become linear.
CHAPTER 1 102 Fig. 6. Normalized frequency (a) and energy dissipation shifts (b) measured at the third (n=3) overtone for CCC-REDV, CC-RGD and the mixture 75% REDV/25% RGD. Four events are distinguished: first, pure buffer (PBS) solution at 23 °C for 3 min; second, exposure to ELR solution at 23 °C for 20 min; third, pure buffer solution at 23 °C for 10 min., and finally, pure buffer solution at 37 °C for 15 min. 3.6. Selective cell adhesion on ELR-bio functionalized model gold surfaces The next step in this work consisted in determining the optimum mixture of CC-RGD and CCC-REDV in order to obtain selective adhesion of endothelial cells. A co-culture of HUVEC and HFF1 cells was used to that end. Adhesion was carried out under serum-free conditions in order to avoid the interference of soluble extracellular matrix (ECM) proteins
CHAPTER 1 103 found in the serum with the observed behavior. To achieve this goal, whole gold surfaces were functionalized with ELR mixtures comprising varying percentages of each ELR: a) 100% CCRGD, b) 25% CCC-REDV/75% CC-RGD, c) 50% CCC-REDV/50% CCRGD, d) 75% CCC-REDV/25% CC-RGD, and e) 100% CCC-REDV. A surface functionalized with CCC EI, which does not contain any bioactive sequence, was used as a negative control. In Fig. 7 the adhesion of HUVEC (green) and HFF1 (red) on each functionalized surface with different percentages of the recombinamer mixture can be seen from top to bottom: phase contrast (A1-A6), FITC channel (B1-B6, only the HUVEC cells are visualized), G-2A channel (C1-C6, for HFF1 visualization) and, finally, all channels merged (D1- D6). For HUVEC cells, there was no significant difference in adhesion on surfaces functionalized with 0%, 25% and 100% CCC-REDV, although a relatively minor increase in adhesion of these cells was observed on surfaces functionalized with 50% CCC-REDV. In contrast, a significant increase in the adhesion of HUVECs on surfaces functionalized with 75% CCC-REDV and 25% CC-RGD was observed. The quantity of cells adhered onto one square centimeter of various surfaces can be seen in Fig. 8. It can clearly be seen that the presence of the REDV sequence minimizes HFF1 adhesion. Thus, as the percentage of CCC-REDV recombinamer increases, the number of HFF1 cells adhered decreases
CHAPTER 1 104 considerably, thereby highlighting the significance of the REDV ligand for selective adhesion of endothelial cells on model gold surfaces. The presence of this motif provides an unfavorable environment for this cell type. In light of the above, we decided to use the mixture 75% CCCREDV/ 25% CC-RGD as the optimal mixture for our spatially selective cell cultures given the enhanced adhesion of endothelial cells. Fig. 7. HUVEC (membrane labeled with PKH67 Green Fluorescent Cell Linker Kit) and HFF1 (membrane labeled with PKH26 Red Fluorescent Cell Linker Kit) adhered to surfaces functionalized with 0% CCC-REDV, 25% CCC-REDV, 50% CCC-REDV, 75% CCC-REDV and 100% CCC-REDV, respectively. From top to bottom: image A shows the phase contrast for each percentage functionalization; image B the FITC channel to visualize HUVEC cells; image C the G-2A channel to visualize HFF1, and finally, all channels are merged in image D. Scale bar: 50 μm.
CHAPTER 1 105 3.7. Spatial control of endothelial cell behaviour Once the optimal percentage for selective adhesion of endothelial cells and the protocol for cleaning gold strips by laser ablation had been established, the next step was the selective functionalization of these strips. Thus, the strips were functionalized with the mixture of 75% CCC-REDV and 25% CC-RGD. This functionalization only takes place on those strips where a bare gold surface is available as the rest of the surface has been previously functionalized with the CC-RGD recombinamer. These surfaces were submitted to a co-culture of endothelial and HFF1 cells for 48 h in order to demonstrate a maximal cell selective confluence onto the strips. Cells were counted using ImageJ software. Interestingly, we observed a considerable increase of endothelial cells on the strips functionalized with 75% CCC-REDV/25% CC-RGD when compared with the other areas functionalized with 100% CC-RGD. Indeed, Fig. 9 clearly shows that the number of endothelial cells (green1) (Fig. 9c) onto the surfaces is higher than that for HFF1 (red) (Fig. 9b). Specifically, the number of endothelial cells present onto the strips is 520 ± 35, while the value for HFF1 cells is 175 ± 20. A noticeable spatial control of HUVEC adherence on the strip is therefore demonstrated. This result suggests that surface biofunctionalized with REDV or RGD-related peptides would likely promote
CHAPTER 1 106 preferential adherence of cell types with the appropriate cell-surface ligand. Fig. 8. Number of HUVEC (black) and HFF1 cells (white) adhered onto surfaces functionalized with different percentages of ELR (100% CC-RGD, 25% CCCREDV/ 75% CC-RGD, 50% CCC-REDV/50% CC-RGD, 75% CCCREDV/25% CCRGD and 100% CCC-REDV). Fig. 9. From left to right: image a shows the phase contrast of the strip ; image b the G-2A channel to visualize HFF1 present onto the strip; image c the FITC channel to visualize HUVEC cells, and finally all channels have been merged in image d. Scale bar: 100 μm.
CHAPTER 1 107 4. Discussion REDV sequence plays a critical role in the adhesion of endothelial cells while exhibits better cell-type selectivity due to its receptor in their membrane which is only expressed in limited cell-lines [15,52]. Although, this sequence is considered highly selective for endothelial cells, when present on its own it promotes only poor and weak adhesion despite its selectivity [15]. This validates the results obtained to date, namely that the presence of the RGD sequence in the mixture used to functionalize the surfaces is necessary to facilitate the adhesion of endothelial cells. Overall, we have demonstrated that the REDV sequence is a selective bioactive domain for endothelial cells by increasing their adhesion to a model gold surface. This selectivity towards endothelial cells in the presence of the REDV sequence further underlies the crucial bioactivity and, more importantly, selectivity provided by this ligand in cell adhesion and allowed us to demonstrate that adhesion of endothelial cells is markedly enhanced on those surfaces functionalized with 75% CCCREDV and 25% CC-RGD. The adhesion ratio of endothelial cells was significantly higher than for HFF1 cells, thus indicating a selective adhesion with respect to endothelial cells. In addition of cell adhesion sequences such as REDV and RGD, the ELRs contain cysteines at the amino-terminal region of their backbone as these are essential for grafting onto gold and avoid the use of
CHAPTER 1 114 [26] B. Kasemo, Biolog. Surf. Sci. Surf. Sci. 500 (2002) 656–677. [27] R.E. Russo, X. Mao, J.J. Gonzalez, V. Zorba, J. Yoo, Laser ablation in analytical chemistry, ACS Pub. (2013). [28] C. Momma, S. Nolte, Chichkov BN, Alvensleben Fv, Tünnermann A. Precise laser ablation with ultrashort pulses, Appl. Surf. Sci. 109 (1997) 15–19. [29] X. Liu, D. Du, G. Mourou, Laser ablation and micromachining with ultrashort laser pulses, IEEE J. Quant. Elect. 33 (1997) 1706–1716. [30] J. Yeh, Laser ablation of polymers, J. Vac. Sci. Tech. A Vac. Surf. Films 4 (1986) 653–658. [31] B.N. Chichkov, C. Momma, S. Nolte, F. Von Alvensleben, A. Tünnermann, Femtosecond, picosecond and nanosecond laser ablation of solids, Appl. Phys. A 63 (1996) 109–115. [32] A. Vogel, V. Venugopalan, Mechanisms of pulsed laser ablation of biological tissues, Chem. Rev. 103 (2003) 577–644. [33] M.E. Marques, A.A. Mansur, H.S. Mansur, Chemical functionalization of surfaces for building three-dimensional engineered biosensors, Appl. Surf. Sci. 275 (2013) 347– 360. [34] C. Momma, B.N. Chichkov, S. Nolte, F. von Alvensleben, A. Tünnermann, H. Welling, et al., Short-pulse laser ablation of solid targets, Optics Commun. 129 (1996) 134–142. [35] M. Shirk, P. Molian, A review of ultrashort pulsed laser ablation of materials, J. Laser Appl. 10 (1998) 18–28. [36] H. Häkkinen, The gold–sulfur interface at the nanoscale, Nat. Chem. 4 (2012) 443. [37] K. Rechendorff, M.B. Hovgaard, M. Foss, F. Besenbacher, Influence of surface roughness on quartz crystal microbalance measurements in liquids, J. Appl. phys. 101 (2007) 114502. [38] F. Höök, B. Kasemo, T. Nylander, C. Fant, K. Sott, H. Elwing, Variations in coupled water, viscoelastic properties, and film thickness of a Mefp-1 protein film during adsorption and cross-linking: a quartz crystal microbalance with dissipation monitoring, ellipsometry, and surface plasmon resonance study, Anal. Chem. 73 (2001) 5796–5804. [39] T. Smith, The hydrophilic nature of a clean gold surface, J. Coll. Interf. Sci. 75 (1980) 51–55. [40] B. Crist, A Review of XPS Data-Banks XPS Reports 2007//XPS Reports.–1 (2007) 1–52.
CHAPTER 1 115 [41] M. Schwartzkopf, A. Hinz, O. Polonskyi, T. Strunskus, F.C. Löhrer, V. Körstgens, et al., Role of sputter deposition rate in tailoring nanogranular gold structures on polymer surfaces, ACS Appl. Mater. Interf. 9 (2017) 5629–5637. [42] P. Malinský, P. Slepička, V. Hnatowicz, V. Švorčík, Early stages of growth of gold layers sputter deposited on glass and silicon substrates, Nanoscale Res. Lett. 7 (2012) 241. [43] K.K. Kanazawa, J.G. Gordon, Frequency of a quartz microbalance in contact with liquid, Anal. Chem. 57 (1985) 1770–1771. [44] G. Dunér, E. Thormann, A. Dėdinaitė, Quartz Crystal Microbalance with Dissipation (QCM-D) studies of the viscoelastic response from a continuously growing grafted polyelectrolyte layer, J. Collid Interf. Sci. 408 (2013) 229–234. [45] A. Granéli, M. Edvardsson, F. Höök, DNA-Based Formation of a Supported, Three- Dimensional Lipid Vesicle Matrix Probed by QCM-D and SPR, ChemPhysChem 5 (2004) 729–733. [46] M. Rodahl, B. Kasemo, On the measurement of thin liquid overlayers with the quartz-crystal microbalance, Sens. Actuat. A Phys. 54 (1996) 448–456. [47] A. Mechler, S. Praporski, K. Atmuri, M. Boland, F. Separovic, L.L. Martin, Specific and selective peptide-membrane interactions revealed using quartz crystal microbalance, Biophys. J. 93 (2007) 3907–3916. [48] C.M. Bailey, E. Kamaloo, K.L. Waterman, K.F. Wang, R. Nagarajan, T.A. Camesano, Size dependence of gold nanoparticle interactions with a supported lipid bilayer: A QCM-D study, Biophys. Chem 203 (2015) 51–61. [49] S.B. Nielsen, D.E. Otzen, Quartz Crystal Microbalances as Tools for Probing Protein- Membrane Interactions, Lipid-Protein Interactions, Springer, 2013, pp. 1–21. [50] T. Kacar, M.T. Zin, C. So, B. Wilson, H. Ma, N. Gul-Karaguler, et al., Directed selfimmobilization of alkaline phosphatase on micro-patterned substrates via genetically fused metal-binding peptide, Biotechnol. Bioeng. 103 (2009) 696–705. [51] J. Malmström, H. Agheli, P. Kingshott, D.S. Sutherland, Viscoelastic modeling of highly hydrated laminin layers at homogeneous and nanostructured surfaces: quantification of protein layer properties using QCM-D and SPR, Langmuir 23 (2007) 9760–9768. [52] S.P. Massia, J.A. Hubbell, Vascular endothelial cell adhesion and spreading promoted by the peptide REDV of the IIICS region of plasma fibronectin is mediated by integrin alpha 4 beta 1, J. Biolog. Chem. 267 (1992) 14019–14026. [53] B.V. Crist, A review of XPS data-banks, XPS Reports 1 (2007). [54] M.-C. Bourg, A. Badia, R.B. Lennox, Gold− sulfur bonding in 2D and 3D selfassembled monolayers: XPS characterization, J. Phys. Chem. B 104 (2000) 6562–6567.
CHAPTER 1 116 [55] M.L. Yola, N. Atar, A novel voltammetric sensor based on gold nanoparticles involved in p-aminothiophenol functionalized multi-walled carbon nanotubes: application to the simultaneous determination of quercetin and rutin, Electrochim. Acta 119 (2014) 24–31. [56] J.R. Reimers, M.J. Ford, S.M. Marcuccio, J. Ulstrup, N.S. Hush, Competition of van der Waals and chemical forces on gold–sulfur surfaces and nanoparticles, Nature Rev. Chem. 1 (2017) 0017. [57] M.J. Humphries, S.K. Akiyama, A. Komoriya, K. Olden, K.M. Yamada, Identification of an alternatively spliced site in human plasma fibronectin that mediates cell typespecific adhesion, J. Cell Biol. 103 (1986) 2637–2647. [58] N. Faucheux, R. Schweiss, K. Lützow, C. Werner, T. Groth, Self-assembled monolayers with different terminating groups as model substrates for cell adhesion studies,Biomaterials 25 (2004) 2721–2730. [59] Y. Lu, S. Chen, Micro and nano-fabrication of biodegradable polymers for drug delivery, Adv. Drug Delivery Rev. 56 (2004) 1621–1633.
CHAPTER 1 117 8. Supporting Information Characterization of materials 1. SDS-PAGE electrophoresis Figure S1. SDS PAGE electrophoresis of a) CC-RGD b) CCC-REDV c) CCC-EI 2. Amino acid analysis CCC-REDV CCC-EI CC-RGD AA Experimental Teoric Experimental Teoric Experimental Teoric D 25.81 25 6.53 6 E 50.28 50 11.31 10 2.64 3 S 11.33 12 H 15.82 16 G 213.51 210 225.43 224 168.90 168 T 4.96 4 R 10.55 10 4.61 4
CHAPTER 1 118 A 10.58 11 Y 19.98 20 C 3.20 3 3 3 3.39 3 V 110.27 111 149.31 150 78.77 80 M 0.4 1 0.39 1 0.25 1 I 95.49 100 59.82 60 64.39 64 L 9.75 10 3.70 4 K 11.51 12 16.86 16 P 119.86 120 109.09 110 85.71 85 Table S1. Aminoacidic composition of CCC-REDV, CCC-EI and CC-RGD 3. Differential scanning calorimetry (DSC)
CHAPTER 1 119 Figure S2. DSC thermograms of the solutions in PBS of CCC-REDV, CCC-EI and CCRGD (from top to bottom). 4. Fourier transformation infrared spectroscopy (FTIR) Figure S4. FTIR spectrum of a) CC-RGD b) CCC-REDV c) CCC-EI
CHAPTER 1 120 5. Matrix-assisted Laser Desorption/Ionization Time-of-flight (MALDI TOF)
CHAPTER 1 121 Figure S5. MALDI TOF spectrum of a) CC-RGD b) CCC-REDV c) CCC-EI 6. Nuclear magnetic resonance (NMR)
CHAPTER 1 122 Figure S5. NMR spectrum of a) CC-RGD b) CCC-REDV c) CCC-EI
CHAPTER 1 123 7. X-Ray photoelectron spectroscopy (XPS) Binding Energy 75 80 85 90 95 100 c/s 0,0 2,0e+4 4,0e+4 6,0e+4 8,0e+4 1,0e+5 1,2e+5 CONTROL CC-RGD 75% CCC-REDV 25% CC-RGD Figure S6. XPS spectrum of bare Au, 100% CC-RGD and 75% CCC-REDV 25% CCRGD.
CHAPTER 2 130 1. Introduction Tissue engineering is an interdisciplinary therapeutic field that aims to repair or even replace damaged tissues and organs, thus resulting in the recovery of their integrity and functionality. This discipline meets tissue- and organ-related medical needs by developing engineered constructs that are able to restore or enhance tissue or organ function. [1] Scaffolds for use in vascular tissue engineering, for example hydrogels, simulate most of the required properties for these tissues, thus making them ideal supports for the promotion of tissue regeneration. [2, 3] The presence of a network of vessel-like structures is essential in engineered constructs for the diffusion of nutrients and oxygen, thus providing a pro-angiogenic environment suitable for cell survival and tissue growth. [4] Neovascularization is obtained as a result of marked cell infiltration into the hydrogels, which can be facilitated by the presence of adhesion sequences that increase the quantity of cells, specifically endothelial cells in this case, along with proteolytic target sequences. These latter sequences are particularly important as they allow enzymatic degradation of the scaffold, thus favouring an adequate space to support extensive angiogenesis. [5]
CHAPTER 2 131 Elastin-like recombinamer (ELR)-based hydrogels are the most recent engineered constructs to have found a use in biomedicine and biotechnology as a result of their potential angiogenic properties. [6] [7] The presence of distinct bioactivities encoded into their backbone results in an increase in cell adhesion, thus contributing to an enhanced release of angiogenic factors and subsequent endothelial cell organization. [8] Moreover, these systems are characterized by other important properties, such as excellent biocompatibility, non-immunogenicity, optimal biomechanical properties and an ability to respond to different stimuli. [9] They also mimic the elastic properties of natural tissues due to the presence of elastin, which is crucial in tissue regeneration since it is one of the main components of the extracellular matrix (ECM). [10] [11] ELRs are obtained using recombinant DNA technologies that allow a clear-cut, complex and absolute control of the sequences, thus providing an ability to include different bioactive sequences, such as those guiding cell adhesion, differentiation and protease sensitivity. They are characterized by a self-assembly behaviour associated with a conformational re-organization at the molecular level. Thus, whereas the polymer chains are soluble in water below a transition temperature, above this temperature they self-assemble into nano- and micro-aggregates and become insoluble. This process is completely reversible. [12] [13, 14]
CHAPTER 2 132 In this work, the bioactivity of the ELR-based hydrogels was enhanced using two cell-adhesion sequences, namely RGD (arginine-glycine- aspartate) and REDV (arginine-glutamic-aspartate-valine), which were coded into their amino acid sequences. Various studies have shown that the RGD sequence promotes the attachment of different cell types and is the principal integrin-binding domain present within ECM proteins such as fibronectin, vitronectin, fibrinogen, osteopontin, and bone sialoprotein. [8] [15] [16-18] In contrast, the REDV sequence, which is derived from fibronectin, binds to endothelial cells selectively via integrin a4b1 and is well known to promote endothelial cell adhesion and migration when immobilized to a wide variety of biomaterials. [19] [20] Furthermore, the proteolytic site VGVAPG (valine-glycine-valine- alanine-proline-glycine), which is coded into one of the ELRs employed in this work, is known for its chemotactic activity with respect to various cell types, such as monocytes or fibroblasts, and it also upregulates metalloproteinases and is sensitive to proteolysis by elastolytic enzymes. [21] Various approaches are currently used to achieve better vascularization in scaffolds, such as implanting scaffolds with endothelial cells, the use of growth factors and the provision of a vascularized tissue. [22] [23] [24] Vascular endothelial growth factor (VEGF) is the main regulator of
CHAPTER 2 133 neovascularization and, specifically, VEGF165 is known to stimulate vascularization both in vitro and in vivo. [25] Several studies have demonstrated that the use of growth factor proteins has several inherent disadvantages, such as immunogenicity, lower stability and loss of bioactivity, therefore the use of shorter bioactive peptide sequences derived from a growth factor protein that confer the same bioactivity and cellular response is becoming increasingly common. [26] A vascular mimetic peptide known as QK has been widely studied as a promising candidate for the promotion and control of angiogenesis in tissue-engineering constructs. Indeed, it has been shown to possess a similar biological activity to VEGF as regards its ability to induce capillary formation and organization. In this regard, D’Andrea et al. designed and synthesized QK peptide and demonstrated that this peptide has a stable helical conformation in aqueous solution and that an alpha helix conformation to bind the ligand-receptor site is necessary for its functionality. QK is a synthetic 15-amino acid peptide based on the 17-25 alpha region of VEGF165 that binds to the main VEGF receptors, such as VEGFR-1 and VEGFR-2, and is required for the cell signalling pathway step in VEGF-R modulated angiogenesis. [27] [28] [29] Although initially used only as a locally delivered soluble factor, QK peptide has demonstrated promising therapeutic outcomes. Furthermore,
CHAPTER 2 134 it has been immobilized to hydrogels and been shown to retain its bioactivity under all conditions tested. [30, 31] [32] This peptide provides different advantages, especially a smaller size, ease of use in chemical reactions, lesser likelihood of triggering an immune response, and an ability to be more easily modified to include variations that allow the tuning of a biomimetic matrix system. The current study aims to demonstrate enhancement of the angiogenic activity of ELR-based hydrogels bearing a VEGF-mimetic peptide (QK peptide) both in vitro and in vivo, thus providing an alternative to the use of growth factor proteins in angiogenic signalling. Moreover, the inclusion of bioactive sequences such as RGD and REDV favours cell adhesion and the proteolytic site VGVAPG favours a customised cell biodegradation, which is an essential pre-requisite for hydrogels in tissue-engineering applications. Cell behaviour was initially studied in vitro employing a coculture of human umbilical vein endothelial cells (HUVEC) and human foreskin fibroblasts (HFF1), comparing the biological activity of hydrogels with a tethered QK peptide (ELR-QK) with that of hydrogels with soluble VEGF (ELR-VEGF) and with control hydrogels, in this case a factor-free ELR hydrogel (ELR). Subsequent in vivo studies were performed in mice by injecting cell-free ELR-based hydrogels (factor-free ELR and ELR-QK hydrogel)
CHAPTER 2 135 intramuscularly into a hind limb region in order to determine if the presence of this pro-angiogenic peptide enhances the formation of new functional capillaries within the hydrogels, which were detected by immunofluorescence staining with CD31. Figure 1. Schematic representation of a) composition of ELR-based hydrogel (REDV-ELR + RGD-QK ELR) b) ELR-QK hydrogel injected in mice c) ELRQK hydrogel invaded by different cell type d) formation of new capillaries into the hydrogel I) REDV-ELR II) RGD-QK ELR III) fibroblast cells IV) immune cells V) HUVEC cells VI) capillaries
CHAPTER 2 136 2. Materials and Methods 2.1 ELR bio-production, modification and characterization The ELRs used in this work have been previously described elsewhere. [33, 34] Briefly, they were produced using a 15‐L bioreactor and purified using a process known as Inverse Transition Cycling (ITC), which involves several cycles of precipitation (heating) and resuspension (cooling) of the supernatant. The final product obtained was dialysed against deionized water with several changes and freeze‐dried prior to storage. The ELRs obtained were characterized by SDS-PAGE electrophoresis, HNMR and FTIR spectroscopy and DSC. Two different ELRs, namely HRGD and REDV, were employed in this study. Chemical modification of these ELRs was achieved using click chemistry and their degree of modification confirmed by NMR and FTIR spectroscopy, respectively. (Figure S5-S6, Supporting Information) 2.2 QK peptide and recombinant human VEGF165 QK peptide (KLTWQELYQLKYKGI) was purchased from BACHEM (Switzerland) as a white powder. This peptide presents an azide group in the amino terminal region (5-Azido-pentanoyl-Lys-Lys-Leu-Thr-Trp- Gln-Glu-Leu-Tyr-Gln-Leu-Lys-Tyr-Lys-Gly-Ile-OH), which can be reacted with RGD-ELR previously modified with a cyclootyne group via a click reaction. The resulting recombinamer, known as RGD-QK, was
CHAPTER 2 137 characterized by NMR and FTIR spectroscopy, DSC and MALDI-TOF, thus confirming that QK peptide was correctly bound to the recombinamer (Figure S1-S4, Supporting Information). Recombinant Human Vascular Endothelial Growth Factor (VEGF165) was purchased from Lonza (Madrid) in a soluble form. 2.4 Mechanical and morphological properties of ELR-based hydrogels The chemically modified ELRs were crosslinked for subsequent formation of the hydrogels via a click reaction. Thus, the recombinamers, with a concentration of 50 mg/mL, were dissolved in PBS 1X and mixed at 4 °C. Specific molds were used to form the hydrogels, and the reaction mixture was maintained at 4 °C for 20 minutes to allow crosslinking. The VEGF hydrogels (ELR-VEGF) were prepared in an identical manner, with the sole difference that the human recombinant VEGF165 was added to the endothelial cell growth medium at a concentration of 10 ng/mL, as per the literature. [35] The elastic modulus of the hydrogels was measured using a TA Instruments AR2000 stress-controlled rheometer equipped with a 12 mm diameter load plate, at 1% strain and 37 °C. The hydrogels were kept in PBS to avoid sample shrinking below the diameter of the plate upon heating. Oscillatory experiments were performed within the linear
CHAPTER 2 138 viscoelasticity region, where storage (G’) and loss (G’’) moduli are independent of the stress magnitude. Three different hydrogels were tested (n = 3). Scanning electron microscopy (SEM) was used to investigate their morphology. Thus, hydrogels with a concentration of 50 mg/mL were dropped into liquid nitrogen, physically fractured, and subsequently freeze-dried. Micrographs were obtained using a scanning electron microscope (FEI Quanta 200 FEG) in low vacuum mode at 3 keV. Morphological details were evaluated quantitatively using the ZEN (Blue Edition, 2012) software package (Carl Zeiss Microscopy). 2.4 Cell cultures Human umbilical vein endothelial cells (HUVEC) were purchased from Lonza (Madrid, Spain) and were cultured in EGM-2 medium (M200500, Life Technologies S.A, Madrid, Spain) supplemented with EGM-2 Single Quot Kit Suppl. & Growth Factor (Lonza, Madrid, Spain) at 37 °C and 5% CO2. Human foreskin fibroblast (HFF1) were purchased from Life Technologies S.A. (Madrid, Spain) and were cultured in DMEM medium supplemented with 15% FBS and 100 U/100 mg/mL penicillin/streptomycin at 37 °C and 10% CO2. Cells between passages 2 and 4 were used in all experiments.
CHAPTER 2 139 2.5 In vitro 3D proliferation tests and histological analysis For in vitro studies, recombinamers with a concentration of 50 mg/mL were dissolved in EGM-2 medium and mixed at 4 °C. 10*106/mL of HUVEC and 3*106/mL of HFF1 cells were added to previously prepared ELR hydrogels. The hydrogels were formed in 96-well plates, with 45 µL of each recombinamer being mixed and kept at 4 °C for 20 minutes to allow crosslinking prior to subsequent addition of basal medium for the QK-hydrogels and with recombinant human VEGF165 for the VEGF- hydrogels. The 96-well plate containing the hydrogels was incubated at 37 °C and 5% CO2 for 21 days. All measurements were carried out in triplicate. Media were replaced every day for all the hydrogels. After incubation for 21 days, the hydrogels were fixed in 10% formalin for 4 hours, then dehydrated by immersion in ethanol solutions of increasing concentration, and then in xylene solution. Finally, they were immersed in paraffin for 3 hours and stored at -20 °C overnight. All samples were sliced on a microtome and stained with Haematoxylin‐Eosin following a general protocol. [36] 2.6 Ethical approval Experimental procedures involving the use of animals were approved by the Animal Care and Use Committee of the University of Valladolid in
CHAPTER 2 146 significantly higher than in factor-free ELR hydrogels (Figure 6-a1). A similar behaviour, namely that the number of cells which form clusters is higher in VEGF-ELR and QK-ELR than in factor free ELR hydrogels, the latter of which present a lower number of fused cells, was observed in samples stained with H&E. Despite these differences, it can be seen that factor-free ELR hydrogels (Figure 6-a1) still contain CD31 expression cells due to the presence of bioactive sequences such as RGD and REDV, which enhance cell adhesion and endothelial cell organization in vitro. Nevertheless, the difference between this latter sample and ELR-VEGF and ELR-QK hydrogels lies in the number of endothelial cell clusters formed. Thus, in ELR-VEGF (Figure 6-a2) and ELR-QK (Figure 6-a3) hydrogels, endothelial cells form a large number of cell aggregates or clusters in unorganized assemblies of more than five cells, whereas factor-free ELR hydrogels are characterized mainly by containing single cells within the hydrogel.
CHAPTER 2 147 Figure 4. H&E staining with 10X magnification of: a1) factor-free ELR hydrogel (ELR); (a2) ELR-VEGF; and (a3) ELR-QK hydrogel after co-culturing HUVEC and HFF1 cells for 21 days. b) 20X Magnification of: b1) factor-free ELR hydrogel (ELR); b2) ELR-VEGF; and b3) ELR-QK hydrogels. Black arrows indicate the presence of endothelial cells clusters. Scale bar: 500µm.
CHAPTER 2 148 Figure 5. Graphical representation of number of cells/cm2, as counted using Image J. Data are reported as mean ± SD (n=3). Statistical analysis was carried out by performing an analysis of variance using the Holm–Sidak method. *p<0.05; n.s.d., no significant difference. Figure 6. CD31 immunostaining of: a) factor-free ELR hydrogel (ELR); (b) ELR-VEGF; and (a3) ELR-QK hydrogel. Blue: DAPI staining. Green: CD31 expression. Scale bar: 50µm.
CHAPTER 2 149 3.3 In vivo behaviour of QK peptide The formation of new vasculature in the ELR hydrogels enhanced by QK peptide was evaluated in vivo using mice in which hydrogels were injected into a hind limb region. Two main samples, namely a factor-free ELR hydrogel (ELR) and ELR-QK hydrogel, were used for the in vivo analysis. This choice was based on the previous in vitro results, which demonstrated that the soluble VEGF and VEGF-mimetic peptides (QK peptide) exhibit similar biological activities. To get an overview of cell invasion in ELR hydrogels, histological H&E staining was performed; the corresponding images are shown in Figure 7 (factor-free ELR hydrogel (7a) and ELR-QK hydrogel (7b)). ELR- hydrogels are surrounded by a discontinuous line and labelled with the letter H, whereas host tissue is indicated with a letter T. Figures 7c and 7d, which are magnifications of Figures 7a and 7b, respectively, both show good biocompatibility as the hydrogels are well infiltrated by different cell types at three weeks post-injection. The hydrogels were entirely present up to 21 days, thus indicating early host cell infiltration, although there were clear differences between them. Thus, in ELR-QK hydrogels (Figure 7b), the cells reached the center of the hydrogel after three weeks, whereas the factor-free ELR hydrogel (Figure 7a) presented different areas that are almost intact, thus indicating
CHAPTER 2 150 a lack of cellular infiltration. This becomes clearer in Figure 8a, which is a magnification of a non-infiltrated area. Upon initial inspection, this difference suggests that QK peptide facilitates the recruitment of cells and tissue integration and increases the rate of cell migration. A closer examination of the ELR-QK sample stained with H&E (Figure 7d) indicated the formation of new capillaries with a uniform distribution inside the hydrogel. These new capillaries are indicated in Figure 7d with a black arrow, and the magnification in Figure 8b shows the presence of red blood cells forming the lumen of blood vessels surrounded by endothelial cells. [X] The size of the new capillaries formed varies between 25- and 50 μm. The total number of capillaries present in the hydrogel (>30) is significantly higher than for the factor-free ELR hydrogel. Indeed, new capillaries are completely absent from the factorfree ELR hydrogel (Figure 7a). This does not mean that they cannot be formed, however, simply that more time is needed for both complete colonization and for the organization of endothelial cells. To further confirm new capillary formation in the scaffolds, CD31 protein expression was also determined by immunohistochemical staining, which allowed us to confirm the presence of endothelial cells junction. (Figure 9) As shown in Figure 9e-9f, the new capillaries (indicated by the presence
CHAPTER 2 151 of green florescence) are located in the ELR-QK hydrogel, which contrasts with the situation for the factor-free ELR hydrogel, Figure 9b-9c. QK peptide therefore stimulates angiogenesis and enhances cellular migration, and therefore subsequent capillary structure formation, in vivo. These results agree with those obtained in vitro upon triggering the autophosphorylation of VEGFR2 intracellular domains, which leads to the induction of HUVEC proliferation, survival and migration. [41]
CHAPTER 2 152 Figure 7. H&E staining images of: a) ELR factor-free hydrogel; and b) ELR-QK hydrogel; c) magnification 20X of image a); d) magnification 20X of image b). The black arrows indicate the presence of capillaries formed. Scale bar: 100µm Figure 8. Magnification of H&E staining images of a non-colonized area of ELR factor-free hydrogel, which is indicated with a black circle. b) Magnification of ELR-QK hydrogel image in Figure 7b to better visualize the presence of new capillaries. Scale bar: 100µm.
CHAPTER 2 153 Figure 9. CD31 immunofluorescent staining images of: a-b-c) factor free ELR hydrogel (ELR) d-e-f) ELR-QK hydrogel. DAPI: nucleus staining (9a; 9d). CD31: expression of CD31 protein (9b; 9e). MERGED: merged channels (DAPI+CD31) (9c; 9f). Scale bar for all the images: 50 µm. 4. Discussion In recent years, one of the most important efforts undertaken to achieve functional vascularization in scaffolds utilized in tissue engineering has involved modulating angiogenesis by targeting VEGF and its receptors. [22] Indeed, a VEGF mimetic peptide known as QK is commonly used to improve vascularization into 3D scaffolds as this protein has been demonstrated to exhibit pro-angiogenic activity in vitro and in vivo by binding to VEGFRs, thus initiating VEGF-induced signalling cascades and giving rise to the formation of new capillaries. [42, 43] In this study, we proposed the use of QK peptide tethered chemically to ELR-based hydrogels via a click reaction to enhance vascularization within engineered constructs, which is also favoured by the presence of two main adhesion sequences, namely the universal cell-adhesion sequence RGD and a specific sequence for endothelial cells (REDV), encoded into their backbone. Moreover, the presence of the VGVAPG sequence codified into the recombinamer chains favours the chemotactic
CHAPTER 2 154 ability of monocytes and facilitates biodegradation of the ELR-based hydrogels by increasing their sensitivity to elastolytic enzymes. [8] Several previous studies reported in the literature used small peptides such as RGD and the collagen-binding CMP domain bonded chemically to PEG scaffolds to increase cell adhesion and proliferation. [44] The proteinaceous nature of ELRs results in an absolute control over the amino acid sequences, thus allowing codification of the adhesion sequences into their backbone and overcoming the limitations that may be presented by these chemically bonded peptides. [45] In addition, proteolytic biodegradation is an essential feature for promoting cellular infiltration, which subsequently induces an enhanced cellular migration into the scaffold. It has been shown herein that the presence of QK peptide does not affect the mechanical properties of the ELR-based hydrogels or their morphological features, although it significantly alters cell behaviour, such as proliferation, in the hydrogels. In light of this, we studied its biological activity in vitro using a co-culture of HUVEC and HFF1 cells, demonstrating that this peptide enhances cell proliferation, which in turn gives rise to the development of cell clusters and, subsequently, the formation of capillary structures. The use of a co-culture is mandatory before in vivo studies to confirm the biocompatibility of the hydrogels as
CHAPTER 2 155 well as their influence on in vitro angiogenesis. [46] These cell types were employed since they are the most widely used in angiogenesis assays given that the majority of ECM components produced provide support for capillary-like structure formation. A quantitative analysis involving in vitro assays showed that QK peptide has a similar biological activity to the soluble VEGF used as positive control. Moreover, an estimation of cell numbers in a histological section of ELR-QK, ELR-VEGF and factor-free ELR hydrogels confirmed that the former two samples contained similar numbers of cells and demonstrated significant differences with respect to factor-free ELR hydrogels. These studies allowed us to determine that the presence of QK peptide enhances cell proliferation. Small peptides have many benefits with respect to large proteins, such as a lack of denaturation, structural stability, ease of synthesis, absence of a need for a secondary conformation to preserve their biological activity, and they tend to be characterized by the absence of immunogenicity and toxicity. [47] Furthermore, the constant delivery of growth factors from a hydrogel to obtain the optimal concentrations and gradients required for precise spatial-temporal control remains a big challenge even though several strategies, such as covalent binding, use of carriers, electrostatic interactions, etc., have been used. [48] A major limitation of natural